Negative electrode and secondary battery including the same

A double-layer structured negative electrode with specific graphite compositions addresses the issues of cycle expansion and energy density in lithium metal secondary batteries, enhancing adhesion and charging performance.

JP2024542625AActive Publication Date: 2024-11-15LG ENERGY SOLUTION LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024531688
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-21
Filing Date
2022-12-20
Publication Date
2024-11-15
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

Conventional lithium metal secondary batteries using natural graphite as the negative electrode face issues such as battery short circuits due to dendrite formation, high electrolyte side reactions, and reduced durability due to cycle expansion, which affect energy density and charging performance.

Method used

A negative electrode with a double-layer structure comprising a lower layer of natural graphite primary particles and artificial graphite primary particles, and an upper layer of artificial graphite secondary particles, optimized for void volume and porosity, enhances adhesion and reduces cycle expansion while improving energy density and charging performance.

Benefits of technology

The double-layer structure improves adhesive strength, reduces cycle expansion, and enhances energy density and rapid charging capabilities of the negative electrode, addressing the limitations of natural graphite in lithium metal secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542625000001_ABST
    Figure 2024542625000001_ABST
Patent Text Reader

Abstract

The present invention relates to a negative electrode including a negative electrode current collector, a lower negative electrode active material layer disposed on the negative electrode current collector, and an upper negative electrode active material layer disposed on the lower negative electrode active material layer, the lower negative electrode active material layer including a first negative electrode active material including natural graphite particles and a second negative electrode active material including artificial graphite particles in a primary particle form, the upper negative electrode active material layer including a third negative electrode active material including artificial graphite particles in a secondary particle form formed by granulating two or more primary particles, and the first negative electrode active material has a pore volume of 0.06 mL / g or less as measured by a mercury porosimeter measurement method.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0184261, filed December 21, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference.

[0002] The present invention relates to a negative electrode and a secondary battery including the same. [Background technology]

[0003] 2. Description of the Related Art With rising energy costs due to the depletion of fossil fuels and growing concerns over environmental pollution, alternative, environmentally friendly energy sources have become an essential factor for future life.

[0004] In particular, with technological development and increasing demand for mobile devices, the demand for secondary batteries as an environmentally friendly alternative energy source is rapidly increasing.

[0005] Conventionally, lithium metal has been used as the negative electrode in the secondary battery. However, due to the risk of battery short circuit caused by the formation of dendrites and the resulting risk of explosion, the use of carbon-based active materials that allow reversible intercalation and deintercalation of lithium ions and maintain structural and electrical properties has been attracting attention.

[0006] As the carbon-based active material, various types of carbon-based materials such as artificial graphite, natural graphite, hard carbon, etc. are used, and among them, graphite-based active materials that can guarantee the life characteristics of lithium secondary batteries due to their excellent reversibility are most widely used. Since the graphite-based active material has a lower discharge voltage of -0.2V compared to lithium, a battery using the graphite-based active material can exhibit a high discharge voltage of 3.6V, providing many advantages in terms of the energy density of lithium batteries.

[0007] Among them, natural graphite has the advantage that it shows higher output and capacity than other carbon-based active materials such as artificial graphite, and has excellent adhesive strength, so that it is possible to reduce the amount of binder used and realize a high-capacity, high-density anode. However, natural graphite has the problem of reduced anode durability due to a large degree of electrolyte side reaction, and has the problem of being highly oriented, which is disadvantageous in cycle expansion characteristics.

[0008] Therefore, there is a need to develop a negative electrode active material that can exhibit the high output and capacity of natural graphite while preventing the problem of cycle expansion.

[0009] Japanese Patent Registration Publication No. 4403327 discloses graphite powder for the negative electrode of a lithium ion secondary battery, but fails to provide an alternative solution to the above-mentioned problems. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Patent No. 4403327 Summary of the Invention [Problem to be solved by the invention]

[0011] An object of the present invention is to provide a negative electrode having high energy density, excellent fast charging performance and improved negative electrode adhesion, and capable of effectively preventing cycle expansion problems.

[0012] Another object of the present invention is to provide a secondary battery including the above-mentioned negative electrode. [Means for solving the problem]

[0013] The present invention provides a negative electrode comprising: a negative electrode current collector; a lower negative electrode active material layer disposed on the negative electrode current collector; and an upper negative electrode active material layer disposed on the lower negative electrode active material layer, wherein the lower negative electrode active material layer comprises a first negative electrode active material including natural graphite particles and a second negative electrode active material including artificial graphite particles in a primary particle form, and the upper negative electrode active material layer comprises a third negative electrode active material including artificial graphite particles in a secondary particle form formed by granulating two or more primary particles, and the first negative electrode active material has a pore volume of 0.06 mL / g or less as measured by a mercury porosimeter measurement method.

[0014] The present invention also provides a secondary battery including the above-mentioned negative electrode, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. Effect of the Invention

[0015] The anode of the present invention includes a double-layered anode active material layer, the lower anode active material layer includes a first anode active material including natural graphite particles and a second anode active material including artificial graphite particles in the form of primary particles, and the upper anode active material layer includes a third anode active material including artificial graphite particles in the form of secondary particles, and the first anode active material has a void volume measured by a mercury porosimeter that satisfies a specific range. The first anode active material and the second anode active material included in the lower anode active material layer improve adhesion to the anode current collector, improve the capacity of the anode, and reduce the degree of cycle expansion, and the third anode active material included in the upper anode active material layer improves fast charging performance, so that the anode of the present invention has high energy density, excellent fast charging performance, improved anode adhesion, and can reduce the degree of cycle expansion. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a schematic side view illustrating a negative electrode according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0018] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless it has a clearly different meaning in the context.

[0019] It should be understood that in this specification, terms such as "comprises," "comprises," or "having" specify the presence of embodied features, numbers, steps, components, or combinations thereof, but do not preclude the presence or additional possibility of one or more different features, numbers, steps, components, or combinations thereof.

[0020] In this specification, D 50 can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50 can be measured by using, for example, a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to several mm, and can provide results with high reproducibility and high resolution.

[0021] In this specification, the BET specific surface area can be measured by a BET (Brunauer-Emmett-Teller) measurement method using an adsorption gas such as nitrogen and a BELSORP (BET equipment) manufactured by BEL JAPAN.

[0022] The present invention will now be described in detail with reference to the drawings, in which: Fig. 1 is a schematic side view illustrating a negative electrode according to the present invention;

[0023] <Negative electrode> The present invention relates to a negative electrode, specifically, to a negative electrode for a lithium secondary battery.

