Polyolefin Filament

A polyolefin composition of propylene and butene-1 polymers with specific properties addresses the balance of toughness and elongation in filaments, enhancing their performance for applications like nets and ropes.

JP2024541401AInactive Publication Date: 2024-11-08BASELL POLIOLEFINE ITALIA SRL
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024529274
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-10
Filing Date
2022-12-05
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing polyolefin filaments struggle to achieve a balance between toughness and elongation, which is crucial for applications such as nets, ropes, and brushes.

Method used

A polyolefin composition comprising 40-78% propylene polymer and 22-60% butene-1 polymer with specific characteristics, including flexural modulus, melt flow indices, and xylene solubility, is used to produce filaments with enhanced toughness and elongation properties.

Benefits of technology

The filaments exhibit an elongation at break of 80% or more and a stretching ratio of 45 or less, providing improved balance and performance for applications like nets, ropes, and brushes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541401000001
    Figure 2024541401000001
  • Figure 2024541401000002
    Figure 2024541401000002
  • Figure 2024541401000003
    Figure 2024541401000003
Patent Text Reader

Abstract

The present disclosure discloses a stretched polyolefin filament having an elongation at break EB of 80% or more and a ratio SR / EB (SR is a stretching ratio) of 45 or less. The stretched polyolefin filament of the present disclosure comprises a polyolefin composition (I), which comprises A) 40 to 78% by weight of a propylene polymer and B) 22 to 60% by weight of a butene-1 polymer having the following characteristics: 1) a flexural modulus value of 100 to 800 MPa; 2) a ratio MI 10 / MI2 is 20 to 40, 3) the content of the xylene soluble fraction at 0°C is 15% by weight or less. The amount of A) and B) is the total weight of A) + B).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to polyolefin filaments. [Background technology]

[0002] The term "filament" is commonly used to distinguish fibers in textile and carpet applications.

[0003] Thus, the filaments of the present invention are preferably characterized by a titer of at least 500 denier (hereinafter "den").

[0004] Typical applications for this filament are ropes and threads for netting, geotextiles and protective netting in the agricultural and building industries.

[0005] According to WO2012049132, filaments, monotapes or drawn tapes having good mechanical properties are obtained from a composition comprising a propylene polymer and up to 95% by weight of a butene-1 polymer. Summary of the Invention [Problem to be solved by the invention]

[0006] However, in many finished products, an improved balance of toughness and elongation is desirable. It has now been found that such an objective can be achieved by producing filaments from a polyolefin composition that combines polypropylene with a specific butene-1 polymer.

[0007] The present disclosure therefore provides a stretched polyolefin filament having an elongation at break EB of 80% or more, preferably 90% or more, in particular 80% to 130%, or 90% to 130%, and a ratio SR / EB (SR is the stretch ratio) of 45 or less, preferably 40 or less, the lower limit being in all cases preferably 15, more preferably 23, most preferably 25, the stretched polyolefin filament comprising a polyolefin composition (hereinafter referred to as "polyolefin composition (I)"), said polyolefin composition (I) comprising A) 40 to 78% by weight, preferably 45 to 75% by weight, of a propylene polymer; B) 22 to 60% by weight, preferably 25 to 55% by weight, of a butene-1 polymer having the following characteristics: 1) The flexural modulus is 100 to 800 MPa, more preferably 250 to 600 MPa, and most preferably 300 to 600 MPa; 2) Philippine MI 10 / MI2 is 20 to 40, preferably 25 to 35, and MI 10 is the melt flow index MI at 190°C and a load of 10 kg, and MI2 is the melt flow index MI at 190°C and a load of 2.16 kg, both measured in accordance with ISO 1133-1:2011. 3) the content of xylene soluble fraction at 0° C., based on the total weight of B), is not more than 15% by weight, preferably not more than 10% by weight, the preferred lower limit being 0.5% by weight in all cases; The amounts of A) and B) refer to the total weight of A)+B), the breaking elongation is measured on one filament 7 days after production using a dynamometer with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min, and the flexural modulus is measured 10 days after molding according to standard ISO 178:2010.

[0008] The balance of tenacity and elongation makes the filaments of the present invention particularly useful in making netting, ropes and brushes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The polyolefin filaments of the invention preferably have the following additional characteristics, measured on a single filament 7 days after production using a dynamometer with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min: a toughness of at least 1.9, more preferably at least 1.95, in particular between 1.9 and 3, or between 1.95 and 3; and / or - The breaking load must be between 2.5 and 5 kg.

[0010] As used herein, the expression "propylene polymer" includes polymers selected from propylene homopolymers, propylene copolymers, especially random copolymers, and mixtures thereof.

[0011] Similarly, as used herein, the expression "butene-1 polymer" includes polymers selected from butene-1 homopolymers, butene-1 copolymers, and mixtures thereof.

[0012] In the polyolefin composition of the present invention, when A) consists of or comprises one or more propylene copolymers, such copolymers may preferably comprise one or more comonomers selected from ethylene and CH22=CHR alpha-olefins, where R is a C2-C8 alkyl radical, in particular butene-1, pentene-1, 4-methyl-pentene-1, hexene-1 and octene-1.

[0013] Ethylene, butene-1 and hexene-1 are preferred.

[0014] When B) consists of or comprises one or more butene-1 copolymers, such copolymers may comprise one or more comonomers preferably selected from ethylene, propylene and CH2=CHR alpha-olefins, where R is a C3-C8 alkyl radical, in particular pentene-1, 4-methyl-pentene-1, hexene-1 and octene-1. Ethylene, propylene and hexene-1 are preferred. From the above definition it is apparent that the term "copolymer" includes polymers containing two or more types of comonomers.

