Anode active material, anode including same, secondary battery including same, and method for producing anode active material
The development of a SiO x -based negative electrode active material with controlled crystalline phases addresses the inefficiencies of silicon-based electrodes by stabilizing the lithium silicate structure, enhancing initial efficiency and charge/discharge performance in lithium secondary batteries.
Patent Information
- Application Number
- JP2024530549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-05
- Filing Date
- 2023-09-06
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2043-09-06
AI Technical Summary
Silicon-based negative electrode active materials for lithium secondary batteries face issues with low initial efficiency due to high irreversible capacity and instability during charging and discharging, leading to poor charge/discharge efficiency and reduced life characteristics, primarily because of the reaction with moisture in the negative electrode slurry.
A negative electrode active material composed of SiO x (0
This approach enhances the initial efficiency and charge/discharge efficiency by minimizing irreversible capacity loss and gas generation in the slurry, improving the quality and performance of the negative electrode and secondary battery.
Smart Images

Figure 2024541737000001 
Figure 2024541737000002 
Figure 2024541737000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0113645 filed with the Korean Intellectual Property Office on September 7, 2022, and Korean Patent Application No. 10-2023-0117434 filed with the Korean Intellectual Property Office on September 5, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a negative electrode active material, a negative electrode containing the same, a secondary battery containing the same, and a method for producing the negative electrode active material. [Background technology]
[0003] In recent years, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have a relatively high capacity is rapidly increasing. In particular, lithium secondary batteries, which are lightweight and have high energy density, have been in the spotlight as a driving power source for portable devices. For this reason, research and development efforts are being actively made to improve the performance of lithium secondary batteries.
[0004] In general, a lithium secondary battery includes a positive electrode, a negative electrode, a separator between the positive electrode and the negative electrode, an electrolyte, an organic solvent, etc. In addition, the positive electrode and the negative electrode may have active material layers formed on current collectors, each of which includes a positive electrode active material and a negative electrode active material. In general, the positive electrode uses a lithium-containing metal oxide such as LiCoO2 or LiMn2O4 as a positive electrode active material, and the negative electrode uses a lithium-free carbon-based active material or a silicon-based active material as a negative electrode active material.
[0005] Among negative electrode active materials, silicon-based active materials have been attracting attention because they have higher capacity and excellent high-speed charging characteristics compared to carbon-based active materials. However, silicon-based active materials have the disadvantage of low initial efficiency due to large volume expansion / contraction during charging / discharging and large irreversible capacity.
[0006] On the one hand, among silicon-based active materials, silicon-based oxides, specifically SiO x In the case of silicon-based oxides represented by (0 < x < 2), there is an advantage in that the degree of volume expansion / contraction due to charge and discharge is lower compared to other silicon-based active materials such as silicon (Si). However, there is still a drawback that the initial efficiency decreases due to the presence of irreversible capacity even in silicon-based oxides.
[0007] In connection with this, research has been continuously conducted to reduce the irreversible capacity and improve the initial efficiency by doping or inserting metals such as Li, Al, and Mg into silicon-based oxides. However, in the case of a negative electrode slurry containing a metal-doped silicon-based oxide as a negative electrode active material, there is a problem that the metal oxide formed by doping reacts with moisture to increase the pH of the negative electrode slurry and change the viscosity, resulting in a poor state of the manufactured negative electrode and a decrease in the charge and discharge efficiency of the negative electrode.
[0008] Therefore, there is a need to develop a negative electrode active material that can improve the phase stability of a negative electrode slurry containing a silicon-based oxide and thereby improve the charge and discharge efficiency of the manufactured negative electrode.
[0009] Korean Registered Patent No. 10-0794192 relates to a method for manufacturing a carbon-coated silicon-graphite composite negative electrode material for a lithium secondary battery and a method for manufacturing a secondary battery including the same, but there are limitations in solving the above-described problems.
Prior Art Documents
Patent Documents
[0010]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0011] The present invention relates to a negative electrode active material, a negative electrode containing the same, a secondary battery containing the same, and a method for manufacturing the negative electrode active material.
Means for Solving the Problems
[0012] One embodiment of the present invention is a negative electrode active material containing silicon-based particles containing SiO x (0 < x < 2) and a Li compound, wherein the Li compound contains at least one crystalline lithium silicate selected from the group consisting of crystalline phase Li2SiO3, crystalline phase Li4SiO4, and crystalline phase Li2Si2O5, and the content of the crystalline phase Li2SiO3 is more than the total of the content of the crystalline phase Li2Si2O5 and the content of the crystalline phase Li4SiO4, and the content of the crystalline phase Li2SiO3 is 60 parts by weight or more based on 100 parts by weight in total of the crystalline lithium silicate, and the total content of the crystalline phases present in the silicon-based particles is more than the total content of the amorphous phases, and a negative electrode active material is provided.
[0013] One embodiment of the present invention is a step of forming particles containing a silicon-based oxide represented by SiO x (0 < x < 2); and a step of heat-treating after mixing the particles containing the silicon-based oxide and a lithium precursor, and a method for manufacturing a negative electrode active material according to one embodiment of the present invention is provided.
[0014] One embodiment of the present invention provides a negative electrode containing the negative electrode active material according to one embodiment of the present invention. One embodiment of the present invention provides a secondary battery containing the negative electrode according to one embodiment of the present invention.
Effects of the Invention
[0015] The anode active material of the present invention has a predominant content of crystalline phase Li2SiO3 in the crystalline phase lithium silicate, and the loss of discharge capacity per weight due to the increase in the Li content in the anode active material is small, and the initial efficiency can be significantly increased because the SiO2 acting as an irreversible capacity during Li doping reacts with Li to form an electrochemically stable lithium silicate structure of Li2SiO3. In addition, the crystalline phase Li2SiO3 has a stable structure during charging and discharging, and has excellent life characteristics.
[0016] In addition, since the negative electrode active material of the present invention has a higher total content of crystalline phase than the total content of amorphous phase, the content of lithium oxide and lithium silicate that react with moisture is low, which can prevent gas generation and viscosity change of the negative electrode slurry and improve the phase stability of the slurry including the negative electrode active material. Therefore, a negative electrode including the negative electrode active material and a secondary battery including the negative electrode have improved quality and improved charge / discharge capacity, initial efficiency, and / or life characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] This specification will be explained in more detail below. In this specification, when a part is said to "comprise" a certain component, this means that it may further include other components, not excluding other components, unless specifically stated to the contrary.
[0018] In this specification, when a member is said to be "located on" another member, this includes not only the case where the member is in contact with the other member, but also the case where another member is present between the two members.
[0019] The terms and words used in this specification should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0020] As used herein, the singular expression of a term includes the plural expression unless the context clearly indicates otherwise.
[0021] In this specification, the crystallinity of the structure contained in the negative electrode active material can be confirmed by X-ray diffraction analysis, which can be performed using an XRD (X-ray diffraction) analysis device (product name: D4-Endeavor, manufacturer: Bruker), and in addition to the above device, any device used in the industry can be appropriately adopted.
[0022] In this specification, the presence or absence of an element in the negative electrode active material and the content of the element can be confirmed by ICP analysis, and the ICP analysis can be performed using an inductively coupled plasma optical emission spectrometer (ICPAES, Perkin-Elmer 7300).
[0023] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size that corresponds to 50% of the cumulative volume in the particle size distribution curve (graph curve of the particle size distribution diagram). 50 ) can be measured, for example, by using a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to several mm, and can provide results with high reproducibility and high resolution.
[0024] Preferred embodiments of the present invention will be described in detail below. However, the embodiments of the present invention may be modified in various ways, and the scope of the present invention is not limited to the embodiments described below.
[0025] <Negative electrode active material> The negative electrode active material will be described in detail below. The present invention relates to a negative electrode active material, and more particularly to a negative electrode active material for lithium secondary batteries.
[0026] One embodiment of the present invention is SiO xA negative electrode active material comprising silicon-based particles containing (0 < x < 2) and a Li compound, wherein the Li compound contains at least one crystalline lithium silicate selected from the group consisting of crystalline Li2SiO3, crystalline Li4SiO4, and crystalline Li2Si2O5, the content of the crystalline Li2SiO3 is more than the sum of the content of the crystalline Li2Si2O5 and the content of the crystalline Li4SiO4, the content of the crystalline Li2SiO3 is 60 parts by weight or more based on 100 total parts by weight of the crystalline lithium silicate, and the total content of the crystalline phases present in the silicon-based particles is more than the total content of the amorphous phases, to provide a negative electrode active material.
[0027] Conventionally, in negative electrode active materials containing silicon-based oxides, research has been conducted to dope or distribute lithium or the like in the negative electrode active material to remove the irreversible capacity of the silicon-based oxide and improve the initial efficiency. However, such negative electrode active materials have a high content of amorphous phases, so that during the production of negative electrode slurries, specifically aqueous negative electrode slurries, gas generation increases due to the reaction of moisture with lithium oxide and / or lithium silicate, increasing the pH of the negative electrode slurry and reducing the phase stability, resulting in poor quality of the produced negative electrode and problems of reducing the charge-discharge efficiency.
[0028] To solve such problems, the negative electrode active material according to one embodiment of the present invention is SiO x (0 < x < 2) and the silicon-based particles containing a Li compound are present in the form of at least one crystalline lithium silicate or amorphous lithium silicate selected from the group consisting of crystalline Li2SiO3, crystalline Li4SiO4, and crystalline Li2Si2O5, among which the content of the crystalline Li2SiO3 is more than the sum of the content of the crystalline Li2Si2O5 and the content of the crystalline Li4SiO4, and the total content of the crystalline phases present in the silicon-based particles is more than the total content of the amorphous phases.
[0029] According to the negative electrode active material of the present invention, the content of the crystal phase Li2SiO3 in the crystal phase lithium silicate is predominantly present, and the loss of discharge capacity per unit weight due to the increase in the content of Li in the negative electrode active material is small. A large amount of SiO2 and Li, which act as irreversible capacity during Li doping, react with each other to form a lithium silicate structure of electrochemically stable Li2SiO3, so that the initial efficiency can be significantly increased. Further, in the case of the crystal phase Li2SiO3, the structure is stable during charge and discharge, and the life characteristics are excellent.
[0030] Moreover, according to the negative electrode active material of the present invention, since the total content of the crystal phase is larger than the total content of the amorphous phase, the content of lithium oxide and lithium silicate that react with moisture is small, and gas generation and viscosity change of the negative electrode slurry can be prevented. Since the phase stability of the slurry containing the negative electrode active material can be improved, the negative electrode containing the negative electrode active material and the secondary battery containing the negative electrode have the effects of improved quality, improved charge and discharge capacity, initial efficiency, and / or life characteristics.
