Method for producing nanosilicon powder from induction plasma pyrolysis silane
The induced plasma pyrolysis method addresses the challenges of producing nanosilicon powder by ensuring high purity and safety through a multi-stage reaction and cooling process, achieving efficient and continuous production of nanosilicon powder with controlled particle size and shape.
Patent Information
- Application Number
- JP2022570526
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-22
- Filing Date
- 2022-04-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-04-16
AI Technical Summary
Existing methods for producing nanosilicon powder face challenges such as high impurity content, difficulty in controlling particle size and shape, safety risks, and low thermal coupling efficiency, making it difficult to achieve high purity and continuous production.
A method involving induced plasma pyrolysis of silane using a multi-stage reaction and cooling process, where silane gas is injected into a high-temperature plasma thermal field, cooled, and collected using a filter system with periodic blowback airflow to produce nanosilicon powder.
The method achieves high silane decomposition rates (>99%), ensures product purity, reduces safety hazards, and enables continuous production of nanosilicon powder with controlled particle size and shape, suitable for industrial use.
Smart Images

Figure 2024541146000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of materials chemistry technology, and in particular to a method for producing nanosilicon powder from induction plasma pyrolysis silane. [Background technology]
[0002] With the development of new energy related industries and the popularity of 3C electronic products, people are seeking higher requirements for lithium-ion batteries, such as larger volume / mass energy density, faster charge / discharge rate, and higher safety. Silicon materials have about 10 times the energy density of graphite, making them a strong competitor for the negative electrode material of lithium-ion batteries. However, when silicon is used as a negative electrode material, it has a rather serious drawback that it expands to about three times its original volume after lithium absorption, which restricts its application in this field. Nanosilicon powder can effectively reduce this negative effect due to its nano effect. By mixing and using nanosilicon powder with carbon-coated surface and graphite, the capacity and effective service life of lithium-ion batteries can be effectively improved, and the expansion rate of the negative electrode material can be controlled within an acceptable range. In addition, nanosilicon powder has a wide application prospect in other fields. For example, nanosilicon powder and diamond are mixed under high pressure to form silicon carbide, which is widely used as abrasive grains, grinding wheels, and cutting tools. Nanosilicon powder can react with organic matter and be used as a raw material for organic silicone polymer materials.
[0003] At present, the methods for producing nano silicon powder include mechanical ball milling, chemical vapor deposition, molten salt electrolysis, plasma evaporation condensation and the like. Mechanical ball milling generally uses zirconia as a milling medium to grind silicon particles with a relatively large particle size into silicon powder with a relatively small size, and the advantages are that the steps are simple and the cost is relatively low. However, the content of impurities in the obtained silicon powder is high, the shape and particle size range of the particles are difficult to control, and it is very difficult to obtain nano-scale products. Chemical vapor deposition heats silane in a high-purity hydrogen diluted atmosphere until it decomposes, and then cools it to obtain nano silicon powder. However, the production process involves high pressure and high concentration hydrogen gas and silane, which has a large potential safety risk. In the molten salt electrolysis method, the size of the silicon particles produced by electrolyzing SiO2 with anhydrous CaCl2 as the electrolyte is non-uniform, and it is difficult to control the further enlargement of the silicon particles. The plasma evaporation condensation method generally adopts micron-scale silicon powder as raw material, uses DC arc plasma as a heat source to instantly vaporize the silicon raw material, and cools the silicon vapor to produce nano-silicon powder. In the production process, contamination caused by the vaporization of electrode materials is easily induced, and the thermal coupling efficiency between the micron-scale raw material powder and plasma is low, making it difficult to ensure the purity and yield of the product.
[0004] Therefore, it is a technical problem that a person skilled in the art must urgently solve to provide a method for producing nanosilicon powder from induction plasma pyrolysis silane, which has a high decomposition rate of silane, strong safety, and is capable of continuous production. Summary of the Invention [Problem to be solved by the invention]
[0005] In view of this, the present invention provides a method for producing nanosilicon powder from induction plasma pyrolysis silane. [Means for solving the problem]
[0006] In order to achieve the above object, the present invention adopts the following technical solutions.
