Method for surface contrast laser marking of anodized aluminum or aluminum alloy parts
The anodizing and fiber laser marking method enhances the visibility and durability of markings on aluminum alloys, addressing the issues of low readability and corrosion resistance by creating high-contrast, biocorrosion-resistant markings without additional treatments.
Patent Information
- Application Number
- JP2024529957
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-29
- Filing Date
- 2022-11-23
- Publication Date
- 2024-11-15
AI Technical Summary
Laser marking on aluminum or aluminum alloys results in low visibility and readability of markings, which are not resistant to corrosion and biocorrosion, and require post-treatment for protection, increasing manufacturing complexity and risk.
A method involving anodizing and sealing with deionized water and alkali metal or alkaline earth metal silicate, combined with fiber laser marking within the anodized layer, to enhance contrast and resistance to corrosion and biocorrosion without additional treatments.
The method produces high-contrast markings that are readable in any environment and resistant to wear and tear, biocorrosion, and corrosive environments, eliminating the need for post-marking conversion treatments.
Smart Images

Figure 2024542502000004 
Figure 2024542502000001 
Figure 2024542502000002
Abstract
Description
[Technical field]
[0001] The field of the invention relates to contrast laser marking or inscription of aluminum or aluminum alloy parts to improve their resistance to biocorrosion and salt spray environments. [Background technology]
[0002] Contrast laser marking can also be used to create contrast markings on the surface of aluminum or aluminum alloy parts without removing any material, facilitating and ensuring, for example, visible, reliable and repeatable reading of Data Matrix Code (DMC) or Unique Device Identification (UDI) codes, regardless of the environment (dark or bright) and the angle at which they are read.
[0003] Contrast laser marked aluminium or aluminium alloy parts are used inter alia in the aviation, aerospace, automotive, railway, watchmaking, medical, nuclear and oil industries.
[0004] Marking metal parts with text, logos, images, numbers, 2D codes, etc. for traceability, anti-counterfeiting and / or part identification purposes is used in many fields such as aircraft, aerospace, automotive, railway, watchmaking, medical, nuclear, oil industry, etc. For the purposes of this description, the terms "marking" and "engraving" may be used interchangeably to refer to the same operation or method. Laser marking is a method that has been gaining interest over the last decades, as it offers many advantages such as being fast, allowing high-precision markings with consistent quality, and being resistant to wear and heat. However, laser marking is a subtractive method based on the use of a laser beam that removes material with each laser pulse. Metal parts, especially those made of aluminum or aluminum alloys marked in this way, are bare (e.g. white-raw aluminum) and are not resistant to corrosion and biocorrosion. Currently, corrosion protection after marking consists of conversion treatment by applying a protective coating, for example with Bonderite MCR1200 from Henkel or Surtec 650 from Surtec. This means more steps in the part or device manufacturing, longer production cycle times and increased non-quality related risks, e.g. due to more steps in the manufacturing cycle and a higher risk of poor application.
[0005] In the case of inscriptions / markings having a white tint, the parts cannot withstand biocorrosion even after treatment (eg conversion coating).
[0006] US 2003 / 0201259 describes a method for marking the surface of an aluminum or aluminum alloy part having an anodized layer on the surface, which method comprises the step of marking an area of the surface with a laser beam having a wavelength of 700-1400 nm, in particular 1000-1100 nm, more particularly 1064 nm. The laser beam penetrates at least a large part of the anodized surface layer and locally causes a visual change that is observable with the naked eye. Zones of the anodized layer that are not marked and are further outwardly located remain unchanged. The protective effect of the anodized layer is not impaired and the layer remains outwardly uniform as before the marking was applied. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] US Patent Application Publication No. 2003 / 0201259 Summary of the Invention [Problem to be solved by the invention]
[0008] Another drawback of laser marking metal parts, especially aluminum or aluminum alloys, is its visibility and readability. Currently, the marking has low contrast and therefore is not very visible / readable or is only readable in certain environments and under certain conditions. Post-marking treatment with conversion coatings can also change the visibility / readability of the marking.
[0009] Therefore, there is a real need for a laser-based method for marking the surface of aluminum or aluminum alloy parts to improve their resistance to biocorrosion and corrosion without the need for a post-marking conversion treatment, which is REACH compliant.
[0010] In particular, there is a practical need for a method for marking the surface of an aluminum or aluminum alloy part using a laser, whereby: - the contrast between the laser marking and the treated substrate is substantially increased, allowing for contrast markings that enhance the visibility, recognizability and readability of said markings in any environment; and / or Allows for highly accurate markings of consistent quality that are resistant to wear and tear and to corrosive environments; and / or - suitable for small and fine marking on small surfaces, such as DMC (Data Matrix Codes) and UDI (Unique Device Identification) codes; and / or - Allows the marked parts to withstand corrosive environments, salt spray and biocorrosion without the need for an additional post-marking conversion treatment step. [Means for solving the problem]
[0011] The object of the present invention is to precisely meet these needs, in particular in terms of resistance to corrosion and biocorrosion of the treated parts and visibility / readability of the marking, by providing a method for surface marking of aluminum or aluminum alloy parts, which comprises at least the following steps: A) an anodization step; B) sealing the anode layer formed on the part at the end of step A, The sealing process is In an aqueous solution of deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more, and an alkali metal or alkaline earth metal silicate of 1 to 500 g / L at a temperature of 60°C to 100°C, Or, carried out in an aqueous solution having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more, at a temperature between 60°C and 100°C; D) The following characteristics: - wavelengths greater than 800 nm, for example equal to 1064 nm, - Pulse duration 0.5~10ns, -Laser frequency 400~3000kHz, -5~80W, for example 8~20W output, -Speed 1000~3000mm / s, -Line spacing 0.0001~0.1mm, - Marking time 4 to 200 seconds, and a marking step using a fiber laser beam having one or more of: Includes.
[0012] Step B is essential, since without sealing the corrosion and biocorrosion resistance is no longer suitable. However, after step B there are two options: sealing with silicate or sealing with boiling water only (without silicate). The former ensures the corrosion and biocorrosion resistance of the actual stamp (subject of the present application), while the latter only ensures the corrosion resistance of the stamp thus produced.
