Cathode material, cathode and lithium secondary battery including same

JP2024540133AActive Publication Date: 2024-10-31LG ENERGY SOLUTION LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024525491
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-29
Filing Date
2022-10-28
Publication Date
2024-10-31
Estimated Expiration
2042-10-28

AI Technical Summary

Benefits of technology

【0011】 本発明による正極材は、大粒径正極活物質として、1個のノジュールからなる単粒子を使用し、小粒径正極活物質として、2個~30個のノジュールの凝集体である疑似-単粒子を使用することで、電極の圧延時に粒子割れが少なく、充放電時の抵抗増加が抑制されるようにした。これにより、本発明の正極材を適用すると、寿命特性および抵抗特性に優れた二次電池を製造することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540133000001_ABST
    Figure 2024540133000001_ABST
Patent Text Reader

Abstract

The present invention relates to a bimodal cathode material including a large particle size cathode active material and a small particle size cathode active material, in which the large particle size cathode active material is a single particle consisting of one nodule, and the small particle size cathode active material is a pseudo-single particle that is an aggregate of 2 to 30 nodules.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0146643 filed on October 29, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a positive electrode material, a positive electrode including the same, and a lithium secondary battery, and more particularly to a bimodal positive electrode material that can achieve excellent life characteristics and resistance characteristics by applying large particle diameter particles and small particle diameter particles of a specific shape, and a positive electrode and a lithium secondary battery including the same. [Background technology]

[0003] A lithium secondary battery generally comprises a positive electrode, a negative electrode, a separator and an electrolyte, and the positive electrode and the negative electrode contain active materials capable of intercalating and deintercalating lithium ions.

[0004] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMnO4, etc.), lithium iron phosphate compound (LiFePO4), etc. have been used as positive electrode active materials for lithium secondary batteries. Among these, lithium cobalt oxide has the advantages of high operating voltage and excellent capacity characteristics, but the raw material cobalt is expensive and its supply is unstable, making it difficult to commercially apply it to large-capacity batteries. Lithium nickel oxide has poor structural stability and is difficult to achieve sufficient life characteristics. On the other hand, lithium manganese oxide has excellent stability but poor capacity characteristics. Therefore, in order to compensate for the problems of lithium transition metal oxides containing Ni, Co, or Mn alone, lithium composite transition metal oxides containing two or more transition metals have been developed, and lithium nickel cobalt manganese oxide containing Ni, Co, and Mn is widely used.

[0005] Conventional lithium nickel cobalt manganese oxides are generally in the form of spherical secondary particles formed by agglomeration of tens to hundreds of primary particles. However, in the case of lithium nickel cobalt manganese oxides in the form of secondary particles formed by agglomeration of many primary particles, there is a problem that particle cracking occurs easily in which the primary particles are separated during the rolling process during the manufacture of the positive electrode, and cracks occur inside the particles during the charge and discharge process. When particle cracking or cracking occurs in the positive electrode active material, the contact area with the electrolyte increases, and gas generation and deterioration of the active material due to side reactions with the electrolyte increase, which leads to a problem of reduced life characteristics.

[0006] In order to solve these problems, lithium nickel cobalt manganese oxide in the form of a single particle has been developed. The lithium nickel cobalt manganese oxide in the form of a single particle is made of one particle, and can be prepared by mixing a precursor for a positive electrode active material with a lithium source, and then over-firing the mixture at a high firing temperature. The positive electrode active material in the form of a single particle has a higher particle strength than the positive electrode active material in the form of a secondary particle, and thus can prevent particle cracking during electrode rolling. However, the single particle positive electrode active material has significantly lower lithium mobility than the positive electrode active material in the form of a secondary particle, and therefore, when the single particle positive electrode active material is used alone, there is a problem that the resistance is too high to ensure sufficient capacity and output characteristics. Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made to solve the above problems, and aims to provide a cathode material that includes a large particle size cathode active material and a small particle size cathode active material with controlled particle shape, thereby reducing particle cracking during electrode rolling and minimizing resistance increase during charge / discharge cycles.

[0008] Another object of the present invention is to provide a positive electrode and a lithium secondary battery having improved life characteristics and resistance characteristics by applying the above-mentioned positive electrode material. [Means for solving the problem]

[0009] According to one embodiment, the present invention provides a bimodal cathode material including a large particle size cathode active material and a small particle size cathode active material, in which the large particle size cathode active material is a single particle consisting of one nodule, and the small particle size cathode active material is a pseudo-single particle that is an aggregate of 2 to 30 nodules.

