Cathode material for lithium-sulfur batteries and lithium-sulfur batteries including the same
A carbon composite with transition metal particles and a carbon coating on a porous substrate addresses the kinetic and conductivity issues in lithium-sulfur batteries, enhancing electrochemical reactions and stabilizing performance.
Patent Information
- Application Number
- JP2024532940
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium-sulfur batteries face challenges with low kinetic activity and conductivity due to the non-conductivity of sulfur, leading to polysulfide elution and reduced reversible capacity and energy density, and existing catalysts like platinum are costly and prone to poisoning.
A carbon composite is developed with a porous carbon substrate and transition metal particles, coated with a carbon layer, containing elements like cobalt or iron, to enhance adsorption of lithium polysulfide and promote 3D-shaped lithium sulfide formation, improving electrochemical reactions.
The carbon composite enhances kinetic activity, suppresses polysulfide elution, and stabilizes performance, resulting in improved initial capacity, capacity retention, and energy density in lithium-sulfur batteries.
Smart Images

Figure 2024542771000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode material for a lithium-sulfur battery and a lithium-sulfur battery including the same.
[0002] This application claims priority to Korean Patent Application No. 2022-0094135 filed on July 28, 2022, and Korean Patent Application No. 2022-0156801 filed on November 21, 2022, to the Korean Intellectual Property Office, and the contents disclosed in the specification of said applications are incorporated in their entirety into this application. [Background technology]
[0003] Lithium-sulfur batteries refer to battery systems that use sulfur-based materials with SS bonds (sulfur-sulfur bonds) as the positive electrode active material and lithium metal as the negative electrode active material. Sulfur, the main material of the positive electrode active material, is a globally abundant resource, non-toxic, and has the advantage of being low in weight per atom.
[0004] As the application areas of secondary batteries expand to electric vehicles (EVs) and energy storage systems (ESSs), lithium-sulfur battery technology is in the spotlight because it can theoretically achieve a relatively high energy storage density (~2,600Wh / kg) relative to its weight, compared to lithium-ion secondary batteries, which have a relatively low energy storage density (~250Wh / kg) relative to their weight.
[0005] During discharge, lithium, the negative electrode active material, is oxidized by giving off electrons and being ionized into lithium cations, and the positive electrode active material, the sulfur-based material, is reduced by receiving electrons. Here, the S-S bond receives two electrons through the reduction reaction of the sulfur-based material and is converted into the form of sulfur anions. The lithium cations generated by the oxidation reaction of lithium are transferred to the positive electrode via the electrolyte, and combine with the sulfur anions generated by the reduction reaction of the sulfur-based compound to form salts. Specifically, sulfur before discharge has a cyclic S8 structure, which is converted into lithium polysulfide (Li2Sx) through a reduction reaction, and the lithium polysulfide is completely reduced to generate lithium sulfide (Li2S, lithium sulfide).
[0006] As described above, sulfur used as the positive electrode active material is a non-conductor, which makes it difficult for electrons generated by the electrochemical reaction to move, resulting in the dissolution of polysulfide (LiSx) during the charge and discharge process. In addition, the low electrical conductivity of sulfur and lithium sulfide slows down the kinetic activity of the electrochemical reaction, resulting in reduced battery life and speed characteristics.
[0007] In this regard, research has been conducted to improve the performance of lithium-sulfur secondary batteries by using platinum (Pt), which has been widely used recently as an electrochemical catalyst, to improve the kinetic activity of the sulfur redox reaction during the charge and discharge process of the lithium-sulfur secondary battery. However, precious metal catalysts such as platinum are expensive and difficult to put into practical use, and there is a problem that they can be poisoned by the sulfur redox reaction during the charge and discharge process, making it difficult to use them as positive electrode materials for lithium-sulfur secondary batteries.
[0008] Therefore, there is a continuous demand for technological development of positive electrode materials that can improve the kinetic activity of the electrochemical reaction during charging and discharging of lithium-sulfur secondary batteries and are also advantageous in terms of cost for practical use.
[0009] Meanwhile, as described above, sulfur, which is a non-conductor, is used in the positive electrode by being supported on a support such as a porous carbon substrate. In this case, when lithium sulfide generated by the oxidation-reduction reaction of the battery is formed in a 2D film shape on the carbon support as described above, the ion transfer characteristics of electrons and lithium are significantly reduced, and the utilization rate of sulfur is also reduced, resulting in a problem that the reversible capacity and energy density of the lithium-sulfur battery are rather reduced.
[0010] Recently, research has been conducted to control the shape of lithium sulfide, which is generated by solvation in the electrolyte, into a 3D shape. However, the solvents used in such research are highly reactive with the lithium metal anode, so it remains difficult to put lithium-sulfur batteries into practical use. Summary of the Invention [Problem to be solved by the invention]
[0011] Therefore, the problem to be solved by the present invention is to solve the above-mentioned problems, The object of the present invention is to provide a positive electrode material that has excellent adsorption power with lithium polysulfide and enhances the kinetic activity of the sulfur oxidation / reduction reaction.
[0012] Furthermore, another problem to be solved by the present invention is to provide a carbon composite capable of generating lithium sulfide in a 3D shape on a porous carbon substrate when operating a lithium-sulfur battery.
[0013] Specifically, the goal is to provide a carbon composite that can generate lithium sulfide in a 3D shape while utilizing the electrolyte used in conventional lithium-sulfur batteries, and a high-performance lithium-sulfur battery that uses the same. [Means for solving the problem]
[0014] In order to solve the above problems, According to one aspect of the present invention, there is provided a carbon composite having the following aspect.
[0015] The carbon composite according to the first aspect comprises: The present invention comprises: a porous carbon substrate; transition metal composite particles, the transition metal composite particles including a core portion located on at least one of the outer surface of the porous carbon substrate and the inner surface of the pores, the core portion including a transition metal particle, and a carbon coating layer covering at least a portion of the surface of the core portion; and at least one different element doped into at least one of the porous carbon substrate and the carbon coating layer, the transition metal particle including at least one of cobalt (Co) and iron (Fe), and the different element including one or more of nitrogen (N), sulfur (S) and oxygen (O).
[0016] According to the second aspect, in the first aspect, The carbon coating layer may cover the entire surface of the core portion.
[0017] According to the third aspect, in the first or second aspect, The average particle diameter of the transition metal composite particles (D 50 The ratio of the thickness of the carbon coating layer to the thickness of the substrate may be 40% or less.
[0018] According to a fourth aspect, in any one of the first to third aspects, The transition metal particles may further include one or more selected from zinc (Zn), vanadium (V), chromium (Cr), manganese (Mn), nickel (Ni), copper (Cu), zirconium (Zr), niobium (Nb), molybdenum (Mo), technetium (Tc), rubidium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), lanthanum (La), hafnium (Hf), tantalum (Ta), tungsten (W), osmium (Os), iridium (Ir), cerium (Ce), gadolinium (Gd), scandium (Sc), titanium (Ti), gallium (Ga), and indium (In).
[0019] According to a fifth aspect, in any one of the first to fourth aspects, The transition metal particles may have a cobalt content of 95 mol % based on 100 mol % of the transition metal element.
[0020] According to a sixth aspect, in any one of the first to fifth aspects, The transition metal particles may have a cobalt content of 100 mol % based on 100 mol % of the transition metal element.
[0021] According to the seventh aspect, in any one of the first to sixth aspects, The transition metal particles may be cobalt nanoparticles.
[0022] According to an eighth aspect, in any one of the first to seventh aspects, The core portion of the transition metal composite particle has an average particle diameter (D 50 ) may be from 1 nm to 90 nm.
[0023] According to the ninth aspect, in any one of the first to eighth aspects, The carbon coating layer may have a thickness of 10 nm or less.
[0024] According to a tenth aspect, in any one of the first to ninth aspects, The carbon coating layer may include crystalline carbon.
[0025] According to an eleventh aspect, in any one of the first to tenth aspects, The carbon coating layer may have a single-layer structure or a multi-layer structure of two or more layers.
[0026] According to a twelfth aspect, in any one of the first to eleventh aspects, The carbon coating layer may have a single-layer structure or a multi-layer structure of 2 to 5 layers.
[0027] According to a thirteenth aspect, in any one of the first to twelfth aspects, The carbon coating layer contains nitrogen as the different element, and may have a single layer structure or a multilayer structure of two to four layers.
[0028] According to a fourteenth aspect, in any one of the first to thirteenth aspects, The transition metal composite particles have an average particle size (D 50 ) may be from 2 nm to 100 nm.
[0029] According to a fifteenth aspect, in any one of the first to fourteenth aspects, The porous carbon substrate may include carbon nanotubes (CNT), graphene, graphene oxide (GO), reduced graphene oxide (rGO), carbon black, graphite, graphite nanofiber (GNF), carbon nanofiber (CNF), activated carbon fiber (ACF), activated carbon, fullerene, or two or more of these.
[0030] According to a sixteenth aspect, in any one of the first to fifteenth aspects, The porous carbon substrate may include carbon nanotubes (CNTs), and the carbon nanotubes may include entangled CNTs.
[0031] According to a seventeenth aspect, in any one of the first to sixteenth aspects, The content of the transition metal composite particles may be 15% by weight or less based on 100% by weight of the carbon composite.
[0032] According to an eighteenth aspect, in any one of the first to seventeenth aspects, The content of the different element may be 10% by weight to 50% by weight based on 100% by weight of the carbon composite.
[0033] According to a nineteenth aspect, in any one of the first to eighteenth aspects, The number of bonds between the transition metal elements in the carbon composite is greater than the number of bonds between the transition metal element and the different element, and the bonds between the elements can be confirmed by extended X-ray absorption fine structure (EXAFS) analysis.
[0034] According to another aspect of the present invention, there is provided a method for producing a carbon composite having the following features.
[0035] A method for producing a carbon composite according to a twentieth aspect includes the steps of: A method for producing a carbon composite according to any one of the first to nineteenth aspects, comprising a step of mixing a transition metal-containing precursor, a carbon precursor, and a porous carbon substrate, and heat-treating the mixture, wherein the transition metal-containing precursor contains at least one of cobalt (Co) and iron (Fe), and the carbon precursor contains one or more different elements selected from nitrogen (N), sulfur (S), and oxygen (O).
[0036] According to the twenty-first aspect, in the twentieth aspect, The carbon precursor may include dopamine, polydopamine, melamine, 1,10-phenanthroline, polyaniline, carbon nitride (g-CN), glucose, phenylenediamine, or mixtures thereof.
[0037] According to the twenty-second aspect, in the twenty-first or twenty-first aspect, The method may include mixing the transition metal-containing precursor and the carbon precursor to produce a metal-carbon precursor composite (MC precursor complex), mixing the metal-carbon precursor composite and the porous carbon substrate to produce a metal-carbon-substrate precursor composite (MC-substrate precursor complex), and heat-treating the metal-carbon-substrate precursor composite.
[0038] According to a twenty-third aspect, in any one of the twentieth to twenty-second aspects, The heat treatment may be carried out at a temperature of 600°C to 1,000°C.
