Metal-ion cell with excellent low-temperature performance

A mixed solvent electrolyte system with 3-methoxypropionitrile and linear carbonates addresses the low temperature performance issue in lithium-ion batteries, enhancing efficiency and capacity retention through improved ionic conductivity.

JP2024541459AInactive Publication Date: 2024-11-08PACIFIC IND DEVELOPMENT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024530429
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-23
Filing Date
2022-11-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium-ion batteries using organic carbonate electrolytes face challenges in low temperature performance due to high melting points of chain carbonates, leading to inadequate ionic conductivity and capacity retention.

Method used

Employing a mixed solvent electrolyte system comprising 3-methoxypropionitrile (MPN) and at least one linear carbonate solvent, with lithium hexafluorophosphate (LiPF6) as the primary lithium salt, to enhance ionic conductivity and improve low temperature performance.

Benefits of technology

The mixed solvent electrolyte system significantly enhances the first cycle Coulombic efficiency and capacity retention of lithium titanium oxide (LTO)-based cells at low temperatures, maintaining or improving performance compared to pure MPN or carbonate solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541459000001_ABST
    Figure 2024541459000001_ABST
Patent Text Reader

Abstract

A metal ion cell includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode has a cathode active material configured to store and release metal ions. The negative electrode has a Li / Li + and an anode active material operating at a potential of 0.6 volts (V) or greater relative to the anode. The electrolyte comprises one or more metal (e.g., lithium) salts and a solvent mixture including 3-methoxypropionitrile (MPN) and at least one chain carbonate. The MPN in the electrolyte may have a mass ratio of 0.1 or greater to the at least one chain carbonate solvent. The at least one chain carbonate solvent includes one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The solvent mixture may further include a mixture of multiple carbonates, and the mass percentage of the chain carbonate is in the range of 10% to 90% relative to the total mass of the carbonate mixture.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of the filing date under 35 U.S.C. § 119(e) of U.S. Provisional Application No. 63 / 282,202, filed November 23, 2021, the entire contents of which are incorporated herein by reference.

[0002] The present disclosure relates generally to metal-ion cells for use in electric devices, appliances, or vehicles. Additionally, the present disclosure describes electrochemical cells, such as lithium-ion cells, that may be used in rechargeable batteries. [Background technology]

[0003] The statements in this section are merely intended to provide background information related to the present disclosure and may not constitute prior art.

[0004] Lithium-ion cells typically incorporate at least four major components: (1) an anode, (2) a cathode, (3) a separator, and (4) an electrolyte. The electrolyte in commercially available lithium-ion cells typically contains a lithium salt dispersed in one or more organic carbonate solvents. The electrolyte provides a medium for the transport of lithium ions between the cathode and the anode. The primary reason for using carbonate solvents is that they provide stability at the respective operating potentials of both the anode (e.g., graphite) and the cathode (e.g., lithiated metal oxide).

[0005] Li4Ti5O 12The use of lithium titanium oxide (LTO), such as ethylene carbonate (EC) and propylene carbonate (PC), as an anode active material offers several advantages over the use of graphite active materials. These advantages include faster charging capability, better low-temperature performance, and improved safety. However, even though the operating potential of lithium titanium oxide is much higher than that of graphite, organic carbonate electrolytes are also used in commercially available LTO-based batteries. Because different carbonate solvents exhibit different properties, electrolytes usually contain a mixture of carbonates to achieve the required level of ionic conductivity and viscosity. Cyclic carbonates, such as ethylene carbonate (EC) and propylene carbonate (PC), provide high dipole moments but high viscosities. Conversely, linear carbonates, such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), provide low viscosities but low dipole moments. By combining at least one cyclic carbonate with one or more linear carbonates, the electrolyte can provide the high ionic conductivity at room temperature required for use in many practical applications. However, carbonate electrolytes, especially chain carbonates, lack low temperature performance due to their high melting points, so finding alternative electrolytes to improve low temperature performance has become of interest to the industry. Summary of the Invention

[0006] The present disclosure generally provides metal-ion cells for use in electric devices, appliances, or vehicles. Additionally, the present disclosure describes electrochemical cells, such as lithium-ion cells, that may be used in rechargeable batteries.