[0010] According to another embodiment, the present invention provides a positive electrode comprising the positive electrode material according to the present invention and a lithium secondary battery comprising the positive electrode. Effect of the Invention

[0011] The cathode material according to the present invention uses a single particle consisting of one nodule as the large particle diameter cathode active material, and uses a pseudo-single particle, which is an aggregate of 2 to 30 nodules, as the small particle diameter cathode active material, so that particle cracking is reduced during rolling of the electrode and an increase in resistance during charging and discharging is suppressed. As a result, by applying the cathode material according to the present invention, a secondary battery with excellent life characteristics and resistance characteristics can be manufactured. [Brief description of the drawings]

[0012] [Figure 1] 1 is a scanning electron microscope image showing the particle shape of large particle diameter positive electrode active material A produced in Production Example 1. [Diagram 2] 1 is a scanning electron microscope image showing the particle shape of large particle diameter positive electrode active material B produced in Production Example 2. [Diagram 3] 1 is a scanning electron microscope image showing the particle shape of large particle diameter positive electrode active material C produced in Production Example 3. [Figure 4] 1 is a scanning electron microscope image showing the particle shape of small particle diameter positive electrode active material D produced in Production Example 4. [Diagram 5] 1 is a scanning electron microscope image showing the particle shape of small particle diameter positive electrode active material E produced in Production Example 5. [Figure 6]FIG. 3 is a diagram showing the press densities of the positive electrode material powders of Examples 1 and 2 and Comparative Examples 1 to 4. [Figure 7] FIG. 2 is a graph showing high-temperature life characteristics of lithium secondary batteries to which the positive electrode materials of Examples 1 and 2 and Comparative Examples 1 to 4 are applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will now be described in more detail.

[0014] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0015] In the present invention, a "single particle" is a particle consisting of one single nodule. In the present invention, a "quasi-single particle" means a particle that is a complex formed by 30 or less nodules.

[0016] In the present invention, the term "nodule" refers to a particle unit body constituting a single particle or a quasi-single particle, and the nodule may be a single crystal lacking a crystalline grain boundary, or a polycrystal lacking a grain boundary when observed at a magnification of 5000 to 20000 times using a scanning electron microscope (SEM) or an electron backscatter diffraction (EBSD). The average grain size of the nodule refers to the arithmetic average value calculated after measuring the grain size of the nodule observed through SEM or EBSD.

[0017] In the present invention, the term "secondary particle" refers to a particle formed by agglomeration of several tens to several hundreds of primary particles. More specifically, a secondary particle is an agglomeration of 40 or more primary particles.

[0018] The term "particle" as used in the present invention includes any one or all of single particles, pseudo-single particles, primary particles, nodules, and secondary particles. 50 " means a particle size at 50% of the volume cumulative particle size distribution of the positive active material powder, and can be measured using a laser diffraction method. For example, the positive active material powder is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), and ultrasonic waves of about 28 kHz are irradiated at an output of 60 W, and a volume cumulative particle size distribution graph is obtained, and the particle size corresponding to 50% of the volume cumulative amount is obtained.

[0019] In the present invention, "particle strength" is measured by placing the positive electrode material powder in a particle strength measuring device (model: MCT-510), confirming the particle shape of the positive electrode active material to be measured under a microscope, and then applying force to the positive electrode active material particle with a tip to measure the force at which the particle breaks. Taking into account the deviation between particles, values ​​measured 30 or more times are mapped, and the average value is used as the particle strength value.

[0020] In the present invention, the "press density" was measured using HPRM-1000. Specifically, 5 g of the positive electrode material powder was placed in a cylindrical mold with a cross-sectional diameter of 1.2 cm, and the mold containing the positive electrode material was then pressed with a force of 2000 kgf. Next, the height of the pressed mold was measured with a Vernier caliper to obtain the press density.

[0021] In the present invention, the average number of nodules in a particle cross section of a positive electrode active material may be measured by the following method. A positive electrode manufactured using a positive electrode material is cut by ion milling, and a cross-sectional image in the thickness direction of the cut positive electrode is obtained using a scanning electron microscope (SEM). At least 30 particles are selected from each of the large particle size positive electrode active material particles and the small particle size positive electrode active material particles in the image, and the number of nodules in the cross section of each positive electrode active material particle is measured by SEM image analysis. The arithmetic mean value of the measured number of nodules is then calculated, and the value is evaluated as the average number of nodules in the particle cross section.

