Jelly-roll type electrode assembly, method for manufacturing the same, and secondary battery including the same

The jelly-roll electrode assembly with a swelling tape addresses deformation and short circuit issues by expanding to protect electrodes, improving battery stability and lifespan.

JP2024541925AActive Publication Date: 2024-11-13LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024524730
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-25
Filing Date
2023-09-26
Publication Date
2024-11-13
Estimated Expiration
2043-09-26

AI Technical Summary

Technical Problem

Cylindrical batteries with jelly-roll electrode assemblies face issues of deformation and internal short circuits due to the contraction and expansion of electrodes, particularly when using multiple tabs or silicon-based active materials, leading to potential heat generation and ignition.

Method used

A jelly-roll electrode assembly design that includes a swelling tape attached to the ends of the electrodes, which expands with electrolyte impregnation to prevent deformation and separator damage, thereby preventing internal short circuits.

Benefits of technology

The swelling tape effectively protects the electrodes and separator from deformation, enhancing battery stability and lifespan by preventing internal short circuits during charging and discharging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024541925000001_ABST
    Figure 2024541925000001_ABST
Patent Text Reader

Abstract

The present invention relates to a jelly-roll type electrode assembly, a method for manufacturing the jelly-roll type electrode assembly, and a secondary battery including the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a jelly roll type electrode assembly, a method for manufacturing the jelly roll type electrode assembly, and a secondary battery including the same, and more particularly to a jelly roll type electrode assembly including a swelling tape, a method for manufacturing the jelly roll type electrode assembly, and a cylindrical secondary battery including the same. This application claims the benefit of the filing date of Korean Patent Application No. 10-2022-0121663 filed in the Korean Intellectual Property Office on September 26, 2022, and all contents disclosed in the documents of the Korean patent application are incorporated herein by reference. [Background technology]

[0002] In the case of cylindrical batteries, a jelly roll-shaped electrode assembly is manufactured by winding a long and narrow electrode with a fixed width into a roll. A cylindrical battery manufactured by inserting such a jelly roll-shaped electrode assembly into a battery case undergoes repeated electrode contraction / expansion during charging and discharging. In particular, if an in-tab is located in the core of the jelly roll-shaped electrode assembly or a silicon-based active material is added to the negative electrode, which increases the degree of contraction / expansion of the electrode assembly, the pressure acting on the core of the electrode assembly increases significantly.

[0003] In recent years, as low resistance / high capacity designs have become more common, jelly roll type electrode assemblies have come to include multiple tabs or have silicon-based active materials added thereto. This increases the possibility of deformation of the electrode assembly located in the core portion due to contraction / expansion of the electrode assembly. In particular, if a separator located between the negative and positive electrodes is damaged, the negative and positive electrodes may come into direct contact with each other, resulting in an internal short circuit, which may cause heat generation and fire.

[0004] In order to solve the problem of separator damage and internal short circuit caused by deformation of the electrode assembly, there is a need to develop technology that can protect the positive electrode and separator in the corresponding area and suppress the occurrence of internal short circuit. Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention aims to provide a jelly-roll type electrode assembly having a modified design of a jelly-roll type electrode assembly, a method for manufacturing the jelly-roll type electrode assembly, and a secondary battery including the same.

[0006] However, the problems to be solved by the present invention are not limited to those mentioned above, and other problems not mentioned will be clearly understood by those skilled in the art from the following description. [Means for solving the problem]

[0007] One embodiment of the present invention provides a jelly roll type electrode assembly in which a first electrode; a first separator; a second electrode; and a second separator are sequentially stacked and wound up, the assembly further comprising a swelling tape attached to at least one side of the first electrode, the first electrode including a first end along its length where winding begins and a second end where winding ends, the swelling tape being attached such that one end of the swelling tape coincides with the first end of the first electrode.

[0008] Another embodiment of the present invention provides a method for manufacturing a jelly roll type electrode assembly in which a first electrode, a first separator, a second electrode, and a second separator are sequentially stacked and wound, the method including the steps of: (a) transporting the first electrode in a roll-to-roll manner; (b) attaching a swelling tape to at least one side of a slitting region included in the first electrode; and (c) slitting a center portion of the slitting region of the first electrode in a longitudinal direction, the step (b) attaching the swelling tape such that a center portion of the swelling tape coincides with a center portion of the slitting region of the first electrode in a longitudinal direction, and the step (c) slitting the center portion of the slitting region in a longitudinal direction to provide a first end portion where winding of the first electrode begins along a longitudinal direction and a second end portion where winding ends, and a jelly roll type electrode assembly manufactured by the method.

[0009] Yet another embodiment of the present invention provides a secondary battery comprising the jelly-roll type electrode assembly; and a battery case for housing the electrode assembly. Effect of the Invention

[0010] A jelly-roll type electrode assembly according to an embodiment of the present invention includes a swelling tape that expands when immersed in an electrolyte and is attached to surround one longitudinal end of a positive electrode. This prevents damage to the positive electrode and separator due to deformation of the electrode assembly caused by contraction / expansion of the electrodes during charging / discharging of the battery. Even if the separator is damaged, the swelling tape prevents internal short circuits between the positive electrode and negative electrode, thereby improving the stability and life characteristics of the battery.

[0011] In a method for manufacturing a jelly-roll type electrode assembly according to an embodiment of the present invention, the jelly-roll type electrode assembly including the swelling tape that expands when immersed in an electrolyte and is attached to surround one longitudinal end of the positive electrode can be produced in a continuous process using conventional roll-to-roll process equipment, thereby ensuring productivity and economy.

[0012] In addition, the secondary battery according to the present invention can prevent an internal short circuit between the positive and negative electrodes even when the electrode assembly is deformed due to the contraction / expansion of the electrodes during charging / discharging of the battery, thereby improving the stability and life characteristics of the battery.

[0013] The effects of the present invention are not limited to those described above, and effects not mentioned herein will be apparent to those skilled in the art from the present specification and the accompanying drawings. [Brief description of the drawings]

[0014] [Figure 1] 1 illustrates a jelly roll type electrode assembly including a swelling tape according to one embodiment of the present invention. [Diagram 2] 1A and 1B are schematic diagrams illustrating a method for manufacturing a jelly roll type electrode assembly including a swelling tape and a method for manufacturing a jelly roll type electrode assembly including a PET tape according to an embodiment of the present invention. [Diagram 3] 1 is an image illustrating an embodiment of a method for manufacturing a jelly-roll type electrode assembly according to an embodiment of the present invention. [Figure 4] 1 illustrates a swelling test result of a swelling tape included in a jelly roll type electrode assembly according to an embodiment of the present invention. [Diagram 5] 4 is an image showing a first end of a first electrode of a jelly-roll type electrode assembly according to Example 1 before and after activation. [Figure 6] 1 is an image showing a first end of a first electrode of a jelly-roll type electrode assembly according to Comparative Example 1 before and after activation. [Figure 7]1 shows the results of evaluating the change in Coulombic efficiency with the progress of cycles and room temperature-voltage tracking over time for the secondary batteries manufactured in Example 1 and Comparative Example 2. [Figure 8] 4 is an image showing a state of a first electrode facing portion of a separator included in secondary batteries produced in Example 1 and Comparative Example 2. [Figure 9] 1 is an image showing an evaluation result of the circularity of secondary batteries manufactured in Example 1 and Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Throughout this specification, when a part is said to "comprise" a certain element, this means that it may further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.

[0016] Throughout this specification, when a member is said to be "on" another member, this includes not only when the member is in contact with the other member, but also when there is another member between the two members.

[0017] One embodiment of the present invention provides a jelly roll type electrode assembly in which a first electrode; a first separator; a second electrode; and a second separator are sequentially stacked and wound up, the assembly further comprising a swelling tape attached to at least one side of the first electrode, the first electrode including a first end along its length where winding begins and a second end where winding ends, the swelling tape being attached such that one end of the swelling tape coincides with the first end of the first electrode.