[0031] The negative electrode active material according to an embodiment of the present invention includes silicon-based particles. The silicon-based particles contain SiO x (0 < x < 2) and a Li compound.
[0032] The SiO x (0 < x < 2) may correspond to a matrix within the silicon-based particles. The SiO x (0 < x < 2) may be in a form containing Si and / or SiO2, and the Si may form a phase. For example, the SiO x (0 < x < 2) may be a composite containing amorphous SiO2 and Si crystals. That is, the x corresponds to the number ratio of O to Si contained in the SiO x (0 < x < 2). When the silicon-based particles contain the SiO x (0 < x < 2), the discharge capacity of the secondary battery can be improved. Specifically, the SiO x (0 < x < 2) is SiO xIt may be a compound represented by (0.5≦x≦1.5).
[0033] The Li compound may correspond to a matrix in the silicon-based composite particles. The Li compound may be present in the silicon-based particles in at least one form of lithium atom, lithium silicate, lithium silicide, and lithium oxide. When the silicon-based particles contain the Li compound, there is an effect of improving initial efficiency.
[0034] The Li compound may be distributed on the surface and / or inside of the silicon-based particles in a doped form. The Li compound is distributed on the surface and / or inside of the silicon-based particles, and can control the volume expansion / contraction of the silicon-based particles to an appropriate level, thereby preventing damage to the active material. The Li compound may also be included to reduce the proportion of irreversible phases (e.g., SiO2) in the silicon-based oxide particles, thereby increasing the efficiency of the active material.
[0035] Specifically, the lithium may be distributed on the surface, inside, or on and inside of the silicon-based particle, and the lithium may be doped into the silicon-based particle.
[0036] In one embodiment of the present invention, the Li element may be included in an amount of more than 7 parts by weight and not more than 10 parts by weight based on a total of 100 parts by weight of the negative electrode active material.
[0037] Preferably, the Li element may be included in an amount of 7.2 to 9.8 parts by weight, 7.5 to 9.7 parts by weight, 8 to 9.5 parts by weight, 8.2 to 9.5 parts by weight, or 8.5 to 9.2 parts by weight based on the total 100 parts by weight of the negative electrode active material. When lithium is included in the above range, the initial efficiency and charge / discharge efficiency of the negative electrode active material can be improved, which is preferable. On the other hand, when Li is included in an amount less than the above amount, the content of Li in the silicon-based particles is insufficient, and the discharge capacity and efficiency are significantly reduced. When the content exceeds the above amount, Li that has not reacted with the silicon-based particles remains as a by-product, and the aqueous slurry exhibits strong basicity, which may adversely affect the processability of the slurry.
[0038] The upper limit of the Li content may be 10 parts by weight, 9.8 parts by weight, 9.7 parts by weight, 9.6 parts by weight, 9.5 parts by weight, 9.4 parts by weight, 9.3 parts by weight, 9.2 parts by weight, 9.1 parts by weight, or 9 parts by weight, based on a total of 100 parts by weight of the negative active material, and the lower limit may be 7.2 parts by weight, 7.5 parts by weight, 7.8 parts by weight, 8 parts by weight, 8.2 parts by weight, or 8.5 parts by weight.
[0039] The content of the Li element can be confirmed by ICP analysis. Specifically, a certain amount (about 0.01 g) of the negative electrode active material is taken, transferred to a platinum crucible, and completely decomposed on a hot plate by adding nitric acid, hydrofluoric acid, and sulfuric acid. Then, using an inductively coupled plasma optical emission spectrometer (ICPAES, Perkin-Elmer 7300), the intensity of a standard solution prepared using a standard solution (5 mg / kg) is measured at a wavelength specific to the element to be analyzed, and a reference calibration curve is created. Then, the pretreated sample solution and a blank sample are introduced into the device, and the intensity of each is measured to calculate the actual intensity. The concentration of each component is calculated based on the created calibration curve, and the total is converted to a theoretical value, so that the content of the elements in the manufactured negative electrode active material can be analyzed.
[0040] In one embodiment of the present invention, the Li compound may be distributed in the form of lithium silicate on the silicon-based particles, thereby removing the irreversible capacity of the particles and playing a role in improving the initial efficiency and charge-discharge efficiency of the negative electrode active material. At this time, silicate means a compound containing silicon, oxygen, and one or more metals.
[0041] Specifically, the Li compound may be distributed on the surface, inside, or both the surface and inside of the silicon-based particles in the form of lithium silicate, and the lithium silicate may correspond to a matrix within the particles. The lithium silicate is represented by Li a Si b O c (2 ≤ a ≤ 4, 0 < b ≤ 2, 2 ≤ c ≤ 5) and can be classified into crystalline lithium silicate and amorphous lithium silicate. The crystalline lithium silicate may exist in the form of at least one lithium silicate selected from the group consisting of Li2SiO3, Li4SiO4, and Li2Si2O5 within the silicon-based particles, and the amorphous lithium silicate is Li a Si b O c (2 ≤ a ≤ 4, 0 < b ≤ 2, 2 ≤ c ≤ 5) and may consist of a complex structure, and is not limited to the above form.
[0042] In one embodiment of the present invention, the Li compound may include at least one crystalline-phase lithium silicate selected from the group consisting of crystalline-phase Li2SiO3, crystalline-phase Li4SiO4, and crystalline-phase Li2Si2O5. Further, the Li compound may further include an amorphous-phase lithium silicate.
[0043] Specifically, the Li compound contained in the silicon-based particles includes crystalline-phase Li2SiO3 and crystalline-phase Li2Si2O5, and may selectively further include crystalline-phase Li4SiO4 or amorphous-phase lithium silicate.
[0044] When the negative electrode active material contains a large amount of the crystalline phase Li2SiO3, the loss of discharge capacity per weight of the active material can be reduced. In the case of the crystalline phase Li2SiO3, the initial efficiency can be significantly increased as the structure is electrochemically stable, and the structure is stable even during charging and discharging, so that the life characteristics can be effectively improved.
[0045] The crystalline phase Li2Si2O5 is stable in the negative electrode active material, and there is little side reaction with water, particularly in the negative electrode slurry, specifically in the aqueous negative electrode slurry. However, when the negative electrode active material contains a large amount of the crystalline phase Li2Si2O5, there is a problem that the loss of discharge capacity per weight of the active material is large, and the crystalline phase Li2Si2O5 has an unstable structure during charging and discharging, which deteriorates the life characteristics.
[0046] In the case of the crystalline phase Li4SiO4, there is a problem that it undergoes a side reaction with moisture in the negative electrode slurry, which causes intensive gas generation, and by-products such as Li2O formed by the side reaction with moisture can increase the pH of the negative electrode slurry, making the slurry phase unstable and causing problems such as a change in viscosity.
[0047] In this regard, the anode active material of the present invention has a content of the crystalline phase Li2SiO3 greater than the content of the crystalline phase Li2SiO5 and the content of the crystalline phase Li4SiO4, and therefore can smoothly remove the irreversible capacity of the anode active material to improve the initial efficiency and charge / discharge efficiency, improve the phase stability of the anode slurry containing the anode active material, prevent the problem of low viscosity, improve the quality of the anode, and exhibit an excellent level of charge / discharge capacity, thereby improving the charge / discharge efficiency. In addition, as described below, the anode active material of the present invention has an increased content of the crystalline phase Li2SiO3 and a reduced total content of the amorphous phase, and therefore can improve the phase stability of the anode slurry, prevent defects in the anode, and significantly improve the charge / discharge capacity and efficiency.
[0048] Furthermore, the negative electrode active material of the present invention may contain Li element in an amount of more than 7 parts by weight and not more than 10 parts by weight, and when the content of crystalline phase Li2SiO3 is greater than the content of crystalline phase Li2Si2O5 in this range, the loss of discharge capacity per weight due to the increase in Li content in the negative electrode active material is small, and since it has an electrochemically stable lithium silicate structure, the structure is stable even during charging and discharging, and a high discharge capacity can be achieved when the same initial efficiency is achieved, and there is an effect of excellent life characteristics. In addition, as described below, there is an effect of preventing side reactions with moisture by reducing the total content of amorphous phase in the negative electrode active material.
[0049] On the other hand, when the content of the crystalline phase Li2Si2O5 is greater than the content of the crystalline phase Li2SiO3, the occurrence of side reactions with moisture is reduced, but the loss of discharge capacity per weight due to the increased Li content in the negative electrode active material is large, and the structure is unstable during charging and discharging, so that problems may occur in that the discharge capacity is low and the life characteristics are poor when the same initial efficiency is achieved.
[0050] In one embodiment of the invention, the content of the crystalline phase Li2SiO3 is greater than the sum of the content of the crystalline phase Li2Si2O5 and the content of the crystalline phase Li4SiO4. In another embodiment, the content of the crystalline phase Li2SiO3 may be greater than the content of the crystalline phase Li2Si2O5.
[0051] In one embodiment of the present invention, the content of the crystalline phase Li2SiO3 may be 60 parts by weight or more based on a total of 100 parts by weight of the crystalline phase lithium silicate. In another embodiment, the content of the crystalline phase Li2SiO3 may be 65 parts by weight or more, 70 parts by weight or more, or 74 parts by weight or more.
[0052] In one embodiment of the present invention, the crystalline phase Li2SiO3 may be included in an amount of 15 to 50 parts by weight based on a total of 100 parts by weight of the silicon-based particles. In another embodiment, the crystalline phase Li2SiO3 may be included in an amount of 17 to 48 parts by weight, 20 to 48 parts by weight, 20 to 45 parts by weight, 25 to 45 parts by weight, 30 to 45 parts by weight, or 35 to 42 parts by weight. When the content of the crystalline phase Li2SiO3 satisfies the above range, it is preferable in that it is advantageous to realize a capacity per gram, and that Li2SiO3 is stable during charging and discharging, thereby realizing a capacity / efficiency and providing excellent life characteristics. If the content exceeds the above range, there is a problem that the reactivity of Li2SiO3 with water is high, which adversely affects the processability of the aqueous slurry, and if the content is less than the above range, there is a problem that it is disadvantageous to realize capacity per gram and that stable Li2SiO3 during charging and discharging is insufficient, resulting in poor capacity / efficiency realization and poor life characteristics.
[0053] The upper limit of the content of the crystalline phase Li2SiO3 may be 50 parts by weight, 48 parts by weight, 45 parts by weight, 42 parts by weight, or 40 parts by weight, based on a total of 100 parts by weight of the silicon-based particles, and the lower limit may be 15 parts by weight, 17 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 33 parts by weight, 35 parts by weight, or 38 parts by weight.