[0007] A metal ion cell includes a positive electrode, a negative electrode, and an electrolyte. The positive electrode has a current collector and a cathode active material configured to store and release metal ions. The negative electrode has a current collector and a Li / Li +and an anode active material operating at a potential of 0.6 volts (V) or greater relative to the anode. The electrolyte comprises one or more metal salts and a solvent mixture including 3-methoxypropionitrile (MPN) and at least one chain carbonate solvent.

[0008] According to one embodiment of the present disclosure, the potential at which the anode active material operates is Li / Li + The MPN in the electrolyte may have a mass ratio of 0.1 or more to the at least one chain carbonate solvent, or the MPN in the electrolyte may have a mass ratio of 2.0 or more to the at least one chain carbonate solvent, or the MPN in the electrolyte may have a mass ratio of 4.0 or more to the at least one chain carbonate solvent.

[0009] According to another embodiment of the present disclosure, the at least one chain carbonate solvent may include one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). Desirably, the solvent mixture in the electrolyte may further include a mixture of multiple carbonate solvents, and the mass percentage of the at least one chain carbonate solvent is in the range of 10% to 90% based on the total mass of the mixture of carbonate solvents. The solvent mixture in the electrolyte may further include a mixture of multiple carbonate solvents and one or more non-carbonate solvents, and the mass percentage of the chain carbonate is in the range of 10% to 90% based on the total mass of the mixture of carbonate solvents and non-carbonate solvents. The one or more non-carbonate solvents may include a sulfone solvent or a fluorocarbon solvent.

[0010] According to another aspect of the present disclosure, the one or more metal salts may be lithium salts, at least a portion of which is LiPF6. Alternatively, the one or more lithium salts may be LiPF6, which accounts for 100% of the lithium salts present in the electrolyte. The electrolyte may include a concentration of LiPF6 in the range of 0.1M to 3.0M, or the concentration of LiPF6 may be in the range of 0.5M to 1.5M. The one or more lithium salts may include more than 50 mol% LiPF6 of all lithium salts present. Desirably, the one or more lithium salts may further comprise at least one of lithium bis(trifluoromethanesulfonyl)imide (LiftSi), lithium bis(fluorosulfonyl)imide (LiFSi), lithium tetrafluoroborate (LiBF4), lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LiDFOB), lithium hypochlorite (LiClO4), and lithium difluorophosphate (LiPO2F2).

[0011] The cathode active material may include one or more of lithium iron phosphate (LFP), lithium iron manganese phosphate (LFMP), lithium manganese oxide (LMO), lithium nickel dioxide (LNO), lithium manganese nickel oxide (LMNO), lithium manganese nickel cobalt oxide (LMNC), lithium cobalt oxide (LCO), lithium vanadium phosphate (LVP), and metal fluorides.

[0012] The anode active material may include one or more of lithium titanate, titanium oxide, titanium niobium oxides having various ratios of titanium to niobium, niobium oxide and its derivatives, tungsten oxide, molybdenum oxide, vanadium oxide, antimony, and antimony oxide.

[0013] According to another aspect of the present disclosure, the one or more metal salts may include sodium ions, potassium ions, magnesium ions, aluminum ions, lithium ions, or mixtures thereof. The one or more metal salts may include tetraethylammonium tetrafluoroborate at a concentration ranging from 0.3 to 1.8 M.

[0014] According to another aspect of the present disclosure, there is provided a battery or battery pack for use in an electric device, appliance, or electric vehicle (EV), the battery or battery pack comprising one or more of the cells as described above or below. The battery or battery pack may comprise multiple cells arranged in a series or parallel configuration to increase overall capacity.

[0015] According to yet another aspect of the present disclosure, there is provided an electrochemical supercapacitor comprising at least one cell as described above or below incorporating activated carbon in one of the positive or negative electrodes.

[0016] Further areas of applicability will become apparent from the description provided herein. It is to be understood that the description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure.

[0017] In order that the disclosure may be fully understood, various aspects of the present disclosure, illustrated by way of example, are described below with reference to the accompanying drawings, in which the components are not necessarily drawn to scale, emphasis instead being placed upon illustrating the principles of the present invention. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram of an electrochemical cell including an active anode material, an active cathode material, an electrolyte, and a separator in accordance with the teachings of the present disclosure. [Diagram 2]1 is a plot of the rate performance at −30° C. of lithium titanium oxide / lithium manganese oxide (LTO / LMO) in 3-methoxypropionitrile (MPN), diethyl carbonate (DEC), and mixtures thereof. [Diagram 3] 1 is a plot of the rate performance at -30° C. of LTO / LMO in MPN, ethylene carbonate / diethyl carbonate (EC / DEC), and their mixtures. [Figure 4] 1 is a plot of rate performance at -30° C. of LTO / LMO in MPN, ethylene carbonate / dimethyl carbonate (EC / DMC), and their mixtures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The drawings described herein are for illustration purposes only and are not intended to limit the scope of the present disclosure in any way. It should be understood that corresponding reference characters indicate like or corresponding parts and features throughout the description and drawings.

