Battery cell including an anode and method for manufacturing same
The 3D printed carbon-based anode with a porous lattice structure addresses the limitations of existing lithium-ion batteries by increasing areal capacity and charging speed while maintaining specific capacity, enhancing energy density and reducing costs.
Patent Information
- Application Number
- JP2024532470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-30
- Filing Date
- 2022-11-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium-ion batteries face challenges in achieving higher areal capacity, maintaining specific capacity during charge-discharge cycles, and improving charging speed due to limitations in electrode design and material utilization, particularly with thicker anodes.
A battery cell design featuring a carbon-based anode composed of interconnected filaments in a predetermined structural arrangement, forming a porous lattice structure with intra-structural pores, manufactured through 3D printing, allowing for increased active material loading and improved electrolyte access.
The design achieves at least 50% higher areal capacity and significantly faster charging speeds, with maintained specific capacity and reduced inert component ratio, resulting in enhanced energy density and reduced costs.
Smart Images

Figure 2024542695000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a battery cell comprising an anode. The present invention also relates to a method for manufacturing a battery cell comprising an anode. The present invention also relates to an anode for use in a battery cell. The present invention also relates to a method for manufacturing an anode for a battery cell. Furthermore, the present invention relates to a battery and a battery cell comprising such an anode. Additionally, the present invention relates to an additive manufacturing system. [Background technology]
[0002] Energy storage devices such as lithium-ion batteries are central to the consumer electronics industry, transportation systems, and energy grids. Typically, Li-based batteries have relatively high capacity, high voltage, and low mass density compared to other battery systems. This makes lithium-ion batteries ideal for a wide range of different products, such as electric vehicle batteries, smartphones, and other rechargeable systems. However, the structure of the battery cell and the materials used in its construction tend to make commercial lithium-ion batteries more expensive than comparable batteries with aqueous electrolytes.
[0003] Currently, rechargeable Li batteries use carbon-based materials or other alloys as the anode, which allow the intercalation of Li+ in the solid electrolyte interphase (SEI) layer. Graphite is often used as the anode material because a high concentration of Li+ can be intercalated / deintercalated or adsorbed / desorbed into the carbon material (C:Li=6:1) during charging / discharging.
[0004] Graphite can be used as an anode material due to its excellent stability. However, the graphene planes easily move along the a-axis direction during lithium intercalation and deintercalation, resulting in volume changes, which makes it a very difficult material to use in 3D printing of anodes. To date, lithium titanate (LTO) has been mainly used for additive manufacturing of anode materials to circumvent this problem.
[0005] Many challenges still need to be overcome in order to more widely adopt and efficiently use renewable energy sources. In particular, increasing storage capacity, increasing charging capacity without reducing charge / discharge rate or power, increasing discharge rate, and extending life span remain the main challenges to be overcome. Increasing charging capacity and discharging power remains a problem to be solved, especially when extending the driving range of electric vehicles. A further challenge involves heat loss during the operation of the battery, which should not be increased any more. Improvement of these aspects of battery performance can be achieved at least in part by modifying the battery chemistry, but this creates scaling barriers and safety risks.
[0006] Conventional electrodes used in energy storage devices usually have a block shape and are fabricated by mixing the electrode material with one or more binders and pressing the mixture into the electrode. However, this method of fabricating the electrode results in an inappropriate pore structure, which results in limited ion transport within the electrode. The slow kinetics associated with ion and electron transport significantly limits the maximum power density / discharge rate of the battery. Additionally, it is estimated that a significant portion of the electrode, 30-50%, remains unutilized during battery operation, especially for lithium-ion batteries (US2020 / 112030A1). Reducing the characteristic ion and electron diffusion lengths within the active battery materials has proven successful in increasing power density and discharge rate. However, this has also resulted in a significant decrease in energy density (US2020 / 112030A1).
[0007] In thick electrode designs, the active material loading can be significantly increased by reducing the inactive component ratio at the cell level, which results in improved battery energy density and reduced cost. If the anode thickness becomes too large, the effect of thickness can be weakened. If the anode thickness exceeds a certain threshold, the resulting capacity can stagnate. Further increase in thickness can have a limited effect on capacity. In some cases, such an increase in thickness beyond a threshold can result in reduced capacity. If the anode thickness is too large, the charge transfer kinetics of the thick electrode can be degraded. Electrolyte penetration can be hindered and ion transfer distances can be significantly increased.
[0008] For example, there is a strong desire for battery cells with anodes that have increased capacity, even at greater thicknesses such as through thick electrode design approaches. Summary of the Invention [Problem to be solved by the invention]
[0009] It is an object of the present invention to provide a battery cell having an improved anode.
[0010] Additionally or alternatively, it is an object of the present invention to provide a method for manufacturing a battery cell with an anode that avoids at least one of the above-mentioned disadvantages.
[0011] Additionally or alternatively, it is an object of the present invention to provide a battery cell with a thicker anode having adequate areal capacity.
[0012] Additionally or alternatively, it is an object of the present invention to provide a battery cell with an anode that has a high specific capacity that can be maintained at a desired level during subsequent charge-discharge cycles. [Means for solving the problem]
[0013] The present invention provides a battery cell including an anode, the anode comprising interconnected filaments of material positioned in a predetermined structural arrangement in multiple layers stacked on top of one another, the filaments positioned such that successive layers are connected to one another to form a porous anode structure with in-structural pores formed between the filaments, the build material comprising a carbon-based active material configured to participate in the battery electrode reactions.
[0014] The anodes of the battery cells can be made with a greater thickness than can be obtained with existing techniques such as doctor blading. Higher areal capacities can be achieved for the same amount of material, i.e., the areal capacity can be increased by at least 50% compared to prior art materials. Additionally, the charging rate can also be substantially increased. Areal capacity can be understood as the capacity per unit of surface area of the anode material. The areal capacity is preferably at least 10 mAh / cm after five cycling steps involving charging and discharging a battery incorporating the anode. 2 , preferably at least 12 mAh / cm 2 It is.
[0015] A higher areal capacity per unit weight of material can be achieved for the same specific capacity of the material, with the specific capacity per gram of anode material (mAh / g) being at least 80%, preferably at least 85%, more preferably at least 90% of the theoretical specific capacity calculated from the composition of the anode material.
[0016] The invention also provides a method of manufacturing a battery cell with such an anode, wherein the anode of the battery cell is produced by depositing interconnected filaments of a building material in multiple layers stacked on top of each other in a predetermined structural arrangement, the filaments positioned such that successive layers are connected to each other to form a porous anode structure with intrastructural pores formed between the filaments, and the building material includes a carbon-based active material configured to participate in the battery electrode reactions.
[0017] The method of the present invention provides a significantly improved battery cell with improved electrode design. The thick electrode design approach can obtain increased loading of active material. Higher areal capacity can be achieved due to the higher achievable electrode loading per unit of surface area. The amount of active material per unit surface area can be increased. Advantageously, the anode of the battery cell can be made thicker while providing adequate areal capacity. Additionally, the charge rate can be improved. Thus, a thick electrode design approach with improved areal capacity can be used. As a result of the spatial design of the mesh / lattice-like anode structure obtained by performing 3D printing of the filament in multiple stacked layers in a predetermined arrangement, various channels or pores can be formed between the filaments (e.g., for lithium-ion batteries) so that the electrolyte can easily access the active material. A larger portion of the anode can be accessed even with anodes having a larger thickness than conventionally used. As a result, lithium ions can more easily access the carbon-based active material. Even the lower and / or bottom portion of the anode can still be accessible. The inactive component ratio can be reduced, thereby resulting in increased battery energy density. Furthermore, the cost of the battery can be reduced. In some examples, the pore design (e.g., size, shape, pattern, etc.) can be selected based on the thickness of the anode, allowing for predictable design of the anode to achieve desired performance.