[0054] In one embodiment of the present invention, the crystalline phase Li2Si2O5 may be included in an amount of 0.5 to 20 parts by weight based on a total of 100 parts by weight of the silicon-based particles. In another embodiment, the crystalline phase Li2Si2O5 may be included in an amount of 1 to 18 parts by weight, 3 to 18 parts by weight, 3 to 15 parts by weight, or 3 to 12 parts by weight.
[0055] The upper limit of the content of the crystalline phase Li2Si2O5 may be 20 parts by weight, 18 parts by weight, 15 parts by weight, or 12 parts by weight, based on a total of 100 parts by weight of the silicon-based particles, and the lower limit may be 0.5 parts by weight, 1 part by weight, 3 parts by weight, or 5 parts by weight.
[0056] If the content of the crystalline phase Li2Si2O5 exceeds the above range, the capacity loss per weight is excessively large and the structure of Li2Si2O5 is unstable, resulting in poor life characteristics. If the content of the crystalline phase Li2Si2O5 is less than the above range, the amount of Li2Si2O5, which has low reactivity with water, is too small, which may reduce the processability of the aqueous slurry. Therefore, if the content of the crystalline phase Li2Si2O5 satisfies the above range, the capacity loss per weight can be minimized, the life characteristics are not excessively reduced, the processability of the aqueous slurry is properly ensured, and it is preferable to realize a discharge capacity, initial efficiency, and life characteristics suitable for the operation of the battery.
[0057] In one embodiment of the present invention, the crystalline phase Li4SiO4 may be included in an amount of 5 parts by weight or less, specifically 3 parts by weight or less, 1 part by weight or less, or less than 0.1 parts by weight based on a total of 100 parts by weight of the silicon-based particles, and more specifically, the crystalline phase Li4SiO4 may not be present in the negative electrode active material. When the content of the crystalline phase Li4SiO4 satisfies the above range, it is preferable in terms of preventing the generation of by-products such as Li2O due to the reaction of the negative electrode active material with water during the preparation of the negative electrode slurry, specifically the aqueous negative electrode slurry, and the resulting increase in the pH of the negative electrode slurry and the deterioration of the quality of the negative electrode.
[0058] In one embodiment of the present invention, the difference between the content of the crystalline phase Li2SiO3 and the content of the crystalline phase Li2Si2O5 may be 1 to 50 parts by weight based on a total of 100 parts by weight of the silicon-based particles. Specifically, the difference between the content of the crystalline phase Li2Si2O5 and the content of the crystalline phase Li2SiO3 may be 5 to 45 parts by weight, 8 to 45 parts by weight, 10 to 40 parts by weight, 20 to 40 parts by weight, or 20 to 35 parts by weight.
[0059] The upper limit of the difference between the content of the crystalline phase Li2SiO3 and the content of the crystalline phase Li2Si2O5 may be 50 parts by weight, 45 parts by weight, 40 parts by weight, or 38 parts by weight, based on a total of 100 parts by weight of the silicon-based particles, and the lower limit may be 1 part by weight, 5 parts by weight, 8 parts by weight, 10 parts by weight, 15 parts by weight, or 20 parts by weight.
[0060] When the difference between the content of the crystalline phase Li2Si2O5 and the content of the crystalline phase Li2SiO3 satisfies the above range, it is possible to improve the phase stability of the negative electrode slurry, prevent defects in the negative electrode, and significantly improve the charge / discharge capacity and efficiency.
[0061] The confirmation and content of the crystalline phase lithium silicate of the crystalline phase Li2SiO3, crystalline phase Li4SiO4, or crystalline phase Li2Si2O5 can be determined by X-ray diffraction profile analysis or 29 Si-MAS-NMR( 29 Si-Magic Angle Spinning-Nuclear Magnetic Resonance, 29 It can be measured by analysis via Si-magic angle spinning-nuclear magnetic resonance.
[0062] Among them, 29 Si-MAS-NMR analysis is a type of solid-state NMR analysis technique. The rotor containing the sample is placed at a magic angle B0 with respect to the magnetic field B0. M This is an NMR analysis performed by fast spinning at an angle of 54.74° (e.g., 54.74°). This allows the presence or absence and content of crystalline phase Li2SiO3, crystalline phase Li4SiO4, crystalline phase Li2Si2O5, crystalline phase Si, and crystalline phase SiO2 contained in the negative active material of the present invention to be measured.
[0063] In one embodiment of the present invention, the negative electrode active material 29In the Si-MAS-NMR analysis, the height of peak p1 of Li2SiO3 appearing in the chemical shift peaks at -70 ppm to -80 ppm may be greater than the height of peak p2 of Li2Si2O5 appearing in the chemical shift peaks at -90 ppm to -100 ppm.
[0064] In one embodiment of the present invention, the negative electrode active material 29 In the Si-MAS-NMR analysis, the ratio p2 / p1 of the height of the peak p2 of Li2Si2O5 appearing in the chemical shift peak of -90 ppm to -100 ppm to the height of the peak p1 of Li2SiO3 appearing in the chemical shift peak of -70 ppm to -80 ppm may be 1 or less. Specifically, it may be 0.01 to 0.8, 0.05 to 0.7, or 0.1 to 0.6. When it is within the above range, the crystalline phase Li2SiO3 is sufficiently present in the negative electrode active material, and the phase stability of the negative electrode slurry described above can be improved, the negative electrode can be prevented from being defective, and the charge / discharge capacity and efficiency can be significantly improved.
[0065] The upper limit of p2 / p1 may be 1, 0.8, 0.7, 0.6, 0.5, or 0.4, and the lower limit may be 0.01, 0.05, 0.1, 0.15, or 0.2.
[0066] In one embodiment of the present invention, the negative electrode active material 29 In the Si-MAS-NMR analysis, the peak p3 of Li4SiO4 appearing in the chemical shift peaks at -60 ppm to -69 ppm may not be present. In this case, it is preferable in terms of preventing the generation of by-products such as Li2O due to a side reaction between Li4SiO4 in the negative electrode active material and moisture, the resulting increase in pH of the negative electrode slurry, and the deterioration of the quality of the negative electrode.
[0067] The contents of the crystalline phase Li2SiO3, crystalline phase Li4SiO4, and crystalline phase Li2Si2O5 may be achieved by performing a heat treatment process, adjusting the heat treatment temperature, an acid treatment process, etc. in the method for producing a negative electrode active material described below, but are not limited thereto.
[0068] In one embodiment of the present invention, the negative electrode active material may contain less than 5 parts by weight, specifically less than 4 parts by weight, based on a total of 100 parts by weight of the silicon-based particles, of crystalline phase SiO2, and in another embodiment, may contain 3 parts by weight or less. Preferably, the negative electrode active material may contain 1 part by weight or less, based on a total of 100 parts by weight of the silicon-based particles, or may not contain crystalline phase SiO2 at all. When the content of the crystalline phase SiO2 satisfies the above range, the negative electrode is easily charged and discharged, and the charge and discharge capacity and efficiency can be improved.
[0069] In one embodiment of the present invention, the negative electrode active material may contain 10 to 50 parts by weight, 15 to 40 parts by weight, 15 to 30 parts by weight, 20 to 30 parts by weight, or 20 to 25 parts by weight of crystalline phase Si based on a total of 100 parts by weight of the silicon-based particles. When the content of the crystalline phase Si satisfies the above range, the negative electrode can be easily charged and discharged, and the charge and discharge capacity and efficiency can be improved.
[0070] In one embodiment of the present invention, the total content of crystalline phases present in the silicon-based particles is greater than the total content of amorphous phases. The total content of crystalline phases means the total content of all crystalline phases present in the silicon-based particles, including crystalline phase Si, crystalline phase SiO2, crystalline phase Li2SiO3, crystalline phase Li4SiO4, crystalline phase Li2Si2O5, etc., and the total content of amorphous phases may mean the content excluding the total content of crystalline phases present in the silicon-based particles. That is, the total content of amorphous phases means the sum of the content of all amorphous phases present in the particles, including amorphous phase SiO2, etc. in addition to amorphous phase lithium silicate.
[0071] The negative electrode active material of the present invention is preferable in that the total content of the crystalline phase present in the silicon-based particles is greater than the total content of the amorphous phase, and therefore the content of amorphous phase lithium silicate and the like, which is highly reactive with moisture, is reduced during the preparation of a negative electrode slurry, specifically, an aqueous negative electrode slurry, and the generation of by-products such as LiO due to side reactions with moisture, which in turn increases the pH of the negative electrode slurry, and thus prevents defects in the quality of the negative electrode.
[0072] In one embodiment of the present invention, the total content of the crystalline phase present in the silicon-based particles may be more than 50 parts by weight and not more than 85 parts by weight based on a total of 100 parts by weight of the silicon-based particles, specifically, 55 parts by weight or more and not more than 85 parts by weight, 55 parts by weight or more and not more than 80 parts by weight, 55 parts by weight or more and not more than 75 parts by weight, 60 parts by weight or more and not more than 70 parts by weight, 62 parts by weight or more and not more than 68 parts by weight, 64 parts by weight or more and not more than 68 parts by weight, or 64 parts by weight or more and not more than 66 parts by weight.
[0073] The upper limit of the total content of the crystalline phase may be 85 parts by weight, 83 parts by weight, 80 parts by weight, 75 parts by weight, 70 parts by weight, 68 parts by weight, or 66 parts by weight, and the lower limit may be 55 parts by weight, 60 parts by weight, 62 parts by weight, or 64 parts by weight, based on a total of 100 parts by weight of the silicon-based particles.
[0074] In one embodiment of the present invention, the total content of the amorphous phase present in the silicon-based particles may be 15 parts by weight or more and less than 50 parts by weight based on 100 parts by weight of the total silicon-based particles, specifically, 20 parts by weight or more and less than 50 parts by weight, 25 parts by weight or more and less than 50 parts by weight, 25 parts by weight or more and less than 45 parts by weight, 30 parts by weight or more and less than 40 parts by weight, 32 parts by weight or more and less than 36 parts by weight, or 34 parts by weight or more and less than 36 parts by weight.
[0075] The upper limit of the total content of the amorphous phase may be 48 parts by weight, 45 parts by weight, 40 parts by weight, 38 parts by weight, or 36 parts by weight, and the lower limit may be 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 32 parts by weight, or 34 parts by weight, based on a total of 100 parts by weight of the silicon-based particles.
