Electrostrictive materials based on doped ceria.
Patent Information
- Application Number
- JP2024525437
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-21
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
【0005】 アリオバレントドープセリアは、大きなヤング率(約200GPa)及び低い誘電率(<30)を示すにもかかわらず、古典的な電歪素子についてのNewnhamのスケーリング則に基づく推定値よりも100倍以上大きい電歪係数を示す。この「非古典的な」挙動は、外部電場下で再配向する分極性の高い弾性双極子の形成に起因する。
Smart Images

Figure 2024542381000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention provides doped ceria-based materials that exhibit electrostrictive properties and methods for their preparation. [Background technology]
[0002] Materials capable of generating large strains in response to an electric field are used in microfabrication as actuators, sensors, or transducers. These materials include piezoelectric materials (strain proportional to the electric field) and electrostrictive materials (strain proportional to the square of the electric field). Piezoelectric materials are more prevalent but suffer from the drawbacks of feedback in electrical systems due to the direct piezoelectric effect, and poor repeatability due to hysteresis and creep. Electrostrictive materials do not suffer from these drawbacks, making them advantageous in certain applications. Most commonly used electrostrictive ceramics are based on lead magnesium niobate. These electrostrictive ceramics can produce a large strain of about 10 at frequencies up to a few kHz. -16 m 2 / V 2 It exhibits a high electrostrictive coefficient.
[0003] However, such electrostrictive ceramics have two major drawbacks: (1) they require large driving currents due to their high dielectric constant (>10,000), which results in very large electrical losses, and (2) they are not compatible with thin-film silicon microfabrication techniques. Moreover, PMN (lead magnesium niobate) contains lead (toxicity), which limits its use.
[0004] Doped ceria has a very high electrostrictive coefficient (10 -16 m 2 / V 2), which is higher than that estimated by classical theory. Ceria is also very compatible with microfabrication processes and has a very low dielectric constant (about 30). Unfortunately, a high electrostrictive coefficient is only achieved at low frequencies (<1 Hz). In addition, at such low frequencies, the strain saturates (does not increase any further) at a value of about 10 ppm. At higher frequencies, the electrostrictive coefficient relaxes by at least an order of magnitude, increasing to 10 -18 m 2 / V 2 ~10 -17 m 2 / V 2 It becomes. Summary of the Invention [Means for solving the problem]
[0005] Despite exhibiting a large Young's modulus (~200 GPa) and a low dielectric constant (<30), the aliovalent-doped ceria exhibits an electrostrictive coefficient that is more than 100 times larger than estimated based on Newnham's scaling law for classical electrostrictive elements. This "non-classical" behavior is due to the formation of highly polarizable elastic dipoles that reorient under an external electric field.
[0006] It is known that the radio frequency electrostriction coefficient increases as the ionic radius of the dopant decreases. The radio frequency electrostriction coefficient of the lanthanide (Lu), which has the smallest ionic radius, is 8·10 -18 m 2 / V 2 No dopants with an ionic radius smaller than that of lanthanides (Lu) have been found so far.
[0007] In one embodiment of the present invention, the oxidized 10 mol% Zr 4+ Doped ceria has a frequency range of 0.1Hz to 3000Hz, |M 33 |≒10 -16 m 2 / V 2 However, the practical application of such ceramics has been hindered by the existence of Ce, which promotes electron hopping. 3+ The relatively large room temperature conductivity (10-10 S / m) and Ce 3+ When ceria is formed, the dielectric constant increases to about 200. By codoping (e.g., doping ceria with Zr and codoping it with additional cations such as Yb, La, or a combination thereof), the Ce 3+ When the formation of ZnO is suppressed, the dielectric constant decreases to about 30, but the electrostrictive constant also decreases to about 10. -17 m 2 / V 2 In one embodiment, the present subject matter suggests that by systematically tuning the composition of ceria-based solid solutions, it is possible to develop technologically useful electrostrictive materials that are fully compatible with silicon micromachining.
[0008] Thus, in one embodiment, the present invention provides a method for producing a 10% strain-reducing ferroelectric capacitor in the frequency range of 0.1 to 150 Hz without apparent strain saturation reaching up to 200 ppm strain. -16 m 2 / V 2 The 10 mol% Zr doped ceria material (10 mol% Zr 4+ ). However, (Ce 4+ From Ce 3+ As a result of spontaneous partial reduction (to ), both the permittivity and conductivity increase by an order of magnitude (see above). In some embodiments, this can be partially improved by co-doping with a lanthanide. Without being bound by any theory, the present disclosure suggests that the elastic dipoles induced in ceria ceramics by small dopants give a stronger electrostrictive response at high frequencies (>10 Hz). Such electrostrictive response is higher than that obtained when larger dopants are used, regardless of the charge of the dopant.
[0009] In one embodiment, the present invention provides a ceria-based material doped with a metal M selected from Hf, Zr, and Ti, which upon application of an electric field produces a displacement, a stress, or a combination thereof.
[0010] In one embodiment, the present invention provides a ceria-based material doped with a metal M selected from Hf, Zr, and Ti, which generates a displacement, stress, or a combination thereof when an electric field is applied, and has an electrostrictive coefficient of 0.1 Hz to 10 5 At frequencies in the range of 10 Hz -15 m 2 / V 2 ~10 -18 m 2 / V 2 The present invention provides a ceria-based material having a composition in the range of
[0011] In one embodiment, the ceria-based material of the present invention has the formula: Ce 1-x M x O2, where x is in the range of 0.02 to 0.7. In one embodiment, the ceria-based material of the present invention is represented by the formula: Ce 1-x M x O 2-d where x is in the range of 0.02 to 0.7, and d is in the range of 0 to 0.03. In one embodiment, the ceria-based material of the present invention is co-doped with a metal having a lower valence than the metal M. In one embodiment, the metal having a lower valence than the metal M is selected from Ca, Mg, Fe, Sc, Sn, Y, and any combination thereof. In one embodiment, the ceria-based material of the present invention is co-doped with a lanthanide L. In one embodiment, the lanthanide L is any lanthanide selected from La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, or any combination thereof.
[0012] In one embodiment, the ceria-based material of the present invention has the formula: Ce 1-x-y M x L y O 2-y / 2 where x is in the range of 0.01 to 0.7 and y is in the range of 0.01 to 0.7. In one embodiment, the lanthanide L is La or Yb. In one embodiment, the lanthanide L is La, x=0.10±0.02 and y=0.10±0.02. In one embodiment, the ceria-based material of the present invention has the formula: Ce 1-x-y M x L y O2-y / 2-d In the formula, x is in the range of 0.01 to 0.7, y is in the range of 0.01 to 0.7, and d is in the range of 0 to 0.03.
[0013] In one embodiment, the ceria-based material of the present invention generates a displacement in the range of 0.1 ppm to 500 ppm. In one embodiment, the ceria-based material of the present invention generates a stress of at least 0.01 MPa. In one embodiment, the ceria-based material of the present invention has a Young's modulus in the range of 100 GPa to 250 GPa.
[0014] In one embodiment, the electrostrictive coefficient of the ceria-based material of the present invention is greater than 10 -15 m 2 / V 2 ~10 -18 m 2 / V 2 In one embodiment, the electrostrictive coefficient of the ceria-based material of the present invention is in the range of 0.1 Hz to 10 5 At frequencies in the range of 10 Hz -15 m 2 / V 2 ~10 -18 m 2 / V 2 In one embodiment, the electrostrictive coefficient is frequency independent.
