Lithium-ion battery silicon carbon anode material and preparation method and use

The use of a porous carbon-based film for uniform nanosilicon deposition in lithium-ion batteries addresses issues of volumetric expansion and cycling performance, resulting in high-capacity and efficient battery performance.

JP2024540227AActive Publication Date: 2024-10-31HUNAN SHINZOOM TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024525882
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-25
Filing Date
2022-10-27
Publication Date
2024-10-31
Estimated Expiration
2042-10-27

AI Technical Summary

Technical Problem

Conventional lithium-ion battery negative electrode materials face challenges such as low theoretical specific capacity, poor cycling performance due to volumetric expansion, and complex preparation methods that hinder industrial production and electrochemical performance.

Method used

A method utilizing a porous carbon-based film material for uniform vapor phase deposition of nanosilicon particles, controlling gas flow and deposition within the porous carbon material to alleviate volumetric expansion and improve electrochemical performance.

Benefits of technology

The method achieves high-capacity and efficient lithium-ion battery performance by uniformly depositing nanosilicon, reducing volumetric expansion and enhancing cycling stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540227000001
    Figure 2024540227000001
  • Figure 2024540227000002
    Figure 2024540227000002
  • Figure 2024540227000003
    Figure 2024540227000003
Patent Text Reader

Abstract

The present application provides a lithium-ion battery silicon carbon anode material and its preparation method and use. [Means] The preparation method includes the steps of: (1) fixing a porous carbon-based film material in a reactor, and then introducing an inert gas to replace the air in the reactor, thereby making the reactor an oxygen-free environment; (2) sequentially heating and keeping the reactor in an oxygen-free environment described in step (1), and then introducing silane gas to carry out a chemical vapor deposition reaction to obtain a precursor of silicon-carbon anode material; and (3) treating the precursor of carbon anode material obtained in step (2) to obtain the lithium-ion battery silicon-carbon anode material. The preparation method uses a porous carbon-based film material to realize uniform vapor deposition of nanosilicon particles, effectively alleviating the problem of volume expansion during silicon cycling, while effectively improving the polarization state of the material through carbon deposition, thereby effectively improving the electrochemical performance of the silicon-carbon anode material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of lithium ion battery anode materials, and in particular to lithium ion battery silicon carbon anode materials and their preparation methods and uses. [Background technology]

[0002] Lithium-ion batteries have great potential applications and wide demand in the fields of portable electronic devices, electric vehicles, and large-scale energy storage. The anode materials selected in traditional lithium-ion battery systems are mainly graphite-based materials. Graphite-based materials have a low theoretical specific capacity of 372 mAh g -1 It is difficult to meet the high energy density requirements of new lithium-ion batteries with only these materials, so the development of new high-capacity lithium-ion battery anode materials is of crucial importance.

[0003] Silicon has an extremely high theoretical capacity (4200mAh / g) and a suitable lithium desorption potential, and is considered a new generation lithium ion battery anode material, attracting much attention and research interest. However, defects such as low initial coulombic efficiency and poor cycle performance due to the extremely large volume change rate (>300%) during the charge and discharge process of silicon are hindering factors that restrict the commercial operation of silicon-based lithium ion battery anode materials.

[0004] In the conventional method of preparing nanosilicon by chemical vapor deposition, the silicon source is easily agglomerated on the carbon base material after decomposition to form particulate or linear products of the order of microns, which causes the unique advantages of nanosilicon to be lost; furthermore, when the silicon carbon anode material made of nanosilicon is used as is, the nanosilicon is difficult to disperse uniformly in the entire system, which leads to the expansion rate of the electrode pieces being too large during the charge and discharge process, which further deteriorates the performance of the material.

