Aqueous graphite lubricant composition containing a dispersant
Alkylphenol ether sulfate dispersants stabilize aqueous graphite dispersions in lubricants, addressing agglomeration and sedimentation issues, ensuring consistent lubrication and die longevity in hot forging processes.
Patent Information
- Application Number
- JP2024531490
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-06
- Filing Date
- 2022-12-01
- Publication Date
- 2024-11-14
AI Technical Summary
Water-based lubricants used in hot forging are prone to agglomeration and sedimentation, leading to inaccurate application of graphite, clogged pipes, and reduced die life, necessitating the development of stable aqueous graphite dispersions.
Incorporation of alkylphenol ether sulfate dispersants with an ether bridge between phenyl and sulfate moieties in lubricant compositions to enhance dispersion stability, using specific ratios and concentrations of water, graphite, and thickeners.
The lubricant compositions maintain over 90% graphite dispersion for 30 days, preventing sedimentation and agglomeration, thus ensuring consistent lubrication and extending die life.
Smart Images

Figure 2024542320000001 
Figure 2024542320000002 
Figure 2024542320000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to lubricant compositions, and more particularly, to lubricant compositions that include an aqueous graphite dispersion. [Background technology]
[0002] Introduction Hot forging is an industrial process in which a metal workpiece is placed in a die and deformed under pressure. The energy applied to the metal workpiece to plastically deform it is converted into heat. The repeated forging of the workpiece and the generation of heat increases the temperature of the die. To reduce friction and ensure that the workpiece can be removed from the die, a lubricant is used at the interface between the workpiece and the die during forging. Good lubrication improves the deformation of the workpiece, favors accurate filling of the die cavity, reduces tool wear at points with free-flowing motion and high specific pressures, and allows for reduced forging forces. Such features reduce the stresses induced in the forging tool and prevent direct contact between the tool and the workpiece, which contributes to longer tool life and better quality control.
[0003] In recent years, the lubricant of choice for hot forging has been water-based lubricants. Water-based lubricants typically contain water as a carrier and lubricating particles such as graphite. Water-based lubricants adhere the graphite to the die to form a solid coating on the die as the water evaporates. Water-based lubricants have an advantage over oil-based lubricants because oil-based lubricants tend to run off the die surface under pressure and be squeezed out of the workpiece / die interface. However, water-based lubricants are not without their drawbacks. Graphite dispersions in water are not stable and require continuous stirring or agglomeration and settling will occur. Agglomeration and settling in the lubricant holding tanks can lead to inaccurate amounts of graphite being applied to the die, thereby reducing the useful life of the die. Agglomeration and settling can also clog pipes and spray nozzles intended to apply the lubricant to the forging die. Ideally, the graphite dispersion will resist settling over long periods of time. One measurement of water-based lubricants determines whether the lubricant is able to maintain 90% dispersion of graphite after 30 days and whether any sediment remains in a dispersible form (the "sedimentation test").
[0004] Attempts have been made to reduce the flocculation and settling of aqueous graphite dispersions using dispersants. There is no consensus on the efficacy of different dispersants on graphite. For example, U.S. Patent Application Publication No. 20090305052(A1) ("'052") discloses a stable aqueous graphite dispersion with high solids content. '052 achieves higher solids loading content in its aqueous graphite dispersion by utilizing dispersants such as polyethylene glycol, polyelectrolytes, and salts of lignosulfonic acid. '052 explains that the dispersants act as spacers that accumulate on the surface of the graphite particles and prevent their steric closeness. '052 does not define any general molecular structure or characteristics that affect the ability of the compound to function as a spacer.
[0005] In contrast to the '052 publication, China Patent Application Publication No. 111925697(A) ("'697 publication") provides a graphene and water-soluble polymer dispersant composite that can be dispersed in water to form a film. The '697 publication explains that enhanced aqueous graphene dispersions can be obtained by including a water-soluble polymer dispersant containing an aromatic ring structure and a hydrophilic group, since the dispersant improves the compatibility between the surface-inert graphene and the water-soluble polymer due to π-π interactions between the dispersant and the graphene. The '697 publication does not mention how the arrangement or amount of the aromatic structure affects the dispersion.