[0015] In one embodiment, the propylene polymer component A) may have at least one of the following additional features:

[0016] the comonomer content (A) is between 0.5 and 15% by weight, in the case of copolymers, more preferably between 1 and 12% by weight, and in particular between 0.5 and 6% by weight, in particular when the comonomer is ethylene or hexene-1,

[0017] - MIL is 0.1 to 400 g / 10 min, in particular 0.5 to 150 g / 10 min or 0.5 to 100 g / 10 min, MIL being the melt flow index at 230 °C and 2.16 kg load, measured according to ISO 1133-2:2011;

[0018] The amount of insoluble fraction in xylene at 25° C. is at least 85% by weight, more preferably at least 90% by weight, especially at least 95% by weight for propylene homopolymers, the upper limit being preferably 99% for all homopolymers and 96% for all copolymers.

[0019] the flexural modulus is higher than 200 MPa, more preferably higher than 400 MPa, the upper limit being preferably in all cases 2000 MPa.

[0020] Both the propylene homopolymers and propylene copolymers are known in the art and are commercially available.

[0021] Examples of commercially available propylene homopolymers and copolymers are the polymer products sold under the trademark Moplen by LyondellBasell Industries.

[0022] These can be produced by using Ziegler-Natta catalysts or metallocene-based catalyst systems in the polymerization process.

[0023] Typically, Ziegler-Natta catalysts comprise the reaction product of an organometallic compound of Group 1, 2 or 13 of the Periodic Table of the Elements with a transition metal compound of Groups 4 to 10 of the Periodic Table of the Elements (new notation). In particular, the transition metal compound can be selected from among compounds of Ti, V, Zr, Cr, Hf, preferably supported on MgCl2.

[0024] Particularly preferred catalysts include the reaction product of said organometallic compounds of Groups 1, 2 or 13 of the Periodic Table of the Elements with a solid catalyst component comprising a Ti compound and an electron donor compound supported on MgCl2.

[0025] The preferred organometallic compounds are aluminum alkyl compounds.

[0026] Thus, preferred Ziegler-Natta catalysts are those which comprise the reaction product of: 1) a solid catalyst component comprising a Ti compound, preferably a halogenated Ti compound, in particular TiCl4, and an electron donor supported on MgCl2 (internal electron donor); 2) an aluminum alkyl compound (cocatalyst), and, optionally, 3) Electron donor compound (external electron donor).

[0027] The solid catalyst component (1) contains as electron donor a compound generally chosen from among ethers, ketones, lactones, compounds containing N, P and / or S atoms, and mono- and dicarboxylic acid esters.

[0028] Catalysts having the above mentioned properties are well known in the patent literature. Particularly advantageous are the catalysts described in US Pat. No. 4,399,054 and EP Pat. No. 45977.

[0029] Among the internal electron donor compounds, particularly preferred are phthalic acid esters, preferably diisobutyl phthalate and succinic acid esters.

[0030] Other internal electron donors are particularly suitable, as shown in published European patent applications EP-A-361 493 and 728769, including 1,3-diethers.

[0031] As cocatalyst (2) it is preferred to use trialkylaluminum compounds such as Al-triethyl, Al-triisobutyl and Al-tri-n-butyl.

[0032] Electron donor compounds (3) that can be used as external electron donors include aromatic acid esters (such as alkyl benzoates), heterocyclic compounds (such as 2,2,6,6-tetramethylpiperidine and 2,6-diisopropylpiperidine), and especially silicon compounds containing at least one Si-OR bond (where R is a hydrocarbon radical).

[0033] Useful silicon compounds include (tert-butyl)2Si(OCH3)2, (cyclohexyl)(methyl)Si(OCH3)2, (phenyl)2Si(OCH3)2, and (cyclopentyl)2Si(OCH3)2.

[0034] The above 1,3 diethers are also suitable as external electron donors. When the internal electron donor is any of the above 1,3-diethers, the external electron donor can be omitted.

[0035] By pre-contacting the catalyst with a small amount of olefin (prepolymerization), keeping it in suspension in a hydrocarbon solvent, and polymerizing it at temperatures ranging from room temperature to 60°C, it is possible to produce a polymerization amount of 0.5 to 3 times the weight of the catalyst.

[0036] The operation can also be carried out in liquid monomer, producing amounts of polymer up to 1000 times the weight of the catalyst.

[0037] Preferred examples of metallocene-based catalyst systems are disclosed in US 20060020096 and WO 98040419.

[0038] The polymerization conditions used with the above catalysts are also generally well known.

[0039] The polymerization can be carried out in one stage or in two or more stages under different polymerization conditions.

[0040] It can occur in the liquid phase (e.g., using liquid propylene as a diluent), gas phase, or liquid-gas phase.

[0041] Conventional molecular weight regulators known in the art, such as chain transfer agents (eg, hydrogen or ZnEt2), can be used.

[0042] The polymerization temperature is preferably from 40 to 120°C, and more preferably from 50 to 80°C.

[0043] The polymerization pressure may be atmospheric or higher.

[0044] When polymerizing in liquid propylene, the pressure is competitive with the vapor pressure of liquid propylene at the operating temperature used, and may be modified by the vapor pressure of small amounts of inert diluent used to provide the catalyst mixture, any monomer overpressure, and hydrogen used as a molecular weight regulator.

[0045] In particular, the propylene polymer A) can be produced by a polymerization process carried out in a gas phase polymerization reactor comprising at least two interconnected polymerization zones, as shown in European Patent Application No. 782587.

[0046] In detail, the method is carried out in first and second interconnected polymerization zones, into which propylene and any comonomers are fed in the presence of a catalyst system and from which the polymer produced is discharged. In said process, the growing polymer particles flow upwards through one of said polymerization zones (the riser) under fast fluidization conditions, leave said riser into another (second) polymerization zone (the downcomer) through which they flow downwards in dense form, leave said downcomer under the action of gravity and are reintroduced into the riser, thus establishing a polymer circulation between the riser and the downcomer.

