Durability improver for PEMFC electrolyte membrane, PEMFC composite electrolyte membrane containing same, and PEMFC membrane-electrode assembly
The composite electrolyte membrane for PEMFCs, using Pt-supported carriers, addresses durability issues by acting as both primary and secondary antioxidants, enhancing stability and efficiency in PEMFCs.
Patent Information
- Application Number
- JP2024527097
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-05-20
- Filing Date
- 2022-09-15
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-09-15
AI Technical Summary
Existing polymer electrolyte membrane fuel cells (PEMFCs) face issues with electrolyte membrane durability due to chemical degradation caused by radicals, leading to performance degradation and reduced lifespan, particularly in thin membranes with high hydrogen ion transmission requirements.
A composite electrolyte membrane for PEMFCs is developed, incorporating a durability improver composed of platinum (Pt) nanoparticles supported by carriers like CeO2, GDC (Gd-doped Ceria), IrO2, SnO2, or Ti4O7, which act as both primary and secondary antioxidants, reducing gas permeability and enhancing membrane stability.
The composite electrolyte membrane exhibits improved durability, dimensional stability, and tensile strength, enabling highly efficient and long-lasting PEMFCs with reduced radical-induced degradation.
Smart Images

Figure 2024542162000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a high durability improving agent that suppresses chemical degradation of an electrolyte membrane in a membrane-electrode assembly for PEMFC, and to a PEMFC composite electrolyte membrane and membrane-electrode assembly produced by applying the same. [Background technology]
[0002] Fuel cells are power generation systems that convert chemical energy generated by electrochemically reacting fuel (hydrogen or methanol) with oxidant (oxygen) directly into electrical energy, and are being researched and developed as a next-generation energy source due to their high energy efficiency and environmental friendliness with low pollutant emissions. Fuel cells can be used for either high-temperature or low-temperature applications depending on the field of application, and are generally classified by the type of electrolyte. For high-temperature applications, there are solid oxide fuel cells (SOFC) and molten carbonate fuel cells (MCFC), while for low-temperature applications, alkaline fuel cells (AFC) and polymer electrolyte membrane fuel cells (PEMFC) are representative.
[0003] Among these, polymer electrolyte fuel cells can be further divided into proton exchange membrane fuel cells (PEMFC), which use hydrogen gas as fuel, and direct methanol fuel cells (DMFC), which use liquid methanol as fuel directly supplied to the anode. Polymer electrolyte fuel cells have been attracting attention as portable, vehicle, and home power sources due to their advantages such as a low operating temperature of less than 100°C, elimination of water leakage problems by using a solid electrolyte, quick start-up and response characteristics, and excellent durability. In particular, they are high-output fuel cells with a higher current density than other types of fuel cells, and can be miniaturized, so research into their use as portable fuel cells is ongoing.
[0004] The unit cell structure of such a fuel cell consists of an electrolyte membrane made of polymer material, with an oxidizing electrode (anode, fuel electrode) and a reducing electrode (cathode, oxygen electrode) applied to either side, which is called a membrane electrode assembly (MEA). This membrane electrode assembly (MEA) is the part where the electrochemical reaction between hydrogen and oxygen occurs, and is composed of a reducing electrode, an oxidizing electrode, and an electrolyte membrane, i.e., an ion-conducting electrolyte membrane (e.g., a proton-conducting electrolyte membrane).
[0005] At the oxidizing electrode, hydrogen or methanol is supplied as fuel, and an oxidation reaction of hydrogen occurs, generating hydrogen ions and electrons. At the reducing electrode, hydrogen ions that have passed through the polymer electrolyte membrane combine with oxygen, and water is produced by a reduction reaction of oxygen.
[0006] This membrane-electrode assembly is formed by coating the electrode catalyst layers of the oxidizing and reducing electrodes on both sides of an ion-conducting electrolyte membrane, and the material that forms the electrode catalyst layer is a catalyst material such as Pt (platinum) or Pt-Ru (platinum-ruthenium) supported on a carbon support. The membrane-electrode assembly (MEA), which is considered the core component of the electrochemical reaction of fuel cells, uses ion-conducting electrolyte membranes and platinum catalysts, which are particularly expensive, and is directly linked to the efficiency of power production, so it is considered the most important part in improving the performance and price competitiveness of fuel cells.
[0007] The commonly used method for manufacturing an MEA is to prepare a paste by mixing a catalyst material and a proton conductive binder, i.e., a fluorine-based Nafion ionomer, with water and / or an alcohol solvent, and then coat this on a carbon cloth or carbon paper, which acts as an electrode support for the catalyst layer and also as a gas diffusion layer, and then dry it and heat-seal it to a proton conductive electrolyte membrane.
[0008] In the catalyst layer, the oxidation-reduction reaction of hydrogen and oxygen by the catalyst, the movement of electrons by the closely packed carbon particles, the provision of a passage for supplying hydrogen, oxygen and moisture and discharging excess gas after the reaction, and the movement of oxidized hydrogen ions must occur simultaneously. Furthermore, to improve performance, the area of the triple phase boundary where the supplied fuel meets the catalyst and the ion-conductive polymer electrolyte membrane must be increased to reduce activation polarization, and the interface between the catalyst layer and the electrolyte membrane and the interface between the catalyst layer and the gas diffusion layer must be uniformly bonded to reduce ohmic polarization at the interface. Therefore, in order to improve the performance of the fuel cell by maximally reducing the interfacial resistance between the catalyst layer and the electrolyte membrane, not only must there be an adhesive force between the catalyst layer and the electrolyte membrane when the MEA is manufactured, but the interfacial adhesion between the catalyst layer and the electrolyte membrane must be continuously maintained even during the operation of the fuel cell.
[0009] For this reason, technological developments for uniformly bonding the interface between the catalyst layer and the electrolyte membrane and the interface between the catalyst layer and the gas diffusion layer have been actively conducted in recent years, but there is still a drawback in that the uniformity of the interface is still limited.
[0010] In addition, in the case of the MEA having the above-mentioned structure, since a thick electrolyte membrane is generally used, the transfer of hydrogen ions may be delayed, resulting in a decrease in performance.
[0011] In addition, as hydrogen ions move during operation of the fuel cell and the time of use increases, the interface between the catalyst layer and the electrolyte membrane and the interface between the catalyst layer and the gas diffusion layer weakens and separates, which can cause a decrease in the performance of the fuel cell when used in the fuel cell.
[0012] In order to shorten the migration time of hydrogen ions, the thickness of the electrolyte membrane must be reduced. To achieve this, one method is to reduce the thickness of the porous support that constitutes the electrolyte membrane. However, reducing the thickness of the support not only significantly reduces the physical properties of the support, such as its strength, during high elongation, but also increases the defect rate during the production of the support, reducing its economic and commercial viability. In particular, the durability of the electrolyte membrane is poor.
[0013] In addition, hydrogen, which is a reactant gas in a fuel cell, and oxygen in the air crossover through the electrolyte membrane to promote the production of hydrogen peroxide, which then generates oxygen-containing radicals such as hydroxyl radical (·H) and hydroperoxyl radical (·OOH). These radicals attack the ionomer electrolyte membrane, inducing chemical degradation of the membrane and ultimately causing a voltage drop in the fuel cell.
[0014] To prevent this, various antioxidants are used. For example, a primary antioxidant with a radical scavenger function and a secondary antioxidant with a hydrogen peroxide decomposer function are mixed and applied to the electrolyte membrane. However, the use of such primary antioxidants increases the antioxidant properties, but it is known that it can cause problems such as a decrease in the long-term stability of the electrolyte membrane (S. Schlick et al., J. Phys. Chem. C, 120, 6885-6890 (2016); S. Deshpande et al., Appl. Phys. Lett., 8, 133113 (2005)).
[0015] Thus, new approaches are required to improve the durability of electrolyte membranes in order to increase the commercial viability of fuel cells.
Summary of the Invention
Problems to be Solved by the Invention
[0016] The present invention has been made in consideration of the above points, and has developed a highly durable enhancer for a PEMFC electrolyte membrane that can be combined with a specific material to not only serve as a primary antioxidant but also simultaneously serve as a secondary antioxidant, applied this to a thinned electrolyte membrane, and provided a composite electrolyte membrane for a PEMFC in which the electrolyte membrane is combined in a multilayer structure, a membrane - electrode assembly for a PEMFC using the same, and a durability improver applied thereto.
Means for Solving the Problems
[0017] The present invention for solving the above - mentioned problems relates to a durability improver for a PEMFC electrolyte membrane, which contains platinum (Pt) and a carrier supporting the platinum, and the carrier contains one or more selected from CeO2, GDC (Gd doped Ceria), IrO2, SnO2, and Ti4O7.
[0018] In a preferred embodiment of the present invention, the platinum is nano - sized platinum powder, and the platinum powder may be bonded to the surface of the carrier and integrated.
[0019] In a preferred embodiment of the present invention, the GDC is a compound represented by the following chemical formula (1), and gadolinium (Gd) may be doped into the ceria lattice.
[0020]
Chemical Formula
[0021] In Chemical Formula (1), x is an integer satisfying 0 < x ≦ 0.3, and y is an oxygen vacancy value that makes the compound electrically neutral, and is an integer satisfying 0 < y ≦ 0.25.
[0022] In a preferred embodiment of the present invention, the platinum content is 0.01 to 6.00% by weight, with the remainder being the carrier.
[0023] In a preferred embodiment of the present invention, the particle size (D 50 ) is 0.1 to 50 nm, and the carrier has a particle size (D 50 ) may be 10 to 2,000 nm.
[0024] In a preferred embodiment of the present invention, the durability improver has a BET specific surface area of 10 to 500 m 2 / g.
[0025] In a preferred embodiment of the present invention, when the carrier is CeO2, the durability improving agent may contain 0.01 to 6.00% by weight of platinum particles based on the total weight of the agent.
[0026] In a preferred embodiment of the present invention, when the carrier is IrO2, the durability improving agent may contain 0.01 to 4.5% by weight of platinum particles based on the total weight of the agent.
[0027] In a preferred embodiment of the present invention, when the carrier is SnO2, the durability improving agent may contain 0.01 to 3.0% by weight of platinum particles based on the total weight of the agent.
[0028] In a preferred embodiment of the present invention, when the carrier is Ti4O7, the durability improving agent may contain 0.01 to 5.5% by weight of platinum particles based on the total weight of the agent.
[0029] In a preferred embodiment of the present invention, the high durability improving agent of the present invention may contain two or more of the above-mentioned composites, or may include a cerium-based composite containing the platinum particles and CeO2 supporting the platinum particles as a carrier; and a non-cerium-based composite containing the platinum particles and a carrier; and the carrier of the non-cerium-based composite may include one or more selected from IrO2, SnO2 and Ti4O7.
[0030] In a preferred embodiment of the present invention, the high durability improver of the present invention may contain the cerium-based complex and the non-cerium-based complex in a weight ratio of 1:0.1-50.
[0031] In a preferred embodiment of the present invention, the high durability improving agent of the present invention may also include the cerium-based complex; and a gadolinium-based complex including platinum (Pt) particles and a GDC (Gd doped Ceria) carrier carrying the platinum particles and represented by the chemical formula (1).
[0032] In a preferred embodiment of the present invention, the high durability improving agent of the present invention may contain the cerium-based complex and the gadolinium-based complex in a weight ratio of 1:0.05-10.
[0033] Another object of the present invention is to provide an electrolyte membrane for a PEMFC, which contains the durability improving agent described above.
[0034] In a preferred embodiment of the present invention, the electrolyte membrane for the PEMFC may be of single layer or multi-layer structure.
[0035] In a preferred embodiment of the present invention, the electrolyte membrane for the PEMFC may be a composite electrolyte membrane.
[0036] In a preferred embodiment of the present invention, the composite electrolyte membrane may have a structure in which a first electrolyte layer, a first support layer and a second electrolyte layer are laminated in order.
[0037] In a preferred embodiment of the present invention, the composite electrolyte membrane may have a multi-layer structure in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer, and a third electrolyte layer are sequentially stacked.
[0038] In a preferred embodiment of the present invention, the electrochemical cell may further include a third support layer formed on one surface of the third electrolyte layer; and a fourth electrolyte layer formed on one surface of the third support layer.
[0039] In a preferred embodiment of the present invention, any one or more layers selected from the first electrolyte layer, the second electrolyte layer, and the third electrolyte layer and / or the fourth electrolyte layer may contain the above-mentioned high durability improving agent.
[0040] In a preferred embodiment of the present invention, the PEMFC composite electrolyte membrane includes a first electrolyte layer and a second electrolyte layer, the first electrolyte layer and the second electrolyte layer include the high durability improving agent, and a weight ratio of the high durability improving agent in the first electrolyte layer to the high durability improving agent in the second electrolyte layer may be 1:0.05 to 1.00.
[0041] In a preferred embodiment of the present invention, at least one selected from the first electrolyte layer and the second electrolyte layer may contain the durability improving agent and an ionomer.
[0042] In a preferred embodiment of the present invention, at least one selected from the first electrolyte layer and the second electrolyte layer may further include a cerium (Ce)-based radical scavenger.
[0043] In a preferred embodiment of the present invention, each of the first electrolyte layer, the second electrolyte layer, the third electrolyte layer and / or the fourth electrolyte layer may include one or more selected from the group consisting of perfluorinated sulfonated ionomers and hydrocarbon-based ionomers.
[0044] In a preferred embodiment of the present invention, each of the first electrolyte layer, the second electrolyte layer, the third electrolyte layer and / or the fourth electrolyte layer may further include, in addition to the durability improving agent, a radical scavenger including one or more selected from CeZnO, CeO2, Ru, Ag, RuO2, WO3, Fe3O4, CePO4, CrPO4, AlPO4, FePO4, CeF3, FeF3, Ce2(CO3)3·8H2O, Ce(CHCOO)3·H2O, CeCl3·6H2O, Ce(NO3)6·6H2O, Ce(NH4)2(NO3)6, Ce(NH4)4(SO4)4·4H2O and Ce(CH3COCHCOCH3)3·3H2O.
[0045] In a preferred embodiment of the present invention, each of the first electrolyte layer, the second electrolyte layer, the third electrolyte layer and / or the fourth electrolyte layer may further include one or more selected from hollow silica and an absorbent.
[0046] In a preferred embodiment of the present invention, each of the first electrolyte layer, the second electrolyte layer, the third electrolyte layer and / or the fourth electrolyte layer of the composite electrolyte membrane for PEMFC independently contains the high durability improving agent, and the content of the high durability improving agent in the electrolyte layer may be configured to have a gradient in which the content becomes lower based on the cathode electrode.
[0047] In a preferred embodiment of the present invention, the composite electrolyte membrane for PEMFC may have a support layer formed between the first electrolyte layer and the second electrolyte layer, between the second electrolyte layer and the third electrolyte layer, and between the third electrolyte layer and the fourth electrolyte layer; or the composite electrolyte membrane may have only one support layer formed between the first electrolyte layer and the second electrolyte layer, between the second electrolyte layer and the third electrolyte layer, or between the third electrolyte layer and the fourth electrolyte layer.
[0048] In a preferred embodiment of the present invention, the composite electrolyte membrane for PEMFC may have an average thickness of 5 to 30 μm.
[0049] In a preferred embodiment of the present invention, each of the first electrolyte layer, the second electrolyte layer, the third electrolyte layer and / or the fourth electrolyte layer may have a thickness of 1 to 20 μm.