[0022] Cathode material The cathode material according to the present invention has an average particle size (D 50 ), that is, a large particle size positive electrode active material having a relatively large particle size and a small particle size positive electrode active material having a relatively small particle size.

[0023] The bimodal positive electrode material has an advantage that the small particle size positive electrode active material fills the voids of the large particle size positive electrode active material during rolling of the electrode, thereby increasing the electrode density, and thus realizing a high energy density. However, in the case of a bimodal positive electrode material using a conventional secondary particle type positive electrode active material, the particle strength of the large particle size positive electrode active material and the small particle size positive electrode active material are different from each other, and there is a problem that the particle cracking of the large particle size positive electrode active material becomes severe. In order to solve the above-mentioned problems, the present invention applies single particles and pseudo-single particles having high particle strength to the large particle size positive electrode active material and the small particle size positive electrode active material. Specifically, the present invention applies single particles as the large particle size positive electrode active material of the bimodal positive electrode material, and applies pseudo-single particles as the small particle size positive electrode active material. Here, the single particle means a particle consisting of one nodule, and the pseudo-single particle means an aggregate of 2 to 30, preferably 2 to 25, and more preferably 2 to 20 nodules.

[0024] The positive electrode active material in the form of single particle or pseudo-single particle has a higher particle strength than the existing positive electrode active material in the form of secondary particle, which is an agglomeration of tens to hundreds of primary particles, and therefore has less particle cracking during rolling, less change due to volume expansion and contraction during charging and discharging, and significantly reduces the occurrence of cracks inside the particles. Therefore, when single particles are used as the large particle size particles and pseudo-single particles are used as the small particle size particles as in the present invention, it is possible to minimize the deterioration of battery performance due to gas generation and cracks inside the positive electrode active material, and to manufacture a lithium secondary battery with excellent life characteristics, especially high temperature life characteristics.

[0025] However, when single particles or pseudo-single particles are used as the positive electrode active material, there is a problem that the lithium mobility is inferior to that of conventional positive electrode active materials in the form of secondary particles, the resistance increases, and the capacity characteristics and output characteristics are deteriorated. As a result of intensive research to develop a positive electrode material with excellent life characteristics and little increase in resistance, the inventors have found that when the particle morphology constituting the large particle size positive electrode active material and the small particle size positive electrode active material satisfies a specific condition, that is, when the large particle size positive electrode active material is in the form of a single particle and the small particle size positive electrode active material is in the form of a pseudo-single particle, the increase in resistance can be suppressed, and have completed the present invention.

[0026] During rolling of the electrode, cracks may occur along the interfaces between subparticles (i.e., primary particles and nodules) that make up the positive electrode active material particles. If cracks occur inside the active material, the electrolyte penetrates the cracks, increasing the resistance. Meanwhile, if cracks occur in a large particle size positive electrode active material, the area that comes into contact with the electrolyte due to the cracks is larger than in a small particle size positive electrode active material, resulting in a greater increase in resistance. Therefore, in the present invention, a single particle consisting of a single nodule is used as the large particle size positive electrode active material, thereby minimizing the occurrence of cracks in the large particle size positive electrode active material and suppressing the increase in resistance.

[0027] On the other hand, the number of nodules constituting the small particle diameter positive electrode active material may be 2 to 30, preferably 2 to 25, more preferably 2 to 20, and further preferably 2 to 10.

[0028] If the number of nodules constituting the small particle diameter positive electrode active material exceeds 30, particle cracking may occur during electrode rolling, resulting in reduced life characteristics. If the small particle diameter positive electrode active material is in the form of a single particle, the electrode rolling properties may decrease, resulting in a lower electrode density and reduced capacity characteristics.

[0029] Preferably, when the average aggregation number of nodules in the particle cross section of the small particle diameter positive electrode active material is r', 1 / r' can be 0.5 or less, preferably 0.1 to 0.5. According to the research of the present inventors, when 1 / r' satisfies the above range, a more excellent improvement effect in life characteristics and resistance characteristics is shown.

[0030] Meanwhile, the number of nodules constituting the large particle diameter positive electrode active material and the small particle diameter positive electrode active material can be adjusted by controlling the sintering conditions. In general, the positive electrode active material is manufactured by mixing a precursor, which is a transition metal hydroxide, with a lithium source and then sintering the mixture. The higher the sintering temperature and the longer the sintering time, the smaller the number of nodules constituting the positive electrode active material particles. Therefore, when manufacturing the positive electrode active material, the number of nodules constituting the positive electrode active material particles can be adjusted by adjusting the sintering temperature and / or sintering time. For example, when the large particle diameter positive electrode active material and the small particle diameter positive electrode active material have the same composition, the sintering temperature of the large particle diameter positive electrode active material can be made 20° C. or more, preferably 20° C. to 80° C. higher than the sintering temperature of the small particle diameter positive electrode active material, so that 1 / r' is 0.5 or less.