[0047] In the downcomer, the density of the solids reaches high values ​​and approaches the bulk density of the polymer. Thus, a positive increase in pressure is obtained along the direction of flow, which makes it possible to reintroduce the polymer into the riser without the help of special mechanical means. In this way, a "loop" circulation is established, which is determined by the balance of pressure between the two polymerization zones and the head losses introduced into the system.

[0048] Generally, the conditions of fast fluidization in the riser are established by feeding a gas mixture containing the relevant monomers to said riser. The feeding of the gas mixture is preferably carried out below the reintroduction point of the polymer into said riser, optionally by using gas distribution means. The velocity of the transport gas to the riser is higher than the transport velocity under operating conditions, preferably between 2 and 15 m / s.

[0049] Typically, the polymer and gas mixture leaving the riser is conveyed to a solid / gas separation zone. Solid / gas separation can be accomplished using conventional separation means. From the separation zone, the polymer enters the downcomer. The gaseous mixture leaving the separation zone is compressed, cooled, and transferred to the riser, optionally with the addition of make-up monomer and / or molecular weight regulator. Transfer can be accomplished using a gaseous mixture recycle line.

[0050] Control of the polymer circulation between the two polymerization zones can be achieved by metering the amount of polymer exiting the downcomer using any suitable means for controlling the flow of solids, such as a mechanical valve.

[0051] The process may be carried out under an operating pressure of 0.5 to 10 MPa, preferably 1.5 to 6 MPa.

[0052] Optionally, an inert gas such as nitrogen or an aliphatic hydrocarbon may be maintained in the polymerization zone in an amount such that the sum of the partial pressures of the inert gas is preferably 5 to 80% of the total gas pressure.

[0053] The catalyst can be fed to the riser at any point in the riser. However, it can also be fed to any point in the downcomer. The catalyst can be in any physical state, so that a catalyst in a solid or liquid state can be used.

[0054] The butene-1 polymers component B) are known to those skilled in the art and are commercially available, as shown in the examples.

[0055] The butene-1 polymer component B) is preferably a highly isotactic linear polymer.

[0056] In particular, the butene-1 polymer component B) operates at 150.91 MHz. 13 It has an isotacticity of 90-99%, more preferably 93-99%, and most preferably 95-99%, as measured by C-NMR as mmmm pentads / total pentads or as the amount by weight of xylene insolubles at 0° C.

[0057] The butene-1 polymer component B) preferably has an MI2 value of 0.05 to 50 g / 10 min, more preferably 0.1 to 10 g / 10 min.

[0058] Butene-1 polymer component B) MI 10The value is preferably from 1 to 100 g / 10 minutes, and more preferably from 2 to 50 g / 10 minutes.

[0059] In one embodiment, the butene-1 polymer component B) may be a homopolymer.

[0060] In a further embodiment the butene-1 polymer B) may be a copolymer having a comonomer content, in particular a copolymerized ethylene content, of 0.5 to 10 mol %, preferably 0.7 to 9 mol %.

[0061] In a further embodiment, the butene-1 polymer component B) may be a butene-1 polymer composition comprising: B1) butene-1 homopolymers or copolymers of butene-1 with at least one comonomer selected from ethylene, propylene, CH2=CHR olefins as defined above and mixtures thereof, the copolymerized comonomer content being less than or equal to 2 mol %; B2) copolymers of butene-1 and at least one comonomer selected from ethylene, propylene, CH2=CHR olefins as defined above and mixtures thereof, having a copolymerized comonomer content of 3 to 25 mol %, Said composition has a total copolymerizable comonomer content, as the sum of B1)+B2), of 0.5-18 mol %, preferably 0.7-15 mol %.

[0062] The relative amounts of B1) and B2) may range from 10% to 50% by weight of B1), in particular from 15% to 45% by weight, and from 90% to 50% by weight, in particular from 85% to 55% by weight. Said amounts refer to the sum of B1)+B2).

[0063] In one embodiment, the butene-1 polymer component B) may have at least one of the following additional features: Mw is the weight average molar mass as measured by gel permeation chromatography, Mn is the number average molar mass as measured by gel permeation chromatography, and the molecular weight distribution Mw / Mn is greater than or equal to 4, preferably greater than or equal to 5, with an upper limit of preferably 10; the melting point TmII, measured by DSC (differential scanning calorimetry) in a second heating run at a scanning rate of -10 ° C / min, is not more than 125 ° C, preferably not more than 120 ° C, the lower limit being preferably 75 ° C in all cases; -X-ray crystallinity is 25-65%.

[0064] Optionally, the butene-1 polymer component B) may have at least one of the following further additional features: the intrinsic viscosity (IV), measured in tetrahydronaphthalene (THN) at -135°C, is less than or equal to 5 dl / g, preferably less than or equal to 3 dl / g, the lower limit being preferably in all cases 0.4 dl / g; Mw is greater than or equal to 100 000 g / mol, in particular from 100 000 to 650 000 g / mol; - the melting point TmI measured by DSC at a scanning rate of 10°C / min is 95°C to 135°C; -Density: 885-925kg / m 3 , preferably 900 to 920 kg / m 3 , especially 912-920kg / m 3 To be.

[0065] The butene-1 polymer component B) can be obtained using known processes and polymerization catalysts.

[0066] For example, to prepare butene-1 polymer component B), it is possible to use TiCl3-based Ziegler-Natta catalysts and aluminium derivatives such as aluminium halides as cocatalysts, as well as the above-mentioned MgCl2-supported catalyst systems.

[0067] Other examples of internal electron donor compounds when using the supported catalyst systems described above include 3,3-dimethyldiethyl or diisobutyl glutarate.

[0068] Preferred examples of external electron donor compounds are cyclohexyltrimethoxysilane, t-butyltrimethoxysilane, diisopropyltrimethoxysilane and thexyltrimethoxysilane. The use of thexyltrimethoxysilane is particularly preferred.

