Method for fabricating a vertical cavity surface emitting laser - Patents.com

By using heteroepitaxy and substrate removal techniques to grow high-crystalline quality III-nitride layers and install DBR mirrors on masked GaN templates, the method addresses the complexity of VCSEL fabrication, resulting in improved yield and performance of VCSELs.

JP2024540892AInactive Publication Date: 2024-11-06RGT UNIV OF CALIFORNIA

Patent Information

Application Number
JP2024523163
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-22
Filing Date
2022-10-24
Publication Date
2024-11-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The challenge in fabricating vertical cavity surface emitting lasers (VCSELs) lies in the difficulty of creating a distributed Bragg reflector (DBR) for the resonant cavity due to significant tensile strain between AlN and GaN, leading to complex manufacturing processes and reduced yield.

Method used

The method employs heteroepitaxy and substrate removal techniques to grow high-crystalline quality III-nitride epitaxial layers on masked GaN templates, allowing for the installation of DBR mirrors on the ELO III-nitride layer after separating it from the host substrate, reducing threading dislocations and enabling curved mirrors to minimize electromagnetic field losses.

Benefits of technology

This approach results in improved crystalline quality, reduced defect density, and increased output power and efficiency of VCSELs by simplifying the manufacturing process and enhancing the device's lifetime.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540892000001_ABST
    Figure 2024540892000001_ABST
Patent Text Reader

Abstract

A method of fabricating a vertical cavity surface emitting laser (VCSEL) using epitaxial lateral overgrowth (ELO). The ELO layer comprises an island-like III-nitride semiconductor layer grown on a substrate using a growth limiting mask, the island-like III-nitride semiconductor layer comprising a light emitting resonant cavity. An opening for the resonant cavity is fabricated on a wing of the ELO layer with a distributed Bragg reflector (DBR) mirror formed on the bottom and top regions of the wings of the ELO layer. In one embodiment, the interface of the ELO III-nitride layer has a patterned surface for the DBR mirror.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims the benefit under 35 USC Section 119(e) of the following co-pending and commonly assigned application, which is incorporated herein by reference: U.S. Provisional Application Docket No. 63 / 270,618, entitled “VERTICAL CAVITY SURFACE EMITTING LASER FABRICATION METHOD,” filed on October 22, 2021 by Srinivas Gandrothula, Shuji Nakamura, and Steven P. DenBaars (Attorney Docket No. G&C30794.0810USP1 (UC2022-768-1)).

[0002] This application is related to the following co-pending and commonly assigned applications: U.S. Utility Patent Application No. 17 / 766,960, filed April 6, 2022 by Srinivas Gandrothula, Takeshi Kamikawa, and Masahiro Araki and entitled “METHOD OF FABRICATING A RESONANT CAVITY AND DISTRIBUTED BRAGG REFLECTOR MIRRORS FOR A VERTICAL CAVITY SURFACE EMITTING LASER ON A WING OF AN EPITAXIAL LATERAL OVERGROWTH REGION” (Attorney Docket No. 30794.06745USWO (UC2020-071-2)), which application was filed October 23, 2020 by Srinivas Gandrothula, Takeshi Kamikawa, and Masahiro Araki under 35 U.S.C. Section 365(c) and entitled “METHOD This application claims the benefit of co-pending and commonly assigned PCT International Patent Application No. PCT / US20 / 57026 (Attorney Docket No. 30794.0745WOU1 (UC2020-071-2)), entitled "A METHOD FOR FABRICATING A RESONANT CAVITY AND DISTRIBUTED BRAGG REFLECTOR MIRRORS FOR A VERTICAL CAVITY SURFACE EMITTING LASER ON A WING OF AN EPITAXIAL LATERAL OVERGROWTH REGION," which application is incorporated by reference in its entirety under 35 U.S.C.This application claims the benefit under 35 U.S.C. Section 119(e) of co-pending and commonly assigned U.S. Provisional Patent Application Serial No. 62 / 924,756, filed October 23, 2019 by Srinivas Gandrothula, Takeshi Kamikawa, and Masahiro Araki, entitled “METHOD OF FABRICATING A RESONANT CAVITY AND DISTRIBUTED BRAGG REFLECTOR MIRRORS FOR A VERTICAL CAVITY SURFACE EMITTING LASER ON A WING OF AN EPITAXIAL LATERAL OVERGROWTH REGION” (Attorney Docket No. G&C30794.0745USP1 (UC2020-071-1)); all of which applications are incorporated herein by reference.

[0003] FIELD OF THEINVENTION The present invention relates to the fabrication of vertical cavity surface emitting lasers (VCSELs) using epitaxial lateral overgrowth (ELO) techniques on foreign substrates. [Background technology]

[0004] Since the first demonstration of (Al,In,Ga)N-based blue VCSELs in 2008, the maximum output power and threshold current density have improved considerably after a decade of technological advances. A key challenge for the realization of mass production of III-nitride VCSELs is the difficulty in fabricating distributed Bragg reflectors (DBRs) for the resonant cavities. The significant tensile strain between AlN and GaN has prevented the intuitive cavity design with two epitaxial DBRs from arsenide-based VCSELs. Thus, many alternative cavity structures and processing techniques have been developed: for example, spatially lattice-matched AlInN / GaN DBRs, nanoporous DBRs, or dual dielectric DBRs via various overgrowth or film transfer processing strategies. VCSELs reported in the literature have drawbacks, either in terms of yield or complex fabrication procedures.

[0005] Thus, there is a need in the art for improved methods for fabricating VCSELs. The present invention satisfies this need. Summary of the Invention [Means for solving the problem]

[0006] The present invention solves the problems mentioned above using heteroepitaxy and substrate removal. A GaN-on-silicon or GaN-on-sapphire template can be used to grow a III-nitride epitaxial layer with reduced threading dislocations by selectively masking and exposing most of the high defects contained by the Ga(Al)N template layer. The resulting high crystal quality layer can be grown on the masked portion. Conventional VCSEL device fabrication can then be employed on the high crystal quality layer. The problematic n-side DBR can be solved by removing the host substrate and utilizing only the layer grown on the masked portion.

[0007] In the case of GaN on silicon, the p-side of the device layer with epitaxial or dielectric DBR can be attached to a submount and then chemical etching can be used to lift off the device layer from the host Si substrate. The interface roughness of the ELO III-nitride layers on the wings of the growth restriction mask, also called ELO mask, can be controlled to the sub-nanometer level so that an external DBR, either epitaxial or dielectric, can be attached to complete the final device. Alternatively, a curved surface can be formed on the lift-off layer to form a curved DBR mirror, minimizing electromagnetic field losses and refocusing the field back into the gain region of the device.

[0008] Similarly, in the case of GaN on sapphire, laser lift-off (LLO) can be used to remove the device layers from the host sapphire substrate. In this particular approach, LLO is used in the open window regions of the wings of the ELO III-nitride layer, so that the subsequent III-nitride device layers grown on the ELO III-nitride layer will not be damaged. Alternatively, the entire device can be exposed to the laser without damaging the device, since the rear portion of the device is protected from the laser irradiation by a growth limiting mask. However, it is preferred to only expose the open window regions to the laser.

[0009] Important aspects of the present invention include the following: The light emission aperture of the device is fabricated on the wing region of the ELO III-nitride layer, and therefore the device aperture is intended to have better crystal quality in terms of defects and stacking faults than a device aperture fabricated directly on the host substrate. At least one of the DBR mirrors of the cavity is located on a wing of the ELO III-nitride layer, and the DBR mirror may be located on a back surface of the ELO III-nitride layer after separating the ELO III-nitride layer from the host substrate. The substrate can be removed by chemical etching in the case of GaN on silicon, by using LLO for GaN on sapphire templates, or by stripping using cryogenic processing. The method is independent of the crystal orientation of the substrate. In the present invention, surface preparation for the DBR mirror for the resonant cavity VCSEL uses only an ELO mask. The invention can be applied to create curved mirrors when long resonant cavities for VCSELs are desired. The present invention includes a method for achieving stress relaxation of the ELO III-nitride layer, which results in a crack-free, long-life element by removing the ELO III-nitride layer from the host substrate followed by placement of one of the DBR mirrors. In the present invention, separate layers of GaN ELO are preferred to avoid cracking and also to provide an easy way to remove the growth limiting mask.

[0010] Some possible designs using this method are illustrated in the following description. The present invention, when combined with the cross-referenced invention relating to removing semiconductor devices from a semiconductor substrate described above, has many advantages over conventional manufacturable device elements.

[0011] Further, to overcome the limitations in the prior art discussed above, as well as other limitations which will become apparent upon reading and understanding of this specification, the present invention discloses a method for fabricating quality apertures for devices that emit light perpendicular to the substrate on which the device is epitaxially fabricated, such as VCSELs.

[0012] Specifically, the present invention implements the following steps: an island-like III-nitride semiconductor layer is grown on a substrate using a growth-limiting mask and an ELO method, where the growth-limiting mask occupies at least 50% or more of a single element; an ELO region is meant to be a wing of an ELO III-nitride layer with reduced dislocation density compared to the area not covered by the wing of the ELO III-nitride layer; the current-limiting aperture of the VCSEL is limited to the ELO region, and thus good crystal quality is guaranteed; the resonant cavity and DBR mirror of the VCSEL element are fabricated on the ELO region and on the top and bottom of the ELO region, respectively.

[0013] The interface between the growth-limiting mask surface and the ELO region is sufficiently smooth to fabricate one of the light-reflecting DBR mirrors. The ELO III-nitride layer and the subsequent III-nitride device layer grown on the ELO III-nitride layer together comprise an island-like III-nitride semiconductor layer that is removed from the substrate, and a DBR mirror is placed on the back side of the ELO III-nitride layer, which is the interface between the growth-limiting mask and the ELO III-nitride layer, and the substrate removal in this particular application is simple since a foreign substrate such as (Al)GaN on silicon or (Al)GaN on sapphire is used.

[0014] ELO methods for forming island-like III-nitride semiconductor layers may include growth by metalorganic chemical vapor deposition (MOCVD), hydride vapor phase epitaxy (HVPE), etc., to precisely control the thickness and therefore the cavity length of the VCSEL device. The III-nitride semiconductor layers are sized to produce one or more of the island-like III-nitride semiconductor layers. Alternatively, the ELO III-nitride layers can be initially fabricated to coalesce, whereby they can be later separated into individual devices.

[0015] Every element fabricated on the ELO wing can be handled separately or together with other elements by designing an appropriate fabrication process. For example, a common cathode or anode for a pair of elements can be fabricated around an open window area in the ELO III-nitride layer. Such a process simplifies monolithic integration or handling of individual elements. As a result, high yields can be obtained. Alternatively, one of the wings can be used for placement of the openings and placement of the electrical pads.

[0016] Furthermore, the present invention can use heterosubstrates to grow island-like III-nitride semiconductor layers forming rods. For example, GaN templates grown on heterosubstrates such as sapphire, Si, SiC, SiN, GaAs, Ga2O3, LiAlO2, etc. can be used in the present invention.

[0017] Furthermore, the ELO method can significantly reduce the dislocation and stacking fault densities when non-Basel GaN crystal planes are used, which is a key issue when using heterosubstrates.

[0018] Thus, the present invention can simultaneously solve many types of problems associated with the use of heterosubstrates: for example, in a laser device, the interface between the growth-limiting mask and the ELO III-nitride layer can be used as a facet for the cavity. [Brief description of the drawings]

[0019] Reference is now made to the drawings in which like reference numbers represent corresponding parts throughout.

