Method for producing an electrode for a lithium secondary battery, and a lithium secondary battery including the electrode

The described method for transferring lithium metal onto silicon-based electrodes in lithium secondary batteries addresses the issue of high irreversible capacity and volume changes by ensuring uniform pre-lithiation without a release layer, thereby maintaining battery performance and reducing resistance.

JP2024540592AActive Publication Date: 2024-10-31LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024529828
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-05-19
Filing Date
2023-05-18
Publication Date
2024-10-31
Estimated Expiration
2043-05-18

AI Technical Summary

Technical Problem

The use of silicon-based negative electrode active materials in lithium secondary batteries results in significant volume changes and high initial irreversible capacity, leading to rapid capacity and cycle life degradation due to surface side reactions and challenges in safely and efficiently pre-lithiating lithium metal.

Method used

A method for manufacturing electrodes involving the transfer of lithium metal onto the electrode active material layer using a transfer laminate with specific temperature and pressure conditions, followed by removal of the release layer to prevent increased resistance, ensuring uniform pre-lithiation without a separate release layer on the electrode.

Benefits of technology

The method enables efficient and safe pre-lithiation of silicon-based electrodes, reducing initial irreversible capacity and maintaining battery performance by preventing resistance increases during cell assembly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540592000001_ABST
    Figure 2024540592000001_ABST
Patent Text Reader

Abstract

The present application relates to a method for producing an electrode for a lithium secondary battery, the method comprising the steps of: forming an electrode current collector layer, and an electrode active material layer on one or both sides of the electrode current collector layer; and transferring lithium metal onto the electrode active material layer, the step of transferring the lithium metal comprising the steps of: preparing a transfer laminate in which a base layer, a release layer, and lithium metal are sequentially laminated; laminating the transfer laminate on the electrode active material layer so that a surface of the lithium metal opposite to a surface that contacts the release layer contacts a surface of the electrode active material layer opposite to a surface that contacts the electrode current collector layer; removing the base layer; and removing the release layer, the laminating step being carried out at a temperature condition of 30° C. or less and a pressure of 10 kgf / cm 2 More than 150kgf / cm 2 The present invention relates to a method for producing an electrode for a lithium secondary battery, in which lamination is performed at a pressure below 1000° C., and a lithium secondary battery including the electrode.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0061177, filed with the Korean Intellectual Property Office on May 19, 2022, the entire contents of which are incorporated herein by reference.

[0002] The present application relates to a method for producing an electrode for a lithium secondary battery, and to a lithium secondary battery including the electrode. [Background technology]

[0003] The rapid increase in the use of fossil fuels has led to an increased demand for alternative and clean energy, and one of the most actively researched fields in this area is the field of power generation and storage using electrochemical reactions.

[0004] At present, a representative example of an electrochemical element that uses such electrochemical energy is a secondary battery, and the range of its use is expanding more and more.

[0005] With the development of technology and increasing demand for mobile devices, the demand for secondary batteries as energy sources is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and voltage, long cycle life, and low self-discharge rate, have been commercialized and widely used. In addition, research on methods for manufacturing high-density electrodes with higher energy density per unit volume as electrodes for such high-capacity lithium secondary batteries is being actively conducted.

[0006] In general, a secondary battery is composed of a positive electrode, a negative electrode, an electrolyte, and a separator. The negative electrode includes a negative electrode active material that inserts and removes lithium ions from the positive electrode, and the negative electrode active material may be silicon-based particles having a large discharge capacity.

[0007] Generally, carbon materials such as graphite are used for the negative electrode of lithium secondary batteries, but the theoretical capacity density of carbon is 372 mAh / g (833 mAh / cm 3). Therefore, in order to improve the energy density of the negative electrode, silicon (Si), tin (Sn), and their oxides and alloys, which are alloyed with lithium, are being considered as negative electrode materials. Among these, silicon-based materials have attracted attention due to their low cost and high capacity (4200mAh / g).

[0008] However, when using silicon-based negative electrode active materials, a problem occurs in that the initial irreversible capacity is large. In the charge / discharge reaction of a lithium secondary battery, lithium released from the positive electrode is inserted into the negative electrode during charging, and is removed from the negative electrode during discharging and returns to the positive electrode. However, in the case of silicon-based negative electrode active materials, the volume change and surface side reaction are significant, and most of the lithium inserted into the negative electrode during initial charging does not return to the positive electrode, resulting in a problem of a large initial irreversible capacity. When the initial irreversible capacity is large, a problem occurs in that the battery capacity and cycle are rapidly reduced.

[0009] In order to solve the above problems, a method of prelithiating a silicon negative electrode containing a silicon-based negative electrode active material is known. Known prelithiating methods include a method of preparing an electrode after lithiating the negative electrode by a physical / chemical method such as electrolytic plating, lithium metal transfer, or lithium metal deposition, and a method of electrochemically prelithiating the negative electrode.

[0010] In particular, in the lithium metal transfer process, it is difficult to transfer lithium metal safely and easily, and lithium is not transferred from the transfer laminate, or even if it is transferred, the highly reactive lithium metal immediately begins to react with the negative electrode active material, causing problems such as particle cracking on the surface of the negative electrode active material layer.

[0011] In addition, in order to adjust the reactivity and transferability of lithium metal, a release layer is used when transferring lithium metal, but after the pre-lithiation process, the adhesive strength of the release layer increases due to an increase in temperature and changes in pressure conditions, making it difficult to remove. In this case, the release layer acts as a resistor in the battery, causing a problem of increased resistance.

[0012] Therefore, there is a need to study a method for prelithiating an electrode more safely and efficiently, without increasing the resistance of the battery, and for uniformly prelithiating lithium in the electrode active material layer. Summary of the Invention [Problem to be solved by the invention]

[0013] The lithium metal transfer process includes a process of transferring lithium metal from a transfer laminate to the top of an electrode active material layer in a pre-lithiation process, and it has been confirmed through research that the transferability of lithium metal can be increased and the removal of the release layer after completion of pre-lithiation can be facilitated by adjusting the amount of heat generated per unit time of the electrode active material layer during pre-lithiation. Therefore, an object of the present application is to provide a method for manufacturing an electrode for a lithium secondary battery, and a lithium secondary battery including the electrode. [Means for solving the problem]

[0014] One embodiment of the present specification is a method for producing an electrode for a lithium secondary battery, comprising the steps of: forming an electrode collector layer and an electrode active material layer on one or both sides of the electrode collector layer; and transferring lithium metal onto the electrode active material layer, wherein the step of transferring the lithium metal comprises the steps of: preparing a transfer laminate in which a base layer, a release layer, and lithium metal are sequentially laminated; laminating the transfer laminate onto the electrode active material layer so that the surface of the lithium metal opposite to the surface that contacts the release layer contacts the surface of the electrode active material layer opposite to the surface that contacts the electrode collector layer; removing the base layer; and removing the release layer, The lamination step is performed under a temperature condition of 30° C. or less and a pressure of 10 kgf / cm 2 More than 150kgf / cm 2 The present invention provides a method for producing an electrode for a lithium secondary battery, in which lamination is performed at a pressure of:

[0015] In yet another embodiment, there is provided a lithium secondary battery comprising: a positive electrode for a lithium secondary battery; a negative electrode for a lithium secondary battery; a separator provided between the positive electrode and the negative electrode; and an electrolyte, wherein at least one of the positive electrode for the lithium secondary battery and the negative electrode for the lithium secondary battery is an electrode for a lithium secondary battery produced by the method described above. Effect of the Invention

[0016] Generally, a release layer must be used to facilitate the transfer of lithium metal from a transfer laminate to the top of an electrode active material layer. However, when a battery is manufactured with the release layer itself included in an electrode after prelithiation, a problem occurs in that the resistance of the battery increases.