[0031] On the other hand, in the present invention, the large particle diameter positive electrode active material has an average particle diameter D 50 The small particle diameter positive electrode active material may have an average particle diameter D 50 The average particle diameter D of the large particle diameter positive electrode active material and the small particle diameter positive electrode active material can be 1 μm to 8 μm, preferably 3 μm to 8 μm, and more preferably 3 μm to 7 μm. 50When the above range is satisfied, the press density of the positive electrode material is increased, which improves the electrode density during electrode production, thereby achieving excellent energy density.

[0032] Meanwhile, in the present invention, the large particle size positive electrode active material and the small particle size positive electrode active material may each independently contain a lithium nickel-based oxide.

[0033] Specifically, the large particle size positive electrode active material and the small particle size positive electrode active material can each independently contain a lithium nickel-based oxide represented by the following [Chemical Formula 1].

[0034] [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O2

[0035] In the above Chemical Formula 1, M 1 can be Mn, Al or a combination thereof, preferably Mn or Mn and Al.

[0036] Said M 2 is at least one selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta and Nb, preferably at least one selected from the group consisting of Zr, Y, Mg and Ti, more preferably Zr, Y or a combination thereof. 2 Although the elements are not necessarily contained, when contained in an appropriate amount, they can play a role in promoting grain growth during firing and improving the stability of the crystal structure.

[0037] The a represents the molar ratio of lithium in the lithium nickel-based oxide, and can be 0.8 ≦ a ≦ 1.3, 0.9 ≦ a ≦ 1.3, or 1.0 ≦ a ≦ 1.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium nickel-based oxide can be stably formed.

[0038] The b represents the molar ratio of nickel among all the metals other than lithium in the lithium nickel-based oxide, and can be 0.8 ≦ b < 1, 0.82 ≦ b < 1, 0.83 ≦ b < 1, 0.85 ≦ b < 1 or 0.87 ≦ b < 1. When the molar ratio of nickel satisfies the above range, it shows a high energy density and enables the realization of a high capacity.

[0039] The c represents the molar ratio of cobalt among all the metals other than lithium in the lithium nickel-based oxide, and can be 0 < c < 0.2, 0 < c < 0.18, or 0.01 ≦ c ≦ 0.17. When the molar ratio of cobalt satisfies the above range, good resistance characteristics and output characteristics can be realized.

[0040] The d represents the molar ratio of the M 1 element among all the metals other than lithium in the lithium nickel-based oxide, and can be 0 < d < 0.2, 0 < d < 0.18, or 0.01 ≦ d ≦ 0.17. When the molar ratio of the M 1 element satisfies the above range, the structure stability of the positive electrode active material is excellent.

[0041] The e represents the molar ratio of the M 2 element among all the metals other than lithium in the lithium nickel-based oxide, and can be 0 ≦ e ≦ 0.1, or 0 ≦ e ≦ 0.05.

[0042] Meanwhile, the large particle diameter positive electrode active material and the small particle diameter positive electrode active material according to the present invention may further include a coating layer on the surface of the lithium nickel-based oxide particles, if necessary. Here, the coating layer may include one or more coating elements selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mn, Sr, Sb, Bi, Si, and S. When a coating layer is present on the surface of the lithium nickel-based oxide, the coating layer reduces the contact between the electrolyte and the lithium nickel-based oxide, thereby reducing the elution of transition metals and the generation of gas due to side reactions with the electrolyte. Preferably, the coating layer may include B, Co, Al, or a combination thereof, and more preferably may include Co. When the coating layer includes Co, it is possible to obtain an effect of suppressing side reactions with the electrolyte, as well as an effect of improving output and reducing resistance.

[0043] The large particle diameter positive electrode active material and the small particle diameter positive electrode active material may have the same composition or different compositions. For example, the Ni molar ratio of the large particle diameter positive electrode active material may be higher than the Ni molar ratio of the small particle diameter positive electrode active material. The large particle diameter positive electrode active material is in a single particle form, and therefore has better structural stability than the small particle diameter positive electrode active material in a pseudo-single particle form, and therefore has less structural deterioration due to heat or repeated charging and discharging even if it contains a high content of Ni. Therefore, when a lithium nickel-based oxide containing a relatively higher content of Ni is used as the large particle diameter positive electrode active material, a secondary battery having a high capacity and excellent life characteristics can be realized. Specifically, the large particle diameter positive electrode active material can contain a lithium nickel-based oxide containing nickel at 85 mol% or more, preferably 87 mol% or more, and the small particle diameter positive electrode active material can contain a lithium nickel-based oxide containing nickel at 80 mol% or more but less than 87 mol%, preferably 80 mol% to 86 mol%, and more preferably 83 mol% to 86 mol%.