[0050] In a preferred embodiment of the present invention, each of the first support layer, the second support layer and / or the third support layer may have a thickness of 0.1 to 10 μm.
[0051] In a preferred embodiment of the present invention, each of the first support layer, the second support layer and / or the third support layer may include a PTFE porous support having an average pore size of 0.080 to 0.200 μm and an average porosity of 60 to 90%.
[0052] In a preferred embodiment of the present invention, when the composite electrolyte membrane has a structure in which a first electrolyte layer, a first support layer and a second electrolyte layer are laminated in order, the composite electrolyte membrane can satisfy the following condition (1):
[0053] Condition (1) B1≦A1, B1≦A2 In the above condition (1), A1 represents the thickness of the first electrolyte layer, A2 represents the thickness of the second electrolyte layer, and B1 represents the thickness of the first support layer.
[0054] In a preferred embodiment of the present invention, when the composite electrolyte membrane is applied to a membrane-electrode assembly for a PEMFC, the composite electrolyte membrane is an electrolyte membrane in which a first electrolyte layer, a first support layer and a second electrolyte layer are sequentially laminated from an anode side to a cathode side, and the composite electrolyte membrane may satisfy the following condition (2):
[0055] Condition (2) A1≦A2 In the condition (2), A1 represents the content of the durability improver in the first electrolyte layer, and A2 represents the content of the durability improver in the second electrolyte layer.
[0056] In a preferred embodiment of the present invention, the composite electrolyte membrane for PEMFC can satisfy all of the following conditions (3) and (4).
[0057] Condition (3) B1≦A1, B1≦A2, B1≦A3 Condition (4) B2≦A1, B2≦A2, B2≦A3 In the above conditions (3) and (4), A1 represents the thickness of the first electrolyte layer, A2 represents the thickness of the second electrolyte layer, A3 represents the thickness of the third electrolyte layer, B1 represents the thickness of the first support layer, and B2 represents the thickness of the second support layer.
[0058] In a preferred embodiment of the present invention, when the composite electrolyte membrane is applied to a membrane-electrode assembly for a PEMFC, the composite electrolyte membrane is a composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer, and a third electrolyte layer are sequentially laminated from the anode direction to the cathode direction, and the composite electrolyte membrane may satisfy the following condition (5) or (6):
[0059] Condition (5) A1≦A2≦A3 Condition (6) A2≦A1, A2≦A3, A1≦A3 In the above conditions (5) and (6), A1 represents the content of the durability improving agent in the first electrolyte layer, A2 represents the content of the durability improving agent in the second electrolyte layer, and A3 represents the content of the durability improving agent in the third electrolyte layer.
[0060] In a preferred embodiment of the present invention, the composite electrolyte membrane for PEMFC of the present invention can satisfy the following condition (3).
[0061]
number
[0062] In a preferred embodiment of the present invention, the composite electrolyte membrane for PEMFC of the present invention can satisfy the following condition (4).
[0063]
number
[0064] Yet another object of the present invention relates to a membrane-electrode assembly for PEMFC comprising a composite electrolyte membrane containing the high durability enhancing agent, which may comprise an anode (oxidation electrode); the composite electrolyte membrane for PEMFC; and a cathode (reduction electrode). Effect of the Invention
[0065] The high durability improving agent of the present invention not only acts as an antioxidant, which has a radical scavenger effect, but also acts as an antioxidant that reduces gas permeability, so it has an excellent effect of improving the durability of the electrolyte membrane without the need to add a separate radical scavenger, and the radical scavenger addition process may be omitted when producing the electrolyte membrane. The composite electrolyte membrane for PEMFC produced by introducing such a high durability improving agent of the present invention has a thin thickness, yet is excellent in durability and dimensional stability, as well as high tensile strength and excellent performance, and therefore a membrane-electrode assembly for PEMFC with excellent long-term stability and high efficiency, and a fuel cell incorporating the same can be produced. [Brief description of the drawings]
[0066] [Figure 1a] FIG. 1a is a schematic diagram of a composite electrolyte membrane for a PEMFC according to a preferred embodiment of the present invention. [Figure 1b] FIG. 1b is a schematic diagram of a composite electrolyte membrane for a PEMFC according to a preferred embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a composite electrolyte membrane for a PEMFC according to another preferred embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram of a composite electrolyte membrane for a PEMFC according to yet another preferred embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram of a composite electrolyte membrane for a PEMFC according to yet another preferred embodiment of the present invention. [Diagram 5] FIG. 5 is a schematic diagram of a membrane-electrode assembly for PEMFC according to a preferred embodiment of the present invention. [Figure 6] FIG. 6 is a graph showing the results of OCV measurements of Example 1, Examples 3 and 4, and Comparative Example 1 carried out in Experimental Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0067] Hereinafter, the embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily carry out the present invention. The present invention may be embodied in various different forms and is not limited to the embodiments described herein. In the drawings, parts that are not related to the description will be omitted in order to clearly explain the present invention, and the same reference numerals will be used throughout the specification to refer to the same or similar components.
[0068] The durability improver for PEMFC electrolyte membrane of the present invention prevents the electrolyte membrane from being deteriorated by radicals generated during the operation of the PEMFC, and plays a role in increasing the durability of the electrolyte membrane. Such a durability improver of the present invention is in the form of a composite powder, and includes platinum (Pt) and a carrier carrying the platinum. Such a composite type durability improver of the present invention simultaneously performs the function of a radical scavenger, which is a function of a primary antioxidant, and the function of decomposing hydrogen peroxide, which is a function of a secondary antioxidant, and also performs the function of gas decomposition and / or gas barrier, and the function of an electron conductor.
[0069] The high durability improver may contain 0.01-6.00% by weight of platinum particles and the remaining amount of a carrier, preferably 0.01-5.50% by weight of platinum particles and the remaining amount of a carrier, more preferably 0.10-5.00% by weight of platinum particles and the remaining amount of a carrier. In this case, if the platinum particle content is less than 0.01% by weight based on the total weight of the high durability improver, the radical scavenging function may be insufficient, which may reduce the deterioration prevention effect, and if the platinum particle content exceeds 6.00% by weight, the deterioration prevention efficiency may be reduced due to side reactions other than the hydrogen peroxide decomposition effect, so it is better to use it within the above range.
[0070] In the high durability improving agent of the present invention, nano-sized platinum particles are bound to the surface of the carrier and integrated therewith. For example, platinum particles can be bound to the surface of the carrier by vapor deposition.
[0071] The particle size of the platinum particles (D 50 ) is 0.1 to 50 nm, preferably 0.1 to 30 nm, and more preferably 3.0 to 20.0 nm. 50 If the particle size of platinum particles (D 50 If the diameter exceeds 50 nm, there may be problems of a reduction in the reaction area and aggregation of platinum particles.
[0072] The support may contain one or more selected from CeO2, GDC (Gd doped Ceria), IrO2, SnO2, and Ti4O7.
[0073] CeO2, GDC, IrO2, SnO2, and Ti4O7 are good catalyst materials for oxygen generation reaction, and when used as a carrier in a high-voltage acidic environment, they have excellent stability and high electrical conductivity, and are stable materials in a high-voltage acidic environment, and when used as a carrier, they can increase the dispersion of Pt. In addition, they are specialized materials for preventing carbon corrosion by decomposing water when reverse voltage occurs due to a lack of fuel while the fuel cell is running, and when water in the electrode blocks the pores or when the fuel cell is turned on and off, a situation occurs where there is insufficient fuel supply, and in this case, CeO2, IrO2, SnO2, and Ti4O7 can play a role in increasing the durability and stability of the fuel cell.
[0074] Moreover, the GDC (Gd doped ceria) is an oxide in which gadolinium (Gd) is doped into a ceria lattice, and may be a compound represented by the following chemical formula (1).
[0075] [ka]
[0076] In Chemical Formula (1), x is an integer satisfying 0 < x ≤ 0.3, preferably 0 < x ≤ 0.25, more preferably 0 < x ≤ 0.20, and y is the oxygen vacancy value that makes the compound electrically neutral and is an integer satisfying 0 < y ≤ 0.25.
[0077] The durability improver of the present invention has nano-sized platinum powder bonded and integrated on the surface of the carrier. For example, the platinum powder can be deposited and bonded on the surface of the carrier.
[0078] And the optimal content of platinum particles in the high-durability improver may vary slightly depending on the type of the carrier.
[0079] When the carrier is CeO2, the platinum particle content may be 0.01 to 6.00% by weight, preferably 0.1 to 5.5% by weight, more preferably 0.5 to 5.5% by weight based on the total weight of the high-durability improver.
[0080] Also, when the carrier is IrO2, the platinum particle content may be 0.01 to 4.50% by weight, preferably 0.1 to 3.5% by weight, more preferably 0.5 to 3.0% by weight based on the total weight of the high-durability improver.
[0081] Also, when the carrier is SnO2, the platinum particle content may be 0.01 to 3.00% by weight, preferably 0.1 to 2.5% by weight, more preferably 0.3 to 2.0% by weight based on the total weight of the high-durability improver.
[0082] Also, when the carrier is Ti4O7, the platinum particle content may be 0.01 to 5.50% by weight, preferably 0.1 to 4.5% by weight, more preferably 0.5 to 3.5% by weight based on the total weight of the high-durability improver.
[0083] In addition, the high durability improving agent of the present invention can use a single type of composite (platinum particles + support), or can use two types of composites to obtain the same or even better durability improving effect while using less or the same amount as that of a single type of composite.
[0084] As a specific example, the durability improving agent of the present invention may contain two or more of the above-mentioned complexes, or may contain a cerium-based complex and a non-cerium-based complex, or preferably may contain a cerium-based complex and a non-cerium-based complex in a weight ratio of 1:0.1 to 50.
[0085] As yet another specific example, the high durability improving agent may contain two or more of the above complexes, may contain a cerium-based complex and a gadolinium-based support complex, and preferably may contain a cerium-based complex and a gadolinium-based complex in a weight ratio of 1:0.05 to 10.
[0086] In this case, the cerium-based composite means a composite containing the platinum particles and CeO2 supporting the platinum particles as a carrier, and the non-cerium-based composite means a composite containing the platinum particles and a carrier containing one or more selected from IrO2, SnO2 and Ti4O7. And, as the gadolinium-based carrier composite, the GDC composite means a composite containing platinum (Pt) particles and the GDC (Gd doped Ceria) carrier represented by the chemical formula (1) supporting the platinum particles.
[0087] The carrier has a particle size (D 50 ) may be 10 to 2,000 nm, preferably 10 to 1,000 nm, more preferably 50 to 800 nm, and even more preferably 50 to 650 nm. 50 If the particle size of the support (D 50 ) exceeds 2,000 nm, there may be a problem of a reduced reaction area.
[0088] The high durability improving agent of the present invention has a BET surface area of 10 to 500 m 2 / g, preferably 80 to 400m 2 / g, more preferably 90 to 250m 2 / g.
[0089] Hereinafter, a PEMFC electrolyte membrane using the durability improving agent of the present invention will be described.
[0090] The electrolyte membrane for PEMFC of the present invention may have a single-layer structure or a multi-layer structure, and an example of the multi-layer structure may be a composite electrolyte membrane as shown below. In this case, the electrolyte layers of the composite electrolyte membrane may be formed from the electrolyte membrane forming solution or from electrolyte membrane forming solutions of other compositions.
[0091] Referring to FIG. 1a, the composite electrolyte membrane for a PEMFC (Polymer Electrolyte Membrane Fuel Cell) of the present invention has a structure in which a first electrolyte layer 21, a first support layer 11, and a second electrolyte layer 22 are laminated in sequence, and at least one of the first electrolyte layer and / or the second electrolyte layer may contain the durability improving agent described above.
[0092] In addition, at least one layer selected from the first electrolyte layer and the second electrolyte layer may further include a cerium (Ce)-based radical scavenger.
[0093] When the composite electrolyte membrane for PEMFC is applied to a membrane-electrode assembly for PEMFC, it is an electrolyte membrane in which a first electrolyte layer, a first support layer, and a second electrolyte layer are sequentially laminated from the anode direction to the cathode direction, and may contain a durability improver in the electrolyte layer so as to satisfy the following condition (2). Since the role and effect of the durability improver is greater in the cathode than in the anode, it is advantageous to satisfy the following condition (2) in terms of the performance and durability of the PEMFC membrane-electrode assembly.
[0094] Condition (2) A1≦A2 In the condition (2), A1 represents the content of the durability improver in the first electrolyte layer, and A2 represents the content of the durability improver in the second electrolyte layer.
[0095] Also, referring to FIG. 1b, the composite electrolyte membrane for a PEMFC (Polymer Electrolyte Membrane Fuel Cell) of the present invention may have a structure in which a first electrolyte layer 21, a first support layer 11, a second electrolyte layer 22, a second support layer 12, and a third electrolyte layer 23 are sequentially laminated.
[0096] Specifically, the PEMFC composite electrolyte membrane of the present invention may include a first electrolyte layer 21, a first support layer 11 formed on one side of the first electrolyte layer 21, a second electrolyte layer 22 formed on one side of the first support layer 11, a second support layer 12 formed on one side of the second electrolyte layer 22, and a third electrolyte layer 23 formed on one side of the second support layer 12. Any one or more of the first to third electrolyte layers may contain the durability improving agent described above.
[0097] When the composite electrolyte membrane for PEMFC is applied to a membrane-electrode assembly for PEMFC, it is a composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer and a third electrolyte layer are laminated in order from the anode direction to the cathode direction, and may satisfy the following condition (5) or condition (6). Satisfying the following condition (5) or condition (6) is advantageous from the viewpoint of optimizing the effect of the durability improving agent for the PEMFC membrane-electrode assembly.
[0098] Condition (5) A1≦A2≦A3 Condition (6) A2≦A1, A2≦A3, A1≦A3 In the above conditions (5) and (6), A1 represents the content of the durability improving agent in the first electrolyte layer, A2 represents the content of the durability improving agent in the second electrolyte layer, and A3 represents the content of the durability improving agent in the third electrolyte layer.
[0099] Also, referring to FIG. 2, the composite electrolyte membrane for PEMFC of the present invention may have a structure in which a first electrolyte layer 21, a first support layer 11, a second electrolyte layer 22, a second support layer 12, a third electrolyte layer 23, a third support layer 13 and a fourth electrolyte layer 24 are laminated in sequence.
[0100] Specifically, the composite electrolyte membrane for PEMFC of the present invention may include a first electrolyte layer 21, a first support layer 11 formed on one side of the first electrolyte layer 21, a second electrolyte layer 22 formed on one side of the first support layer 11, a second support layer 12 formed on one side of the second electrolyte layer 22, a third electrolyte layer 23 formed on one side of the second support layer 12, a third support layer 13 formed on one side of the third electrolyte layer 23, and a fourth electrolyte layer 24 formed on one side of the third support layer 13.
[0101] Also, referring to FIG. 3, the composite electrolyte membrane for PEMFC of the present invention may have a structure in which a fifth electrolyte layer 25, a fourth support layer 14, a first electrolyte layer 21, a first support layer 11, a second electrolyte layer 22, a second support layer 12, a third electrolyte layer 23, a third support layer 13 and a fourth electrolyte layer 24 are laminated in sequence.