[0018] A jelly-roll type electrode assembly according to an embodiment of the present invention includes a swelling tape that expands when immersed in an electrolyte and is attached to surround one longitudinal end of a positive electrode. This prevents damage to the positive electrode and separator due to deformation of the electrode assembly caused by contraction / expansion of the electrodes during charging / discharging of the battery. Even if the separator is damaged, the swelling tape prevents internal short circuits between the positive electrode and negative electrode, thereby improving the stability and life characteristics of the battery.

[0019] According to one embodiment of the present invention, the jelly roll type electrode assembly may include a swelling tape attached to at least one surface of the first electrode. Specifically, the swelling tape may be attached to one surface of the first electrode facing the winding shaft, or the surface opposite to the one surface facing the winding shaft, or may be attached to both surfaces of the first electrode.

[0020] As described below, the swelling tape may expand and increase in length when immersed in an electrolyte. When the swelling tape is attached to one side of a first electrode, the swelling tape after expansion surrounds one end of the first electrode in the longitudinal direction, thereby preventing direct contact between the opposing first and second electrodes through the separator even if the separator is damaged.

[0021] Therefore, when the swelling tape is attached to one side of the first electrode facing the winding shaft, it can more efficiently prevent internal short circuit between the positive and negative electrodes when the separator is damaged. Also, when the swelling tape is attached to both sides of the first electrode, the ends of the swelling tape after expansion surround the ends of the first electrode and contact each other, so that the effect of protecting the longitudinal ends of the first electrode can be more excellent. Also, when the swelling tape after expansion surrounds the longitudinal ends of the first electrode, the properties of the porous material of the swelling tape can provide excellent effects of relieving internal stress and improving the roundness of the core portion.

[0022] According to one embodiment of the present invention, the first electrode may include a first end where winding starts along the length direction, and a second end where winding ends. In other words, the first electrode may be wound starting from the first end and being wound toward the second end. That is, the first end may refer to one end in the length direction located at a core portion of the jelly roll type electrode assembly after winding, and the second end may refer to one end in the length direction located at an outer portion of the jelly roll type electrode assembly after winding.

[0023] According to one embodiment of the present invention, the swelling tape may be attached such that one end coincides with one end in the length direction of the first electrode. Specifically, the swelling tape may be attached such that one end coincides with a first end of the first electrode. In other words, the swelling tape may be attached such that one end coincides with one end in the length direction located at a core portion of the first electrode.

[0024] As a result, the swelling tape can prevent deformation of the electrode assembly due to contraction / expansion of the electrodes during charging / discharging of the battery, particularly damage to the separator due to sliding of the first end of the core first electrode. Specifically, one end of the swelling tape after expansion surrounds the end of the first electrode, or the ends of the swelling tape attached to both sides of the first end of the first electrode surround the end of the first electrode and are in contact with each other, so that even if the separator is damaged, the swelling tape can efficiently prevent internal shorts between the positive and negative electrodes.

[0025] According to an embodiment of the present invention, the width direction length of the swelling tape may be 60% to 100% based on the 100% width of the first electrode. Specifically, the width direction length of the swelling tape may be 70% to 100%, 80% to 100%, 60% to 90%, 60% to 80%, 60% to 70%, or 70% to 90% based on the 100% width of the first electrode. When the width direction length of the swelling tape satisfies the above-mentioned range, the length of the swelling tape after expansion can correspond to the width direction length of the first electrode, and one end of the swelling tape effectively surrounds one end of the first electrode in the length direction, so that even if the separator is damaged, the role of preventing internal short circuit between the positive and negative electrodes can be more efficiently performed.

[0026] If the width of the swelling tape is less than the above range, the effect of protecting the first end of the first electrode is poor, and one end of the first electrode is exposed, causing damage to the separator, and when the separator is damaged, an internal short circuit may occur due to direct contact between the first electrode and the second electrode. Meanwhile, if the width of the swelling tape is more than the above range, the manufacturing cost increases due to the use of excessive material, one end of the swelling tape after expansion is excessively exposed in the width direction of the jelly-roll type electrode assembly, causing defects during the insertion process into the battery case, and local problems such as lithium precipitation due to the formation of steps in the swelling tape overlapping area may occur. Meanwhile, the preferred width of the swelling tape may be adjusted according to the physical properties of the swelling tape, particularly the length change rate before / after expansion.

[0027] According to one embodiment of the present invention, the length of the swelling tape in the longitudinal direction may be 250% or more and 3500% or less based on the 100% thickness of the first electrode. Specifically, the length of the swelling tape in the longitudinal direction may be 300% or more, 350% or more, 400% or more, 450% or more, or 500% or more based on the 100% thickness of the first electrode, and the length of the swelling tape in the longitudinal direction may be 3000% or less, 2500% or less, 2000% or less, or 1500% or less based on the 100% thickness of the first electrode, and preferably 1000% or less, 850% or less, or 700% or less.

[0028] When the length of the swelling tape in the longitudinal direction satisfies the above-mentioned range, the length of the swelling tape in the longitudinal direction after expansion can correspond to the thickness of the first electrode, and one end of the swelling tape effectively surrounds one end of the first electrode in the longitudinal direction, so that even if the separator is damaged, the swelling tape can more efficiently perform its role of preventing internal short circuits between the positive and negative electrodes.

[0029] Specifically, the swelling tape may expand by 40% or more on both sides in the width direction and the length direction, and may expand by 20% or more on one side. That is, when the length of the swelling tape attached on both sides of the first electrode in the length direction is 250% or more based on the thickness of the first electrode at 100%, the total length of the expanded swelling tape in the length direction can correspond to the thickness of the first electrode, and one ends of the swelling tapes attached on both sides of the first electrode can be in contact with each other to effectively surround one end of the first electrode in the length direction.

[0030] In addition, when the length of the swelling tape in the longitudinal direction is 500% or more based on 100% of the thickness of the first electrode, even if the swelling tape is attached only to one side of the first electrode facing the winding shaft, the length of the expanded swelling tape in the longitudinal direction can correspond to the thickness of the first electrode, and the swelling tape can efficiently perform the role of preventing internal short circuits between the positive and negative electrodes when the separator is damaged.

[0031] In contrast, if the length of the swelling tape in the longitudinal direction is less than 250% based on 100% of the thickness of the first electrode, the swelling tape after expansion cannot completely surround one end of the first electrode and a portion of the electrode is exposed, which may result in a poor effect of preventing damage to the separator and an internal short circuit between the positive and negative electrodes when the separator is damaged.

[0032] Meanwhile, when the length in the longitudinal direction of the swelling tape attached on both sides of the first electrode is 1000% or less based on 100% of the thickness of the first electrode, defects due to the swelling tape overlapping area that may occur due to one end of the swelling tape being excessively exposed in the longitudinal direction of the first electrode can be minimized.

[0033] In addition, when the length in the longitudinal direction of the swelling tape is 700% or less based on 100% of the thickness of the first electrode, the inactivated area that may be formed in the swelling tape attachment area can be adjusted to an appropriate level to minimize the influence on electrochemical properties such as the capacity reduction rate of the battery including the swelling tape, and to achieve the above-mentioned effect of preventing damage to the separator and internal short circuit.

[0034] According to an embodiment of the present invention, the first end of the first electrode may be formed at the same position of the current collector of the first electrode and the active material layer of the first electrode. In other words, the first end of the first electrode may be in the form of a free edge. This can reduce the area of ​​the unnecessary uncoated portion of the first electrode collector to ensure economy, and since the slitting process can be performed after the active material layer is formed on the electrode, the roll-to-roll process including the slitting process and the winding process can be performed more efficiently. Here, "the same position" means that the end in the length direction is the same, and may include the case where the end is formed at substantially the same position due to a process error that may occur in the slitting process, etc.