[0044] On the other hand, the particle strength of the large particle diameter positive electrode active material is preferably higher than that of the small particle diameter positive electrode active material. Specifically, the particle strength of the large particle diameter positive electrode active material can be at least twice, preferably 2 to 4 times, more preferably 2 to 3 times, the particle strength of the small particle diameter positive electrode active material. When the particle strength of the large particle diameter positive electrode active material is at least twice the particle strength of the small particle diameter positive electrode active material, particle cracking of the large particle diameter positive electrode active material is minimized, and an excellent effect of suppressing resistance increase can be obtained.

[0045] Specifically, the particle strength of the large particle diameter positive electrode active material may be 150 MPa to 300 MPa, preferably 180 MPa to 220 MPa, and the particle strength of the small particle diameter positive electrode active material may be 75 MPa to 150 MPa, preferably 90 MPa to 110 MPa. When the particle strengths of the large particle diameter positive electrode active material and the small particle diameter positive electrode active material satisfy the above ranges, particle cracking during electrode rolling is minimized, and the porosity and electrode density of the active material layer of the positive electrode can be appropriately formed.

[0046] Meanwhile, the positive electrode material may contain the large particle diameter positive electrode active material and the small particle diameter positive electrode active material in a weight ratio of 60:40 to 90:10, preferably 70:30 to 80:20. When the weight ratio of the large particle diameter positive electrode active material and the small particle diameter positive electrode active material satisfies the above range, excellent capacity characteristics and life characteristics can be realized.

[0047] Meanwhile, the positive electrode material may have a press density of 3.0 g / cc to 4.0 g / cc, preferably 3.0 g / cc to 3.8 g / cc, and more preferably 3.0 g / cc to 3.6 g / cc, measured by pressing the positive electrode material powder at 2000 kgf. When the press density of the positive electrode material satisfies the above range, a secondary battery with excellent energy density can be manufactured.

[0048] positive electrode Next, the positive electrode according to the present invention will be described.

[0049] The positive electrode according to the present invention includes the positive electrode material according to the present invention. Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer includes the positive electrode material according to the present invention.

[0050] Since the positive electrode material has been described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.

[0051] The positive electrode current collector may contain a metal with high electrical conductivity, and is not particularly limited as long as the positive electrode active material layer is easily attached and is non-reactive in the voltage range of the battery. The positive electrode current collector may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode current collector may usually have a thickness of 3 μm to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive force of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0052] The positive electrode active material layer may optionally contain a conductive material and a binder, in addition to the positive electrode material, as necessary.

[0053] Here, the positive electrode material may be included in an amount of 80 wt% to 99 wt%, more specifically, 85 wt% to 98.5 wt%, based on the total weight of the positive electrode active material layer, and excellent capacity characteristics can be exhibited when included in the above content range.

[0054] The conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and among these, one type alone or a mixture of two or more types can be used. The conductive material can be included in an amount of 0.1% by weight to 10% by weight based on the total weight of the positive electrode active material layer.

[0055] The binder plays a role of improving adhesion between the positive electrode particles and the adhesive strength between the positive electrode and the current collector.Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and polymers in which hydrogen is replaced by Li, Na, or Ca, or various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be contained in an amount of 0.1% by weight to 15% by weight based on the total weight of the positive electrode active material layer.

[0056] The positive electrode can be manufactured by a normal method for manufacturing a positive electrode, except for using the positive electrode material described above. Specifically, the positive electrode can be manufactured by applying a positive electrode mixture, which is manufactured by dissolving or dispersing the positive electrode material described above and, if necessary, a binder, a conductive material, and a dispersant in a solvent, onto a positive electrode current collector, followed by drying and rolling, or by casting the positive electrode mixture onto another support, followed by peeling it off from the support and laminating the resulting film onto a positive electrode current collector.

[0057] The solvent may be a solvent commonly used in the art, and examples of the solvent include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethyl formamide (DMF), acetone, and water, and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, binder, and dispersant in consideration of the coating thickness of the slurry and the manufacturing yield, and to have a viscosity that can show excellent thickness uniformity when applied to manufacture a positive electrode.