[0005] CN104103821A discloses a method for preparing silicon carbon anode material. The method includes the steps of: (1) introducing a catalyst into a chemical vapor deposition reaction chamber; (2) heating the chemical vapor deposition reaction chamber, introducing a reactive gas source and a carrier gas into the chemical vapor deposition reaction chamber, and passing the Si-Siox generated during the chemical vapor reaction through the dynamically rotating carboxylated carbon substrate to prepare a precursor of the silicon carbon anode material; and (3) coating the precursor with organic pyrolytic carbon and then baking in a non-oxidizing atmosphere to obtain a silicon carbon anode material. Although this method can prepare nanosilicon with a high specific capacity, silicon cannot be distributed sufficiently and uniformly over the entire surface of the carbon substrate, which may cause deterioration of cycle performance and excessive volume expansion of the material.

[0006] CN1903793 discloses a carbon silicon composite material and its preparation method and use. The silicon carbon composite material includes a silicon substrate and carbon nanotubes or nano carbon fibers grown thereon. The carbon nanotubes or nano carbon fibers have a straight geometric appearance, or a bent or spiral geometric appearance. There are several methods for preparing the carbon silicon composite material. After loading a catalyst on a silicon material, or mixing the catalyst with silicon particles or preparing an alloy, the carbon nanotubes or nano carbon fibers can be deposited by chemical vapor deposition. The carbon nanotubes or nano carbon fibers grown on the surface by this method have a large specific surface area and a large porosity, but the silicon particles cannot be distributed uniformly on the surface, so the problem of the volume expansion of the silicon particles during the cycle process cannot be solved.

[0007] CN109449388A discloses a method for preparing a lithium-ion battery carbon silicon anode material. The preparation method includes the steps of: (1) homogeneously mixing starch and catalyst, carbonizing under vacuum conditions, and washing, drying, grinding and sieving to obtain porous carbon; (2) mixing an aqueous graphite solution and an aqueous nanosilicon solution, adding them to the porous carbon prepared in step (1) and mixing, drying, grinding and sieving the mixture; and (3) dissolving an organic carbon source in water, sequentially adding the product in step (2) and concentrated sulfuric acid, stirring the mixed solution, keeping warm, washing and drying, and then vacuum carbonizing to obtain a lithium-ion battery carbon silicon anode material. The method uses graphite as a buffer for the volume expansion of silicon particles, but the theoretical specific capacity of graphite-based materials is low, making it difficult to meet the requirements for high energy density of new lithium-ion batteries, and the preparation method is complicated, which is disadvantageous for industrialized production.

[0008] Therefore, providing a method for preparing industrial silicon-carbon composite materials using silicon, which can alleviate the problem of volume expansion during the silicon cycle while reducing production difficulty, is one of the problems that need to be solved urgently in the field. Summary of the Invention [Problem to be solved by the invention]

[0009] The following is a general summary of the subject matter described herein that is not intended to limit the scope of the claims.

[0010] In view of the deficiencies in the prior art, the present application aims to provide a lithium-ion battery silicon carbon anode material and its preparation and use, which utilizes a porous carbon-based film material to realize uniform nano-silicon particle vapor deposition, effectively alleviating the problem of volume expansion during silicon cycling, while effectively improving the polarization state of the material through carbon deposition, thereby effectively improving the electrochemical performance of the silicon carbon anode material. [Means for solving the problem]

[0011] To achieve this objective, the present application provides the following technical solutions:

[0012] In a first aspect, the present application provides a method for preparing a lithium ion battery silicon carbon anode material, comprising: (1) fixing the porous carbon-based film material inside a reactor, and then introducing an inert gas to replace the air inside the reactor, thereby making the inside of the reactor an oxygen-free environment; Step (2) of sequentially heating and maintaining the temperature of the reactor in an oxygen-free environment described in step (1), and then introducing silane gas to carry out a chemical vapor deposition reaction to obtain a precursor of a silicon carbon anode material; and (3) sequentially subjecting the precursor of the silicon-carbon anode material obtained in the step (2) to carbon coating, crushing, secondary coating and carbonization to obtain the lithium-ion battery silicon-carbon anode material.

[0013] The preparation method of the silicon-carbon negative electrode material of the lithium-ion battery according to the present application uses a porous carbon-based film material as a base to realize the vapor deposition of uniform nano-silicon particles, and effectively solves the problem of volume expansion during the silicon cycling process.

