Electrode assembly, secondary battery, battery module, battery pack, and power consuming device
A two-layer negative electrode assembly with graphite and hard carbon layers and a ferroelectric coating in secondary batteries addresses energy density and charging rate limitations, enhancing ion storage and cycle life while preventing dendrites.
Patent Information
- Application Number
- JP2024523512
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2022-07-05
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2042-07-05
AI Technical Summary
Existing secondary batteries face limitations in energy density, high-rate charging performance, and cycle life due to the inherent deficiencies of graphite and hard carbon as negative electrode active materials, with issues such as dendrite formation and inefficient ion storage.
A two-layer negative electrode design is implemented, combining graphite and hard carbon layers on the current collector, with a functional coating layer containing a ferroelectric material on the separator to control ion deposition and suppress dendrite growth, enhancing ion storage and cycle life.
The design achieves high energy density, high-rate charging capability, and extended cycle life by optimizing ion storage and preventing dendrite formation, thereby improving safety and performance.
Smart Images

Figure 2024540920000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to the technical field of batteries, and in particular to electrode assemblies, secondary batteries, battery modules, battery packs and power consuming devices. [Background technology]
[0002] In recent years, secondary batteries have been widely used in many fields, such as energy storage power systems such as hydroelectric, thermal, wind and solar power plants, as well as electric tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. With the application and popularity of secondary batteries, the requirements for the energy density, cycle performance and high-rate charging performance of secondary batteries are becoming increasingly higher, but the negative electrode active material, as an important component of secondary batteries, will affect the performance of secondary batteries to a certain extent. Graphite is one of the most commonly used negative electrode active materials in secondary batteries, and has the advantages of small polarization and high cycle stability, but its theoretical gram capacity (capacity per gram) is only 372mAh / g. At present, the performance of commercial graphite has been almost fully developed, and the space for improving its reversible gram capacity and energy density is very limited. At the same time, the layer spacing of graphite is small, and its high-rate charging performance has also been almost fully developed. Hard carbon, as a new negative electrode active material, can rapidly absorb and release active ions during the charging and discharging process of secondary batteries, and has a very broad development prospect. However, the compression density and initial coulombic efficiency of commercial hard carbon are low, limiting the improvement of the energy density of secondary batteries. Summary of the Invention
[0003] The present application aims to provide an electrode assembly, a secondary battery, a battery module, a battery pack and a power consuming device, which simultaneously combine a high charge rate and a long cycle life, provided that the secondary battery has a high energy density.
[0004] A first aspect of the present application provides an electrode assembly including a negative electrode sheet, a positive electrode sheet, and a separator located between the negative electrode sheet and the positive electrode sheet, the negative electrode sheet including a negative electrode current collector and a first negative electrode film layer and a second negative electrode film layer provided on at least one surface of the negative electrode current collector, the first negative electrode film layer being located between the negative electrode current collector and the second negative electrode film layer and including a first negative electrode active material including graphite, the second negative electrode film layer including a second negative electrode active material including hard carbon, the separator including a base film and a functional coating layer located at least on a side of the base film facing the negative electrode sheet, and the functional coating layer including a ferroelectric material.
[0005] In the electrode assembly of the present application, a first negative electrode film layer containing graphite and a second negative electrode film layer containing hard carbon are sequentially provided on the surface of the negative electrode current collector to perform a two-layer combination design, thereby compensating for the defects of graphite and hard carbon and making the advantages of each of them apparent. The large layer spacing of the hard carbon can provide a higher charging rate, and the graphite is interposed between the hard carbon and the negative electrode current collector to compensate for the initial coulombic efficiency of the hard carbon. In addition, the potential at which active ions are absorbed in the microporous structure of the hard carbon is about 0 V, which is close to the potential at which active ions are precipitated from the graphite surface, so that the function of the microporous structure of the hard carbon as a storage site for active ions cannot be fully exerted. However, the inventors of the present application have surprisingly found that the above problem can be solved by providing a functional coating layer containing a ferroelectric material at least on the side of the separator close to the second negative electrode film layer. The ferroelectric material can control the deposition method of the active ions, thereby realizing the advantage of the large capacity of the microporous structure of the hard carbon, and can also suppress the active ions from being continuously reduced and precipitated on the graphite surface, thereby improving the cycle life of the secondary battery. Therefore, the secondary battery using the electrode assembly of the present application has a long cycle life, can be charged at a high rate, has a high output voltage, and has a high energy density.
[0006] In any embodiment of the present application, the thickness of the functional coating layer is H1 μm, the thickness of the second negative electrode film layer is H2 μm, the thickness of the first negative electrode film layer is H3 μm, and the electrode assembly has H1 / (H2+H3) of 0.01-0.15, optionally 0.01-0.08, so that the comprehensive performance of the secondary battery is better and high-rate charging can be realized with high energy density.
[0007] In any embodiment of the present application, the thickness of the functional coating layer is H1 μm, H1 is 2 to 10, optionally 4 to 6. This improves the overall performance of the secondary battery, and can realize high rate charging together with high energy density.
[0008] In any embodiment of the present application, the thickness of the second negative electrode film layer is H2 μm, the thickness of the first negative electrode film layer is H3 μm, and the negative electrode sheet has an H2 / H3 ratio of 0.10 to 5, optionally 0.5 to 4. This allows the second negative electrode film layer and the first negative electrode film layer to exhibit a better synergistic effect.
[0009] In any embodiment of the present application, the volume average particle diameter Dv50 of the ferroelectric material is d1 μm, where d1 is less than or equal to 1, and optionally 0.05 to 0.8, thereby improving the overall performance of the secondary battery and realizing high-rate charging together with high energy density, while at the same time reducing production costs.
[0010] In any embodiment of the present application, the volume average particle diameter Dv50 of the second negative electrode active material is d2μm, the volume average particle diameter Dv50 of the first negative electrode active material is d3μm, and d2 / d3 is 0.1-1, optionally 0.2-0.8. In this case, it is advantageous that the second negative electrode film layer fully exerts the effect of improving the high-rate charging ability of the secondary battery, and the first negative electrode film layer fully exerts the effect of improving the initial coulombic efficiency and cycle life of the secondary battery. This improves the overall performance of the secondary battery, and can realize high-rate charging together with high energy density.
[0011] In any embodiment of the present application, the mass percentage of the ferroelectric material in the functional coating layer is W1, which is calculated based on the total mass of the functional coating layer, and W1 is 70%-95%, optionally 80%-95%, so that the overall performance of the secondary battery is better and high-rate charging can be realized with high energy density.
[0012] In any embodiment of the present application, the functional coating layer further comprises an adhesive, optionally including one or more of the following: styrene butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, fluorine-containing acrylate resin, polytetrafluoroethylene, homopolymer of vinylidene fluoride, and copolymers thereof.
[0013] In any embodiment of the present application, the separator further includes an adhesive layer provided on the surface of the functional coating layer. Optionally, the adhesive layer includes one or more combinations of a homopolymer of vinylidene fluoride and a copolymer thereof, which can improve the winding effect of the electrode assembly and extend the cycle life of the secondary battery.
[0014] In any embodiment of the present application, the dielectric constant of the ferroelectric material is 50 or more, optionally 50-100,000.
[0015] In any embodiment of the present application, the ferroelectric material includes one or more combinations selected from inorganic ferroelectric materials and organic ferroelectric materials. Optionally, the inorganic ferroelectric material includes one or more combinations selected from perovskite structure oxides, tungsten bronze type compounds, bismuth oxide type layered structure compounds, lithium niobate, lithium tantalate, lead metaniobate, and barium lithium lead niobate. The organic ferroelectric material may include one or more combinations selected from vinylidene fluoride homopolymer or copolymer, 2,5-dibromo-3,6-dihydroxy-p-benzoquinone, phenazine-chloranilic acid, and croconium.
[0016] In any embodiment of the present application, calculated based on the total mass of the second negative electrode film layer, the mass percentage of hard carbon in the second negative electrode film layer is W2, W2 is 68% or more, and optionally 90% to 98%, which is advantageous for the secondary battery to have a higher charging rate.
[0017] In any embodiment of the present application, calculated based on the total mass of the first negative electrode film layer, the mass percentage of graphite in the first negative electrode film layer is W3, W3 is 78% or more, optionally 90% to 98%, which is favorable for the secondary battery to have higher initial coulombic efficiency and longer cycle life.
[0018] In any embodiment of the present application, the volume average particle diameter Dv50 of the second negative electrode active material is d2 μm, and d2 is 3 to 11, optionally 3 to 7. This is advantageous for improving the capacity and energy density of the secondary battery.
[0019] In any embodiment of the present application, the particle size distribution index (Dv90-Dv10) / Dv50 of the second negative electrode active material is α1, which is 0.6 to 5, and optionally 1 to 4. This is advantageous for improving the high-rate charging capability and charge / discharge efficiency of the secondary battery.
[0020] In any embodiment of the present application, the specific surface area of the second negative electrode active material is 3 m 2 / g~7m 2 / g, optionally 4m 2 / g~6m 2 This is advantageous for improving the high rate charging capability of the secondary battery.
[0021] In any embodiment of the present application, the second negative electrode active material has a powder compression density of 0.9 g / cm at 20000 N. 3 ~1.3g / cm 3 and can be selected to be 1g / cm 3 ~1.2g / cm 3This is advantageous for improving the energy density of the secondary battery.
[0022] In any embodiment of the present application, the second negative electrode active material includes primary particles, secondary particles, or a combination thereof. Optionally, the quantity ratio of the primary particles in the second negative electrode active material is 90% to 100%, which is advantageous for improving the high-rate charging ability of the secondary battery.
[0023] In any embodiment of the present application, the volume average particle diameter Dv50 of the first negative electrode active material is d3 μm, and d3 is 9 to 18, optionally 11 to 15. This is advantageous in that the secondary battery has high initial coulombic efficiency, high energy density, and long cycle life.
[0024] In any embodiment of the present application, the particle size distribution index (Dv90-Dv10) / Dv50 of the first negative electrode active material is α2, which is 0.2 to 5, and optionally 0.3 to 4. This is advantageous for improving the cycle performance of the secondary battery.
[0025] In any embodiment of the present application, the specific surface area of the first negative electrode active material is 0.6 m 2 / g~1.5m 2 / g, optionally 0.8m 2 / g~1.4m 2 This is advantageous for improving the cycle performance of the secondary battery.
[0026] In any embodiment of the present application, the first negative electrode active material has a powder compression density of 1.4 g / cm at 20000 N. 3 ~1.85g / cm 3 and optionally 1.6g / cm 3 ~1.75g / cm 3 This is advantageous for improving the energy density of the secondary battery.
[0027] In any embodiment of the present application, the graphitization degree of the first negative electrode active material is 91% to 95%, and optionally 92% to 94%, which is advantageous for improving the cycle performance of the secondary battery.
[0028] In any embodiment of the present application, the first negative electrode active material includes artificial graphite, natural graphite, or a combination thereof, and optionally, the surface of the artificial graphite has a carbon coating layer, which is advantageous for improving the cycle performance and high-rate charging ability of the secondary battery.
[0029] In any embodiment of the present application, the first negative electrode active material includes primary particles, secondary particles, or a combination thereof, and optionally, the quantity ratio of the secondary particles in the first negative electrode active material is 90% to 100%, which is advantageous for improving the cycle performance, storage performance, and high-rate charging ability of the secondary battery.
[0030] A second aspect of the present application provides a secondary battery including the electrode assembly of the first aspect of the present application.
[0031] A third aspect of the present application provides a battery module including the secondary battery of the second aspect of the present application.
[0032] A fourth aspect of the present application provides a battery pack including one of the secondary battery of the second aspect of the present application and the battery module of the third aspect.
[0033] A fifth aspect of the present application provides a power consuming device including at least one of the secondary battery of the second aspect of the present application, the battery module of the third aspect, and the battery pack of the fourth aspect.
[0034] The secondary battery using the electrode assembly of the present application has a long cycle life, can be charged at a high rate, has a high output voltage, and has a high energy density. The battery module, battery pack, and power consuming device of the present application include the secondary battery of the present application, and therefore have at least the same advantages as the secondary battery. [Brief description of the drawings]
[0035] In order to more clearly describe the technical solutions of the embodiments of the present application, the drawings necessary for the embodiments of the present application are briefly described below. It is clear that the drawings described below are only some embodiments of the present application. Those skilled in the art can further obtain other drawings based on the drawings even without creative labor.
