Negative electrode material for secondary batteries and its manufacturing method
A method for producing a silicon-carbon composite negative electrode material through curing and pitch coating addresses structural issues, improving the performance and lifespan of secondary batteries by ensuring uniform and dense coating on silicon particles.
Patent Information
- Application Number
- JP2024531715
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-11-29
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-11-29
AI Technical Summary
Existing methods for producing negative electrode materials using silicon-based composites face challenges such as structural destruction due to volume expansion, poor dispersion and oxidation issues, leading to decreased performance and short lifespan of secondary batteries.
A method involving the formation of spherical powder particles from nanosilicon, organic resin, and conductive material, followed by a curing process and coating with high softening point pitch, then carbonizing, to achieve uniform and dense pitch coating on silicon particles, forming a high-quality silicon-carbon composite.
The method results in improved initial discharge capacity, efficiency, and life characteristics of secondary batteries by maintaining the shape and uniformity of the spherical powder particles, enhancing the performance of the negative electrode material.
Smart Images

Figure 2024540676000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a negative electrode material for a secondary battery, which can improve the initial discharge capacity (IDC), initial efficiency (ICE) and life characteristics of the secondary battery. [Background technology]
[0002] The improvement of secondary battery performance is based on the components of the positive electrode material, the negative electrode material, and the electrolyte.
[0003] Among the above components, graphite-based materials, which are mainly used as anode materials, are widely used commercially due to their excellent electrochemical performance and low price. However, their theoretical capacity is limited to 370 mAh / g, which limits their application to high-capacity secondary batteries.
[0004] To overcome the above limitations, non-graphite anode materials such as silicon, tin, and germanium have emerged as alternative materials, of which silicon has a theoretical capacity of 4000-4200mAh / g, which is more than 10 times higher than graphite, and is therefore attracting attention as a material that can replace graphite. However, compared to its high theoretical capacity, silicon experiences a large volume expansion of up to 400% during charging and discharging, which can lead to structural destruction of the material and a short lifespan.
[0005] To mitigate the volume expansion of silicon, a method has been devised in which a carbon material is mixed in to produce a composite material, but it remains difficult to effectively bond silicon with the carbon material.
[0006] For this reason, a method has been developed in which spherical powder particles are formed from a slurry containing nano silicon particles, and then the surfaces of the spherical powder particles are coated with pitch as a carbon material. In this case, in order to turn nano silicon into spherical powder particles, an organic resin or water-based resin capable of bonding nano silicon to each other can be mixed, but the properties of the resin used can affect the performance of the negative electrode material and the secondary battery to which it is ultimately applied.
[0007] Specifically, when a water-based resin is used, water is added as a solvent, but since an organic solvent is used when producing nanosilicon particles, the water solvent reacts with the nanosilicon, causing oxidation, which leads to problems with dispersion and oxidation degree, resulting in a decrease in the performance of the secondary battery produced.
[0008] If an organic resin is used, there is a problem that in the next step of coating the pitch, the organic resin is also dissolved in the organic solvent used in the pitch solution, causing the shape of the silicon-containing particles to be destroyed.
[0009] In the case of the dry coating method, which does not use a solvent, coating is performed by a physical rubbing method, so there is a problem that the spherical powder particles are broken, a lot of fine powder is generated, and the uniformity of the coating is significantly reduced.
[0010] Therefore, it is necessary to develop a method for producing a high-quality negative electrode material for secondary batteries that can solve the above problems and improve the initial discharge capacity, initial efficiency, and life characteristics of secondary batteries. Summary of the Invention [Problem to be solved by the invention]
[0011] An object of the present invention is to provide a method for producing a negative electrode material for secondary batteries, comprising a high-quality nanosilicon-carbon composite material in which the surfaces of nanosilicon particles are uniformly and densely coated with pitch.
[0012] Another object of the present invention is to provide a negative electrode material for a secondary battery manufactured according to the manufacturing method of the negative electrode material for a secondary battery, so as to improve the initial discharge capacity, initial efficiency and life characteristics of the secondary battery, and a secondary battery including the same.