[0017] Therefore, a method for producing an electrode for a lithium secondary battery according to one embodiment of the present invention is characterized in that it includes a step of removing the release layer in the lithiation prior to the transfer step.

[0018] In particular, the present invention relates to a process in which a release layer can be easily separated from the upper part of an electrode active material layer by adjusting process conditions in a pre-lithiation process of an electrode active material layer, and to a process in which the release layer on the upper part of a pre-lithiated electrode can be easily removed by adjusting the pressure, temperature, and heat generation per time during the transfer of lithium metal.

[0019] The electrode manufactured by the above process does not have a separate layer, such as a release layer, on the electrode active material layer, so that after assembling the cell, the resistance does not increase when the battery is operated. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a diagram showing a process of transferring lithium metal to an electrode for a lithium secondary battery according to one embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Before describing the present invention, some terms will first be defined.

[0022] In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, rather than excluding other components, unless specifically stated to the contrary.

[0023] In this specification, "p to q" means a range of "not less than p and not more than q."

[0024] In this specification, the "specific surface area" is measured by the BET method, and specifically, is calculated from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using a BELSORP-mini II manufactured by BEL Japan Co., Ltd. That is, in this application, the BET specific surface area can mean the specific surface area measured by the above-mentioned measurement method.

[0025] In this specification, "Dn" means particle size distribution, and refers to the particle size at n% of the cumulative particle number distribution by particle size. That is, D50 is the particle size (median particle size) at 50% of the cumulative particle number distribution by particle size, D90 is the particle size at 90% of the cumulative particle number distribution by particle size, and D10 is the particle size at 10% of the cumulative particle number distribution by particle size. Meanwhile, the particle size distribution may be measured using a laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500), and when the particles pass through a laser beam, the difference in the diffraction pattern according to the particle size is measured to calculate the particle size distribution.

[0026] In the present specification, when a polymer contains a certain monomer as a monomer unit, it means that the monomer participates in a polymerization reaction and is contained as a repeating unit in the polymer. In the present specification, when a polymer contains a monomer, this is interpreted as the same as when a polymer contains a monomer as a monomer unit.

[0027] It is understood that in this specification, the term "polymer" is used in a broad sense, including copolymers, unless specifically referred to as a "homopolymer".

[0028] In this specification, the weight average molecular weight (Mw) and number average molecular weight (Mn) are polystyrene-equivalent molecular weights measured by gel permeation chromatography (GPC) using monodisperse polystyrene polymers (standard samples) of various degrees of polymerization commercially available for molecular weight measurement as standard substances. In this specification, the molecular weight means the weight average molecular weight unless otherwise specified.

[0029] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings in order to enable those skilled in the art to easily practice the present invention. However, the present invention may be embodied in many different forms and should not be construed as limited to the disclosed embodiments.

[0030] One embodiment of the present specification is a method for producing an electrode for a lithium secondary battery, comprising the steps of: forming an electrode collector layer and an electrode active material layer on one or both sides of the electrode collector layer; and transferring lithium metal onto the electrode active material layer, the step of transferring the lithium metal comprising the steps of: preparing a transfer laminate in which a base layer, a release layer, and lithium metal are sequentially laminated; laminating the transfer laminate onto the electrode active material layer so that the surface of the lithium metal opposite to the surface that contacts the release layer contacts the surface of the electrode active material layer opposite to the surface that contacts the electrode collector layer; removing the base layer; and removing the release layer, the lamination step being performed at a temperature condition of 30° C. or less and a pressure of 10 kgf / cm 2 More than 150kgf / cm 2 The present invention provides a method for producing an electrode for a lithium secondary battery, in which lamination is performed at a pressure of:

[0031] In one embodiment of the present application, the electrode may be a negative electrode or a positive electrode.

[0032] FIG. 1 is a diagram showing a process of transferring lithium metal onto an electrode for a lithium secondary battery according to an embodiment of the present application. Specifically, after laminating a transfer laminate 100 in which a substrate layer 10, a release layer 35, and lithium metal 20 are sequentially laminated on an electrode 200 for a lithium secondary battery formed of an electrode current collector layer 40 and an electrode active material layer 30, a process of removing the substrate layer 10 of the transfer laminate 100 can be confirmed.

[0033] Hereinafter, specific details of the method for manufacturing an electrode for a lithium secondary battery according to the invention of the present application will be described.

[0034] The method for manufacturing an electrode for a lithium secondary battery according to an embodiment of the present application may include a step of forming an electrode current collector layer and an electrode active material layer on one or both surfaces of the electrode current collector layer.

[0035] In one embodiment of the present application, the step of forming an electrode current collector layer and an electrode active material layer on one or both surfaces of the electrode current collector layer includes a step of coating an electrode slurry containing an electrode active material layer composition on one or both surfaces of the electrode current collector layer, and the electrode active material layer composition includes one or more selected from the group consisting of an electrode active material, an electrode conductive material, and an electrode binder. A method for manufacturing an electrode for a lithium secondary battery is provided.

[0036] At this time, the electrode active material includes a silicon-based active material, and the silicon-based active material includes one or more selected from the group consisting of SiO x (x = 0), SiO x (0 <x <2), SiC, and Si alloy. A method for pre-lithiation of an electrode for a lithium secondary battery is provided.

[0037] In one embodiment of the present application, the electrode may be a negative electrode, and hereinafter, an explanation of a method for manufacturing a negative electrode for a lithium secondary battery will be described.

[0038] The method for manufacturing an electrode for a lithium secondary battery according to an embodiment of the present application may include a step of forming a negative electrode current collector layer and a negative electrode active material layer on one or both surfaces of the negative electrode current collector layer.

[0039] In one embodiment of the present application, the negative electrode current collector layer usually has a thickness of 1 μm to 100 μm. Such a negative electrode current collector layer is not particularly limited as long as it does not induce chemical changes in the battery and has high conductivity, and for example, copper, stainless steel, aluminum, nickel, titanium, plastic carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy may be used. In addition, fine irregularities may be formed on the surface to strengthen the binding force of the negative electrode active material, and it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0040] In one embodiment of the present application, the negative electrode current collector layer may have a thickness of 1 μm or more and 100 μm or less, and the negative electrode active material layer may have a thickness of 20 μm or more and 500 μm or less.

[0041] However, the thickness may vary depending on the type and application of the negative electrode used, and is not limited thereto.