[0013] In a preferred embodiment, the fiber laser is a Master Oscillator Power Amplifier (MOPA) laser.
[0014] The surface marking of the aluminum or aluminum alloy parts by the method of the present invention is well contrasted, i.e. the contrast between the laser marking and the surface of the treated part is substantially increased, thereby facilitating the visibility and reading of said marking regardless of the environment and light intensity. Furthermore, the aluminum or aluminum alloy parts provided with the marking produced by the method of the present invention have good resistance to biocorrosion, corrosion, especially salt spray, and corrosive or acidic environments without any post-marking chemical treatment.
[0015] Another object of the invention relates to the use of the marking method according to the invention for manufacturing or marking aluminium or aluminium alloy parts intended for the aviation, aerospace, automotive, railway, watchmaking, medical, nuclear and oil industries, etc.
[0016] Further features and advantages of the present invention will become apparent from the following detailed description, for an understanding of which reference should be made to the accompanying drawings. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a diagram of a setup for performing biocorrosion tests on specimens treated by the method of the present invention, according to section 4.7.19 of standard MIL-C-27725B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The object of the present invention is to precisely meet these needs, in particular in terms of corrosion and biocorrosion resistance of the treated parts and visibility / readability of the marking, by providing a method for surface marking of aluminum or aluminum alloy parts, which comprises at least the following steps: A) an anodization step; B) sealing the anode layer formed on the part at the end of step A, The sealing process is In an aqueous solution having deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more at a temperature of 60°C to 100°C and 1 to 500 g / L of an alkali metal or alkaline earth metal silicate, or carried out in deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more, at a temperature between 60°C and 100°C; D) The following characteristics: - wavelengths greater than 800 nm, for example equal to 1064 nm, - Pulse duration 0.5~10ns, -Laser frequency 400~3000kHz, -5~80W, for example 8~20W output, -Speed 1000~3000mm / s, -Line spacing 0.0001~0.1mm, - Marking time 4 to 200 seconds, and a marking step using a fiber laser beam having one or more of: Includes.
[0019] The method according to the invention makes it possible to produce contrast markings on aluminium or aluminium alloy parts such that the marked parts are resistant to corrosion, in particular in salt spray environments, and to biocorrosion.
[0020] The anodization step A) is carried out under the conditions described in patent application FR 3 106 837.
[0021] The sealing treatment step B), as defined above, when carried out in an aqueous solution of deionized water and of an alkali metal or alkaline earth metal silicate, is carried out under the conditions described in patent application FR 3 106 837 A1.
[0022] According to a preferred embodiment of the invention, the anodizing step A) is an anodizing step in which the part is immersed in a water bath containing sulfuric acid at a concentration of 150-250 g / L to a temperature of 14-21° C. and a direct current voltage is applied to the immersed part according to a voltage profile comprising a voltage increase at a rate of less than 1 V / min until a voltage value of 5-13 V, referred to as a plateau value, is reached.
[0023] Once a voltage value, referred to as the plateau value, has been reached, the applied voltage is maintained at said plateau value for a suitable period of time to obtain an anodic layer on the surface of the part having a thickness of 2 to 7 μm.
[0024] The voltage applied to the immersed portion may be maintained at a plateau value for a period of 20 to 80 minutes.
[0025] The voltage value, called the plateau value, can be maintained at 6 to 10V.
[0026] This anodization is fine OAS (fine sulfuric acid anodization).
[0027] In the process according to the invention, the anodization step A) may also be an anodization step of the TSA, OAS, PSAA, BSAA or OAC type. These anodizations are well known to those skilled in the art and are also described in: TSA (oast-tartric sulfuric anodization), https: / / www.a3ts.org / actualite / commissions-techniques / fiches-techniques-traitement-surface / anodization-sulfo-tartrique-oast-tartric-sulfuric-anodizing-tsa / ; OAS (oxidative anodization sulfuric acid), https: / / www.a3ts.org / actualite / commissions-techniques / fiches-techniques-traitement-surface / anodization-sulfurique-version-5-2 / ; BSAA (boric sulfuric acid anodization), https: / / www.anoplate.com / finishes / boric-sulfuric-acid-anodize-bsaa / ; and PSAA (phosphoric acid anodization), http: / / www.metroplating.co.uk / phosphoric-acid-anodizing.php.
[0028] Preferably, the anodization in step A) is a fine OAS.
[0029] The method of the invention is particularly suitable for aluminium and aluminium alloy parts selected from the group consisting of 2014, 2017A, 2024, 2214, 2219, 2618, AU5NKZr, 7175, 5052, 5086, 6061, 6063, 7010, 7020, 7050, 7050 T7451, 7055 T77, 7068, 7085 T7651, 7075, 7175 and 7475, AS7G06, AS7G03, AS10G, AS9U3, AS7G06 and AS10G obtained by different manufacturing methods, i.e. additive manufacturing.
[0030] As shown, the voltage profile applied to the part comprises a voltage rise from a starting value of 0 V at a rate of less than 1 V / min, preferably between 0.3 V / min and 0.7 V / min, until a voltage value called plateau value of 5 to 13 V (preferably between 6 and 10 V) is reached. The voltage applied to the part immersed in the bath is then maintained at said plateau value for a suitable period of time in order to obtain an anodic layer of aluminium oxide / hydroxide on the surface of the part, having a thickness between 2 and 7 μm, for example equal to about 5 μm.
[0031] According to one embodiment of the present invention, the voltage applied to the immersed portion is maintained at a plateau value for a period of 20 to 80 minutes, preferably 30 to 60 minutes.
[0032] In the anodization step A) according to a preferred embodiment of the invention, the sulfuric acid concentration in the water bath is preferably between 160 g / L and 220 g / L, for example equal to 190 g / L.
[0033] In the anodization step A) according to a preferred embodiment of the invention, the temperature of the water bath can be between 10 and 25°C, preferably between 14 and 21°C, for example 18°C.
[0034] The anodization step A) is followed by step B), which is a sealing step of the anodic layer formed on said part during step A).