[0006] Given the competing theories behind the effectiveness of graphite dispersants, the unclear influence of different molecular moieties on dispersion performance, and the complexity of intermolecular forces present in aqueous graphene dispersions, it would be surprising to find a dispersant that could pass the sedimentation test. Summary of the Invention
[0007] The present disclosure provides a dispersant capable of passing a settling test. The inventors of the present application have found that an alkylphenol ether sulfate dispersant can pass a settling test. Compared to other dispersants, an alkylphenol ether sulfate dispersant has the distinctive feature of having an ether bridge extending between the alkylphenol and sulfate moieties of the dispersant. Without being bound by theory, it is believed that the spacing between the phenyl and sulfate moieties of the dispersant provided by the ether bridge increases the interaction / wetting of the dispersant with the graphite and the surrounding aqueous medium. Such a result is surprising because conventional dispersants that contain both phenyl and sulfate moieties, such as sodium dodecylbenzenesulfonate, contain a phenyl group and a sulfate group immediately adjacent to each other.
[0008] The present disclosure is particularly useful in formulating lubricants that utilize graphite.
[0009] According to a first aspect of the present disclosure, a lubricant composition includes water, graphite, a thickener, and an alkylphenol ether sulfate dispersant.
[0010] According to a second aspect of the present disclosure, the lubricant composition comprises 20% to 60% by weight of water, based on the total weight of the lubricant composition.
[0011] According to a third aspect of the present disclosure, the lubricant composition comprises 10 wt % to 60 wt % graphite, based on the total weight of the lubricant composition.
[0012] According to a fourth feature of the present disclosure, the graphite has a D90 particle size of 0.5 μm to 5.0 μm.
[0013] According to a fifth feature of the present disclosure, the thickening agent is a polysaccharide.
[0014] According to a sixth aspect of the present disclosure, the lubricant composition comprises 0.01 wt % to 1.0 wt % of a dispersant, based on the total weight of the lubricant composition.
[0015] According to a seventh feature of the present disclosure, the dispersant has the structure (I), 5 ~C 20 The variable x is an average value between 1.0 and 7.0, and the variable Z+ is Li, K, NH 4 and Na.
[0016] According to an eighth feature of the present disclosure, variable Z+ in structure (I) is NH 4 It is.
[0017] According to a ninth feature of the present disclosure, variable x of structure (I) has an average value of 4.2.
[0018] According to a tenth feature of the present disclosure, the variable R is C 9 It is an alkyl. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] As used herein, the term "and / or," when used with a list of two or more items, means that any one of the listed items can be used by itself, or any combination of two or more of the listed items can be used. For example, if a composition is described as containing components A, B, and / or C, the composition can contain A alone, B alone, C alone, A and B in combination, A and C in combination, B and C in combination, or A, B, and C in combination.
[0020] Unless otherwise stated, all ranges are inclusive of the endpoints.
[0021] As used herein, the term weight percent ("wt %"), unless otherwise specified, refers to the weight percentage that a component represents of the total weight of the polymer composition.
[0022] As used herein, Chemical Abstract Services Registry Number ("CAS#") refers to the unique numerical identifier last assigned to a chemical compound by the Chemical Abstract Service as of the priority date of this document.
[0023] Lubricant composition The present disclosure relates to a lubricant composition. The lubricant composition includes water, graphite, a thickener, and an alkylated diphenyl oxide sulfonate dispersant. The lubricant composition may include 20% to 60% by weight of water based on the total weight of the lubricant composition. For example, the lubricant composition includes 20% or more by weight, or 25% or more by weight, or 30% or more by weight, or 35% or more by weight, or 40% or more by weight, or 45% or more by weight, or 50% or more by weight, or 55% or more by weight, while simultaneously 60% or less by weight, or 55% or less by weight, or 50% or less by weight, or 45% or less by weight, or 40% or less by weight, or 35% or less by weight, or 30% or less by weight, or 25% or less by weight of water based on the total weight of the lubricant composition. The lubricant composition may include one or more other additives designed to change the characteristics of the lubricant composition.