[0013] The object of the present invention is not limited to the object mentioned above, and other objects and advantages of the present invention not mentioned can be understood from the following description and can be more clearly understood from the embodiments of the present invention. In addition, it is easy to understand that the object and advantages of the present invention can be realized by the means and combinations thereof as set forth in the claims. [Means for solving the problem]
[0014] According to one aspect of the present invention, there is provided a method for manufacturing an anode material for a secondary battery, the method including: mixing nanosilicon particles, an organic resin, and a conductive material in a first solvent to form a slurry; drying the slurry to form spherical powder particles; hardening the spherical powder particles; dissolving a high softening point pitch in a second solvent to form a pitch solution; coating the hardened spherical powder particles with the pitch solution; and carbonizing the pitch-coated powder.
[0015] According to another aspect of the present invention, there is provided a method for manufacturing an anode material for a secondary battery, the method including: mixing nanosilicon particles, an organic resin, a conductive material, and a curing agent in a first solvent to form a slurry; drying the slurry to form spherical powder particles; curing the spherical powder particles; dissolving a high softening point pitch in a second solvent to form a pitch solution; coating the hardened spherical powder particles with the pitch solution; and carbonizing the pitch-coated powder.
[0016] According to yet another aspect of the present invention, there can be provided a negative electrode material for a secondary battery produced according to the method for producing a negative electrode material for a secondary battery of the present invention. Effect of the Invention
[0017] According to the method for producing a negative electrode material for a secondary battery according to the present invention, the surface of silicon particles can be uniformly and densely coated with pitch, and a high-quality negative electrode material for a secondary battery containing a silicon-carbon composite can be produced.
[0018] By applying the negative electrode material for secondary batteries produced according to the method for producing a negative electrode material for secondary batteries according to the present invention, the initial discharge capacity, initial efficiency and life characteristics of the secondary battery can be improved.
[0019] The above-mentioned effects and specific effects of the present invention will be described in conjunction with the following description of the preferred embodiment of the invention. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 is a flow chart showing a method for producing a negative electrode material for a secondary battery according to one embodiment of the present invention. [Figure 2a] FIG. 2 is a SEM image of a silicon-carbon composite material in which the surfaces of silicon particles are coated with pitch in Example 1 according to the present invention. [Figure 2b] FIG. 2 is a graph showing the results of particle size analysis (PSA) of a silicon-carbon composite material in which the surfaces of silicon particles are coated with pitch in Example 1 according to the present invention. [Figure 3a] FIG. 2 is a SEM image of a silicon-carbon composite material in which the surfaces of silicon particles are coated with pitch in Comparative Example 1 according to the present invention. [Figure 3b] FIG. 2 is a graph showing the results of particle size analysis (PSA) of a silicon-carbon composite material in which the surfaces of silicon particles are coated with pitch in Comparative Example 1 according to the present invention. [Figure 4a] FIG. 2 shows an SEM image of a silicon-carbon composite material in which the surfaces of silicon particles are coated with pitch in Comparative Example 2 according to the present invention. [Figure 4b]FIG. 2 is a graph showing the results of particle size analysis (PSA) of a silicon-carbon composite material in which the surfaces of silicon particles are coated with pitch in Comparative Example 2 according to the present invention. [Diagram 5] FIG. 2 is a graph showing the results of a half-cell test of Example 1 according to the present invention and Comparative Example 1. BEST MODE FOR CARRYING OUT THEINVENTION
[0021] The above-mentioned objects, features and advantages will be described in detail below with reference to the accompanying drawings, so that a person having ordinary skill in the art to which the present invention pertains can easily implement the technical idea of the present invention. In describing the present invention, if a detailed description of a known technology according to the present invention is deemed to make the gist of the present invention unclear, the detailed description will be omitted. Hereinafter, a preferred embodiment according to the present invention will be described in detail with reference to the accompanying drawings. The same reference numerals in the drawings are used to indicate the same or similar components.
[0022] Of the contents not described in this specification, those that can be technically inferred by a person of ordinary skill in this technical field will not be described.
[0023] In the following, when an arbitrary structure is arranged on the "top (or bottom)" of a component or "above (or below)" a component, it means that the arbitrary structure is not only arranged in contact with the upper surface (or lower surface) of the component, but also that other structures may be interposed between the component and the arbitrary structure arranged on (or below) the component.
[0024] In addition, when a component is described as being "coupled," "coupled," or "connected" to another component, it should be understood that the components may be directly coupled or connected to each other, but that there may be other components "intervening" between each component, or each component may be "coupled," "coupled," or "connected" via other components.
[0025] The method for producing the negative electrode material for secondary batteries according to the present invention will be described in detail below.
