Adhesive composition, positive electrode plate, secondary battery and power consuming device
A fluorine-containing polymer blend with tailored molecular weights and crystallinities addresses the adhesion and flexibility issues in secondary batteries, enhancing cycle performance and energy density by minimizing adhesive usage.
Patent Information
- Application Number
- JP2024531169
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-08-30
- Filing Date
- 2023-04-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-04-14
AI Technical Summary
Conventional adhesives used in secondary batteries require large amounts to ensure adhesion, which reduces the loading of active material and affects battery energy density and cycle performance.
An adhesive composition comprising a blend of fluorine-containing polymers with specific molecular weights and crystallinities, including a first fluorine-containing polymer with a weight average molecular weight of 3 million to 10 million, a second polymer with 600,000 to 1,100,000, and a third polymer with 0.5 million to 150,000, to achieve excellent adhesive strength and flexibility at low loadings.
The adhesive composition ensures sufficient adhesion and flexibility of electrode plates, improving battery cycle performance and safety while reducing the amount of adhesive used, thereby enhancing energy density and capacity retention.
Smart Images

Figure 2024542555000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to the field of secondary battery technology, and in particular to a fluorine-containing polymer, a manufacturing method, an adhesive composition, a positive electrode plate, a secondary battery, and a power consuming device.
[0002] [CROSS REFERENCE TO RELATED APPLICATIONS] This application is a continuation of PCT patent application No. PCT / CN2022 / 099187, filed on June 16, 2022, entitled "Adhesive and its manufacturing method and application", CN patent application No. 202211044631.4, filed on August 30, 2022, entitled "Fluorine-containing polymer, its manufacturing method and application, positive electrode slurry, secondary battery, battery module, battery pack, and power consumption device", and CN patent application No. 2022110520, filed on August 30, 2022, entitled "Fluorine-containing polymer, its manufacturing method and application, positive electrode slurry, secondary battery, battery module, battery pack, and power consumption device". See CN Patent Application No. 14.9, CN Patent Application No. 202211046282.X, filed on August 30, 2022, entitled "Adhesive, Manufacturing Method, Positive Electrode Plate, Secondary Battery, and Power Consumption Device," CN Patent Application No. 202211044756.7, filed on August 30, 2022, entitled "Adhesive, Manufacturing Method, Positive Electrode Plate, Secondary Battery, and Power Consumption Device," and CN Patent Application No. 202211043966.4, filed on August 30, 2022, entitled "Adhesive, Manufacturing Method, Positive Electrode Plate, Secondary Battery, and Power Consumption Device," all of which are incorporated by reference into this application. [Background technology]
[0003] In recent years, secondary batteries have been widely applied in energy storage power systems such as hydroelectric, thermal, wind and solar power plants, as well as in multiple fields such as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. As the application of secondary batteries becomes more widespread, higher requirements are being placed on their cycle performance, service life, etc.
[0004] Adhesives are commonly used materials in secondary batteries, and are in high demand for battery plates, separators, packaging, etc. However, conventional adhesives have poor adhesion and often require large amounts of additives to meet the adhesive strength requirements of the plates, which limits the improvement of the energy density of batteries. Therefore, conventional adhesives still need to be improved. Summary of the Invention
[0005] The present application has been made in view of the above problems, and has an object to provide an adhesive composition that can exhibit excellent adhesive strength even at a low addition amount and has good processability.
[0006] In order to achieve the above object, the present application provides an adhesive composition, the adhesive composition comprising a first fluorine-containing polymer, a second fluorine-containing polymer, and a third fluorine-containing polymer, wherein the first fluorine-containing polymer has a weight average molecular weight of 3 million to 10 million, the second fluorine-containing polymer has a weight average molecular weight of 600,000 to 1.1 million, and the third fluorine-containing polymer has a weight average molecular weight of 5,000 to 150,000.
[0007] This adhesive composition ensures that the electrode plates have sufficient adhesive strength even at a low additive amount, and can improve the cycle performance of the battery. Furthermore, this adhesive composition combines excellent flexibility and processability, and can further improve the safety and cycle performance of the battery.
[0008] In any embodiment, the mass content of the first fluorine-containing polymer is 10% to 86% based on the total mass of the adhesive composition.
[0009] The mass content of the first fluorine-containing polymer can be controlled within a suitable range to ensure that the adhesive composition has sufficient adhesive strength, so that the membrane layer does not fall off during the cycle process of the battery.In addition, a certain content of the first fluorine-containing polymer can effectively reduce the amount of adhesive composition used, and improve the loading amount of active material in the electrode plate.
[0010] In any embodiment, the mass content of the second fluorine-containing polymer is 10% to 86% based on the total mass of the adhesive composition.
[0011] The weight average molecular weight of the second fluorine-containing polymer is relatively low, which can effectively improve the crystallinity of the first fluorine-containing polymer, improve the flexibility of the electrode plate, and reduce the battery cost.
[0012] In either embodiment, the adhesive composition has a crystallinity of no more than 40%, optionally between 5%-40%.
[0013] Adding the second fluorine-containing polymer and the third fluorine-containing polymer to the first fluorine-containing polymer can effectively reduce the crystallinity of the adhesive, improve the flexibility of the electrode plate and the processability of the slurry, and improve the cycle performance of the battery.
[0014] In either embodiment, the first fluorine-containing polymer comprises structural units derived from vinylidene fluoride.
[0015] In any embodiment, the first fluorine-containing polymer further comprises a structural unit according to formula I: TIFF2024542555000002.tif32150 where R1 is a C group containing hydrogen, fluorine, chlorine, and at least one fluorine atom. 1-3 and alkyl groups.
[0016] In any embodiment, the first fluorine-containing polymer includes one or more of polyvinylidene fluoride, vinylidene fluoride-trifluorochloroethylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-trifluorochloroethylene-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer, and vinylidene fluoride-trifluorochloroethylene-tetrafluoroethylene-hexafluoropropylene copolymer.
[0017] In any embodiment, the second fluorine-containing polymer comprises a structural unit shown in formula II: TIFF2024542555000003.tif32150 where R2 and R3 are each independently a hydrogen atom, a halogen atom, or a C group containing at least one fluorine atom. 1-3 and an alkyl group.
[0018] The second fluorine-containing polymer contains chlorine.
[0019] The second fluorine-containing polymer containing chlorine can further reduce the crystallinity of the adhesive composition, improve the flexibility of the electrode plate, and enhance the safety performance of the battery.
[0020] In either embodiment, the chlorine content in the second fluorine-containing polymer does not exceed 8%, based on the total weight of the second fluorine-containing polymer.
[0021] The second fluorine-containing polymer having a chlorine content not exceeding 8% has a low crystallinity and can significantly improve the flexibility of the electrode plate.
[0022] In either embodiment, the crystallinity of the second fluorine-containing polymer does not exceed 47%, optionally does not exceed 30%.
[0023] In either embodiment, the weight average molecular weight of the second fluorine-containing polymer is 600,000 to 1,100,000.
[0024] In any embodiment, the second fluorine-containing polymer comprises at least one of polyvinylidene fluoride, chlorinated polyvinylidene fluoride, chlorinated poly(vinylidene fluoride-hexafluoropropylene), and poly(vinylidene fluoride-trifluorochloroethylene).
[0025] In either embodiment, the third fluorine-containing polymer comprises structural units shown in Formula III.
[0026] TIFF2024542555000004.tif32150 wherein R4 and R5 each independently contain at least one of hydrogen, fluorine, chlorine or a trifluoromethyl group.
[0027] In any of the embodiments, the end group of the third fluorine-containing polymer contains a hydroxyl group or an ester group. In any of the embodiments, the third fluorine-containing polymer includes one of polytetrafluoroethylene, polyvinylidene fluoride, poly(vinylidene fluoride-hexafluoropropylene) copolymer, poly(vinylidene fluoride-tetrafluoroethylene) copolymer, poly(vinylidene fluoride-trifluorochloroethylene) copolymer, and poly(vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene) copolymer.
[0028] A second aspect of the present application provides a fluorine-containing polymer, the fluorine-containing polymer comprising a structural unit derived from vinylidene fluoride and a structural unit represented by formula IV, TIFF2024542555000005.tif32150Here, R6 contains at least one of hydrogen, Cl, and F.
[0029] In any embodiment, the chlorine content in the fluorine-containing polymer does not exceed 8%, based on the total weight of the fluorine-containing polymer.
[0030] In any embodiment, the crystallinity of the fluorine-containing polymer does not exceed 30%.In any embodiment, the weight average molecular weight of the fluorine-containing polymer is 600,000 to 1,100,000.
[0031] In any embodiment, the fluorine-containing polymer comprises at least one of chlorinated polyvinylidene fluoride, chlorinated poly(vinylidene fluoride-hexafluoropropylene), and poly(vinylidene fluoride-trifluorochloroethylene).
[0032] A third aspect of the present application provides a method for producing a fluorine-containing polymer, the method comprising: employing a chlorinating agent to chlorinate polyvinylidene fluoride to produce a fluorine-containing polymer.
[0033] In any of the embodiments, the method specifically includes dispersing polyvinylidene fluoride in a solvent to prepare a polyvinylidene fluoride suspension, and adding an initiator and a chlorinating agent to chlorinate the polyvinylidene fluoride to prepare a fluorine-containing polymer.
[0034] In any embodiment, the chlorinating agent includes at least one of chlorine gas, hydrogen chloride, phosphorus pentachloride, phosphorus trichloride, sulfuryl chloride SO2Cl2, and phosgene COCl2.
[0035] In any embodiment, the initiator includes at least one of dibenzoyl oxide, dilauroyl peroxide, azobisisobutyronitrile (AIBN), and azobisisoheptonitrile (ABVN).
[0036] In either embodiment, the solvent comprises at least one of carbon tetrachloride and water.
[0037] A fourth aspect of the present application provides a positive electrode plate, the positive electrode plate including a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer including a positive electrode active material, a conductive agent, and the adhesive of any of the embodiments or the adhesive composition produced by the production method of any of the embodiments.
[0038] This positive electrode plate has excellent adhesive strength even with a low amount of adhesive added.
[0039] In any embodiment, the mass fraction of the adhesive composition does not exceed 1.5%, and optionally is 0.8%-1.2%, based on the total mass of the positive electrode membrane layer.
