High-rate, long-cycle, high-safety positive electrode plate for lithium batteries, its manufacturing method and use

The positive electrode plate for lithium batteries, incorporating specific components to form a stable protective film, addresses the compromise between rate, cycle, and safety issues, enhancing battery performance without altering the manufacturing process.

JP2024542668AActive Publication Date: 2024-11-15BEIJING WELION NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024532331
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-30
Filing Date
2023-01-28
Publication Date
2024-11-15
Estimated Expiration
2043-01-28

AI Technical Summary

Technical Problem

Existing methods to improve lithium battery performance, particularly in terms of rate characteristics, cycle stability, and safety, often compromise one another, and there is a need for a method that can enhance both without altering the mainstream manufacturing process.

Method used

A positive electrode plate for lithium batteries comprising a current collector with a positive electrode material layer containing a first component, such as Li1-x1Ti1-x1A1-x1OPO4 or Li1-y1Ti1-y1A1-y1OM1O4, and a second component, such as LiM2.2(P.O.4)3 or M3PO4, blended with the active material to form a stable protective film on the electrode surface, enhancing electrical properties and safety.

Benefits of technology

The proposed solution significantly improves the rate characteristics, cycle stability, and safety of lithium batteries by forming a stable protective film on the electrode surface, while being compatible with existing manufacturing processes and suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542668000001_ABST
    Figure 2024542668000001_ABST
Patent Text Reader

Abstract

The present invention discloses a positive electrode plate for a lithium battery with high rate, long cycle and high safety. The positive electrode plate includes a current collector and a positive electrode material layer located on the surface of the current collector. The positive electrode material layer is Li 1-x1 Ti 1-x1 A x1 OPO4, Li 1-x1 Ti 1-x1 A x1 PO5, Li 2-y1 Ti 1-y1 A y1 OM1O4, Li 2-y1 Ti 1-y1 A y1 At least one first component selected from M1O5, where 0≦x1≦0.7, 0≦y1≦1, A includes at least one of Nb, Ta, and Sb, and M1 is at least one of Si and Ge. The positive electrode material layer further includes a second component. The first component or a mixture of the first component and the second component in the positive electrode material layer is dispersed between the positive electrode active material particles. A lithium battery including the positive electrode exhibits excellent rate characteristics, cycle characteristics, and safety. The present invention does not change the current mainstream manufacturing process of positive electrode plates, separators, and batteries, is compatible with the conventional mainstream manufacturing process of positive electrode plates of lithium ion batteries, and is suitable for large-scale application.
Need to check novelty before this filing date? Find Prior Art

Description

CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of Chinese patent application No. 202210113791.3, filed on January 30, 2022, the contents of which are incorporated herein by reference. [Technical field]

[0002] The present invention relates to the technical field of lithium batteries, and in particular to a high-rate, long-cycle, high-safety positive electrode plate for lithium batteries, its manufacturing method, and its use. [Background technology]

[0003] Lithium-ion batteries have the advantages of high energy density, good cycle characteristics, long service life, low self-discharge, and no memory effect. Their application in energy storage, power batteries, 3C electronics and other fields is gradually expanding, and their future applications are promising.

[0004] Lithium batteries have an increasing energy density, providing better range for power electronics products such as electric vehicles and digital products. Increasing the loading and compression density of the electrode plate, especially the positive electrode plate, is an effective way to increase the energy density of the battery. However, as the loading and compression density of the positive electrode plate increase, the positive electrode active material layer becomes thicker and the porosity decreases, making it difficult to transport lithium ions in the positive electrode plate, resulting in serious polarization of the battery, which reduces the discharge specific capacity and rate characteristics of the battery, and also reduces cycle stability. In addition, as the energy density of the battery increases, it tends to become more difficult to ensure the safety of the battery. There has been no technology to solve these problems simultaneously.

[0005] Existing methods for improving the rate performance of batteries are as follows:

[0006] Cathode surface doping: The invention application with publication number CN113224287A describes a strontium-doped ternary lithium-ion battery cathode material (Li 1-x Srx [Ni 1-y-z Co y M z O₂, where M is one of the metals Mn and Al, 0 < x ≤ 0.1, 0 < y ≤ 1, 0 < z ≤ 1), its manufacturing method, and its use are disclosed. By doping strontium metal ions to replace lithium sites, the degree of cation mixing is reduced, the lithium ion channel is expanded, the layered structure is stabilized, and the rate performance of the lithium battery is effectively improved. However, this method often brings the problem of accelerating the capacity decay of the material while improving the rate performance.

[0007] Existing methods to improve the safety of the battery are as follows.