[0026] The present invention provides a high-quality anode material for secondary batteries that can improve the performance of a secondary battery by improving the limitations of the conventional technology in coating silicon particles with pitch, which is a carbon material, and significantly improving the uniformity and denseness of the pitch coating in producing a silicon-carbon composite material as an anode material for secondary batteries.
[0027] In particular, in the present invention, when preparing a slurry containing silicon particles, an organic resin is used and a curing process step is included before the pitch coating step. Therefore, the organic resin is not dissolved in the organic solvent of the pitch solution used in the subsequent pitch coating step, so that the shape of the spherical powder particles of the active material containing silicon particles can be maintained, and the pitch coatability of the silicon surface can be significantly improved.
[0028] As described above, the present invention is characterized in that it further includes a curing process after forming spherical powder particles from a slurry containing silicon particles and before coating with a pitch solution, so that even if the pitch coating is performed in a liquid state, the organic resin does not dissolve in the organic solvent of the pitch solution.
[0029] In the present invention, the curing process is divided into two types. The first is a thermal curing process, and the second is a process in which a curing agent is added and mixed together when preparing a silicon-containing slurry, so that curing can occur without applying heat for a suitable period of time.
[0030] FIG. 1 is a flow chart of a method for manufacturing a negative electrode active material according to an embodiment of the present invention. As described above, the curing process is a thermal curing process. Each step will be described below with reference to FIG. 1.
[0031] S1: Mixing nanosilicon particles, an organic resin, and a conductive material in a first solvent to form a slurry. First, nanosilicon particles, an organic resin and a conductive material are mixed in a first solvent to form a slurry.
[0032] The first solvent may be selected from those having excellent solubility in the nanosilicon particles, the organic resin, and the conductive material. For example, the first solvent may contain ethanol, methanol, acetone, isopropyl alcohol, etc., and preferably contains ethanol.
[0033] The organic resin may be a thermosetting resin that is cured when heat is applied. For example, the thermosetting resin may include phenol resin, epoxy resin, thermosetting polyimide, polyester, polyurethane, melamine resin, amino resin, etc. Phenol resin may be preferable, and resol type phenol resin having excellent thermosetting properties is more preferable.
[0034] The conductive material may be included to impart electrical conductivity to the negative electrode material, and may be used without limitation as long as it has electrical conductivity without causing chemical changes. For example, the conductive material may include one or more of a carbon-based material, a metal powder, a metal fiber, a metal oxide, and a conductive polymer, and is preferably a carbon-based material, and more preferably includes carbon black.
[0035] The mixing ratio of the nanosilicon particles, organic resin and conductive material in the slurry is not particularly limited and can be mixed at a normal mixing ratio, for example, the ratio of nanosilicon particles:organic resin:conductive material may be 60-70:20-30:5-10.
[0036] In addition, additives such as stearic acid can be mixed together to prevent oxidation of the nanosilicon particles and improve dispersibility.
[0037] S2: Drying the slurry to form spherical powder particles. The silicon-containing slurry may be dried to form spherical powder particles. As long as spherical powder particles can be formed, the drying method is not particularly limited, but is preferably spray drying.
[0038] Spray drying is a technique in which liquid materials are rapidly dried with hot air to produce powder, and can be carried out using a spray dryer that includes a sprayer, heater, and dryer to atomize liquid materials.
[0039] Spray drying allows the size and shape of particles to be adjusted depending on various conditions such as experimental conditions and liquid state, and is suitable for mass production.
[0040] The average particle size of the spherical powder particles produced as described above can be selected depending on the application of the negative electrode material to be used, but is preferably, for example, 5 to 10 μm.
[0041] S3: Hardening the spherical powder particles Before carrying out the step of coating the spherical powder particles containing nanosilicon particles obtained in the step S2 with pitch, the method may include a step of hardening the spherical powder particles, which has the advantage that even if the spherical powder is subsequently coated with pitch in a liquid state, the organic resin can be prevented from dissolving in the organic solvent used to prepare the pitch solution (hereinafter, corresponding to the second solvent in the step S4), and the shape of the spherical powder particles can be maintained.
[0042] As described above, the curing process step (S3) can be a thermal curing process or a curing process that is carried out without heating for a suitable period of time by mixing the curing agent together when preparing the slurry.
[0043] When the heat curing process is performed, it is preferable to use a thermosetting resin as the organic resin. For example, the heat curing process can be performed at a temperature of 120 to 250°C for 30 to 90 minutes, but is not necessarily limited thereto, and the temperature and time can be adjusted depending on the type of organic resin selected, and curing occurs by a condensation reaction of the resin.