[0020] [Figure 1-1] 1(a), 1(b), 1(c), and 1(d) are schematic diagrams, where FIG. 1(a) shows a foreign substrate with a III-nitride template, FIG. 1(b) shows the template designed in the form of a stripe, FIG. 1(c) shows a schematic of a stripe design accommodating one VCSEL on each side of the stripe, and FIG. 1(d) shows a schematic of a continuous stripe with two or more VCSELs on each ELO wing. [Figure 1-2] 1(a), 1(b), 1(c), and 1(d) are schematic diagrams, where FIG. 1(a) shows a foreign substrate with a III-nitride template, FIG. 1(b) shows the template designed in the form of a stripe, FIG. 1(c) shows a schematic of a stripe design accommodating one VCSEL on each side of the stripe, and FIG. 1(d) shows a schematic of a continuous stripe with two or more VCSELs on each ELO wing.

[0021] [Figure 2-1] FIGS. 2(a), 2(b), 2(c), and 2(d) are schematic diagrams similar to FIGS. 1(a), 1(b), 1(c), and 1(d), but a growth-limiting mask has been deposited and windows have been opened in the III-nitride stripes to allow ELO growth. [Figure 2-2] FIGS. 2(a), 2(b), 2(c), and 2(d) are schematic diagrams similar to FIGS. 1(a), 1(b), 1(c), and 1(d), but a growth-limiting mask has been deposited and windows have been opened in the III-nitride stripes to allow ELO growth.

[0022] [Figure 3-1] 3(a), 3(b), 3(c), and 3(d) are schematic diagrams of the structure after the base ELO layer has been grown. [Figure 3-2] 3(a), 3(b), 3(c), and 3(d) are schematic diagrams of the structure after the base ELO layer has been grown.

[0023] [Figure 4A] FIG. 4(a) is a schematic diagram of the engineered base design, engineered ion implantation (current blocking), regrowth of the tunnel junction and current spreading layers, and the planar DBR mirror.

[0024] [Figure 4B] FIG. 4(b) is a schematic diagram of a side-injection VCSEL design with the top contact prepared for bonding.

[0025] [Figure 5A] 5(a) and 5(b) are schematic diagrams of the removal method using laser irradiation aimed at the open window areas after the VCSEL device is mounted on a carrier, and the resulting damage is only visible in the open window areas. [Figure 5B] 5(a) and 5(b) are schematic diagrams of the removal method using laser irradiation aimed at the open window areas after the VCSEL device is mounted on a carrier, and the resulting damage is only visible in the open window areas.

[0026] [Figure 5C] 5(c) and 5(d) are schematic diagrams of the removal method after mounting the VCSEL device on the carrier using SU-8 and thermal release layer, where chemical lift-off is performed to etch the foreign substrate. [Figure 5D] 5(c) and 5(d) are schematic diagrams of the removal method after mounting the VCSEL device on the carrier using SU-8 and thermal release layer, where chemical lift-off is performed to etch the foreign substrate.

[0027] [Figure 5E] 5(e) and 5(f) are schematic diagrams of the resulting ELO interfacial layer after removing the substrate. [Figure 5F] 5(e) and 5(f) are schematic diagrams of the resulting ELO interfacial layer after removing the substrate.

[0028] [Figure 5G] 5(g) and 5(h) are schematic diagrams of the final VCSEL device after fabricating the curved mirror DBR on the removed ELO interface. [Figure 5H] 5(g) and 5(h) are schematic diagrams of the final VCSEL device after fabricating the curved mirror DBR on the removed ELO interface.

[0029] [Figure 5I] 5(i) and 5(j) are schematic diagrams of a short cavity VCSEL fabricated using the present invention, where thinning is performed on the ELO interface while bonding the VCSEL device layers to the carrier. [Figure 5J] 5(i) and 5(j) are schematic diagrams of a short cavity VCSEL fabricated using the present invention, where thinning is performed on the ELO interface while bonding the VCSEL device layers to the carrier.

[0030] [Figure 6A] 6(a) and 6(b) illustrate the process of obtaining a short-cavity VCSEL by polishing the ELO base layer from the top. [Figure 6B] 6(a) and 6(b) illustrate the process of obtaining a short-cavity VCSEL by polishing the ELO base layer from the top.

[0031] [Figure 6C] 6(c) and 6(d) are scanning electron micrograph (SEM) images of an ELO GaN base layer grown on a foreign substrate, which can be used for the fabrication of a VCSEL with a curved DBR mirror or a short-cavity VCSEL. [Figure 6D] 6(c) and 6(d) are scanning electron micrograph (SEM) images of an ELO GaN base layer grown on a foreign substrate, which can be used for the fabrication of a VCSEL with a curved DBR mirror or a short-cavity VCSEL.

[0032] [Figure 6E] 6(e) and 6(f) are schematic diagrams of the continuation of the device from FIGS. 6(a), 6(b), 6(c), and 6(d), where the device layers are grown after polishing and the ELO interface is used for the DBR mirror after removing the substrate. [Figure 6F] 6(e) and 6(f) are schematic diagrams of the continuation of the device from FIGS. 6(a), 6(b), 6(c), and 6(d), where the device layers are grown after polishing and the ELO interface is used for the DBR mirror after removing the substrate.

[0033] [Figure 6G] 6(g) and 6(h) are schematics of a long cavity VCSEL where a p-GaN side curved mirror is fabricated and a flat DBR mirror is fabricated on the ELO interface. [Figure 6H] 6(g) and 6(h) are schematics of a long cavity VCSEL where a p-GaN side curved mirror is fabricated and a flat DBR mirror is fabricated on the ELO interface.

[0034] [Figure 7A] 7(a) and 7(b) are schematic diagrams of process steps for achieving a curved surface ELO base layer, where FIG. 7(a) shows a host substrate having a patterned curved region covered with a growth-limiting mask, and FIG. 7(b) shows the ELO growth of the VCSEL device layers. [Figure 7B] 7(a) and 7(b) are schematic diagrams of process steps for achieving a curved surface ELO base layer, where FIG. 7(a) shows a host substrate having a patterned curved region covered with a growth-limiting mask, and FIG. 7(b) shows the ELO growth of the VCSEL device layers.

[0035] [Figure 7C] 7(c) and 7(d) are schematic diagrams, where FIG. 7(c) shows the long cavity VCSEL with the top side finished before attachment of the submount, and FIG. 7(d) shows the final VCSEL device using the curved surface of the ELO interface. [Figure 7D] 7(c) and 7(d) are schematic diagrams, where FIG. 7(c) shows the long cavity VCSEL with the top side finished before attachment of the submount, and FIG. 7(d) shows the final VCSEL device using the curved surface of the ELO interface.

[0036] [Figure 8] FIG. 8 is a schematic diagram of an example long cavity VCSEL with a vertical current injection configuration using the ELO interface as one of the metal contacts.

[0037] [Figure 9A] 9(a), 9(b), 9(c), 9(d), and 9(e) are graphs and images of the experimental demonstration of obtaining a curved surface on an ELO layer, where FIG. 9(a) is a profile of the resin on the host substrate, FIG. 9(b) is the profile after a growth limiting mask has been deposited, FIG. 9(c) is the prepared host substrate with the curved surface covered within the growth limiting mask and an open window to assist ELO growth, FIG. 9(d) is the removed ELO base layer with the curved features attached, and FIG. 9(e) is a laser microscope image of the successfully transferred curved features on the ELO interface. [Figure 9B]9(a), 9(b), 9(c), 9(d), and 9(e) are graphs and images of the experimental demonstration of obtaining a curved surface on an ELO layer, where FIG. 9(a) is a profile of the resin on the host substrate, FIG. 9(b) is the profile after a growth limiting mask has been deposited, FIG. 9(c) is the prepared host substrate with the curved surface covered within the growth limiting mask and an open window to assist ELO growth, FIG. 9(d) is the removed ELO base layer with the curved features attached, and FIG. 9(e) is a laser microscope image of the successfully transferred curved features on the ELO interface. [Figure 9C] 9(a), 9(b), 9(c), 9(d), and 9(e) are graphs and images of the experimental demonstration of obtaining a curved surface on an ELO layer, where FIG. 9(a) is a profile of the resin on the host substrate, FIG. 9(b) is the profile after a growth limiting mask has been deposited, FIG. 9(c) is the prepared host substrate with the curved surface covered within the growth limiting mask and an open window to assist ELO growth, FIG. 9(d) is the removed ELO base layer with the curved features attached, and FIG. 9(e) is a laser microscope image of the successfully transferred curved features on the ELO interface. [Figure 9D] 9(a), 9(b), 9(c), 9(d), and 9(e) are graphs and images of the experimental demonstration of obtaining a curved surface on an ELO layer, where FIG. 9(a) is a profile of the resin on the host substrate, FIG. 9(b) is the profile after a growth limiting mask has been deposited, FIG. 9(c) is the prepared host substrate with the curved surface covered within the growth limiting mask and an open window to assist ELO growth, FIG. 9(d) is the removed ELO base layer with the curved features attached, and FIG. 9(e) is a laser microscope image of the successfully transferred curved features on the ELO interface. [Figure 9E]9(a), 9(b), 9(c), 9(d), and 9(e) are graphs and images of the experimental demonstration of obtaining a curved surface on an ELO layer, where FIG. 9(a) is a profile of the resin on the host substrate, FIG. 9(b) is the profile after a growth limiting mask has been deposited, FIG. 9(c) is the prepared host substrate with the curved surface covered within the growth limiting mask and an open window to assist ELO growth, FIG. 9(d) is the removed ELO base layer with the curved features attached, and FIG. 9(e) is a laser microscope image of the successfully transferred curved features on the ELO interface.

[0038] [Figure 10] FIG. 10 is a flow chart of the process steps used to realize one of the designs discussed in this invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] In the following description of the preferred embodiment, reference is made to specific embodiments in which the present invention may be practiced. It is to be understood that other embodiments may be utilized and structural changes may be made without departing from the scope of the present invention.

[0040] (overview) The present invention describes a method for fabricating semiconductor devices such as plano-concave VCSELs by appropriately designing growth restriction masks accordingly. Since ELO is relied upon in the present invention, the method is easily applicable to foreign substrates (sapphire, Si, SiC, SiN, GaAs, Ga2O3, LiAlO2, etc.) or host substrates including semiconductor layer templates or ELO engineering layer templates. The ELO engineering layer templates can be used with GaN-on-sapphire substrates and GaN-on-silicon substrates.

[0041] 1(a), 1(b), 1(c), and 1(d) are schematic diagrams illustrating a method, which includes providing a III-nitride based substrate 101 (such as GaN on silicon, GaN on sapphire, or bulk GaN substrate). In the case of a foreign substrate, a III-nitride template 102 can be deposited on the substrate 101, and the design of the template 102 can be a uniform layer overlying the host foreign substrate 101, or the template 102 can be designed only as an opening area stripe 103. In such a case, the area of ​​the host substrate 101 adjacent to the opening area stripe 103 can be used to fabricate a concave shape or any user-designed shape. For example, foreign substrates such as Si and GaAs can be more easily modified using chemical etching compared to III-nitride layers. III-nitride stripes 103 including the host substrate 101, such as stripes 103A and 103B, are shown in the schematic diagrams of FIG. 1(c) and 1(d), respectively. The aperture area stripes 103 can be modified to be limited to a single element by shortening their length, as shown by stripes 103A in FIG. 1(c), or the aperture area stripes 103 can be modified to be limited to multiple elements by increasing their length, as shown by stripes 103B in FIG. 1(d).