[0042] In one embodiment of the present application, there is provided a method for producing an electrode for a lithium secondary battery, wherein the step of forming a negative electrode current collector layer and a negative electrode active material layer on one or both sides of the negative electrode current collector layer includes coating one or both sides of the negative electrode current collector layer with a negative electrode slurry including a negative electrode active material layer composition, and the negative electrode active material layer composition includes one or more selected from the group consisting of a negative electrode active material, a negative electrode conductive material, and a negative electrode binder.

[0043] In one embodiment of the present application, the negative electrode slurry may include a negative electrode active material layer composition and a slurry solvent.

[0044] In one embodiment of the present application, the solid content of the negative electrode slurry may be 5% or more and 40% or less.

[0045] In another embodiment, the solid content of the negative electrode slurry may be in the range of 5% to 40%, preferably 7% to 35%, and more preferably 10% to 30%.

[0046] The solid content of the negative electrode slurry may refer to the content of the negative electrode active material layer composition contained in the negative electrode slurry, or may refer to the content of the negative electrode active material composition based on 100 parts by weight of the negative electrode slurry.

[0047] When the solid content of the negative electrode slurry satisfies the above range, the viscosity is appropriate during the formation of the negative electrode active material layer, and a caking phenomenon of particles of the negative electrode active material layer composition is minimized, thereby making it possible to efficiently form the negative electrode active material layer.

[0048] In one embodiment of the present application, the slurry solvent is not limited to the above as long as it can dissolve the negative electrode active material layer composition, and specifically, distilled water may be used.

[0049] The negative electrode according to one embodiment of the present application may be formed by coating and drying the negative electrode slurry on a negative electrode current collector layer.

[0050] The drying step may dry out a slurry solvent in the negative electrode slurry.

[0051] In one embodiment of the present application, the negative electrode active material layer composition may include one or more selected from the group consisting of a negative electrode active material, a negative electrode conductive material, and a negative electrode binder.

[0052] In one embodiment of the present application, the negative electrode active material may be a silicon-based active material, or a negative electrode containing a silicon-based active material and a carbon-based active material together may be used. In this case, a lithium secondary battery having improved performance such as cycle life characteristics can be manufactured.

[0053] In one embodiment of the present application, the silicon-based active material is SiOx (x = 0), SiO x It may contain one or more selected from the group consisting of (0 < x < 2), SiC, and Si alloys.

[0054] In one embodiment of the present application, the silicon-based active material is SiO x (x = 0) and SiO x It may contain one or more selected from the group consisting of (0 < x < 2), and based on 100 parts by weight of the silicon-based active material, the SiO x (x = 0) may contain 70 parts by weight or more.

[0055] In another embodiment, based on 100 parts by weight of the silicon-based active material, the SiO x (x = 0) may contain 70 parts by weight or more, preferably 80 parts by weight or more, more preferably 90 parts by weight or more, and may contain 100 parts by weight or less, preferably 99 parts by weight or less, more preferably 95 parts by weight or less.

[0056] In one embodiment of the present application, the silicon-based active material may particularly use pure silicon (Si) as the silicon-based active material. Using pure silicon (Si) as the silicon-based active material means that, as described above, when based on 100 parts by weight of the entire silicon-based active material, it may mean containing pure Si particles (SiO x (x = 0)) within the above range and not bonded to other particles or elements.

[0057] In the charge and discharge reaction of a lithium secondary battery, during charging, lithium released from the positive electrode is inserted into the negative electrode, and during discharging, it desorbs from the negative electrode and returns to the positive electrode again. However, in the case of a silicon-based negative electrode active material, volume change and surface side reactions are serious, and during the initial charging, most of the lithium inserted into the negative electrode cannot return to the positive electrode again. Therefore, the problem of an increase in the initial irreversible capacity occurs. When the initial irreversible capacity increases, problems such as a rapid decrease in battery capacity and cycles occur.

[0058] In the present invention, in order to solve the above problems, the negative electrode of the lithium secondary battery is pre-lithiated to solve the initial irreversible capacity problem. Specifically, in the pre-lithiation process, when performing the lithium transfer process, lithium metal is easily transferred from the transfer laminate, and the lithium in the negative electrode active material layer is uniformly pre-lithiated by suppressing the generation of by-products and preventing an increase in the resistance of the manufactured cell.

[0059] Meanwhile, the average particle size (D50) of the silicon-based active material of the present invention may be 1 μm to 10 μm, specifically, 3 μm to 8 μm, and more specifically, 3.5 μm to 7 μm. When the average particle size is within the above range, the specific surface area of ​​the particles is within a suitable range, and the viscosity of the negative electrode slurry is formed within a suitable range. As a result, the particles constituting the negative electrode slurry are smoothly dispersed. In addition, when the size of the silicon-based active material is equal to or greater than the lower limit of the above range, the contact area between the silicon particles and the conductive material is excellent due to the complex of the conductive material and the binder in the negative electrode slurry, and the conductive network is more likely to be maintained, thereby increasing the capacity retention rate. Meanwhile, when the average particle size satisfies the above range, silicon particles that are too large are excluded, and the surface of the negative electrode is formed smoothly, thereby preventing the phenomenon of non-uniform current density during charging and discharging.

[0060] In one embodiment of the present application, the silicon-based active material usually has a characteristic BET specific surface area. The BET specific surface area of ​​the silicon-based active material is preferably less than 0.01 m 2 / g~150.0m 2 / g, more preferably 0.1m 2 / g~100.0m 2 / g, particularly preferably 0.2m 2 / g~80.0m 2 / g, most preferably 0.2m 2 / g~18.0m 2 / g. The BET specific surface area is determined according to DIN 66131 (using nitrogen).

[0061] In one embodiment of the present application, the silicon-based active material may be present, for example, in crystalline or amorphous form, and is preferably not porous.The silicon particles are preferably spherical or shard particles.Alternatively, the silicon particles may have a fibrous structure or may be present in the form of a silicon-containing thin film or coating, but less preferably.

[0062] In one embodiment of the present application, the silicon-based active material may be 60 parts by weight or more based on 100 parts by weight of the negative electrode active material layer composition.

[0063] In yet another embodiment, the silicon-based active material may be included in an amount of 60 parts by weight or more, preferably 65 parts by weight or more, more preferably 70 parts by weight or more, based on 100 parts by weight of the negative electrode active material layer composition, and may be included in an amount of 95 parts by weight or less, preferably 90 parts by weight or less, more preferably 80 parts by weight or less.

[0064] The negative electrode active material layer composition according to the present application includes a negative electrode conductive material and a negative electrode binder capable of controlling the volume expansion rate during charging and discharging, even when a silicon-based active material having a remarkably high capacity is used within the above range, and thus has the characteristics of excellent output characteristics during charging and discharging without deteriorating the performance of the negative electrode even when the silicon-based active material is used within the above range.

[0065] In one embodiment of the present application, the silicon-based active material may have a non-spherical morphology, and the sphericity is, for example, 0.9 or less, for example, 0.7 to 0.9, for example, 0.8 to 0.9, for example, 0.85 to 0.9.