[0020] The following description is merely exemplary in nature and is not intended to limit the present disclosure or its application or uses in any manner. For example, electrochemical cells prepared and used in accordance with the teachings set forth herein are described throughout this disclosure as lithium-ion cells in order to more fully illustrate and explain the structural elements and their uses. However, based on the principles of operation, the mixed solvent concepts of the present disclosure are also applicable to other metal ion cells that utilize salts containing or derived from any of the following: sodium ions, potassium ions, magnesium ions, aluminum ions, mixtures thereof, and the cells may be Li / Li +provided that the electrochemical cell has an anode that operates at 0.6 V or higher versus 0.5 V. Additionally, the incorporation and use of the mixed solvent system of the present disclosure is also applicable to electrochemical supercapacitors having activated carbon in one of the electrodes (e.g., cathode and anode). The LiPF6 salt may be replaced with a Li-free salt, including but not limited to tetraethylammonium tetrafluoroborate, provided that the salt concentration is in the range of 0.3-1.8 molar (M). It is considered within the scope of the present disclosure to incorporate multiple such electrochemical cells into various electrical devices, electrical equipment, and electrical systems. Various electrical devices, electrical equipment, and electrical systems include, but are not limited to, large capacity rechargeable batteries and batteries or battery packs for electric vehicles (EVs).

[0021] As used herein, a "battery cell" or "cell" refers to the basic electrochemical device of a battery, including electrodes, separators, and an electrolyte. In contrast, a "battery" or "battery pack" refers to a collection of cells, e.g., one or more cells, including a housing, electrical connections, and possibly control and protection electronics.

[0022] For purposes of this disclosure, the terms "about" and "substantially" are used herein in reference to measurable values ​​and ranges, which account for expected variations (e.g., limitations and variability of measurement) known to those of ordinary skill in the art.

[0023] For purposes of this disclosure, when referring to "at least one" and "one or more" of an element, these terms may be used interchangeably and may have the same meaning. These terms referring to the inclusion of a singular element or multiple elements may also be indicated by the suffix "(plural)" at the end of the element. For example, "at least one metal," "one or more metals," and "metals (plural)" may be used interchangeably and are intended to have the same meaning.

[0024] The present disclosure generally provides an electrolyte system for use in lithium-ion cells, such as lithium titanium oxide (LTO)-based cells. The electrolyte system typically includes LiPF6 as a primary lithium salt dispersed in a solvent, which consists of, comprises, or consists essentially of a mixture of 3-methoxypropionitrile (MPN) and at least one organic carbonate solvent. Organic nitrile solvents, such as MPN, generally exhibit lower viscosities than cyclic carbonates, but higher dipole moments than linear carbonates. Organic nitrile solvents also have lower melting points, allowing them to be used as solvents to provide more efficient battery cell performance at low temperatures.

[0025] In battery cells, lithium titanium oxide (LTO) anodes are typically Li / Li + The graphite anode operates at about 1.0V to 3.0V relative to Li / Li + The LTO anode operates at a potential between 0.01 V and 1.0 V relative to the Li / Li anode. The minimum potential of the LTO anode is high, about 1.0 V, which is higher than the minimum potential of the graphite anode. This large potential difference allows the use of alternative solvents (such as solvents other than organic carbonates) that cannot be used with the graphite anode. For example, acetonitrile is used for the Li / Li + The reduction potential of the LTO anode is about 0.5 V vs. Li / Li, which means that it cannot be used with graphite anodes. However, the operating potential of the LTO anode is about 0.5 V vs. Li / Li +Since the potential difference between the anode and the cathode is much higher than 0.5 V vs. 0.1 V, acetonitrile can be used in LTO anodes. In another example, 3-methoxypropionitrile (MPN) can be used as a solvent for electrolytes in LTO-based cells that contain lithium salts such as LiTFSi or LiPF6. LTO-based cells that contain LiTFSi dispersed in MPN have shown acceptable performance. However, the cost associated with LiTFSi salts makes the battery cells expensive to manufacture, as LiPF6 salts are the predominant lithium salt used in commercially available cells. Therefore, electrolytes used with LiPF6-based salts dispersed in MPN are desirable for use in LTO-based cells.