[0102] Specifically, the composite electrolyte membrane for PEMFC of the present invention may include a fifth electrolyte layer 25, a fourth support layer 14 formed on one side of the fifth electrolyte layer 25, a first electrolyte layer 21 formed on one side of the fourth support layer 14, a first support layer 11 formed on one side of the first electrolyte layer 21, a second electrolyte layer 22 formed on one side of the first support layer 11, a second support layer 12 formed on one side of the second electrolyte layer 22, a third electrolyte layer 23 formed on one side of the second support layer 12, a third support layer 13 formed on one side of the third electrolyte layer 23, and a fourth electrolyte layer 24 formed on one side of the third support layer 13. In this case, the fourth support layer 13 may be the same as the first support layer 11, the second support layer 12, and / or the third support layer 13 described above, and the fifth electrolyte layer 25 may be the same as the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23, and / or the fourth electrolyte layer 24 described above.
[0103] In addition, the composite electrolyte membrane for PEMFC may have only one support layer formed between the first electrolyte layer and the second electrolyte layer, between the second electrolyte layer and the third electrolyte layer, or between the third electrolyte layer and the fourth electrolyte layer. As a preferred embodiment, as shown in the schematic diagram of FIG. 4, the composite electrolyte membrane may include a first electrolyte layer 21, a second electrolyte layer 22 formed on one side of the first electrolyte layer, a support layer 11 formed on one side of the second electrolyte layer 22, a third electrolyte layer 23 formed on one side of the support layer 11, and a fourth electrolyte layer 24 formed on one side of the third electrolyte layer 23.
[0104] The first support layer, second support layer, and third support layer of the present invention may each use a common porous support used in the industry, and preferably may include a PTFE (Polytetrafluoroethylene) porous support having specific physical properties manufactured by the manufacturing method described below.
[0105] The PTFE porous support of the present invention can be manufactured by carrying out a process including: step 1-1 of mixing and stirring PTFE powder and a lubricant to prepare a paste; step 1-2 of maturing the paste; step 1-3 of extruding and rolling the matured paste to prepare a green tape; step 1-4 of drying the green tape and then removing the liquid lubricant; step 1-5 of uniaxially stretching the green tape from which the lubricant has been removed; step 1-6 of biaxially stretching the uniaxially stretched green tape; and step 1-7 of firing.
[0106] In step 1-1, the paste may contain 15 to 35 parts by weight, preferably 15 to 30 parts by weight, and more preferably 15 to 25 parts by weight of a lubricant relative to 100 parts by weight of the PTFE powder. If the amount of the lubricant is less than 15 parts by weight relative to 100 parts by weight of the PTFE powder, the porosity may be reduced when the PTFE porous support is formed by the biaxial stretching process described below, and if the amount of the lubricant is more than 35 parts by weight, the pore size may be large when the PTFE porous support is formed, and the strength of the support may be weakened.
[0107] The average particle size of the PTFE powder may be, but is not limited to, 300 μm to 800 μm, preferably 450 μm to 700 μm. The lubricant may be, as a liquid lubricant, a hydrocarbon oil such as liquid paraffin, naphtha, white oil, toluene, xylene, or various alcohols, ketones, esters, etc., and preferably one or more selected from liquid paraffin, naphtha, and white oil.
[0108] Next, the aging in the 1-2 step is a preforming process, and the paste can be aged for 12 to 24 hours at a temperature of 30° C. to 70° C., and preferably for 16 to 20 hours at a temperature of 35° C. to 60° C. If the aging temperature is less than 35° C. or the aging time is less than 12 hours, the lubricant coating on the surface of the PTFE powder becomes non-uniform, which may limit the stretching uniformity of the PTFE porous support during biaxial stretching described below.
[0109] In addition, if the aging temperature exceeds 70° C. or the aging time exceeds 24 hours, the pore size of the PTFE porous support after the biaxial stretching process may become very small due to evaporation of the lubricant.
[0110] Next, in the extrusion of the first to third steps, the matured paste is compressed by a compressor to produce a PTFE block, and then the PTFE block is compressed at a pressure of 0.069 to 0.200 Ton / cm 2 Preferably, the pressure is 0.090 to 0.175 Ton / cm 2 The extrusion can be carried out by pressure extrusion at a pressure of 1000 MPa.
[0111] At this time, the pressurized extrusion pressure is 0.069 Ton / cm 2 If it is less than 0.200 Ton / cm, the pore size of the porous support may become large and the strength of the porous support may become weak. 2 If it exceeds this value, there may be a problem that the pore size of the porous support after the biaxial stretching step becomes small.
[0112] In addition, the rolling in steps 1-3 can be performed as a calendar process at an oil pressure of 5-10 MPa and at 50-100° C. In this case, if the oil pressure is less than 5 MPa, the pore size of the porous support may become large, weakening the strength of the porous support, whereas if the oil pressure exceeds 10 MPa, the pore size of the porous support may become small.
[0113] Next, the drying in steps 1-4 can be performed by a general drying method used in the art, and in one preferred example, the rolling-prepared unsintered tape can be transported on a conveyer belt at a temperature of 100° C. to 200° C. and a speed of 1 to 5 m / min, preferably at a temperature of 140° C. to 190° C. and a speed of 2 to 4 m / min. In this case, if the drying temperature is 100° C. or lower or the drying speed exceeds 5 m / min, air bubbles may be generated during the stretching process due to non-evaporation of the lubricant, and if the drying temperature is 200° C. or higher or the drying speed is less than 1 m / min, the stiffness of the dried tape increases and slip may occur during the stretching process.
[0114] Next, the uniaxial stretching in the 1-5th step is a process of stretching the unsintered tape from which the lubricant has been removed in the length direction, and the uniaxial stretching is performed by using the speed difference between the rollers when transporting the tape through rollers. The uniaxial stretching is performed by stretching the unsintered tape from which the lubricant has been removed in the length direction by 3 to 10 times, preferably 6 to 9.5 times, more preferably 6.2 to 9 times, and even more preferably 6.3 to 8.2 times. In this case, if the uniaxial stretching ratio is less than 3 times, sufficient mechanical properties cannot be secured, and if the uniaxial stretching ratio exceeds 10 times, the mechanical properties are rather reduced and the pores of the support may become very large.
[0115] In addition, the uniaxial stretching is preferably performed at a stretching temperature of 260°C to 350°C and a stretching speed of 6 to 12 M (meter) / min, and preferably at a stretching temperature of 270°C to 330°C and a stretching speed of 8 to 11.5 M / min. If the stretching temperature is less than 260°C or the stretching speed is less than 6 M / min during uniaxial stretching, the heat applied to the dry sheet increases, which may cause a problem of a baked section occurring. If the stretching temperature exceeds 350°C or the stretching speed exceeds 12 M / min during uniaxial stretching, slip occurs during the uniaxial stretching process, which may cause a problem of reduced thickness uniformity.
[0116] Next, the biaxial stretching in the 1-6th step may be performed by stretching the uniaxially stretched unsintered tape in the width direction (perpendicular to the uniaxial stretching) and then stretching the tape in the lateral direction while the end of the tape is fixed. However, the stretching is not limited thereto, and the tape may be stretched by a stretching method commonly used in the art. In the present invention, the biaxial stretching may be performed in the width direction at a ratio of 15 to 50 times, preferably 25 to 45 times, more preferably 28 to 45 times, and even more preferably 29 to 42 times. In this case, if the biaxial stretching ratio is 15 times or less, sufficient mechanical properties may not be secured, and if it exceeds 50 times, not only is there no improvement in mechanical properties, but there may also be a problem of deterioration in the uniformity of physical properties in the length direction and / or width direction, so it is better to perform the stretching within the above range.
[0117] In addition, the biaxial stretching is preferably performed at a stretching temperature of 150°C to 260°C and a stretching speed of 10 to 20 M / min, and preferably at a stretching temperature of 200°C to 250°C and a stretching speed of 11 to 18 M / min. If the biaxial stretching temperature is less than 150°C or the stretching speed is less than 10 M / min, there may be a problem of reduced stretching uniformity in the transverse direction, and if the biaxial stretching temperature exceeds 260°C or the stretching speed exceeds 20 M / min, there may be a problem of unbaked areas occurring and reduced physical properties.
[0118] Finally, the calcination in the 1st to 7th steps may be performed by moving the stretched porous support on a conveyer belt at a speed of 10 to 18 M / min, preferably 13 to 17 M / min, while applying a temperature of 350°C to 450°C, preferably 380°C to 440°C, more preferably 400°C to 435°C, thereby fixing the stretch ratio and improving the strength. If the calcination temperature is less than 350°C, the strength of the porous support may be reduced, and if it exceeds 450°C, there may be a problem that the physical properties of the support are reduced due to a reduction in the number of fibrils caused by excessive calcination.
[0119] Furthermore, the PTFE porous support produced by carrying out steps 1-7 of the process may have a uniaxial (length direction) and biaxial (width direction) stretch ratio (or aspect ratio) of 1:3.00 to 8.5, preferably 1:4.0 to 7.0, more preferably 1:4.00 to 5.50, and even more preferably 1:4.20 to 5.00. It is preferable that the uniaxial and biaxial stretch ratios (or aspect ratios) are within the above ranges from the viewpoints of high mechanical properties, ensuring an appropriate pore size in the support, and ensuring appropriate current flow.
[0120] The produced PTFE porous support of the present invention may have an average pore size of 0.080 μm to 0.200 μm, preferably 0.090 μm to 0.180 μm, more preferably 0.095 μm to 0.150 μm, and even more preferably 0.100 to 0.140 μm. The PTFE porous support of the present invention may have an average porosity of 60% to 90%, more preferably 60% to 79.6%.
[0121] If the average pore size of the PTFE porous support of the present invention is less than 0.080 μm or the porosity is less than 60%, the degree of impregnation of the electrolyte in the PTFE porous support may be limited when the PTFE porous support is impregnated with an electrolyte to manufacture an electrolyte membrane. Also, if the average pore size exceeds 0.200 μm or the porosity exceeds 90%, the structure of the PTFE porous support may be deformed during impregnation with the electrolyte, resulting in a decrease in dimensional stability and a decrease in product life.
[0122] In addition, the PTFE porous support of the present invention can have uniaxial modulus and biaxial modulus values that satisfy the following equation 1 when measured based on ASTM D 882.
[0123] [Equation 1] 0≦|(1-axis direction modulus-2-axis direction modulus) / (1-axis direction modulus)×100%|≦54%, preferably 0≦|(1-axis direction modulus-2-axis direction modulus) / (1-axis direction modulus)×100%|≦40%, more preferably 1≦|(1-axis direction modulus-2-axis direction modulus) / (1-axis direction modulus)×100%|≦26% The PTFE porous support of the present invention may have a uniaxial (lengthwise) modulus of 40 MPa or more, preferably a uniaxial modulus of 50 MPa or more, more preferably a uniaxial modulus of 48 to 75 MPa, and even more preferably a uniaxial modulus of 65 to 75 MPa, when measured according to ASTM D 882. The biaxial (widthwise) modulus may be 40 MPa or more, preferably a biaxial (widthwise) modulus of 55 MPa or more, more preferably a biaxial (widthwise) modulus of 46 to 75 MPa, and even more preferably a uniaxial (widthwise) modulus of 55 to 75 MPa.
[0124] The PTFE porous support of the present invention may have a uniaxial (lengthwise) tensile strength of 40 MPa or more and a biaxial (widthwise) tensile strength of 40 MPa or more, preferably a uniaxial tensile strength of 50 MPa or more, more preferably a uniaxial tensile strength of 54 to 65 MPa, when measured according to ASTM D882, and may have a biaxial tensile strength of 52 MPa or more, more preferably a biaxial tensile strength of 52 to 70 MPa.
[0125] The first support layer, second support layer, and third support layer of the present invention can each have a thickness of 0.1 to 10 μm, preferably a thickness of 1 to 7 μm, more preferably a thickness of 1 to 5 μm, even more preferably a thickness of 1.5 to 4 μm, and even more preferably a thickness of 1.5 to 2.5 μm. If the thickness is less than 0.1 μm, there may be a problem of reduced tensile strength, and if it exceeds 10 μm, there may be a problem that it is difficult to make the film thin.
[0126] The first electrolyte layer, the second electrolyte layer, the third electrolyte layer and / or the fourth electrolyte layer may each independently include the high durability improving agent, and the content of the high durability improving agent may be different for each electrolyte layer. For example, when the PEMFC composite electrolyte membrane is a composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer and a third electrolyte layer are sequentially stacked from an anode electrode to a cathode electrode; or a composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer, a third electrolyte layer, a third support layer and a fourth electrolyte layer are sequentially stacked from an anode electrode to a cathode electrode, the content of the high durability improving agent in the electrolyte layer may be adjusted so that the content of the high durability improving agent in the electrolyte layer decreases with increasing distance from the cathode electrode, thereby forming a gradient in which the content of the high durability improving agent in the electrolyte layer decreases based on the cathode electrode.
[0127] As a preferred example, the content of the high durability improving agent may be adjusted so that the weight ratio of the content of the high durability improving agent among the fourth electrolyte layer, the third electrolyte layer, the second electrolyte layer, and the first electrolyte layer is 1:0.1-0.99:0-0.80:0-0.70, thereby producing a composite electrolyte membrane.
[0128] Next, each of the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23 and the fourth electrolyte layer 24 of the present invention may contain an ionomer including one or more selected from a perfluorinated sulfonated ionomer (PFSA ionomer) and a hydrocarbon-based ionomer.
[0129] The perfluorinated sulfonated ionomer of the present invention may comprise one or more selected from Nafion, Flemion, aquivion and Aciplex, and preferably comprises aquivion.
[0130] The hydrocarbon-based ionomer may include at least one selected from a polyaryl ether sulfone (PAES)-based material, a polyether ether ketone (PEEK)-based material, and a polyimide (PI)-based material.
[0131] The ionomer may not only constitute each of the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23 and the fourth electrolyte layer 24, but may also be contained within the pores of the first support layer 11 and / or the second support layer 12.
[0132] Each of the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23 and the fourth electrolyte layer 24 of the present invention may contain a durability improving agent, and the durability improving agent includes platinum (Pt) and a carrier supporting the platinum, as described above.
[0133] In addition, when preparing an electrolyte solution for forming an electrolyte layer (or electrolyte membrane), the electrolyte solution may contain 0.01 to 20% by weight of the durability improver and the remaining amount of the ionomer, preferably 0.1 to 10% by weight of the durability improver and the remaining amount of the ionomer, more preferably 0.1 to 1.0% by weight of the durability improver and the remaining amount of the ionomer. In this case, if the content of the durability improver is less than 0.01% by weight, the amount used is too small and there may be no effect of preventing deterioration of the electrolyte layer (or electrolyte membrane), and if the content of the durability improver exceeds 20% by weight, there may be a problem that the ion conductivity decreases as it acts as an impurity, so it is better to use it within the above range.
[0134] In addition, each of the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23 and the fourth electrolyte layer 24 may further include a radical scavenger for PEMFC in addition to the ionomer and the durability improver.
[0135] The radical scavenger for PEMFC of the present invention is [Zn(OH)4] 2- The CeZnO metal oxide particles having a ZnO crystal structure doped with cerium ions can be produced by mixing the Ce precursor aqueous solution with the containing solution and carrying out a reduction reaction. Here, "ZnO crystal structure doped with Ce ions" means that a new crystal structure is formed in which some of the Zn atoms are replaced with Ce atoms in a ZnO crystal structure having a crystal structure such as wurtzite.