[0035] According to an embodiment of the present invention, the swelling tape may expand or become flexible due to an electrolyte. Specifically, the swelling tape may include a portion made of a polymer material, as described below, and when the swelling tape is immersed in an electrolyte, the portion made of the polymer material may absorb the electrolyte and expand or become flexible. More specifically, the polymer material may have a characteristic that solvent molecules penetrate between the chains of the polymer material to increase in volume. Thus, the swelling tape may expand or become flexible when absorbing an electrolyte.

[0036] According to one embodiment of the present invention, the swelling tape may expand due to an electrolyte solution, and the swelling tape after expansion may surround the first end of the first electrode. Specifically, the swelling tape may expand by absorbing an electrolyte solution containing an organic solvent, as described below, and the length in the longitudinal direction may increase, and one end of the swelling tape after expansion may extend and be folded to surround the first end of the first electrode. In other words, the swelling tape after expansion may increase in length and be folded to cover at least one edge of the first end of the first electrode.

[0037] This prevents the sharp free edges of the positive electrode from coming into direct contact with the separator or negative electrode, thereby preventing damage to the positive electrode and separator due to deformation of the electrode assembly caused by contraction / expansion of the electrodes during charging / discharging of the battery. Even if damage to the separator does occur, the swelling tape prevents internal short circuits between the positive and negative electrodes, thereby improving the stability and life characteristics of the battery.

[0038] FIG. 1 illustrates a jelly roll type electrode assembly including a swelling tape according to one embodiment of the present invention.

[0039] Specifically, FIG. 1(a) shows a first electrode including swelling tape attached to both sides of the first electrode before the first electrode is immersed in an electrolyte, FIG. 1(b) shows a first electrode including swelling tape attached to both sides of the first electrode after the first electrode is immersed in an electrolyte, and FIG. 1(c) shows a first electrode including swelling tape attached to one side of the first electrode after the first electrode is immersed in an electrolyte.

[0040] Referring to Fig. 1(a), the swelling tape may be attached to both sides of the first electrode such that one end of the swelling tape coincides with the first end of the first electrode, and referring to Fig. 1(b), the swelling tape may expand due to the electrolyte when immersed in the electrolyte, and the swelling tape after expansion may surround the first end of the first electrode. Meanwhile, referring to Fig. 1(c), the swelling tape may be attached to one side of the first electrode such that one end of the swelling tape coincides with the first end of the first electrode, and the swelling tape may expand due to the electrolyte when immersed in the electrolyte, and the swelling tape after expansion may surround the first end of the first electrode.

[0041] According to one embodiment of the present invention, the length of the swelling tape after immersion for 60 minutes in an electrolytic solution containing 45% by weight of dimethyl carbonate, 20% by weight of ethylene carbonate, 15% by weight of ethyl methyl carbonate, and 15% by weight of LiPF6 as an electrolyte may be 120% to 160% based on the length of the swelling tape before expansion (100%). Specifically, the length of the swelling tape after expansion may be 120% to 150%, 120% to 140%, 120% to 130%, 130% to 160%, 140% to 160%, 150% to 160%, or 130% to 150% based on the length of the swelling tape before expansion (100%).

[0042] Here, the length of the swelling tape after expansion may include both the length direction and the width direction. That is, the ratio of the length of the swelling tape after expansion to the length of the swelling tape before expansion may be the same in the length direction and the width direction. Also, the length of the swelling tape may mean the length measured from one end to the other end in a specific direction of the swelling tape. For example, when the length of the swelling tape after expansion is measured from one end to the other end in the length direction, it may be 120% or more and 160% or less, and when the length of the swelling tape after expansion is measured based on the center of the length direction of the swelling tape before expansion, it may be 110% or more and 130% or less.

[0043] When the length of the swelling tape after expansion satisfies the above-mentioned range, even if the swelling tape is attached to at least one surface of the first electrode so that one end of the swelling tape coincides with the first end of the first electrode, the swelling tape can expand to a length suitable for effectively surrounding the first end of the first electrode by being subsequently immersed in an electrolyte, thereby providing an excellent effect of protecting the first end of the first electrode, and further providing an excellent effect of preventing internal short circuits and improving the stability of the battery.

[0044] According to one embodiment of the present invention, the swelling tape may include a portion made of a polymer material that expands or becomes flexible by absorbing an electrolyte, and an adhesive portion that attaches the swelling tape to the first electrode.

[0045] According to one embodiment of the present invention, the swelling tape may include a base layer and an adhesive layer, and the adhesive layer may be provided on at least one side of the base layer. Specifically, the swelling tape may include a multi-layer structure including a base layer that absorbs the electrolyte solution and expands when impregnated with the electrolyte solution, and an adhesive layer that attaches the swelling tape to the first electrode, and the adhesive layer may be provided on one or both sides of the base layer.

[0046] According to an embodiment of the present invention, the adhesive layer may include a pressure sensitive adhesive including a polyacrylic resin, that is, the adhesive strength of the adhesive layer may be influenced by the magnitude of pressure acting on the surface of the swelling tape.

[0047] According to an embodiment of the present invention, the adhesive layer may include one or more comonomers selected from the group consisting of PMMA (poly methyl methacrylate), PEMA (poly ethyl methacrylate), and PBMA (poly butyl methacrylate). Specifically, the adhesive layer may include a polyacrylic resin prepared by copolymerizing a monomer such as EA (ethyl acrylate), BA (butyl acrylate), or 2-EHA (2-ethylhexyl acrylate) with a comonomer selected from the group consisting of PMMA (poly methyl methacrylate), PEMA (poly ethyl methacrylate), and PBMA (poly butyl methacrylate). When the adhesive layer includes the above-mentioned material, it is possible to minimize the influence on the electrochemical properties of a battery including the swelling tape and to maintain the adhesive strength of the swelling tape at an appropriate level.

[0048] According to one embodiment of the present invention, the base layer may include a urethane-based resin. For example, the base layer may include a polyurethane resin. When the base layer includes the above-mentioned material, the swelling tape can absorb the electrolyte more easily, and when the swelling tape is immersed in the electrolyte, the swelling tape can expand to a length suitable for effectively surrounding the first end of the first electrode.

[0049] According to one embodiment of the present invention, the electrolytic solution may include an organic solvent. Specifically, the organic solvent may include 70% by weight or more of any one of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and mixtures thereof. Specifically, the electrolytic solution may include a mixed organic solvent including 45% by weight or more of dimethyl carbonate. For example, the electrolytic solution may include a mixed organic solvent including 45% by weight of dimethyl carbonate, 20% by weight of ethylene carbonate, and 15% by weight of ethyl methyl carbonate.

[0050] Specifically, when the base layer includes a urethane-based resin, the base layer can absorb the electrolyte and expand, and when the electrolyte includes the above-mentioned type of organic solvent, the base layer including the urethane-based resin can expand more easily. That is, the swelling tape including the base layer can expand more easily, and the expanded swelling tape can effectively surround the first end of the first electrode, preventing damage to the separator.

[0051] According to an embodiment of the present invention, the electrolytic solution may further include an electrolyte, which may be, but is not limited to, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten inorganic electrolyte that can be used in the manufacture of a lithium secondary battery.

[0052] Specifically, the electrolyte may include a metal salt such as LiPF6 as an electrolyte, and for example, an electrolyte including 45% by weight of dimethyl carbonate, 20% by weight of ethylene carbonate, 15% by weight of ethyl methyl carbonate, and 15% by weight of LiPF6 as an electrolyte may be used. When the electrolyte further includes the above-mentioned types of electrolytes, the swelling characteristics of the swelling tape may be more excellent than when the electrolyte is not included, and the expanded swelling tape may effectively surround the first end of the first electrode, thereby preventing damage to the separator.