[0007] A method for producing nanosilicon powder from induction plasma pyrolysis silane, comprising the steps of exciting a working gas in an induction plasma reactor to form a stable high-temperature plasma, mixing silane gas with a dilution gas and injecting the mixture into a high-temperature plasma thermal field, decomposing the silane gas under the cooperative action of the hot air flow in the high-temperature plasma thermal field and the high-temperature circulating cooling air flow, and condensing the silicon atoms or silicon ions produced by pyrolysis into nano-scale spherical silicon powder after cooling; allowing the air flow containing the silicon powder to enter a collection chamber including a filter, depositing the nanosilicon powder on the surface of the filter after passing through the filter, and collecting the nanosilicon powder by blowing it down with a periodic backflow air flow.
[0008] Furthermore, the above method specifically comprises: (1) flushing the entire pyrolysis system with argon gas or nitrogen gas and conducting a leak check; (2) flowing the working gas into the plasma reactor, and forming a stable high-temperature plasma of a predetermined power through excitation; and using a compressor to flow a high-temperature circulating cooling air flow into the first high-temperature cooling region, and flowing a low-temperature circulating cooling air flow and a nitrogen gas cooling air flow into the second low-temperature cooling region; (3) using a feeding probe to inject silane gas into the high-temperature plasma thermal field while wrapping it in dilution gas flow, decomposing the silane in the high-temperature plasma thermal field, and cooling the silicon atoms or silicon ions generated by pyrolysis in the first high-temperature cooling area to form fine silicon powder, while the undecomposed silane gas is further pyrolyzed to generate silicon powder and hydrogen gas, and the silicon powder is transported by the mixed gas flow to the second low-temperature cooling area for further cooling; The silicon powder cooled in the secondary low-temperature cooling region is transported to a collection chamber by the mixed gas flow, and after the gas passes through a filter in the collection chamber, a portion of the gas is treated and then discharged, while the remaining gas is repeatedly used as a circulating cooling gas. The nanosilicon powder is trapped by the filter and deposited on the surface of the filter, and then blown down by a periodic backflow of air, and the nanosilicon powder is collected. (4)
[0009] Furthermore, the working gas includes a center gas and a sheath gas.
[0010] Furthermore, the center gas is argon gas with a flow rate of 5 to 100 slpm, the sheath gas is a mixed gas of argon gas and hydrogen gas, the flow rate of the argon gas in the sheath gas is 20 to 250 slpm, and the flow rate of the hydrogen gas in the sheath gas is 0 to 30 slpm.
[0011] The beneficial effects of adopting the above-mentioned further solution are as follows: By introducing an appropriate amount of hydrogen gas into the sheath gas, the thermal conductivity of the plasma thermal flow can be effectively improved, and the heating efficiency of the plasma thermal field can be further improved.
[0012] Furthermore, in step (2), the power of the plasma reactor is 15-80 kW, and the operating pressure of the system is 14-17 Psig.
[0013] The beneficial effects of adopting the above further solution are as follows: The working pressure of the system is set to about 1 atmosphere, which can reduce the airtightness requirement of the system and reduce the possibility of causing a fire or explosion hazard when a relatively large leak occurs in the system.
[0014] Furthermore, the high-temperature circulating cooling airflow is a mixed gas of nitrogen gas, argon gas and hydrogen gas, the temperature of the high-temperature circulating cooling airflow is 420 to 650° C., and the flow rate is 1000 to 3000 slpm.
[0015] Furthermore, in the mixed gas of the high-temperature circulating cooling airflow, the volume ratio of nitrogen gas, argon gas and hydrogen gas is 50% nitrogen gas, 40% argon gas and 10% nitrogen gas.
[0016] Furthermore, the low-temperature circulating cooling airflow is a mixed gas of nitrogen gas, argon gas and hydrogen gas, the temperature of the low-temperature circulating cooling airflow is 18 to 35° C., the flow rate is 5000 to 15000 slpm, and the flow rate of the nitrogen gas cooling airflow is 150 to 450 slpm.
[0017] Furthermore, in the mixed gas of the low-temperature circulating cooling airflow, the volume ratio of nitrogen gas, argon gas and hydrogen gas is 50% nitrogen gas, 40% argon gas and 10% nitrogen gas.