[0042] As shown in the schematic diagrams of Figures 2(a), 2(b), 2(c) and 2(d), a growth-limiting mask 104 is formed on or above a GaN-based substrate 101. Specifically, the growth-limiting mask 104 is placed in direct contact with the substrate 101 or indirectly through a template layer 102, made of a III-nitride-based semiconductor grown, such as by MOCVD, and deposited on the substrate 101, while leaving open area stripes 103 (which may comprise shorter stripes 103A or longer stripes 103B).

[0043] The growth limiting mask 104 can be formed from an insulator film (e.g., a SiO2 film) that is deposited on the substrate 101 by, for example, plasma enhanced chemical vapor deposition (CVD), sputtering, ion beam deposition (IBD), etc., and the SiO2 film is then photolithographically patterned to include opening areas 105 using a predetermined photomask and etch.

[0044] As shown in the schematic diagrams of Figures 3(a), 3(b), 3(c), and 3(d), an epitaxial III-nitride layer 301, such as a GaN-based layer, is grown by ELO on a GaN substrate 101 and a growth-limiting mask 104. Growth of the ELO III-nitride layer 301 occurs first on the GaN-based substrate 101 in the opening area 105, and then laterally from the opening area 105 over the growth-limiting mask 104. Growth of the ELO III-nitride layer 301 is stopped or interrupted before the ELO III-nitride layer 301 from an adjacent opening area 105 can coalesce on top of the growth-limiting mask 104. Alternatively, growth of the ELO III-nitride layer 301 can continue and coalesce with a neighboring ELO III-nitride layer 301. The wings 302 of the ELO III-nitride layer 301 are areas of reduced defect density on either side of the aperture area 105. Depending on the composition of the ELO III-nitride layer 301, additional III-nitride device layers 303 are deposited on or above the ELO III-nitride layer 301, which may include active regions, p-type layers, electron blocking layers (EBLs), and cladding layers as well as other layers. Fabrication of the device 304 is then performed, which may include ion implantation layers (current blocking layers) to define the aperture, tunnel junctions including n++ / p++ layers are regrown or a transparent ITO current spreading layer is placed over the device layers 303 before finalizing fabrication of the device 304 with DBR mirrors and p-type and n-type contact deposition.

[0045] 4(a) is a schematic diagram illustrating dual VCSELs 304, each of which is fabricated on a wing 302 of an ELO III-nitride layer 301 using III-device layers 303. Each of the VCSELs 304 includes a UID GaN layer 401, an n-GaN layer 402, an active region 403, and a p-GaN layer 404, where a mesa is etched and then a current blocking layer 405 is deposited, followed by a tunnel junction or transparent conducting layer 406, and a DBR 407.

[0046] The design described here is referred to as base design I and does not involve p- and n-contacts. However, in this particular design, there is the freedom to choose horizontal current injection by placing contact pads on one side of the element 304, or vertical current injection by utilizing part of the interface of the ELO wings 302 or the open window area between the two ELO wings 302 (if the two VCSELs 304 are packaged as a single unit).

[0047] In the present context, base Design I uses LLO or chemical etching to obtain either: a horizontal current injection configuration with a reflowed curved long cavity VCSEL 304 on the n-side (referred to as Design IA); or a vertical current injection configuration with a polished short cavity VCSEL 304 (referred to as Design IB); or a polished and regrown VCSEL 304 (referred to as Design IC); or a VCSEL 304 with a concave shape transferred onto either the ELO mask 104 or the host substrate 101 (referred to as Design ID); or a reflowed curved long cavity VCSEL 304 on the p-side (referred to as Design IE).

[0048] 4(b) is a schematic diagram illustrating a double VCSEL 304, each of which is fabricated on a wing 302 of the ELO III-nitride layer 301 using III-device layers 303. The VCSEL 304 includes a UID GaN layer 401, an n-GaN layer 402, an active region 403, and a p-GaN layer 404, where a mesa is etched and then a current blocking layer 405 is deposited, followed by a tunnel junction or transparent conducting layer 406 and a DBR 407. Finally, an n-contact 408 and a p-contact 409 are deposited.

[0049] (Method of removing foreign substrates) The proposed VCSEL device 304 is fabricated on the wings 302 of the ELO III-nitride layer 301 from a foreign substrate 101 such as GaN on silicon or GaN on sapphire. From the base design I structure, two versions of current injection are proposed, namely horizontal current injection structure and vertical current injection structure, which are described with designs IA, IB, IC, ID, and IE.

[0050] One such design, e.g., removability in case of horizontal implantation, is illustrated in Figures 5(a), 5(b), 5(c), and 5(d). A carrier substrate 501, such as glass, is attached to the prefabricated VCSEL 304, e.g., using solder 502, as shown in Figure 5(a), followed by LLO of the substrate 101, as shown in Figure 5(b). The attachment of the carrier substrate 501 may be performed after planarization, e.g., using photoresist 503, e.g., SU-8, as shown in Figure 5(c). For example, the isolated VCSEL 304 is passivated by a few microns of photoresist 503, and the resulting structure can then be captured by heat release tape 504 on the carrier substrate 501.

[0051] LLO is a proven fast and non-chemical method to remove a thin GaN layer stack from a sapphire substrate and then transfer it onto a carrier substrate. The first LLO-based GaN film separation from a sapphire substrate was demonstrated using a third harmonic Q-switched Nd:YAG laser with a wavelength of 355 nm. A laser pulse with this wavelength was transmitted through the sapphire substrate onto the GaN / sapphire interface and absorbed in the GaN interface region. Photon absorption induced the decomposition of GaN into metallic Ga and gaseous N2.

[0052] Traditionally, LLO can be performed using a variety of short-pulse lasers, including excimer lasers (e.g., 193 nm ArF, 248 nm KrF, and 308 nm XeCl lasers), and Q-switched lasers (e.g., frequency-tripled (355 nm) or frequency-quadrupled (266 nm) nanosecond lasers). In the optoelectronics industry, KrF excimer lasers with an emission wavelength of 248 nm are often applied for LLO procedures using a raster scanning method. This traditional LLO approach requires direct absorption in the semiconductor.

[0053] As shown in Figures 5(a) and 5(c), after fabricating the VCSEL 304 on the ELO wings 302, the carrier substrate 501 is attached and then a laser 505 is focused on the open window region 506 from the back of the host substrate 101 (GaN on sapphire). In the present invention, the irradiation of the laser 505 is selective only at the open window region 506. The laser 505 can be focused very narrowly at the open window region 506, eliminating the need for irradiation over the entire VCSEL 304, and as a result, this method is highly advantageous for lifting off the fabricated VCSEL 304 without significant damage to the device layer of the VCSEL 304. Furthermore, the interface 507 of the ELO wings 302 with the substrate 101 is completely covered with the ELO mask 104 during irradiation, which will protect it from further damage and leave Ga melt only at the interface 507, as shown in Figures 5(b) and 5(d). A similar process would be performed for lift-off of the GaN-on-silicon template 102, except using a chemical similar to KOH instead of LLO.

[0054] When a SiO2 ELO mask 104 is used, the ELO mask 104 is then dissolved using a chemical solution, e.g., BHF. The resulting VCSEL device unit 304 is placed on a carrier substrate 501 with an open interface 507, as shown in Figures 5(e) and 5(f). The interface 507 is further modified for the process of fabricating the resonant cavity DBR mirror and for placing metal contacts for vertical implantation, as described below.

[0055] (VCSEL design IA) In design IA, a resin disk with the desired diameter is photolithographed onto the interface 507 of the ELO wing 302. Alternatively, a printer can be used to place a resist disk when uniform spin coating creates challenges due to the discreteness of the ELO layer 301. By heating the sample, the disk melts into droplets. RIE can be used to transfer the surface shape of the resin droplets onto the interface 507 by removing them as a sacrificial mask, which will leave a lens-shaped surface on the interface 507. An n-side DBR (e.g., Ta2O5 / SiO2 bilayer) is deposited to form a curved mirror 508, as shown in FIG. 5(g).

[0056] FIG. 5(h) shows the completed VCSEL 304, which includes the UID GaN layer 401, the n-GaN layer 402, the active region 403, the p-GaN layer 404, the current blocking layer 405, the tunnel junction or transparent conducting layer 406, the DBR 407, the n-contact 408, and the p-contact 409.

[0057] This design is specifically for long cavity VCSELs 304, typically with resonant cavity lengths greater than 20 μm.

[0058] (VCSEL design IB) Design IB can be used in designing a short cavity VCSEL 304, where the resonant cavity thickness is about a few wavelengths, e.g., xλ=7λ, 13λ, 23λ, etc., where λ is the emission wavelength of the device. The short cavity length can be used to obtain a single longitudinal mode emission due to the large mode spacing. In this design, after removing the host substrate 101, thinning to line 509 can be performed on the interface 507 to obtain the desired cavity length, as shown in FIG. 5(i), and then a second DBR mirror 407 can be placed at the interface 507 to complete the fabrication of the VCSEL 304, as shown in FIG. 5(j).

[0059] (VCSEL design IC) Design IC is an alternative approach to achieve a short cavity VCSEL as in Design IB, but by polishing from the top surface before introducing the active region and p-GaN layer on the ELO base layer 301. After reaching the desired ELO wing 302 width, as shown in FIG. 6(a), the ELO III-nitride layer 301 is polished from the top surface to reach point 601 (the desired pre-calculated value), as shown in FIG. 6(b), and then regrowth is performed to grow III-nitride semiconductor device layer 303 including the active region and p-GaN layer. Then, a process is performed to fabricate the structure of the VCSEL 304, including a current blocking layer, a current spreading layer, a DBR mirror, and one or more metal contacts. Using one of the methods described in substrate removal, the host substrate 101 is removed, and the interface 507 of the ELO wing 302 is used to deposit a second DBR mirror.

[0060] Figure 6(c) is an SEM image showing a GaN-on-sapphire substrate 101 with an ELO III-nitride layer 301. Figure 6(d) is an SEM image showing a GaN-on-silicon substrate 101 with an ELO III-nitride layer 301.

[0061] The resulting VCSEL 304 before lift-off is shown in Figure 6(e) and includes the UID GaN layer 401, the n-GaN layer 402, the active region 403, and the p-GaN layer 404, with the mesa etched and then the current blocking layer 405 deposited, followed by the tunnel junction 406, the DBR 407, and the ion implantation aperture 602. After lift-off, a second DBR mirror 407 is placed at the interface 507 to complete the fabrication of the VCSEL 304, as shown in Figure 6(f).

[0062] (VCSEL design ID) Design ID replicates the long cavity VCSEL of Design IA, however, resist reflow on the interface 507 is not required to achieve the curved mirror 508. Resist reflow is used in the first stage when preparing the ELO mask 104. For example, as shown in FIG. 7(a), a concave shape 701 is transferred onto the host substrate 101 or onto the ELO mask 104 material. The transfer process may involve nanoimprinting or resist disk thermal reflow mechanism. Then, similar to the previous design, the opening area 105 is opened on the GaN-on-silicon or GaN-on-sapphire template 102 to grow the base ELO layer 301, followed by the VCSEL device layers 303 including the UID GaN layer 401, the n-GaN layer 402, the active region 403, and the p-GaN layer 404, as shown in FIG. 7(b).