[0053] According to one embodiment of the present invention, the first electrode may be a positive electrode and the second electrode may be a negative electrode. That is, the jelly roll type electrode assembly according to one embodiment of the present invention may be a jelly roll type electrode assembly in which a positive electrode, a first separator, a negative electrode, and a second separator are sequentially stacked and wound, and may include a swelling tape attached to at least one surface of the positive electrode, the positive electrode including a first end where winding starts along the length direction and a second end where winding ends, and the swelling tape may be attached so that one end coincides with the first end of the positive electrode.

[0054] According to one embodiment of the present invention, the first electrode may include a current collector and an active material layer provided on the current collector. That is, the positive electrode may include a positive electrode current collector and a positive electrode active material layer provided on the positive electrode current collector. Specifically, the positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on one or both sides of the positive electrode current collector and containing a positive electrode active material. In other words, the positive electrode active material layer is formed on the positive electrode active material coating portion of the positive electrode current collector, and the surface on which the positive electrode active material layer is not provided can be referred to as a positive electrode non-coating portion.

[0055] According to an embodiment of the present invention, the positive electrode current collector may include a positive electrode active material-coated portion on which a positive electrode active material is coated, and a positive electrode uncoated portion on which a positive electrode active material is not coated, and may include a tab on the positive electrode uncoated portion. Specifically, the positive electrode current collector may include a positive electrode uncoated portion, and may include a positive electrode tab formed on the positive electrode uncoated portion.

[0056] According to one embodiment of the present invention, the positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and specifically, the positive electrode current collector may be stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, etc. That is, the positive electrode current collector may be provided in the form of surface-treated stainless steel, aluminum foil, etc.

[0057] The positive electrode current collector may have a thickness of, but is not limited to, 3 to 50 μm, and may have fine irregularities on the surface of the current collector to enhance the adhesive strength of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0058] According to one embodiment of the present invention, the positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+x Mn 2-x O4 (0≦x≦0.33), lithium manganese oxides such as LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-y M yLithium nickel oxide with Ni site represented by the chemical formula LiMnO2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and 0.01≦y≦0.3 is satisfied); 2-z M z Examples of the lithium manganese composite oxide include, but are not limited to, lithium manganese composite oxide represented by Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≦z≦0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); and LiMn2O4 in which part of the Li in the chemical formula is replaced with an alkaline earth metal ion. The positive electrode may be Li-metal.

[0059] According to one embodiment of the present invention, the positive electrode active material layer may further include a positive electrode conductive material and a positive electrode binder. The positive electrode conductive material is used to impart electrical conductivity to the electrode, and can be used without any particular limitation as long as it has electronic conductivity without causing a chemical change in the battery that is constructed. Specifically, the positive electrode conductive material may be graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one or more of these may be used alone or in mixture.

[0060] The positive electrode binder plays a role of improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector.Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene-butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination.

[0061] According to one embodiment of the present invention, the second electrode may include a current collector and an active material layer provided on the current collector. That is, the negative electrode may include a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector. Specifically, the negative electrode may include a negative electrode current collector and a negative electrode active material layer formed on one or both sides of the negative electrode current collector and including a negative electrode active material. In other words, the negative electrode active material layer is formed on a negative electrode active material coated portion of the negative electrode current collector, and the surface on which the negative electrode active material layer is not provided may be referred to as a negative electrode non-coating portion.

[0062] According to one embodiment of the present invention, the negative electrode current collector may include a negative electrode active material coated portion where a negative electrode active material layer is formed, and a negative electrode uncoated portion where a negative electrode active material layer is not formed, and may include a tab on the negative electrode uncoated portion. Specifically, the negative electrode current collector may include a negative electrode uncoated portion, and may include a negative electrode tab formed on the negative electrode uncoated portion. Thus, the manufactured electrode assembly may include one or more negative electrode tabs.

[0063] According to an embodiment of the present invention, the negative electrode active material layer may include a negative electrode active material including at least one selected from the group consisting of a silicon-based material and a carbon-based material. The negative electrode active material layer may further include a negative electrode conductive material and a negative electrode binder, and the negative electrode active material, the negative electrode conductive material, and the negative electrode binder may be any material used in the art without limitation.

[0064] According to one embodiment of the present invention, the negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has electrical conductivity. For example, the negative electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel whose surface is treated with carbon, nickel, titanium, silver, or the like. Specifically, a transition metal that easily adsorbs carbon, such as copper or nickel, may be used as the negative electrode current collector. The thickness of the negative electrode current collector may be 6 μm or more and 80 μm or less, but is not limited thereto.

[0065] According to one embodiment of the present invention, the negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, polyacrylic acid, and substances in which hydrogen is substituted with Li, Na, Ca, or the like, or may include various copolymers thereof.

[0066] According to one embodiment of the present invention, the negative electrode conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples thereof include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0067] One embodiment of the present invention provides a method for manufacturing a jelly roll type electrode assembly in which a first electrode, a first separator, a second electrode, and a second separator are sequentially stacked and wound, the method including the steps of: (a) transporting the first electrode in a roll-to-roll manner; (b) attaching a swelling tape to at least one side of a slitting region included in the first electrode; and (c) slitting a center portion of the slitting region of the first electrode in a longitudinal direction, wherein the step (b) is for attaching the swelling tape so that the center portion of the swelling tape coincides with the center portion of the slitting region of the first electrode in a longitudinal direction, and the step (c) is for slitting the center portion of the slitting region of the first electrode in a longitudinal direction to provide a first end portion where winding of the first electrode begins and a second end portion where winding ends.

[0068] According to an embodiment of the present invention, the method for manufacturing a jelly-roll type electrode assembly includes a swelling tape that expands when immersed in an electrolyte and is attached to surround one end of the positive electrode in the longitudinal direction, and the jelly-roll type electrode assembly can be produced in a continuous process using conventional roll-to-roll process equipment, thereby ensuring productivity and economic efficiency. In addition, the jelly-roll type electrode assembly manufactured by the manufacturing method includes a swelling tape that expands when immersed in an electrolyte and is attached to surround one end of the positive electrode in the longitudinal direction, thereby preventing damage to the positive electrode and separator due to deformation of the electrode assembly caused by contraction / expansion of the electrodes during charging / discharging of the battery, and even if the separator is damaged, the swelling tape prevents internal short circuit between the positive electrode and the negative electrode, thereby improving the stability and life characteristics of the battery.

[0069] According to an embodiment of the present invention, the method for manufacturing the jelly roll type electrode assembly may include (a) transferring the first electrode in a roll-to-roll manner. Specifically, the step (a) may be performed in a roll-to-roll processing manner in which a plurality of bendable metal foils are processed while being moved between rollers. Here, the roll-to-roll processing may refer to a method in which a roll on which a flexible and thin metal sheet-like electrode collector is wound is unwound to supply the electrode collector, an electrode slurry including an electrode active material is applied to at least one side of the electrode collector and dried to form an electrode mixture layer, and then the electrode collector processed by another roll is rewound and collected. That is, the step (a) may be a step of transferring the first electrode for processing in the roll-to-roll manner, and may be referred to as a first electrode transferring step (S11).

[0070] According to an embodiment of the present invention, the method for manufacturing the jelly roll type electrode assembly may include (b) attaching a swelling tape on at least one side of a slitting region included in the first electrode. Here, the slit region means a region for cutting the first electrode by a slitting process for cutting the first electrode or an electrode assembly including the first electrode into a set length, and the slit region may mean a part of a longitudinal region including a first electrode collector and a first electrode active material layer included in the first electrode, and the length of the slit region may be adjusted according to process conditions. In addition, the length and position of the slit region may be changed according to the length and position of the swelling tape attached to the slit region. That is, the slit region can be set by changing the length and position of the swelling tape attached to one or both sides of the first electrode according to process conditions.