[0035] According to one embodiment of the present invention, the method comprises an anodizing step A), a sealing step B) and a marking step D).
[0036] In a variant of the invention, the sealing treatment in step B) is deionized water having a resistivity of at least 0.01 MOhm, preferably at least 0.1 MOhm, more preferably at least 10 MOhm; - 1 to 500 g / L of an alkali metal or alkaline earth metal silicate; The method is carried out in an aqueous solution containing
[0037] The alkali or alkaline earth metal silicate may be selected from the group consisting of lithium silicate, sodium silicate, potassium silicate, calcium silicate and magnesium silicate.
[0038] The water quality of the sealing bath is important since it has an influence on the resistance of the anodic layer formed on the surface portion to biocorrosion. Purer water, such as water with a resistivity of 10 MOhm or more, may result in better performance over time than water with a resistivity of less than 10 MOhm. According to a preferred variant, the deionized water is the associated water, i.e. the water used to fill the active bath during its association / filling, said water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more.
[0039] In the sealing step B), the concentration of the alkali metal or alkaline earth metal silicate in the solution is preferably between 15 and 40 g / L, for example equal to 23 g / L.
[0040] In another variant, the sealing treatment of step B) is carried out in deionized water having a resistivity of at least 0.01 MOhm, preferably at least 0.1 Mohm, more preferably at least 10 Mohm.
[0041] In all variants and embodiments of the invention, the temperature of the sealing solution in step B) can be between 60°C and 100°C, preferably between 97°C and 100°C, for example 98°C.
[0042] In all variants and embodiments of the invention, the duration of the sealing step B) is between 1 and 40 minutes, preferably between 15 and 40 minutes, for example 30 minutes, which is applicable when the sealing is carried out only with water free of said silicates.
[0043] When sealing is performed using silicate, the period is 15 to 25 minutes, preferably 20 minutes.
[0044] According to one embodiment of the present invention, after step A) and before the silicate sealing step (step B), the immersion step A1) comprises: - carried out on the part in a water bath containing a trivalent chromium salt selected from the group consisting of CrF3·xH2O, CrCl3·xH2O, Cr(NO3)3·xH2O, (CH3CO2)2Cr·xH2O, (CH3CO2)7Cr3(OH)2·xH2O, Cr2(SO4)3·xH2O, CrK(SO4)2·xH2O (step A1-1), Then, optionally, - This can be carried out in a water bath containing an oxidizing compound selected from the group consisting of hydrogen peroxide (H2O2), ammonium fluoride (NH4F), potassium fluorozirconate (K2ZrF6), potassium permanganate (KMnO4), and sodium permanganate (NaMnO4) (step A1-2).
[0045] The trivalent chromium salt can be, for example, one of the following commercial products: Surtec 650 from SURTEC, Lanthane 613.3 from COVENTYA, TCS from SOCOMORE, Bonderite MNT 65000 from HENKEL.
[0046] The oxidizing compound can be, for example, PACS, a product of the company SOCOMORE.
[0047] In the immersion step A1), steps A1-1) and A1-2) can be carried out successively in the order of step A1-1) followed by step A1-2). The immersion step A1) can also be carried out by itself without subsequent step A1-2).
[0048] The temperature of the water bath containing the trivalent chromium salt and the temperature of the water bath containing the oxidizing compound in steps A1-1) and A1-2) are 20 to 80° C., preferably 20 to 60° C. The temperatures of the two baths can be the same or different.
[0049] The immersion time in each bath in step A1) may be the same or different, it may be between 5 and 40 minutes, preferably between 5 and 20 minutes.
[0050] The pH of the bath containing the trivalent chromium salt may be 3 to 4.5, preferably 3 to 4, for example 3.5.
[0051] The concentration of the trivalent chromium salt in the bath is preferably 0.5 to 500 g / L.
[0052] The pH of the bath containing the oxidizing compound is 3-6.
[0053] The concentration of the oxidizing compound in the bath is preferably 0.1 to 500 g / L.
[0054] According to another embodiment of the invention, the process also comprises a final hot water sealing treatment, designated step C), before step D and after the sealing treatment described in step B). The final hot water sealing treatment C) is carried out at a temperature above 96°C, for example between 97 and 100°C, in deionized water with a resistivity of at least 0.01 MOhm, preferably at least 0.1 MOhm, more preferably at least 10 MOhm.
[0055] In the final hot water sealing treatment C), the part is immersed in deionized water, advantageously having a resistivity of at least 10 MOhm. The immersion of the part in this step can be between 10 and 30 minutes, preferably between 15 and 25 minutes.
[0056] The marking step D) has the following characteristics: - wavelengths greater than 800 nm, for example equal to 1064 nm, - Pulse duration 0.5~10ns, -Laser frequency 400~3000kHz, -5~80W, for example 8~20W output, -Speed 1000~3000mm / s, -Line spacing 0.0001~0.1mm, - Marking time 4 to 200 seconds, The present invention is implemented with a fiber laser beam having one or more of:
[0057] The inventors have demonstrated that the corrosion behavior of aluminum and aluminum alloy parts after the fiber laser treatment of step D) is (1) Using skillful and appropriate selection of parameters, surface contrast marks with different geometric shapes and structural features can be generated; (2) the ultrafast and efficient laser treatment according to step D) produces a contrast marking on the surface without affecting and / or modifying the microstructure of the aluminum or aluminum alloy part; It was found that this shows the following.
[0058] In fact, by the laser treatment of step D) it is possible to produce a dark, or even black, mark, which provides contrast on the aluminium or aluminium alloy part and is therefore high contrast and easy to read in all light conditions.
[0059] The marking in step D) involves marking the anodized surface with a fiber-enhanced laser beam without penetrating the anode layer, creating a high-contrast, dark inscription into the layer. This marking can be seen as a laser processing method that creates a high-contrast, extremely dark marking on a surface without removing any material. Extremely short laser pulses create nanoscale structures on the surface. This microstructured surface reduces light scattering and the resulting mark has a deep, stable blackened area.