[0063] Specifically, Figures 7(a) and 7(b) are schematic diagrams illustrating process steps for achieving a curved surface feature 701 in the ELO base layer 301, where Figure 7(a) shows the host substrate 101 having a patterned curved region 701 covered with a growth limiting mask 104, and Figure 7(b) shows the ELO III-nitride layer 301 and the device layers 401, 402, 403, 404 of the VCSEL 304. Front-end processing is then performed to fabricate the current blocking layer, current spreading layer, DBR mirror, metal contacts, etc., as shown in Figure 7(c). The host substrate 101 is then removed using either LLO in the case of GaN-on-sapphire or chemical etching in the case of GaN-on-silicon, as shown in FIG. 7( d ), and after lift-off, a second DBR mirror 407 is placed at the interface 507 to complete the fabrication of the VCSEL 304, which includes the UID GaN layer 401, the n-GaN layer 402, the active region 403, the p-GaN layer 404, the tunnel junction 406, the DBR 407, the n-contact 408, and the ion implantation aperture 602.

[0064] (VCSEL design IE) Design IE replicates the long cavity VCSEL design IA, however, no resist reflow on interface 507 was required to achieve curved mirror 508. The resist reflow process is performed on the p-side of element 304.

[0065] As shown in Fig. 6(g), a long cavity VCSEL 304 is fabricated on the ELO wings 302 of the heterosubstrate 101, including the UID GaN layer 401, the n-GaN layer 402, the active region 403, the p-GaN layer 404, the tunnel junction 406, the n-contact 408, the ion implantation aperture 602, and the first curved mirror 508 on the p-side of the VCSEL 304. As shown in Fig. 6(h), the device 304 is lifted off using the carrier substrate 501. The ELO wing interface 507, together with the n-contact 408, is then used for the second flat DBR mirror 407 on the n-side of the VCSEL 304. In this embodiment, the ELO III-nitride layer 301 may be polished after the substrate 101 is removed and before the second flat DBR mirror 407 is placed on the ELO wing interface 507 as described in the design IC.

[0066] 8 is a schematic diagram of an exemplary long cavity VCSEL 304 with a vertical current injection configuration using a metal 801 deposited on the ELO interface 507, which bonds the VCSEL 304 to another carrier 802 as an n-contact. The long cavity VCSEL 304 otherwise includes a UID GaN layer 401, an n-GaN layer 402, an active region 403, a p-GaN layer 404, a tunnel junction 406, a DBR 407, an n-contact 408, and an ion implantation aperture 602.

[0067] (Production steps) Exemplary fabrication steps for the present invention are described in further detail below. Step 1: Start with forming the growth limiting mask 104, which can be accomplished by: Placing the growth limiting mask 104 on the host substrate 101. The growth limiting mask 104 can be patterned using nanoimprint lithography, or the desired shape can be transferred onto the growth limiting mask 104 using photolithography+wet etching or photolithography+dry etching. Alternatively, a planar mask 104 can be used. Step 2: A plurality of stripe-shaped opening areas 105 are opened on the substrate 101, the substrate 101 being a group III nitride semiconductor, or the substrate being a hetero-substrate 101 such as sapphire, Si, SiC, SiN, GaAs, Ga2O3, LiAlO2, or the substrate 101 including a template 102. Step 3: Multiple ELO III-nitride layers 301 are grown on the substrate 101 using the growth-limiting mask 104, the growth extends in a direction parallel to the stripe-shaped opening areas 105 of the growth-limiting mask 104, the ELO III-nitride layers 301 take the shape designed on the growth-limiting mask 104, and the designed pattern is transferred onto the interface 507, which is the surface between the ELO III-nitride layers 301 and the growth-limiting mask 104. For a planar mask 104, the interface 507 is a planar surface. Step 4: Fabricate VCSELs 304 on the wings 302 (most likely on the flat surface areas) of the ELO III-nitride layer 301 by conventional methods. Step 5: The element 304 units are divided, and the element 304 units on the host substrate 101 are isolated. Step 6: Attach the submount or carrier 501. Step 7: Irradiate or chemically etch to lift off the host substrate 101. Step 8: Separate the device 304 unit from the host substrate 101. Step 9: Dissolve the growth limiting mask 104 using a chemical etch such as buffered hydrofluoric acid (BHF) or hydrofluoric acid (HF). Step 10: Place the second DBR 407 on the ELO wing interface 507, or use resist reflow to prepare the curved mirror surface 701 and place the second DBR 407.

[0068] (Forming a growth restriction mask) In one embodiment, the GaN-based layer 301 is grown by ELO on a growth-limiting mask 104 comprising SiO2, and the GaN-based layer 301 may or may not coalesce on top of the growth-limiting mask 104.

[0069] The growth limiting mask 104 consists of open area stripes 103, with the stripes 103 between the open areas 105 having a width of 1 μm to 20 μm and a spacing of 10 μm to 100 μm. If a non-polar substrate 101 is used, the open areas 105 are <0001> The aperture areas 105 are oriented along the [-1014] or

[1014] axis, respectively, when a semi-polar (20-21) or (20-2-1) substrate 101 is used. Other faces of the substrate 101 with the aperture areas 105 oriented in other directions may be used as well.

[0070] The present invention can obtain high quality III-nitride semiconductor layers 301 using the growth limiting mask 104. As a result, the present invention can also easily obtain devices with reduced defect densities such as dislocations and stacking faults. These techniques can be used with hetero-substrates 101 such as sapphire, Si, SiC, SiN, GaAs, Ga2O3, LiAlO2, etc., as long as the substrate 101 allows the growth of ELO GaN-based layers 301 through the growth limiting mask 104.

[0071] (Pattern growth restriction mask) Before generating the opening area 105 on the growth-limiting mask 104, pre-processing is performed on the growth-limiting mask 104. This application focuses on preparing VCSELs. The opening area stripes 103 can be of limited length 103A, such as those shown in Figures 2(a), 2(b), 2(c), and 2(d), to accommodate a VCSEL on each wing, or can be stripes 103 of long length 103B to accommodate several VCSEL elements on each wing 302. In some cases, for example, in the design ID, a concave shape is transferred onto the ELO mask 104 or the host substrate 101, and then the opening area 105 for ELO growth is transferred. The opening area 105 is selected such that the growth parameters optimize the larger ratio of the wing 302 to the thickness of the layer 301.

[0072] (Multiple epitaxial layers are grown on a substrate using growth-limiting masks) The group III-nitride device layer 303 is grown by conventional methods on the ELO GaN-based layer 301. In one embodiment, MOCVD is used for epitaxial growth of the island-like group III-nitride semiconductor layer, including both the ELO GaN-based layer 301 and the group III-nitride device layer 303. The island-like group III-nitride semiconductor layers 301, 303 are isolated from each other because the MOCVD growth is stopped before the ELO GaN-based layer 301 coalesces.

[0073] Trimethylgallium (TMGa), trimethylindium (TMIn), and triethylaluminum (TMAl) are used as III-element sources. Ammonia (NH3) is used as the raw gas to provide nitrogen. Hydrogen (H2) and nitrogen (N2) are used as carrier gases for the III-element sources. Including hydrogen in the carrier gas is important to obtain a smooth surface epilayer.

[0074] Salts and bis(cyclopentadienyl)magnesium (Cp2Mg) are used as n-type and p-type dopants. Pressure settings are typically 50-760 Torr. III-nitride semiconductor layers are generally grown at temperatures ranging from 700-1,250°C.

[0075] For example, the growth parameters include: TMG is 12 sccm, NH3 is 8 slm, carrier gas is 3 slm, SiH4 is 1.0 sccm, and the V / III ratio is about 7,700.

[0076] (ELO of Limited Area Epitaxy (LAE) III-Nitride Layers) In the prior art, some pyramidal hillocks have been observed on the surface of m-plane III-nitride films following growth (see, for example, US Patent Application Publication No. 2017 / 0092810). In addition, wavy surfaces and recessed areas appear on the growth surface, which aggravate the surface roughness. This is a very serious problem. For example, according to some papers, a smooth surface can be obtained by controlling the off-angle (>1 degree) of the growth surface of the substrate and using N2 carrier gas conditions. However, these are very limited conditions for mass production due to high production costs. Furthermore, GaN substrates have a large variation of off-angle with respect to the origin from their fabrication method. For example, if the substrate has a large in-plane distribution of off-angle, the substrate will have different surface morphology at these points in the wafer. In this case, the yield is reduced by the large in-plane distribution of off-angle. Therefore, it is necessary that the technique does not depend on the off-angle in-plane distribution.

[0077] The present invention solves these problems as described below: 1. The growth area is limited by the area of ​​the growth limiting mask 104 from the edge of the substrate 101. 2. The substrate 101 is a non-polar or semi-polar III-nitride substrate 101 with an off-angle orientation ranging from -16 degrees to +30 degrees from the m-plane towards the c-plane and C-plane. Alternatively, a heterosubstrate 101 with a deposited III-nitride based semiconductor layer 102 can be used, where the layer 102 has an off-angle orientation ranging from +16 degrees to -30 degrees from the m-plane towards the c-plane. 3. The island-shaped III-nitride semiconductor layers 301 and 303 have long sides perpendicular to the a-axis of the III-nitride semiconductor crystal. 4. During MOCVD growth, a hydrogen atmosphere can be used.

[0078] In the present invention, a hydrogen atmosphere can be used during non-polar and semi-polar growth.

[0079] In one embodiment, the growth pressure ranges from 60 to 760 Torr, but preferably the growth pressure ranges from 100 to 300 Torr to obtain a wide width for the island-like III-nitride semiconductor layers 301, 303, the growth temperature ranges from 900 to 1,200°C, the V / III ratio ranges from 10 to 30,000, the TMG is 2 to 20 sccm, the NH3 ranges from 0.1 to 10 slm, and the carrier gas is hydrogen gas only or both hydrogen and nitrogen gas. To obtain a smooth surface, the growth conditions of each side need to be optimized by conventional methods.

[0080] After growth for about 2-8 hours, the ELO GaN-based layer 301 will have a thickness of about 1-50 μm and a bar width of about 50-150 μm.

[0081] (Making elements) The elements 304 are fabricated on the flat surface regions of the ELO wings 302 by conventional methods, and various element 304 designs are possible. For example, regrowth of the VCSEL, current blocking regions, and tunnel junctions, placement of a transparent conducting layer such as ITO, and metal contacts and DBR mirrors may be required. These can be fabricated on the p-side of the VCSEL 304 before removing the host substrate 101.

[0082] (Forming a structure for separating element units) The purpose of this step is to isolate the device 304 units from the host substrate 101 using the ELO III-nitride device layer 301. At least two methods can be used to transfer the device 304 units onto the carrier substrate 501.

[0083] In one method, using a selective etch mask, the III-nitride device layer 303 is separated on the host substrate 101 by etching to expose at least the growth limiting mask 104 .

[0084] Alternatively, marking can be performed with a diamond-tipped or laser scriber, or other methods such as RIE (reactive ion etching) or ICP (inductively coupled plasma) etching can be used to isolate the element 304 units.

[0085] The isolated VCSEL element 304 units are then filled with a photoresist 503 such as SU-8 and attached to a carrier substrate 501 via a heat release film 504, or simply bonded to the carrier wafer 501 using solder 502, and then a removal step is performed.

[0086] (Curved surface structure formed on ELO mask) For device 304 described in Design ID, growth-limiting mask 104 or host substrate 101 must be pre-fabricated to create curved features 701 for transfer onto interface 507 of ELO layer 301 .

[0087] To transfer the concave shaped pattern 701 onto the interface 507 of the ELO layer 301, the mask 104 must contain the same pattern. A very promising patterning technique is the nanoimprint technique. First a stamp with the inverse pattern, the so-called master, is fabricated. By pressure or capillary forces the pattern is printed into a resist which is deposited onto the host substrate 101 or mask 104 material. After heating and / or UV curing the stamp is removed and the resist can serve as an etching mask. This patterning process can be done on a wafer scale, thus resulting in a high throughput. The master pattern has to be fabricated first by conventional photolithography techniques.