[0071] According to one embodiment of the present invention, in the step (b), the swelling tape may be attached so that the center of the swelling tape in the length direction coincides with the center of the slit region of the first electrode in the length direction. Specifically, in the step (b), the swelling tape may be attached to at least one side of the slit region included in the first electrode so that the center of the swelling tape in the length direction coincides with the center of the slit region of the first electrode in the length direction. Thus, in the subsequent step of slitting the center of the slit region in the length direction, the first electrode can provide a first end where winding starts along the length direction and a second end where winding ends, and the first electrode can be provided in a state where a predetermined length of swelling tape is attached to at least one side of the first end and the second end after the slitting step.

[0072] According to one embodiment of the present invention, the step (b) may be a step of attaching a swelling tape to at least one side of the slit region included in the first electrode, specifically, the step (b) may be a step of attaching a swelling tape to one or both sides of the slit region included in the first electrode, and can be referred to as a swelling tape attachment step (S12).

[0073] According to an embodiment of the present invention, the method for manufacturing the jelly-roll type electrode assembly may include (c) slitting the center of the slit region of the first electrode in the longitudinal direction. Specifically, the (c) step may be a step of cutting the first electrode or an electrode assembly including the first electrode to a set length, and the cutting may be performed using a cutting knife or the like, but is not limited thereto.

[0074] According to one embodiment of the present invention, the step (c) may include slitting the center of the slit region in the length direction to provide a first end where winding of the first electrode begins along the length direction and a second end where winding ends. Specifically, the step (c) may include slitting the center of the slit region in the length direction to provide a first end where winding of the first electrode or a first electrode included in the electrode assembly begins along the length direction and a second end where winding ends. The step (c) may include a plurality of steps, and when the step (c) is performed during the first electrode preparation step (S10), the step (c) may be referred to as a slitting step (S13).

[0075] According to one embodiment of the present invention, the steps (a) and (b) may be performed during the first electrode preparation step (S10), and the step (c) may be performed during or after the first electrode preparation step (S10). Specifically, the step (c) may be performed before or after the winding step (S50). More specifically, the step (c) may be performed after the winding step (S50).

[0076] When a protective tape is used to protect the end of the electrode exposed by the slitting step, a separate process is required after the electrode is slit to confirm the position of the slit end of the electrode and to properly attach the protective tape to surround it, and an inspection process, for example, a vision inspection process, is further required to eliminate defective attachment after attaching the protective tape to the end of the electrode. Furthermore, if the winding process is performed only after the vision inspection process to reduce defects in the electrode assembly, there is a problem that the production speed of the jelly roll type electrode assembly is significantly reduced and a roll-to-roll process is practically impossible.

[0077] In contrast, the method for manufacturing a jelly roll type electrode assembly according to an embodiment of the present invention can produce a jelly roll type electrode assembly including the swelling tape in a continuous process using conventional roll to roll process equipment. In other words, the method for manufacturing a jelly roll type electrode assembly can include the swelling tape attachment step (S12) in the first electrode preparation step (S10), so that the step (c) can be performed during or after the first electrode preparation step (S10), and therefore the entire process can be performed by a roll to roll process used in the industry. That is, the method for manufacturing a jelly roll type electrode assembly according to an embodiment of the present invention can ensure productivity and economy by continuously producing a jelly roll type electrode assembly including a swelling tape that expands when immersed in the electrolyte and is attached to surround one end of the positive electrode in the longitudinal direction using conventional roll to roll process equipment.

[0078] FIG. 2 is a schematic diagram showing a method for manufacturing a jelly roll type electrode assembly including a swelling tape and a method for manufacturing a jelly roll type electrode assembly including a PET tape according to an embodiment of the present invention.

[0079] Specifically, FIG. 2(a) illustrates a schematic diagram of a method for manufacturing a jelly roll type electrode assembly including a swelling tape according to one embodiment of the present invention, the method including a step (S12) of attaching a swelling tape, and FIG. 2(b) illustrates a schematic diagram of a method for manufacturing a jelly roll type electrode assembly including a PET tape, in which a PET protective tape is attached to surround a first end of the first electrode instead of the swelling tape.

[0080] 2(b), an additional process is required to attach a protective tape to surround a first end of a first electrode, as in the jelly roll type electrode assembly including a swelling tape according to an embodiment of the present invention. That is, when a protective tape (PET) attachment step (S12') is included instead of the swelling tape attachment step (S12), an additional process is required to produce an electrode of a similar structure.

[0081] Specifically, when a protective tape (PET) attaching step (S12') is included instead of a swelling tape attaching step (S12), a first electrode transferring step (S11) is followed by a first electrode separating step (S11') of separating the slit first electrode by a predetermined distance in order to attach a protective tape made of PET material, and an additional slitting step (S13') of slitting the attached protective tape to surround the longitudinal end of the first electrode is further required.

[0082] More specifically, when a protective tape (PET) attaching step (S12') is included instead of the swelling tape attaching step (S12), a slitting step (S11') is required after stopping the winder of the running first electrode, and a step (S11'') of separating the first electrode in consideration of the thickness of the first electrode so as to sufficiently surround the first end of the slit first electrode is further required. Then, a protective tape is attached to both sides of the separated first electrode (S12'); and an additional slitting step (S13') of cutting the attached protective tape is further required.

[0083] That is, when a PET protective tape is used instead of a swelling tape, certain additional processes are required to manufacture a structure similar to the jelly roll type electrode assembly including the swelling tape according to an embodiment of the present invention.

[0084] In other words, the method for manufacturing a jelly roll type electrode assembly according to an embodiment of the present invention includes the swelling tape attachment step (S12), thereby minimizing additional processes and providing a jelly roll type electrode assembly including a swelling tape attached to surround one end of the positive electrode in the longitudinal direction. In addition, the method can be produced in a continuous process using conventional roll-to-roll process equipment, ensuring productivity and economy.

[0085] FIG. 3 is an image showing an embodiment of a method for manufacturing a jelly-roll type electrode assembly according to an embodiment of the present invention.

[0086] Specifically, FIG. 3(a) shows a state in which the swelling tape is attached to a slitting area included in the first electrode in the winding process (S50) after the swelling tape attachment step (S12), FIG. 3(b) shows a state in which the swelling tape is attached to one end of the first electrode after the slitting step (S13), and FIG. 3(c) is an image showing a state in which the jelly roll type electrode assembly is disassembled after the winding process (S50) and the swelling tape is attached.

[0087] Referring to FIG. 2(a), the method for manufacturing a jelly roll type electrode assembly according to an embodiment of the present invention may further include a supplying process (S20), a positioning process (S30), a laminating process (S40), a winding process (S50), a taping process (S60), and an inspection process (S70), etc.

[0088] Specifically, the supplying step (S20) may be a step of supplying the first electrode and the second electrode together with a first separator and a second separator after the first electrode preparing step (S10), and the arranging step (S30) may be a step of sequentially arranging the first electrode, the first separator, the second electrode, and the second separator supplied in the supplying step (S20) to form a laminate.

[0089] The lamination process (S40) may also involve pressurizing and heat-sealing the laminate produced in the arrangement process (S30), i.e., a laminate including the first electrode, the first separator, the second electrode, and the second separator, to provide an electrode assembly.

[0090] Meanwhile, the winding process (S50) may involve winding up the electrode assembly after the lamination process, and may further include a slitting process of cutting the electrode assembly to a set length before or after the winding process.

[0091] Next, the taping process (S60) may be a process of finishing the outer surface of the electrode assembly wound in the winding process (S50) with a sealing tape, and the taping process can prevent defects such as the electrode assembly becoming unraveled due to the longitudinal ends of the first electrode, first separator, second electrode, and second separator becoming separated.

[0092] The inspection process (S70) may include a vision inspection step of inspecting the shape, arrangement, damage, etc. of the first electrode, first separator, second electrode, and second separator included in the electrode assembly to determine whether they are defective, and a voltage resistance inspection step of supplying power to the electrode assembly and measuring a voltage resistance to determine whether they are defective.

[0093] According to an embodiment of the present invention, the swelling tape used in the method for manufacturing the jelly roll type electrode assembly may be the same as the swelling tape described above for the jelly roll type electrode assembly.