[0036] [Figure 1] FIG. 1 is a schematic diagram of one embodiment of an electrode assembly of the present application.
[0037] [Diagram 2] FIG. 2 is a schematic diagram of another embodiment of an electrode assembly of the present application.
[0038] [Diagram 3] FIG. 1 is a schematic diagram of an embodiment of a secondary battery of the present application.
[0039] [Figure 4] 4 is an exploded schematic view of the embodiment of the secondary battery of FIG. 3.
[0040] [Diagram 5] FIG. 1 is a schematic diagram of one embodiment of a battery module of the present application.
[0041] [Figure 6] FIG. 1 is a schematic diagram of one embodiment of a battery pack of the present application.
[0042] [Figure 7] 7 is an exploded schematic view of the embodiment of the battery pack shown in FIG. 6.
[0043] [Figure 8] 1 is a schematic diagram of an embodiment of a power consuming device including a secondary battery of the present application as a power source.
[0044] In the drawings, the drawings are not necessarily drawn to actual size. Explanation of symbols 1 battery pack, 2 upper case, 3 lower case, 4 battery module, 5 secondary battery, 51 housing, 52 electrode assembly, 53 cover plate, 6 electrode assembly, 10 negative electrode sheet, 100 negative electrode current collector, 101 first negative electrode film layer, 102 second negative electrode film layer, 20 positive electrode sheet, 200 positive electrode current collector, 201 positive electrode film layer, 30 separator, 300 base film, 301 functional coating layer, 302 adhesive layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045] Hereinafter, embodiments specifically disclosing the electrode assembly, secondary battery, battery module, battery pack, and power consumption device of the present application will be described in detail with appropriate reference to the drawings. However, unnecessary detailed description may be omitted. For example, detailed description of known matters or duplicate description of substantially the same configuration may be omitted. This is to avoid the following description from becoming unnecessarily redundant and to facilitate understanding by those skilled in the art. Note that the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0046] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such defined ranges may be inclusive or exclusive of the end values, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, when ranges of 60-120 and 80-110 are recited for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also contemplated. Also, when minimum range values 1 and 2 and maximum range values 3, 4 and 5 are recited, ranges of 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5 may all be contemplated. In this application, unless otherwise stated, the numerical range "a-b" is an abbreviation indicating any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0-5" refers to all real numbers between "0-5" throughout this specification, with "0-5" being an abbreviation for combinations of these numerical values. Furthermore, expressing a parameter as an integer greater than or equal to 2 (≧2) is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0047] Unless otherwise specified, all the embodiments and optional embodiments of the present application may be combined with each other to form a new technical solution, and such technical solution is considered to be included in the disclosure content of the present application.
[0048] Unless otherwise specified, all the embodiments and optional embodiments of the present application may be combined with each other to form a new technical solution, and such technical solution is considered to be included in the disclosure content of the present application.
[0049] Unless otherwise stated, all steps in this application may be performed in sequence or randomly, but are preferably performed in sequence. For example, the method includes steps (a) and (b) and may include steps (a) and (b) performed in sequence, or may include steps (b) and (a) performed in sequence. For example, when it is stated that the method may further include step (c), it means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.
[0050] Unless otherwise specified, the terms "comprise" and "include" used in this application mean open-ended and may also be closed-ended. For example, the terms "comprise" and "include" can mean "comprise" or "include" other components not listed, or "comprise" or "include" only the listed components.
[0051] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, any of the following conditions are met: A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), or both A and B are true (or exist).
[0052] In this application, the terms "plurality" and "multiple types" mean two or more than two types.
[0053] In this application, the terms "primary particle" and "secondary particle" have the meanings well known in the art. A primary particle refers to a particle that is not in an aggregated state, and a secondary particle refers to a particle in an aggregated state in which two or more primary particles are aggregated. Primary particles and secondary particles can be easily distinguished from each other by taking SEM images using a scanning electron microscope.
[0054] Hard carbon is carbon that is difficult to graphitize, and is difficult to graphitize even at high temperatures of 2500°C or higher. Hard carbon is usually obtained by pyrolyzing a precursor such as a polymer. In the pyrolysis process, the structure in which carbon atoms in the precursor are cross-linked with each other inhibits the growth of the carbon layer in the planar direction, so that the hard carbon structure contains many crystallites of a disordered pseudo-graphite structure (abbreviated as graphite crystallites). Hard carbon has a complex structure, and in addition to graphite crystallites, it contains defect structures (e.g., surface defects, lattice defects, etc.) and microporous structures (e.g., open hole structures, closed hole structures, etc.). Therefore, active ions are absorbed and released from various angles of hard carbon, which allows secondary batteries to have excellent high-rate charging capabilities, and hard carbon has unique advantages, especially in the field of power batteries. Compared with graphite, the interplanar spacing of the crystal plane of hard carbon (002) is larger, so that the structural stability of hard carbon is higher during charging and discharging, and no obvious volume expansion and contraction effects occur.
[0055] Hard carbon has many defect structures, which catalyze the decomposition of the electrolyte to form a thick solid electrolyte interface (SEI) film, which increases the irreversible loss of active ions. In addition, hard carbon has a sparse porous structure on the surface, which easily adsorbs moisture and oxygen gas in the air to form various CH functional groups on the surface. These functional groups react with active ions, further increasing the irreversible loss of active ions. Therefore, compared with graphite, hard carbon has a low initial coulombic efficiency and poor cycle performance, for example, the initial coulombic efficiency is usually less than 80%, and the advantage of its high capacity cannot be fully exerted.
[0056] Through extensive research, the inventors of the present application have proposed an electrode assembly that can improve the capacity of hard carbon and, on the premise of providing a high energy density to a secondary battery, can further improve the high-rate charging capability and cycle life. Electrode Assembly
[0057] Specifically, the electrode assembly of the present application includes a negative electrode sheet, a positive electrode sheet, and a separator located between the negative electrode sheet and the positive electrode sheet, the negative electrode sheet includes a negative electrode current collector, and a first negative electrode film layer and a second negative electrode film layer provided on at least one surface of the negative electrode current collector, the first negative electrode film layer is located between the negative electrode current collector and the second negative electrode film layer, and includes a first negative electrode active material including graphite, the second negative electrode film layer includes a second negative electrode active material including hard carbon, the separator includes a base film and a functional coating layer located at least on a side of the base film facing the negative electrode sheet, the functional coating layer includes a ferroelectric material. In some embodiments, the positive electrode sheet, the separator, and the negative electrode sheet can be manufactured into an electrode assembly by a winding process and / or a stacking process.
[0058] Graphite has the advantages of high initial coulombic efficiency and high cycle stability, but poor continuous charging performance at high rates. Hard carbon has the advantages of high active ion absorption and release rate, so it has excellent charging ability at high rates, but its initial coulombic efficiency is low and capacity decay is fast, so the actual capacity of the secondary battery is poor. The inventors of the present application found in the actual investigation process that the defects of graphite and hard carbon can be compensated for by sequentially providing graphite and hard carbon on the surface of the negative electrode current collector to perform a two-layer combination design. By providing graphite close to the negative electrode current collector, the initial coulombic efficiency of hard carbon can be compensated for, and by providing hard carbon away from the negative electrode current collector, more active ions can be absorbed into the negative electrode more quickly, so that the poor performance of graphite during continuous charging at high rates can be avoided.
[0059] However, in the course of further research, the inventors of the present application found that when a two-layer combination is formed by sequentially providing graphite and hard carbon on the surface of the negative electrode current collector, the effect of improving the high-rate charge capacity and energy density of the secondary battery is not favorable. As a result of intensive research, the inventors found that the formation of "dendrites" during charging of the secondary battery, especially at the end of charging, is a possible factor that affects the improvement of the high-rate charge capacity and energy density of the secondary battery.
[0060] During the charging process of the secondary battery, if the negative electrode active ion storage space is insufficient, the resistance of the active ion to be stored in the negative electrode is too large, and the active ion is rapidly released from the positive electrode but is not stored in the negative electrode in equal amounts, the active ion that is not stored in the negative electrode can only obtain electrons from the surface of the negative electrode and precipitate as a metal element, that is, form "dendrites". Therefore, the higher the charging rate of the secondary battery, the more serious the problem of "dendrites". The formation of dendrites not only reduces the performance of the secondary battery, for example, shortening the cycle life, and in serious cases, it may form sharp topography to pierce the separator and cause a short circuit inside the battery, which may result in combustion, explosion, and other consequences, thereby increasing the safety risk of the secondary battery. In addition, the dendrites that continue to accumulate fall off from the surface of the negative electrode and are no longer in electrical contact with the negative electrode current collector, so they cannot continue to participate in the charge and discharge reaction and cannot contribute to the capacity, thereby reducing the energy density of the secondary battery.
[0061] After the graphite and hard carbon are sequentially placed on the surface of the negative electrode current collector to form a two-layer combination, in the initial charging stage of the secondary battery, the active ions are first adsorbed at the positions of the surface defects and lattice defects of the hard carbon, and this process corresponds to the "high potential slope region" in the charge / discharge curve of the hard carbon, and at this time, the negative electrode potential is generally -2V to -0.1V. As charging continues, the active ions are absorbed between the layers of the graphite crystallites of the hard carbon, and a behavior similar to the absorption of graphite occurs, and this process corresponds to the "low potential plateau region" in the charge / discharge curve of the hard carbon, and at this time, the negative electrode potential is generally -0.1V to 0V. Since the hard carbon has a more abundant microporous structure, when the negative electrode potential drops to about 0V during the second charging, the active ions are further stored in the microporous structure of the hard carbon, providing extra active ion storage sites, thereby improving the capacity and initial coulombic efficiency of the hard carbon. The longer the discharge plateau in the low potential plateau region, the higher the reversible capacity of the corresponding hard carbon, and the better the capacity is exhibited. However, the potential of the low potential plateau region of hard carbon is close to the potential of dendrite formation on the graphite surface layer, both of which are about 0V, so that in order to prevent the formation of dendrites, the capacity of the low potential plateau region of hard carbon is limited, and the function of the microporous structure of hard carbon as a storage site for active ions cannot be fully exhibited. At the same time, in order to prevent the formation of dendrites, the cutoff voltage of the negative electrode is generally set high, which reduces the output voltage of the entire secondary battery and further reduces the energy density of the secondary battery. Therefore, after the graphite and hard carbon are sequentially provided on the surface of the negative electrode current collector to perform the two-layer combination, the effect of improving the high-rate charging ability, energy density and / or cycle life of the secondary battery is limited.
[0062] The electrode assembly of the present application is designed by sequentially providing a first negative electrode film layer containing graphite and a second negative electrode film layer containing hard carbon on the surface of a negative electrode current collector, and a functional coating layer containing a ferroelectric material is further provided on the separator near the second negative electrode film layer. The ferroelectric material has a spontaneous polarization phenomenon, and when electrons accumulate on the surface of the dendrite, the ferroelectric material is spontaneously polarized under the influence of the electric field, and the center of the positive charge of the ferroelectric material moves to the electron accumulation region and wraps the electron accumulation region, and at the same time, the center of the positive charge of the ferroelectric material becomes positively charged, which repels the polarity of the positively charged active ions on the surface of the dendrite, balances the electron density, and reduces the abundance of active ions, thereby suppressing the dendrite from continuing to grow in a direction perpendicular to the electrode sheet.
[0063] Therefore, in the electrode assembly of the present application, a first negative electrode film layer containing graphite and a second negative electrode film layer containing hard carbon are sequentially provided on the surface of the negative electrode current collector to perform a two-layer combination design, thereby compensating for the defects of graphite and hard carbon and making the advantages of each of them apparent. Since the hard carbon has a large layer spacing, a higher charging rate can be provided, and since graphite is interposed between the hard carbon and the negative electrode current collector, the initial coulombic efficiency of the hard carbon can be compensated for. In addition, the potential at which active ions are absorbed in the microporous structure of the hard carbon is about 0 V, which is close to the potential at which active ions are precipitated on the surface of the graphite, so that the function of the microporous structure of the hard carbon as a storage site for active ions cannot be fully exerted. However, the inventors of the present application have surprisingly found that the above problem can be solved by providing a functional coating layer containing a ferroelectric material at least on the side of the separator close to the second negative electrode film layer. The ferroelectric material can control the deposition method of the active ions, thereby realizing the large capacity advantage of the microporous structure of the hard carbon, and also suppressing the continuous reduction and precipitation of the active ions on the graphite surface, thereby improving the cycle life of the secondary battery.