[0136] More specifically, the Zn precursor is dissolved in alcohol to prepare a Zn precursor solution, and then the Zn precursor solution is heated to form a first step; [Zn(OH)4] 2- The second step is to prepare a solution containing [Zn(OH)4] 2-A radical scavenger for PEMFC can be manufactured by carrying out a process including a third step of mixing a Ce precursor aqueous solution with the containing solution and carrying out a reduction reaction to form CeZnO metal oxide particles having a ZnO crystal structure doped with Ce ions, a fourth step of recovering and washing the CeZnO metal oxide particles, and a fifth step of drying the washed CeZnO metal oxide particles. For more detailed description of this, Korean Patent Registration No. 10-1860870 by the same applicant may be incorporated by reference.
[0137] The radical scavenger for PEMFC of the present invention is a metal oxide particle having a crystal structure composed of cerium (Ce) atoms, zinc (Zn) atoms, and oxygen (O) atoms, and as a preferred example, may have a crystal structure in which a portion of the Zn atoms in a ZnO crystal structure having a crystal structure such as wurtzite is substituted with Ce atoms.
[0138] The radical scavenger for PEMFC of the present invention may also contain one or more selected from CeZnO, CeO2, Ru, Ag, RuO2, WO3, Fe3O4, CePO4, CrPO4, AlPO4, FePO4, CeF3, FeF3, Ce2(CO3)3·8H2O, Ce(CHCOO)3·H2O, CeCl3·6H2O, Ce(NO3)6·6H2O, Ce(NH4)2(NO3)6, Ce(NH4)4(SO4)4·4H2O and Ce(CH3COCHCOCH3)3·3H2O.
[0139] The radical scavenger for PEMFC of the present invention may contain 12 to 91% by weight of Ce, 7 to 84.5% by weight of Zn, and the balance O (oxygen atom), or preferably, 13.40 to 89.20% by weight of Ce, 7.55 to 88.20% by weight of Zn, and the balance O. It may further contain other inevitable impurities.
[0140] In addition, the radical scavenger of the present invention can be measured for particle size (D) using a nano particle size analyzer using the DLS (Dynamic Light Scattering) method. 50) During analysis, the wavelength may be 500 nm or less, preferably 300 nm or less, and more preferably 200 to 300 nm.
[0141] Each of the first electrolyte layer, the second electrolyte layer, the third electrolyte layer and the fourth electrolyte layer of the present invention may contain 0.001 to 10 parts by weight, preferably 0.01 to 10 parts by weight, more preferably 0.1 to 8 parts by weight of a radical scavenger for PEMFC relative to 100 parts by weight of the perfluorinated sulfonated ionomer. If the amount is less than 0.001 part by weight, there may be a problem that durability is poor, whereas if the amount exceeds 10 parts by weight, durability is improved but ion conductivity is reduced, which may be a problem that the performance of the composite electrolyte membrane of the present invention is reduced.
[0142] In addition, each of the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23 and the fourth electrolyte layer 24 may further contain hollow silica and / or the above-mentioned radical scavenger for PEMFC in addition to the ionomer and the high durability improving agent.
[0143] The hollow silica may be spherical and have an average particle size of 10 to 300 nm, more preferably 10 to 100 nm. Here, the particle size means the diameter when the hollow silica has a spherical shape, and when the shape is not spherical, means the maximum linear distance from any one point to any other point on the surface of the hollow silica.
[0144] In addition, each of the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23 and the fourth electrolyte layer 24 of the present invention may further contain one or more absorbents selected from zeolite, titania, zirconia and montmorillonite.
[0145] Each of the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23 and the fourth electrolyte layer 24 of the present invention can have a thickness of 1 to 10 μm, preferably a thickness of 1 to 8 μm, more preferably a thickness of 2 to 5 μm, and even more preferably a thickness of 2.5 to 4.5 μm. If the thickness is less than 1 μm, there may be a problem of reduced tensile strength, and if it exceeds 10 μm, there may be a problem of being disadvantageous in making the film thin.
[0146] Furthermore, each of the first electrolyte layer 21, the second electrolyte layer 22, the third electrolyte layer 23 and the fourth electrolyte layer 24 of the present invention may have an equivalent weight (EW) of the -SO3H group of 1,100 or less, preferably 900 or less, more preferably 500 to 900, even more preferably 600 to 830, and even more preferably 680 to 750. If the equivalent weight of the -SO3H group exceeds 1,100, there may be a problem of reduced performance.
[0147] Furthermore, the PEMFC composite electrolyte membrane of the present invention may have a dimensional change rate in the MD direction (=length direction) measured by the following relational formula 1 of 10% or less, preferably 0 to 5%, more preferably 0 to 3%, and even more preferably 0.5 to 2%, and may have a dimensional change rate in the TD direction (=width direction) measured by the following relational formula 1 of 10% or less, preferably 2 to 8%, more preferably 3 to 7%, and even more preferably 4 to 6%.
[0148]
number
[0149] In the above Relational Formula 1, A represents the initial length of the PEMFC composite electrolyte membrane, and B represents the length measured after leaving the PEMFC composite electrolyte membrane at a temperature of 80° C. for 20 minutes.
[0150] Thus, the composite electrolyte membrane for PEMFC of the present invention exhibits a low rate of dimensional change not only in the MD direction but also in the TD direction, and is therefore remarkably excellent in dimensional stability.
[0151] The composite electrolyte membrane for PEMFC of the present invention may have an average thickness of 5 to 30 μm, preferably 7 to 20 μm, more preferably 10 to 18 μm, and even more preferably 12 to 16 μm. Despite its thin thickness, it is excellent in durability and dimensional stability, and also has high tensile strength and excellent performance.
[0152] Furthermore, when the PEMFC composite electrolyte membrane of the present invention is an electrolyte membrane in which a first electrolyte layer, a first support layer, and a second electrolyte layer are laminated in this order, it can satisfy the following condition (1).
[0153] Condition (1) B1≦A1, B1≦A2 In the above condition (1), A1 represents the thickness of the first electrolyte layer, A2 represents the thickness of the second electrolyte layer, and B1 represents the thickness of the first support layer.
[0154] In addition, when the composite electrolyte membrane for PEMFC of the present invention is a composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer, and a third electrolyte layer are laminated in order, it can satisfy all of the following conditions (3) and (4).
[0155] Condition (3) B1≦A1, B1≦A2, B1≦A3 Condition (4) B2≦A1, B2≦A2, B2≦A3 In the condition (3), A1 represents the thickness of the first electrolyte layer 21, A2 represents the thickness of the second electrolyte layer 22, A3 represents the thickness of the third electrolyte layer 23, and B1 represents the thickness of the first support layer 11, and in the condition (4), A1 represents the thickness of the first electrolyte layer 21, A2 represents the thickness of the second electrolyte layer 22, A3 represents the thickness of the third electrolyte layer 23, and B2 represents the thickness of the second support layer 12.
[0156] If the PEMFC composite electrolyte membrane of the present invention does not satisfy both of the conditions (3) and (4), there may be a problem of reduced uniformity.
[0157] In addition, the composite electrolyte membrane for PEMFC of the present invention satisfies the value of condition (7).
number
[0158] Condition (7) 1.5≦value of condition (7)≦12, preferably 1.5≦value of condition (7)≦9, more preferably 2≦value of condition (7)≦7, even more preferably 2.2≦value of condition (7)≦5, and even more preferably 2.5≦value of condition (7)≦3.0. In the above condition (7), A1 represents the thickness of the first electrolyte layer 21, A2 represents the thickness of the second electrolyte layer 22, A3 represents the thickness of the third electrolyte layer 23, B1 represents the thickness of the first support layer 11, and B2 represents the thickness of the second support layer 12.
[0159] If the value of condition (7) is less than 1.5, a composite electrolyte membrane may not be produced, whereas if it exceeds 12, durability may decrease.
[0160] In addition, the composite electrolyte membrane for PEMFC of the present invention satisfies the value of condition (8).
number
[0161] Condition (8): 0.2≦value of condition (8)≦10, preferably 0.5≦value of condition (8)≦8, more preferably 1.0≦value of condition (8)≦6, and even more preferably 1.5≦value of condition (8)≦4. In the condition (8), A1 represents the thickness of the first electrolyte layer 21, A2 represents the thickness of the second electrolyte layer 22, and A3 represents the thickness of the third electrolyte layer .
[0162] If the value of condition (8) is less than 0.2, there may be a problem of reduced durability, and if it exceeds 10, there may be a problem of reduced performance.
[0163] [Manufacturing method of composite electrolyte membrane for PEMFC] The method for producing the PEMFC composite electrolyte membrane of the present invention can include a process including the first to fourth stages.
[0164] First, in the first step of the manufacturing method of the PEMFC composite electrolyte membrane of the present invention, a first support layer and a second support layer can be prepared. At this time, a PTFE (Poly tetra fluoro ethylene) porous support can be used as the first support layer and the second support layer, and the PTFE porous support that can be used is the same as the PTFE porous support and the manufacturing method thereof described above.
[0165] Next, in the second step of the manufacturing method of the composite electrolyte membrane for PEMFC of the present invention, a first electrolyte layer may be formed on one side of the first support layer prepared in the first step, and a third electrolyte layer may be formed on one side of the second support layer prepared in the first step.
[0166] Specifically, in the second step of the manufacturing method for the PEMFC composite electrolyte membrane of the present invention, the ionomer mixed solution may be applied to one side of the first support layer, or the one side of the first support layer may be impregnated with the ionomer mixed solution, and then dried to form the first electrolyte layer.
[0167] Also, the third electrolyte layer can be formed by applying the ionomer mixed solution to one surface of the second support layer, or by impregnating one surface of the second support layer with the ionomer mixed solution and then drying it.
[0168] The second drying step can be carried out by applying heat at 60° C. to 200° C. for 1 minute to 30 minutes, or preferably by applying heat at 70° C. to 150° C. for 15 minutes to 25 minutes. If the drying temperature is less than 60° C., the liquid retention of the ionomer-containing solution impregnated into the first support layer and / or the second support layer may decrease, whereas if the temperature exceeds 200° C., the adhesion to the electrodes during the production of the electrolyte membrane and / or the membrane-electrode assembly may decrease.
[0169] Next, in the third step of the method for manufacturing a PEMFC composite electrolyte membrane of the present invention, a second electrolyte layer may be formed on the other surface of the first support layer prepared in the first step.
[0170] Specifically, the third step is a process of forming a second electrolyte layer on the other side of the first support layer on which the first electrolyte layer has been formed. The second electrolyte layer can be formed by applying an ionomer mixed solution to the other side of the first support layer or by impregnating the other side of the first support layer with the ionomer mixed solution and then drying it.
[0171] The third drying step can be carried out by applying heat at 60° C. to 200° C. for 1 minute to 30 minutes, or preferably by applying heat at 70° C. to 150° C. for 5 minutes to 15 minutes. If the drying temperature is less than 60° C., the liquid retention of the ionomer mixed solution impregnated into the first support layer may decrease, whereas if the temperature exceeds 200° C., the bonding with the electrodes during the production of the electrolyte membrane and / or membrane-electrode assembly may decrease.
[0172] The ionomer mixed solution in the second and third steps may contain an ionomer including at least one selected from perfluorinated sulfonated ionomers and hydrocarbon-based ionomers; and the durability improver described above.
[0173] The ionomer mixed solution may further contain at least one selected from the radical scavenger, hollow silica, and absorbent.
[0174] Finally, in the fourth step of the manufacturing method for the composite electrolyte membrane for PEMFC of the present invention, the second electrolyte layer is laminated on the other side of the second support layer prepared in the first step, and heat-treated to manufacture the composite electrolyte membrane for PEMFC of the present invention in which the first electrolyte layer, the first support layer, the second electrolyte layer, the second support layer, and the third electrolyte layer are laminated in sequence.
[0175] Specifically, the fourth step is a process of stacking and integrating a first support layer having a first electrolyte layer formed on one side and a second electrolyte layer formed on the other side with a second support layer having a third electrolyte layer formed on one side, and the second electrolyte layer formed on the other side of the first support layer and the second support layer are stacked so as to be in contact with each other, and heat-treated to produce the composite electrolyte membrane for PEMFC of the present invention in which the first electrolyte layer, the first support layer, the second electrolyte layer, the second support layer and the third electrolyte layer are stacked in sequence.
[0176] The fourth stage heat treatment can be carried out at 100°C to 200°C for 1 to 20 minutes, preferably at 140°C to 180°C for 1 to 15 minutes. If the heat treatment temperature is less than 100°C or the heat treatment time is less than 1 minute, the liquid retention of the first electrolyte layer, the second electrolyte layer and / or the third electrolyte layer may decrease, and if the heat treatment temperature exceeds 200°C, the adhesion (bonding) between the first, second and third electrolyte layers and the first and second support layers may decrease.
[0177] The first support layer and / or the second support layer of the composite electrolyte membrane that has been subjected to the fourth heat treatment may have a volume of blocked pores of 85 vol. % or more, preferably 90 vol. % or more, relative to the total pore volume.
[0178] [Membrane-electrode assembly for PEMFC] 5A and 5B, the membrane-electrode assembly for PEMFC of the present invention includes an anode (oxidation electrode) 200, the above-described composite electrolyte membrane for PEMFC of the present invention 100, and a cathode (reduction electrode) 300.
[0179] A membrane-electrode assembly according to one embodiment of the present invention (A in FIG. 5) includes an anode (oxidation electrode) 200 and a cathode (reduction electrode) 300 positioned opposite each other with a composite electrolyte membrane 100 sandwiched therebetween. In this case, the anode 200 may include an anode gas diffusion layer 3, an anode catalyst layer 2, and an anode electrode substrate 1, and the cathode 300 may include a cathode gas diffusion layer 4, a cathode catalyst layer 5, and a cathode electrode substrate 6.
[0180] Specifically, the anode 200 may be formed by sequentially stacking an anode gas diffusion layer 3, an anode catalyst layer 2, and an anode electrode substrate 1, and the anode gas diffusion layer 3 may be bonded to one side of the composite electrolyte membrane 200. The cathode 300 may be formed by sequentially stacking a cathode gas diffusion layer 4, a cathode catalyst layer 5, and a cathode electrode substrate 6, and the cathode gas diffusion layer 4 may be bonded to the other side of the composite electrolyte membrane 200.
[0181] In addition, the anode 200 of the membrane-electrode assembly (FIG. 5B) according to one embodiment of the present invention may include an anode gas diffusion layer 3 and an anode electrode substrate 1, and the cathode 300 may include a cathode gas diffusion layer 4 and a cathode electrode substrate 6. In this case, the anode electrode substrate may be formed of an anode catalytic electrode, and the cathode electrode substrate may be formed of a cathode catalytic electrode.
[0182] The membrane-electrode assembly of the present invention can be formed by arranging the anode 200, the composite electrolyte membrane 100, and the cathode 300, and then fastening them together, or by compressing them under high temperature and pressure.
[0183] The anode gas diffusion layer 3 can be formed by coating one surface of the composite electrolyte membrane 100 with a gas diffusion layer forming material, or by coating one surface of the anode electrode substrate 1 with a gas diffusion layer forming material.