[0094] According to an embodiment of the present invention, the width direction length of the swelling tape may be 60% to 100% based on the 100% width of the first electrode. Specifically, the width direction length of the swelling tape may be 70% to 100%, 80% to 100%, 60% to 90%, 60% to 80%, 60% to 70%, or 70% to 90% based on the 100% width of the first electrode. When the width direction length of the swelling tape satisfies the above-mentioned range, the length of the swelling tape after expansion can correspond to the width direction length of the first electrode, and one end of the swelling tape effectively surrounds one end of the first electrode in the length direction, so that even if the separator is damaged, the role of preventing internal short circuit between the positive and negative electrodes can be more efficiently performed.

[0095] According to one embodiment of the present invention, the length of the swelling tape in the longitudinal direction may be 500% or more and 7000% or less based on the 100% thickness of the first electrode. Specifically, the length of the swelling tape in the longitudinal direction may be 600% or more, 700% or more, 800% or more, or 1000% or more based on the 100% thickness of the first electrode, and the length of the swelling tape in the longitudinal direction may be 6000% or less, 5000% or less, 4000% or less, or 3000% or less based on the 100% thickness of the first electrode, and preferably 2000% or less, 1700% or less, or 1400% or less. When the length of the swelling tape in the longitudinal direction satisfies the above-mentioned range, the length of the swelling tape slit after step (c) may be within a suitable range, i.e., 250% to 3500%, preferably 250% to 1000%, based on the thickness of the first electrode (100%). The length of the swelling tape in the longitudinal direction after expansion may correspond to the thickness of the first electrode, and one end of the swelling tape may effectively surround one end of the first electrode in the longitudinal direction. This minimizes the influence on electrochemical properties such as the capacity reduction rate of a battery including the swelling tape, and more efficiently prevents internal short circuit between the positive and negative electrodes even if the separator is damaged.

[0096] According to an embodiment of the present invention, the length of the swelling tape in the longitudinal direction may be 0.75 mm or more and 10 mm or less. Specifically, the length of the swelling tape in the longitudinal direction may be 1 mm or more, 1.25 mm or more, 1.5 mm or more, 1.75 mm or more, or 2 mm or more, and the length of the swelling tape in the longitudinal direction may be 2.75 mm or less, 2.5 mm or less, 2.25 mm or less, or 2 mm or less. When the length of the swelling tape in the longitudinal direction satisfies the above-mentioned range, even if there is a certain process deviation, it is easy to manufacture a swelling tape whose length in the longitudinal direction corresponds to the thickness of the first electrode.

[0097] According to one embodiment of the present invention, the first electrode may be a positive electrode and the second electrode may be a negative electrode. The positive electrode and the negative electrode used in the manufacturing method of the jelly roll type electrode assembly may be the same as those described above for the jelly roll type electrode assembly.

[0098] One embodiment of the present invention provides a jelly-roll type electrode assembly manufactured by the above-mentioned method for manufacturing a jelly-roll type electrode assembly.

[0099] A jelly-roll type electrode assembly according to an embodiment of the present invention includes a swelling tape that expands when immersed in an electrolyte and is attached to surround one longitudinal end of a positive electrode, thereby preventing damage to the positive electrode and separator due to deformation of the electrode assembly caused by contraction / expansion of the electrodes during charging / discharging of the battery, and even if the separator is damaged, the swelling tape prevents internal shorts between the positive electrode and negative electrode, thereby improving stability and life characteristics of the battery. In addition, when the swelling tape surrounds the longitudinal end of the first electrode, the properties of the porous material of the swelling tape can provide excellent effects of relieving internal stress and improving the roundness of the core portion.

[0100] An embodiment of the present invention provides a secondary battery including the jelly-roll type electrode assembly and a battery case for housing the electrode assembly. Specifically, the secondary battery may include the electrode assembly according to the embodiment described above and a battery case for housing the electrode assembly.

[0101] The secondary battery according to the present invention can prevent an internal short circuit between the positive and negative electrodes even when the electrode assembly is deformed due to the contraction / expansion of the electrodes during charging / discharging of the battery, thereby improving the stability and life characteristics of the battery.

[0102] According to one embodiment of the present invention, the battery case may be cylindrical. Specifically, the battery case may be cylindrical, square, or pouch-shaped depending on the application, but is not limited thereto.

[0103] According to one embodiment of the present invention, the battery case may contain an electrolyte inside. Specifically, the electrolyte may be, but is not limited to, an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a molten inorganic electrolyte that can be used in manufacturing a lithium secondary battery. Specifically, the electrolyte may contain a non-aqueous organic solvent and a metal salt.

[0104] According to one embodiment of the present invention, the non-aqueous organic solvent may be, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, or ethyl propionate.

[0105] According to one embodiment of the present invention, the metal salt may be a lithium salt, and the lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte. For example, the anion of the lithium salt is F - , Cl - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3- , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.

[0106] According to one embodiment of the present invention, in addition to the constituent components of the electrolyte, the electrolyte may further contain one or more additives such as a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing a decrease in battery capacity, and improving the discharge capacity of the battery. EXAMPLES

[0107] Hereinafter, the present invention will be described in detail with reference to examples in order to specifically explain the present invention. However, the examples according to the present invention may be modified in various different forms, and the scope of the present invention should not be construed as being limited to the examples described below. The examples in the present specification are provided to more completely explain the present invention to those having average knowledge in the art.

[0108] [Example 1] <Manufacturing of electrode assembly> An Al foil having a thickness of 15 μm and a width of 63.9 mm was prepared as a positive electrode current collector. A positive electrode active material layer was formed by applying and drying a positive electrode active material slurry containing an NMCA (Ni-Mn-Co-Al) composite with a Ni content of 92% or more as a positive electrode active material and CNT as a conductive material onto the positive electrode current collector, and a positive electrode active material layer was produced with a total thickness of 154 μm.

[0109] Then, a 52 μm thick swelling tape having an adhesive layer containing a copolymer of ethyl acrylate (EA) and polyethyl methacrylate (PEMA) on one side of a base layer of polyurethane (PU) material was prepared, and the swelling tape was attached to one side of the slit region of the positive electrode so that the width was 62 mm and the length was 10 mm.

[0110] Next, a Cu foil having a thickness of 10 μm and a length of 62 mm in the width direction was prepared as a negative electrode current collector, and a negative electrode active material slurry containing 50 parts by weight each of artificial graphite and natural graphite as negative electrode active materials was applied onto the negative electrode current collector and dried to form a negative electrode active material layer, thereby producing a negative electrode with a total thickness of 187 μm.

[0111] Meanwhile, two sheet-shaped polyethylene separators were prepared as a first separator and a second separator.

[0112] Then, the positive electrode, the first separator, the negative electrode, and the second separator were sequentially arranged to form a laminate, which was then pressed and heat-sealed, the center of the slit region was slit, the laminate was wound so that the first end where the winding of the positive electrode begins was located at the core, and a seal tape made of PET material was attached to the second end where the winding ends so as to surround the outer periphery of the upper and lower ends of the jelly roll, to manufacture a jelly roll type electrode assembly. In this case, the seal tape used was 62 mm long, 10 mm wide, and 22 μm thick, and the length of the swelling tape after slitting was 5 mm.

[0113] <Secondary battery manufacturing> The jelly-roll type electrode assembly was inserted into a cylindrical battery case, and an electrolyte solution prepared by mixing ethylene carbonate (EC): dimethyl carbonate (DMC): ethyl methyl carbonate (EMC) in a weight ratio of 4:9:3 and dissolving LiPF6 to contain 15 wt% was poured into the cylindrical battery case, and the cylindrical battery case was sealed with a cap assembly to manufacture a secondary battery.

[0114] [Example 2] A jelly-roll type electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that swelling tapes were attached to both sides of the slit region of the positive electrode to a width of 62 mm and a length of 5 mm.

