Non-oriented silicon steel for new energy drive motors and its production method

A non-oriented silicon steel with a controlled chemical composition and optimized production process achieves balanced magnetic performance and strength, addressing the contradiction in existing technologies, and meets the demands of new energy vehicle drive motors with improved production efficiency and reduced costs.

JP2024540901AActive Publication Date: 2024-11-06INST OF RES OF IRON & STEEL JIANGSU PROVINCE +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024523397
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-26
Filing Date
2022-01-27
Publication Date
2024-11-06
Estimated Expiration
2042-01-27

AI Technical Summary

Technical Problem

Existing non-oriented silicon steel used in new energy vehicle drive motors faces a contradiction between improving magnetic performance and strength, as adding alloying elements like Cu, Cr, Ni, Nb, and Ti deteriorates magnetic performance while increasing strength.

Method used

A non-oriented silicon steel with a specific chemical composition (2.95%~3.15% Si, 0.75%~0.95% Al, 0.5%~0.7% Mn, 0.03%~0.04% Sn, controlled impurities) and a production process involving hot rolling, normalizing, single-stand cold rolling, and annealing, without adding alloying elements like Cu, Cr, Ni, Nb, and Ti, to achieve refined crystal strengthening and balanced magnetic performance and strength.

Benefits of technology

The solution results in non-oriented silicon steel with high strength, low core loss, and high magnetic flux density, meeting the requirements of new energy vehicle drive motors, while reducing production costs and energy consumption, and avoiding cracking issues during cold rolling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024540901000001
    Figure 2024540901000001
  • Figure 2024540901000002
    Figure 2024540901000002
  • Figure 2024540901000003
    Figure 2024540901000003
Patent Text Reader

Abstract

The present invention discloses a non-oriented silicon steel for new energy drive motors and a method for producing the same. The silicon steel is produced by sequentially carrying out steelmaking, continuous casting, hot rolling, normalizing, pickling, single stand cold rolling without preheating, annealing, cooling, coating and finishing. No Cu, Cr, Ni, Nb, V or Ti is added in the steelmaking process, and the chemical composition of the silicon steel is Si: 2.95%-3.15%, Al: 0.75%-0.95%, Si+2Al: 4.6%-4.9%, Mn: 0.5%-0.7%, Sn: 0.03%-0.04%, C≦0.0025%, the balance being iron, Mn / S≧380, Al / N≧200. The present invention improves strength while ensuring magnetic performance, solving the problem of compatibility between magnetic performance and strength that exists in the prior art, and can meet the requirements for application to drive motors of new energy vehicles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the technical field of steel material preparation, and relates to a non-oriented silicon steel for new energy drive motors and a method for producing the same. [Background technology]

[0002] Non-oriented silicon steel is the core material of the rotor of electric motors and generators operating in a rotating magnetic field, and good magnetic performance including low core loss and high magnetic flux density is required, and the improvement of magnetic performance is the central research topic of non-oriented silicon steel for those skilled in the art. From the viewpoint of chemical composition, the addition of a series of alloying elements such as Cu, Cr, Ni, Nb, V, Ti, etc. is usually strictly limited to avoid the deterioration of the magnetic performance of non-oriented silicon steel due to the high content of these alloying elements.

[0003] In recent years, with the rapid development of new energy vehicles, the non-oriented silicon steel used in the drive motor is required to have higher performance. Specifically, the drive motor of the new energy vehicle has a higher rotation speed than other conventional motors, and with the development of technology, the rotation speed of the drive motor of the new energy vehicle is still increasing, so the non-oriented silicon steel used is required to have high strength in addition to good magnetic performance.

[0004] However, in the prior art of improving the strength of steel, from the viewpoint of chemical composition, it is usually necessary to increase the amount of a series of alloying elements such as Cu, Cr, Ni, Nb, V, Ti, etc., to achieve the purpose of improving the strength of steel, and as mentioned above, the increase in the amount of these alloying elements leads to the deterioration of the magnetic performance of non-oriented silicon steel.

[0005] It can be seen from this that the design direction of the chemical composition is contradictory with respect to the influence of the magnetic performance and strength of the non-oriented silicon steel. Therefore, how to ensure the magnetic performance and strength of the non-oriented silicon steel at the same time is an important problem faced by the non-oriented silicon steel applied to the drive motor of the new energy vehicle. Summary of the Invention

[0006] An object of the present invention is to provide a non-oriented silicon steel for new energy drive motors, which improves strength while ensuring magnetic performance, and solves the problem of balancing magnetic performance and strength that exists in the prior art, and to provide a method for producing the same.