[0058] Lithium secondary battery Next, the lithium secondary battery according to the present invention will be described.

[0059] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. Since the positive electrode is as described above, a detailed description thereof will be omitted, and only the remaining components will be described in detail below.

[0060] Also, the lithium secondary battery may optionally further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0061] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0062] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 μm to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0063] The negative electrode active material layer includes a negative electrode active material, and optionally a binder and a conductive material.

[0064] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. Also, a metallic lithium thin film may be used as the negative electrode active material. The negative electrode active material may be included in an amount of 80 wt% to 99 wt% based on the total weight of the negative electrode active material layer.

[0065] The binder is a component that facilitates bonding between the conductive material, the active material, and the current collector, and is usually added in an amount of 0.1% by weight to 10% by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.

[0066] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0067] The negative electrode active material layer may be manufactured by coating a negative electrode mixture, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material, in a solvent, on a negative electrode current collector and drying the coated negative electrode mixture. Alternatively, the negative electrode mixture may be cast on a separate support, and then peeled off from the support to obtain a film, which may be laminated on the negative electrode current collector.

[0068] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single-layer or multi-layer structure.

[0069] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0070] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0071] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as polycarbonate (PC) and polycarbonate-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a straight-chain, branched or cyclic hydrocarbon group having 2 to 20 carbon atoms, which may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low-viscosity straight-chain carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred.

[0072] The lithium salt can be used without any particular limitation as long as it is a compound that can provide lithium ions used in lithium secondary batteries. Specifically, the anion of the lithium salt is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - The lithium salt may be at least one selected from the group consisting of LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The lithium salt is preferably used in a concentration range of 0.1M to 4.0M. When the lithium salt concentration is within the above range, the electrolyte has appropriate conductivity and viscosity, and therefore excellent electrolyte performance can be exhibited, and lithium ions can be effectively transferred.

[0073] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethyl alcohol amine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethyl alcohol, and aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery. Here, the additives may be contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.

[0074] As described above, the lithium secondary battery including the bimodal cathode material according to the present invention stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0075] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0076] The battery module or the battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0077] The external shape of the lithium secondary battery of the present invention is not particularly limited, and may be a cylindrical shape using a can, a square shape, a pouch shape, a coin shape, or the like.

[0078] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for a small device, but also preferably as a unit battery in a medium- to large-sized battery module including a large number of battery cells.

[0079] Examples of the medium to large devices include, but are not limited to, electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0080] The present invention will now be described in more detail with reference to specific examples.

[0081] Production Example 1 - Production of large particle size positive electrode active material A (single particle) Average particle size D 50 Ni with a thickness of 12 μm 0.88 Co 0.08 Mn 0.04 (OH)2 and LiOH were mixed so that the molar ratio of transition metals (Ni+Co+Mn):Li was 1:1.03, and the mixture was fired at 850°C for 12 hours to produce large particle size positive electrode active material A (LiNi 0.88 Co 0.08 Mn 0.04 The prepared positive electrode active material A powder was observed with a scanning electron microscope (SEM) to confirm the particle morphology. FIG 1 shows an SEM image of the positive electrode active material A prepared by the above method. As shown in FIG 1, the positive electrode active material A had a single particle morphology consisting of one nodule.

[0082] Production Example 2 - Production of large particle size positive electrode active material B (secondary particles) The large particle size positive electrode active material B (LiNi 0.88 Co 0.08 Mn 0.04The powder of the prepared positive electrode active material B was observed with a scanning electron microscope to confirm the particle morphology. Figure 2 shows an SEM image of the positive electrode active material B prepared by the above method. As shown in Figure 2, the positive electrode active material B had a secondary particle morphology in which one or more primary particles were aggregated.

[0083] Production Example 3 - Production of large particle size positive electrode active material C (pseudo-single particle) The large particle size positive electrode active material C (LiNi 0.88 Co 0.08 Mn 0.04 The powder of the prepared positive electrode active material C was observed by a scanning electron microscope to confirm the particle morphology. FIG. 3 shows an SEM image of the positive electrode active material C prepared by the above method. As shown in FIG. 3, the positive electrode active material C had a pseudo-single particle morphology in which 10 to 20 nodules were aggregated.

