Molded parts of flame-retardant elastomer compositions for structural fire protection and method for producing corresponding molded parts - Patents.com

A crosslinker system combining sulfur and peroxide crosslinkers with a double bond-containing elastomer and vinyl acetate polymer improves mechanical properties and lowers glass transition temperature, addressing the limitations of conventional materials for structural fire protection in extreme cold.

JP2024542552AActive Publication Date: 2024-11-15HILTI AG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024531138
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-11-14
Publication Date
2024-11-15
Estimated Expiration
2042-11-14

AI Technical Summary

Technical Problem

Conventional elastomeric materials used for structural fire protection lack optimal mechanical properties and high glass transition temperatures, especially when combined with flame retardants, limiting their effectiveness in extreme low-temperature environments.

Method used

A crosslinker system comprising a sulfur crosslinker and a small amount of peroxide crosslinker is used to combine a double bond-containing elastomer and a vinyl acetate-containing thermoplastic polymer, resulting in a molded part with improved glass transition temperature and mechanical properties.

Benefits of technology

The combination achieves a lower glass transition temperature, expanding the usable temperature range and maintaining desirable mechanical properties, making it suitable for applications in extreme cold environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542552000001_ABST
    Figure 2024542552000001_ABST
Patent Text Reader

Abstract

The present invention relates to a molded part for structural fire protection, which can be produced or has been produced by vulcanizing a flame-retardant elastomer composition comprising a polymer blend of a double bond-containing elastomer and a vinyl acetate-containing thermoplastic polymer, and a crosslinker system comprising a sulfur crosslinker or a sulfur-containing crosslinker and a peroxide crosslinker, and which comprises at least one flame retardant, wherein the sulfur crosslinker or the sulfur-containing crosslinker is present in the crosslinker system in an amount greater than the peroxide crosslinker. The present invention further relates to a corresponding method for producing such a molded part, and to the use of such a molded part for applications with a minimum approved use temperature of -40°C or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] explanation The present invention relates to a molded part for structural fire protection, which can be produced or has been produced by vulcanizing a flame-retardant elastomer composition comprising a double bond-containing elastomer and a vinyl acetate-containing thermoplastic polymer, a crosslinker system comprising a sulfur crosslinker or a sulfur-containing crosslinker and a peroxide crosslinker, and at least one flame retardant, wherein the sulfur crosslinker or the sulfur-containing crosslinker is present in the crosslinker system in greater amounts than the peroxide crosslinker. The present invention further relates to a method for producing the corresponding molded part, and to the use of the molded part for applications with a minimum allowable use temperature of -40°C or less. [Background technology]

[0002] Elastic elements made, for example, from rubber or raw rubber, do not have the flame retardant or fire protection properties required in some applications, partly based on standards or regulations. It is known that flame retardants or fire retardants can be added to elastomers or rubber or natural rubber to give them the desired flame retardant properties. However, such additives usually reduce the elastic properties, which often results in the fact that such elements made of rubber or raw rubber do not meet or even exceed the necessary elastic properties in terms of the desired static and dynamic properties. It is therefore not possible to fully meet the required fire protection regulations, for example when used as spring or damping elements or similar elements in vehicles, which are usually subjected to high dynamic loads.

[0003] Due to this problem, it has been suggested that elements should not be made entirely of elastomers with flame retardants, but that such elements should only be provided with a flame retardant coating. Such composite elements are described, for example, in DE 38 31 894 A1 or WO 2010 / 069842 A1.

[0004] Of essential importance to the properties of elastomers is the crosslinker system used to convert the initially flowable rubber into an elastomeric material with typical elastomeric properties. Properties such as hardness, modulus, strength, elongation at break, tear resistance and elasticity can be adjusted to the desired level by the type and density of crosslinks.

[0005] Furthermore, polymer compositions containing flame retardants are known from the prior art, which can be formed, for example, from mixtures of ethylene vinyl acetate and ethylene propylene diene monomer rubbers, which are partially crosslinked with silanes, but mostly crosslinked by peroxides or irradiation.

[0006] Such mixtures are mainly used for the coating of cables or wires. For example, EP-A-2 343 334 describes flame-retardant compositions of EVA, EPDM and LLDPE crosslinked with a peroxide crosslinker system based on dicumyl peroxide. Peroxides are often used as crosslinkers when crosslinking rubbers that do not contain double bonds and / or when achieving a particularly high crosslink density and tight mesh structure, which in turn has a positive effect on mechanical properties such as compression set, especially at high temperatures. On the other hand, a high crosslink density and short crosslink bridges usually result in a lower elongation at break compared to materials of the same hardness. If the surface of the product is not further treated, peroxide crosslinking requires the exclusion of atmospheric oxygen during the crosslinking process. Furthermore, peroxide crosslinker systems have a negative effect on elastic and dynamic properties, especially if the composition also contains a large amount of flame retardant. Finally, cyclic crosslinkers also have the disadvantage of being relatively expensive, especially when compared to sulfur as crosslinker.