[0015] In one embodiment, the dielectric constant of the ceria-based material of the present invention is in the range of 10 to 1000. In one embodiment, the electrical conductivity of the ceria-based material of the present invention is in the range of 10 -9 S / m~10 -5 The range is S / m.
[0016] In one embodiment, the material form of the ceria-based material of the present invention is selected from a disk, a film, a powder, a bar, a pellet, and any combination thereof. In one embodiment, the thickness of the disk, film, bar, or pellet is in the range of 0.1 mm to 10 mm. In one embodiment, the ceria-based material of the present invention is single crystalline, polycrystalline, or amorphous. In one embodiment, the density of the ceria-based material of the present invention is in the range of 5 to 7.3 g / ml.
[0017] In one embodiment, the present invention provides a method for producing the ceria-based material of the present invention, comprising the steps of: adding an aqueous alkaline solution to an aqueous solution containing Ce ions, ions of metal M, and optionally ions of metal L; maintaining the resulting mixture at elevated temperature, optionally with stirring, for at least 25 minutes; and optionally washing the resulting precipitate.
[0018] In one embodiment, the source of the Ce ions, the ions of metal M, and the optional ions of metal L are salts of the above ions. In some embodiments, the metal L is a lanthanide.
[0019] In one embodiment, the salts of the above ions are Ce(NO3)3·6H2O, ZrO(NO3)2·6H2O, and optionally L(NO3)3·6H2O.
[0020] In one embodiment, the alkaline aqueous solution comprises (NH4)2CO3.
[0021] In one embodiment, the above step of adding the aqueous alkaline solution is performed by dropwise addition. In one embodiment, the resulting precipitate is a powder. In one embodiment, the resulting precipitate powder is ground and optionally calcined. In one embodiment, the resulting precipitate powder is pressed in a mold or die to form a disk, bar, or pellet.
[0022] In one embodiment, the dimensions of the disc, bar, or pellet are in the range of 5-20 mm in diameter or any other lateral dimension, and in the range of 0.5-5 mm in thickness.
[0023] In one embodiment, the porosity of the disc, bar or pellet is in the range of 0.01% to 5%. In one embodiment, the porosity of the disc or pellet is less than 5%. In one embodiment, the disc, bar or pellet is polished. In one embodiment, the top and bottom surfaces of the disc or pellet are made parallel to each other by polishing. [Brief description of the drawings]
[0024] The subject matter which is regarded as the invention is particularly pointed out and distinctly claimed in the concluding portion of the specification, however, the invention, both as to organization and method of operation, together with its objects, features, and advantages, may best be understood by reading the following detailed description when read in conjunction with the accompanying drawings.
[0025] [Figure 1A] Figure 1A is a graph showing the relative dielectric constant (εr, real part) and electrical conductivity of Zr-doped ceria, Yb-doped ceria, or ceria co-doped with Zr and 10 mol% Yb as a function of dopant concentration as measured by impedance spectroscopy. Values were measured at 100 Hz. [Figure 1B] FIG. 1B is a graph showing the electrical conductivity of Zr-doped ceria, Yb-doped ceria, or ceria co-doped with Zr and 10 mol % Yb as a function of dopant concentration as measured by impedance spectroscopy. Values were measured at 100 Hz. [Figure 2A] FIG. 2A shows the frequency dependence of the electrostrictive coefficient of Zr-doped ceria. [Figure 2B] FIG. 2B shows the frequency dependence of the electrostrictive coefficient of ceria co-doped with 10 mol % Zr and Yb. [Figure 2C] FIG. 2C shows the frequency dependence of the electrostrictive coefficient of ceria co-doped with 10 mol % Zr and La. [Diagram 3]Figure 3 shows the saturation magnetization measurements at 2K for varying Zr doping and oxidation state of the material. Samples doped with 10mol% or 20mol% Zr were measured before the reduced "Red" state and after the oxidized "Ox" state. Co-doped samples showed no differences. M is the magnetization in Amperes / Meter (A / m) and μH is the magnetic field / flux in Tesla. [Figure 4A] Figure 4A is a graph showing the dielectric constant (ε) versus the applied compressive pressure (-σ) divided by the vacuum dielectric constant (ε) measured at various frequencies for oxidized, 10 mol % Zr-doped ceria. [Figure 4B] Figure 4B shows the inverse and direct electrostrictive constants as a function of frequency measured for oxidized, 10 mol % Zr-doped ceria. [Figure 5A] FIG. 5A is a graph showing the high frequency electrostrictive coefficients measured for 10 mol % doped ceria samples (various dopants). [Figure 5B] FIG. 5B is a graph showing the high frequency electrostriction coefficient measured for the Zr-doped sample. [Figure 5C] FIG. 5C is a graph showing the high frequency electrostrictive coefficients measured for 10 mol % Zr samples (FIG. 5C) co-doped with Yb or La at various concentrations and oxidation states. [Figure 6A] FIG. 6 shows magnetization curves constructed from FIG. 3, with FIG. 6A showing the magnetization curve of the oxidized sample subtracted from the magnetization curve of the reduced sample. [Figure 6B] Figure 6B shows the magnetization curve of the 10 mol% Zr and 0.5 mol% La co-doped sample subtracted from the reduced / oxidized sample, with fitting parameters for each curve to the Langevin curve shown. [Figure 7] FIG. 7 shows the lattice constants of oxidized Ce(1-xy)ZrxLyO(2-y / 2) ceramics (where L is Yb or La).
number
[0026] It will be understood that for simplicity and clarity of illustration, elements shown in the figures have not necessarily been drawn to scale. For example, dimensions of some elements may be exaggerated relative to other elements for clarity. Further, where considered appropriate, reference numerals have been repeated among the figures to indicate corresponding or similar elements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] In the following detailed description, numerous specific details are set forth in order to provide a thorough understanding of the present invention. However, it will be understood by those skilled in the art that the present invention may be practiced without these specific details. In other instances, well-known methods, procedures, and components have not been described in detail so as not to obscure the present invention.
[0028] In one embodiment, the present invention provides a doped ceria-based material that exhibits electrostrictive properties and a method for its manufacture.
[0029] definition
[0030] In an embodiment of the present invention, the abbreviations are as follows: PMN-PT is lead magnesium niobate-lead titanate. ZrDC10 is Zr doped ceria with a doping amount of 10 mol%. The number 10 means 10 mol%. Similarly, the number 20 means 20 mol%. M 33 is the electrostrictive coefficient.
[0031] The Newnham scaling law for classical electrostrictors is an empirical correlation between the dielectric constant, the mechanical properties (Young's modulus), and the electrostrictive coefficient.
[0032] In the embodiment of the present invention, the electrostrictive coefficient |M 33 The unit of | is m 2 / V 2 The longitudinal electrostriction (i.e., the electrostriction parallel to the applied electric field) is expressed in ppm as u 33 The subscript 33 indicates that the electric field direction and the strain direction are the same, both perpendicular to the pellet / film surface.
[0033] In an embodiment of the present invention, electrostriction refers to the change in shape of a material under the application of an electric field. In an embodiment of the present invention, "electrostrictive coefficient" is used interchangeably with "electrostrictive coefficient." In an embodiment of the present invention, the electrostrictive coefficient is defined as M 33 In one embodiment, the electrostrictive coefficients are |M|, M 33 , |M 33 |m 2 / V 2 The electrostriction in the longitudinal direction (i.e., the electrostriction in the direction parallel to the applied electric field) is expressed as u 33 It is written as follows.