[0084] Production Example 4 - Production of small particle diameter positive electrode active material D (pseudo-single particle) Average particle size D 50 Ni with a thickness of 3.7 μm 0.86 Co 0.08 Mn 0.06 (OH)2 and LiOH were mixed so that the molar ratio of transition metals (Ni+Co+Mn):Li was 1:1.05, and the mixture was baked at 800°C for 12 hours to produce small particle diameter positive electrode active material D (LiNi 0.86 Co 0.08 Mn 0.06 The prepared positive electrode active material D powder was observed with a scanning electron microscope to confirm the particle morphology. FIG. 4 shows an SEM image of the positive electrode active material D prepared by the above method. As shown in FIG. 4, the positive electrode active material D prepared by the above method had a pseudo-single particle morphology in which 10 to 20 nodules were aggregated.

[0085] Production Example 5 - Production of small particle size positive electrode active material E (secondary particles) The particle positive electrode active material E (LiNi 0.86 Co 0.08Mn 0.06 The powder of the prepared positive electrode active material E was observed with a scanning electron microscope to confirm the particle morphology. FIG. 5 shows an SEM image of the positive electrode active material E prepared by the above method. As shown in FIG. 5, the positive electrode active material E had a secondary particle morphology in which several tens of primary particles were aggregated.

[0086] Example 1 The large particle diameter positive active material A prepared in Preparation Example 1 and the small particle diameter positive active material D prepared in Preparation Example 4 were mixed in a weight ratio of 80:20 to prepare a positive electrode material.

[0087] Example 2 The large particle diameter positive active material A prepared in Preparation Example 1 and the small particle diameter positive active material D prepared in Preparation Example 4 were mixed in a weight ratio of 70:30 to prepare a positive electrode material.

[0088] Comparative Example 1 The large particle diameter positive active material B prepared in Preparation Example 2 and the small particle diameter positive active material E prepared in Preparation Example 5 were mixed in a weight ratio of 80:20 to prepare a positive electrode material.

[0089] Comparative Example 2 The large particle diameter positive active material B prepared in Preparation Example 2 and the small particle diameter positive active material D prepared in Preparation Example 4 were mixed in a weight ratio of 80:20 to prepare a positive electrode material.

[0090] Comparative Example 3 The small particle diameter positive electrode active material D produced in Production Example 4 was used alone to produce a positive electrode material.

[0091] Comparative Example 4 The large particle diameter positive active material C prepared in Preparation Example 3 and the small particle diameter positive active material D prepared in Preparation Example 4 were mixed in a weight ratio of 80:20 to prepare a positive electrode material.

[0092] Experimental example 1: Press density 5 g of the cathode material powder of Examples 1 and 2 and Comparative Examples 1 to 4 was placed in a cylindrical mold with a cross-sectional diameter of 1.2 cm, and the mold containing the cathode material was then pressed with loads of 400 kgf, 800 kgf, 1200 kgf, 1600 kgf, and 2000 kgf. The height of the pressed mold was then measured with a Vernier caliper to determine the press density. The measurement results are shown in FIG. 6 below. Referring to FIG. 6, it can be seen that the cathode materials of Examples 1 and 2 exhibit higher press density than the cathode materials of Comparative Examples 1 to 4.

[0093] Experimental Example 2: Measurement of the number of subparticle agglomerates on the cross section of a particle The positive electrode materials prepared in Examples 1 to 2 and Comparative Examples 1 to 4, conductive material (carbon nanotubes, LB-CNT), and PVdF binder were mixed in a weight ratio of 97.2:1.2:1.6 in N-methylpyrrolidone to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried, and rolled to prepare a positive electrode.

[0094] The manufactured positive electrode was cut by ion milling to obtain a cross-sectional image in the thickness direction, and 30 particles were selected from each of the large particle size positive active material and the small particle size positive active material by image analysis to measure the number of nodules or primary particles in each particle cross section. The arithmetic mean value of the number of nodules or primary particles in the particle cross section measured for the 30 large particle size positive active material particles was taken as the average aggregation number r of nodules or primary particles in the particle cross section of the large particle size positive active material, and the arithmetic mean value of the number of nodules or primary particles in the particle cross section measured for the 30 small particle size positive active material particles was taken as the average aggregation number r' of primary particles in the particle cross section of the small particle size positive active material. The measurement results are shown in Table 1 below.

[0095] [Table 1]

[0096] Experimental example 3: Evaluation of life characteristics <Secondary battery manufacturing> The positive electrode materials prepared in Examples 1 to 2 and Comparative Examples 1 to 4, conductive material (carbon nanotubes, LB-CNT), and PVdF binder were mixed in a weight ratio of 97.2:1.2:1.6 in N-methylpyrrolidone to prepare a positive electrode slurry. The positive electrode slurry was applied to one side of an aluminum current collector, dried, and rolled to prepare a positive electrode.