[0007] To solve these problems, EP 2 880 093 proposes mixtures of double bond-containing elastomers, such as EPDM, and vinyl acetate-containing thermoplastic polymers, such as EVA, vulcanized exclusively with sulfur or a sulfur-containing crosslinking agent system. The sulfur crosslinking agent is intended to ensure that only the double bond-containing elastomer is involved in the crosslinking and that a material with high elongation at break is obtained.

[0008] In structural fire protection, one usually tries to prevent mainly the passage of smoke gases, as well as the transfer of heat from one room to the next, or from different building areas to adjacent areas, due to the fire. Obviously, for fire protection here, the closure of the passages in the walls or ceilings that exist between adjacent rooms or building areas must be taken into account. Of particular importance here are the passages of electrical wires and pipes or ventilation flaps.

[0009] Conventional elastomeric materials that can be used here for sealing purposes often use sulfur crosslinkers, which are said to provide advantageous dynamic properties and good filling with flame retardants. Here, reference can be made by way of example to the aforementioned EP 2880093. However, these materials do not have optimal properties in terms of glass transition temperature. The glass transition temperature influences the potential use temperature of the material, below which the material becomes inflexible and can no longer provide the desired elastomeric properties. Against this background, it is desirable to have materials for producing moldings for structural fire protection that have as low a glass transition temperature as possible in the vulcanized state, thereby broadening the temperature range that can be addressed by such components. In other fields of use, the materials should provide properties as comparable as possible to conventional materials based on double bond-containing elastomers and vinyl acetate-containing thermoplastic polymers. A low glass transition temperature would be particularly advantageous in applications in regions and areas around the world where the outside air temperature can fall to the range of -40°C or lower, such as, for example, pipeline systems in Siberia or the Arctic.

[0010] Against this background, there was a need for elastomeric compounds for producing moldings for structural fire protection, and corresponding moldings which exhibit mechanical properties as similar as possible to those of commercially available products, but which have a lower glass transition temperature and encompass a wider range of use temperatures. The present invention addresses this need. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In the research that is the basis of this application, it has surprisingly been found that when a molding is prepared from a composition that includes a double bond-containing elastomer and a vinyl acetate-containing thermoplastic polymer, and the composition is crosslinked with a mixture of a peroxide crosslinker and a sulfur crosslinker or a sulfur-containing crosslinker, improved glass transition temperature properties and advantageous elastic and mechanical properties can be obtained. In this case, a small amount of the peroxide crosslinker is sufficient to achieve a significantly lower glass transition temperature, so that the peroxide crosslinker can be used in a mixture with a sulfur crosslinker or a sulfur-containing crosslinker. The lower glass transition temperature of the crosslinked molding can expand the temperature range in which the molding with elastomeric properties can be used.

[0012] Thus, according to a first aspect, the present invention relates to a moulded part for structural fire protection which can be produced or has been produced by vulcanising a flame-retardant elastomeric composition, the moulded part containing as polymer components i) a double bond-containing elastomer and ii) a vinyl acetate-containing thermoplastic polymer, the polymer components being present as a homogeneous polymer blend, a crosslinker system consisting of a sulphur or sulphur-containing crosslinker and a peroxide crosslinker, the amount of peroxide crosslinker being less than the amount of the sulphur or sulphur-containing crosslinker, and a flame retardant or a combination of flame retardants.

[0013] In this context, the term "molded parts for structural fire protection" refers to shaped parts used in applications in which the spread of fire or gas, e.g. fire gases, from one space to another adjacent space or from different building areas to adjacent areas is prevented or at least slowed down. Molded parts of this kind are usually designed to be inserted in a form that fits tightly into a wall opening between rooms or building areas, the cross section of the opening may be circular, rectangular or square. In contrast, for example cable insulation, which is primarily intended to prevent the combustion of the insulation itself, is not a shaped part for structural fire protection within the meaning of the invention described herein. Molded parts for structural fire protection are typically dimensioned based on the dimensions of the opening in which they are used, i.e. the length of the shaped part is equal to or greater than the thickness of the wall, but not significantly longer (e.g. not more than 5 times, preferably not more than 2 times the thickness of the wall).

[0014] In the context described herein, the term "building area" also encompasses areas of fixed, immobile structures ("buildings"), including technical and industrial installations in the land and offshore sectors, wind and solar installations, and areas of mobile structures, such as ships in particular, which have areas or units separated from one another for fire protection purposes to prevent gas exchange.