[0184] The anode gas diffusion layer 3 may be provided to prevent the rapid diffusion of fuel injected into the fuel cell and to prevent a decrease in ion conductivity. The anode gas diffusion layer 3 may be subjected to a heat treatment or an electrochemical treatment to adjust the diffusion rate of the fuel. The anode gas diffusion layer 3 serves as a current conductor between the PEMFC composite electrolyte membrane 100 and the anode catalyst layer 2, and serves as a passage for gas as a reactant and water as a product. Therefore, the anode gas diffusion layer 3 may have a porous structure with a porosity of 20% to 90% so that gas can easily pass through. The thickness of the anode gas diffusion layer 3 may be appropriately selected as necessary, and may be, for example, 100 to 400 μm. If the thickness of the anode gas diffusion layer 3 is 100 μm or less, the electrical contact resistance between the anode catalyst layer 2 and the anode electrode substrate 1 may increase, and the structure may become unstable due to compression. If the thickness of the anode gas diffusion layer 3 is more than 400 μm, the movement of the reactant gas may become difficult.
[0185] The anode gas diffusion layer 3 may be formed including a carbon-based material and a fluororesin. The carbon-based material may include, but is not limited to, one or more selected from the group consisting of graphite, carbon black, acetylene black, denka black, ketjen black, activated carbon, porous hollow carbon, carbon nanotube, carbon nanofiber, carbon nanohorn, carbon nanoring, carbon nanowire, fullerene (C60) and super P. The fluororesin may include, but is not limited to, one or more selected from the group consisting of polytetrafluoroethylene, polyvinylidene fluoride (PVdF), polyvinyl alcohol, cellulose acetate, polyvinylidene fluoride-hexafluoropropylene copolymer, or styrene-butadiene rubber (SBR). The fuel may be a liquid fuel such as a formic acid solution, methanol, formaldehyde, or ethanol.
[0186] The anode catalyst layer 2 is a layer in which an oxidation catalyst is introduced. The anode catalyst layer 2 can be formed by applying a catalyst layer forming material onto the anode gas diffusion layer 3. The catalyst layer forming material may be a metal catalyst or a metal catalyst supported on a carbon-based support. The metal catalyst may be at least one selected from the group consisting of platinum, ruthenium, platinum-ruthenium alloy, platinum-osmium alloy, platinum-palladium alloy, and platinum-transition metal alloy. The carbon-based support may include at least one selected from the group consisting of graphite, carbon black, acetylene black, denka black, ketjen black, activated carbon, porous hollow carbon, carbon nanotube, carbon nanofiber, carbon nanohorn, carbon nanoring, carbon nanowire, fullerene, and super P.
[0187] The anode catalyst layer 2 may also include a conductive support and an ion-conductive binder (not shown). In addition, the anode catalyst layer 2 may include a main catalyst attached to a conductive support. The conductive support may be carbon black, and the ion-conductive binder may be Nafion ionomer or a sulfonated polymer. The main catalyst may also be a metal catalyst, for example, platinum (Pt). The anode catalyst layer 2 may be formed using an electroplating method, a spraying method, a painting method, a doctor blade method, or a transfer method.
[0188] The anode electrode substrate 1 may be a conductive substrate selected from the group consisting of carbon paper, carbon cloth, and carbon felt, but is not limited thereto, and may be any anode electrode material applicable to a polymer electrolyte fuel cell. The anode electrode substrate 1 may be formed on one side of the anode catalyst layer 2 by a conventional deposition method, or may be formed by forming the anode catalyst layer 2 on the anode electrode substrate 1 and then arranging the anode catalyst layer 2 and the anode electrode substrate 1 on the anode gas diffusion layer 3 so that they are in contact with each other (see FIG. 5A). Alternatively, the anode gas diffusion layer 3 may be formed on one side of the anode electrode substrate 1 (see FIG. 5B).
[0189] The cathode gas diffusion layer 4 may be formed by applying a gas diffusion layer forming material to the other surface of the composite electrolyte membrane 100 or by applying a gas diffusion layer forming material to one surface of the cathode electrode substrate 6 .
[0190] The cathode gas diffusion layer 4 may be provided to prevent the gas injected into the cathode 300 from diffusing rapidly and to uniformly disperse the gas injected into the cathode 300. The cathode gas diffusion layer 4 also serves as a current conductor between the PEMFC composite electrolyte membrane 100 and the cathode catalyst layer 5, and serves as a passage for the gas as a reactant and water as a product. Therefore, the cathode gas diffusion layer 4 may have a porous structure with a porosity of 20% to 90% so that the gas can easily pass through. The thickness of the cathode gas diffusion layer 4 may be appropriately selected as necessary, and may be, for example, 100 to 400 μm. If the thickness of the cathode gas diffusion layer 4 is 100 μm or less, the electrical contact resistance between the cathode catalyst layer 5 and the cathode electrode substrate 6 increases, and the structure may become unstable due to compression. If the thickness of the cathode gas diffusion layer 4 is more than 400 μm, the movement of the gas as a reactant may become difficult.
[0191] The cathode gas diffusion layer 4 may be formed to include a carbon-based material and a fluororesin. The carbon-based material may include, but is not limited to, one or more selected from the group consisting of graphite, carbon black, acetylene black, denka black, ketjen black, activated carbon, porous hollow carbon, carbon nanotube, carbon nanofiber, carbon nanohorn, carbon nanoring, carbon nanowire, fullerene (C60) and super P. The fluororesin may include, but is not limited to, one or more selected from the group consisting of polytetrafluoroethylene, polyvinylidene fluoride (PVdF), polyvinyl alcohol, cellulose acetate, polyvinylidene fluoride-hexafluoropropylene copolymer, or styrene-butadiene rubber (SBR). The fuel may be a liquid fuel such as a formic acid solution, methanol, formaldehyde, or ethanol.
[0192] The cathode catalyst layer 5 is a layer in which a reduction catalyst is introduced, and the cathode catalyst layer 5 can be formed by applying a catalyst layer forming material onto the cathode gas diffusion layer 4 .
[0193] The catalyst layer forming material may be a metal catalyst or a metal catalyst supported on a carbon-based support. The metal catalyst may be at least one selected from the group consisting of platinum, ruthenium, platinum-ruthenium alloy, platinum-osmium alloy, platinum-palladium alloy, and platinum-transition metal alloy. The carbon-based support may include at least one selected from the group consisting of graphite, carbon black, acetylene black, denka black, ketjen black, activated carbon, porous hollow carbon, carbon nanotube, carbon nanofiber, carbon nanohorn, carbon nanoring, carbon nanowire, fullerene, and super P.
[0194] The cathode catalyst layer 5 may also include a conductive support and an ion-conductive binder (not shown). In addition, the cathode catalyst layer 5 may include a main catalyst attached to the conductive support. The conductive support may be carbon black, and the ion-conductive binder may be Nafion ionomer or a sulfonated polymer. The main catalyst may also be a metal catalyst, for example, platinum (Pt). The cathode catalyst layer 5 may be formed using an electroplating method, a spraying method, a painting method, a doctor blade method, or a transfer method.
[0195] The cathode electrode substrate 6 may be a conductive substrate selected from the group consisting of carbon paper, carbon cloth, and carbon felt, but is not limited thereto, and any cathode electrode material applicable to a polymer electrolyte fuel cell may be used. The cathode electrode substrate 6 may be formed on one side of the cathode catalyst layer 5 by a conventional deposition method, or may be formed by forming the cathode catalyst layer 5 on the cathode electrode substrate 6 and then arranging the cathode catalyst layer 5 and the cathode electrode substrate 6 on the cathode gas diffusion layer 4 so that they are in contact with each other (see FIG. 5A). Alternatively, the cathode gas diffusion layer 4 may be formed on one side of the cathode electrode substrate 6 (see FIG. 5B).
[0196] In addition, a polymer electrolyte membrane fuel cell according to an embodiment of the present invention includes at least one electricity generating unit that generates electrical energy through an oxidation reaction of a fuel and a reduction reaction of an oxidant, a fuel supplying unit that supplies the fuel to the electricity generating unit, and an oxidant gap unit that supplies an oxidant to the electricity generating unit.
[0197] An electricity generating unit may be configured by including one or more membrane-electrode assemblies of the present invention and disposing separators for supplying fuel and oxidant to both ends of the membrane-electrode assemblies of the present invention. At least one such electricity generating unit may be assembled to form a stack.
[0198] In this regard, the arrangement or manufacturing method of the polymer electrolyte membrane fuel cell of the present invention can be formed without any restrictions as long as it is applicable to a polymer electrolyte fuel cell, and therefore can be applied in various ways with reference to the prior art.
[0199] The present invention will be described in more detail with reference to the following examples. However, it should be understood that the following examples are not intended to limit the scope of the present invention, but are intended to aid in the understanding of the present invention.
[0200] [Example] Example 1: Preparation of durability improver (Pt / GDC) and electrolyte membrane forming solution (1) Manufacturing of durability improvers A method of preparing gadolinium-doped ceria (GDC) represented by the following chemical formula (1-1) as a carrier was used. A mixed solution of a cerium precursor (cerium nitrate) and a gadolinium precursor (gadolinium nitrate) was dropped into an aqueous solution under certain environmental conditions to obtain a coprecipitate. At this time, the particle size (D 50 ) of the carrier was 180 nm.
[0201]
Chemical formula
[0202] In Chemical formula (1-1), x is 0.1, and y is the oxygen vacancy value that makes the compound electrically neutral, and is an integer that satisfies 0 < y ≤ 0.25.
[0203] Next, platinum in the precursor state was prepared. After mixing the carrier therewith, a step of inducing a reduction reaction from platinum in the precursor state to platinum metal in the nanoparticle state using a reducing agent was performed to produce a durability improver (Pt / GDC) in which platinum nanoparticles were deposited and integrated on the surface of the carrier.
[0204] The content of platinum nanoparticles in the produced durability improver was 0.10% by weight, and the average particle size (D 50 ) of the platinum powder was about 17 nm.
[0205] (2) Preparation of electrolyte membrane forming solution A perfluorosulfonic acid-based ionomer (trade name: Aquivion® D72-25DS, manufactured by Solvay) with an equivalent weight of -SO3H group of 720 was prepared.
[0206] 0.5% by weight of the durability improver (Pt / GDC), 0.97% by weight of a radical scavenger (CeZnO), and the balance of the ionomer were mixed to produce an electrolyte membrane forming solution.
[0207] Example 2: Preparation of durability improver (Pt / GDC) and electrolyte membrane forming solution (1) Preparation of durability improver The durability improver was produced in the same manner as in Example 1, except that the durability improver was produced using GDC represented by the following chemical formula (1-2) as a carrier.
[0208] [Chemical formula]
[0209] In Chemical formula (1-2), x is 0.2, y is the oxygen vacancy value that makes the compound electrically neutral, and is an integer satisfying 0 < y ≤ 0.25.
[0210] (2) Preparation of the electrolyte membrane forming solution Using the same perfluorosulfonic acid-based ionomer as in Example 1, 0.5% by weight of the durability improver (Pt / GDC) and the balance of the ionomer were mixed to prepare an electrolyte membrane forming solution.
[0211] Example 3: Preparation of the durability improver (Pt / CeO2) and the electrolyte membrane forming solution (1) Preparation of the durability improver CeO2 with a particle size (D 50 ) of 177 nm was prepared as a carrier, and the same platinum precursor as used in Example 1 was prepared.
[0212] Next, platinum in the precursor state was prepared, and after mixing the carrier therewith, a step of inducing a reduction reaction from platinum in the precursor state to platinum metal in the nanoparticle state using a reducing agent was performed to produce a durability improver (Pt / CeO2) in which platinum nanoparticles were deposited and integrated on the surface of the carrier.
[0213] The content of platinum nanoparticles in the produced durability improver was 0.10% by weight, and the average particle size (D 50 ) of the platinum powder was about 15 nm.
[0214] (2) Preparation of the electrolyte membrane forming solution Using the same perfluorosulfonic acid-based ionomer as in Example 1, 0.5% by weight of the durability improver (Pt / CeO2) and the balance of the ionomer were mixed to prepare an electrolyte membrane forming solution.
[0215] Example 4: Preparation of durability improver (Pt / IrO2) and electrolyte membrane forming solution (1) Durability improver manufacturing Particle size (D 50 ) was prepared as a support, and the platinum precursor used in Example 1 was prepared.
[0216] Next, platinum in precursor form was prepared and mixed with the carrier. After that, a reducing agent was used to induce a reduction reaction from the platinum in precursor form to platinum metal in nanoparticle form, producing a durability improver (Pt / IrO2) in which platinum nanoparticles were deposited and integrated on the surface of the carrier.
[0217] The content of platinum nanoparticles in the durability improver produced was 0.10 wt %, and the average particle size of the platinum powder (D 50 ) was approximately 25 nm.
[0218] (2) Preparation of electrolyte membrane forming solution The same perfluorosulfonic acid-based ionomer as in Example 1 was used and mixed with 0.5 wt % of the durability improver (Pt / IrO2) and the remaining amount of the ionomer to prepare an electrolyte membrane forming solution.
[0219] Comparative Example 1 No high durability improving agent was used, and the perfluorosulfonic acid-based ionomer of Example 1 itself was prepared as an electrolyte membrane forming solution.
[0220] Examples 5 to 8 and Comparative Examples 2 to 6 The durability improver and the electrolyte membrane forming solution were prepared in the same manner as in Example 1, but the durability improver or its content was varied as shown in Table 1 below to prepare the electrolyte membrane forming solutions.
[0221] [Table 1]
[0222] Experimental Example 1: Evaluation of durability of electrolyte membrane and analysis of fluoride ion release rate In order to evaluate the durability of the electrolyte membrane, each of the electrolyte membrane forming solutions prepared in Examples 1 to 8 and Comparative Examples 2 to 6 was coated on a film and then dried to prepare a single-layer electrolyte membrane having a thickness of 10 um.
[0223] (1) Measurement of fluoride ion release rate (FER, umol / g h) A pentone solution was prepared by mixing ferrous sulfate hydrate and hydrogen peroxide, and the electrolyte membranes prepared in the examples and comparative examples were placed in the pentone solution and left at 80° C. for 120 hours, after which the fluorine ion release rate was measured. The electrolyte membrane was deteriorated by the radicals in the pentone solution, resulting in the release of fluorine ions (F - ) and the durability was evaluated by measuring the fluorine ion concentration in the pentone solution. The results are shown in Table 2 below.
[0224] Moreover, the OCV measurement graphs of Example 1, Examples 3 and 4, and Comparative Example 1 are shown in FIG.
[0225] (2) OCV (open circuit voltage) holding durability test A catalyst and a gas diffusion layer (GDL) were attached to each of the electrolyte membranes of the examples and comparative examples to prepare membrane-electrode assemblies, and the open circuit voltage (OCV) was measured under conditions (90°C / relative humidity 30%) that are more severe than the actual cell operating conditions. The results are shown in Table 2 below.
[0226] [Table 2]
[0227] The measurement results of the fluorine ion release rate in Table 2 show that the electrolyte membrane of Comparative Example 1 showed a high fluorine ion release rate of about 15.1 umol / g·h. In contrast, the electrolyte membrane of Example 3, in which Pt / CeO2 was used as a durability improver, showed a fluorine ion release rate of 2.45 umol / g·h, and the electrolyte membranes of Examples 1 and 4, in which Pt / GDC and Pt / IrO2 were used as durability improvers, showed fluorine ion release rates of 1.83 umol / g·h and 2.81 umol / g·h, respectively, and it was confirmed that the fluorine ion release rate was significantly reduced by using the durability improver.