[0060] By judicious selection of parameters, step D) keeps the mark within the thickness of the oxide layer, avoiding affecting the part. Unlike currently known and used marking methods, parts marked under the conditions of step D) do not require post-marking treatment (e.g. conversion coating) to be protected against corrosion and biocorrosion, since the marking is contained in the (underlying) anodic layer without reaching the aluminum substrate. The resistance of the marked part to biocorrosion and corrosion is improved compared to other engraving / marking techniques, especially when exposed to salt and salt spray.
[0061] The marking step D) can be carried out using any kind of fiber laser having the characteristics described above.
[0062] In the case of fiber lasers, the amplification medium is an optical fiber doped with rare earth elements such as samarium, erbium, ytterbium, neodymium, dysprosium, praseodymium, thulium and holmium. The wavelength obtained varies depending on the element selected. As examples for some elements, the following wavelengths are given: samarium 0.6 μm, ytterbium 1.05 μm, erbium 1.55 μm, thulium 1.94 μm, holmium 2.1 μm.
[0063] The spot produced by the fiber laser beam is small, limiting the amount of energy that is converted into thermal energy, which means that the treated surface is protected from damage caused by heat or destruction.
[0064] Another advantage is that fiber lasers are energy efficient.
[0065] In one embodiment of the present invention, the fiber laser is a system in which the gain medium is an ytterbium-doped optical fiber.
[0066] In a preferred embodiment, the marking in step D) is carried out using a fiber laser that is a Master Oscillator Power Amplifier (MOPA) laser. Examples of this type of laser are the TF 420 laser from TECHNIFOR or the SpeedMarker 700 from TROTEC.
[0067] As already indicated, the marking in step D) is carried out within the thickness of the aluminium oxide / aluminium hydroxide layer without removing any material and without reaching the part itself. Thus, the laser marking in step D) is carried out on a layer of aluminium oxide / aluminium hydroxide that is at least 3 μm thick, for example at least 4 μm thick, for example 4-6 μm thick. Preferably, the laser marking in step D) is carried out on a layer of aluminium oxide / aluminium hydroxide that is about 5 μm thick.
[0068] Step D) can be carried out using a fiber laser with a wavelength above 800 nm, for example 1064 nm.
[0069] The laser pulse duration can be from 0.5 to 10 ns, preferably from 1 to 7 ns, and more preferably from 1 to 4 ns.
[0070] The laser frequency can be between 400 and 3000 kHz.
[0071] The output of the fiber laser is 5 to 80W, for example, 8 to 20W.
[0072] The speed of the fiber laser beam can be 1000 to 3000 mm / s.
[0073] The line spacing can be 0.0001 to 0.1 mm.
[0074] The marking time in step D) may be from 4 to 200 seconds.
[0075] The laser beam is pulsed, emitting energy at specific intervals. The speed and line spacing are two parameters that determine the distance between two pulses.
[0076] In one embodiment of the present invention, a method for surface marking of an aluminum or aluminum alloy component comprises the following steps: A) The part is immersed in a water bath containing sulfuric acid at a concentration of 150 to 250 g / L and a temperature of 14 to 21° C.; an anodization step in which a direct current voltage is applied to the immersed part according to a voltage profile with a voltage increase at a rate of less than 1 V / min until a voltage value, referred to as a plateau value, of 5 to 13 V is reached; B) sealing the anode layer formed on the component at the end of step A), Sealing is done in place, In an aqueous solution of deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more at a temperature of 60°C to 100°C and 1 to 500 g / L of an alkali metal or alkaline earth metal silicate, Or, in deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more, at a temperature of 60°C to 100°C; D) The following characteristics: - wavelengths greater than 800 nm, for example equal to 1064 nm, - Pulse duration 0.5~10ns, -Laser frequency 400~3000kHz, -5~80W, for example 8~20W output, -Speed 1000~3000mm / s, -Line spacing 0.0001~0.1mm, - Marking time 4 to 200 seconds, and a fiber laser marking step having one or more of:
[0077] In another embodiment of the present invention, a method for marking the surface of an aluminum or aluminum alloy part comprises the following steps: A) The part is immersed in a water bath containing sulfuric acid at a concentration of 150 to 250 g / L and a temperature of 14 to 21° C.; an anodization step in which a direct current voltage is applied to the immersed part according to a voltage profile with a voltage increase at a rate of less than 1 V / min until a voltage value, referred to as a plateau value, of 5 to 13 V is reached; A1) The part, - immersing in a water bath containing a trivalent chromium salt selected from the group consisting of CrF3·xH2O, CrCl3·xH2O, Cr(NO3)3·xH2O, (CH3CO2)2Cr·xH2O, (CH3CO2)7Cr3(OH)2·xH2O, Cr2(SO4)3·xH2O, and CrK(SO4)2·xH2O (step A1-1); Then (optionally) - immersion in a water bath containing an oxidizing compound selected from the group consisting of hydrogen peroxide (H2O2), ammonium fluoride (NH4F), potassium fluorozirconate (K2ZrF6), potassium permanganate (KMnO4), and sodium permanganate (NaMnO4) (step A1-2); B) sealing the anode layer formed on the component at the end of step A), Sealing is done in place, In an aqueous solution of deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more at a temperature of 60°C to 100°C and 1 to 500 g / L of an alkali metal or alkaline earth metal silicate, Or, in deionized water at a temperature between 60°C and 100°C and having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more; D) The following characteristics: - wavelengths greater than 800 nm, for example equal to 1064 nm, - Pulse duration 0.5~10ns, -Laser frequency 400~3000kHz, -5~80W, for example 8~20W output, -Speed 1000~3000mm / s, -Line spacing 0.0001~0.1mm, - a fiber laser marking step having a marking time of 4 to 200 seconds; Includes.