[0008] Positive electrode coating: The invention application with publication number CN113809280A discloses a positive electrode material, its manufacturing, and its use, which manufactures a positive electrode material with a substantially planar coating effect by changing sintering technical means and utilizing the interaction of coating agents. The positive electrode material manufactured by this method has a wide coating range of the surface coating layer, greatly reduces the degree of erosion of material particles by the electrolyte, effectively reduces the occurrence probability of side reactions, and improves the safety of the material. However, there are disadvantages that the process of the method is complex and it affects the rate performance of the battery.

[0009] Use of electrolyte additives: The invention application with publication number CN113690490A discloses a phosphite-based lithium ion battery electrolyte additive that can effectively prevent the combustion and explosion of organic solvents, improve the thermal stability of the electrolyte itself, improve the stability of the positive electrode, and improve the cycle stability and safety of the battery. However, there are disadvantages that it impairs the electrical properties of the battery such as cycle performance and rate performance.

[0010] Applying adhesive to separator: The invention patent application with publication number CN108963153B discloses a separator for lithium ion batteries and a manufacturing method thereof, which comprises coating at least one surface of a base film layer with an aqueous ceramic slurry coating, and then coating a composite adhesive layer made of polyethylene glycol and polymethyl methacrylate on the aqueous ceramic slurry coating and / or the surface of the base film layer, so that the resulting separator for lithium ion batteries has good adhesion, can prevent short circuits caused by the misalignment of the electrodes, improve the hardness of the battery, and greatly improve the safety of the battery. However, it has the disadvantage of impairing the rate characteristics of the battery.

[0011] Existing methods for improving both the electrical properties and safety of batteries are:

[0012] CN108365260B discloses a quasi-solid electrolyte comprising a polymer, a ceramic electrolyte, a lithium salt and an ionic liquid as a raw material composition. The ceramic electrolyte comprises a lithium titanium aluminum phosphate as a main phase and a heterophase TiP2O7 / TiO2. Preferably, the content of the heterophase in the ceramic electrolyte is 2-7%, and the mass ratio of TiP2O7 to TiO2 is 1.5-2.5:1. The overall properties of the quasi-solid electrolyte manufactured using the ceramic electrolyte with the above content of the heterophase are optimal. The heterophase with the special composition and content has lithium absorption properties, can improve the transportability of lithium ions, and can reduce the contact between the lithium titanium aluminum phosphate as a main phase and metallic lithium, and can improve the interface stability with metallic lithium. However, this patent does not improve the electrical properties and safety of the positive electrode, and the method is not compatible with the mainstream manufacturing process of existing lithium ion battery positive plate, and is not suitable for large-scale application.

[0013] CN113707880A relates to a positive electrode plate containing a solid electrolyte, its manufacturing method and its use, for the purpose of improving the rate characteristics of a battery and improving the cycle characteristics and safety. The solid electrolyte contained in the positive electrode slurry facilitates the permeation and infiltration of the electrolyte in the transverse and longitudinal directions of the plate, and facilitates the storage and infiltration of the electrolyte, thereby alleviating the expansion of the plate during the cycle of the cell, reducing the amount of electrolyte extruded under pressure during the expansion of the plate, so that the plate contains abundant electrolyte even after the cell has been cycled for a long time, ensuring normal transport of lithium ions, and improving the cycle characteristics. However, from the data of the examples, it was found that the battery capacity and safety were only slightly increased, and the effect on the rate characteristics was not supported by data, and the addition of the conventional solid electrolyte could not achieve the purpose of comprehensively improving the electrical characteristics and safety of the battery.

[0014] Therefore, there is a need to find a method that can improve the electrical properties and safety of batteries while also having simple steps and low costs. Summary of the Invention

[0015] In response to the limitations of the prior art, the present invention provides a high-rate, long-cycle, and high-safety positive electrode plate for lithium batteries, a method for producing the same, and use thereof. The positive electrode plate of the present invention includes a current collector and a positive electrode material layer located on the surface of the current collector, the positive electrode material layer including a positive electrode active material, a conductive agent, a binder, and a first component.

[0016] The first component is Li 1-x1 Ti 1-x1 A x1 OPO4, Li 1-x1 Ti 1-x1 A x1 PO5, Li 2-y1 Ti 1-y1 A y1 OM1O4, Li 2-y1 Ti 1-y1 A y1It contains at least one of M1O5. Here, 0 ≦ x1 ≦ 0.7, 0 ≦ y1 ≦ 1, A contains at least one of Nb, Ta, and Sb, and M1 is at least one of Si and Ge.

[0017] Preferably, the first component is at least one of LiTiOPO4, Li 0.9 Nb 0.1 Ti 0.9 OPO4, Li 0.9 Ta 0.1 Ti 0.9 OPO4, Li2TiOSiO4, LiTaOGeO4, or the like.