[0069] Alternatively, the butene-1 polymer component B) can be obtained by polymerizing the monomers in the presence of a metallocene catalyst system obtained by contacting them with: - stereo-rigid metallocene compounds, alumoxanes or compounds capable of forming alkylmetallocene cations, and optionally - Organoaluminum compounds.

[0070] The polymerization process can be carried out with said catalysts by operating in the liquid phase, optionally in the presence of an inert hydrocarbon solvent, or in the gas phase using fluidized bed or mechanically agitated gas phase reactors.

[0071] The hydrocarbon solvent may be either aromatic (such as toluene) or aliphatic (such as propane, hexane, heptane, isobutane, cyclohexane, and 2,2,4-trimethylpentane, isododecane, etc.).

[0072] Preferably, the polymerization process is carried out by using liquid butene-1 as the polymerization medium.

[0073] The polymerization temperature may be between 20°C and 150°C, particularly between 50°C and 90°C, for example 65°C to 82°C.

[0074] To control the molecular weight, molecular weight regulators, in particular hydrogen, are provided to the polymerization environment.

[0075] Mw / Mn values ​​of 4 or greater and MI as previously defined 10 The value of the / MI2 ratio is generally considered to result in a broad molecular weight distribution (MWD).

[0076] Broad molecular weight butene-1 polymers can be obtained in several ways. One method consists in using a catalyst that is capable of producing inherently broad MWD polymers when (co)polymerizing butene-1. Another possibility is to mechanically blend butene-1 polymers with sufficiently different molecular weights using conventional mixing equipment.

[0077] It is also possible to operate according to a multistage polymerization process, in which said butene-1 polymers having different molecular weights are produced in succession in two or more reactors having different reaction conditions, e.g. the concentration of molecular weight regulator fed to each reactor.

[0078] It is also possible to feed different amounts of monomer to each reactor.

[0079] In particular, when the butene-1 polymer component B) contains the two components B1) and B2) described above, the polymerization process can be carried out in two or more reactors connected in series, with components B1) and B2) being prepared separately in subsequent stages, each stage, except the first one, operating in the presence of the polymer formed and of the catalyst used in the previous stage.

[0080] The catalyst can be added to only the first reactor or to multiple reactors.

[0081] The above polymer components can achieve high MI values ​​directly during polymerization, or by subsequent chemical treatment (chemical visbreaking).

[0082] Chemical visbreaking of polymers is carried out in the presence of a free radical initiator such as a peroxide.

[0083] The peroxides most conveniently used in the polymer visbreaking process preferably have a decomposition temperature in the range of 150° C. to 250° C. As the peroxides, for example, di-tert-butyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, etc. are commercially available.

[0084] The amount of peroxide required for the visbreaking process is preferably in the range of 0.001-0.5% by weight of the polymer, more preferably 0.001-0.2%.

[0085] The polyolefin composition (I) is obtained by melt-mixing the components, and the mixing temperature in the mixer is usually 180 to 310°C, preferably 190 to 280°C, and more preferably 200 to 250°C.

[0086] All known devices and techniques can be used for this purpose.

[0087] Useful melt mixing devices in this connection are in particular extruders or kneaders, with twin-screw extruders being particularly preferred. It is also possible to premix the components at room temperature in a mixing device and to feed the mixture thus obtained directly into the device used to produce the filaments.

[0088] During the preparation of the polyolefin composition (I), in addition to the main components A) and B) and other optional components, additives commonly used in the art, such as stabilizers (against heat, light, UV rays), plasticizers, acid inhibitors, antistatic agents, water repellents, pigments, may also be introduced.

[0089] The filaments of the present invention comprise at least 70% by weight of polyolefin composition (I), more preferably at least 80% by weight, in particular at least 90% or 95% by weight of polyolefin composition (I), relative to the total weight of the filament or fiber, the upper limit being in all cases 100% by weight.

[0090] The filaments of the present invention are typically characterized by a cross-section that is rounded (circular, elliptical, lenticular, or more complex such as multilobal) or angular, such as rectangular.

[0091] Filaments with a rounded cross section are also called "monofilaments", whereas filaments with an angular, especially rectangular, cross section are also called "tapes". The definition of "filament" according to the present invention therefore includes said monofilaments and tapes.

[0092] The tape preferably has a thickness of 0.03 to 1 mm and a width of 2 to 20 mm.

[0093] As stated above, the filaments are preferably characterized by a titer of 500 den or greater.

[0094] The filament titer is particularly preferably 800 denier or more, in particular 1000 or 1300 or more, the upper limit being preferably 7000 denier for monofilaments and 25000 denier for tapes. As described above, the filaments are stretched. In particular, the stretch ratio is preferably 3.5:1 to 4.5:1.

[0095] All of the filaments can be used in bundle or reel form for the production of a variety of finished products.

[0096] The polyolefin filaments or fibers of the present invention can be produced using processes and equipment well known in the relevant art.

[0097] Generally, the process for producing polyolefin filaments includes the following steps: (a) The polyolefin composition (I) and other polymeric components, if present, are melted. (b) Spinning filaments or extruding a precursor film or tape. (c) stretching the filaments or precursor film or tape, if not previously stretched, and / or cutting the precursor film or tape and stretching the filaments so obtained.

[0098] The melting step (a) and the spinning or extrusion step (b) are generally carried out continuously in succession by using a single or twin screw extruder equipped with a suitable spinning or extrusion head. Thus, the aforementioned melt mixing step can also be carried out in the same spinning or extrusion equipment.

[0099] The spinning head is equipped with a number of holes having the same shape as the cross-section of the filament (monofilament or tape).

[0100] A film extrusion head is typically a flat or annular die commonly used in the production of films.