[0024] Referring to FIG. 1, an anode 10 of the present invention includes an anode current collector 100, a lower anode active material layer 210 disposed on the anode current collector 100, and an upper anode active material layer 220 disposed on the lower anode active material layer 210, the lower anode active material layer 210 including a first anode active material including natural graphite particles and a second anode active material including artificial graphite particles in a primary particle form, the upper anode active material layer 220 including a third anode active material including artificial graphite particles in a secondary particle form formed by granulating two or more primary particles, and a void volume of the first anode active material measured by a mercury porosimeter is 0.06 mL / g or less.

[0025] According to the anode of the present invention, the first anode active material and the second anode active material included in the lower anode active material layer can improve adhesion with the anode current collector, thereby improving the capacity of the anode and reducing the degree of cycle expansion. The third anode active material included in the upper anode active material layer can improve fast charge performance, thereby providing high energy density, excellent fast charge performance, improved anode adhesion, and reduced cycle expansion.

[0026] [Negative electrode current collector 100] The negative electrode current collector 100 may be any negative electrode current collector commonly used in the art, and may be any current collector that does not cause chemical changes in the lithium secondary battery and has high electrical conductivity. For example, the negative electrode current collector 100 may include at least one selected from copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy, and may preferably include copper.

[0027] The negative electrode current collector 100 may have fine irregularities on its surface to strengthen the binding force of the negative electrode active material, and may be used in various forms such as a film, a sheet, a foil, a mesh, a porous body, a foam, a nonwoven fabric, etc.

[0028] The negative electrode current collector 100 may generally have a thickness of 3 μm to 500 μm.

[0029] [Lower negative electrode active material layer 210] The lower negative electrode active material layer 210 is disposed on the negative electrode current collector 100 .

[0030] The lower negative electrode active material layer 210 may be disposed on at least one surface of the negative electrode current collector 100, specifically, on one or both surfaces.

[0031] The lower negative electrode active material layer 210 includes a first negative electrode active material and a second negative electrode active material.

[0032] The first negative electrode active material includes natural graphite particles. By including the natural graphite particles, the first negative electrode active material can improve adhesion between the lower negative electrode active material layer and the negative electrode current collector, which can help improve the capacity of the negative electrode.

[0033] The first negative electrode active material has a pore volume of 0.06 mL / g or less as measured by a mercury porosimeter method.

[0034] The mercury porosimeter is a method for measuring the size, porosity, and pore volume of voids present on the surface of a sample by injecting mercury into the sample. The mercury porosimeter is different from the BET nitrogen adsorption method in that it injects mercury, not gas, into the sample, and therefore can measure large voids in the negative active material, specifically void volumes having sizes of about 5 nm to 1,000 nm. On the other hand, the BET nitrogen adsorption method measures void volumes by adsorbing nitrogen gas into the sample, and can measure the presence, specific surface area, and pore volume of small voids, specifically voids having sizes of several nm to 100 nm, but has limitations in measuring voids of 100 nm or more. In this respect, it is considered that the measurement ranges of voids by the mercury porosimeter and the BET nitrogen adsorption method are different from each other.

[0035] The first negative electrode active material has a pore volume measured by a mercury porosimeter adjusted to the above-mentioned level, thereby reducing the ratio, content, or volume of pores having a large pore size within a particle, for example, a pore size of 100 nm or more. The lower negative electrode active material layer includes the first negative electrode active material, thereby improving electrode adhesion and energy density of the negative electrode and reducing cycle expansion. In addition, the first negative electrode active material is included in the lower negative electrode active material layer together with a second negative electrode active material described below, thereby further improving the effects of improving the negative electrode adhesion and reducing cycle expansion of the negative electrode.

[0036] For example, if the pore volume of the first negative electrode active material measured by a mercury porosimeter exceeds 0.06 mL / g, the cycle expansion cannot be sufficiently reduced, and the occurrence of negative electrode swelling may increase.

[0037] Specifically, the pore volume of the first negative electrode active material measured by a mercury porosimeter measurement method can be 0.001 mL / g to 0.06 mL / g, more specifically, 0.010 mL / g to 0.045 mL / g. When the pore volume is within the above range, the above-mentioned effects of improving the energy density of the negative electrode, improving the rapid charging performance, improving the negative electrode adhesion, and reducing cycle expansion can be further improved.

[0038] The first negative electrode active material has a BET specific surface area of ​​0.6 m 2 / g~2.5m 2 / g, specifically 1.5m 2 / g~2.2m 2 When the negative electrode active material has a specific surface area of ​​the above level, the contact area with the electrolyte can be sufficiently secured, the output characteristics can be improved, and the above-mentioned electrolyte side reaction can be prevented and the cycle expansion can be reduced.

[0039] The BET specific surface area can be measured by a BET (Brunauer-Emmett-Teller) method. For example, the BET specific surface area can be measured by a BET 6-point method using a porosimetry analyzer (Belsorp-II mini, Bell Japan Inc.) by a nitrogen gas adsorption flow method.

[0040] The average particle size (D 50 The average particle size (D) of the negative electrode active material may be 8 μm to 25 μm, specifically 12 μm to 20 μm, and more specifically 15 μm to 20 μm. 50 When the average particle size of the natural graphite particles is adjusted to the above range, the BET specific surface area is adjusted to a preferred level, the voids between the particles are reduced, and swelling is prevented. In addition, the problem of significant volume expansion during charging and discharging due to an excessively large average particle size of the natural graphite particles and the problem of reduced rapid charging performance due to an increased diffusion distance of lithium are prevented.

[0041] The first negative electrode active material may be spherical. When the first negative electrode active material is spherical, the void structure is smoothly maintained when the first negative electrode active material is included in the negative electrode, thereby ensuring the diffusion path of lithium ions and improving the output characteristics of the negative electrode. In addition, when the first negative electrode active material is spherical, the adhesive force in the negative electrode can be improved and the amount of binder used can be relatively reduced, which is advantageous for reducing the output characteristics and resistance. In this specification, the term "spherical" refers to a concept that includes not only a perfect sphere, but also a shape that is substantially spherical even if it is somewhat crushed.

[0042] The tap density of the first negative electrode active material may be 1.0 g / cc to 1.3 g / cc, specifically 1.05 g / cc to 1.30 g / cc, more specifically 1.11 g / cc to 1.20 g / cc, which is preferable in terms of improving the sphericity of the negative electrode active material and reducing the degree of cycle expansion of the negative electrode including the negative electrode active material.

[0043] The tap density can be determined, for example, by filling 40 g of the first negative electrode active material into a cylindrical container having a diameter of 30 mm and a capacity of 100 mL, vibrating the container up and down 1,000 times with an amplitude of 10 mm, measuring the final volume, and calculating the apparent density.