[0088] As a demonstration, due to the unavailability of the required nanoimprinting technology, the inventors have fabricated convex features on the growth limiting mask 104 using a resist reflow method, as shown in Figures 9(a), 9(b), 9(c), 9(d), and 9(e), and successfully transferred the same features onto the interface 507 of the ELO layer 301.

[0089] The graph in FIG. 9(a) is the shape of the resist pattern after reflow has been applied, the image in FIG. 9(b) is the convex shape after deposition of mask 104, and the image in FIG. 9(c) combines the convex pattern from mask 104 with open window areas 506 for ELO growth. Using MOCVD, an n-GaN ELO base layer 301 was grown from the open window areas 506, and layer 301 was removed using a method described in [Applied Physics Express 13,041003 (2020)]. The interface 507 of the ELO layer 301 after removal is shown in the image in FIG. 9(d), and laser scanning was performed to show the transferred structure in the image in FIG. 9(e).

[0090] (Definition of terms) III-nitride substrates The III-nitride substrate 101 may comprise any type of III-nitride substrate, so long as the III-nitride substrate 101 allows for the growth of the III-nitride semiconductor layers 301, 303 through the growth limiting mask 104: any GaN substrate 101 sliced ​​from bulk GaN on the {0001}, {11-22}, {1-100}, {20-21}, {20-2-1}, {10-11}, {10-1-1} plane, etc., or other planes; and AlN crystalline substrates.

[0091] Foreign or heterogeneous substrates The present invention is primarily used with foreign or heterogeneous substrates 101. For example, a GaN template 102 or other III-nitride based semiconductor layer 102 can be grown on a heterogeneous substrate 101, such as sapphire, Si, SiC, SiN, GaAs, Ga2O3, LiAlO2, etc., followed by a growth limiting mask 104. The GaN template 102 or other III-nitride based semiconductor layer 102 is typically grown on the heterogeneous substrate 101 to a thickness of about 2-6 μm, and then a growth limiting mask 104 is placed on the GaN template 102 or other III-nitride based semiconductor layer 102.

[0092] Growth restriction mask The growth limiting mask 104 comprises a dielectric layer such as SiO2, SiN, SiON, Al2O3, AlN, AlON, MgF, ZrO2, TiN, or a refractory or noble metal such as W, Mo, Ta, Nb, Rh, Ir, Ru, Os, Pt, etc. The growth limiting mask 104 can be a laminated structure selected from the above materials. It can also be a multi-stacking layer structure selected from the above materials.

[0093] In one embodiment, the thickness of the growth limiting mask 104 is about 0.05-3 μm. The width of the mask 104 is preferably greater than 20 μm, and more preferably the width is greater than 40 μm. The growth limiting mask 104 is deposited by, but not limited to, sputtering, e-beam evaporation, plasma enhanced chemical vapor deposition (PECVD), ion beam deposition (IBD), and the like.

[0094] On the m-plane freestanding GaN substrate 101, the growth limiting mask 104 includes a plurality of opening areas 105, which are arranged in a first direction parallel to the 11-20 direction of the substrate 101 and a second direction parallel to the 0001 direction of the substrate 101, and the plurality of opening areas 105 are arranged periodically at intervals extending in the second direction. The length of the opening areas 105 is, for example, 100 to 35,000 μm, the width is, for example, 2 to 180 μm, and the interval between the opening areas 105 is, for example, 20 to 180 μm. The width of the opening areas 105 is typically constant in the second direction, but may be varied in the second direction as necessary.

[0095] On the c-plane freestanding GaN substrate 101 , the open areas 105 are disposed in a first direction parallel to the 11-20 direction of the substrate 101 and in a second direction parallel to the 1-100 direction of the substrate 101 .

[0096] On a semi-polar (20-21) or (20-2-1) GaN substrate 101, the open areas 105 are oriented parallel to [-1014] and [10-14], respectively.

[0097] Alternatively, a hetero substrate 101 can be used. When the c-plane GaN template 102 is grown on the c-plane sapphire substrate 101, the opening area 105 is in the same direction as the c-plane freestanding GaN substrate 101, and when the m-plane GaN template 102 is grown on the m-plane sapphire substrate 101, the opening area 105 is in the same direction as the m-plane freestanding GaN substrate 101. By doing so, the m-plane cleavage plane can be used to split the rod of the device with the c-plane GaN template, and the c-plane cleavage plane can be used to split the rod of the device with the m-plane GaN template 102, which is very preferable.

[0098] Group III nitride semiconductor layer The ELO III-nitride layer 301 and the III-device layer 303 may contain In, Al, and / or B as well as other impurities such as Mg, Si, Zn, O, C, H, and the like.

[0099] The III-nitride semiconductor device layer 303 generally comprises three or more layers, including at least one of an n-type layer, an undoped layer, and a p-type layer. Specifically, the III-nitride semiconductor device layer 303 comprises one or more of a GaN layer, an AlGaN layer, an AlGaInN layer, an InGaN layer, etc. When the device 304 has a plurality of III-nitride semiconductor layers 303, the distance between the adjacent island-like III-nitride semiconductor layers 301, 303 is generally 30 μm or less, preferably 10 μm or less, but is not limited to these figures. In the semiconductor device 304, several electrodes are arranged at predetermined positions according to the type of the semiconductor device 304.

[0100] Semiconductor Device The semiconductor element 304 may be, for example, a Schottky diode, a light emitting diode, a semiconductor laser, a photodiode, a transistor, etc., but is not limited to these elements 304. The present invention is particularly useful for a VCSEL 304. The present invention is particularly useful for a semiconductor laser 304 that requires a smooth region for cavity formation.

[0101] Alternative Embodiments The present invention and the following embodiments disclose a III-nitride VCSEL 304 that incorporates a curved mirror 508 on either the n-side or p-side of the element 304. The use of a curved mirror 508 allows for the following: 1. Use of a long cavity without suffering from excessive diffraction losses. When using two plane mirrors defining a cavity, losses due to diffraction increase with cavity length [Applied Physics Express 12, 044004 (2009), Sci. Rep., 8, 10350 (2018)]. When using a curved mirror 508, the reflected light can be concentrated back into the aperture minimizing diffraction losses. 2. Better thermal management, increased lifetime, output power, efficiency and reliability of the device 304. Highly efficient VCSEL 304 operation requires that the gain spectrum be well aligned to the cavity modes. As the cavity length increases, the mode spacing decreases. Therefore, there is a number of efficient cavity modes to ensure good mode overlap with the gain spectrum. In addition, tighter cavity mode spacing allows for better tolerances in cavity length and active region location. Having a long cavity design can increase yields during growth and fabrication of the device 304. 3. It has been experimentally shown that there are many advantages of III-nitride long cavity VCSELs where curved mirrors are employed behind the substrate [Applied Physics Express 12,044004 (2009)]. However, the design described herein removes the substrate 101 using conventional methods; the design also uses high crystal quality ELO wings 302 for the resonant cavity, which increases the lifetime of the device 304. The present invention avoids surface preparation in some designs, which in fact omits processing steps and is not affected by the crystallinity of the substrate 101, even for one-time use bulk GaN substrates 101. The present invention focuses on large-scale manufacturing by using GaN templates 102 on foreign substrates 101.

[0102] In the present invention, the advantage of forming the curved mirror 508 on the top or bottom eliminates the need to thin the substrate 101. For a visible wavelength VCSEL 304, the long cavity length should be 8-30 μm considering the number of cavity modes and spacing. It is difficult to thin the substrate 101 to precisely control the thickness. In the present invention, using ELO provides an advantage in achieving good wing 302 width and thickness, which has the advantage in increasing the cavity thickness without adding threading dislocations.

[0103] Not having to thin the substrate 101 also reduces process complexity and cost. Thinned substrates are susceptible to breakage during handling processes, however, the carrier substrate 501 of the present invention avoids such problems.

[0104] (First embodiment) In a first embodiment, a long cavity VCSEL 304 is fabricated on the ELO wings 302 of a heterosubstrate 101 , the device 304 is lifted off, and then a curved DBR mirror 407 is fabricated at the interface 507 .

[0105] A substrate 101 with a III-nitride template 102 is provided, and a growth restriction mask 104 or ELO mask 104 is placed on the host substrate 101. The III-nitride layers can be stripes as illustrated in Figures 1(a), 1(b), 1(c), and 1(d), and 2(a), 2(b), 2(c), and 2(d). Then, an n-GaN ELO layer 301 is grown from the opening area 105. Wings 302 of the ELO layer 301 with appropriate width for a long cavity VCSEL are achieved, and device layers 303, such as InGaN, p-GaN layers, including the active region, are grown.

[0106] The device layer 303 is then activated so that the ELO layer 301 is not allowed to coalesce with the neighboring ELO layer 301. The activation of the p-GaN layer 404 is better in these devices 304 because the sidewalls in the non-coalesced regions provide a better path for hydrogen diffusion. A hard mask, e.g. Ti / Au, was then deposited to protect the open areas during ion implantation to create the current blocking regions 405. After implantation, the hard mask was removed using heated aqua regia and the sample was directly cleaned prior to the regrowth of the tunnel junction 406. Alternatively, ITO could also be chosen as the current spreading layer 406. A highly doped n++ GaN tunneling layer, followed by the n-GaN current spreading layer 406 and the n++ GaN contact layer 402, was grown by MOCVD. Afterwards, the p-GaN 404 was reactivated again through the sidewalls.

[0107] SiO of p-DBR mirror 407 2 / Alternating pairs of Ta2O5 layers were deposited and the p-contact metal 409 around the DBR mirror 407 was lithographically defined. A transparent carrier substrate 501 is bonded to the p-side of the element 304. Laser or chemical lift-off is then used to remove the host substrate 101.

[0108] The ELO mask 104 on the interface 507 is dissolved in chemical etching, and a resin disk with a desired diameter is photolithographed on the interface 507 of the ELO wing 302. By heating the sample, the disk is melted into a droplet. RIE can be used to transfer the surface shape of the resin droplet onto the ELO interface 507 by removing them as a sacrificial mask, which will leave a lens-shaped surface on the ELO interface 507. An n-side DBR 407, e.g., Ta2O5 / SiO2 bilayer, was deposited to form a curved mirror 508, as shown in Figures 5(g) and 5(h). This design is specifically dedicated to long-cavity VCSELs 304, where the resonant cavity length is greater than 20 μm. An n-metal pad 408 was then defined on the ELO interface 507 for vertical current injection. Alternatively, a top-side metal contact 408 can also be used for lateral injection.

[0109] An exemplary process includes the following steps: 1. Grow an ELO III-nitride layer 301 on the GaN template 102 of a heterosubstrate 101, typically greater than 20 μm. The ELO III-nitride layer 301 comprises a UID GaN layer 401. 2. Growing the following device layers 303 on the ELO III-nitride layer 301, in order: an n-GaN layer 402 (1,000 nm thick) for cladding and n-contact; InGaN multiple quantum wells and GaN barriers as the active region 403; an AlGaN electron blocking layer 405 (50 nm); p-GaN (300 nm thick); and a p++GaN (10 nm thick) layer 404. 3. Performing ion implantation and defining openings. 4. After surface cleaning, re-grow an n++ GaN layer (10 nm thick) to complete the tunnel junction 406. 5. Depositing an n-GaN layer 402 (10-100 nm thick) for damping and current spreading. 6. Dry etch the mesas to define elements 304. 7. Depositing the dielectric DBR mirror 407. 8. Depositing contacts 408, 409 and flip-chip bonding / attaching to transparent carrier 501. 9. Removing the substrate 101 through LLO or chemical etching. 10. Dissolving ELO mask 104 on ELO wing interface 507. 11. Etching curved mirror features 508 with curved surfaces 701 in the UID-GaN 301 using RIE using thermal reflow of resin. 12. Depositing dielectric DBR mirror 407 over curved surface 701. 13. Dry etch selective portions of interface 507 to expose the n-GaN layer 402 outside the curved mirror 508 and deposit metal contacts 408, 409 (for vertical implantation). 14. The resulting structure of element 304 is shown in Figures 5(g) and 5(h) (side implant case), by following these steps, a vertical implant design can be obtained.