[0034] The application of an electric field to the ceria-based material of the present invention can be carried out in a variety of ways. In one embodiment, the ceria-based material is placed between electrodes and a voltage is applied across the ceria-based material. In some embodiments, the ceria-based material is connected to a measuring means for impedance spectroscopy. In some embodiments, the voltage is measured as a function of frequency. The ceria-based material can be used in any form, e.g., pellets, disks, bars, etc., when placed between the electrodes. The terms "voltage" and "bias" are used interchangeably in some embodiments. In one embodiment, the electrodes are made of metal. In some embodiments, a voltage of 10 V is applied. In some embodiments, a voltage of 5 to 50 V is applied. In some embodiments, a direct current is used. In some embodiments, an alternating current is used. In some embodiments, the ceria-based material of the present invention can be measured by applying a voltage / electric field of 10 V. -15 m 2 / V 2 ~10 -18 m 2 / V 2 The electrostrictive coefficient is obtained.
[0035] Typically, impedance spectroscopy measurements require frequency-dependent measurements. Therefore, alternating voltages are commonly used to measure the electrostrictive coefficient, as described herein. In one embodiment, the electrodes are made of at least one metal. Examples of electrode materials include, but are not limited to, aluminum, steel, stainless steel, iron, silver, gold, copper, and the like. In further embodiments, the electrodes are connected to a waveform generator. The waveform generator applies a waveform of any frequency and any waveform shape. In some embodiments, the frequency is in the range of 150 mHz to 1 kHz. In other embodiments, the frequency is in the range of 1 kHz to 10 kHz. In other embodiments, the frequency is in the range of 50 mHz to 150 mHz. In some embodiments, the frequency is in the range of 0.1 Hz to 10 kHz. 5Hz range. In some embodiments, the waveform form is selected from sine wave, square wave, triangle wave, sawtooth wave, pulse wave, and any combination thereof. In one embodiment, one electrode is spring loaded. In some embodiments, the spring loaded electrode is connected to a displacement measuring means. In some embodiments, the electrode is connected to a dielectric analyzer and a force sensor.
[0036] The electrodes connected to the ceria-based material are applied in various ways according to embodiments of the present invention. In one embodiment, the electrodes are physically pressed onto different portions of the ceria-based material. In some embodiments, additional bonding materials are used to connect the electrodes to the ceria-based material. For example, the electrodes are bonded to the ceria-based material using, but not limited to, conductive grease, conductive adhesive, conductive material, conductive tape, conductive gel, carbon nanowire-based tape, clamps, clips, or any combination thereof. In some embodiments, the electrodes are deposited on the ceria-based material using known manufacturing techniques.
[0037] Lanthanides are rare earth elements. In some embodiments, lanthanides are designated as "L" and in other embodiments as "RE" (rare earth). In one embodiment, "L" refers to lanthanides in general (e.g., lanthanides of any ionic charge). In one embodiment, "L" refers to lanthanides of 3+ ionic charge. The designation of L is clear from the material formula given, as known in the art.
[0038] In embodiments of the present invention, "ceria" refers to an oxide of the rare earth metal cerium, and therefore in some embodiments, "ceria-based material" refers to a material that includes ceria.
[0039] In embodiments of the present invention, "single-doped ceria" refers to ceria doped with a single type of dopant. As used herein, "co-doped" refers to doping with at least two types of dopants. In some embodiments of the present invention, "co-doped" refers to doping with one of Zr, Hf, and Ti and a lanthanide. For example, in one embodiment, Ce doped with Zr and Yb is co-doped Ce.
[0040] In one embodiment, the materials of the present invention are referred to as active materials. In one embodiment, the active material is a material that exhibits an electromechanical effect. In one embodiment, the active material is a substance that undergoes a mechanical change in response to an applied electric field. In one embodiment, the active material is an electrostrictive material.
[0041] In one embodiment, the displacement is a change in position of the active material or a portion thereof. In one embodiment, the displacement refers to a change in position or a change in coordinates of the active material or a portion thereof. In one embodiment, the displacement refers to the movement of the active material or a portion thereof as a result of the application of an electric field. In one embodiment, the displacement is observed as a change in length, an increase or decrease in curvature, bending, an increase / decrease in bending, elongation, contraction, a change in volume, a change in width, or other change in the size or shape of the active material or a portion thereof. In one embodiment, the active material generates a force due to the application of an electric field. In one embodiment, the force is generated within the active material. In one embodiment, when the active material is under the influence of an electric field, the active material is capable of resisting an external force. In one embodiment, the active material of the present invention generates a mechanical force.
[0042] In one embodiment, the deformation is a change in a dimension of the material, hi one embodiment, the deformation is equivalent to or includes the displacements described herein above.
[0043] In one embodiment, strain is the amount of deformation a material undergoes in response to a stress per unit of the material's original length. In one embodiment, in-plane strain is the strain in a film in a direction perpendicular to the film's smallest dimension. In one embodiment, the in-plane strain of a film can be described as follows: In thin film technology, most properties can be broadly categorized into two classes, in-plane and out-of-plane, due to the fact that a film has one dimension that is much smaller than the other two. In-plane parameters refer to parameters in a direction perpendicular to the "film" or smallest dimension of the film. In one embodiment, the in-plane strain is the strain in the film or active material. In one embodiment, the longitudinal electrostriction is calculated as the ratio of the displacement of the ceramic pellet to the original thickness.
[0044] In one embodiment, the elastic modulus is the ratio of stress to the corresponding strain within the proportionality limit. In one embodiment, elasticity is the tendency of a material to return to its original shape after it has been stretched or compressed.
[0045] In one embodiment, pm represents the units of picometers. In one embodiment, nm represents the units of nanometers. In one embodiment, MPa represents the units of megapascals. In one embodiment, V represents volts. In one embodiment, μm represents micrometers. In one embodiment, ppm represents parts per million.
[0046] In one embodiment, stress is the force experienced by a material per unit of the material's original area. In one embodiment, stress in the materials of the present invention is dependent on the applied voltage (bias / electric field).
[0047] In some embodiments, the co-doped material is Ce. 1-x-y M x L y O 2-y / 2In one embodiment, x, y, 1-xy represent the amount / ratio of various ions in the material. M is a cation with a 4+ charge and L is a lanthanide with a 3+ charge. The percentage of each atom / ion in the material can be calculated for known x, y, z, 1-xyz, etc.
[0048] In one embodiment, M is an isovalent metal and L is an aliovalent metal, hi one embodiment, M is selected from Zr, Ti, and Hf, and L is an element selected from the group of lanthanides.
[0049] In one embodiment, the active material is Ce 1-x-y-z M x L y N z O 2-y / 2-z-δ In one embodiment, x, y, z, 1-xyz indicate the amount / ratio of various ions in the crystal. M is a cation with a 4+ charge, L is a lanthanide with a 3+ charge, and N is a cation with a 2+ charge. δ is the spontaneous reduction that depends on the oxygen partial pressure (usually about 100 ppm at standard conditions). The percentage of each atom / ion in the material can be calculated for a known x, y, z, 1-xyz, etc. In an embodiment of the invention, either L or N, or a combination thereof, can be present in the material of the invention. In one embodiment, y, which represents the amount of L, is 0, or ranges from 0 to 0.7, and z, which represents the amount of N, is 0, or ranges from 0 to 0.7. In some embodiments where the material is single doped Ce (e.g., CeZrO2), y=0 and z=0. In one embodiment, both L and N are lanthanides. In some embodiments, L and M can represent lanthanides of specific charges possible for a particular lanthanide, independent of each other. The chemical formulas can be adjusted accordingly, as is known in the art.