[0018] Furthermore, a high charge / discharge reversibility can be obtained, i.e., after being discharged, the anode can be recharged to nearly its initial capacity, and this reversibility is maintained over time, i.e., after many charge-discharge steps.
[0019] Furthermore, the accessibility of the carbon anode active material is less impaired or slowed by diffusion phenomena during charging (lithiation) and discharging (delithiation), and is significantly improved over conventional materials.
[0020] The battery cell electrode architecture according to the present disclosure can be used in thick electrode designs, which can advantageously significantly increase electrolyte permeability and ion transport rates.
[0021] Optionally, the interconnected filaments form a lattice structure. The lattice structure may be a predefined porous structure having pores. Various shapes and sizes are possible. Advantageously, the lattice structure may have a large specific surface area.
[0022] Typically, the anode having a carbon-based active material is configured for use at a relatively low operating voltage. Optionally, the battery cell anode is configured for use at an operating voltage of less than 1 V with Li metal as the counter electrode.
[0023] The carbon-based build materials used may be particularly suitable for use in robocasting, a technique in which a viscous paste is fed into a nozzle having a desired cross-section, travels through the nozzle, and is expelled from the nozzle to be deposited on a printing surface as a viscous paste in the shape of a filament, or fiber, or strut, or bead, etc. Robocasting may also be referred to as 3D printing, 3DFD, 3D fiber deposition, filament deposition, microextrusion, etc., or a combination of two or more of these. Specifically, the paste composition described above is suitable for use in a system for manufacturing a three-dimensional structure, the system including an extrusion unit including a nozzle having a nozzle outlet and a paste reservoir in fluid communication with the nozzle outlet, the extrusion unit being configured to deposit a filament of the paste composition through the nozzle outlet in a plurality of stacked layers in a predetermined interconnected arrangement to form a three-dimensional structure, a measurement unit including at least one sensor in the nozzle for monitoring a pressure value applied to a building material in a material reservoir of the nozzle for discharging the building material through the nozzle outlet during discharging of the filament by the extrusion unit, and a processing unit configured to adjust the extrusion when an irregular increase and / or decrease in the pressure value occurs. Examples of deposition parameters that may be adjusted during the printing process to correct for irregular increases or decreases in pressure values include, but are not limited to, adjusting, i.e., increasing or decreasing, the pressure exerted on the build material in the build material reservoir or in the nozzle, or at any point in the build material supply line before the build material exits the nozzle; adjusting the viscosity of the build material, for example, by heating or cooling the build material, by adjusting the amount of solvent contained in the build material, by supplying a release agent in the reservoir, in the nozzle, or at any point in the build material supply line before the build material exits the nozzle; adjusting the flow rate of the build material; applying vibration to the build material; adjusting the nozzle opening; and the like.
[0024] Optionally, a mesh of pores is formed in each layer.
[0025] The carbon-based active material and the specific mesh-like structure offer several important advantages: such a structure with pores obtained by a specific deposition arrangement allows the anode to be designed even thicker, thus allowing easier access to the active material and significantly increasing the energy capacity of the battery.
[0026] A 3D printed anode can be constructed by printing a series of filaments positioned to form a porous structure with a regular pattern of pores formed between the filaments. The porous structure can have an interconnected arrangement of filaments that forms a mesh / lattice structure.
[0027] Optionally, the mesh of pores has a regular pattern, and the pores are interconnected in the porous anode structure.
[0028] 3D printed carbon-based anodes can provide high areal capacitance. For example, graphite anodes can be printed with a lattice structure with regular patterns of pores. A large amount of active material per surface area can be obtained in an efficient manner, resulting in high capacitance per unit surface area.
[0029] Optionally, the build material comprises at least 60 wt. % of the carbon-based anode active material, more preferably at least 80 wt. %, and even more preferably at least 85 wt. %, based on the total weight of the build material.
[0030] Advantageously, the amount of active material in the battery anode can be effectively increased.
[0031] In some examples, a binder is used in the build material, hi some examples, the weight percentage of the binder in the build material is less than 10 weight percent based on the total weight of the build material.
[0032] Various binders and additives may be added to the build material, such as one or more conductive additives. In some examples, the weight percentage of carbon in the build material ranges from greater than 85% by weight, preferably greater than 90% by weight, and more preferably greater than 92% by weight, based on the total weight of the build material.
[0033] The amount of binder present in the building material may vary over a wide range, but the amount of binder in the building material is preferably at least 0.01% by weight, preferably at least 0.025% by weight, more preferably at least 0.10% by weight or 0.25% by weight, most preferably at least 0.50% by weight or at least 0.75% by weight, or at least 1.0% by weight, based on the total weight of the building material. It is further understood that the at least one binder component is usually contained in the paste composition in an amount of up to 7.5% by weight, preferably up to 6.0% by weight, more preferably up to 5.0% by weight, most preferably up to 3.0% by weight, especially up to 2.5% by weight, based on the total weight of the building material, based on the weight percentage of dry matter.
[0034] When the building material contains at least one binder, the at least one binder component can be an inorganic or organic compound, or a mixture of one or more inorganic compounds and one or more organic compounds. The binder can be more hydrophilic or more hydrophobic in nature. Preferably, the at least one binder is an organic compound, more preferably an organic compound that can modify the rheology or flow properties of the paste composition under the influence of pressure. The at least one binder component may be selected from one or more of the following: plasticizers, hydrocolloids, cellulose derivatives such as methylcellulose, ethylcellulose and / or derivatives such as carboxymethylcellulose, carboxyethylcellulose, and / or combinations thereof, polyvinylidene fluoride (PVDF, polyvinylidene fluoride), polytetrafluoroethylene (PTFE), polymeric alcohols, especially polyvinyl alcohols, polyalcohols such as polyethylene glycol, polyvinylpyrrolidones, poloxamers, i.e. a central hydrophobic chain of polyoxypropylene (poly(propylene oxide)) flanked by two hydrophilic chains of polyoxyethylene (poly(ethylene oxide)), capable of self-assembly and thermal gelation, generally available under the names Syperonic (Croda), Pluronic (BASF), Kolliphor (BASF), and combinations of two or more of the aforementioned binder materials. It should be clear to the skilled person that other materials exhibiting equivalent properties may be used as well.
[0035] In some examples, a conductive binder such as PEDOT:PSS is used.
[0036] Optionally, the carbon-based active material includes at least one of graphite, soft carbon, hard carbon, or a composite thereof.
[0037] Electrode active material refers to the material that participates in the actual electrode reaction. As the electrode active material, carbon-based materials can be used. Carbon-based materials are preferred for the anode due to their availability, low cost, and performance. In addition, the carbon material protects the lithium from the formation of dendrites while recharging the battery. Carbon-based materials are available in various forms. Preferably, carbon materials that are economical, environmentally friendly, and have a large specific surface area can be used. Carbon materials used as electrode active materials include activated carbon, hard carbon that cannot be converted to graphite by heat treatment, soft carbon that can be easily converted to graphite by heat treatment, carbon nanotubes (CNTs), carbon nanosprings, carbon nanorods, graphite, graphite flakes, graphene, carbon aerogel, acetylene black, Ketjen black, Super-P (registered trademark), etc. Preferred carbon materials include activated carbon, soft carbon, graphite, graphite flakes, graphene, carbon aerogel, acetylene black, Ketjen black, and Super-P, which have the ability to reversibly incorporate metal ions into their layered structures. These materials have high electrical conductivity.
[0038] Other carbon-based materials or compositions may also be used, such as, for example, Si-C active materials. In some instances, the majority of the capacity achieved by using carbon-based active materials may come from the carbon.
