Improved current collector for secondary batteries

The improved current collector with a conductive layer and copolymer binder addresses corrosion and interfacial resistance issues in lithium-ion batteries, enhancing electrochemical performance and stability.

JP2024542731AInactive Publication Date: 2024-11-15GRST INTERNATIONAL LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024532721
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-12-02
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current lithium-ion battery electrodes face issues with corrosion of current collectors due to the use of aqueous slurries, particularly when nickel-containing cathode active materials are used, and high interfacial resistance between the electrode layer and the current collector, leading to unsatisfactory electrochemical performance.

Method used

An improved current collector is introduced, comprising a substrate with a conductive layer that includes a copolymer binder material, which acts as a physical barrier to prevent corrosion and reduces interfacial resistance, using an aqueous solvent to enhance adhesion and conductivity.

Benefits of technology

The improved current collector effectively prevents corrosion and reduces interfacial resistance, resulting in enhanced electrochemical performance and stability of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024542731000001_ABST
    Figure 2024542731000001_ABST
Patent Text Reader

Abstract

The present invention discloses an improved current collector for a secondary battery comprising a substrate and a conductive layer applied to one or both sides of the substrate, the conductive layer comprising a conductive material and a binder material, the binder material comprising a copolymer. Also provided herein is an electrode for a secondary battery comprising the improved current collector and an electrode layer, the electrode layer being located on a surface of the conductive layer(s). In an electrode comprising the improved current collector of the present invention, the presence of the conductive layer inhibits corrosion of the substrate and reduces the interfacial resistance between the electrode layer and the substrate. As a result, a battery comprising an electrode made with the improved current collector disclosed herein exhibits superior electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of batteries. In particular, the present invention relates to an improved current collector in a battery electrode of a secondary battery. [Background technology]

[0002] Among various kinds of batteries, lithium-ion batteries (LIBs) have been widely used in various applications over the past decades, especially in consumer electronics, due to their excellent energy density, long cycle life, and high discharge capability. With the rapid market development of electric vehicles (EVs) and grid energy storage, LIBs with high performance and low cost currently provide one of the most promising options for large-scale energy storage devices. However, many problems still exist in the current lithium-ion battery technology, especially with respect to the electrodes of lithium-ion batteries.

[0003] Generally, lithium-ion battery electrodes are fabricated by casting an organic-based slurry onto a current collector. The slurry contains electrode active material, conductive carbon, and a binder in an organic solvent. The binder provides good electrochemical stability and binds the electrode active material together and adheres it to the current collector in the fabrication of the electrode. Polyvinylidene fluoride (PVDF) is currently one of the most commonly used binders in the commercial lithium-ion battery industry. However, PVDF requires specific handling because it is insoluble in water and only soluble in some specific organic solvents, for example N-methyl-2-pyrrolidone (NMP), which is flammable and toxic.

[0004] In order to recover the NMP vapor, an NMP recovery system needs to be installed during the drying process. This requires a large capital investment, which adds a large cost to the manufacturing process. Given the shortcomings of organic-based slurries, the present invention favors the use of aqueous slurries that utilize cheaper and more environmentally friendly solvents, such as aqueous solvents (most commonly water). These aqueous solvents are significantly safer and easier to handle than NMP, and do not require the implementation of a recovery system.

[0005] However, the use of aqueous slurries in the manufacture of lithium-ion batteries is problematic. In particular, the electrode active materials may react with water and have undesirable effects on the current collector. The complications are particularly pronounced when nickel-containing positive electrode active materials, such as lithium nickel-manganese-cobalt oxide (NMC), are used, as they react strongly with water to form a basic solution. As a result, when a positive electrode is formed by coating a current collector with an aqueous slurry containing nickel, the basicity of the slurry is likely to corrode the current collector. This problem strongly prevents the use of nickel-containing positive electrode active materials in aqueous battery manufacture, despite their high specific capacity.

[0006] There are also several other issues affecting current collectors in existing lithium-ion battery technology. A typical electrode comprises a current collector and an electrode layer located on one or both sides of the current collector, where the electrode layer contacts the current collector at an electrode layer-current collector interface. This interface acts as a source of electrical resistance for electrons moving between the electrode layer and the current collector. The interfacial resistance between the electrode layer and the current collector in a battery contributes significantly to the overall internal resistance of the battery, leading to poor electrochemical performance of the battery.

[0007] It is worth noting that the above problem is not unique to lithium-ion batteries: other types of batteries, such as sodium-ion batteries, may face similar issues.

[0008] In view of the above-mentioned problems, attempts have been made to mitigate the damage caused to the current collector or to reduce the interfacial resistance between the electrode layer and the current collector in a battery electrode.

[0009] US Patent Publication No. 20130295458A1 discloses a current collector comprising a metal foil and a layer comprising conductive particles, a binder, and an organic acid, the layer being provided on one or both sides of the metal foil. Preferably, polysaccharides and their derivatives are used as binders due to their excellent adhesion to the metal foil and high ion permeability. The organic acid acts as a crosslinker for the binder, allowing the conductive particles to adhere more firmly to the metal foil. It is believed that such a configuration can reduce the internal resistance and impedance of an electrochemical device comprising the current collector. However, a drawback of this system is the need for an additional crosslinker to promote adhesion of the conductive particles to the metal foil, and the use of a simple binder is insufficient to perform this function. When the organic acid is included in the layer as a crosslinker in contact with the metal foil in forming the current collector, it is likely to cause corrosion of the underlying metal foil over time.

[0010] It is therefore an object of the present invention to provide an improved current collector for use in a battery electrode, which is less susceptible to the above-mentioned problems of conventional current collectors and which can improve the electrochemical performance of any battery equipped with such an electrode. Summary of the Invention

[0011] The above-mentioned needs are met by various aspects and embodiments disclosed herein. In one aspect, provided herein is an improved current collector for a secondary battery, comprising a substrate and a conductive layer applied to one or both sides of the substrate, the conductive layer comprising a conductive material and a binder material, the binder material comprising a copolymer comprising a structural unit (a), the structural unit (a) being represented by the formula (1):

[0012] [ka] wherein each of R1, R2, R3, and R4 in formula (1) is independently H, hydroxyl, alkyl, or hydroxyalkyl.

[0013] In some embodiments, the copolymer further comprises a structural unit (b), the structural unit (b) being represented by formula (2):

[0014] [ka] wherein each of R5, R6, R7, and R8 in formula (2) is independently H, alkyl, acyloxy, or acyloxyalkyl.

[0015] In another aspect, provided herein is an electrode comprising an improved current collector and an electrode layer overlying the conductive layer, the electrode layer comprising an electrode active material and a binder.

[0016] The invention disclosed herein solves the above problems affecting the current collector in the battery electrode. First, the conductive layer of the improved current collector can act as a physical barrier between the substrate and the alkaline electrode active material in the electrode layer. This prevents corrosion of the substrate without compromising electrical conductivity within the electrode.

[0017] Second, the conductive material in the conductive layer of the improved current collector reduces the interfacial resistance between the electrode layer and the improved current collector itself, improving the power performance of the electrode.

[0018] Furthermore, when the conductive layer of the improved current collector is applied with an aqueous electrode slurry to form an electrode, there is a risk that the conductive layer will dissolve back into the electrode slurry and become fluid. This can result in delamination of the conductive layer. The binder material in the conductive layer of the improved current collector disclosed herein has excellent adhesion to the substrate, thereby enhancing the mechanical strength of the electrode and preventing such delamination of the conductive layer.

[0019] As a result of the above-mentioned advantages, batteries containing electrodes fabricated with the improved current collectors of the present invention exhibit superior electrochemical performance. [Brief description of the drawings]

[0020] [Figure 1a]1a and 1b show simplified diagrams of two different embodiments of improved current collectors in electrodes as disclosed herein. [Figure 1b] 1a and 1b show simplified diagrams of two different embodiments of improved current collectors in electrodes as disclosed herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] In one embodiment, provided herein is an improved current collector in an electrode for a battery, the improved current collector comprising a substrate and a conductive layer located on one or both sides of the substrate. The conductive layer itself comprises a binder material and a conductive material, the binder material comprising a suitable copolymer. The conductive layer can be produced by coating a conductive slurry onto the substrate, the conductive slurry comprising a conductive material, a binder material, and an aqueous solvent. In another embodiment, provided herein is an electrode comprising an improved current collector and an electrode layer located on the improved current collector, the electrode layer comprising an electrode active material and a binder, and may further comprise a conductive agent. The electrode layer can be produced by coating an improved current collector of the present invention with an electrode slurry, the electrode slurry comprising an electrode active material, a binder, and an aqueous solvent (and optionally a conductive agent).

[0022] The term "electrode" refers to either a "positive electrode" or a "negative electrode."

[0023] The term "electrode component" refers to any material present in the electrode layer of an electrode, including but not limited to electrode active materials, conductive agents, and binders.

[0024] The term "cathode" is used interchangeably with positive electrode. Similarly, the term "negative electrode" is used interchangeably with negative electrode.

[0025] The terms "binder", "binder material", or "binding agent" refer to a chemical compound, mixture of compounds, or polymer used to hold a material(s) in place and attach it to a surface. In some embodiments, the binder material refers to a chemical compound, mixture of compounds, or polymer used to hold a conductive material in place and attach it to a substrate to form an improved current collector. In some embodiments, the binder refers to a chemical compound, mixture of compounds, or polymer used to hold an electrode material and / or a conductive agent in place and attach it to an improved current collector to form an electrode. In some embodiments, the electrode does not include a conductive material or a conductive agent. In some embodiments, the binder material and the binding agent each independently form a colloid in an aqueous solvent, e.g., water. In some embodiments, the binder material and the binding agent each independently form a solution or dispersion in an aqueous solvent, e.g., water.

[0026] The term "conductive material" or "conductive agent" refers to a material that has good electrical conductivity. Thus, conductive materials are often added during the manufacture of improved current collectors to enhance electrical conductivity. In some embodiments, conductive agents are mixed with the electrode active material during the formation of the electrode to enhance the electrical conductivity of the electrode. In some embodiments, each of the conductive material and conductive agent is independently chemically active. In some embodiments, each of the conductive material and conductive agent is independently chemically inactive.

[0027] The term "polymer" refers to a compound prepared by polymerizing monomers, whether of the same or different types. The general term "polymer" includes a "homopolymer" or a "copolymer."

[0028] The term "homopolymer" refers to a polymer prepared by polymerization of monomers of the same type.

[0029] The term "copolymer" refers to a polymer prepared by the polymerization of two or more different types of monomers.

[0030] The term "aqueous solvent" refers to a solution that contains water as a major component and that contains one or more minor components in addition to water, or a solution that consists solely of water.

[0031] With respect to a slurry, the term "aqueous" means that the solvent of the slurry is an aqueous solvent. With respect to the mode of manufacture of an electrode or battery, the term "aqueous" means that at least one element of the electrode or battery is formed in whole or in part using an aqueous slurry.

[0032] The term "unsaturated" refers to a moiety having one or more units of unsaturation.

[0033] The term "alkyl" or "alkyl group" refers to a group of the general formula C obtained by removing a hydrogen atom from a saturated, unbranched, or branched aliphatic hydrocarbon. n H 2n+1 where n is an integer.

[0034] The term "cycloalkyl" or "cycloalkyl group" refers to a saturated or unsaturated cyclic non-aromatic hydrocarbon radical having a single ring or multiple condensed rings. Examples of cycloalkyl groups include, but are not limited to, C3-C7 cycloalkyl groups, such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and cycloheptyl, and saturated cyclic and bicyclic terpenes, and C3-C7 cycloalkenyl groups, such as cyclopropenyl, cyclobutenyl, cyclopentenyl, cyclohexenyl, and cycloheptenyl, and unsaturated cyclic and bicyclic terpenes. Cycloalkyl groups can be unsubstituted or substituted with one or two suitable substituents. Furthermore, cycloalkyl groups can be monocyclic or polycyclic. In some embodiments, cycloalkyl groups contain at least 5, 6, 7, 8, 9, or 10 carbon atoms.

[0035] The term "alkenyl" refers to a monovalent group obtained by removing a hydrogen atom from any carbon atom of an unsaturated aliphatic hydrocarbon having at least one carbon-carbon double bond. Similarly, the term "alkynyl" refers to a monovalent group obtained by removing a hydrogen atom from any carbon atom of an unsaturated aliphatic hydrocarbon having at least one carbon-carbon triple bond. Furthermore, the term "enynyl" refers to a monovalent group obtained by removing a hydrogen atom from any carbon atom of an unsaturated aliphatic hydrocarbon having at least one carbon-carbon double bond and at least one carbon-carbon triple bond. The alkenyl, alkynyl, or enynyl unsaturated aliphatic hydrocarbon may be branched or unbranched.

[0036] The term "alkoxy" refers to an alkyl group, as defined above, attached to the main carbon chain through an oxygen atom. Some non-limiting examples of alkoxy groups include methoxy, ethoxy, propoxy, butoxy, and the like. Alkoxy, as defined above, can be substituted or unsubstituted, and the substituents can be, but are not limited to, deuterium, hydroxy, amino, halo, cyano, alkoxy, alkyl, alkenyl, alkynyl, mercapto, nitro, and the like.

[0037] The term "alkylene" refers to a saturated divalent hydrocarbon group obtained by removing two hydrogen atoms from a branched or unbranched saturated hydrocarbon. Examples of alkylene groups include methylene (-CH-), ethylene (-CHCH-), isopropylene (-CH(CH)CH-), and the like. Alkylene groups are optionally substituted with one or more substituents described herein.

[0038] The term "aryl" or "aryl group" refers to an organic radical obtained by removing a hydrogen atom from a monocyclic or polycyclic aromatic hydrocarbon. Non-limiting examples of aryl groups include phenyl, naphthyl, benzyl, tolanyl, sexiphenyl, phenanthrenyl, anthracenyl, coronenyl, and tolanylphenyl. An aryl group can be unsubstituted or substituted with one or more suitable substituents. Furthermore, an aryl group can be monocyclic or polycyclic. In some embodiments, an aryl group contains at least 6, 7, 8, 9, or 10 carbon atoms.

[0039] The term "alkylamino" refers to a group obtained by removing a hydrogen atom from a primary or secondary amine. Alkylamino encompasses the terms "N-alkylamino" and "N,N-dialkylamino," in which the amino group is independently substituted with one or two alkyl groups, respectively. The alkylamino group is optionally substituted with one or more substituents described herein.

[0040] The term "alkylthio" refers to a group containing a branched or unbranched alkyl group attached to a divalent sulfur atom. Some non-limiting examples of alkylthio groups include methylthio (CH3S-). Alkylthio groups are optionally substituted with one or more substituents described herein.

[0041] The term "heteroatom" refers to one or more of oxygen (O), sulfur (S), nitrogen (N), phosphorus (P), or silicon (Si), and includes any oxidized form of nitrogen (N), sulfur (S), or phosphorus (P), the quaternized form of any basic nitrogen, or a substitutable heterocyclic nitrogen, such as N (in 3,4-dihydro-2H-pyrrolyl), NH (in pyrrolidinyl), or NR (in N-substituted pyrrolidinyl).

[0042] The term "carbonyl" refers to -(C=O)-.

[0043] The term "acyl" refers to -(C=O)-Z, where Z is alkyl.

[0044] The term "acyloxy" refers to -O-(C=O)-Z, where Z is alkyl.

[0045] The term "acyloxyalkyl" refers to -YO-(C=O)-Z, where Z is alkyl and Y is alkylene.

[0046] The term "hydroxyalkyl" refers to -YOH, where Y is an alkylene. Thus, a hydroxyalkyl consists of a hydroxyl bonded to an alkylene.

[0047] The term "amide" refers to -NH(C=O)-R.

[0048] The term "aliphatic" refers to a non-aromatic hydrocarbon or a group derived therefrom. Some non-limiting examples of aliphatic compounds include alkanes, alkenes, alkynes, alkyl groups, alkenyl groups, alkynyl groups, alkylene groups, alkenylene groups, or alkynylene groups. In some embodiments, the term "aliphatic" refers to a C1-C 30 Alkyl groups, C2-C 30 Alkenyl groups, C2-C 30 Alkynyl groups, C1-C 30 Alkylene group, C2-C 30 Alkenylene group, or C2-C 30 It refers to an alkynylene group. In some embodiments, the alkyl group contains at least 2, 3, 4, 5, 6, 7, or 8 carbon atoms.

[0049] The term "aromatic" refers to a group comprising an aromatic hydrocarbon ring, optionally containing heteroatoms or substituents. Examples of such groups include, but are not limited to, phenyl, tolyl, biphenyl, o-terphenyl, m-terphenyl, p-terphenyl, naphthyl, anthryl, phenanthryl, pyrenyl, triphenylenyl, and derivatives thereof.

[0050] The term "substituted" is used to describe a compound or chemical moiety in which at least one hydrogen atom of the compound or chemical moiety has been replaced with a second chemical moiety. Examples of substituents are halogen, alkyl, heteroalkyl, alkenyl, alkynyl, enynyl, aryl, heteroaryl, hydroxyl, alkoxyl, amino, nitro, thiol, alkylthio, imine, cyano, amido, phosphonato, phosphinato, carboxyl, thiocarbonyl, sulfonyl, sulfonamido, acyl, formyl, acyloxy, alkoxycarbonyl, oxo, haloalkyl (e.g., trifluoromethyl), carbocyclic cycloalkyl (e.g., cyclopropyl, cyclobutyl, cyclopentyl, or cyclohexyl) which may be monocyclic or fused or non-fused polycyclic or heterocycloalkyl (e.g., pyrrolidinyl, piperidinyl, morpholinyl, or thiazinyl) which may be monocyclic or fused or non-fused polycyclic, carbocyclic or heterocyclic aryl (e.g., phenyl, naphthyl, pyrrolyl, indolyl, furanyl, thiophenyl, , imidazolyl, oxazolyl, isoxazolyl, thiazolyl, triazolyl, tetrazolyl, pyrazolyl, pyridinyl, quinolinyl, isoquinolinyl, acridinyl, pyrazinyl, pyridazinyl, pyrimidinyl, benzimidazolyl, benzothiophenyl, or benzofuranyl), amino, monoalkylamino, and dialkylamino, o-lower alkyl, o-aryl, aryl, aryl-lower alkyl, -CO2CH3, -CONH2, -OCH2 These include, but are not limited to, CONH2, -NH2, -SON2NH2, -OCHF2, -CF3, -OCF3, -NH(alkyl), -N(alkyl)2, -NH(aryl), -N(alkyl)(aryl), -N(aryl)2, -CHO, -CO(alkyl), -CO(aryl), -CO2(alkyl), and -CO2(aryl), and such moieties may be optionally substituted with fused ring structures or bridges, such as, for example, -OCHO-. These substituents may be optionally further substituted with a substituent selected from such groups. All chemical groups disclosed herein may be substituted unless otherwise specified.

[0051] The term "linear" refers to an organic compound or moiety that does not include side chains or cyclic structures, i.e., the carbon atoms of the organic compound or moiety all form a single linear arrangement. Linear compounds or moieties may be substituted or unsubstituted, saturated or unsaturated.

[0052] The term “halogen” or “halo” refers to F, Cl, Br, or I.

[0053] The term "monomer unit" refers to a building block for a polymer structure that is derived from a single monomer.

[0054] The term "structural unit" refers to the total monomer units derived from the same monomer type within a polymer.

[0055] The term "homogenizer" refers to a device that can be used to homogenize materials, i.e., to disperse materials evenly throughout a fluid. Where homogenization is disclosed herein, any conventional homogenizer can be used in the homogenization process. Some non-limiting examples of homogenizers include agitator mixers, planetary agitator mixers, blenders, and sonicators.

[0056] The term "planetary mixer" refers to a device that can be used to mix or stir different materials to produce a homogenous mixture, comprising a vessel and blades that perform planetary motion within the vessel. In some embodiments, the planetary mixer comprises at least one planetary blade and at least one high-speed dispersion blade. The planetary blade and the high-speed dispersion blade rotate on their respective axes and rotate continuously around the vessel. The rotational speed can be expressed in revolutions per minute (rpm), which refers to the number of revolutions the rotor completes in one minute.

[0057] The term "sonicator" refers to a device capable of applying ultrasonic energy to agitate particles within a sample. Some non-limiting examples of sonicators include ultrasonic baths, probe sonicators, and ultrasonic flow cells.