[0014] Normally, silane gas is difficult to deposit, but in the present application, the pressure difference created before and after the silane gas is introduced into the porous carbon-based film material causes the silane gas to be deposited in the voids of the porous carbon-based film material, and the porous carbon-based film material controls the direction of the gas flow, thereby enabling the deposition and adsorption of silane molecules in a directionally directed manner inside the voids, so that the silane gas can be effectively partially adsorbed inside the voids as it passes through the voids of the porous carbon-based film material.

[0015] In the present application, the reactor is not specifically limited, and may be any device capable of ensuring that gas passes therethrough in a direction and capable of being heated.

[0016] Preferably, the porous carbon-based film material described in step (1) comprises one of carbon paper, carbon nanotube film or graphene film.

[0017] Preferably, the thickness of the porous carbon-based film material described in step (1) is 100 to 500 μm, and may be, for example, 100 μm, 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm or 500 μm, but is not limited to the recited numerical values, and other unrecited numerical values ​​within the numerical range also apply.

[0018] If the porous carbon-based film material of the present application is too thick, there will be a large difference in the amount of silane deposited on both the front and back sides of the porous carbon-based film material, resulting in the disadvantage that the deposition is not uniform. If the thickness is too thin, the silane gas may penetrate the porous carbon-based film material when passing through at a certain flow rate, and the silane gas may not be able to deposit in the porous carbon-based film, resulting in material waste.

[0019] Preferably, the tortuosity of the porous carbon-based film material described in step (1) is 1.5 to 5, for example, it may be 1.5, 2, 2.5, 3, 3.5, 4, 4.5 or 5, but is not limited to the listed values, and other unlisted values ​​within the numerical range apply as well.

[0020] Preferably, the end point of the heating described in step (2) is 600 to 800°C, and may be, for example, 600°C, 620°C, 640°C, 660°C, 680°C, 700°C, 720°C, 740°C, 760°C, 780°C or 800°C, but is not limited to the recited numerical values, and other unrecited numerical values ​​within the numerical range also apply.

[0021] Preferably, the incubation time described in step (2) is 0.5 to 2 hours, and may be, for example, 0.5 hours, 0.8 hours, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours, but is not limited to the listed values, and other unlisted values ​​within the range of values ​​also apply.

[0022] Preferably, the angle between the position of the porous carbon-based film material described in step (1) and the flow direction of the silane gas described in step (2) is 60 to 120°, and may be, for example, 60°, 70°, 80°, 90°, 100°, 110° or 120°, but is not limited to the numerical values ​​listed, and other numerical values ​​not listed within the numerical range also apply.

[0023] Preferably, the angle between the position of the porous carbon-based film material described in step (1) and the flow direction of the silane gas described in step (2) is 90°.

[0024] By arranging the position of the porous carbon base film material of the present application at a certain angle to the flow direction of the silane gas, the silane gas can pass through the porous carbon base film material, and the silane can easily accumulate inside the pores of the porous carbon base film material.

[0025] Preferably, the gas flow rate of the silane gas described in step (2) is 0.1 to 2 L / min, and may be, for example, 0.1 L / min, 0.5 L / min, 1 L / min, 1.5 L / min or 2 L / min, but is not limited to the listed values, and other unlisted values ​​within the range of values ​​also apply.

[0026] If the gas flow rate of the silane gas in the present application is too fast, the silane gas will not stay in the film material for long enough to effectively adsorb it. If the gas flow rate is too high, the film material will not be able to withstand the strength of the film material, leading to bursting. In addition, the film material has a certain tortuosity, which has a certain inhibiting effect on the gas. If the gas flow rate is too slow, the silane gas cannot pass through the film, and will only stay on the surface of the film material.

[0027] Preferably, the flow time of the silane gas described in step (2) is 2 to 5 h, and may be, for example, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, or 5 h, but is not limited to the recited numerical values, and other numerical values ​​not recited within the numerical range also apply.

[0028] Preferably, the carbon coating described in step (3) is carried out in an inert gas atmosphere.

[0029] Preferably, the inert gas includes helium gas and / or argon gas.

[0030] Preferably, the temperature of the carbon coating described in step (3) is 800-1200°C, and may be, for example, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range apply as well.