[0101] If a precursor film or tape is obtained in step (b), it is cut into tapes of the desired size in step (c) and processed. If the precursor film or tape is subjected to a drawing process, it is not necessary to perform a drawing process on the final filament.

[0102] Usually, the melting step (a) and the spinning / extrusion step (b) are carried out at a temperature predetermined in the melt mixing step, ie, 180 to 310°C, preferably 190 to 280°C, more preferably 200 to 250°C.

[0103] Typical spinning conditions are as follows: -The temperature inside the extruder head is 200-300℃. - The winding speed of the primary web (unstretched) is 1-50 m / min.

[0104] The film extrusion conditions were as follows: -The temperature inside the extruder head is 200-300℃. - Output value is 20-1000 kg / hour (for industrial plants).

[0105] The filaments or precursor film obtained in step (b) are typically cooled, for example using one or more chill rolls or by immersion in water at a temperature between 5 and 40°C.

[0106] To carry out the drawing process, the filament (monofilament or tape) or precursor tape is preheated at a temperature of 40° C. to 120° C. to 140° C. Heating can be achieved, for example, by using a hot air oven, a boiling water bath, a heated roll, or by irradiation or other known means.

[0107] The stretching can be accomplished by passing the precursor tape or filament through a series of rollers having different rotational speeds. The preferred range of stretch ratios thus achieved is a predefined range.

[0108] The draw ratio is the ratio of the fast speed of the rollers in the draw unit to the speed of the rollers in the take-off unit (primary speed). As mentioned before, in the take-off unit the slow moving tape or filament is heated before being drawn at a faster speed. Thus, by dividing the value of such ratio, e.g., 3.5 for 3.5:1, 4.5 for 4.5:1, by the elongation at break, the SR / EB value is obtained. EXAMPLES

[0109] Examples and advantages of the various embodiments, compositions and methods provided herein are disclosed in the following examples, which are merely illustrative and are not intended to limit the scope of the appended claims in any manner.

[0110] The following analytical methods are used to evaluate the polymer composition and filament properties.

[0111] density

[0112] Measured at 23°C according to ISO 1183-1:2012.

[0113] Melt Flow Index

[0114] Measured at 190°C and specified load in accordance with ISO 1133-12012-03.

[0115] Intrinsic viscosity (IV)

[0116] The sample was dissolved in tetrahydronaphthalene at 135°C and then injected into the capillary viscometer. The viscometer tube (Ubbelohde type) was surrounded by a cylindrical glass jacket, which allowed for temperature control by a circulating thermostated liquid. The time of passage down the meniscus was measured by an optoelectronic device.

[0117] The meniscus in front of the upper ramp is realized by starting a counter with a quartz crystal oscillator. When the meniscus passes the lower ramp, the counter is stopped and the flow time is recorded, which is converted into a value of intrinsic viscosity through Huggins' equation (Huggins, ML, J. Am. Chem. Soc., 1942, 64, 2716), provided, however, that the flow time of the pure solvent under the same experimental conditions (same viscometer and same temperature) is known. [η] was measured using single polymer solutions.

[0118] Molecular weight distribution measurement

[0119] The determination of the molar mass distribution and the derived average Mn, Mw, Mz and Mw / Mn were carried out using a GPC-IR instrument from PolymerChar. The instrument was equipped with a column set consisting of four PLgel Olexis mixed beds (Polymer Laboratories) and an IR5 infrared detector (PolymerChar). The column dimensions were 300 × 7.5 mm, with a particle size of 13 μm. The flow rate of the mobile phase was maintained at 1.0 mL / min. All measurements were carried out at 150 °C. The solution concentration was 2.0 mg / mL (at 150 °C), and 0.3 g / L of 2,6-ditert-butyl-p-cresol was added to prevent decomposition. For the GPC calculations, a universal calibration curve was obtained using 12 polystyrene (PS) standard samples provided by PolymerChar (peak molecular weights ranged from 266 to 1220000). A third-order polynomial fit was used to interpolate the experimental data to obtain the relevant calibration curve. Data acquisition and processing were performed using Empower 3 (Waters). The Mark-Houwink relationship was used to determine the molecular weight distribution and associated average molecular weight: K values ​​were calculated as K for PS and polybutene (PB), respectively. PS =1.21×10 -4 dL / g and K PB =1.78×10 -4 dL / g, whereas for PS a Mark-Howinck exponent α of 0.706 and for PB a Mark-Howinck exponent α of 0.725 were used.

[0120] In the case of butene / ethylene copolymers, as far as data evaluation is concerned, for each sample, the composition was assumed to be constant over the entire range of molecular weights, and the K values ​​of the Mark-Houwink relationship were calculated using linear combinations as reported below.

number

[0121] Here, K EB is the copolymer constant. K PE (4.06×10 -4 , dL / g) and KPB (1.78×10 -4 dL / g) is a constant for polyethylene (PE) and PB. x E and x B is the relative weight amount of ethylene and butene, and x E +x B = 1. The Mark-Howink exponent α = 0.725 was used for all butene / ethylene copolymers, independent of their composition. Final processing data processing was modified for all samples to include fractions up to 1000 in terms of molecular weight equivalent. Fractions below 1000 were considered via GC.

[0122] Comonomer Content

[0123] Propylene Polymer A)

[0124] For propylene copolymers, the comonomer content was determined by infrared spectroscopy by collecting IR spectra of the sample and air background using a Fourier transform infrared spectrometer (FTIR). The data collection parameters of the instrument were as follows: -Purge time: minimum 30 seconds. -Collection time: Minimum 3 minutes. -Apodization: Happ-Genzel. -Resolution: 2cm -1 .

[0125] Sample Production

[0126] A thick sheet was obtained by pressing approximately 1 g of sample between two pieces of aluminum foil using a hydraulic press. If there are uniformity issues, it is suggested to perform a minimum of two pressing operations. A small portion was cut from this sheet to form a film. The recommended film thickness range is 0.02-0.05 cm (8-20 mils).