[0039] According to still another aspect of the present invention, there are provided a positive electrode active material, a positive electrode, and a lithium-sulfur battery having the following embodiments.
[0040] According to a twenty-fourth aspect, There is provided a positive electrode active material including the carbon composite according to any one of the first to nineteenth aspects and a sulfur-based compound.
[0041] According to the twenty-fifth aspect, A positive electrode is provided, comprising the positive electrode active material according to the twenty-fourth embodiment.
[0042] According to the twenty-sixth aspect, There is provided a lithium-sulfur battery comprising: a positive electrode; a negative electrode; a separator (separation membrane) interposed between the positive electrode and the negative electrode; and an electrolyte, wherein the positive electrode comprises the positive electrode according to the twenty-fifth embodiment.
[0043] According to the twenty-seventh aspect, A positive electrode is provided, the positive electrode comprising a positive electrode active material including a sulfur-based compound and the carbon composite according to any one of the first to nineteenth aspects as a conductive material.
[0044] According to the twenty-eighth aspect, There is provided a lithium-sulfur battery comprising: a positive electrode; a negative electrode; a separator interposed between the positive electrode and the negative electrode; and an electrolyte; wherein the positive electrode is the positive electrode according to the twenty-seventh embodiment. Effect of the Invention
[0045] The carbon composite according to one aspect of the present invention has an excellent adsorption force with lithium polysulfide (LiPS, Li2Sx, 2≦x≦8) and has an excellent kinetic activity in the oxidation / reduction reaction of sulfur.
[0046] In particular, the carbon composite has the effect of smoothing ion transfer by controlling the shape of lithium sulfide formed on the surface to a 3D shape, and suppressing the overpotential increase of 2D lithium sulfide, thereby providing excellent kinetic activity in the oxidation / reduction reaction of sulfur during charge / discharge processes.
[0047] Therefore, a lithium-sulfur secondary battery using the carbon composite as a positive electrode additive and / or a support for supporting a positive electrode active material has an effect of stably realizing high performance by suppressing the dissolution of lithium polysulfide into an electrolyte and improving the conversion rate of sulfur, and stably maintaining such performance.
[0048] Furthermore, the lithium-sulfur battery according to one embodiment of the present invention has excellent effects in terms of initial capacity, capacity retention rate through charge / discharge cycles, and battery energy density.
[0049] The drawings attached to this specification are intended to illustrate preferred embodiments of the present invention and serve to facilitate a further understanding of the technical ideas of the present invention as well as the content of the invention, and therefore the present invention should not be interpreted as being limited to only the matters depicted in the drawings. [Brief description of the drawings]
[0050] [Figure 1]FIG. 2 is a schematic diagram showing the function of controlling the shape of lithium sulfide generated on the surface of a carbon composite according to one embodiment of the present invention in a positive electrode during charging and discharging of a lithium-sulfur secondary battery. [Figure 2a] 1 shows transmission electron microscopy (TEM) photographs of carbon composites according to Example 1, Example 2, and Comparative Example 2 in the present specification. [Figure 2b] 4A-4C are TEM pictures at different magnifications of a carbon composite according to Example 3 herein. [Figure 2c] 1 is a SEM photograph of a carbon composite according to Example 4 herein. [Diagram 3] 1 is a graph showing the results of thermogravimetric analysis (TGA) of carbon composites according to Example 1, Example 2, and Comparative Example 2 in the present specification. [Figure 4] 1 is a graph showing the 1s state of nitrogen element as a result of X-ray photoelectron spectroscopy (XPS) analysis of carbon composites according to Example 1, Example 2, and Comparative Example 2 in the present specification. [Figure 5a] 1 is a graph showing the state of transition metal elements as a result of XPS analysis of carbon composites according to Example 1, Example 2, and Comparative Example 2 in this specification. [Figure 5b] 1 is a graph showing the results of an extended X-ray absorption fine structure (EXAFS) analysis of the bonding states of transition metals in carbon composites according to Example 1, Example 2, and Comparative Example 2 in the present specification. [Figure 6] 1 is a graph showing the results of chronoamperometry (time-current method) analysis of the carbon composites according to Example 1, Example 2, and Comparative Example 2 herein, and Comparative Example 1 (CNT). [Figure 7]1 shows scanning electron microscopy (SEM) photographs of carbon composites according to Examples 1, 2, and Comparative Example 2 in the present specification and Comparative Example 1 (CNT) after the first discharge was performed at a current density of 0.05 C. [Figure 8] FIG. 1 is a graph showing the results of performance evaluation of batteries using carbon composites according to Examples 1 and 2 and Comparative Example 2 herein and Comparative Example 1 (CNT), in which (a) is a graph showing the results of constant current characteristic evaluation, and (b) is a graph showing the capacity-voltage curve in the first charge-discharge cycle. [Figure 9] 1A is a TEM image showing a carbon composite according to Comparative Example 4 in the present specification, and FIG. 1B is a graph showing the results of performance evaluation of the batteries of Comparative Examples 3 and 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0051] The present invention will be described in detail below. However, the present invention is not limited to the following content, and each component may be modified or mixed selectively as necessary. Therefore, it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.
[0052] Throughout this specification, when a certain configuration "comprises" certain components, this does not mean that it excludes certain other components, but that it may further include other components, unless otherwise specified.
[0053] Throughout this specification, the phrase "A and / or B" means "A or B or both."
[0054] Certain terminology used herein is for convenience and is not limiting. For example, positional terms such as "top," "bottom," "left," "right," "front," "rear," "inside," and "outside" are used to describe relative positions and orientations of components relative to one another and may represent positions and orientations in the drawings to which reference is made, rather than absolute positions. The above terms include themselves as well as words containing them, their derivatives, and words of similar meaning.
[0055] According to one aspect of the present invention, there is provided a carbon composite that can be used as an electrochemical catalyst in the positive electrode of a lithium-sulfur secondary battery.
[0056] FIG. 1 is a schematic diagram showing an example of the function of the carbon composite.
[0057] A carbon composite according to one aspect of the present invention is intended to generate 3D shaped lithium sulfide (LiS) on the surface of the carbon composite by adjusting the adsorption strength between the surface of the carbon composite and lithium polysulfide (LiPS) solvated by electrolyte solvent molecules.
[0058] Previously, research has been reported on growing lithium sulfide into a 3D shape by designing an electrolyte with a high donor number. However, such electrolytes are prone to react with lithium metal, and there is a problem that irreversible decomposition reactions occur violently on the lithium metal surface.
[0059] Therefore, the inventors of the present invention have conducted extensive research to provide a cathode catalyst that can promote the adsorption and conversion reaction of lithium polysulfide in a normal electrolyte while growing lithium sulfide into a 3D shape, and have completed the present invention.
[0060] A carbon composite according to one aspect of the present invention includes a porous carbon substrate; transition metal composite particles, the transition metal composite particles including a core portion located on at least one of an outer surface of the porous carbon substrate and an inner surface of a pore, the core portion including a transition metal particle, and a carbon coating layer covering at least a part of the surface of the core portion; and at least one different element doped into at least one of the porous carbon substrate and the carbon coating layer. The transition metal particle includes at least one of cobalt (Co) and iron (Fe), and the different element is one or more selected from nitrogen (N), sulfur (S), and oxygen (O).
[0061] In one embodiment of the present invention, the transition metal composite particles may be disposed on the outer surface of the porous carbon substrate, on the inner surface of the pores, or both. The inner surface of the pores may mean the inside of the pores of the porous carbon substrate on the surface of the porous carbon substrate.
[0062] In one aspect of the present invention, the transition metal composite particles have catalytic activity for the oxidation and reduction reactions of sulfur-based compounds such as sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 2≦x≦8), disulfide compounds, and mixtures of two or more of these, as a positive electrode active material for a lithium-sulfur battery. In one aspect of the present invention, the transition metal composite particles can be called a catalyst, but the function of the transition metal composite particles is not limited thereto.
[0063] The transition metal composite particle includes a core portion containing a transition metal particle, and a carbon coating layer covering at least a portion of the surface of the core portion.
[0064] The transition metal composite particle contains a transition metal particle as an active component of a catalyst in a core portion. Specifically, the core portion of the transition metal composite particle may be composed only of the transition metal particle.
[0065] In one aspect of the present invention, the core portion of the transition metal composite particle may contain a transition metal element liberated from the transition metal particle in a single atomic size, and for catalytic activity of the carbon composite, the core portion of the transition metal composite particle may contain a transition metal particle formed by bonding between transition metal atoms.
[0066] The transition metal particles contained in the core part contain a transition metal element that has catalytic activity for the oxidation and reduction reactions of the sulfur-based compound itself and controls the shape of the lithium sulfide produced. For this purpose, the transition metal particles contain at least one of cobalt (Co) and iron (Fe).
[0067] According to one embodiment of the present invention, the transition metal particles may further include, in addition to the cobalt and iron, one or more selected from, for example, zinc (Zn), vanadium (V), chromium (Cr), manganese (Mn), nickel (Ni), copper (Cu), zirconium (Zr), niobium (Nb), molybdenum (Mo), technetium (Tc), rubidium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), lanthanum (La), hafnium (Hf), tantalum (Ta), tungsten (W), osmium (Os), iridium (Ir), cerium (Ce), gadolinium (Gd), scandium (Sc), titanium (Ti), gallium (Ga), and indium (In).
[0068] Each of the cobalt and iron can provide catalytic activity for the oxidation-reduction of sulfur. At this time, since they exert an appropriate binding force to lithium sulfide generated by the oxidation-reduction of sulfur, the shape of the lithium sulfide formed on the surface of the carbon composite can be made three-dimensional, i.e., a 3D shape.
[0069] FIG. 6 shows a graph showing the results of a chronoamperometry analysis for predicting the shape of lithium sulfide generated when a battery is operated using a carbon composite according to one embodiment of the present invention. When Li2S particles grow into a 2D shape, the Bewick, Fleischman, and Thirsk (BFT) model is followed. On the other hand, when they grow into a 3D shape, the Scharifker-Hills (SH) model is followed. Referring to FIG. 6, which shows an analysis of the measured graph by fitting, it can be confirmed that the shape of lithium sulfide formed on the surface of the carbon composite is a three-dimensional shape because it fits the SH model.
[0070] In one embodiment of the present invention, the chronoamperometry can be carried out in a thermostatic chamber at 25° C. using a PESC05-0.1 instrument from PNE Solution.
[0071] Therefore, in one embodiment of the present invention, when the transition metal particles contained in the core portion contain cobalt and / or iron elements, the shape of lithium sulfide generated by oxidation-reduction of sulfur may be a three-dimensional shape, i.e., a 3D shape.
[0072] On the other hand, when the core of the transition metal composite particle contains a transition metal particle composed of a transition metal element having a stronger binding strength to lithium sulfide than cobalt and iron, the lithium sulfide is generated in a film shape, i.e., a 2D shape, on the surface of the carbon composite due to the strong binding strength to the generated lithium sulfide. In this case, there is a possibility that the catalytic activity of the carbon composite is reduced due to the lithium sulfide formed in a film shape on the surface of the carbon composite.