[0064] Specifically, in the early stage of charging the secondary battery, the active ions are rapidly adsorbed on the surface defects and lattice defects of the hard carbon, so that the negative electrode sheet has high dynamic performance, and in the later stage of charging the secondary battery, the overvoltage can be precisely controlled under the action of the functional coating layer, allowing a large amount of active ions to be stored in the microporous structure of the hard carbon, increasing the length of the low potential plateau region, and increasing the reversible capacity of the secondary battery, thereby improving the high rate charging ability and energy density of the secondary battery. In addition, the overvoltage generates a reverse electric field in the functional coating layer, reducing the abundance of active ions and inhibiting the dendrites from continuing to grow in a direction perpendicular to the electrode sheet, thereby improving the safety and cycle performance of the secondary battery.
[0065] In addition, in the electrode assembly of the present application, the functional coating layer is provided on the surface of the separator, which is advantageous for the secondary battery to have better overall performance without increasing extra production steps, damaging the negative electrode sheet, and not affecting the processing performance of the negative electrode sheet. The functional coating layer is provided on the surface of the separator, which further improves the heat resistance of the separator and reduces the thermal shrinkage rate of the separator, thereby contributing to improving the safety performance of the secondary battery, especially the thermal safety performance.
[0066] Therefore, a secondary battery using the electrode assembly of the present application has a long cycle life, and can be charged at a high rate, has a high output voltage, and further has a high energy density. [Separator]
[0067] The separator of the present application includes a base film and a functional coating layer located at least on the side of the base film facing the negative electrode sheet. The base film has two surfaces facing each other in its thickness direction, and the functional coating layer may be provided on both sides of the base film, or may be provided only on the surface of the base film facing the negative electrode sheet, or optionally, the functional coating layer may be provided on both surfaces of the base film.
[0068] The type of the base film of the present application is not particularly limited, and any well-known porous structure film having good chemical stability and mechanical stability can be selected. In some embodiments, the material of the base film may include one or more combinations selected from glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The base film may be a single-layer film or a multi-layer composite film. When the base film is a multi-layer composite film, the materials of each layer may be the same or different.
[0069] In some embodiments, the thickness of the base film may be 7 μm to 12 μm, but the present application is not limited thereto.
[0070] The functional coating layer includes a ferroelectric material. In some embodiments, the dielectric constant of the ferroelectric material is optionally greater than or equal to 50. The higher the dielectric constant of the ferroelectric material, the higher the effect of suppressing the continued growth of dendrites in a direction perpendicular to the electrode sheet, but the effect does not always continue to increase. At the same time, the higher the dielectric constant, the higher the requirements for the manufacturing process of the ferroelectric material, which increases the production cost. In some embodiments, the dielectric constant of the ferroelectric material may optionally be 50 to 100,000, for example, 50 to 50,000, 50 to 25,000, 50 to 10,000, 50 to 5,000, 50 to 4,000, 50 to 3,000, 50 to 2,000, 100 to 100,000, 100 to 50,000, 100 to 2,500. It may be 0, 100 to 10,000, 100 to 5,000, 100 to 4,000, 100 to 3,000, 100 to 2,000, 200 to 100,000, 200 to 50,000, 200 to 25,000, 200 to 10,000, 200 to 5,000, 200 to 4,000, 200 to 3,000, 200 to 2,000, or 200 to 1,000.
[0071] In this application, the dielectric constant of a ferroelectric material refers to the dielectric constant at room temperature (25±5°C), which has a meaning well known in the art, and can be tested by devices and methods well known in the art. For example, after the ferroelectric material is made into a circular sample, the capacitance C can be tested using an LCR meter, and the dielectric constant ε can be calculated according to the formula: ε = (C × d) / (ε0 × A) C is the capacitance and is in Farads (F), d is the thickness of the sample and is in cm, and A is the area of the sample and is in cm 2 where ε0 is the vacuum permittivity and ε0=8.854×10 -14 F / cm. In this application, the test conditions may be 1KHz, 1.0V, 25±5℃. The test standard may conform to GB / T 11297.11-2015. The sample preparation may refer to Chinese patent application CN114217139A.
[0072] In some embodiments, the ferroelectric material may include one or a combination of inorganic ferroelectric materials, organic ferroelectric materials, or optionally, inorganic ferroelectric materials.
[0073] In some embodiments, the inorganic ferroelectric material may optionally include one or more selected from perovskite-structure oxides, tungsten bronze-type compounds, bismuth oxide-type layered structure compounds, lithium niobate (LiNbO3), lithium tantalate (LiTaO3), lead metaniobate, and barium lithium lead niobate. Optionally, the inorganic ferroelectric material is selected from perovskite-structure oxides.
[0074] Optionally, the molecular formula of the perovskite oxide is Ba 1-x A x Ti 1-y B yIt is O3. A may contain one or a combination of multiple types selected from Pb, Sr, Ca, K, Na, and Cd, B may contain one or a combination of multiple types selected from Sn, Hf, Zr, Ce, Nb, and Th, and 0 ≦ x ≦ 1, 0 ≦ y ≦ 1. For example, the perovskite-structured oxide may be BaTiO3, Ba 1-x1 Sr x1 TiO3 (0 ≦ x1 ≦ 1), SrTiO3, PbTiO3, PbZr y1 Ti 1-y1 O3 (0 ≦ y1 ≦ 1), BaZr y2 Ti 1-y2 O3 (0 < y2 < 1), KNbO3, NaNbO3, or a combination of one or more types selected therefrom.
[0075] Optionally, the molecular formula of the tungsten bronze-type compound is M z WO3. M may contain one or a combination of multiple types selected from Na, K, Rb, and Cs, and 0 < z < 1. For example, the tungsten bronze-type compound may be Na z1 WO3 (0 < z1 < 1), K z2 WO3 (0 < z2 < 1), or a combination of one or more types selected therefrom.
[0076] Optionally, the molecular formula of the bismuth oxide-type layered structure compound is (Bi2O2)(C n-1 D n O 3n+1 ). C may contain one or a combination of multiple types selected from Na, K, Ba, Sr, Pb, Ca, Ln, and Bi, D may contain one or a combination of multiple types selected from Zr, Cr, Nb, Ta, Mo, W, Fe, Ti, and V, and 2 ≦ n ≦ 5. For example, the bismuth oxide-type layered structure compound may be SrBi2Nb2O9, SrBi2Ta2O9, SrBi2Nb2O9, Bi4Ti3O 12 or a combination of one or more types thereof.
[0077] In some embodiments, the organic ferroelectric material may include one or more combinations selected from the following: homopolymer or copolymer of vinylidene fluoride, 2,5-dibromo-3,6-dihydroxy-p-benzoquinone, phenazine-chloranilic acid, and croconium.
[0078] In some embodiments, the ferroelectric material has a volume average particle size Dv50 of d1 μm, where d1 is 1 or less, e.g., 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, etc. Optionally, d1 may be 0.01-1, 0.02-1, 0.03-1, 0.04-1, 0.05-1, 0.06-1, 0.07-1, 0.08-1, 0.01-0.8, 0.02-0.8, 0.03-0.8, 0.04-0.8, 0.05-0.8, 0.06-0.8, 0.07-0.8, 0.08-0.8, 0.09-0.8, or 0.1-0.8.
[0079] When the Dv50 of the ferroelectric material is within an appropriate range, the overall performance of the secondary battery is improved, and high energy density and high rate charging can be realized, while the production cost can be reduced. In addition, when the Dv50 of the ferroelectric material is large, the interference of the reverse electric field caused by it is large, and it may not perform the function of balancing the electron density and the function of suppressing the dendrite from continuing to grow in the direction perpendicular to the electrode sheet, so that when the output voltage of the secondary battery is increased to improve the energy density, the safety risk of the secondary battery increases, and when the output voltage of the secondary battery is reduced to reduce the safety risk of the secondary battery, the function of the microporous structure of the hard carbon as a storage site for active ions cannot be fully exerted, and when the Dv50 of the ferroelectric material is small, the manufacturing process becomes complicated and the production cost increases.
[0080] In some embodiments, the thickness of the functional coating layer is H1 μm, the thickness of the second negative electrode film layer is H2 μm, the thickness of the first negative electrode film layer is H3 μm, and the electrode assembly has a thickness H1 / (H2+H3) of 0.01 to 0.15, optionally 0.01 to 0.08.
[0081] Through intensive research, the inventors have found that when the thickness H1 μm of the functional coating layer, the thickness H2 μm of the second negative electrode film layer, and the thickness H3 μm of the first negative electrode film layer satisfy H1 / (H2+H3) being in the range of 0.01 to 0.15, the overall performance of the secondary battery is improved and charging at a high rate with a high energy density can be realized. In addition, when the thickness of the functional coating layer is low and the total thickness of the first negative electrode film layer and the second negative electrode film layer is high, the strength of the reverse electric field by the functional coating layer may be insufficient, and the function of balancing the electron density and the function of suppressing the dendrite from continuing to grow in the direction perpendicular to the electrode sheet may not be achieved. This may increase the safety risk of the secondary battery when increasing the output voltage of the secondary battery to improve the energy density. When the output voltage of the secondary battery is reduced to reduce the safety risk of the secondary battery, the function of the microporous structure of the hard carbon as the storage site of active ions cannot be fully achieved. When the thickness of the functional coating layer is high and the total thickness of the first negative electrode film layer and the second negative electrode film layer is low, the functional coating layer does not have electrochemical activity and cannot contribute to capacity, so it occupies a lot of volume space and mass parts, which can effectively avoid the effect on the energy density of the secondary battery.
[0082] In some embodiments, the thickness of the functional coating layer is H1 μm, H1 being 2-10, optionally 4-6. When the thickness of the functional coating layer is within a suitable range, the overall performance of the secondary battery is better, and high energy density and high rate charging can be realized. In addition, when the functional coating layer is thin, the strength of the reverse electric field generated thereby may be insufficient, and the function of balancing the electron density and the function of suppressing the dendrite from continuing to grow in a direction perpendicular to the electrode sheet may not be achieved, which may increase the safety risk of the secondary battery when increasing the output voltage of the secondary battery to improve the energy density, and when the output voltage of the secondary battery is reduced to reduce the safety risk of the secondary battery, the function of the microporous structure of the hard carbon as a storage site for active ions cannot be fully achieved, and when the functional coating layer is thick, it does not have electrochemical activity and cannot contribute to the capacity, so it occupies a lot of volume space and mass parts, which can effectively avoid affecting the energy density of the secondary battery.
[0083] In some embodiments, the mass percentage of the ferroelectric material in the functional coating layer is W1, calculated based on the total mass of the functional coating layer, W1 being 70% to 95%, optionally 80% to 95%.
[0084] The inventors have found through intensive research that when the content of the ferroelectric material is within an appropriate range, the overall performance of the secondary battery is better, and high energy density and high rate charging can be achieved. In addition, when the content of the ferroelectric material is low, the strength of the reverse electric field generated thereby may not be sufficient, and the function of balancing the electron density and the function of suppressing the dendrite from continuing to grow in a direction perpendicular to the electrode sheet may not be achieved, which may increase the safety risk of the secondary battery when increasing the output voltage of the secondary battery to improve the energy density, and when the output voltage of the secondary battery is reduced to reduce the safety risk of the secondary battery, the function of the microporous structure of the hard carbon as an active ion storage site cannot be fully achieved, and when the content of the ferroelectric material is high, other components (for example, the content of the adhesive) in the functional coating layer are reduced, which effectively avoids the functional coating layer becoming poorly bonded to the base film and easily falling off from the base film.