[0058] The term "apply" refers to the act of laying or spreading a substance onto a surface.

[0059] The term "current collector" refers to a conductive substrate capable of conducting electrical current to an electrode during discharge or charging of a secondary battery. Some non-limiting examples of current collectors include a single metal layer or substrate, and a single metal layer or substrate overlaid with a conductive layer, such as a carbon black-based conductive layer. In some embodiments, the current collector may be in contact with the electrode layer.

[0060] The term "modified current collector" refers to a substrate having a conductive layer applied to one or both sides of the substrate.

[0061] The term "electrode layer" refers to a layer that includes an electrochemically active material. In some embodiments, the electrode layer is in contact with a current collector, an improved current collector, or a substrate. In some embodiments, the electrode layer is made by applying a coating to a current collector, an improved current collector, or a substrate and drying the coating. In some embodiments, the electrode layer is located on a surface of the current collector or improved current collector. In other embodiments, a three-dimensional porous current collector or improved current collector is conformally coated with the electrode layer.

[0062] The term "doctor blading" refers to a process for producing large area films on rigid or flexible substrates. The coating thickness can be controlled by an adjustable gap width between the coating blade and the coating surface, which allows the deposition of variable wet layer thicknesses.

[0063] The term "room temperature" refers to an indoor temperature of about 18° C. to about 30° C., e.g., 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30° C. In some embodiments, room temperature refers to a temperature of about 20° C. + / - 1° C. or + / - 2° C. or + / - 3° C. In other embodiments, room temperature refers to a temperature of about 22° C. to about 25° C.

[0064] The term "solids" refers to the amount of non-volatile material remaining after evaporation.

[0065] The term "peel strength" refers to the amount of force required to separate two materials that are adhered to one another, such as a current collector and an electrode layer. It is a measure of the bond strength between such two materials and is usually expressed in N / cm.

[0066] The term "adhesive strength" refers to the amount of force required to separate a substrate and a binder material that is adhered to the substrate. It is a measure of the strength of adhesion between two such materials and is usually expressed in N / cm.

[0067] The term "C-rate" refers to the charge or discharge rate of a cell or battery, expressed in units of total storage capacity, Ah or mAh. For example, a rate of 1C means that all of the stored energy is utilized in 1 hour, 0.1C means that 10% of the energy is utilized in 1 hour or the entire energy is utilized in 10 hours, and 5C means that the entire energy is utilized in 12 minutes.

[0068] The term "ampere-hour (Ah)" refers to the unit used to specify the storage capacity of a battery. For example, a battery with a capacity of 1 Ah can supply 1 ampere of current for 1 hour or 0.5 A for 2 hours. Thus, 1 ampere-hour (Ah) is equivalent to 3,600 coulombs of charge. Similarly, the term "milliampere-hour (mAh)" also refers to the unit of storage capacity of a battery and is 1 / 1,000 of an ampere-hour.

[0069] The term "battery cycle life" refers to the number of complete charge / discharge cycles a battery can undergo before the nominal capacity of the battery drops to less than 80% of its initial rated capacity.

[0070] The term "capacity" is a property of an electrochemical cell that refers to the total amount of charge that the electrochemical cell, e.g., a battery, can hold. Capacity is usually expressed in ampere-hours. The term "specific capacity" refers to the capacity output per unit weight of an electrochemical cell, e.g., a battery, and is usually expressed in Ah / kg or mAh / g.

[0071] In the following description, all numerical values ​​disclosed herein are approximate, regardless of whether the word "about" or "approximately" is used in connection therewith. They may vary by 1 percent, 2 percent, 5 percent, or in some cases by 10 to 20 percent. L and upper limit R U Whenever a numerical range having a value R = R is disclosed, any number falling within that range is specifically disclosed. L +k * (R U -R L ) is expressly disclosed, where k is a variable ranging from 0 percent to 100 percent. Additionally, any numerical range defined by two R numbers as defined above is also expressly disclosed.

[0072] As used herein, all references to the singular include references to the plural and vice versa. As used herein, where the context permits, references to "aqueous solvents" may also refer specifically to water.

[0073] A battery electrode generally comprises a current collector and an electrode layer located on one or both sides of the current collector. Typically, the electrode is prepared by dispersing an electrode active material and a binder in a solvent to form an electrode slurry, and then coating the electrode slurry on a current collector and drying to form an electrode layer. The electrode slurry (and the resulting electrode layer) may further comprise conductive carbon. Regardless of the components present in the electrode layer, discontinuities between the electrode layer and the current collector of the electrode mean that there is a large interfacial resistance between the electrode layer and the current collector. Batteries comprising such electrodes will have less than optimal electrochemical performance as a result of such interfacial resistance.

[0074] Among batteries, lithium-ion batteries are one of the most widely studied and used. A typical electrode slurry composition for lithium-ion batteries includes PVDF as a binder and NMP as a solvent, but the use of NMP presents significant environmental, health, and safety risks in addition to additional costs associated with the recovery system. Therefore, aqueous electrode slurries, including aqueous solvents such as water, have been proposed as an alternative. Lithium-ion batteries with electrodes manufactured using such electrode slurries have reduced environmental, health, and safety risks.

[0075] However, positive electrodes fabricated using aqueous slurries containing nickel-containing positive electrode active materials, such as NMC, are particularly susceptible to current collector corrosion due to the high basicity of such slurries.

[0076] To solve the above problems, the inventors of the present invention propose the use of a novel improved current collector comprising a substrate and a conductive layer located on one or both sides of the substrate. In battery electrodes, the conductive layer of the improved current collector disclosed herein helps to mitigate the corrosion tendency of the substrate by reducing the interfacial resistance between the electrode layer and the improved current collector and acting as a physical barrier between the substrate and the electrode layer. The conductive layer of the present invention also has the advantage that it does not revert to a fluid when an aqueous electrode slurry is applied over the conductive layer.

[0077] The improved current collector described herein refers to a substrate having a conductive layer applied to one or both sides of the substrate, the conductive layer comprising a conductive material and a binder material. Figure 1a shows a simplified diagram of an embodiment of an improved current collector of the present invention, designated 10, in an electrode 100. The improved current collector 10 comprises a substrate 101 having a conductive layer 102 applied to one side of the substrate 101. In the manufacture of a battery electrode, an electrode layer 20 may be located on the surface of the conductive layer 102.

[0078] 1b shows a simplified diagram of another embodiment of an improved current collector of the present invention, designated 11, for an electrode 110. The improved current collector 11 comprises a substrate 111 having conductive layers 112a and 112b applied to both sides of the substrate 111. In the manufacturing process of a battery electrode, electrode layers 21a and 21b may be applied to the surfaces of the conductive layers 112a and 112b, respectively.

[0079] When applied to a battery system, the substrate in the improved current collector of the present invention functions, inter alia, to collect electrons produced by the electrochemical reaction of the positive electrode active material or to supply electrons required for the electrochemical reaction.

[0080] In some embodiments, the substrate may be in the form of a foil, sheet, film, or a porous body with a three-dimensional network structure. In some embodiments, the substrate may be made of a polymer or metal material or a metallized polymer. In some embodiments, the substrate is coated with a conformal carbon layer. In some embodiments, the substrate is made of a single material. In other embodiments, the substrate is made of multiple materials.

[0081] In some embodiments, the substrate is a metal. In some embodiments, the substrate has a single-layer structure. In some embodiments, the substrate is selected from the group consisting of stainless steel, titanium, nickel, aluminum, copper, platinum, gold, silver, chromium, zirconium, tungsten, molybdenum, silicon, tin, vanadium, zinc, cadmium, alloys thereof, conductive resins, and combinations thereof.

[0082] In certain embodiments, the substrate has a two-layer structure with an outer layer and an inner layer, the outer layer containing a conductive additive and the inner layer containing an insulating material or another conductive additive, such as aluminum with a conductive resin layer or a polymer insulating material coated with an aluminum layer. In some embodiments, the conductive additive is selected from the group consisting of stainless steel, titanium, nickel, aluminum, copper, platinum, gold, silver, chromium, zirconium, tungsten, molybdenum, silicon, tin, vanadium, zinc, cadmium, alloys thereof, conductive resins, and combinations thereof.

[0083] In some embodiments, the substrate has a three-layer structure with an outer layer, a middle layer, and an inner layer, the outer layer and the inner layer containing a conductive additive, and the middle layer containing an insulating material or another conductive additive, such as a plastic coated with a metal film on both sides. In certain embodiments, each of the outer layer, the middle layer, and the inner layer is independently selected from the group consisting of stainless steel, titanium, nickel, aluminum, copper, platinum, gold, silver, chromium, zirconium, tungsten, molybdenum, silicon, tin, vanadium, zinc, cadmium, alloys thereof, conductive resins, and combinations thereof.

[0084] In some embodiments, the insulating material is a polymeric material selected from the group consisting of polycarbonate, polyacrylate, polyacrylonitrile, polyester, polyamide, polystyrene, polyurethane, polyepoxy, poly(acrylonitrile butadiene styrene), polyimide, polyolefin, polyethylene, polypropylene, polyphenylene sulfide, poly(vinyl ester), polyvinyl chloride, polyether, polyphenylene oxide, cellulose polymers, and combinations thereof. In certain embodiments, the substrate has more than three layers.

[0085] In some embodiments, the conductive layer comprises a conductive material and a binder material, hi certain embodiments, the conductive layer further comprises a surfactant or dispersant.

[0086] In battery electrodes comprising the improved current collector and electrode layer of the present invention, the conductive material in the conductive layer of the improved current collector provides a conductive path for electrons to travel between the electrode layer and the substrate of the improved current collector, thereby significantly reducing the interfacial resistance between the electrode layer and the improved current collector, i.e., the electrode layer-improved current collector interface.

[0087] In some embodiments, the conductive material in the conductive layer is selected from the group consisting of natural graphite particulate, synthetic graphite particulate, hard carbon, soft carbon, mesocarbon microbeads (MCMB), carbon black, graphite, expanded graphite, graphene, graphene nanoplatelets, carbon fibers, carbon nanofibers, graphitized carbon flakes, carbon tubes, carbon nanotubes, activated carbon, Super P, KS6, vapor grown carbon fiber (VGCF), mesoporous carbon, and combinations thereof.

[0088] In battery electrodes comprising the improved current collectors and electrode layers of the present invention, the binder material in the conductive layer of the improved current collector provides adhesion of the components in the conductive layer to each other and to the substrate.

[0089] In some embodiments, the binder material in the conductive layer comprises a copolymer. In some embodiments, the copolymer comprises structural unit (a) and structural unit (b). In some embodiments, structural unit (a) constitutes a hydrophilic portion of the copolymer. In some embodiments, structural unit (b) constitutes a hydrophobic portion of the copolymer.

[0090] In some embodiments, the structural unit (a) in the copolymer of the binder material is represented by the formula (1):

[0091] [ka] The monomer unit (s) may include one or more monomer units having the formula:

[0092] In some embodiments, R1, R2, R3, and R4 in formula (1) are independently H, hydroxyl, alkyl, hydroxyalkyl, halogen, or halogenated alkyl. In certain embodiments, at least one of R1, R2, R3, and R4 is hydroxyl or hydroxyalkyl. In some embodiments, at least two of R1, R2, R3, and R4 are the same. In other embodiments, each of R1, R2, R3, and R4 is different from each other.

[0093] In some embodiments, the alkyl group has the general formula C n H 2n+1 and n is an integer from 1 to 40, 1 to 20, or 1 to 8. In some embodiments, the alkyl group has a C1 to C 40 Alkyl groups, C1-C 30 Alkyl groups, C1-C 20 Alkyl groups, C1-C 10 Alkyl groups, C5-C 40 Alkyl groups, C5-C 30 Alkyl groups, C5-C 20 Alkyl groups, C5-C 10 Alkyl group, C 10 ~C 40 Alkyl group, C 10 ~C 30 Alkyl groups, and C 10 ~C 20 The alkyl group may be selected from the group consisting of alkyl groups.

[0094] Examples of alkyl groups include, but are not limited to, C1-C8 alkyl groups, such as, for example, methyl, ethyl, propyl, isopropyl, 2-methyl-1-propyl, 2-methyl-2-propyl, 2-methyl-1-butyl, 3-methyl-1-butyl, 2-methyl-3-butyl, 2,2-dimethyl-1-propyl, 2-methyl-1-pentyl, 3-methyl-1-pentyl, 4-methyl-1-pentyl, 2-methyl-2-pentyl, 3-methyl-2-pentyl, 4-methyl-2-pentyl, 2,2-dimethyl-1-butyl, 3,3-dimethyl-1-butyl, 2-ethyl-1-butyl, butyl, isobutyl, t-butyl, pentyl, isopentyl, neopentyl, hexyl, heptyl, and octyl. Longer alkyl groups include nonyl and decyl groups. The alkyl groups can be unsubstituted or substituted with one or more suitable substituents. Additionally, the alkyl groups can be branched or unbranched. In some embodiments, an alkyl group contains at least 2, 3, 4, 5, 6, 7, or 8 carbon atoms.

[0095] In some embodiments, the hydroxyalkyl group is a C-C 40 Hydroxyalkyl groups, C1-C 30 Hydroxyalkyl groups, C1-C 20 Hydroxyalkyl groups, C1-C 10 Hydroxyalkyl groups, C5-C 40 Hydroxyalkyl groups, C5-C 30 Hydroxyalkyl groups, C5-C 20 Hydroxyalkyl groups, C5-C 10 Hydroxyalkyl group, C 10 ~C 40 Hydroxyalkyl group, C 10 ~C 30 Hydroxyalkyl group, C 10 ~C 20 The alkyl group may be selected from the group consisting of hydroxyalkyl groups.

[0096] Examples of hydroxyalkyl groups include, but are not limited to, hydroxymethyl, hydroxyethyl, hydroxypropyl, hydroxymethylpropyl, hydroxybutyl, and hydroxymethylbutyl, hydroxydimethylpropyl, hydroxymethylpentyl, hydroxydimethylbutyl, hydroxyethylbutyl, hydroxypentyl, hydroxyneopentyl, hydroxyneopentyl, hydroxyhexyl, hydroxyheptyl, and hydroxyoctyl. The alkyl group within the hydroxyalkyl group may be branched or unbranched.

[0097] In some embodiments, the halogen may be selected from the group consisting of fluorine, chlorine, bromine, iodine, astatine, and combinations thereof.

[0098] Some non-limiting examples of alkyl halides include methyl fluoride, methyl chloride, methyl bromide, methyl iodide, methyl astatide, ethyl fluoride, ethyl chloride, ethyl bromide, ethyl iodide, ethyl astatide, propyl fluoride, propyl chloride, propyl bromide, propyl iodide, and propyl astatide.

[0099] In general, the structural unit (a) is hydrophilic. Therefore, each of R1, R2, R3, and R4 of formula (1) in the monomer unit(s) in the structural unit (a) does not independently contain a long hydrocarbon chain. The presence of a long hydrocarbon chain(s) in the monomer unit(s) of the structural unit (a) causes the structural unit (a) to lose its hydrophilicity in the copolymer. This can affect the overall dispersion of the binder material during the manufacture of the conductive layer, and therefore affect the homogeneity. This not only leads to inconsistent adhesion across the substrate-conductive layer interface, but also the conductive network developed to facilitate the transfer of electrons between the electrode layer and the substrate can be significantly weakened, increasing the interfacial resistance between the electrode layer and the improved current collector. In some embodiments, the alkyl group and the hydroxyalkyl group are C1-C8 alkyl groups and C1-C8 hydroxyalkyl groups, respectively.

[0100] Conversely, it is undesirable that each of R1, R2, R3, and R4 of formula (1) in the monomer unit(s) in structural unit (a) is independently hydroxyl or hydroxyalkyl. Structural unit (a) containing an excessive amount of hydroxyl or hydroxyalkyl may result in excessive hydrogen bonding interactions between hydroxyl and / or hydroxyalkyl groups, both within the copolymer chain and between different copolymer chains. As a result, during the manufacture of the conductive layer, aggregation and poor dispersion of the binder material and other material(s) (e.g., conductive material) in the conductive slurry produced is induced. In some embodiments, no more than three of R1, R2, R3, and R4 of formula (1) are hydroxyl or hydroxyalkyl. In certain embodiments, no more than two of R1, R2, R3, and R4 of formula (1) are hydroxyl or hydroxyalkyl. In certain embodiments, only one of R1, R2, R3, and R4 of formula (1) is hydroxyl or hydroxyalkyl. In other embodiments, only one of R1, R2, R3, and R4 of formula (1) is hydroxyl. In certain embodiments, only one of R1, R2, R3, and R4 of formula (1) is hydroxyl, and the remaining three of R1, R2, R3, and R4 of formula (1) are independently alkyl or H. In further embodiments, only one of R1, R2, R3, and R4 of formula (1) is hydroxyl, and the remaining three of R1, R2, R3, and R4 of formula (1) are independently H.

[0101] In some embodiments, the structural unit (b) in the copolymer of the binder material is represented by formula (2):

[0102] [ka] The monomer unit (s) may include one or more monomer units having the formula:

[0103] In some embodiments, each of R5, R6, R7, and R8 in formula (2) is independently H, alkyl, acyloxy, acyloxyalkyl, halogen, or halogenated alkyl. In certain embodiments, at least one of R5, R6, R7, and R8 is acyloxy or acyloxyalkyl. In some embodiments, at least two of R5, R6, R7, and R8 are the same. In other embodiments, each of R5, R6, R7, and R8 is different from each other.

[0104] An acyloxy group has the structure -O-(C=O)-Z, where Z is an alkyl group.

[0105] An acyloxyalkyl group has the structure -YO-(C=O)-Z, where Y is an alkylene group and Z is an alkyl group.

[0106] In some embodiments, the alkyl group (Z) in each of the acyloxy group or acyloxyalkyl group is independently C1 to C 40 Alkyl groups, C1-C 30 Alkyl groups, C1-C 20 Alkyl groups, C1-C 10 Alkyl groups, C5-C 40 Alkyl groups, C5-C 30 Alkyl groups, C5-C 20 Alkyl groups, C5-C 10 Alkyl group, C 10 ~C 40 Alkyl group, C 10 ~C 30 Alkyl group, C 10 ~C 20 The alkyl group may be selected from the group consisting of alkyl groups.

[0107] Examples of alkyl groups in each of the acyloxy or acyloxyalkyl groups include, but are not limited to, C1-C8 alkyl groups, such as, for example, methyl, ethyl, propyl, isopropyl, 2-methyl-1-propyl, 2-methyl-2-propyl, 2-methyl-1-butyl, 3-methyl-1-butyl, 2-methyl-3-butyl, 2,2-dimethyl-1-propyl, 2-methyl-1-pentyl, 3-methyl-1-pentyl, 4-methyl-1-pentyl, 2-methyl-2-pentyl, 3-methyl-2-pentyl, 4-methyl-2-pentyl, 2,2-dimethyl-1-butyl, 3,3-dimethyl-1-butyl, 2-ethyl-1-butyl, butyl, isobutyl, t-butyl, pentyl, isopentyl, neopentyl, hexyl, heptyl, and octyl. Longer alkyl groups include nonyl and decyl groups. The alkyl groups can be unsubstituted or substituted with one or more suitable substituents. Additionally, the alkyl group may be branched or unbranched, hi some embodiments, the alkyl group comprises at least 2, 3, 4, 5, 6, 7, or 8 carbon atoms.

[0108] In some embodiments, the alkylene groups (Y) in the acyloxyalkyl group are independently C1 to C 40 Alkylene group, C1-C 30 Alkylene group, C1-C 20 Alkylene group, C1-C 10 Alkylene group, C5-C 40 Alkylene group, C5-C 30 Alkylene group, C5-C 20 Alkylene group, C5-C 10 Alkylene group, C 10 ~C 40 Alkylene group, C 10 ~C 30 Alkylene group, C 10 ~C 20The acyloxyalkyl group may be selected from the group consisting of alkylene groups. The alkylene group in the acyloxyalkyl group may be branched or unbranched. Examples of alkylene groups in the acyloxyalkyl group include, but are not limited to, methylene, ethylene, propylene, butylene, pentylene, hexylene, heptylene, octylene, nonylene, decylene, undecylene, dodecylene, tridecylene, tetradecylene, pentadecylene, hexadecylene, heptadecylene, octadecylene, nonadecylene, icosylene, and stereoisomers thereof. Some non-limiting examples of acyloxyalkyl groups include acyloxymethyl, acyloxyethyl, acyloxypropyl, acyloxy(methyl)propyl, and acyloxy(methyl)butyl.