[0007] In order to achieve the above object of the invention, an embodiment of the present invention provides a non-oriented silicon steel for new energy drive motors, and its chemical composition, in mass%, is as follows: Si: 2.95%-3.15%, Al: 0.75%-0.95%, Si+2Al: 4.6%-4.9%, Mn: 0.5%-0.7%, Sn: 0.03%-0.04%, Cu≦0.03%, Cr≦0.03%, Ni ≦0.03%, Cr+Ni+Cu≦0.07%, Nb≦0.004%, V≦0.004%, Ti≦0.004%, Nb+V+Ti≦0.008%, C≦0.0025%, P≦0.015%, S≦0.0015%, N≦0.004%, C+S+N≦0.007%, and the balance is Fe and unavoidable impurities. Mn / S≧380, Al / N≧200.

[0008] Furthermore, the recrystallized grain size of the non-oriented silicon steel is 50 μm to 80 μm.

[0009] Furthermore, the non-oriented silicon steel is a steel plate having a thickness of 0.25 mm to 0.35 mm, and has a yield strength of ≥ 460 MPa, a tensile strength of ≥ 550 MPa, and an iron loss P 1.0 / 400 ≦18.5W / kg, magnetic flux density B 5000 ≧1.67T.

[0010] Furthermore, the non-oriented silicon steel is a steel plate having a thickness of 0.25 mm, and the iron loss P 1.0 / 400 ≦17.5W / kg, or 0.30mm thick steel plate with iron loss P 1.0 / 400 ≦18.0W / kg, or steel plate with a thickness of 0.35mm, iron loss P 1.0 / 400 ≦18.5W / kg.

[0011] In order to achieve the above object of the invention, an embodiment of the present invention provides a method for producing non-oriented silicon steel for new energy drive motors, and the chemical composition of the non-oriented silicon steel is, in mass%, Si: 2.95%-3.15%, Al: 0.75%-0.95%, Si+2Al: 4.6%-4.9%, Mn: 0.5%-0.7%, Sn: 0.03%-0.04%, Cu≦0.03%, Cr≦0.0 3%, Ni≦0.03%, Cr+Ni+Cu≦0.07%, Nb≦0.004%, V≦0.004%, Ti≦0.004%, Nb+V+Ti≦0.008%, C≦0.0025%, P≦0.015%, S≦0.0015%, N≦0.004%, C+S+N≦0.007%, with the balance being Fe and unavoidable impurities; Mn / S≧380, Al / N≧200; The recrystallized grain size of the non-oriented silicon steel is 50 μm to 80 μm, The method includes sequentially carrying out steelmaking, continuous casting, hot rolling, normalizing, pickling, single-stand cold rolling, annealing, cooling, coating and finishing to produce non-oriented silicon steel; In the hot rolling process, the continuous casting billet obtained in the continuous casting process is heated to 1080°C to 1110°C and held for 160min to 180min, and then rough rolling, finish rolling, and coiling are sequentially performed to obtain a hot rolled coil plate. The rolling start temperature during the finish rolling is 950±20°C, the rolling end temperature is 840±20°C, the total rolling reduction is 94 to 95%, and the coiling temperature during coiling is 620±20°C. In the normalizing process, the normalizing temperature is set to 840°C to 860°C and held for 180s to 200s. In the annealing step, the annealing temperature is set to 960° C. to 980° C., and is held for 40 s to 45 s.

[0012] Preferably, in the single stand cold rolling process, multi-pass rolling is performed, the total rolling reduction is 85±3%, and the rolling reduction of each pass other than the final pass is 30% or more.

[0013] Preferably, the obtained non-oriented silicon steel is a steel plate having a thickness of 0.25 mm to 0.35 mm, and in the hot rolling step, a continuous casting billet having a thickness of 220 mm is roughly rolled into an intermediate billet having a thickness of 35 mm to 40 mm, and then finish rolled into a hot rolled plate having a thickness of 2.00 mm to 2.30 mm.