[0039] Optionally, the carbon-based active material has a carbon mass content of at least 50% by weight, more preferably at least 60% by weight, and even more preferably at least 80% by weight, based on the weight of the carbon-based active material.
[0040] Optionally, the carbon-based active material is a compound of a non-carbon material and a carbon material, and the carbon material is present in a mass percentage of at least 50 wt.%, more preferably at least 60 wt.%, and even more preferably at least 80 wt.%, based on the weight of the carbon-based active material.
[0041] Optionally, the porous anode structure of the battery cell has a thickness in the range of 0.1 to 5 millimeters, preferably in the range of 0.2 to 1 millimeter, and even more preferably in the range of 0.4 to 0.7 millimeters.
[0042] 3D printed carbon-based anodes can enable thicker electrode designs with advantageous properties. Carbon-based anodes can have high areal capacity. The anode has open pores through its thickness, forming a series of channels between the filaments. This can effectively increase the capacity of the battery.
[0043] Advantageously, the anode of the battery cell can be operated at a low operating voltage. Carbon-based anodes can have an operating voltage of less than 1 V with Li metal as the counter electrode. In some embodiments, the filament contains at least 85% by weight of carbon material.
[0044] Optionally, the anode of the battery cell has at least two stacked layers, more preferably at least three stacked layers, and even more preferably at least four stacked layers.
[0045] Optionally, the anode of the battery cell has a current limiting capability of at least 8 milliamp hours / cm 2 , more preferably at least 10 milliamp-hours / cm 2 , and even more preferably at least 12 milliamp-hours / cm 2 It has a capacity per unit surface area of
[0046] Optionally, the anode of the battery cell has a specific capacity per gram of anode material that is at least 80%, preferably at least 85%, more preferably at least 90% of the theoretical specific capacity calculated from the composition of the materials of construction.
[0047] Most of the material in the anode of a battery cell can become active. Conventional thick electrodes do not provide such increased capacity.
[0048] The amount of active material provides the storage of energy in the battery. It is therefore desirable to have a large amount of active material. In this way, the capacity and / or weight of the battery can be effectively reduced. Reducing the gap distance between adjacent filaments in a layer can result in an increase in load. Furthermore, layers of filaments can be stacked in different ways.
[0049] Optionally, the filaments have a diameter of from 50 to 750 microns, more preferably from 75 to 500 microns.
[0050] Optionally, the filaments in each layer are spaced apart, with the gap distance between opposing adjacent filaments in each layer being less than the thickness of the filaments.
[0051] Advantageously, the areal capacity can be significantly increased.
[0052] Optionally, the filaments are shaped such that the structural pores have a wider opening near a first end of the porous anode structure and a narrower opening near a second end of the porous anode structure, the second end being positioned opposite the first end, the wider opening being formed in one or more upper layers of the stacked layers.
[0053] In the thickness direction of the porous anode, the size of the pores may vary. The upper layer may be positioned on top of the lower layer during printing. For example, the top (free end) of the anode may be more open than the bottom. As a result, the bottom part of the anode has a larger contact area for electrical conductivity, and the pores in the upper / top part (see the free end opposite the bottom / lower) may be more open, favoring the diffusion of liquid. This may be achieved by manufacturing the anode by the 3D printing method according to the present disclosure.
[0054] The method of printing anodes for battery cells according to the present disclosure has a significant beneficial effect on the achievable areal capacity. A variety of porous anode structures can be 3D printed.
[0055] The pores of the stacked layers may have various shapes. The shape of the pores may be determined by the particular arrangement of the filaments in the layers. For example, the pores may have a polygonal shape.
[0056] Optionally, the pores in the stack layers have a rectangular shape.
[0057] Advantageously, the filaments can be deposited along straight lines to effectively reduce the manufacturing time even for complex lattice structures. The filaments can be deposited along straight paths, resulting in rectangular shaped pores. Since a fast deposition process can be obtained, the method can be adopted for mass production of such anodes. Additionally or alternatively, material waste as a result of the additive manufacturing process can be reduced. Additionally or alternatively, precise fabrication for good quality anode lattice structures can be obtained.
[0058] Other shapes are possible. For example, the pores may have a triangular, hexagonal, etc. Additionally or alternatively, the pores may have curved sides. Additionally or alternatively, the pores may have a lobed design, for example, a quarter-lobed shape.
[0059] According to one aspect, the present invention provides a battery cell / system including a three-dimensional porous anode structure according to the present disclosure.
[0060] According to one aspect, the present invention relates to an additive manufacturing system including a controller configured to implement a method according to the present disclosure.
[0061] According to one aspect, the present invention provides a battery cell with a carbon-based anode having a three-dimensional structure and including a plurality of interconnected filaments of anode material positioned in a predetermined three-dimensional arrangement in a plurality of successive stacked layers, the anode material having a density of at least 24 mg / cm 2 (e.g. at least 8mAh / cm 2anode active material in an amount equivalent to about 100 nm (equivalent to about 100 nm), a binder, and a solvent, wherein the anode active material comprises a carbon-based particulate material, and the filaments of successive layers are connected to each other at least at contact points between the filaments of successive layers to provide a porous structure having interconnected pores between the filaments, and the filaments of successive layers are at an angle to each other.
[0062] Optionally, the carbon-based anode of the battery cell has a capacity of at least 10 mAh / cm after five cycling steps including charging and discharging a battery incorporating the anode. 2 , preferably at least 12 mAh / cm 2 capacity per unit of surface area.
[0063] Optionally, the carbon-based anode of the battery cell has a specific capacity per gram of anode material (mAh / g) that is at least 80%, preferably at least 85%, and more preferably at least 90% of the theoretical specific capacity calculated from the composition of the anode material.
[0064] Optionally, the carbon-based anode of the battery cell has a charge / discharge reversibility of at least 90%, preferably at least 95%, more preferably at least 98%, and most preferably 99.5% when the anode is cycled.
[0065] Optionally, the carbon-based anode of the battery cell has macropores between the filaments and mesopores and / or micropores within the filaments, at least some of which allow access to the macropores.
[0066] According to one aspect, the present invention provides a method for manufacturing a three-dimensional carbon-based battery anode by producing a three-dimensional porous structure, the method comprising depositing interconnected filaments of a build material exiting an extrusion nozzle in a predetermined arrangement into a plurality of successive stacked layers, the build material comprising a viscous material composition comprising a carbon-based particulate material, the filaments of the successive layers being connected to each other at least at points of contact between the filaments of the successive layers to result in a porous structure having interconnected pores between the filaments, the filaments of the successive layers being at angles to each other, and the build material comprising at least 50 wt%, preferably at least 60 wt%, and more preferably at least 70 wt% carbon-based anode active material.
[0067] Optionally, the build material further comprises 0.5-25 wt. % of at least one binder material, preferably 1-15 wt. %, more preferably 1-10 wt. %. The amount of binder should be high enough to achieve as high a specific capacity as possible.
[0068] Optionally, the solvent includes one or more of water, alcohol, and the like.
[0069] Typically, the solvent is water, preferably deionized water. Alternatively, the solvent can be water, an organic solvent, an ionic liquid, or a mixture of two or more of the present invention or one of the mixtures of two or more of the present invention. Suitable solvents include one or more solvents selected from the group of water, alkanols, ketones, or a mixture of two or more of the present invention, more preferably water, deionized water, ethanol, isopropyl alcohol, acetone, ethyl acetate, or a mixture of two or more of the present invention. Other solvents that may be considered for use in the present invention include 1,2-propanediol, 1,3-dioxolane, 1,4-dioxane, 1-methyl-2-pyrrolidinone, 2-(2-butoxyethoxy)ethyl acetate, acetonitrile, butoxyethyl acetate, dimethyl adipate, dimethyl carbonate, hexane, methyl ethyl ketone, methyl isobutyl ketone, n-pentane, xylene, etc.