[0024] Thickener A thickening agent is included in the lubricant composition to aid in application and retention of the lubricant composition on a surface. The thickening agent may include polysaccharides such as agar, sodium alginate, rhamsam gum, locust bean gum, carrageenan, gum arabic, neem gum, gum chatti, caranna, galactomannan, tragacanth gum, karaya gum, guar gum, welan gum, β-glucan, cellulose, chicle gum, kino gum, dammar gum, glucomannan, acacia gum, cassia gum, mastic gum, spruce gum, psyllium seed husk, gellan gum, xanthan gum, diutan gum, fenugreek gum, ghatti gum, methylcellulose, hydroxyethylcellulose, hydroxypropylmethylcellulose, karaya gum, konjac gum, pectin, and combinations thereof. Additionally or alternatively, the thickener may include other viscosity modifying components such as polyethylene glycol, polyacrylic acid, polyethyleneimine, polyvinyl alcohol, polyacrylamide, carboxyvinyl polymers, poly(vinylpyrrolidinone) and copolymers, polyoxypropylene, and combinations thereof.
[0025] The lubricant composition may include 0.1 wt% to 5.0 wt% of the thickener based on the total weight of the lubricant composition. For example, the lubricant composition may include 0.1 wt% or more, 0.2 wt% or more, 0.4 wt% or more, or 0.6 wt% or more, or 0.8 wt% or more, or 1.0 wt% or more, or 1.5 wt% or more, or 2.0 wt% or more, or 2.5 wt% or more, or 3.0 wt% or more, or 3.5 wt% or more, or 4.0 wt% or more, or 4.5 wt% or more, while simultaneously including 5.0 wt% or less, or 4.5 wt% or less, or 4.0 wt% or less, or 3.5 wt% or less, or 3.0 wt% or less, or 2.5 wt% or less, or 2.0 wt% or less, or 1.5 wt% or less, or 1.0 wt% or less, or 0.5 wt% or less of the thickener based on the total weight of the lubricant composition.
[0026] Graphite The lubricant composition includes graphite. The graphite may have a spherical, platelet, elliptical, and / or irregular shape. The graphite particles may have a D90 of 0.5 micrometers ("μm") to 10 μm. As used herein, the term "D90" means that 90% of the graphite particles have a diameter or longest length smaller than the specified value and 10% of the particles have a diameter or longest length larger than the specified value. The graphite has a particle size of 0.5 μm or more, or 1.0 μm or more, or 1.5 μm or more, or 2.0 μm or more, or 2.5 μm or more, or 3.0 μm or more, or 3.5 μm or more, or 4.0 μm or more, or 4.5 μm or more, or 5.0 μm or more, or 5.5 μm or more, or 6.0 μm or more, or 6.5 μm or more, or 7.0 μm or more, or 7.5 μm or more, or 8.0 μm or more, or 8.5 μm or more, or 9.0 μm or more, or 9.5 μm or more, while the same Sometimes, the graphite may have a D90 particle size of 10 μm or less, or 9.5 μm or less, or 9.0 μm or less, or 8.5 μm or less, or 8.0 μm or less, or 7.5 μm or less, or 7.0 μm or less, or 6.5 μm or less, or 6.0 μm or less, or 5.5 μm or less, or 5.0 μm or less, or 4.5 μm or less, or 4.0 μm or less, or 3.5 μm or less, or 3.0 μm or less, or 2.5 μm or less, or 2.0 μm or less, or 1.5 μm or less, or 1.0 μm or less. The D90 particle size of the graphite is determined using a Malvern Mastersizer™ laser diffraction particle size analyzer.