[0073] For example, when the transition metal particles contained in the core portion of the transition metal composite particle are composed only of nickel (Ni) element, there is a problem that the shape of the generated lithium sulfide is formed into a flatter film shape, i.e., a 2D shape, compared to when the transition metal particles are composed only of iron and / or cobalt elements.
[0074] In another embodiment of the present invention, when the transition metal particles contained in the core part are composed of iron (Fe) element only, the size of the 3D shaped lithium sulfide generated may be larger than when composed of cobalt element only. Conversely, when composed of cobalt element only, the size of the 3D shaped lithium sulfide generated is smaller, and thus the total surface area of the lithium sulfide generated is larger, and the reversible capacity and life stability of the lithium-sulfur battery using the same can be improved.
[0075] From this viewpoint, in still another embodiment of the present invention, the transition metal particles may have a cobalt content of 95 mol % or more based on 100 mol % of the transition metal element.
[0076] In yet another embodiment of the present invention, the transition metal particles may have a cobalt element content of 100 mol % based on 100 mol % of the transition metal element. That is, the transition metal particles may be cobalt metal particles. Specifically, the transition metal particles may be cobalt metal nanoparticles.
[0077] In one embodiment of the present invention, the transition metal particles are grown from a transition metal-containing precursor and may have, for example, a spherical, elliptical, sheet-like, plate-like, fibrous, needle-like, or hollow shape.
[0078] In one embodiment of the present invention, the core portion of the transition metal composite particle may be composed of 100% of the transition metal particle, and thus the size of the core portion of the transition metal composite particle may be the same as the size of the transition metal particle.
[0079] In one embodiment of the present invention, the transition metal particles have an average particle size (D 50 Specifically, the transition metal particles may have an average particle size (D 50) may be 1 nm to 80 nm, 2 nm to 50 nm, 5 nm to 40 nm, 5 nm to 35 nm, 5 nm to 30 nm, or 10 nm to 20 nm. When the size of the transition metal particles is within the above range, the electrical conductivity of electrons and / or ions is excellent, which can have an advantageous effect in terms of improving the performance of the battery and the manufacturing process, but the present invention is not limited thereto.
[0080] In this specification, the particle size can be measured by a known method, and the measurement method is not particularly limited. For example, the particle size can be measured by a scanning electron microscope (SEM), a field-emission electron microscopy, or a laser diffraction method. The measurement by the laser diffraction method can be performed, for example, using a commercially available laser diffraction type particle size distribution measurement device (e.g., Microtrac MT 3000). The average particle size (D 50 ) means the particle size at the point where the cumulative distribution of particle numbers by particle size is 50%.
[0081] The transition metal composite particles have a form in which at least a part of the surface of the transition metal particles as described above is covered with a carbon coating layer.
[0082] The carbon coating layer may function to control the size of the transition metal particles and provide a binding site with the porous carbon substrate on which the transition metal composite particles are supported, thereby allowing the transition metal composite particles to be supported on the porous carbon substrate. The carbon coating layer may also function to stably maintain the metallic phase of the transition metal particles in the core portion. For example, the carbon coating layer may function to prevent lithium polysulfide in an electrolyte from directly chemically bonding to the surface of the transition metal particles, thereby stably maintaining the catalytic activity of the transition metal particles during operation of a lithium-sulfur battery. In the present invention, the function of the carbon coating layer is not limited to the above-mentioned functions.
[0083] In one embodiment of the present invention, the area of the core portion covered by the carbon coating layer may be, for example, 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, 95% or more, or 99% or more based on the total area of the core portion, but is not limited thereto.
[0084] In one embodiment of the present invention, the carbon coating layer may cover the entire surface of the core portion. As described later, the carbon coating layer may be formed on the entire surface of the core portion, which may provide an advantageous effect in terms of stabilizing the activity of the transition metal composite particles by the carbon coating layer, but the present invention is not limited thereto.
[0085] In this specification, the area of the core covered by the carbon coating layer can be measured, for example, by TEM. The TEM can be, but is not limited to, G2 F30 S-Twin manufactured by Tecnai.
[0086] In one embodiment of the present invention, the average particle size (D 50 For example, the ratio of the thickness of the carbon coating layer to the average particle diameter (D 50 ) may be 30% or less, 25% or less, 20% or less, or 15% or less. For example, the ratio of the thickness of the carbon coating layer to the average particle diameter (D 50 ) may be 1% or more, 5% or more, 7.5% or more, or 10% or more. For example, the ratio of the thickness of the carbon coating layer to the average particle diameter (D 50 The ratio of the thickness of the carbon coating layer to the average particle diameter of the transition metal composite particles may be 10% to 20%, or 10% to 15%. When the ratio of the thickness of the carbon coating layer to the average particle diameter of the transition metal composite particles is within the above range, an advantageous effect can be exhibited in terms of stabilizing the activity of the transition metal composite particles by the carbon coating layer, but the present invention is not limited thereto.
[0087] In one embodiment of the present invention, the carbon coating layer covering the surface of the transition metal composite particle may have a uniform thickness. For example, the standard deviation (Δd) of the thickness measured at any 10 points of the carbon coating layer formed on the surface of the core portion may be 0.5 nm or less.
[0088] In one embodiment of the present invention, the carbon coating layer covers the entire surface of the transition metal composite particle, and the carbon coating layer may have a standard deviation (Δd) of thickness measured at any 100 points over the entire surface of the carbon coating layer of 0.5 nm or less.
[0089] In one aspect of the present invention, the carbon coating layer may include crystalline carbon. For example, in another aspect of the present invention, the carbon coating layer may be composed of crystalline carbon. For example, the carbon coating layer may be formed by carbonization of a carbon precursor and may be composed of only crystalline carbon.
[0090] As used herein, the term "crystalline" carbon refers to the presence of carbon on a three-dimensional scale at the atomic dimension level. For example, the crystallinity can be confirmed by diffraction techniques, heat of fusion measurements, TEM, etc. For example, the crystallinity can be confirmed by each carbon having at least one distinct peak in the XRD spectrum.
[0091] Referring to FIG. 2a, a TEM image of a carbon composite according to one embodiment of the present invention shows that the carbon coating layer formed on the surface of the core portion including the transition metal composite particle is composed of crystalline carbon.
[0092] In one embodiment of the present invention, the carbon coating layer may contain at least one different element as a doping element in addition to carbon, specifically, the different element may include one or more elements selected from the group consisting of nitrogen (N), sulfur (S) and oxygen (O).
[0093] As described below, in order to prepare the carbon composite, the porous carbon substrate, the transition metal-containing precursor, and the carbon precursor may be mixed and then heat-treated. At this time, the carbon precursor contains one or more different elements selected from nitrogen, sulfur, and oxygen. As a result, a carbon coating layer is formed on the surface of the transition metal particles by carbon derived from the carbon precursor, and the different elements derived from the carbon precursor are doped into at least one of the porous carbon substrate and the carbon coating layer.
[0094] The carbon coating layer can be coated with a thickness of 40% or less, specifically 30% or less, 25% or less, 20% or less, or 15% or less, for example 1% or more, 2% or more, 5% or more, 7.5% or more, or 10% or more, based on the average particle diameter of the transition metal composite particles. For example, the carbon coating layer can be coated with a thickness of 10% to 20% or 10% to 15% based on the average particle diameter of the transition metal composite particles. The carbon coating layer coats the surface of the transition metal particles with a thin thickness, thereby enabling the transition metal particles to be supported on the porous carbon substrate with a uniform size and allowing the transition metal particles to exhibit good catalytic activity. For example, the thickness of the carbon coating layer is formed to be within 40% of the total thickness of the transition metal composite particles, thereby maintaining smooth interaction between the transition metal particles located inside the carbon coating layer and lithium polysulfide approaching from the outside of the carbon coating layer. In one embodiment of the present invention, the carbon coating layer is thinned to improve the interaction between the transition metal particles and the lithium polysulfide, which can have a beneficial effect on the catalytic activity of the transition metal particles, but the present invention is not limited thereto.
[0095] In one embodiment of the present invention, the ratio of the thickness of the carbon coating layer to the average particle size of the transition metal composite particles may be 1 to 40%, 1 to 25%, 5 to 20%, or 10 to 20%.
[0096] If the transition metal particles are supported on the carbon composite without being covered with a carbon coating layer, the transition metal particles are formed to have non-uniform sizes, which significantly reduces the stability of the catalyst. As a result, when a battery is driven using the transition metal particles, the battery life stability is deteriorated.
[0097] From this viewpoint, in one embodiment of the present invention, the carbon coating layer may cover the entire surface of the core portion of the transition metal composite particle.
[0098] In one embodiment of the present invention, the carbon coating layer may have a thickness of, for example, 10 nm or less. Specifically, the carbon coating layer may have a thickness of 5 nm or less. In one embodiment of the present invention, the carbon coating layer may have a thickness of, for example, 0.5 nm or more. More specifically, the carbon coating layer may have a thickness of, for example, 1 nm to 5 nm, or 0.5 nm to 2 nm.
[0099] The thickness of the carbon coating layer can be measured by, for example, observing a SEM image, a TEM image, or the like of the carbon composite with a microscope; however, the method for measuring the thickness of the carbon coating layer is not limited thereto.
[0100] In this specification, unless otherwise specified, SEM images can be obtained using a Hitachi S-4800 field emission scanning electron microscope, and TEM images can be obtained using a Tecnai G2 F30 S-Twin.
[0101] In one embodiment of the present invention, the carbon coating layer may be composed of one single layer.
[0102] In another embodiment of the present invention, the carbon coating layer may be formed of a multi-layer structure of two or more layers. For example, the carbon coating layer may be formed of a multi-layer structure of two to five layers, a multi-layer structure of two to four layers, or a multi-layer structure of two to three layers. When the carbon coating layer is formed of a multi-layer structure, an advantageous effect can be expected in terms of the catalytic activity of the carbon composite, but the present invention is not limited thereto.
[0103] In another embodiment of the present invention, the carbon coating layer has a multilayer structure of two to three layers that covers the entire surface of the core portion of the transition metal composite particle, has a total thickness of 5 nm or less, and can be composed of crystalline carbon doped with at least one nitrogen element.
[0104] The transition metal composite particle, which includes a core portion including the above-mentioned transition metal particles and a carbon coating layer covering at least a part of the surface of the core portion, is a catalyst that provides activity for the oxidation and reduction of sulfur, and is located on at least one of the outer surface and the inner surface of the pores of the porous carbon substrate.
[0105] In one embodiment of the present invention, the shape of the transition metal composite particle can correspond to the shape of the transition metal particle contained in the core portion, and can be, for example, spherical, elliptical, sheet-like, plate-like, fibrous, needle-like, or hollow.