[0040] Controlling the mass fraction of the adhesive composition within an appropriate range can ensure that the electrode plate has sufficient adhesive strength while maintaining the flexibility of the electrode plate, and can also improve the cycle performance and safety performance of the battery.
[0041] In either embodiment, the positive electrode active material is a lithium-containing transition metal oxide.
[0042] In any embodiment, the lithium-containing transition metal oxide is at least one of lithium iron phosphate or lithium nickel cobalt manganese oxide, or doped modifications thereof, or conductive carbon-coated, conductive metal-coated, or conductive polymer-coated modifications thereof.
[0043] A fifth aspect of the present application provides a secondary battery, the secondary battery including an electrode assembly and an electrolyte, the electrode assembly including a separator, a negative electrode plate, and the positive electrode plate of the fourth aspect of the present application.
[0044] A sixth aspect of the present application provides a power consuming device, the power consuming device including the secondary battery of the fifth aspect of the present application. [Brief description of the drawings]
[0045] [Figure 1] 1 is a schematic diagram of a secondary battery according to an embodiment of the present application; [Diagram 2] FIG. 2 is an exploded view of the secondary battery according to the embodiment of the present application shown in FIG. [Diagram 3] 1 is a schematic diagram of a battery module according to an embodiment of the present application; [Figure 4] 1 is a schematic diagram of a battery pack according to an embodiment of the present application; [Diagram 5] FIG. 5 is an exploded view of the battery pack according to the embodiment of the present application shown in FIG. 4. [Figure 6] 1 is a schematic diagram of a power consuming device in which a secondary battery according to an embodiment of the present application is used as a power source; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0046] Hereinafter, with reference to the drawings, embodiments specifically disclosing the positive electrode active material and its manufacturing method, the positive electrode plate, the secondary battery, the battery module, the battery pack, and the electric device of the present application will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of well-known matters and duplicated description of the same structure may be omitted. This is to avoid the following description from becoming unnecessarily long and to allow those skilled in the art to easily understand. Note that the drawings and the following description are provided to allow those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0047] The "ranges" disclosed in this application are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, and the selected lower and upper limits define the boundaries of the particular range. Such defined ranges may be inclusive or exclusive of the extreme values, and may be arbitrarily combined, i.e., any lower limit may be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is understood that ranges of 60-110 and 80-120 are also envisaged. However, if 1 and 2 are listed as minimum range values, and 3, 4, and 5 are listed as maximum range values, the ranges 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are all envisaged. In this application, unless otherwise specified, the numerical range "ab" represents a shorthand representation of any combination of real numbers from a to b, where a and b are both real numbers. For example, the numerical range "0-5" represents a list of all real numbers between "0-5" already listed in this specification, and "0-5" is just a shorthand representation of combinations of these numbers. Also, expressing a parameter as an integer ≧2 is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0048] Unless otherwise stated, all the embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0049] Unless otherwise stated, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0050] Unless otherwise stated, all steps in this application may be performed in sequence or randomly, and preferably in sequence. For example, the method includes steps (a) and (b) to mean that the method may include steps (a) and (b) performed in sequence, or may include steps (b) and (a) performed in sequence. For example, the method mentioned above may further include step (c) to mean that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.
[0051] Unless otherwise specified, the terms "comprise" and "comprises" referred to in this application may be open ended or closed ended. For example, the terms "comprise" and "comprises" may further include or include other ingredients not listed, or may include or include only the ingredients listed.
[0052] Unless otherwise stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, "A or B" is satisfied if A is true (or exists) and B is false (or does not exist), if A is false (or does not exist) but B is true (or exists), or if both A and B are true (or exist).
[0053] Fluorine-containing polymers are one of the most widely used adhesives in secondary batteries at present. However, traditional fluorine-containing polymers have low viscosity, and often need to be added in large amounts to ensure effective adhesion of active materials, thereby achieving effective adhesion of electrodes. However, while increasing the amount of traditional fluorine-containing polymers reduces the load of active materials on electrodes, which affects the improvement of the energy density of batteries, adhesives with low content are also difficult to maintain sufficient adhesion during use, and are difficult to meet the market requirements for cycle performance of batteries.
[0054] [Adhesive composition] The present application provides an adhesive composition, comprising a first fluorine-containing polymer, a second fluorine-containing polymer, and a third fluorine-containing polymer, wherein the first fluorine-containing polymer has a weight average molecular weight of 3 million to 10 million, the second fluorine-containing polymer has a weight average molecular weight of 600,000 to 1.1 million, and the third fluorine-containing polymer has a weight average molecular weight of 5,000 to 150,000.
[0055] As used herein, the term "adhesive composition" refers to a mixture that forms a colloidal solution or dispersion in a dispersing medium.
[0056] In this specification, the term "fluorine-containing polymer" refers to a polymer whose main synthetic monomer is a fluorine-containing monomer, and the polymer includes, on the one hand, a chemically uniform aggregate of macromolecules produced by polymerization reaction, but with different degrees of polymerization, molar masses and chain lengths. On the other hand, the term also includes derivatives of such macromolecular aggregates formed by polymerization reaction, i.e. compounds obtained by reaction, for example addition or substitution, of functional groups in the macromolecules, and which may be chemically uniform or chemically heterogeneous. In this specification, the fluorine-containing polymer includes homopolymers and also copolymers.
[0057] As used herein, the term "weight average molecular weight" is the sum of the products of the weight fractions of molecules of different molecular weights in a polymer and their corresponding molecular weights.
[0058] In some embodiments, the dispersion medium of the adhesive composition is an oil-based solvent, examples of which include, but are not limited to, dimethylacetamide, N,N-dimethylformamide, N-methylpyrrolidone, acetone, dimethylcarbonate, ethylcellulose, and polycarbonate, i.e., the adhesive is dissolved in the oil-based solvent.
[0059] In some embodiments, the adhesive composition is used to hold the electrode active material and / or conductive agent in place and adhere them to the conductive metal members to form the electrode.
[0060] In some embodiments, the adhesive composition is used as a positive electrode adhesive to adhere a positive electrode active material and / or a conductive agent to form an electrode.
[0061] In some embodiments, the adhesive composition is used as a negative electrode adhesive to adhere a negative electrode active material and / or a conductive agent to form an electrode.
[0062] In some embodiments, the weight average molecular weight of the first fluorine-containing polymer is 3 million to 10 million. In some embodiments, the weight average molecular weight of the first fluorine-containing polymer is 3 million, 3.5 million, 4 million, 4.5 million, 5 million, 5.5 million, 6 million, 6.5 million, 7 million, 7.5 million, 8 million, 8.5 million, 9 million, 9.5 million, 10 million, or any number therein.
[0063] In some embodiments, the weight average molecular weight of the second fluorine-containing polymer is 600,000 to 1,100,000. In some embodiments, the weight average molecular weight of the second fluorine-containing polymer is optionally 600,000, 650,000, 700,000, 750,000, 800,000, 850,000, 900,000, 950,000, 1,000,000, 1,050,000, 1,100,000, or any number therein.
[0064] In some embodiments, the weight average molecular weight of the third fluorine-containing polymer is 5000-150000. In some embodiments, the weight average molecular weight of the second fluorine-containing polymer is optionally 5000, 10000, 20000, 30000, 40000, 50000, 60000, 70000, 80000, 90000, 10000, 110000, 120000, 130000, 140000, 150000 or any number therein.
[0065] In this application, the weight average molecular weight of the fluorine-containing polymer can be tested by selecting a method known in the art, for example, by adopting a gel chromatography method, for example, by adopting a Waters 2695 Isocratic HPLC type gel chromatograph (differential refractive index detector 2141). In some embodiments, the test method is to take a polystyrene solution sample with a mass fraction of 3.0% as the standard and select a matching chromatographic column (oil-based: Styragel HT5DMF7.8*300mm+Styragel HT4). Prepare a 3.0% adhesive glue solution with purified N-methylpyrrolidone (NMP) solvent, and leave the prepared solution for one day to prepare for use. During the test, first draw tetrahydrofuran into the syringe, wash, and repeat several times. Then draw 5 ml of the experimental solution, eliminate the air in the syringe, and wipe the needle tip to dry. Finally, slowly inject the sample solution into the injection port. After the reading has stabilized, the data is acquired and the weight average molecular weight is read.
[0066] The first fluorine-containing polymer, which has a weight-average molecular weight of 3 million to 10 million, can improve the adhesive strength of the electrode plate at a low addition amount and improve the capacity retention rate during the cycle process of the battery. The addition of the low molecular weight second fluorine-containing polymer and the third fluorine-containing polymer can effectively improve the processing performance of the slurry, improve the quality of the electrode plate, improve the brittleness problem of the electrode plate, reduce the processing and raw material costs, and the uniform adhesive composition can further improve the cycle performance of the battery.
[0067] In some embodiments, the mass content of the first fluorine-containing polymer is 10% to 86% based on the total mass of the adhesive composition.
[0068] In some embodiments, the mass content of the first fluorine-containing polymer, based on the total mass of the adhesive composition, is optionally 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 86%, or any number therein.
[0069] The mass content of the first fluorine-containing polymer can be controlled within a suitable range to ensure that the adhesive composition has sufficient adhesive strength, so that the membrane layer does not fall off during the cycle process of the battery.In addition, a certain content of the first fluorine-containing polymer can effectively reduce the amount of adhesive composition used, and improve the loading amount of active material in the electrode plate.
[0070] In some embodiments, the mass content of the second fluorine-containing polymer is 10% to 86%, based on the total mass of the adhesive composition.
[0071] In some embodiments, the mass content of the second fluorine-containing polymer, based on the total mass of the adhesive composition, is optionally 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 86%, or any number therein.
[0072] The weight average molecular weight of the second fluorine-containing polymer is relatively low, which can effectively improve the crystallinity of the first fluorine-containing polymer, improve the flexibility of the electrode plate, and reduce the battery cost.
[0073] In some embodiments, the adhesive composition has a crystallinity of no more than 40%, optionally between 5%-40%.
[0074] In some embodiments, the adhesive composition has a crystallinity of optionally 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, or any value therein.
[0075] As used herein, the term "crystallinity" refers to the proportion of crystalline regions in a polymer, and in the microstructure there are regions having some molecules that are stably arranged in an orderly fashion, and the regions in which the molecules are closely and regularly arranged are referred to as crystalline regions.