[0044] On the other hand, when the thermal curing process is omitted, a curing agent must be used and it is not necessary to apply heat to a high temperature required for thermal curing. However, time restrictions may occur since the entire process must be completed within the curing time to prevent over-curing due to the curing agent. The curing time varies depending on the amount of curing agent added and the type of curing agent, and can be adjusted according to knowledge in the art. Examples of the curing agent include amine-based curing agents, acid anhydride-based curing agents, and amide-based curing agents. In this case, since it is not necessary to use a thermosetting organic resin, there are many more types of organic resins that can be selected. For example, novolac-type phenol resin, which is a phenolic resin that does not exhibit thermosetting properties, can also be used as the resin.
[0045] As described above, the curing process may be performed by heat curing, or by including a curing agent, and heat curing may be omitted, each of which has different advantages, and may be selected according to the objectives and conditions of each process.
[0046] S4: Dissolving the high softening point pitch in a second solvent to form a pitch solution As described above, when pitch is coated by a dry method, the shape of the spherical powder particles may be destroyed due to the use of a rubbing method, and the uniformity and density of the coating may be reduced. Therefore, in the present invention, in order to coat the spherical powder particles containing silicon with pitch, the pitch may be dissolved in a second solvent to form a pitch solution. The second solvent may include, for example, tetrahydrofuran (THF), quinoline, toluene, pyridine, N-methylpyrrolidone (NMP), xylene, chloroform, dimethyl sulfoxide, n-hexane, etc., and may preferably include tetrahydrofuran (THF).
[0047] In the present invention, in particular, high softening point pitch (HSPP) is used. However, pitch that is liquid at room temperature is incompatible due to its low molecular weight, which causes problems of low carbonization yield and low electrical conductivity after carbonization. Therefore, it is preferable to mix the high softening point pitch with the second solvent to form a pitch solution.
[0048] S5: Coating the hardened spherical powder particles with the pitch solution. The hardened spherical powder particles are mixed with the high softening point pitch solution, and then the mixture is evaporated so that the high softening point pitch is wet-coated on the spherical powder particles. In this case, the mixture can be evaporated and dried in a water bath at 35 to 40°C using an evaporator.
[0049] S6: Carbonizing the pitch-coated powder. The powder coated with the high softening point pitch is carbonized to remove the organic resin, and a silicon-carbon composite material with a surface coated with pitch is obtained as the final particle. For example, the carbonization can be performed by heating up to 1000 to 1100°C in an inert gas atmosphere (e.g., nitrogen atmosphere) and maintaining the temperature for about 1 hour, and the heating rate may be, for example, 5 to 10°C / min. If the carbonization temperature is increased, the effect of removing hydrogen, oxygen, etc. from the organic resin is further increased, but if the carbonization temperature exceeds 1100°C, there is a problem that SiC is formed, so it is preferable to carbonize at a temperature of 1000 to 1100°C.
[0050] As described above, the negative electrode material for secondary batteries manufactured according to the manufacturing method of the negative electrode material for secondary batteries of the present invention includes a silicon-carbon composite material in which high softening point pitch is uniformly and densely coated on silicon particles, and thus has the effect of improving initial discharge capacity, initial efficiency, and life characteristics when applied to secondary batteries. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0051] The present invention will be described in more detail below with reference to preferred embodiments thereof, which are presented as preferred examples of the present invention and are not to be construed as limiting the present invention in any way.
[0052] 1. Manufacturing of negative electrode materials for secondary batteries Example 1 Nano silicon particles (D 50 Average value of 111 nm, D 90 A slurry was formed by mixing 65% by weight of cellulose acetate (average particle diameter: 158 nm), 18% by weight of stearic acid, 10% by weight of resol-type phenolic resin (Konami Chemical Industry Co., Ltd., KC-4300N) as an organic resin, and 7% by weight of carbon black (Imerys Graphite & Carbon Co., Ltd., Super-P product) as a conductive material in ethanol (solid content 20%).
[0053] Then, the slurry is spray dried to obtain a particle size (D 50 The spherical powder particles were then heated at 150° C. for 1 hour to effect thermal curing through a condensation reaction of the resin.