[0015] The description "for structural fire protection" does not exclude that the molded part performs other functions, such as sealing against the passage of gases, water, sound (to improve acoustics) or pathogens such as bacteria-containing aerosols, mold or its spores, etc. The envisagement of such functions is obviously desirable and preferred for the molded part according to the invention.

[0016] Using only small amounts of peroxide crosslinker has the advantage that the cost of the crosslinker system can be minimized.

[0017] The double bond-containing elastomer is preferably a homopolymer, copolymer or terpolymer of or having diene monomer units. Particularly suitable are terpolymers of ethylene, propylene and a diene-containing termonomer, preferably the termonomer content in the terpolymer is at least 2% to 12% by weight.

[0018] It is particularly advantageous if the elastomer contained in the double bond is a rubber with unsaturated side groups, in particular ethylene-propylene-diene rubber (EPDM). Ethylene-propylene-diene monomer rubbers (EPDM) have great advantages in case of fire due to their low smoke density and low toxicity, but are not fire resistant per se. On the other hand, EPDM rubbers can be highly filled with fillers and plasticizers and therefore can absorb a high proportion of flame retardants in solid and liquid form. The hardness and mechanical properties of EPDM rubber can therefore be adjusted over a wide range, making the rubber advantageous in terms of resistance to weathering, UV rays, ozone and heat.

[0019] Particularly useful EPDM rubbers in the flame retardant elastomer composition from which the molded articles of the present invention are formed are 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-cyclopentadiene, dicyclopentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,4-hexadiene, 1,4-cyclohexadiene, tetrahydrofuran ... The ethylene-propylene-diene monomer rubber (EPDM) comprises non-conjugated diene monomer units selected from the group consisting of ethylene, propylene and 5-ethylidene-2-norbornene (ENB), 5-methylene-2-norbornene (MNB), 1,6-octadiene, 5-methyl-1,4-hexadiene, 3,7-dimethyl-1,6-octadiene, 5-isopropylidene-2-norbornene and 5-vinyl-norbornene. It is particularly advantageous if the ethylene-propylene-diene monomer rubber (EPDM) is a terpolymer of ethylene, propylene and 5-ethylidene-2-norbornene (ENB) or dicyclopentadiene (DCPD), preferably with a termonomer content (according to ASTM D 6047) of at least 2 to 12% by weight, in particular 4 to 12% by weight, based on the terpolymer. The most preferred diene component for EPDM rubber is 5-ethylidene-2-norbornene (ENB).

[0020] In the research on which the present invention is based, it was also found that very favorable properties are obtained when the EPDM is formed from a mixture of two EPDM grades, one of which has a diene content in the range of 8-12% by weight and the other of which has a diene content in the range of 4-7% by weight. Furthermore, in this case, other EPDM grades may also be present, but these are preferably present in the mixture in an amount of 5% by weight or less, in particular 2% by weight or less, based on the total amount of EPDM with high and low diene content. In the mixture, the EPDM with a diene content in the range of 8-12% by weight preferably constitutes the predominant proportion of EPDM (i.e. 50-95% by weight, preferably 60-80% by weight of the total EPDM in the mixture).

[0021] The thermoplastic vinyl acetate-containing polymer contained in the elastomer composition forming the molded article of the present invention is preferably a vinyl acetate homopolymer, copolymer or terpolymer, particularly preferably polyvinyl acetate (PVAc) or ethylene vinyl acetate (EVA). For ethylene vinyl acetate copolymers, the vinyl acetate content is preferably in the range of 40 to 75% by weight, particularly preferably 50 to 65% by weight.

[0022] Alternatively, or in addition, it is preferred that the melting temperature or beginning of the melting range of the vinyl acetate containing polymer is below 150°C, preferably below 100°C.

[0023] The ratio of polymer components i) and ii) in the elastomeric composition according to the invention is preferably in the range of from 5:1 to 20:1, in particular from 6:1 to 12:1, i.e. the double bond-containing elastomer is present in excess of the vinyl acetate-containing thermoplastic polymer.

[0024] All peroxide crosslinkers known to those skilled in the art can be considered as peroxide crosslinkers in the crosslinker system of the present invention. Dialkyl peroxides and ketal peroxides are particularly useful. Suitable dialkyl peroxides include dicumyl peroxide, di-t-butyl peroxide, t-butyl-cumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)-hexane, 2,5-dimethyl-2,5-bis(t-butylperoxy)-hexyne-(3), α,α'-bis(t-butylperoxy)-diisopropylbenzene, di-t-amyl peroxide, 1,3,5-tris(2-t-butylperoxy-isopropyl)benzene, 1-phenyl-1-t-butylperoxy-phthalide. Suitable ketal peroxides include 1,1-bis(t-butylperoxy)-3,3,5-trimethyl-cyclohexane, 1,1-bis(t-butylperoxy)-cyclohexane, 2,2'-bis(t-butylperoxy)-butane, ethyl-3,3-bis(t-butylperoxy)-butyrate, n-n-butyl-4,4-bis(t-butylperoxy)-valerate. Particularly preferred in the present invention is the use of 2,5-dimethyl-2,5-bis(t-butylperoxy)-hexane.