[0066] In this application, the circularity is determined by the following formula A, where A is the area and P is the perimeter.

[0067] [Formula A] 4πA / P 2

[0068] In the past, it was common to use only graphite-based compounds as negative electrode active materials, but recently, as the demand for high-capacity batteries has increased, attempts to mix and use silicon-based active materials to increase capacity have been increasing. However, silicon-based active materials have the limitation that their volume expands rapidly during the charge / discharge process, damaging the conductive path formed in the negative electrode active material layer and reducing the performance of the battery, so the type of negative electrode conductive material used together with the silicon-based active material is important.

[0069] In one embodiment of the present application, the negative electrode conductive material may include one or more selected from the group consisting of a dot-like conductive material, a sheet-like conductive material, and a linear conductive material.

[0070] In one embodiment of the present application, the dot-shaped conductive material refers to a conductive material that can be used to improve the conductivity of the negative electrode, does not induce chemical changes, and has conductivity. Specifically, the dot-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and preferably includes carbon black in terms of realizing high conductivity and excellent dispersibility.

[0071] In one embodiment of the present application, the dot-shaped conductive material has a BET specific surface area of ​​40 m 2 / g or more 70m 2 / g or less, preferably 45m 2 / g or more 65m 2 / g or less, more preferably 50m 2 / g or more 60m 2 / g or less.

[0072] In one embodiment of the present application, the particle size of the dotted conductive material may be 10 nm to 100 nm, preferably 20 nm to 90 nm, and more preferably 40 nm to 60 nm.

[0073] In one embodiment of the present application, the negative electrode conductive material may include a sheet conductive material.

[0074] The planar conductive material can improve conductivity by increasing surface contact between silicon particles in the negative electrode, and at the same time, can suppress the disconnection of the conductive path due to volume expansion, and is used in a concept including a bulk type conductive material or a plate type conductive material.

[0075] In one embodiment of the present application, the sheet conductive material may include at least one selected from the group consisting of platelet graphite, graphene, graphene oxide, and graphite flakes, and may preferably be platelet graphite.

[0076] In one embodiment of the present application, the average particle size (D50) of the sheet conductive material may be 2 μm to 7 μm, specifically, 3 μm to 6 μm, and more specifically, 4 μm to 5 μm. If the above range is satisfied, the particle size is sufficient, so that the viscosity of the negative electrode slurry is not increased too much, and dispersion is easy. Therefore, when dispersing using the same equipment and time, the dispersion effect is excellent.

[0077] In one embodiment of the present application, there is provided a negative electrode composition, wherein the sheet conductive material has a D10 of 0.5 μm or more and 1.5 μm or less, a D50 of 2.5 μm or more and 3.5 μm or less, and a D90 of 7.0 μm or more and 15.0 μm or less.

[0078] In one embodiment of the present application, the sheet conductive material may be a sheet conductive material having a high BET specific surface area; or a sheet conductive material having a low specific surface area.

[0079] In one embodiment of the present application, the sheet conductive material may be a sheet conductive material with a high specific surface area or a sheet conductive material with a low specific surface area without any restrictions. In particular, the sheet conductive material of the present application may be affected to some extent by dispersion in terms of electrode performance, and it is particularly preferable to use a sheet conductive material with a low specific surface area in which dispersion problems do not occur.

[0080] In one embodiment of the present application, the sheet conductive material has a BET specific surface area of ​​5 m 2 / g or more.

[0081] In another embodiment, the sheet conductive material has a BET specific surface area of ​​5 m 2 / g or more 500m 2 / g or less, preferably 5m 2 / g or more 300m 2 / g or less, more preferably 5m 2 / g or more 250m 2 / g.

[0082] In another embodiment, the sheet conductive material is a sheet conductive material having a high specific surface area, and the BET specific surface area is 50 m 2 / g or more 500m 2 / g or less, preferably 80m 2 / g or more 300m 2 / g or less, more preferably 100m 2 / g or more 300m 2 / g or less.

[0083] In another embodiment, the sheet conductive material is a sheet conductive material having a low specific surface area and a BET specific surface area of ​​5 m 2 / g or more 40m 2 / g or less, preferably 5m 2 / g or more 30m 2 / g or less, more preferably 5m 2 / g or more 25m 2 / g or less.

[0084] Alternatively, the conductive material may be a linear conductive material such as a carbon nanotube. The carbon nanotube may be a bundle-type carbon nanotube. The bundle-type carbon nanotube may include a plurality of carbon nanotube units. Specifically, unless otherwise specified, the term "bundle type" refers to a secondary shape in which a plurality of carbon nanotube units are arranged in parallel with the longitudinal axis of the carbon nanotube units being substantially aligned in the same direction or twisted into a bundle or rope. The carbon nanotube unit has a graphite sheet having a nano-sized cylindrical shape and an sp2 bond structure. In this case, the graphite sheet may exhibit conductive or semiconductive properties depending on the angle and structure at which it is wound. The bundle-type carbon nanotube may be uniformly dispersed during the manufacture of the negative electrode compared to an entangled-type carbon nanotube, and may smoothly form a conductive network in the negative electrode, thereby improving the conductivity of the negative electrode.

[0085] In one embodiment of the present application, the negative electrode conductive material may be 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the negative electrode active material layer composition.

[0086] In another embodiment, the negative electrode conductive material may be included in an amount of 10 parts by weight or more and 40 parts by weight or less, preferably 10 parts by weight or more and 30 parts by weight or less, and more preferably 15 parts by weight or more and 25 parts by weight or less, based on 100 parts by weight of the negative electrode active material layer composition.

[0087] The negative electrode conductive material according to the present application has a completely different structure from the positive electrode conductive material applied to the positive electrode. That is, the negative electrode conductive material according to the present application plays a role of controlling the contact between the silicon-based active material, which has a very large volume expansion of the electrode due to charging and discharging, and the positive electrode conductive material plays a role of providing some conductivity while acting as a buffer when rolled, and has a completely different structure and role from the negative electrode conductive material of the present invention.

[0088] In addition, the negative electrode conductive material according to the present application is applied to a silicon-based active material, and has a completely different structure from a conductive material applied to a graphite-based active material. That is, a conductive material used in an electrode having a graphite-based active material has particles that are simply smaller than the active material, and therefore has the properties of improving output characteristics and imparting some electrical conductivity, and has a completely different structure and role from a negative electrode conductive material applied together with a silicon-based active material as in the present invention.

[0089] In one embodiment of the present application, the dot-shaped conductive material used as the negative electrode conductive material has a structure and function different from that of a carbon-based active material usually used as a negative electrode active material. Specifically, the carbon-based active material used as the negative electrode active material may be artificial graphite or natural graphite, and refers to a material that is processed into a spherical or dot-shaped form to facilitate the storage and release of lithium ions.

[0090] Meanwhile, the planar conductive material used as the negative electrode conductive material is generally a material having a planar or plate-like shape, and may be expressed as plate-type graphite. That is, it is a material contained in the negative electrode active material layer to maintain a conductive path, and it means a material that does not play a role in storing and releasing lithium, but secures a planar conductive path inside the negative electrode active material layer.