[0026] Referring to FIG. 1, an electrochemical cell generally comprises a positive electrode 10 and a negative electrode 20. The positive electrode 10 has an active material (cathode) 5 and a current collector 7, and the negative electrode 20 has an active material (anode) 15 and a current collector 17. The cell further comprises a non-aqueous electrolyte 30 containing lithium ions, and a separator 25, as described above and further defined herein. All of these components are sealed in a case, enclosure, pouch, bag, cylindrical shell, or the like (commonly referred to as the battery's "enclosure"). The separator 25 electrically insulates the cathode active material 5 from the anode 15 while allowing metal (e.g., lithium) ions to flow between them. The flow of ions may be conducted by the separator (i.e., via a solid-state reaction mechanism) or may be conducted by the presence of a liquid electrolyte 30 that permeates the multiple pores of the separator 25 (e.g., a membrane).

[0027] 1, the anode active material 15 may include lithium titanium oxide (LTO) or any other anode active material capable of operating within a similar potential range or slightly lower potential limits. For example, the anode active material 15 may be Li / Li + Li / Li + It may be operated at potentials up to 0.6 V vs. +The anode active material 15 also has a Li / Li + 0.7V, Li / Li + 0.8V for Li / Li + The anode active material 15 may be operated at potentials up to 0.9 V versus the MPN solvent. As long as the minimum operating potential of the anode active material 15 is higher than the reduction potential of the MPN solvent, these anode active materials may be used to replace the LTO anode for a given application. Some examples of anode active materials 15 include, but are not limited to, lithium titanate (LTO), titanium oxide, titanium niobium oxides with various ratios of titanium to niobium, niobium oxide and its derivatives, tungsten oxide, molybdenum oxide, vanadium oxide, antimony, antimony oxide, and the like.

[0028] The cathode active material 5 may be selected from any currently available cathode active material used in conventional lithium ion cells. Some examples of cathode active materials 5 include, but are not limited to, lithium iron phosphate (LFP), lithium iron manganese phosphate (LFMP), lithium manganese oxide (LMO), lithium nickel dioxide (LNO), lithium manganese nickel oxide (LMNO), lithium manganese nickel cobalt oxide (LMNC), lithium cobalt oxide (LCO), lithium vanadium phosphate (LVP), metal fluorides.

[0029] 1 , electrolyte 30 is located between and in contact with positive electrode 10 and negative electrode 20 such that electrolyte 30 supports the reversible flow of metal (e.g., lithium) ions between negative electrode 20 and positive electrode 10. Separator 25 is configured to electrically insulate positive electrode 10 from negative electrode 20 while being permeable to the reversible flow of metal (e.g., lithium) ions through separator 25.

[0030] The electrolyte 30 is based on lithium hexafluorophosphate (LiPF6) with a molar concentration in the range of 0.1 molar (M) to 3.0 M, alternatively in the range of 0.2 M to 2.0 M, alternatively in the range of about 0.5 M to about 1.5 M. If the concentration of the lithium salt in the electrolyte 30 is too high, it may cause salt precipitation at low temperatures. If the concentration of the lithium salt is too low, the ionic conductivity of the electrolyte 30 may be insufficient for practical use. The lithium salt may consist of 100% LiPF6. The lithium salt may be a mixture of LiPF6 and at least one additional lithium salt. In this mixture, the amount of LiPF6 is high enough to be present as the main lithium salt. In other words, the molar percentage of lithium hexafluorophosphate (LiPF6) with respect to the total lithium salt content of the mixture is greater than 0.5, alternatively 0.6 or more, alternatively 0.7 or more. The at least one additional lithium salt includes, but is not limited to, lithium bis(trifluoromethanesulfonyl)imide (LiftSi), lithium bis(fluorosulfonyl)imide (LiFSi), lithium tetrafluoroborate (LiBF4), lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LiDFOB), lithium hypochlorite (LiClO4), lithium difluorophosphate (LiPO2F2), or mixtures thereof.