[0044] The first negative electrode active material may further include an amorphous carbon coating layer located on at least a portion of a surface of the natural graphite particle.

[0045] The amorphous carbon coating layer is useful for reducing the specific surface area of ​​the first negative electrode active material, improving cell performance, and facilitating the mobility of lithium ions, thereby reducing resistance and improving fast charging performance. More specifically, the first negative electrode active material may be composed of the natural graphite particles and the amorphous carbon coating layer.

[0046] The amorphous carbon coating layer may be included in the first negative electrode active material in an amount of 1 wt % to 10 wt %, specifically, 2 wt % to 5 wt %.

[0047] The method for preparing the first negative electrode active material is not particularly limited as long as the pore volume measured by a mercury porosimeter can be adjusted to the above-mentioned level. More specifically, the first negative electrode active material can be prepared by a method including the following steps.

[0048] (a) isostatically pressing a natural graphite raw material; (b) mixing the isostatically pressed natural graphite feedstock and a binder material to produce a mixture; (c) heat treating the mixture to carbonize it; and (d) crushing the carbonized mixture.

[0049] According to the manufacturing method, the natural graphite raw material is isostatically pressed, mixed with the isostatically pressed natural graphite binder material, heat-treated, carbonized, and then crushed to manufacture the first negative electrode active material.

[0050] The natural graphite raw material may be spherical natural graphite particles.

[0051] The isostatic pressing process can be cold isostatic pressing or hot isostatic pressing.

[0052] The isostatic pressing treatment can be carried out at a pressure of 20 MPa to 100 MPa, specifically at a pressure of 45 MPa to 95 MPa. By carrying out the isostatic pressing treatment at a pressure within the above range, it is possible to reduce voids in the natural graphite raw material, and to prevent an increase in defects in the natural graphite raw material due to pressing at an excessive pressure.

[0053] The isostatic pressing treatment may be performed for 0.1 to 20 minutes, specifically 0.5 to 3 minutes, and when the time is within the above range, it is preferable in that the desired physical properties of the first negative electrode active material can be appropriately adjusted and maintained.

[0054] The binder material may include at least one selected from the group consisting of polymer resin and pitch. Specifically, the polymer resin may include at least one selected from the group consisting of sucrose, phenol resin, naphthalene resin, polyvinyl alcohol resin, furfuryl alcohol resin, polyacrylonitrile resin, polyamide resin, furan resin, cellulose resin, styrene resin, polyimide resin, epoxy resin, vinyl chloride resin, and polyvinyl chloride. The pitch may include at least one selected from the group consisting of coal-based pitch, petroleum-based pitch, and mesophase pitch.

[0055] The natural graphite raw material and the binder substance can be mixed in a weight ratio of 100:4 to 100:14, specifically, in a weight ratio of 100:5 to 100:10.

[0056] The heat treatment of the mixture may be performed at 1,000° C. to 1,500° C., specifically 1,150° C. to 1,300° C., and within the above range, carbonization of the binder material may be preferably performed. The heat treatment may be performed for 20 hours to 48 hours.

[0057] After the carbonized mixture is crushed, a sieving process may be further performed. The crushing and sieving may be performed, for example, to obtain the average particle size (D 50 ) range can be satisfied.

[0058] The lower negative electrode active material layer includes a second negative electrode active material. The second negative electrode active material includes artificial graphite particles in a primary particle form. Specifically, the second negative electrode active material may consist of only artificial graphite particles in a primary particle form.

[0059] The lower negative electrode active material layer includes a second negative electrode active material together with the first negative electrode active material, thereby achieving a fast charging characteristic and a low degree of cycle expansion of the negative electrode. In particular, the second negative electrode active material includes artificial graphite particles in the form of primary particles, rather than artificial graphite particles in the form of secondary particles. Since the artificial graphite particles in the form of primary particles have a higher tap density than the artificial graphite particles in the form of secondary particles, the packing of the lower negative electrode active material layer can be improved, the thickness of the electrode can be reduced, and the energy density can be improved. In addition, since the second negative electrode active material includes artificial graphite particles in the form of primary particles, which have excellent cycle expansion performance, the cycle expansion can be reduced to an excellent level when mixed with the first negative electrode active material.

[0060] Here, the term "primary particle-type artificial graphite particles" refers to artificial graphite particles in the form of a single particle, and is used as a term to distinguish it from "secondary particle-type artificial graphite particles", which are aggregates of two or more primary particle-type artificial graphite particles aggregated by an intentional granulation or bonding process.

[0061] The average particle size (D 50 ) may be 4 μm to 13 μm, specifically 7 μm to 10 μm. When it is within this range, the specific surface area of ​​the second negative electrode active material can be reduced to a preferable level, which not only helps to improve the capacity of the negative electrode, but also allows the second negative electrode active material to densely fill empty spaces formed between the first negative electrode active material described below, thereby improving rolling performance.

[0062] The BET specific surface area of ​​the second negative electrode active material is 0.1 m 2 / g~3.0m 2 / g, specifically 0.8m 2 / g~1.5m 2 When the specific surface area is within the above range, it is preferable in terms of suppressing side reactions and reducing resistance. The BET specific surface area can be measured using a BEL Sorption instrument (manufactured by BEL Japan).

[0063] The second negative electrode active material may be spherical. When the second negative electrode active material is spherical, a smooth void structure is maintained when the second negative electrode active material is included in a negative electrode, thereby ensuring a diffusion path for lithium ions and improving the output characteristics of the negative electrode.

[0064] The tap density of the second negative electrode active material may be 1.0 g / cc to 1.3 g / cc, specifically 1.15 g / cc to 1.30 g / cc, which is preferable in terms of improving the sphericity of the negative electrode active material and reducing the degree of cycle expansion of the negative electrode including the negative electrode active material.

[0065] The weight ratio of the first negative electrode active material to the second negative electrode active material may be 50:50 to 90:10. When the weight ratio is within this range, it is preferable in that the energy density and cycle expansion characteristics can be simultaneously improved to a preferable level.

[0066] The average particle size (D 50 ) to the average particle size (D 50 The ratio of may be 1 to 8, specifically 1.5 to 3.0, and when it is within the above range, it is preferable in terms of minimizing electrolyte side reactions and improving cycle expansion characteristics.

[0067] The total weight of the first and second negative electrode active materials may be 80% to 99% by weight, and preferably 90% to 98% by weight, based on the weight of the lower negative electrode active material layer 210.