[0018] The positive electrode material layer further contains a second component, and the second component is at least one or a combination of one or more selected from LiM22(PO4)3, Li 1+x2 Al x2 M2 2-x2 (PO4)3, M2O2, Li 16-4y2 M2 y2 O8, M2P2O7, M3PO4, M32SiO5, M43(PO4)2, M42SiO4, where M2 is one selected from Ti, Ge, Zr, and Hf, where 0 < x2 < 0.6, and M3 and M4 are one of Al, Ga, Sc, Y, Ca, Sr, Zn, Si, In, Lu, La, Fe, Cr, Ge, and 3 < y2 < 4.

[0019] The second component is preferably one of InPO4, LATP, AlPO4, LAGP, LATP + AlPO4, LAGP + Al2SiO5, InPO4 + LATP, Al2SiO5, TiO2 + LiTi2(PO4)3, TiP2O7 + LiGe2(PO4)3.

[0020] The form of the mixed component composed of the first component and the second component is one in which the first component particles and the second component particles are uniformly mixed with each other, or one in which the first component crystal form and the second component crystal form are contained in each primary particle.

[0021] When the mass ratio of the first component to the cathode active material in the cathode material layer is w1, 0 < w1 < 5%, preferably 0.1 < w1 < 3%.

[0022] When the mass ratio of the second component to the cathode active material in the cathode material layer is w2, 0 ≤ w2 < 5%, preferably 0 ≤ w2 < 3%.

[0023] The particle size of the first component is 10 nm to 10 μm. Preferably, the particle size of the first component is 50 nm to 500 nm.

[0024] The particle size of the second component is 10 nm to 10 μm. Preferably, the particle size of the second component is 50 nm to 500 nm.

[0025] Preferably, taking the weight of the cathode material layer as 100%, the content of the cathode active material particles is 80 - 99 wt%, the content of the conductive agent is 0.1 - 8 wt%, the content of the binder is 0.1 - 10 wt%, the content of the first component or the mixed component composed of the first component and the second component is 0.1 - 6 wt%, Preferably, the cathode active material particles are at least one selected from lithium cobalt oxide cathode and its modified materials, NCM ternary cathode and its modified materials, NCA ternary cathode and its modified materials, nickel manganese lithium oxide cathode and its modified materials, lithium-rich cathode and its modified materials, lithium iron phosphate cathode and its modified materials, the conductive agent is at least one selected from Super - P, KS - 6, carbon black, carbon nanofiber, carbon nanotube, acetylene black, or graphene, the binder is selected from polyvinylidene fluoride, polyvinylidene fluoride - hexafluoropropylene, polytetrafluoroethylene, homopolymers, copolymers, modified compounds of the above polymers, or mixtures of the above polymers with other polymers or small molecules.

[0026] The second object of the present invention is to provide a method for producing a positive electrode plate for a lithium battery according to the first object of the present invention, in which the first component or the mixture of the first component and the second component is blended into a positive electrode slurry during homogenization. In the production of the positive electrode plate, the first component or the mixture of the first component and the second component is added and dispersed among the positive electrode active material particles.

[0027] Preferably, the method comprises the steps of: Step 1: uniformly mixing a first component or a mixture of the first component and the second component, a positive electrode active material, a conductive additive, a binder, and a solvent to form a slurry; Step 2 is to apply the slurry obtained in step 1 to the surface of an aluminum current collector to form a positive electrode plate; and step 3 of blowing and vacuum drying the electrode plate obtained in step 2 to obtain a final positive electrode plate.

[0028] Preferably, In step 1, NMP is used as the solvent in the slurry, and the mass ratio of NMP:positive electrode material is (2000-10):100.

[0029] In step 2, The manufacturing slurry used has a viscosity value of 3500 to 8500 mPa·S at 25°C.

[0030] In step 3, The air drying is carried out at a temperature of 80 to 180° C. for 10 minutes to 9 hours, and the vacuum drying is carried out at a temperature of 80 to 180° C. for 3 to 100 hours.

[0031] A third object of the present invention is to provide the use of the positive plate according to the first object of the present invention in a lithium battery.