[0031] Preferably, the coating time of the carbon coating described in step (3) is 2 to 6 h, and may be, for example, 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, 5.5 h or 6 h, but is not limited to the recited values, and other unrecited values ​​within the numerical range also apply.

[0032] Preferably, the carbon-containing gas source in the carbon coating process described in step (3) comprises any one or a combination of at least two of methane, ethane, propane, ethylene, propylene, or acetylene. Exemplary combinations include, but are not limited to, a combination of methane and ethane, a combination of methane and propane, a combination of methane and ethylene, a combination of methane and propylene, a combination of methane and acetylene, a combination of methane, ethane, and acetylene, or a combination of methane, ethane, propane, ethylene, and acetylene.

[0033] Preferably, the average particle size D50 of the crushed particles described in step (3) is 5 to 20 μm, and may be, for example, 5 μm, 8 μm, 10 μm, 12 μm, 14 μm, 16 μm, 18 μm or 20 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range also apply.

[0034] Preferably, the coating material of the secondary coating described in step (3) comprises an organic carbon source.

[0035] Preferably, the organic carbon source comprises any one or a combination of at least two of asphalt, tar, and phenolic resin.Typical combinations include, but are not limited to, a combination of asphalt and tar, a combination of asphalt and phenolic resin, a combination of tar and phenolic resin, or a combination of asphalt, tar, and phenolic resin.

[0036] Preferably, the coverage ratio of the secondary coating described in step (3) is 5-20%, and may be, for example, 5%, 8%, 10%, 12%, 14%, 16%, 18% or 20%, but is not limited to the listed values, and other unlisted values ​​within the numerical range also apply.

[0037] Preferably, the carbonization temperature described in step (3) is 800 to 1200°C, and may be, for example, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C, but is not limited to the recited numerical values, and other unrecited numerical values ​​within the numerical range apply as well.

[0038] Preferably, the carbonization time described in step (3) is 3 to 10 h, and may be, for example, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range apply as well.

[0039] As a preferred technical solution of the preparation method according to the first aspect of the present application, the preparation method includes: Step (1) of fixing a porous carbon-based film material in a reactor, and then introducing an inert gas to replace the air in the reactor, so that the reactor is in an oxygen-free environment, wherein the porous carbon-based film material has a thickness of 100-500 μm and a tortuosity of 1.5-5; Step (2) is a step in which the reactor in the oxygen-free environment described in step (1) is heated to 600 to 800°C and kept at the temperature for 0.5 to 2 hours, and then silane gas is introduced at a gas flow rate of 0.1 to 2 L / min for 2 to 5 hours, so that the silane gas undergoes a chemical vapor deposition reaction in the porous carbon-based material to form nanosilicon particles, and a precursor of a silicon carbon negative electrode material is obtained, in which the angle between the flow direction of the silane gas and the arrangement position of the porous carbon-based film material described in step (1) is 60 to 120°; and (3) performing carbon coating on the precursor of the silicon carbon negative electrode material obtained in step (2) in an inert gas atmosphere at a temperature of 800-1200°C for 2-6 hours using a carbon-containing gas source, crushing the precursor to obtain crushed particles having an average particle size D50 of 5-20 μm, performing secondary coating using a coating material, and carbonizing the resulting particles at 800-1200°C for 3-10 hours to obtain the lithium ion battery silicon carbon negative electrode material, in which the coating ratio of the secondary coating is 5-20%.

[0040] In a second aspect, the present application provides a lithium-ion battery silicon carbon anode material obtainable by the preparation method according to the first aspect.

[0041] In a third aspect, the present application provides a use of a lithium ion battery silicon carbon anode material prepared by the preparation method according to the first aspect, wherein the lithium ion battery silicon carbon anode material is used as an anode material of a lithium ion battery.