[0076] In the present application, the crystallinity test may be performed by selecting a method known in the art, for example, by adopting differential scanning calorimetry. In some embodiments, 0.5g of the adhesive composition is placed in an aluminum crucible, flattened, the crucible is covered with a lid, and the test is performed in a nitrogen gas atmosphere, with a purge gas of 50 ml / min, a protective gas of 70 ml / min, a heating rate of 10 ° C / min, and a test temperature range of -100 ° C - 400 ° C, using a US TA instrument model Discovery 250 differential scanning calorimeter (DSC) to remove thermal history.
[0077] In this test, the temperature change curve of the DSC / (Mw / mg) of the adhesive composition is obtained and integrated, and the peak area is the melting enthalpy ΔH (J / g) of the fluorine-containing polymer composition, and the adhesive crystallinity=ΔH / (ΔHm)×100%, where ΔHm is the standard melting enthalpy (crystalline heat of fusion) of the fluorine-containing polymer, and ΔHm=104.7 J / g.
[0078] By adding the second fluorine-containing polymer and the third fluorine-containing polymer to the first fluorine-containing polymer, the crystallinity of the adhesive can be effectively reduced, the flexibility of the electrode plate and the processability of the slurry can be improved, and the cycle performance of the battery can be improved.
[0079] In some embodiments, the first fluorine-containing polymer comprises structural units derived from vinylidene fluoride. In some embodiments, the first fluorine-containing polymer is a vinylidene fluoride homopolymer. In some embodiments, the first fluorine-containing polymer is a vinylidene fluoride copolymer.
[0080] In some embodiments, the first fluorine-containing polymer further comprises a structural unit according to formula I: TIFF2024542555000006.tif32150 where R1 is a C group containing hydrogen, fluorine, chlorine, and at least one fluorine atom. 1-3 and alkyl groups.
[0081] In some embodiments, R1 includes one or more of hydrogen, fluorine, chlorine, and a trifluoromethyl group.
[0082] In some embodiments, the first fluorine-containing polymer comprises one or more of polyvinylidene fluoride, vinylidene fluoride-trifluorochloroethylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-trifluorochloroethylene-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer, and vinylidene fluoride-trifluorochloroethylene-tetrafluoroethylene-hexafluoropropylene copolymer.
[0083] In some embodiments, the second fluorine-containing polymer comprises structural units according to formula II: TIFF2024542555000007.tif32150 where R2 and R3 are each independently a hydrogen atom, a halogen atom, or a C group containing at least one fluorine atom. 1-3 and an alkyl group.
[0084] In some embodiments, R2, R3 each independently comprise hydrogen, fluorine, chlorine, or a trifluoromethyl group.
[0085] In some embodiments, the second fluorine-containing polymer comprises chlorine.
[0086] The second fluorine-containing polymer containing chlorine can further reduce the crystallinity of the adhesive composition, improve the flexibility of the electrode plate, and enhance the safety performance of the battery.
[0087] In some embodiments, the second fluorine-containing polymer is produced by chlorinating a fluorine-containing polymer.
[0088] In some embodiments, the second fluorine-containing polymer is prepared by copolymerizing polyvinylidene fluoride monomers and chlorine-containing monomers.
[0089] In some embodiments, the chlorine content of the second fluorine-containing polymer is not more than 8% based on the total mass of the second fluorine-containing polymer.In some embodiments, the chlorine content of the second fluorine-containing polymer is 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8% or any value therein based on the total mass of the second fluorine-containing polymer.
[0090] The second fluorine-containing polymer having a chlorine content not exceeding 8% has a low crystallinity and can significantly improve the flexibility of the electrode plate.
[0091] In some embodiments, the crystallinity of the second fluorine-containing polymer is not more than 47%, and optionally not more than 30%. In some embodiments, the crystallinity of the second fluorine-containing polymer is 47%, 45%, 40%, 35%, 30%, 25%, 20%, 15%, 10%, 5%, 4%, 3%, or any number therein. In some embodiments, the weight average molecular weight of the second fluorine-containing polymer is 600,000-1.1 million. In some embodiments, the weight average molecular weight of the second fluorine-containing polymer is 600,000, 700,000, 800,000, 900,000, 1 million, 1.1 million, or any number therein.
[0092] In some embodiments, the second fluorine-containing polymer comprises at least one of polyvinylidene fluoride, chlorinated polyvinylidene fluoride, chlorinated poly(vinylidene fluoride-hexafluoropropylene), and poly(vinylidene fluoride-trifluorochloroethylene).
[0093] In some embodiments, the third fluorine-containing polymer comprises a structural unit shown in formula III: TIFF2024542555000008.tif32150 wherein R4 and R5 each independently contain at least one of hydrogen, fluorine, chlorine or a trifluoromethyl group.
[0094] In some embodiments, the end groups of the third fluorine-containing polymer contain hydroxyl or ester groups.
[0095] The third fluorine-containing polymer has a small weight average molecular weight and a high mass content of end group, so the end group has a relatively large effect on the performance of the third fluorine-containing polymer.The end group of the third fluorine-containing polymer contains a hydroxyl group or an ester group, which can effectively improve the adhesion of the third fluorine-containing polymer, and reduce the decrease in plate adhesion performance caused by adding the third fluorine-containing polymer with a low molecular weight.
[0096] The end group structure of the polymer can be studied by nuclear magnetic resonance techniques. 19 F-NMR and 1 The end group structure of the polymer can be analyzed by H-NMR. For example, dimethylsulfoxide is used as the solvent, CFCl3 is used as the fluorine spectrum standard, and TMS is used as the hydrogen spectrum standard.
[0097] In some embodiments, the third fluorine-containing polymer comprises one of polytetrafluoroethylene, polyvinylidene fluoride, poly(vinylidene fluoride-hexafluoropropylene) copolymer, poly(vinylidene fluoride-tetrafluoroethylene) copolymer, poly(vinylidene fluoride-trifluorochloroethylene) copolymer, and poly(vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene) copolymer.
[0098] In one embodiment of the present application, there is provided a fluorine-containing polymer, the fluorine-containing polymer comprising a structural unit derived from vinylidene fluoride and a structural unit represented by formula IV, TIFF2024542555000009.tif32150Here, R6 contains at least one of hydrogen, Cl, and F.
[0099] The fluorine-containing polymer containing chlorine can further reduce the crystallinity of the adhesive composition, improve the flexibility of the electrode plate, and enhance the safety performance of the battery.
[0100] In some embodiments, the fluorine-containing polymer is obtained by producing a fluorine-containing polymer after chlorination.
[0101] In some embodiments, the fluorine-containing polymer is prepared by copolymerizing vinylidene fluoride with a chlorine-containing monomer.
[0102] In some embodiments, the chlorine content of the fluorine-containing polymer is not more than 8% based on the total weight of the fluorine-containing polymer.In some embodiments, the chlorine content of the fluorine-containing polymer is 0.1%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, or any value therein based on the total weight of the fluorine-containing polymer.
[0103] The fluorine-containing polymer with a chlorine content not exceeding 8% has a low crystallinity and can significantly improve the flexibility of the electrode plate.
[0104] In some embodiments, the crystallinity of the fluorine-containing polymer does not exceed 30%.
[0105] In some embodiments, the crystallinity of the fluorine-containing polymer is optionally 30%, 25%, 20%, 15%, 10%, 5%, or any number therein. In some embodiments, the weight average molecular weight of the fluorine-containing polymer is 600,000-1.1 million. In some embodiments, the weight average molecular weight of the fluorine-containing polymer is 600,000, 700,000, 800,000, 900,000, 1 million, 1.1 million, or any number therein.
[0106] In some embodiments, the fluorine-containing polymer comprises at least one of polyvinylidene fluoride, chlorinated polyvinylidene fluoride, chlorinated poly(vinylidene fluoride-hexafluoropropylene), and poly(vinylidene fluoride-trifluorochloroethylene).
[0107] In one embodiment of the present application, a method for preparing a fluorine-containing polymer is provided, the method including the step of employing a chlorinating agent to chlorinate polyvinylidene fluoride to prepare a fluorine-containing polymer.
[0108] In some embodiments, the method specifically includes dispersing polyvinylidene fluoride in a solvent to produce a polyvinylidene fluoride suspension, and adding an initiator and a chlorinating agent to chlorinate the polyvinylidene fluoride to produce a fluorine-containing polymer.
[0109] In some embodiments, the chlorinating agent includes at least one of chlorine gas, phosphorus pentachloride (PCl5), hydrogen chloride (HCl), phosphorus trichloride (PCl3), sulfuryl chloride (SO2Cl2), and phosgene (COCl2).
[0110] In some embodiments, the initiator comprises at least one of dibenzoyl oxide, dilauroyl peroxide, azobisisobutyronitrile (AIBN), and azobisisoheptonitrile (ABVN).
[0111] In some embodiments, the solvent comprises at least one of carbon tetrachloride and water.
[0112] In one embodiment of the present application, there is provided a method for producing an adhesive composition, specifically comprising the steps of: Production of a first fluorine-containing polymer: A first polymerization reaction is carried out on a raw material containing a vinylidene fluoride monomer under polymerization conditions to produce a first fluorine-containing polymer, and the weight average molecular weight of the first fluorine-containing polymer is 3 million to 10 million; Preparation of a third fluorine-containing polymer: carrying out a second polymerization reaction under polymerization conditions to prepare a second fluorine-containing polymer, and the weight average molecular weight of the third fluorine-containing polymer is not more than 600,000; Blending: A first fluorine-containing polymer, a second fluorine-containing polymer having a weight average molecular weight of 600,000 to 1,100,000, and a third fluorine-containing polymer are blended to produce an adhesive composition.
[0113] As used herein, the term "blending" refers to the process of producing two or more substances as a macroscopically homogeneous material under certain conditions such as temperature and / or shear stress.
[0114] The adhesive manufacturing method is simple, environmentally friendly, reduces costs, and is favorable for industrial production. At the same time, the adhesive composition manufactured by this method can achieve both the flexibility of the electrode plate and the cycle performance of the battery at a low additive amount, and can improve the capacity retention rate during the cycle process of the battery.
[0115] In some embodiments, the synthesis step of the first fluorine-containing polymer comprises carrying out a polymerization reaction of a raw material including vinylidene fluoride monomer in a non-reactive gas atmosphere, under a reaction pressure of 6 MPa to 8 MPa and at a reaction temperature of 45°C to 60°C for 6 h to 10 h; adding a chain transfer agent, lowering the pressure in the reaction system to 2 MPa to 2.5 MPa, stopping the reaction, performing solid-liquid separation, and leaving a solid phase to produce the first fluorine-containing polymer.