[0109] Despite the hydrophobicity of the structural unit (b), it is undesirable that each of R5, R6, R7, and R8 of formula (2) in the monomer unit(s) in the structural unit (b) independently comprises a long hydrocarbon chain. Excessively long hydrocarbon chains in the monomer unit(s) in the structural unit (b) may cause insufficient interaction between the structural unit (b) and the aqueous solvent (e.g., water) in the conductive slurry, promoting aggregation of the entire copolymer chain. Also, winding motion between different copolymer chains may occur, forming small globular structures. As a result, the binder material produced therefrom and other materials in the conductive slurry may not be properly dispersed. In some embodiments, no more than three of R5, R6, R7, and R8 of formula (2) are alkyl, acyloxy, or acyloxyalkyl. In certain embodiments, no more than two of R5, R6, R7, and R8 of formula (2) are alkyl, acyloxy, or acyloxyalkyl. In certain embodiments, only one of R5, R6, R7, and R8 of formula (2) is acyloxy or acyloxyalkyl. In other embodiments, only one of R5, R6, R7, and R8 of formula (2) is acyloxy. In certain embodiments, only one of R5, R6, R7, and R8 of formula (2) is acetoxy, and the remaining three of R5, R6, R7, and R8 of formula (2) are independently alkyl or H. In further embodiments, only one of R5, R6, R7, and R8 of formula (2) is acetoxy, and the remaining three of R5, R6, R7, and R8 of formula (2) are independently H.

[0110] In some embodiments, the proportion of structural units (a) in the copolymerization of the binder material is from about 90 mol % to about 100 mol %, from about 91 mol % to about 100 mol %, from about 92 mol % to about 100 mol %, from about 93 mol % to about 100 mol %, from about 94 mol % to about 100 mol %, from about 95 mol % to about 100 mol %, from about 96 mol % to about 100 mol %, from about 97 mol % to about 100 mol %, from about 98 mol % to about 100 mol %, from about 99 mol % to about 100 mol %, from ... %, about 90 mol% to about 99.8 mol%, about 91 mol% to about 99.8 mol%, about 92 mol% to about 99.8 mol%, about 93 mol% to about 99.8 mol%, about 94 mol% to about 99.8 mol%, about 95 mol% to about 99.8 mol%, about 96 mol% to about 99.8 mol%, about 90 mol% to about 99.5 mol%, about 91 mol% to about 99.5 mol%, about 92 mol% to about 99.5 ... mol% to about 99.5 mol%, about 94 mol% to about 99.5 mol%, about 95 mol% to about 99.5 mol%, about 96 mol% to about 99.5 mol%, about 90 mol% to about 99 mol%, about 91 mol% to about 99 mol%, about 92 mol% to about 99 mol%, about 93 mol% to about 99 mol%, about 94 mol% to about 99 mol%, about 95 mol% to about 99 mol%, about 90 mol% to about 98.5 ... % to about 98.5 mol%, about 92 mol% to about 98.5 mol%, about 93 mol% to about 98.5 mol%, about 94 mol% to about 98.5 mol%, about 95 mol% to about 98.5 mol%, about 90 mol% to about 98 mol%, about 91 mol% to about 98 mol%, about 92 mol% to about 98 mol%, about 93 mol% to about 98 mol%, about 94 mol% to about 98 mol%, or about 95 mol% to about 98 mol%.

[0111] In some embodiments, the proportion of structural units (a) in the copolymerization of the binder material is less than 100 mol%, less than 99.9 mol%, less than 99.8 mol%, less than 99.7 mol%, less than 99.6 mol%, less than 99.5 mol%, less than 99.4 mol%, less than 99.3 mol%, less than 99.2 mol%, less than 99.1 mol%, less than 99 mol%, less than 98.8 mol%, less than 98.5 mol%, less than 98 mol%, less than 97 mol%, less than 96 mol%, less than 95 mol%, less than 94 mol%, less than 93 mol%, or less than 92 mol%, based on the total moles of monomer units in the copolymerization. In some embodiments, the proportion of structural units (a) in the copolymerization of the binder material is 90 mol% or more, 91 mol% or more, 92 mol% or more, 93 mol% or more, 93.5 mol% or more, 94 mol% or more, 94.5 mol% or more, 95 mol% or more, 95.5 mol% or more, 96 mol% or more, 96.5 mol% or more, 97 mol% or more, 97.5 mol% or more, or 98 mol% or more, based on the total moles of monomer units in the copolymerization.

[0112] In some embodiments, the proportion of structural unit (b) in the copolymerization of the binder material is from about 0.1 mol % to about 10 mol %, from about 0.1 mol % to about 9 mol %, from about 0.1 mol % to about 8 mol %, from about 0.1 mol % to about 7 mol %, from about 0.1 mol % to about 6 mol %, from about 0.1 mol % to about 5 mol %, from about 0.1 mol % to about 4 mol %, from about 0.5 mol % to about 10 mol %, from about 0.5 mol % to about 9 mol %, from about 0.5 mol % to about 8 mol %, from about 0.5 mol % to about 7 mol %, from about 0.5 mol % to about 6 mol %, from about 0.5 mol % to about 5 mol %, from about 0.5 mol % to about 6 mol %, about 4 mol%, about 1 mol% to about 10 mol%, about 1 mol% to about 9 mol%, about 1 mol% to about 8 mol%, about 1 mol% to about 7 mol%, about 1 mol% to about 6 mol%, about 1 mol% to about 5 mol%, about 1 mol% to about 4 mol%, about 1.5 mol% to about 10 mol%, about 1.5 mol% to about 9 mol%, about 1.5 mol% to about 8 mol%, about 1.5 mol% to about 7 mol%, about 1.5 mol% to about 6 mol%, about 1.5 mol% to about 5 mol%, about 2 mol% to about 10 mol%, about 2 mol% to about 9 mol%, about 2 mol% to about 8 mol%, about 2 mol% to about 7 mol%, about 2 mol% to about 6 mol%, or about 2 mol% to about 5 mol%.

[0113] In some embodiments, the proportion of structural units (b) in the copolymerization of the binder material is less than 10 mol%, less than 9 mol%, less than 8 mol%, less than 7 mol%, less than 6 mol%, less than 5 mol%, less than 4.5 mol%, less than 4 mol%, less than 3.5 mol%, less than 3 mol%, less than 2.5 mol%, or less than 2 mol%, based on the total number of moles of monomer units in the copolymerization. In some embodiments, the proportion of structural units (b) in the copolymerization of the binder material is 0.1 mol% or more, 0.2 mol% or more, 0.4 mol% or more, 0.6 mol% or more, 0.8 mol% or more, 1 mol% or more, 1.2 mol% or more, 1.4 mol% or more, 1.6 mol% or more, 1.8 mol% or more, 2 mol% or more, 3 mol% or more, 4 mol% or more, 5 mol% or more, 6 mol% or more, 7 mol% or more, or 8 mol% or more, based on the total number of moles of monomer units in the copolymerization.

[0114] The relative ratio of structural units (a) and (b) in the copolymer in the binder material is important in that it determines the functionality of the binder material (i.e., adhesive strength, dispersibility in aqueous solvent, and resistance to redissolution in aqueous solvent). When the molar ratio of structural units (a) and structural units (b) in the copolymer of the binder material is within the ranges disclosed herein, the binder material is observed to exhibit very good adhesive strength. Furthermore, the binder material used in the present invention is capable of being homogeneously dispersed in aqueous solvent, allowing for good processability of the conductive slurry formed therefrom in the manufacture of improved current collectors. Most importantly, the binder material exhibits a high level of resistance to redissolution in aqueous solvent. This is particularly evident when the electrode layer slurry is applied to the surface of the binder material-containing conductive layer in the formation of an electrode. It is observed that the binder material disclosed herein is capable of retaining its adhesive ability to bond the conductive layer to the substrate upon contact with aqueous solvent without reverting to a fluid. This allows the conductive layer that forms a physical barrier between the substrate and the electrode layer to remain intact on the substrate, helping to reduce the possibility of corrosion of the substrate. The presence of this conductive layer reduces the interfacial resistance between the electrode layer and the improved current collector, improving the electrochemical performance of the battery.

[0115] In some embodiments, the molar ratio of structural unit (a) to structural unit (b) in the copolymer of the binder material is from about 9 to about 1000, from about 9 to about 900, from about 9 to about 800, from about 9 to about 700, from about 9 to about 700, from about 9 to about 600, from about 9 to about 500, from about 9 to about 400, from about 9 to about 300, from about 9 to about 200, from about 9 to about 150, from about 9 to about 100, from about 10 to about 1000, from about 10 to about 900, from about 10 to about 800, from about 1 0 to about 700, about 10 to about 600, about 10 to about 500, about 10 to about 400, about 10 to about 300, about 10 to about 200, about 10 to about 150, about 10 to about 100, about 12 to about 500, about 12 to about 300, about 12 to about 100, about 14 to about 500, about 14 to about 300, about 14 to about 100, about 16 to about 500, about 16 to about 300, about 16 to about 100, about 18 to about 500, about 18 to about 300, and about 18 to about 100.

[0116] In some embodiments, the molar ratio of structural units (a) to structural units (b) in the copolymer of the binder material is less than 1000, less than 800, less than 600, less than 400, less than 200, less than 100, less than 80, less than 60, less than 40, less than 30, less than 20, or less than 15. In some embodiments, the molar ratio of structural units (a) to structural units (b) in the copolymer of the binder material is greater than 9, greater than 10, greater than 12, greater than 14, greater than 16, greater than 18, greater than 20, greater than 30, greater than 40, greater than 50, greater than 100, greater than 250, greater than 500, or greater than 700.

[0117] In some embodiments, the weight average molecular weight (M w) is about 10,000 g / mol to about 300,000 g / mol, about 15,000 g / mol to about 300,000 g / mol, about 20,000 g / mol to about 300,000 g / mol, about 30,000 g / mol to about 300,000 g / mol, about 40,000 g / mol to about 300,000 g / mol, about 50,000 g / mol to about 300,000 g / mol, about 75,000 g / mol to about 300,000 g / mol, 0 g / mol, about 100,000 g / mol to about 300,000 g / mol, about 125,000 g / mol to about 300,000 g / mol, about 150,000 g / mol to about 300,000 g / mol, about 200,000 g / mol to about 300,000 g / mol, about 10,000 g / mol to about 200,000 g / mol, about 15,000 g / mol to about 200,000 g / mol, about 20,000 g / mol to about 200,000 g / mol, about 30,000 g / mol to about 200,000 g / mol, about 40,000 g / mol to about 200,000 g / mol, about 50,000 g / mol to about 200,000 g / mol, about 75,000 g / mol to about 200,000 g / mol, about 100,000 g / mol to about 200,000 g / mol, about 10,000 g / mol to about 150,000 g / mol, about 15,000 g / mol mol to about 150,000 g / mol, about 20,000 g / mol to about 150,000 g / mol, about 30,000 g / mol to about 150,000 g / mol, about 40,000 g / mol to about 150,000 g / mol, about 50,000 g / mol to about 150,000 g / mol, about 75,000 g / mol to about 150,000 g / mol, or about 100,000 g / mol to about 150,000 g / mol.

[0118] In some embodiments, the weight average molecular weight of the copolymer in the binder material is less than 300,000 g / mol, less than 250,000 g / mol, less than 200,000 g / mol, less than 175,000 g / mol, less than 150,000 g / mol, less than 125,000 g / mol, less than 100,000 g / mol, less than 90,000 g / mol, less than 80,000 g / mol, less than 70,000 g / mol, less than 60,000 g / mol, or less than 50,000 g / mol. In some embodiments, the weight average molecular weight of the copolymer in the binder material is greater than 10,000 g / mol, greater than 15,000 g / mol, greater than 20,000 g / mol, greater than 25,000 g / mol, greater than 30,000 g / mol, greater than 35,000 g / mol, greater than 40,000 g / mol, greater than 50,000 g / mol, greater than 60,000 g / mol, greater than 70,000 g / mol, greater than 80,000 g / mol, greater than 100,000 g / mol, or greater than 150,000 g / mol.

[0119] In some embodiments, the viscosity of the binder material at a 4% concentration in DI water at 20° C. is from about 5 mPa·s to about 80 mPa·s, from about 8 mPa·s to about 80 mPa·s, from about 10 mPa·s to about 80 mPa·s, from about 15 mPa·s to about 80 mPa·s, from about 20 mPa·s to about 80 mPa·s, from about 25 mPa·s to about 80 mPa·s, from about 30 mPa·s to about 80 mPa·s, from about 35 mPa·s to about 80 mPa·s, from about 40 mPa·s to about 80 mPa·s, about 5 mPa·s to about 50 mPa·s, about 8 mPa·s to about 50 mPa·s, about 10 mPa·s to about 50 mPa·s, about 15 mPa·s to about 50 mPa·s, about 20 mPa·s to about 50 mPa·s, about 25 mPa·s to about 50 mPa·s, about 30 mPa·s to about 50 mPa·s, about 5 mPa·s to about 30 mPa·s, about 10 mPa·s to about 30 mPa·s, about 15 mPa·s to about 30 mPa·s, or about 5 mPa·s to about 25 mPa·s.

[0120] In some embodiments, the viscosity of the binder material at a 4% concentration in DI water at 20° C. is less than 80 mPa·s, less than 70 mPa·s, less than 60 mPa·s, less than 50 mPa·s, less than 45 mPa·s, less than 40 mPa·s, less than 35 mPa·s, less than 30 mPa·s, less than 25 mPa·s, less than 20 mPa·s, less than 15 mPa·s, less than 10 mPa·s, or less than 8 mPa·s. In some embodiments, the viscosity of the binder material at a 4% concentration in DI water at 20° C. is greater than 5 mPa·s, greater than 7 mPa·s, greater than 10 mPa·s, greater than 15 mPa·s, greater than 20 mPa·s, greater than 25 mPa·s, greater than 30 mPa·s, greater than 35 mPa·s, greater than 40 mPa·s, greater than 45 mPa·s, greater than 50 mPa·s, greater than 60 mPa·s, or greater than 70 mPa·s.

[0121] The binder material used in the present invention exhibits strong adhesive ability. In some embodiments, the adhesive strength between the binder material and the substrate is about 2 N / cm to about 8 N / cm, about 2 N / cm to about 7.5 N / cm, about 2 N / cm to about 7 N / cm, about 2 N / cm to about 6.5 N / cm, about 2 N / cm to about 6 N / cm, about 2 N / cm to about 6 N / cm, about 2 N / cm to about 5.5 N / cm, about 2 N / cm to about 5 N / cm, about 2 N / cm to about 4.5 N / cm, about 2 N / cm to about 4 N / cm, about 2 N / cm to about 3.8 N / cm, about 2 N / cm to about 3.6 N / cm, about 2 N / cm to about 3.4N / cm, about 2N / cm to about 3.2N / cm, about 2N / cm to about 3N / cm, about 2.5N / cm to about 8N / cm, about 3N / cm to about 8N / cm, about 3.5N / cm to about 8N / cm, about 4N / cm to about 8N / cm, about 4.5N / cm to about 8N / cm, about 5N / cm to about 8N / cm, about 5.5N / cm to about 8N / cm, about 6N / cm to about 8N / cm, about 3N / cm to about 7N / cm, about 3N / cm to about 6N / cm, about 3N / cm to about 5.5N / cm, or about 4N / cm to about 6N / cm.

[0122] In some embodiments, the adhesion strength between the binder material and the substrate is less than 8 N / cm, less than 7.5 N / cm, less than 7 N / cm, less than 6.5 N / cm, less than 6 N / cm, less than 5.5 N / cm, less than 5 N / cm, less than 4.5 N / cm, less than 4 N / cm, less than 3.8 N / cm, less than 3.6 N / cm, less than 3.4 N / cm, less than 3.2 N / cm, less than 3 N / cm, less than 2.8 N / cm, or less than 2.6 N / cm. In some embodiments, the adhesive strength between the binder material and the substrate is greater than 2 N / cm, greater than 2.2 N / cm, greater than 2.4 N / cm, greater than 2.6 N / cm, greater than 2.8 N / cm, greater than 3 N / cm, greater than 3.2 N / cm, greater than 3.4 N / cm, greater than 3.6 N / cm, greater than 3.8 N / cm, greater than 4 N / cm, greater than 4.5 N / cm, greater than 5 N / cm, greater than 5.5 N / cm, greater than 6 N / cm, greater than 6.5 N / cm, greater than 7 N / cm, or greater than 7.5 N / cm.

[0123] The respective ratios of binder material and conductive material in the conductive layer of the improved current collector are of paramount importance in determining the effectiveness of the conductive layer in forming a non-deforming conductive layer structure, reducing the tendency of corrosion of the substrate, and minimizing the interfacial resistance between the electrode layer and the improved current collector. Insufficient amount of conductive material in the conductive layer may result in the formation of a conductive network with insufficient coverage to facilitate efficient and effective transfer of electrons between the electrode layer and the substrate, resulting in increased interfacial resistance. On the other hand, insufficient amount of binder material in the conductive layer may make it difficult to hold the entire conductive layer in place. The conductive layer may easily disintegrate with its internal components breaking apart when subjected to slight changes in the external environment (e.g. scratches, pressure, etc.). As a result, problems related to corrosion of the substrate may persist.

[0124] In some embodiments, the percentage of each of the binder material and the conductive material in the conductive layer of the improved current collector is, independently, based on the total weight of the conductive layer, about 20% to about 75% by weight, about 25% to about 75% by weight, about 30% to about 75% by weight, about 35% to about 75% by weight, about 40% to about 75% by weight, about 45% to about 75% by weight, about 50% to about 75% by weight, about 55% to about 75% by weight, about 60% to about 75% by weight, about 20% to about 70% by weight, about 25% to about 70% by weight, about 30% to about 70% by weight, about 35% to about 70% by weight, about 40% to about 70% by weight, about 45% to about 70% by weight, about 50% to about 70% by weight, about 55% to about 70% by weight, about 20% to about 70% by weight, or about 25% to about 70% by weight. %~about 65 weight%, about 25 weight%~about 65 weight%, about 30 weight%~about 65 weight%, about 35 weight%~about 65 weight%, about 40 weight%~about 65 weight%, about 45 weight%~about 65 weight% %, about 50% to about 65% by weight, about 20% to about 60% by weight, about 25% to about 60% by weight, about 30% to about 60% by weight, about 35% to about 60% by weight, about 40% by weight % to about 60% by weight, about 45% to about 60% by weight, about 20% to about 55% by weight, about 25% to about 55% by weight, about 30% to about 55% by weight, about 35% to about 55% by weight, about 40% to about 55% by weight, about 20% to about 50% by weight, about 25% to about 50% by weight, about 30% to about 50% by weight, or about 35% to about 50% by weight.

[0125] In some embodiments, the proportion of each of the binder material and the conductive material in the conductive layer of the improved current collector is, independently, less than 75 weight percent, less than 70 weight percent, less than 65 weight percent, less than 60 weight percent, less than 55 weight percent, less than 50 weight percent, less than 45 weight percent, less than 40 weight percent, less than 35 weight percent, less than 30 weight percent, or less than 25 weight percent, based on the total weight of the conductive layer. In some embodiments, the proportion of each of the binder material and the conductive material in the conductive layer of the improved current collector is, independently, more than 20 weight percent, more than 25 weight percent, more than 30 weight percent, more than 35 weight percent, more than 40 weight percent, more than 45 weight percent, more than 50 weight percent, more than 55 weight percent, more than 60 weight percent, more than 65 weight percent, or more than 70 weight percent, based on the total weight of the conductive layer.

[0126] In certain embodiments, the conductive layer further comprises a surfactant or dispersant. These surfactants may be added during the manufacture of the conductive slurry to improve the dispersion of the conductive material in the slurry. There is no particular restriction on the type of surfactant or dispersant used, except that it should be capable of dispersing the conductive material in the conductive slurry and not affect the overall performance of the manufactured conductive layer. In other embodiments, the conductive layer does not comprise a surfactant or dispersant.