[0070] Optionally, the materials of construction include at least one thermoplastic material for the purpose of reducing volume change during charge / discharge.
[0071] Optionally, the build material is a viscous paste or suspension of inorganic particulate material.
[0072] It will be understood that the weight percentages may be based on dry matter content, e.g., moisture (e.g., solvent such as water) removed after a drying / conditioning step. Solvent may be added to the build material in an amount to have a composition that is more suitable for some additive manufacturing techniques, such as, for example, extrusion printing or robocasting.
[0073] It will be appreciated that various additive manufacturing techniques can be used to generate the anode. Additive manufacturing can be based on a layer-by-layer process from a computer-aided design model. For example, an extrusion process can be used in which a build material is extruded from a nozzle. A lattice anode structure can be printed as a result of the relative movement between the nozzle and the surface on which the build material is deposited.
[0074] It will be understood that any of the aspects, features, and options described in view of the method apply equally to the anode, additive manufacturing system, and battery described. It will also be apparent that any one or more of the above aspects, features, and options may be combined. [Brief description of the drawings]
[0075] The invention will be further explained on the basis of exemplary embodiments represented in the drawings, which are given by way of non-limiting example. It should be noted that the drawings are only schematic representations of embodiments of the invention, given by way of non-limiting example. In the drawings:
[0076] [Figure 1a] FIG. 2 shows a schematic diagram of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 1b]FIG. 2 shows a schematic diagram of an exemplary embodiment of an anode porous structure of a battery cell. [Diagram 2] FIG. 2 shows a schematic diagram of an exemplary embodiment of an anode porous structure of a battery cell. [Diagram 3] FIG. 2 shows a schematic diagram of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 4a] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 4b] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 4c] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Diagram 5] 1 shows a schematic diagram of an exemplary graph. [Figure 6] 1 shows a schematic diagram of an exemplary graph. [Figure 7a] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 7b] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 7c] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 8] 1 shows a schematic diagram of an exemplary graph. [Figure 9] 1 shows a schematic diagram of an exemplary graph. [Figure 10] 1 shows a schematic diagram of an exemplary graph. [Figure 11a] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 11b] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 11c] 1 shows an image of an exemplary embodiment of an anode porous structure of a battery cell. [Figure 12] 1 shows a schematic diagram of an exemplary graph. [Figure 13] 1 shows a schematic diagram of an exemplary graph. [Figure 14] 1 shows a schematic diagram of an exemplary graph. [Figure 15] FIG. 2 shows a schematic diagram of an exemplary embodiment of an anode porous structure of a battery cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0077] 1a and 1b show schematic diagrams of an exemplary embodiment of an anode porous structure 10 of a battery cell. FIG. 1a shows a cross-sectional side view and FIG. 1b shows a top view. The anode comprises interconnected filaments 2 of a carbon-based active building material positioned in a predetermined arrangement in a number of stacked layers 11, the filaments of successive layers being connected to each other to obtain a porous anode structure 10 with in-structure pores 3 formed between the filaments 2. The manner in which the filament-shaped building material is stacked into the multiple layers of the porous anode structure has a significant impact on the areal capacity achievable by the anode.
[0078] The filament may be printed, for example, by employing an extrusion additive manufacturing process or a dispenser printing process. In an exemplary extrusion process, a printing path may be followed to produce a three-dimensional anode porous structure 10. The filament may be deposited by a nozzle along said printing path. The filaments of successive layers are angled with respect to each other. In the extrusion process, the nozzle may be moved / scanned along the printing surface depositing the filament along the printing path. It is understood that it is also envisaged that the printing surface is moved instead of the nozzle 1 (kinematic reversal). A combination is also possible. In an alternative example, both the nozzle 1 and the printing surface may be moved during at least a portion of the deposition process.
[0079] It will be appreciated that a wide variety of print path configurations are possible to achieve the interconnected filament arrangement of the porous structure. By varying the deposition pattern, the properties of the anode porous structure 10 can be altered to achieve a desired areal capacity. In this example, the printed porous anode structure has a uniform interfilament spacing (interspace), although non-uniform interfilament spacing can also be employed, for example, on the sides of the anode.
[0080] In some examples, the spacing between the filaments of the anode porous structure 10 is less than the thickness of the filaments. Too large a spacing can have a detrimental effect on loading, as the total pore space increases (i.e., less active material per unit surface area). In some examples, the spacing between the filaments is in the range of 30 to 200 micrometers, more preferably in the range of 50 to 180 micrometers. For example, the spacing can be about 150 micrometers and the filaments can have a thickness of about 200 micrometers.
[0081] The pores can have a variety of shapes, for example the pores can be rectangular or square, however various other shapes are also possible (not shown in this figure).
[0082] The filaments 2 are deposited in a predetermined interconnected arrangement in multiple stacked layers 11 to form an anode porous structure 10 having interconnected pores 3. The porosity affects the areal capacity. The size and shape of the pores may depend on the deposited filaments and their printing path. For example, the size of the filaments, the orientation of the filaments, the distance between the filaments, the thickness of the anode porous structure 10, or the number of layers stacked on top of each other, etc., may have a significant effect on one or more performance characteristics of the battery (e.g., lithium-ion battery) in which the anode is used. For example, porous structures with filament orientations of 0 / 90, 0 / 60 / 120 and 0 / 45 / 90 / 135 may result in different pores and therefore different areal capacities. It will be understood that other laydown patterns are also envisioned, such as triangular, rectangular, hexagonal, curved, zigzag patterns, etc. These laydown patterns may also affect the pore size.
[0083] The anode porous structure 10 includes a plurality of filaments 2 spaced apart from one another in a plurality of stacked layers 11. As a result of the particular arrangement of the filaments 2, the anode porous structure 10 forms a plurality of voids (i.e., void spaces) that form the interconnected pores of the anode porous structure 10.
[0084] Advantageously, thicker electrodes can be obtained. Optionally, the porosity of the printed anode is selected based on the thickness of the anode. The thickness of the anode can be increased while mitigating the effect of the reduction in the amount of active material. As a result, the capacity can be effectively increased.
[0085] 2 shows a schematic diagram of a perspective view of an exemplary embodiment of an anode porous structure 10 of a battery cell. The anode porous structure 10 is 3D printed on a printing surface 5 by depositing a filament in different layers stacked on top of each other. The anode porous structure 10 has a top portion 6a and a bottom portion 6b. The bottom portion 6b may be in contact with the printing surface 5.
[0086] At least two layers can be stacked on top of each other. Preferably, at least three layers are stacked. For example, the total number of layers stacked on top of each other can range from 3 to 5. In this example, the exemplary anode porous structure 10 has five layers.
[0087] From a production standpoint, it may be beneficial to manufacture the anode by performing the deposition of the filaments along straight lines. The printing process may be accelerated by printing the filaments along straight lines in an arrangement that forms a regular pattern of intrastructural pores within the anode porous structure 10 (see lattice / mesh porous structures).
[0088] In some examples, the filament is printed by employing an extrusion printing process.
[0089] FIG. 3 shows a schematic diagram of a cross-sectional side view of an exemplary embodiment of an anode porous structure 10 of a battery cell. The porous structure 10 comprises a plurality of layers 11 of deposited filaments 2 stacked on top of each other. The filaments 2 have a filament diameter D and an interfilament distance A. The layers may have a height H. This height may substantially correspond to the filament diameter D. However, variations are also possible. By adopting different heights H, the vertical and horizontal pores can be modified. In this way, the areal capacity can be further increased.
[0090] The porous 3D printed anode structure allows for the production of batteries with significantly higher areal capacities compared to batteries known in the art. In some instances, a minimum areal capacity of 8 milliamp hours per square centimeter can be obtained. In some instances, the areal capacity is greater than 10 milliamp hours per square centimeter, or even greater than 14 milliamp hours per square centimeter.