[0110] Key advantages include: Foreign substrates 101 can be used, so scaling would not be an issue. The high crystalline quality device layer 303 on the ELO III-nitride layer 301 results in less leakage, longer lifetime, and higher output power. The DBR mirror 407 is a curved mirror 508 whose curved surface 701 is the interface 507 of the ELO wing 302 on the growth constraining mask 104, and no special preparation is required to make the surface smooth. Laser or chemical lift-off will not damage the VCSEL 304. The ELO wing interface 507 is covered with the ELO mask 104 during the removal process. Alternatively, the invention can be practiced by first partially or totally removing the growth limiting mask 104 before growth of the device layer 303 to avoid any compensation effect, in which case exposing the open window areas 506 to the laser 505 from the host substrate 101 will not cause any damage to the device 304.

[0111] Second embodiment The second embodiment is also a long-cavity VCSEL 304 fabricated on the ELO wings 302 of a heterosubstrate 101, and the device 304 is lifted off from the interface 507 after removal of the substrate 101. The only difference is that a curved mirror 508 is pre-fabricated either on the host substrate 101 or on the ELO mask 104. The ELO III-nitride layer 301 from the opening area 105 has the shape of the curved mirror 508, which eliminates the additional resin reflow fabrication step and simplifies the process.

[0112] A host substrate 101 with a III-nitride template 102 is provided, and a growth-limiting mask 104 or ELO mask 104 is placed on the pre-fabricated curved surface 701 of the host substrate 101. The ELO III-nitride layer 301 can be stripes as illustrated in Figures 1(a), 1(b), 1(c), and 1(d), and Figures 2(a), 2(b), 2(c), and 2(d). A base n-GaN ELO layer 301 is grown from the opening area 105. ELO wings 302 with appropriate width for a long-cavity VCSEL 304 are achieved, and then device layers 303, such as n-GaN layer 402, InGaN including active region 403, and p-GaN layer 404, are grown.

[0113] The device layer 303 is then activated. The activation of the p-GaN layer 404 is completed since the ELO III-nitride layer 301 does not coalesce with the neighboring ELO III-nitride layer 301 and therefore the sidewalls in the non-coalesced regions provide a better path for hydrogen diffusion. A hard mask, e.g. Ti / Au, is then deposited to protect the open areas during ion implantation for the current blocking region 405. After implantation, the hard mask is removed using heated aqua regia and the sample is directly cleaned prior to the regrowth of the tunnel junction 406. Alternatively, ITO can also be chosen as the current spreading layer 406. The tunnel junction 406 consisting of a highly doped n++ GaN tunneling layer, followed by the n-GaN current spreading layer 402 and the n++ GaN contact layer 402 are grown by MOCVD. The p-GaN layer 404 is then reactivated again through the sidewalls.

[0114] SiO 2 / A p-side DBR mirror 407 consisting of alternating pairs of Ta2O5 bilayers is deposited and p-contact metal 409 around the periphery of the DBR mirror 407 is defined by lithography. A transparent carrier substrate 501 is bonded to the p-side of the element 304. Laser or chemical lift-off is then used to remove the host substrate 101.

[0115] The ELO mask 104 on the ELO wing interface 507 is dissolved in a chemical etch, and then an n-side DBR 407 consisting of Ta2O5 / SiO2 bilayer is deposited on the curved shape 701 of the ELO interface 507, as shown in Figures 7(c) and 7(d). Specifically, Figure 7(c) shows the top-side finished long cavity VCSEL 304 before attachment of the submount 501, and Figure 7(d) shows the final VCSEL device 304 using the curved surface 701 of the ELO interface 507. This design is specifically dedicated to the long cavity VCSEL 304, where the resonant cavity length is greater than 20 μm. An n-metal pad 408 is then defined on the ELO interface 507 for vertical current injection. Alternatively, a top-side metal contact 408 can also be used for lateral injection.

[0116] An exemplary process includes the following steps. 1. Preparing a curved surface 701 on the host substrate 101 or ELO mask 104. 2. Grow a base ELO III-nitride layer 301 on the GaN template 102 on the heterosubstrate 101, typically greater than 20 μm. The ELO III-nitride layer 301 takes the shape of the curved surface 701. In this case, the ELO III-nitride layer 301 is a UID GaN layer 401. 3. Growing the following device layers 303 on the base ELO III-nitride layer 301, in order: an n-GaN layer 402 (1,000 nm thick) for cladding and n-contact; InGaN multiple quantum wells and GaN barriers as the active region 403; an AlGaN electron blocking layer 405 (50 nm); p-GaN (300 nm thick); and a p++ GaN (10 nm thick) layer 404. 4. Performing ion implantation and defining openings. 5. After surface cleaning, re-grow n++ GaN (10 nm thick) to complete the tunnel junction 406. 6. Depositing an n-GaN layer 402 (10-100 nm thick) for damping and current spreading. 7. Dry etch the mesas to define elements 304. 8. Depositing a planar dielectric DBR mirror 407. 9. Depositing contacts 408, 409 and flip-chip bonding / attaching to transparent carrier 501. 11. Removing the substrate 101 through LLO or chemical etching. 12. Dissolving ELO mask 104 on ELO wing interface 507. 13. Depositing dielectric DBR mirror 407 over curved surface 701 of ELO wing interface 507. 14. Dry etch selective portions of interface 507 to expose the n-GaN layer 402 outside of curved mirror 407 and deposit contacts 408, 409. 15. The resulting structure of element 304 is shown in Figures 7(c) and 7(d) (side implant case), by following these steps, a vertical implant design can be obtained.

[0117] Important advantages include: Foreign substrates 101 can be used and scaling would not be an issue. The high crystalline quality device layer 303 resulting from the ELO III-nitride layer 301 results in less leakage, longer lifetime, and higher output power. The curved surface 701 of the DBR mirror 407 is the interface 507 of the ELO wing 302 on the growth constraining mask 104, and therefore no special preparation is required to make the surface smooth. · The curved surface 701 is fabricated on the host substrate 101 or ELO mask 104, therefore the interface 507 does not undergo further processing to form the curvature. Laser or chemical lift-off does not damage the VCSEL 304. The ELO wing interface 507 is covered by the ELO mask 104 during the removal process.

[0118] (Third embodiment) The third embodiment is also a long cavity VCSEL 304 fabricated on the ELO wings 302 of a heterosubstrate 101, and the lifted off device 304 uses the ELO wing interface 507 for the second DBR mirror 407. The difference is that a curved mirror 508 is fabricated on the p-side of the VCSEL 304. Before doing so, the base ELO III-nitride layer 301 is polished as in the design IC, however the layers 301, 303 for the longer cavity are grown on the p-side of the device 304, and after removing the host substrate 101, uses the ELO wing interface 507 as the second DBR 407.

[0119] The III-nitride layers 301, 303 with the cavity can be grown by MOCVD to have a total thickness of more than 8 μm. A tunnel junction 406, a highly doped p++ / n++ junction, is grown on the p-side of the device 304, followed by 1-2 μm of n-GaN 402 or UID GaN 401. The top n-GaN 402 or UID-GaN 401 is processed to have a curved surface above an opening defined as a current blocking region 405 with ion implantation. To etch a lens shape into the GaN 401, 402, the etched layers 401, 402 must be as thick as or thicker than the lens thickness, often several microns thick. An ohmic contact 408 should be present on the n-GaN 402 or n++ GaN of the tunnel junction 406. Instead of the lossy n-GaN 402, the contact 408 on the UID GaN 401 minimizes the absorption losses within the VCSEL 304 cavity.

[0120] An exemplary process includes the following steps. 1. Grow a base ELO III-nitride layer 301 on the GaN template 102 of a heterosubstrate 101, typically greater than 10 μm. The ELO III-nitride layer 301 comprises a UID GaN layer 401. 2. Polishing may or may not be used to control cavity thickness. 3. The following device layers 303 are grown, in order, on the base ELO III-nitride layer 301: an n-GaN layer 402 (1,000 nm thick) for cladding and n-contact; InGaN multiple quantum wells and GaN barriers as the active region 403; an AlGaN electron blocking layer 405 (50 nm); a p-GaN (300 nm thick); and a p++GaN (10 nm thick) layer 404. 4. Performing ion implantation and defining openings. 5. After surface cleaning, re-grow n++ GaN (10 nm thick) to complete the tunnel junction 406. 6. Depositing an n-GaN layer 402 (1,000 nm thick) for damping and current spreading, and a UID GaN layer 401 (3 μm) for lensing. 7. Dry etch the mesas to define elements 304. 8. Etch a lens shape with curved surface 701 in the UID-GaN layer 401 down to the n-GaN layer 402 using thermal reflow of resin using RIE. 9. Depositing a dielectric DBR mirror 407 over the curved surface. 10. Depositing contacts 408, 409 and flip-chip bonding to carrier 501. 11. Removing the substrate 101 through LLO or chemical etching. 12. Dissolving ELO mask 104 on ELO wing interface 507. 13. Dry etch interface 507 to expose n-GaN layer 402 outside the opening and deposit contacts 408, 409. 14. Depositing a planar dielectric DBR 407 onto the pristine ELO wing interface 507. The cavity is made fairly thick. 15. The resulting structure of element 304 is shown in Figures 6(g) and 6(h) (side implant case), by following these steps, a vertical implant design can be obtained.

[0121] Important advantages include: Foreign substrates 101 can be used and scaling would not be an issue. High crystalline quality device layer 303 on ELO III-nitride layer 301 results in less leakage, longer lifetime, and higher output power. The curved surface of the DBR mirror 407 is on the p-side surface, therefore the smoothness can be epitaxially controlled. · The flat DBR mirror 407 is fabricated on the ELO wing interface 507, therefore both surface preparations for both mirrors 407 are simple. Laser or chemical lift-off will not damage the VCSEL 304. The ELO wing interface 507 is covered with the ELO mask 104 during the removal process.

[0122] (Fourth embodiment) In a fourth embodiment, a short cavity VCSEL 304 is fabricated on the ELO wings 302 of a heterosubstrate 101 , the device 304 is lifted off, and then a curved mirror 508 is fabricated on the ELO wing interface 507 .

[0123] A substrate 101 with a III-nitride template 102 is provided, and a growth-limiting mask 104 or ELO mask 104 is placed on the host substrate 101. The III-nitride template 102 can be stripes as illustrated in Figures 1(a), 1(b), 1(c), and 1(d) and Figures 2(a), 2(b), 2(c), and 2(d). A base ELO III-nitride layer 301 is grown from the opening area 105, and includes an n-GaN layer 401. ELO wings 302 with appropriate width for a long-cavity VCSEL 304 are achieved, and then the remaining device layers 303, such as InGaN, p-GaN layer 404, including the active region 403, are grown.