[0025] The ratio of the peroxide crosslinking agent to the polymer blend is preferably 0.2 to 1.5 phr, more preferably 0.5 to 1.2 phr, where "phr" refers to the total amount of the double bond-containing elastomer and the vinyl acetate-containing thermoplastic polymer contained in the polymer blend.

[0026] Sulfur (eg, in the form of ground sulfur) crosslinker, or sulfur-containing crosslinkers such as bis[3-(triethoxysilyl)propyl] polysulfide, or mixtures thereof, may be used as the sulfur crosslinker in the elastomeric composition of the present invention.

[0027] The proportion of the sulfur crosslinking agent or sulfur-containing crosslinking agent in the polymer blend is preferably in the range from 1 to 7 phr, in particular from 2 to 5 phr, particularly preferably from 2.8 to 4.0 phr.

[0028] For the purposes of the present invention, it is essential that the sulfur crosslinker or sulfur-containing crosslinker is present in greater amounts than the peroxide crosslinker, with "more" meaning that the weight percentage of the total amount of sulfur crosslinker or sulfur-containing crosslinker is higher than that of the peroxide crosslinker. Preferably, the peroxide crosslinker and the sulfur crosslinker or sulfur-containing crosslinker are present in a ratio of about 1:1.5 to 1:5, in particular 1:2 to 1:4, particularly preferably 1:2.5 to 1:3.8.

[0029] The flame retardant contained in the molded part according to the invention is not subject to any relevant restrictions, and may be, for example, an intumescent flame retardant (such as intumescent graphite) or a hydrolytic flame retardant, such as a metal hydroxide. In order to achieve good fire properties with as little influence as possible on the material properties, it has proven advantageous for magnesium hydroxide (MDH), aluminum hydroxide (ATH), antimony trioxide, nanoclay and / or zinc borate, preferably a synergistic mixture of two or more thereof, to be contained in the elastomer composition according to the invention. Preferably, the elastomer composition according to the invention contains aluminum hydroxide, alone or mixed with other flame retardants. In particular, the flame retardant(s) is / are solid and powdery or crystalline.

[0030] In most cases, the flame retardant is present in a relatively high proportion in the elastomer composition. Preferably, the elastomer composition contains 100 to 300 phr, in particular 140 to 250 phr, of the flame retardant. If the flame retardant content is below this level, it may no longer be possible in individual cases to ensure a sufficient flame retardant effect, whereas a higher proportion of flame retardant may have a significantly unfavorable effect on mechanical properties such as tensile strength, elongation at break, tear resistance or elasticity.

[0031] The elastomer composition for producing the moulded bodies according to the invention may contain, in addition to the abovementioned components, further additives and / or auxiliaries for desired control of the final properties of the moulded body.

[0032] The main class of such additives that can be used to control vulcanization or crosslinking are accelerators, each of which can specifically accelerate sulfur crosslinking or peroxide crosslinking. Accelerators commonly used for sulfur crosslinking include sulfenamides, such as N-cyclohexyl-2-benzothiazylsulfenamide (CBS), thiazoles, such as 2-mercaptobenzothiazole (MBT), dithiocarbamates, such as zinc dibenzyldithiocarbamate (ZBEC) or zinc dibutyldithiocarbamate (ZDBC), guanidines, such as diphenylguanidine (DPG), or thiophosphates. Suitable sulfur donors that can be added to control sulfur crosslinking include thiurams, such as tetramethylthiuram disulfide (TMDT) or tetramethylthiuram sulfide (TMTM), caprolactam disulfides or phosphoryl polysulfides. Such accelerators and sulfur donors can be advantageously included in the elastomeric composition according to the invention in a total proportion of 1 to 5 phr.

[0033] Antioxidants such as 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ) or 1,3-dihydro-4 (or 5)-methyl-2H-benzimidazole-2-thione can be used to assist in peroxide crosslinking. Such antioxidants and sulfur donors may be present in the elastomeric composition in a combined proportion of 1 to 5 phr.