[0127] In some embodiments, the proportion of surfactant or dispersant in the conductive layer is from about 0% to about 5% by weight, from about 0.5% to about 5% by weight, from about 1% to about 5% by weight, from about 1.5% to about 5% by weight, from about 2% to about 5% by weight, from about 2.5% to about 5% by weight, from about 3% to about 5% by weight, from about 0% to about 4% by weight, from about 0.5% to about 4% by weight, based on the total weight of the conductive layer. %, about 1 wt % to about 4 wt %, about 1.5 wt % to about 4 wt %, about 2 wt % to about 4 wt %, about 0 wt % to about 3 wt %, about 0.5 wt % to about 3 wt %, about 1 wt % to about 3 wt %, about 0 wt % to about 2.5 wt %, about 0.5 wt % to about 2.5 wt %, about 1 wt % to about 2.5 wt %, about 1.5 wt % to about 2.5 wt %, or about 2 wt % to about 2.5 wt %.

[0128] In some embodiments, the proportion of the surfactant or dispersant in the conductive layer is less than 5 wt%, less than 4.5 wt%, less than 4 wt%, less than 3.5 wt%, less than 3 wt%, less than 2.5 wt%, less than 2 wt%, less than 1.5 wt%, less than 1 wt%, or less than 0.5 wt%, based on the total weight of the conductive layer. In some embodiments, the proportion of the surfactant or dispersant in the conductive layer is greater than 0 wt%, greater than 0.5 wt%, greater than 1 wt%, greater than 1.5 wt%, greater than 2 wt%, greater than 2.5 wt%, greater than 3 wt%, greater than 3.5 wt%, greater than 4 wt%, or greater than 4.5 wt%, based on the total weight of the conductive layer.

[0129] The thickness of the improved current collector in the electrode can affect the volume it occupies in the battery, the space available to the electrode active material in the electrode layer, and the capacity of the battery. In certain embodiments, the improved current collector has a thickness of about 5 μm to about 70 μm, about 5 μm to about 60 μm, about 5 μm to about 50 μm, about 5 μm to about 40 μm, about 5 μm to about 30 μm, about 5 μm to about 20 μm, about 10 μm to about 70 μm, about 10 μm to about 60 μm, about 10 μm to about 50 μm, about 10 μm to about 40 μm, about 10 μm to about 30 μm, about 15 μm to about 70 μm, about 15 μm to about 60 μm, about 15 μm to about 50 μm. m, about 15 μm to about 40 μm, about 15 μm to about 30 μm, about 20 μm to about 70 μm, about 20 μm to about 60 μm, about 20 μm to about 50 μm, about 20 μm to about 40 μm, about 25 μm to about 70 μm, about 25 μm to about 60 μm, about 25 μm to about 50 μm, about 20 μm to about 40 μm, about 25 μm to about 70 μm, about 25 μm to about 60 μm, about 25 μm to about 50 μm, or about 25 μm to about 40 μm.

[0130] In some embodiments, the improved current collector has a thickness of less than 70 μm, less than 60 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 25 μm, less than 20 μm, less than 15 μm, or less than 10 μm. In some embodiments, the improved current collector has a thickness of more than 5 μm, more than 10 μm, more than 15 μm, more than 20 μm, more than 25 μm, more than 30 μm, more than 40 μm, more than 50 μm, or more than 60 μm.

[0131] The thickness of the substrate in the improved current collector can affect the volume it occupies in the improved current collector and / or electrode. This can affect the available space for the conductive and binder materials in the conductive layer and / or the electrode active material in the electrode layer. Thus, the conductivity of the battery system, the ability of the conductive layer to bond to the substrate, and the capacity of the battery can be affected. In some embodiments, the substrate in the improved current collector has a thickness of about 5 μm to about 50 μm, about 5 μm to about 45 μm, about 5 μm to about 40 μm, about 5 μm to about 35 μm, about 5 μm to about 30 μm, about 5 μm to about 25 μm, about 10 μm to about 50 μm, about 10 μm to about 45 μm, about 10 μm to about 40 μm, about 10 μm to about 35 μm, about 10 μm to about 30 μm, about 15 μm to about 50 μm, about 15 μm to about 45 μm, about 15 μm to about 40 μm, about 15 μm to about 35 μm, about 20 μm to about 50 μm, about 20 μm to about 45 μm, or about 20 μm to about 40 μm.

[0132] In some embodiments, the substrate in the improved current collector has a thickness of less than 50 μm, less than 45 μm, less than 40 μm, less than 35 μm, less than 30 μm, less than 25 μm, less than 20 μm, less than 15 μm, or less than 10 μm. In some embodiments, the substrate in the improved current collector has a thickness of more than 5 μm, more than 10 μm, more than 15 μm, more than 20 μm, more than 25 μm, more than 30 μm, more than 35 μm, more than 40 μm, or more than 45 μm.

[0133] In some embodiments, the conductive layer in the improved current collector has a thickness of about 1 μm to about 20 μm, about 1 μm to about 16 μm, about 1 μm to about 12 μm, about 1 μm to about 10 μm, about 2 μm to about 20 μm, about 2 μm to about 16 μm, about 2 μm to about 12 μm, about 2 μm to about 10 μm, about 3 μm to about 20 μm, about 3 μm to about 16 μm, about 3 μm to about 12 μm, about 3 μm to about 10 μm, about 4 μm to about 20 μm, about 4 μm to about 16 μm, about 4 μm to about 12 μm, or about 4 μm to about 10 μm.

[0134] In some embodiments, the conductive layer in the improved current collector has a thickness of less than 20 μm, less than 18 μm, less than 16 μm, less than 14 μm, less than 12 μm, less than 10 μm, less than 8 μm, less than 6 μm, or less than 4 μm. In some embodiments, the conductive layer in the improved current collector has a thickness of more than 1 μm, more than 2 μm, more than 4 μm, more than 6 μm, more than 8 μm, more than 10 μm, more than 12 μm, more than 14 μm, more than 16 μm, or more than 18 μm.

[0135] As discussed above, in some embodiments, the conductive layer in the improved current collector of the present invention is produced via a conductive slurry. In some embodiments, the conductive slurry comprises a conductive material, a binder material, and a solvent. In some embodiments, the binder material comprises a copolymer as described above. In some embodiments, the solvent in the conductive slurry is an aqueous solvent.

[0136] In certain embodiments, the aqueous solvent is water. In some embodiments, the aqueous solvent is selected from the group consisting of tap water, bottled water, purified water, pure water, distilled water, deionized water (DI water), DO, and combinations thereof.

[0137] In some embodiments, the aqueous solvent in the conductive slurry further comprises a minor component in addition to water. In some embodiments, the volume ratio of water to the minor component is 51:49 to 99:1. Any water-miscible or volatile solvent may be used as the minor component of the aqueous solvent. Some non-limiting examples of the minor component include alcohols, lower aliphatic ketones, lower alkyl acetates, and combinations thereof. The addition of the minor component may improve the processability of the conductive slurry.

[0138] Some non-limiting examples of alcohols include C1-C4 alcohols such as methanol, ethanol, isopropanol, n-propanol, tert-butanol, n-butanol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, ethylene glycol, propylene glycol, glycerol, and combinations thereof. Some non-limiting examples of lower aliphatic ketones include acetone, dimethyl ketone, methyl ethyl ketone (MEK), and combinations thereof. Some non-limiting examples of lower alkyl acetates include ethyl acetate (EA), isopropyl acetate, propyl acetate, butyl acetate (BA), and combinations thereof. Some other non-limiting examples of water-miscible or volatile solvents include 1,4-dioxane, diethyl ether, methyl tert-butyl ether, cyclopentyl methyl ether, tetrahydrofuran (THF), 2-methyltetrahydrofuran, acetonitrile, dimethyl sulfoxide (DMSO), sulfolane, nitromethane, propylene carbonate, ethylene carbonate, dimethyl carbonate, pyridine, acetaldehyde, formic acid, acetic acid, propanoic acid, butyric acid, gamma-valerolactone (GVL), furfuryl alcohol, methyl lactate, ethyl lactate, diethanolamine, dimethylacetamide (DMAc), dimethylformamide (DMF), N-methylpyrrolidone (NMP), dihydrolevoglucosenone (Cyrene®), N,N'-dimethylpropyleneurea (DMPU), and dimethylisosorbide (DMI). In some embodiments, minor components are not present in the aqueous solvent of the conductive slurry.

[0139] In some embodiments, the solids content of the conductive slurry is about 5% to about 25% by weight, about 6% to about 25% by weight, about 7% to about 25% by weight, about 8% to about 25% by weight, about 9% to about 25% by weight, about 10% to about 25% by weight, about 11% to about 25% by weight, about 12% to about 25% by weight, about 13% to about 25% by weight, about 14% to about 25% by weight, about 15% to about 25% by weight, about 5% to about 20% by weight, about 6% to about 20% by weight, based on the total weight of the conductive slurry. , about 7% by weight to about 20% by weight, about 8% by weight to about 20% by weight, about 9% by weight to about 20% by weight, about 10% by weight to about 20% by weight, about 5% by weight to about 17% by weight, about 6% by weight to about 17% by weight, about 7% by weight to about 17% by weight, about 8% by weight to about 17% by weight, about 9% by weight to about 17% by weight, about 10% by weight to about 17% by weight, about 5% by weight to about 15% by weight, about 6% by weight to about 15% by weight, about 7% by weight to about 15% by weight, about 8% by weight to about 15% by weight, about 9% by weight to about 15% by weight, or about 10% by weight to about 15% by weight.

[0140] In some embodiments, the solids content of the conductive slurry is less than 25%, less than 23%, less than 20%, less than 19%, less than 18%, less than 17%, less than 16%, less than 15%, less than 14%, less than 13%, less than 10%, less than 8%, or less than 6% by weight based on the total weight of the conductive slurry. In some embodiments, the solids content of the conductive slurry is greater than 5%, greater than 6%, greater than 7%, greater than 8%, greater than 9%, greater than 10%, greater than 11%, greater than 12%, greater than 13%, greater than 14%, greater than 15%, greater than 16%, greater than 17%, greater than 18%, greater than 19%, greater than 20%, or greater than 22% by weight based on the total weight of the conductive slurry.

[0141] The method used to generate the conductive slurry is not particularly limited, except that all components of the slurry (e.g., conductive material, binder material, aqueous solvent) should be mixed uniformly, for example, by using a homogenizer, to form a homogenous slurry. In some embodiments, all components of the conductive slurry are added to the homogenizer in a single batch. In other embodiments, each component of the conductive slurry may be added to the homogenizer in one or more batches, and each batch may comprise one or more components. However, if the conductive slurry includes a surfactant or dispersant, it is preferred that the surfactant or dispersant be added to the homogenizer before adding the conductive material to ensure that the conductive material can be well dispersed in the slurry by the action of the surfactant or dispersant.

[0142] Any homogenizer capable of reducing or eliminating particle agglomeration and promoting homogeneous dispersion of the various components of the conductive slurry may be used herein. In some embodiments, the homogenizer is a planetary agitator mixer, an agitator mixer, a blender, or an ultrasonicator. There is no particular limit to the agitation speed and duration, except that it should be sufficient to allow good dispersion of the conductive material and binder material in the aqueous medium to ensure that the coating can be homogeneous when the conductive slurry is coated on a substrate.

[0143] Additionally, there are no particular limitations on the temperature at which homogenization of the conductive slurry occurs, except that the temperature must be high enough to ensure that the binder material can be readily dissolved in the slurry while not being so viscous that the slurry is not so viscous that it affects processability, while at the same time not being so high that it boils the aqueous solvent. In some embodiments, homogenization of the conductive slurry occurs at a temperature of about 20°C to about 95°C, about 25°C to about 95°C, about 30°C to about 95°C, about 20°C to about 75°C, about 25°C to about 75°C, about 30°C to about 75°C, about 35°C to about 75°C, about 40°C to about 75°C, about 20°C to about 60°C, about 25°C to about 60°C, about 30°C to about 60°C, about 35°C to about 60°C, about 40°C to about 60°C, about 25°C to about 50°C, or about 30°C to about 50°C.

[0144] In some embodiments, homogenization of the conductive slurry occurs at a temperature below 95° C., below 85° C., below 75° C., below 65° C., below 55° C., below 50° C., below 45° C., below 40° C., below 35° C., below 30° C., or below 25° C. In some embodiments, homogenization of the conductive slurry occurs at a temperature above 20° C., above 25° C., above 30° C., above 35° C., above 40° C., above 45° C., above 50° C., above 55° C., above 60° C., above 65° C., above 70° C., or above 75° C.

[0145] In some embodiments, after homogenization of the conductive slurry, the slurry can be coated on one or both sides of a substrate to form a conductive layer film. There are no particular limitations on the equipment and conditions used to coat the conductive slurry, except that it should result in a uniform, flat and smooth coating layer. In certain embodiments, the coating process is carried out using a doctor blade coater, a slot die coater, a transfer coater, a spray coater, a roll coater, a gravure coater, a dip coater, or a curtain coater.

[0146] In some embodiments, after the conductive slurry is coated onto the substrate, the coating is dried to form the improved current collector of the present invention. Any equipment capable of drying the coating to attach the resulting conductive layer to the substrate may be used herein. Some non-limiting examples of such drying equipment include batch drying ovens, conveyor drying ovens, and microwave drying ovens.

[0147] There are no particular limitations on the conditions used for drying, except that the drying conditions should be sufficient to ensure that the conductive layer is strongly adhered to the substrate. However, drying the conductive layer at a temperature above 100° C. may result in undesirable deformation of the resulting improved current collector, affecting the performance of any electrodes made therefrom. The drying temperature should be optimized relative to other drying conditions, such as drying time, to ensure that the aqueous solvent is sufficiently removed from the conductive layer.

[0148] In some embodiments, the improved current collector is mechanically compressed after drying to densify the conductive layer, after which an electrode layer may be formed on the improved current collector to form a completed electrode, hi other embodiments, the improved current collector is not compressed.

[0149] In some embodiments, after coating and drying of the conductive slurry on a substrate, whether compressed or not, the resulting conductive layer in the improved current collector has a thickness of about 0.1 μm to about 5.0 μm. The thickness of the conductive layer affects the total volume of the improved current collector, which in turn affects the total volume occupied by an electrode comprising the improved current collector, and the corresponding amount of electrode active material required for the electrode layer of the electrode, and thus the capacity of a battery comprising the electrode.

[0150] In certain embodiments, the thickness of the conductive layer in the improved current collector of the present invention is about 0.1 μm to about 5.0 μm, about 0.1 μm to about 4.5 μm, about 0.1 μm to about 4 μm, about 0.1 μm to about 3.5 μm, about 0.1 μm to about 3 μm, about 0.1 μm to about 2.5 μm, about 0.1 μm to about 2 μm, about 0.5 μm to about 5.0 μm, about 0.5 μm to about 4.5 μm, about 1.0 μm to about 4.0 μm, about 1.0 μm to about 3.5 μm, about 1.0 μm to about 3.0 μm, about 1.0 μm to about 2.5 μm, or about 1.0 μm to about 2.0 μm. In some embodiments, the thickness of the conductive layer is less than 5.0 μm, less than 4.5 μm, less than 4.0 μm, less than 3.5 μm, less than 3.0 μm, less than 2.5 μm, less than 2.0 μm, less than 1.5 μm, less than 1.0 μm, less than 0.5 μm, or less than 0.3 μm. In some embodiments, the thickness of the conductive layer is greater than 0.1 μm, greater than 0.2 μm, greater than 0.5 μm, greater than 1.0 μm, greater than 1.2 μm, greater than 1.5 μm, greater than 1.8 μm, greater than 2.0 μm, greater than 2.5 μm, greater than 3.0 μm, greater than 3.5 μm, or greater than 4.0 μm.

[0151] An electrode can then be made with the improved current collector of the present invention by forming an electrode layer on the improved current collector. There is no particular limit to the composition of the electrode layer, and any composition known in the art is suitable for use in the present invention, provided that such an electrode can achieve good electrochemical performance. The composition of such an electrode layer depends on the type of battery being manufactured and whether the electrode layer is used in the negative or positive electrode of the battery. In some embodiments, the type of battery can be a primary or secondary battery. Some non-limiting examples of battery types include alkaline batteries, aluminum-air batteries, lithium batteries, lithium-air batteries, magnesium batteries, silver oxide batteries, zinc-air batteries, aluminum-ion batteries, lead-acid batteries, lithium-ion batteries, magnesium-ion batteries, potassium-ion batteries, sodium-ion batteries, sodium-air batteries, silicon-air batteries, zinc-ion batteries, and sodium-sulfur batteries. Furthermore, depending on the state of the electrolyte used (i.e., liquid or solid state), the battery can be classified as a conventional battery (when a liquid electrolyte is used) or a solid-state battery (when a solid electrolyte is used).

[0152] In some embodiments, the electrode layer comprises an electrode active material and a binder. In certain embodiments, the electrode layer further comprises a conductive agent. The electrode active material in the electrode layer may be a positive electrode active material or a negative electrode active material. When the electrode layer comprises a positive electrode active material, the electrode layer is a positive electrode layer. When the electrode layer comprises a negative electrode active material, the electrode layer is a negative electrode layer.

[0153] In some embodiments, the electrode active material is a positive electrode active material. In some embodiments, the positive electrode active material is LiCoO2, LiNiO2, LiNi 1-x M x O2, LiNi x Mn y O2, LiCo x Ni y O2, Li 1+z Ni x Mn y Co 1-x-y O2, LiNi x Co y Alz each y is independently 0 to 0.9; each z is independently 0 to 0.4; and M is selected from the group consisting of Co, Mn, Al, Fe, Ti, Ga, Mg, and combinations thereof. In certain embodiments, each x in the general formula is independently selected from 0.1, 0.125, 0.15, 0.175, 0.2, 0.225, 0.25, 0.275, 0.3, 0.325, 0.35, 0.375, 0.4, 0.425, 0.45, 0.475, 0.5, 0.525, 0.55, 0.575, 0.6, 0.625, 0.65, 0.675, 0.7, 0.725, 0.75, 0.775, 0.8, 0.825, 0.85, 0.875, and 0.9; and each y in the general formula is independently selected from 0, 0.025, 0.05, 0.075, 0.1, 0.125, 0.15, 0.175, 0.2 ,0.225,0.25,0.275,0.3,0.325,0.35,0.375,0.4,0.425,0.45,0.475,0.5,0.525,0.55,0.575,0.6,0.625,0.65,0.675,0.7,0.725,0.75,0.775,0.8,0.825,0 In some embodiments, each x, y, and z in the general formula is independently selected from 0, 0.025, 0.05, 0.075, 0.1, 0.125, 0.15, 0.175, 0.2, 0.225, 0.25, 0.275, 0.3, 0.325, 0.35, 0.375, and 0.4. In some embodiments, each x, y, and z in the general formula is independently selected from 0.01 intervals.