[0076] In one embodiment of the present invention, the difference between the total content of the crystalline phase and the total content of the amorphous phase present in the silicon-based particles may be 10 parts by weight or more and 70 parts by weight or less, 20 parts by weight or more and 68 parts by weight or less, 20 parts by weight or more and 50 parts by weight or less, 25 parts by weight or more and 40 parts by weight or less, 28 parts by weight or more and 36 parts by weight or less, or 30 parts by weight or more and 36 parts by weight or less, based on a total of 100 parts by weight of the silicon-based particles.
[0077] The upper limit of the difference between the total content of the crystalline phase and the total content of the amorphous phase present in the silicon-based particles may be 70 parts by weight, 68 parts by weight, 66 parts by weight, 60 parts by weight, 50 parts by weight, 40 parts by weight, or 36 parts by weight, based on a total of 100 parts by weight of the silicon-based particles, and the lower limit may be 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 28 parts by weight, or 30 parts by weight.
[0078] In one embodiment of the present invention, the ratio of the total weight of the crystalline phase to the total weight of the amorphous phase present in the silicon-based particles (total weight of the crystalline phase:total weight of the amorphous phase) may be 55:45 to 85:15, 60:40 to 80:20, or 60:40 to 75:25.
[0079] When the relationship between the contents of the crystalline phase and the amorphous phase present in the silicon-based particles satisfies the above range, the contents of the crystalline phase and the amorphous phase present in the negative electrode active material are appropriately adjusted, and the content of amorphous phase lithium silicate, which is highly reactive with moisture, is reduced during the preparation of the negative electrode slurry (specifically, an aqueous negative electrode slurry), and the generation of by-products such as Li2O due to side reactions with moisture, which can prevent an increase in pH and a change in viscosity of the negative electrode slurry, is prevented. This is preferable in that the content of the crystalline phase SiO2, which is an obstacle to the expression of charge / discharge capacity and efficiency, is not excessively increased.
[0080] Even if the content of the crystalline phase Li2SiO3 in lithium silicate is the highest, if the total content of the crystalline phases present in the negative electrode active material exceeds the above range, the crystalline phases are excessively contained in the negative electrode active material, which may result in problems such as difficulty in charging and discharging, difficulty in achieving capacity / efficiency, and deterioration in life characteristics. If the content is below the above range, the crystalline phases are not sufficiently contained, which may result in problems such as difficulty in effectively controlling side reactions with moisture.
[0081] The total content of the crystalline phase and the total content of the amorphous phase present in the silicon-based particles can be measured by a quantitative analysis method using X-ray diffraction analysis (XRD).
[0082] In one embodiment of the present invention, the silicon-based particles may include additional metal atoms. The metal atoms may be present in the silicon-based particles in the form of at least one of metal atoms, metal silicates, metal silicides, and metal oxides. The metal atoms may include at least one selected from the group consisting of Mg, Li, Al, and Ca. This can improve the initial efficiency of the negative electrode active material.
[0083] In one embodiment of the present invention, the silicon-based particles have a carbon layer on at least a part of the surface. In this case, the carbon layer may be partially coated on at least a part of the surface, i.e., the surface of the particle, or may be coated on the entire surface of the particle. The carbon layer imparts electrical conductivity to the negative electrode active material, and the initial efficiency, life characteristics, and capacity characteristics of the secondary battery can be improved.
[0084] In one embodiment of the present invention, the carbon layer contains amorphous carbon. The carbon layer may further contain crystalline carbon.
[0085] The crystalline carbon may further improve the electrical conductivity of the negative electrode active material. The crystalline carbon may include at least one selected from the group consisting of fullerene, carbon nanotube, and graphene.
[0086] The amorphous carbon can appropriately maintain the strength of the carbon layer and suppress the expansion of the silicon-based particles. The amorphous carbon may be a carbon-based material formed by using at least one carbide or hydrocarbon selected from the group consisting of tar, pitch, and other organic substances as a source of a chemical vapor deposition process.
[0087] The other carbonized organic matter may be a carbonized organic matter selected from carbonized sucrose, glucose, galactose, fructose, lactose, mannose, ribose, aldohexose, or ketohexose, and combinations thereof.
[0088] The hydrocarbon may be a substituted or unsubstituted aliphatic or alicyclic hydrocarbon, or a substituted or unsubstituted aromatic hydrocarbon. The aliphatic or alicyclic hydrocarbon of the substituted or unsubstituted aliphatic or alicyclic hydrocarbon may be methane, ethane, ethylene, acetylene, propane, butane, butene, pentane, isobutane, or hexane, etc. The aromatic hydrocarbon of the substituted or unsubstituted aromatic hydrocarbon may be benzene, toluene, xylene, styrene, ethylbenzene, diphenylmethane, naphthalene, phenol, cresol, nitrobenzene, chlorobenzene, indene, coumarone, pyridine, anthracene, or phenanthrene, etc.
[0089] In one embodiment of the present invention, the carbon layer may be an amorphous carbon layer. In one embodiment of the present invention, the carbon layer may be included in an amount of 0.1 to 50 parts by weight, 0.1 to 30 parts by weight, or 0.1 to 20 parts by weight based on a total of 100 parts by weight of the negative electrode active material. More specifically, the carbon layer may be included in an amount of 0.5 to 15 parts by weight, 1 to 10 parts by weight, or 1 to 5 parts by weight. When the amount is within the above range, it is possible to prevent a decrease in the capacity and efficiency of the negative electrode active material.
[0090] In one embodiment of the present invention, the thickness of the carbon layer may be 1 nm to 500 nm, specifically 5 nm to 300 nm. When the thickness satisfies the above range, the conductivity of the negative electrode active material is improved, the volume change of the negative electrode active material is easily suppressed, the side reaction between the electrolyte and the negative electrode active material is suppressed, and the initial efficiency and / or life of the battery are improved.
[0091] Specifically, the carbon layer may be formed by chemical vapor deposition (CVD) using at least one hydrocarbon gas selected from the group consisting of methane, ethane, and acetylene.
[0092] In the present invention, the crystallinity of the carbon layer can be confirmed by calculating the D / G band ratio using Raman spectroscopy. Specifically, the measurement can be performed using a Renishaw 2000 Raman microscope system and 532 nm laser excitation, with a 100x optical lens at a low laser power density and an exposure time of 30 seconds to avoid the thermal effect of the laser. In order to reduce positional deviations, a total of 25 points are measured for an area of 5 μm×5 μm, and the average values of the D band and G band are calculated after fitting using a Lorentzian function.
[0093] In one embodiment of the present invention, lithium by-products may be present on the silicon-based particles. Specifically, the lithium by-products may be present on the surface of the silicon-based particles or on the surface of the carbon layer. The lithium by-products may also be present between a surface layer described below and the silicon-based particles.
[0094] Specifically, the lithium by-product may refer to a lithium compound remaining near the surface of the silicon-based particles or the carbon layer after the silicon-based particles are manufactured. As described above, even after the acid treatment process, lithium by-products that have not reacted with the acid may remain.
[0095] The lithium by-products may include one or more selected from the group consisting of Li2O, LiOH, and Li2CO3.
[0096] The presence or absence of the lithium by-product can be confirmed by X-ray diffraction analysis (XRD) or X-ray photoelectron spectroscopy (XPS).
[0097] The lithium by-product may be contained in an amount of 5 parts by weight or less based on 100 parts by weight of the total negative electrode active material. Specifically, the lithium by-product may be contained in an amount of 0.01 to 5 parts by weight, 0.05 to 2 parts by weight, or 0.1 to 1 part by weight. More specifically, the lithium by-product may be contained in an amount of 0.1 to 0.8 parts by weight, or 0.1 to 0.5 parts by weight. When the content of the lithium by-product satisfies the above range, the side reaction in the slurry can be reduced, the viscosity change can be reduced, and the aqueous processability characteristics can be improved. On the other hand, when the content of the lithium by-product is higher than the above range, the slurry shows basicity during formation, which causes side reactions and changes in viscosity, resulting in problems in aqueous processability.
[0098] The content of the lithium by-product can be calculated by measuring the amount of the HCl solution in a specific range where the pH changes during titration of the aqueous solution containing the negative active material with the HCl solution using a titrator.
[0099] In one embodiment of the present invention, the surface of the negative electrode active material may be substantially free of lithium by-products selected from the group consisting of crystalline lithium silicate, Li2O, LiOH, and Li2CO3. The lithium by-products may increase the pH of the negative electrode slurry, lower the viscosity, and cause the electrode condition of the negative electrode to deteriorate. Thus, by performing an acid treatment process on the negative electrode active material and removing by-products such as lithium silicate and Li2O present on the surface of the negative electrode active material, the quality of the negative electrode and the effect of improving the charge and discharge efficiency can be realized at a preferable level.
[0100] A silicon-based particle according to one embodiment of the present invention includes a surface layer disposed on at least a portion of the silicon-based particle, the surface layer may include Al, P, and O. In one embodiment of the present invention, the surface layer may further contain Li element.
[0101] The surface layer may be in a form covering at least a part of silicon-based particles having a carbon layer provided on the surface. That is, the surface layer may be in a form partially covering the surface of the particles or covering the entire surface of the particles. Examples of the shape of the surface layer include an island type or a thin film type, but the shape of the surface layer is not limited thereto.
[0102] The surface layer may be provided on at least a part of the outer surface of the carbon layer. That is, the surface layer is coated adjacent to the carbon layer, and SiO x (0 < x < 2) and may be provided in the form of silicon-based particles - carbon layer - surface layer containing a Li compound. The surface layer may substantially or completely cover the carbon layer or may partially cover the carbon layer.
[0103] The surface layer is the SiO x (0 < x < 2) and may be provided on a region where the carbon layer is not provided in the surface of the silicon-based particles containing a Li compound. That is, the surface layer is coated adjacent to the silicon-based particles containing SiO x (0 < x < 2) and a Li compound, and may be provided in the form of silicon-based particles - surface layer containing SiO x (0 < x < 2) and a Li compound.
[0104] In one embodiment of the present invention, the Al may be contained in an amount of 0.05 parts by weight to 0.4 parts by weight based on 100 parts by weight in total of the negative electrode active material. Specifically, it may be contained in an amount of 0.1 parts by weight to 0.4 parts by weight, may be contained in an amount of 0.12 parts by weight to 0.35 parts by weight, or may be contained in an amount of 0.15 parts by weight to 0.3 parts by weight.
[0105] In one embodiment of the present invention, the P may be contained in an amount of 0.05 parts by weight to 2 parts by weight based on 100 parts by weight in total of the negative electrode active material. Specifically, it may be contained in an amount of 0.1 parts by weight to 1.5 parts by weight, or may be contained in an amount of 0.15 parts by weight to 1 part by weight.