[0068] In addition, the lower negative electrode active material layer 210 may further include at least one additive selected from the group consisting of a binder, a thickener, and a conductive material, in addition to the first negative electrode active material and the second negative electrode active material.

[0069] The binder, which is a component that helps bind between the conductive material, the active material, and the current collector, may be added in an amount of 1 to 30 wt % into the lower negative electrode active material layer 210. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0070] As the thickener, any thickener that has been used in the prior art lithium secondary batteries may be used, and an example thereof is carboxymethyl cellulose (CMC).

[0071] The conductive material is a component for further improving the conductivity of the negative electrode material, and may be added in an amount of 1 to 20 wt % in the lower negative electrode active material layer 210. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Specific examples of commercially available conductive materials include acetylene black-based products from Chevron Chemical Company, Denka Singapore Private Limited, Gulf Oil Company, Ketjenblack, EC-based products (manufactured by Armak Company), Vulcan XC-72 (manufactured by Cabot Company), and Super P (manufactured by Timcal).

[0072] [Top negative electrode active material layer 220] The upper negative electrode active material layer 220 is disposed on the lower negative electrode active material layer 210. Specifically, the upper negative electrode active material layer 220 may be formed on one side of the lower negative electrode active material layer 210 that does not face the negative electrode current collector 100. If the lower negative electrode active material layers are formed on both sides of the negative electrode current collector, the upper negative electrode active material layers may be disposed on the lower negative electrode active material layers formed on both sides of the negative electrode current collector, respectively.

[0073] The upper negative electrode active material layer 220 includes a third negative electrode active material. The third negative electrode active material includes artificial graphite particles in a secondary particle form in which two or more primary particles are granulated. The artificial graphite particles in a secondary particle form include voids formed between the primary particles, so that lithium ions can be smoothly diffused through the voids.

[0074] The upper negative electrode active material layer is disposed on the upper part of the negative electrode and includes a third negative electrode active material including artificial graphite particles in a secondary particle form, thereby facilitating the diffusion of lithium ions, thereby further improving the fast charging performance of the negative electrode.

[0075] The secondary particle-form artificial graphite particles have an average particle size (D 50 When the average particle size of the primary artificial graphite particles contained in the uncoated artificial graphite particles is within the above range, the capacity is adjusted to a preferred level, and the average particle size (D 50 ) is too large, the deterioration of the quick charging performance can be prevented.

[0076] The third negative electrode active material may further include an amorphous carbon coating layer located on the secondary particle type artificial graphite particles, and the amorphous carbon coating layer may be included in the third negative electrode active material in an amount of 1 wt % to 10 wt %, specifically, 2 wt % to 5 wt %.

[0077] The amorphous carbon coating layer may be formed by providing a carbon precursor to the secondary particle-shaped artificial graphite particles and then heat-treating the carbon precursor. The carbon precursor may be, but is not limited to, polymer resins such as sucrose, phenol resin, naphthalene resin, polyvinyl alcohol resin, furfuryl alcohol resin, polyacrylonitrile resin, polyamide resin, furan resin, cellulose resin, styrene resin, polyimide resin, epoxy resin, vinyl chloride resin, polyvinyl chloride, etc.; pitches such as coal-based pitch, petroleum-based pitch, mesophase pitch, etc. The heat treatment temperature may be 1,000°C to 1,800°C.

[0078] The average particle size (D 50 ) may be 15 μm to 25 μm, specifically 17 μm to 22 μm. When it is within this range, a decrease in quick charging performance due to an excessive particle size is prevented, and the specific surface area of ​​the active material is adjusted to a preferable level, which is favorable for improving high temperature performance.

[0079] The third negative electrode active material has a BET specific surface area of ​​0.1 m 2 / g~3.0m 2 / g, specifically 0.6m 2 / g~1.0m 2 / g, and when it is within this range, it is preferable in that electrolyte side reactions can be minimized.

[0080] The third negative electrode active material may have a tap density of 1.0 g / cc or less, in the range of 0.85 g / cc to 0.99 g / cc.

[0081] The weight of the third negative electrode active material may be 80% to 99% by weight, preferably 90% to 98% by weight, based on the weight of the upper negative electrode active material layer 220 .

[0082] In addition, the upper negative electrode active material layer 220 may further include at least one additive selected from the group consisting of a binder, a thickener, and a conductive material, in addition to the third negative electrode active material.

[0083] The binder is a component that helps bind the conductive material, active material, and current collector, and may be added in an amount of 1 to 30 wt % into the upper negative electrode active material layer 220. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0084] As the thickener, any thickener that has been used in the prior art lithium secondary batteries may be used, and an example thereof is carboxymethyl cellulose (CMC).

[0085] The conductive material is a component for further improving the conductivity of the negative electrode material, and may be added in an amount of 1 to 20 wt % in the upper negative electrode active material layer 220. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material that can be used include graphite such as natural graphite and artificial graphite; carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Specific examples of commercially available conductive materials include acetylene black-based products from Chevron Chemical Company, Denka Singapore Private Limited, Gulf Oil Company, Ketjenblack, EC-based products (manufactured by Armak Company), Vulcan XC-72 (manufactured by Cabot Company), and Super P (manufactured by Timcal).

[0086] The sum of the thickness of the lower negative electrode active material layer 210 and the thickness of the upper negative electrode active material layer 220 may be 30 μm to 200 μm, specifically 100 μm to 150 μm, and more specifically 110 μm to 130 μm.

[0087] The ratio of the thickness of the lower negative electrode active material layer to the thickness of the upper negative electrode active material layer may be 1:0.5 to 1:2, specifically 1:0.8 to 1:1.3, which is preferable in that the overall charge / discharge performance, adhesion, and energy density of the negative electrode can be improved at the same time when the ratio is within the above range.

[0088] The sum of the loading amount of the lower negative electrode active material layer and the loading amount of the upper negative electrode active material layer is 3 mAh / cm2 ~4mAh / cm 2 , specifically 3.4mAh / cm 2 ~3.8mAh / cm 2 It can be.

[0089] The ratio of the loading amount of the lower negative electrode active material layer to the loading amount of the upper negative electrode active material layer may be 1:0.5 to 1:2, specifically 1:0.8 to 1:1.3, which is preferable in that the overall charge / discharge performance, adhesion, and energy density of the negative electrode can be improved simultaneously when the ratio is within the above range.