[0078] In another embodiment of the present invention, a method for marking the surface of an aluminum or aluminum alloy part comprises the following steps: A) The part is immersed in a water bath containing sulfuric acid at a concentration of 150 to 250 g / L and a temperature of 14 to 21° C.; an anodization step in which a direct current voltage is applied to the immersed part according to a voltage profile with a voltage increase at a rate of less than 1 V / min until a voltage value, referred to as a plateau value, of 5 to 13 V is reached; A1) The part, - immersing in a water bath containing a trivalent chromium salt selected from the group consisting of CrF3·xH2O, CrCl3·xH2O, Cr(NO3)3·xH2O, (CH3CO2)2Cr·xH2O, (CH3CO2)7Cr3(OH)2·xH2O, Cr2(SO4)3·xH2O, and CrK(SO4)2·xH2O (step A1-1); Then (optionally) - immersion in a water bath containing an oxidizing compound selected from the group consisting of hydrogen peroxide (H2O2), ammonium fluoride (NH4F), potassium fluorozirconate (K2ZrF6), potassium permanganate (KMnO4), and sodium permanganate (NaMnO4) (step A1-2); B) sealing the anode layer formed on the component at the end of step A), The sealing process is performed in place. In an aqueous solution of deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more at a temperature of 60°C to 100°C and 1 to 500 g / L of an alkali metal or alkaline earth metal silicate, Or, in deionized water at a temperature between 60°C and 100°C and having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more; C) performing a final hot water sealing treatment in deionized water at a temperature of 97°C to 100°C and having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more; D) The following characteristics: - wavelengths greater than 800 nm, for example equal to 1064 nm, - Pulse duration 0.5~10ns, -Laser frequency 400~3000kHz, -5~80W, for example 8~20W output, -Speed 1000~3000mm / s, -Line spacing 0.0001~0.1mm, - a fiber laser marking step having a marking time of 4 to 200 seconds; Includes.
[0079] In another embodiment of the present invention, a method for surface marking an aluminum or aluminum alloy component comprises the steps of: A) The part is immersed in a water bath containing sulfuric acid at a concentration of 150 to 250 g / L and a temperature of 14 to 21° C.; an anodization step in which a direct current voltage is applied to the immersed part according to a voltage profile with a voltage increase at a rate of less than 1 V / min until a voltage value, referred to as a plateau value, of 5 to 13 V is reached; A1) The part, - a step of immersing in a water bath containing a trivalent chromium salt selected from the group consisting of CrF3·xH2O, CrCl3·xH2O, Cr(NO3)3·xH2O, (CH3CO2)2Cr·xH2O, (CH3CO2)7Cr3(OH)2·xH2O, Cr2(SO4)3·xH2O, and CrK(SO4)2·xH2O (step A1-1); B) sealing the anode layer formed on the component at the end of step A), The sealing process is performed in place. In an aqueous solution of deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more at a temperature of 60°C to 100°C and 1 to 500 g / L of an alkali metal or alkaline earth metal silicate, Or, in deionized water at a temperature between 60°C and 100°C and having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more; D) The following characteristics: - wavelengths greater than 800 nm, for example equal to 1064 nm, - Pulse duration 0.5~10ns, -Laser frequency 400~3000kHz, -5~80W, for example 8~20W output, -Speed 1000~3000mm / s, -Line spacing 0.0001~0.1mm, - a fiber laser marking step having a marking time of 4 to 200 seconds; Includes.
[0080] In another embodiment of the present invention, a method for marking the surface of an aluminum or aluminum alloy part comprises the following steps: A) The part is immersed in a water bath containing sulfuric acid at a concentration of 150 to 250 g / L and a temperature of 14 to 21° C.; an anodization step in which a direct current voltage is applied to the immersed part according to a voltage profile with a voltage increase at a rate of less than 1 V / min until a voltage value, referred to as a plateau value, of 5 to 13 V is reached; Im) impregnating said anodized part at the end of step A) in a bath of an organic or inorganic dye; Then, optionally, A1) The part, - immersing in a water bath containing a trivalent chromium salt selected from the group consisting of CrF3·xH2O, CrCl3·xH2O, Cr(NO3)3·xH2O, (CH3CO2)2Cr·xH2O, (CH3CO2)7Cr3(OH)2·xH2O, Cr2(SO4)3·xH2O, and CrK(SO4)2·xH2O (step A1-1); Then (optionally) - immersion in a water bath containing an oxidizing compound selected from the group consisting of hydrogen peroxide (H2O2), ammonium fluoride (NH4F), potassium fluorozirconate (K2ZrF6), potassium permanganate (KMnO4), sodium permanganate (NaMnO4) (step A1-2), followed optionally by B) sealing the anode layer formed on the component at the end of step A), The sealing process is performed in place. In an aqueous solution of deionized water having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more at a temperature of 60°C to 100°C and 1 to 500 g / L of an alkali metal or alkaline earth metal silicate, Or, in deionized water at a temperature between 60°C and 100°C and having a resistivity of 0.01 MOhm or more, preferably 0.1 MOhm or more, more preferably 10 MOhm or more; D) The following characteristics: - wavelengths greater than 800 nm, for example equal to 1064 nm, - Pulse duration 0.5~10ns, -Laser frequency 400~3000kHz, -5~80W, for example 8~20W output, -Speed 1000~3000mm / s, -Line spacing 0.0001~0.1mm, - a fiber laser marking step having a marking time of 4 to 200 seconds; Includes.
[0081] Step Im), which follows step A), may be carried out using any technique known to the skilled artisan. For example, it may be realized in a dyebath adapted for surface treatment, available from companies such as Clariant. As an example, mention may be made of the organic dye Sanodal Blue (Clariant) in a concentration of 3 g / L, to which 2 g / L of sodium acetate must be added, at a pH of 5 to 6, at a temperature of 40 to 65°C, preferably equal to 50°C, for a period of 5 to 35 minutes, preferably for a duration equal to 20 minutes. The active ingredient of the organic dye is an anthraquinone molecule.
[0082] In all embodiments, before subjecting the part to the surface treatment method of the invention, and therefore before the anodizing step A), the part may be subjected to a surface preparation step by degreasing and / or pickling in order to remove grease, dirt and oxides present on the surface.