[0042] The numerical ranges set forth in this application include not only the recited point values, but also any point values ​​between the recited numerical ranges that are not recited, and for reasons of space and brevity, this application does not exhaustively recite specific point values ​​included in the ranges. Effect of the Invention

[0043] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0044] The preparation method of the silicon carbon anode material of the lithium ion battery according to the present application utilizes a porous carbon-based film material to realize the vapor deposition of uniform nano silicon particles, effectively alleviating the problem of volume expansion during silicon cycling, while effectively improving the polarization state of the material through carbon deposition, so as to effectively improve the electrochemical performance of the silicon carbon anode material.

[0045] Other aspects may be appreciated upon reading and understanding the detailed description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0046] The technical solution of the present application will be further described below by way of specific embodiments. The above examples are merely intended to help those skilled in the art understand the present application, and should not be construed as limiting the present application in any way.

[0047] Example 1 This embodiment provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material includes the following steps:

[0048] (1) After the carbon paper was fixed inside the reactor, helium gas was introduced to replace the air inside the reactor, creating an oxygen-free environment inside the reactor. The porous carbon-based film material had a thickness of 250 μm and a tortuosity of 3.

[0049] (2) The reactor in the oxygen-free environment described in step (1) was heated to 700°C and kept at this temperature for 1.2 hours, after which silane gas was introduced at a gas flow rate of 0.5 L / min for 3.5 hours to carry out a chemical vapor deposition reaction to obtain a precursor of a silicon carbon anode material. The angle between the flow direction of the silane gas and the arrangement position of the porous carbon-based film material described in step (1) was 90°.

[0050] (3) The precursor of the silicon carbon anode material obtained in step (2) was carbon-coated with methane in a helium gas atmosphere at 1000°C for 4 hours, then crushed to obtain crushed particles with an average particle size D50 = 10 μm, which were then secondary-coated with asphalt and carbonized at 1000°C to obtain the lithium-ion battery silicon carbon anode material. The secondary coating ratio was 10%.

[0051] Example 2 This embodiment provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material includes the following steps:

[0052] (1) After the carbon paper was fixed inside the reactor, helium gas was introduced to replace the air inside the reactor, creating an oxygen-free environment inside the reactor. The porous carbon-based film material had a thickness of 100 μm and a tortuosity of 1.5.

[0053] (2) The reactor in the oxygen-free environment described in step (1) was heated to 600°C and kept at that temperature for 2 hours, after which silane gas was introduced at a gas flow rate of 0.1 L / min for 5 hours to carry out a chemical vapor deposition reaction, thereby obtaining a precursor of a silicon carbon negative electrode material. The angle between the flow direction of the silane gas and the position of the carbon paper described in step (1) was 60°.

[0054] (3) The precursor of the silicon carbon anode material obtained in step (2) was coated with carbon using acetylene at 1200°C for 2 hours in a helium gas atmosphere, then crushed to obtain crushed particles with an average particle size D50 = 20 μm, and secondary coating was performed using tar. After carbonization at 1200°C for 3 hours, the lithium ion battery silicon carbon anode material was obtained. The coating ratio of the secondary coating was 8%.

[0055] Example 3 This embodiment provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material includes the following steps:

[0056] (1) After the carbon paper was fixed inside the reactor, helium gas was introduced to replace the air inside the reactor, so that the inside of the reactor became an oxygen-free environment. The porous carbon-based film material had a thickness of 500 μm and a tortuosity of 5.

[0057] (2) The reactor in the oxygen-free environment described in step (1) was heated to 800°C and kept at that temperature for 0.5 hours, after which silane gas was introduced at a gas flow rate of 2 L / min for 2 hours to carry out a chemical vapor deposition reaction, thereby obtaining a precursor of a silicon carbon negative electrode material. The angle between the flow direction of the silane gas and the position of the carbon paper described in step (1) was 120°.

[0058] (3) The precursor of the silicon carbon anode material obtained in step (2) was carbon-coated in a helium gas atmosphere using a mixed gas of ethane and propane at a temperature of 800°C for 6 hours, then crushed to obtain crushed particles with an average particle size D50 = 5 μm, secondary coating was performed using phenol resin, and carbonization was performed at 800°C for 10 hours to obtain the lithium ion battery silicon carbon anode material. The coating ratio of the secondary coating was 12%.