[0106] The surface layer is Alz P w O v (0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) may include a phase. The Al z P w O v phase may include aluminum oxide, phosphorus oxide, aluminum phosphate, etc. z, y, and v represent the atomic number ratios. As an example, the Al z P w O v phase may include a mixture or compound formed from AlPO4 or Al(PO3)3, etc., but is not limited thereto.
[0107] The surface layer may include Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) may include a phase. The Li y Al z P w O v phase may include aluminum oxide, phosphorus oxide, lithium oxide, aluminum phosphate, lithium salt, lithium phosphate, lithium aluminate, etc. y, z, w, and v represent the atomic number ratios. As an example, the Li y Al z P w O v phase may include a mixture or compound formed from Li3PO4, AlPO4, Al(PO3)3, or LiAlO2, etc., but is not limited thereto.
[0108] The y may satisfy 0 < y ≤ 3. The z may satisfy 0 < z ≤ 1. The w may satisfy 0.5 ≤ w ≤ 3. The v may satisfy 4 < v ≤ 10.
[0109] When an inorganic surface layer including such a phase is provided, it is possible to prevent the Li compound included in the silicon-based particles from reacting with the water in the slurry to reduce the viscosity of the slurry, thereby improving the stability of the electrode state and / or the charge / discharge capacity.
[0110] In one embodiment of the present invention, the surface layer may include an amorphous phase. Specifically, the surface layer may be an amorphous phase.
[0111] When the surface layer contains an amorphous phase as described above, Li ions can enter and leave the battery more easily than when the surface layer does not contain an amorphous phase, which has the effect of effectively reducing side reactions in the slurry and stably achieving capacity and / or efficiency.
[0112] In one embodiment of the present invention, the surface layer may further include one or more selected from the group consisting of Li2O, LiOH, and Li2CO3. Generally, when a substance remaining in the process of doping lithium into a silicon-based particle is exposed to moisture or air, it may form lithium by-products such as Li2O, LiOH, and Li2CO3, so the surface layer may be in a form containing one or more selected from the group consisting of Li2O, LiOH, and Li2CO3.
[0113] In one embodiment of the present invention, the negative electrode active material may not show a crystalline peak derived from the surface layer in an X-ray diffraction analysis. y Al z P w O v(0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) It is not necessary to detect a crystalline peak derived from the phase. When a crystalline peak derived from the surface layer appears, there is a problem that the surface layer contains an excessive amount of crystal and the capacity and / or efficiency decreases. As an example, in the case of a crystalline peak derived from the surface layer, it can be known through the change before / after the surface layer coating. Specifically, in the case of XRD, a crystalline peak is detected. When there is no difference in the XRD graph of the negative electrode active material before / after the surface layer coating, it means that no crystalline peak derived from the surface layer appears, and it can be confirmed that the surface layer is formed in an amorphous phase.
[0114] In one embodiment of the present invention, the amorphous phase contained in the surface layer may be contained in an amount exceeding 50 parts by weight based on 100 parts by weight in total of the surface layer. Specifically, the amorphous phase may be contained in an amount of 60 parts by weight or more, 70 parts by weight or more, 80 parts by weight or more, 90 parts by weight or more, 95 parts by weight or more, or 99 parts by weight or more, and may be contained in an amount of 100 parts by weight or less, or less than 100 parts by weight based on 100 parts by weight in total of the surface layer. By satisfying the above range, side reactions in the slurry can be efficiently suppressed, and there is an effect that the capacity and / or efficiency can be stably realized.
[0115] In one embodiment of the present invention, the surface layer may be contained in an amount of 10 parts by weight or less based on 100 parts by weight in total of the negative electrode active material. Specifically, it may be contained in an amount of 8 parts by weight or less, 6 parts by weight or less, or 5 parts by weight or less, and may be contained in an amount of 0.1 parts by weight or more, or 0.5 parts by weight or more. More specifically, it may be contained in an amount of 1 part by weight or more and 5 parts by weight or less, or 1.5 parts by weight or more and 3 parts by weight or less. When the content of the surface layer is less than the above range, it is difficult to prevent gas generation in the slurry, and when it is excessive compared to the above range, there is a problem that it is difficult to realize the capacity or efficiency.
[0116] In one embodiment of the present invention, the weight ratio of the surface layer to the carbon layer may be 1:0.1 to 1:30. Specifically, it may be 1:0.5 to 1:5, 1:1 to 1:4, or 1:1 to 1:3. By satisfying the above range, the carbon layer and the surface layer can effectively cover the silicon-based composite particles, and side reactions in the slurry can be efficiently suppressed, and capacity and / or efficiency can be stably achieved. On the other hand, if the content of the surface layer is excessively higher than that of the carbon layer, it is difficult to achieve capacity or efficiency, and if the content of the carbon layer is excessively higher than that of the surface layer, it is difficult to prevent gas generation in the slurry.
[0117] In one embodiment of the present invention, the surface layer may be included in an amount of 90 parts by weight or less based on 100 parts by weight of the carbon layer. Specifically, the surface layer may be included in an amount of 80 parts by weight or less, 70 parts by weight or less, 60 parts by weight or less, or 50 parts by weight or less based on 100 parts by weight of the carbon layer. In addition, the surface layer may be included in an amount of 0.1 parts by weight or more, 1 part by weight or more, 5 parts by weight or more, or 10 parts by weight or more based on 100 parts by weight of the carbon layer. By satisfying the above ranges, the carbon layer and the surface layer can effectively cover the silicon-based composite particles, thereby efficiently suppressing side reactions in the slurry, and the capacity and / or efficiency can be stably achieved.
[0118] The average particle size (D 50 ) may be 0.1 μm to 14 μm, specifically 1 μm to 12 μm, and more specifically 1 μm to 10 μm. When the above range is satisfied, the structure of the active material during charging and discharging can be stabilized, the problem of the volume expansion / contraction level increasing due to the particle size being too large can be prevented, and the problem of the initial efficiency decreasing due to the particle size being too small can be prevented.
[0119] The BET specific surface area of the negative electrode active material is 1 m 2 / g~100m 2 / g, specifically 1m 2 / g~70m 2It may be / g, more specifically 1 m 2 / g to 50 m 2 / g, for example 2 m 2 / g to 30 m 2 It may be / g. When the above range is satisfied, side reactions with the electrolyte during charging and discharging of the battery can be reduced, so that the life characteristics of the battery can be improved.
[0120] <Method for manufacturing negative electrode active material> The present invention provides a method for manufacturing a negative electrode active material, specifically, the method for manufacturing the negative electrode active material described above.
[0121] One embodiment of the present invention is SiO x Forming particles containing a silicon-based oxide represented by (0 < x < 2); and heat-treating after mixing the particles containing the silicon-based oxide and a lithium precursor. The present invention provides a method for manufacturing a negative electrode active material.
[0122] The SiO x The step of forming particles containing a silicon-based oxide represented by (0 < x < 2) may include heating and vaporizing Si powder and SiO2 powder in a vacuum, and then depositing the vaporized mixed gas.
[0123] Specifically, the mixed powder of the Si powder and SiO2 powder may be heat-treated at 1300 °C to 1800 °C, 1400 °C to 1800 °C, or 1400 °C to 1600 °C under vacuum.
[0124] The particles formed by the above method are represented by SiO x (0 < x < 2), and the silicon-based oxide is preferably a compound represented by SiO x (0.5 ≤ x ≤ 1.5) in terms of the structural stability of the active material. The formed silicon-based oxide may have the form of SiO.
[0125] In the method for manufacturing a negative electrode active material according to one embodiment of the present invention, before mixing the lithium precursor, SiO xA step of forming a carbon layer on the surface of particles containing a silicon-based oxide represented by (0 < x < 2) may be further included.
[0126] The carbon layer is disposed or formed on the particles and can function as a protective layer that appropriately controls the volume expansion due to charge and discharge of the negative electrode active material and prevents side reactions with the electrolyte. On the other hand, the carbon layer formation step may be performed before the mixing step of the particles and the lithium precursor in terms of preventing changes in the crystalline phase and amorphous phase of the negative electrode active material.
[0127] The carbon layer may be formed by using a chemical vapor deposition method (CVD) using a hydrocarbon gas or by a method of carbonizing a substance serving as a carbon source.
[0128] Specifically, after the formed particles are put into a reactor, chemical vapor deposition (CVD) may be performed at 600°C to 1200°C with a hydrocarbon gas so as to prevent changes in the crystalline phase and amorphous phase. The hydrocarbon gas may be at least one hydrocarbon gas selected from the group consisting of methane, ethane, propane, and acetylene, and may be heat-treated at 900°C to 1000°C.
[0129] The particle size of the particles containing the silicon-based oxide may be adjusted by a method such as a ball mill, a jet mill, or air classification, and is not limited thereto.
[0130] The method for manufacturing a negative electrode active material according to an embodiment of the present invention may include a step of heat-treating after mixing the particles containing the silicon-based oxide and a lithium precursor.
[0131] By the step of heat-treating after mixing the particles containing the silicon-based oxide and the lithium precursor, SiO xSilicon-based particles containing (0 < x < 2) and a Li compound can be produced. In the silicon-based particles, the content of the crystalline phase Li2SiO3 in the particles is higher than the content of the crystalline phase Li2Si2O5 and the content of the crystalline phase Li4SiO4, and the total content of the crystalline phases present in the particles may be higher than the total content of the amorphous phase.
[0132] The lithium precursor can be made to contain a Li compound in the particles containing the silicon-based oxide by a heat treatment step described later. Specifically, the lithium precursor may contain at least one selected from the group consisting of lithium metal, LiOH, LiH, and Li2CO3. Specifically, in terms of preventing additional oxidation during the reaction between the particles containing the silicon-based oxide and the lithium precursor, it may contain lithium metal. The lithium precursor may be in particulate form, specifically, it may be lithium metal powder.
[0133] Specifically, the lithium precursor may contain lithium metal powder (SLMP, stabilized lithium metal powder).
[0134] In one embodiment of the present invention, the particles containing the silicon-based oxide and the lithium precursor may be solid mixed. Specifically, during the mixing, the particles containing the silicon-based oxide and the lithium precursor may be in a solid state. In this case, since the porosity and specific surface area in the negative electrode active material can be controlled to appropriate levels during the formation of the negative electrode active material by heat treatment described later, volume expansion control of the negative electrode active material due to charge and discharge can be preferably performed.
[0135] In one embodiment of the present invention, the weight ratio of the particles containing the silicon-based oxide to the lithium precursor may be 80:20 to 94:6. Specifically, it may be 85:15 to 93:7, 88:12 to 93:7, or 90:10 to 92:8.