[0116] In some embodiments, the step of synthesizing the first fluorine-containing polymer includes providing a raw material including a vinylidene fluoride monomer and a reaction solvent, carrying out a first-stage polymerization reaction to obtain a first product, carrying out a second-stage polymerization reaction of the first product in a non-aqueous gas atmosphere, and adding a chain transfer agent and carrying out a third-stage polymerization reaction to obtain the first fluorine-containing polymer.
[0117] The first product may refer to the reaction liquid obtained after the first-stage polymerization reaction, or may be a product obtained after the reaction liquid is purified after the first-stage polymerization reaction.
[0118] In some embodiments, multiple first products are mixed and subjected to a second-stage polymerization reaction in a non-aqueous gas atmosphere. That is, the second-stage polymerization reaction is the self-polymerization of the first products. As can be understood, multiple first products can be produced simultaneously in multiple reactors, or multiple times in one reactor. The multiple-stage synthesis method can improve the uniformity of the poly product.
[0119] By adopting the split polymerization method, it is possible to produce and obtain polyvinylidene fluoride with an ultra-high molecular weight, so that the adhesive can meet the demand for the adhesive strength of the electrode plate with a low addition amount, which is conducive to improving the loading amount of the positive active material in the electrode plate and is favorable for improving the capacity retention rate during the cycle process of the battery. At the same time, it is used to first form a first product in the first polymerization reaction, form a molecular chain segment with a target molecular weight in the second polymerization reaction, and adjust and control the molecular weight of the polymer in the third polymerization reaction, so as to avoid the reduction in the uniformity of the weight average molecular weight of polyvinylidene fluoride caused by the molecular weight being too high, and to improve the uniformity of the product. And split polymerization can increase the utilization rate of the reactor in the polyvinylidene fluoride production process, save time, and reduce the residence time of polyvinylidene fluoride in the reactor. It is used to further improve the production efficiency of polyvinylidene fluoride by combining the first polymerization reaction, the second polymerization reaction, and the third polymerization reaction with each other.
[0120] In some embodiments, the reaction temperature of the first stage polymerization reaction is 45° C. to 60° C. In some embodiments, the reaction temperature of the first stage polymerization reaction is optionally 45° C. to 50° C., 50° C. to 55° C., 55° C. to 60° C., or 45° C. to 55° C.
[0121] In some embodiments, the reaction time of the first stage polymerization reaction is 4h to 10h. In some embodiments, the reaction time of the first stage polymerization reaction is optionally 4h to 5h, 5h to 6h, 6h to 7h, 7h to 8h, 8h to 9h, 9h to 10h, 4h to 6h, 6h to 8h, 8h to 10h, or 5h to 10h.
[0122] In some embodiments, the initial polymerization pressure is 4 MPa to 6 MPa. In some embodiments, the initial polymerization pressure is optionally 4 MPa to 5 MPa, 5 MPa to 6 MPa. In some embodiments, the initial polymerization pressure is higher than the critical pressure of vinylidene fluoride.
[0123] In some embodiments, the reaction temperature of the second stage polymerization reaction is 60° C. to 80° C. In some embodiments, the reaction temperature of the second stage polymerization reaction is optionally 60° C. to 70° C., 70° C. to 80° C.
[0124] In some embodiments, the reaction time of the second stage polymerization reaction is 2h to 4h. In some embodiments, the reaction time of the second stage polymerization reaction is alternatively 2h to 3h, 3h to 4h.
[0125] In some embodiments, the reaction pressure of the second stage polymerization reaction is 6Mpa to 8Mpa. In some embodiments, the reaction pressure of the second stage polymerization reaction is selectively 6Mpa to 7Mpa, 7Mpa to 8Mpa.
[0126] In some embodiments, the reaction time of the third stage polymerization reaction is 1 h to 2 h.
[0127] By controlling the reaction pressure, reaction time and reaction temperature of the polymerization reaction at each stage within an appropriate range, the weight average molecular weight of polyvinylidene fluoride can be improved, and at the same time, the uniformity of the weight average molecular weight of the polymerization product can be controlled and the product can have a relatively low polydispersity coefficient, thereby improving the balance of the performance of the first polyvinylidene fluoride, so that the electrode plate has excellent adhesion even with a low additive amount of adhesive, and the cycle capacity retention of the battery can be further improved.
[0128] In some embodiments, the chain transfer agent comprises one or more of cyclohexane, isopropyl alcohol, methanol, and acetone.
[0129] A water-insoluble gas is a gas whose solubility is less than 0.1 L. Gas solubility is the pressure of a gas at 20°C of 1.013 x 10 5 The volume of the gas when dissolved in 1 L of water and saturated, is Pa. In some embodiments, the water-insoluble gas is one or more selected from nitrogen gas, oxygen gas, hydrogen gas, and methane.
[0130] In some embodiments, the amount of chain transfer agent used is between 1.5% and 3% of the total weight of vinylidene fluoride monomer. The amount of chain transfer agent used may even be, for example, 2% or 2.5%.
[0131] By controlling the amount of chain transfer agent used within an appropriate range, the chain length of the polymer can be made controllable, thereby obtaining a polymer with an appropriate molecular weight range and uniform distribution.
[0132] In some embodiments, the first stage polymerization reaction comprises: Adding a water solvent and a dispersant to the vessel and removing oxygen gas from the reaction system; Adding a first initiator and a pH adjusting agent to the vessel, adjusting the pH value to 6.5-7, and adding vinylidene fluoride monomer, and making the pressure in the vessel 4MPa-6MPa; After stirring for 30 to 60 minutes, the mixture is heated to 45° C. to 60° C. to carry out the first-stage polymerization reaction.
[0133] Before the polymerization reaction is carried out at elevated temperature, the materials are first mixed uniformly, so that the reaction can be more thorough and the weight-average molecular weight, crystallinity and particle size of the produced polymer can be more uniform.
[0134] In some embodiments, the amount of the aqueous solvent used in the process for producing the first fluorine-containing polymer is 2 to 8 times the total mass of the vinylidene fluoride monomer. The amount of the solvent used may be, for example, 3, 4, 5, 6, or 7 times the total mass of the vinylidene fluoride monomer. In some embodiments, the aqueous solvent is deionized water.
[0135] In some embodiments, during the preparation of the first fluorine-containing polymer, the dispersing agent comprises one or more of a cellulose ether and a polyvinyl alcohol.
[0136] In some embodiments, in the preparation of the first fluorine-containing polymer, the dispersing agent comprises one or more of a methyl cellulose ether and a carboxyethyl cellulose ether.
[0137] In some embodiments, the amount of dispersant used in the process for producing the first fluorine-containing polymer is 0.1% to 0.3% of the total mass of vinylidene fluoride monomers. The amount of dispersant used may be, for example, 0.2% of the total mass of vinylidene fluoride monomers.
[0138] In some embodiments, the first initiator is an organic peroxide.
[0139] In some embodiments, the first initiator comprises one or more of tert-amyl peroxypivalate, peroxy tert-amyl pivalate, 2-ethyl peroxydicarbonate, diisopropyl peroxydicarbonate, and tert-butyl peroxypivalate.
[0140] In some embodiments, in the process of preparing the first fluorine-containing polymer, the amount of the first initiator used is 0.15% to 1% of the total mass of the vinylidene fluoride monomer. The amount of the first initiator used may be, for example, 0.2%, 0.4%, 0.6% or 0.8% of the mass of the vinylidene fluoride monomer.
[0141] In some embodiments, the pH adjuster comprises one or more of potassium carbonate, potassium bicarbonate, sodium carbonate, sodium bicarbonate, and aqueous ammonia.
[0142] In some embodiments, the amount of pH adjuster used is between 0.05% and 0.2% of the total weight of vinylidene fluoride monomers. The amount of pH adjuster used may be, for example, even 0.1% or 0.15% of the total weight of vinylidene fluoride monomers.
[0143] In some embodiments, the third method for producing a fluorine-containing polymer comprises the steps of: A second polymerization reaction is carried out for 0.5 to 8 hours with at least one monomer represented by formula V in a non-reactive gas atmosphere, at 0.1-5 MPa and at a reaction temperature of 60°C to 90°C, and the reaction is terminated and separated into a solid and liquid to obtain a third fluorine-containing polymer while leaving a solid phase; TIFF2024542555000010.tif26150 Wherein, R4 and R5 are each independently hydrogen, halogen or C containing at least one fluorine atom. 1-3 The alkyl group is selected from the group consisting of aryl, ... and alkyl groups.
[0144] In some embodiments, the reaction pressure of the second polymerization reaction is 0.1 MPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, or any value therein.
[0145] In some embodiments, the reaction temperature of the second polymerization reaction is 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., or any value therein.
[0146] By carrying out the polymerization reaction at high temperature and pressure, it is possible to improve the reaction efficiency, shorten the reaction time, increase the reaction conversion rate, and improve the uniformity and purity of the product.
[0147] In some embodiments, the second polymerization reaction comprises: adding a solvent and a dispersant to a vessel and filling said vessel with a non-reactive gas; The method further includes the steps of adding the monomer represented by formula III, raising the temperature to 60° C. to 90° C., and then adding a second initiator and a chain transfer agent.
[0148] In some embodiments, the second initiator comprises an inorganic peroxide and may be selected from potassium persulfate or ammonium persulfate.
[0149] According to the nuclear magnetic results, when inorganic peroxide is used as initiator, the end group of the second fluorine-containing polymer includes -CF2-CH2OH or -CF2-CH2OOCCH3. The presence of hydroxyl group and ester group in the end group can effectively improve the adhesion of the second fluorine-containing polymer, and reduce the deterioration of the adhesive performance of the adhesive composition caused by its addition.
[0150] In some embodiments, the weight content of the initiator is 3%-12%, based on the total weight of the monomers of formula V.
[0151] High initiator content contributes to improving reaction efficiency, reducing reaction time, and improving product uniformity.
[0152] In some embodiments, the chain transfer agent comprises one or more of cyclohexane, isopropyl alcohol, methanol, and acetone.
[0153] [Positive electrode plate] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer including a positive electrode active material, a conductive agent, and in some embodiments, an adhesive composition.