[0027] The lubricant composition comprises 10 wt% to 60 wt% graphite based on the total weight of the lubricant composition. For example, the lubricant composition comprises 10 wt% or more, or 15 wt% or more, or 20 wt% or more, or 25 wt% or more, or 30 wt% or more, or 35 wt% or more, or 40 wt% or more, or 45 wt% or more, or 50 wt% or more, or 55 wt% or more, while simultaneously 60 wt% or less, or 55 wt% or less, or 50 wt% or less, or 45 wt% or less, or 40 wt% or less, or 35 wt% or less, or 30 wt% or less, or 25 wt% or less, or 20 wt% or less, or 15 wt% or less graphite based on the total weight of the lubricant composition.
[0028] Dispersants The lubricant composition includes a dispersant that is an alkylphenol ether sulfate dispersant. The dispersant may have the structure (I):
[0029] [ka] Variable R in structure (I) is C 5 ~C 20 where x is an average value between 1.0 and 7.0, and Z+ is Li, K, NH 4 and Na. R is selected from the group consisting of C 5 Alkyl, or C 6 Alkyl, or C 7 Alkyl, or C 8 Alkyl, or C 9 Alkyl, or C 10 Alkyl, or C 11 Alkyl, or C 12 Alkyl, or C 13 Alkyl, or C 14 Alkyl, or C 15 Alkyl, or C 16 Alkyl, or C 17 Alkyl, or C 18 Alkyl, or C 19 Alkyl, or C 20R may be an alkyl. R may be a straight or branched alkyl. R may contain one or more carbons that are secondary or tertiary.
[0030] The variable "x" in Structure (I) represents the average molar units of oxyethylene in Structure (I). As defined herein, the value of x is tested and determined by proton nuclear magnetic resonance spectroscopy and carbon-13 nuclear magnetic resonance spectroscopy. x may be a value of 1.0 or more, or 1.2 or more, or 1.4 or more, or 1.6 or more, or 1.8 or more, or 2.0 or more, or 2.2 or more, or 2.4 or more, or 2.6 or more, or 2.8 or more, or 3.0 or more, or 3.2 or more, or 3.4 or more, or 3.6 or more, or 3.8 or more, or 4.0 or more, or 4.2 or more, or 4.4 or more, or 4.6 or more, or 4.8 or more, or 5.0 or more, or 5.2 or more, or 5.4 or more, or 5.6 or more, or 5.8 or more, or 6.0 or more, or 6.2 or more, or 6.4 or more, or 6.6 or more, or 6.8 or more. , or at the same time may be 7.0 or less, or 6.8 or less, or 6.6 or less, or 6.4 or less, or 6.2 or less, or 6.0 or less, or 5.8 or less, or 5.6 or less, or 5.4 or less, or 5.2 or less, or 5.0 or less, or 4.8 or less, or 4.6 or less, or 4.4 or less, or 4.2 or less, or 4.0 or less, or 3.8 or less, or 3.6 or less, or 3.4 or less, or 3.2 or less, or 3.0 or less, or 2.8 or less, or 2.6 or less, or 2.4 or less, or 2.2 or less, or 2.0 or less, or 1.8 or less, or 1.6 or less, or 1.4 or less, or 1.2 or less.