[0154] In certain embodiments, the positive electrode active material is LiNi x Mn y O2, Li 1+z Ni x Mn y Co 1-x-y O2(NMC), LiNi x Co y Al zO2(NCA), LiCo x Ni y Each x is independently 0.4 to 0.6, each y is independently 0.2 to 0.4, and each z is independently 0 to 0.1. In other embodiments, the active cathode material is not LiCoO2, LiNiO2, LiV2O5, LiTiS2, LiMoS2, LiMnO2, LiCrO2, LiMn2O4, LiFeO2, or LiFePO4. In further embodiments, the active cathode material is LiNi x Mn y O2, Li 1+z Ni x Mn y Co 1-x-y O2, LiNi x Co y Al z O2, or LiCo x Ni y Each x is independently 0.1 to 0.9, each y is independently 0 to 0.45, and each z is independently 0 to 0.2. 1+x Ni a Mn b Co c Al (1-a-b-c) O2, where -0.2≦x≦0.2, 0≦a<1, 0≦b<1, 0≦c<1, and a+b+c≦1. In some embodiments, the positive electrode active material is represented by the general formula Li 1+x Ni a Mn b Co c Al (1-a-b-c)Having O2, where 0.33 ≦ a ≦ 0.92, 0.33 ≦ a ≦ 0.9, 0.33 ≦ a ≦ 0.8, 0.4 ≦ a ≦ 0.92, 0.4 ≦ a ≦ 0.9, 0.4 ≦ a ≦ 0.8, 0.5 ≦ a ≦ 0.92, 0.5 ≦ a ≦ 0.9, 0.5 ≦ a ≦ 0.8, 0.6 ≦ a ≦ 0.92, or 0.6 ≦ a ≦ 0.9, 0 ≦ b ≦ 0.5, 0 ≦ b ≦ 0.4, 0 ≦ b ≦ 0.3, 0 ≦ b ≦ 0.2, 0.1 ≦ b ≦ 0.5, 0.1 ≦ b ≦ 0.4, 0.1 ≦ b ≦ 0.3, 0.1 ≦ b ≦ 0.2, 0.2 ≦ b ≦ 0.5, 0.2 ≦ b ≦ 0.4, or 0.2 ≦ b ≦ 0.3, 0 ≦ c ≦ 0.5, 0 ≦ c ≦ 0.4, 0 ≦ c ≦ 0.3, 0.1 ≦ c ≦ 0.5, 0.1 ≦ c ≦ 0.4, 0.1 ≦ c ≦ 0.3, 0.1 ≦ c ≦ 0.2, 0.2 ≦ c ≦ 0.5, 0.2 ≦ c ≦ 0.4, or 0.2 ≦ c ≦ 0.3. In some embodiments, the positive electrode active material has the general formula LiMPO4, and M is selected from the group consisting of Fe, Co, Ni, Mn, Al, Mg, Zn, Ti, La, Ce, Sn, Zr, Ru, Si, Ge, or combinations thereof.

[0155] In some embodiments, the positive electrode active material is selected from the group consisting of LiFePO4, LiCoPO4, LiNiPO4, LiMnPO4, LiMnFePO4, LiMn x Fe (1-x) PO4, and combinations thereof, where 0 < x < 1. In some embodiments, the positive electrode active material is LiNi x Mn y O4, where 0.1 ≦ x ≦ 0.9 and 0 ≦ y ≦ 2. In certain embodiments, the positive electrode active material is xLi2MnO3·(1 - x)LiMO2, where M is selected from the group consisting of Ni, Co, Mn, and combinations thereof, and 0 < x < 1. In some embodiments, the positive electrode active material is Li3V2(PO4)3 or LiVPO4F. In certain embodiments, the positive electrode active material has the general formula Li2MSiO4, and M is selected from the group consisting of Fe, Co, Mn, Ni, and combinations thereof.

[0156] In certain embodiments, the positive electrode active material is doped with a dopant selected from the group consisting of Co, Cr, V, Mo, Nb, Pd, F, Na, Fe, Ni, Mn, Al, Mg, Zn, Ti, La, Ce, Sn, Zr, Ru, Si, Ge, and combinations thereof. In some embodiments, the positive electrode active material is not doped with Co, Cr, V, Mo, Nb, Pd, F, Na, Fe, Ni, Mn, Mg, Zn, Ti, La, Ce, Ru, Si, or Ge. In certain embodiments, the positive electrode active material is not doped with Al, Sn, or Zr.

[0157] In some embodiments, the positive electrode active material is LiNi 0.33 Mn 0.33 Co 0.33 O2(NMC333), LiNi 0.4 Mn 0.4 Co 0.2 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2(NMC532), LiNi 0.6 Mn 0.2 Co 0.2 O2(NMC622), LiNi 0.7 Mn 0.15 Co 0.15 O2, LiNi 0.7 Mn 0.1 Co 0.2 O2, LiNi 0.8 Mn 0.1 Co 0.1 O2(NMC811), LiNi 0.92 Mn 0.04 Co 0.04 O2, LiNi 0.85 Mn 0.075 Co 0.075 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.88 Co 0.1 Al 0.02 O2, LiNiO2 (LNO) or a combination thereof.

[0158] In other embodiments, the positive electrode active material is LiCoO2, LiNiO2, LiMnO2, LiMn2O4, or Li2MnO3. In further embodiments, the positive electrode active material is LiNi 0.33 Mn 0.33 Co 0.33 O2, LiNi 0.4 Mn 0.4 Co 0.2 O2, LiNi 0.5 Mn 0.3 Co 0.2 O2, LiNi 0.6 Mn 0.2 Co 0.2 O2, LiNi 0.7 Mn 0.15 Co 0.15 O2, LiNi 0.7 Mn 0.1 Co 0.2 O2, LiNi 0.8 Mn 0.1 Co 0.1 O2, LiNi 0.92 Mn 0.04 Co 0.04 O2, LiNi 0.85 Mn 0.075 Co 0.075 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, or LiNi 0.88 Co 0.1 Al 0.02 It's O2.

[0159] In certain embodiments, the cathode active material comprises a core-shell composite having a core and shell structure, or is a core-shell composite, the core being Li 1+x Ni a Mn b Co c Al (1-a-b-c) O2, LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li2MnO3, LiCrO2, Li4Ti5O 12 , LiV2O5, LiTiS2, LiMoS2, LiCo a Ni b O2, LiMn a Ni bThe core comprises a lithium transition metal oxide selected from the group consisting of Fe2O3, MnO2, Al2O3, MgO, ZnO, TiO2, La2O3, CeO2, SnO2, ZrO2, RuO2, and combinations thereof, where -0.2≦x≦0.2, 0≦a<1, 0≦b<1, 0≦c<1, and a+b+c≦1. In some embodiments, the shell also comprises a lithium transition metal oxide. In certain embodiments, the lithium transition metal oxide of the shell is selected from the above group of lithium transition metal oxides used in the core. In other embodiments, the shell comprises a transition metal oxide. In certain embodiments, the transition metal oxide of the shell is selected from the group consisting of Fe2O3, MnO2, Al2O3, MgO, ZnO, TiO2, La2O3, CeO2, SnO2, ZrO2, RuO2, and combinations thereof. In certain embodiments, the shell comprises a lithium transition metal oxide and a transition metal oxide.

[0160] In certain embodiments, each of the core and the shell independently comprises two or more lithium transition metal oxides. In some embodiments, one of the core or the shell comprises only one lithium transition metal oxide, and the other comprises two or more lithium transition metal oxides. The lithium transition metal oxides in the core and the shell may be the same, or may be different or partially different. In some embodiments, the two or more lithium transition metal oxides are uniformly distributed throughout the core. In certain embodiments, the two or more lithium transition metal oxides are not uniformly distributed throughout the core.

[0161] In some embodiments, each of the metal oxides in the core and shell is independently doped with a dopant selected from the group consisting of Co, Cr, V, Mo, Nb, Pd, F, Na, Fe, Ni, Mn, Al, Mg, Zn, Ti, La, Ce, Sn, Zr, Ru, Si, Ge, and combinations thereof. In some embodiments, the active cathode material is not a core-shell composite.

[0162] In some embodiments, the electrode active material is a positive electrode active material for a sodium ion battery. In some embodiments, the positive electrode active material has the formula Na x M y Az where M is one or more metals and A is one or more anions including one or more of O, P, N, C, H, or halogen. In certain embodiments, the active cathode material for a sodium-ion battery is a sodium analog of the active cathode materials described above, in which lithium is replaced by sodium. In some embodiments, the active cathode material for a sodium-ion battery is selected from the group consisting of NaCoO2, NaFeO2, NaNiO2, NaCrO2, NaVO2, and NaTiO2, NaFePO4, Na3V2(PO4)3, Na3V2(PO4)2F3, NMC-type mixed oxides, and combinations thereof. In some embodiments, the active cathode material for a sodium-ion battery is an organic material, such as, for example, disodium naphthalene diimide, doped quinone, pteridine derivatives, polyimides, polyamic acids, or combinations thereof.

[0163] In some embodiments, the positive electrode active material for sodium ion batteries includes or is a core-shell composite having a core and shell structure. In some embodiments, the positive electrode active material for sodium ion batteries is doped with a dopant. The same dopants as those listed above for the positive electrode active material for lithium ion batteries can be used to dope the positive electrode active material for sodium ion batteries.

[0164] In some embodiments, the average diameter of the positive electrode active material particles is about 0.1 μm to about 100 μm, about 0.1 μm to about 50 μm, about 0.5 μm to about 50 μm, about 0.5 μm to about 30 μm, about 0.5 μm to about 20 μm, about 1 μm to about 20 μm, about 2.5 μm to about 20 μm, about 5 μm to about 20 μm, about 7.5 μm to about 20 μm, about 10 μm to about 20 μm, about 15 μm to about 20 μm, about 2.5 μm to about 50 μm, about 5 μm to about 50 μm, about 10 μm to about 50 μm, about 15 μm to about 50 μm, about 20 μm to about 50 μm, or about 50 μm to about 100 μm.

[0165] In some embodiments, the average diameter of the positive electrode active material particles is less than 100 μm, less than 80 μm, less than 60 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 20 μm, less than 15 μm, less than 10 μm, less than 7.5 μm, less than 5 μm, less than 2.5 μm, less than 1 μm, less than 0.75 μm, or less than 0.5 μm. In some embodiments, the average diameter of the positive electrode active material particles is greater than 0.1 μm, greater than 0.25 μm, greater than 0.5 μm, greater than 0.75 μm, greater than 1 μm, greater than 2.5 μm, greater than 5 μm, greater than 7.5 μm, greater than 10 μm, greater than 15 μm, greater than 20 μm, greater than 30 μm, greater than 40 μm, or greater than 50 μm.

[0166] In some embodiments, the electrode active material is a negative electrode active material. In some embodiments, the negative electrode active material is natural graphite particulate, synthetic graphite particulate, hard carbon, soft carbon, mesocarbon microbeads (MCMB), Sn particulate, SnO2, SnO, Li4T 15 O 12 The particulate material is selected from the group consisting of fine particles, Si fine particles, Si-C composite fine particles, and combinations thereof.

[0167] In certain embodiments, the negative electrode active material is doped with a metal element or a nonmetal element. In some embodiments, the metal element is selected from the group consisting of Fe, Ni, Mn, Al, Mg, Zn, Ti, La, Ce, Sn, Zr, Ru, and combinations thereof. In some embodiments, the nonmetal element is B, Si, Ge, N, P, F, S, Cl, I, Se, or combinations thereof.

[0168] In some embodiments, the negative electrode active material includes or is a core-shell composite having a core and shell structure, and each of the core and shell is independently selected from natural graphite particulate, synthetic graphite particulate, hard carbon, soft carbon, mesocarbon microbeads (MCMB), Sn particulate, SnO2, SnO, Li4T 15 O 12The particulate material is selected from the group consisting of fine particles, Si fine particles, Si-C composite fine particles, and combinations thereof.

[0169] In certain embodiments, the anode active material in the form of a core-shell composite includes a core comprising a carbonaceous material and a shell coated on the carbonaceous material core. In some embodiments, the carbonaceous material is selected from the group consisting of soft carbon, hard carbon, natural graphite particulate, synthetic graphite particulate, mesocarbon microbeads, kish graphite, pyrolytic carbon, mesophase pitch, mesophase pitch-based carbon fiber, and combinations thereof. In certain embodiments, the shell is selected from the group consisting of natural graphite particulate, synthetic graphite particulate, hard carbon, soft carbon, mesocarbon microbeads (MCMB), Sn particulate, SnO2, SnO, Li4T 15 O 12 The particulate material is selected from the group consisting of fine particles, Si fine particles, Si-C composite fine particles, and combinations thereof.

[0170] In certain embodiments, the negative electrode active material is not doped with a metallic or non-metallic element. In some embodiments, the negative electrode active material is not doped with Fe, Ni, Mn, Al, Mg, Zn, Ti, La, Ce, Sn, Zr, Ru, B, Si, Ge, N, P, F, S, Cl, I, or Se.

[0171] In some embodiments, the electrode active material is a sodium-ion battery anode active material. Many embodiments of anode active materials used in lithium-ion batteries are also suitable for use as anode active materials in sodium-ion batteries, although graphite is not suitable because the pores in the material are too small to hold the sodium ions. Also, Li4T 15 O 12 Fine particles are also not suitable as negative electrode active materials for sodium ion batteries because of the presence of lithium, which affects the reaction mechanism in sodium ion batteries.

[0172] In some embodiments, the anode active material for a sodium-ion battery is hard carbon, soft carbon, tin oxides such as SnO2 and SnO, sodium titanates such as NaTi2(PO4)3 and Na2Ti3O7, SnS2, NbS2, SbO x (0 < x ≦ 2), etc., Sn-P compounds and composites, sodium alloys, and combinations thereof. In some embodiments, the anode active material for a sodium-ion battery has the formula Na x M y A z and is a Prussian blue-type sodium compound satisfying the formula, where M is one or more metals and A is one or more anions containing one or more of O, P, N, C, H, or halogen. In some embodiments, the cathode active material for a sodium-ion battery is an organic material such as, for example, naphthalenediimide disodium, doped quinone, pteridine derivatives, polyimide, polyamic acid, or combinations thereof.

[0173] In some embodiments, the anode active material for a sodium-ion battery includes or is a core-shell composite having a core and shell structure. In some embodiments, the anode active material for a sodium-ion battery is doped with one or more elements selected from the group consisting of Sb, Sn, P, S, B, Al, Ga, In, Ge, Pb, As, Bi, Ti, Mo, Se, Te, Co, and combinations thereof.

[0174] The improved current collector of the present invention is particularly suitable for use in electrodes in which the electrode layer is formed using an aqueous slurry and includes a nickel-containing positive active material. Such slurries are highly basic and therefore corrode conventional current collectors (most commonly aluminum foil). However, when an aqueous basic positive electrode slurry is coated onto the improved current collector of the present invention to form a positive electrode, the conductive layer in the improved current collector forms a physical barrier to prevent the conventional current collector (here the substrate of the improved current collector) from contacting the slurry. Thus, corrosion of the substrate is prevented. Nevertheless, the improved current collector of the present invention is suitable for use in electrodes for any type of battery, including any suitable electrode active material (both positive and negative active materials), using any method of forming an electrode layer on the improved current collector.

[0175] There is no particular limit to the binder used in the electrode layer, but the binder should have the desired properties as a bond. Furthermore, when the electrode layer is produced in a slurry, it is preferable that the binder can be well dispersed in the electrode slurry to ensure a uniform and smooth coating. The coating of the electrode slurry containing the binder used herein on the improved current collector should not be able to dissolve the underlying conductive layer in the improved current collector. In some embodiments, various types of binders can be used in the electrode layer as long as they do not tend to cause dissolution of the conductive layer in the improved current collector. In some embodiments, the binder is water-based.

[0176] In some embodiments, the binder in the electrode layer comprises a polymer. In some embodiments, the binder polymer in the electrode layer is a copolymer. In other embodiments, the binder polymer in the electrode layer is a homopolymer.

[0177] In certain embodiments, the binder in the electrode layer is selected from the group consisting of styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyacrylonitrile (PAN), polyacrylamide (PAM), acrylic acid-acrylonitrile-acrylamide copolymers, latex, alginate, polyvinylidene fluoride (PVDF), poly(vinylidene fluoride)-hexafluoropropene (PVDF-HFP), polytetrafluoroethylene (PTFE), The polystyrene, poly(vinyl alcohol) (PVA), poly(vinyl acetate), polyisoprene, polyaniline, polyethylene, polyimide, polyurethane, polyvinyl butyral, polyvinylpyrrolidone (PVP), gelatin, chitosan, starch, agar, xanthan gum, gum arabic, gellan gum, guar gum, karaya gum, tara gum, tragacanth gum, casein, amylose, pectin, PEDOT:PSS, carrageenan, or combinations thereof. In certain embodiments, the binder in the electrode layer does not include styrene-butadiene rubber, carboxymethylcellulose, polyacrylic acid, polyacrylonitrile, polyacrylamide acrylic acid-acrylonitrile-acrylamide copolymer, latex, alginate, polyvinylidene fluoride, poly(vinylidene fluoride)-hexafluoropropene, polytetrafluoroethylene, polystyrene, poly(vinyl alcohol), poly(vinyl acetate), polyisoprene, polyaniline, polyethylene, polyimide, polyurethane, polyvinyl butyral, polyvinylpyrrolidone, gelatin, chitosan, starch, agar, xanthan gum, gum arabic, gellan gum, guar gum, karaya gum, tara gum, tragacanth gum, casein, amylose, pectin, PEDOT:PSS, or carrageenan. In certain embodiments, the binder in the electrode layer does not include a fluorine-containing polymer, such as, for example, PVDF, PVDF-HFP, or PTFE.

[0178] In some embodiments, the binder in the electrode layer includes one or more functional groups including halogen, O, N, S, or combinations thereof. Some non-limiting examples of suitable functional groups include alkoxy, aryloxy, nitro, thiol, alkylthio, imine, cyano, amide, amino (primary, secondary, or tertiary), carboxyl, epoxy, ketone, aldehyde, ester, hydroxyl, halo (fluoro, chloro, bromo, or iodo), and combinations thereof. In some embodiments, the functional group is or includes carboxylic acid (i.e., -COOH), carboxylate, sulfonic acid, sulfonate, sulfuric acid, sulfate, phosphonic acid, phosphonate, phosphoric acid, phosphate, nitric acid, nitrate, amide, hydroxyl, nitrile, ester, epoxy, or -NH2.

[0179] In certain embodiments, the binder in the electrode layer comprises a copolymer having a composition as described below. The presence of hydrophilic functional groups in the binder ensures that the copolymer can be well dispersed in the aqueous medium and that the various electrode components can be bonded to each other. Meanwhile, the presence of hydrophobic functional groups in the binder ensures that the binder does not self-aggregate to impair dispersion and that the electrode slurry containing the copolymer does not become so viscous that it affects processability. The combination of both hydrophilic and hydrophilic effects means that the various electrode components are well bonded to each other while remaining dispersed in the solvent of the highly processable aqueous electrode slurry. The electrode slurries produced with such slurries are smooth and homogeneous, and batteries with such electrodes have excellent capacity and electrochemical performance.

[0180] In some embodiments, the binder in the electrode layer comprises a structural unit (i) derived from an acid group-containing monomer, and the acid group is selected from the group consisting of carboxylic acid, sulfonic acid, sulfuric acid, phosphonic acid, phosphoric acid, nitric acid, and combinations thereof. The acids listed above also include their salts and derivatives. In some embodiments, the acid salt comprises an alkali metal cation. Examples of alkali metals that form alkali metal cations include lithium, sodium, and potassium. In some embodiments, the acid salt comprises an ammonium cation.

[0181] In some embodiments, the carboxylic acid is acrylic acid, methacrylic acid, crotonic acid, 2-butylcrotonic acid, cinnamic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, itaconic anhydride, tetraconic acid, or a combination thereof. In certain embodiments, the carboxylic acid is 2-ethylacrylic acid, isocrotonic acid, cis-2-pentenoic acid, trans-2-pentenoic acid, Engellic acid, tiglic acid, 3,3-dimethylacrylic acid, 3-propylacrylic acid, trans-2-methyl-3-ethylacrylic acid, cis-2-methyl-3-ethylacrylic acid, 3-isopropylacrylic acid, trans-3-methyl-3-ethylacrylic acid, cis-3-methyl-3-ethylacrylic acid, 2-isopropylacrylic acid, trimethylacrylic acid, 2-methyl-3,3-dimethylacrylic acid, 3-butylacrylic acid, 2-butylacrylic acid, 2-pentylacrylic acid, 2-methyl-2-hexenoic acid, trans-3-methyl-2-hexenoic acid, 3-methyl-3-propylacrylic acid, 2-methyl-3-propylacrylic acid, 2, 3-diethylacrylic acid, 3,3-diethylacrylic acid, 3-methyl-3-hexylacrylic acid, 3-methyl-3-tert-butylacrylic acid, 2-methyl-3-pentylacrylic acid, 3-methyl-3-pentylacrylic acid, 4-methyl-2-hexenoic acid, 4-ethyl-2-hexenoic acid, 3-methyl-2-ethyl-2-hexenoic acid, 3-tert-butylacrylic acid, 2,3-diethyl-3-ethylacrylic acid, 3,3-dimethyl-2-ethylacrylic acid, 3-methyl-3-isopropylacrylic acid, 2-methyl-3-isopropylacrylic acid, trans-2-octenoic acid, cis-2-octenoic acid, trans-2-decenoic acid, α-acetoxyacrylic acid, β-trans-allyloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, or combinations thereof.