[0154] This positive electrode plate has excellent adhesive strength even with a low addition amount of the adhesive composition.
[0155] In some embodiments, the mass fraction of the adhesive composition is not more than 1.5%, optionally 0.8%-1.2%, based on the total mass of the positive electrode membrane layer. In some embodiments, the mass content of the adhesive composition is 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, or any value therein.
[0156] The adhesive composition can effectively improve the adhesive performance of the electrode plate even in a small amount, and the electrode plate has excellent flexibility and processability, so that the battery has high energy density and cycle performance.
[0157] In some embodiments, the positive electrode active material is a lithium-containing transition metal oxide.
[0158] In some embodiments, the positive electrode active material is at least one of lithium iron phosphate or lithium nickel cobalt manganese oxide, or doped modifications thereof, or conductive carbon-coated, conductive metal-coated, or conductive polymer-coated modifications thereof.
[0159] In some embodiments, the positive electrode current collector may be a metal foil sheet or a composite current collector. For example, an aluminum foil may be used as the metal foil sheet. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base layer. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0160] In some embodiments, the positive electrode active material may be a positive electrode active material used in batteries known in the art. For example, the positive electrode active material may include at least one of lithium-containing phosphates with an olivine structure, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials in batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Here, examples of the lithium transition metal oxide include lithium cobalt oxide (e.g., LiCoO2), lithium nickel oxide (e.g., LiNiO2), lithium manganese oxide (e.g., LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM 333 (may be abbreviated as LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM 523 (may be abbreviated as LiNi 0.5 Co 0.25 Mn 0.25 O2(NCM 211 (may be abbreviated as LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM 622 (may be abbreviated as LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM 811 Lithium nickel cobalt aluminum oxide (e.g., LiNi 0.85 Co 0.15 Al 0.05Examples of the lithium-containing phosphate having an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (e.g., LiFePO4 (which may be abbreviated as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (e.g., LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon.
[0161] In some embodiments, the positive electrode film layer further optionally includes a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0162] In some embodiments, the positive electrode plate can be manufactured in the following manner: The components for manufacturing the positive electrode plate, such as the positive electrode active material, the conductive agent, the adhesive, and any other components, are dispersed in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry, which is then coated on a positive electrode current collector, and the positive electrode plate is obtained after processes such as drying and cold pressing.
[0163] [Negative electrode plate] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer including a negative electrode active material.
[0164] For example, the negative electrode current collector has two opposing surfaces in the thickness direction of the negative electrode current collector, and the negative electrode film layer is disposed on either one or both of the two opposing surfaces of the negative electrode current collector.
[0165] In some embodiments, the negative electrode current collector may be a metal foil sheet or a composite current collector. For example, the metal foil sheet may be a copper foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (such as copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0166] In some embodiments, the negative electrode active material may be a negative electrode active material for batteries known in the art. For example, the negative electrode active material may include at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicone-based material, tin-based material, and lithium titanate. The silicone-based material may be selected from at least one of silicone, silicone oxide, silicone carbon composite, silicone nitrogen composite, and silicone alloy. The tin-based material may be selected from at least one of tin, tin oxide, and tin alloy. However, the present application is not limited to these materials, and other conventional materials that can be used as a battery negative electrode active material may be used. These negative electrode active materials may be used alone or in combination of two or more.
[0167] In some embodiments, the negative electrode membrane layer further optionally comprises an adhesive, which may be selected from at least one of styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0168] In some embodiments, the negative electrode film layer further optionally comprises a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0169] In some embodiments, the negative electrode membrane layer optionally further comprises other auxiliary agents, such as a thickening agent (eg, sodium carboxymethylcellulose (CMC-Na)).
[0170] In some embodiments, the negative electrode plate can be manufactured in the following manner: Components for manufacturing the negative electrode plate, such as a negative electrode active material, a conductive agent, an adhesive, and any other components, are dispersed in a solvent (e.g., deionized water) to form a negative electrode slurry, which is then coated on a negative electrode current collector, and the negative electrode plate is obtained after processes such as drying and cold pressing.
[0171] [Electrolytes] The electrolyte serves to conduct ions between the positive and negative electrodes. The present application is not specifically limited to the type of electrolyte, which can be selected according to need. For example, the electrolyte may be liquid, gel, or all solid.
[0172] In some embodiments, the electrolyte is an electrolytic solution, the electrolytic solution including an electrolyte salt and a solvent.
[0173] In some embodiments, the electrolyte salt may be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonate), lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluoro(oxalato)borate, lithium bis(oxalato)borate, lithium difluorobis(oxalato)phosphate, and lithium tetrafluoro(oxalato)phosphate.
[0174] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, ethyl methyl sulfone, and diethyl sulfone.
[0175] In some embodiments, the electrolyte solution may further include optional additives, for example, additives for forming a negative electrode film, additives for forming a positive electrode film, and additives for improving some performance of the battery, such as additives for improving the overcharge performance of the battery, additives for improving the high temperature or low temperature performance of the battery, etc.
[0176] [Separator] In some embodiments, the secondary battery further includes a separator. The present application is not particularly limited to the type of separator, and any known porous structure separator having good chemical stability and mechanical stability may be selected.
[0177] In some embodiments, the material of the separator may be at least one selected from glass fiber, nonwoven fabric, polyethylene, polypropylene, and fluorine-containing polymers. The separator may be a monolayer film or a multilayer composite film, and there is no particular limitation. When the separator is a multilayer composite film, the materials of each layer may be the same or different, and there is no particular limitation.
[0178] In some embodiments, the positive plates, negative plates and separators can be fabricated into an electrode assembly by a winding process or a lamination process.
[0179] In some embodiments, the secondary battery may include an exterior body, which may be used to package the electrode assembly and the electrolyte.
[0180] In some embodiments, the exterior of the secondary battery may be a hard case, such as a hard plastic case, an aluminum case, a steel case, etc. The exterior of the secondary battery may be a pouch, such as a bag-shaped pouch. The material of the pouch may be plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0181] The present application is not particularly limited to the shape of the secondary battery, which may be cylindrical, rectangular, or any other shape. For example, FIG. 1 shows a secondary battery 5 with a rectangular structure as an example.
[0182] In some embodiments, referring to FIG. 2, the exterior body may include a case 51 and a cover plate 53. Here, the case 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate surround and form a receiving cavity. The case 51 has an opening communicating with the receiving cavity, and the cover plate 53 can cover the opening to seal the receiving cavity. The positive electrode plate, the negative electrode plate and the separator can form an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is packaged in the receiving cavity. An electrolyte is infiltrated into the electrode assembly 52. The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and those skilled in the art can select it according to the actual needs.
[0183] In some embodiments, the secondary batteries may be assembled into a battery module, and the number of secondary batteries included in the battery module may be one or more, with the specific number being selectable by one skilled in the art depending on the application and capacity of the battery module.
[0184] Fig. 3 shows an example of a battery module 4. Referring to Fig. 3, in the battery module 4, the multiple secondary batteries 5 may be arranged in sequence along the longitudinal direction of the battery module 4. Of course, they may be arranged in any other manner. Furthermore, the multiple secondary batteries 5 may be fixed by fasteners.
[0185] Optionally, the battery module 4 may further include a housing having an accommodating space, and the multiple secondary batteries 5 are accommodated in the accommodating space.
[0186] In some embodiments, the battery modules may be further assembled into a battery pack, and the number of battery modules included in the battery pack may be one or more, and the specific number can be selected by one skilled in the art according to the application and capacity of the battery pack.
[0187] 4 and 5 show an example of a battery pack 1. Referring to Fig. 4 and Fig. 5, the battery pack 1 may include a battery box and a plurality of battery modules 4 installed in the battery box. The battery box may include an upper housing 2 and a lower housing 3, and the upper housing 2 may cover the lower housing 3 to form a sealed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner.
[0188] The present application further provides a power consuming device, the power consuming device including at least one of the secondary battery, the battery module, or the battery pack according to the present application. The secondary battery, the battery module, or the battery pack may be used as a power source for the power consuming device, or may be used as an energy storage unit for the power consuming device. The power consuming device may include, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.
[0189] The power consumption device can be a secondary battery, a battery module, or a battery pack depending on its usage demand.
[0190] 6 shows an example of a power consumption device, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. A battery pack or a battery module can be employed to meet the demand for high power output and high energy density of the secondary battery of the power consumption device.
[0191] Other example devices may be mobile phones, tablet computers, notebook computers, etc. These devices generally require thinness and can employ secondary batteries as their power source.
[0192] Working Example The following is a description of the examples of the present application. The examples described below are illustrative and are only used to interpret the present application, and should not be understood as limitations to the present application. If no specific techniques or conditions are specified in the examples, they are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. If no manufacturer is specified, the reagents or instruments used are all commercially available ordinary products.
[0193] Example 1 1) Production of adhesive composition Preparation of the first fluorine-containing polymer: First-stage polymerization reaction: Add 4 kg of deionized water and 2 g of methylcellulose ether to the 10 L autoclaves No. 1 and No. 2, evacuate and replace O2 with N2 three times, add 5 g of tert-butyl peroxypivalate and 2 g of sodium bicarbonate again, add 1 kg of vinylidene fluoride monomer, and make the pressure reach 5 MPa. Mix and stir for 30 min, heat to 45 °C, and react for 4 h. Second-stage polymerization reaction: The reaction liquid in the No. 1 and No. 2 reactors was transferred to the No. 3 reactor, and nitrogen gas was charged up to a pressure of 7 MPa. The temperature was raised to 70°C, and the reaction was allowed to proceed with stirring for 3 hours. Third-stage polymerization reaction: After adding 40 g of cyclohexane, the reaction was continued for 1 h and then stopped. After centrifuging the reaction system, the solid phase was collected, washed and dried to obtain polyvinylidene fluoride adhesive.
[0194] Preparation of the second fluorine-containing polymer: A certain amount of PVDF powder (commercially available) with a weight average molecular weight of 1 million and a reaction medium (carbon tetrachloride) were prepared as a suspension and added to a 500ml three-neck flask, and N2 was passed through while stirring, and the mixture was heated to 75°C and refluxed for 15 minutes (the temperature was controlled by a constant temperature water bath). Then, an initiator (5g / L BPO was used as an initiator) was added, and a chlorinating agent (chlorinating agent was Cl2, and the traffic was 170mL / min) was added, and the HCl produced by the reaction was absorbed with water, and the chlorination degree of PVDF was controlled by weighing the amount of HCl absorbed. After the reaction was completed, nitrogen was passed through to remove residual chlorine, and the product was washed with alcohol, filtered, and then vacuum dried to a constant weight. Finally, PVDF with a chlorine content of about 8.0% was obtained.