[0127] Press temperature: 180±10℃ (356℃), approx. 10kg / cm 2(142.2 PSI) pressure was applied for approximately 1 minute. The pressure was then released and the sample was removed from the press and allowed to cool to room temperature.

[0128] Spectra of pressed polymer films were plotted as absorbance vs. wavenumber (cm -1 The following measurements were used to calculate the ethylene and butene-1 content: - 4482~3950cm, used for spectroscopic normalization of film thickness -1 The area of ​​the combined absorption bands (At). - 750-700 cm after appropriate successive spectroscopic subtraction of the spectrum of isotactic non-additive polypropylene in the presence of ethylene -1 and, in the presence of butene-1, the area of ​​the absorption band between 800 and 690 cm -1 Reference spectra of butene-1-propylene random copolymers in the range. In the presence of -butene-1, the spectrum of isotactic non-additive polypropylene was appropriately subtracted in two successive spectra at 769 cm -1 (maximum) of the absorption band (DC4), and in the presence of ethylene, 800–690 cm -1 Reference spectra of ethylene-propylene random copolymers in the range.

[0129] To calculate the ethylene and butene-1 content, a calibration line for ethylene and butene-1 is required, obtained using samples of known amounts of ethylene and butene-1.

[0130] Butene-1 Polymer B)

[0131] The comonomer content of the butene-1 polymers was measured via FT-IR.

[0132] Spectra of pressed polymer films were plotted as absorbance vs. wavenumber (cm -1 The following measurements were used to calculate the ethylene content: a) 4482-3950 cm, used for spectroscopic normalization of film thickness-1 The area of ​​the combined absorption band (A t ), b) Spectra of polymer samples and subtraction coefficients (FCR) for digital subtraction between absorption bands due to the sequences of methylene groups (CH2 locking) BEE and BEB (B: 1, butene unit, E: ethylene unit). C2 )vibration) c) The area of ​​the remaining band after subtracting the C2PB spectrum (A C2,block)。 It is derived from the arrangement of methylene groups EEE (CH2 rocking vibration).

[0133] Device

[0134] A Fourier transform infrared spectrometer (FTIR) can be used to perform the spectroscopic measurements reported above.

[0135] A hydraulic press (Carver or equivalent) with platens that can be heated to 200° C. was used.

[0136] method

[0137] Calibration of (BEB+BEE) sequence

[0138] %(BEB+BEE)wt vs. FCR C2 / A t A calibration line is obtained by plotting the slope G r and intercept I r is calculated by linear regression.

[0139] Calibrating the EEE sequence

[0140] %(EEE)wt vs A C2,block / A t A calibration line is obtained by plotting the slope G H and intercept I H is calculated by linear regression.

[0141] Sample preparation

[0142] A thick sheet was obtained by pressing approximately 1.5 g of sample between two pieces of aluminum foil using a hydraulic press. If there are problems with uniformity, it is suggested to perform a minimum of two pressing operations. A small portion was cut from this sheet to form a membrane. The recommended membrane thickness is 0.1-0.3 mm.

[0143] The press temperature is 140(10°C.

[0144] Since changes in the crystalline phase occur over time, it is suggested to collect IR spectra of the sample films immediately after casting.

[0145] procedure

[0146] The data collection parameters of the instrument are as follows: Purge time: 30 seconds minimum. Collection time: Minimum 3 minutes. Apodization:Happ-Genzel. Resolution: 2cm -1 . IR spectra of the samples against an air background were collected.

[0147] calculation The weight concentration of the BEE+BEB sequence of ethylene units was calculated.

number

number

[0148]

number

[0149] X-ray crystallinity determination

[0150] X-ray crystallinity was measured using an X-ray powder diffraction analyzer (XDPD) capable of collecting spectra between diffraction angles 2θ = 5° and 2θ = 35° every 6 seconds with a step size of 0.1° using Cu-Kα1 radiation with a fixed slit.

[0151] The samples were diskettes made by pressing and measuring approximately 1.5-2.5 mm thick and 2.5-4.0 cm in diameter. The diskettes were aged at room temperature (23° C.) for 96 hours.

[0152] After this preparation, the specimen was inserted into the XRPD sample holder. The XRPD instrument was adjusted to collect XRPD spectra of the sample from diffraction angles 2θ = 5° to 2θ = 35° with a step size of 0.1° using a counting time of 6 seconds and collecting a final spectrum at the end.

[0153] Define Ta as the total area between the spectral profile and the baseline in counts / sec·2θ, Aa as the total amorphous area in counts / sec·2θ, and Ca as the total crystalline area in counts / sec·2θ. The spectra or diffraction patterns were analyzed by the following procedure. 1) define an appropriate linear baseline for the entire spectrum and calculate the total area (Ta) between the spectral contour and the baseline; 2) defining an appropriate amorphous profile along the entire spectrum that separates the amorphous regions from the crystalline regions based on a phase model; 3) Calculate the amorphous area (Aa), which is the area between the amorphous contour and the baseline; 4) Calculate the crystalline area (Ca) as the area between the spectral contour and the amorphous contour, e.g. Ca=Ta-Aa; 5) Calculate the crystallinity (%Cr) of the sample using the following formula:

number

[0154] Xylene soluble and insoluble fractions at 25℃ (XS-25℃)

[0155] 2.5 g of polymer was dissolved in 250 ml of xylene with stirring at 135° C. After 20 min, the solution was cooled to 25° C. with stirring and then allowed to stand for 30 min. The precipitate was filtered through filter paper, the solution was evaporated in a nitrogen stream, and the residue was dried under vacuum at 80° C. until a constant weight was reached. Thus, the weight percentage of soluble (xylene soluble-XS) and insoluble polymer at room temperature (25° C.) was calculated.