[0182] In some embodiments, the sulfonic acid is vinyl sulfonic acid, methyl vinyl sulfonic acid, allyl vinyl sulfonic acid, allyl sulfonic acid, methallyl sulfonic acid, styrene sulfonic acid, 2-sulfoethyl methacrylic acid, 2-methylprop-2-ene-1-sulfonic acid, 2-acrylamido-2-methyl-1-propanesulfonic acid, 3-allyloxy-2-hydroxy-1-propanesulfonic acid, or a combination thereof.

[0183] In some embodiments, the sulfate is allyl hydrogen sulfate, vinyl hydrogen sulfate, 4-allylphenol sulfate, or a combination thereof.

[0184] In some embodiments, the phosphonic acid is phosphonoxyethyl acrylate, phosphonoxyethyl methacrylate, vinyl phosphonic acid, allyl phosphonic acid, 3-butenyl phosphonic acid, styrene phosphonic acid, vinylbenzyl phosphonic acid, (2-chloro-2-phenyl-vinyl)-phosphonic acid, acrylamidoalkyl phosphonic acid, methacrylamidoalkyl phosphonic acid, acrylamidoalkyl diphosphonic acid, acryloyl phosphonic acid, 2-methacryloyloxyethyl phosphonic acid, bis(2-methacryloyloxyethyl)phosphonic acid, ethylene 2-methacryloyloxyethyl phosphonic acid, ethyl-methacryloyloxyethyl phosphonic acid, or a combination thereof.

[0185] In some embodiments, the phosphate is selected from the group consisting of mono(2-acryloyloxyethyl)phosphate, mono(2-methacryloyloxyethyl)phosphate, diphenyl(2-acryloyloxyethyl)phosphate, diphenyl(2-methacryloyloxyethyl)phosphate, phenyl(2-acryloyloxyethyl)phosphate, phosphoxyethyl methacrylate, 3-chloro-2-phosphoryloxypropyl methacrylate, phosphoryloxypoly(ethylene glycol) monomethacrylate, phosphoryloxypoly(propylene glycol) methacrylate, (meth)acryloyloxyethyl phosphate, (meth)acryloyloxypropyl phosphate, phosphate, (meth)acryloyloxy-2-hydroxypropyl phosphate, (meth)acryloyloxy-3-hydroxypropyl phosphate, (meth)acryloyloxy-3-chloro-2 hydroxypropyl phosphate, allyl hydrogen phosphate, vinyl hydrogen phosphate, allyl hydrogen pyrophosphate, vinyl hydrogen pyrophosphate, allyl hydrogen tripolyphosphate, vinyl hydrogen tripolyphosphate, allyl hydrogen tetrapolyphosphate, vinyl hydrogen tetrapolyphosphate, allyl hydrogen trimetaphosphate, vinyl hydrogen trimetaphosphate, isopentenyl phosphate, isopentenyl pyrophosphate, or a combination thereof.

[0186] In some embodiments, the nitrate is allyl hydrogen nitrate, ethenyl hydrogen nitrate, or a combination thereof.

[0187] In some embodiments, the ratio of the structural unit (i) in the binder is, based on the total number of moles of monomer units in the copolymerization, about 15 mol% to about 95 mol%, about 15 mol% to about 85 mol%, about 15 mol% to about 75 mol%, about 15 mol% to about 65 mol%, about 15 mol% to about 55 mol%, about 20 mol% to about 95 mol%, about 20 mol% to about 90 mol%, about 20 mol% to about 80 mol%, about 20 mol% to about 70 mol%, about 20 mol% to about 60 mol%, about 20 mol% to about 50 mol%, about 25 mol% to about 95 mol%, about 25 mol% to about 85 mol%, about 25 mol% to about 75 mol%, about 25 mol% to about 65 mol%, about 25 mol% to about 55 mol%, about 30 mol% to about 95 mol%, about 30 mol% to about 85 mol%, about 30 mol% to about 75 mol%, about 30 mol% to about 65 mol%, about 35 mol% to about 95 mol%, about 35 mol% to about 85 mol%, about 35 mol% to about 75 mol%, about 35 mol% to about 65 mol%, about 40 mol% to about 95 mol%, about 40 mol% to about 85 mol%, about 40 mol% to about 75 mol%, about 40 mol% to about 65 mol%, about 45 mol% to about 95 mol%, about 45 mol% to about 85 mol%, about 45 mol% to about 75 mol%, about 50 mol% to about 95 mol%, about 50 mol% to about 85 mol%, about 50 mol% to about 75 mol%, about 55 mol% to about 95 mol%, about 55 mol% to about 85 mol%, about 55 mol% to about 75 mol%, about 60 mol% to about 95 mol%, or about 60 mol% to about 85 mol%.

[0188] In some embodiments, the ratio of structural unit (i) in the binder is less than 95 mol%, less than 85 mol%, less than 75 mol%, less than 65 mol%, less than 55 mol%, less than 45 mol%, less than 35 mol%, or less than 25 mol%, based on the total number of moles of monomer units in the copolymerization. In some embodiments, the ratio of structural unit (i) in the binder is more than 15 mol%, more than 25 mol%, more than 35 mol%, more than 45 mol%, more than 55 mol%, more than 65 mol%, more than 75 mol%, or more than 85 mol%, based on the total number of moles of monomer units in the copolymerization.

[0189] In some embodiments, the binder in the electrode layer further comprises a structural unit (ii) derived from a monomer selected from the group consisting of an amide group-containing monomer, a hydroxyl group-containing monomer, and combinations thereof.

[0190] In some embodiments, the amide group-containing monomer is acrylamide, methacrylamide, N-methyl methacrylamide, N-ethyl methacrylamide, Nn-propyl methacrylamide, N-isopropyl methacrylamide, isopropyl acrylamide, Nn-butyl methacrylamide, N-isobutyl methacrylamide, N,N-diethyl methacrylamide, N-methylol methacrylamide, N-(methoxymethyl) methacrylamide, N-(ethoxymethyl) methacrylamide, N-(propoxymethyl) methacrylamide, N-(but ... N,N'-dimethylmethacrylamide, N,N'-dimethylaminopropyl methacrylamide, N,N'-dimethylaminoethyl methacrylamide, N,N'-dimethylol methacrylamide, diacetone methacrylamide, diacetone acrylamide, methacryloylmorpholine, N-hydroxyl methacrylamide, N-methoxymethyl acrylamide, N-methoxymethyl methacrylamide, N,N'-methylene-bis-acrylamide (MBA), N-hydroxymethyl acrylamide, or combinations thereof.

[0191] In some embodiments, the hydroxyl-containing monomer is a C1-C 20 Alkyl or C5-C 20It is an acrylate or methacrylate containing a cycloalkyl. In some embodiments, the hydroxyl group-containing monomer is 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 2-hydroxybutyl methacrylate, 3-hydroxypropyl acrylate, 3-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 5-hydroxypentyl acrylate, 6-hydroxyhexyl methacrylate, 1,4-cyclohexanedimethanol monoacrylate, 1,4-cyclohexanedimethanol monomethacrylate, 3-chloro-2-hydroxypropyl methacrylate, diethylene glycol monoacrylate, diethylene glycol monomethacrylate, allyl alcohol, or a combination thereof.

[0192] In some embodiments, the ratio of the structural unit (ii) in the binder is about 5 mol% to about 50 mol%, about 5 mol% to about 45 mol%, about 5 mol% to about 40 mol%, about 5 mol% to about 35 mol%, about 5 mol% to about 30 mol%, about 5 mol% to about 25 mol%, about 10 mol% to about 50 mol%, about 10 mol% to about 45 mol%, about 10 mol% to about 40 mol%, about 10 mol% to about 35 mol%, about 10 mol% to about 30 mol%, about 15 mol% to about 50 mol%, about 15 mol% to about 45 mol%, about 15 mol% to about 40 mol%, about 20 mol% to about 50 mol%, about 20 mol% to about 45 mol%, about 20 mol% to about 40 mol%, or about 25 mol% to about 50 mol%, based on the total number of moles of monomer units in the copolymerization.

[0193] In some embodiments, the ratio of structural unit (ii) in the binder is less than 50 mol%, less than 45 mol%, less than 40 mol%, less than 35 mol%, less than 30 mol%, less than 25 mol%, less than 20 mol%, or less than 15 mol%, based on the total number of moles of monomer units in the copolymerization. In some embodiments, the ratio of structural unit (ii) in the binder is more than 5 mol%, more than 10 mol%, more than 15 mol%, more than 20 mol%, more than 25 mol%, more than 30 mol%, more than 35 mol%, or more than 40 mol%, based on the total number of moles of monomer units in the copolymerization.

[0194] In some embodiments, the binder in the electrode layer further comprises a structural unit (iii) derived from a monomer selected from the group consisting of a nitrile group-containing monomer, an ester group-containing monomer, an epoxy group-containing monomer, and combinations thereof.

[0195] In some embodiments, the nitrile group-containing monomer is or comprises an α,β-ethylenically unsaturated nitrile monomer. In some embodiments, the nitrile group-containing monomer is acrylonitrile, α-halogenoacrylonitrile, α-alkylacrylonitrile, or a combination thereof. In some embodiments, the nitrile group-containing monomer is α-chloroacrylonitrile, α-bromoacrylonitrile, α-fluoroacrylonitrile, methacrylonitrile, α-ethylacrylonitrile, α-isopropylacrylonitrile, α-n-hexylacrylonitrile, α-methoxyacrylonitrile, 3-methoxyacrylonitrile, 3-ethoxyacrylonitrile, α-acetoxyacrylonitrile, α-phenylacrylonitrile, α-tolylacrylonitrile, α-(methoxyphenyl)acrylonitrile, α-(chlorophenyl)acrylonitrile, α-(cyanophenyl)acrylonitrile, vinylidene cyanide, or a combination thereof.

[0196] In some embodiments, the ester group-containing monomer is a C1-C 20 Alkyl acetate, C1-C 20In some embodiments, the ester group-containing monomer is methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, sec-butyl acrylate, tert-butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 3,3,5-trimethylhexyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, octadecyl acrylate, cyclohexyl acrylate, phenyl acrylate, methoxymethyl acrylate, methoxyethyl acrylate, ethoxymethyl acrylate, ethoxyethyl acrylate, perfluorooctyl acrylate, stearyl acrylate, or a combination thereof.

[0197] In some embodiments, the epoxy group-containing monomer is vinyl glycidyl ether, allyl glycidyl ether, allyl 2,3-epoxypropyl ether, butenyl glycidyl ether, butadiene monoepoxide, chloroprene monoepoxide, 3,4-epoxy-1-butene, 4,5-epoxy-2-pentene, 3,4-epoxy-1-vinylcyclohexane, 1,2-epoxy-4-vinylcyclohexane, 3,4-epoxycyclohexylethylene, epoxy-4-vinylcyclohexene, 1,2-epoxy-5,9-cyclododecadiene, or a combination thereof.

[0198] In some embodiments, the ratio of the structural unit (iii) in the binder is, based on the total moles of monomer units in the copolymerization, about 5 mol % to about 80 mol %, about 5 mol % to about 70 mol %, about 5 mol % to about 60 mol %, about 5 mol % to about 50 mol %, about 5 mol % to about 40 mol %, about 5 mol % to about 30 mol %, about 10 mol % to about 80 mol %, about 10 mol % to about 70 mol %, about 10 mol % to about 60 mol %, about 10 mol % to about 50 mol %, about 10 mol % to about 40 mol %, about 15 mol % to about 80 mol %, about 15 mol % to about 70 mol %, about 15 mol % to about 60 mol %, about 15 mol % to about 50 mol %, about 15 mol % to about 40 mol %, about 20 mol % to about 60 mol %, about 20 mol % to about 70 mol %, about 20 mol % to about 60 mol %, about 20 mol % to about 70 mol %, about 20 mol % to about 60 mol %, about 20 mol % to about 5 ... % to about 80 mol%, about 20 mol% to about 70 mol%, about 20 mol% to about 60 mol%, about 20 mol% to about 50 mol%, about 25 mol% to about 80 mol%, about 25 mol% to about 70 mol%, about 25 mol% to about 60 mol%, about 25 mol% to about 50 mol%, about 30 mol% to about 80 mol%, about 30 mol% to about 70 mol%, about 30 mol% to about 60 mol%, about 35 mol% to about 80 mol%, about 35 mol% to about 70 mol%, about 35 mol% to about 60 mol%, about 40 mol% to about 80 mol%, about 40 mol% to about 70 mol%, about 45 mol% to about 80 mol%, about 45 mol% to about 70 mol%, about 50 mol% to about 80 mol%, or about 50 mol% to about 70 mol%.

[0199] In some embodiments, the ratio of structural unit (iii) in the binder is less than 80 mol%, less than 70 mol%, less than 60 mol%, less than 50 mol%, less than 40 mol%, less than 30 mol%, less than 20 mol%, or less than 15 mol%, based on the total number of moles of monomer units in the copolymerization. In some embodiments, the ratio of structural unit (iii) in the binder is more than 5 mol%, more than 15 mol%, more than 25 mol%, more than 35 mol%, more than 45 mol%, more than 55 mol%, or more than 60 mol%, based on the total number of moles of monomer units in the copolymerization.

[0200] In some embodiments, the electrode layer further comprises a conductive agent. The presence of the conductive agent improves the conductive properties of the electrode layer in the electrode. It may therefore be advantageous for the electrode layer to comprise a conductive agent. Any suitable material may act as the conductive agent. Any embodiment of the conductive material suitable for use in the conductive layer of the improved current collector of the present invention is also suitable for use as a conductive agent in the electrode layer. In other embodiments, the conductive agent is not the conductive material used in the conductive layer of the improved current collector. The conductive agent used in the electrode layer of the improved current collector and the conductive material used in the conductive layer may be the same, different, or partially different.

[0201] In some embodiments, the conductive agent comprises a conductive polymer selected from the group consisting of polypyrrole, polyaniline, polyacetylene, polyphenylene sulfide (PPS), polyphenylene vinylene (PPV), poly(3,4-ethylenedioxythiophene) (PEDOT), polythiophene, and combinations thereof. In some embodiments, the conductive polymer serves two roles at the same time, acting as both a conductive agent and a binder. In other embodiments, the conductive agent does not comprise a conductive polymer.

[0202] In some embodiments, the ratio of the electrode active material in the electrode layer is about 60% by weight to about 99% by weight, about 70% by weight to about 99% by weight, about 75% by weight to about 99% by weight, about 80% by weight to about 99% by weight, about 85% by weight to about 99% by weight, about 90% by weight to about 99% by weight, about 60% by weight to about 95% by weight, about 65% by weight to about 95% by weight, about 70% by weight to about 95% by weight, about 75% by weight to about 95% by weight, about 80% by weight to about 99% by weight, about 90% by weight to about 99% by weight, about 90% by weight to about 99% by weight, about 90% by weight to about 99% by weight, about 90% by weight to about 99% by weight, about 90% by weight to about 95 ... % to about 95% by weight, about 85% to about 95% by weight, about 60% to about 90% by weight, about 65% to about 90% by weight, about 70% to about 90% by weight, about 75% to about 90% by weight, about 80% to about 90% by weight, about 60% to about 85% by weight, about 70% to about 85% by weight, about 75% to about 85% by weight, about 60% to about 80% by weight, about 65% to about 80% by weight, or about 70% to about 80% by weight.

[0203] In some embodiments, the proportion of electrode active material in the electrode layer is less than 99 weight percent, less than 95 weight percent, less than 90 weight percent, less than 85 weight percent, less than 80 weight percent, less than 75 weight percent, less than 70 weight percent, or less than 65 weight percent, based on the total weight of the electrode layer. In some embodiments, the proportion of electrode active material in the electrode layer is greater than 60 weight percent, greater than 65 weight percent, greater than 70 weight percent, greater than 75 weight percent, greater than 80 weight percent, greater than 85 weight percent, greater than 90 weight percent, or greater than 95 weight percent, based on the total weight of the electrode layer.

[0204] In some embodiments, the ratio of the binder and the conductive agent in the electrode layer is each independently about 1% to about 20%, about 2% to about 20%, about 3% to about 20%, about 4% to about 20%, about 5% to about 20%, about 6% to about 20%, about 7% to about 20%, about 8% to about 20%, about 9% to about 20%, about 10% to about 20%, about 11% to about 20%, about 12% to about 20%, about 13% to about 20%, about 14% to about 20%, about 15% to about 20%, about 1% to about 15%, about 2% to about 15%, about 3% to about 15%, about 4% to about 15%, about 5% to about 15%, about 6% to about 15%, about 7% to about 15%, about 8% to about 15%, about 9% to about 15%, about 10% to about 15%, about 1% to about 10%, about 2% to about 10%, about 3% to about 10%, about 4% to about 10%, about 5% to about 10%, about 1% to about 5%, about 2% to about 5%, or about 3% to about 5%.

[0205] In some embodiments, the ratio of the binder and conductive agent in the electrode layer is each independently less than 20% by weight, less than 19% by weight, less than 18% by weight, less than 17% by weight, less than 16% by weight, less than 15% by weight, less than 14% by weight, less than 13% by weight, less than 12% by weight, less than 11% by weight, less than 10% by weight, less than 9% by weight, less than 8% by weight, less than 7% by weight, or less than 6% by weight, based on the total weight of the electrode layer. In some embodiments, the ratio of the binder and conductive agent in the electrode layer is each independently greater than 1% by weight, greater than 2% by weight, greater than 3% by weight, greater than 4% by weight, greater than 5% by weight, greater than 6% by weight, greater than 7% by weight, greater than 8% by weight, greater than 9% by weight, greater than 10% by weight, greater than 11% by weight, greater than 12% by weight, greater than 13% by weight, greater than 14% by weight, or greater than 15% by weight, based on the total weight of the electrode layer.

[0206] In some embodiments, the electrode layer of the electrode may further include other additives to enhance the electrode properties, hi some embodiments, the additives may include surfactants, dispersants, and flexibility enhancing additives, salts, ion conducting polymers, and inorganic solid electrolytes.

[0207] In certain embodiments, the electrode slurry is used to form an electrode layer of an electrode, and is coated on the improved current collector of the present invention and then dried. In some embodiments, the electrode slurry includes a solvent in addition to various electrode components for forming the electrode layer, such as, for example, an electrode active material, a binder, and a conductive agent. In some embodiments, the solvent of the electrode slurry is an aqueous solvent. Any aqueous solvent suitable for use as a solvent for the conductive slurry is also suitable for use as a solvent for the electrode slurry. In certain embodiments, when both the conductive slurry and the electrode slurry use an aqueous solvent, the composition of the aqueous solvent of the two slurries may be the same, may be different, or may be partially different.

[0208] In some embodiments, the solids content of the electrode slurry is about 40% by weight to about 80% by weight, about 40% by weight to about 75% by weight, about 40% by weight to about 70% by weight, about 40% by weight to about 65% by weight, about 40% by weight to about 60% by weight, about 40% by weight to about 55% by weight, about 45% by weight to about 80% by weight, about 45% by weight to about 75% by weight, about 45% by weight to about 70% by weight, about 45% by weight to about 65% by weight, about 45 ... % to about 60% by weight, about 50% to about 80% by weight, about 50% to about 75% by weight, about 50% to about 70% by weight, about 50% to about 65% by weight, about 55% to about 80% by weight, about 55% to about 75% by weight, about 55% to about 70% by weight, about 60% to about 80% by weight, about 60% to about 75% by weight, about 65% to about 80% by weight, about 65% to about 75% by weight, or about 70% to about 80% by weight.

[0209] In some embodiments, the solids content of the electrode slurry is less than 80 wt%, less than 75 wt%, less than 70 wt%, less than 65 wt%, less than 60 wt%, less than 55 wt%, or less than 50 wt%, based on the total weight of the electrode slurry. In some embodiments, the solids content of the electrode slurry is greater than 40 wt%, greater than 45 wt%, greater than 50 wt%, greater than 55 wt%, greater than 60 wt%, greater than 65 wt%, or greater than 70 wt%, based on the total weight of the electrode slurry.