[0195] Preparation of the third fluorine-containing polymer: In a 0.5L autoclave, 219g of deionized water and 0.1g of hydroxypropyl methylcellulose were added, and the atmosphere was replaced with nitrogen gas several times to remove oxygen, after which 120g of vinylidene fluoride monomer gas was added. After the monomer was added, the reaction temperature was controlled at 82°C, and the reaction was started after adding 0.12g of water-soluble ammonium persulfate initiator and isopropyl alcohol chain transfer agent, and the amount of initiator added was about 8% of the total amount of monomer added. The polymerization reaction time was 1.5h, and the pressure was maintained at 4.4MPa. After the reaction product was washed with water and dried, polyvinylidene fluoride polymer was obtained.
[0196] The first fluorine-containing polymer, the second fluorine-containing polymer and the third fluorine-containing polymer were blended such that the mass ratio of the first fluorine-containing polymer, the second fluorine-containing polymer and the third fluorine-containing polymer was 86:10:4, and an adhesive composition containing the first fluorine-containing polymer, the second vinylidene fluoride and the third vinylidene fluoride was obtained.
[0197] The production method in Examples 2-9 was the same as that in Example 1, with the difference being that the mass ratio of each fluorine-containing polymer in the adhesive composition was adjusted, as specifically shown in the table.
[0198] The manufacturing methods in Examples 10 to 13 were the same as those in Example 3, with the difference being that the degree of chlorination of PVDF was adjusted, as shown in the table below.
[0199] The preparation method in Example 14 was the same as that in Example 3, except that the second fluorine-containing polymer was replaced with a (vinylidene fluoride-trifluorochloroethylene) copolymer.
[0200] The manufacturing method in Comparative Example 1 was the same as that in Example 1, with the difference being that the adhesive composition contained only polyvinylidene fluoride having a weight average molecular weight of 5,000,000.
[0201] The adhesive composition used in Examples 15-17 and 20 is the same as that used in Examples 10, 11, 3 and 12, and the battery is manufactured using the adhesive composition as an adhesive, and the specific method is as follows.
[0202] 2) Manufacturing of positive electrode plates Lithium iron phosphate, an adhesive composition, and acetylene black are stirred in a planetary stirring tank at a revolution speed of 25 r / min for 30 min, where the mass fraction of the adhesive composition is 1% based on the total mass of the positive electrode film layer; Add 2.4 kg of N-methylpyrrolidone (NMP) solution to the stirring tank and stir for 70 minutes at a revolution speed of 25 r / min and a rotation speed of 900 r / min. Add 12.3 g of polyvinylpyrrolidone dispersant to the stirring tank, and stir for 60 minutes at a revolution speed of 25 r / min and a rotation speed of 1300 r / min. After the stirring was finished, the slurry viscosity was tested and the viscosity was controlled at 8000-15000 mpa·s.
[0203] If the viscosity was high, an N-methylpyrrolidone (NMP) solution was added to reduce the viscosity to the above range, and after adding the NMP solution, the mixture was stirred for 30 minutes at a revolution speed of 25 r / min and a rotation speed of 1200 to 1500 r / min to obtain a positive electrode slurry. The produced positive electrode slurry was applied onto a carbon-coated aluminum foil, baked at 110°C for 15 minutes, cold pressed, and then cut into a ring shape with a diameter of 15 mm to obtain a positive electrode plate.
[0204] 3) Negative electrode plate A piece of metallic lithium served as the negative electrode plate.
[0205] 4) Separator A polypropylene membrane served as the separator.
[0206] 5) Electrolyte production In a glove box with an argon gas atmosphere (H2O<0.1ppm, O2<0.1ppm), the organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed uniformly in a volume ratio of 3 / 7, LiPF6 lithium salt was added and dissolved in the organic solvent, and the mixture was stirred uniformly to prepare a 1M LiPF6EC / EMC solution, thereby obtaining the electrolyte.
[0207] 6) Battery manufacturing The positive electrode plate, negative electrode plate, separator and electrolyte in Example 1 were assembled into a button cell box to form a button battery.
[0208] The manufacturing method of the batteries of Examples 18, 19, 21, and 22 was basically the same as that of Example 20, except that the amount of adhesive composition used in the electrode plate was changed, as shown in the table.
[0209] The manufacturing method of the batteries of Examples 23-26 was basically the same as that of Example 20, except that the ratio of each fluorine-containing polymer in the adhesive composition was changed, as shown in the table.
[0210] The manufacturing method of the batteries in Examples 27 to 29 was basically the same as that in Example 20, except that the weight average molecular weight of the third fluorine-containing polymer was changed.
[0211] In Example 27, the preparation method of polyvinylidene fluoride having a weight average molecular weight of 5,000 includes the following:
[0212] In a 0.5L autoclave, 219g of deionized water and 0.1g of hydroxypropyl methylcellulose were added, and the atmosphere was replaced with nitrogen gas several times to remove oxygen, after which 120g of vinylidene fluoride monomer gas was added. After the monomer was added, the reaction temperature was controlled at 87°C, and the reaction was started after adding 0.15g of water-soluble ammonium persulfate initiator and isopropyl alcohol chain transfer agent, and the amount of initiator added was about 8% of the total amount of monomer added. The polymerization reaction time was 0.8h, and the pressure was maintained at 4.4MPa. After the reaction product was washed with water and dried, a polyvinylidene fluoride polymer was obtained.
[0213] In Example 28, the preparation method of polyvinylidene fluoride having a weight average molecular weight of 20,000 includes the following:
[0214] In a 0.5L autoclave, 219g of deionized water and 0.1g of hydroxypropyl methylcellulose were added, and the atmosphere was replaced with nitrogen gas several times to remove oxygen, after which 120g of vinylidene fluoride monomer gas was added. After the monomer was added, the reaction temperature was controlled at 83°C, and the reaction was started after adding 0.14g of water-soluble ammonium persulfate initiator and isopropyl alcohol chain transfer agent, and the amount of initiator added was about 8% of the total amount of monomer added. The polymerization reaction time was 1h, and the pressure was maintained at 4.4MPa. After the reaction product was washed with water and dried, polyvinylidene fluoride polymer was obtained.
[0215] In Example 29, the preparation method of polyvinylidene fluoride having a weight average molecular weight of 150,000 includes the following:
[0216] In a 0.5L autoclave, 219g of deionized water and 0.1g of hydroxypropyl methylcellulose were added, and the atmosphere was replaced with nitrogen gas several times to remove oxygen, after which 120g of vinylidene fluoride monomer gas was added. After the monomer was added, the reaction temperature was controlled at 79°C, and after adding 0.12g of water-soluble ammonium persulfate initiator and isopropyl alcohol chain transfer agent, the reaction was started, the amount of initiator added was about 7.0% of the total amount of monomer added, the polymerization reaction time was 1.5h, and the pressure was maintained at 4.4MPa. After the reaction product was washed with water and dried, a polyvinylidene fluoride polymer was obtained.
[0217] The manufacturing method of the battery in Examples 30-31 is basically the same as that in Example 20, except that the weight average molecular weight of the second fluorine-containing polymer is changed, and all of them are commercially available.
[0218] The manufacturing method of the battery in Examples 32-33 was basically the same as that in Example 20, except that the weight average molecular weight of the first fluorine-containing polymer was changed.
[0219] The method for producing the polyvinylidene fluoride having a weight average molecular weight of 3,000,000 in Example 32 is as follows.
[0220] Add 4kg of deionized water and 2g of methylcellulose ether to a 10L autoclave, evacuate and replace O2 with N2 three times, add 5g of tert-butyl peroxypivalate and 2g of sodium bicarbonate again, add 1kg of vinylidene fluoride monomer, and make the pressure reach 7MPa. Mix and stir for 30min, heat to 45℃, and carry out polymerization reaction. After polymerization reaction for 10h, add 20g of cyclohexane to continue the reaction. When the pressure in the reactor drops to 2MPa, the reaction is stopped. After centrifuging the reaction system, collect the solid phase, wash and dry to obtain polyvinylidene fluoride adhesive.
[0221] The method for producing polyvinylidene fluoride having a weight average molecular weight of 10 million in Example 33 is as follows.
[0222] 4 kg of deionized water and 2 g of methylcellulose ether were added to a 10 L autoclave, and the inside was evacuated and replaced with N2.
[0223] First-stage polymerization reaction: Add 4 kg of deionized water and 2 g of methylcellulose ether to the 10 L autoclaves No. 1 and No. 2, evacuate and replace O2 with N2 three times, add 5 g of tert-butyl peroxypivalate and 2 g of sodium bicarbonate again, add 1 kg of vinylidene fluoride monomer, and make the pressure reach 5 MPa. Mix and stir for 30 min, heat to 45 °C, and react for 9 h. Second-stage polymerization reaction: The reaction liquid in the No. 1 and No. 2 reactors was transferred to the No. 3 reactor, and nitrogen gas was charged up to a pressure of 7 MPa. The temperature was raised to 70°C, and the reaction was allowed to proceed with stirring for 3 hours. Third-stage polymerization reaction: After adding 20 g of cyclohexane, the reaction was continued for 1 h and then stopped. After centrifuging the reaction system, the solid phase was collected, washed and dried to obtain polyvinylidene fluoride adhesive.
[0224] The manufacturing method of the battery in Examples 34-35 is basically the same as that in Example 20, and the difference is that the type of the second fluorine-containing polymer is changed. The second fluorine-containing polymer in Example 34 is vinylidene fluoride-trifluorochloroethylene copolymer, and the second fluorine-containing polymer in Example 35 is not subjected to chlorination treatment.
[0225] The vinylidene fluoride-trifluorochloroethylene copolymer in Example 34 was produced in the following manner.