[0228] Also, looking at the measurement results of OCV (open circuit voltage) holding durability in Table 2, differences in degradation (voltage drop) between each Example and Comparative Example after long-term operation were confirmed. Also, referring to Fig. 5, Comparative Example 1, in which a high durability improving agent was not applied, experienced a rapid voltage drop and reached the end of its life after 318 hours, while Example 3 (Pt / CeO2) showed durability performance of over 914 hours, Example 1 (Pt / GDC) showed durability of over 1,027 hours, and Example 4 (Pt / IrO2) showed durability of over 851 hours.
[0229] In the case of Comparative Example 2, in which the Pt content in the durability improving agent exceeded 6.0 wt%, there was a problem that the FER value increased and the life time was shortened compared to Example 5, and in the case of Comparative Example 3, in which the Pt content in the durability improving agent was less than 0.01 wt%, there was a problem that the FER value was high and the life time was also significantly shortened compared to Example 6 (Pt 0.05 wt%).
[0230] Furthermore, in the case of Comparative Example 4, in which the average particle size of Pt in the durability improving agent exceeded 100 nm, and in the case of Comparative Example 5, in which the average particle size of the carrier in the durability improving agent exceeded 1000 nm, the durability was actually decreased and the FER value was high compared to Example 4.
[0231] In addition, in the case of Comparative Example 6, in which the content of the durability improver in the electrolyte forming solution exceeded 20.0 wt %, the results showed that there was no benefit from using an excessive amount of the durability improver.
[0232] Example 9-1: Preparation of high durability improver (Pt / CeO2 composite) and electrolyte membrane forming solution (1) Manufacturing of high durability improvers Particle size (D 50 ) was prepared using CeO2 with a diameter of 177 nm as a support.
[0233] Next, platinum in a precursor state was prepared, and the CeO2 support was mixed therewith. A process was then carried out in which a reducing agent was used to induce a reduction reaction from the platinum in the precursor state to platinum metal in a nanoparticle state, thereby producing a high durability improving agent (Pt / CeO2 composite) in which platinum nanoparticles were deposited and integrated on the surface of the support.
[0234] The platinum nanoparticle content in the manufactured high durability improving agent was 0.10 wt %, and the average particle size of the platinum particles (D 50 ) was approximately 5 nm.
[0235] (2) Preparation of electrolyte membrane forming solution A perfluorinated sulfonic acid ionomer (product name: Aquivion (registered trademark) D72-25DS, Solvay) having an equivalent weight of -SO3H group of 720 was prepared.
[0236] 0.5 wt % of the high durability improver (Pt / CeO2 composite) and the remaining amount of the ionomer were mixed to prepare an electrolyte membrane forming solution.
[0237] Examples 9-2 to 9-4 and Comparative Examples 7-1 to 7-2 The electrolyte membrane forming solution was prepared in the same manner as in Example 9-1, but the electrolyte membrane forming solution was prepared so that the platinum particle content of the high durability improving agent (Pt / CeO2 composite) was 1.0 wt%, 3.0 wt%, and 5.5 wt%, as shown in Table 3 below, and Examples 9-2 to 9-4 were carried out.
[0238] However, in Comparative Example 7-1, no platinum particles were used, and only CeO2 was used as the durability improving agent, and in Comparative Example 7-2, a high durability improving agent was produced so that the platinum particles were contained at 6.0 wt %.
[0239] Example 10-1: Preparation of high durability improver (Pt / IrO2 composite) and electrolyte membrane forming solution (1) Manufacturing of high durability improvers Particle size (D 50 ) was prepared as a carrier, and the platinum precursor used in Example 9-1 was prepared.
[0240] Next, platinum in precursor form was prepared and mixed with the carrier. After that, a reducing agent was used to induce a reduction reaction from the platinum in precursor form to platinum metal in nanoparticle form, producing a high durability improving agent (Pt / IrO2 composite) in which platinum nanoparticles were deposited and integrated onto the surface of the carrier.
[0241] The platinum nanoparticle content in the manufactured high durability improving agent was 1.0 wt %, and the average particle size of the platinum particles (D 50 ) was approximately 12 nm.
[0242] (2) Preparation of electrolyte membrane forming solution The same perfluorosulfonic acid-based ionomer as in Example 9-1 was used and mixed with 0.5 wt % of the high durability improver (Pt / IrO2 composite) and the remaining amount of the ionomer to prepare an electrolyte membrane forming solution.
[0243] Example 10-2 A high durability improver (Pt / IrO2 composite) was prepared in the same manner as in Example 10-1, except that the high durability improver was prepared so that the platinum content was 0.1 wt %. Then, 0.5 wt % of the high durability improver (Pt / IrO2 composite) and the remaining amount of the ionomer were mixed to prepare an electrolyte membrane forming solution.
[0244] Example 11-1: Preparation of high durability improver (Pt / SnO2 composite) and electrolyte membrane forming solution (1) Manufacturing of high durability improvers Particle size (D 50 ) of 353 nm was prepared as a support, and the platinum precursor used in Example 9-1 was prepared.
[0245] Next, platinum in precursor form was prepared and mixed with the carrier. After that, a reducing agent was used to induce a reduction reaction from the platinum in precursor form to platinum metal in nanoparticle form, producing a high durability improving agent (Pt / SnO2 composite) in which platinum nanoparticles were deposited and integrated on the surface of the carrier.
[0246] The platinum nanoparticle content in the manufactured high durability improving agent was 1.0 wt %, and the average particle size of the platinum particles (D 50 ) was approximately 9 nm.
[0247] (2) Preparation of electrolyte membrane forming solution The same perfluorosulfonic acid-based ionomer as in Example 9-1 was used and mixed with 0.5 wt % of the high durability improver (Pt / SnO2 composite) and the remaining amount of the ionomer to prepare an electrolyte membrane forming solution.
[0248] Example 11-2 A high durability improver (Pt / SnO2 composite) was prepared in the same manner as in Example 11-1, except that the platinum content was adjusted to 0.1 wt %. Then, 0.5 wt % of the high durability improver (Pt / SnO2 composite) and the remaining amount of the ionomer were mixed to prepare an electrolyte membrane forming solution.
[0249] Example 12-1: Preparation of high durability improver (Pt / Ti4O7 composite) and electrolyte membrane forming solution (1) Manufacturing of high durability improvers Particle size (D 50 ) of 502 nm was prepared as a support, and the platinum precursor used in Example 1 was prepared.
[0250] Next, platinum in precursor form was prepared and mixed with the carrier. After that, a reducing agent was used to induce a reduction reaction from the platinum in precursor form to platinum metal in nanoparticle form, producing a high durability improving agent (Pt / Ti4O7 composite) in which platinum nanoparticles were deposited and integrated onto the surface of the carrier.
[0251] The platinum nanoparticle content in the manufactured high durability improving agent was 1.0 wt %, and the average particle size of the platinum particles (D 50 ) was approximately 7 nm.
[0252] (2) Preparation of electrolyte membrane forming solution The same perfluorosulfonic acid-based ionomer as in Example 9-1 was used and mixed with 0.5 wt % of the high durability improver (Pt / Ti4O7 composite) and the remaining amount of the ionomer to prepare an electrolyte membrane forming solution.
[0253] Example 12-2 A high durability improver (Pt / Ti4O7 composite) was prepared in the same manner as in Example 12-2, except that the high durability improver was prepared so that the platinum content was 0.1 wt %. Then, 0.5 wt % of the high durability improver (Pt / Ti4O7 composite) and the remaining amount of the ionomer were mixed to prepare an electrolyte membrane forming solution.
[0254] Example 13 The electrolyte membrane forming solution was prepared in the same manner as in Example 9-1, except that the content of the durability improving agent was adjusted to 17.0 wt %.
[0255] Comparative Examples 7-3 to 7-5 The high durability improving agent and the electrolyte membrane forming solution were prepared in the same manner as in Example 1-1, but the particle size of platinum in the high durability improving agent, the particle size of the carrier, or the content of the high durability improving agent was varied as shown in Table 1 below to prepare the electrolyte membrane forming solutions.
[0256] [Table 3]
[0257] Experimental Example 2: Evaluation of durability of electrolyte membrane and analysis of fluoride ion release rate In order to evaluate the durability of the electrolyte membrane, each of the electrolyte membrane forming solutions prepared in Examples 9-1 to 13 and Comparative Examples 7-1 to 7-5 was coated on a film and then dried to prepare a single-layer electrolyte membrane having a thickness of 10 um.
[0258] The fluorine ion release rate and OCV holding durability were measured in the same manner as in Experimental Example 1, and the results are shown in Table 4 below.
[0259] The control group in Table 4 below is an electrolyte membrane produced without using any platinum catalyst or carrier.
[0260] [Table 4]
[0261] As shown in Table 4, the control electrolyte membrane not using Pt or a carrier exhibited a fluoride ion release rate of about 15.10 umol / g h, while the electrolyte membrane of Comparative Example 7-1 using only a carrier exhibited a high fluoride ion release rate of about 9.21 umol / g h.
[0262] In contrast, the electrolyte membranes of Examples 9-1 to 9-4, which used Pt / CeO2 as a high durability improving agent, were confirmed to have a very low fluoride ion release rate (FER) of 3.50 umol / g h or less. Examples 10-1 to 10-2, 11-1 to 11-2, and 12-1 to 12-2, which were manufactured using IrO2, SnO2, or Ti4O7 as the carrier, respectively, also showed excellent results in terms of FER reduction.
[0263] In general, the results showed that the FER (fluorine ion release rate) decreased as the platinum content in the high durability improving agent increased, but in the case of Comparative Example 7-2, in which 6.0 wt% of CeO2 was used as a carrier, the FER reduction effect did not increase compared to Example 9-4.
[0264] Also, looking at the OCV (open circuit voltage) holding durability measurement results in Table 4, it was possible to confirm the difference in degradation (voltage drop) between the examples and the comparative example after long-term operation.
[0265] In the case of Comparative Example 7-2, in which the Pt content in the high durability improving agent exceeded 5.5% by weight, there was a problem that the FER value increased and the life time was shortened compared to Example 9-4, and in the case of Comparative Example 7-1, in which no Pt was used in the high durability improving agent, there was a problem that the FER value was high and the life time was also significantly shortened.
[0266] In addition, in the case of Comparative Example 7-3, in which the particle size of the platinum particles in the high durability improving agent exceeded 50 nm, there was a problem that the Pt specific surface area was smaller compared to the same Pt content, and since the size of the Pt particles and the carrier particle size were similar, the Pt particles were located on the carrier and aggregated with each other, resulting in a decrease in durability efficiency and a decrease in the electrochemical performance of the cell during long-term operation.
[0267] In addition, in the case of Comparative Example 7-4, in which the average particle size of the carrier in the high durability improving agent exceeded 2,000 nm, the carrier particle size was large, and as a result, the nano-sized Pt particles did not disperse uniformly due to the low specific surface area, resulting in problems such as a decrease in the efficiency of Pt reaction characteristics and Pt aggregation, resulting in poor durability and electrochemical performance.
[0268] In addition, in the case of Comparative Example 7-5 in which the content of the high durability improving agent in the electrolyte forming solution exceeded 20.0 wt %, the results showed that there was no benefit from using an excessive amount of the high durability improving agent.
[0269] Examples 10-3 to 10-4 and Comparative Examples 8-1 to 8-2 The same carrier as in Example 10-1 was used, but the Pt particle content was varied as shown in Table 5 below to prepare a high durability improver (Pt / IrO2). Then, 0.5 wt % of the high durability improver (Pt / IrO2) and the remaining amount of the ionomer were mixed using the above to prepare an electrolyte membrane forming solution.
[0270] Experimental Example 3: Evaluation of durability of electrolyte membrane and analysis of fluoride ion release rate Using the electrolyte membrane forming solutions prepared in Examples 10-3 to 10-4 and Comparative Examples 8-1 to 8-2, single-layer electrolyte membranes having a thickness of 10 um were prepared in the same manner as in Experimental Example 1, and then the FER and OCV were measured. The results are shown in Table 5 below.
[0271] [Table 5]
[0272] From Table 5, it was confirmed that the appropriate content of Pt nanoparticles in the composite when IrO2 is used as a carrier is 0.01 to 4.5 wt%.
[0273] Examples 11-3 to 11-4 and Comparative Examples 9-1 to 9-2 The same carrier as in Example 11-1 was used, but the Pt particle content was varied as shown in Table 6 below to prepare a high durability improver (Pt / SnO2). Then, 0.5 wt % of the high durability improver (Pt / SnO2) and the remaining amount of the ionomer were mixed using the above to prepare an electrolyte membrane forming solution.
[0274] Experimental Example 4: Evaluation of electrolyte membrane durability and analysis of fluoride ion release rate Using the electrolyte membrane forming solutions prepared in Examples 11-3 to 11-4 and Comparative Examples 9-1 to 9-2, single-layer electrolyte membranes having a thickness of 10 um were prepared in the same manner as in Experimental Example 1, and then the FER and OCV were measured. The results are shown in Table 6 below.
[0275] [Table 6]
[0276] From Table 6, it was confirmed that the appropriate content of Pt nanoparticles in the composite when SnO2 is used as a carrier is 0.01 to 3.0 wt%.
[0277] Examples 12-3 to 12-4 and Comparative Examples 10-1 to 10-2 The same carrier as in Example 12-1 was used, but the Pt particle content was varied as shown in Table 7 below to prepare a high durability improver (Pt / IrO2), which was then mixed with 0.5 wt% of a high durability improver (Pt / Ti4O7) and the remaining amount of the ionomer to prepare an electrolyte membrane forming solution.
[0278] Experimental Example 5: Evaluation of durability of electrolyte membrane and analysis of fluoride ion release rate Using the electrolyte membrane forming solutions prepared in Examples 12-3 to 12-4 and Comparative Examples 10-1 to 10-2, single-layer electrolyte membranes having a thickness of 10 um were prepared in the same manner as in Experimental Example 1, and then the FER and OCV were measured. The results are shown in Table 7 below.
[0279] [Table 7]
[0280] From the OCV final life and voltage performance values in Table 7, it was confirmed that the appropriate content of Pt nanoparticles in the composite is 0.01 to 5.50 wt % when Ti4O7 is used as the carrier.
[0281] Example 14 The composite prepared in Example 9-1 and the composite prepared in Example 10-1 were mixed in a weight ratio of 1:0.3, and 0.5 wt % of a high durability improver and the remaining amount of the ionomer were mixed to prepare an electrolyte membrane forming solution.
[0282] Example 15 (1) Preparation of Pt / GDC composite GDC, represented by the following chemical formula (1-1), was prepared as a carrier by dropping a mixed solution of a cerium precursor (cerium nitrate) and a gadolinium precursor (gadolinium nitrate) into an aqueous solution under certain environmental conditions to obtain a coprecipitate. 50 ) was 180 nm.
[0283] [Chemical formula]
[0284] In Chemical formula (1-1), x is 0.1, y is the oxygen vacancy value that makes the compound electrically neutral, and is an integer satisfying 0 < y ≤ 0.25.
[0285] Next, platinum in the precursor state was prepared, a carrier was mixed therewith, and then a step of inducing a reduction reaction from platinum in the precursor state to platinum metal in the nanoparticle state using a reducing agent was performed to produce a Pt / GDC composite in which platinum nanoparticles were deposited and integrated on the surface of the carrier.
[0286] The content of platinum nanoparticles in the produced Pt / GDC composite was 0.1% by weight, and the average particle size (D 50 ) of the platinum powder was about 5 nm.
[0287] (2) Production of the electrolyte membrane forming solution A high-durability improver of 0.5% by weight and the balance of the ionomer were mixed with the composite produced in Example 9-1 and the Pt / GDC composite at a weight ratio of 1:0.3 to produce an electrolyte membrane forming solution.