[0032] In the present invention, a first component or a mixture of the first and second components having a particle diameter D50 of 0.01 to 10 μm is added to a positive electrode plate, and is mixed with a conductive agent and a binder to improve the rate characteristics, cycle characteristics, and safety of the battery, thereby providing the battery with high rate, long cycle, and high safety. Conventionally, the first component in the present application is usually a hetero phase generated during the sintering process of a solid electrolyte, and the presence of the hetero phase generally reduces the ionic conductivity of the solid electrolyte, and usually needs to be removed when manufacturing the solid electrolyte. In the prior art, the first component is not actively introduced into the electrolyte in high safety and high rate lithium batteries. However, in many experiments, it has been found that the first component in the present application has completely different characteristics from a solid electrolyte, and the ionic conductivity of such a component is relatively low, about 10, which is the ionic conductivity of a general solid electrolyte. -4 S / cm (i.e., it cannot be added to the electrode material to replace the solid electrolyte), which is the ionic conductivity of the electrolyte, 10 -2 It was found that the ionic conductivity of the first component is smaller than S / cm, and the first component cannot directly contribute to the ionic conductivity after mixing with the electrolyte, but its specific chemical composition can participate in the formation of CEI on the surface of the positive electrode material when added to the positive electrode material, changing the composition of the CEI to make it more stable, avoiding the rupture of the CEI and the resulting battery polarization and thermal runaway, and further improving the rate characteristics, cycle characteristics and safety of the positive electrode plate in the actual operation of the battery; and that the addition of the second component to the mixed positive electrode inhibits the decomposition of the electrolyte and inhibits the formation of insulating components on the surface of the positive electrode material, i.e., the simultaneous use of the second component and the first component produces a synergistic effect, constructs an excellent CEI, and comprehensively improves the electrical properties and safety of the battery. In addition, the introduction of the first component or a mixture of the first component and the second component into the positive electrode simultaneously by blending eliminates the need to change the current mainstream manufacturing processes of the positive electrode plate, separator and battery, and has the advantages of high stability and low cost, making it suitable for large-scale application.

[0033] Compared with the prior art, the present invention has the following advantages and significant effects.

[0034] The first component or the mixed component particles of the first component and the second component added to the positive plate of the lithium battery of the present invention has high chemical stability and can be directly blended into the positive active material before the production of the positive plate, without changing the mainstream manufacturing process of the current positive plate, separator and battery, is compatible with the mainstream manufacturing process of the positive plate of the existing lithium ion battery, does not affect the manufacturing process of the positive electrode and cell, has the advantages of high stability and low cost, and is suitable for large-scale application. On the other hand, the methods of doping the positive electrode material and coating the positive electrode surface both require changes to the manufacturing technology of the existing positive electrode material, and are difficult to improve the discharge specific capacity and rate characteristics.

[0035] The first component added to the positive electrode plate for lithium batteries of the present invention is completely different from conventional solid electrolytes, has low lithium ion conductivity, and is not suitable for solid electrolyte materials at all. In the prior art, it was common to select an additive component with high lithium ion conductivity to improve the electrical characteristics of a battery. However, in the present invention, the first component with low lithium ion conductivity is creatively added to the positive electrode, improving the CEI on the surface of the positive electrode, thereby significantly improving the rate characteristics, cycle characteristics, and safety of the battery, thereby overcoming the prejudice of the existing technology. The mixed component particles of the first component and the second component simultaneously added to the positive electrode plate for lithium batteries of the present invention can improve the stability of the CEI on the surface of the positive electrode particles, suppress oxygen release from the positive electrode during thermal runaway and reaction with the electrolyte, suppress decomposition of the electrolyte, and improve the electrical characteristics and safety of the battery. Experiments have proven that the synergistic effect is better when the first component and the second component are used simultaneously.

[0036] The content of the first component or the mixed component particles of the first component and the second component added to the lithium battery positive electrode plate of the present invention is specially designed. If the content is less than 0.1% by weight, it is difficult to form an effective CEI layer, and the improvement of electrical properties and safety is insufficient. If the content is more than 6% by weight, the content of inactive materials in the battery increases, and the energy density of the battery decreases. The obtained positive electrode shows excellent rate characteristics, cycle characteristics, and safety. [Brief description of the drawings]

[0037] [Figure 1] FIG. 4 is a structural schematic diagram of a positive electrode plate for a lithium battery in Example 2. [Diagram 2] FIG. 2 is a structural schematic diagram of a positive electrode plate for a lithium battery in Example 1. [Diagram 3] FIG. 2 is a schematic diagram of a heavy-duty impact test of the lithium battery of the present invention. [Figure 4] FIG. 11 is a schematic diagram showing the structure of a positive electrode plate for a lithium battery in Example 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] The present invention will be specifically described below with reference to certain figures and examples. It should be noted that the following examples are only used to further explain the present invention and are not to be understood as limiting the scope of protection of the present invention. Non-essential improvements and adjustments of the present invention made by those skilled in the art based on the content of the present invention also belong to the scope of protection of the present invention. Example 1