[0034] Furthermore, the elastomeric composition may contain plasticizers, for example in the form of paraffinic mineral oils, or processing aids, for example in the form of Ca and Zn soaps of fatty acids, fatty alcohols or low molecular weight polyethylene or polyethylene glycol. Furthermore, additives such as ZnO or MgO can be added to improve the thermal stability and / or pigments for coloring or imparting UV protection, such as TiO2, UV stabilizers or carbon black. The proportion of plasticizers is preferably in the range of 5 to 50 phr, in particular 10 to 30 phr, more preferably 12 to 25 phr. Other auxiliaries and additives are advantageously included in the flame-retardant elastomeric composition in a maximum proportion of 20 phr, in particular 15 phr.

[0035] As flame retardant compositions which are particularly suitable in the context of the present invention for producing moldings according to the invention, compositions can be disclosed as follows: A mixture of a double bond-containing elastomer and a vinyl acetate-containing thermoplastic polymer; 130 to 250 phr of a flame retardant, preferably in the form of aluminum hydroxide; 10~30phr of plasticizer, 1 to 5 phr each of sulfur donors / accelerators for sulfur vulcanization and antioxidants; 5-30 phr, preferably 8-15 phr, of other additives and auxiliaries A crosslinker system comprising a sulfur or sulfur-containing crosslinker and a peroxide crosslinker, wherein the amount of the peroxide crosslinker is less than the amount of the sulfur or sulfur-containing crosslinker.

[0036] For use in fire protection purposes, it is preferred that the moldings according to the invention made from the flame-retardant elastomer composition do not contain any relevant amount of halogen, because in the event of a fire, toxic hydrogen halides can be released from halogen-containing compounds.Therefore, it is preferred that in the moldings according to the invention, the polymeric components of the elastomer composition, preferably the entire composition, do not contain halogen.

[0037] The moldings according to the invention can be made only from the flame-retardant elastomer compound or can contain further components, such as reinforcements. In one embodiment, the surface of the molding is made only from the flame-retardant elastomer mixture, and another material is present inside the molding.

[0038] As already mentioned, the molded parts according to the invention are molded parts that can be used for structural fire protection, and their dimensions are usually adapted to the wall thickness in which they are used. Here, the molded parts according to the invention preferably have an aspect ratio of at most 10, particularly preferably at most 5. The "aspect ratio" in this case refers to the ratio of the maximum to the minimum spatial extent of the molded part.

[0039] In a particularly preferred embodiment, the molded part according to the invention is a ventilation flap or a component thereof. In another particularly preferred embodiment, the molded part according to the invention is a device for the fire-resistant passage of conduits, cables, tubes, etc. through an opening arranged in a wall or shaft, formed in at least one rectangular support frame. In this case, the device comprises one or more packing pieces that can be inserted into the rectangular support frame and have a passage of the flame-retardant elastomer composition extending over the depth of the rectangular support frame.

[0040] For the sake of clarity, here the moulded part according to the invention refers to the entire device, but it should be noted that it may also be formed from a number of individual parts (in particular a number of packing pieces and, where appropriate, further components), in which case the rectangular support frame is not part of the device.

[0041] In a preferred embodiment, the device comprises at least one unit of two packing pieces formed from two symmetrically shaped sealing elements, the sealing elements having one or more substantially semi-cylindrical recesses, arranged one above the other such that one or more cylindrical recesses are formed. Advantageously, in this case, the device may have two semi-cylindrical insert parts, each formed with a semi-cylindrical recess, arranged opposite each other such that the recesses form a passage adapted for the insertion of a conduit.

[0042] The device may contain exactly two packing pieces (=1 pair), or a multiple of two, which may be inserted into a rectangular support frame (e.g. in a 2x2, 3x2, 4x2, or 4x4 pair arrangement). In the case of an odd number of pairs of packing pieces, the space free to the rectangular support frame may be filled by a molding (as a "filling module"), the dimensions of which exactly match the free space. Such a filling module is also advantageously formed from the flame-retardant elastomeric composition described above. Similarly, a plurality of such filling modules may be arranged in a rectangular support frame, which in combination with the packing pieces forms the device.

[0043] With regard to the above-mentioned device, it is further preferred that semi-annular ribs are formed in the wall defining the recess in the sealing element and semi-annular grooves are formed between these ribs. Some of these grooves may be formed with recesses, preferably extending over only a portion of the semi-annular wall. In this embodiment, it is further preferred that the semi-cylindrical insert part is provided with projections corresponding to the grooves and recesses in the wall defining the sealing element, which projections engage in the grooves and recesses so that when the insert part is placed in the sealing element, it cannot be displaced in the direction of the defined path or rotate around this path. In this way, the insert part inserted in the sealing element is prevented from moving or rotating. Such a sealing element is described in detail, for example, in EP 1 134 472 B1, the relevant content of which is incorporated in its entirety into the present application by reference.