[0106] In one embodiment of the present invention, the transition metal composite particles have an average particle diameter (D 50 ) may be 1 nm to 90 nm, more specifically 5 nm to 40 nm, 5 nm to 30 nm, 5 nm to 25 nm, or 10 nm to 20 nm, and may include a carbon coating layer covering the surface of the core portion with a thickness of 40% or less, more specifically 25% or less, 20% or less, 15% or less, 10% or less, or 5% or less of the average particle size of the transition metal composite particle.
[0107] In another embodiment of the present invention, the average particle size (D 50) may be, for example, 2 nm to 100 nm, 2 nm to 90 nm, 5 nm to 80 nm, 5 nm to 75 nm, 5 nm to 60 nm, 5 nm to 50 nm, 5 nm to 40 nm, 5 nm to 30 nm, 5 nm to 25 nm, 5 nm to 21 nm, 10 nm to 21 nm, or 11 nm to 21 nm. When the size of the transition metal composite particles is within the above range, the conductivity of electrons and / or ions is excellent, which can improve the performance of the battery and provide advantageous effects in the manufacturing process, but the present invention is not limited thereto.
[0108] In one embodiment of the present invention, the porous carbon substrate has a function of a support for improving the electrical conductivity of the transition metal composite particles and providing the transition metal composite particles as a component of an electrode.
[0109] In the present invention, the transition metal composite particles can be used alone as a catalyst in the positive electrode of a lithium-sulfur battery to activate the reduction reaction of lithium polysulfide. However, according to the present invention, the transition metal composite particles are located on the outer surface and / or the inner surface of the pores of the porous carbon substrate, thereby exhibiting the effect of further improving the adsorption of lithium polysulfide and the activation of the oxidation / reduction reaction of sulfur.
[0110] The porous carbon substrate is a material containing a large number of micropores, and the transition metal composite particles are supported on at least one of the outer surface of the porous carbon substrate and the inner surfaces of the pores.
[0111] In one embodiment of the present invention, the porous carbon substrate may contain at least one different element as a doping element in addition to carbon. Specifically, the different element may include one or more elements selected from the group consisting of nitrogen (N), sulfur (S) and oxygen (O).
[0112] Specifically, in one embodiment of the present invention, at least one carbon atom present in the porous carbon substrate and / or the carbon coating layer may have a structure in which it is substituted with the different element.
[0113] In another aspect of the invention, when both the porous carbon substrate and the carbon coating layer in the transition metal composite particle contain at least one different element as a doping element in addition to carbon, the different elements may be derived from the same precursor, as described below, and therefore may contain the same element as each other.
[0114] In another embodiment of the present invention, the heterogeneous elements contained in the porous carbon substrate and the carbon coating layer may each independently include one or more elements selected from nitrogen, sulfur, and oxygen. Specifically, the heterogeneous elements doped in the porous carbon substrate may be derived from a precursor different from the heterogeneous elements contained in the carbon coating layer. For example, the porous carbon substrate may be doped with a precursor containing one or more elements selected from nitrogen, sulfur, and oxygen in order to improve the binding strength with the transition metal composite particles or the binding strength with lithium polysulfide in the electrolyte, and then mixed with the transition metal particles to form a carbon composite.
[0115] In one embodiment of the present invention, the transition metal composite particles may be chemically and / or physically bonded to at least one of the outer surface and the inner surfaces of the pores of the porous carbon substrate.
[0116] In one embodiment of the present invention, the transition metal composite particles may be physically adsorbed on the outer surface and / or the inner surface of the pores of the porous carbon substrate. Alternatively, the transition metal composite particles may be chemically bonded to the outer surface and / or the inner surface of the pores of the porous carbon substrate by C-C covalent bonds and / or pi-pi interactions between the elements present in the transition metal composite particles and the carbon of the porous carbon substrate. In addition, the above-mentioned physical adsorption and chemical bonds may simultaneously exist between the transition metal composite particles and the porous carbon substrate.
[0117] In one embodiment of the present invention, the porous carbon substrate includes a large number of micropores on the outer surface and inside. The average diameter (D 50 ) may be, for example, 5 nm to 100 nm, specifically 5 nm to 80 nm, 5 nm to 60 nm, or 5 nm to 50 nm. The average diameter (D50) of the micropores indicates the diameter of the pores at a point where the pore size distribution is 50%. The pore diameter can be measured, for example, by TEM analysis of the diameter of the pores in the direction perpendicular to the surface of the porous carbon substrate, but the measurement method is not limited thereto.
[0118] The material of the porous carbon substrate is not particularly limited as long as it contains a large number of fine pores as described above and can support the transition metal composite particles.
[0119] In one embodiment of the present invention, the material of the porous carbon substrate may include, for example, carbon nanotubes (CNTs), graphene, graphene oxide (GO), reduced graphene oxide (rGO), carbon black, graphite nanofibers (GNFs), carbon nanofibers (CNFs), activated carbon fibers (ACFs), natural graphite, artificial graphite, expanded graphite, activated carbon, fullerene, or two or more of these.
[0120] In one embodiment of the present invention, when the porous carbon substrate comprises carbon nanotubes as a material, the carbon nanotubes may comprise single-walled carbon nanotubes (SWCNTs), multi-walled carbon nanotubes (MWCNTs), or both.
[0121] In another aspect of the present invention, when the porous carbon substrate contains carbon nanotubes as a material, the carbon nanotubes may include entangled carbon nanotubes (entangled CNTs) formed as a secondary structure by agglomeration of a plurality of primary structures having carbon nanotubes as a primary structure.
[0122] According to one aspect of the present invention, the entangled carbon nanotubes may have the characteristic of having improved porosity compared to the primary structure carbon nanotubes due to the interstitial volume formed when the primary structure carbon nanotubes are entangled.
[0123] In one embodiment of the present invention, the size of the porous carbon substrate may be, for example, 10 μm to 100 μm, specifically, 20 μm to 50 μm, but is not limited thereto. When the size of the porous carbon substrate is within the above range, advantageous effects can be exhibited in terms of solid content adjustment and electrode properties, such as adhesive strength and battery performance (output, capacity, etc.), in the preparation of a slurry for forming an electrode active material layer.
[0124] In one embodiment of the present invention, the pore volume of the porous carbon substrate is, for example, 1 cm 3 / g~5cm 3 / g, specifically 1cm 3 / g~4cm 3 The pore volume may be a value calculated or measured by, for example, N2 isotherm analysis obtained based on the adsorption of liquid nitrogen.
[0125] In one embodiment of the present invention, the BET specific surface area of the porous carbon substrate is, for example, 150 m 2 / g~2,000m 2 / g, specifically 250m 2 / g~700m 2 / g, but is not limited thereto.
[0126] The BET specific surface area is measured by the BET method and may indicate a value measured according to a known method for measuring a BET specific surface area. For example, the BET specific surface area may be a value calculated from the amount of nitrogen gas adsorbed at liquid nitrogen temperature (77K) using BELSORP-mini II manufactured by BEL Japan.
[0127] As described above, one aspect of the present invention provides a carbon composite including the transition metal composite particles on at least one of an outer surface of the porous carbon substrate and inner surfaces of the pores.
[0128] In one embodiment of the present invention, the carbon composite has an average particle size (D 50 The carbon composite may have a thickness of, for example, 0.5 cm 3 / g~4cm 3 / g, specifically 1cm 3 / g~3cm 3 The carbon composite may have a pore volume of, for example, 150 m 2 / g~500m 2 / g, specifically 250m 2 / g~300m 2 / g.
[0129] In one embodiment of the present invention, the content of the transition metal composite particles may be, for example, 15% by weight or less, based on 100% by weight of the entire carbon composite. Specifically, the content of the transition metal composite particles may be 5% by weight to 15% by weight. When the content of the transition metal composite particles is within the above range, it is possible to sufficiently secure positions that exhibit catalytic activity, while exhibiting advantageous effects in terms of electron and / or ion conductivity (electrical conductivity) in the electrode. Therefore, it is possible to exhibit excellent effects in terms of improving the performance of a battery using this, but the present invention is not limited thereto.
[0130] In another embodiment of the present invention, the weight ratio of the porous carbon substrate to the transition metal composite particles in the carbon composite may be, for example, 95:5 to 70:30. Specifically, the weight ratio of the porous carbon substrate to the transition metal composite particles may be 90:10 to 80:20, or 95:5 to 85:15. When the weight ratio of the porous carbon substrate to the transition metal composite particles is within the above range, it is possible to exert an effect of improving the resistance characteristics by improving the aggregation phenomenon between the transition metal composite particles while sufficiently securing the positions exhibiting catalytic activity. Therefore, it is possible to exert an excellent effect in terms of improving the performance of the battery using this, but the present invention is not limited thereto.
[0131] In one embodiment of the present invention, the carbon composite contains a heterogeneous element in at least one of the porous carbon substrate and the carbon coating layer. In one embodiment of the present invention, the content of the heterogeneous element may be, for example, 0.1% by weight or more or 0.5% by weight or more, based on 100% by weight of the carbon composite. In addition, the content of the heterogeneous element may be, for example, 20% by weight or less or 10% by weight or less, based on 100% by weight of the carbon composite, but is not limited thereto. Specifically, the content of the heterogeneous element may be, for example, 0.1% by weight to 20% by weight, specifically 0.5% by weight to 10% by weight, based on 100% by weight of the entire carbon composite. When the content of the heterogeneous element is within the above range, it is possible to exhibit an advantageous effect in terms of adsorbing lithium polysulfide while promoting the catalytic activity of transition metal.
[0132] In one embodiment of the present invention, as described above, the core portion of the transition metal composite particle comprises a transition metal particle formed by bonds between transition metal atoms.
[0133] In another embodiment of the present invention, the carbon composite may further contain a transition metal element liberated from the transition metal particles in a monoatomic state, to the extent that the catalytic activity of the carbon composite is not impaired.
[0134] The form in which the transition metal atom is contained in the carbon composite can be confirmed, for example, by extended X-ray absorption fine structure (EXAFS) analysis. Specifically, when the transition metal atom in the transition metal particle in the carbon composite is not metallically bonded and is contained in a single atomic state, the result of EXAFS analysis confirms the bond between the transition metal element and the different element. On the other hand, when two or more transition metal atoms are metallically bonded to each other and contained in a metallic particle state, the result of EXAFS analysis confirms the bond between the transition metal elements.
[0135] In one embodiment of the present invention, when bonds between elements in the carbon composite are confirmed by EXAFS analysis, the carbon composite may include bonds between the transition metal elements in a number greater than the number of bonds between the transition metal element and the dissimilar element.
[0136] In another embodiment of the present invention, when bonds between elements in the carbon composite are confirmed by EXAFS analysis, the peak intensity indicating bonds between the transition metal elements may be, for example, 10 times or more, specifically 20 times or more, and more specifically 50 times or more, higher than the peak intensity indicating bonds between the transition metal element and a heterogeneous element.
[0137] The carbon composite of the present invention as described above provides binding sites with lithium polysulfide, and exhibits catalytic activity for the oxidation-reduction reaction of sulfur. At the same time, the lithium sulfide formed on the surface is formed into a three-dimensional shape, and thus can have the effect of improving the life characteristics of a lithium-sulfur battery using the carbon composite; however, the mechanism of the present invention is not limited to this.