[0054] Meanwhile, a high softening point pitch (HSPP, OCI) was dissolved in tetrahydrofuran (THF) to prepare a pitch solution, and then 32.4 parts by weight of the pitch solution was added to 100 parts by weight of the spherical powder particles, mixed, and then evaporated and dried in a water bath at 35 to 40°C using an evaporator, thereby wet-coating the spherical powder particles with pitch.
[0055] Next, the temperature was raised to 1000 to 1100° C. at a rate of 5° C. in a nitrogen atmosphere, and the temperature was maintained for 1 hour for carbonization, and finally a negative electrode material for secondary batteries was produced.
[0056] Comparative Example 1 A negative electrode material for secondary batteries was produced in the same manner as in Example 1 above, but this differs in that a water-based resin, dextrin resin, was used instead of an organic resin, resol-type phenolic resin, and water was used as a solvent instead of ethanol, and no thermal curing was performed.
[0057] Comparative Example 2 A negative electrode material for a secondary battery was produced in the same manner as in Example 1, but it was different in that no heat curing was carried out.
[0058] 2. Evaluation of the surface of the negative electrode material 2-1. Observation of SEM images Cross sections of the negative electrode materials (silicon-carbon composite materials) prepared in Example 1 and Comparative Examples 1 and 2 were observed using a SEM, and the SEM images are shown in FIG. 2a, FIG. 3a, and FIG. 4a, respectively.
[0059] As can be seen from FIG. 2a, the size of the silicon-carbon composite according to Example 1 is relatively uniform, maintains a round spherical shape, and has excellent shape retention before and after pitch coating.
[0060] As can be seen from FIG. 3a, the silicon-carbon composite according to Comparative Example 1 had non-uniform sizes, was a mixture of large particles and small fine powder, and had a relatively rough surface.
[0061] As can be seen from FIG. 3b, the silicon-carbon composite material according to Comparative Example 2 had an organic resin dissolved in THF, and the spheres were destroyed or clumped together, making it impossible to use it as an anode material.
[0062] 2-2.PSA (Particle size analysis) The negative electrode materials (silicon-carbon composite materials) manufactured in Example 1 and Comparative Examples 1 and 2 were analyzed by a laser diffraction method using a PSA (Particle Size Analyzer) analysis device, BECKMAN COULTER life Sciences, LS 13 320 Particle Size Analyzer. 10 , D 50 and D. 90 The particle size distribution was analyzed by measuring the average diameter and volume (see Table 1 below). The above measurement was carried out three times, and the average diameter and volume were then floated on the horizontal and vertical axes, respectively, and the graphs of the results are shown in Figures 2b, 3b, and 4b, respectively.
[0063] In addition, the differential volume (average) (hereinafter abbreviated as "CV") was calculated based on the above graph. The CV value is a percentage (%) value of the standard deviation of the particle size / average size, and the smaller the value, the more consistent the size is and the narrower the size distribution is. The resulting values are shown in Table 1 below. In order to show a particle size with a very high degree of uniformity, the CV value is preferably 50% or less, and more preferably 40% or less.
[0064] As a result of the analysis, the peak width in the graph of Figure 2b for Example 1 was the narrowest, with a single peak being observed, the peak width in the graph of Figure 3b for Comparative Example 1 was wider than that in Figure 2b, with two peaks being observed, and the peak width in the graph of Figure 4b for Comparative Example 2 was the widest, with three or more peaks being observed.
[0065] Also, as can be seen from Table 1 below, Example 1 had the smallest particle size and the lowest CV value, meeting the target value of 50% or less, and was found to have a very high degree of uniformity. On the other hand, Comparative Examples 1 and 2 not only had larger particle size, but also had relatively high or very high CV values, resulting in a decrease in uniformity.
[0066] [Table 1]
[0067] 3. Half-Cell Test In order to analyze the electrochemical properties of the negative electrode material for secondary batteries, a negative electrode plate was prepared by using a powder obtained by mixing 15% by weight of the negative electrode material prepared in Example 1 and Comparative Example 1 and 85% by weight of artificial graphite as an active material. The negative electrode plate was prepared by casting a slurry obtained by mixing the active material, conductive material (Super-P, Imerys Graphite & Carbon Co.), and binder in a weight ratio of 94:1:5 on copper foil, and the binder was a mixture of CMC and SBR in a weight ratio of 3:7. The prepared negative electrode plate was made into a coin cell using Li metal as a counter electrode, and the electrochemical properties were confirmed. The charge and discharge conditions were charge CC / CV: 0.01V / 0.01C, discharge CC 1.5V, and the rate limiting was 0.2C.