[0050] In some embodiments of the invention, δ is so small that it is not described in the formula for oxygen ions. In one embodiment, the amount / ratio of oxygen ions is described as "2-y / 2" or "2-y / 2-z". Note that such descriptions and in some embodiments, the amount / ratio includes deviations from the value of 0.01% or 0.02%, or deviations in the range of 0.001% to 0.07% of the stated or calculated value. Such deviations account for the small amount of reduced cations, if any, present, and the corresponding change in the amount of oxygen ions. In one embodiment, the value of δ is 0.0001 or 0.0002, or δ is in the range of 00001 to 0.0007.
[0051] In one embodiment, the metal ion is abbreviated as "metal." In some embodiments, the terms constant and coefficient are used interchangeably. In one embodiment, when referring to displacement, deformation, or strain, parts per million (ppm) represents one micrometer change per meter of original / initial dimension.
[0052] Materials, Dimensions and Values
[0053] In one embodiment, the present invention provides a ceria-based material doped with a metal M selected from Hf, Zr, and Ti, which generates a displacement, a stress, or a combination thereof when an electric field is applied. In one embodiment, the ceria-based material of the present invention generates only a displacement when an electric field is applied. In another embodiment, the ceria-based material of the present invention generates only a stress when an electric field is applied.
[0054] In one embodiment, the present invention provides a ceria-based material doped with a metal M selected from Hf, Zr, and Ti, the ceria-based material having electrostrictive properties.
[0055] In one embodiment, the present invention provides a Zr-doped ceria-based material that generates a displacement, a stress, or a combination thereof upon application of an electric field.
[0056] In one embodiment, the present invention provides a ceria-based material doped with Zr and having electrostriction properties.
[0057] In one embodiment, the ceria-based material of the present invention has the formula: Ce 1-x M x O2, where x ranges from 0.02 to 0.7. In one embodiment, x ranges from 0.02 to 0.45. In one embodiment, x ranges from 0.05 to 0.3, from 0.02 to 0.20, or from 0.08 to 0.12. In one embodiment, x is 0.1 ± 0.01, 0.1 ± 0.5, 0.2 ± 0.5, or 0.05 ± 0.01.
[0058] In one embodiment, the ceria-based material of the present invention has the formula: Ce 1-x M x O 2-d where "d" represents the natural reduction of the material. In one embodiment, "d" and "δ" are used interchangeably. In one embodiment, x ranges from 0.02 to 0.45. In one embodiment, x ranges from 0.05 to 0.3, from 0.02 to 0.20, or from 0.08 to 0.12. In one embodiment, x is 0.1 ± 0.01, 0.1 ± 0.5, 0.2 ± 0.5, or 0.05 ± 0.01. In one embodiment, d ranges from 0 < d < 0.03. In another embodiment, d ranges from 0 < d < 0.01. In one embodiment, d ranges from 0 < d < 0.02. In one embodiment, d ranges from 0.01 < d < 0.02. In one embodiment, d ranges from 0.02 < d < 0.03. In one embodiment, d is approximately 0.01. In one embodiment, d is approximately 0.02. In one embodiment, d is approximately 0.03.
[0059] In one embodiment, the ceria-based material of the present invention is co-doped with a metal having a lower valence than the metal M. In another embodiment, the metal having a lower valence than the metal M is selected from Ca, Mg, Fe, Sc, Sn, Y, and any combination thereof. In one embodiment, the co-doped material comprises Ca, Mg, Fe, Se, Sn, or Y. In one embodiment, the co-doped material consists of Ca, Mg, Fe, Se, Sn, or Y. As used herein, "valence" (or "valence number") refers to a property of an element that determines the number of other atoms to which an atom of the element can be bonded.
[0060] In one embodiment, the ceria-based material of the present invention is co-doped with a lanthanide L.
[0061] In one embodiment, the lanthanide L is any lanthanide selected from La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, or any combination thereof.
[0062] In one embodiment, L is an ion having a 3+ charge. In some embodiments, L has a 2+ or 4+ charge.
[0063] In one embodiment, the ceria-based material of the present invention has the formula: Ce 1-x-y M x L y O 2-y / 2 In one embodiment, the ceria-based material of the present invention has the formula: Ce 1-x-y M x L y O 2-y / 2 where x is in the range of 0.01 to 0.7 and y is in the range of 0.01 to 0.7. In one embodiment, x, y, or a combination thereof is in the range of 0.02 to 0.45. In one embodiment, x, y, or a combination thereof is in the range of 0.05 to 0.3, 0.02 to 0.20, or 0.08 to 0.12. In one embodiment, x, y, or a combination thereof is 0.1±0.01, 0.1±0.5, 0.2±0.5, or 0.05±0.01.
[0064] In one embodiment, the ceria-based material has the formula: Ce 1-x-y M x L y O 2-y / 2-d In one embodiment, the ceria-based material has the formula: Ce 1-x-y M x L y O 2-y / 2-d wherein x ranges from 0.01 to 0.7 and y ranges from 0.01 to 0.7. In one embodiment, x, y, or a combination thereof ranges from 0.02 to 0.45. In one embodiment, x, y, or a combination thereof ranges from 0.05 to 0.3, from 0.02 to 0.20, or from 0.08 to 0.12. In one embodiment, x, y, or a combination thereof is 0.1±0.01, 0.1±0.5, 0.2±0.5, or 0.05±0.01. In one embodiment, d ranges from 0 < d < 0.03. In another embodiment, d ranges from 0 < d < 0.01. In one embodiment, d ranges from 0 < d < 0.02. In one embodiment, d ranges from 0.01 < d < 0.02. In one embodiment, d ranges from 0.02 < d < 0.03. In one embodiment, d is about 0.01. In one embodiment, d is about 0.02. In one embodiment, d is about 0.03.
[0065] In one embodiment, the lanthanide L is La or Yb.
[0066] In one embodiment, M is Zr, L is Yb, x=0.10±0.02, and y=0.10±0.02. In one embodiment, M is Zr, L is La, x=0.10±0.02, and y=0.03±0.01. In one embodiment, M is Zr, x is in the range of 0.001 to 0.2, L is Yb, and y is in the range of 0.005 to 0.25. In one embodiment, M is Zr, x is in the range of 0.001 to 0.2, L is La, and y is in the range of 0.005 to 0.25. In one embodiment, L is La, x=0.10±0.02, and y is in the range of 0.01 to 0.08. In one embodiment, L is Yb, x=0.10±0.02, and y is in the range of 0.05 to 0.15.
[0067] In one embodiment, the ceria-based material of the present invention generates a displacement in the range of 0.1 ppm to 500 ppm. In one embodiment, the ceria-based material of the present invention generates a stress of at least 0.01 MPa. In one embodiment, the ceria-based material of the present invention has a Young's modulus in the range of 100 GPa to 250 GPa. In one embodiment, the ceria-based material of the present invention has a Young's modulus in the range of 200 GPa to 250 GPa.