[0018] The beneficial effects of adopting the above-mentioned further solution are as follows: By adopting nitrogen gas with a relatively low price as the main cooling gas, the production cost can be effectively reduced, and at the same time, nitrogen gas has a relatively high specific heat capacity, and the cooling efficiency can be effectively improved. By adopting the circulating cooling air flow with a relatively high temperature (higher than the thermal decomposition temperature of silane gas) as the primary cooling, it can cool silicon atoms or silicon ions to generate silicon particles, and at the same time, it can provide energy and reaction atmosphere for a small amount of unreacted silane gas as a supplementary heat source, and greatly improve the thermal decomposition rate of silane gas (greater than 99%). By adopting the ultra-large flow rate low-temperature circulating gas as the secondary cooling, it can effectively prevent the silicon particles generated by the reaction from becoming larger, and the temperature of the gas in the system can be controlled within a relatively low range as the main cooling means, effectively avoiding the interference of powder with the cooling process, and achieving the purpose of long-term stable operation.
[0019] Furthermore, the flow rate of the silane gas flow is 15 to 120 slpm, and the dilution gas flow is argon gas with a flow rate of 50 to 200 slpm.
[0020] The beneficial effects of the above-mentioned further solution are as follows: the use of silane as raw material gas can realize molecular-level contact between the raw material and the plasma thermal field, and improve the thermal coupling efficiency; at the same time, the generation of micron-scale large particles formed due to the incomplete vaporization of crude silicon powder when crude silicon powder is used as raw material can be avoided; the introduction of dilution gas restricts the flow direction of silane gas, and prevents it from dissipating before being injected into the high-temperature thermal field; at the same time, the dilution gas can initially dilute the silane gas before it is injected, which contributes to the generation of nano-silicon powder products with smaller particle size.
[0021] Furthermore, the blowback gas is argon gas or nitrogen gas.
[0022] The beneficial effects of adopting the above-mentioned further solution are as follows: By using argon gas or nitrogen gas as the blowing gas, the blowing step can be completed without introducing more kinds of gases, and the complexity of the process conditions can be reduced. Effect of the Invention
[0023] The beneficial effects of the present invention are as follows: The present invention uses silane gas as raw material, induction plasma as the main heat source, and general electric heating tube as the auxiliary heat source, and produces nano silicon powder by multi-stage reaction and multi-stage cooling. This method has the advantages of high silane decomposition rate, strong safety, and continuous production.
[0024] The present invention employs induction plasma as the main heat source, thereby enabling concentrated heating of the raw material gas under the condition that the raw material and the equipment do not come into contact with each other at all, without causing contamination of the electrodes, contributing to improving the purity of the product, preventing the powder generated by the reaction in the heating process from adhering to the surface of the heating device, improving the heating efficiency, and reducing the maintenance costs of the equipment, which is advantageous for industrial continuous production.
[0025] The present invention uses silane gas as raw material to realize molecular level contact between raw material and plasma hot airflow, greatly improving thermal coupling efficiency and improving energy utilization rate. At the same time, the use of silane gas as raw material can avoid the generation of micron-scale large particles formed due to incomplete vaporization of crude silicon powder when crude silicon powder is used as raw material for production, which is favorable for improving the quality of nano silicon powder products in terms of particle size.
[0026] In the present invention, a general electric heating tube is used as an auxiliary heat source, combined with an induction plasma heat source, and a multi-stage reaction and multi-stage cooling mode is newly introduced, which fully exerts the advantages of the two heating modes, and greatly improves the thermal decomposition rate of silane gas. By adopting the method described in the present invention, the thermal decomposition rate of silane can reach more than 99%, effectively improving the utilization rate of silane gas, reducing the environmental protection costs for treating exhaust gas, and further achieving the purpose of reducing production costs.
[0027] In the manufacturing process of the present invention, about 90% of the working gas is reused and used as a cooling airflow with a super-high flow rate, which can not only effectively control the particle size of the nanoparticles, but also reduce the amount of working gas used and save costs. At the same time, the working gas with a relatively large flow rate can dilute the total concentration of hydrogen gas and silane in the system to less than 10%, which can greatly reduce the possibility of leakage and danger in the system in extreme cases.