[0138] According to one aspect of the present invention, the carbon composite is a support that supports a sulfur-based compound that is a positive electrode active material, and may be further composited with the sulfur-based compound to be used as a positive electrode active material, or the carbon composite itself may be used as an additive for a positive electrode.
[0139] According to one aspect of the present invention, the carbon composite may be used as an additive in a separator for a lithium-sulfur battery.
[0140] Another aspect of the present invention provides a method for producing the above carbon composite.
[0141] A method for producing a carbon composite according to another aspect of the present invention includes a step of mixing a transition metal-containing precursor, a carbon precursor, and a porous carbon substrate, followed by heat treatment. Specifically, the transition metal-containing precursor includes at least one of cobalt (Co) and iron (Fe), and the carbon precursor includes one or more different elements selected from nitrogen (N), sulfur (S), and oxygen (O).
[0142] First, the transition metal-containing precursor contains at least one of cobalt (Co) and iron (Fe) as a precursor for forming the transition metal particles contained in the core portion of the transition metal composite particle.
[0143] In one embodiment of the present invention, the transition metal-containing precursor may include a metal salt, a metal acetyl acetonate, a metal hydroxide, a metal chloride, a metal oxide, a metal chloride hydrate, or two or more of these that contain the transition metal element.
[0144] In another embodiment of the present invention, the transition metal-containing precursor may contain only a metal salt containing the transition metal element. By containing only the metal salt as the transition metal-containing precursor, the method for producing the transition metal composite particle can be simplified, and the size of the produced transition metal composite particle can be easily controlled, which is advantageous in terms of improving the catalytic activity.
[0145] In one embodiment of the present invention, the transition metal-containing precursor may include, as a cobalt metal salt, for example, cobalt acetyl acetonate, cobalt hydroxide, cobalt chloride, cobalt oxide, cobalt chloride hydrate, or two or more of these.
[0146] In one embodiment of the present invention, the transition metal-containing precursor may include cobalt chloride hexahydrate as a cobalt metal salt.
[0147] In one embodiment of the present invention, the transition metal-containing precursor may include, as an iron metal salt, for example, iron acetyl acetonate, iron hydroxide, iron chloride, iron oxide, iron chloride hydrate, or two or more of these.
[0148] In one embodiment of the present invention, the transition metal-containing precursor may include iron chloride hexahydrate as an iron metal salt.
[0149] In one embodiment of the present invention, the transition metal-containing precursor may further include a precursor containing other transition metal elements in addition to the precursor providing cobalt and / or iron. In this case, the transition metal elements that may be further included are, for example, one or more selected from zinc (Zn), vanadium (V), chromium (Cr), manganese (Mn), nickel (Ni), copper (Cu), zirconium (Zr), niobium (Nb), molybdenum (Mo), technetium (Tc), rubidium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), lanthanum (La), hafnium (Hf), tantalum (Ta), tungsten (W), osmium (Os), iridium (Ir), cerium (Ce), gadolinium (Gd), scandium (Sc), titanium (Ti), gallium (Ga), and indium (In).
[0150] In another embodiment of the present invention, the transition metal-containing precursor may further include a nickel metal salt, such as nickel acetyl acetonate, nickel hydroxide, nickel chloride, nickel oxide, nickel chloride hydrate, or two or more of these.
[0151] In one embodiment of the present invention, the carbon precursor is a precursor for forming a carbon coating layer for covering at least a portion of the surface of the transition metal particles.
[0152] In the present invention, the carbon precursor contains at least one different element selected from nitrogen, sulfur, and oxygen, and thus can function as a precursor for doping at least one of the carbon coating layer and the porous carbon substrate with the different element.
[0153] In one aspect of the present invention, the carbon precursor contains, in addition to carbon, one or more heteroelements selected from nitrogen, sulfur, and oxygen, as described above, and the carbon precursor is not particularly limited as long as it can be carbonized to provide a crystalline carbon coating layer.
[0154] The carbon precursor may include, for example, carbon and nitrogen elements, such as dopamine, polydopamine, melamine, 1,10-phenanthroline, polyaniline, carbon nitride (g-CN), glucose, phenylenediamine, or a mixture thereof.
[0155] In one embodiment of the present invention, the above description is incorporated with respect to the porous carbon substrate.
[0156] The method for producing the carbon composite includes the steps of mixing the transition metal-containing precursor, the carbon precursor and the porous carbon substrate, and heat treating the mixture.
[0157] In one embodiment of the present invention, the weight ratio of the transition metal-containing precursor to the carbon precursor can be, for example, 1:0.5 to 1:5, specifically 1:0.5 to 1:2, and more specifically 1:0.5 to 1:1.
[0158] In one embodiment of the present invention, the weight ratio of the transition metal-containing precursor to the porous carbon substrate can be, for example, 1:1 to 1:10, specifically 1:3 to 1:8, and more specifically 1:3 to 1:7.
[0159] In one embodiment of the present invention, the weight ratio of the carbon precursor to the porous carbon substrate can be, for example, 0.5:10 to 5:1, specifically 0.5:8 to 2:3, and more specifically 0.5:7 to 1:3.
[0160] In one embodiment of the present invention, the weight ratio of the transition metal-containing precursor, the carbon precursor, and the porous carbon substrate may be, for example, 1:0.5 to 5:1 to 10, specifically 1:0.5 to 2:3 to 8, and more specifically 1:0.5 to 1:3 to 7. When the weight ratio of the transition metal-containing precursor, the carbon precursor, and the porous carbon substrate is within the above range, an advantageous effect can be exhibited in terms of the performance of the produced carbon composite, but the present invention is not limited thereto.
[0161] In one aspect of the present invention, the method for producing the carbon composite may include a step of first mixing the transition metal-containing precursor and the carbon precursor, then mixing the porous carbon substrate, and heat treating the mixture. When the transition metal-containing precursor and the carbon precursor are first mixed, and then the porous carbon substrate is mixed, in order to produce the carbon composite, it may have an advantageous effect in terms of the uniformity of the thickness of the carbon coating layer and the uniformity of the size of the transition metal composite particles, but the present invention is not limited thereto.
[0162] According to one aspect of the present invention, the method for producing the carbon composite includes the steps of: (S1) mixing the transition metal-containing precursor and the carbon precursor to produce a metal-carbon precursor complex; (S2) mixing the metal-carbon precursor composite and the porous carbon substrate to prepare a metal-carbon-substrate precursor composite (MC-substrate precursor complex); (S3) heat treating the metal-carbon-substrate precursor composite.
[0163] The step (S1) is for producing a metal-carbon precursor complex (MC precursor complex) in which, when the transition metal-containing precursor and the carbon precursor are mixed, transition metal particles are formed from the transition metal-containing precursor and a carbon precursor is bonded to the surface of the transition metal particles by physical and / or chemical bonds.
[0164] In one embodiment of the present invention, the transition metal-containing precursor and the carbon precursor are mixed in a suitable solvent and may be stirred. In this case, when the transition metal-containing precursor is a metal salt containing a transition metal element, the solvent is preferably water, but is not limited thereto.
[0165] In one embodiment of the present invention, the mixing in step (S1) may be carried out at room temperature, for example, 23°C to 25°C.
[0166] In one embodiment of the present invention, when stirring is performed during the mixing in step (S1), the stirring may be performed, for example, at 200 rpm to 250 rpm, specifically, at 220 rpm to 240 rpm. When the stirring is performed under the above-mentioned conditions, an advantageous effect can be obtained in terms of uniformity of the size of the generated transition metal particles, but the present invention is not limited thereto.
[0167] In one embodiment of the present invention, in the step (S1), the solution in which the transition metal-containing precursor and the carbon precursor are mixed may have a solid content of, for example, 10% by weight to 50% by weight.
[0168] In one embodiment of the present invention, the transition metal-containing precursor and the carbon precursor may be mixed, for example, in a molar ratio of 1:2 to 2:1, specifically, in a molar ratio of 1:1. When the molar ratio of the transition metal-containing precursor and the carbon precursor is within the above range, an advantageous effect can be exhibited in terms of the uniformity of the thickness and size of the carbon coating layer on the surface of the transition metal composite particles produced, but the present invention is not limited thereto.
[0169] The step (S2) is for producing a metal-carbon-substrate precursor complex in which the metal-carbon precursor composite produced above is supported on at least one of the outer surface and the inner surfaces of the pores of the porous carbon substrate.
[0170] In one embodiment of the present invention, the metal-carbon precursor composite produced above may be present in a form dispersed in the solvent used in step (S1), for example, water, and a dispersion in which the metal-carbon precursor composite and the porous carbon substrate are dispersed may be produced by adding the porous carbon substrate to a dispersion in which the metal-carbon precursor composite is dispersed.
[0171] In one embodiment of the present invention, for producing the metal-carbon-substrate precursor composite, the pH of the dispersion in which the metal-carbon precursor composite and the porous carbon substrate are dispersed may be, for example, 8 to 9.
[0172] In another aspect of the present invention, the step (S2) may further include a step of adding a pH adjuster to adjust the acidity of the mixture of the metal-carbon precursor composite and the porous carbon substrate, for example, a dispersion in which the metal-carbon precursor composite and the porous carbon substrate are dispersed.
[0173] The pH adjuster may be a basic or acidic compound, depending on the pH of the dispersion produced.
[0174] In one embodiment of the present invention, the pH adjuster may include a basic compound, and the basic compound may be, for example, an amine compound. The amine compound may include, for example, tris(hydroxymethyl)aminomethane (TRIS).
[0175] In another embodiment of the present invention, the pH adjuster may include an acidic compound, which may be, for example, an organic carboxylic acid. The organic carboxylic acid may include, for example, formic acid, acetic acid, propionic acid, butyric acid, pivalic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, acrylic acid, benzoic acid, phthalic acid, or two or more of these.
[0176] In one embodiment of the present invention, when the process further includes a step of adding the pH adjuster, the pH adjuster may be added in an amount of 100 to 800 parts by weight, for example, 200 to 700 parts by weight or 300 to 600 parts by weight, specifically, 300 to 400 parts by weight or 300 to 350 parts by weight, relative to 100 parts by weight of the transition metal-containing precursor used in step (S1), but is not limited thereto.
[0177] In one embodiment of the present invention, the step (S2) may be accompanied by stirring. The stirring may be performed, for example, at room temperature for 12 hours to 48 hours, specifically 20 hours to 30 hours, for example, 24 hours.
[0178] In one embodiment of the present invention, the step (S2) may further include a step of filtering and washing the metal-carbon precursor composite and the porous carbon substrate after mixing the metal-carbon precursor composite and the porous carbon substrate.
[0179] In one embodiment of the present invention, the washing may be performed using, for example, water, an organic solvent, or a mixture thereof. In one embodiment of the present invention, the washing may be performed by a method in which washing is performed 1 to 3 times with water and then once with an alcohol-based organic solvent such as ethanol, but the present invention is not limited thereto. In one embodiment of the present invention, the step (S2) may further include the steps of filtering, washing, and drying the metal-carbon precursor composite and the porous carbon substrate after mixing the metal-carbon precursor composite and the porous carbon substrate.