[0091] That is, in this application, the use of plate-like graphite as a conductive material means that it is processed into a planar or plate-like shape and used as a material that ensures a conductive path that does not serve the role of storing or releasing lithium. At this time, the negative electrode active material contained therein has high capacity characteristics for storing and releasing lithium, and serves to store and release all the lithium ions transferred from the positive electrode.

[0092] Meanwhile, in the present application, the carbon-based active material being used as an active material means that it is processed into a dotted or spherical shape and used as a material that plays a role in storing or releasing lithium.

[0093] That is, in one embodiment of the present application, the carbon-based active material, artificial graphite or natural graphite, has a BET specific surface area of ​​0.1 m 2 / g or more 4.5m 2 / g or less. The plate-shaped graphite, which is a planar conductive material, is planar and has a BET specific surface area of ​​5 m 2 / g or more.

[0094] In one embodiment of the present application, the negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, Ca, or the like, or may include various copolymers thereof.

[0095] The negative electrode binder according to one embodiment of the present application plays a role in controlling the negative electrode active material and the negative electrode conductive material in order to prevent twisting and deformation of the negative electrode structure during volume expansion and relaxation of the silicon-based active material. When the above role is fulfilled, all common negative electrode binders may be applied, specifically, a water-based binder may be used, and more specifically, a PAM-based binder or an SBR binder may be used.

[0096] In one embodiment of the present application, based on 100 parts by weight of the negative electrode active material layer composition, the negative electrode binder may be contained in an amount of 30 parts by weight or less, preferably 25 parts by weight or less, more preferably 20 parts by weight or less, or may be contained in an amount of 1 part by weight or more, preferably 3 parts by weight or more.

[0097] In one embodiment of the present application, the electrode may be a positive electrode, and the following describes a method for manufacturing a positive electrode for a lithium secondary battery. In this case, the same description as for the method for manufacturing a negative electrode for a lithium secondary battery may be applied, except for the positive electrode.

[0098] A method for manufacturing an electrode for a lithium secondary battery according to an embodiment of the present application may include forming a positive electrode current collector layer, and a positive electrode active material layer on one or both sides of the positive electrode current collector layer.

[0099] In one embodiment of the present application, the positive electrode current collector layer is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, plastic carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector layer may usually have a thickness of 3 μm to 500 μm, and fine irregularities may be formed on the surface of the positive electrode current collector layer to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0100] The thickness of the positive electrode current collector layer may vary depending on the type and use of the positive electrode, but is not limited thereto.

[0101] In one embodiment of the present application, there is provided a method for producing an electrode for a lithium secondary battery, wherein the step of forming a positive electrode current collector layer and a positive electrode active material layer on one or both sides of the positive electrode current collector layer includes a step of coating one or both sides of the positive electrode current collector layer with a positive electrode slurry containing a positive electrode active material layer composition, and the positive electrode active material layer composition includes one or more selected from the group consisting of a positive electrode active material, a positive electrode conductive material, and a positive electrode binder.

[0102] In one embodiment of the present application, the content of the positive electrode slurry may be the same as that of the negative electrode slurry, except for the positive electrode.

[0103] In one embodiment of the present application, the positive electrode active material layer composition may include one or more selected from the group consisting of a positive electrode active material, a positive electrode conductive material, and a positive electrode binder.

[0104] The positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), or compounds substituted with one or more transition metals; LiFe 3 O 4 Lithium iron oxide, etc.; chemical formula Li 1+c1 Mn 2-c1 O 4 (0≦c1≦0.33), LiMnO 3 , LiMn 2 O 3 , LiMnO 2 Lithium manganese oxides such as lithium copper oxide (Li 2 CuO 2 );LiV 3 O 8 , V 2 O 5 , Cu 2 V 2 O 7 Vanadium oxides such as LiNi 1-c2 M c2 O 2(wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01≦c2≦0.3); Ni-site type lithium nickel oxide represented by the chemical formula LiMn 2-c3 M c3 O 2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c3≦0.1) or Li 2 Mn 3 MO 8 Lithium manganese composite oxide represented by the formula LiMn (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); 2 O 4 The positive electrode may be, but is not limited to, Li metal.

[0105] At this time, the positive electrode conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed.Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in mixture.

[0106] In addition, the positive electrode binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector.Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination.

[0107] In addition, the contents of the positive electrode active material, the positive electrode conductive material, and the positive electrode binder included in the positive electrode active material layer composition may be the same as those applied to the negative electrode active material layer composition.

[0108] In one embodiment of the present application, the present invention may include a method for pre-lithiation of an electrode for a lithium secondary battery, the method including a step of transferring lithium metal onto the electrode active material layer.

[0109] In general, the prelithiation process is performed by chemically or physically prelithiating lithium metal to an electrode, and specifically, may be performed by a lithium metal transfer process, a lithium metal powder deposition process, an electro / chemical process, or a lithium metal deposition process, and the prelithiation process according to the present application may include a lithium metal transfer process.

[0110] The lithium metal transfer process has the characteristic that highly reactive lithium metal can be more stably transferred onto the upper part of the electrode active material layer. At this time, a process is required that can easily transfer the lithium metal from the transfer laminate onto the upper part of the electrode active material layer.

[0111] In one embodiment of the present application, the method may include the steps of: preparing the transfer laminate; laminating the transfer laminate onto the electrode active material layer so that the surface of the lithium metal opposite to the surface that contacts the release layer contacts the surface of the electrode active material layer opposite to the surface that contacts the electrode current collector layer; removing the base layer; and removing the release layer.

[0112] In one embodiment of the present application, the step of preparing the transfer laminate includes a step of coating and laminating a release layer on the substrate layer; a drying step; and a step of laminating the lithium metal on the release layer, and the drying step may include a step of drying for 5 minutes to 1 hour at a drying temperature of 30°C to 90°C.

[0113] That is, by controlling the conditions of the drying step, the adhesive strength of the release layer can be set to a specific range, which can facilitate the transfer of lithium metal during pre-lithiation in the transfer process.

[0114] In one embodiment of the present application, the base layer may be any layer that can withstand process conditions such as high temperatures during the deposition of lithium metal and can prevent a reverse peeling problem in which lithium metal is transferred onto the base layer during a winding process for transferring the deposited lithium metal.

[0115] Specifically, in one embodiment of the present application, the base layer may be one or more selected from the group consisting of polyethylene terephthalate (PET), polyimide (PI), poly(methylmethacrylate) (PMMA), polypropylene, polyethylene, and polycarbonate.

[0116] In one embodiment of the present application, the thickness of the base layer may be in the range of 1 μm or more and 300 μm or less, 5 μm or more and 200 μm or less, or 10 μm or more and 30 μm or less.

[0117] In one embodiment of the present application, the thickness of the lithium metal may be 1 μm or more and 10 μm or less, and preferably may be 3 μm or more and 10 μm or less.

[0118] When the thicknesses of the substrate layer and the lithium metal satisfy the above ranges, the lithium metal can be efficiently transferred to the electrode active material layer, and reverse transfer can be prevented.