[0156] The weight percentage of the polymer that is insoluble in xylene at room temperature (25° C.) is considered to be the isotactic index of the polymer. This value corresponds substantially to the isotactic index determined by extraction with boiling n-heptane, which by definition constitutes the isotactic index of propylene polymers.

[0157] Xylene soluble and insoluble fractions at 0℃ (XS-0℃)

[0158] 2.5 g of the polymer sample was dissolved in 250 ml of xylene with stirring at 135 °C. After 30 minutes, the solution was cooled to 100 °C with stirring and then cooled to 0 °C in a water and ice bath. The solution was then left in the water and ice bath for 1 hour. The precipitate was filtered with filter paper. During the filtration, the flask was left in an ice water bath in order to keep the temperature inside the flask as close as possible to 0 °C. During the filtration, the flask was left in an ice water bath in order to keep the temperature inside the flask as close as possible to 0 °C. An aliquot of the solution was evaporated in a nitrogen stream and the residue was dried under vacuum at 80 °C until a constant weight was reached. The weight difference between both residues should be less than 3%. Otherwise, the test must be repeated. Thus, the weight percentage of the polymer solubles (xylene solubles at 0 °C = XS 0 °C) is calculated from the average weight of the residue. The insoluble fraction in o-xylene at 0 °C (xylene insolubles at 0 °C = XI % 0 °C) is:

number

[0159] Melting and crystallization temperatures of butene-1 polymers (B) determined by differential scanning calorimetry (DSC)

[0160] Differential scanning calorimetry (DSC) data were obtained on a PerkinElmer DSC-7 instrument using weighed samples (5–10 mg) sealed in aluminum pans.

[0161] To determine the melting temperature (Tml) of polybutene-1 crystalline form I, the sample was heated to 200°C at a scan rate corresponding to 10°C / min, held at 200°C for 5 minutes, and then cooled to 20°C at a cooling rate of 10°C / min. The sample was then stored at room temperature for 10 days. After 10 days, the sample was subjected to DSC, cooled to -20°C, and then heated to 200°C at a scan rate corresponding to 10°C / min. In this heating procedure, the highest temperature peak of the thermogram was used as the melting temperature (Tml).

[0162] Melting temperature and crystallization temperature T of polybutene-1 crystalline form II (TmII) c To determine the crystallization temperature (T), the sample was heated to 200 °C at a scan rate equivalent to 10 °C / min and held at 200 °C for 5 min to completely melt all crystallites and cancel the thermal history of the sample. It was then cooled to -20 °C at a scan rate equivalent to 10 °C / min to determine the peak temperature as the crystallization temperature (T c ) and the area was taken as the crystallization enthalpy. After standing at -20 °C for 5 min, the sample was heated again to 200 °C with a scan rate corresponding to 10 °C / min. In this second heating run, the peak temperature was taken as the melting temperature of polybutene-1 crystalline form II (TmII) and the area was taken as the melting enthalpy (ΔHfII).

[0163] NMR analysis of chain structure

[0164] 13C NMR spectra were acquired on a Bruker AV-600 spectrometer equipped with a cryoprobe, operating at 120 °C and 150.91 MHz in Fourier transform mode.

[0165] Tβδ carbon peak (CJ Carman, RA Harrington and CE Wilkes, Macromolecules, 10, 3 , 536 (1977)) was used as the internal standard at 37.24 ppm. Samples were dissolved in 1,1,2,2-tetrachloroethane d2 at 120 °C at a concentration of 8% wt / v. Each spectrum was 1 H- 13 Acquired using a 90° pulse, a 15 second delay between pulses, and CPD to remove C coupling. Approximately 512 transients were stored in 32,000 data points using a 9000 Hz spectral window.

[0166] Kakugo[M. Kakugo, Y. Naito, K. Mizunuma and T. Miyatake,<Polymer>, 16, 4 Based on [J.C. Randall, Macromol. Chem Phys., C30, 211 (1989)] and Randall [J.C. Randall, Macromol. Chem Phys., C30, 211 (1989)], the following terms are used to assign values ​​to the spectra and evaluate the ternary distribution and composition: BBB=100(T ββ ) / S=I5 BBE=100T βδ / S=I4 EBE=100P δδ / S=I14 BEB=100S ββ / S=I13 BEE=100S αδ / S=I7 EEE = 100 (0.25S γδ +0.5S δδ ) / S=0.25I9+0.5I10 [Table 1]

[0167] As a first approximation, mmmm was calculated using 2B2 carbons as follows: [Table 2]

[0168]

number

[0169] Filament toughness, elongation at break, and load at break

[0170] Titer in denier is commonly used to measure the size of fibers or filaments in textiles and is defined as the weight (in grams) of 9000m of filament or tape. On a laboratory scale, the actual titer value (in denier) is determined by multiplying the weight of 100m of filament or tape by 90.

[0171] Toughness, elongation at break and load at break are measured on a single filament 7 days after manufacture using a dynamometer such as LLOYD RX-Plus with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min. The load cell provides the load at break (grams or kilograms) and the elongation at break (%) is calculated as follows: (Clamp distance at break-Initial clamp distance / Initial clamp distance)*100.

[0172] The tenacity (at break) is obtained by dividing the breaking load (grams) by the strength (denier).

[0173] Flexural modulus

[0174] The measurements were taken 10 days after molding according to standard ISO 178:2010.

[0175] Example 1, Example 2, and Comparative Example 1

[0176] The following materials were used to prepare the polyolefin composition (I):

[0177] Propylene Polymer A)

[0178] A propylene homopolymer having the properties set out in Table 1 below.

[0179] It is available on the market under the trademark MoplenHP556E sold by LyondellBasell.