[0083] These preliminary steps of surface preparation include the following operations: - Solvent degreasing to dissolve the grease on the surface of the part. This operation can be achieved by immersion, spraying or any other method known to those skilled in the art. - alkaline degreasing to dissolve the grease on the surface of the parts. This operation can be achieved by immersion, spraying or any other technique known to those skilled in the art; - alkaline pickling to dissolve the oxides naturally formed on the surface of the part. This operation can be achieved by immersion, spraying or any other technique known to those skilled in the art. At the end of this operation, the part is covered with a powder layer formed by oxidation products of the intermetallic compounds, which must be removed by a pickling step. Pickling to dissolve the oxides naturally formed on the surface of the part and / or the oxide layers formed on the surface of the part during the alkaline cleaning step, this operation may include one or more of the following: immersion, spraying or may be achieved by any other technique known to the person skilled in the art.
[0084] These steps are described in detail, for example, in WO 2013 / 117759.
[0085] In particular, intermediate rinsing with deionized water is preferably performed between the above successive steps and before the part is treated by anodization.
[0086] The method of the present invention is of great interest in any type of industry where contrast marking of aluminum or aluminum alloy parts with good resistance to corrosion, biocorrosion, salt spray and salt exposure is required.
[0087] For example, when marking is performed using the method of the present invention (without physicochemical post-treatment) on an aluminum or aluminum alloy part, such as alloy 2024T3, - when the parts are subjected to a salt spray test (168 hours exposure according to ISO 9227), no corrosion is observed at the end of the test, while ensuring the readability and visibility of the marking, and - When the parts are subjected to a 15-day immersion biocorrosion test according to § 4.7.19 of the standard MIL-C-27725B, the markings are not corroded at the end of the test, while ensuring their readability and visibility. It should be noted that biocorrosion resistance is only guaranteed when the scope and related variants contain at least the step of sealing with the abovementioned silicates.
[0088] It should be noted that laser marking, with or without contrast, penetrated (through the oxide layer) into aluminum or aluminum alloy parts such as 2024T3 alloy without physicochemical post-treatment, shows signs of corrosion before the 168 hours exposure to saline solution required according to ISO 9227.
[0089] One of the advantages of the markings using the method described in this invention is that they are visually stable at any observation angle. The highly visible and uniform contrast from all angles is due to the periodic nanostructures that reflect and absorb light and scatter it as widely as possible. This feature represents a guarantee of quality, especially in the watch or automotive industry, which implements many visible components.
[0090] The high contrast, dark markings produced by this method greatly improve the visibility and readability of marking detail in both manual and automated applications.
[0091] Furthermore, the marking method of the present invention is suitable for small and fine markings or for DMC (Data Matrix Codes) and UDI (Unique Device Identification) codes on small surfaces.
[0092] For example, European and US FDA (Food and Drug Administration) regulations on medical devices require that medical technology products carry a UDI (Unique Device Identification) code that ensures their traceability and remains readable over time. Marking by the method of the present invention fits nicely into the requirements for UDI-compatible marking. UDI codes, especially very small UDI codes, remain readable over time due to their corrosion resistance, stability at all viewing angles, and contrast or very dark black color.
[0093] Another object of the invention relates to the use of the marking method according to the invention for manufacturing or marking aluminium or aluminium alloy parts intended for the aviation, aerospace, automotive, railway, watchmaking, medical, nuclear and oil industries, etc. EXAMPLES
[0094] Example 1: Surface marking method for aluminum alloy parts Aluminium alloy parts 2024 T3 and AS7G06T6 machined and laminated on one of the two sides with dimensions 120 x 60 x 2 mm are processed according to the method described below. The surface preparation steps of the part are first realized in sequence: - alkaline degreasing by immersing the parts in a bath of ALUMAL CLEAN 101 (manufactured by Coventya) at a temperature of 60°C for 20 minutes; - Rinse with tap water or deionized water, - pickling by immersing the parts in a solution of ALUMAL DEOX 411 (manufactured by COVENTYA); - Rinse with tap water or deionized water.
[0095] The pickled and rinsed parts are subsequently subjected to an anodizing process according to the invention, during which they are immersed in a water bath comprising sulfuric acid at a concentration between 160 g / L and 220 g / L, for example equal to 190 g / L. The bath is held and maintained at a temperature of 18° C. A direct voltage is applied to said immersed part according to the following voltage profile: voltage rise from a value of 0 V at a rate of 0.7 V / min until a voltage value of 10 V, referred to as the plateau value, is reached. The voltage is maintained at the plateau value for 40 minutes. An anodic layer of 3 to 6 μm thickness is formed on the surface of the part.
[0096] As a comparative example, the same parts subjected to the same surface preparation operation are anodized using the conventional chromic acid anodization (OAC) and fine sulfuric acid anodization (fine OAS) methods. The operating conditions for these anodizations are shown in Table 1.
[0097] [Table 1]
[0098] The thickness of the anode layer formed on the components is measured by eddy current according to standard ISO 2360.
[0099] The anodized part is then subjected to one or more rinses, preferably with deionized water, followed by a sealing operation according to the invention under the conditions and in the sequence set out below. - Step A1.1) and Step A1.2): The parts are placed in a water bath containing 29 Vol / Vol% of trivalent chromium salt (potassium chromium (III) sulfate, with the chemical formula KCr(SO4)2) at a temperature of 40°C for 20 minutes at a pH of 3.9, followed by Successive immersion steps in a water bath containing 7 Vol / Vol % H2O2 at a temperature of 25°C for 5 minutes and pH 4.2; Step B): At the end of the two preceding operations, sealing treatment by immersing the parts in a mounting solution of deionized water containing 23 g / L of sodium silicate and having a resistivity of 10 MOhm, at a temperature of 98° C., for 20 minutes.
[0100] Between each sealing step, a deionized water rinse is performed at a temperature of about 20° C. for 1 minute.
[0101] The non-drill marking step D) using the MOPA fiber laser beam (without affecting the part) was carried out using a SpeedMarker 700 laser from TROTEC under the conditions specified in [Table 2].
[0102] [Table 2]
[0103] Alodine conversion coating refers to Alodine 1200 type conversion coatings, which are an exclusive chemical method for the long term protection of aluminum or aluminum alloy surfaces against oxidation. The Alodine 1200 treatment was developed to protect surfaces that do not require a paint finish or only a topical finish (>168 hours salt spray resistance).