[0068] In one embodiment, the electrostrictive coefficient of the ceria-based material of the present invention is greater than 10 -15 m 2 / V 2 ~10 -18 m 2 / V 2 In one embodiment, the electrostrictive coefficient of the ceria-based material of the present invention is in the range of 10 -15 m 2 / V 2 ~10 -17 m 2 / V 2 Range, 10 -16 m 2 / V 2 ~10 -18 m 2 / V 2 or 10 -16 m 2 / V 2 ~10 -17 m 2 / V2 In one embodiment, the electrostrictive coefficient of the ceria-based material of the present invention is in the range of 0.1 Hz to 10 5 At frequencies in the range of 10 Hz -15 m 2 / V 2 ~10 -18 m 2 / V 2 In one embodiment, the electrostrictive coefficient of the ceria-based material of the present invention is in the range of 0.1 Hz to 10 3 Hz range: 0.1Hz~4×10 3 Hz range, or frequencies in the range 0.1Hz to 100Hz. -15 m 2 / V 2 ~10 -18 m 2 / V 2 In one embodiment, the electrostrictive coefficient is frequency independent. In one embodiment, the electrostrictive coefficient is frequency independent over a particular frequency range.
[0069] In one embodiment, the dielectric constant of the ceria-based material of the present invention is in the range of 10 to 1000. In one embodiment, the dielectric constant of the ceria-based material of the present invention is in the range of 100 to 500, 20 to 50, 20 to 400, or 100 to 200.
[0070] In one embodiment, the electrical conductivity of the ceria-based material of the present invention is greater than 10 -9 S / m~10 -5 In one embodiment, the electrical conductivity of the ceria-based material of the present invention is in the range of 10 -9 S / m~10 -8 The range is S / m.
[0071] In one embodiment, the strain of the ceria-based material of the present invention is in the range of 50 ppm to 500 ppm. In one embodiment, the strain of the ceria-based material of the present invention is in the range of 50 ppm to 150 ppm. In one embodiment, the strain of the ceria-based material of the present invention is up to 200 ppm.
[0072] In one embodiment, the reduced Ce ions (Ce3+ The concentration of reduced Ce ions is in the range of 50 ppm to 750 ppm, in the range of 50 ppm to 250 ppm, or in the range of 50 ppm to 150 ppm. In one embodiment, the concentration of reduced Ce ions is about 100 ppm. In one embodiment, the concentration of reduced Ce ions is about 500 ppm.
[0073] In one embodiment, the ceria-based material of the present invention has the form of a disk, film, powder, rod, or pellet. In one embodiment, the thickness of the disk, film, bar, or pellet ranges from 0.1 mm to 10 mm. Other forms of the ceria-based material of the present invention can be formed using a mold, die, press, container, ring, or other conventional tool known in the art.
[0074] In one embodiment, the ceria-based material of the present invention is single crystal or polycrystalline. In one embodiment, the ceria-based material of the present invention is an amorphous material. In one embodiment, the density of the ceria-based material of the present invention is in the range of 5 to 7.3 g / ml. In one embodiment, the density of the ceria-based material of the present invention is in the range of 7 to 7.7 g / ml, or 5 to 7 g / ml.
[0075] The embodiments of the present invention relating to ceria-based materials are also applicable to thorium (Th)-based materials. In one embodiment, the doped material of the present invention has the formula: Th 1-x M x For co-doped materials represented by O2 and co-doped with ions having a charge of 4+, 3+, or 2+, the formula: Th 1-x-y M x L y O 2-y / 2 , or the formula: Th 1-x-y-z M x L y N z O 2-y / 2-z For co-doped materials, where the amount of reduced ions is represented by δ, the formula: Th 1-x-y-z M x N y L z O 2-y / 2-z-δSome embodiments disclosed herein for Ce relate to materials in which Ce is replaced by Th. Such Th-related embodiments are also encompassed by the present invention.
[0076] The method for producing the ceria-based material of the present invention
[0077] In one embodiment, the present invention provides a method for producing the ceria-based material of the present invention, comprising the steps of: adding an aqueous alkaline solution to an aqueous solution containing Ce ions, ions of metal M, and optionally ions of metal L; maintaining the resulting mixture at elevated temperature, optionally with stirring, for at least 25 minutes; and optionally washing the resulting precipitate.
[0078] In one embodiment, the present invention provides a method for producing the ceria-based material of the present invention, comprising the steps of: adding an aqueous alkaline solution to an aqueous solution containing Ce ions, ions of metal M, and optionally ions of metal L; maintaining the resulting mixture at elevated temperature for at least 25 minutes; and optionally washing the resulting precipitate.
[0079] In one embodiment, the elevated temperature is any temperature above room temperature. In another embodiment, the elevated temperature is in the range of 30°C to 50°C. In another embodiment, the elevated temperature is in the range of 50°C to 70°C. In another embodiment, the elevated temperature is in the range of 70°C to 100°C. In another embodiment, the elevated temperature is in the range of 100°C to 200°C.
[0080] In one embodiment, the time period during which the resulting mixture is kept at elevated temperature, optionally with stirring, ranges from 25 minutes to 1 hour. In one embodiment, the time period during which the resulting mixture is kept at elevated temperature, optionally with stirring, ranges from 1 to 2 hours. In one embodiment, the time period during which the resulting mixture is kept at elevated temperature, optionally with stirring, ranges from 2 to 5 hours. In one embodiment, the time period during which the resulting mixture is kept at elevated temperature, optionally with stirring, is about 25 minutes.
[0081] In one embodiment, the source of the Ce ions, ions of metal M, and optional ions of metal L are salts of the above ions. In some embodiments, the metal L is a lanthanide. In some embodiments, the metal L comprises at least one lanthanide.
[0082] In one embodiment, the salts of the ions are Ce(NO3)3·6H2O, ZrO(NO3)2·6H2O, and optionally L(NO3)3·6H2O.
[0083] In one embodiment, the aqueous alkaline solution comprises (NH4)2CO3. In one embodiment, the aqueous alkaline solution comprises a carbonate. In one embodiment, the aqueous alkaline solution comprises a hydroxide.
[0084] In one embodiment, the above step of adding the aqueous alkaline solution is performed by dripping. As used herein, the term "drip" refers to the addition of liquid drops in some embodiments. In some aspects, the dripping is performed by a pipette. In some aspects, the dripping is automated.
[0085] In one embodiment, the resulting precipitate is a powder and the formed powder is ground. In a further embodiment, the formed powder is optionally calcined. In one embodiment, the resulting precipitate powder is not ground. In one embodiment, the resulting precipitate powder is ground but not calcined. In one embodiment, the resulting precipitate powder is both ground and calcined.
[0086] The pellets of the present invention
[0087] In one embodiment, the powder formed by the method of the present invention is pressed into a mold or die to form a disc, bar, or pellet. In some embodiments, the terms "pellet," "disc," and "bar" are used interchangeably.
[0088] In one embodiment, the dimensions of the disc, bar, or pellet are in the range of 5-20 mm in diameter or any other lateral dimension, and in the range of 0.5-5 mm in thickness.
[0089] In one embodiment, the thickness of the pellet / disc is in the range of 500 nm to 1000 nm. In one embodiment, the thickness of the pellet / disc is 500 nm. In one embodiment, the thickness of the pellet / disc is in the range of 500 nm to 750 nm, 750 nm to 1000 nm, 100 nm to 1000 nm, 500 nm to 2000 nm, 400 nm to 4000 nm, 600 nm to 800 nm, or 1000 nm to 10,000 nm. In one embodiment, the thickness of the pellet / disc is in the range of 10,000 nm to 100,000 nm.