[0014] Preferably, the obtained non-oriented silicon steel is a steel plate having a thickness of 0.25 mm, the intermediate billet has a thickness of 35 mm, and the hot rolled plate has a thickness of 2.00 mm; or the obtained non-oriented silicon steel is a steel plate having a thickness of 0.30 mm, the intermediate billet has a thickness of 37.5 mm, and the hot rolled plate has a thickness of 2.15 mm; or the obtained non-oriented silicon steel is a steel plate having a thickness of 0.35 mm, the intermediate billet has a thickness of 40 mm, and the hot rolled plate has a thickness of 2.30 mm.

[0015] Preferably, in the single stand cold rolling step, rolling is started directly without preheating the steel sheet after the pickling step. Effect of the Invention

[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) From the viewpoint of chemical composition, alloy elements such as Cu, Cr, Ni, Nb, V, Ti and other elements are not added, and combined with the design of element contents such as Si, Al, Mn, Sn, the magnetic performance of non-oriented silicon steel is improved to ensure that non-oriented silicon steel has low core loss and high magnetic flux density. At the same time, the grain size is controlled to 50μm-80μm based on the chemical composition to realize the refined crystal strengthening of the steel sheet, ensuring that non-oriented silicon steel has high strength, ensuring low cost and low production difficulty, and achieving the comprehensive optimization of the magnetic performance and strength of non-oriented silicon steel, so that non-oriented silicon steel can meet the application requirements for the drive motor of new energy vehicles. (2) Furthermore, through the series of process control of the hot rolling process, normalizing process, single-stand cold rolling process and annealing process based on the design of the chemical composition, on the one hand, the recrystallized grain size of the non-oriented silicon steel can be refined, and non-oriented silicon steel with excellent magnetic performance and high strength can be reliably obtained; on the other hand, the cracking and fracture problem in cold rolling can be avoided, and the pre-roll preheating or secondary cold rolling commonly used in the existing production process can be omitted, and the final rolling can be realized only by the single-stand cold rolling process without preheating, so as to ensure low production difficulty, low cost and stable and continuous production; on the other hand, through the low-temperature control of the heating temperature, rolling start temperature, normalizing temperature, etc., the production energy consumption can be greatly reduced; in addition, the normalizing temperature can be lowered and the holding time can be shortened, and the thickness of the oxide scale on the surface of the steel sheet before the pickling process can be reduced, the pickling efficiency can be increased, and the surface quality and yield of the final non-oriented silicon steel can be improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The technical solutions of the present invention are further described below in connection with specific embodiments.

[0018] In an embodiment of the present invention, a non-oriented silicon steel is provided, which has a chemical composition, in mass%, of Si: 2.95% to 3.15%, Al: 0.75% to 0.95%, Si+2Al: 4.6% to 4.9%, Mn: 0.5% to 0.7%, Sn: 0.03% to 0.04%, Cu≦0.03%, Cr≦0.03%, Ni≦0.03%, Cr+Ni+Cu≦0.07%, N b≦0.004%, V≦0.004%, Ti≦0.004%, Nb+V+Ti≦0.008%, C≦0.0025%, P≦0.015%, S≦0.0015%, N≦0.004%, C+S+N≦0.007%, and the balance being Fe and unavoidable impurities; Mn / S≧380, Al / N≧200.

[0019] Here, the action and effect of each element in the chemical composition is explained as follows. C, S, N, Cu, Cr, Ni, Nb, V, Ti, P: An increase in the content of these elements leads to a decrease in the magnetic performance of non-oriented silicon steel, including an increase in iron loss and a decrease in magnetic flux density. In the present invention, the upper limits of the content of these elements are appropriately lowered to C≦0.0025%, S≦0.0015%, N≦0.004%, C+S+N≦0.007%, Cu≦0.03%, Cr≦0.03%, Ni≦0.03%, Cr+Ni+Cu≦0.07%, Nb≦0.004%, V≦0.004%, Ti≦0.004%, Nb+V+Ti≦0.008%, and P≦0.015%, without increasing the difficulty and cost of steelmaking.

[0020] Si, Al: Si is a solid solution strengthening element, and an increase in its content can increase the strength of the steel sheet, increase the resistivity of the steel sheet, and decrease the iron loss. When the Si content (in mass%) in the present invention is controlled to 2.95% to 3.15% and the Al content is increased, the resistivity of the steel sheet is increased and the iron loss is decreased, but the magnetic flux density is decreased. The Al content (in mass%) in the present invention is controlled to 0.75% to 0.95%. In addition, Al is likely to form coarse AlN precipitates with N, which decreases the iron loss of the steel sheet. The Al content (in mass%) and the N content (in mass%) in the present invention further satisfy Al / N≧200, which can convert the adverse effect of the N element on the magnetic performance of the steel sheet into an advantageous effect, and reduce the difficulty of controlling the N element in steelmaking. Furthermore, in order to avoid an increase in production cost due to an increase in production difficulty caused by an increase in the Si and Al contents, the Si content (in mass%) and the Al content (in mass%) in the present invention further satisfy Si+2Al: 4.6% to 4.9%.