[0091] The building material may be extruded in the form of a first layer, the first layer comprising a plurality of filaments 2. The filaments 2 may be, for example, part of an elongated strand of deposited carbon-based building material. In one example, the elongated strand is deposited continuously. However, discontinuous deposition is also possible. Furthermore, one or more additional layers may be extruded, each additional layer comprising a plurality of filaments 2 stacked vertically on a previously extruded layer and also angled with respect to some of the filaments 2 of the previous layer. The predetermined pattern is distributed to define the three-dimensional object being manufactured.
[0092] Volume per unit surface area (e.g., 1 cm 2 The areal capacitance is influenced by the structural characteristics of the anode. Areal capacitance relates to the active material per unit surface area. By depositing the filaments in multiple stacked layers in a predefined arrangement, the filaments of successive layers are connected to each other, resulting in a porous anode structure with in-structure pores formed between the filaments, resulting in a high capacitance per unit surface area (e.g., 1 cm2). 2 This allows for more active material to be obtained per unit.
[0093] The areal capacity of an electrode is a function of the thickness and volumetric capacity of the electrode. Active material properties such as specific capacity, crystalline density, volume fraction within the electrode also affect the areal capacity. Advantageously, a specific capacity that is at least 80%, preferably at least 85%, more preferably at least 90% of the theoretical specific capacity based on the composition of the anode material can be obtained. This specific capacity can be maintained over time, i.e. after many charge-discharge cycles.
[0094] (Example) The test conditions, instrumentation and preparation of the cells are described in this paragraph. Coin-cell batteries (CR2032) were charged with 3D-printed graphite-based electrodes (area: 1.80 cm) in an argon-filled glove box (Jacomex GP-concept) with HO < 1 ppm and O < 1 ppm. 2The coin batteries were assembled using a 15.1 mm diameter lithium metal disk (Alfa Aesar 99.9%) as the negative electrode and a 16 mm diameter lithium metal disk (Alfa Aesar 99.9%) as the negative electrode. A polymer separator (Celgard 2400, 19 mm diameter) was positioned between the two electrodes. Each cell was filled with 200 μL of standard LP30 electrolyte (SoulBrain MI), i.e., 1 M hexafluorophosphate LiPF6 in ethylene carbonate (EC) and dimethyl carbonate (DMC) in a 1:1 weight ratio. The cells were sealed with a pneumatic press in a glove box, transferred to a temperature chamber at 25 °C, and connected to a Bio-Logic battery tester BCS-810 for galvanostatic cycling. The coin batteries were equilibrated at open circuit voltage (OCV) for 6 h and then galvanostatic charging and discharging, i.e., constant current, were used to charge and discharge the Li + The electrodes were cycled over a voltage range of 0.02-1.0 V vs. / Li. The C-rate is defined as 1C, which corresponds to one full charge or discharge in 1 hour. Based on the theoretical specific capacity of graphite of 372 mAh / g, 1C-rate = 372 mA / g and C / 10-rate = 37.2 mA / g of graphite. Other components of the electrode (carbon additives, binder, carbon fiber, etc.) are assumed not to contribute to the capacity of the electrode.
[0095] 4a, 4b, and 4c show images of an exemplary embodiment of the anode porous structure of a battery cell. The images are obtained using a scanning electron microscope. The printed structure contains 90 w.% graphite and 10 w.% CMC (pH=3) as binder. The anode composition is 90 / 10 wt.%.
[0096] The SEM images shown in Figures 4a-4c show the expanded network of graphite electrodes. The shape and diameter of the fibers are very regular and close to 150-160 micrometers. Considering an initial diameter of 200 μm (the size of the nozzle used), a shrinkage of about 25% in diameter and about 45% in volume occurred during dyeing. The dried 3D printed electrodes show a homogeneous aspect and even surface cracks or breaks of the fibers cannot be observed despite the stresses caused by such significant shrinkage. The fibers appear to be composed of randomly packed irregular spheres ("potato shaped" in battery vocabulary) with a diameter of about 15 μm, in agreement with the particle size distribution of the graphite powder. There was no change in the morphology of the graphite particles during the paste preparation and printing of the electrodes. The presence of the CMC polymer can hardly be seen. This proves a very fine dispersion of the polymer binder within all 3D printed graphite electrodes, ensuring good mechanical cohesion. Higher magnification shows that the 3D printed electrodes are clearly porous, even at the micrometer scale, due to the irregular packing of the graphite particles. A minimum amount of porosity is necessary to allow good wetting of all graphite particles, even those present in the depth of the fiber, to obtain sufficient lithium-ion exchange between the graphite particle surfaces and the electrolyte.
[0097] 5 shows a schematic diagram of an exemplary graph showing the evolution of specific capacity and coulombic efficiency versus cycles for a graphite 3D printed electrode with CMC pH3 as binder. The electrode composition is 90 / 10% by weight.
[0098] The capacity of the 3D printed graphite electrodes in the battery cell was measured in a half-cell configuration using standard components (Celgard separator, LP30 electrolyte), see the cell preparation part. The initial specific capacity was limited to 87 and 108 mAh / g for the first discharge (i.e., oxidation, delithiation) and charge (i.e., reduction, lithiation), respectively (Figure 5), with a limited coulombic efficiency of 87%.
[0099] The specific capacity and coulombic efficiency increase dramatically for the second cycle, with values of 305 (discharge) and 312 (charge) mAh / g, respectively, with a coulombic efficiency of 97.9%. In the following cycles, the specific capacity increases continuously to reach during the fifth cycle, a discharge of about 335 mAh / g, a charge of 338 mAh / g, and a coulombic efficiency of 99.3%. The specific capacity of 335 mAh / g during discharge corresponds to 90.8% of the theoretical capacity of the graphite material of 372 mAh / g, and with reference to the practical capacity of commercial spherical graphite of 364 mAh / g, it reaches 92.9%.
[0100] From cycle 6 to cycle 20, the capacity changes very little and can reasonably be considered stable. The coulombic efficiency, on the other hand, increases slowly and continuously until it reaches 99.7% at cycle 20.
[0101] Higher coulombic efficiencies are unlikely due to the half-cell configuration (the SEI at the Li metal / electrolyte interface is not stable) and the use of standard LP30 electrolyte without additives.
[0102] After 20 cycles, the charge / discharge rate is increased to C / 20. After 10 cycles at C / 20, a significant loss in the ability to achieve a charge of 311 mAh / g is observed (#30, Figures 5 and 6), while the coulombic efficiency remains at 99.7%. The corresponding discharge capacity is 304 mA / g, with a coulombic efficiency of 99.9%.
[0103] 6 shows a schematic diagram of an exemplary graph showing the charge / discharge profile of a graphite 3D printed electrode with CMCpH3 as the binder. The electrode composition is 90 / 10% by weight.
[0104] The galvanostatic profile of the first cycle (FIG. 6) is not typical of the reduction and oxidation of graphite. Only the final stage IV of the delithiation of reduced graphite LiC6 occurs with the addition of Li +A potential hysteresis between charge and discharge shows a minimum close to 0.17 V.