[0090] The manufacturing method of the negative electrode is not particularly limited as long as it is possible to realize the lower negative electrode active material layer and the upper negative electrode active material layer having the above-mentioned characteristics. For example, the first negative electrode active material, the second negative electrode active material, and at least one additive selected from a binder, a conductive material, and a thickener are added to a solvent to prepare a slurry for the lower negative electrode active material layer, and the third negative electrode active material and at least one additive selected from a binder, a conductive material, and a thickener are added to a solvent to prepare a slurry for the upper negative electrode active material layer, and then these are applied to a negative electrode current collector to manufacture the negative electrode according to the present invention. More specifically, the slurry for the lower negative electrode active material layer prepared as above is applied to a negative electrode current collector, rolled, and dried to form a lower negative electrode active material layer, and the slurry for the upper negative electrode active material layer prepared as above is applied to the lower negative electrode active material layer, rolled, and dried to form an upper negative electrode active material layer, thereby manufacturing the negative electrode according to the present invention. Meanwhile, the slurry for the lower negative electrode active material layer may be applied to a negative electrode current collector, and at substantially the same time, the slurry for the upper negative electrode active material layer may be applied onto the slurry for the lower negative electrode active material layer to be applied, followed by rolling and drying, thereby manufacturing the negative electrode according to the present invention.

[0091] <Secondary battery> The present invention also provides a secondary battery including the above-mentioned negative electrode. Specifically, the secondary battery may be a lithium secondary battery.

[0092] Specifically, the secondary battery includes the above-described negative electrode, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte.

[0093] The positive electrode can include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector.

[0094] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel, aluminum, nickel, titanium, fired carbon, or a material obtained by surface-treating the surface of aluminum or stainless steel with carbon, nickel, titanium, silver, etc. can be used.

[0095] Generally, the positive electrode current collector can have a thickness of 3 μm to 500 μm.

[0096] The positive electrode active material layer is formed on the positive electrode current collector and contains a positive electrode active material.

[0097] The positive electrode active material can include a compound capable of reversible intercalation and deintercalation of lithium, specifically, a lithium composite metal oxide containing one or more metals such as cobalt, manganese, nickel, or aluminum and lithium. More specifically, the lithium composite metal oxide is a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese-based oxide (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2), etc.), a lithium-nickel-cobalt-based oxide (e.g., LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1), etc.), a lithium-manganese-cobalt-based oxide (e.g., LiCo 1-Y2 MnY2 O2 (where 0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (where 0 < Z1 < 2), etc.), lithium-nickel-manganese-cobalt oxide (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc.), or lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li(Ni p2 Co q2 Mn r3 M S2 )O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are, as atomic fractions of independent elements, 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1), etc.), and one or more of these compounds can be included. Among them, in terms of being able to enhance the capacity characteristics and stability of the battery, the lithium composite metal oxide is LiCoO2, LiMnO2, LiNiO2, lithium nickel manganese cobalt oxide (e.g., Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc.), or lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Mn 0.15 Co 0.05 )O2, etc.).

[0098] The positive electrode active material can be contained in an amount of 80% to 99% by weight based on the total weight of the positive electrode active material layer.

[0099] The positive electrode active material layer may further contain, in addition to the above-mentioned positive electrode active material, at least one additive selected from the group consisting of a binder and a conductive material.

[0100] The binder is a component that helps bind the active material and conductive material and the current collector, and is usually added in an amount of 1 to 30% by weight based on the total weight of the positive electrode active material layer. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, various copolymers, and the like.

[0101] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples of the conductive material include graphite; carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and other carbon-based materials; conductive fibers such as carbon fibers and metal fibers; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives. Specific examples of commercially available conductive materials include acetylene black-based Chevron Chemical Company products, Denka Singapore Private Limited, Gulf Oil Company products, Ketjenblack, EC-based (manufactured by Armak Company), Vulcan XC-72 (manufactured by Cabot Company), and Super P (manufactured by Timcal).

[0102] The conductive material may be contained in an amount of 1 to 30% by weight based on the total weight of the positive electrode active material layer.

[0103] The positive electrode active material layer may be manufactured by preparing a positive electrode slurry by adding a positive electrode active material and, optionally, an additive including a binder and / or a conductive material to a solvent, and then coating, rolling, and drying the positive electrode slurry on the positive electrode current collector.

[0104] The solvent may include an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the positive electrode active material, and optionally a binder and a conductive material, are included. For example, the solvent may be included so that the concentration of solids including the positive electrode active material, and optionally a binder and a conductive material, is 50 wt % to 95 wt %, preferably 70 wt % to 90 wt %.

[0105] In the lithium secondary battery, the separator separates the negative electrode and the positive electrode to provide a path for lithium ions to move, and may be any separator that is generally used in lithium secondary batteries, and may be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymeric material may be used to ensure heat resistance or mechanical strength, and may be selectively used in a single-layer or multi-layer structure.

[0106] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0107] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0108] The organic solvent can be any organic solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, examples of the organic solvent that can be used include ester-based solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2 to C20 linear, branched, or cyclic hydrocarbon group that may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes. Among them, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, so that the electrolyte can exhibit excellent performance.

[0109] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2 can be used as the lithium salt. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0110] As described above, the secondary battery according to the present invention is useful in portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs), and can be particularly preferably used as a constituent battery of a medium- to large-sized battery module. Thus, the present invention also provides a medium- to large-sized battery module including the above-described secondary battery as a unit cell.

[0111] Such a medium- to large-sized battery module can be preferably applied to power sources that require high output and large capacity, such as electric vehicles, hybrid electric vehicles, and power storage devices.

[0112] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in many different forms and should not be construed as limited to the embodiments set forth herein.

[0113] [Examples and Comparative Examples] Example 1: Preparation of negative electrode <Production of the first negative electrode active material, the second negative electrode active material, and the third negative electrode active material> 1. Preparation of the first negative electrode active material Spherical natural graphite particles (average particle size (D 50 The spherical natural graphite particles were subjected to cold iso-pressing at a pressure of 90 MPa for 1 minute.

[0114] The isostatically pressed spherical natural graphite particles were mixed with pitch as a binder in a weight ratio of 100:6, and the mixture was carbonized by heat treatment at 1,250°C for 24 hours. The carbonized mixture was then crushed and sieved to prepare a first negative electrode active material in which an amorphous carbon coating layer was formed on natural graphite particles.

[0115] The first negative electrode active material has an average particle size (D 50 ) is 17 μm, and the BET specific surface area is 1.8 m 2 / g and the tap density was 1.12 g / cc.

[0116] The first negative electrode active material was coated with an amorphous carbon coating layer of 3 wt %.

[0117] The pore volume of the first negative electrode active material measured by a mercury porosimeter was 0.042 mL / g.

[0118] 2. Preparation of the second negative electrode active material The primary particle form is spherical artificial graphite particles with an average particle size (D 50 ) is 9 μm, and the BET specific surface area is 1.27 m 2 / g and a tap density of 1.23 g / cc was used as the second negative electrode active material.