[0104] This ensures maximum adhesion and durability of the applied finish due to the perfect chemical stability of the treated surface.
[0105] Alodine 1200 used in the hardening process forms a protective coating on the aluminum or alloy with virtually no excess thickness. The color of this coating varies from yellow to brown depending on the type of alloy or the degree of purity of the metal.
[0106] Alodine 1200 is approved to standard MIL C 5541.
[0107] Biocorrosion Resistance At the end of these operations, a sealed and marked anodic layer was obtained on each treated part. Once treated, the parts were subjected to an immersion test in a medium exhibiting biocorrosion according to the protocol of § 4.7.19 of the standard MIL-C-27725B. The assembly diagram with the various parts for carrying out the biocorrosion test according to § 4.7.19 of the standard MIL-C-27725B is shown in Figure 1.
[0108] The parts were removed from the medium and the results were visually evaluated by checking the visibility and readability of the markings and any signs of damage caused by the process and / or attack of the substrate by the medium (lower phase). Visual degradation can be checked by measuring the ohmic resistivity of the layer, which, when not infinite, highlights any degradation of the layer that may have progressed down to the substrate.
[0109] Before the test, the Ohmic Resistivity method is useful for predicting the fact that if the current passes through two points of the marking, the biocorrosion resistance will not be met. On the other hand, if there is no attack on the marking, there is no requirement for the after biocorrosion test.
[0110] This method is only systematically performed after the biocorrosion test for any signs of potential corrosion and at the end of the 15 day biocorrosion test.
[0111] Method for measuring resistance using an ohmmeter: A multimeter can be used to measure resistance. It must be used in ohmmeter mode.
[0112] Using the multimeter in ohmmeter mode: Terminal selection: COM terminal and terminal holding the symbol ohms.
[0113] Connections: At the end of the test, a multimeter is connected directly to two points on the test specimen in the area that was in contact with the lower phase of the two-phase medium.
[0114] Size: The largest size is selected and this is reduced until the smallest size above the measurement is found.
[0115] [Table 3] summarizes the results of biocorrosion resistance tests of different surface treatments as a function of the number of days of immersion in a two-phase medium.
[0116] [Table 3]
[0117] "NOK" means that the criteria for either reading or predicted resistance to biocorrosion were not met.
[0118] Pit corrosion is a localized corrosion that results in the formation of irregularly shaped cavities on the surface of an aluminum alloy part. Such corrosion occurs when the aluminum alloy part comes into contact with an aqueous solution containing halide ions, most frequently chloride ions. Based on the results shown in Table 3, the resistance at 168 hours according to ISO 9227 is good for all three samples. At the end of the test, there is no corrosion and the markings remain legible.
[0119] Various black marking tests were carried out on different substrates (2024T3 and AS7G06T6), some of which remained on the layer and did not reach the substrate, while others did reach the substrate. This last case can be detected by measuring the current at two points on the marking (if the current flows, the layer is completely perforated).
[0120] 1) Fine OAS test tubes after marking and before exposure to salt spray according to ISO 9227, by sulfuric acid anodization (as mentioned above and / or according to French Patent No. 3106837) For the 2024 T3 alloy specimen (fine OAS with silicate sealing treatment) and for the AS7G06T6 alloy specimen (standard fine OAS without silicate), the markings were intact and legible.
[0121] 2) Micro-OAS test tubes by sulfuric acid anodization (as above and / or according to French Patent No. 3106837) after marking and after 168 hours of exposure to salt spray according to ISO 9227 For the 2024 T3 alloy specimens (fine OAS with silicate sealing treatment), no corrosion was detected on the markings (electrically insulating markings prior to testing) after exposure to salt spray. The markings were intact and still legible.
[0122] For the AS7G06T6 alloy specimen (fine OAS standard without silicates), no corrosion was detected on the markings (electrically insulating markings before the test) after exposure to salt spray. The markings were intact and still legible. However, significant corrosion was detected on the other markings (all of which were conductive before the test, indicating that the laser markings had perforated the anode layer and reached the substrate).
[0123] 3) Micro-OAS test tubes by sulfuric acid anodization (as mentioned above and / or according to French Patent No. 3106837) after a 15-day immersion biological corrosion test according to § 4.7.19 of the standard MIL-C-27725B For the 2024 T3 alloy specimens (fine OAS with silicate sealing treatment) and for the AS7G06T6 alloy specimens (standard fine OAS without silicate), no corrosion was detected on the markings after 15 days of immersion according to § 4.7.19 of standard MIL-C-27725B. The markings were intact and maintained their contrast and legibility.
[0124] These tests are intended to achieve the desired objectives, i.e. - Producing contrast markings to facilitate visibility and legibility, as well as reading of the markings; - eliminating the need for post-marking conversion treatments, e.g. with Bonderite MCR 1200; - to obtain a high-contrast laser marking that is resistant to neutral salt spray according to ISO 9227 for a minimum of 168 hours; - obtaining a contrast laser marking that is resistant to biological corrosion after immersion for 15 days according to § 4.7.19 of the standard MIL-C-27725B; is clearly shown to be achieved by parts treated using the method described above.
[0125] The aviation requirements for resistance to salt spray (168 hours exposure according to ISO 9227) and resistance to biocorrosion after 15 days of immersion according to § 4.7.19 of standard MIL-C-27725B are also met by the marking process of the present invention.
[0126] In conclusion, the method of marking aluminum or aluminum alloy parts according to the invention makes the marking easy to read with a digital code reader. Marking these parts ensures that they will withstand salt corrosion without the need for a post conversion treatment and ensures that they will withstand biological corrosion.
[0127] The marking method according to the invention is therefore of great interest in all areas using data matrices or markings which require a minimum contrast to facilitate reading and resistance to (bio)corrosion, such as, for example, aviation and space equipment in general, nuclear, offshore (oil), automotive, railways, etc.