[0136] In one embodiment of the present invention, the particles containing a silicon-based oxide and the lithium precursor may be mixed while being heat-treated in an inert gas atmosphere.
[0137] The heat treatment temperature of the particles containing the silicon-based oxide and the lithium precursor mixture may be 650° C. to 950° C., specifically 670° C. to 900° C., or 700° C. to 850° C. When the particles are mixed while being heat treated under the above conditions, it is preferable in that the crystalline phase of lithium silicate, Li2SiO3, is easily developed.
[0138] The heat treatment process in the above temperature range allows the silicon-based particles produced to contain an appropriate level of Li compound, specifically, the Li compound may be distributed on the surface, inside, or on the surface and inside of the silicon-based particles. The silicon-based particles may further contain lithium silicide or lithium oxide, etc., as the Li compound.
[0139] The above-mentioned negative active material can be manufactured by the heat treatment process in the above temperature range. Specifically, the lithium can be distributed in the form of lithium silicate in the particles by the heat treatment process in the above temperature range, and thus the irreversible capacity of the particles containing the silicon-based oxide can be removed, thereby improving the initial efficiency and the charge / discharge efficiency of the negative active material. Specifically, the lithium may be present in the form of at least one crystalline phase lithium silicate selected from the group consisting of crystalline phase Li2SiO3, crystalline phase Li4SiO4, and crystalline phase Li2Si2O5, or amorphous phase lithium silicate. In this case, in the negative active material manufactured by the method for manufacturing a negative active material of the present invention, the content of the crystalline phase Li2SiO3 may be greater than the sum of the content of the crystalline phase Li2Si2O5 and the content of the crystalline phase Li4SiO4, and the content of the crystalline phase Li2SiO3 may be 60 parts by weight or more based on 100 parts by weight of the total of the crystalline phase lithium silicate.
[0140] In addition, by the heat treatment process in the above temperature range, the total content of the crystalline phase present in the silicon-based particles may be greater than the total content of the amorphous phase, and thus the content of lithium oxide and lithium silicate that react with moisture is small, gas generation and viscosity change of the negative electrode slurry can be prevented, and the phase stability of the slurry including the negative electrode active material can be improved, so that the quality and charge / discharge efficiency of the negative electrode including the negative electrode active material and the secondary battery including the negative electrode can be improved.
[0141] If the heat treatment process is performed at a temperature below 650°C, the content of the amorphous phase in the negative active material prepared by the above-mentioned method increases, which may cause problems in the processability of the aqueous slurry.If the heat treatment process is performed at a temperature above 950°C, the content of the crystalline SiO2 increases, which acts as a resistor during charging and discharging, making charging and discharging difficult, and causing problems such as reduced charge and discharge capacity and efficiency.
[0142] The heat treatment may be performed for 1 to 12 hours, specifically 2 to 8 hours. When the heat treatment is performed within the above range, lithium silicate can be uniformly distributed within the silicon-based particles, and thus the above-mentioned effect of improving the charge / discharge efficiency can be further improved.
[0143] The heat treatment may be performed in an inert atmosphere to prevent additional oxidation of the silicon-based oxide-containing particles and the lithium precursor. Specifically, the heat treatment may be performed in an inert atmosphere of at least one gas selected from the group consisting of nitrogen gas, argon gas, and helium gas.
[0144] The method for preparing a negative active material of the present invention may further include a step of performing an acid treatment after the heat treatment.
[0145] After the heat treatment, at least a portion of the surface of the formed silicon-based particles is provided with a lithium compound (lithium by-product). xIn the process of doping particles containing (0 < x < 2) with a Li compound, lithium compounds, that is, lithium by-products formed by unreacted lithium, will remain near the surface of the silicon-based particles. The lithium by-products may be lithium silicate, Li2O, etc., which can increase the pH of the negative electrode slurry containing the negative electrode active material, lower the viscosity, and cause deterioration of the electrode state of the negative electrode. Accordingly, by performing an acid treatment step after the heat treatment step to remove by-products such as lithium silicate and Li2O present on the surface of the negative electrode active material, the quality of the negative electrode and the improvement effect of charge and discharge efficiency can be realized at a preferable level.
[0146] Specifically, the acid treatment may be performed for 0.3 hours to 6 hours, specifically 0.5 hours to 4 hours, with an acid aqueous solution containing at least one acid selected from the group consisting of hydrochloric acid (HCl), sulfuric acid (H2SO4), nitric acid (HNO3), and phosphoric acid (H3PO4), specifically at least one acid selected from the group consisting of hydrochloric acid (HCl), sulfuric acid (H2SO4), and nitric acid (HNO3). This is preferable in that by-products present on the surface of the negative electrode active material can be easily removed by this step.
[0147] The pH of the acid aqueous solution at 23°C may be 3 or less, specifically 2 or less, more specifically 1 or less, in terms of easily removing by-products present on the surface of the negative electrode active material.
[0148] The method for manufacturing a negative electrode active material of the present invention may further include a step of providing a surface layer on at least a part of the silicon-based particles formed after the heat treatment step. As an example, when the acid treatment step is performed after the heat treatment step, it may further include a step of providing the surface layer after the acid treatment step.
[0149] The surface layer may be provided by mixing the silicon-based particles and aluminum phosphate. Specifically, i) a step of dry-mixing the silicon-based particles and aluminum phosphate and then performing heat treatment, or ii) a step of mixing the silicon-based particles and aluminum phosphate in a solvent, followed by heat treatment to vaporize the solvent while reacting the silicon-based particles and aluminum phosphate, may be used to form a surface layer on at least a part of the silicon-based particles. When forming the surface layer by the above method, the lithium by-products formed or remaining in the manufacturing process of the silicon-based particles can be reacted with aluminum phosphate to easily form the surface layer.
[0150] The aluminum phosphate may be in the form of Al b P c O d (0 < b ≤ 10, 0 < c ≤ 10, 0 < d ≤ 10). Specifically, it may be Al(PO3)3 or AlPO4, but is not limited thereto, and salts used in the art for forming the surface layer may be appropriately employed.
[0151] Alternatively, iii) a step of dry-mixing the silicon-based particles, aluminum precursor, and phosphorus precursor and then performing heat treatment, or iv) a step of mixing the silicon-based particles, aluminum precursor, and phosphorus precursor in a solvent, followed by heat treatment to vaporize the solvent while reacting the silicon-based composite particles, aluminum precursor, and phosphorus precursor, may be used to form a surface layer on at least a part of the silicon-based particles. When forming the surface layer by the above method, the lithium by-products, aluminum precursor, and phosphorus precursor formed in the manufacturing process of the silicon-based composite particles can be reacted to easily form the surface layer.
[0152] The aluminum precursor may be aluminum oxide in the form of Al a O b (0 < a ≤ 10, 0 < b ≤ 10), and specifically, it may be Al2O3.
[0153] Alternatively, the aluminum precursor may be aluminum hydroxide, aluminum nitrate, aluminum sulfate, etc. Specifically, it may be Al(OH)3, Al(NO3)3·9H20, or Al2(SO4)3, but is not limited thereto, and an aluminum precursor used in the art to form the surface layer may be appropriately employed.
[0154] The phosphorus precursor is P c O d It may be phosphorus oxide in the form of P(0 < c ≦ 10, 0 < d ≦ 10).
[0155] Alternatively, the phosphorus precursor may be ammonium phosphate, diammonium phosphate, phosphoric acid, etc. Specifically, it may be (NH4)3PO4, (NH4)2HPO4, H3PO4, or NH4H2PO4, but is not limited thereto, and a phosphorus precursor used in the art to form the surface layer may be appropriately employed.
[0156] Alternatively, in step v), the silicon-based particles and the Li-Al-P-O-based precursor are dry-mixed and heat-treated, or in step vi), after the silicon-based composite particles and the Li-Al-P-O-based precursor are mixed in a solvent and then heat-treated to vaporize the solvent, the silicon-based composite particles and the Li-Al-P-O-based precursor are reacted to form a surface layer on at least a part of the silicon-based particles. When forming the surface layer by the above method, the Li-Al-P-O-based precursor can be directly introduced to form the surface layer.
[0157] The Li-Al-P-O-based precursor is Li y Al z P w O v It may be in the form of Li3PO4, AlPO4, Al(PO3)3, or LiAlO2, etc., and may be a mixture or compound formed complexly therefrom, but is not limited thereto, and a configuration used in the art to form the surface layer may be appropriately employed.
[0158] In the step of providing a surface layer on at least a part of the silicon-based particles, the heat treatment may be performed at 500°C to 700°C, specifically, it may be performed at 550°C to 650°C. However, it is not limited thereto and may vary depending on the salt or precursor used, etc.
[0159] When the heat treatment temperature satisfies the above range, the reaction between the salt or precursor and the Li by-product occurs well, and since the surface layer contains Li, the durability of the formed negative electrode active material against moisture increases, the entry and exit of Li ions by the surface layer becomes easy, the lithium diffusion resistance on the surface of the negative electrode active material becomes low, and there is an effect that the discharge rate capability is excellent.
[0160] The solvent may be water or ethanol, and is not limited thereto, and solvents used in the art may be appropriately employed.
[0161] The surface layer formed on the silicon-based particles preferably contains Li y Al z P w O v (0 < y ≤ 10, 0 < z ≤ 10, 0 < w ≤ 10, 0 < v ≤ 10) phase, and the Li y Al z P w O v phase may be an amorphous phase.
[0162] <Negative electrode> The negative electrode according to an embodiment of the present invention may contain the above-described negative electrode active material. Specifically, the negative electrode may include a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer may contain the negative electrode active material. Further, the negative electrode active material layer may further contain a binder, a thickener, and / or a conductive material.
[0163] The negative electrode active material layer may be formed by applying a negative electrode slurry containing a negative electrode active material, a binder, a thickener, and / or a conductive material to at least one surface of a current collector, followed by drying and rolling. The negative electrode slurry may further include an additional negative electrode active material.
[0164] The additional negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, lithium titanium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, either low-crystalline carbon or high-crystalline carbon may be used as the carbon material. Typical low-crystalline carbons are soft carbon and hard carbon, and typical high-crystalline carbons are amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, mesocarbon microbeads, mesophase pitches, and high-temperature fired carbons such as petroleum or coal tar pitch derived cokes.
[0165] The additional anode active material may be a carbon-based anode active material. In an embodiment of the present invention, the weight ratio of the negative electrode active material to the additional negative electrode active material contained in the negative electrode slurry may be 10:90 to 90:10, specifically, 10:90 to 50:50.