[0021] Mn: Adding an appropriate amount of Mn is beneficial to improving the magnetic properties of steel sheet, and Mn can suppress the thermal brittleness caused by S, and easily forms coarse MnS precipitates with S, thereby reducing the iron loss of the steel sheet. The Mn content (in mass%) and S content (in mass%) in the present invention further satisfy Mn / S≧380, so that the adverse effect of S element on the magnetic properties of the steel sheet can be converted into an advantageous effect, and the difficulty and cost of controlling S element in steelmaking can be reduced.

[0022] Sn: A grain boundary segregation element that can improve magnetic performance. The Sn content (in mass%) in the present invention is 0.03% to 0.04%.

[0023] As described above, in the present embodiment, while aiming to reduce alloy costs, ease production difficulty, and reduce production costs in terms of chemical composition, alloy elements such as Cu, Cr, Ni, Nb, V, Ti, etc. are not added, and in combination with the design of the contents of elements such as Si, Al, Mn, Sn, etc., the magnetic performance of the non-oriented silicon steel is improved, and it is possible to ensure that the non-oriented silicon steel has low iron loss and high magnetic flux density.

[0024] In this embodiment, the recrystallized grain size of the non-oriented silicon steel is 50 μm to 80 μm, and the chemical composition ensures low core loss and high magnetic flux density of the non-oriented silicon steel, while controlling the grain size to 50 μm to 80 μm to realize refined crystal strengthening of the steel sheet and ensure high strength of the non-oriented silicon steel, achieving comprehensive optimization of the magnetic performance and strength of the non-oriented silicon steel while achieving low cost and low production difficulty, and the non-oriented silicon steel meets the requirements for application to the drive motor of a new energy vehicle.

[0025] Specifically, the non-oriented silicon steel is a steel plate having a thickness of 0.25 mm to 0.35 mm, a yield strength of ≥ 460 MPa, a tensile strength of ≥ 550 MPa, and an iron loss P 1.0 / 400 ≦18.5W / kg, magnetic flux density B 5000 ≧1.67T.

[0026] Here, the non-oriented silicon steel is specifically a steel plate having a thickness of 0.35 mm, and its iron loss P 1.0 / 400 ≦18.5W / kg, or steel plate with a thickness of 0.30mm, iron loss P 1.0 / 400 ≦18.0W / kg, or steel plate with a thickness of 0.25mm, iron loss P 1.0 / 400 ≦17.5W / kg.

[0027] Furthermore, the present embodiment further provides a preferred production method for the non-oriented silicon steel, which includes sequentially carrying out steelmaking, continuous casting, hot rolling, normalizing, pickling, single-stand cold rolling, annealing, cooling, coating and finishing to produce the non-oriented silicon steel. That is, the non-oriented silicon steel can be prepared by the preferred production method. The production method of the present embodiment not only allows the non-oriented silicon steel with excellent magnetic properties and high strength to be smoothly produced, but also has the advantages of low production difficulty and low production cost, and ensures stable production of the non-oriented silicon steel.

[0028] Specifically, in the steelmaking process, molten iron is refined into molten steel, and in the continuous casting process, the molten steel obtained in the steelmaking process is made into a continuous cast billet using a continuous casting machine. As will be understood, the chemical composition of the molten steel obtained in the steelmaking process and the chemical composition of the continuously cast billet obtained in the continuous casting process are both identical to the chemical composition of the non-oriented silicon steel finally obtained from the production method. That is, in mass%, it contains Si: 2.95%~3.15%, Al: 0.75%~0.95%, Si+2Al: 4.6%~4.9%, Mn: 0.5%~0.7%, Sn: 0.03%~0.04%, Cu≦0.03%, Cr≦0.03%, Ni≦0.03%, Cr+Ni+Cu≦0.07%, Nb≦0.004%, V≦0.004%, Ti≦0.004%, Nb+V+Ti≦0.008%, C≦0.0025%, P≦0.015%, S≦0.0015%, N≦0.004%, C+S+N≦0.007%, and the remainder is Fe and unavoidable impurities, and Mn / S≧380, Al / N≧200.