[0119] In one embodiment of the present application, the transfer laminate includes a release layer on the surface where the base material layer and the lithium metal come into contact in order to improve the peelability of the lithium metal, ensure transferability to the electrode active material layer, and act as a protective layer after transfer of the lithium metal.

[0120] That is, the base layer may have a release layer formed on at least one surface thereof, or may have release layers formed on both surfaces thereof. The release layer can prevent a reverse peeling problem in which lithium metal is transferred onto the base layer during a winding process for transferring the deposited lithium metal to an electrode, and can easily separate the base layer after the lithium metal is transferred onto the electrode active material layer.

[0121] In one embodiment of the present application, there is provided a method for producing an electrode for a lithium secondary battery, wherein the release layer comprises one or more selected from the group consisting of polyvinylidene fluoride (PVDF), polyethylene (PE), polypropylene (PP), polyacrylic acid (PAA), and polyester.

[0122] In one embodiment of the present application, there is provided a method for producing an electrode for a lithium secondary battery, wherein the release layer has a thickness of 0.1 μm or more and 2 μm or less.

[0123] When the thickness of the release layer satisfies the above range, lithium metal can be easily transferred from the transfer laminate to the electrode active material layer, and when the release layer is removed from the top of the electrode active material layer after pre-lithiation, the release layer can be easily removed without being cut or peeled off.

[0124] In one embodiment of the present application, a deposition method for depositing the lithium metal on the substrate layer on which the release layer is formed may be selected from among vacuum deposition, chemical vapor deposition (CVD), and physical vapor deposition, but is not limited thereto, and various deposition methods used in the art may be used.

[0125] In one embodiment of the present application, a physical vapor deposition method may be used as a deposition method for depositing the lithium metal on the base layer on which the release layer is formed.

[0126] At this time, the lithium secondary battery electrode on which the transfer laminate was laminated was subjected to a pressure of 5 kgf / cm 2 ~500kgf / cm 2 The lamination process can be performed by roll pressing while applying a load of 10 ...

[0127] In one embodiment of the present application, the release layer may be formed by a coating method, for example, the coating method may be a method selected from the group consisting of dip coating, spray coating, spin coating, die coating, gravure coating, micro-gravure coating, comma coating, and roll coating, but is not limited thereto, and various coating methods available in the art for forming a coating layer may be used.

[0128] In one embodiment of the present application, the transfer laminate is laminated on the electrode active material layer so that a surface of the lithium metal opposite to a surface contacting the release layer is in contact with a surface of the electrode active material layer opposite to a surface contacting the current collector layer, and the lamination is performed at a temperature of 30° C. or less and a pressure of 10 kgf / cm 2 More than 150kgf / cm 2 The following pressures may be used for lamination:

[0129] After the lamination step, prelithiation of the electrode active material layer with highly reactive lithium metal may be performed.

[0130] In another embodiment, the lamination step may be performed at a temperature of 30° C. or less, preferably 25° C. or less, or at a temperature of 10° C. or more, preferably 15° C. or more.

[0131] That is, as described above, when lamination is performed under conditions that allow the heat generated in the electrode to be easily released and corresponds to the above temperature condition range, the pre-lithiation reaction rate is appropriate when performing lamination, so that heat is not accumulated and a state in which it is easy to remove the release layer later can be formed.

[0132] In one embodiment of the present application, the laminating step is performed at a pressure of 10 kgf / cm 2 More than 150kgf / cm 2 The following pressures may be used for lamination:

[0133] In yet another embodiment, the laminating step is performed at a pressure of 150 kgf / cm 2 Preferably, 100 kgf / cm or less 2 It may be less than or equal to 50 kgf / cm 2 It may be less than 10kgf / cm 2 The above range may be satisfied.

[0134] As described above, the pressure range is satisfied during the lamination step, and the pressure conditions are suitable for transferring the lithium metal, and the release layer can be prevented from being detached from the surface of the electrode. Furthermore, the pressure and temperature conditions are satisfied, and the release layer can be easily removed later, thereby preventing an increase in resistance during assembly of the cell.

[0135] Specifically, the lamination step is performed at 150 kgf / cm 2 If lamination is performed with a pressure exceeding 10 kgf / cm, the adhesive strength of the release layer to the lithium metal increases, making it difficult to remove the release layer, and if the release layer is forcibly removed, the electrode may detach. 2 If lamination is performed with a pressure less than this, the transfer of lithium metal to the electrode active material layer may not be performed well.

[0136] In one embodiment of the present application, there is provided a method for producing an electrode for a lithium secondary battery, wherein the step of transferring the lithium metal includes a step of laminating the transfer laminate onto the electrode active material layer to prelithiate the electrode active material layer, and the step of prelithiating the electrode active material layer comprises prelithiating the electrode active material layer within 30 minutes to 24 hours after transferring the lithium metal.

[0137] When the electrode active material layer is prelithiated, the electrode active material layer generates heat at a rate of 5° C. / min for 30 seconds to 3 minutes and then cools down.

[0138] The step of prelithiating the electrode active material layer is performed at 25° C. and 1 atm within 30 minutes to 24 hours.

[0139] The pre-lithiation step is a step of setting conditions for lithium metal to diffuse into the electrode active material layer, and whether the pre-lithiation is completed can be determined by whether lithium at the top of the electrode active material layer is completely consumed.

[0140] In one embodiment of the present application, the activation reaction time may be 30 minutes to 48 hours, preferably 1 hour to 2 hours.

[0141] In one embodiment of the present application, the step of transferring the lithium metal includes removing the substrate layer.

[0142] In the conventional lithium metal transfer process, there was a problem that the base layer was difficult to peel off during the prelithiation process after lamination of the transfer laminate. As a result, the prelithiation was performed without removing the base layer, and the heat generated during the prelithiation was blocked by the base layer and not released, and by-products were formed on the surface during the prelithiation of the lithium metal, which caused polymer crosslinking in the release layer, making it difficult to remove the release layer.

[0143] However, by adjusting the lamination pressure, temperature, and heat generation per hour in the pre-lithiation process within appropriate ranges, the substrate layer was easily peeled off after laminating the transfer laminate, and as a result, polymer crosslinking in the release layer did not occur, making it possible to easily remove the release layer.

[0144] In one embodiment of the present application, the step of removing the substrate layer may be performed within 1 hour after the step of laminating the transfer laminate onto the electrode active material layer, preferably within 30 minutes after the step of laminating, and most preferably, the substrate layer is removed immediately after the lamination step.

[0145] The step of removing the substrate layer is preferably performed within the above-mentioned time range. In particular, if the substrate layer is removed after 1 hour from the lamination step, a large amount of lithium by-products are rapidly generated, which increases the adhesive strength between the release layer and the electrode active material layer, making it difficult to remove the release layer.

[0146] In one embodiment of the present application, the step of transferring the lithium metal includes removing the release layer, specifically, removing the release layer on top of the pre-lithiated electrode active material layer after pre-lithiation as described above.