[0059] Example 4 This embodiment provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material includes the following steps:

[0060] (1) After the carbon paper was fixed inside the reactor, helium gas was introduced to replace the air inside the reactor, creating an oxygen-free environment inside the reactor. The porous carbon-based film material had a thickness of 300 μm and a tortuosity of 2.7.

[0061] (2) The reactor in the oxygen-free environment described in step (1) was heated to 680°C and kept at that temperature for 1.6 hours, after which silane gas was introduced at a gas flow rate of 0.8 L / min for 4 hours to carry out a chemical vapor deposition reaction, thereby obtaining a precursor of a silicon carbon negative electrode material. The angle between the flow direction of the silane gas and the position of the carbon paper described in step (1) was 85°.

[0062] (3) The precursor of the silicon carbon anode material obtained in step (2) was carbon-coated with a mixture of methane and acetylene gas at 1050°C for 3.5 hours in a helium gas atmosphere, then crushed to obtain crushed particles with an average particle size D50 = 15 μm, which were then secondary-coated with asphalt and carbonized at 1050°C for 8 hours to obtain the lithium-ion battery silicon carbon anode material. The secondary coating ratio was 16%.

[0063] Example 5 This embodiment provides a lithium ion battery silicon carbon negative electrode material, the preparation method of said lithium ion battery silicon carbon negative electrode material is the same as that of Example 1, except that the carbon paper in step (1) is replaced with carbon nanotube film.

[0064] Example 6 This embodiment provides a lithium ion battery silicon carbon anode material, the preparation method of the lithium ion battery silicon carbon anode material is the same as that of Example 1, except that the carbon paper in step (1) is replaced with graphene film.

[0065] Example 7 This embodiment provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material is the same as that of Example 1, except that the thickness of the carbon paper described in step (1) is changed to 80 μm.

[0066] Example 8 This embodiment provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material is the same as that of Example 1, except that the thickness of the carbon paper described in step (1) is changed to 600 μm.

[0067] Example 9 This embodiment provides a lithium ion battery silicon carbon negative electrode material. The preparation method of the lithium ion battery silicon carbon negative electrode material is the same as that of Example 1, except that the angle between the flow direction of the silane gas described in step (2) and the arrangement position of the carbon paper described in step (1) is changed to 20°.

[0068] Example 10 This embodiment provides a lithium ion battery silicon carbon negative electrode material. The preparation method of the lithium ion battery silicon carbon negative electrode material is the same as that of Example 1, except that the angle between the flow direction of the silane gas described in step (2) and the arrangement position of the carbon paper described in step (1) is changed to 0°.

[0069] Example 11 This embodiment provides a lithium ion battery silicon carbon anode material, the preparation method of the lithium ion battery silicon carbon anode material is the same as that of Example 1, except that the end point of heating in step (2) is changed to 500°C.

[0070] Example 12 This embodiment provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material is the same as that of Example 1, except that the end point of heating in step (2) is changed to 900°C.

[0071] Comparative Example 1 This comparative example provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material includes the following steps:

[0072] The chemical vapor deposition apparatus was evacuated, and a mixture of silane and argon gas was introduced into the chemical vapor deposition apparatus and heated at 800°C for 7 hours to prepare silicon particles. Then, a mixture of acetylene and argon gas was introduced into the chemical vapor deposition apparatus and heated at 800°C for 1 hour to prepare a carbon coating layer on the surface of the silicon particles, preparing a silicon carbon anode material.

[0073] Comparative Example 2 This comparative example provides a lithium ion battery silicon carbon negative electrode material, the preparation method of the lithium ion battery silicon carbon negative electrode material includes the following steps:

[0074] (a) The nanosilicon dispersion, conductive additive, and coating material were mixed, dispersed and stirred for 2 hours, and then spray-dried to obtain a powder material.

[0075] (b) The temperature was increased to 1000°C at a rate of 3°C / min, and the powder material obtained in step (a) was subjected to a carbonization heat treatment for 6 hours, after which it was pulverized to obtain a precursor of the silicon carbon negative electrode material.