[0090] In one embodiment, the length and width of the disk / pellet are equal to each other. In one embodiment, the length of the ceria-based material of the present invention is greater than the width of the material. In one embodiment, the length and width of the ceria-based material of the present invention are greater than the thickness (height) of the material. In one embodiment, the length of the ceria-based material of the present invention is 4 cm and the width is 0.8 cm. In one embodiment, the ceria-based material of the present invention has a circular shape and a diameter in the range of 0.2 cm to 7 cm. In one embodiment, the ceria-based material of the present invention has an elliptical shape and a diameter in the range of 0.2 cm to 7 cm.
[0091] In one embodiment, the length of the ceria-based material of the present invention, the width of the material, or a combination thereof, ranges from 0.5 cm to 5 cm. In one embodiment, the length of the ceria-based material of the present invention, the width of the material, or a combination thereof, ranges from 0.1 cm to 1 cm. In one embodiment, the length of the active material, the width of the active material, or a combination thereof, ranges from 1 cm to 10 cm, 10 cm to 100 cm, 0.01 cm to 0.1 cm, 10 μm to 100 μm, or 1 μm to 10 μm. In one embodiment, the active material of the present invention is in the form of a disk. In one embodiment, the diameter of the disk includes any value described above for the width / length of a square / rectangular active material. In one embodiment, the thickness of the disk includes any value described above for the thickness of the active material. In one embodiment, the active material may include any geometric shape or may be an undefined or partially defined geometric shape. In cases where the geometric shape of the active material is not fully defined, the length / width and thickness values described herein represent the maximum and / or minimum dimensions of the active material. In one embodiment, "active material" refers to the ceria-based material of the present invention, and vice versa. In one embodiment, the dimensions and values given for the ceria-based material of the present invention refer to the pellets / discs / films of the present invention. The terms disk and disc are used interchangeably in embodiments of the present invention and refer to a thin cylindrical (or approximately cylindrical) body or shape.
[0092] In one embodiment, the porosity of the disc, bar, or pellet is in the range of 0.05% to 5%. In one embodiment, the porosity of the disc, bar, or pellet is in the range of 0.01% to 5%. In one embodiment, the porosity of the disc, bar, or pellet is in the range of 0.15% to 0.25%. In some embodiments, the porosity of the ceria-based material of the present invention is less than 2%. In some embodiments, the porosity of the ceria-based material of the present invention is less than 5%.
[0093] In one embodiment, the disk, bar, or pellet is ground. In one embodiment, the top and bottom surfaces of the disk or pellet are made parallel to one another. In one embodiment, the top and bottom surfaces of the disk or pellet are made parallel to one another by grinding.
[0094] In one embodiment, the term "a, an, one" refers to at least one. In one embodiment, the term "two or more" may be any number suitable for a particular purpose. In one embodiment, the term "about" or "approximately" includes deviations from the indicated numerical value by +1%, in some embodiments -1%, in some embodiments ±2.5%, in some embodiments ±5%, in some embodiments ±7.5%, in some embodiments ±10%, in some embodiments ±15%, in some embodiments ±20%, and in some embodiments ±25%.
[0095] The following examples are presented in order to more fully illustrate the preferred embodiments of the invention, but they should in no way be construed as limiting the broad scope of the invention.
[0096] Working Example
[0097] Example 1 Sample preparation and characterization
[0098] Sample preparation
[0099] RE=La or Yb solid solution Zr x RE y Ce 1-x-y O 2-y / 2was synthesized by rapid sintering as previously described. Briefly, an aqueous solution of (NH4)2CO3 (Acros Organics, ultrapure, 99%) was dropped into an aqueous solution containing C(NO3)3·6H2O (Strem, purity 99.9%). Doped ceria was prepared by co-precipitating cerium nitrate with ZrO(NO3)2·6H2O. Co-doped ceria was prepared by co-precipitating cerium nitrate with the appropriate RE(NO3)3·6H2O (Strem, purity 99.9%) and ZrO(NO3)2·6H2O. The resulting mixture was kept at 80 °C for 1 h with stirring. The resulting precipitate was washed with deionized water and then ethanol to obtain a powder. The powder was ground and calcined. Flat disks with a diameter of 11 mm and a thickness of 2 mm were fabricated by cold isostatic pressing (300 MPa) in a polyurethane mold. The porosity of all sintered pellets was estimated from the mass density measured by the conventional Archimedes method. The pellets were polished with silicon carbide abrasive paper (maximum 1600 mesh) to make the top and bottom surfaces parallel to each other. Silicon carbide residues were removed by cleaning in 100% ethanol for 30 min in an ultrasonic bath. Where specified, all samples were heated at 500 °C for 5 h in a pure oxygen atmosphere to compensate for oxygen loss that occurs during sintering.
[0100] Electrostriction
[0101] The electrostriction in the longitudinal direction (i.e., parallel to the applied electric field), u 33was measured using the previously described apparatus. Briefly, the ceramic pellet was placed between two stainless steel electrodes, with the upper electrode spring loaded. Voltage was applied using a Keithley 3390 waveform generator and a Trek 610E amplifier. A push rod was used to transfer the displacement from the electrodes to a proximity sensor (capacitance, CPL190 Lion), and the signal from the proximity sensor was read by a lock-in amplifier (DSP7265). The longitudinal electrostriction was calculated as the ratio of the ceramic pellet displacement, measured with a Mitutoyo screw gauge (193-111, ±2 μm), to the original thickness of the ceramic pellet. Measurements were performed under ambient conditions (24 ± 2 °C, 20% to 55% relative humidity). Calibration of the measurement setup was performed using a Pb(Mg 1 / 3 Nb 2 / 3 We used a commercial sample of PMN-PT (TRS Technologies) and a 100-cut quartz single crystal with no additional sputtered metal contacts. We obtained electromechanical values that are consistent with literature values: the electrostrictive M of PMN-PT 33 =(1.5±0.5)·10 -16 m 2 / V 2 , the piezoelectric coefficient of the crystal d 33 =2.3±0.2 pm / V. Measurements were performed in the frequency range of 150 mHz to 1 kHz.
[0102] Impedance spectroscopy and inverse electrostriction
[0103] Room temperature impedance spectroscopy measurements were performed using a Novocontrol Alfa dielectric analyzer in high voltage mode. The applied voltages were 10 VAC, 1 MHz–1 mHz, and 0 VDC. The impedance measurements were within 1% of the impedance analyzer's accuracy.
[0104] Moreover, electrostriction can be defined as follows.
[0105]
number
[0106] In the above formula, ε r is the real part of the relative permittivity measured using impedance spectroscopy. σ is the stress applied to the sample (using a vice) and was calculated using the force sensor and sample dimensions. By measuring the change in permittivity with changing pressure, the electrostrictive constant can be back-calculated and determined.
[0107]
number
[0108] Superconducting quantum interference device (SQUID)
[0109] The temperature-dependent magnetization of the ceramic pellets was measured using a SQUID (superconducting quantum interference device) magnetometer MPMS3 (Quantum Design Inc.) in VSM (vibrating sample magnetometry) mode. The rod-shaped samples were attached to a quartz plate using polyvinyl alcohol adhesive, with the long axis of the rod coinciding with the long axis of the quartz plate. The magnetization (M) values (A m -1 ) was normalized using the rod density calculated from the lattice constant. The temperature dependence of the magnetization in a constant magnetic field (μ0H=0.5T) was measured in the range 5K≦T≦300K. Both the zero-field cooling (ZFC) and field cooling (FC) modes were applied, but no observable difference was found between both modes.
[0110] The magnetic saturation (M) plots were fitted to a Langevin curve.