[0105] The galvanostatic profile of the second cycle is not a typical profile of the lithiation and delithiation of a graphite electrode, especially in the reduction, but it does show a positive and dramatic evolution compared to the first cycle. In the early stages of the second reduction (about 20-40 mAh / g), Li + A first cathodic pseudo-plateau was observed at 0.17–0.18 V vs Li, followed by a potential drop at approximately 75 mAh / g Li + / Li at approximately 0.02 V, then rises again to 130 mAh / g Li + / Li, then decreases again, reaching 170-270 mAh / g Li + A long pseudo-plateau of 0.045 V vs Li is reached. The second oxidation is typical of the delithiation of reduced graphite LiC6, which shows a standard profile with successive potential plateaus that correlate to the four transition stages of graphite lithiation. Stage I (theoretical formula for highly lithiated graphite, LiC6) is Li + / Li is close to 0 V. Stage II is LiC 12 It has the chemical formula Li + The anode plateau at 0.11 V vs Li is the transition from LiC6 to LiC 12 Stage III corresponds to the transition to LiC 18 This is achieved by: + The anodic plateau at 0.155 V vs Li is 12 From LiC 18 Stage IV corresponds to the transition to Li + The minimum potential hysteresis is achieved after the 0.240 V anodic plateau vs. Li. The minimum potential hysteresis decreases to a value of 0.074 V, supporting a beneficial change in the electrochemical kinetics of the graphite electrode during the second cycle compared to the first cycle.
[0106] The following cycles, representing the 10th and 20th, are typical of the electrochemical lithiation / delithiation of a graphite electrode with three well-known constant potential plateaus in both cathodic (lithiation) and anodic (delithiation) modes. The minimum potential hysteresis value is 0.044 V. No clear difference is observed between the galvanostatic profiles of the 10th and 20th cycles, confirming the stable electrochemical behavior of the 3D printed graphite electrode at this test condition. Increasing the charge / discharge rate to C / 20 logically reduces the specific capacity. The expected capacity loss between the 20th cycle (C / 40 rate) and the 21st cycle (C / 20 rate) is less than 10% and is considered acceptable for such a thick graphite electrode. The capacity loss by increasing the C rate is attributed to the resistance effect, which is increased by the higher current density. Interestingly, the galvanostatic profile between the 20th and 21st cycles is almost unchanged, and all constant potential plateaus are visible. Only limited overpotentials of about 0.016 V are recorded in both reduction and oxidation, which corresponds to an increase in the minimum potential hysteresis of 0.032 V, i.e., close to 0.076 V. Upon reaching the 30th cycle, a small increase of 0.01 V in the cathodic overpotential after 200 mAh / g and a loss of 6 mAh / g specific capacity compared to the 21st cycle are observed.
[0107] Very similar observations were obtained by repeating the battery tests with other 3D printed graphite electrodes from the same production batch.
[0108] The 3D printed graphite electrode with CMC at pH = 3 as the binder can yield a reversible specific capacity close to that of graphite at 340 mAh / g, exceeding 95% of the electrode capacity when Li + It can be concluded that a working potential as low as 0.4 V vs. .mu.l / Li can be achieved.
[0109] The low specific capacity of the first cycle is due to a kind of electrode activation. Due to lithium ion intercalation between the graphene sheets, the graphite volume changes (about 10% in the c-axis when the LiC6 state is reached), which may induce different structural micro-rearrangements in the 3D printed electrode during the initial reduction / oxidation steps. It is speculated that this micro-rearrangement increases the contact area at the boundaries between the graphite particles, thus increasing the electron transmission and ultimately the electrode capacity. At the same time that these micro-arrangements occur, the SEI is formed on the surface of the graphite electrode (including the pores).
[0110] 7a, 7b, and 7c show images of an exemplary embodiment of an anode porous structure of a battery cell according to the present disclosure. SEM images of a graphite 3D printed electrode with CMC and carbon microfibers. The electrode composition is 85 / 10 / 5 graphite / CMC / fiber by weight.
[0111] To improve the mechanical properties and electronic conductivity of the 3D printed graphite electrodes, carbon microfibers (Sigrafil milled carbon fiber C M80-3.0 / 200-UN) were added to the paste formulation. The shape of the graphite electrode in Figure 7 is generally the same as in Figure 4, i.e. without carbon fibers. The size of the diameter of the fibers themselves is somewhat less regular, the latter being significantly larger (about 200 μm) at the intersections where the fibers lie below the intersections (about 170 μm). The surface of the fibers is obviously rougher in Figure 7 than in Figure 4, and the scratches on the straight surface have the same dimensions as the carbon microfibers present on the surface. These scratches are suspected to be the residues of microfibers present on the surface of the freshly printed electrodes and most likely lost during the drying process. Thus, scratches on electrodes containing microfibers are hardly avoidable. The highest magnification also confirms the presence of carbon microfibers within the printed fibers.
[0112] FIG. 8 shows a schematic of an exemplary graph. It shows the evolution of the specific capacitance and coulombic efficiency versus cycles for 3D printed electrodes of graphite with CMC and carbon microfibers. The electrode composition is graphite / fiber / CMC 85 / 5 / 10 in weight percent. The surface graphite loading is graphite / cm 2 The C rate is C / 40.
[0113] Figure 8 shows the evolution of the specific capacity and coulombic efficiency versus cycles for a 3D printed anode containing graphite / carbon microfiber / CMC in a weight ratio of 85 / 5 / 10. The presence of carbon microfibers does not affect the maximum specific capacity and coulombic efficiency values of the graphite material present in the 3D printed electrode, 332 mAh / g during discharge and 333 mAh / g during charge, and 99.6%, in comparison with Figure 5. 40 mg / cm 2 The thicker electrode, containing 5 layers, which is a better graphite loading than the previous one, shows no loss in terms of the performance of graphite as a lithium intercalation material. Thus, after 10 cycles, the electrode shows a capacity of 14 mAh / cm 2 A reversible areal capacitance (Figure 6) superior to that of the conventional graphite-based anodes is reached. Such high areal capacitance has not been described for carbon-based anodes in the known art. According to the present disclosure, the sluggish electrochemical kinetics of thick graphite-based electrodes produced by standard tape-casting "doctor blade" methods can be effectively prevented. Another parameter to take into account the advantages of our 3D printing graphite-based electrode protocol is the simpler and faster preparation process of the dispersion (paste). The mixing time of the 3D printing paste is much shorter than 2 hours and no exfoliation step under vacuum is required.
[0114] FIG. 9 shows a schematic of an exemplary graph showing the evolution of areal capacitance vs. cycles for graphite 3D printed electrodes with CMC and carbon microfibers. The electrode composition is 85 / 5 / 10 graphite / fiber / CMC in wt. %. The surface graphite loading is in graphite / cm 2 The C rate is C / 40.
[0115] FIG. 10 shows a schematic of an exemplary graph. The charge / discharge profile of a graphite 3D printed electrode with CMC and carbon microfibers is shown. The electrode composition is graphite / fiber / CMC 85 / 5 / 10 in weight percent. The surface graphite loading is graphite / cm 2 This is approximately 42.2 mg.
[0116] The LTO anode is Li + The LFP / Graphite anode has an operating voltage at about 1.5 V vs. U / Li, which is more than a volt better than that of graphite-based anodes (see Figures 6 and 10). High voltage anodes are very detrimental to the energy density of full-cell lithium-ion batteries, E (energy) = U (volts) * Q (capacity). While the operating voltage of LFP / Graphite cells exceeds 3.0 V, the operating voltage of LFP / LTO cells is in the range of 2.0 V or even lower. In addition, the LTO material presents a limited specific capacity of about 170 mAh / g, which significantly hinders the gravimetric capacity of the cell.