[0119] 3. Preparation of the third negative electrode active material Multiple primary artificial graphite particles (average particle size (D 50 Artificial graphite particles (average particle size (D): about 11 μm) in the form of secondary particles agglomerated 50 ):18 μm) was prepared.

[0120] Specifically, the artificial graphite particles are obtained by dispersing the coke raw material into a powder having an average particle size (D 50The coke was then mixed with pitch to produce an intermediate granulated in the form of secondary particles. The temperature was gradually raised to 3,000°C, maintained at 3,000°C for 60 hours, and gradually lowered to room temperature to heat treat the intermediate to graphitize and produce secondary particles. The average particle diameter (D 50 The total heat treatment time of the intermediate was 2 weeks.

[0121] The artificial graphite particles were mixed with pitch and then heat-treated at 1,200° C. for 24 hours to form an amorphous carbon coating layer on the artificial graphite particles, which was used as a third negative electrode active material.

[0122] The amorphous carbon coating layer was included in the third negative electrode active material at 3.5 wt %.

[0123] The average particle size (D 50 ) is 18 μm, and the BET specific surface area is 0.75 m 2 / g and the tap density was 0.92 g / cc.

[0124] <Production of negative electrodes> 1. Preparation of slurry for lower negative electrode active material layer A mixture of the first negative electrode active material and the second negative electrode active material in a weight ratio of 60:40, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 96.1:1.0:1.7:1.2, and water was added to prepare a slurry for the lower negative electrode active material layer.

[0125] 2. Preparation of slurry for upper negative electrode active material layer A third negative electrode active material, carbon black as a conductive material, styrene-butadiene (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 95.3:1.0:2.5:1.2, and water was added to prepare a slurry for an upper negative electrode active material layer.

[0126] 3. Formation of the lower and upper negative electrode active material layers The slurry for the lower negative electrode active material layer prepared above was coated on a copper foil (thickness: 15 μm) as a negative electrode current collector, and substantially at the same time, the slurry for the upper negative electrode active material layer prepared above was coated on the coated slurry for the lower negative electrode active material layer, roll pressed, and dried in a vacuum oven at 130° C. for 10 hours to prepare a negative electrode in which the negative electrode current collector, the lower negative electrode active material layer, and the upper negative electrode active material layer were sequentially stacked.

[0127] The loading amount of the lower negative electrode active material layer is 1.8 mAh / cm 2 The loading amount of the upper negative electrode active material layer is 1.8 mAh / cm 2 The sum of the loading amounts of the lower and upper negative electrode active material layers is 3.6 mAh / cm 2 It was.

[0128] Example 2: Preparation of negative electrode <Production of the first negative electrode active material, the second negative electrode active material, and the third negative electrode active material> 1. Preparation of the first negative electrode active material As a natural graphite raw material, the average particle size (D 50 A first negative electrode active material was prepared in the same manner as in Example 1, except that spherical natural graphite particles having a particle diameter of 18 μm were used.

[0129] The first negative electrode active material has an average particle size (D 50 ) is 18 μm, and the BET specific surface area is 1.8 m 2 / g, tap density was 1.13 g / cc, and the pore volume measured by mercury porosimetry was 0.041 mL / g.

[0130] 2. Preparation of the second negative electrode active material The primary particle form is spherical artificial graphite particles with an average particle size (D 50 ) is 8 μm, and the BET specific surface area is 1.30 m 2 / g and a tap density of 1.25 g / cc was used as the second negative electrode active material.

[0131] 3. Preparation of the third negative electrode active material Multiple primary artificial graphite particles (average particle size (D 50 : Approximately 11.5 μm) are agglomerated secondary particles of artificial graphite particles (average particle size (D 50 ):19 μm) was prepared.

[0132] Specifically, the artificial graphite particles are obtained by dispersing the coke raw material into a powder having an average particle size (D 50 The coke was then mixed with pitch to produce an intermediate granulated in the form of secondary particles. The temperature was gradually increased to 3,000°C, maintained at 3,000°C for 60 hours, and gradually decreased to room temperature for heat treatment to graphitize and produce secondary particles. The average particle diameter (D 50 The total heat treatment time of the intermediate was 2 weeks.

[0133] The artificial graphite particles were mixed with pitch and then heat-treated at 1,200° C. for 24 hours to form an amorphous carbon coating layer on the artificial graphite particles, which was used as a third negative electrode active material.

[0134] The amorphous carbon coating layer was included in the third negative electrode active material at 3.5 wt %.

[0135] The average particle size (D 50 ) is 19 μm, and the BET specific surface area is 0.7 m 2 / g and the tap density was 0.90 g / cc.

[0136] <Production of negative electrodes> A negative electrode was prepared in the same manner as in Example 1, except that the first negative electrode active material, the second negative electrode active material, and the third negative electrode active material prepared above were used, and the first negative electrode active material and the second negative electrode active material were mixed in a weight ratio of 70:30 when preparing the lower negative electrode active material layer.

[0137] Example 3: Preparation of negative electrode <Production of the first negative electrode active material, the second negative electrode active material, and the third negative electrode active material> 1. Preparation of the first negative electrode active material As a natural graphite raw material, the average particle size (D 50 A first negative electrode active material was prepared in the same manner as in Example 1, except that spherical natural graphite particles having a particle diameter of 18 μm were used.

[0138] The first negative electrode active material has an average particle size (D 50 ) is 18 μm, and the BET specific surface area is 1.8 m 2 / g, tap density was 1.14 g / cc, and the pore volume measured by mercury porosimetry was 0.039 mL / g.

[0139] 2. Preparation of the second negative electrode active material The same second negative electrode active material as that used in Example 2 was prepared.

[0140] 3. Preparation of the third negative electrode active material The same third negative electrode active material as that used in Example 1 was prepared.

[0141] <Production of negative electrodes> A negative electrode was prepared in the same manner as in Example 1, except that the first negative electrode active material, the second negative electrode active material, and the third negative electrode active material prepared above were used, and the first negative electrode active material and the second negative electrode active material were mixed in a weight ratio of 90:10 when preparing the lower negative electrode active material layer.

[0142] Comparative Example 1: Production of negative electrode 1. Preparation of slurry for lower negative electrode active material layer A negative electrode active material was produced in the same manner as the method for producing the first negative electrode active material in Example 1, except that the isostatic pressing treatment was not performed.

[0143] The average particle size (D 50 ) is 18μm, and the specific surface area is 2.7m 2 / g, tap density was 1.10 g / cc, and the pore volume measured by mercury porosimetry was 0.080 mL / g.