[0180] In one embodiment of the present invention, the drying may be carried out, for example, in vacuum at a temperature of 50°C to 70°C, specifically 60°C.
[0181] The step (S3) is for producing a carbon composite supported with transition metal composite particles, the transition metal composite particles including a core part including transition metal particles and a carbon coating layer covering at least a part of the surface of the core part, on at least one of the outer surface of the porous carbon substrate and the inner surface of the pores by heat-treating the metal-carbon-substrate precursor composite produced above. The heat treatment can dope at least one of the porous carbon substrate and the carbon coating layer with a different element contained in the carbon precursor.
[0182] In one embodiment of the present invention, the heat treatment may be performed at a temperature of, for example, 600°C to 1,000°C. Specifically, the heat treatment may be performed at a temperature of 750°C to 850°C, for example, 800°C.
[0183] In one embodiment of the present invention, the heat treatment can involve increasing the temperature at a constant rate selected from the range of 0.5° C. / min to 2° C. / min.
[0184] In one embodiment of the present invention, the heat treatment may be carried out while increasing the temperature at a rate of 1° C. / min.
[0185] According to the above-described method, the above-mentioned carbon composite can be produced.
[0186] According to still another aspect of the present invention, there is provided a positive electrode active material including the above-mentioned carbon composite and a sulfur-based compound, and a positive electrode including the same.
[0187] The positive electrode may include, as a positive electrode active material, a composite formed by using the above-mentioned carbon composite as a support for a positive electrode active material and mixing the carbon composite with a sulfur-based compound as a positive electrode active material.
[0188] In one embodiment of the present invention, the sulfur-based compound may be, for example, sulfur (S8), lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 2≦x≦8), a disulfide compound, or a mixture of two or more of these, but is not limited thereto.
[0189] In one embodiment of the present invention, the carbon composite and the sulfur-based compound may be mixed, for example, in a content ratio of 1:9 to 9:1. Specifically, the carbon composite and the sulfur-based compound may be mixed in a content ratio of 1:9 to 5:5, more specifically, 2:8 to 4:6.
[0190] In one embodiment of the present invention, the positive electrode active material may be formed by mixing the carbon composite and a sulfur-based compound, followed by heat treatment. The heat treatment may be performed at a temperature of, for example, 130° C. to 200° C., specifically, 130° C. to 180° C. or 150° C. to 160° C.
[0191] In one aspect of the present invention, the positive electrode for a lithium-sulfur battery may further include a binder in addition to the positive electrode active material including the carbon composite and the sulfur-based compound. The binder is not particularly limited as long as it is a binder that can be used in a positive electrode of a lithium-sulfur battery.
[0192] In one embodiment of the present invention, the binder may include, for example, poly(vinylidene fluoride) (PVDF), and more particularly, may include PVDF dispersed in N-methyl-2-pyrrolidone (NMP). In another embodiment of the invention, the binder may include an aqueous binder such as, for example, styrene butadiene rubber (SBR), and in particular, may include an aqueous binder dispersed in an aqueous solvent such as water.
[0193] In another embodiment of the present invention, the positive electrode for a lithium-sulfur battery may further include, in addition to the positive electrode active material and the binder, a conductive material, an additive, etc. In this case, the specific types of the binder, the conductive material, and the additive may be conventional ones, and therefore the description thereof will be omitted.
[0194] In yet another aspect of the present invention, the positive electrode for a lithium-sulfur battery may include a positive electrode current collector and a positive electrode active material layer in which the positive electrode active material is applied to one or both sides of the current collector together with a binder.
[0195] In this case, the positive electrode current collector is not particularly limited as long as it has high conductivity and does not cause chemical changes in the battery.
[0196] In one embodiment of the present invention, a positive electrode containing the carbon composite can exhibit excellent effects in terms of initial capacity and cycle stability, but the effects of the present invention are not limited thereto.
[0197] In one embodiment of the present invention, the positive electrode for a lithium-sulfur battery has a composition of, for example, 2 mg / cm 2 Specifically, 2.0 mg / cm 2 ~2.5mg / cm 2 The sulfur (S) loading may be
[0198] A lithium-sulfur battery according to yet another aspect of the present invention includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the positive electrode includes the carbon composite described above as a positive electrode active material and a sulfur-based compound.
[0199] In one embodiment of the present invention, the negative electrode and the separator are not particularly limited as long as they can be used in a lithium-sulfur battery within a range that does not impair the object of the present invention.
[0200] In one embodiment of the present invention, the negative electrode may be, for example, lithium metal.
[0201] In one embodiment of the present invention, the separator is not particularly limited as long as it is one that can be generally used as a separator for lithium-sulfur batteries.
[0202] In one embodiment of the present invention, the separator may include a porous polyolefin substrate, and may further include inorganic particles on at least one surface of the porous polyolefin substrate, and may further include a binder that binds the inorganic particles, as necessary.
[0203] In another embodiment of the present invention, the separator may be a film-like electrolyte membrane containing a solid electrolyte, and may further contain a binder for binding the solid electrolyte as necessary. The solid electrolyte is not particularly limited as long as it is one that can be normally used in lithium-sulfur batteries, such as a polymer solid electrolyte, an inorganic solid electrolyte, or a mixed composition thereof.
[0204] In one embodiment of the present invention, the electrolyte includes those typically used in lithium-sulfur batteries. The electrolyte may include a lithium salt and a non-aqueous solvent.
[0205] The lithium salt is not particularly limited as long as it is one that can be normally used in the electrolyte of a lithium-sulfur battery. Examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (C2F5SO2)2NLi, (SO2F)2NLi, (CF3SO2)3CLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium 4-phenylborate, lithium imide, or two or more of these.
[0206] The non-aqueous solvent is not particularly limited as long as it is one that can be normally used in the electrolyte of a lithium-sulfur battery. The non-aqueous solvent may include, for example, a cyclic carbonate solvent, a linear carbonate solvent, an ester solvent, a ketone solvent, or a mixed solvent of two or more of these, but is not limited thereto.
[0207] In one embodiment of the present invention, the electrolyte may include (CF3SO2)2NLi as a lithium salt and a dioxolane (DOL) / dimethoxyethane (DME) binary system as a non-aqueous solvent. For example, the electrolyte may further include a common additive such as LiNO3.
[0208] In one embodiment of the present invention, the lithium-sulfur battery may have an outer shape, such as, but not limited to, a coin type, a cylindrical type, a pouch type, or a rectangular type. The lithium-sulfur battery can be used not only as a battery cell used as a power source for a small device, but also as a unit battery for a medium- to large-sized battery module including a plurality of battery cells, and the form of use is not particularly limited.
[0209] In one aspect of the present invention, a lithium-sulfur battery using a positive electrode containing the carbon composite has excellent kinetic activity for a sulfur oxidation-reduction reaction, and can also exhibit excellent effects in terms of initial capacity and cycle stability of the battery, but the effects of the present invention are not limited thereto.
[0210] In one aspect of the present invention, the lithium-sulfur battery can exhibit an effect of improving the energy density by increasing the sulfur loading amount in the electrode, but the effect of the present invention is not limited thereto.
[0211] In one embodiment of the present invention, the lithium-sulfur battery may have an electrolyte / sulfur (E / S) ratio of, for example, 10 μL / mg or less. Conventionally, there was a limit to lowering the E / S ratio due to low activity of the positive electrode, but the present invention has an effect of stably lowering the E / S ratio, so that the E / S ratio of the lithium-sulfur battery may have a value larger than the above range, and it is obvious to those skilled in the art that the lower limit is not limited, and the present invention is not limited thereto.
[0212] According to still another aspect of the present invention, there are provided a positive electrode active material including a sulfur-based compound, a positive electrode including the above-mentioned carbon composite as a positive electrode additive, and a lithium-sulfur battery including the same.
[0213] In one aspect of the present invention, in addition to the aspect of the present invention in which the carbon composite is included in a positive electrode in the form of a positive electrode active material formed by compounding a sulfur-based compound with the carbon composite as a support, the carbon composite can be included as an additive separately from the positive electrode active material.
[0214] In one aspect of the present invention, when the carbon composite is used as a positive electrode additive, not only can the capacity of a battery be improved, but also the reactivity with lithium polysulfide is improved, so that the effect of improving the performance of the battery can be expected.
[0215] In one embodiment of the present invention, when the carbon composite is used as a positive electrode additive, the carbon composite may be included in an amount of 1 to 25 wt %, for example, 1 to 15 wt %, or 1 to 10 wt %, based on the total weight of the positive electrode active material, the binder, and the carbon composite included in the positive electrode active material layer, but is not limited thereto.
[0216] In one aspect of the present invention, the positive electrode may be a sulfur-based compound or a common carbon support having the sulfur-based compound supported thereon as a positive electrode active material. The sulfur-based compound is the same as the configuration of the positive electrode according to the above aspect of the present invention. The common carbon support may be, for example, the porous carbon substrate itself, but is not limited thereto.
[0217] The lithium-sulfur battery according to one aspect of the present invention can be used, for example, in an electric vehicle (EV), a drone, or urban air mobility (UAM), but the application of the present invention is not limited thereto.
[0218] Hereinafter, a method for producing a carbon composite and a method for producing a positive electrode active material using the carbon composite according to one embodiment of the present invention will be described in detail with reference to examples. However, the following examples are provided for the purpose of illustrating the present invention, and the scope of the present invention is not limited thereto.
[0219] [Manufacturing of carbon composites] Carbon composites according to Examples 1 to 4 and Comparative Examples 1 to 4 were prepared using the compositions in Table 1 below and according to the methods described below.
[0220] [Table 1]
[0221] Example 1 (FeC@CNT) First, as shown in the composition in Table 1, ferric chloride hydrate (FeCl2·6H2O, 99%, Sigma-Aldrich) and dopamine hydrochloride (98 wt%, Sigma-Aldrich) were added in a molar ratio of 1:1 to 500 mL of distilled water, and the mixture was stirred at 230 rpm for 30 minutes at room temperature (23°C) to produce an iron-carbon precursor complex (Fe-C precursor complex).
[0222] A certain amount of multi-walled carbon nanotubes (MWCNTs) (BET specific surface area 275 m / g, Carbon Nano-material Technology Co., LTD) was added to the mixture and stirred at room temperature for 30 minutes to produce a dispersion. Next, a certain amount of Trizma base (tris(hydroxymethyl)aminomethane, TRIS) was added to the prepared dispersion to maintain the pH at 8.5. The obtained dispersion was stirred at room temperature for 24 hours, filtered, washed three times with distilled water and once with ethanol, and then dried at 60°C to produce an iron-carbon-CNT precursor complex (Fe-C-CNT precursor complex).