[0039] Step 1: First component LiTiOPO4 and second component Li 1.4 Al 0.4 Ti 1.6 1 kg of a mixture composed of (PO4)3, 100 kg of NCM90 as a positive electrode active material, 1 kg of Super P, 1 kg of PVDF, and 500 kg of NMP solvent were uniformly mixed to form a slurry. Step 2: The slurry obtained in step 1 was applied to the surface of an aluminum current collector to form a positive electrode plate. Step 3: The electrode plate obtained in step 2 was baked at 95°C for 5 minutes, roll pressed at 28T, and die-cut to obtain a positive electrode plate with a layer thickness of 126 μm. The positive electrode plate was then vacuum-dried at 105°C for 24 hours to obtain the final positive electrode plate. The content ratio of the first component to the second component is 1:4, and the particle diameter D50 of the particles of the first component and the second component is each 200 nm. The positive electrode plate for lithium batteries manufactured by the above method includes a positive electrode material layer and a current collector 3, as shown in the structural schematic diagram of FIG. 2, and the positive electrode material layer includes a positive electrode active material 1, a conductive agent, a binder, a first component 2, and a second component 4, and the first component 2 and the second component 4 in the positive electrode material layer are dispersed between the particles of the positive electrode active material 1. The positive electrode plate and a SiOC650 negative electrode are combined to assemble a soft-pack lithium battery, and the lithium battery manufactured as above is subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests are respectively performed. Specific test results of electrochemical properties are shown in Table 1, and safety test results are shown in Table 2. The test method for the electrochemical properties of the lithium battery used in this application is as follows. 1. Cycling characteristic test a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Discharge the battery at a constant current of 1C until the end-of-discharge voltage is reached, then stop discharging and record the discharge capacity, completing one cycle. c) Repeat steps a and b until the discharge capacity falls below 80% of the first cycle discharge capacity, at which point record the total number of cycles the battery has undergone. 2. Rate Test a) At 23℃±2℃, charge the battery at rates of 0.1C, 0.2C, 0.33C, 1C, 2C, and 3C to the charge end voltage, then discharge at the same rate current to the discharge end voltage, and repeat 4 cycles at the same rate. b) Record the discharge capacity at each rate. c) The ratio of the 2C or 3C discharge capacity to the 0.33C discharge capacity is calculated, expressed as 2C / 0.33C or 3C / 0.33C, and the rate characteristics are evaluated. 3. High temperature cycle a) At 45°C, charge at a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging, and stop charging when the charging current rate drops to 0.05C. b) Leave the battery at 45°C for 5 hours. c) Under high temperature conditions of 45°C, the battery is discharged at a constant current of 1C until the discharge end voltage is reached, then the discharge is stopped and the discharge capacity is recorded, which completes one cycle. d) Repeat steps a through c until the discharge capacity falls below 80% of the first cycle discharge capacity, at which point record the battery's discharge capacity and the total number of cycles. The safety test method for lithium-ion batteries is as follows: 1. Overcharging a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Continue charging the battery at a constant current of 1C until the battery begins to experience thermal runaway, and record the battery voltage when thermal runaway begins. 2. Hotbox a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Place the battery in the test box. Heat the test box at a rate of 5℃ / min. After the temperature inside the box reaches 160℃±2℃, keep the temperature constant for 1 hour. If the battery does not emit smoke, fire or explode, it passes; if not, it fails. 3. Falling a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Free fall from a height of 1 m onto a concrete slab. The soft-pack battery is dropped once on each side for a total of six tests. After six tests, if the battery does not emit smoke, catch fire or explode, it is considered to have passed the test; otherwise, it has failed the test. 4. Heavy object impact a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) A battery 8 is placed on the surface of the platform, and a metal rod 9 with a diameter of 15.8 mm±0.2 mm is placed horizontally on the upper surface of the geometric center of the battery. A weight of 9.1 kg±0.1 kg is allowed to fall freely from a height of 610 mm±25 mm onto the surface of the battery on which the metal rod is placed, and the battery is observed for 6 hours. A schematic diagram of the heavy-weight impact test is shown in Figure 3, where 5 is a towing rope, 6 is a guide pipe, and 7 is a steel impact box (hinged door is not shown). Only the large surfaces of the soft-pack batteries are impact tested, ensuring that only one impact test is performed per sample. If the battery does not emit smoke, fire or explode, it passes; if not, it fails. 5. Stab a) Charge at 23℃±2℃ with a constant current of 1C until the end-of-charge voltage is reached, then switch to constant voltage charging. When the charging current rate drops to 0.05C, stop charging and leave to rest for 1 hour. b) Using a φ8 mm high-temperature resistant steel needle (the cone angle of the needle tip is 45°, the surface of the needle is shiny and free of rust, oxide layers and oil stains), pierce the battery at the geometric center of the piercing surface from a direction perpendicular to the battery plate at a speed of 25 mm / s, and leave the steel needle inside the battery. c) Observe for 1 hour. If the battery does not emit smoke, fire or explode, it passes; if not, it fails. Example 2