[0166] The negative electrode slurry may include a solvent for forming a negative electrode slurry. Specifically, the solvent for forming a negative electrode slurry may include at least one selected from the group consisting of distilled water, ethanol, methanol, and isopropyl alcohol, specifically, distilled water, in order to facilitate dispersion of components.
[0167] The negative electrode slurry containing the negative electrode active material according to one embodiment of the present invention may have a pH of 7 to 11 at 25° C. When the pH of the negative electrode slurry satisfies the above range, the rheological properties of the slurry are stabilized. On the other hand, when the pH of the negative electrode slurry is less than 7 or exceeds 11, decomposition of carboxymethyl cellulose (CMC) used as a thickener occurs, causing a decrease in the viscosity of the slurry, and a problem occurs in that the degree of dispersion of the active material contained in the slurry decreases.
[0168] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has electrical conductivity. For example, the current collector may be made of copper, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, or the like. Specifically, a transition metal that easily adsorbs carbon, such as copper or nickel, may be used as the current collector. The thickness of the current collector may be 6 μm to 20 μm, but is not limited thereto.
[0169] The binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, Ca, or the like, or may include various copolymers thereof.
[0170] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive, and examples of the conductive material that may be used include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0171] The thickener may be carboxymethyl cellulose (CMC), but is not limited thereto, and any thickener used in the present technical field may be appropriately adopted.
[0172] In an embodiment of the present invention, the weight ratio of the negative electrode active material to the additional negative electrode active material contained in the negative electrode slurry may be 1:99 to 30:70, specifically, 5:95 to 30:70, or 10:90 to 20:80.
[0173] In an embodiment of the present invention, the total amount of the negative electrode active material contained in the negative electrode slurry may be 60 parts by weight to 99 parts by weight, specifically 70 parts by weight to 98 parts by weight, based on 100 parts by weight of a total solid content of the negative electrode slurry.
[0174] In one embodiment of the present invention, the binder may be included in an amount of 0.5 to 30 parts by weight, specifically 1 to 20 parts by weight, based on 100 parts by weight of the total solid content of the negative electrode slurry.
[0175] In one embodiment of the present invention, the conductive material may be included in an amount of 0.5 to 25 parts by weight, specifically 1 to 20 parts by weight, based on 100 parts by weight of the total solid content of the negative electrode slurry.
[0176] In one embodiment of the present invention, the thickener may be included in an amount of 0.5 parts by weight to 25 parts by weight, specifically 0.5 parts by weight to 20 parts by weight, and more specifically 1 part by weight to 20 parts by weight, based on 100 parts by weight of the total solid content of the negative electrode slurry.
[0177] The negative electrode slurry according to an embodiment of the present invention may further include a solvent for forming a negative electrode slurry. Specifically, the solvent for forming a negative electrode slurry may include at least one selected from the group consisting of distilled water, ethanol, methanol, and isopropyl alcohol, specifically, distilled water, in order to facilitate dispersion of the components.
[0178] In one embodiment of the present invention, the weight of the solid content of the negative electrode slurry may be 20 parts by weight to 75 parts by weight, specifically 30 parts by weight to 70 parts by weight, based on 100 parts by weight of the total of the negative electrode slurry.
[0179] <Secondary battery> A secondary battery according to an embodiment of the present invention may include the negative electrode according to the embodiment described above. Specifically, the secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the negative electrode is the same as the negative electrode described above. The negative electrode has been described above, so a detailed description thereof will be omitted.
[0180] The positive electrode may include a positive electrode current collector, and a positive electrode active material layer formed on the positive electrode current collector and including the positive electrode active material.
[0181] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and may be, for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. The positive electrode current collector may usually have a thickness of 3 to 500 μm, and fine irregularities may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.
[0182] The positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+c1 Mn 2-c1 O4 (0≦c1≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 M c2 Lithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01≦c2≦0.5); 2-c3 Mc3 Examples of the lithium manganese composite oxide include, but are not limited to, lithium manganese oxide represented by Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦c3≦0.1); or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); or LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion. The positive electrode may be metallic lithium (Li-metal).
[0183] The positive electrode active material layer may contain a positive electrode conductive material and a positive electrode binder in addition to the positive electrode active material described above.
[0184] In this case, the positive electrode conductive material is used to impart conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing chemical changes in the battery that is constructed.Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in mixture.
[0185] The positive electrode binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector.Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination.
[0186] The separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is normally used as a separator in a secondary battery can be used without any particular limitation. In particular, it is preferable that the separator has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a normal porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, in order to ensure heat resistance or mechanical strength, a coated separator containing a ceramic component or a polymeric substance may be used, and may be selectively used as a single layer or multilayer structure.
[0187] Examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries. Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0188] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0189] In particular, ethylene carbonate and propylene carbonate, which are cyclic carbonates among the carbonate-based organic solvents, can be preferably used as high-viscosity organic solvents, because they have a high dielectric constant and dissociate lithium salts well. When such cyclic carbonates are mixed in an appropriate ratio with linear carbonates having low viscosity and low dielectric constant, such as dimethyl carbonate and diethyl carbonate, an electrolyte having high electrical conductivity can be prepared, and therefore such a mixture can be used even more preferably.
[0190] The metal salt may be a lithium salt, which is a substance that is easily dissolved in the non-aqueous electrolyte. For example, the anion of the lithium salt may be F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 -, (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.
[0191] In addition to the constituent components of the electrolyte, the electrolyte may further include one or more additives such as a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery.
[0192] According to another embodiment of the present invention, there is provided a battery module including the secondary battery as a unit cell, and a battery pack including the same. The battery module and the battery pack include the secondary battery having high capacity, high rate characteristics and high cycle characteristics, and therefore can be used as a power source for medium- to large-sized devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems. EXAMPLES
[0193] <Examples and Comparative Examples> Example 1 100 g of a powder of Si and SiO2 mixed in a 1:1 molar ratio was vacuum heated in a reactor at a sublimation temperature of 1,400°C. The vaporized Si and SiO2 mixed gas was then reacted in a vacuum cooling zone with a cooling temperature of 800°C and condensed into a solid phase. Then, a heat treatment was performed in an inert atmosphere at a temperature of 800°C to produce preliminary silicon-based particles. The preliminary silicon-based particles were then milled for 3 hours using a ball mill after adding 15 sus ball media, to obtain a powder of 6 μm (D 50 Then, while maintaining an inert atmosphere by flowing Ar gas, the silicon-based particles were placed in the hot zone of a CVD apparatus, and methane was blown into the hot zone at 900° C. using Ar as a carrier gas to produce silicon-based particles having a size of 100 nm. -1 The reaction was carried out at 1000 rpm for 20 minutes at 1000 rpm for 20 minutes to form a carbon layer on the surface of the silicon-based particles.
[0194] The silicon-based particles on which the carbon layer was formed and lithium metal powder as a lithium precursor were mixed in a weight ratio of 90:10 to prepare a composition for forming a negative electrode active material. The negative electrode active material forming composition was heat-treated at 800° C. for 3 hours.
[0195] The heat-treated composition for forming a negative electrode active material was subjected to an acid treatment with an aqueous hydrochloric acid solution having a pH of 1 at 23° C. for 1 hour.
[0196] The material obtained by the acid treatment was used as the negative electrode active material of Example 1. 50 is 6μm, and the specific surface area is 3m 2 / g.
[0197] Example 2 A negative electrode active material was prepared in the same manner as in Example 1, except that the silicon-based particles on which the carbon layer was formed and lithium metal powder as a lithium precursor were mixed in a solid phase at a weight ratio of 92:8 to prepare a composition for forming a negative electrode active material.
[0198] Example 3 The silicon-based particles on which the carbon layer was formed and lithium metal powder as a lithium precursor were mixed in a weight ratio of 90:10 to prepare a composition for forming an anode active material. The anode active material was prepared in the same manner as in Example 1, except that no acid treatment was performed.
[0199] Example 4 The silicon-based particles on which the carbon layer was formed and lithium metal powder as a lithium precursor were mixed in a weight ratio of 90:10 to prepare a composition for forming an anode active material, and the composition for forming an anode active material was heat-treated at 850° C. for 3 hours, except that the anode active material was prepared in the same manner as in Example 1.
[0200] Example 5 98.5 g of the negative electrode active material obtained in Example 1 was mixed with 1.5 g of Al(PO3), and then heat-treated at 600°C to form a surface layer containing Li, Al, P, and O on the surface, which was used as the negative electrode active material of Example 5.
[0201] Example 6 The negative electrode active material obtained in Example 1 was 50 A negative electrode active material was produced in the same manner as in Example 1, except that the powder was pulverized to a size of 8 μm.
[0202] Comparative Example 1 The composition for forming a negative electrode active material was heat-treated at 500° C. for 3 hours, and a negative electrode active material was produced in the same manner as in Example 1, except that the acid treatment was not performed.
[0203] Comparative Example 2 The negative electrode active material was produced in the same manner as in Example 1, except that the composition for forming the negative electrode active material was heat-treated at 1000 °C for 3 hours and no acid treatment was performed.
[0204] Comparative Example 3 The negative electrode active material was produced in the same manner as in Example 1, except that the composition for forming the negative electrode active material was heat-treated at 1000 °C for 3 hours and acid treatment was performed for 3 hours.
[0205] Comparative Example 4 A composition for forming a negative electrode active material was produced by solid-phase mixing silicon-based oxide particles having a carbon layer formed thereon and lithium metal powder as a lithium precursor at a weight ratio of 94:6. The negative electrode active material was produced in the same manner as in Example 1, except that the composition for forming the negative electrode active material was heat-treated at 500 °C for 3 hours and no acid treatment was performed.
[0206] Comparative Example 5 A composition for forming a negative electrode active material was produced by solid-phase mixing silicon-based oxide particles having a carbon layer formed thereon and lithium metal powder as a lithium precursor at a weight ratio of 94:6. The negative electrode active material was produced in the same manner as in Example 1, except that the composition for forming the negative electrode active material was heat-treated at 1000 °C for 3 hours and acid treatment was performed for 3 hours.
[0207] Comparative Example 6 The negative electrode active material obtained in Example 1 was 50 The negative electrode active material was produced in the same manner as in Example 1, except that it was pulverized to a size of 15 μm. The negative electrode active materials produced in Examples 1 to 6 and Comparative Examples 1 to 6 were analyzed by the following method and shown in Table 1.