[0028] The present invention uses a feed probe with a double-layer coaxial tube structure to feed the raw material, and the silane gas is wrapped in an argon gas curtain and directly injected into the high-temperature plasma thermal field, which not only prevents the silane gas from escaping before entering the plasma thermal field, but also uses argon gas to initially dilute the silane gas, contributing to improving the heating efficiency and reducing the particle size of the nanosilicon powder.
[0029] The present invention performs gas-solid separation using a long cylindrical filter bank made of porous cermet material, and by blowing back the filters one by one with a periodic backflow of air, it achieves higher filtering efficiency and a longer usage cycle than conventional bug catchers, and enables long-term continuous production.
[0030] The nanosilicon powder produced by the present invention has an average particle size of 30 to 120 nm, which is adjustable, and has the characteristics of high purity, narrow distribution, spherical shape, easy dispersion, excellent fluidity, large specific surface area, and high surface activity.
[0031] The present invention further provides an apparatus for producing nanosilicon powder from the above-mentioned induction plasma pyrolysis silane, the apparatus including a plasma generator, a feed probe, a primary high-temperature cooling zone, a secondary low-temperature cooling zone, a collection chamber, a filter, a compressor, an electric heating tube, a water-cooled heat exchanger, and an exhaust gas treatment device.
[0032] wherein the plasma generator and the feed probe are both fixed to the primary high-temperature cooling area, the secondary low-temperature cooling area is fixed to a bottom end of the primary high-temperature cooling area, the bottom end of the secondary low-temperature cooling area is connected to one side of a collection chamber, the other side of the collection chamber is connected to a water-cooled heat exchanger, a compressor is installed between the collection chamber and the water-cooled heat exchanger, an electric heating tube is installed between the compressor and the water-cooled heat exchanger, and an exhaust gas treatment device is installed between the compressor and the collection chamber, A high-temperature circulating cooling air inlet is provided on the surface of the first high-temperature cooling area, a low-temperature circulating cooling air inlet is provided in the second low-temperature cooling area, and a nitrogen gas cooling air inlet is further provided in the low-temperature circulating cooling air inlet; A powder collection tank is disposed at the bottom end of the collection chamber, and a filter is disposed within the collection chamber.
[0033] Furthermore, the structure of the feed probe is a double-layered coaxial tube, the inner tube is a silane gas channel, and the middle layer between the inner and outer tubes is a dilution gas flow channel. Three to four of the feed probes are provided.
[0034] Furthermore, 10 to 30 filters are provided in the collection chamber, the material of the filters is porous cermet, and the shape of the filters is a long cylinder. [Brief description of the drawings]
[0035] [Figure 1] FIG. 1 is a schematic flow chart of the apparatus structure and method for producing nanosilicon powder from induction plasma pyrolysis silane of the present invention. [Diagram 2] 1 is an electron microscope photograph of a nanosilicon powder sample produced in Example 1 according to the present invention. [Diagram 3] 1 is an electron microscope photograph of a nanosilicon powder sample produced in Example 2 according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0036] The following clearly and completely describes the technical solutions in the embodiments of the present invention in conjunction with the drawings in the embodiments of the present invention, and of course, the described embodiments are only some of the embodiments of the present invention, and not all of the embodiments. All other embodiments obtained by those skilled in the art based on the embodiments in this application without any creative effort are all within the scope of protection of this application.
[0037] The purity of the silane used in the present embodiment is 99.9999%, the purity of the hydrogen gas is 99.999%, the purity of the argon gas is 99.999%, and the purity of the nitrogen gas is >99.99%. EXAMPLES
[0038] 1) Preparation process: The system was cleaned for 10 minutes using argon gas with a flow rate of 300slpm, and a leak test was performed. The leak test process is divided into high pressure leak test and low pressure leak test. The pass standards are as follows: when the system is at a high pressure of 18psi, the leak rate is less than 5slpm, and when the system is at a low pressure of 2psi, the leak rate is less than 2slpm. 30slpm of center gas (argon gas) and sheath gas (a mixture of 90slpm argon gas and 10slpm hydrogen gas) were flowed into the induction plasma generator. The induction plasma was excited, the system pressure was adjusted to 14.5psi, and the power of the induction plasma generator was adjusted to 40kw. Then, the compressor was started, and a 1500slpm, 430℃ high temperature circulating cooling airflow was flowed into the primary high temperature cooling area, and a 6500slpm, 28℃ low temperature circulating cooling airflow and a 250slpm nitrogen gas cooling airflow were flowed into the secondary low temperature cooling area.