[0029] In this embodiment, in the hot rolling process, the continuous cast billet obtained in the continuous casting process is heated to 1080°C to 1110°C and held for 160 min to 180 min, and then rough rolling, finish rolling, and coiling are sequentially performed to obtain a hot rolled coil plate. The rolling start temperature in the finish rolling is 950±20°C, the rolling end temperature is 840±20°C, the total rolling reduction is 94 to 95%, and the coiling temperature in the coiling is 620±20°C. In the normalizing process, the normalizing temperature is 840°C to 860°C and held for 180 s to 200 s. In the annealing process, the annealing temperature is 960°C to 980°C and held for 40 s to 45 s.

[0030] In this way, in the production method of this embodiment, the heating temperature in the hot rolling process is controlled to be low, thereby avoiding the solid solution of coarse precipitates such as MnS and AlN in the continuous casting billet, and more reliably controlling the precipitates in the subsequent rough rolling and finish rolling processes, thereby solidifying the basis for the magnetic performance of the finally obtained grain-oriented silicon steel. The rolling start temperature, rolling end temperature, total reduction rate and coiling temperature in the finish rolling process are controlled, and combined with the design of Si+2Al: 4.6%-4.9% in the chemical composition, the structure of the hot rolled coil plate is stable and the storage capacity is consistent. The recrystallization temperature of the hot rolled coil plate in the subsequent normalizing process is stably maintained, providing conditions for accurate control of the recrystallization degree in the subsequent normalizing process. Based on the hot rolling process, the design of the normalizing temperature and holding time in the normalizing process prevents partial recrystallization from occurring in the normalizing process (i.e., complete recrystallization is not completed). In the conventional cold rolling process, the pre-roll preheating or secondary cold rolling commonly used in the prior art is omitted, and the final rolling can be completed only with a low-cost single-stand cold rolling process without preheating. Based on the normalizing process, the annealing temperature and holding time are designed to allow complete recrystallization to occur in the annealing process, and the recrystallized grain size is not large, so that the recrystallized grain size in the final non-oriented silicon steel is small.

[0031] As described above, in the production method of the present embodiment, a series of processes including the hot rolling process, the normalizing process, the single stand cold rolling process and the annealing process are controlled based on the design of the chemical composition, thereby realizing the refinement of the recrystallized grain size of the non-oriented silicon steel, and ensuring the obtained non-oriented silicon steel with excellent magnetic properties and high strength; on the other hand, the cracking and fracture problem in cold rolling is avoided, and the pre-roll preheating or secondary cold rolling commonly used in the existing production process is omitted, and the final rolling can be completed only through the single stand cold rolling process without preheating, ensuring low production difficulty, low cost and stable continuous production; on the other hand, the low temperature control of the heating temperature, the rolling start temperature, the normalizing temperature and the like greatly reduces the production energy consumption; furthermore, the low normalizing temperature and short holding time reduce the thickness of the oxide scale on the surface of the steel sheet before the pickling process, which is favorable for improving the pickling efficiency, and can improve the surface quality and yield of the final non-oriented silicon steel.

[0032] More preferably, based on the chemical composition required for the final molten steel, no alloying materials such as Cu, Cr, Ni, Nb, V, and Ti are added in the steelmaking process, which can reduce the cost of alloying materials.

[0033] More preferably, in the single stand cold rolling process, the steel sheet after the pickling process is directly rolled without preheating. In the prior art, the steel sheet usually needs to be preheated before cold rolling, but in this embodiment, the steel sheet is directly rolled without preheating after the normalizing process, which can save production costs.

[0034] In the single stand cold rolling process, multi-pass rolling is performed and the total reduction is 85±3%. By controlling in this manner, the cold rolling storage capacity of non-oriented silicon steels of different thicknesses in the single stand cold rolling process is basically the same, and further, the same annealing temperature and holding time are used in the subsequent annealing process. This has the effect of eliminating the need for frequent changeover operations when continuously producing non-oriented silicon steels of different thicknesses on the same production line.

[0035] In the single stand cold rolling process, multi-pass rolling is performed, and the reduction ratio of each pass except the final pass is 30% or more. For example, when five passes are performed, the reduction ratios of the first to fourth passes are 30% or more, and the reduction ratio of the fifth pass is selectively smaller than 30%. This not only effectively avoids the generation of cold rolled fragments in the single stand cold rolling process, but also reduces the number of rolling passes, and ensures a good plate shape of the final non-oriented silicon steel.