[0085] In some embodiments, the functional coating layer may further include an adhesive to bond the ferroelectric materials together and to bond the functional coating layer to the second negative electrode film layer of the negative electrode sheet, thereby improving the winding effect of the electrode assembly and extending the cycle life of the secondary battery. In some embodiments, the adhesive may optionally include one or more of styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMA), carboxymethyl chitosan (CMCS), fluorine-containing acrylate resin, polytetrafluoroethylene (PTFE), homopolymer of vinylidene fluoride, and copolymer thereof. For example, the vinylidene fluoride copolymer may include one or a combination of a plurality of copolymers selected from vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-tetrafluoroethylene-propylene ternary copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternary copolymer.
[0086] In some embodiments, the functional coating layer may further include other auxiliary agents. For example, the other auxiliary agents may include a dispersing agent, such as sodium carboxymethylcellulose (CMC).
[0087] In some embodiments, the separator may further include an adhesive layer provided on the surface of the functional coating layer, which can further improve the winding effect of the electrode assembly and extend the cycle life of the secondary battery. Optionally, the adhesive layer includes one or more combinations of vinylidene fluoride homopolymers and copolymers thereof. Thus, the adhesive layer can have a certain dielectric constant in addition to the adhesive function. This can better suppress the dendrites from continuing to grow in a direction perpendicular to the electrode sheet. For example, the vinylidene fluoride copolymer may include one or more combinations selected from vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-tetrafluoroethylene-propylene ternary copolymer, and vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternary copolymer. Optionally, the adhesive layer has a thickness of 1 μm or less.
[0088] The method for manufacturing the separator of the present application is well known. In some embodiments, the separator can be manufactured by dispersing the ferroelectric material, the adhesive, and any other components in a solvent to form a slurry, applying the slurry to at least one surface of the base film, and drying, i.e., obtaining a separator. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water. In some embodiments, the method for manufacturing the separator may further include applying a slurry to form an adhesive layer on the surface of the functional coating layer.
[0089] In addition, the parameters of the functional coating layer in this application refer to the parameter range of the functional coating layer on one side of the base film. When the functional coating layer is provided on both sides of the base film, if the parameters of the functional coating layer on either one of the surfaces satisfy the parameters of this application, it is considered to be within the protection scope of this application.
[0090] The thickness of the functional coating layer of the separator is a well-known meaning in the art and can be measured by instruments and methods well-known in the art. For example, a scanning electron microscope (e.g., ZEISS Sigma 300) test can be performed to more accurately determine the boundary area between the functional coating layer and the base film. The test standard can refer to JY / T010-1996. In order to ensure the accuracy of the test results, multiple (e.g., 5 or more) different areas in the test sample can be randomly selected to perform a scan test, and the respective thicknesses of the functional coating layer and the base film in the scale test area can be read at a certain magnification (e.g., 500 times or more). For the accuracy of the test, multiple test areas can be taken and tested, and the average value can be taken. [Negative electrode sheet]
[0091] In some embodiments, the second negative electrode film layer has a thickness H2 μm, the first negative electrode film layer has a thickness H3 μm, and the negative electrode sheet has a H2 / H3 ratio of 0.10 to 5, optionally 0.5 to 4.
[0092] The inventors have found through intensive research that when the ratio of the thickness H2μm of the second negative electrode film layer to the thickness H3μm of the first negative electrode film layer is within a suitable range, the second negative electrode film layer and the first negative electrode film layer can achieve a better synergistic effect. The second negative electrode film layer mainly bears the pressure of high-rate charging, ensuring that the secondary battery has a high charging rate, while the first negative electrode film layer mainly provides a long cycle life and at the same time ensures a high initial coulombic efficiency, which improves the overall performance of the secondary battery and can realize high-rate charging with high energy density. In addition, when the second negative electrode layer is thin and the first negative electrode layer is thick, the high-rate charging pressure borne by the hard carbon in the second negative electrode layer during charging is relatively small, and in this case, the graphite in the first negative electrode layer still plays a leading role, so the effect of improving the charging rate of secondary battery is not obvious; and when the second negative electrode layer is thick and the first negative electrode layer is thin, the hard carbon surface contains a large amount of inactive functional groups, so the irreversible consumption of active ions increases, which affects the initial coulombic efficiency of secondary battery and may also reduce the cycle life of secondary battery.
[0093] In some embodiments, the thickness of the second negative electrode film layer is H2 μm, and H2 is 10-120 μm, optionally 35-110 μm, and more preferably 40-100 μm. When the thickness of the second negative electrode film layer is within a suitable range, it is advantageous for the secondary battery to have a high charging rate.
[0094] In some embodiments, the thickness of the first negative electrode film layer is H3 μm, and H3 is 20-100, optionally 25-70, more preferably 28-60. When the thickness of the first negative electrode film layer is within a suitable range, it is advantageous for the secondary battery to have high initial coulombic efficiency and long cycle life.
[0095] The second negative electrode film layer includes a second negative electrode active material, and the second negative electrode active material includes hard carbon. Optionally, the mass percentage of the hard carbon in the second negative electrode active material is 70% to 100%, and optionally 80% to 98%, calculated based on the total mass of the second negative electrode active material. This is advantageous in that the second negative electrode film layer includes a large amount of hard carbon, and the secondary battery has a higher charge rate. In some embodiments, the second negative electrode active material may include only hard carbon, and in other embodiments, the second negative electrode active material may further include other negative electrode active materials, such as graphite, soft carbon, mesocarbon microbeads, silicon-based materials, and tin-based materials, in addition to hard carbon, and optionally, the mass percentage of the other negative electrode active materials in the second negative electrode active material is 30% or less, and more preferably 20% or less, calculated based on the total mass of the second negative electrode active material.
[0096] In some embodiments, the mass percentage of hard carbon in the second negative electrode film layer is W2, W2 is 68% or more, optionally 90%-98%, calculated based on the total mass of the second negative electrode film layer. When the content of hard carbon is within a suitable range, it is advantageous for the secondary battery to have a higher charge rate.
[0097] In some embodiments, the second negative electrode film layer may further include a conductive agent, which plays a role of collecting microcurrent between the second negative electrode active material (e.g., hard carbon), reducing the contact resistance of the electrode, accelerating the electron transfer rate, and at the same time, reducing polarization, and improving the charge and discharge efficiency of the secondary battery. For example, the conductive agent may include one or more combinations selected from superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the conductive agent is 5% or less, calculated based on the total mass of the second negative electrode film layer.
[0098] In some embodiments, the second negative electrode film layer may further include an adhesive to bond the second negative electrode active material (e.g., hard carbon) to each other and to bond the second negative electrode film layer to the first negative electrode film layer. For example, the adhesive may include one or more combinations selected from styrene butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-soluble acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PSMA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the binder is 5% or less, calculated based on the total mass of the second negative electrode film layer.
[0099] In some embodiments, the second negative electrode film layer may further include other additives. For example, the other additives may include thickeners such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, etc. In some embodiments, calculated based on the total mass of the second negative electrode film layer, the mass percentage of the other additives is 2% or less.
[0100] The first negative electrode film layer includes a first negative electrode active material including graphite. Optionally, the mass percentage of the graphite in the first negative electrode active material is 80% to 100%, and optionally 90% to 98%, calculated based on the total mass of the first negative electrode active material. This is advantageous in that the first negative electrode film layer includes a large amount of graphite, and the secondary battery has a higher initial coulombic efficiency and a longer cycle life. In some embodiments, the first negative electrode active material may include only graphite, and in other embodiments, the first negative electrode active material may further include other negative electrode active materials other than graphite, such as hard carbon, soft carbon, mesocarbon microbeads, silicon-based materials, and tin-based materials, and optionally, the mass percentage of the other negative electrode active materials in the first negative electrode active material is 20% or less, and more preferably 10% or less, calculated based on the total mass of the first negative electrode active material.
[0101] In some embodiments, the mass percentage of graphite in the first negative electrode film layer is W3, calculated based on the total mass of the first negative electrode film layer, and W3 is 78% or more, optionally 90% to 98%. When the graphite content is within a suitable range, it is advantageous for the secondary battery to have higher initial coulombic efficiency and longer cycle life.
[0102] In some embodiments, the first negative electrode film layer may further include a conductive agent, which serves to collect microcurrent between the first negative electrode active material (e.g., graphite), reduce the contact resistance of the electrode, accelerate the electron transfer rate, and at the same time, reduce polarization, thereby improving the charge and discharge efficiency of the secondary battery. For example, the conductive agent may include one or more combinations selected from superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, the mass percentage of the conductive agent is 5% or less, calculated based on the total mass of the first negative electrode film layer.
[0103] In some embodiments, the first negative electrode film layer may further include an adhesive to bond the first negative electrode active material (e.g., graphite) to each other, to bond the first negative electrode film layer to the second negative electrode film layer, and to bond the first negative electrode film layer to the negative electrode current collector. For example, the adhesive may include one or more combinations selected from styrene butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-soluble acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PSMA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS). In some embodiments, the mass percentage of the binder is 5% or less, calculated based on the total mass of the first negative electrode film layer.
[0104] In some embodiments, the first negative electrode film layer may further include other additives. For example, the other additives may include thickeners such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, etc. In some embodiments, the mass percentage of the other additives is 2% or less, calculated based on the total mass of the first negative electrode film layer.
[0105] In some embodiments, the second negative electrode active material has a volume average particle diameter Dv50 of d2 μm, the first negative electrode active material has a volume average particle diameter Dv50 of d3 μm, and d2 / d3 is 0.1 to 1, optionally 0.2 to 0.8.
[0106] In the negative electrode sheet of the present application, the first negative electrode film layer adopts the first negative electrode active material with a large particle size, so that the first negative electrode film layer has a higher compression density, which is favorable for the secondary battery to have a high initial coulombic efficiency, a high energy density and a long cycle life.In the negative electrode sheet of the present application, the second negative electrode film layer adopts the second negative electrode active material with a small particle size, so that its specific surface area is high, which can increase the contact area with the electrolyte and shorten the liquid phase diffusion path and solid phase diffusion path of active ions, and at the same time, the integrity of the tunnel structure of the second negative electrode film layer is better maintained, which is favorable for the secondary battery to have a higher charging rate. In addition, the second negative electrode active material has a small particle size and a high pressure resistance, so that the microporous structure of the second negative electrode active material, especially the hard carbon, can be better maintained, so that the microporous structure of the hard carbon can fully exert its function as an active ion storage site, and the capacity and energy density of the secondary battery can be improved. At the same time, the second negative electrode film layer has a low compression density, so that the electrolyte can quickly infiltrate into the first negative electrode film layer, which is advantageous for reducing the polarization of the negative electrode and improving the charge and discharge efficiency of the secondary battery.
[0107] Through further research, the inventors have found that when the ratio d2 / d3 of the particle size of the second negative electrode active material to the particle size of the first negative electrode active material is within an appropriate range, it is favorable for the second negative electrode film layer to fully exert the effect of improving the high-rate charging ability of the secondary battery and the effect of the first negative electrode film layer to improve the initial Coulombic efficiency and cycle life of the secondary battery, thereby improving the overall performance of the secondary battery and realizing high-rate charging together with high energy density.
[0108] In some embodiments, the volume average particle diameter Dv50 of the second negative electrode active material is d2μm, d2 is 3-11, and optionally 3-7. When the particle diameter of the second negative electrode active material is within a suitable range, its microporous structure can be better maintained, so that the function of the microporous structure of hard carbon as active ion storage site can be fully utilized to improve the capacity and energy density of the secondary battery; at the same time, when the particle diameter of the second negative electrode active material is within a suitable range, the second negative electrode film layer can have a smooth tunnel structure, so that the electrolyte can smoothly pass through the tunnel structure of the second negative electrode film layer and quickly infiltrate into the first negative electrode film layer, which is favorable to reduce the polarization of the negative electrode and improve the charge and discharge efficiency of the secondary battery.
[0109] In some embodiments, the particle size distribution index (Dv90-Dv10) / Dv50 of the second negative active material is α1, α1 being 0.6-5, optionally 1-4. When the particle size distribution index of the second negative active material is within a suitable range, it is favorable for improving the processing performance of the second negative film layer, and for the second negative film layer to have high particle distribution uniformity and smooth tunnel structure, so that different regions of the second negative film layer have high active ion transmission performance, thereby further improving the high rate charging ability of the secondary battery, and at the same time, it is favorable for the electrolyte to quickly infiltrate into the first negative film layer, reduce the polarization of the negative electrode, and improve the charging and discharging efficiency of the secondary battery.