[0124] The p-GaN layer 404 is then activated. Since the ELO layer 301 is not coalesced with neighboring ELO layers 301, activation of the p-GaN layer 404 is achieved using the sidewalls in the non-coalesced regions, which provide better paths for hydrogen diffusion. A hard mask, e.g., Ti / Au, is then deposited to protect the open areas during ion implantation to create the current blocking region 405. After implantation, the hard mask is removed using heated aqua regia and the sample is directly cleaned prior to regrowth of the tunnel junction 406. Alternatively, ITO can also be chosen as the current spreader 406. The tunnel junction 406 comprises a highly doped n++ GaN tunneling layer, followed by an n-GaN current spreading layer 402 and an n++ GaN contact layer 402 grown by MOCVD. The p-GaN layer 405 is then reactivated again through the sidewalls.

[0125] SiO 2 / A DBR mirror 407 consisting of alternating pairs of Ta2O5 bilayers is deposited and a p-contact 409 around the periphery of the DBR mirror 407 is defined by lithography. A transparent carrier substrate 501 is bonded to the p-side of the element 304. Laser or chemical lift-off is then used to remove the host substrate 101.

[0126] The ELO mask 104 on the ELO wing interface 507 is dissolved in a chemical etch, and then the ELO III-nitride layer 301 is thinned to the desired resonant cavity length to achieve a short cavity design. An n-side DBR 407 consisting of a Ta2O5 / SiO2 bilayer is deposited as shown in Figures 5(i) and 5(j). This design is particularly useful for short cavity VCSELs 304. An n-contact 408 is then defined on the ELO wing interface 507 for vertical current injection. Alternatively, a top-side contact 408 can also be used for lateral injection.

[0127] An exemplary process includes the following steps. 1. Preparing an ELO mask 104 with a planar surface on a host substrate 101. 2. Grow a base ELO III-nitride layer 301 on the GaN template 102 on the host substrate 101, typically greater than 20 μm. The ELO III-nitride layer 301 comprises a UID GaN layer 401. 3. Growing the following device layers 303, in order, on the ELO III-nitride layer 301: an n-GaN layer 402 (1,000 nm thick) for cladding and n-contact; InGaN multiple quantum wells and GaN barriers as the active region 403; an AlGaN electron blocking layer 405 (50 nm); a p-GaN (300 nm thick); and a p++GaN (10 nm thick) layer 404. 4. Performing ion implantation and defining openings. 5. After surface cleaning, re-grow n++ GaN (10 nm thick) to complete the tunnel junction 406. 6. Depositing an n-GaN layer 402 (10-100 nm thick) for damping and current spreading. 7. Dry etch the mesas to define elements 304. 8. Depositing a planar dielectric DBR mirror 407. 9. Depositing contacts 408, 409 and flip-chip bonding / attaching to transparent carrier 501. 11. Removing the substrate 101 through LLO or chemical etching. 12. Dissolving ELO mask 104 on ELO wing interface 507. 13. Thinning the ELO wing interface 507 to reach the designed short cavity thickness. 14. Deposit dielectric DBR mirror 407 over the thinned surface on ELO wing 302. 15. Dry etching selective portions of interface 507 to expose the n-GaN layer 402 outside the opening and depositing contacts 408, 409. 16. The resulting structure of element 304 is shown in Figures 5(i) and 5(j) (side-implant case), by following these steps, a side-implant design can be obtained.

[0128] Important advantages include: Foreign substrates 101 can be used and scaling would not be an issue. The high crystalline quality device layer 303 resulting from the ELO III-nitride layer 301 results in less leakage, longer lifetime, and higher output power. Thinning the ELO wing interface 507 by bonding the VCSEL element 304 to the carrier 501. Laser or chemical lift-off does not damage the VCSEL 304. The ELO wing interface 507 is covered by the ELO mask 104 during the removal process.

[0129] Fifth embodiment In a fifth embodiment, a short cavity VCSEL 304 is fabricated on the ELO wings 302 of a heterosubstrate 101 , the device 304 is lifted off, and then a DBR mirror 407 is placed on the ELO wing interface 507 .

[0130] A substrate 101 with a III-nitride template 102 is provided, and a growth-limiting mask 104 or ELO mask 104 is placed on the host substrate 101. The III-nitride template 102 can be stripes as illustrated in Figures 1(a), 1(b), 1(c), and 1(d) and Figures 2(a), 2(b), 2(c), and 2(d). A base ELO III-nitride layer 301 is grown from the opening area 105, and includes an n-GaN layer 402. ELO wings 302 with appropriate width for a long-cavity VCSEL 304 are achieved, and device layers 303, such as InGaN, p-GaN layer 404, including an active region 403, are grown, as shown in Figures 6(a) and 6(b).

[0131] The device layer 303 is activated. Since the ELO III-nitride layer 301 is not coalesced with the neighboring ELO III-nitride layer 301, activation of the p-GaN layer 404 is easier since the sidewalls in the non-coalesced regions provide better paths for hydrogen diffusion. Then, a hard mask, e.g. Ti / Au, is deposited to protect the open areas during ion implantation to create the current blocking region 405. After implantation, the hard mask is removed using heated aqua regia and the sample is directly cleaned prior to the regrowth of the tunnel junction 406. Alternatively, ITO can also be chosen as the current spreading layer 406. The tunnel junction 406 comprises a highly doped n++ GaN tunneling layer, followed by an n-GaN current spreading layer 402 and an n++ GaN contact layer 402 grown by MOCVD. Then, the p-GaN layer 404 is reactivated again through the sidewalls.

[0132] SiO 2 / A DBR mirror 407 consisting of alternating pairs of Ta2O5 bilayers is deposited and a p-contact 409 around the periphery of the DBR mirror 407 is defined by lithography. A transparent carrier substrate 501 is bonded to the p-side of the element 304. Laser or chemical lift-off is then used to remove the host substrate 101.

[0133] The ELO mask 104 on the ELO wing interface 507 is dissolved in a chemical etch, and then an n-side DBR 407 consisting of a Ta2O5 / SiO2 bilayer is deposited as shown in Figures 6(e) and 6(f) to form the second DBR mirror 407 of the VCSEL 304. This design is specifically dedicated to the short cavity VCSEL 304. An n-contact 408 is then defined on the ELO wing interface 507 for vertical current injection. Alternatively, a top side n-contact 408 can also be used for lateral injection.

[0134] An exemplary process includes the following steps. 1. Preparing an ELO mask 104 with a planar surface on a host substrate 101. 2. Grow an ELO III-nitride layer 301 on the GaN template 102 of the substrate 101, typically greater than 20 μm. The ELO III-nitride layer 301 comprises a UID GaN layer 401. 3. Thinning the ELO III-nitride layer 301 from the top of the surface (in this design, the thinning is performed with the host substrate 101 still attached). 4. Growing the following device layers 303 on the ELO III-nitride layer 301, in order: an n-GaN layer 402 (1,000 nm thick) for cladding and n-contact; InGaN multiple quantum wells and GaN barriers as the active region 403; an AlGaN electron blocking layer 405 (50 nm); p-GaN (300 nm thick); and a p++ GaN (10 nm thick) layer 404. 5. Performing ion implantation and defining openings. 6. After surface cleaning, re-grow n++ GaN (10 nm thick) to complete the tunnel junction 406. 7. Depositing an n-GaN layer 402 (10-100 nm thick) for damping and current spreading. 8. Dry etch the mesas to define elements 304. 9. Depositing a planar dielectric DBR mirror 407. 10. Depositing contacts 408, 409 and flip-chip bonding / attaching to carrier 501. 11. Removing the substrate 101 through LLO or chemical etching. 12. Dissolving ELO mask 104 on ELO wing interface 507. 13. Depositing dielectric DBR mirror 407 over ELO wing interface 507. 14. Dry etch interface 507 to expose the n-GaN layer 402 outside the opening and deposit contacts 408, 409. 15. The resulting structure of element 304 is shown in Figures 6(e) and 6(f) (side-implant case), by following these steps, a side-implant design can be obtained.

[0135] Key advantages include: Foreign substrates 101 can be used and scaling would not be an issue. The high crystalline quality device layer 303 resulting from the ELO III-nitride layer 301 results in less leakage, longer lifetime, and higher output power. Thinning is performed on the ELO layer 301 with the host substrate 101 still attached. Laser or chemical lift-off does not damage the element 304. The ELO wing interface 507 is covered by the ELO mask 104 during the removal process.

[0136] (Process Step) 10 is a flow chart illustrating a method 1000 of fabricating a semiconductor device in accordance with the present invention. Specifically, FIG. 10 illustrates a method 1000 of fabricating a VCSEL 304.

[0137] Block 1001 represents the step of providing a host substrate 101. In this step, the host substrate 101 comprises a III-nitride substrate 101 or a foreign substrate 101 with a III-nitride template 102 deposited thereon. The III-nitride template 102 comprises one or more selective growth supporting portions formed on the host substrate.

[0138] Block 1002 represents the step of depositing a growth-limiting mask 104 on or above the host substrate 101, where the growth-limiting mask 104 may be patterned. Specifically, the growth-limiting mask 104 is deposited directly on the substrate 101, or the growth-limiting mask 104 is deposited directly on a III-nitride template 102 that is deposited on the substrate 101. The use of a III-nitride template 102 may result in one or more non-growth-supporting portions of the host substrate 101 being in direct contact with a bottom surface of the growth-limiting mask 104.

[0139] The growth limiting mask 104 is typically an insulating film, such as SiO2, SiN, SiON, TiN, etc., deposited by, for example, plasma enhanced chemical vapor deposition (CVD), sputtering, ion beam deposition (IBD), or the like.

[0140] Growth-limiting mask 104 is fabricated with a patterned surface that is transferred to interface 507 of ELO III-nitride layer 301. Alternatively, host substrate 101 is fabricated with a patterned surface that is transferred to growth-limiting mask 104 and then to interface 507 of ELO III-nitride layer 301.

[0141] Block 1003 represents forming one or more ELO III-nitride layers 301 on the growth-limiting mask 104, first from the open areas 105 in the growth-limiting mask 104 and then laterally over the growth-limiting mask 104, which may or may not coalesce with adjacent (or neighboring) ELO III-nitride layers 301. The ELO III-nitride layers 301 may comprise a UID GaN layer 401 and / or an n-type GaN layer 402.

[0142] Block 1004 represents the step of forming at least one VCSEL 304 on the ELO III-nitride layer 301, the VCSEL 304 being comprised of a group III device layer 303 including at least a group III-nitride active region 403 between an n-type group III-nitride layer 402 and a p-type group III-nitride layer 404 grown on or above the ELO group III-nitride layer 301, the ELO group III-nitride layer 301 and the group III device layer 303 together comprising island-like group III-nitride semiconductor layers 301, 303.

[0143] In one embodiment, the group III device layers 303 may include a UID GaN layer 401, an n-GaN layer 402 for cladding and n-contact, InGaN multiple quantum wells and GaN barriers as the active region 403, p-GaN and p++ GaN layers 404, an electron blocking layer 405, a tunnel junction 406, or a transparent conducting layer 406.

[0144] Preferably, the group III-nitride device layers 303 are grown on the wings 302 of the ELO group III-nitride layer 301. Additionally, the light emission aperture of the VCSEL 304 is fabricated on the wings 302 of the ELO group III-nitride layer 301. In situations where multiple VCSELs 304 may be fabricated, the group III-nitride device layers 303 of the first and second VCSELs 304 are fabricated on adjacent wings 302 of the ELO group III-nitride layer 301.