[0226] 0.8 g of benzoyl peroxide (BPO) was weighed and added to a 1 L autoclave containing 1,1,2-trifluorotrichloroethane (400 mL). The reaction vessel was sealed and cooled in a dry ice bath, then evacuated. 25 g of trifluorochloroethylene was passed through, followed by 420 g of vinylidene fluoride. The temperature was raised to room temperature, and the reaction was continued for 7.5 hours at 45°C. The temperature was then lowered to room temperature, and the unreacted gas was released. The reaction vessel was opened, and the colorless precipitate in the solution was taken out and dried in a vacuum drying box at 55°C for 8 hours, finally obtaining a P(VDF-TrFE) copolymer.
[0227] The manufacturing method of the battery in Example 36 is basically the same as that in Example 20, except that the type of the first fluorine-containing polymer in the adhesive composition is changed to a (vinylidene fluoride-hexafluoropropylene) copolymer, and the third fluorine-containing polymer is changed to a (vinylidene fluoride-hexafluoropropylene) copolymer.
[0228] The method for producing a vinylidene fluoride-hexafluoropropylene copolymer having a weight average molecular weight of 5,000,000 is as follows.
[0229] First-stage polymerization reaction: Add 4 kg of deionized water and 2.5 g of methylcellulose ether to the 10 L autoclaves No. 1 and No. 2, evacuate and replace O2 with N2 three times, add 5 g of tert-butyl peroxypivalate and 2 g of sodium bicarbonate again, fill with 0.94 kg of vinylidene fluoride and 0.06 kg of hexafluoropropylene, and allow the pressure to reach 5 MPa. Mix and stir for 30 min, heat to 45 °C, and react for 4 h. Second-stage polymerization reaction: The reaction liquid in the No. 1 and No. 2 reactors was transferred to the No. 3 reactor, and nitrogen gas was charged up to a pressure of 7 MPa. The temperature was raised to 70°C, and the reaction was allowed to proceed with stirring for 3 hours. Third-stage polymerization reaction: After adding 38 g of cyclohexane, the reaction was continued for 1 h and then stopped. After centrifuging the reaction system, the solid phase was collected, washed and dried to obtain vinylidene fluoride-trifluorochloroethylene copolymer adhesive.
[0230] The method for producing a vinylidene fluoride-hexafluoropropylene copolymer having a weight average molecular weight of 80,000 is as follows.
[0231] In a 0.5L autoclave, 219g of deionized water and 0.1g of hydroxypropyl methylcellulose were added, and nitrogen gas was added and substituted several times to remove oxygen, and then 100g of vinylidene fluoride monomer gas and 11.9g of hexafluoropropylene were added. After the monomers were added, the reaction temperature was controlled at 85°C. After adding 0.12g of water-soluble ammonium persulfate initiator and isopropyl alcohol chain transfer agent, the reaction was started, and the amount of initiator added was about 8% of the total amount of monomer. The polymerization reaction time was 1h, and the pressure was maintained at 4.6MPa. After the reaction product was washed with water and dried, a second fluorine-containing polymer was obtained.
[0232] The compositions of the adhesive compositions in Comparative Examples 1-3 are different, see Tables 1 and 2 for details.
[0233] Second, battery performance test 1. Polymer property test 1) Weight average molecular weight test A Waters 2695 Isocratic HPLC type gel chromatograph (differential refractive index detector 2141) was adopted. A polystyrene solution sample with a mass fraction of 3.0% was used as the standard, and a matching chromatographic column (oil-based: Styragel HT5DMF7.8*300mm+Styragel HT4) was selected. A 3.0% polymer glue solution was prepared with purified N-methylpyrrolidone (NMP) solvent, and the prepared solution was left to stand for one day in preparation for use. During the test, tetrahydrofuran was first sucked into the syringe, washed, and repeated several times. Then 5 ml of the experimental solution was sucked, the air in the syringe was eliminated, and the needle tip was wiped and dried. Finally, the sample solution was slowly injected into the injection port. After the display value became stable, the data was acquired and the weight average molecular weight was read.
[0234] 2) Crystallinity test 0.5g of fluorine-containing polymer was placed in an aluminum crucible, flattened, and the crucible was covered with a lid. The test was performed in a nitrogen gas atmosphere with 50ml / min of purge gas and 70ml / min of protective gas, with a heating rate of 10℃ / min and a test temperature range of -100℃~400℃, using a US TA Instruments Model Discovery 250 differential scanning calorimeter (DSC) to remove thermal history.
[0235] In this test, the temperature change curve of DSC / (Mw / mg) of the fluorine-containing polymer is obtained and integrated, and the peak area is the melting enthalpy ΔH (J / g) of the fluorine-containing polymer, and the adhesive crystallinity=ΔH / (ΔHm100%)*100%, where ΔHm100% is the standard melting enthalpy (crystallization heat of fusion) of the fluorine-containing polymer, and ΔHm100%=104.7 J / g.
[0236] 3) Chlorine content test The alkali fusion method was used to measure the chlorine content of chlorinated PVDF, and the specific operation is as follows: 0.6 grams (to the accuracy of 1 mg) of the second fluorine-containing polymer already ground was accurately weighed and placed in a 40 ml porcelain crucible. First, a layer of a mixture of anhydrous sodium carbonate and potassium nitrate was laid on the bottom of the porcelain crucible, and after the sample was added, another layer of a mixture of anhydrous sodium carbonate and potassium nitrate was laid on top of it. The mass ratio of anhydrous sodium carbonate to potassium nitrate was 3:2, and both were chlorine-free reagents. The amount of this mixture used per part of sample was about 10 g. The crucible containing the sample was covered with a lid, but it was not sealed, and the gas could still escape. The crucible was placed in a muffle furnace and gradually heated to 600 ° C., and the heating was stopped when it was melted for about 4 hours, there was no volatile gas of taste, the melt was uniform and consistent, and did not contain black mass points. The crucible was removed, cooled slightly, and then boiled water was added to dissolve the solution. After cooling, the solution was transferred to a 250ml measuring flask and deionized water was added up to the mark. 5ml of the above solution was placed in an Erlenmeyer flask, 1 drop of bromophenol blue indicator was added, and 5 drops of anhydrous ethanol were added. The solution was shaken to make it uniform, and most of the alkali was neutralized with concentrated nitric acid. Then, 0.2ml / L of nitric acid was added to make the bromophenol blue yellow, and several drops were added in excess to make the pH value of the solution 1.5-2. Five drops of diphenylcarbazone solution were added, and the solution was titrated with mercury nitrate standard solution. At the end point, the color changed from yellow-red to red-purple. A blank experiment was performed under the same conditions. Three tests were performed for each of the above samples.
[0237] The mass fraction of chlorine, Cl%, was calculated using the following formula:
[0238] Cl%=[(Vl-V2)×C×35.46×2 / W]×100 where V1 and V2 are the volumes of mercuric nitrate standard solution consumed in the titration of the sample and blank, respectively, in mL, C is the concentration of mercuric nitrate standard solution, in mol / L, and W is the mass of the sample, in mg.
[0239] 2. Slurry performance test 1) Slurry fluidity test An appropriate amount of the positive electrode slurry was taken with a chemical spoon, and the slurry was observed to see if it naturally flowed smoothly. If it naturally flowed smoothly, it was judged as OK, but if the fluidity was poor and the slurry became jelly-like and formed lumps, indicating the appearance of gel, it was judged as NG.
[0240] 2) Slurry filtration performance test A 500 ml beaker was placed on the lower end of the 200 mesh filter bracket, 500 ml of the slurry was taken and placed on the filter to filter, and the time when the slurry volume in the beaker reached 300 ml was recorded. This time was used to judge the filtration performance of the slurry. If the filtration time was less than 120 s, it indicated that the filtration performance of the slurry was "OK", and if the slurry could not pass through the filter, it indicated that the filtration performance of the slurry was poor and was judged as "NG".
[0241] 3. Electrode plate performance test 1) Adhesion test According to the national standard GB-T2790-1995 "Testing method for 180° peel strength of adhesives", the adhesive strength testing process of the examples and comparative examples of this application is as follows:
[0242] A blade was used to cut out a sample with a width of 30 mm and a length of 100-160 mm, and a special double-sided tape was attached to a steel plate, making the tape width 20 mm and the length 90-150 mm. The positive electrode film layer surface of the electrode plate sample cut in the previous step was attached to the double-sided tape, and then rolled three times in the same direction with a 2 kg press roller.
[0243] A paper tape having the same width as the electrode plate and a length of 250 mm was fixed to the electrode plate current collector and was also fixed with masking tape.
[0244] The power supply of the Sansi tensioning device (sensitivity is 1N) was turned on, the indicator lamp was lit, the stopper block was adjusted to the appropriate position, and the end of the steel plate where the electrode plate was not attached was fixed with the lower jig. The paper tape was folded up and fixed with the upper jig, and the position of the upper jig was adjusted using the "up" and "down" buttons on the manual controller attached to the tensioning device. Then the test was performed and the numerical value was read. The force when the electrode plate was balanced under the force was divided by the width of the tape to characterize the adhesive strength of the electrode plate per unit length, which was the adhesive strength between the positive electrode film layer and the current collector.
[0245] 2) Measurement of positive electrode film layer resistance: After drying, the positive electrode slurry (film layer) was cut from the left, center, and right of the positive plate, and cut into small rings with a diameter of 3 mm. Turn on the power of the Yuan Neng Technology Plate Resistor, place it on the appropriate position of the "probe" of the plate resistor, click the "Start" button, and read the display value when it becomes stable. Each small ring is tested in two positions, and finally calculate the average value of the six measurements, which is the film layer resistance of this plate.
[0246] 3) Plate brittleness test The positive electrode plate in the embodiment was cut into a test sample of 20 x 100 mm in size and prepared for use. The electrode plate was bent and folded in half, fixed, and pressed once with a rolling roller weighing 2 kg, and the presence or absence of light transmission and metal leakage was checked at the folded part of the electrode plate. If there was no light transmission or metal leakage, the electrode plate was folded in half again, fixed, pressed once with a rolling roller weighing 2 kg, and the presence or absence of light transmission and metal leakage was checked at the folded part of the electrode plate. The above steps were repeated until there was light transmission and metal leakage at the folded part of the electrode plate, and the number of light transmissions of the folded positive electrode plate was recorded. Three sets were measured in parallel, and the average value was calculated.