[0110] In some embodiments, the second negative electrode active material has a specific surface area of 3 m 2 / g~7m 2 / g, optionally 4m 2 / g~6m 2 / g. When the specific surface area of the second negative electrode active material is within a suitable range, the charge exchange resistance can be reduced, and the second negative electrode film layer can have a smoother tunnel structure, so that the active ion transmission performance is higher, and the high-rate charging ability of the secondary battery can be further improved. When the specific surface area of the second negative electrode active material is within a suitable range, the film formation efficiency of the SEI film can be improved, the formation of an excessively thick SEI film can be avoided, and the irreversible consumption of active ions can be reduced, thereby further improving the capacity and cycle performance of the secondary battery.
[0111] In some embodiments, the second negative electrode active material has a powder compression density of 0.9 g / cm at 20,000 N. 3 ~1.3g / cm 3 and can be selected to be 1g / cm 3 ~1.2g / cm 3 If the compressed density of the powder of the second negative electrode active material is within an appropriate range, this is advantageous for improving the energy density of the secondary battery.
[0112] In some embodiments, the second negative active material comprises primary particles, secondary particles or a combination thereof, and optionally the proportion of primary particles in the second negative active material is 90%-100%. When the second negative active material comprises a suitable proportion of primary particles, it is advantageous for the second negative film layer to have a short active ion transmission path, which can further improve the high-rate charging capability of the secondary battery. In addition, the polarization of the negative electrode and the side reaction of the electrolyte can be reduced, which can further improve the cycle performance and storage performance of the secondary battery.
[0113] In some embodiments, the volume average particle diameter Dv50 of the first negative active material is d3 μm, and d3 is 9 to 18, optionally 11 to 15. When the particle diameter of the first negative active material is within a suitable range, it is advantageous for the first negative film layer to have a high compression density, so that the secondary battery has a high initial coulombic efficiency, a high energy density and a long cycle life.
[0114] In some embodiments, the particle size distribution index (Dv90-Dv10) / Dv50 of the first negative active material is α2, α2 being 0.2-5, optionally 0.3-4. When the particle size distribution index of the first negative active material is within a suitable range, it is favorable to improve the processing performance of the first negative film layer, and to have a high particle distribution uniformity and a smooth tunnel structure throughout the first negative film layer, so that different regions of the first negative film layer all have high active ion transmission performance, which is favorable to further improve the cycle performance of the secondary battery.
[0115] In some embodiments, the first negative electrode active material has a specific surface area of 0.6 m 2 / g~1.5m 2 / g, optionally 0.8m 2 / g~1.4m 2 When the specific surface area of the first negative electrode active material is within a suitable range, the charge exchange resistance can be reduced, and the first negative electrode film layer has a smoother tunnel structure, which allows the first negative electrode film layer to have a higher active ion transmission performance, thereby further improving the cycle performance of the secondary battery.
[0116] In some embodiments, the first negative electrode active material has a powder compression density of 1.4 g / cm at 20,000 N. 3 ~1.85g / cm 3 and optionally 1.6g / cm 3 ~1.75g / cm 3 If the compressed density of the powder of the first negative electrode active material is within an appropriate range, this is advantageous for improving the energy density of the secondary battery.
[0117] In some embodiments, the graphitization degree of the first negative electrode active material is 91% to 95%, and optionally 92% to 94%. If the graphitization degree of the first negative electrode active material is within an appropriate range, it is advantageous to improve the cycle performance of the secondary battery.
[0118] In some embodiments, the first negative electrode active material includes artificial graphite, natural graphite, or a combination thereof. Optionally, the mass percentage of the artificial graphite in the first negative electrode active material is 50% or more, and optionally 60% to 100%, calculated based on the total mass of the first negative electrode active material. Optionally, a carbon coating layer is further provided on the surface of the artificial graphite to further reduce the charge transfer resistance and improve the cycle performance and high rate charging ability of the secondary battery, and optionally, the carbon coating layer includes amorphous carbon.
[0119] In some embodiments, the first negative active material comprises primary particles, secondary particles or a combination thereof, and optionally the quantity ratio of the secondary particles in the first negative active material is 90%-100%. When the first negative active material comprises a suitable proportion of secondary particles, its degree of isotropy is improved, which is favorable for the first negative film layer to have many active ion transmission channels, thereby further improving the high-rate charging ability of the secondary battery; at the same time, the first negative film layer has a high compression density, which is favorable for improving the energy density of the secondary battery. In addition, the side reaction between the polarization of the negative electrode and the electrolyte can be reduced, which further improves the cycle performance and storage performance of the secondary battery.
[0120] In some embodiments, the negative electrode sheet has a compressed density of 1.4 g / cm 3 ~1.85g / cm 3 and optionally 1.6g / cm 3 ~1.75g / cm 3 If the compressed density of the negative electrode sheet is within an appropriate range, it is advantageous for improving the high-rate charging capability, cycle performance, and energy density of the secondary battery.
[0121] In some embodiments, the negative electrode current collector may be a metal foil film sheet or a composite current collector. Examples of the metal foil include copper foil and copper alloy foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more combinations selected from copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. The polymeric material base layer may include one or more combinations selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0122] The manufacturing method of the negative electrode sheet of the present application is well known. In some embodiments, the negative electrode sheet can be manufactured by dispersing a first negative electrode active material, a conductive agent, an adhesive, and any other components in a solvent (e.g., deionized water) to form a first slurry, dispersing a second negative electrode active material, a conductive agent, an adhesive, and any other components in a solvent (e.g., deionized water) to form a second slurry, applying the first slurry to a negative electrode current collector and drying to form a first negative electrode film layer, applying the second slurry to the first negative electrode film layer, and obtaining a negative electrode sheet after processes such as drying and cold pressing.
[0123] The negative electrode current collector has two surfaces facing each other in the thickness direction thereof, and the first negative electrode film layer and the second negative electrode film layer may be provided on either one or both of the two facing surfaces of the negative electrode current collector. Optionally, the functional coating layer may be provided only on the surface of the base film facing the second negative electrode film layer of the negative electrode sheet, thereby reducing the mass of inactive components and improving the energy density of the secondary battery.
[0124] In addition, the first negative electrode film layer and the second negative electrode film layer in the present application both refer to the parameter range of the coating layer on one side of the negative electrode current collector. When the first negative electrode film layer and the second negative electrode film layer are provided on two surfaces of the negative electrode current collector, if the parameters of the coating layer on either surface satisfy the present application, it is considered to be within the protection scope of the present application.
[0125] In the negative electrode sheet of the present application, the Dv90, Dv50, and Dv10 of the material have the meanings well known in the art and can be measured by instruments and methods well known in the art. For example, referring to the particle size distribution laser diffraction method of GB / T 19077-2016, they can be easily tested using a laser particle size analyzer such as the Mastersizer 2000E laser particle size analyzer from Malvern, UK. Dv90 is the particle size corresponding to the material cumulative volume distribution percentage reaching 90%, Dv50 is the particle size corresponding to the material cumulative volume distribution percentage reaching 50%, and Dv10 is the particle size corresponding to the material cumulative volume distribution percentage reaching 10%.
[0126] In the negative electrode sheet of the present application, the specific surface area of the material has a meaning well known in the art and can be measured by instruments and methods well known in the art. For example, it can be tested by adopting the nitrogen adsorption specific surface area analysis test method with reference to GB / T 19587-2017, and calculated by the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis test can be performed by a Tri-Star 3020 type specific surface area pore size analysis tester from Micromeritics, USA.
[0127] In the negative electrode sheet of the present application, the graphitization degree of the material has a meaning well known in the art and can be measured by an apparatus and method well known in the art. For example, the test is performed using an X-ray diffraction apparatus (Bruker D8 Discover), and the test is performed with reference to JIS K 0131-1996 and JB / T 4220-2011, 002 After obtaining the formula g=(0.344-d 002The degree of graphitization of the material can be calculated based on the formula: d / (0.344-0.3354)×100%. 002 is the layer spacing of the (002) crystal plane in the crystal structure of the material expressed in nanometers (nm).
[0128] In the negative electrode sheet of the present application, the compressed density of the material powder has a meaning well known in the art and can be measured by instruments and methods well known in the art. For example, it can be tested by an electronic pressure tester (e.g., UTM7305 type) with reference to GB / T24533-2009. One exemplary test method is to weigh 1 g of material and measure the density of the material having a base area of 1.327 cm2. 2 The method includes a process of placing the powder in a mold, applying a pressure of 2000 kg (equivalent to 20,000 N), holding the pressure for 30 seconds, releasing the pressure, holding the pressure for 10 s, and then recording and calculating the compressed density of the powder at the applied force of 20,000 N of the material.
[0129] In the negative electrode sheet of the present application, the quantity ratio of primary particles and secondary particles can be measured by instruments and methods well known in the art, for example, by using a scanning electron microscope. In order to ensure the accuracy of the test results, a plurality of different regions (e.g., 5 or more) are randomly selected in the test sample to perform a scan test, and the proportion of the number of primary particles and secondary particles in each region to the number of total particles can be calculated at a certain magnification (e.g., 1000 times or more), that is, the respective quantity ratios of primary particles and secondary particles in the region. In order to ensure the accuracy of the test results, the above test can be repeated by taking a plurality of test samples (e.g., 10 or more), and the average value of each test sample can be taken as the final test result. The test standard can refer to JY / T010-1996.
[0130] In the negative electrode sheet of the present application, the thickness of the first negative electrode film layer and the second negative electrode film layer is a meaning well known in the art, and can be measured by an instrument and a method well known in the art. For example, by performing a test with a scanning electron microscope (e.g., ZEISS Sigma 300), the boundary region between the second negative electrode film layer and the first negative electrode film layer can be more accurately determined. One exemplary test method is to cut the negative electrode sheet into a test sample of a certain size (e.g., 2 cm x 2 cm), fix the negative electrode sheet to a sample stage with paraffin, insert the sample stage into a sample holder and fix it, turn on the power of an argon ion cross-section polishing device (e.g., IB-19500CP) and vacuum (e.g., 10 -4 The steps include setting the argon gas flow rate (e.g., 0.15MPa) and voltage (e.g., 8KV) and polishing time (e.g., 2 hours), adjusting the sample stage to swing mode, and starting polishing. The test standard can refer to JY / T010-1996. In order to ensure the accuracy of the test results, a plurality of different areas (e.g., 5 or more) can be randomly selected in the test sample to perform a scan test, and the thicknesses of the first and second negative electrode film layers in the scale test area can be read at a certain magnification (e.g., 500 times or more). For the accuracy of the test, a plurality of test areas can be taken and tested, and the average value can be taken.
[0131] In the negative electrode sheet of the present application, the compression density of the negative electrode sheet has a meaning well known in the art and can be measured by an apparatus and method well known in the art. The compression density of the negative electrode sheet = the areal density of the negative electrode sheet / the thickness of the coating layer on one side of the negative electrode current collector. The areal density of the negative electrode sheet has a meaning well known in the art and can be measured by an apparatus and method well known in the art. One exemplary test method is to punch a negative electrode sheet coated on one side and cold pressed (if the negative electrode sheet is coated on both sides, the coating layer on one side can be wiped off first) into a small wafer with an area of S1, weigh it and record it as M1, then wipe off the coating layer of the weighed negative electrode sheet, weigh the weight of the negative electrode current collector and record it as M0, and record the areal density of the negative electrode sheet = (M1-M0) / S1.