[0223] The produced iron-carbon-CNT precursor composite was placed in a tubular electric furnace under an argon atmosphere and heat-treated at 800°C for 2 hours (heating rate 1°C / min) to produce a carbon composite (D 50 The carbon composite thus obtained contained a porous carbon substrate made of multi-walled carbon nanotubes (MWCNTs); transition metal composite particles located on at least one of the outer surface of the MWCNTs and the inner surface of the pores, the core portion including iron particles, and a carbon coating layer covering at least a part of the surface of the core portion; and doped nitrogen element. At this time, the average particle size (D 50 The ratio of the thickness of the carbon coating layer to the thickness of the substrate was 15%.
[0224] Example 2 (CoC@CNT) A carbon composite (D) was prepared in the same manner as in Example 1 according to the composition in Table 1, except that CoCl2·6H2O (99%, Sigma-Aldrich) was used instead of FeCl2·6H2O as the metal salt. 50 The carbon composite thus obtained contained a porous carbon substrate made of multi-walled carbon nanotubes (MWCNTs); transition metal composite particles located on at least one of the outer surface of the MWCNTs and the inner surface of the pores, the core portion including cobalt particles, and a carbon coating layer covering at least a part of the surface of the core portion; and doped nitrogen element. At this time, the average particle size (D 50The ratio of the thickness of the carbon coating layer to the thickness of the substrate was 15%.
[0225] Example 3 (CoC@CNT, one-pot method) A carbon composite was produced by simultaneously mixing a transition metal-containing precursor, a carbon precursor, and a porous carbon substrate according to the composition in Table 1 and heat treating the mixture according to the following method.
[0226] First, a fixed amount of cobalt chloride hydrate (CoCl2 6H2O), dopamine hydrochloride (98 wt%), and multi-walled carbon nanotubes (MWCNTs) (BET specific surface area 275 m) were added to 500 mL of distilled water. 2 1000g) and Trizma base (tris(hydroxymethyl)aminomethane, TRIS, TRIS) were added and stirred at 230 rpm for 24 hours at room temperature (23°C), filtered, washed three times with distilled water and once with ethanol, and then dried at 60°C to produce a cobalt-carbon-CNT precursor complex (Co-C-CNT precursor complex).
[0227] The produced cobalt-carbon-CNT precursor composite was placed in a tubular electric furnace under an argon atmosphere and heat-treated at 800°C for 2 hours (heating rate 1°C / min) to obtain a carbon composite. The obtained carbon composite contained a porous carbon substrate made of multi-walled carbon nanotubes (MWCNTs); transition metal composite particles located on at least one of the outer surface of the MWCNTs and the inner surface of the pores, the core portion including cobalt particles, and a carbon coating layer covering at least a part of the surface of the core portion; and doped nitrogen element. At this time, the average particle size (D 50 The ratio of the thickness of the carbon coating layer to the thickness of the substrate was 100% (1:1).
[0228] Example 4 (CoC@CNT, using glucose as carbon precursor) A carbon composite was obtained in the same manner as in Example 2, except that glucose was used instead of dopamine hydrochloride (98 wt%) as the carbon precursor. The obtained carbon composite contained a porous carbon substrate made of multi-walled carbon nanotubes (MWCNTs); transition metal composite particles located on at least one of the outer surface of the MWCNTs and the inner surface of the pores, the core portion including cobalt particles, and a carbon coating layer covering at least a part of the surface of the core portion; and doped oxygen element. In this case, the carbon coating layer was formed only on a part of the surface of the transition metal composite particles, and the thickness of the formed carbon coating layer was approximately equal to the average particle size (D 50 ) was 100% (1:1).
[0229] Comparative Example 1 Without supporting transition metal composite particles, multi-walled carbon nanotubes (MWCNTs) (BET specific surface area 275 m) were used as carbon composites. 2 / g) was produced.
[0230] Comparative Example 2 Carbon composites (D) were prepared in the same manner as in Example 1, using NiCl3·6H2O instead of FeCl2·6H2O as the metal salt, and in accordance with the composition in Table 1. 50 The carbon composite thus obtained contained a porous carbon substrate made of multi-walled carbon nanotubes (MWCNTs); transition metal composite particles, each of which was located on at least one of the outer surface of the MWCNTs and the inner surface of the pores, and which contained a core portion containing nickel particles and a carbon coating layer covering at least a part of the surface of the core portion; and doped nitrogen element. At this time, the ratio of the thickness of the carbon coating layer to the average particle size of the transition metal composite particles was 15%.
[0231] Comparative Example 3 A carbon composite (D 50The carbon composite thus obtained contained a porous carbon substrate made of multi-walled carbon nanotubes (MWCNTs); and transition metal composite particles, the core portion being located on at least one of the outer surface of the MWCNTs and the inner surface of the pores, and including an iron particle-containing core portion and a carbon coating layer covering at least a part of the surface of the core portion. In this case, the ratio of the thickness of the carbon coating layer to the average particle size of the transition metal composite particles was 55%.
[0232] Comparative Example 4 A carbon composite (D 50 The carbon composite thus obtained contained a porous carbon substrate made of multi-walled carbon nanotubes (MWCNTs); and transition metal composite particles, which were located on at least one of the outer surface of the MWCNTs and the inner surface of the pores, and contained a core portion containing cobalt particles, and a carbon coating layer covering at least a part of the surface of the core portion. In this case, the ratio of the thickness of the carbon coating layer to the average particle size of the transition metal composite particles was 55%.
[0233] [Confirmation of carbon composite structure] Microscopic observation of carbon composites TEM images of the carbon composites of Examples 1, 2, and Comparative Example 2 prepared above are shown in FIG. 2a, a TEM image of the carbon composite of Example 3 is shown in FIG. 2b, and an SEM image of the carbon composite of Example 4 is shown in FIG. 2c.
[0234] Referring to FIG. 2a, in the carbon composites of Example 1, Example 2, and Comparative Example 2, transition metal composite particles (the core part is made of transition metal particles, and the shell part is made of a carbon coating layer) are uniformly formed on the surface of the MWCNT, and the average particle size (D 50 ) were 10 nm (Example 1), 20 nm (Example 2), and 30 nm (Comparative Example 2), respectively.
[0235] Furthermore, it was confirmed that in all of Example 1, Example 2 and Comparative Example 2, a carbon coating layer was formed on the surface of the transition metal particles, and the thickness of each carbon coating layer was 1 nm (Example 1), 1 nm (Example 2) and 1 nm (Comparative Example 2), respectively, and the deviation between the thicknesses of the carbon coating layers at 10 randomly measured points was 0.5 nm or less.
[0236] 2b, the carbon composite of Example 3 was formed in a form in which transition metal composite particles (the core part was made of cobalt, and the shell part was made of a carbon coating layer) were partially aggregated on the surface of the MWCNT. As a result of comparing the shapes of the carbon composites of Example 2 and Example 3, it was confirmed that the carbon composite produced as in Example 2 was advantageous in terms of the uniformity of the size of the transition metal composite particles.
[0237] Also, referring to Figure 2c, it was confirmed that the carbon composite of Example 3, which uses glucose as a carbon precursor and contains oxygen as a doping element, had poor uniformity in the thickness of the carbon coating layer formed on the shell of the transition metal composite particle compared to Example 2. In other words, the carbon coating layer of Example 2 had a standard deviation (Δd) of thickness measured at any 10 points of 5 nm or less, whereas the carbon coating layer of Example 3 had thicknesses measured at any 10 points of 10 nm to 100 nm, with a standard deviation (Δd) between thicknesses of 50 nm.
[0238] Confirmation of transition metal particle content A TGA analysis was performed to measure the content of transition metal particles supported on the carbon composites of Example 1, Example 2, and Comparative Example 2 prepared above, and the results are shown in Figure 3. In the TGA analysis, the prepared carbon composites were heated from 100°C to 800°C (heating rate 10°C / min) and the weight loss was measured.
[0239] Referring to FIG. 3, the weight at the point when the temperature change during heating stops corresponds to the weight of the transition metal particles, and therefore it was confirmed that the carbon composites of Example 1, Example 2, and Comparative Example 2 all supported 10 wt % transition metal particles.
[0240] Confirmation of doping with different elements The carbon composites of Example 1, Example 2, and Comparative Example 2 prepared above were subjected to XPS analysis, and the results of confirming the peak of the nitrogen element by XPS analysis are shown in FIG.
[0241] 4, it was confirmed that the carbon composites of Example 1, Example 2, and Comparative Example 2 prepared above contained nitrogen element. The nitrogen element was presumably derived from dopamine as a carbon precursor, and it was confirmed that most of the nitrogen element was contained in the form of graphitic nitrogen and pyridinic nitrogen.
[0242] Confirmation of the bonding form of transition metal elements XPS analysis was performed on the carbon composites of Example 1, Example 2, and Comparative Example 2, and the 2p spectra of each transition metal element were confirmed, and the results are shown in Figure 5a. Referring to Figure 5a, it was confirmed that most of the transition metal elements exist in a metallic state in Example 1 (Fe), Example 2 (Co), and Comparative Example 2 (Ni).
[0243] Furthermore, the carbon composites of Example 1, Example 2, and Comparative Example 2 were subjected to EXAFS analysis to confirm the bonding form of each transition metal element in the carbon composite, and the results are shown in Fig. 5b. In order to facilitate confirmation of the bonding form of the transition metal elements, Fig. 5b shows graphs of Co foil, Fe foil, and Ni foil, which are metal foils made of each transition metal atom, together with graphs of CoO, FeO, and NiO, which are each transition metal oxide showing bonds between the transition metal element and an oxygen atom (O).
[0244] 5b, it was confirmed that the carbon composites of Example 1, Example 2, and Comparative Example 2 all contained more metallic bonds between transition metal elements than bonds between transition metal elements and different elements, suggesting that the catalytic activity of the carbon composites was derived from the transition metal particles.
[0245] [Manufacturing lithium-sulfur batteries] In order to evaluate the performance of a lithium-sulfur battery using the carbon composite produced above, a lithium-sulfur coin-type battery was prepared as follows.
[0246] Cathode manufacturing 30% by weight of each of the carbon composites of Example 1, Example 2, and Comparative Examples 1 to 4 prepared above was mixed with 70% by weight of sulfur (sulfur powder, manufactured by Sigma-Aldrich Corporation) and subjected to isothermal heat treatment at 155° C. for 8 hours to obtain a positive electrode active material.
[0247] To prepare a working electrode, the positive electrode active material prepared above and a polyacrylonitrile binder (PAN binder, LA 132) as a binder were mixed in a weight ratio of 9:1 using NMP (N-methyl-2-pyrrolidone) solvent to prepare a positive electrode slurry.
[0248] The prepared positive electrode slurry was applied to a carbon-coated Al foil and then dried for 8 hours at 60° C. The electrode was then pressed and cut into coins to prepare positive electrodes.
[0249] Battery manufacturing A positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte were housed in a case to manufacture a battery.
[0250] The positive electrode produced above was prepared as the positive electrode, and a porous polypropylene film (Celgard 2400, manufactured by Welcos Co., Ltd.) was prepared as the separator. Lithium metal (200 μm thick) was prepared as the reference electrode and the counter electrode.