[0031] The lubricant composition may include 0.1 wt% to 5.0 wt% of a dispersant based on the total weight of the lubricant composition. For example, the lubricant composition may include 0.1 wt% or more, or 0.2 wt% or more, or 0.3 wt% or more, or 0.4 wt% or more, or 0.5 wt% or more, or 0.6 wt% or more, or 0.7 wt% or more, or 0.8 wt% or more, or 0.9 wt% or more, or 1.0 wt% or more, or 1.5 wt% or more, or 2.0 wt% or more, or 2.5 wt% or more, or 3.0 wt% or more, or 3.5 wt% or more, or 4.0 wt% or more, or 4. 5% or more by weight, while at the same time comprising 5.0% or less by weight, or 4.5% or less by weight, or 4.0% or less by weight, or 3.5% or less by weight, or 3.0% or less by weight, or 2.5% or less by weight, or 2.0% or less by weight, or 1.5% or less by weight, or 1.0% or less by weight, or 0.9% or less by weight, or 0.8% or less by weight, or 0.7% or less by weight, or 0.6% or less by weight, or 0.5% or less by weight, or 0.4% or less by weight, or 0.3% or less by weight, or 0.2% or less by weight of dispersant. EXAMPLES
[0032] material The following materials were used in the examples:
[0033] The graphite was a powder of graphite particles having a D90 of 5.0 μm and was commercially available from Molygraph Lubricants (Mumbai, India).
[0034] The thickening agent is xanthan gum available from Loba Chemie Mumbai (India).
[0035] Dispersant 1 is a solution of alkylammonium salts of polycarboxylic acids sold under the trade name ANTI-TERRA® and is commercially available from BYK-Chemie GmbH (Wesel, Germany).
[0036] Dispersant 2 is a 97% by weight active powder having structure (II), CAS number 9084-06-4, available from The Dow Chemical Company, Midland Michigan.
[0037] [ka]
[0038] Dispersant 3 is pure sodium dodecyl sulfate having CAS number 151-21-3 and is commercially available from Loba Chemie Mumbai (India).
[0039] Dispersant 4 is a poly(phthalaldehyde) endcapped acrylic acid homopolymer having a weight average molecular weight of 2000 g / mol and a solids content of 47-49 wt. % available from The Dow Chemical Company, Midland Michigan.
[0040] Dispersant 5 is an aqueous solution of water, Structure (I), and (2-hydroxyethyl)ammonium nonylphenol ethoxylate sulfate. Dispersant 5 comprises 30% to 54% by weight of Structure (I), 6% to 30% by weight of (2-hydroxyethyl)ammonium nonylphenol ethoxylate sulfate, and 6% to 24% by weight of water. Structure (I) of Dispersant 5 is as follows: The variable R is a C 1 -C 2 -C 3 -C 4 -C 5 -C 6 -C 7 -C 8 -C 9 -C 10 -C 11 -C 12 -C 13 -C 14 -C 15 -C 16 -C 17 -C 18 -C 19 -C 20 -C 21 -C 22 -C 23 -C 24 -C 25 -C 26 -C 27 -C 28 -C 29 -C 30 -C 31 -C 32 -C 33 -C 34 -C 35 -C 36 -C 37 -C 38 -C 39 -C 40 -C 41 -C 42 -C 43 -C 44 -C 45 -C 46 -C 47 -C 48 -C 49 -C 50 -C 51 -C 52 -C 53 -C 54 -C 55 -C 56 -C 57 -C 58 -C 59 -C 60 -C 61 -C 62 -C 63 -C 64 -C 65 -C 66 -C 67 -C 68 -C 69 -C 70 -C 71 -C 72 -C 73 -C 74 -C 75 -C 76 -C 77 -C 78 -C 79 -C 80 -C 81 - 9 alkyl, the variable x has an average value of 4.2, and the variable Z+ is NH 4 Dispersant 5 is available from The Dow Chemical Company, Midland Michigan.
[0041] The water is distilled.
[0042] Sample preparation The examples were prepared by first combining the thickener, dispersant, and a portion of the water, then mixing the solution for 1 minute using a stirrer. Next, graphite powder was slowly added to the solution and mixed until a paste was formed. The graphite paste was then diluted with the remaining water and mixed using an overhead stirrer to form a dispersion having the composition listed in Table 1. The diluted paste was then added to a 100 milliliter ("mL") volumetric flask and filled to the 100 mL line.