[0132] In addition, the above-mentioned first negative electrode active material and second negative electrode active material may be sampled and tested before coating, or may be sampled and tested from the negative electrode sheet, battery assembly, or secondary battery after cold pressing. When the test sample is sampled from the negative electrode sheet, battery assembly, or secondary battery after cold pressing, for example, the following steps may be performed: (1) arbitrarily select a cold-pressed coating layer on one side of the negative electrode current collector, and sample the second negative electrode active material (for example, a blade may be used to scrape off the powder and sample), with the scraping depth not exceeding the boundary area between the second negative electrode film layer and the first negative electrode film layer; and (2) sample the first negative electrode active material (a blade may be used to scrape off the powder and sample), and in the cold pressing process, the second negative electrode film layer is sampled. Since there may be a mutual fusion layer at the boundary region between the first negative electrode film layer and the first negative electrode film layer, in order to ensure the accuracy of the test, when sampling the first negative electrode active material, the mutual fusion layer is first scraped off, and then the first negative electrode active material is scraped off to sample; and (3) the first negative electrode active material and the second negative electrode active material collected above are respectively put into deionized water, and then subjected to suction filtration and drying. The dried powder is sintered at a certain temperature and time (e.g., 400°C, 2h) to remove the adhesive and conductive agent, etc., to obtain a test sample. [Positive electrode sheet]
[0133] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, for example, the positive electrode current collector has two surfaces facing each other in the thickness direction of the positive electrode current collector, and the positive electrode film layer is provided on one or both of the two facing surfaces of the positive electrode current collector.
[0134] The positive electrode film layer includes a positive electrode active material, and the positive electrode active material may be a positive electrode active material for secondary batteries known in the art. For example, the positive electrode active material may include one or more combinations selected from lithium transition metal oxides, lithium-containing phosphates, and their respective modified compounds. Examples of lithium transition metal oxides include lithium cobalt oxides (e.g., LiCoO2), lithium nickel oxides (e.g., LiNiO2), lithium manganese oxides (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, and lithium nickel cobalt manganese oxides (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.5 Co 0.25 Mn 0.25 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2), lithium nickel cobalt aluminum oxide (e.g., LiNi 0.85 Co 0.15 Al 0.05 O2) and their respective modifying compounds. Examples of the lithium-containing phosphate may include one or more combinations selected from lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and their respective modifying compounds.
[0135] In some embodiments, to further increase the energy density of the secondary battery, the positive electrode active material may include one or more combinations of lithium transition metal oxides and their modifying compounds as shown in Formula 1.
[0136] Li a Ni b Co c M d O e A f Formula 1
[0137] In Formula 1, 0.8 ≤ a ≤ 1.2, 0.5 ≤ b < 1, 0 < c < 1, 0 < d < 1, 1 ≤ e ≤ 2, 0 ≤ f ≤ 1, M may include one or more combinations selected from Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti, and B, and A may include one or more combinations selected from N, F, S, and Cl.
[0138] In the present application, the modified compound of each of the above positive electrode active materials is obtained by performing doping modification and / or surface coating modification on the above positive electrode active material.
[0139] In some embodiments, the positive electrode film layer may further include a conductive agent. The conductive agent plays a role in collecting microcurrents between the positive electrode active materials, reducing the contact resistance of the electrode, accelerating the electron transfer rate, reducing polarization, and improving the charge and discharge efficiency of the secondary battery. For example, the conductive agent may include one or more combinations selected from superconducting carbon, conductive graphite, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. In some embodiments, based on the total mass of the positive electrode film layer, the mass percentage of the conductive agent is 5% or less.
[0140] In some embodiments, the positive electrode film layer may further include an adhesive to bond the positive electrode active materials to each other and to bond the positive electrode film layer to the positive electrode current collector. For example, the adhesive may include one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene ternary copolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene ternary copolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. In some embodiments, the mass percentage of the adhesive is 5% or less, calculated based on the total mass of the positive electrode film layer.
[0141] In some embodiments, the positive electrode current collector may be a metal foil film sheet or a composite current collector. Examples of the metal foil film sheet include aluminum foil or aluminum alloy foil. The composite current collector may include a polymeric material base layer and a metal material layer formed on at least one surface of the polymeric material base layer. For example, the metal material may include one or more combinations selected from aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. The polymeric material base layer may include one or more combinations selected from polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0142] The positive electrode film layer is generally formed by applying a positive electrode slurry to a positive electrode current collector, drying, and cold pressing. The positive electrode slurry is generally formed by dispersing a positive electrode active material, a conductive agent, an adhesive, and other optional components in a solvent and uniformly stirring the mixture. The solvent may be, but is not limited to, N-methylpyrrolidone (NMP).
[0143] The electrode assembly 6 of the present application will now be described with reference to the drawings.
[0144] FIG. 1 is a schematic diagram of one embodiment of an electrode assembly 6 of the present application. As shown in FIG. 1, the electrode assembly 6 includes a negative electrode sheet 10, a positive electrode sheet 20, and a separator 30 located between the negative electrode sheet 10 and the positive electrode sheet 20. The negative electrode sheet 10 includes a negative electrode current collector 100, a first negative electrode film layer 101 and a second negative electrode film layer 102 located on both sides of the negative electrode current collector 100, and the first negative electrode film layer 101 is located between the negative electrode current collector 100 and the second negative electrode film layer 102. The separator 30 includes a base film 300 and a functional coating layer 301 located on both sides of the base film 300. The positive electrode sheet 20 includes a positive electrode current collector 200 and a positive electrode film layer 201 located on both sides of the positive electrode current collector 200.
[0145] FIG. 2 is a schematic diagram of an embodiment of an electrode assembly 6 of the present application. As shown in FIG. 2, the electrode assembly 6 includes a negative electrode sheet 10, a positive electrode sheet 20, and a separator 30 located between the negative electrode sheet 10 and the positive electrode sheet 20. The negative electrode sheet 10 includes a negative electrode current collector 100, a first negative electrode film layer 101 and a second negative electrode film layer 102 located on both sides of the negative electrode current collector 100, and the first negative electrode film layer 101 is located between the negative electrode current collector 100 and the second negative electrode film layer 102. The separator 30 includes a base film 300, a functional coating layer 301 and an adhesive layer 302 located on both sides of the base film 300. The positive electrode sheet 20 includes a positive electrode current collector 200 and a positive electrode film layer 201 located on both sides of the positive electrode current collector 200.
[0146] As shown in FIG. 1 and FIG. 2, the first negative electrode film layer 101 and the second negative electrode film layer 102 are provided on two surfaces of the negative electrode current collector 100. Of course, in some embodiments, the first negative electrode film layer 101 and the second negative electrode film layer 102 may be provided on only one surface of the negative electrode current collector 100. The positive electrode film layer 201 is provided on two surfaces of the positive electrode current collector 200. Of course, in some embodiments, the positive electrode film layer 201 may be provided on only one surface of the positive electrode current collector 200. The functional coating layer 301 is provided on both sides of the base film 300. Of course, in some embodiments, the functional coating layer 301 may be provided on only one surface of the base film 300 facing the second negative electrode film layer 102 of the negative electrode sheet 10. secondary battery
[0147] An embodiment of the present application further provides a secondary battery. A secondary battery is also called a rechargeable battery or a storage battery, and is a battery that can be used continuously after discharging by activating the active material by charging. The secondary battery of the present application includes the electrode assembly and the electrolyte of the present application. The secondary battery of the present application may be a lithium-containing secondary battery, and in particular may be a lithium-ion secondary battery.
[0148] The electrolyte includes a lithium salt and a solvent. For example, the lithium salt may include one or more combinations selected from the following: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bisfluorosulfonyl imide (LiFSI), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium disoxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorodisoxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP). By way of example, the organic solvent may comprise one or a combination of more selected from ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).
[0149] In some embodiments, the electrolyte may further include additives, including, for example, an anode film-forming additive, a cathode film-forming additive, and may further include additives that can improve the performance of a portion of the battery, such as, for example, an additive that improves the overcharge performance of the battery, or an additive that improves the high or low temperature performance of the battery.
[0150] In some embodiments, the secondary battery may include an exterior case that can be used to seal the electrode assembly and electrolyte of the present application.
[0151] In some embodiments, the exterior of the secondary battery may be a hard package, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a soft package, such as a bag soft package. The material of the soft package may be plastic, such as one or a combination of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0152] The shape of the secondary battery of the present application is not particularly limited, and may be cylindrical, rectangular, or any other shape. Fig. 3 shows a secondary battery 5 having a rectangular structure as an example.
[0153] In some embodiments, as shown in FIG. 4, the exterior may include a housing 51 and a cover plate 53. The housing 51 includes a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate are surrounded to form a storage chamber. The housing 51 has an opening communicating with the storage chamber, and the cover plate 53 is provided to cover the opening so as to seal the storage chamber. The positive electrode sheet, the negative electrode sheet and the separator can be formed into an electrode assembly 52 by a winding process and / or a stacking process. The electrode assembly 52 is packaged in the storage chamber. The electrolyte is impregnated into the electrode assembly 52. The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and may be adjusted according to requirements.
[0154] The method for manufacturing the secondary battery of the present application is well known. In some embodiments, a secondary battery can be formed by assembling a positive electrode sheet, a separator, a negative electrode sheet, and an electrolyte. For example, a positive electrode sheet, a separator, and a negative electrode sheet can be formed into an electrode assembly by a winding process or a stacking process, and the electrode assembly can be placed in an outer casing, dried, and then an electrolyte can be injected, and a secondary battery can be obtained through processes such as vacuum sealing, standing, chemical formation, and shaping.
[0155] In some embodiments of the present application, the secondary battery of the present application may be assembled into a battery module, and the number of secondary batteries included in the battery module may be multiple, and the specific number may be adjusted according to the application and capacity of the battery module.
[0156] Fig. 5 is a schematic diagram of an example battery module 4. As shown in Fig. 5, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed by a fastener.
[0157] Optionally, the battery module 4 further includes an outer case having an accommodating space, and the plurality of secondary batteries 5 are accommodated in the accommodating space.
[0158] In some embodiments, the battery modules may be assembled into a battery pack, and the number of battery modules included in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0159] 6 and 7 are schematic diagrams of an example battery pack 1. As shown in Fig. 6 and 7, the battery pack 1 may include a battery case and a plurality of battery modules 4 provided in the battery case. The battery case includes an upper case 2 and a lower case 3, and the upper case 2 is provided to cover the lower case 3 to form an enclosed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery case in any manner. power consumption equipment
[0160] An embodiment of the present application provides a power consuming device including at least one of the secondary batteries, battery modules, or battery packs of the present application. The secondary batteries, battery modules, or battery packs may be used as a power source for the power consuming device, or may be used as an energy storage means for the power consuming device. The power consuming device may be, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), a train, a ship, and a satellite, an energy storage system, etc.
[0161] The power consumption device can select a secondary battery, a battery module or a battery pack according to the demand.
[0162] 8 is a schematic diagram of an example power consuming device, such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, etc. A battery pack or battery module may be employed to meet the high power and high energy density requirements of the power consuming device.
[0163] Another example of the power consuming device may be a mobile phone, a tablet computer, a notebook computer, etc. Generally, the power consuming device is required to be thin and may employ a secondary battery as a power source. Working Example
[0164] The following examples are provided to more specifically describe the contents of the present application, but these examples are merely illustrative, and it will be apparent to those skilled in the art that various modifications and changes may be made within the scope of the disclosure of the present application. Unless otherwise specified, all parts, percentages, and ratios described in the following examples are based on mass. In addition, all reagents used in the examples are commercially available or may be synthesized according to conventional methods, and can be used as is without further treatment. In addition, all devices used in the examples are commercially available. Example 1-1
[0165] Step (1): Manufacturing the negative electrode sheet
[0166] S10 Manufacturing of artificial graphite
[0167] After pretreatment of the raw petroleum non-acicular coke powder, impurities are removed, and then the raw petroleum coke powder is mixed with coal pitch and granulated to obtain secondary particles with a Dv50 of 10 μm. The granulated material is then put into an Acheson graphitization furnace and graphitized at 3000 ° C for 24 hours to obtain graphite particles. The graphite particles obtained are mixed with petroleum pitch and carbonized at 1000 ° C for 15 hours to obtain artificial graphite. The artificial graphite has a Dv50 of 12 μm, a Dv90 of 20 μm, a Dv10 of 6.5 μm, a graphitization degree of 92%, and a specific surface area of 0.86 m 2 / g and the compressed density of the powder is 1.6 g / cm 3 , and the topography is secondary.