[0036] As described above, the non-oriented silicon steel is a steel plate having a thickness of 0.25 mm to 0.35 mm. In a preferred embodiment, the thickness of the continuous cast billet obtained in the continuous casting process is 220 mm, and in the hot rolling process, the continuous cast billet having a thickness of 220 mm is roughly rolled into an intermediate billet having a thickness of 35 mm to 40 mm, and then is finish-rolled into a hot rolled plate having a thickness of 2.00 mm to 2.30 mm. As will be understood, in the single stand cold rolling process, the hot rolled plate having a thickness of 2.00 mm to 2.30 mm is further rolled into a finished product of non-oriented silicon steel having a target thickness.

[0037] For example, when the non-oriented silicon steel finally obtained by the production method is a steel plate having a thickness of 0.25 mm, in the hot rolling step, a continuous cast billet having a thickness of 220 mm is roughly rolled into an intermediate billet having a thickness of 35 mm, and then finish rolled into a hot rolled plate having a thickness of 2.00 mm. Also, when the non-oriented silicon steel finally obtained by the production method is a steel plate having a thickness of 0.30 mm, in the hot rolling step, a continuous cast billet having a thickness of 220 mm is roughly rolled into an intermediate billet having a thickness of 37.5 mm, and then finish rolled into a hot rolled plate having a thickness of 2.15 mm. Also, when the non-oriented silicon steel finally obtained by the production method is a steel plate having a thickness of 0.35 mm, in the hot rolling step, a continuous cast billet having a thickness of 220 mm is roughly rolled into an intermediate billet having a thickness of 40 mm, and then finish rolled into a hot rolled plate having a thickness of 2.30 mm. Of course, these are merely preferred embodiments, and the present invention is not limited to these specific embodiments.

[0038] Preferably, in the normalizing step, pure dry N 2 Normalizing is performed in an atmosphere at a constant speed, i.e., the head, middle and tail ends of the steel plate are normalized at a constant roll speed.

[0039] Furthermore, in the annealing process, H 2 +N 2 Annealing is performed at a constant speed in a mixed atmosphere of the above. That is, the head, middle and tail ends of the steel sheet are annealed at a constant roll speed.

[0040] Furthermore, in said production method, the pickling process, cooling process, coating process and finishing process can be carried out by feasible techniques disclosed in the prior art, so they will not be repeated here.

[0041] As described above, compared with the prior art, the embodiments of the present invention have the following beneficial effects: (1) In the chemical composition, alloying elements such as Cu, Cr, Ni, Nb, V, and Ti are not added, and in combination with the design of the contents of elements such as Si, Al, Mn, and Sn, the magnetic performance of the non-oriented silicon steel is improved to ensure that the non-oriented silicon steel has low core loss and high magnetic flux density. At the same time, the particle size is controlled to 50 μm to 80 μm based on the chemical composition, thereby realizing refined crystal strengthening of the steel sheet and ensuring that the non-oriented silicon steel has high strength. This achieves comprehensive optimization of the magnetic performance and strength of the non-oriented silicon steel at low cost and low production difficulty, and makes the non-oriented silicon steel meet the requirements for use in the drive motors of new energy vehicles.

[0042] (2) Furthermore, by controlling a series of processes including the hot rolling process, normalizing process, single-stand cold rolling process and annealing process based on the design of the chemical composition, the recrystallized grain size of the non-oriented silicon steel can be refined, and the non-oriented silicon steel with excellent magnetic properties and high strength can be obtained. On the other hand, the cracking and fracture problem during cold rolling can be avoided, and the pre-roll preheating or secondary cold rolling commonly used in the traditional production process can be omitted, and the final rolling can be completed only through the single-stand cold rolling process without preheating, ensuring low production difficulty, low cost and stable continuity. On the other hand, the low temperature control of the heating temperature, rolling start temperature, normalizing temperature, etc. can greatly reduce the production energy consumption. Furthermore, the low normalizing temperature and short holding time can reduce the thickness of the oxide scale on the surface of the steel sheet before the pickling process, which is favorable to improving the efficiency of pickling, and can improve the surface quality and yield of the final non-oriented silicon steel.

[0043] The above detailed description is merely a specific description of the possible embodiments of the present invention, and does not define the protection scope of the present invention; all equivalent embodiments or modifications obtained without departing from the technical spirit of the present invention shall be included within the protection scope of the present invention.