[0251] The electrolyte used was a solution of 1,3-dioxolane and dimethoxymethane (DOL / DME) mixed in a 1:1 volume ratio (PANAX E-TEC Co., Korea), containing 1.0 M LiTFSI (lithium salt of bis(trifluoromethane)sulfonamide) as an electrolyte and 2.0 wt% LiNO3 (99.99% metal basis, Sigma-Aldrich) as an additive.
[0252] The sulfur loading in the positive electrode is 2.25 mg / cm 2 and the E / S ratio of the battery was 10 μL / mg.
[0253] The coin-type batteries were manufactured according to the CR2032 standard, and 200 μm thick lithium metal was used as the reference electrode and the counter electrode for the following electrochemical performance experiments.
[0254] [Performance evaluation of lithium-sulfur batteries] Lithium sulfide shape evaluation Chronoamperometry analysis was performed to evaluate the shape of lithium sulfide growing on the surface of the carbon composite when the battery prepared above was operated, and the results are shown in FIG. 6. (a) shows the current-time curve, and (b) shows the relative current-relative time curve. The battery was charged and discharged under conditions of a current density of 0.5C and a voltage range of 1.7V-2.8V. The analysis evaluation was performed in a constant temperature chamber at 25°C using a PESC05-0.1 device manufactured by PNE Solution.
[0255] Referring to FIG. 6(b), in the case of Comparative Example 1 in which CNT was used as the carbon composite and Comparative Example 2 in which a carbon composite supporting Ni metal particles as the transition metal particles was used, the lithium sulfide formed had a planar (2D) shape, whereas in the case of Example 1 in which a carbon composite supporting Fe metal particles as the transition metal particles was used, and in the case of Example 2 in which a carbon composite supporting Co metal particles as the transition metal particles was used, it was confirmed that the lithium sulfide formed had a three-dimensional (3D) shape.
[0256] Moreover, the SEM image of the carbon composite after the first discharge at a current density of 0.05 C is shown in Figure 7 .
[0257] Referring to FIG. 7, it was confirmed that three-dimensional lithium sulfide was formed on the surfaces of the carbon composites of Examples 1 and 2, whereas film-like lithium sulfide was formed on the surfaces of the carbon composites of Comparative Examples 1 and 2.
[0258] Furthermore, referring to FIG. 7, it was confirmed that the size of the lithium sulfide generated in Example 2, in which a carbon composite supporting Co metal particles was used, was smaller than the size of the lithium sulfide generated in Example 1, in which a carbon composite supporting Fe metal particles was used.
[0259] Battery capacity and life evaluation Each battery was charged and discharged 50 times at a voltage of 1.7 V to 2.8 V and a current density of 0.5 C (1 C rate = 1675 mA / g), and the constant current characteristics at this time are shown in Figure 8(a). The capacity-voltage curve for the first charge-discharge cycle is shown in Figure 8(b).
[0260] 8(a), it was confirmed that the carbon composites of Example 1, Example 2, and Comparative Example 1 had stable battery operation after 50 charge / discharge cycles, whereas the battery operation of the carbon composite of Comparative Example 2 became significantly poor after 20 charge / discharge cycles. On the other hand, it was confirmed that the reversible capacity of the battery was highest in the following order: Example 2 (up to 1200mAh / g) > Example 1 (up to 1050mAh / g) > Comparative Example 1 (up to 950mAh / g).
[0261] Referring to FIG. 8(b), the reactivity of the lithium sulfide (Li2S) conversion reaction was evaluated in the order of Example 2>Example 1>Comparative Example 1>Comparative Example 2. In particular, the Q L and Q H Q for H / Q LThe ratios were, respectively, Example 2 (0.409) < Example 1 (0.420) < Comparative Example 1 (0.482) < Comparative Example 2 (0.568), and it was confirmed that the effect of improving the reactivity of the lithium sulfide (LiS) conversion reaction in Example 2 was the most excellent.
[0262] Evaluation of activity with and without carbon coating layer FIG. 9(a) shows a TEM image of the carbon composite of Comparative Example 4, and FIG. 9(b) shows the capacity evaluation results of the batteries produced above using the carbon composites of Comparative Examples 3 and 4 through charge-discharge cycles at 0.5 C.
[0263] First, the carbon composites of Comparative Examples 3 and 4 were manufactured without adding dopamine hydrochloride, i.e., a carbon precursor, during the manufacturing process. Referring to Fig. 9(a), it was confirmed that a plurality of transition metal particles of non-uniform size were supported on the CNTs in the carbon composite of Comparative Example 4.
[0264] Referring to FIG. 9(b), the capacity of the carbon composite of Comparative Example 4 is higher than that of the carbon composite of Comparative Example 3. However, it was confirmed that the capacity of both Comparative Examples 3 and 4 rapidly decreased with increasing charge / discharge cycles, resulting in poor driving stability.
[0265] This confirmed that the carbon coating layer of the transition metal composite particles in the carbon composite according to the present invention is essential for ensuring the driving stability of the battery.
Claims
1. A porous carbon substrate; transition metal composite particles, the core portion being located on at least one of an outer surface of the porous carbon substrate and an inner surface of a pore, the core portion including a transition metal particle, and a carbon coating layer covering at least a part of a surface of the core portion; at least one different element doped into at least one of the porous carbon substrate and the carbon coating layer; The transition metal particles contain at least one of cobalt (Co) and iron (Fe), The different elements include one or more selected from the group consisting of nitrogen (N), sulfur (S) and oxygen (O).
2. The carbon composite body according to claim 1 , wherein the carbon coating layer covers an entire surface of the core portion.
3. The average particle diameter of the transition metal composite particles (D 50 2. The carbon composite of claim 1, wherein a ratio of a thickness of the carbon coating layer to a thickness of the carbon composite is 40% or less.
4. The transition metal particles include zinc (Zn), vanadium (V), chromium (Cr), manganese (Mn), nickel (Ni), copper (Cu), zirconium (Zr), niobium (Nb), molybdenum (Mo), technetium (Tc), rubidium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), lanthanum (La), hafnium (Hf), tantalum (Ta), tungsten (W), osmium (Os), iridium (Ir), cerium (Ce), gadolinium (Gd), scandium (Sc), titanium (Ti), gallium (Ga), and indium (In). The carbon composite according to claim 1, further comprising at least one selected from the group consisting of:
5. The carbon composite according to claim 1 , wherein the transition metal particles have a cobalt content of 95 mol % based on 100 mol % of the transition metal element.
6. The carbon composite according to claim 5 , wherein the transition metal particles have a cobalt element content of 100 mol % based on 100 mol % of the transition metal element.
7. The carbon composite of claim 1 , wherein the transition metal particles are cobalt nanoparticles.
8. The core portion of the transition metal composite particle has an average particle diameter (D 50 2. The carbon composite according to claim 1, wherein the average particle diameter is 1 nm to 90 nm.
9. The carbon composite of claim 1 , wherein the carbon coating layer has a thickness of 10 nm or less.
10. The carbon composite of claim 1 , wherein the carbon coating layer comprises crystalline carbon.
11. The carbon composite according to claim 1 , wherein the carbon coating layer has a single-layer structure or a multi-layer structure of two or more layers.
12. The carbon composite according to claim 11, wherein the carbon coating layer has a single-layer structure of one layer or a multi-layer structure of two to five layers.
13. The carbon composite according to claim 1 , wherein the carbon coating layer contains nitrogen as the different element and has a single-layer structure or a multilayer structure of two to four layers.
14. The transition metal composite particles have an average particle size (D 50 2. The carbon composite according to claim 1, wherein the average particle diameter is 2 nm to 100 nm.
15. 2. The carbon composite of claim 1, wherein the porous carbon substrate comprises carbon nanotubes (CNTs), graphene, graphene oxide (GO), reduced graphene oxide (rGO), carbon black, graphite, graphite nanofibers (GNFs), carbon nanofibers (CNFs), activated carbon fibers (ACFs), activated carbon, fullerenes, or two or more of these.
16. The porous carbon substrate comprises carbon nanotubes (CNTs); 16. The carbon composite of claim 15, wherein the carbon nanotubes comprise entangled carbon nanotubes.
17. 2. The carbon composite according to claim 1, wherein the content of the transition metal composite particles is 15% by weight or less based on 100% by weight of the carbon composite.
18. The carbon composite according to claim 1 , wherein the content of the different element is 10% by weight to 50% by weight based on 100% by weight of the carbon composite.
19. the number of bonds between the transition metal elements in the carbon composite is greater than the number of bonds between the transition metal element and the different element, 2. The carbon composite of claim 1, wherein the bonding between the elements is confirmed by extended X-ray absorption fine structure (EXAFS) analysis.
20. A method for producing a carbon composite according to any one of claims 1 to 19, comprising the steps of: mixing a transition metal-containing precursor, a carbon precursor and a porous carbon substrate and heat treating the mixture; The transition metal-containing precursor contains at least one of cobalt (Co) and iron (Fe); The carbon precursor contains one or more different elements selected from the group consisting of nitrogen (N), sulfur (S) and oxygen (O).
21. The method for producing a carbon composite according to claim 20, wherein the carbon precursor comprises dopamine, polydopamine, melamine, 1,10-phenanthroline, polyaniline, carbon nitride (g-CN), glucose, phenylenediamine, or a mixture thereof.
22. mixing the transition metal-containing precursor and the carbon precursor to prepare a metal-carbon precursor complex; mixing the metal-carbon precursor complex and the porous carbon substrate to prepare a metal-carbon-substrate precursor complex; heat treating the metal-carbon-substrate precursor composite; The method of claim 20 comprising:
23. The method for producing a carbon composite according to claim 20, wherein the heat treatment is carried out at a temperature of 600°C to 1,000°C.
24. A positive electrode active material comprising the carbon composite according to claim 1 and a sulfur-based compound.
25. A positive electrode comprising the positive electrode active material of claim 24.
26. The battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte solution; 26. A lithium-sulfur battery, wherein the positive electrode comprises the positive electrode of claim 25.
27. A positive electrode comprising: a positive electrode active material containing a sulfur-based compound; and the carbon composite according to claim 1 as a conductive material.
28. The battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte solution; 28. A lithium-sulfur battery, wherein the positive electrode is the positive electrode of claim 27.
29. The lithium-sulfur battery has an E / S ratio of 10 μL / mg or less and a sulfur loading of 2 mg / cm 2 The lithium-sulfur battery of claim 28.
30. 30. The lithium-sulfur battery of claim 28, wherein the lithium-sulfur battery is for an electric vehicle (EV), a drone, or an urban air mobility (UAM).
Citation Information
Patent Citations
Iron nitride@nitrogen-doped graphene composite material as well as preparation method and application thereof
CN112264070A
Non-aqueous electrolyte secondary battery
JP2008077990A
Carbon-coated transition metal nanocomposites, their preparation and applications
JP2020528499A
Catalyst for cathode material for lithium secondary battery and lithium secondary battery including same
JP2022505581A
Lithium-sulfur secondary battery
JP2022528136A