[0044] In the case where the device has a semi-cylindrical insert, the device may further have a molded body component, the dimensions of which are adapted to the dimensions of the passage formed by the semi-cylindrical insert and which may be inserted into the semi-cylindrical insert as a placeholder for later occupying said passage with a cable. Preferably, these placeholders also have protrusions which can engage with corresponding recesses in the semi-cylindrical insert and fix the position of the placeholder in the insert. Preferably, the placeholders are also formed from the flame-retardant elastomer composition described above. [Brief description of the drawings]

[0045] The above mentioned device is shown in more detail in Figures 1 to 5. In the drawings: [Figure 1] FIG. 2 is a front view of a packing piece having two sealing elements. [Diagram 2] FIG. [Diagram 3] FIG. 2 is a longitudinal cross-sectional view of a sealing element. [Figure 4] FIG. [Diagram 5] FIG.

[0046] The cubic packing piece 1 shown in Fig. 1 consists of two symmetrically formed sealing elements 11, each formed with a substantially semi-cylindrical recess and serving to receive a semi-cylindrical insert 21 also formed with a semi-cylindrical recess, through which the conduit 3 can be inserted. The sealing elements 11 and the insert 21 arranged therein must be designed to tightly surround the conduit 3 in order to ensure the desired safety against the passage of fire gases.

[0047] 2 and 3 show a top view and a longitudinal cross-section of a sealing element 11 having ribs 12 and grooves 13, as well as an additional recess 14 which, unlike grooves 13, does not extend over the entire semicircular inner surface of the sealing element.

[0048] Figures 4 and 5 show top and side views of the insert part 21 with the grooves 22 and ribs 23 as well as the protrusions 24. Figure 5 also shows semi-annular ribs 25 on the inner wall of the insert part and semi-annular grooves 26 between them. The ribs can be used to compensate for differences in thickness of the inserted cable to the extent that the ribs can displace it with a given flexibility. When the insert part is inserted into the sealing element, the ribs 23 and protrusions 24 engage with the corresponding grooves 13 and recesses 14 of the sealing element.

[0049] In a further aspect, the invention relates to the use of a moulded part, as detailed above, for structural fire protection applications, the moulded part being preferably inserted into a wall opening or a wall opening between two rooms and sealing said opening in the contact area between the moulded part and the wall. In such applications, pipes or other conduits may be integrated into or inserted into the moulded part.

[0050] In a further aspect, the present invention provides a method for producing the above-mentioned molded body, comprising the steps of: a) mixing the aforementioned polymer components to form a homogeneous mixture, in particular subsequently incorporating a crosslinker system, a flame retardant and optional further additives and / or auxiliaries, while avoiding crosslinking and / or vulcanization; b) introducing said mixture into a mold; c) subsequently vulcanizing said mixture; d) demolding the molded body formed in c); The present invention relates to a method comprising the steps of:

[0051] Mixing is conveniently carried out under conditions where crosslinking or vulcanization does not occur, i.e. preferably at a temperature below 110° C. Subsequent vulcanization can be carried out at elevated temperatures, for example in the range of 130° C. to 200° C., especially 130° C. to 170° C., optionally under pressure. During vulcanization crosslinking of the polymeric components occurs as a result of activation of the crosslinking agent.

[0052] The elastomeric compositions used to produce the moulded bodies according to the invention preferably have at least one of the following properties after vulcanisation: i) a glass transition temperature, measured by DSC, of ​​at most -39°C, in particular at most -40°C, particularly preferably at most -41°C; ii) a compression set in the range of 10 to 40%, preferably 15 to 25%, measured at 70° C. / 24 h according to DIN ISO 815, and / or a compression set in the range of 45 to 75%, preferably 55 to 68%, measured at 100° C. / 24 h according to DIN ISO 815, iii) a Shore A hardness of 65 to 85, preferably 70 to 83, measured according to DIN ISO 7619-1 (2012); iv) an elongation at break of 200 to 600%, preferably 300 to 500%, measured according to DIN 53504; v) A tear resistance measured according to DIN ISO 34-1A of >2.5 N / mm, preferably >3.5 N / mm.

[0053] Yet another aspect of the invention relates to the use of the above-mentioned molded parts for applications with a minimum allowable use temperature below -40° C. Preferred applications of this kind include buildings, technical and industrial installations, wind and solar installations, and wall or ceiling penetrations in ships, or pipelines and cables, etc., in the onshore and offshore sectors, especially when located in regions and areas around the world where very low outdoor temperatures in the range of up to -40° C. can occur.

[0054] A further aspect of the invention relates to the use of the moulded parts described above for sealing buildings against water, gas, sound or pathogens, in particular pathogens in the form of bacteria or moulds.