[0031] A mixture of solvents is used to disperse the lithium salt in the electrolyte 30. The mixture of solvents includes 3-methoxypropionitrile (MPN) and at least one type of linear carbonate. Linear carbonates that exhibit low viscosity include, but are not limited to, dimethyl carbonate (DMC), diethyl carbonate (DEC), or ethyl methyl carbonate (EMC). Desirably, the mixture of solvents used in the electrolyte may also include cyclic carbonates, such as, but not limited to, ethylene carbonate (EC) and propylene carbonate (PC). One skilled in the art will appreciate that the mixture of solvents used in the electrolyte 30 may also include solvents that do not contain carbonates (non-carbonate solvents) without going beyond the scope of this disclosure. Some examples of non-carbonate solvents include, but are not limited to, sulfone solvents and fluorocarbon solvents. The mass ratio of MPN to other solvents in the electrolyte 30 is 0.1 or more, alternatively 1.0 or more, alternatively 2.0 or more, alternatively 4.0 or more, or alternatively 9.0 or more. The mass percentage of the chain carbonate present in the solvent mixture may range from 10% to 90%, alternatively from about 15% to about 85%, alternatively from 20% to 80%.

[0032] Referring now to Table 1, the advantages associated with the use of mixtures of solvents in the present disclosure are shown. For Lithium Titanium Oxide / Lithium Manganese Oxide (LTO / LMO) cells, the first cycle Coulombic Efficiency (CE) was 86% when using an electrolyte containing 1M LiPF6 dispersed in MPN. When a mixture of MPN and chain carbonate (i.e., DEC) in a 1 / 1 ratio was used, the first cycle CE increased to 90%. When a mixture of ethylene carbonate and diethyl carbonate (EC / DEC or EC-DC) was mixed with MPN in a 4 / 1 ratio, the first cycle CE increased to 92%. Similarly, when other carbonate solvents (e.g., EC-DMC) were used with MPN in various ratios, the first cycle CE ranged from 90% to 93%. Thus, mixing carbonate solvents with MPN electrolytes improves the first cycle CE of LTO / LMO cells. This improvement in first cycle CE is important for enhancing the utilization of electrolyte materials and increasing the energy density of the cell.

[0033] Coulombic efficiency (CE) as used herein is defined as the ratio of discharge capacity (mAh / g) to charge capacity (mAh / g). At each electrode (i.e., positive electrode 10 or negative electrode 20), the CE is usually less than 100%, especially at the first charge / discharge cycle, due to irreversible capacity loss caused by side reactions. For example, at the anode side (i.e., negative electrode 20) of the electrochemical cell, the organic electrolyte 30 may decompose at low potential ranges and form a solid electrolyte interface (SEI) film on the surface of the anode active material 15, which irreversibly consumes capacity. At the cathode side (i.e., positive electrode 10) of the electrochemical cell, decomposition of the electrolyte 30 also occurs at the surface of the cathode active material 5, but at a lower level than that occurring at the anode active material 15. This decomposition may also result in the formation of irreversible crystalline changes.

[0034] [Table 1]

[0035] The anode active material 15 and cathode active material 5 can be formed into the desired shape for use in the anode 20 and cathode 10 by mixing the active materials with one or more binders in various weight ratios. For example, cathode active material 5, including currently available cathode active materials used in conventional lithium ion cells, with or without additives, can be mixed with a binder, including but not limited to polyvinylidene fluoride (PVDF), carboxymethyl cellulose (cmc), polytetrafluoroethylene (PTFE), polyacrylates, or mixtures or blends thereof. Anode active material 15, including lithium titanium oxide (LTO), or any other active material capable of operating within a similar potential range or slightly lower potential limits, can be mixed with a binder, including but not limited to carboxymethyl cellulose (cmc), styrene butadiene rubber (SBR), polyacrylic acid, polyacrylates, polyimides, or mixtures or blends thereof. The mass ratio of active material (i.e., anode or cathode) to binder may range from 70:30 to 99.9:0.1, alternatively 70:30 to 99:1, alternatively 80:20 to 99:1, alternatively 80:20 to 95:5, with higher active material to binder ratios being used in applications requiring higher energy density.

[0036] The current collector 7 of the positive electrode 10 can be made of any metal known in the art for use in electrodes in lithium batteries, including, but not limited to, aluminum, titanium, stainless steel, nickel, copper, carbon, zinc, gallium, silver, and combinations or alloys thereof. The current collector 17 used in the negative electrode 20 can be a metal foil that does not react with metal (e.g., lithium) ions. Some examples of such metal foils include, but are not limited to, Cu, Fe, Ti, Ni, Mo, W, Zr, Mn, carbon, and lithium metal alloys. Alternatively, the metal foil for the current collector 17 of the negative electrode 20 includes Cu, Fe, Ni, or mixtures or alloys thereof. The current collectors 7, 17 used in the positive electrode 10 and negative electrode 20 can include at least one metal capable of forming an alloy with lithium.