[0168] S20 Hard Carbon Manufacturing
[0169] The phenolic resin is heated at 500°C for 30 min to obtain a precursor, which is then crushed and heat-treated at 1200°C for 20 h in a nitrogen gas atmosphere and crushed again to obtain hard carbon. The hard carbon has a Dv50 of 5 μm, a Dv90 of 10 μm, a Dv10 of 2.5 μm, and a specific surface area of 5 m. 2 / g and the topography is primary particle.
[0170] S30 Preparation of first slurry
[0171] The artificial graphite produced above, conductive carbon black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener are mixed in a mass ratio of 96.8:0.8:1.2:1.2, then added to deionized water and stirred with a vacuum mixer until the system becomes uniform, to obtain a first slurry with a solid content of 66%.
[0172] S40 Preparation of second slurry
[0173] The hard carbon produced above, conductive carbon black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener are mixed in a mass ratio of 95:1.5:3.1:0.4, and then added to deionized water. The mixture is stirred under the action of a vacuum mixer until the system becomes uniform, to obtain a second slurry with a solid content of 66%.
[0174] S50 Slurry Application
[0175] The first slurry is applied to one surface of a copper foil as a negative electrode current collector with a thickness of 8 μm and dried to form a first negative electrode film layer, the second slurry is applied to the first negative electrode film layer and dried to form a second negative electrode film layer, and then the above process is repeated on the other surface of the copper foil as a negative electrode current collector, and after further processes such as cold pressing, a negative electrode sheet is obtained. The thickness of the first negative electrode film layer on one side of the negative electrode current collector is 59 μm, and the thickness of the second negative electrode film layer is 82 μm. The compressed density of the negative electrode sheet is 1.55 g / cm 3 It is.
[0176] Step (2): Manufacturing the positive electrode sheet
[0177] Positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1O2 (NCM811), conductive carbon black as a conductive agent, and polyvinylidene fluoride (PVDF) as an adhesive are mixed in a mass ratio of 98:1:1, then added to the solvent NMP and stirred with a vacuum mixer until the system becomes uniform, obtaining a positive electrode slurry with a solid content of 75%. The positive electrode slurry is evenly applied to two surfaces of 13μm-thick aluminum foil, dried at 90℃, and then cold pressed to obtain a positive electrode sheet with a positive electrode film layer thickness of 114μm on one side of the positive electrode current collector.
[0178] Step (3): Preparation of electrolyte
[0179] In an environment with a water content of less than 10 ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then thoroughly dried LiPF6 is dissolved in the organic solvent to prepare an electrolyte solution with a concentration of 1 mol / L.
[0180] Step (4): Manufacturing the separator
[0181] Barium titanate (dielectric constant 3000 or more) with a Dv50 of 100 nm, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a dispersant were mixed in a mass ratio of 85:10:5, then added to deionized water and stirred with a vacuum mixer until the system was uniform, obtaining a slurry with a solid content of 40%. The slurry was then applied to both surfaces of a porous polyethylene film (thickness 10 μm) and dried to form a functional coating layer with a thickness of 2 μm on each side.
[0182] Step (5): Manufacturing a secondary battery
[0183] The positive electrode sheet, separator, and negative electrode sheet are stacked in order so that the side of the separator that covers the functional coating layer faces the second functional layer of the negative electrode sheet, and then rolled up to obtain an electrode assembly. The electrode assembly is placed in an outer casing and dried. After that, an electrolyte is injected, and the secondary battery is obtained through processes such as vacuum sealing, leaving it to stand, chemical conversion, and shaping. Examples 1-2 to 1-7
[0184] The secondary battery was manufactured in a similar manner to Example 1-1, except that the coating thickness of the slurry in the preparation of the separator and the thickness of the functional coating layer obtained thereby were different. See Table 1 for specific parameters. Comparative Example 1-1
[0185] The secondary battery was manufactured in a similar manner to that of Example 1-1, except that the separator was a porous polyethylene film. Comparative Example 1-2
[0186] The secondary battery was manufactured in a similar manner to Example 1-1, except that the separator was a porous polyethylene film and the order of applying the slurry in manufacturing the negative electrode sheet was different.
[0187] First, the second slurry is applied to one surface of the copper foil, which is a negative electrode current collector with a thickness of 8 μm, and then dried to form a first negative electrode film layer, and then the first slurry is applied to the first negative electrode film layer and dried to form a second negative electrode film layer, and then the above process is repeated on the other surface of the copper foil, which is a negative electrode current collector, and after undergoing processes such as cold pressing, a negative electrode sheet is obtained. The thickness of the first negative electrode film layer on one side of the negative electrode current collector is 82 μm, and the thickness of the second negative electrode film layer is 59 μm. Comparative Examples 1 to 3
[0188] The secondary battery was manufactured in a similar manner to that of Example 1-1, except that the separator was a porous polyethylene film and the second slurry was not applied in the manufacture of the negative electrode sheet.
[0189] The first slurry is applied to both surfaces of the copper foil negative current collector with a thickness of 8 μm, and then the negative electrode sheet is obtained after processes such as drying and cold pressing. The thickness of the negative electrode film layer on one side of the negative electrode current collector is 141 μm. Comparative Example 1-4
[0190] The secondary battery is manufactured in a similar manner to Example 1-1, except that a porous polyethylene film is used as the separator, and the first slurry is not applied in the manufacture of the negative electrode sheet.
[0191] The second slurry is applied to both surfaces of the 8 μm-thick copper foil negative current collector, and the negative electrode sheet is obtained after drying, cold pressing, and other processes. The thickness of the negative electrode film layer on one side of the negative electrode current collector is 141 μm. Comparative Examples 1-5
[0192] The secondary battery was manufactured in a similar manner to that of Example 1-1, except that the separator used was a porous polyethylene film and the manufacturing process of the negative electrode sheet was different.
[0193] S10 to S20 are the same as in Example 1-1.
[0194] S30 Slurry Preparation
[0195] The artificial graphite and hard carbon produced above, conductive carbon black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener are mixed in a mass ratio of 40:55:1.5:3.1:0.4, and then added to deionized water and stirred with a vacuum mixer until the system becomes uniform, to obtain a slurry with a solid content of 66%.
[0196] S40 Slurry Application
[0197] The slurry is applied to both surfaces of the 8μm-thick copper foil negative current collector, and the negative electrode sheet is obtained after processes such as drying and cold pressing. The thickness of the negative electrode film layer on one side of the negative current collector is 141μm. Comparative Examples 1-6
[0198] The secondary battery is manufactured in a similar manner to that of Example 1-1, except that the separator is a porous polyethylene film and the manufacturing process of the negative electrode sheet is different.
[0199] S10 to S30 are the same as in the first embodiment.
[0200] S40 Preparation of second slurry
[0201] The hard carbon produced above, barium titanate (Dv50 of 100 nm, dielectric constant of 3000 or more), conductive carbon black as a conductive agent, styrene butadiene rubber (SBR) as an adhesive, and sodium carboxymethylcellulose (CMC) as a thickener are mixed in a mass ratio of 93:1:1.5:3.1:0.4, and then added to deionized water and stirred with a vacuum stirrer until the system becomes uniform, to obtain a second slurry with a solid content of 66%.
[0202] S50 Slurry Application
[0203] The first slurry is applied to one surface of the copper foil, which is a negative electrode current collector with a thickness of 8 μm, and dried to form a first negative electrode film layer, and the second slurry is applied to the first negative electrode film layer and dried to form a second negative electrode film layer, and then the above process is repeated on the other surface of the copper foil, which is a negative electrode current collector, and after further processes such as cold pressing, a negative electrode sheet is obtained. The thickness of the first negative electrode film layer on one side of the negative electrode current collector is 59 μm, and the thickness of the second negative electrode film layer is 82 μm. Testing Part
[0204] (1) Maximum charging rate test
[0205] At 25 ° C., the secondary battery prepared above is fully discharged at a rate of 0.33 C, and then fully charged at a rate of 0.33 C. The fully charged secondary battery is left to stand for 5 min, and then fully discharged at a rate of 0.33 C. The discharge capacity obtained at this time is the actual capacity of the secondary battery at a rate of 1 C, and is denoted as C0. The secondary battery is fully charged at a rate of xC0 (indicating the gradient of the charge rate, for example, 1C0, 1.1C0, 1.2C0, 1.3C0, 1.4C0, etc.), left to stand for 5 min, and then fully discharged at 1 C. After 10 cycles in this manner, the secondary battery is further fully charged at 1 C. The secondary battery is disassembled and the state of lithium deposition on the surface of the negative electrode sheet is observed. If lithium is not deposited on the surface of the negative electrode sheet, the charge rate is increased until lithium is deposited on the surface of the negative electrode sheet, and the maximum charge rate at which lithium is not deposited on the surface of the negative electrode sheet is measured again, and the maximum charge rate at which lithium is not deposited on the surface of the negative electrode sheet is recorded. The higher the maximum charge rate of the secondary battery, the better the charging ability at a high rate.
[0206] (2) Energy density test
[0207] At 25°C, the secondary battery prepared above is fully charged at a rate of 0.33C and fully discharged at a rate of 0.33C, and after three cycles in this manner, the discharge energy of the secondary battery is recorded. Energy density of secondary battery = discharge energy of secondary battery / mass of secondary battery. In each of the examples and comparative examples of the present application, the energy density of the secondary battery prepared in Comparative Example 1-1 is taken as 100%, and the energy densities of the secondary batteries of the other examples and comparative examples are shown.
[0208] (3) Cycle life test
[0209] At 25°C, the secondary battery produced above is fully discharged at a rate of 1C, fully charged at a rate of 1C, and then the fully charged secondary battery is left to stand for 5 minutes and then fully discharged at a rate of 1C. The discharge capacity C0 obtained at this time is the initial capacity of the secondary battery. The secondary battery is fully charged at a rate of 3C and fully discharged at a rate of 1C. In this manner, a cycle charge / discharge test is performed, and the discharge capacity after each cycle is recorded until the discharge capacity of the secondary battery decays to 80% of the initial capacity. The number of cycles at this time represents the cycle life of the secondary battery. It is expected that the cycle life will be longer as the number of cycles of the secondary battery increases. [Table 1]
[0210] Summarizing the test results of Examples 1-1 to 1-7 and Comparative Examples 1-1 to 1-6, it was found that the secondary battery using the electrode assembly of the present application had both a high charge rate and a long cycle life. In Comparative Example 1-1, since no functional coating layer was provided on the surface of the separator, the secondary battery produced could not have both a high charge rate and a long cycle life. In Comparative Example 1-2, since no functional coating layer was provided on the surface of the separator and a hard carbon layer and a graphite layer were provided in that order on the surface of the negative electrode current collector, it was difficult for the secondary battery to achieve both a high charge rate and a long cycle life. In Comparative Example 1-3, since no functional coating layer was provided on the surface of the separator and a graphite layer was provided only on the surface of the negative electrode current collector, the secondary battery had a long cycle life but was difficult to obtain a high charge rate. In Comparative Example 1-4, since no functional coating layer was provided on the surface of the separator and a hard carbon layer was provided only on the surface of the negative electrode current collector, the secondary battery could have a high charge rate but was difficult to obtain a long cycle life. In Comparative Example 1-5, the separator surface is not provided with a functional coating layer, and a mixed layer of graphite and hard carbon is provided on the surface of the negative electrode current collector, so it is difficult for the secondary battery to achieve both a high charge rate and a long cycle life.Compared to Comparative Example 1-1, the hard carbon layer of Comparative Example 1-6 also contains barium titanate, but barium titanate has a low effect of suppressing the continued growth of lithium dendrites in a direction perpendicular to the electrode sheet, and is therefore unlikely to clearly improve the charge rate and cycle life of the secondary battery.
[0211] To summarize the test results of Examples 1-1 to 1-7, it was found that the thickness of the functional coating layer of the separator increased, and both the maximum charge rate and cycle life of the secondary battery increased. The increase in reverse electric field strength due to the functional coating layer increases the effect of suppressing the continued growth of lithium dendrites in a direction perpendicular to the electrode sheet, which is a possible factor in improving the high-rate charge capacity and cycle performance of the secondary battery.