[0040] The 1 kg mixed component consisting of the first and second components was changed to 1 kg of the first component and not to the second component, the positive electrode active material was changed to NCM83, and the battery structure was changed to NCM83||SiOC650, with the other parameters being the same as in Example 1. The manufactured positive electrode plate for lithium batteries includes a positive electrode material layer and a current collector 3, as shown in the structural schematic diagram of FIG. 1, and the positive electrode material layer includes a positive electrode active material 1, a conductive agent, a binder, and a first component 2, and the first component 2 in the positive electrode material layer is dispersed between the particles of the positive electrode active material 1. The lithium battery manufactured as described above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed. Specific test results of the electrochemical properties of the lithium battery manufactured using this positive electrode plate are shown in Table 1, and safety test results are shown in Table 2. Example 3

[0041] The second component was changed to AlPO4, the negative electrode was changed to SiOC450, and the battery structure was changed to NCM83||SiOC450, and the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 4

[0042] The second component is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in the first and second components 1.4 Al 0.4 Ti 1.6The mass ratio of (PO4)3 and AlPO4 was 1:8:1, the positive electrode active material was changed to LCO, the negative electrode was changed to SiOC450, and the battery structure was changed to LCO||SiOC450, and the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 5

[0043] The 1 kg mixed component consisting of the first and second components was changed to one containing only 1 kg of the first component LiTaOSiO4 and not containing the second component, the positive electrode active material was changed to LFP, the negative electrode was changed to graphite, and the battery structure was graphite||LFP, with the other parameters being the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium battery, and Table 2 shows the results of the safety tests. Example 6

[0044] The first component was changed to LiTaOSiO4, and the second component was changed to Li 1.4 Al 0.4 Ge 1.6 The other parameters were the same as in Example 1, except that the active material of the positive electrode was changed to (PO4)3, the active material of the positive electrode was changed to NCM83, the negative electrode was changed to graphite, and the battery structure was graphite||NCM83. The lithium batteries manufactured as described above were subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium batteries are shown in Table 1, and the results of the safety tests are shown in Table 2. Example 7

[0045] The 1 kg mixed component consisting of the first and second components was changed to one containing only the first component LiTaOGeO41 kg and not the second component, and the other parameters were the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium battery, and Table 2 shows the results of the safety tests. Example 8 The first component was changed to LiTaOGeO4, the second component was changed to Al2SiO5, the positive electrode active material was changed to NCM83, and the battery structure was changed to NCM83||SiOC650, and the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 9

[0046] The second component is Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in the first and second components 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was 1:8:1, and the particle diameter D50 of the first and second component particles was changed to 50 nm, and the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 10

[0047] The second component is Li 1.4 Al 0.4 Ti 1.6(PO4)3 and AlPO4, the ratio of the first and second components was changed to 1:8:1, and the particle diameter D50 of the first and second component particles was changed to 500 nm, with the other parameters being the same as in Example 1. After the above-mentioned lithium battery was subjected to processes such as injection, formation, and capacity grading, electrochemical tests and safety tests were respectively carried out. The specific test results of the electrochemical properties of the lithium battery manufactured are shown in Table 1, and the safety test results are shown in Table 2. Example 11

[0048] The total amount of the mixture consisting of the first and second components was changed to 0.5 kg, and the second component was changed to Li 1.4 Al 0.4 Ti 1.6 (PO4)3 and AlPO4, and Li in the first and second components 1.4 Al 0.4 Ti 1.6 The mass ratio of (PO4)3 and AlPO4 was 1:8:1. Each primary particle of the mixed component contained first component crystalline form and second component crystalline form particles, and the particle diameter D50 of the primary particle of the mixed component was 200 nm. The mixed morphology is shown in FIG. 4, where 1 is the active material, 2 is the mixed component of the first component and the second component in the same particle, and 3 is the current collector. Other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed. Specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Example 12

[0049] The total amount of the mixture consisting of the first and second components was changed to 5 kg, and the second component was changed to Li 1.4 Al 0.4 Ti 1.6(PO4)3 and AlPO4, and the ratio of the first and second components was changed to 1:8:1, with the other parameters being the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium battery, and Table 2 shows the results of the safety tests. Comparative Example 1

[0050] Except for not including the first component and the second component, the other parameters were the same as in Example 1. The lithium battery manufactured as described above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 2

[0051] The first and second components were not included, the positive electrode active material was changed to NCM83, and the battery structure was changed to NCM83||SiOC650, and other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 3

[0052] The first and second components were not included, the positive electrode active material was changed to NCM83, the negative electrode was changed to SiOC450, and the battery structure was changed to NCM83||SiOC450, and the other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 4