[0037] Separator 25 ensures that the active anode material 15 and the active cathode material 5 do not contact each other and allows metal (e.g., lithium) ions to flow therethrough. Separator 25 can be a polymeric membrane, including, but not limited to, polyolefin-based materials having a semi-crystalline structure (such as polyethylene, polypropylene, and mixtures thereof), microporous poly(methyl methacrylate)-grafted, siloxane-grafted polyethylene, and polyvinylidene fluoride (PVDF) nanofiber webs.

[0038] The specific examples presented in this disclosure are intended to illustrate various embodiments of the present invention and should not be construed as limiting the scope of the disclosure. The embodiments described herein have been described so as to enable a clear and concise specification to be written, but it is intended and will be understood that the embodiments may be combined or separated in various ways without departing from the invention. For example, it will be understood that all preferred features described herein are applicable to all aspects of the invention described herein.

[0039] Several LTO / LMO cells with different electrolytes were fabricated and evaluated. All battery materials were purchased from Gelon, China. The LMO coating was fabricated from a mixture of lithium manganese oxide (LMO), carbon black (C65), carbon nanotubes (CNT) and polyvinylidene fluoride (PVDF) in a mass ratio of 92 / 2 / 2 / 4, with an areal capacity loading of the coating of approximately 0.8 mAh / cm. 2 The LTO coating was made from a mixture of lithium titanium oxide (LTO), carbon black (C65), and PVDF (in a mass ratio of 92 / 5 / 3) with an areal capacity loading of approximately 0.8 mAh / cm 2 A full or complete cell was created by stacking one LMO electrode, one ceramic oxide coated PE separator, and one LTO electrode in an aluminum pouch filled with a given type and amount of electrolyte. The full or complete cell was then cycled between 3.0V and 4.2V at room temperature and -30 degrees Celsius at different C-rates with C / 10 being the slowest rate to demonstrate the advantage of using MPN based electrolyte in combination with at least one carbonate solvent. For the purposes of this disclosure, C-rate is a measure of the rate at which a battery discharges relative to its maximum capacity.

[0040] Referring now to FIG. 2, a plot of the rate performance at −30° C. of lithium titanium oxide / lithium manganese oxide (LTO / LMO) in 3-methoxypropionitrile (MPN), diethyl carbonate (DEC), and mixtures thereof is shown. In this example (EX-1), the capacity retention of an LTO / LMO cell containing 1M LiPF6 at −30° C. DEC was about 47% of the capacity at room temperature (see curves a and d). The capacity retention of an LTO / LMO cell containing 1M LiPF6 in MPN / DEC (1 / 1 by mass) at −30° C. was about 82% at a charge / discharge rate of about C / 10 (see curves b and e). Meanwhile, the capacity retention of a cell using pure 100% MPN solvent was about 78% (see curves c and f).

[0041] The low temperature performance was substantially or significantly improved using the MPN and carbonate solvent mixture (see curves b and e) compared to the carbonate solvent alone (see curves a and d). The mixed solvent (see curves b and e) even showed slightly better capacity retention than the pure MPN (see curves c and f) at low temperatures. Without being strictly bound by theory, it is believed that the improved capacity retention of the mixed solvent compared to the pure MPN is due to the relatively high viscosity of the MPN, and the addition of the low viscosity carbonate solvent helped to improve the ionic conductivity that occurs at low temperatures.

[0042] Referring now to FIG. 3, a plot of the rate performance at −30° C. of LTO / LMO in MPN, ethylene carbonate / diethyl carbonate (EC / DEC), and their mixtures is shown. In this example (EX-2), 1M LiPF6 in MPN electrolyte was prepared and mixed with commercially available 1M LiPF6 in EC / DEC (1 / 3) that also contained 1% vinylene carbonate (VC) and 1% fluoroethylene carbonate (FEC). The cell containing only the commercially available electrolyte had a capacity retention of about 57% at −30° C. at about C / 10 rate (see curves g and j). Meanwhile, the cell containing the solvent mixture according to the present disclosure showed a capacity retention of about 77% (see curves h and k). The capacity retention of the solvent mixture (see curves h and k) is comparable to the 78% capacity retention of the cell containing 100% MPN (see curves i and l). The addition of commercially available carbonate electrolyte to the MPN electrolyte increased the first cycle CE compared to the MPN electrolyte while maintaining a similar capacity retention at -30 °C.