[0076] (c) Compounding the graphite material and the precursor of the silicon carbon anode material obtained in step (b) to obtain the lithium ion battery silicon carbon anode material.

[0077] The lithium ion battery silicon carbon negative electrode materials prepared in Examples 1-12 and Comparative Examples 1-2 were applied to lithium ion batteries, and electrochemical performance detection was performed on the lithium ion batteries. The test was performed on Wuhan Blue-Energy CT2001A battery tester, with the voltage range of 0.005-1.5V, the capacity test rate of 0.05C / 0.05C, and the cycle test rate of 0.5C / 0.5C. The specific test structure is shown in Table 1.

[0078] The cycle test of the battery is to prepare a 420mAh / g anode material by mixing the material with a commercial graphite material, and combine it with a ternary cathode material to produce a full cell for testing. 1 / 3 Co 1 / 3 Mn 1 / 3 A soft pack battery was manufactured using O2) as the positive electrode, LiPF6 (solvent was EC+DEC, volume ratio 1:1, concentration 1.3 mol / l) as the electrolyte, and Celegard 2400 as the separator.

[0079] Full charge rebound test: First, the capacity was measured, and then the soft pack battery was disassembled to measure the thickness D1 of the negative electrode piece. Then, after fully charging the soft pack battery by 100 cycles, the soft pack battery was disassembled to measure the thickness D2 of the negative electrode piece. Then, the full charge rebound rate = (D2-D1) / D1 was calculated. [Table 1]

[0080] As can be seen from Table 1, the silicon carbon anode material of the present application has a high capacity of more than 1530mAh / g, and has high initial efficiency and excellent cycle performance. Different carbon nanofilm substrates can effectively realize the deposition of nanosilicon, ensuring the improvement of the cycle performance of the battery. As can be seen from the comparison, if the thickness of the film material is too low, the film material will be damaged during the reaction process, and the silane gas adsorption film cannot be effectively formed, resulting in a decrease in the capacity of the material. However, if the film thickness is too thick, the gas passage rate will be low, resulting in the uneven phenomenon that the deposition of silane gas is too much at the front and too little at the rear. In addition, if the deposition at the front is too much, the silicon nanoparticles will aggregate, resulting in a decrease in the cycle performance of the battery. As can be seen from the comparison, when the film arrangement angle is small, the silane gas will selectively bypass the film material, resulting in a small amount of deposition in the film material, and as a result, the preparation of nanosilicon particles in the film material cannot be realized, and the function of preparing a high-capacity silicon carbon anode material cannot be achieved. High or low temperature of the pyrolysis reaction was unfavorable to the deposition of nanosilicon in the material, and the capacity of the material was reduced.

[0081] In summary, the preparation method of the silicon carbon anode material of the lithium ion battery according to the present application realizes the uniform vapor deposition of nano silicon particles by using the porous carbon-based film material, effectively alleviates the problem of volume expansion during the silicon cycling process, and effectively improves the polarization state of the material through carbon deposition, thereby effectively improving the electrochemical performance of the silicon carbon anode material.

[0082] The above describes in more detail the objectives, technical solutions and beneficial effects of the present application through the above specific examples, but the applicant declares that these are only specific embodiments of the present application and are not intended to limit the present application. Those skilled in the art should understand that any modifications, equivalent replacements, improvements, etc. made within the concept and principles of the present application are all within the scope of protection of the present application.

Claims

1. A method for preparing a lithium ion battery silicon carbon anode material, comprising: (1) a porous carbon-based film material is fixed inside a reactor, and then an inert gas is introduced to replace the air inside the reactor, thereby making the inside of the reactor an oxygen-free environment; Step (2) of sequentially heating and maintaining the temperature of the reactor in an oxygen-free environment described in step (1), and then introducing silane gas to carry out a chemical vapor deposition reaction to obtain a precursor of a silicon carbon anode material; and (3) sequentially carrying out carbon coating, crushing, secondary coating and carbonization on the precursor of silicon carbon anode material obtained in step (2), to obtain the lithium ion battery silicon carbon anode material.