[0068] Using a half-cell device, TOSCAT-3100, the initial charge efficiency (ICE; discharge amount relative to initial charge amount), initial charge capacity (ICC; initial charge capacity), and initial discharge capacity (IDC; initial discharge capacity) were measured and shown in Table 1 below. In order to confirm the life characteristics, the discharge specific capacity at 50 cycles was measured and shown in the graph of FIG. 5 (horizontal axis: number of cycles, vertical axis: specific capacity).
[0069] [Table 2]
[0070] As can be seen from Table 2 and FIG. 5, when the negative electrode material of Example 1 was used, the performance was superior in electrochemical performance to when the negative electrode material of Comparative Example 1 was used.
[0071] Although the present invention has been described above with reference to the illustrative drawings, the present invention is not limited to the embodiments and drawings disclosed in this specification, and it is obvious that various modifications can be made by those skilled in the art within the scope of the technical concept of the present invention. Furthermore, even if the effects of the configuration of the present invention are not explicitly described and explained while describing the embodiments of the present invention, it is natural that the effects that can be predicted by the configuration should also be recognized.
Claims
1. mixing the nanosilicon particles, the organic resin and the conductive material in a first solvent to form a slurry; drying the slurry to form spherical powder particles; hardening the spherical powder particles; dissolving the high softening point pitch in a second solvent to form a pitch solution; coating the hardened spherical powder particles with the pitch solution; and carbonizing the pitch-coated powder; Including, A method for producing negative electrode material for secondary batteries.
2. mixing the nanosilicon particles, the organic resin, the conductive material, and the curing agent in a first solvent to form a slurry; drying the slurry to form spherical powder particles; hardening the spherical powder particles; dissolving the high softening point pitch in a second solvent to form a pitch solution; coating the hardened spherical powder particles with the pitch solution; and carbonizing the pitch-coated powder; Including, A method for producing negative electrode material for secondary batteries.
3. The first solvent includes one or more selected from the group consisting of ethanol, methanol, acetone, and isopropyl alcohol. The method for producing the negative electrode material for secondary batteries according to claim 1 or 2.
4. The organic resin includes at least one selected from the group consisting of a phenolic resin, an epoxy resin, a thermosetting polyimide, a polyester, a polyurethane, a melamine resin, and an amino resin. The method for producing the negative electrode material for secondary batteries according to claim 1 or 2.
5. The conductive material includes carbon black. The method for producing the negative electrode material for secondary batteries according to claim 1 or 2.
6. The drying step is carried out by spray drying. The method for producing the negative electrode material for secondary batteries according to claim 1 or 2.
7. The average particle size of the spherical powder particles is 5 to 10 μm. The method for producing the negative electrode material for secondary batteries according to claim 1 or 2.
8. The second solvent includes at least one selected from the group consisting of tetrahydrofuran (THF), quinoline, toluene, pyridine, N-methylpyrrolidone (NMP), xylene, chloroform, dimethyl sulfoxide, and n-hexane; The method for producing the negative electrode material for secondary batteries according to claim 1 or 2.
9. The curing is carried out by heat curing at a temperature of 120 to 250 ° C for 30 minutes or more. The method for producing the negative electrode material for secondary batteries according to claim 1 .
10. The curing agent includes at least one curing agent selected from the group consisting of an amine-based curing agent, an anhydride-based curing agent, and an amide-based curing agent. The method for producing the negative electrode material for secondary batteries according to claim 2.
11. The curing is carried out at a temperature of 20 to 27°C. The method for producing the negative electrode material for secondary batteries according to claim 2.
12. The carbonization is carried out at a temperature of 1000 to 1100°C. The method for producing the negative electrode material for secondary batteries according to claim 1 or 2.
13. A negative electrode material for a secondary battery, produced by the method according to claim 1 or 2.
14. A secondary battery comprising a negative electrode material for a secondary battery produced according to the production method of claim 1 or 2.
Citation Information
Patent Citations
Preparation method of modified graphite negative material of lithium-ion battery
CN103311514A
Preparation method of high-performance silicon carbon anode material
CN107394137A
Silicon-carbon composite material, lithium ion battery, preparation method and application
CN111312996A
Silicon-carbon negative electrode precursor material, silicon-carbon negative electrode material and preparation method thereof
CN111653745A
Silicon monoxide composite material, electrode, lithium ion battery and preparation method and application thereof
CN112713262A