[0043] Referring now to FIG. 4, rate performance plots of LTO / LMO in MPN, ethylene carbonate / dimethyl carbonate (EC / DMC), and their mixtures at −30° C. are shown. In this example (EX-3), 1M LiPF6 in MPN electrolyte was prepared and mixed with commercially available 1M LiPF6 in EC / DMC (1 / 1) electrolyte. At −30° C., due to the high melting points of the EC and DMC solvents, the capacity retention of the cell containing only EC / DMC electrolyte was close to 0 (see curves m and p). The cell containing the electrolyte consisting of the MPN and carbonate (4 / 1) solvent mixture showed the highest capacity retention of 81% (see curves n and q) at about C / 10 charge / discharge rate compared to 78% for the cell containing 100% MPN electrolyte (see curves o and r). Additionally, the cell containing the electrolyte consisting of the mixture of MPN and carbonate solvents showed better discharge rate capability (see curves q versus curves r).

[0044] The examples (EX-1, EX-2, EX-3) demonstrate some of the advantages associated with the electrolytes of the present disclosure that include a mixture of MPN and at least one carbonate solvent. More specifically, the use of the solvent mixture improves the first cycle CE exhibited by the cell while maintaining or even improving performance at low temperatures.

[0045] According to yet another aspect of the present disclosure, one or more electrochemical cells can be combined to form a larger capacity battery or battery pack, for example, for use in a high capacity lithium ion secondary battery or a battery pack incorporated in an electric vehicle (EV). One or more electrochemical cells may be combined in series, parallel, or a combination thereof to form a battery or battery pack. Those skilled in the art will appreciate that, in addition to using electrochemical cells in a lithium ion secondary battery, the one or more electrochemical cells can also be encapsulated in a housing and used in other applications using the same principles.

[0046] The housing may be constructed of any material known in the art to be used for such applications and may be in any shape required or desired for a particular application. For example, lithium ion batteries are generally housed in three different primary forms or shapes: cylindrical, prismatic, or soft pouch. Cylindrical battery housings can be made of aluminum, steel, etc. Prismatic batteries generally have a rectangular housing rather than a cylindrical one. Soft pouch housings can be made in a variety of shapes and sizes. These soft housings may consist of an aluminum foil pouch coated with plastic on the inside, outside, or both. The soft housing may be a polymeric type case. The polymeric composition used for the housing may be any known polymeric material conventionally used in lithium ion secondary batteries. One specific example among many is the use of a laminate pouch having a polyolefin layer on the inside and a polyamide layer on the outside.

[0047] Although the embodiments have been described herein in a manner that enables a clear and concise specification to be written, it is intended and will be understood that the embodiments may be combined or separated in various ways without departing from the invention, and for example, it will be understood that all preferred features described herein are applicable to all aspects of the invention described herein.

[0048] Those skilled in the art will appreciate in light of this disclosure that many changes can be made in the specific embodiments disclosed herein without departing from or exceeding the spirit or scope of the disclosure and still obtain like or similar results. Those skilled in the art will further appreciate that any properties reported herein represent properties that are typically measured and that can be obtained in a number of different ways. The method described herein represents one such method, and the use of other methods does not depart from the scope of the disclosure.

[0049] The foregoing description of various forms of the present invention has been presented for purposes of illustration and description. The foregoing description is not intended to be exhaustive or to limit the present invention to the precise forms disclosed. Numerous modifications or variations are possible in light of the above teachings. The forms discussed have been chosen and described in order to best explain the principles of the present invention and its practical application. This will enable those skilled in the art to best utilize the present invention with various modifications in various forms suited to the particular uses contemplated. All such modifications and variations are within the scope of the present invention, as determined by the appended claims, when interpreted in accordance with the extent to which they are fairly, legally, and equitably entitled.

Claims

1. 1. A metal ion cell comprising: A positive electrode, A current collector; a cathode active material configured to store and release metal ions; A positive electrode having A negative electrode, A current collector; Li / Li + an anode active material operating at a potential of 0.6 volts (V) or greater relative to the A negative electrode having An electrolyte comprising: one or more metal salts; A solvent mixture comprising 3-methoxypropionitrile (MPN) and at least one linear carbonate solvent; an electrolyte having Equipped Metal ion cells.