[0053] The first and second components were not included, the positive electrode active material was changed to LCO, the negative electrode was changed to SiOC450, and the battery structure was LCO||SiOC450, and other parameters were the same as in Example 1. The lithium battery manufactured as above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 5

[0054] The other parameters were the same as in Example 1, except that the first and second components were not included, the positive electrode active material was changed to LFP, the negative electrode was graphite, and the battery structure was LFP||graphite. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 6

[0055] The other parameters were the same as in Example 1, except that the first and second components were not included, the positive electrode active material was changed to NCM83, the negative electrode was graphite, and the battery structure was NCM83||graphite. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 7

[0056] The other parameters were the same as in Example 1, except that the 1 kg of the mixed component consisting of the first and second components was changed to 1 kg of Al2O3. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 8

[0057] The other parameters were the same as in Example 1, except that 1 kg of the mixed component consisting of the first and second components was changed to 1 kg of ZnO, the positive electrode active material was changed to NCM83, and the battery structure was changed to NCM83||SiOC650. The lithium battery manufactured as described above was subjected to processes such as injection, chemical formation, and capacity grading, and then electrochemical tests and safety tests were performed. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium battery, and Table 2 shows the results of the safety tests. Comparative Example 9

[0058] 1 kg of the mixture consisting of the first and second components is added to Li 1.4 Al 0.4 Ti 1.6 The other parameters were the same as in Example 1, except that the weight of the battery was changed to 31 kg (PO4), the positive electrode active material was changed to NCM83, the negative electrode was changed to SiOC450, and the battery structure was changed to NCM83||SiOC450. The lithium batteries manufactured as described above were subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium batteries, and Table 2 shows the results of the safety tests. Comparative Example 10

[0059] The other parameters were the same as in Example 1, except that 1 kg of the mixed component consisting of the first and second components was changed to 1 kg of AlPO4, the positive electrode active material was changed to LCO, the negative electrode was changed to SiOC450, and the battery structure was changed to LCO||SiOC450. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. Table 1 shows the specific test results of the electrochemical properties of the manufactured lithium battery, and Table 2 shows the results of the safety tests. Comparative Example 11

[0060] 1 kg of the mixture consisting of the first and second components is added to Li 0.5 La 0.5The other parameters were the same as in Example 1, except that the amount of TiO3 was changed to 1 kg, the second component was not included, the positive electrode active material was changed to LFP, the negative electrode was changed to graphite, and the battery structure was LFP||graphite. The lithium battery manufactured as described above was subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were performed. The specific test results of the electrochemical properties of the manufactured lithium battery are shown in Table 1, and the safety test results are shown in Table 2. Comparative Example 12

[0061] 1 kg of the mixture consisting of the first and second components is Li7La3Zr2O 12 The weight of the battery was changed to 1 kg, the positive electrode active material was changed to NCM83, the negative electrode was changed to graphite, and the battery structure was changed to NCM83||graphite, with the other parameters being the same as in Example 1. The lithium batteries manufactured as described above were subjected to processes such as injection, formation, and capacity grading, and then electrochemical tests and safety tests were carried out. The specific test results of the electrochemical properties of the manufactured lithium batteries are shown in Table 1, and the safety test results are shown in Table 2. Table 1 shows the electrochemical property data of the examples.

[0062] [Table 1] Table 2 shows safety data for the examples.

[0063] [Table 2]

[0064] From the data in Tables 1 and 2, the rate characteristics, cycle characteristics and safety of the battery can be significantly improved by blending the first component or the mixed component of the first component and the second component into the positive electrode. Comparing Example 5 with Comparative Example 11, it was found that blending the first component into the positive electrode has a much stronger effect of improving the battery rate characteristics, cycle characteristics and safety than blending a solid electrolyte with high lithium ion conductivity, since constructing a high-efficiency CEI is the key to improving the electrical characteristics and safety of liquid batteries and mixed solid-liquid batteries. As can be seen from the comparison between Example 1 and Example 7, the mixed component in which the first component and the second component are simultaneously blended can further improve the rate characteristics, cycle characteristics and safety of the battery compared to the case in which only the first component is blended, since the first component and the second component can synergistically improve the CEI. As can be seen from the comparison between Example 1 and Examples 9 and 10, there is an optimal particle size for the first component and the second component, and optimizing the particle size can improve the rate characteristics and cycle characteristics of the battery. If the particle size is too small, the first component or the mixed component particles composed of the first component particles and the second component are likely to aggregate, and if the particle size is too large, the first component or the mixed component particles composed of the first component and the second component cannot sufficiently contact the active material particle surface, and if the particle size is too small or too large, it is disadvantageous for the construction of a stable CEI. As can be seen from the comparison between Example 1 and Comparative Examples 11 and 12, there is an optimal ratio for the amount of the first component and the second component added, and if the amount is too low, the rate characteristics and safety of the battery cannot be improved, and if the amount is too high, the first component or the mixed component composed of the first component and the second component is too high, the particles accumulate and a region with low lithium ion conductivity is formed, so that higher rate characteristics cannot be exhibited.