[0111]
number
[0112] In the above formula, N is the number of magnetic species per unit volume (m -3 ) where g is the Landé g factor; μ β is the Bohr magneton; J=|L±S|. The Langevin function is expressed by the following formula:
[0113]
number
[0114] In the above formula, η is the ratio of thermal energy to magnetic energy;
[0115]
number
[0116] μ0 is the vacuum permeability; k β is the Boltzmann constant; T is the absolute temperature (K); and H is the magnetic field strength (A / m).
[0117] The magnetic susceptibility (χ) plot was fitted to the Curie-Weiss law.
[0118]
number
[0119] In the above formula, C is the Curie constant and T C is the Curie temperature. χ0 is the temperature-independent contribution that accounts for diamagnetism and Van Vleck susceptibility.
[0120] result
[0121] X-ray diffraction patterns of ceria solid solution ceramic pellets doped with various concentrations of aliovalent ions (Yb, La) or isovalent ions (Zr) show that the ceria solid solution ceramic pellets are composed of disorganized cubic fluorite polycrystals.
[0122]
number
[0123] It can be indexed as . The lattice constant decreased when doped with Zr or Yb and increased when doped with La. The change in lattice constant is proportional to the dopant concentration (Fig. 7). SEM (Zeiss Sigma 500) images of the pellets' peripheral surfaces revealed that the grain size estimated by the line intercept method was about 500 nm (Fig. 8(A)-(D)). All samples showed very low porosity (<2%). Young's modulus measured by USTOF (ultrasonic time of flight) was about 200 GPa for all Zr-doped samples, but not for the co-doped samples. Sintered pellets of Zr-doped ceria were reduced (dark green) by heating at 500 °C for 5 h in oxygen atmosphere and oxidized after sintering (turned yellowish white). The reduced and oxidized Zr-doped samples showed differences in electrostrictive coefficients, whereas the other pellets (co-doped) showed no change in the measured parameters before and after sintering.
[0124] Electrical Impedance
[0125] As shown in Figure 1A, when ceria is doped with Zr, the Zr content increases compared to undoped ceria (ε r The dielectric constant (ε r , real part) increased by several orders of magnitude. An increase of more than one order of magnitude was also observed in the electrical conductivity (Fig. 1B). Codoping with aliovalent cations (e.g., Yb or La) significantly reduced the electrical conductivity and permittivity. The permittivity of undoped and aliovalent-doped ceria was close to the predicted value of the Clausius-Mossotti relation (see Choy, TC (2015) Effective medium theory: principles and applications (Vol. 165). Oxford University Press. P. 5-9). No significant change in permittivity / conductivity was observed between oxidized and reduced pellets of Zr-doped ceria (i.e., before and after oxidation (500 °C, 5 h in pure oxygen) of pellets of Zr-doped ceria (10 mol % and 20 mol %). The values in Fig. 1 are those of oxidized pellets (see also reduction vs. oxidation, sintering vs. sintering in oxygen atmosphere above).
[0126] Electrostriction
[0127] The electrostrictive value of Zr-doped ceria is highly dependent on the oxidation state of the pellets. The reduced pellets showed much lower electrostrictive values than the oxidized pellets (Fig. 2A). The electrostrictive constant of the oxidized samples did not show a significant dependence on frequency. In addition, co-doping of 10 mol% Zr with Yb or La did not show a significant difference before and after the oxidation treatment, nor did it show a clear dependence on frequency (Fig. 2B). Co-doping of Zr with Yb (Fig. 2B) or La (Fig. 2C) reduced the electrostrictive constant and induced relaxation (decrease in the electrostrictive coefficient with frequency) in some samples.
[0128] SQUID
[0129] The saturation magnetization at 2 K (Figure 3) increased with increasing Zr doping. In addition, the oxidized samples saturated at a much lower value compared to the reduced samples. In an embodiment of the present invention, the magnetization results were used to determine the saturation magnetization of Ce. 3+ The concentration was measured.
[0130] Reverse electrostriction
[0131] When a compressive stress was applied to an oxidized pellet of 10 mol% Zr-doped ceria, the dielectric constant increased (Figure 4A), and the slope was used to calculate the electrostrictive coefficient (see Equation 2 above), which agreed well with the direct electrostrictive coefficient (Figure 4B).
[0132] Consideration
[0133] The high-frequency electrostrictive coefficient of doped ceria was observed to increase with decreasing ionic crystal radius (Figure 5A). This was investigated for lanthanides, with the 10 mol% Lu doped sample exhibiting a ∼10 -17 m 2 / V 2However, Lu is too expensive for commercial use, and no other lanthanides with smaller ionic radii exist. However, in this disclosure, it has been found that ceria can be easily doped with other non-lanthanide ions, such as Zr (0.98 Å). Ceria doped with 10 mol % Zr has a 10 -16 m 2 / V 2 The electrostrictive coefficient was very high at 1000 ppm. Without being bound by any theory, the results indicate that for a given dopant concentration, the most important factor determining the magnitude of the electrostrictive coefficient in single-doped ceria is the dopant size. This high electrostrictive coefficient is independent of frequency (0.15-3000 Hz) and the strain does not saturate (i.e., the strain remains proportional to the square of the electric field). The strain reached 200 ppm at 1 MV / m. This high electrostrictive coefficient was only achieved after the sample was oxidized (in a pure oxygen environment, at 500 °C for 5 h) and when doped with 10 mol% Zr (Figure 4B). The oxidation state remains stable.
[0134] The electrostrictive coefficient after oxidation becomes very small at high or low Zr concentrations (Fig. 5B), but the electrostrictive coefficient of the reduced sample does not change significantly with the Zr concentration. When the 10 mol% Zr sample is co-doped with Yb or La (Fig. 5C), the electrostrictive coefficient decreases at low doping levels, but further doping with Yb results in an optimum at 10 mol% co-doping. Co-doping with La did not show any significant concentration dependence.
[0135] The high conductivity of reduced Zr is due to the 3+ The Ce ion is easily reduced in the presence of Zr. 3+ The concentration of the ions can be calculated from the magnetization measurements. The curves in Figure 3 cannot be fitted to a Langevin curve within reasonable parameters. This is probably because the concentration of magnetic impurities is Ce. 3+This is probably because the concentration of Ce in the reduced Zr sample is about 100 ppm. However, when the magnetization curves of the oxidized sample at each concentration of Zr are subtracted from those of the reduced sample (Figure 6A), or when the magnetization curves of the sample doped with a small amount of La are subtracted from those of the reduced / oxidized sample (Figure 6B), curves that can be fitted to the Langevin curve are obtained. This fitting reveals that the Ce concentration in the reduced Zr sample is about 100 ppm. 3+ It has been calculated with a very high statistical certainty that the concentration of the ion is about 500 ppm, and that upon oxidation it will be about 100 ppm (which is the concentration in undoped or aliovalently doped ceria).
[0136] Although the dielectric constant increased due to Zr doping, the electrostrictive value was much higher than that predicted by Newnham's scaling law. These results suggest that the elastic dipoles induced in ceria ceramics by small dopants give a stronger electrostrictive response at high frequencies (>1 Hz) than dopants with large dopants. When reduced ceria isovalently doped with Zr, the optimum Zr concentration was found around 10 mol%, suggesting that the Ce 3+ It is believed that the presence of Ce is essential to obtain a large electrostriction constant (see FIG. 5B). The present disclosure suggests an optional mechanism of local polarization due to the reduction of the vicinity of Zr atoms. 4+ From Ce 3+ The reduction to Ce distorts the cubic structure by forming vacancies, which creates polarons. The creation of polarons also explains the increase in the dielectric constant. The concentration of these elastic dipoles increases with the increase in the dielectric constant. 3+ Assuming that the concentration of ZnO is similar to that of ZnO, the Clausius-Mossotti relation gives a polarizability of about 8000 10 -24 cm 3 which is a very high value not even observed in conjugated polymers.