[0044] Hereinafter, six embodiments of the present invention will be provided to further illustrate the technical solutions of the present invention, of course, these embodiments are only a part, not all, of the multiple variations included in the present invention.

[0045] Examples 1 to 6 each provide a non-oriented silicon steel. The chemical composition in mass% is as shown in Table 1. The non-oriented silicon steel of each example is specifically a steel plate having a thickness shown in Table 1.

[0046] [Table 1] JPEG2024540901000001.jpg122170

[0047] The non-oriented silicon steels of Examples 1 to 6 were sampled and detected. (1) The recrystallized grain size measured in the metallographic structure test is shown in Table 2. (2) The yield strength and tensile strength measured in the mechanical performance test are shown in Table 2. (3) The iron loss P measured in the magnetic performance test is shown in Table 2. 1.0 / 400 and magnetic flux density B 5000 are shown in Table 2.

[0048] [Table 2] JPEG2024540901000002.jpg55170

[0049] The non-oriented silicon steels of Examples 1 to 6 were produced in the following manner. (1) Molten iron was refined into molten steel having the chemical composition shown in Table 1. No alloying materials of Cu, Cr, Ni, Nb, V, or Ti were added during the steelmaking process. The molten steel refined using a continuous casting billet was made into a continuous casting billet with a thickness of 220 mm. The chemical composition of the continuous casting billet is also shown in Table 1. (2) The continuous cast billet obtained in step 1 was heated in a heating furnace. The heating temperature and holding time are shown in Table 3. Then, a hot rolled coil plate was obtained by rough rolling, finish rolling, and coiling in sequence. Table 3 shows the thickness of the intermediate billet obtained by rough rolling, the rolling start temperature, rolling end temperature, and total rolling reduction rate during finish rolling, the thickness of the obtained hot rolled plate, and the coiling temperature during coiling.

[0050] [Table 3] JPEG2024540901000003.jpg65170

[0051] (3) The hot-rolled coil plate obtained in step 2 is dried in pure N 2 The steel sheets were normalized in a normalizing atmosphere. The normalizing process was carried out at a constant speed. The normalizing temperature and holding time are shown in Table 4. After normalizing was completed, the metal structure of the steel sheets of each example was examined. The area ratio of the non-recrystallized structure and the recrystallized grain size measured are shown in Table 4. Here, the area ratio of the non-recrystallized structure is the ratio of the area of ​​the non-recrystallized structure to the total area of ​​the sampled cross section of the steel sheet.

[0052] [Table 4] JPEG2024540901000004.jpg55170

[0053] (4) The steel sheet obtained in step 3 was pickled, and after pickling, it was directly subjected to single-stand cold rolling without preheating. Here, five passes of rolling were performed during the single-stand cold rolling period. The total reduction was 85±3%, and the reduction of each pass except the final pass was 30% or more. The thickness of the obtained steel sheet is shown in Table 1. The reduction gauge of each pass is shown in Table 5.

[0054] [Table 5] JPEG2024540901000005.jpg67170

[0055] (5) The steel plate obtained in step 4 is H 2 +N 2 The steel sheets were annealed in a mixed atmosphere of 0.1% by weight, 1.0 ...

[0056] [Table 6] JPEG2024540901000006.jpg55170

[0057] As can be seen from the above Examples 1 to 6, the non-oriented silicon steel according to the embodiment of the present invention not only has excellent magnetic properties, but also has high strength, low alloying material costs, low production difficulty, and low production costs, which meets the requirements for application to the drive motor of new energy vehicles.

Claims

1. A non-oriented silicon steel having a thickness of 0.25 mm to 0.35 mm is prepared by sequentially carrying out steel making, continuous casting, hot rolling, normalizing, pickling, single stand cold rolling without preheating, annealing, cooling, coating and finishing; In the continuous casting process, the chemical composition of the obtained continuous cast billet is, in mass%, Si: 2.95% to 3.15%, Al: 0.75% to 0.95%, Si + 2Al: 4.6% to 4.9%, Mn: 0.5% to 0.7%, Sn: 0.03% to 0.04%, Cu≦0.03%, Cr≦0.03%, Ni≦0.03%, Cr + Ni + C. u≦0.07%, Nb≦0.004%, V≦0.004%, Ti≦0.004%, Nb+V+Ti≦0.008%, C≦0.0025%, P≦0.015%, S≦0.0015%, N≦0.004%, C+S+N≦0.007%, Mn / S≧380, Al / N≧200, with the balance being Fe and unavoidable impurities, In the hot rolling step, the continuous cast billet obtained in the continuous casting step is successively heated, rough rolled, finish rolled, and coiled to obtain a hot rolled coil plate, the rolling start temperature in the finish rolling step is 950±20°C, the rolling end temperature is 840±20°C, the total rolling reduction is 94-95%, and the coiling temperature in the coiling step is 620±20°C; A method for producing non-oriented silicon steel for new energy drive motors, characterized in that in the normalizing process, the area ratio of unrecrystallized structure is 5% to 20%.