Claims
1. A method for surface marking of an aluminum or aluminum alloy part, comprising at least the following steps: A) an anodization step; B) sealing the anode layer formed on the part at the end of step A, The sealing process is In an aqueous solution of deionized water having a resistivity of 0.01 MOhm or more at a temperature of 60° C. to 100° C. and 1 to 500 g / L of an alkali metal or alkaline earth metal silicate, or In deionized water having a resistivity of 0.01 MOhm or more at a temperature of 60°C to 100°C, The steps to be performed; D) The following characteristics: - Wavelength over 800 nm, - pulse duration 0.5-10 ns, - laser frequency 400-3000 kHz, - Output power 5 to 80 W, -Speed 1000-3000mm / s, - Line spacing 0.0001-0.1 mm, - marking time 4 to 200 seconds, and a marking step using a fiber laser beam having one or more of: The method includes:
2. 2. The method according to claim 1, characterized in that step A) is an anodization of the TSA (tartaric acid anodization), OAS (sulfuric acid anodization), fine OAS (fine sulfuric acid anodization), PSAA (phosphoric acid anodization), BSAA (boric acid anodization) or OAC (chromic acid anodization) type.
3. anodizing step A) is an anodizing step in which the part is immersed in a water bath containing sulfuric acid at a concentration of 150-250 g / L at a temperature of 14-21° C., 3. A method according to claim 1, characterized in that a direct voltage is applied to the immersed part according to a voltage profile comprising a voltage increase at a rate of less than 1 V / min until a voltage value of 5-13 V, referred to as a plateau value, is reached.
4. 4. The method according to claim 1, wherein the aluminum alloy is selected from the group consisting of 2014, 2017A, 2024, 2214, 2219, 2618, AU5NKZr, 7175, 5052, 5086, 6061, 6063, 7010, 7020, 7050, 7050 T7451, 7055 T77, 7068, 7085 T7651, 7075, 7175 and 7475, AS7G06, AS7G03, AS10G, AS9U3, AS7G06, AS7G06 and AS10G obtained by additive manufacturing.
5. 5. The method according to claim 1, wherein the alkali or alkaline earth metal silicate is selected from the group consisting of lithium silicate, sodium silicate, potassium silicate, calcium silicate and magnesium silicate.
6. Method according to any one of claims 1 to 5, characterized in that step D is carried out using a fibre laser, the system in which the gain medium is an ytterbium-doped optical fibre.
7. The method according to any one of claims 1 to 6, characterized in that step D is performed with a fibre laser which is a Master Oscillator Power Amplifier laser or MOPA.
8. After step A) and before the silicate sealing step (step B), -CrF 3 ・xH 2 O, CrCl 3 ・xH 2 O, Cr(NO 3 ) 3 ・xH 2 O, (CH 3 CO 2 ) 2 Cr x H 2 O, (CH 3 CO 2 ) 7 Cr 3 (OH) 2 ・xH 2 O, Cr 2 (SO 4 ) 3 ・xH 2 O, CrK(SO 4 ) 2 ・xH 2 In a water bath containing a trivalent chromium salt selected from the group consisting of O (Step A1-1), Then, optionally, - Hydrogen peroxide (H 2 O 2 ), ammonium fluoride (NH 4 F), potassium fluorozirconate (K 2 ZrF 6 ), potassium permanganate (KMnO 4 ), sodium permanganate (NaMnO 4 (Step A1-2), in a water bath containing an oxidizing compound selected from the group consisting of The method according to any one of the preceding claims, characterized in that it comprises a step A1) of immersing the part.
9. 9. The method according to any one of claims 1 to 8, characterized in that it comprises, before step D) and after the sealing treatment according to step B), a step C) of a final hot water sealing treatment in deionized water at a temperature above 96°C and with a resistivity of ≥ 0.01 MOhm.
10. The following steps: A) an anodization step carried out under conditions according to claim 3; B) sealing the anode layer formed on the part at the end of step A), the sealing being carried out under conditions as described in claim 1; D) a fiber laser marking step having one or more of the features of claim 1.
11. The following steps: A) an anodization step carried out under conditions according to claim 3; A1) a step of immersing the part, wherein step A1-1) and the subsequent step A1-2) are carried out under conditions as claimed in claim 8; B) sealing the anode layer formed on the part at the end of step A), the sealing being carried out under conditions as described in claim 1; D) a fiber laser marking step having one or more of the features according to claim 1; The method according to any one of claims 1 to 8, characterized in that it comprises
12. The following steps: A) an anodization step carried out under conditions according to claim 3; A1) a step of immersing the part, wherein step A1-1) and the subsequent step A1-2) are carried out under conditions as claimed in claim 8; B) sealing the anode layer formed on the part at the end of step A), the sealing being carried out under conditions as described in claim 1; C) a final hot water sealing treatment under the conditions described in claim 9; D) a fiber laser marking step having one or more of the features according to claim 1; The method according to any one of claims 1 to 9, characterized in that it comprises:
13. The following steps: A) an anodization step carried out under conditions according to claim 3; A1) immersing the part, step A1-1) being carried out under conditions as claimed in claim 8; B) sealing the anode layer formed on the part at the end of step A), the sealing being carried out under conditions as described in claim 1; D) a fiber laser marking step having one or more of the features according to claim 1; The method according to any one of claims 1 to 8, characterized in that it comprises
14. The following steps: A) an anodization step carried out under conditions according to claim 3; Im) infiltrating said anodized part at the end of step A) in a bath of an organic or inorganic dye, then, optionally, A1) a step of immersing said part, where step A1-1) and the subsequent step A1-2) are carried out under conditions as claimed in claim 8; B) sealing the anode layer formed on said part at the end of step A), the sealing being carried out under conditions as described in claim 1; D) a fiber laser marking step having one or more of the characteristics according to claim 1; The method according to any one of claims 1 to 8, characterized in that it comprises
15. Use of the marking method according to any one of claims 1 to 14 for the manufacture or marking of aluminium or aluminium alloy parts intended for the aviation, aerospace, automotive, railway, watchmaking, medical, nuclear and oil industries, etc.
Citation Information
Patent Citations
Marking of an anodized layer of an aluminium object
CN1336878A
Marking of anodized layers of aluminum objects
JP2003513828A
Laser marking method
JP2010064144A
Laser system and method for wide range modification
JP2018507782A
Surface treatment method for aluminum parts
JP2023511727A