[0212] To summarize the test results of Examples 1-1 to 1-7, when H1 / (H2+H3) is smaller than 0.01, the functional coating layer of the separator is set to be small relative to the total thickness of the first negative electrode film layer and the second negative electrode film layer, and the effect of suppressing the continuous growth of lithium dendrites in the direction perpendicular to the electrode sheet is not clear, and therefore the effect of improving the maximum charging rate of the secondary battery is not clear.
[0213] To summarize the test results of Examples 1-6 and 1-7, when H1 is greater than 10, the effect of the separator's functional coating layer in inhibiting the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet does not increase continuously, and at the same time, the functional coating layer does not have electrochemical activity and cannot contribute to capacity, so that when its thickness is greater than 10 μm, the energy density of the secondary battery is significantly reduced.
[0214] Next, the inventors studied the effect of the mass percentage of the ferroelectric material in the functional coating layer of the separator on the performance of the secondary battery. The secondary batteries of Example 2-1 to Example 2-6 were manufactured in a similar manner to Example 1-2, except that the mass percentage of the ferroelectric material in the functional coating layer of the separator was different. [Table 2]
[0215] To summarize the test results of Examples 1-2, 2-1 to 2-6, it was found that when the thickness of the functional coating layer of the separator was fixed at 4 μm, the maximum charge rate and cycle life of the secondary battery both increased as the mass percentage of the ferroelectric material in the functional coating layer increased. In this case, the increase in the reverse electric field strength caused by the functional coating layer increases the effect of suppressing the continued growth of the lithium dendrite in the direction perpendicular to the electrode sheet, which is a possible factor in improving the high-rate charge capacity and cycle performance of the secondary battery.
[0216] To summarise the test results of Comparative Example 1-1 and Example 2-1, it was further found that when the mass percentage of the ferroelectric material in the functional coating layer of the separator is small, the resulting functional coating layer does not clearly have the effect of suppressing the continued growth of lithium dendrites in a direction perpendicular to the electrode sheet, and as a result, the effect of improving the maximum charging rate of the secondary battery is not clearly evident.
[0217] Summarizing the test results of Examples 2-5 and 2-6, it can be seen that when the mass percentage of the ferroelectric material in the functional coating layer of the separator is greater than 95%, the cycle performance of the secondary battery is obviously poor. In this case, the possible reason is that the content of the adhesive in the functional coating layer of the separator is too small, which may cause the functional coating layer to fall off from the surface of the base film during the long-term cycle charge-discharge process of the secondary battery.
[0218] Next, the inventors studied the effect of the volume average particle diameter Dv50 of the ferroelectric material in the functional coating layer of the separator on the performance of the secondary battery. The secondary batteries of Examples 3-1 to 3-6 were manufactured in a similar manner to Example 1-2, except that the volume average particle diameter Dv50 of the ferroelectric material in the functional coating layer of the separator was different. [Table 3]
[0219] Summarizing the test results of Examples 1-2, 3-1 to 3-6, it was found that when the thickness of the functional coating layer of the separator was fixed at 4 μm and the mass percentage of the ferroelectric material was fixed at 85%, the maximum charge rate and cycle life of the secondary battery both decreased as the volume average particle diameter Dv50 of the ferroelectric material increased. As the volume average particle diameter Dv50 of the ferroelectric material increased, the interference of the reverse electric field generated by it increased, which deteriorated the effect of suppressing the continued growth of lithium dendrites in the direction perpendicular to the electrode sheet, which is a possible factor in the decrease of both the maximum charge rate and cycle life of the secondary battery.
[0220] Next, the inventors studied the influence of the thickness of the first negative electrode film layer and the thickness of the second negative electrode film layer on the performance of the secondary battery. The secondary batteries of Examples 4-1 to 4-7 were manufactured in a similar manner to Example 1-2, except that the thicknesses of the first negative electrode film layer and the second negative electrode film layer were different. [Table 4]
[0221] To summarize the test results of Examples 4-1 to 4-7, it was found that the maximum charge rate of the secondary battery increased when the thickness of the second negative electrode film layer increased.
[0222] Summarizing the test results of Examples 4-1 to 4-7, it was found that when the thickness H2μm of the second negative electrode film layer and the thickness H3μm of the first negative electrode film layer satisfy that H2 / H3 is between 0.25 and 4, the secondary battery can have a high maximum charge rate and a long cycle life at the same time. When H2 / H3 is less than 0.25, the second negative electrode film layer is thin, and the effect of improving the maximum charge rate of the secondary battery is not significant; when H2 / H3 is greater than 4, the second negative electrode film layer is thick, and the cycle performance of the hard carbon itself is poor, resulting in poor cycle performance of the secondary battery. Summarizing the test results of Examples 4-7 and Comparative Example 1-4, it was found that when H2 / H3 is greater than 4, the improvement of the cycle life of the secondary battery is not significant.
[0223] The present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is an example, and any configuration that has substantially the same technical idea and produces similar effects within the technical scope of the present application is included in the technical scope of the present application. In addition, various modifications to the embodiment that a person skilled in the art can conceive, and other forms constructed by combining some of the components in the embodiment, are also included in the scope of the present application, within the scope of the present application, as long as they do not deviate from the gist of the present application.
Claims
1. An electrode assembly comprising: a negative electrode sheet; a positive electrode sheet; and a separator disposed between the negative electrode sheet and the positive electrode sheet; The negative electrode sheet includes a negative electrode current collector and a first negative electrode film layer and a second negative electrode film layer provided on at least one surface of the negative electrode current collector, the first negative electrode film layer is located between the negative electrode current collector and the second negative electrode film layer, and includes a first negative electrode active material including graphite, and the second negative electrode film layer includes a second negative electrode active material including hard carbon, The separator includes a base film and a functional coating layer located at least on a side of the base film facing the negative electrode sheet, the functional coating layer including a ferroelectric material. Electrode assembly.
2. The thickness of the functional coating layer is H 1 μm, and the thickness of the second negative electrode film layer is H 2 μm, and the thickness of the first negative electrode film layer is H 3 μm, and the electrode assembly is H 1 / (H 2 +H 3 ) is 0.01 to 0.15, and optionally 0.01 to 0.08; The electrode assembly of claim 1 .
3. The thickness of the functional coating layer is H 1 μm, and H 1 is 2 to 10, optionally 4 to 6; 3. An electrode assembly according to claim 1 or 2.
4. The thickness of the second negative electrode film layer is H 2 μm, and the thickness of the first negative electrode film layer is H 3 μm, and the negative electrode sheet is H 2 / H 3 is 0.10 to 5, and optionally 0.5 to 4; 4. An electrode assembly according to any one of claims 1 to 3.
5. The volume average particle diameter Dv50 of the ferroelectric material is d 1 μm, and d 1 is less than or equal to 1, optionally between 0.05 and 0.8; 5. An electrode assembly according to any one of claims 1 to 4.
6. The volume average particle diameter Dv50 of the second negative electrode active material is d 2 μm, and the volume average particle diameter Dv50 of the first negative electrode active material is d 3 μm, and d 2 / d 3 is between 0.1 and 1, optionally between 0.2 and 0.8; 6. An electrode assembly according to any one of claims 1 to 5.
7. The mass percentage of the ferroelectric material in the functional coating layer is W1, calculated based on the total mass of the functional coating layer, W1 being 70%-95%, optionally 80%-95%; 7. An electrode assembly according to any one of claims 1 to 6.
8. The functional coating layer further includes an adhesive, and optionally, the adhesive includes one or more combinations of styrene butadiene rubber, polyacrylic acid, sodium polyacrylate, polyacrylamide, polyvinyl alcohol, sodium alginate, polymethacrylic acid, carboxymethyl chitosan, fluorine-containing acrylate resin, polytetrafluoroethylene, homopolymer of vinylidene fluoride, and copolymers thereof; 8. An electrode assembly according to any one of claims 1 to 7.
9. The separator further includes an adhesive layer provided on a surface of the functional coating layer, and optionally, the adhesive layer includes one or a combination of a homopolymer of vinylidene fluoride and a copolymer thereof.
9. An electrode assembly according to any one of the preceding claims.
10. The dielectric constant of the ferroelectric material is 50 or more, optionally 50 to 100,000.
10. An electrode assembly according to any one of the preceding claims.
11. The ferroelectric material includes one or a combination of a plurality of ferroelectric materials selected from inorganic ferroelectric materials and organic ferroelectric materials; Optionally, the inorganic ferroelectric material comprises one or more combinations of perovskite structure oxides, tungsten bronze type compounds, bismuth oxide type layer structure compounds, lithium niobate, lithium tantalate, lead metaniobate, and lead barium lithium niobate; Optionally, the organic ferroelectric material may include one or more combinations selected from the group consisting of homopolymers or copolymers of vinylidene fluoride, 2,5-dibromo-3,6-dihydroxy-p-benzoquinone, phenazine-chloranilic acid, and croconium; The negative electrode sheet according to claim 1 .
12. The mass percentage of hard carbon in the second negative electrode film layer is W2, calculated based on the total mass of the second negative electrode film layer, W2 is 68% or more, optionally 90% to 98%; and / or The mass percentage of graphite in the first negative electrode film layer is W3, and calculated based on the total mass of the first negative electrode film layer, W3 is 78% or more, and optionally 90% to 98%; 12. An electrode assembly according to any one of the preceding claims.
13. The second negative electrode active material satisfies at least one of the following conditions (1) to (5): (1) The volume average particle diameter Dv50 of the second negative electrode active material is d 2 μm, and d 2 is 3 to 11, optionally 3 to 7; (2) The particle size distribution index (Dv90-Dv10) / Dv50 of the second negative electrode active material is α 1 and α 1 is 0.6 to 5, optionally 1 to 4; (3) The specific surface area of the second negative electrode active material is 3 m 2 / g ~ 7m 2 / g, optionally 4m 2 / g to 6m 2 / g, (4) The compressed density of the powder of the second negative electrode active material at 20,000 N is 0.9 g / cm 3 ~1.3g / cm 3 and optionally 1 g / cm 3 ~1.2g / cm 3 and (5) The second negative electrode active material includes primary particles, secondary particles, or a combination thereof, and optionally, the proportion of primary particles in the second negative electrode active material is 90% to 100%.
13. An electrode assembly according to any one of the preceding claims.
14. The first negative electrode active material satisfies at least one of the following conditions (1) to (7): (1) The volume average particle diameter Dv50 of the first negative electrode active material is d 3 μm, and d 3 is 9 to 18, optionally 11 to 15; (2) The particle size distribution index (Dv90-Dv10) / Dv50 of the first negative electrode active material is α 2 and α 2 is 0.2 to 5, optionally 0.3 to 4; (3) The specific surface area of the first negative electrode active material is 0.6 m 2 / g to 1.5m 2 / g, optionally 0.8m 2 / g to 1.4m 2 / g, (4) The compressed density of the powder of the first negative electrode active material at 20,000 N is 1.4 g / cm 3 ~1.85g / cm 3 and optionally 1.6 g / cm 3 ~1.75g / cm 3 and (5) the graphitization degree of the first negative electrode active material is 91% to 95%, optionally 92% to 94%; (6) The first negative electrode active material includes artificial graphite, natural graphite, or a combination thereof, and optionally, a surface of the artificial graphite has a carbon coating layer; (7) The first negative electrode active material includes primary particles, secondary particles, or a combination thereof, and optionally, the quantity ratio of the secondary particles in the first negative electrode active material is 90% to 100%.
14. An electrode assembly according to any one of claims 1 to 13.
15. Comprising an electrode assembly according to any one of claims 1 to 14, Secondary battery.
16. The secondary battery according to claim 15 is provided. Battery module.
17. The secondary battery according to claim 15 and the battery module according to claim 16 are included. Battery pack.
18. The battery pack according to claim 17 includes at least one of the secondary battery according to claim 15, the battery module according to claim 16, and the battery pack according to claim 17. Power consumption equipment.
Citation Information
Patent Citations
Negative electrode and nonaqueous electrolyte secondary battery using it
JP2008059999A
Organic / inorganic composite separation membrane coated with a porous active layer and electrochemical element equipped therewith
JP2010517811A
Insulating porous layer for non-aqueous electrolyte secondary battery and laminated separator for non-aqueous electrolyte secondary battery
JP2017107853A
Improved battery separator and related methods
JP2018530106A
Semiconductor device
JP2019041013A