[0039] 2) Reaction process: A total of 30slpm of silane gas was flowed through the inner tubes of the three feed probes, and a total of 90slpm of argon gas was flowed as a dilution gas in the intermediate layer between the inner and outer tubes. The silane gas was enveloped and diluted by the argon gas and directly injected into the plasma hot air stream whose core temperature reached 10,000℃, and was rapidly decomposed into silicon and hydrogen in atomic or ionic states. When passing through the first high-temperature cooling area, the silicon atoms or ions were rapidly cooled to form fine silicon particles. At the same time, a small amount of silane gas that was not decomposed was further pyrolyzed in this area to produce fine silicon particles and hydrogen gas. Then the mixed gas carried the silicon powder into the second low-temperature cooling area, and after cooling, the temperature of the gas and silicon powder dropped rapidly to below 200℃.
[0040] 3) Collection process: The silicon powder produced in the reaction zone was carried to the collection chamber by the airflow. Here, after passing through multiple filters hung in the collection chamber, a part of the gas was burned and cleaned by exhaust gas treatment and then discharged, and the remaining gas was compressed by a compressor and reused repeatedly, a part was heated by an electric heating tube and then flowed to the primary high-temperature cooling zone, and another part was cooled by a water-cooled heat exchanger and then flowed to the secondary low-temperature cooling zone. The nanosilicon powder was blocked by the filter and deposited on the surface of the filter. Argon gas was adopted as the blowback airflow to blow back the multiple filters one by one periodically, and the deposited nanosilicon powder was blown down into the powder collection tank at the bottom of the collection chamber. The reaction process continued for 8 hours, and the powder collection tank was replaced online and collected after stopping, resulting in a total of 15.8 kg of nanosilicon powder.
[0041] The nanosilicon powder obtained in this example is a light yellow powder, with a BET average particle size of 61 nm, and the particle shape is spherical or nearly spherical, as shown in FIG. EXAMPLES
[0042] Example 1 is repeated with the following differences:
[0043] In step 1), 40slpm of center gas (argon gas) and sheath gas (mixture of 120slpm argon gas and 15slpm hydrogen gas) were flowed into the induction plasma generator. The induction plasma was excited, the system pressure was adjusted to 14.7psi, and the power of the induction plasma generator 1 was adjusted to 60kW. Then, the compressor was started, and 1700slpm of 450°C high-temperature circulating cooling airflow was flowed into the primary high-temperature cooling area, and 7500slpm of 30°C low-temperature circulating cooling airflow and 300slpm of nitrogen gas cooling airflow were flowed into the secondary low-temperature cooling area.
[0044] In step 2), a total of 60 lpm of silane airflow was flowed through the inner tubes of the three feed probes, and a total of 150 slpm of argon gas was flowed as a dilution airflow through the intermediate layer between the inner and outer tubes.
[0045] In step 3), the reaction process was continued for 24 hours, the powder collection tank 14 was replaced online, and collected after stopping, to obtain a total of 86.2 kg of nanosilicon powder.
[0046] The nanosilicon powder obtained in this example is a dark yellow powder, with a BET average particle size of 98 nm, and the particle shape is spherical or near spherical, as shown in FIG.