[0137] Ce 3+ La 3+ Since the magnitude of the elastic dipole in the Zr-doped reduced ceria is almost the same as that observed in the aliovalent doped ceria, we conclude that the elastic dipole acting in the Zr-doped reduced ceria is fundamentally different from that observed in the aliovalent doped ceria.
[0138] [Table 1]
[0139] In one embodiment, the material of the present invention has a lower dielectric constant than conventional lead-based materials. Such a lower dielectric constant is advantageous because it means that the material requires less current to operate. Compared to conventional materials, ceria is easier to deposit as a thin film or to form into pellets. Also, the material of the present invention does not require poling. In one embodiment, the material of the present invention is lead-free. In one embodiment, the material of the present invention has a high Young's modulus.
[0140] conclusion
[0141] Most commonly used electrostrictive ceramics are based on lead manganese niobate. These ceramics have a high resistance to 1000 kV at frequencies up to several kHz. -16 m 2 / V 2 However, such electrostrictive ceramics have two major drawbacks: they require large driving currents due to their high dielectric constant (>10,000), and they are not compatible with thin-film Si microfabrication techniques. Despite their large Young's modulus (~200 GPa) and low dielectric constant (<30), aliovalently doped ceria exhibits an electrostrictive coefficient that is more than 100 times larger than the Newnham scaling law-based estimate for classical electrostrictive elements. This "non-classical" behavior is due to the formation of highly polarizable elastic dipoles that reorient under an external electric field. The present disclosure describes the electrostrictive properties of oxidized 10 mol % Zr 4+ Doped ceria has a 10% reduction in the frequency range of 0.1 to 3000 Hz. -16 m 2 / V 2 However, the practical application of such ceramics requires the use of Ce, which promotes electron hopping. 3+ The relatively large room temperature conductivity (10 -10 S / m) and Ce3+ When Ce is formed, the dielectric constant increases to about 200. 3+ When the formation of ZnO is suppressed, the dielectric constant decreases to about 30, but the electrostrictive constant also decreases to about 10. -17 m 2 / V 2 These results suggest that by systematically tailoring the composition of ceria-based solid solutions, it is possible to develop technologically useful electrostrictive materials that are fully compatible with Si microfabrication.
[0142] While certain features of the invention have been illustrated and described herein, various modifications, substitutions, changes, and equivalents will occur to those skilled in the art, and it is therefore to be understood that the appended claims are intended to cover all such modifications and changes that fall within the true spirit and scope of the invention.
Claims
1. A ceria-based material doped with a metal M selected from Hf, Zr, and Ti, The material experiences a displacement, a stress, or a combination thereof when an electric field is applied to it; The electrostrictive coefficient of the material is 0.1 Hz to 10 5 At frequencies in the range of 10 -15 m 2 / V 2 ~10 -18 m 2 / V 2 The range of materials.
2. 2. The material of claim 1 , The material has the formula: Ce 1-x M x O 2-d Represented by, material. In the above formula, x is in the range of 0.02 to 0.7; d is in the range of 0 to 0.
03.
3. 2. The material of claim 1 , A material which is co-doped with a metal having a lower valence than said metal M.
4. 4. The material according to claim 3, The metal having a lower valence than the metal M is selected from Ca, Mg, Fe, Sc, Sn, Y, and any combination thereof.
5. 4. The material according to claim 3, The metal having a lower valence than the metal M comprises a lanthanide L.
6. 6. The material according to claim 5, The lanthanide L is any lanthanide selected from La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, or any combination thereof.
7. 7. The material according to claim 6, The material has the formula: Ce 1-x-y M x L y O 2-y/2-d Represented by, material. In the above formula, x is in the range of 0.01 to 0.7; y is in the range of 0.01 to 0.7; d is in the range of 0 to 0.
03.
8. 8. The material according to claim 7, The lanthanide L is La or Yb.
9. 9. The material of claim 8, the lanthanide L is La, x=0.10±0.02, and y is in the range of 0.01 to 0.08; or The material, wherein the lanthanide L is Yb, x=0.10±0.02, and y is in the range of 0.05 to 0.
15.
10. 2. The material of claim 1 , The displacement ranges from 0.1 ppm to 500 ppm.
11. 2. The material of claim 1 , The material, wherein the stress is at least 0.01 MPa.
12. 2. The material of claim 1 , A material having a Young's modulus in the range of 100 GPa to 250 GPa.
13. 2. The material of claim 1 , The electrostrictive coefficient of the material is independent of frequency.
14. 2. The material of claim 1 , A material having a dielectric constant in the range of 10-1000.
15. 2. The material of claim 1 , 10 -9 S / m~10 -5 A material having a conductivity in the range of S / m.
16. 2. The material of claim 1 , The material has a material form selected from a disk, a film, a powder, a bar, a pellet, and any combination thereof.
17. 17. The material of claim 16, The material has a material form of a disc, film, bar, or pellet, and the thickness of the disc, film, bar, or pellet is in the range of 0.1 mm to 10 mm.
18. 2. The material of claim 1 , the material is monocrystalline or polycrystalline; A material having a density in the range of 5 to 7.3 g / ml.
19. 2. A method for producing the ceria-based material of claim 1, comprising the steps of: (a) adding an aqueous alkaline solution to an aqueous solution containing Ce ions, ions of a metal M, and optionally ions of a metal L; (b) maintaining the resulting mixture at elevated temperature, optionally with stirring, for at least 25 minutes; (c) optionally washing the resulting precipitate.
20. 20. The method of claim 19, The source of the Ce ions, the ions of metal M, and optionally the ions of metal L are salts of said ions.
21. 21. The method of claim 20, The salt of the ion is Ce(NO 3 ) 3 ・6H 2 O, ZrO(NO 3 ) 2 ・6H 2 O, and optionally L(NO 3 ) 3 ・6H 2 O, a method.
22. 20. The method of claim 19, The alkaline aqueous solution is (NH 4 ) 2 CO 3 A method comprising:
23. 20. The method of claim 19, The method, wherein the step of adding the aqueous alkaline solution is performed dropwise.
24. 20. The method of claim 19, The precipitate obtained is a powder, The method wherein the powder is ground and optionally calcined.
25. 25. The method of claim 24, The powder is pressed into a mold or die to form a disc, bar, or pellet.
26. 26. The method of claim 25, The dimensions of said discs, bars or pellets are in the range of 5-20 mm in diameter or any other lateral dimension, and in the range of 0.5-5 mm in thickness.
27. 26. The method of claim 25, The method wherein the porosity of said disc, bar or pellet is in the range of 0.01% to 5%.
28. 26. The method of claim 25, The method wherein the disc, bar, or pellet is ground, optionally making the top and bottom surfaces of the disc or pellet parallel to one another.
Citation Information
Patent Citations
Production of perovskite ceramic powder containing zirconium
JP1988218514A
Piezoelectric / electrostrictive film type element
JP2004274014A
Multiple oxide and catalyst for purification of exhaust gas
JP2005231951A
Oxygen storage and release material, catalyst, exhaust gas purification system, and exhaust gas treatment method
US20210355851A1
Oxygen absorbing and releasing material, catalyst, exhaust gas purifying system, and exhaust gas treatment method
WO2019088302A1