[0043] Test Method Sedimentation Test: The sedimentation test determines what percentage of a dispersion remains dispersed after a given period of time. A 100 mL volumetric flask is filled with the example up to the 100 mL mark and the flask is allowed to stand for a specified period of time. The amount of example that remains dispersed is measured by visually observing the phase separation interface between the clear or cloudy aqueous phase and the dispersed graphite phase. Phase separation is determined by determining how many mL the boundary between the graphite dispersed phase and the aqueous phase is at after a specified period of time, dividing by the original 100 mL, and multiplying by 100. For example, if the interface between the graphite dispersed phase and the aqueous phase is 95 mL, then 95% of the dispersion has survived phase separation. An example is considered to have passed the sedimentation test if 90% of the example remains in the graphite dispersed phase after 720 hours (i.e., 30 days).
[0044] result Table 1 below provides the composition of each comparative example ("comparative example" (CE")) and each inventive example ("IE") in terms of weight percent of the components, and Table 2 provides performance data for each IE and CE. The data in Table 2 provides the percent of the example remaining in the graphite dispersed phase. The heading "nm" indicates that the particular time interval was not measured.
[0045] [Table 1]
[0046] [Table 2]
[0047] As can be seen from Tables 1 and 2, IE1 and IE2 are significantly better than CE1-CE10 in producing lubricant compositions that pass the settling test, as shown by IE1 and IE2 all maintaining 90% graphite dispersion after 720 hours. CE1 and CE2 represent a baseline of stability that can be expected from an aqueous graphite dispersion in the absence of a dispersant. CE3-CE10 demonstrate that the inclusion of certain dispersants can actually reduce the stability of graphite in water compared to dispersions without dispersant, as evidenced by the lower percentage of retained graphite dispersed phase in CE3-CE10 compared to CE1 and CE2.
[0048] Unlike CE1-CE10, IE1 and IE2 each pass the settling test as they are able to maintain 90% or more of the graphite dispersed phase after 30 days of testing. Such results are surprising as all comparative examples utilizing dispersants performed worse than CE1 and CE2 which did not contain a dispersant. As explained above, it is believed that the spacing between the phenyl and sulfate moieties of the dispersant provided by the ether bridge of the dispersant used in IE1 and IE2 increases the ability of the dispersant to interact / bond with the graphite surface and is enhanced compared to other dispersants.
Claims
1. 1. A lubricant composition comprising: Water, Graphite and A thickener; and an alkylphenol ether sulfate dispersant.
2. 10. The lubricant composition of claim 1, comprising 20% to 60% by weight of water, based on the total weight of the lubricant composition.
3. 10. The lubricant composition of claim 1, comprising 10 to 60 percent by weight of graphite, based on the total weight of the lubricant composition.
4. 4. The lubricant composition of claim 3, wherein the graphite has a D90 particle size of 0.5 μm to 5.0 μm.
5. 10. The lubricant composition of claim 1, wherein the thickening agent is a polysaccharide.
6. 10. The lubricant composition of claim 1, comprising from 0.01 to 1.0 wt. % of a dispersant, based on the total weight of the lubricant composition.
7. The dispersant has the structure (I): [Formula 1] The variable R is C 5 ~C 20 The variable x is an average value between 1.0 and 7.0, and the variable Z+ is Li, K, NH 4 The lubricant composition according to any one of claims 1 to 6, wherein the molar ratio is selected from the group consisting of Na and Na.
8. Variable Z+ in structure (I) is NH 4 The lubricant composition of claim 7, wherein
9. 9. The lubricant composition of claim 8, wherein variable x in structure (I) has an average value of 4.
2.
10. The variable R is C 9 9. The lubricant composition of claim 8, wherein the alkyl group is alkyl.
Citation Information
Patent Citations
Lubricant for producing seamless steel pipe
JP1991221598A
Stable aqueous particle dispersion the use thereof and method for producing said dispersion
US20070197705A1
Stable Aqueous Graphite Dispersion With High Solids Content
US20090305052A1
Lubricant composition for hot forming
WO2005056740A1