[0210] The method used to generate the electrode slurry from the various electrode components is not particularly limited, except that all the electrode components should be mixed, for example, by mixing in a homogenizer, to form a homogenous electrode slurry. In some embodiments, all materials used to generate the electrode slurry are added to the homogenizer in a single batch. In other embodiments, each electrode component of the electrode slurry may be added to the homogenizer in one or more batches, and each batch may include multiple electrode components. Any homogenizer capable of reducing or eliminating particle agglomeration in the electrode slurry and / or promoting homogenous dispersion of the electrode components may be used herein. Homogeneous dispersion plays an important role in producing a battery with good battery performance. In some embodiments, the homogenizer is a planetary agitator mixer, an agitator mixer, a blender, or an ultrasonicator.

[0211] There are no particular limitations on the conditions used to form the electrode slurry, except that such conditions should be sufficient to produce a homogenous slurry with good dispersion of the electrode components therein. There are no particular limitations on the duration or temperature or agitation speed used to homogenize the electrode slurry, except that the duration, temperature, and agitation speed should be sufficient to ensure homogenous dispersion of the various electrode components in the electrode slurry and that the electrode slurry is easily processed.

[0212] In some embodiments, after homogenization of the electrode slurry, the electrode slurry can be coated on one or both sides of the improved current collector of the present invention to form an electrode layer. There are no particular limitations on the equipment and conditions used for coating the slurry, except that a homogeneous, flat and smooth electrode layer film should be formed. In certain embodiments, the coating process is carried out using a doctor blade coater, a slot die coater, a transfer coater, a spray coater, a roll coater, a gravure coater, a dip coater, or a curtain coater. In some embodiments, the electrode slurry is applied directly to the improved current collector. In other embodiments, the electrode slurry is first applied to a release film to form a free-standing electrode layer. The free-standing electrode layer is then combined with the improved current collector and pressed to form the electrode layer.

[0213] In some embodiments, after coating the electrode slurry onto the improved current collector of the present invention, the coating is dried. Any device capable of drying the coating to affix the electrode layer to the improved current collector may be used herein.

[0214] There are no particular limitations on the conditions used for drying, other than being sufficient to ensure that the electrode layer adheres strongly to the improved current collector, although drying the electrode slurry at temperatures above 100° C. may result in undesirable deformation of the electrode and affect the performance of the resulting electrode. In some embodiments, the resulting electrode is mechanically compressed after drying of the film to densify the electrode.

[0215] In certain embodiments, the thickness of the electrode layer is about 5 μm to about 90 μm, about 5 μm to about 50 μm, about 5 μm to about 25 μm, about 10 μm to about 90 μm, about 10 μm to about 50 μm, about 10 μm to about 30 μm, about 15 μm to about 90 μm, about 20 μm to about 90 μm, about 25 μm to about 90 μm, about 25 μm to about 80 μm, about 25 μm to about 70 μm, about 25 μm to about 50 μm, about 30 μm to about 90 μm, or about 30 μm to about 80 μm. In some embodiments, the thickness of the electrode layer is greater than 5 μm, greater than 10 μm, greater than 15 μm, greater than 20 μm, greater than 25 μm, greater than 30 μm, greater than 40 μm, greater than 50 μm, greater than 60 μm, greater than 70 μm, or greater than 80 μm. In some embodiments, the thickness of the electrode layer is less than 90 μm, less than 80 μm, less than 70 μm, less than 60 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 25 μm, less than 20 μm, less than 15 μm, or less than 10 μm.

[0216] In some embodiments, the surface density of the electrode layer is about 1 mg / cm 2 ~about 50mg / cm 2 , about 2.5mg / cm 2 ~about 50mg / cm 2 , about 5mg / cm 2 ~about 50mg / cm 2 , about 10mg / cm 2 ~about 50mg / cm 2 , about 15mg / cm 2 ~about 50mg / cm 2 , about 20mg / cm 2 ~about 50mg / cm 2 , about 30mg / cm 2 ~about 50mg / cm 2 , about 1mg / cm 2 ~about 30mg / cm 2 , about 2.5mg / cm 2 ~about 30mg / cm 2 , about 5mg / cm 2 ~about 30mg / cm 2 , about 10mg / cm 2 ~about 30mg / cm 2 , about 15mg / cm 2 ~about 30mg / cm 2 , about 20mg / cm2 ~about 30mg / cm 2 , about 1mg / cm 2 ~about 20mg / cm 2 , about 2.5mg / cm 2 ~about 20mg / cm 2 , about 5mg / cm 2 ~about 20mg / cm 2 , about 10mg / cm 2 ~about 20mg / cm 2 , about 1mg / cm 2 ~Approx. 15mg / cm 2 , about 2.5mg / cm 2 ~Approx. 15mg / cm 2 , about 5mg / cm 2 ~Approx. 15mg / cm 2 , or about 10 mg / cm 2 ~Approx. 15mg / cm 2 It is.

[0217] In some embodiments, the surface density of the electrode layer is 50 mg / cm 2 Less than 40 mg / cm 2 Less than 30 mg / cm 2 Less than 20 mg / cm 2 Less than 15 mg / cm 2 Less than 10 mg / cm 2 Less than 5 mg / cm 2 Less than 2.5 mg / cm 2 In some embodiments, the surface density of the electrode layer is less than 1 mg / cm 2 Over 2.5mg / cm 2 More than 5mg / cm 2 Over 10mg / cm 2 Over 15mg / cm 2 Over 20mg / cm 2 Over 30mg / cm 2 or more than 40 mg / cm 2 Beyond that.

[0218] In the electrode with the improved current collector of the present invention, the electrode layer exhibits strong adhesion to the improved current collector. It is important that the electrode layer has high peel strength to the improved current collector, which prevents the electrode from peeling or separating, which has a significant impact on the mechanical stability of the electrode and the cyclability of the battery with the electrode. Therefore, the electrode should have sufficient peel strength to withstand the rigors of battery manufacturing.

[0219] In some embodiments, the peel strength between the electrode layer and the improved current collector is about 1.0 N / cm to about 8.0 N / cm, about 1.0 N / cm to about 6.0 N / cm, about 1.0 N / cm to about 5.0 N / cm, about 1.0 N / cm to about 4.0 N / cm, about 1.0 N / cm to about 3.0 N / cm, about 1.0 N / cm to about 2.5 N / cm, about 1.0 N / cm to about 2.0 N / cm, about 1.2 N / cm to about 3.0 N / cm, about 1.2 N / cm to about 2.5 N / cm, about 1.2 N / cm to about 2.0 N / cm, about 1.5 N / cm to about 3.0 N / cm, about 1.5 N / cm to about 2.5 N / cm, about 1.5 N / cm to about 2.0 N / cm, about 1.8 N / cm to about 3.0 N / cm, about 1.8 N / cm to about 2.5 N / cm, about 2.0 N / cm to about 6.0 N / cm, about 2.0 N / cm to about 5.0 N / cm, about 2.0 N / cm to about 3.0 N / cm, about 2.0 N / cm to about 2.5 N / cm, about 2.2 N / cm to about 3.0 N / cm, about 2.5 N / cm to about 3.0 N / cm, about 3.0 N / cm to about 8.0 N / cm, about 3.0 N / cm to about 6.0 N / cm, or about 4.0 N / cm to about 6.0 N / cm.

[0220] In some embodiments, the peel strength between the electrode layer and the improved current collector is greater than 1.0 N / cm, greater than 1.2 N / cm, greater than 1.5 N / cm, greater than 2.0 N / cm, greater than 2.2 N / cm, greater than 2.5 N / cm, greater than 3.0 N / cm, greater than 3.5 N / cm, greater than 4.0 N / cm, greater than 4.5 N / cm, greater than 5.0 N / cm, greater than 5.5 N / cm, greater than 6.0 N / cm, greater than 6.5 N / cm, or greater than 7.0 N / cm. In some embodiments, the peel strength between the electrode layer and the improved current collector is less than 8.0 N / cm, less than 7.5 N / cm, less than 7.0 N / cm, less than 6.5 N / cm, less than 6.0 N / cm, less than 5.5 N / cm, less than 5.0 N / cm, less than 4.5 N / cm, less than 4.0 N / cm, less than 3.5 N / cm, less than 3.0 N / cm, less than 2.8 N / cm, less than 2.5 N / cm, less than 2.2 N / cm, less than 2.0 N / cm, less than 1.8 N / cm, or less than 1.5 N / cm.

[0221] In some embodiments, once an electrode with an improved current collector is formed, the electrode can be assembled with a counter electrode and an electrolyte to form a battery: if the electrode is a positive electrode, the counter electrode is a negative electrode, and if the electrode is a negative electrode, the counter electrode is a negative electrode.

[0222] In some embodiments, the electrolyte is a liquid electrolyte. Such a liquid electrolyte includes an electrolyte solvent and a salt. In some embodiments, the electrolyte solvent is water, and the liquid electrolyte is an aqueous solvent. In other embodiments, the electrolyte solvent is a liquid composed of one or more organic solvents, and the liquid electrolyte is a non-aqueous electrolyte. In some embodiments, each organic solvent is selected from carbonate-based, ester-based, ether-based, or other aprotic solvents. Some non-limiting examples of carbonate-based solvents include dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, and combinations thereof. Some non-limiting examples of ester-based solvents include methyl acetate, methyl propanoate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, and combinations thereof. Some non-limiting examples of ethereal solvents include dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, tetrahydrofuran, and combinations thereof. Some non-limiting examples of other aprotic solvents include methyl bromide, ethyl bromide, methyl formate, acetonitrile, dimethylsulfoxide, dimethylformamide, N-methyl-2-pyrrolidone, and combinations thereof.

[0223] In some embodiments, the liquid electrolyte is for a conventional lithium ion battery. The salt in the liquid electrolyte is a lithium salt. In some embodiments, the lithium salt present in the liquid electrolyte for a conventional lithium ion battery is selected from the group consisting of LiPF6, LiBO2, LiBF4, LiSbF6, LiAsF6, LiAlCl4, LiClO4, LiCl, LiI, LiNO3, LiB(C2O4)2, LiSO3CF3, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2CF2CF3)2, LiC2H3O2, and combinations thereof.

[0224] In some embodiments, the liquid electrolyte is for a conventional sodium-ion battery. The salt in the liquid electrolyte is a sodium salt. In some embodiments, the sodium salt present in the liquid electrolyte for a conventional sodium-ion battery is a sodium analogue of the lithium salts mentioned above, with lithium replaced by sodium. Such sodium salts include NaPF6, NaBF4, NaN(SO2CF3)2, NaN(SO2F)2, NaClO4, NaSO3CF3, and combinations thereof. In some embodiments, the salt present in the liquid electrolyte for a conventional sodium-ion battery is NaMF x where each x=4 or 6, and each M is one or more of Al 3+ , B 3+ , Ga 3+ , In 3+ , Sc 3+ , Y 3+ , La 3+ , P 5+ , As 5+ and combinations thereof.

[0225] In some embodiments, the electrolyte is a solid electrolyte. In some embodiments, the solid electrolyte is a polymer electrolyte. Such a polymer electrolyte includes an ion-conducting polymer and a salt. In some embodiments, the ion-conducting polymer is selected from the group consisting of polyethers, polycarbonates, polyacrylates, polysiloxanes, polyphosphazenes, polyethylene derivatives, alkylene oxide derivatives, phosphate polymers, poly-lysine, polyester sulfides, polyvinyl alcohols, polyvinylidene fluorides, polymers containing one or more ionically dissociable groups, copolymers thereof, and combinations thereof. In some embodiments, the ion-conducting polymer is selected from the group consisting of polyacrylonitrile (PAN), polyethylene carbonate (PEC), polyacrylamide (PAM), polyethylene glycol (PEG), polyethylene oxide (PEO), polyhydroxyethyl methacrylate (P(HEMA)), polyphosphonate (PPh), polysiloxane, polyamide (PA), polydilactone, polydiester, polyphosphazene (PPHOS), polyurethane (PU), copolymers thereof, and combinations thereof.

[0226] In some embodiments, the polymer electrolyte is for use in a solid-state lithium ion battery. In certain embodiments, the salt present in the polymer electrolyte for a solid-state lithium ion battery is one or more of the lithium salts described above. Similarly, in some embodiments, the polymer electrolyte is for use in a solid-state sodium ion battery. In certain embodiments, the salt present in the polymer electrolyte for a solid-state sodium ion battery is one or more of the sodium salts described above.

[0227] In some embodiments, the solid electrolyte is an inorganic solid electrolyte. In certain embodiments, the inorganic solid electrolyte is for use in solid-state lithium-ion batteries. In some embodiments, the inorganic solid electrolyte for solid-state lithium-ion batteries is a sulfide, such as Li2S-P2S5, Li 4-x Ge 1-x P x S4 (LGPS, x is 0.1 to 2), Li 10± 1MP2X12 (M=Ge, Si, Sn, Al;X=S,Se), Li 3.833 Sn 0.833 As 0.166 S4, Li4SnS4, B2S3-Li2S, xLi2S-(100-x)P2S5 (x is 70~80), Li2S-SiS2-Li3N, Li2S-P2S5-LiI, Li2S-SiS2-LiI, Li2S-B2S3-LiI, Li 10 SnP2S 12 , Li6PS5X arginine (X is a halogen), e.g. Li 3.25 Ge 0.25 P 0.75 Thio-LISICON compounds such as S4, antiperovskites such as Li3SX (X is Cl or Br), lithium phosphorus iodine oxygen sulfide, lithium phosphorus oxygen sulfide, lithium zinc germanium sulfide, lithium germanium sulfide, LLTO compounds such as (La,Li)TiO3, Li6La2CaTa6O 12 , Li6La2ANb2O 12 (A is Ca and / or Sr), Li2Nd3TeSbO 12 , LiBO 2.5 N 0.5 , Li9SiAlO8, LAGP compound (Li 1+x Al x Ge 2-x (PO4)3, where 0≦x≦1, 0≦y≦1), such as Al2O3-TiO2-P2O5Li2O-LATP compounds, Li 1+x Al x Ti 2-x (PO4)3 (in the formula, 0≦x≦1, 0≦y≦1), Li 1+x Ti 2-x Al x S y (PO4) 3-y (In the formula, 0≦x≦1, 0≦y≦1), LiAl x Zr 2-x (PO4)3 (in the formula, 0≦x≦1, 0≦y≦1), LiTi x Zr 2-x (PO4)3 (where 0≦x≦1, 0≦y≦1), LISICON type solid electrolyte, LIPON compound (Li 3+y PO4-x N x , where 0≦x≦1, 0≦y≦1), perovskite compounds ((La,Li)TiO3), NASICON compounds such as LiTi2(PO4)3, antiperovskites such as Li3OX (X is Cl or Br), lithium aluminum titanium silicon phosphates (LATSP), lithium aluminum oxide, lithium vanadium germanium oxide, lithium zinc germanium oxide, lithium filled garnets such as lithium lanthanum zinc oxide, lithium lanthanum zinc aluminum oxide, lithium lanthanum zinc tantalum oxide, Li3N, lithium aluminum chloride, and combinations thereof.

[0228] In certain embodiments, the inorganic solid electrolyte is for use in a solid-state sodium-ion battery. In some embodiments, the inorganic solid electrolyte for a solid-state sodium-ion battery is a sodium analog of the inorganic solid electrolyte suitable for use in a solid-state lithium-ion battery described above, with lithium substituted for sodium. In some embodiments, the solid electrolyte for a solid-state sodium-ion battery is a NASICON-type inorganic solid electrolyte, e.g., NaPS sulfide containing sulfur and phosphorus, such as 75Na2S-25P2S5, sodium polyaluminate, and combinations thereof.

[0229] In some embodiments, the solid electrolyte is a gel electrolyte. Such a gel electrolyte includes a polymer electrolyte and an electrolyte solvent.

[0230] Due to the presence of the conductive layer in the improved current collector of the present invention, batteries with electrodes using the improved current collector exhibit significantly better electrochemical performance. Compared to conventional current collectors, the improved current collector of the present invention provides significant improvements to the electrode, and such improvements are made possible by the contributions of each of the individual components present in the conductive layer of the improved current collector. More specifically, the conductive material reduces the interfacial resistance between the improved current collector and the electrode layer, thereby reducing capacity loss resulting from the internal resistance of the electrode in the battery. The conductive layer also acts as a physical barrier to prevent corrosion of the substrate. The binder material not only provides more effective bonding performance between the conductive material particles and between the conductive material particles and the substrate, but also improves the mechanical strength of the entire electrode. Furthermore, when an aqueous slurry is used to produce the conductive layer, the binder material in the conductive layer continues to maintain excellent bonding properties when an aqueous electrode slurry is subsequently applied to the conductive layer. The conductive layer does not decompose or peel off from the substrate.

[0231] The following examples are presented to illustrate embodiments of the present invention, but are not intended to limit the present invention to the specific embodiments described. Unless otherwise indicated, all parts and percentages are by weight. All numerical values ​​are approximate. When numerical ranges are described, it should be understood that embodiments outside the described ranges may also be within the scope of the present invention. The specific details described in each example should not be construed as essential features of the present invention.

[0232] The present invention has been described with respect to a limited number of embodiments, and the specific features of one embodiment should not be attributed to other embodiments of the invention. In some embodiments, the method may include a number of steps not mentioned herein. In other embodiments, the method does not include, or is substantially free of, any steps not listed herein. There are variations and modifications from the described embodiments. It is intended that the appended claims cover such modifications and variations as fall within the scope of the present invention.

[0233] example The composite volume resistance of the positive electrode and the interface resistance between the positive electrode layer and the improved current collector were measured using an electrode resistance measurement system (RM2610, HIOKI).

[0234] The viscosity of the binder material used in the conductive layer was measured at a concentration of 4% in DI water at 20 °C using a rotational viscometer (NDJ-5S, Shanghai JT Electronic Technology Co. Ltd., China).

[0235] Example 1 A) Preparation of the Conductive Material Mixture 150 g of graphite powder (Timcal Ltd, Bodio, Switzerland) was added to 500 g of DI water. After addition, the mixture was stirred at 25° C. at a speed of 1000 rpm for 75 minutes to form a conductive material mixture.

[0236] B) Preparation of binder material solution The binder material was prepared by a method known in the art. In the structural unit (a) of the copolymer, any three of R1, R2, R3, and R4 are H, and any one of R1, R2, R3, and R4 is hydroxyl. In the structural unit (b) of the copolymer, any three of R5, R6, R7, and R8 are H, and any one of R5, R6, R7, and R8 is acetoxy. The ratio of the structural unit (a) and the structural unit (b) in the copolymer of the binder material is 99 mol % and 1 mol %, respectively, based on the total moles of monomer units in the copolymer. The components and respective ratios of the binder material of Example 1 are shown in Table 1 below.

[0237] Then, 75 g of the binder material was added to 750 g of DI water and heated to 70 °C. The mixture was stirred with a magnetic stirrer at 600 rpm for 30 minutes to form the binder material solution. The solids content of the binder material solution is 9.1 wt%. The weight average molecular weight of the copolymer is 130,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20 °C is 30 mPa·s.

[0238] C) Preparation of conductive slurry 150g of the binder material solution was added to 50g of the conductive material mixture. After the addition, the mixture was stirred at 25°C at a speed of 1000 rpm for 15 minutes to form a conductive slurry. The solid content of the conductive slurry is 12.6% by weight.

[0239] D) Preparation of improved current collector Aluminum foil with a thickness of 16 μm was used as the substrate. Both sides of the substrate were coated with the conductive slurry using a doctor blade coater with a gap width of 8 μm. The 4.5 μm slurry coated on the aluminum foil was dried using an electric heating oven at 85 °C to form a conductive layer. The drying time was about 30 min.

[0240] E) Preparation of the binder solution 16 g of sodium hydroxide (NaOH) was added to a round-bottom flask containing 380 g of distilled water. The sodium hydroxide solution was stirred at 80 rpm for 30 minutes to obtain a first suspension.

[0241] 36.04 g of acrylic acid was added to the first suspension, and the mixture was further stirred at 80 rpm for 30 minutes to obtain a second suspension.

[0242] 19.04 g of acrylamide (AM) was dissolved in 10 g of DI water to form an AM solution. Then, 29.04 g of the AM solution was added to the second suspension. This mixture was further stirred at 80 rpm for 45 minutes to obtain a third suspension.

[0243] To the third suspension, 12.92 g of acrylonitrile (AN) was added, and the mixture was further stirred at 80 rpm for 10 minutes to obtain a fourth suspension.