[0055] With regard to these aspects, the preferred embodiments explained in connection with the moulded parts according to the invention apply as preferred in an analogous manner, unless a contradiction arises.

[0056] Hereinafter, the present application will be described in more detail by means of some embodiments, which should by no means be construed as limiting the scope of the present application. EXAMPLES

[0057] The compositions shown in Table 1 below were homogenized in a mixer and then vulcanized under nitrogen atmosphere at a temperature of 180° C. for 10 minutes (2 mm thick sheets) or 20 minutes (6 mm thick sheets). The mechanical properties of the plates were subsequently measured. To determine the glass transition temperature, the mixtures were first equilibrated at −120° C. for 15 minutes and then heated to 250° C. with a heating rate of 10 K / min. The glass temperature was measured as the midpoint Tg according to DIN 51007. The measured mechanical properties are also shown in Table 1 below.

[0058] [Table 1]

[0059] From Table 1 it is clear that, despite otherwise comparable mechanical properties, a decrease in glass transition temperature of about 2.6° C. was observed for crosslinking in combination with sulfur and peroxide accelerators. This change allows the use of elastomer formulations suitable for applications at very low temperature extremes.

[0060] In a similar measurement of the glass transition temperatures in an air atmosphere, a Tg of −41.5° C. was measured for E1 and a Tg of −39.1° C. was measured for V1 (average value of two measurements).

Claims

1. A molded structural fire protection part that can be or has been produced by vulcanizing a flame retardant elastomeric composition, a double bond-containing elastomer and a vinyl acetate-containing thermoplastic polymer as polymeric components, the polymeric components being present as a homogeneous polymer blend; a crosslinker system of a sulfur crosslinker or a sulfur-containing crosslinker and a peroxide crosslinker, the amount of the peroxide crosslinker being less than the amount of the sulfur crosslinker or the sulfur-containing crosslinker; and a flame retardant or combination of flame retardants.

2. 2. The molded part according to claim 1, characterized in that the peroxide crosslinking agent is present in the polymer blend of the flame retardant elastomeric composition in a proportion of 0.2 to 1.5 phr, preferably 0.5 to 1.2 phr.

3. 3. The molded part according to claim 1 or 2, characterized in that the sulfur crosslinker or sulfur-containing crosslinker is present in the polymer blend of the flame-retardant elastomeric composition in a proportion of 1 to 7 phr, preferably 2 to 5 phr, particularly preferably 2.8 to 4.0 phr.

4. 4. Moulded part according to at least one of claims 1 to 3, characterised in that the double bond-containing elastomer in the flame-retardant elastomer composition is a homopolymer, copolymer or terpolymer of or respectively having diene monomer units, in particular a terpolymer consisting of ethylene, propylene and a diene-containing termonomer, preferably with a termonomer content of at least 2% to 12% by weight, based on the terpolymer.

5. The double bond-containing elastomer in the flame retardant elastomer composition is a rubber having unsaturated pendant groups, in particular an ethylene-propylene-diene rubber (EPDM), preferably 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-cyclopentadiene, dicyclopentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 1,4-hexadiene, 1,4-cyclohexadiene, tetrahydroindene, methyltetrahydroindene, ethylidenenorbornene or 5-ethylidene-2-norbornene.

5. The molded part according to claim 1, further comprising non-conjugated diene monomer units selected from the group consisting of ethylene, propylene and 5-ethylidene-2-norbornene (ENB) or dicyclopentadiene (DCPD), the non-conjugated diene monomer units being selected from the group consisting of ethylene, propylene and 5-ethylidene-2-norbornene (ENB) or dicyclopentadiene (DCPD).

6. 6. Moulded part according to at least one of claims 1 to 5, characterised in that the vinyl acetate containing polymer in the flame retardant elastomeric composition is a homopolymer, copolymer or terpolymer of vinyl acetate, in particular selected from the group consisting of polyvinyl acetate (PVAc) or ethylene vinyl acetate (EVA), and / or that it has a melting temperature or beginning of the melting range below 150°C, preferably below 100°C, and / or that it has a vinyl acetate content of 40 to 75% by weight.

7. 7. Moulded part according to at least one of claims 1 to 6, characterized in that the polymer components in the flame-retardant elastomeric composition are present in the elastomeric composition in a ratio of 5:1 to 20:1, in particular 6:1 to 12:

1.

8. The peroxide crosslinking agent in the flame retardant elastomer composition is selected from the group consisting of dialkyl peroxides, in particular dicumyl peroxide, di-t-butyl peroxide, t-butyl-cumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)-hexane, 2,5-dimethyl-2,5-bis(t-butylperoxy)-hexyne-(3), α,α'-bis(t-butylperoxy)-diisopropylbenzene, di-t-amyl peroxide, 1,3,5-tris(2-t-butylperoxy-isopropyl)benzene, 1-phenyl-1-t-butylperoxy-phthalide.