[0247] 3. Battery performance test 1) Battery capacity retention test The battery capacity retention test process is as follows: At 25℃, the button battery is charged to 3.65V at 1 / 3C constant current, then charged to 0.05C at 3.65V constant voltage, left for 5min, and discharged to 2.5V at 1 / 3C, the resulting capacity is the initial capacity C0. The above steps are repeated for the same battery, and the discharge capacity Cn of the battery after the nth cycle is recorded at the same time. The battery capacity retention after each cycle is Pn=Cn / C0*100%, and the values of these 500 points P1, P2...P500 are taken as the ordinate and the corresponding cycle number is taken as the abscissa to obtain a curve of battery capacity retention vs cycle number.
[0248] In this test process, the first cycle corresponds to n = 1, the second cycle corresponds to n = 2, ... the 500th cycle corresponds to n = 500. The battery capacity retention data corresponding to the examples and comparative examples in the table are the data measured after 500 cycles under the above test conditions, i.e., the P500 value.
[0249] 3. Analysis of the Test Results of Each Example and Comparative Example According to the above-mentioned method, the batteries of the examples and comparative examples were manufactured, and the performance parameters were measured. The results are shown in Tables 1 and 2 below.
[0250] [Table 1-1] [Table 1-2] [Table 1-3]
[0251] [Table 2-1] [Table 2-2] [Table 2-3] [Table 2-4] [Table 2-5] [Table 2-6] [Table 2-7] [Table 2-8] [Table 2-9] [Table 2-10] [Table 2-11] [Table 2-12] [Table 2-13]
[0252] As can be seen from the comparison between Examples 1-14 and Comparative Example 1, the inclusion of fluorine-containing polymers with different weight average molecular weights in the adhesive composition can reduce the crystallinity of the polymer. As can be seen from Examples 1-9, the crystallinity of the adhesive composition decreases with an increase in the content of the second fluorine-containing polymer. As can be seen from Examples 10-13, when the chlorine content of the chlorinated polyvinylidene fluoride is 8%, the crystallinity is only 4.2%, and the adhesive composition is basically in an amorphous state.
[0253] As can be seen from Example 14, the (vinylidene fluoride-trifluorochloroethylene) copolymer, as the second fluorine-containing polymer, can also effectively reduce the crystallinity of the adhesive composition. However, when the chlorine content of the (vinylidene fluoride-trifluorochloroethylene) copolymer is 8%, its crystallinity is higher than that of chlorinated polyvinylidene fluoride.
[0254] As can be seen from the comparison between Examples 15-36 and Comparative Examples 1-2, the adhesive composition can significantly reduce the amount of fluorine-containing polymer used, and the inclusion of a third fluorine-containing polymer in the adhesive composition can effectively improve the processing performance of the slurry, improve the flexibility of the battery, and further optimize the cycle performance of the battery while maintaining high adhesive performance.
[0255] As can be seen from the comparison of Examples 15-17, 20 with Examples 35, 36, the addition of the second fluorine-containing polymer after chlorination could further improve the flexibility of the polymer and reduce the possibility of embrittlement of the plate.
[0256] As can be seen from Examples 18-22, with the increase in the dosage of the adhesive composition, the adhesive strength of the electrode plate increased continuously, and the flexibility and cycle capacity retention first increased and then decreased.
[0257] It should be noted that the present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment having substantially the same configuration as the technical idea and achieving the same effect within the scope of the technical solution of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can make to the embodiment and other methods configured by combining some of the components in the embodiment are also included in the scope of the present application, within the scope of the purpose of the present application. [Explanation of symbols]
[0258] 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 secondary battery, 51 case, 52 electrode assembly, 53 cover plate.
Claims
1. An adhesive composition comprising a first fluorine-containing polymer, a second fluorine-containing polymer, and a third fluorine-containing polymer, wherein the first fluorine-containing polymer has a weight average molecular weight of 3 million to 10 million, the second fluorine-containing polymer has a weight average molecular weight of 600,000 to 1,100,000, and the third fluorine-containing polymer has a weight average molecular weight of 5,000 to 150,000.
2. 2. The adhesive composition according to claim 1, wherein the mass content of the first fluorine-containing polymer is 10% to 86% based on the total mass of the adhesive composition.
3. 3. The adhesive composition according to claim 1, wherein the mass content of the second fluorine-containing polymer is 10% to 86% based on the total mass of the adhesive composition.
4. Adhesive composition according to any one of claims 1 to 3, characterized in that the crystallinity of the adhesive composition is not higher than 40%, preferentially 5%-40%.
5. The adhesive composition according to any one of claims 1 to 4, wherein the first fluorine-containing polymer contains a structural unit derived from vinylidene fluoride.
6. The first fluorine-containing polymer further comprises a structural unit shown in formula I, Here, R 1 is a C group containing fluorine, chlorine and at least one fluorine atom 1-3 The adhesive composition according to any one of claims 1 to 5, characterized in that it contains one or more of the following:
7. The adhesive composition according to any one of claims 1 to 6, wherein the first fluorine-containing polymer comprises one or more of polyvinylidene fluoride, vinylidene fluoride-trifluorochloroethylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-trifluorochloroethylene-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer, and vinylidene fluoride-trifluorochloroethylene-tetrafluoroethylene-hexafluoropropylene copolymer.
8. The second fluorine-containing polymer comprises a structural unit shown in Formula II, Here, R 2 , R 3 each independently represents a C group containing hydrogen, a halogen, and at least one fluorine atom; 1-3 The adhesive composition according to any one of claims 1 to 7, characterized in that it contains at least one of:
9. The adhesive composition according to any one of claims 1 to 8, wherein the second fluorine-containing polymer contains chlorine.
10. The adhesive composition according to any one of claims 1 to 9, characterized in that the chlorine content in the second fluorine-containing polymer does not exceed 8%, based on the total mass of the second fluorine-containing polymer.
11. 11. The adhesive composition according to claim 1, wherein the crystallinity of the second fluorine-containing polymer does not exceed 47%, optionally does not exceed 30%.
12. The adhesive composition according to any one of claims 1 to 11, wherein the second fluorine-containing polymer has a weight average molecular weight of 600,000 to 1,100,000.
13. The fluorine-containing polymer according to any one of claims 1 to 12, characterized in that the second fluorine-containing polymer includes at least one of polyvinylidene fluoride, chlorinated polyvinylidene fluoride, chlorinated poly(vinylidene fluoride-hexafluoropropylene), and poly(vinylidene fluoride-trifluorochloroethylene).
14. The third fluorine-containing polymer comprises a structural unit shown in Formula III: Here, the R 4 , R 5 The adhesive composition according to any one of claims 1 to 13, wherein each independently contains at least one of hydrogen, fluorine, chlorine, or a trifluoromethyl group.
15. The adhesive composition according to any one of claims 1 to 14, wherein an end group of the third fluorine-containing polymer contains a hydroxyl group or an ester group.
16. The adhesive composition according to any one of claims 1 to 15, wherein the third fluorine-containing polymer comprises one of polytetrafluoroethylene, polyvinylidene fluoride, poly(vinylidene fluoride-hexafluoropropylene) copolymer, poly(vinylidene fluoride-tetrafluoroethylene) copolymer, poly(vinylidene fluoride-trifluorochloroethylene) copolymer, and poly(vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene) copolymer.
17. A fluorine-containing polymer comprising structural units derived from vinylidene fluoride and structural units shown in formula IV: Here, R 6 A fluorine-containing polymer, comprising at least one of hydrogen, Cl, and F.
18. 18. The fluorine-containing polymer according to claim 17, wherein the chlorine content in the fluorine-containing polymer does not exceed 8%, based on the total mass of the fluorine-containing polymer.
19. 19. The fluorine-containing polymer according to claim 17 or 18, wherein the crystallinity of the fluorine-containing polymer does not exceed 30%.
20. The fluorine-containing polymer according to any one of claims 17 to 19, characterized in that the fluorine-containing polymer has a weight average molecular weight of 600,000 to 1,100,000.
21. The fluorine-containing polymer according to any one of claims 17 to 20, characterized in that the fluorine-containing polymer includes at least one of chlorinated polyvinylidene fluoride, chlorinated poly(vinylidene fluoride-hexafluoropropylene), and poly(vinylidene fluoride-trifluorochloroethylene).
22. A method for producing a fluorine-containing polymer, comprising the steps of: A method for producing a fluorine-containing polymer, comprising: chlorinating polyvinylidene fluoride by using a chlorinating agent to produce a fluorine-containing polymer.
23. Specifically, the manufacturing method includes: dispersing polyvinylidene fluoride in a solvent to produce a polyvinylidene fluoride suspension; and adding an initiator and a chlorinating agent to chlorinate the polyvinylidene fluoride to produce a fluorine-containing polymer.
24. 24. The method according to claim 22 or 23, wherein the chlorinating agent includes at least one of chlorine gas, hydrogen chloride, phosphorus trichloride, sulfuryl chloride, and phosgene.
25. 25. The method according to claim 22, wherein the initiator comprises at least one of dibenzoyl oxide, dilauroyl peroxide, azobisisobutyronitrile, and azobisisoheptonitrile.
26. 17. A positive electrode plate comprising: a positive electrode current collector; and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer comprising a positive electrode active material, a conductive agent, and the adhesive composition according to claim 1.
27. The positive electrode plate according to claim 26, wherein the mass fraction of the adhesive composition is not more than 1.5%, and optionally 0.8%-1.2%, based on the total mass of the positive electrode membrane layer.
28. 28. The positive electrode plate according to claim 26 or 27, characterized in that the positive electrode active material is a transition metal oxide containing lithium, and optionally at least one of lithium iron phosphate or lithium nickel cobalt manganese oxide, or a doping modification thereof, or a conductive carbon-coated modification thereof, a conductive metal-coated modification thereof, or a conductive polymer-coated modification thereof.
29. A secondary battery comprising an electrode assembly and an electrolyte, the electrode assembly comprising a separator, a negative electrode plate, and the positive electrode plate according to any one of claims 26 to 28.
30. 30. A power consuming device comprising the secondary battery of claim 29.
Citation Information
Patent Citations
Electrolyte and battery using the same
JP2005038789A
Solar cell backsheet containing a fluorine-based copolymer and method for manufacturing the same
JP2012521088A
Binder composition, electrode mixture, electrode, and non-aqueous electrolyte secondary battery
JP2022061830A
Solar cell back sheet including a fluorine-based copolymer, and method for manufacturing same
US20120031475A1
Chlorination of poly (vinylidene fluoride) using U-V radiation