[0144] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 96.1:1.0:1.7:1.2, and water was added to prepare a slurry for a lower negative electrode active material layer.

[0145] 2. Preparation of slurry for upper negative electrode active material layer The same third negative electrode active material as that produced in Example 2 was prepared as a negative electrode active material.

[0146] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 95.3:1.0:2.5:1.2, and water was added to prepare a slurry for an upper negative electrode active material layer.

[0147] 3. Formation of the lower and upper negative electrode active material layers A negative electrode was manufactured in the same manner as in Example 1, except that the above-prepared slurry for the lower negative electrode active material layer and the slurry for the upper negative electrode active material layer were used.

[0148] Comparative Example 2: Production of negative electrode 1. Preparation of slurry for lower negative electrode active material layer The same negative electrode active material as the third negative electrode active material prepared in Example 2 was used as the negative electrode active material.

[0149] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 95.3:1.0:2.5:1.2, and water was added to prepare a slurry for a lower negative electrode active material layer.

[0150] 2. Preparation of slurry for upper negative electrode active material layer A negative electrode active material was produced in the same manner as the method for producing the first negative electrode active material in Example 1, except that the isostatic pressing treatment was not performed.

[0151] The average particle size (D 50 ) is 19 μm, and the specific surface area is 2.8 m 2 / g, tap density was 1.10 g / cc, and the pore volume measured by mercury porosimetry was 0.090 mL / g.

[0152] The negative active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 96.1:1.0:1.7:1.2, and water was added to prepare a slurry for an upper negative active material layer.

[0153] 3. Formation of the lower and upper negative electrode active material layers A negative electrode was manufactured in the same manner as in Example 1, except that the above-prepared slurry for the lower negative electrode active material layer and the slurry for the upper negative electrode active material layer were used.

[0154] Comparative Example 3: Production of negative electrode 1. Preparation of slurry for lower negative electrode active material layer The same slurry for the lower negative electrode active material layer as in Comparative Example 1 was prepared.

[0155] 2. Preparation of slurry for upper negative electrode active material layer The primary particle form is spherical artificial graphite particles with an average particle size (D 50 ) is 10 μm, and the BET specific surface area is 1.25 m 2 / g and a tap density of 1.15 g / cc was used as the negative electrode active material.

[0156] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 95.3:1.0:2.5:1.2, and water was added to prepare a slurry for an upper negative electrode active material layer.

[0157] 3. Formation of the lower and upper negative electrode active material layers A negative electrode was manufactured in the same manner as in Example 1, except that the above-prepared slurry for the lower negative electrode active material layer and the slurry for the upper negative electrode active material layer were used.

[0158] Comparative Example 4: Production of negative electrode 1. Preparation of slurry for lower negative electrode active material layer The primary particle form is spherical artificial graphite particles with an average particle size (D 50 ) is 10 μm, and the BET specific surface area is 1.25 m 2 / g and a tap density of 1.15 g / cc was used as the negative electrode active material.

[0159] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 95.3:1.0:2.5:1.2, and water was added to prepare a slurry for a lower negative electrode active material layer.

[0160] 2. Preparation of slurry for upper negative electrode active material layer A negative electrode active material was produced in the same manner as the method for producing the first negative electrode active material in Example 1, except that the isostatic pressing treatment was not performed.

[0161] The average particle size (D 50 ) is 19 μm, and the specific surface area is 2.8 m 2 / g, tap density was 1.10 g / cc, and the pore volume measured by mercury porosimetry was 0.090 mL / g.

[0162] The negative active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 96.1:1.0:1.7:1.2, and water was added to prepare a slurry for an upper negative active material layer.

[0163] 3. Formation of the lower and upper negative electrode active material layers A negative electrode was manufactured in the same manner as in Example 1, except that the above-prepared slurry for the lower negative electrode active material layer and the slurry for the upper negative electrode active material layer were used.

[0164] Comparative Example 5: Production of negative electrode <Production of the first negative electrode active material, the second negative electrode active material, and the third negative electrode active material> 1. Preparation of the first negative electrode active material A negative electrode active material was produced in the same manner as the method for producing the first negative electrode active material in Example 1, except that the isostatic pressing treatment was not performed.

[0165] The average particle size (D 50 ) is 18μm, and the specific surface area is 2.7m 2 / g, tap density was 1.10 g / cc, and the pore volume measured by mercury porosimetry was 0.080 mL / g.

[0166] 2. Preparation of the second negative electrode active material The same second negative electrode active material as in Example 1 was prepared.

[0167] 3. Preparation of the third negative electrode active material The same third negative electrode active material as in Example 1 was prepared.

[0168] <Production of negative electrodes> A negative electrode was manufactured in the same manner as in Example 1, except that the first negative electrode active material, the second negative electrode active material, and the third negative electrode active material prepared above were used.

[0169] Comparative Example 6: Production of negative electrode 1. Preparation of slurry for lower negative electrode active material layer The same second negative electrode active material as in Example 1 was prepared as a negative electrode active material.

[0170] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 95.3:1.0:2.5:1.2, and water was added to prepare a slurry for a lower negative electrode active material layer.

[0171] 2. Preparation of slurry for upper negative electrode active material layer The same third negative electrode active material as that produced in Example 2 was prepared as a negative electrode active material.

[0172] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 95.3:1.0:2.5:1.2, and water was added to prepare a slurry for an upper negative electrode active material layer.

[0173] 3. Formation of the lower and upper negative electrode active material layers A negative electrode was manufactured in the same manner as in Example 1, except that the above-prepared slurry for the lower negative electrode active material layer and the slurry for the upper negative electrode active material layer were used.

[0174] Comparative Example 7: Production of negative electrode 1. Preparation of slurry for lower negative electrode active material layer As a natural graphite raw material, the average particle size (D 50 A negative electrode active material was prepared in the same manner as in the manufacturing method of the first negative electrode active material in Example 1, except that spherical natural graphite particles having a diameter of 18 μm were used and the pressure during the isostatic pressing treatment was 40 MPa.

[0175] The negative electrode active material has an average particle size (D 50 ) is 18 μm, and the BET specific surface area is 1.9 m 2 / g, tap density was 1.07 g / cc, and the pore volume measured by mercury porosimetry was 0.050 mL / g.

[0176] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 96.1:1.0:1.7:1.2, and water was added to prepare a slurry for a lower negative electrode active material layer.

[0177] 2. Preparation of slurry for upper negative electrode active material layer The same third negative electrode active material as that produced in Example 2 was prepared as a negative electrode active material.