8. Moulded part according to claim 1, characterized in that the moulded part is present in the composition in the form of a dialkyl peroxide selected from the group consisting of 1,1-bis(tert-butylperoxy)-3,3,5-trimethyl-cyclohexane, 1,1-bis(tert-butylperoxy)-cyclohexane, 2,2'-bis(tert-butylperoxy)-butane, ethyl-3,3-bis(tert-butylperoxy)-butyrate, n-butyl-4,4-bis(tert-butylperoxy)-valerate.

9. 9. Moulded part according to at least one of claims 1 to 8, characterized in that the flame retardant in the flame retardant elastomeric composition is selected from the group comprising metal hydroxides, in particular in the form of magnesium hydroxide and / or aluminium hydroxide, and zinc borate, preferably present as aluminium hydroxide.

10. 10. Moulded part according to at least one of the preceding claims, characterized in that the flame retardant is present in the flame retardant elastomeric composition in a proportion of 100 to 300 phr, in particular 140 to 250 phr, of the elastomeric composition.

11. 11. Moulded part according to at least one of the preceding claims, characterized in that the flame-retardant elastomeric composition further comprises at least one additive and / or auxiliary selected from the group comprising colourants, especially in the form of one or more pigments, plasticisers, especially based on mineral oil, antiaging agents, especially for improving the thermal stability, and crosslinking accelerators.

12. Moulded part according to at least one of the preceding claims, characterized in that the polymeric components of the flame-retardant elastomeric composition, in particular the entire composition, are halogen-free.

13. 13. Moulded part according to at least one of claims 1 to 12, characterized in that the vulcanized flame-retardant elastomeric composition forming the moulded part has a Shore A hardness, measured according to DIN ISO 7619-1 (2012), in the range from 65 to 85, in particular from 70 to 83, and / or a glass transition temperature of at most -39°C, in particular at most -41°C.

14. Moulded part according to at least one of the preceding claims, characterized in that it has an aspect ratio of at most 10, preferably at most 5.

15. Moulded part according to at least one of the claims 1 to 14, designed as an apparatus for the fire-resistant passage of conduits, cables, tubes etc. through an opening arranged in a wall or shaft, having at least one rectangular support frame, characterized in that the apparatus comprises one or more packing pieces (1) with a path of elastic material extending over the depth of the rectangular support frame, the packing pieces being insertable into the rectangular support frame.

16. 16. A molded part according to claim 15, characterized in that the device comprises a number of packing pieces (1) formed from two symmetrically formed sealing elements (11), the sealing elements (11) having an approximately semi-cylindrical recess and arranged one above the other so as to form a cylindrical recess, and the device preferably further comprises two semi-cylindrical insert parts (21) also formed with a semi-cylindrical recess, whereby the recess forms a passage suitable for the insertion of a conduit.

17. 17. Moulded part according to claim 16, characterized in that the wall defining the recess of the sealing element (11) is formed with semi-annular ribs (12), between which semi-annular grooves (13) are formed, and in some of the grooves may be formed recesses (14), preferably extending only over a part of the semi-annular wall.

18. 18. The molded part according to claim 17, characterized in that the semi-cylindrical insert part (21) comprises ribs (23) and protrusions (24) which correspond to the grooves (13) and the recesses (14) of the walls defining the sealing element (11) and which engage with the grooves (13) and the recesses (14) when the insert part (21) is placed in the sealing element (11) in such a way that the insert part cannot be displaced in the direction of the formed path or rotate around the path.

19. A method for producing the molded body according to any one of claims 1 to 18. mixing the polymer components according to claim 1 to form a homogeneous mixture, in particular subsequently incorporating said crosslinker system, said flame retardant and optional further additives and / or auxiliaries, while avoiding crosslinking and / or vulcanization; introducing said mixture into a mold; followed by vulcanizing the mixture; and c) releasing the molded body formed in the mold.

20. Use of molded parts according to at least one of claims 1 to 18 for applications with a minimum permissible use temperature below -40°C, in particular for wall or ceiling penetrations, preferably gas piping, in buildings, technical and industrial installations, wind and solar installations, in the onshore and offshore sectors, as well as in ships.

Citation Information

Patent Citations

  • High-flame retardant rubber material in extrusion molding and preparation method thereof

    CN103146081A

  • Flame-resistant rubber composition and flame-resistant elastomer

    JP2002167482A

  • Flame-retardant polyolefin composition, electric wire and cable

    JP2009280631A

  • Rubber foam, laminate, and method for producing rubber foam

    JP2022038938A

  • Conductive roller for electrophotography

    JP2022168615A