[0115] [Comparative Example 1] A jelly-roll type electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that a PET tape was attached to one side of the slit region of the positive electrode so as to have a width of 62 mm and a length of 10 mm.

[0116] [Comparative Example 2] A jelly-roll type electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that no swelling tape was attached to the slit region of the positive electrode.

[0117] [Comparative Example 3] A jelly-roll type electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that no swelling tape was attached to the slit region of the positive electrode, the center of the slit region was slit, the slit positive electrode was separated, and then PET tapes were attached to both sides of the slit region to a length of 62 mm in the width direction and a length of 10 mm in the length direction, and the center was further slit to obtain the structure shown in FIG. 1(b).

[0118] [Experimental Example] <Experimental Example 1 - Swelling Evaluation> A sample (length 10 mm in the length direction, length 62 mm in the width direction) made of the same material as the swelling tape used in the examples 1 and 2 was prepared, and an electrolyte solution was prepared by dissolving LiPF6 as an electrolyte in a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). The swelling tape sample was then immersed in the electrolyte solution for 60 minutes, and the length of the swelling tape before and after expansion was measured. The composition of the electrolyte solution used in the swelling evaluation is shown in Table 1 below. The swelling characteristics of the swelling tape samples were evaluated in the same manner in Experimental Examples 1-1 to 1-6, except that the electrolyte solutions having the compositions shown in Table 1 below were used for impregnation.

[0119] [Table 1]

[0120] Thereafter, the ratio of the length of the swelling tape after expansion to the length of the swelling tape before expansion was calculated and shown in Table 1 and Figure 4. Specifically, Figure 4 shows the ratios of the length in the transverse direction (TD) and the machine direction (MD) of the swelling tape after expansion to the length of the swelling tape before expansion, calculated after the swelling tape sample was immersed in DMC and an electrolyte solution having the composition of Experimental Example 1-1 for 60 minutes.

[0121] Referring to Table 1, it was confirmed that the length of the swelling tape in the length direction and width direction after expansion when impregnated with the electrolyte solution having the composition of Experimental Example 1-1 to Experimental Example 1-6 was about 140% of the length of the swelling tape before expansion. Specifically, referring to Experimental Example 1-1 to Experimental Example 1-6, it was confirmed that when the presence or absence and content of other solvent components, i.e., ethylene carbonate (EC), propylene carbonate (PC), and ethyl methyl carbonate (EMC), in addition to dimethyl carbonate (DMC), were adjusted, the swelling characteristics of the swelling tape were slightly affected depending on the composition of the mixed solvent, but there was no significant difference. Meanwhile, referring to Reference Example 1-1 and Experimental Example 1-1 to Experimental Example 1-6, it was confirmed that when about 7 wt % and about 15 wt % of LiPF6 used as the electrolyte were added, that is, when the electrolyte content was different, the difference in the degree of expansion was within about 3%, which was not significant. In contrast, when the electrolyte content was 0%, i.e., when no electrolyte was added, the difference in the degree of swelling was about 15%, indicating that the presence or absence of electrolytes makes a relatively large difference in the swelling properties of the swelling tape.

[0122] 4, it was confirmed that the length of the swelling tape in the length and width directions after expansion when immersed in the electrolyte having the composition of Experimental Example 1-1 was about 140% of the length of the swelling tape before expansion. Specifically, it was confirmed that the length of the swelling tape expanded at the same rate in both the length and width directions, and expanded to about 120% on one side from the center of the swelling tape before expansion to one end. This shows the minimum length in the width and length directions of the swelling tape that should be attached so that one end of the expanded swelling tape protects one end of the first electrode.

[0123] <Experimental Example 2 - Evaluation of activation> The secondary batteries prepared in Example 1 and Comparative Example 1 were activated by performing two cycles at 4.2 V-2.5 V, 0.2 C charge, and 0.2 C discharge, respectively, and then disassembled to prepare jelly-roll type electrode assemblies before and after activation. The ends of the positive electrodes of the jelly-roll type electrode assemblies were observed with the naked eye, and the evaluation results are shown in FIGS. 5 and 6.

[0124] Specifically, FIG. 5(a) shows a first end of the first electrode of the jelly roll type electrode assembly according to Example 1 before activation, FIG. 5(b) shows a first end of the first electrode of the jelly roll type electrode assembly according to Example 1 after activation, FIG. 6(a) shows a first end of the first electrode of the jelly roll type electrode assembly according to Comparative Example 1 before activation, and FIG. 6(b) shows a first end of the first electrode of the jelly roll type electrode assembly according to Comparative Example 1 after activation.

[0125] 5, in the case of the jelly-roll type electrode assembly according to Example 1, it was confirmed that the swelling tape attached so that one end of the swelling tape coincides with the first end of the first electrode before activation expands after activation to surround the first end of the first electrode. In this case, the length 2L of the swelling tape attached on at least one side of the slitting region included in the first electrode is 10 mm, and after the step of slitting the center in the longitudinal direction of the slitting region of the first electrode, the length (L) of the swelling tape before expansion is 5 mm, the length (L') of the swelling tape after expansion is 7 mm, and the expanded length (L -s ) was measured to be 2 mm in total. In other words, it was confirmed that the length (L') of the swelling tape after expansion was expanded to about 140% of the length (L) of the swelling tape before expansion, and that the swelling tape expanded 1 mm on one side from the center of the swelling tape before expansion to one end, i.e., 120% of the length (L) of the swelling tape before expansion. As a result, it was confirmed that the jelly roll type electrode assembly including the swelling tape according to the present invention expands due to the electrolyte, and the swelling tape after expansion effectively surrounds the first end of the first electrode.

[0126] In contrast, referring to FIG. 6, in the case of the jelly-roll type electrode assembly according to Comparative Example 1, the PET tape that was attached so that one end of the first electrode coincided with the first end of the first electrode before activation did not expand even after activation, and the first end of the first electrode was exposed.

[0127] <Experimental Example 3 - Evaluation of cycle stability> The secondary batteries prepared in Example 1 and Comparative Example 2 were subjected to a cycle test at 25° C. to test the battery characteristics.

[0128] Specifically, after 500 cycles, the coulomb efficiency was analyzed to check for short circuit behavior during the cycles, and room temperature voltage tracking was performed to evaluate abnormal behavior in more detail. The evaluation results are shown in Figure 7.

[0129] Specifically, FIG. 7(a) shows the change in Coulombic efficiency with the progress of cycles of the secondary batteries manufactured in Example 1 and Comparative Example 2, and FIG. 7(b) shows the evaluation results of room temperature-voltage tracking with time of the secondary batteries manufactured in Example 1 and Comparative Example 2.

[0130] 7(a), it was confirmed that the secondary battery according to Example 1 did not exhibit any particular abnormal behavior, but the secondary battery according to Comparative Example 2 exhibited abnormal behavior in Coulomb efficiency, i.e., leakage current. Also, referring to FIG. 7(b), it was confirmed that the secondary battery according to Example 1 maintained a voltage of 1.0V or more even after 12 hours, but the secondary battery according to Comparative Example 2 was unable to maintain a constant voltage and the voltage gradually decreased as time passed. This indicates that the separator was damaged and an internal short circuit occurred.

[0131] Thereafter, each of the secondary batteries according to Example 1 was disassembled, and the presence or absence of separator damage was evaluated with the naked eye. The results are shown in FIG.

[0132] Specifically, (a) of FIG. 8 is an image showing the state of the first electrode facing portion of the separator included in the secondary battery manufactured in Example 1, and (b) of FIG. 8 is an image showing the state of the first electrode facing portion of the separator included in the secondary battery manufactured in Comparative Example 2.

[0133] Referring to FIG. 8, it was confirmed that damage occurred in the separator of the secondary battery according to Comparative Example 2, in which no swelling tape was attached.

[0134] As a result, it has been confirmed that the secondary battery according to the present invention prevents an internal short circuit between the positive and negative electrodes even when the electrode assembly is deformed due to the contraction / expansion of the electrodes during charging / discharging of the battery, thereby improving the stability and life characteristics of the battery.