[0288] Experimental Example 6: Evaluation of the durability of the electrolyte membrane and analysis experiment of the fluorine ion release rate After producing electrolyte membranes having a single-layer structure with a thickness of 10 μm in the same manner as in Experimental Example 1 using the electrolyte membrane forming solutions produced in Examples 14 to 15, FER and OCV were measured, and the results are shown in Table 8 below.
[0289] [Table 8]
[0290] Referring to Table 8 above, it was confirmed that Examples 14 and 15 in which two types of composites were used in combination had a more excellent durability improvement effect because only one type of high-durability improver was used.
[0291] Production Example 1-1: Production of PTFE porous support 100 parts by weight of PTFE fine powder having an average particle size of 570 μm was mixed with 23 parts by weight of naphtha as a liquid lubricant, and stirred to uniformly disperse the powder into a paste.
[0292] Next, the paste was left to stand at 50° C. for 18 hours to mature, and then compressed using a molding jig to produce a PTFE block.
[0293] Next, the PTFE block is put into an extrusion die and then compressed at about 0.10 Ton / cm 2 Pressurized extrusion was carried out under pressure.
[0294] Next, the mixture was rolled using a rolling roll to produce a green tape having an average thickness of 850 μm.
[0295] Next, the unsintered tape was transported on a conveyor belt at a speed of 3 M / min, while being heated at 180° C. to dry it and remove the lubricant.
[0296] Next, the unsintered tape from which the lubricant had been removed was uniaxially stretched (lengthwise stretched) at a stretching temperature of 280° C. and a stretching speed of 10 M / min at a magnification of 6.5 times.
[0297] Next, the uniaxially stretched unsintered tape was biaxially stretched (widthwise stretched) at a stretching temperature of 250° C. and a stretching speed of 10 M / min at a magnification of 30 times to produce a porous support.
[0298] Next, the uniaxially and biaxially stretched porous support was sintered at a temperature of 420°C at a speed of 15M / min on a conveyor belt to produce a PTFE porous support with an average thickness of 16 μm and an average pore size of 0.114 μm.
[0299] Production Example 1-2: Production of PTFE porous support A PTFE porous support was prepared in the same manner as in Preparation Example 1-1. However, unlike Preparation Example 1-1, the uniaxial and biaxial stretching conditions were changed to prepare a PTFE porous support having an average thickness of 5 μm and an average pore size of 0.114 μm.
[0300] Production Example 1-3: Production of PTFE porous support A PTFE porous support was prepared in the same manner as in Preparation Example 1-1. However, unlike Preparation Example 1-1, the uniaxial and biaxial stretching conditions were changed to prepare a PTFE porous support having an average thickness of 12 μm and an average pore size of 0.114 μm.
[0301] Production Example 1-4: Production of PTFE porous support A PTFE porous support was prepared in the same manner as in Preparation Example 1-1. However, unlike Preparation Example 1-1, the uniaxial and biaxial stretching conditions were changed to prepare a PTFE porous support having an average thickness of 3 μm and an average pore size of 0.114 μm.
[0302] Manufacturing Example 2-1: Manufacturing of composite electrolyte membrane for PEMFC (1) Preparation of electrolyte membrane forming solution 0.5 wt% of the durability improver (Pt / GDC) prepared in Example 1 and 95.5 wt% of a perfluorinated sulfonated ionomer (solvay, aquivion D72-25DS) with an equivalent weight of -SO3H group of 720 were mixed to prepare a solution for forming an electrolyte membrane.
[0303] (2) The PTFE porous support produced in Production Example 1-2 was prepared as the first support layer and the second support layer.
[0304] (3) A first support layer was fixed to a glass substrate, and one side of the first support layer was immersed in the electrolyte membrane forming solution using an applicator (Film Applicator), and then dried in a vacuum oven at 80°C for 20 minutes to form a first electrolyte layer having an average thickness of 4 μm on one side of the first support layer.
[0305] (4) A second support layer was fixed to a glass substrate, and one side of the second support layer was immersed in the electrolyte membrane forming solution using an applicator (Film Applicator), and then dried in a vacuum oven at 80°C for 20 minutes to form a third electrolyte layer having an average thickness of 4 μm on one side of the second support layer.
[0306] (5) The other surface of the first support layer having the first electrolyte layer formed on one surface thereof was immersed in the electrolyte membrane forming solution, and then dried in a vacuum oven at 80°C for 20 minutes to form a second electrolyte layer having an average thickness of 3 µm on the other surface of the first support layer.
[0307] (6) The second support layer having the third electrolyte layer formed on one side was laminated on the other side of the second electrolyte layer, and heat-treated at 160°C for 10 minutes to produce a composite electrolyte membrane for PEMFC having an average thickness of 15μm, in which the first electrolyte layer, the first support layer (=thinned to an average thickness of 2μm due to shrinkage during manufacturing), the second electrolyte layer, the second support layer (=thinned to an average thickness of 2μm due to shrinkage during manufacturing), and the third electrolyte layer were laminated in sequence as shown in FIG. 1.
[0308] Manufacturing Example 2-2: Manufacturing of composite electrolyte membrane for PEMFC (1) The PTFE porous support produced in Support Production Example 1-1 was prepared as the first support layer and the second support layer.
[0309] (2) to (4) Using the PTFE porous support of Production Example 1-1 and the electrolyte membrane forming solution produced in Production Example 2-1, a laminate in which a first electrolyte layer-a first support layer-a second electrolyte layer-a second support layer-a third electrolyte layer were laminated was produced, and a first electrolyte layer (average thickness 2.0 μm), a second electrolyte layer (average thickness 1.0 μm), and a third electrolyte layer (average thickness 2.0 μm) were formed.
[0310] (5) Next, the laminate was heat-treated at 160° C. for 10 minutes to produce a composite electrolyte membrane for PEMFC having an average thickness of 15 μm, in which the first electrolyte layer, the first support layer (= thinned to an average thickness of 5 μm due to shrinkage during manufacturing), the second electrolyte layer, the second support layer (= thinned to an average thickness of 5 μm due to shrinkage during manufacturing), and the third electrolyte layer were sequentially laminated as shown in FIG. 1.
[0311] Manufacturing Example 2-3: Manufacturing of composite electrolyte membrane for PEMFC (1) to (4) Using the same PTFE porous support as in Preparation Example 2-2 and the electrolyte membrane forming solution prepared in Preparation Example 2-1, a laminate having a first electrolyte layer-first support layer-second electrolyte layer-second support layer-third electrolyte layer stacked thereon was produced, and each of the first electrolyte layer, second electrolyte layer, and third electrolyte layer was formed so that the average thickness of the entire layer was 1 μm.
[0312] (5) Next, the laminate was heat-treated at 160° C. for 10 minutes to produce a composite electrolyte membrane for PEMFC having an average thickness of 13 μm, in which the first electrolyte layer, the first support layer (= thinned to an average thickness of 5 μm due to shrinkage during manufacturing), the second electrolyte layer, the second support layer (= thinned to an average thickness of 5 μm due to shrinkage during manufacturing), and the third electrolyte layer were laminated in sequence as shown in FIG. 1.
[0313] Manufacturing Example 2-4: Manufacturing of composite electrolyte membrane for PEMFC (1) The PTFE porous support produced in Production Example 1-3 was prepared as a first support layer and a second support layer.
[0314] (2) to (4) Using the PTFE porous support of Production Example 1-3 and the electrolyte membrane forming solution produced in Production Example 2-1, a laminate in which a first electrolyte layer-a first support layer-a second electrolyte layer-a second support layer-a third electrolyte layer were laminated was produced, and a first electrolyte layer (average thickness: 2.5 μm), a second electrolyte layer (average thickness: 2.0 μm), and a third electrolyte layer (average thickness: 2.5 μm) were formed.
[0315] (5) Next, the laminate was heat-treated at 160° C. for 10 minutes to produce a composite electrolyte membrane for PEMFC having an average thickness of 15 μm, in which the first electrolyte layer, the first support layer (= the average thickness of which is thinned to 4 μm due to shrinkage during manufacturing), the second electrolyte layer, the second support layer (= the average thickness of which is thinned to 4 μm due to shrinkage during manufacturing), and the third electrolyte layer were sequentially laminated as shown in FIG. 1.
[0316] Manufacturing Example 2-5: Manufacturing of composite electrolyte membrane for PEMFC (1) The PTFE porous support produced in Production Example 1-4 was prepared as a first support layer and a second support layer.
[0317] (2) to (4) Using the PTFE porous support of Production Example 1-4 and the electrolyte membrane forming solution produced in Production Example 2-1, a laminate having a first electrolyte layer-first support layer-second electrolyte layer-second support layer-third electrolyte layer laminated therein was produced, and the first electrolyte layer (average thickness 5.0 μm), the second electrolyte layer (average thickness 3.0 μm), and the third electrolyte layer (average thickness 5.0 μm) were formed.
[0318] (5) Next, the laminate was heat-treated at 160° C. for 10 minutes to produce a composite electrolyte membrane for PEMFC having an average thickness of 15 μm, in which the first electrolyte layer, the first support layer (= thinned to an average thickness of 1 μm due to shrinkage during manufacturing), the second electrolyte layer, the second support layer (= thinned to an average thickness of 1 μm due to shrinkage during manufacturing), and the third electrolyte layer were sequentially laminated as shown in FIG. 1.
[0319] Comparative Manufacturing Example 2-1: Manufacturing of composite electrolyte membrane for PEMFC (1) Preparation of electrolyte membrane forming solution A solution for forming an electrolyte membrane without using a durability improver was prepared by mixing 95.5 wt% of perfluorinated sulfonated ionomer (solvay, aquivion D72-25DS) with an equivalent weight of 720 of -SO3H group.
[0320] (2) to (4) Using the PTFE porous support of Production Example 1-1 and the electrolyte membrane forming solution produced in Production Example 2-1, a laminate in which a first electrolyte layer-a first support layer-a second electrolyte layer-a second support layer-a third electrolyte layer were laminated was produced, and a first electrolyte layer (average thickness 4.0 μm), a second electrolyte layer (average thickness 3.0 μm), and a third electrolyte layer (average thickness 4.0 μm) were formed.
[0321] (5) Next, the laminate was heat-treated at 160° C. for 10 minutes to produce a composite electrolyte membrane for PEMFC having an average thickness of 15 μm, in which the first electrolyte layer, the first support layer (= thinned to an average thickness of 5 μm due to shrinkage during manufacturing), the second electrolyte layer, the second support layer (= thinned to an average thickness of 5 μm due to shrinkage during manufacturing), and the third electrolyte layer were sequentially laminated as shown in FIG. 1.
[0322] Experimental Example 7: Measurement of physical properties of composite electrolyte membrane for PEMFC (1) Durability measurement experiment (Fenton test) Test pieces of 5 cm x 5 cm (horizontal x vertical) were prepared from each of the composite electrolyte membranes for PEMFC manufactured in Manufacturing Examples 2-1 to 2-5 and Comparative Manufacturing Example 2-1, and the mass was measured after drying in an oven at 80°C for 5 hours or more. The test pieces were then soaked in hydrogen peroxide with a concentration of 2% by volume to obtain Fe. 2+ The specimen was immersed in 200 g of a solution containing 3 ppm of uranium and then left at 80° C. for 120 hours.
[0323] The concentration of fluoride ions eluted from the test piece was measured using a fluoride ion selective electrode, and the results are shown in Table 9 below. In the Penton test, the lower the measured value, the lower the amount of fluoride ions eluted, i.e., the more durable the electrolyte membrane is.
[0324] (2) Dimensional stability measurement experiment Each of the PEMFC composite electrolyte membranes produced in Production Examples 2-1 to 2-5 and Comparative Production Example 2-1 was cut to a size of 5 cm x 1 cm (MD direction x TD direction), and the dimensional change rates in the MD direction (= length direction) and TD direction (= width direction) of each of the cut PEMFC composite electrolyte membranes were measured using the following Relation 1, and the results are shown in Table 9 below.
[0325] [Equation 1] Dimensional change rate (%) = (BA) / AX100 In the above Relational Formula 1, A represents the initial length of the PEMFC composite electrolyte membrane, and B represents the length measured after leaving the PEMFC composite electrolyte membrane at a temperature of 80° C. for 20 minutes.
[0326] In the dimensional change rate experiment, the lower the measured value, the higher the dimensional stability, that is, the better the mechanical properties of the electrolyte membrane.
[0327] (3) Performance measurement experiment Each of the PEMFC composite electrolyte membranes manufactured in Manufacturing Examples 2-1 to 2-5 and Comparative Manufacturing Example 2-1 was cut to 8 cm x 8 cm (MD direction x TD direction), and a PEMFC membrane-electrode assembly including each cut PEMFC composite electrolyte membrane was manufactured as shown in Figure 2. Then, the voltage (V) measured at a current of 1 A under conditions of a temperature of 65°C and a relative humidity of 100% was measured, and the performance was calculated, and the results are shown in Table 9 below.
[0328] (4) Tensile strength measurement experiment The tensile strength of each of the PEMFC composite electrolyte membranes prepared in Preparation Examples 2-1 to 2-5 and Comparative Preparation Example 2-1 was measured according to ASTM D882, and the results are shown in Table 9 below.
[0329] [Table 9]
[0330] As can be seen from Table 9, the PEMFC composite electrolyte membranes manufactured in Manufacturing Examples 2-1 to 2-5 were confirmed to have excellent durability and dimensional stability, as well as high tensile strength and excellent performance. In addition, compared to Comparative Manufacturing Example 2-1, Manufacturing Examples 2-1 to 2-5, which contain a durability improver in the electrolyte layer, were confirmed to have relatively specialized durability.
[0331] Manufacturing Example 3-1: Manufacturing of composite electrolyte membrane for PEMFC A laminate was manufactured in which the thickness of each layer was the same as in Preparation Example 2-1, that is, first electrolyte layer (4 μm)-first support layer (2 μm)-second electrolyte layer (3 μm)-second support layer (2 μm)-third electrolyte layer (4 μm), but the first and second support layers were made of the PTFE porous support manufactured in Preparation Example 1-2.
[0332] As shown in Table 10 below, electrolyte membrane-forming solutions having different contents of the durability improving agent of Example 1 were prepared, and then the first to third electrolyte layers were formed using the solutions to produce composite electrolyte membranes.
[0333] Production Example 3-2 and Comparative Production Examples 3-1 to 3-2 A laminate having a first electrolyte layer (4 μm)-first support layer (2 μm)-second electrolyte layer (3 μm)-second support layer (2 μm)-third electrolyte layer (4 μm) was manufactured using the same electrolyte layer thickness and the same support as in Manufacturing Example 3-1, but the content of the durability improver in the electrolyte membrane-forming solution was varied. Then, composite electrolyte membranes were manufactured by varying the content of the durability improver in the electrolyte layer as shown in Table 10 below, to carry out Manufacturing Example 3-2 and Comparative Manufacturing Examples 3-1 to 3-2.
[0334] Experimental Example 8: Measurement of physical properties of composite electrolyte membrane for PEMFC As shown in the schematic diagram of FIG. 5, a membrane-electrode assembly for PEMFC was manufactured, which included an anode electrode 1, an anode catalyst layer 2, an anode gas diffusion layer 3, a composite electrolyte membrane 100, a cathode gas diffusion layer 4, a cathode catalyst layer 5, and a cathode electrode substrate 6.