[0117] The galvanostatic profile of the graphite / fiber / CMC electrode is shown in Figure 10. Only the profile of the first cycle is anomalous. All galvanostatic profiles of the following cycles are typical of galvanostatic lithiation and delithiation of graphitic materials. The activation phenomenon (see above) may be present in this case, even if it is much less dramatic than in Figure 6 and is mainly limited to the first reduction step. The initial stage of the first reduction is clearly anomalous, with a Li + / There is a rapid drop to a potential of 0.085 V vs Li. The potential then increases to 57 mAh / g vs Li + / Li, then quickly decreases, and at 100 mAh / g Li + A pseudopotential plateau is reached at approximately 0.08 V vs Li / g, and finally at 190 mAh / g Li +The final constant potential plateau is reached at 0.05 V vs. / Li. Although the capacity of the reduction is the highest, the SEI formation must take into account a coulombic efficiency of 90.8%, corresponding to an irreversible capacity of 31 mAh / g. The galvanostatic profile of the first oxidation is very similar to that of the post-oxidation one, taking into account the limited reversibility. The potential hysteresis of the first cycle is about 0.066 V, only 0.01 V larger than that of the following cycles. As previously reported, the galvanostatic profiles from the second to the tenth cycles are almost the same except for a limited (even beneficial) increase in the specific capacity, thus supporting the high stability of the 3D-printed graphite electrode in these test conditions.
[0118] 11a, 11b, and 11c show images of an exemplary embodiment of the anode porous structure of a battery cell. SEM images of graphite 3D printed electrodes with CMC and PEDOT:PSS as binders are shown. The electrode composition is graphite / CMC / PEDOT:PSS 90 / 7.85 / 2.15 (wt%).
[0119] A conductive PEDOT:PSS conductive polymer was added as a binder in the formulation of the 3D printed graphite anode to increase the electronic transparency in the electrode and therefore its electrochemical properties. The shape of the graphite electrode in Figure 11 is generally the same as in Figures 4 and 7. The spacing between the fibers is not monotonic and has a limited wavy shape. Similar to Figure 11, the printed fibers show a significantly larger diameter at the intersection (about 180 μm) and fibers below the intersection (about 165 μm).
[0120] FIG. 12 shows a schematic diagram of an exemplary graph. It shows the evolution of the specific capacitance and coulombic efficiency versus cycles of graphite 3D printed electrodes with CMC and PEDOT:PSS as binders. The electrode composition is graphite / CMC / PEDOT:PSS 90 / 7.85 / 2.15 (wt%). The areal graphite loading is graphite / cm 2 This is approximately 26.6 mg.
[0121] Figure 12 highlights the positive effect of adding the conductive polymer PEDOT:PSS as a co-binder in the formulation of 3D printed graphite electrodes. In the first cycle, high specific capacities of 358 and 335 mAhg / g are obtained for charging (reduction) and discharging (oxidation). This means that since the first cycle, reversible capacity (better than 90% and 92% for theoretical and practical capacity, respectively) and high coulombic efficiency (better than 90%) are reached. The second cycle presents a reversible capacity better than 342 mAh / g (about 92% and 94% for theoretical and practical capacity, respectively) and a coulombic efficiency of 99.0%.
[0122] FIG. 13 shows a schematic of an exemplary graph. Areal capacity vs. cycles for graphite 3D printed electrodes with CMC and PEDOT:PSS as binders. Electrode composition is graphite / CMC / PEDOT:PSS 90 / 7.85 / 2.15 (wt%). Areal graphite loading is graphite / cm 2 This is approximately 26.6 mg.
[0123] The capacity remains stable for the next cycles at C / 40 and the coulombic efficiency increases until it reaches 99.7% at the 10th cycle. The corresponding areal capacity (Figure 13) is 26.6 mg / cm 2 9.0mAh / cm with graphite load 2 At a higher C rate of C / 20, it is about 310 mAh / g (about 8.24 mAh / cm 2 A limited loss of capacity of about 10% is observed to reach a value of 0.01% for the 11th cycle, with a coulombic efficiency of 99.7% observed for the 11th cycle. The capacity reaches about 306 mAh / g (about 8.14 mAh / cm) at the 16th cycle. 2 ) value and a coulombic efficiency of 99.8%.
[0124] FIG. 14 shows a schematic diagram of an exemplary graph. It shows the charge / discharge profile of a graphite 3D printed electrode with CMC and PEDOT:PSS as binder. The electrode composition is graphite / CMC / PEDOT:PSS 90 / 7.85 / 2.15 (wt%). The area graphite loading is graphite / cm 2 This is approximately 26.6 mg.
[0125] In contrast, the 3D printed graphite electrode containing the CMC / PEDOT:PSS binder presents a typical graphite electrode galvanostatic profile (Figure 14) at both C / 40 and C / 20, with four well-defined constant potential plateaus for both reduction (lithiation) and oxidation (delithiation). The minimum potential hysteresis is 0.042 and 0.064 V at C / 40 and C / 20 rates, respectively, which are clearly smaller than the potential hysteresis of other 3D printed graphite electrodes (with only CMC as binder, with or without carbon microfibers). This value should be compared with Figure 6, where the potential hysteresis is 0.044 (C / 40) and 0.076 V (C / 20). The minimum potential hysteresis at C / 40 is close for the two electrode formulations, but considering that in Figure 6 (without conductive PEDOT:PSS) it is at the 20th cycle, in Figure 14 (with conductive PEDOT:PSS) this value is reached from the second cycle onwards, with the latter load being about 30% better compared to the former. The difference in potential hysteresis at higher charge rates (C / 20) is clear and is better than 0.01 V, i.e., a reduction of more than 15% in the minimum potential hysteresis is obtained by adding PEDOT:PSS to the electrode formulation. These observations support the positive effect of using a conductive binder in the formulation to improve the electrochemical kinetics of the electrode, due to better grain boundary electrical transport. It is also suggested that the addition of other conductive additives (carbon black, hard carbon, carbon nanotubes, carbon fibers, etc.) can further beneficially increase the electronic permeability in the 3D printed electrodes.
[0126] Considering the above examples, 3D printed based carbon electrodes can have the following important advantageous features with respect to electrodes known in the art: More than 95% of the total capacity, Li + / A low operating voltage of less than 0.5 V vs. Li; 13mAh / cm 2 Even better than 6mAh / cm 2 High areal capacitance superior to the standard high capacitance of Reaching a high first coulombic efficiency, better than 90% and even better than 93%.
[0127] 15 shows a schematic diagram of a cross-sectional side view of an exemplary embodiment of a battery cell anode porous structure 10. The filaments 2 are positioned such that the pores within the structure have a wide opening 30 near one end of the porous anode structure 10 and a narrow opening 40 near the other end of the porous anode structure 10, the wide opening 30 being formed in one or more upper layers of the stack of layers.
[0128] Thus, in some instances, the size of the pores may vary across the thickness of the anode porous structure. For example, the top (free end) of the anode may be more open than the bottom (end in contact with the surface). As a result, the bottom portion of the anode has a larger contact area for electrical conductivity, and the pores in the top portion (see the free end opposite the bottom) may be more open, favoring the diffusion of liquid.
[0129] It will be understood that the carbon-based active material can be a material having mainly carbon as the active material. For example, the carbon-based material can be graphite. Using graphite can provide high capacity. However, various other materials can be used. For example, the carbon-based active material can be carbon silicon, hard carbon, or a compound thereof. For example, a compound including hard carbon and graphite can be used. Also, a compound including one or more metals can be used, for example, a compound including tin and carbon (e.g., more than 95% by weight carbon and less than 5% by weight tin).
[0130] Some embodiments may be implemented, for example, using a machine or tangible computer-readable medium or article that may store instructions or sets of instructions that, when executed by the machine, cause the machine to perform methods and / or operations in accordance with the embodiments.
[0131] Various embodiments may be implemented using hardware elements, software elements, or a combination of both. Examples of hardware elements may include a processor, a microprocessor, a circuit, an application specific integrated circuit (ASIC), a programmable logic device (PLD), a digital signal processor (DSP), a field programmable gate array (FPGA), logic gates, registers, semiconductor devices, microchips, chipsets, etc. Examples of software may include a software component, a program, an application, a computer program, an application program, a system program, a machine program, an operating system software, a mobile app, middleware, firmware, a software module, a routine, a subroutine, a function, a computer implemented method, a procedure, a software interface, an application program interface (API), a method, an instruction set, computing code, computer code, etc.