[0097] Anode active material (SiO and graphite mixture, graphite:Si weight ratio = 94.5:3.3), conductive material Super C65 and single-walled CNT mixed in a weight ratio of 98:2, and SBR binder (M37, LG Chem) were mixed in water in a weight ratio of 95.57:1:3.43 to prepare anode slurry. The anode slurry was applied to one side of a copper current collector, dried, and rolled to prepare anode.

[0098] A separator was disposed between the positive electrode and the negative electrode, and the resulting mixture was inserted into a battery case, and an electrolyte was injected to prepare a lithium secondary battery.

[0099] The lithium secondary battery manufactured as described above was charged at 45° C. at 0.5 C to 4.25 V and discharged at 1 C to 2.5 V as one cycle, and 50 charge / discharge cycles were performed to measure the DCIR increase and capacity retention. The measurement results are shown in FIG. 7 and Table 2 below.

[0100] Here, the resistance increase rate and the capacity retention rate were calculated according to the following formulas 1 and 2.

[0101] Equation 1: Resistance increase rate (%) = {(resistance after 50 cycles / resistance after 1 cycle) x 100} - 100

[0102] Equation 2: Capacity retention rate (%) = (discharge capacity after 50 cycles / discharge capacity after 1 cycle) x 100

[0103] [Table 2]

[0104] As shown in Table 2 and FIG. 7, the lithium secondary batteries using the positive electrode materials of Examples 1 and 2 exhibited superior effects in terms of capacity retention rate and resistance increase rate compared to the lithium secondary batteries using the positive electrode materials of Comparative Examples 1 to 4.

Claims

1. A bimodal positive electrode material including a large particle size positive electrode active material and a small particle size positive electrode active material, the large particle size positive electrode active material is a single particle consisting of one nodule, The small particle size positive electrode active material is a pseudo-single particle that is an agglomerate of 2 to 30 nodules.

2. 2. The positive electrode material according to claim 1, wherein when an average agglomeration number of nodules in a cross section of a particle of the small particle diameter positive electrode active material is r', 1 / r' is 0.5 or less.

3. 3. The cathode material according to claim 2, wherein the 1 / r′ is 0.1 to 0.

5.

4. The large particle diameter positive electrode active material has an average particle diameter D 50 is 10 μm to 20 μm, The small particle diameter positive electrode active material has an average particle diameter D 50 The cathode material according to claim 1, wherein the average particle size is 1 μm to 8 μm.

5. The positive electrode material according to claim 1, wherein the large particle diameter positive electrode active material and the small particle diameter positive electrode active material each independently contain a lithium nickel-based oxide represented by the following [Chemical Formula 1]: [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O 2 In the above Chemical Formula 1, M 1 is Mn, Al or a combination thereof, M 2 is one or more selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta, and Nb, and 0.8≦a≦1.2, 0.83≦b<1, 0<c<0.17, 0<d<0.17, and 0≦e≦0.

1.

6. 2. The positive electrode material according to claim 1, wherein the particle strength of the large particle size positive electrode active material is at least twice as high as the particle strength of the small particle size positive electrode active material.

7. The particle strength of the large particle diameter positive electrode active material is 150 MPa to 300 MPa, 2. The positive electrode material according to claim 1, wherein the particle strength of the small particle diameter positive electrode active material is 75 MPa to 150 MPa.

8. The cathode material according to claim 1, wherein the cathode material contains a large particle size cathode active material and a small particle size cathode active material in a weight ratio of 60:40 to 90:

10.

9. 2. The cathode material according to claim 1, wherein the cathode material has a press density of 3.0 g / cc to 4.0 g / cc, as measured by pressing the cathode material at 2000 kgf.

10. A positive electrode comprising the positive electrode material according to any one of claims 1 to 9.

11. A lithium secondary battery comprising the positive electrode according to claim 10.

Citation Information

Patent Citations

  • Lithium cobaltate, manufacturing method of the same and non-aqueous electrolyte secondary battery

    JP2004182564A

  • High Performance Cathode Materials for Lithium Batteries

    JP2009530224A

  • Cathode material, cathode, and lithium secondary battery containing lithium manganese-based cathode active material with spinel structure

    JP2020532842A

  • Alkoxysilyl group-containing organic silazane compound, method for producing same, composition containing same and cured product

    KR1020200122240A

  • Non-aqueous electrolyte secondary battery

    WO2021059857A1