[0244] Further, 0.015 g of a water-soluble free radical initiator (ammonium persulfate, APS, from Aladdin Industries Corporation, China) was dissolved in 3 g of DI water, and 0.0075 g of a reducing agent (sodium bisulfite, from Tianjin Damao Chemical Reagent Factory, China) was dissolved in 1.5 g of DI water. 3.015 g of the APS solution and 1.5075 g of the sodium bisulfite solution were added to the fourth suspension. The mixture was stirred at 55° C. and 200 rpm for 24 hours to obtain a fifth suspension.

[0245] After the reaction was completed, the temperature of the fifth suspension was lowered to 25° C. 3.72 g of NaOH was dissolved in 400 g of DI water. Then, 403.72 g of sodium hydroxide solution was added dropwise to the fifth suspension to adjust the pH to 7.31 to form a sixth suspension. The binder was filtered using a 200 μm nylon mesh. The solid content of the binder solution is 9.00 wt.%.

[0246] F) Preparation of the positive electrode A first mixture was prepared by dispersing 12 g of conductive agent (Super P, Timcal Ltd, Bodio, Switzerland) and 100 g of binder solution (solid content 9.00 wt.%) in 74 g of deionized water while stirring with an overhead stirrer (R20, IKA). After addition, the first mixture was further stirred at 25° C. and a speed of 1,200 rpm for about 30 minutes.

[0247] A second mixture was then prepared by adding 276 g of NMC811 (manufactured by Shandong Tianjiao New Energy Co., Ltd., China) to the first mixture at 25° C. while stirring with an overhead stirrer. The second mixture was then degassed for 1 hour under a pressure of about 10 kPa. The second mixture was further stirred at 25° C. and a speed of 1,200 rpm for about 60 minutes to form a homogenized cathode slurry.

[0248] The homogenized positive electrode slurry was coated on both surfaces of the improved current collector prepared above using a doctor blade coater with a gap width of 120 μm. The 80 μm slurry coated on the improved current collector was dried at 70° C. using an electric heating oven to form a positive electrode layer. The drying time was about 10 minutes. The electrode was then compressed to reduce the thickness of the positive electrode layer to 23 μm. The surface density of the positive electrode layer on the improved current collector was 7.00 mg / cm. 2 The volume resistivity of the positive electrode is 2.120 Ω·cm. The interfacial resistance between the electrode layer of Example 1 and the improved current collector was measured and is shown in Table 1 below.

[0249] G) Coin Cell Assembly The electrochemical performance of the above prepared positive electrode was tested in a CR2032 coin Li cell assembled in an argon-filled glove box. The positive electrode was cut into a disk shape for coin cell assembly. A lithium metal foil with a thickness of 500 μm was used as the counter electrode. The positive electrode and the counter electrode were separated by a separator. The separator was a ceramic-coated microporous membrane made of non-woven fabric (MPM, Japan) with a thickness of about 25 μm. Then, the electrode assembly was dried at 105 °C for 16 h in a box resistance oven (DZF-6020, Shenzhen Kejing Star Technology Co.Ltd., China) under vacuum.

[0250] The electrolyte was then injected into the case holding the filled electrodes under a high-purity argon atmosphere with moisture and oxygen contents less than 3 ppm each. The electrolyte was a solution of LiPF6 in a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 1:1:1. After electrolyte filling, the coin cells were mechanically pressed using a standard circular punch.

[0251] H) Electrochemical measurements The coin cells were analyzed in constant current mode using a multi-channel battery tester (BTS-4008-5V10mA, Neware Electronics Co.,Ltd, China). The coin cells were charged and discharged at a rate of C / 2 after one cycle at C / 20. Charge / discharge cycle testing of the cells was performed at 3.0-4.3V, a current density of C / 2, and 25°C to obtain the discharge capacity. The electrochemical performance of the coin cell of Example 1 was measured and is shown in Table 1 below.

[0252] Preparation of conductive material mixtures of Examples 2 to 5, 7 to 9, 14 to 18 and Comparative Examples 1 to 2, 4 to 5 The conductive material mixtures of Examples 2 to 5, 7 to 9, and 14 to 18 and Comparative Examples 1 to 2, and 4 to 5 were prepared in the same manner as in Example 1.

[0253] Preparation of the Conductive Material Mixture of Example 6 The conductive material mixture was prepared in the same manner as in Example 1, except that 200 g of graphite powder was added to 500 g of DI water.

[0254] Preparation of the conductive material mixture of Example 10 The conductive material mixture was prepared in the same manner as in Example 1, except that 150 g of carbon black (Timcal Ltd, Bodio, Switzerland) was used instead of the graphite powder.

[0255] Preparation of the Conductive Material Mixture of Example 11 The conductive material mixture was prepared in the same manner as in Example 1, except that first, 25 g of carbon black was added to 500 g of DI water and stirred at 25° C. and 1000 rpm for 15 minutes to form a mixture, and then 125 g of graphite powder was added to the mixture and further stirred at 25° C. and 1000 rpm for 60 minutes to form a conductive material mixture.

[0256] Preparation of the Conductive Material Mixture of Example 12 The conductive material mixture was prepared in the same manner as in Example 1, except that 25 g of vapor grown carbon nanofiber (VGCF; Showa Denko K.K., Japan) was first added to 500 g of DI water and stirred at 25° C. and 1000 rpm for 15 minutes to form a mixture, and then 125 g of graphite powder was added to the mixture and further stirred at 25° C. and 1000 rpm for 60 minutes to form a conductive material mixture.

[0257] Preparation of the conductive material mixture of Example 13 The conductive material mixture was prepared in the same manner as in Example 1, except that first, 25 g of carbon nanotubes (CNTs; manufactured by Jiangsu Cnano Technology Co. Ltd., China) were added to 500 g of DI water and stirred at 25° C. and 1000 rpm for 15 minutes to form a mixture, and then 125 g of graphite powder was added to the mixture and further stirred at 25° C. and 1000 rpm for 60 minutes to form a conductive material mixture.

[0258] Preparation of conductive material mixture of Comparative Example 3 For Comparative Example 3, no conductive material mixture was prepared.

[0259] Preparation of binder material solution for Example 2 The binder solution was prepared in the same manner as in Example 1, except that the ratios of structural unit (a) and structural unit (b) in the copolymer of the binder material were 98 mol % and 2 mol %, respectively, based on the total moles of monomer units in the copolymer. The weight average molecular weight of the copolymer is 110,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20 °C is 20 mPa s.

[0260] Preparation of binder material solution for Example 3 The binder material solution was prepared in the same manner as in Example 1, except that the weight average molecular weight of the copolymer was prepared to be 20,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20° C. is 6 mPa·s.

[0261] Preparation of binder material solution for Example 4 The binder material solution was prepared in the same manner as in Example 1, except that the ratios of structural unit (a) and structural unit (b) in the copolymer of the binder material were 98 mol % and 2 mol %, respectively, based on the total moles of monomer units in the copolymer. The weight average molecular weight of the copolymer was 16,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20°C was 5 mPa·s.

[0262] Preparation of binder material solution for Example 5 The binder material solution was prepared in the same manner as in Example 1, except that the weight average molecular weight of the copolymer was prepared to be 200,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20° C. is 66 mPa·s.

[0263] Preparation of binder material solution for Example 6 The binder material solution was prepared in the same manner as in Example 1, except that the weight average molecular weight of the copolymer was prepared to be 120,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20° C. is 32 mPa·s.

[0264] Preparation of binder material solution for Example 7 The binder material solution was prepared in the same manner as in Example 1, except that the ratios of structural unit (a) and structural unit (b) in the copolymer of the binder material were 96 mol % and 4 mol %, respectively, based on the total moles of monomer units in the copolymer. The weight average molecular weight of the copolymer is 78,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20°C is 17 mPa s.

[0265] Preparation of binder material solution for Example 8 The binder material solution was prepared in the same manner as in Example 1, except that the ratios of structural unit (a) and structural unit (b) in the copolymer of the binder material were 96 mol % and 4 mol %, respectively, based on the total moles of monomer units in the copolymer. The weight average molecular weight of the copolymer was 80,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20°C was 17 mPa s.

[0266] Preparation of binder material solution of Example 9 The binder material solution was prepared in the same manner as in Example 1, except that the ratios of structural unit (a) and structural unit (b) in the copolymer of the binder material were 92 mol % and 8 mol %, respectively, based on the total moles of monomer units in the copolymer. The weight average molecular weight of the copolymer was 82,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20°C was 17 mPa s.

[0267] Preparation of binder material solutions for Examples 10 to 18 and Comparative Examples 4 to 5 The binder material solutions of Examples 10 to 18 and Comparative Examples 4 to 5 were prepared in the same manner as in Example 1.

[0268] Preparation of binder material solution of Comparative Example 1 The binder material solution was prepared in the same manner as in Example 1, except that the ratios of structural unit (a) and structural unit (b) in the copolymer of the binder material were 89 mol % and 11 mol %, respectively, based on the total moles of monomer units in the copolymer. The weight average molecular weight of the copolymer was 75,000 g / mol. The viscosity of the binder material at a concentration of 4% in DI water at 20°C was 13 mPa s.

[0269] Preparation of binder material solution of Comparative Example 2 As the binder material solution, 750 g of a polyacrylic acid (PAA) solution with a solid content of 9.1 wt. % was used.

[0270] Preparation of binder material solution of Comparative Example 3 For Comparative Example 3, no binder material solution was prepared.

[0271] Preparation of conductive slurries for Examples 2 to 5, 7 to 18 and Comparative Examples 1 to 2 The conductive slurries of Examples 2 to 5, 7 to 18 and Comparative Examples 1 and 2 were prepared in the same manner as in Example 1.

[0272] Preparation of Conductive Slurry for Example 6 The conductive slurry was prepared in the same manner as in Example 1. The solid content of the conductive slurry was 14.0% by weight.

[0273] Preparation of Conductive Slurry of Comparative Example 3 For Comparative Example 3, no conductive slurry was prepared.

[0274] Preparation of Conductive Slurry of Comparative Example 4 The conductive slurry was prepared in the same manner as in Example 1, except that 150 g of the binder material solution was added to 250 g of the conductive material mixture. The solid content of the conductive slurry was 17.8 wt %.

[0275] Preparation of Conductive Slurry of Comparative Example 5 The conductive slurry was prepared in the same manner as in Example 1, except that 680 g of the binder material solution was added to 50 g of the conductive material mixture. The solid content of the conductive slurry was 10.0 wt %.

[0276] Preparation of improved current collectors in Examples 2 to 18 and Comparative Examples 1 to 2 and 4 to 5 The improved current collectors of Examples 2 to 18 and Comparative Examples 1 to 2, 4 to 5 were prepared in the same manner as in Example 1.

[0277] Preparation of improved current collector of Comparative Example 3 For Comparative Example 3, no improved current collector was made.

[0278] Preparation of binder solutions for Examples 2 to 18 and Comparative Examples 1 to 5 The binder solutions of Examples 2 to 18 and Comparative Examples 1 to 5 were prepared in the same manner as in Example 1.

[0279] Preparation of positive electrodes in Examples 2 to 13 and Comparative Examples 1 to 2 and 4 to 5 The positive electrodes of Examples 2 to 13 and Comparative Examples 1 to 2, 4 to 5 were prepared in the same manner as in Example 1.

[0280] Preparation of the positive electrode of Example 14 The positive electrode was prepared in the same manner as in Example 1, except that 276 g of NMC811 was replaced with the same weight of NMC622 in preparing the positive electrode.

[0281] Preparation of the positive electrode of Example 15 The positive electrode was prepared in the same manner as in Example 1, except that 276 g of NMC811 was replaced with the same weight of NMC532 in the preparation of the positive electrode.

[0282] Preparation of the positive electrode of Example 16 The positive electrode was prepared in the same manner as in Example 1, except that 276 g of NMC811 was substituted for the same weight of NCA in the preparation of the positive electrode.

[0283] Preparation of the positive electrode of Example 17 The positive electrode is made of 276g of NMC811 with NMC532 as the core and Li as the shell. 0.95 Ni 0.53 Mn 0.29 Co 0.15 Al 0.03 It was prepared in the same manner as in Example 1, except that the same weight of the core-shell positive electrode active material (CS) with O2 was replaced.

[0284] Preparation of the positive electrode of Example 18 The positive electrode was prepared in the same manner as in Example 1, except that 276 g of NMC811 was replaced with the same weight of LFP in preparing the positive electrode.

[0285] Preparation of Positive Electrode of Comparative Example 3 The positive electrode was prepared in the same manner as in Example 1, except that the homogenized positive electrode slurry was coated on both sides of the substrate. The substrate used was an aluminum foil with a thickness of 16 μm. The volume resistivity of the positive electrode was 11.414 Ω·cm.

[0286] Assembly of coin cells of Examples 2 to 18 and Comparative Examples 1 to 5 The coin cells of Examples 2 to 18 and Comparative Examples 1 to 5 were assembled in the same manner as in Example 1.

[0287] Electrochemical measurements of Examples 2 to 17 and Comparative Examples 1 to 3 The electrochemical performance of the coin cells of Examples 2-17 and Comparative Examples 1-3 was measured in the same manner as in Example 1, and the test results are shown in Table 1 below.

[0288] Electrochemical measurements of Example 18 The electrochemical performance of the coin cell of Example 18 was measured in the same manner as in Example 1, except that the charge / discharge cycle test of the cell was performed at 2.00-3.65 V, a current density of C / 2, and 25° C. to obtain the discharge capacity.

[0289] Electrochemical measurements of Comparative Example 4 The electrochemical performance of the coin cell of Comparative Example 4 was measured in the same manner as in Example 1. The interfacial resistance between the electrode layer and the improved current collector was 8.437 Ω cm 2 The initial discharge capacity at 0.5C is 164mAh / g, and the capacity retention after 50 cycles is 78.03%.

[0290] Electrochemical measurements of Comparative Example 5 The electrochemical performance of the coin cell of Comparative Example 5 was measured in the same manner as in Example 1. The interfacial resistance between the electrode layer and the improved current collector was 18.385 Ω cm 2 The initial discharge capacity at 0.5C is 161mAh / g, and the capacity retention after 50 cycles is 78.71%.

[0291] [Table 1]

Claims

1. A conductive layer is provided on one or both sides of a substrate, the conductive layer comprising a conductive material and a binder material, the binder material comprising a copolymer comprising a structural unit (a), the structural unit (a) being represented by formula (1); [Formula 1] Here, R in formula (1) 1 , R 2 , R 3 and R 4 each of which is independently H, hydroxy, alkyl, hydroxyalkyl, halogen, or alkyl halide.

2. The copolymer further comprises a structural unit (b), the structural unit (b) being represented by formula (2); [Case 2] Here, R in formula (2) 5 , R 6 , R 7 and R 8 10. The improved current collector of claim 1 comprising one or more monomer units having: each of which is independently H, alkyl, acyloxy, acyloxyalkyl, halogen, or alkyl halide.

3. 2. The improved current collector of claim 1, wherein the proportion of said structural unit (a) in said copolymer is at least 90 mole percent, based on the total moles of monomer units in said copolymer.

4. 10. The improved current collector of claim 1, wherein the proportion of said structural unit (a) in said copolymer is from about 90 mol % to about 99.8 mol %, based on the total number of moles of monomer units in said copolymer.

5. 3. The improved current collector of claim 2, wherein the proportion of said structural unit (b) in said copolymer is from about 0.1 mol % to about 10 mol %, based on the total number of moles of monomer units in said copolymer.

6. 3. The improved current collector of claim 2, wherein the molar ratio of said structural units (a) to said structural units (b) in said copolymer is from about 9 to about 1000.

7. 10. The improved current collector of claim 1, wherein said improved collector has a thickness of about 5 μm to about 70 μm.

8. 10. The improved current collector of claim 1, wherein said substrate is selected from the group consisting of stainless steel, titanium, nickel, aluminum, copper, platinum, gold, silver, chromium, zirconium, tungsten, molybdenum, silicon, tin, vanadium, zinc, cadmium, or alloys thereof, electrically conductive resins, or combinations thereof.

9. 2. The improved current collector of claim 1, wherein the conductive material is selected from the group consisting of carbon, carbon black, graphite, expanded graphite, graphene, graphene nanoplatelets, carbon fibers, carbon nanofibers, graphitized carbon flakes, carbon tubes, carbon nanotubes, activated carbon, Super P, KS6, vapor grown carbon fiber (VGCF), mesoporous carbon, and combinations thereof.

10. 3. The improved current collector of claim 2, wherein said copolymer has a weight average molecular weight of from about 10,000 g / mol to about 300,000 g / mol.

11. 10. The improved current collector of claim 1, wherein the percentage of said conductive material in said conductive layer is from about 25% to about 75% by weight, based on the total weight of said conductive layer.

12. 2. The improved current collector of claim 1, wherein the proportion of said copolymer in said conductive layer is from about 25% to about 75% by weight, based on the total weight of said conductive layer.

13. 2. The improved current collector of claim 1, wherein said hydroxyalkyl is selected from the group consisting of hydroxymethyl, hydroxyethyl, hydroxypropyl, hydroxy(methyl)propyl, hydroxy(methyl)butyl, and combinations thereof.

14. 3. The improved current collector of claim 2, wherein said acyloxyalkyl is selected from the group consisting of acyloxymethyl, acyloxyethyl, acyloxypropyl, acyloxy(methyl)propyl, acyloxy(methyl)butyl, and combinations thereof.

15. 10. An electrode comprising the improved current collector of claim 1 and an electrode layer, the electrode layer being located on a surface of the conductive layer and comprising an electrode active material and a binder.

16. The electrode active material is LiCoO 2 , LiNiO 2 , LiNi 1-x M x O 2 , LiNi x Mn y O 2 , LiCo x Ni y O 2 , Li 1+z Ni x Mn y Co 1-x-y O 2 , LiNi x Co y A z O 2 , LiV 2 O 5 , LiTiS 2 , LiMoS 2 , LiMnO 2 , LiCrO 2 , LiMn 2 O 4 , Li 2 MnO 3 , LiFeO 2 , LiFePO 4 and combinations thereof, wherein each x is independently from 0.1 to 0.9, each y is independently from 0 to 0.9, each z is independently from 0 to 0.4, and M is selected from the group consisting of Co, Mn, Al, Fe, Ti, Ga, Mg, and combinations thereof.

17. The electrode active material is NaC O O 2, NaFeO 2 , NaNiO 2 , NaCrO 2 , NaVO 2 , NaTiO 2 , NaFePO 4 , Na 3 V 2 (P.O. 4 ) 3 , Na 3 V 2 (P.O. 4 ) 2 F 3 16. The electrode of claim 15, wherein the positive electrode active material is selected from the group consisting of: NMc-type mixed oxides, Prussian Blue-type sodium compounds, and combinations thereof.

18. The electrode active material may be natural graphite particles, synthetic graphite particles, hard carbon, soft carbon, mesocarbon microbeads (MCMB), tin particles, SnO 2 , SnO, Li 4 Ti 5 O 12 16. The electrode of claim 15, wherein the negative electrode active material is selected from the group consisting of Si particles, Si particles, Si-C composite particles, and combinations thereof.

19. 16. The electrode of claim 15, wherein the binder comprises a polymer that includes one or more functional groups containing halogen, O, N, S, or combinations thereof.

20. Each functional group is a carboxylic acid, a carboxylate, a sulfonic acid, a sulfonate, a sulfuric acid, a sulfate, a phosphonic acid, a phosphonate, a phosphoric acid, a phosphate, a nitric acid, a nitrate, an amide, a hydroxyl, a nitrile, an ester, an epoxy, an -NH 2 20. The electrode of claim 19, wherein the electrode is independently selected from the group consisting of:

Citation Information

Patent Citations

  • Primers for battery electrodes

    JP2011501383A

  • Negative electrode material for sodium secondary battery, method for producing the same, negative electrode for sodium secondary battery, sodium secondary battery, and electrical equipment including the same

    JP2013171798A

  • Conductive adhesive composition for electrochemical element electrode

    JP2014137915A

  • Electricity storage element

    JP2017201589A

  • Electrodes with collectors containing protective conductive layers and corresponding manufacturing methods for electrical energy storage systems

    JP2017508307A