[0208] <Measurement of p2 / p1> In Table 1, p2 / p1 was 29 Calculated as follows by Si MAS NMR analysis. -p2 / p1: 29In the Si MAS NMR analysis, the ratio of the Li2Si2O5 peak height (p2) to the Li2SiO3 peak height (p1)
[0209] <Measurement of crystalline phase Li2Si2O5, crystalline phase Li2SiO3, crystalline phase Li4SiO4, crystalline phase SiO2, crystalline phase Si, total content of crystalline phase, total content of amorphous phase> The measurements were performed using an XRD (X-ray diffraction) instrument (product name: D4-endeavor, manufacturer: Bruker). The type and wavelength of the light source used were X-ray wavelengths generated by Cu Kα, and the wavelength (λ) of the light source was 0.15406 nm. The reference material MgO and the negative electrode active material were mixed in a weight ratio of 20:80, and then placed in a cylindrical holder with a diameter of 2.5 cm and a height of 2.5 mm. The sample was flattened with a slide glass so that the height of the sample in the holder was constant, and the sample was prepared for XRD analysis. The SCAN TIME was set to 1 hour and 15 minutes, the measurement area was set to the 2θ range of 10° to 90°, and the STEP TIME and STEP SIZE were set to scan 2θ at 0.02° per second. The measurement results were analyzed for X-ray diffraction profile by Rietveld refinement using X-ray diffraction pattern analysis software. By the above analysis, the crystalline phase Li2Si2O5, the crystalline phase Li2SiO3, the crystalline phase Li4SiO4, the crystalline phase SiO2, the crystalline phase Si, the total content of the crystalline phase, and the total content of the amorphous phase were measured.
[0210] [Table 1]
[0211] The negative electrode active materials of Examples 1 to 6 and Comparative Examples 1 to 6 do not contain the crystalline phase Li4SiO4. D of the negative electrode active material 50 was analyzed by PSD measurement method using a microtrac instrument.
[0212] The specific surface area of the negative active material was measured by degassing at 200° C. for 8 hours and performing N 2 adsorption / desorption at 77K using a BET measuring device (BEL-SORP-MAX, Nippon Bell).
[0213] Experimental example: Evaluation of discharge capacity, initial efficiency, and life (capacity retention rate) characteristics Negative electrodes and batteries were manufactured using the negative electrode active materials of the examples and comparative examples, respectively. The negative electrode active material, carbon black as a conductive material, and PAA (poly acrylic acid) as a binder were mixed in a weight ratio of 80:10:10 to prepare a mixture. Then, 7.8g of distilled water was added to 5g of the mixture and stirred to prepare a negative electrode slurry. The negative electrode slurry was applied to a copper (Cu) metal thin film as a negative electrode current collector having a thickness of 20μm and dried. At this time, the temperature of the circulating air was 60°C. Next, the mixture was rolled and dried in a vacuum oven at 130°C for 12 hours to prepare a negative electrode.
[0214] The manufactured negative electrode and 1.7671 cm 2 A lithium (Li) metal thin film cut into a circular shape was used as the positive electrode. A porous polyethylene separator was placed between the positive electrode and the negative electrode, and an electrolyte solution in which 0.5 parts by weight of vinylene carbonate was dissolved in a mixed solution of ethyl methyl carbonate (EMC) and ethylene carbonate (EC) with a volume ratio of 7:3 and LiPF6 was dissolved at a concentration of 1M was injected to manufacture a lithium coin half-cell.
[0215] The produced batteries were charged and discharged to evaluate the discharge capacity, initial efficiency, and capacity retention rate. The results are shown in Table 2 below.
[0216] The first and second cycles were charged and discharged at 0.1 C, and the third to 49th cycles were charged and discharged at 0.5 C. The 50th cycle was completed in a charged state (with lithium in the negative electrode).
[0217] Charging conditions: CC (constant current) / CV (constant voltage) (5mV / 0.005C current cut-off) Discharge condition: CC (constant current) condition 1.5V
[0218] From the results of one charge / discharge cycle, the discharge capacity (mAh / g) and initial efficiency (%) were derived. Specifically, the initial efficiency (%) was derived by the following calculation. Initial efficiency (%) = (1st discharge capacity / 1st charge capacity) x 100 The capacity retention rates were calculated as follows. Capacity retention rate (%) = (49th discharge capacity / 1st discharge capacity) × 100
[0219] [Table 2]
[0220] In Table 2, it can be seen that in Examples 1 to 6 using the negative active material according to the present invention, the content of the crystalline phase Li2SiO3 is high, and the loss of discharge capacity per weight due to the increase in the Li content in the negative active material is small. Since the total content of the crystalline phase in the negative active material is higher than the total content of the amorphous phase, the phase stability of the slurry is improved. Furthermore, the initial efficiency and life characteristics are significantly improved due to the electrochemically stable lithium silicate structure of Li2SiO3.
[0221] In the case of Example 5, a surface layer containing Li, Al, P, and O is provided on the surface of the negative electrode active material, which prevents the Li compound contained in the silicon-based particles from reacting with the moisture in the slurry to reduce the viscosity of the slurry, thereby further improving the initial efficiency and life characteristics.
[0222] In contrast, in Comparative Examples 1 to 6, the crystalline phase Li2SiO3 is contained in an amount of less than 60 parts by weight based on a total of 100 parts by weight of the crystalline phase silicate, or the total content of the crystalline phase is low, so that the capacity loss per weight is large, or the structure of Li2Si2O5 is unstable, and it can be confirmed that the initial efficiency and / or life characteristics are low. In particular, in the case of Comparative Examples 4 and 5, the Li content is low, so the discharge capacity is large, but the efficiency is reduced by 10% or more, and the life is shortened by about 50% or more.
Claims
1. SiO x (0<x<2) and a negative electrode active material comprising silicon-based particles containing a Li compound, The Li compound has a crystalline phase of Li 2 SiO 3 , crystal phase Li 4 SiO 4 , and the crystalline phase Li 2 S 2 O 5 At least one crystalline phase lithium silicate selected from the group consisting of: The crystalline phase Li 2 SiO 3 The content of the crystalline phase Li 2 S 2 O 5 and the crystalline phase Li 4 SiO 4 More than the sum of the contents of The crystalline phase Li 2 SiO 3 is contained in an amount of 60 parts by weight or more based on a total of 100 parts by weight of the crystalline lithium silicate; A negative electrode active material, wherein a total content of crystalline phases present in the silicon-based particles is greater than a total content of amorphous phases.
2. The negative electrode active material of claim 1 , wherein the Li element is contained in an amount of more than 7 parts by weight and not more than 10 parts by weight based on a total of 100 parts by weight of the negative electrode active material.
3. The Li compound has a crystalline phase of Li 2 SiO 3 and crystalline phase Li 2 S 2 O 5 The negative electrode active material of claim 1 .
4. 2 . The negative active material of claim 1 , wherein a total content of the crystalline phase present in the silicon-based particles is more than 50 parts by weight and not more than 85 parts by weight based on a total of 100 parts by weight of the silicon-based particles.
5. The crystalline phase Li 2 SiO 3 The negative electrode active material according to claim 1 , wherein the amount of is 15 parts by weight or more and 50 parts by weight or less based on a total of 100 parts by weight of the silicon-based particles.
6. The crystalline phase Li 2 SiO 3 Content and crystalline phase of Li 2 S 2 O 5 2. The negative electrode active material according to claim 1, wherein the difference between the content of the silicon-based particles and the content of the silicon-based particles is 1 to 50 parts by weight based on a total of 100 parts by weight of the silicon-based particles.
7. The crystalline phase Li 4 SiO 4 The negative electrode active material according to claim 1 , which does not contain
8. 29 During Si-MAS-NMR analysis, Li appears in the chemical shift peak at -70 ppm to -80 ppm. 2 SiO 3 The height of peak p1 is the height of Li that appears in the chemical shift peak of -90 ppm to -100 ppm. 2 S 2 O 5 The negative electrode active material according to claim 1 , wherein the height (Height) of peak p2 is greater than the height (Height) of peak p1 of
9. 29 During Si-MAS-NMR analysis, Li appears in the chemical shift peak at -70 ppm to -80 ppm. 2 SiO 3 Li appearing in the chemical shift peak of -90 ppm to -100 ppm relative to the height of peak p1 2 S 2 O 5 2. The negative electrode active material according to claim 1, wherein a ratio p2 / p1 of the heights of the peaks p2 and p1 is 1 or less.
10. 29 During Si-MAS-NMR analysis, Li appears in the chemical shift peak at -60 ppm to -69 ppm. 4 SiO 4 The negative electrode active material according to claim 1 , wherein peak p3 of
11. Crystal phase SiO 2 The negative electrode active material according to claim 1 , wherein the amount of is less than 5 parts by weight based on a total of 100 parts by weight of the silicon-based particles.
12. The negative electrode active material of claim 1 , further comprising a carbon layer disposed on the silicon-based particles.
13. The negative electrode active material of claim 1 , further comprising a surface layer comprising Al, P, and O provided on the silicon-based particles.
14. SiO x forming particles including a silicon-based oxide represented by (0<x<2); and mixing the silicon-based oxide-containing particles with a lithium precursor and then heat-treating the resulting mixture; The method for producing the negative electrode active material according to any one of claims 1 to 13, comprising:
15. The method of claim 14, further comprising the step of performing an acid treatment after the heat treatment.
16. The method of claim 14, further comprising providing a surface layer on at least a portion of the silicon-based particles formed after the heat treatment.
17. The method for producing a negative electrode active material according to claim 14, wherein the heat treatment is performed at 650°C to 950°C.
18. The method for producing a negative electrode active material according to claim 14, wherein the heat treatment is performed for 1 hour to 12 hours.
19. A negative electrode current collector, and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector; Including, The negative electrode active material layer comprises a negative electrode material containing the negative electrode active material according to any one of claims 1 to 13.
20. The negative electrode according to claim 19 . a positive electrode facing the negative electrode; A separator interposed between the negative electrode and the positive electrode, and electrolyte A secondary battery comprising:
Citation Information
Patent Citations
Negative electrode active substance, mixed negative electrode active substance material, negative electrode for nonaqueous electrolyte secondary battery, lithium ion secondary battery, manufacturing method of negative electrode active material, and manufacturing method of lithium ion secondary battery
JP2017097952A
Negative electrode active material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and method for manufacturing negative electrode material for nonaqueous electrolyte secondary battery
JP2017152358A
Negative electrode active material for non-aqueous electrolyte secondary cell, negative electrode for non-aqueous electrolyte secondary cell, and non-aqueous electrolyte secondary cell
WO2016136180A1
Negative electrode active material, mixed negative electrode active material, and method for producing negative electrode active material
WO2017208625A1
Negative electrode active material, mixed negative electrode active material, and method for producing negative electrode active material
WO2017208627A1