[0178] The negative electrode active material, carbon black as a conductive material, styrene-butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a weight ratio of 95.3:1.0:2.5:1.2, and water was added to prepare a slurry for an upper negative electrode active material layer.

[0179] 3. Formation of the lower and upper negative electrode active material layers A negative electrode was manufactured in the same manner as in Example 1, except that the above-prepared slurry for the lower negative electrode active material layer and the slurry for the upper negative electrode active material layer were used.

[0180] Experimental Example Experimental example 1: Swelling evaluation <Manufacturing lithium secondary batteries> A positive electrode active material, LiCoO2, a conductive material, Li-435 (Denka), a binder, KF9700 (Kureha), and a thickener, BH-730H (Zeon), were mixed in a weight ratio of 97.68:1.20:1.00:0.12, and N-methylpyrrolidone (NMP) was added to prepare a positive electrode slurry. The positive electrode slurry was applied to an aluminum foil, and the aluminum foil was vacuum dried and rolled at about 130°C for 8 hours to prepare a positive electrode. Here, the loading of the positive electrode was about 3.4mAh / cm. 2 It was manufactured to be.

[0181] A polyolefin separator was interposed between the negative and positive electrodes produced in each of Examples 1 to 3 and Comparative Examples 1 to 7, and then an electrolyte was injected to produce secondary batteries of Examples and Comparative Examples. The electrolyte was prepared by adding 0.5% by weight of vinylene carbonate (VC) to a non-aqueous electrolyte solvent made by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 2:8, and dissolving LiPF6 at 1M.

[0182] <Swelling evaluation> The lithium secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 7 prepared above were charged and discharged in the range of SOC0 to SOC95 at 0.1C in the first cycle, 0.2C in the second cycle, and 0.5C from the third cycle to the 50th cycle. The swelling ratio was then measured and calculated according to the following formula. The results are shown in Table 1 below.

[0183] Swelling ratio (%) = {(t2-t1) / t1} × 100 (t1 is the thickness of the negative electrode for the secondary battery before the first charge-discharge cycle, and t2 is the thickness of the negative electrode for the secondary battery after the 50th charge-discharge cycle)

[0184] Experimental example 2: Initial discharge capacity evaluation <Manufacturing coin-type half-cell secondary batteries> A lithium metal counter electrode was used as the positive electrode.

[0185] A polyolefin separator was interposed between the negative and positive electrodes produced in each of Examples 1 to 3 and Comparative Examples 1 to 7, and then an electrolyte was injected to produce coin-type half-cell secondary batteries of Examples and Comparative Examples. The electrolyte was prepared by adding 0.5% by weight of vinylene carbonate (VC) to a non-aqueous electrolyte solvent made by mixing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 2:8, and dissolving LiPF6 at 1M.

[0186] <Measurement of initial discharge capacity> The coin-type half-cell secondary battery was charged and discharged under the following charge and discharge conditions to measure the initial discharge capacity. The results are shown in Table 1 below.

[0187] Charging conditions: CCCV mode, 0.1C charging, cut-off at 0.005C and 5mV Discharge conditions: CC mode, 0.1C discharge, cut-off at 1.5V

[0188] [Table 1]

[0189] Referring to Table 1, it can be seen that the negative electrodes and secondary batteries according to the embodiments of the present invention have an excellent level of energy density and an improved effect of reducing cycle expansion. [Explanation of symbols]

[0190] 10 negative electrode 100 Negative electrode current collector 210 Lower negative electrode active material layer 220 Upper negative electrode active material layer

Claims

1. A negative electrode current collector; a lower negative electrode active material layer disposed on the negative electrode current collector; an upper negative electrode active material layer disposed on the lower negative electrode active material layer, the lower negative electrode active material layer includes a first negative electrode active material including natural graphite particles and a second negative electrode active material including artificial graphite particles in the form of primary particles, the upper negative electrode active material layer includes a third negative electrode active material including artificial graphite particles in a secondary particle form formed by granulating two or more primary particles, A negative electrode, wherein the first negative electrode active material has a pore volume of 0.06 mL / g or less as measured by a mercury porosimeter method.

2. 2. The negative electrode of claim 1, wherein the first negative electrode active material has a pore volume of 0.001 mL / g to 0.06 mL / g as measured by a mercury porosimeter method.

3. The average particle size (D 50 2. The negative electrode according to claim 1, wherein the thickness of the first electrode is 8 μm to 25 μm.

4. The first negative electrode active material has a BET specific surface area of ​​0.6 m 2 / g to 2.5m 2 / g.

5. The average particle size (D 50 2. The negative electrode according to claim 1, wherein the thickness of the first electrode is 4 μm to 13 μm.

6. The BET specific surface area of ​​the second negative electrode active material is 0.1 m 2 / g to 3.0 m 2 / g.

7. The average particle size (D 50 2. The negative electrode according to claim 1, wherein the thickness of the first electrode is 15 μm to 25 μm.

8. The third negative electrode active material has a BET specific surface area of ​​0.1 m 2 / g to 3.0 m 2 / g.

9. 2. The negative electrode of claim 1, wherein a weight ratio of the first negative electrode active material to the second negative electrode active material is 50:50 to 90:

10.

10. 2. The negative electrode of claim 1, wherein a total weight of the first negative electrode active material and the second negative electrode active material is 80% by weight to 99% by weight based on a weight of the lower negative electrode active material layer.

11. The average particle size (D 50 ) to the average particle size (D 50 2. The negative electrode of claim 1, wherein the ratio of

12. 2. The negative electrode of claim 1, wherein a weight of the third negative electrode active material is 80% to 99% by weight based on a weight of the upper negative electrode active material layer.

13. 2. The negative electrode of claim 1, wherein a ratio of a thickness of the lower negative electrode active material layer to a thickness of the upper negative electrode active material layer is 1:0.5 to 1:

2.

14. 2. The negative electrode of claim 1, wherein a ratio of a loading amount of the lower negative electrode active material layer to a loading amount of the upper negative electrode active material layer is 1:0.5 to 1:

2.

15. The negative electrode according to any one of claims 1 to 14, A positive electrode facing the negative electrode; a separator interposed between the negative electrode and the positive electrode; and an electrolyte.

Citation Information

Patent Citations

  • Electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

    JP2017062911A

  • Negative electrode for nonaqueous electrolyte power storage device, nonaqueous electrolyte power storage device, and method for manufacturing negative electrode for nonaqueous electrolyte power storage device

    JP2018137133A

  • Graphite powder for the negative electrode of a lithium-ion secondary battery and a method for producing the same, and lithium-ion secondary battery

    JP4403327B2