[0335] In this case, the composite electrolyte 100 was prepared by using the composite electrolyte membranes of Preparation Examples 2-1, 3-1 to 3-2, and Comparative Preparation Examples 3-1 to 3-2, with the first electrolyte layer facing the anode and the third electrolyte layer facing the cathode.
[0336] The performance and durability measurement results according to the durability improver content and applied design in the produced membrane-electrode assembly are shown in Table 10 below.
[0337] [Table 10]
[0338] As shown in Table 10, all of Preparations 2-1, 3-1, and 3-2 showed excellent durability results. Comparing Preparations 3-1 to 3-2 and Comparative Preparations 3-1 to 3-2, the durability improvement effect was relatively more excellent and the performance was also favorable when the content of the durability improver in each of the first to third electrolytic layers constituting the composite electrolyte increased from the anode direction to the cathode direction (first electrolyte layer<second electrolyte layer<third electrolyte layer) or when the content of the durability improver in the first and second electrolyte layers was higher than that in the second electrolyte layer (second electrolyte layer<first electrolyte layer, third electrolyte layer).
[0339] Production Example 4: Production of composite electrolyte membrane for PEMFC (1) Preparation of electrolyte membrane forming solution 0.5 wt% of the high durability improver (Pt / CeO2) prepared in Example 9-2 and 95.5 wt% of a perfluorinated sulfonated ionomer (solvay, aquivion D72-25DS) with an equivalent weight of -SO3H group of 720 were mixed to prepare a solution for forming an electrolyte membrane.
[0340] (2) The PTFE porous support produced in Production Example 1-2 was prepared as the first support layer and the second support layer.
[0341] (3) A first support layer was fixed to a glass substrate, and one side of the first support layer was immersed in the electrolyte membrane forming solution using an applicator (Film Applicator), and then dried in a vacuum oven at 80°C for 20 minutes to form a first electrolyte layer having an average thickness of 4 μm on one side of the first support layer.
[0342] (4) A second support layer was fixed to a glass substrate, and one side of the second support layer was immersed in the electrolyte membrane forming solution using an applicator (Film Applicator), and then dried in a vacuum oven at 80°C for 20 minutes to form a third electrolyte layer having an average thickness of 4 μm on one side of the second support layer.
[0343] (5) The other surface of the first support layer having the first electrolyte layer formed on one surface thereof was immersed in the electrolyte membrane forming solution, and then dried in a vacuum oven at 80°C for 20 minutes to form a second electrolyte layer having an average thickness of 3 µm on the other surface of the first support layer.
[0344] (6) The second support layer having the third electrolyte layer formed on one side was laminated on the other side of the second electrolyte layer, and heat-treated at 160°C for 10 minutes to produce a composite electrolyte membrane for PEMFC having an average thickness of 15μm, in which the first electrolyte layer, the first support layer (=thinned to an average thickness of 2μm due to shrinkage during manufacturing), the second electrolyte layer, the second support layer (=thinned to an average thickness of 2μm due to shrinkage during manufacturing), and the third electrolyte layer were laminated in sequence as shown in FIG. 1.
[0345] Manufacturing Example 5-1: Manufacturing of composite electrolyte membrane for PEMFC A laminate was prepared in which the thickness of each layer was the same as in Preparation Example 4, that is, first electrolyte layer (4 μm)-first support layer (2 μm)-second electrolyte layer (3 μm)-second support layer (2 μm)-third electrolyte layer (4 μm), but the first and second support layers were made of the PTFE porous support prepared in Preparation Example 1-2.
[0346] As shown in Table 11 below, electrolyte membrane forming solutions having different contents of the high durability improving agent of Example 9-1 were prepared, and then the first electrolyte layer to the third electrolyte layer were formed using the solutions to prepare composite electrolyte membranes.
[0347] Production Example 5-2 and Comparative Production Examples 4-1 to 4-2 A laminate having a first electrolyte layer (4 μm)-first support layer (2 μm)-second electrolyte layer (3 μm)-second support layer (2 μm)-third electrolyte layer (4 μm) was manufactured using the same electrolyte layer thickness and the same support as in Manufacturing Example 5-1, but the content of the high durability improver in the electrolyte membrane forming solution was varied, and then composite electrolyte membranes were manufactured by varying the content of the high durability improver in the electrolyte layer as shown in Table 11 below, to carry out Manufacturing Example 5-2 and Comparative Manufacturing Examples 4-1 to 4-2.
[0348] Experimental Example 9: Measurement of physical properties of composite electrolyte membrane for PEMFC As in Experimental Example 8, a membrane-electrode assembly for PEMFC including an anode electrode 1, an anode catalyst layer 2, an anode gas diffusion layer 3, a composite electrolyte membrane 100, a cathode gas diffusion layer 4, a cathode catalyst layer 5, and a cathode electrode substrate 6 was manufactured.
[0349] In this case, the composite electrolyte 100 used was the composite electrolyte membrane of Production Example 4, Production Examples 5-1 to 5-2, and Comparative Production Examples 4-1 to 4-2, with the first electrolyte layer facing the anode and the third electrolyte layer facing the cathode.
[0350] The performance and durability measurement results according to the content of the durability improving agent added to the produced membrane-electrode assembly and the applied design are shown in Table 11 below.
[0351] [Table 11]
[0352] As shown in Table 11, all of Preparations 4, 5-1 and 5-2 showed excellent durability measurement results. Comparing Preparations 5-1 to 5-2 and Comparative Preparations 4-1 to 4-2, the durability improvement effect was relatively more excellent and the performance was also favorable when the content of the durability improver in each of the first to third electrolytic layers constituting the composite electrolyte increased from the anode direction to the cathode direction (first electrolyte layer<second electrolyte layer<third electrolyte layer) or when the content of the durability improver in the first and second electrolyte layers was higher than that in the second electrolyte layer (second electrolyte layer<first electrolyte layer, third electrolyte layer).
[0353] Although one embodiment of the present invention has been described above, the concept of the present invention is not limited to the embodiment presented in this specification, and a person skilled in the art who understands the concept of the present invention can easily propose other embodiments by adding, changing, deleting, or adding components within the scope of the same concept, which can also be said to fall within the scope of the concept of the present invention. [Explanation of symbols]
[0354] 1: Anode electrode substrate 2: Anode catalyst layer 3: Anode gas diffusion layer 4: Cathode gas diffusion layer 5: Cathode catalyst layer 6: Cathode electrode substrate 11: First support layer 12: Second support layer 13: Third support layer 14: Fourth support layer 21: First electrolyte layer 22: Second electrolyte layer 23: Third electrolyte layer 24: Fourth electrolyte layer 25: 5th electrolyte layer 100: Composite electrolyte membrane for PEMFC 200: Anode 300: Cathode
Claims
1. Contains platinum (Pt) and a carrier carrying the platinum, The platinum is a nano-sized platinum powder, and the platinum powder is bound to and integrated with the surface of the carrier; The support is CeO 2 , GDC (Gd doped Ceria), IrO 2 , SnO 2 and Ti 4 O 7 The durability improver for a PEMFC electrolyte membrane comprises at least one selected from the following:
2. The durability improver for PEMFC electrolyte membrane according to claim 1, wherein GDC is a compound represented by the following chemical formula (1), in which gadolinium (Gd) is doped into a ceria lattice: [Formula 1] In the chemical formula (1), x is an integer satisfying 0<x≦0.3, and y is an oxygen vacancy value that renders the compound electrically neutral and is an integer satisfying 0<y≦0.
25.
3. The particle size of the platinum powder (D 50 ) is 0.1 to 50 nm; The carrier has a particle size (D 50 2. The durability improver for a PEMFC electrolyte membrane according to claim 1, wherein the average particle diameter is 10 to 2,000 nm.
4. The durability improver has a BET specific surface area of 10 to 500 m 2 The durability improver for a PEMFC electrolyte membrane according to claim 1, characterized in that the durability improver for a PEMFC electrolyte membrane is 0.01 to 0.15g.
5. 2. The durability improver for a PEMFC electrolyte membrane according to claim 1, comprising 0.01 to 6.00 wt % platinum and the remainder being a carrier carrying said platinum based on the total weight %.
6. The support is CeO 2 and the durability improving agent contains platinum particles in an amount of 0.01 to 6.00% by weight based on the total weight of the durability improving agent. The carrier is IrO 2 and the durability improving agent contains platinum particles in an amount of 0.01 to 4.50% by weight based on the total weight of the durability improving agent. The support is SnO 2 and the durability improving agent contains platinum particles in an amount of 0.01 to 3.00% by weight based on the total weight of the durability improving agent. The support is Ti 4 O 7 2. The high durability improver for PEMFC electrolyte membrane according to claim 1, wherein the high durability improver contains platinum particles in an amount of 0.01 to 5.50% by weight based on the total weight of the high durability improver.
7. The platinum particles and CeO carrying the platinum particles 2 a cerium-based complex comprising as a support; a non-cerium based composite comprising said platinum particles and a carrier; The support for the non-cerium-based composite is IrO 2 , SnO 2 and Ti 4 O 7 The high durability improver for a PEMFC electrolyte membrane according to claim 1, characterized in that it contains at least one selected from the following:
8. The high durability improver for a PEMFC electrolyte membrane according to claim 7, wherein the cerium-based complex and the non-cerium-based complex are contained in a weight ratio of 1:0.1 to 50.
9. The platinum particles and CeO carrying the platinum particles 2 a cerium-based complex comprising as a support; 2. The high durability improving agent for PEMFC electrolyte membrane according to claim 1, further comprising: a gadolinium-based composite containing platinum (Pt) particles and a GDC carrier carrying the platinum particles.
10. The high durability improver for a PEMFC electrolyte membrane according to claim 9, wherein the cerium-based complex and the gadolinium-based complex are contained in a weight ratio of 1:0.05-10.
11. A composite electrolyte membrane for PEMFC, comprising the durability improver according to claim 1 .
12. The composite electrolyte membrane for PEMFC is an electrolyte membrane in which a first electrolyte layer, a first support layer and a second electrolyte layer are sequentially laminated, At least one layer selected from the first electrolyte layer and the second electrolyte layer contains the durability improver, a cerium (Ce)-based radical scavenger, and an ionomer; The composite electrolyte membrane for PEMFC according to claim 11, wherein the average thickness of the composite electrolyte membrane for PEMFC is 5 to 30 μm.
13. 13. The composite electrolyte membrane for a PEMFC according to claim 12, wherein at least one of the first electrolyte layer and the second electrolyte layer further comprises a cerium (Ce)-based radical scavenger.
14. the first electrolyte layer is an electrolyte layer toward an anode electrode, and the second electrolyte layer is an electrolyte layer toward a cathode electrode; the first electrolyte layer and the second electrolyte layer contain the durability improving agent; The composite electrolyte membrane for PEMFC according to claim 11, wherein the content of the high durability improving agent in the first electrolyte layer and the content of the high durability improving agent in the second electrolyte layer are in a weight ratio of 0.05 to 1.0:
1.
15. The composite electrolyte membrane for PEMFC is arranged in the anode electrode to cathode electrode direction as follows: A composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer and a third electrolyte layer are laminated in this order; or a composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer, a third electrolyte layer, a third support layer and a fourth electrolyte layer are laminated in this order; 12. The composite electrolyte membrane for PEMFC according to claim 11, wherein each of the first electrolyte layer, the second electrolyte layer, the third electrolyte layer and the fourth electrolyte layer independently contains the high durability improving agent, and the content of the high durability improving agent in the electrolyte layers has a gradient in which the content decreases based on the cathode electrode.
16. The composite electrolyte membrane for PEMFC is arranged in the anode electrode to cathode electrode direction as follows: a composite electrolyte membrane in which a first electrolyte layer, a second electrolyte layer, and a third electrolyte layer are laminated in sequence; or a composite electrolyte membrane in which a first electrolyte layer, a second electrolyte layer, a third electrolyte layer and a fourth electrolyte layer are laminated in this order; the composite electrolyte membrane includes a support layer between the first electrolyte layer and the second electrolyte layer, between the second electrolyte layer and the third electrolyte layer, or between the third electrolyte layer and the fourth electrolyte layer; 12. The composite electrolyte membrane for PEMFC according to claim 11, wherein each of the first electrolyte layer, the second electrolyte layer, the third electrolyte layer and the fourth electrolyte layer independently contains the high durability improving agent, and the content of the high durability improving agent in the electrolyte layers has a gradient in which the content decreases based on the cathode electrode.
17. The composite electrolyte membrane for PEMFC is an electrolyte membrane in which a first electrolyte layer, a first support layer and a second electrolyte layer are sequentially laminated from an anode direction to a cathode direction when applied to a membrane-electrode assembly for PEMFC, The composite electrolyte membrane for PEMFC according to claim 11, which satisfies the following condition (2): Condition (2) A 1 ≦A 2 In the above condition (2), A 1 is the content of the durability improving agent in the first electrolyte layer, A 2 indicates the content of the durability improving agent in the second electrolyte layer.
18. The composite electrolyte membrane for PEMFC is a composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer and a third electrolyte layer are sequentially laminated from an anode direction to a cathode direction when applied to a membrane-electrode assembly for PEMFC, any one or more layers selected from the first electrolyte layer, the second electrolyte layer, and the third electrolyte layer contain the durability improving agent; The composite electrolyte membrane for PEMFC according to claim 11, which satisfies both of the following conditions (3) and (4): (3) B 1 ≦A 1 , B 1 ≦A 2 , B 1 ≦A 3 (4) B 2 ≦A 1 , B 2 ≦A 2 , B 2 ≦A 3 In the above condition (3), A 1 is the thickness of the first electrolyte layer, A 2 is the thickness of the second electrolyte layer, A 3 is the thickness of the third electrolyte layer, B 1 represents the thickness of the first support layer, and in the above condition (4), A 1 is the thickness of the first electrolyte layer, A 2 is the thickness of the second electrolyte layer, A 3 is the thickness of the third electrolyte layer, B 2 indicates the thickness of the second support layer.
19. The composite electrolyte membrane for PEMFC is a composite electrolyte membrane in which a first electrolyte layer, a first support layer, a second electrolyte layer, a second support layer and a third electrolyte layer are sequentially laminated from an anode direction to a cathode direction when applied to a membrane-electrode assembly for PEMFC, The composite electrolyte membrane for PEMFC according to claim 11, which satisfies the following condition (5) or condition (6): Condition (5) A 1 ≦A 2 ≦A 3 Condition (6) A 2 ≦A 1 , A 2 ≦A 3 , A 1 ≦A 3 In the above conditions (5) and (6), A 1 is the content of the durability improving agent in the first electrolyte layer, A 2 is the content of the durability improving agent in the second electrolyte layer, A 3 indicates the content of the durability improving agent in the third electrolyte layer.
20. 12. A membrane-electrode assembly for a PEMFC, comprising: an anode (oxidation electrode); the composite electrolyte membrane for a PEMFC according to claim 11; and a cathode (reduction electrode).
Citation Information
Patent Citations
Porous carbon-free catalyst for proton exchange membrane fuel cell and preparation method thereof
CN108736030A
Polymer electrolyte fuel cell and fuel cell system
JP2007257965A
Membrane electrode assembly with hydrogen peroxide decomposition catalyst
JP2008525981A
Fuel cell electrode and method for manufacturing membrane electrode assembly using the same
JP2013084540A
Composite electrolyte membrane for fuel cell, method for producing same, and membrane electrode assembly and fuel cell comprising same