2. The porous carbon-based film material described in step (1) includes any one of carbon paper, carbon nanotube film, and graphene film; Preferably, the thickness of the porous carbon-based film material described in step (1) is 100-500 μm; The preparation method according to claim 1, wherein the tortuosity of the porous carbon-based film material in step (1) is preferably 1.5-5.

3. The end point of the heating described in step (2) is 600 to 800° C., The preparation method according to claim 1 or 2, wherein the incubation time in step (2) is preferably 0.5 to 2 h.

4. the angle between the position of the porous carbon-based film material described in step (1) and the flow direction of the silane gas described in step (2) is 60 to 120°; Preferably, the angle between the position of the porous carbon-based film material described in step (1) and the flow direction of the silane gas described in step (2) is 90°; Preferably, the gas flow rate of the silane gas described in step (2) is 0.1 to 2 L / min; The preparation method according to any one of claims 1 to 3, wherein the flow time of the silane gas in step (2) is preferably 2 to 5 h.

5. The carbon coating described in step (3) is carried out in an inert gas atmosphere; Preferably, the inert gas comprises helium gas and / or argon gas; Preferably, the temperature of the carbon coating described in step (3) is 800 to 1200° C.; Preferably, the coating time of the carbon coating described in step (3) is 2 to 6 h; The preparation method according to any one of claims 1 to 4, wherein preferably, in the carbon coating process described in step (3), the carbon-containing gas source comprises any one or a combination of at least two of the following: methane, ethane, propane, ethylene, propylene or acetylene.

6. The method according to any one of claims 1 to 5, wherein the average particle size D50 of the crushed particles described in step (3) is 5 to 20 μm.

7. The coating material of the secondary coating described in step (3) comprises an organic carbon source; Preferably, the organic carbon source comprises any one or a combination of at least two of asphalt, tar, and phenolic resin; Preferably, the coverage of the secondary coating described in step (3) is 5-20%; Preferably, the temperature of the carbonization described in step (3) is 800 to 1200° C.; The preparation method according to any one of claims 1 to 6, wherein the time of carbonization according to step (3) is 3 to 10 h.

8. Step (1) of fixing a porous carbon-based film material in a reactor, and then introducing an inert gas to replace the air in the reactor, so that the reactor is in an oxygen-free environment, wherein the porous carbon-based film material has a thickness of 100-500 μm and a tortuosity of 1.5-5; Step (2) of heating the reactor to 600-800° C. and keeping the temperature for 0.5-2 hours, and then introducing silane gas at a gas flow rate of 0.1-2 L / min for 2-5 hours to carry out a chemical vapor deposition reaction to obtain a precursor of a silicon carbon negative electrode material, in which the angle between the flow direction of the silane gas and the arrangement position of the porous carbon base film material described in step (1) is 60-120°; and (3) in an inert gas atmosphere, the precursor of the silicon carbon negative electrode material obtained in step (2) is carbon-coated using a carbon-containing gas source at a temperature of 800-1200°C for 2-6 h, then crushed to obtain crushed particles with an average particle size D50 = 5-20 μm, and then secondary-coated using a coating material, and carbonized at 800-1200°C for 3-10 h to obtain the lithium ion battery silicon carbon negative electrode material, in which the coating ratio of the secondary coating is 5-20%. The preparation method according to any one of claims 1 to 7.

9. A lithium ion battery silicon carbon anode material obtainable by the preparation method according to any one of claims 1 to 8.

10. 10. The use of the lithium ion battery silicon carbon anode material according to claim 9, The lithium ion battery silicon carbon negative electrode material is used as a negative electrode material of a lithium ion battery.

Citation Information

Patent Citations

  • Preparation method of carbon nanotube-silicon composite cathode material

    CN102983311A

  • Lithium ion battery silicon-carbon negative electrode material, and preparation process and equipment thereof

    CN112768667A

  • Lithium ion battery silicon-carbon negative electrode material, and preparation process and equipment thereof

    CN112768669A

  • Method for preparing electroactive materials for metal-ion batteries

    JP2022515227A

  • Process for preparing electroactive materials for metal-ion batteries

    US10508335B1