2. 2. The cell of claim 1 , The potential at which the anode active material operates is Li / Li + 0.8V or more to cell.

3. 3. A cell according to claim 1 or 2, The MPN in the electrolyte has a mass ratio of 0.1 or more to the at least one chain carbonate solvent. cell.

4. A cell according to any one of claims 1 to 3, The MPN in the electrolyte has a mass ratio of 2.0 or more to the at least one chain carbonate solvent. cell.

5. A cell according to any one of claims 1 to 4, The MPN in the electrolyte has a mass ratio of 4.0 or more to the at least one chain carbonate solvent. cell.

6. A cell according to any one of claims 1 to 5, The at least one chain carbonate solvent comprises one or more of dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC); cell.

7. A cell according to any one of claims 1 to 6, the solvent mixture in the electrolyte further comprises a mixture of multiple carbonate solvents; the mass percentage of the at least one chain carbonate solvent ranges from 10% to 90% based on the total mass of the mixture of carbonate solvents; cell.

8. A cell according to any one of claims 1 to 7, the solvent mixture in the electrolyte further comprises a mixture of carbonate solvents and one or more non-carbonate solvents; The mass percentage of the chain carbonate is in the range of 10% to 90% based on the total mass of the mixture of the carbonate solvent and the non-carbonate solvent. cell.

9. 9. The cell of claim 8, The one or more non-carbonate solvents include a sulfone solvent or a fluorocarbon solvent. cell.

10. A cell according to any one of claims 1 to 9, At least a part of the one or more metal salts is LiPF 6 is a lithium salt of cell.

11. A cell according to any one of claims 1 to 10, The cathode active material is Lithium iron phosphate (LFP), lithium iron manganese phosphate (LFMP), lithium manganese oxide (LMO), lithium nickel dioxide (LNO), lithium manganese nickel oxide (LMNO), lithium manganese nickel cobalt oxide (LMNC), lithium cobalt oxide (LCO), lithium vanadium phosphate (LVP), metal fluorides; cell.

12. A cell according to any one of claims 1 to 11, The anode active material is Lithium titanate, titanium oxide, titanium niobium oxides with various ratios of titanium to niobium, niobium oxide and its derivatives, tungsten oxide, molybdenum oxide, vanadium oxide, antimony, antimony oxide, cell.

13. A cell according to any one of claims 10 to 12, The electrolyte is LiPF with a concentration ranging from 0.1 molar (M) to 3.0 M. 6 Including, cell.

14. 14. The cell of claim 13, The LiPF 6 is in the range of 0.5 molar (M) to 1.5 M; cell.

15. A cell according to any one of claims 10 to 14, The one or more lithium salts are LiPF 5 which accounts for 100% of the lithium salts present in the electrolyte. 6 That is, cell.

16. A cell according to any one of claims 10 to 15, The one or more lithium salts comprise more than 50 mol % of all lithium salts present. 6 Including, cell.

17. A cell according to any one of claims 10 to 16, The one or more lithium salts are Lithium bis(trifluoromethanesulfonyl)imide (LiftSi), lithium bis(fluorosulfonyl)imide (LiFSi), lithium tetrafluoroborate (LiBF 4 ), lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LiDFOB), lithium hypochlorite (LiClO 4 ), lithium difluorophosphate (LiPO 2 F 2 ), cell.

18. A cell according to any one of claims 1 to 9, The one or more metal salts include sodium ions, potassium ions, magnesium ions, aluminum ions, lithium ions, or mixtures thereof; cell.

19. A cell according to any one of claims 1 to 9, the one or more metal salts include tetraethylammonium tetrafluoroborate at a concentration ranging from 0.3 to 1.8 M; cell.

20. 1. A battery or battery pack for use in an electrical device, appliance, or electric vehicle (EV), comprising: Comprising one or more cells according to any one of claims 1 to 19, Batteries or battery packs.

21. 21. The battery or battery pack of claim 20, The battery or battery pack comprises a plurality of the cells arranged in a series or parallel configuration to increase overall capacity. Batteries or battery packs.

22. 1. An electrochemical supercapacitor, comprising: At least one cell according to claims 1 to 9, in which activated carbon is incorporated into one of the positive and negative electrodes. Supercapacitor.