[0147] At this time, if the above process conditions are met, polymer crosslinking of the release layer does not occur, and thus the release layer can be easily removed. If the above conditions are not met, crosslinking of the release layer occurs, and the release layer cannot be removed, and the force required for removal increases, which may cause problems such as detachment of the electrode.

[0148] That is, the pre-lithiation method of an electrode for a lithium secondary battery according to the present application has the following characteristics: by controlling the process conditions as described above, the base layer can be easily peeled off immediately after lamination of the transfer laminate, the generation of by-products during pre-lithiation can be suppressed, and the release layer can be easily removed by preventing an increase in the adhesive force between the release layer and the pre-lithiated electrode active material layer.

[0149] At this time, the release layer 35 used in the pre-lithiation can be removed as described above, and thus it does not remain on the top of the electrode, preventing an unnecessary increase in resistance. That is, the release layer can be used to improve the transfer force and also to protect the lithium metal before the pre-lithiation, and may be removed before the electrolyte is injected.

[0150] In one embodiment of the present application, examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries, but are not limited thereto.

[0151] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.

[0152] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0153] In particular, among the carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are highly viscous organic solvents having a high dielectric constant and capable of dissociating lithium salts, and therefore can be preferably used. When such a cyclic carbonate is mixed with a linear carbonate having a low viscosity and a low dielectric constant, such as dimethyl carbonate and diethyl carbonate, in an appropriate ratio, an electrolyte having high electrical conductivity can be produced, and therefore such a cyclic carbonate can be more preferably used.

[0154] The metal salt may be a lithium salt, and the lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte solution. For example, the anion of the lithium salt is F - , Cl - , I - , NO 3 - , N(CN) 2 - , B.F. 4 - , ClO 4 - , P.F. 6 - , (CF 3 ) 2 PF 4 - , (CF 3 ) 3 PF 3 - , (CF 3 ) 4 PF 2 - , (CF 3 ) 5 PF - , (CF 3 ) 6 P - , C.F. 3 SO 3 - , C.F. 3 CF 2 SO 3 - , (CF 3 SO 2 ) 2 N - , (FSO 2 ) 2 N- , C.F. 3 CF 2 (CF 3 ) 2 CO - , (CF 3 SO 2 ) 2 CH - ,(SCIENCE FICTION 5 ) 3 C - , (CF 3 SO 2 ) 3 C - , C.F. 3 (CF 2 ) 7 SO 3 - , C.F. 3 CO 2 - , C.H. 3 CO 2 - , SCN - and (CF 3 CF 2 SO 2 ) 2 N - One or more selected from the group consisting of may be used.

[0155] In addition to the components of the electrolyte, the electrolyte may further include one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride, for the purpose of improving battery life characteristics, suppressing a decrease in battery capacity, and improving battery discharge capacity.

[0156] In one embodiment of the present invention, there is provided a lithium secondary battery comprising: a positive electrode for a lithium secondary battery; a negative electrode for a lithium secondary battery; a separator provided between the positive electrode and the negative electrode; and an electrolyte, wherein at least one of the positive electrode for the lithium secondary battery and the negative electrode for the lithium secondary battery is a lithium secondary battery electrode that has been prelithiated according to the present application.

[0157] According to an embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same. The battery module and the battery pack include the secondary battery having high capacity, high rate characteristics, and high cycle characteristics, and may be used as a power source for a medium- to large-sized device selected from the group consisting of an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, and a power storage system. EXAMPLES

[0158] In the following, preferred embodiments are presented to aid in understanding the present invention. However, these embodiments are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope of the scope and technical ideas of the present description. Naturally, such changes and modifications fall within the scope of the claims.

[0159] <Example> <Production of Transfer Laminate> An acrylate polymer release layer was coated on the top of the PET (25 um) layer as the substrate layer to improve the transferability, and then lithium metal was deposited on the top of the PET substrate to a thickness of 6 μm using the PVD method to produce a transfer laminate.

[0160] <Production of negative electrodes> A negative electrode slurry was prepared by adding Si (average particle size (D50): 3.5 μm) as a silicon-based active material, Denka Black as a conductive material, SBR as a binder, and CMC as a thickener in a weight ratio of 80:15.8:3:1.2 to distilled water as a solvent for forming a negative electrode slurry (solid concentration 25 wt%).

[0161] The mixing method was as follows: the conductive material, binder, thickener and water were dispersed using a homomixer at 2500 rpm for 30 minutes, the active material was then added, and the mixture was dispersed at 2500 rpm for 30 minutes to prepare a slurry.

[0162] The negative electrode current collector was a copper current collector (thickness: 8 μm) with the negative electrode slurry applied to both sides at 85 mg / 25 cm. 2 The coated layer was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a negative electrode active material layer (thickness: 33 μm), which was used as a negative electrode (negative electrode thickness: 41 μm, negative electrode porosity: 40.0%).

[0163] Example 1 Thereafter, in order to transfer the transfer laminate to the negative electrode active material layer, the lithium metal of the transfer laminate was placed on top of the negative electrode active material layer, and then the lithium metal and the negative electrode active material layer were bonded by roll pressing under external pressure conditions of the load and temperature conditions in Table 1. Immediately after lamination, the PET layer of the transfer laminate was removed, and the negative electrode was pre-lithiated.

[0164] The conditions for pre-lithiation are as shown in Table 1. After the negative electrode was pre-lithiated, the release layer remaining on the surface of the negative electrode active material layer was removed using Scotch tape (3M tape).

[0165] Example 2 and Example 3 In Example 2, the negative electrode was prelithiated in the same manner as in Example 1, except that the external pressure condition was slightly higher than that in Example 1. In Example 3, the negative electrode was prelithiated in the same manner as in Example 1, except that the lithium metal in Example 1 was deposited on the top of the PET substrate to a thickness of 8 μm.

[0166] Comparative Example 1 to Comparative Example 4 In Comparative Example 1, the negative electrode was prelithiated in the same manner as in Example 1, except that the PET substrate was removed 1 hour after lamination. In Comparative Example 2, the external pressure was 180 kgf / mm 2 The external pressure was set to 180 kgf / mm. The PET substrate was removed immediately after lamination, but the release layer was not removed. 2 The negative electrode was prelithiated in the same manner as in Example 1, except that the external pressure was set high at 5 kgf / mm and the PET substrate was removed 1 hour after lamination. 2 The negative electrode was prelithiated in the same manner as in Example 1, except that the temperature was set to a low value of 0.01 V.

[0167] At this time, the adhesive strength between the release layer and the electrode active material layer in Examples 1 to 3 and Comparative Examples 1 to 4 is as shown in Table 1 below, and the evaluation results before and after lithiation are as shown in Table 2 below.

[0168] [Table 1]

[0169] In Table 1, the adhesive strength was measured by attaching 3M double-sided tape to glass (22 mm wide) and then cutting the electrodes to a width of 20 mm and attaching them. The sample was then placed at a 90° angle on the adhesive strength measurement equipment and the force was measured while peeling it off at a specified speed. The unit of measurement was gf, and since the sample width was 20 mm, the unit gf / 20 mm was used. The physical properties in Table 2 below were measured by preparing a bi-cell type battery with the negative electrode and NCM as the positive electrode as counter electrodes. The electrolyte used in this battery was 1M LiPF 6The mixture was dissolved in ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 3 / 7 (volume ratio).