2. 2. The method for producing non-oriented silicon steel for new energy drive motors according to claim 1, characterized in that in the hot rolling process, the continuously cast billet obtained in the continuous casting process is heated to 1080°C to 1110°C and held for 160min to 180min.

3. 2. The method for producing non-oriented silicon steel for new energy drive motors according to claim 1, wherein in the normalizing process, the normalizing temperature is 840° C. to 860° C., and is maintained for 180 s to 200 s.

4. The method for producing non-oriented silicon steel for new energy drive motors according to claim 1, characterized in that in the annealing process, the annealing temperature is 960°C to 980°C and is maintained for 40s to 45s.

5. 2. The method for producing non-oriented silicon steel for new energy drive motors according to claim 1, characterized in that in the single stand cold rolling process, multi-pass rolling is performed, the total reduction is 85±3%, and the reduction of each pass other than the final pass is 30% or more.

6. 2. The method for producing non-oriented silicon steel for new energy drive motors according to claim 1, wherein in the hot rolling process, the continuous casting billet having a thickness of 220 mm is roughly rolled into an intermediate billet having a thickness of 35 mm to 40 mm, and then the intermediate billet is finish rolled into a hot rolled plate having a thickness of 2.00 mm to 2.30 mm.

7. 7. The method for producing non-oriented silicon steel for new energy traction motors according to claim 6, wherein the non-oriented silicon steel is a steel plate having a thickness of 0.25 mm, the intermediate billet has a thickness of 35 mm, and the hot-rolled plate has a thickness of 2.00 mm; or the non-oriented silicon steel is a steel plate having a thickness of 0.30 mm, the intermediate billet has a thickness of 37.5 mm, and the hot-rolled plate has a thickness of 2.15 mm; or the non-oriented silicon steel is a steel plate having a thickness of 0.35 mm, the intermediate billet has a thickness of 40 mm, and the hot-rolled plate has a thickness of 2.30 mm.

8. 2. The method for producing non-oriented silicon steel for new energy traction motors as claimed in claim 1, characterized in that in the steelmaking process, no alloying materials such as Cu, Cr, Ni, Nb, V and Ti are added.

9. A non-oriented electrical steel for new energy drive motors, which is prepared by the production method according to claim 1.

10. 10. The method for producing non-oriented silicon steel for new energy traction motors according to claim 9, wherein the recrystallized grain size of the non-oriented silicon steel is 50 μm to 80 μm.

11. The non-oriented silicon steel has a yield strength of 460 MPa or more, a tensile strength of 550 MPa or more, and an iron loss P 1.0/400 ≦18.5W / kg, magnetic flux density B 5000 10. The method for producing non-oriented silicon steel for new energy traction motors as claimed in claim 9, wherein the hardness is ≧1.67T.

12. The non-oriented silicon steel is a steel plate having a thickness of 0.25 mm, and the iron loss P 1.0/400 ≦17.5 W / kg, or the steel plate is 0.30 mm thick, and the iron loss P 1.0/400 ≦18.0 W / kg, or a steel plate having a thickness of 0.35 mm, and iron loss P 1.0/400 12. The non-oriented electrical steel according to claim 11, characterized in that it has a strength of ≦18.5 W / kg.

Citation Information

Patent Citations

  • Cold-rolled non-oriented silicon steel strip with high magnetic induction strength for driving motor of electric vehicle and manufacturing method

    CN111206192A

  • Non-oriented electromagnetic steel sheet for motor and manufacturing method therefor

    JP2017145453A

  • Electromagnetic steel sheet

    JP2017166023A

  • Non-oriented electrical steel sheet and manufacturing method thereof

    JP2017509799A

  • Non-oriented electromagnetic steel sheet and method for producing the same

    JP2018508646A