[0132] The present invention is described herein with reference to specific examples of embodiments of the invention. However, it will be apparent that various modifications, variations, substitutions, and changes can be made therein without departing from the essence of the invention. For the purpose of clarity and concise description, features are described herein as part of the same or different embodiments, however, alternative embodiments combining all or part of the features described in these different embodiments are also envisioned and are understood to be within the framework of the invention as outlined in the claims. Thus, the specification, drawings, and examples should be regarded in an illustrative, rather than a restrictive, sense. The present invention is intended to embrace all alternatives, modifications, and variations that are within the scope of the appended claims. Moreover, many of the described elements are functional entities that can be implemented as separate or distributed components, or in combination with other components, in any suitable combination and location.
[0133] In the claims, any reference signs placed between parentheses shall not be construed as limiting the scope of the claim. The word "comprising" does not exclude the presence of other features or steps than those recited in the claim. Moreover, the words "a" and "an" are used to mean "at least one" and not to be limited to "only one", but do not exclude a plurality. The mere fact that certain measures are recited in mutually different claims does not indicate that a combination of these measures cannot be used to advantage.
[0134] (Additional Note) (Appendix 1) 1. A battery cell including an anode, the anode comprising interconnected filaments of material positioned in a predetermined structural arrangement in multiple layers stacked on top of one another, the filaments positioned such that filaments of successive layers are connected to one another to form a porous anode structure with in-structural pores formed between the filaments, the material as constructed comprising a carbon-based active material configured to participate in a battery electrode reaction.
[0135] (Appendix 2) 2. The battery cell of claim 1, wherein a mesh of pores is formed in each layer.
[0136] (Appendix 3) 3. The battery cell of claim 2, wherein the interconnected filaments form a lattice structure and the pores are interconnected within the lattice structure.
[0137] (Appendix 4) 4. The battery cell of any one of claims 1 to 3, wherein the constructed material comprises at least 60 wt.%, more preferably at least 80 wt.%, and even more preferably at least 85 wt.%, of a carbon-based anode active material, based on the total weight of the constructed material.
[0138] (Appendix 5) 4. The battery cell of any one of claims 1 to 3, wherein the carbon-based active material comprises at least one of graphite, soft carbon, hard carbon, or a composite material comprising one or more of the foregoing materials.
[0139] (Appendix 6) 6. The battery cell of claim 1, wherein the porous anode structure has a thickness in the range of 0.1 to 5 millimeters, preferably in the range of 0.2 to 1 millimeters, and more preferably in the range of 0.4 to 0.7 millimeters.
[0140] (Appendix 7) 7. The battery cell of any one of claims 1 to 6, wherein the anode has at least two stacked layers, more preferably at least three stacked layers, and even more preferably at least four stacked layers.
[0141] (Appendix 8) The anode has a capacitance of at least 8 milliamp-hours / cm 2 , more preferably at least 10 milliamp-hours / cm 2 , and even more preferably at least 12 milliamp-hours / cm 2 8. The battery cell according to claim 1, having a capacity per unit surface area of 1.
[0142] (Appendix 9) 10. The battery cell of any one of claims 1-9, wherein the anode has a specific capacity per gram of anode material that is at least 80%, preferably at least 85%, and more preferably at least 90% of the theoretical specific capacity calculated from the composition of the materials from which it is constructed.
[0143] (Appendix 10) 10. The battery cell according to any one of claims 1 to 9, wherein the filaments have a diameter of 50 to 750 microns, more preferably 75 to 500 microns.
[0144] (Appendix 11) 11. The battery cell of any one of claims 1 to 10, wherein the filaments in each layer are spaced apart, and a gap distance between opposing adjacent filaments in each layer is less than a thickness of the filaments.
[0145] (Appendix 12) 12. The battery cell of any one of claims 1-11, wherein the filament has a shape such that the structural pores have a wider opening near a first end of the porous anode structure and a narrower opening near a second end of the porous anode structure, the second end being positioned opposite the first end, and the wider opening being formed in one or more upper layers of the stacked layers.
[0146] (Appendix 13) 13. The battery cell of any one of claims 1 to 12, wherein the pores in the stacked layers have a rectangular shape.
[0147] (Appendix 14) 14. A method for manufacturing a battery cell according to any one of claims 1 to 13, wherein the battery cell is provided with a three-dimensional porous anode, the anode being produced by depositing interconnected filaments of structured material in a predetermined structural arrangement in a plurality of layers stacked on top of each other, the filaments being positioned such that filaments of successive layers are connected to each other to form a porous anode structure with intrastructural pores formed between the filaments, the structured material comprising a carbon-based active material configured to participate in a battery electrode reaction.
Claims
1. 1. A battery cell including an anode, the anode comprising interconnected filaments of material positioned in a predetermined structural arrangement in multiple layers stacked on top of one another, the filaments positioned such that filaments of successive layers are connected to one another to form a porous anode structure with in-structural pores formed between the filaments, the material as constructed comprising a carbon-based active material configured to participate in a battery electrode reaction.
2. The battery cell of claim 1 , wherein a mesh of pores is formed in each layer.
3. 3. The battery cell of claim 2, wherein the interconnected filaments form a lattice structure, and the pores are interconnected within the lattice structure.
4. 4. The battery cell of claim 1, wherein the material of construction comprises at least 60 wt.%, more preferably at least 80 wt.%, and even more preferably at least 85 wt.%, of a carbon-based anode active material, based on the total weight of the material of construction.
5. The battery cell of any one of claims 1 to 3, wherein the carbon-based active material comprises at least one of graphite, soft carbon, hard carbon, or a composite material comprising one or more of the foregoing materials.
6. 6. The battery cell of claim 1, wherein the porous anode structure has a thickness in the range of 0.1 to 5 millimeters, preferably in the range of 0.2 to 1 millimeter, more preferably in the range of 0.4 to 0.7 millimeters.
7. The battery cell of any one of claims 1 to 6, wherein the anode has at least two stacked layers, more preferably at least three stacked layers, and even more preferably at least four stacked layers.
8. The anode has a current of at least 8 milliamp hours / cm 2 , more preferably at least 10 milliamp-hours / cm 2 , and even more preferably at least 12 milliamp hours / cm 2 The battery cell according to any one of claims 1 to 7, having a capacity per unit surface area of
9. 10. The battery cell of claim 1, wherein the anode has a specific capacity per gram of anode material that is at least 80%, preferably at least 85%, and more preferably at least 90% of the theoretical specific capacity calculated from the composition of the materials of construction.
10. The battery cell of any one of claims 1 to 9, wherein the filaments have a diameter of 50 to 750 microns, more preferably 75 to 500 microns.
11. 11. The battery cell of claim 1, wherein the filaments in each layer are spaced apart, the gap distance between opposing adjacent filaments in each layer being less than a thickness of the filaments.
12. 12. The battery cell of claim 1, wherein the filaments have a shape such that the structural pores have a wider opening near a first end of the porous anode structure and a narrower opening near a second end of the porous anode structure, the second end being positioned opposite the first end, and the wider openings being formed in one or more upper layers of the stacked layers.
13. The battery cell of any one of claims 1 to 12, wherein the pores in the stacked layers have a rectangular shape.
14. 14. A method for manufacturing a battery cell according to any one of claims 1 to 13, wherein the battery cell is provided with a three-dimensional porous anode, the anode being produced by depositing interconnected filaments of structured material in a predetermined structural arrangement in a plurality of layers stacked on top of each other, the filaments being positioned such that filaments of successive layers are connected to each other to form a porous anode structure with intrastructural pores formed between the filaments, the structured material comprising a carbon-based active material configured to participate in a battery electrode reaction.