[0065] It should be understood that the above embodiments are merely exemplary embodiments adopted to explain the principles of the present invention, but the present invention is not limited thereto. Those skilled in the art can make various modifications and improvements without departing from the spirit and essence of the present invention, and these modifications and improvements are considered to be within the protection scope of the present invention.

Claims

1. A positive electrode plate for a lithium battery, comprising a positive electrode material layer including a positive electrode active material, a conductive agent, a binder, and a first component, The first component is Li 1-x1 Ti 1-x1 A x1 O.P.O. 4 , Li 1-x1 Ti 1-x1 A x1 P.O. 5 , Li 2-y1 Ti 1-y1 A y1 OM1O 4 , Li 2-y1 Ti 1-y1 A y1 M1O 5 wherein 0≦x1≦0.7, 0≦y1≦1, A includes at least one of Nb, Ta, and Sb, and M1 is at least one of Si and Ge; The first component is preferably LiTiOPO 4 , Li 0.9 Nb 0.1 Ti 0.9 O.P.O. 4 , Li 0.9 T 0.1 Ti 0.9 O.P.O. 4 , Li 2 TiOSiO 4 , LiTaOGeO 4 A positive electrode plate for a lithium battery, characterized in that the positive electrode plate is at least one of the above.

2. The positive electrode layer further includes a second component, the second component being LiM2 2 (P.O. 4 ) 3 , Li 1+x2 A x2 M2 2-x2 (P.O. 4 ) 3 , M2O 2 , Li 16-4y2 M2 y2 O 8 , M2P 2 O 7 , M3PO 4 , M3 2 SiO 5 , M4 3 (P.O. 4 ) 2 , M4 2 SiO 4 wherein M2 is one selected from Ti, Ge, Zr, and Hf, where 0<x2<0.6; M3 and M4 are independently any one selected from Al, Ga, Sc, Y, Ca, Sr, Zn, Si, In, Lu, La, Fe, Cr, and Ge, where 3<y2<4; The second component is preferably InPO 4 , LATP, AlPO 4 , LAGP, LATP+AlPO 4 , LAGP+Al 2 SiO 5 , InPO 4 + LATP, Al 2 SiO 5 , TiO 2 +LiTi 2 (P.O. 4 ) 3 , TiP 2 O 7 + LiGe 2 (P.O. 4 ) 3 2. The positive electrode plate for a lithium battery according to claim 1, wherein the positive electrode plate is one of the following:

3. The form of the mixed component composed of the first component and the second component is a mixture of the first component particles and the second component particles uniformly mixed with each other, or each primary particle contains the first component crystal form and the second component crystal form. The positive electrode plate according to claim 1 .

4. The mass ratio of the first component to the positive electrode active material in the positive electrode material layer is w 1 Then, 0 < w 1 <5%, preferably 0.1 < w 1 2. The positive electrode plate for a lithium battery according to claim 1, characterized in that the content of the first component is 0.1% or less and the particle size of the first component is between 10 nm and 10 μm, preferably between 50 nm and 500 nm.

5. The mass ratio of the second component to the positive electrode active material is w 2 Then, 0≦w 2 < 5%, preferably 0 ≤ w 2 3% and the particle size of the second component is between 10 nm and 10 μm, preferably between 50 nm and 500 nm.

6. 2. The positive electrode plate for lithium batteries according to claim 1, wherein the positive electrode active material comprises at least one of a lithium cobalt oxide positive electrode and a modified material thereof, an NCM ternary positive electrode and a modified material thereof, an NCA ternary positive electrode and a modified material thereof, a lithium nickel manganate positive electrode and a modified material thereof, a lithium rich positive electrode and a modified material thereof, and a lithium iron phosphate positive electrode and a modified material thereof.

7. Step 1: uniformly mixing a first component or a mixture of the first component and the second component, a positive electrode active material, a conductive additive, a binder, and a solvent to form a slurry; Step 2 of applying the slurry obtained in step 1 to a surface of an aluminum current collector to form a positive electrode plate; and step 3 of blowing and vacuum drying the positive electrode plate obtained in step 2 to obtain a final positive electrode plate. The method for producing a positive electrode plate for a lithium battery according to any one of claims 1 to 5.

8. A lithium battery cell comprising a positive electrode plate, a negative electrode plate, a separator, an electrolyte, and a case, the positive electrode plate being the positive electrode plate according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • All solid battery