[0047] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are illustrative and should not be construed as limiting the present invention, and that those skilled in the art may make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention. [Explanation of symbols]
[0048] 1-induction plasma generator, 2-center gas, 3-sheath gas, 4-feeding probe, 5-silane airflow, 6-dilution airflow, 7-first-stage high-temperature cooling area, 8-second-stage low-temperature cooling area, 9-high-temperature circulating cooling airflow inlet, 10-low-temperature circulating cooling airflow inlet, 11-nitrogen gas cooling airflow inlet, 12-collection chamber, 13-filter, 14-powder collection tank, 15-compressor, 16-electric heating tube, 17-water-cooled heat exchanger, 18-exhaust gas treatment device
Claims
1. A method for producing nanosilicon powder from silane by induction plasma pyrolysis, comprising the steps of: exciting a working gas in an induction plasma reactor to form a stable high-temperature plasma; mixing silane gas with a dilution gas and injecting the mixture into a high-temperature plasma thermal field; decomposing the silane gas under the combined action of the hot air flow in the high-temperature plasma thermal field and the high-temperature circulating cooling air flow; and condensing the silicon atoms or silicon ions produced by pyrolysis into nano-scale spherical silicon powder after cooling; and allowing the air flow containing the silicon powder to enter a collection chamber including a filter, filtering the nanosilicon powder through the filter, depositing the nanosilicon powder on the surface of the filter, and then blowing down the nanosilicon powder with a periodic blowback air flow.
2. (1) flushing the entire pyrolysis system with argon gas or nitrogen gas and conducting a leak check; (2) flowing the working gas into the plasma reactor, and forming a stable high-temperature plasma of a certain power through excitation; and using a compressor to flow a high-temperature circulating cooling air flow into the first high-temperature cooling region, and flowing a low-temperature circulating cooling air flow and a nitrogen gas cooling air flow into the second low-temperature cooling region; (3) adopting a feeding probe to inject silane gas into the high-temperature plasma thermal field while wrapping it with dilution gas flow, decomposing the silane in the high-temperature plasma thermal field, and cooling the silicon atoms or silicon ions generated by pyrolysis in the first high-temperature cooling area to form fine silicon powder, while further pyrolyzing the undecomposed silane gas to generate silicon powder and hydrogen gas, and transporting the silicon powder to the second low-temperature cooling area by the mixed gas flow for further cooling; The method for producing nanosilicon powder from induction plasma pyrolysis silane according to claim 1, further comprising: (4) transporting the silicon powder cooled in the secondary low-temperature cooling region to a collection chamber by the mixed gas flow; after the gas passes through a filter in the collection chamber, the nanosilicon powder is blocked by the filter and adheres to the surface of the filter, and then blown down by a periodic backflow of gas, thereby collecting the nanosilicon powder.
3. 3. The method for producing nanosilicon powder from induction plasma pyrolysis silane as claimed in claim 2, wherein the working gas comprises a center gas and a sheath gas.
4. The method for producing nanosilicon powder from induced plasma pyrolysis silane according to claim 3, characterized in that: the center gas is argon gas and has a flow rate of 5-100 slpm; the sheath gas is a mixed gas of argon gas and hydrogen gas, the flow rate of argon gas in the sheath gas is 20-250 slpm, and the flow rate of hydrogen gas in the sheath gas is 0-30 slpm.
5. The method for producing nanosilicon powder from induction plasma pyrolysis silane according to claim 2, characterized in that in step (2), the power of the plasma reactor is 15-80 kW, and the working pressure of the system is 14-17 Psig.
6. The method for producing nanosilicon powder from induction plasma pyrolysis silane according to claim 2, characterized in that the high-temperature circulating cooling airflow is a mixed gas of nitrogen gas, argon gas and hydrogen gas, the temperature of the high-temperature circulating cooling airflow is 420-650°C, and the flow rate is 1000-3000slpm.
7. The method for producing nanosilicon powder from induction plasma pyrolysis silane according to claim 2, characterized in that the low-temperature circulating cooling airflow is a mixed gas of nitrogen gas, argon gas and hydrogen gas, the temperature of the low-temperature circulating cooling airflow is 18-35°C, the flow rate is 5000-15000 slpm, and the flow rate of the nitrogen gas cooling airflow is 150-450 slpm.
8. 3. The method for producing nanosilicon powder from induction plasma pyrolysis silane according to claim 2, wherein the flow rate of the silane gas stream is 15-120 slpm, and the dilution gas stream is argon gas with a flow rate of 50-200 slpm.
9. 3. The method for producing nanosilicon powder from induction plasma pyrolysis silane as claimed in claim 2, wherein the blowback gas is argon gas or nitrogen gas.
Citation Information
Patent Citations
Preparation method for nanometer silicon powder
CN108101061A
Nanoscale crystalline silicon powder