[0180] Butene-1 Polymer B)

[0181] Butene-1 homopolymers produced with Ziegler-Natta catalysts in liquid monomer polymerizations have the properties listed in Table 1 below. It is available commercially under the trademark ToppylPB 0110M sold by LyondellBasell. Table I [Table 3]

[0182] Preparation of polyolefin composition (I) and filament spinning

[0183] Components A) and B), including a conventional stabilizing additive composition, were dry mixed in a drum blender for 15 minutes and then spun into filaments of round cross section.

[0184] The equipment used was an extruder Leonard+ gear pump with a diameter of 25 mm and a length of 27 L / D. The die had 10 circular holes and a diameter of 1.2 mm.

[0185] The main process conditions are as follows: Temperature profile:-Cylinder 180-185-190-195℃; - Pump 200℃; - Adapter 205℃; - Head die 210℃; Melting temperature: 212+ / -3℃; Output used: approx. 4kg / h Cooling water bath: 21+ / -1℃; Stretching oven set: 106+ / -2℃(hot air); Annealing oven set: 106+ / -2℃(hot air); Annealing factor: average -5.0% (slow).

[0186] The resulting filament properties are listed for all examples in Table II. Table II [Table 4] Table II continued [Table 5]

Claims

1. Stretched polyolefin filaments having an elongation at break EB of 80% or more, preferably 90% or more, in particular 80% to 130%, or 90% to 130%, and a ratio SR / EB (SR is the stretching ratio) of 45 or less, preferably 40 or less, the lower limit being in all cases preferably 15, more preferably 23, most preferably 25, said stretched polyolefin filaments comprising a polyolefin composition (I), said polyolefin composition (I) being A) 40 to 78% by weight, preferably 45 to 75% by weight, of a propylene polymer; B) 22 to 60% by weight, preferably 25 to 55% by weight, of a butene-1 polymer having the following characteristics: 1) the flexural modulus is 100 to 800 MPa, more preferably 250 to 600 MPa, and most preferably 300 to 600 MPa; 2) Ratio MI 10 / M.I. 2 is 20 to 40, preferably 25 to 35, and MI 10 is the melt flow index MI at 190° C. and a load of 10 kg, and MI 2 is the melt flow index MI at 190°C and a load of 2.16 kg, both of which are measured in accordance with ISO 1133-1:2011; 3) the content of xylene soluble fraction at 0° C. based on the total weight of B) is 15% by weight or less, preferably 15% by weight or less, the lower limit being preferably 0.5% by weight in all cases; Stretched polyolefin filaments, the amounts of A) and B) refer to the total weight of A)+B), the breaking elongation being measured on one filament 7 days after production using a dynamometer with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min, and the flexural modulus being measured 10 days after moulding according to standard ISO 178:2010.

2. 2. The drawn polyolefin filament according to claim 1, having a titer of at least 800 Den.

3. 3. The drawn polyolefin filament according to claim 1 or 2, which is a monofilament.

4. The drawn polyolefin filament according to claim 1 or 2, wherein the SR is from 3.5:1 to 4.5:

1.

5. 3. The drawn polyolefin filament according to claim 1 or 2, further having the following characteristics measured on one filament 7 days after production using a dynamometer with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min: a toughness of at least 1.9, preferably at least 1.95, in particular between 1.9 and 3, or between 1.95 and 3; and / or - The load at break is 2.5 to 5 kg.

6. 3. The drawn polyolefin filament according to claim 1 or 2, wherein the butene-1 polymer B) is selected from butene-1 homopolymers and butene-1 copolymers, and mixtures thereof, having a comonomer content, in particular a copolymerized ethylene content, of 0.5 mol % to 10 mol %, preferably 0.7 mol % to 9 mol %.

7. 3. The drawn polyolefin filament according to claim 1 or 2, wherein said butene-1 polymer B) has a molecular weight distribution Mw / Mn greater than or equal to 4, preferably greater than or equal to 5, the upper limit being in all cases preferably 10, Mw being the weight average molar mass measured by gel permeation chromatography and Mn being the number average molar mass measured by gel permeation chromatography.

8. 3. The drawn polyolefin filament according to claim 1 or 2, wherein said butene-1 polymer B) has one or more of the following additional characteristics: the melting point TmII, measured by DSC (differential scanning calorimetry) in a second heating run at a scanning rate of 10° C. / min, is not more than 125° C., preferably not more than 120° C., the lower limit being in all cases preferably 75° C. g) X-ray crystallinity is 25-65% The intrinsic viscosity (I.V.) measured in tetrahydronaphthalene (THN) at -135°C is not more than 5 dl / g, preferably not more than 3 dl / g, the lower limit being preferably 0.4 dl / g in all cases. ii) Mw is 100,000 g / mol or more, in particular 100,000 to 650,000 g / mol. The melting point Tml measured by DSC at a scanning rate of 10°C / min is 95°C to 135°C. - Density is 885-925 kg / m 3 , preferably 900 to 920 kg / m 3 , especially 912 to 920 kg / m 3 To be

9. 3. The drawn polyolefin filament according to claim 1 or 2, wherein the propylene polymer A) is selected from propylene homopolymers, propylene copolymers and mixtures thereof, the amount of xylene insoluble fraction at 25 ° C is 85 wt % or more, more preferably 90 wt % or more, in particular for propylene homopolymers 95 wt % or more, the upper limit being preferably 99% for all homopolymers and 96% for all copolymers.

10. 2. An article comprising the drawn polyolefin filaments according to any one of the preceding claims.

11. 11. The article of claim 10 in the form of a net, rope, brush or the like.

Citation Information

Patent Citations

  • 1-butene and propylene polymer composition

    JP1990024339A

  • Resonator and manufacture of inductor in the resonator

    JP1991026011A

  • Polybutene-1 (CO)polymer, and method for producing the same

    JP2011046953A

  • Polyolefin fibers

    JP2012512919A

  • Polymer filament

    US20130217831A1