[0145] Block 1005 represents the step of fabricating a light emitting device 304, such as a VCSEL 304, on the wings 302 of the ELO III-nitride layer 301 covered by a mostly flat surface region by conventional lithographic methods. This step may include performing ion implantation to define openings, etching mesas to define the devices 304, etc.

[0146] Block 1006 represents the step of disposing at least one first DBR mirror 407 on or above the III-nitride device layers 303 that defines a resonant cavity of the VCSEL 304. Specifically, the DBR mirror 407 that defines the resonant cavity of the VCSEL 304 is disposed on the p-side of the III-nitride device layers 303.

[0147] The DBR mirror 407 may be formed on or above the p-type III-nitride layer 404 such that the p-type III-nitride layer 404 is between the III-nitride active region 403 and the DBR mirror 407 .

[0148] The VCSEL 304 may further comprise one or more tunnel junction 406 layers on the p-type III-nitride layer 404, with a DBR mirror 407 formed below the tunnel junction 406 layers, such that the ELO III-nitride layer 301 is between the DBR mirror 407 and the tunnel junction 406 layers.

[0149] The VCSEL 304 may further comprise one or more tunnel junction 406 layers on the p-type III-nitride layer 404, with a DBR mirror 407 formed on or above the tunnel junction 406 layer such that the tunnel junction 406 layer is between the DBR mirror 407 and the p-type III-nitride layer 404.

[0150] This step may include, after surface cleaning, regrowing an n++ GaN layer to complete the tunnel junction 406, depositing an additional n-type GaN layer 402 on or above the tunnel junction 406 for current spreading, etc. The additional n-type III-nitride layer 402 has a curvature shape for the DBR mirror 407.

[0151] Block 1007 represents the step of attaching the device 304 structure to a carrier 501 and then removing the ELO III-nitride layer 301 and VCSEL 304 from the host substrate 101 to expose the interface 507 of the ELO III-nitride layer 301 .

[0152] Specifically, the p-side of III-nitride device layer 303 with DBR 407 is attached to a carrier 501 or submount, and then LLO or chemical etching is used to lift-off ELO III-nitride layer 301 and III-nitride device layer 303 from host substrate 101. A laser 505 is used to lift-off ELO III-nitride layer 301 and III-nitride device layer 303 from host substrate 101 at open window regions 506 of wings 302 of ELO III-nitride layer 301, thereby leaving III-nitride device layer 303 grown on ELO III-nitride layer 301 undamaged.

[0153] This step involves dissolving the growth limiting mask 104 on the ELO wing interface 507 and using thermal reflow of the resin to etch a curved mirror 508 shape with a curved surface 701 into the UID-GaN layer 401 using RIE.

[0154] Block 1008 represents the step of placing at least one second DBR mirror 407 on the interface 507 of the ELO III-nitride layer 301 that defines a resonant cavity for the VCSEL 304. In one embodiment, the DBR mirror 407 is placed on the wing 302 of the ELO III-nitride layer.

[0155] The interface 507 of the ELO III-nitride layer 301 may have a patterned surface for the DBR mirror 407 , the patterned surface comprising a curvature shape 701 for the DBR mirror 407 .

[0156] In an embodiment in which the VCSEL 304 is comprised of a first and second DBR mirror 407, the first DBR 407 mirror may comprise a flat DBR mirror 407, the second DBR mirror 407 may comprise a flat DBR mirror 407 or a curved DBR mirror 407, and the III-nitride active region 403 is positioned between the first DBR mirror and the second DBR mirror 407.

[0157] The ELO III-nitride layer 301 may comprise more than 50% of the resonant cavity between the first and second DBR mirrors 407, with the ELO III-nitride layer 301 comprising the UID GaN layer 401 or the n-type GaN layer 402. The interface 507 of the ELO III-nitride layer 301 is on the n-side of the VCSEL 304.

[0158] In one embodiment, the total cavity length of the resonant cavity is greater than 8 μm; alternatively, the interface 507 of the host substrate 101 or the ELO III-nitride layer 107 is thinned to reduce the total cavity length of the resonant cavity to less than 8 μm.

[0159] Block 1009 represents the step of depositing contacts 408, 409 for the VCSEL 304. In one embodiment in which the VCSEL 304 includes a tunnel junction 406, the contacts may comprise an n-contact 408, while in other embodiments the contacts may comprise both an n-contact 408 and a p-contact 409.

[0160] This step may include etching selective portions of interface 507 to expose n-GaN layer 402 for deposition of metal n-contact 408.

[0161] This step may also include forming lateral or vertical injection configurations for injecting current into the elements 304, and depositing n-contacts 408 and p-contacts 409 on the elements 304. These configurations allow each element 304 in the bar of elements 304 to be addressed separately or together with the other elements 304.

[0162] Block 1010 represents the step of transferring the device 304 to a submount or other external carrier. In one embodiment, this step includes flip-chip bonding of the device 304 including the island-like III-nitride semiconductor layers 301, 303 to a transparent submount or other external carrier.

[0163] Block 1011 represents the step of completing the fabrication of the VCSEL 304. This step may include packaging the VCSEL 304, etc.

[0164] Block 1012 represents the end result of the method, ie, the completed device 304 and any applications that include the completed device 304 .

[0165] (References) The following references are incorporated herein by reference: 1. U.S. Patent Application Publication No. 2017 / 0092810, filed June 11, 2014, and published March 30, 2017, by Raring et al., entitled “Surface morphology of non-polar gallium nitride containing substrates.” 2.Applied Physics Express 13,041003 (2020) 3.Applied Physics Express 12,044004 (2009) 4.Sci.Rep.,8,10350 (2018)

[0166] (Conclusion) The description of the preferred embodiments of the present invention now concludes. The foregoing description of one or more embodiments of the present invention has been presented for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Many modifications and variations are possible in light of the above teachings. It is intended that the scope of the present invention be limited not by this detailed description, but rather by the claims appended hereto.

Claims

1. 1. A method, comprising: Providing a host substrate; depositing a growth limiting mask onto the host substrate; forming one or more epitaxial lateral overgrowth (ELO) III-nitride layers over the growth-limiting mask; forming at least one vertical cavity surface emitting laser (VCSEL) on the ELO III-nitride layers, the VCSEL comprising III-nitride device layers including at least a III-nitride active region between an n-type III-nitride layer and a p-type III-nitride layer; removing the ELO III-nitride layer and the VCSEL from the host substrate to expose an interface of the ELO III-nitride layer; providing at least one distributed Bragg reflector (DBR) mirror on the interface of the ELO III-nitride layer that defines a resonant cavity of the VCSEL; A method comprising:

2. The method of claim 1 , wherein selective growth assist portions are formed on the host substrate.

3. The method of claim 1 , wherein the non-growth-supporting portion of the host substrate is in direct contact with a bottom surface of the growth-limiting mask.

4. The method of claim 1 , wherein the DBR mirrors are located on wings of the ELO III-nitride layer.

5. The method of claim 1 , wherein the interface of the ELO III-nitride layer comprises a patterned surface for the DBR mirror.

6. The method of claim 5 , wherein the patterned surface comprises a curvature shape for the DBR mirror.

7. The method of claim 5 , wherein the growth-limiting mask is fabricated to have the patterned surface that is transferred to the interface of the ELO III-nitride layer.

8. The method of claim 5 , wherein the host substrate is fabricated having the patterned surface that is transferred to the interface of the ELO III-nitride layer.

9. 10. The method of claim 1 , wherein the VCSEL further comprises one or more tunnel junction layers on the p-type III-nitride layer, and the DBR mirror is formed below the tunnel junction layer such that the ELO III-nitride layer is between the DBR mirror and the tunnel junction layer.

10. 10. The method of claim 9, wherein the DBR mirror is formed on or above the p-type III-nitride layer such that the p-type III-nitride layer is between the III-nitride active region and the DBR mirror.

11. 10. The method of claim 1 , wherein the VCSEL further comprises one or more tunnel junction layers on the p-type III-nitride layer, and the DBR mirror is formed on or above the tunnel junction layers such that the tunnel junction layers are between the DBR mirror and the p-type III-nitride layer.

12. 12. The method of claim 11, wherein the VCSEL further comprises an additional n-type III-nitride layer on or above the tunnel junction layer, the additional n-type III-nitride layer having a curved shape that forms the DBR mirror.

13. the at least one DBR mirror comprises a first and a second DBR mirror; the first DBR mirror comprises a flat DBR mirror; the second DBR mirror comprises a flat DBR mirror or a curved DBR mirror; The method of claim 1 , wherein the III-nitride active region is positioned between the first and second DBR mirrors.

14. 10. The method of claim 1 , wherein the ELO III-nitride layer comprises greater than 50% of the resonant cavity, the ELO III-nitride layer comprising GaN, unintentionally doped GaN, or n-type GaN.

15. The method of claim 1 , wherein the total cavity length of the resonant cavity is greater than 8 μm.

16. The method of claim 1 , wherein the interface of the ELO III-nitride layer is thinned to reduce a total cavity length of the resonant cavity to less than 8 μm.

17. The method of claim 1 , wherein the host substrate is thinned to reduce a total cavity length of the resonant cavity to less than 8 μm.

18. The method of claim 1 , wherein the interface of the ELO III-nitride layer is on an n-side of the VCSEL.

19. 20. The method of claim 18, wherein the DBR mirror that defines the resonant cavity of the VCSEL is located on a p-side of the III-nitride device layers.

20. 20. The method of claim 19, wherein the p-side of the III-nitride device layer with the DBR is attached to a submount and then laser or chemical etching is used to lift off the III-nitride device layer from the host substrate.

21. 21. The method of claim 20, wherein the laser is used in open window regions of wings of the ELO III-nitride layer to lift off the III-nitride device layers from the host substrate such that the III-nitride device layers grown on the ELO III-nitride layer are not damaged.

22. The method of claim 1 , wherein the device layer of the VCSEL is fabricated on wings of the ELO III-nitride layer.

23. The method of claim 22 , wherein a light emission aperture of the VCSEL is fabricated on the wings of the ELO III-nitride layer.

24. 2. The method of claim 1 , wherein the at least one VCSEL comprises a first and a second VCSEL, the III-nitride device layers of the first VCSEL and the second VCSEL being fabricated on adjacent wings of the ELO III-nitride layer.

25. 13. A vertical cavity surface emitting laser (VCSEL) fabricated by the method of claim 1.

26. An element, the element comprising: A host substrate; a growth limiting mask deposited on the host substrate; one or more epitaxial lateral overgrowth (ELO) Group III nitride layers formed on the growth limiting mask; at least one vertical cavity surface emitting laser (VCSEL) formed on the ELO III-nitride layer; Equipped with the VCSEL comprises III-nitride device layers including at least a III-nitride active region between an n-type III-nitride layer and a p-type III-nitride layer; the ELO III-nitride layer and the VCSEL are removed from the host substrate to expose an interface of the ELO III-nitride layer; At least one distributed Bragg reflector (DBR) mirror defining a resonant cavity of the VCSEL is disposed on the interface of the ELO III-nitride layer.

Citation Information

Patent Citations

  • Vertical cavity surface emitting laser based on Van der Waals epitaxy and manufacturing method thereof

    CN112436380A

  • Method for removing a substrate using a cleaving technique

    JP2020534687A

  • Contact architectures for tunnel junction devices

    US20210104504A1

  • Light emitting device

    WO2020075428A1

  • Method of fabricating a resonant cavity and distributed bragg reflector mirrors for a vertical cavity surface emitting laser on a wing of an epitaxial lateral overgrowth region

    WO2021081308A1

Cited By

  • Optical element substrate, method for manufacturing optical element substrate, and method for manufacturing optical communication substrate

    WO2026203285A1