[0170] The capacity of the bi-cell type battery prepared above was confirmed using an electrochemical charger / discharger. It was charged to 4.2V (vs. Li / Li+) at 0.05C with a current density of 1C, and discharged to 2.5V at 0.5C (vs. Li / Li+). It was then charged again to 4.2V and discharged to SOC50, at which point a 2.5C current pulse was applied for 30 seconds to observe the voltage change, and the resistance was calculated for 0.1 seconds, 0.1 to 30 seconds, and 0 to 30 seconds, as shown in Table 2 below. The results are shown in Table 2 below.

[0171] [Table 2]

[0172] As can be seen from Examples 1 to 3 in Tables 1 and 2, it was confirmed that the release layer can be easily separated from the upper part of the electrode active material layer by adjusting the process conditions in the pre-lithiation process of the electrode active material layer according to the present application. In particular, it was confirmed in detail from Table 2 that the release layer can be easily removed, and since the electrode manufactured by the above process does not have a separate layer such as a release layer on the upper part of the electrode active material layer, the electrode has a characteristic that the resistance does not increase during the operation of the battery after the cell is assembled.

[0173] In the case of Example 3, when the thickness of the lithium was changed to be thicker than in Examples 1 and 2, the thicker the lithium, the more the amount of lithium that enters the electrode and secures space, so the thickness of the electrode becomes thicker, which may be a cause of an increase in resistance due to by-products of lithium that are not inserted into the active material. However, as can be seen in Table 2, it was confirmed that the release layer was easily removed, and therefore the increase rate of resistance was not as high as in Comparative Examples 1 and 2.

[0174] In the case of Comparative Example 1, since the PET film is not immediately removed after pre-lithiation and heat is not generated, lithium by-products are rapidly generated in large quantities. As a result, it was confirmed that the adhesive strength between the release layer and the electrode active material layer is increased, and therefore the release layer cannot be removed. In particular, it was confirmed that when the release layer is forcibly removed, the electrode detaches, causing problems and increasing resistance.

[0175] In the case of Comparative Example 2, since the release layer was not removed, it was confirmed that the resistance was increased compared to Examples 1 to 3 when the electrode was driven, as shown in Table 2.

[0176] In the case of Comparative Example 3, the pressure in the lamination step was high, which increased the adhesive force between the release layer and the electrode active material layer, and therefore the release layer was not removed. In the case of Comparative Example 4, the pressure in the lamination step was too low, which prevented pre-lithiation from being performed well, and therefore it was confirmed that the electrode resistance of Comparative Examples 3 and 4 was increased.

[0177] As a result, compared to Comparative Examples 1 to 4, in the case of Examples 1 to 3, the release layer was easily removed by satisfying a predetermined pressure condition in the lamination step in the pre-lithiation process, and it was confirmed that the resistance was reduced as shown in Table 2 when the electrode from which the release layer was removed was operated. [Explanation of symbols]

[0178] 10...Base material layer 20 Lithium metal 30...electrode active material layer 35...Release layer 40 Electrode current collector layer 100 ···Transfer laminate 200 ···Electrodes for lithium secondary batteries

Claims

1. forming an electrode current collector layer, and an electrode active material layer on one or both sides of the electrode current collector layer; transferring lithium metal onto the electrode active material layer; A method for producing an electrode for a lithium secondary battery, comprising: The step of transferring the lithium metal includes the steps of: preparing a transfer laminate in which a base layer, a release layer, and lithium metal are sequentially laminated; laminating the transfer laminate on the electrode active material layer so that a surface of the lithium metal opposite to a surface that contacts the release layer contacts a surface of the electrode active material layer opposite to a surface that contacts the electrode current collector layer; removing the base layer; and removing the release layer. The lamination step is performed under a temperature condition of 30° C. or less and a pressure of 10 kgf / cm 2 More than 150kgf / cm 2 A method for manufacturing an electrode for a lithium secondary battery, comprising lamination at the following pressure:

2. The lamination step is performed under a temperature condition of 30° C. or less and a pressure of 10 kgf / cm 2 More than 100kgf / cm 2 The method for producing an electrode for a lithium secondary battery according to claim 1 , wherein lamination is performed at a pressure of:

3. the step of transferring the lithium metal includes laminating the transfer laminate onto the electrode active material layer to prelithiate the electrode active material layer; 2 . The method of claim 1 , further comprising removing the release layer after prelithiating the electrode active material layer. 3 . The method of claim 1 , further comprising removing the release layer after prelithiating the electrode active material layer.

4. 4. The method of claim 3, wherein when the electrode active material layer is prelithiated, the electrode active material layer is heated at a rate of 5° C. / min for 30 seconds to 3 minutes and then cooled down.

5. The method of claim 1 , wherein the removing of the base layer is performed within one hour after the lamination of the transfer laminate on the electrode active material layer.

6. 2. The method for producing an electrode for a lithium secondary battery according to claim 1, wherein the release layer comprises one or more selected from the group consisting of polyvinylidene fluoride (PVDF), polyethylene (PE), polypropylene (PP), polyacrylic acid (PAA), and polyester.

7. The method for producing an electrode for a lithium secondary battery according to claim 1 , wherein the release layer has a thickness of 0.1 μm or more and 2 μm or less.

8. The method for producing an electrode for a lithium secondary battery according to claim 1 , wherein the thickness of the substrate layer is 10 μm or more and 30 μm or less.

9. The step of forming the electrode current collector layer and the electrode active material layer on one or both sides of the electrode current collector layer includes coating one or both sides of the electrode current collector layer with an electrode slurry including an electrode active material layer composition; 2. The method for producing an electrode for a lithium secondary battery according to claim 1, wherein the electrode active material layer composition comprises one or more selected from the group consisting of an electrode active material; an electrode conductive material; and an electrode binder.

10. The electrode active material includes a silicon-based active material, The silicon-based active material is SiO x (x=0), SiO x The method for producing an electrode for a lithium secondary battery according to claim 9 , comprising at least one selected from the group consisting of (0<x<2), SiC, and a Si alloy.

11. Positive electrodes for lithium secondary batteries; Negative electrodes for lithium secondary batteries; A separator disposed between the positive electrode and the negative electrode; and electrolyte A lithium secondary battery comprising: A lithium secondary battery, wherein at least one of the positive electrode for the lithium secondary battery and the negative electrode for the lithium secondary battery is an electrode for a lithium secondary battery produced by the method according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Transfer film, electrode plate for electrochemical element formed using the same, and lithium secondary battery

    JP2007273459A

  • Method for manufacturing negative electrode for lithium secondary battery

    JP2020501315A

  • The funeral service management system in which the funeral reservation process is included

    KR1020210126413A

  • Swing check valve with decreasing friction force of a hinge part, and control method thereof

    KR1020230014312A

  • Method for manufacturing negative electrode for secondary battery and negative electrode for secondary battery

    US20190237750A1