[0135] <Experimental Example 4 - Evaluation of roundness and productivity> In order to confirm the degree of improvement in deformation of the secondary batteries manufactured in Example 1 and Comparative Example 3, circularity was evaluated after 20 cycles at 25° C., and the results are shown in Table 2 and Fig. 9 below. Here, circularity (%) indicates the degree to which the shape of the electrode assembly is closer to a circle, and the maximum and minimum separation distances between the winding shaft and the positive electrode were measured from a computed tomography (CT) image of the positive electrode, and the ratio (%) of the minimum separation distance between the winding shaft and the positive electrode to the maximum separation distance between the winding shaft and the positive electrode (100%) was calculated.

[0136] In addition, in order to evaluate the productivity of each jelly-roll type electrode assembly, the time required to manufacture the jelly-roll type electrode assembly, i.e., the takt time, was measured and is shown in Table 2 below.

[0137] [Table 2]

[0138] 9 is an image showing the evaluation results of the circularity of the secondary batteries manufactured in Example 1 and Comparative Example 3. Referring to Table 2, it was confirmed that the secondary battery according to Comparative Example 3, which has a structure similar to that of the secondary battery according to Example 1 including the swelling tape after expansion by surrounding the longitudinal end of the positive electrode with a PET protective tape, has a takt time of 3.0 seconds, which is approximately double that of the secondary battery according to Example 1, and is inferior in productivity.

[0139] As a result, the method for manufacturing a jelly roll type electrode assembly according to an embodiment of the present invention includes a swelling tape attachment step, thereby minimizing additional processes, and can provide a jelly roll type electrode assembly including a swelling tape attached to surround one longitudinal end of a positive electrode. It can also be seen that the method can be produced in a continuous process using conventional roll-to-roll process equipment, thereby ensuring productivity and economy.

[0140] Meanwhile, referring to Table 2 and FIG. 9, it was confirmed that the secondary battery according to Comparative Example 3 had a circularity of 90% or less and had a similar or inferior improvement in safety compared to the secondary battery according to Example 1.

[0141] As a result, the secondary battery according to the present invention includes a structure in which the expanded swelling tape surrounds the longitudinal end of the first electrode, thereby preventing internal short circuits between the positive and negative electrodes even when the electrode assembly is deformed due to the contraction / expansion of the electrodes during charging / discharging of the battery, thereby improving the stability and life characteristics of the battery. It can also be seen that the properties of the porous material of the swelling tape provide excellent effects in relieving internal stress and improving the roundness of the core portion.

[0142] The above detailed description is illustrative and explanatory of the present invention. Moreover, the above-mentioned contents are merely illustrative and explanatory of preferred embodiments of the present invention. As mentioned above, the present invention can be used in various other combinations, modifications, and environments, and changes or modifications can be made within the scope of the inventive concept disclosed herein, the scope of the above-mentioned disclosure, and / or the skill or knowledge of the art. Therefore, the above detailed description of the invention is not intended to limit the present invention to the disclosed embodiments. Moreover, the appended claims should be construed to include other embodiments. [Explanation of symbols]

[0143] 100...1st electrode 101: First electrode collector 102, 103...first electrode active material layer 110 First end of first electrode 20 Separator 30, 30' Swelling Tape 40 ···PET tape L: Length of swelling tape before expansion L': Length of the swelling tape after expansion Ls: Swelling length of the swelling tape S10, S10'...First electrode preparation process S11: First electrode transfer step S11' Slit stage S11'' First electrode separation stage S12: Swelling tape application step S12' Protective tape application stage S13, S13' slit stage S20...Supply process S30...Placement process S40 ···Lamination process S50 Winding process S60 ···Taping process S70: Inspection process TD...Width direction MD: Length direction

Claims

1. A jelly roll type electrode assembly in which a first electrode, a first separator, a second electrode, and a second separator are sequentially stacked and wound up, A swelling tape is attached to at least one surface of the first electrode, the first electrode includes a first end along its length where winding begins; and a second end along its length where winding terminates; The swelling tape is attached such that one end of the swelling tape coincides with the first end of the first electrode, forming a jelly roll type electrode assembly.

2. 2. The jelly-roll type electrode assembly of claim 1, wherein the length of the swelling tape in a width direction is 60% to 100% based on 100% of the width of the first electrode.

3. The jelly-roll type electrode assembly of claim 1 , wherein the length of the swelling tape in a longitudinal direction is from 250% to 3500% based on 100% of the thickness of the first electrode.

4. The swelling tape expands due to an electrolyte solution, 4. The jelly roll type electrode assembly of claim 1, wherein the swelling tape after expansion surrounds the first end of the first electrode.

5. 5. The jelly-roll type electrode assembly of claim 4, wherein the electrolyte contains 70% by weight or more of any one of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and a mixture thereof.

6. 45% by weight of dimethyl carbonate, 20% by weight of ethylene carbonate, 15% by weight of ethyl methyl carbonate, and LiPF as an electrolyte 6 The length of the swelling tape after immersion for 60 minutes in an electrolyte solution containing 15% by weight of 5. The jelly roll type electrode assembly of claim 4, wherein the length of the swelling tape before expansion is 120% to 160% based on 100%.

7. The swelling tape includes a base layer and an adhesive layer, The jelly roll type electrode assembly according to any one of claims 1 to 3, wherein the adhesive layer is provided on at least one surface of the base material layer.

8. 8. The jelly roll type electrode assembly of claim 7, wherein the adhesive layer comprises a pressure-sensitive adhesive comprising a polyacrylic resin.

9. 8. The jelly roll type electrode assembly of claim 7, wherein the adhesive layer comprises at least one comonomer selected from the group consisting of poly methyl methacrylate (PMMA), poly ethyl methacrylate (PEMA), and poly butyl methacrylate (PBMA).

10. The jelly roll type electrode assembly according to claim 7 , wherein the base layer comprises a urethane-based resin.

11. 4. The jelly roll type electrode assembly according to claim 1, wherein the first electrode is a positive electrode and the second electrode is a negative electrode.

12. 4. The jelly roll type electrode assembly according to claim 1, wherein the first electrode includes a current collector and an active material layer provided on the current collector.

13. A method for manufacturing a jelly roll type electrode assembly in which a first electrode, a first separator, a second electrode, and a second separator are sequentially stacked and wound, comprising: (a) transporting the first electrode; (b) attaching a swelling tape onto at least one surface of a slitting region included in the first electrode; and (c) slitting the first electrode at a center portion in a longitudinal direction of the slit region. Including, In the step (b), the swelling tape is attached such that a center portion of the swelling tape in a longitudinal direction coincides with a center portion of the slit region of the first electrode in a longitudinal direction; wherein step (c) comprises slitting a center portion of the slit region in a longitudinal direction to provide the first electrode with a first end where winding begins and a second end where winding ends along a longitudinal direction.

14. 14. The method of claim 13, wherein the length of the swelling tape in a width direction is 60% to 100% based on 100% of the width of the first electrode.

15. 14. The method of claim 13, wherein the length of the swelling tape in a longitudinal direction is from 500% to 7000% based on 100% of the thickness of the first electrode.

16. 14. The method of claim 13, wherein the first electrode is a positive electrode and the second electrode is a negative electrode.

17. The jelly roll type electrode assembly according to any one of claims 1 to 3; and a battery case for housing the electrode assembly;

18. The secondary battery according to claim 17 , wherein the battery case is cylindrical.

Citation Information

Patent Citations

  • Negative electrode plate, energy storage element, method for manufacturing negative electrode plate, and method for manufacturing energy storage element

    JP2017130439A

  • secondary battery

    JP2017510043A

  • Power storage element

    JP2021002422A

  • Vehicle battery charging device

    KR1020230168377A

  • Secondary battery

    US20170207438A1