Double-sided coated battery separator and battery including same
The double-sided coated battery separator with differential adhesive coatings addresses uneven adhesion issues by using a more adhesive formulation on one side, enhancing uniformity and stability for improved battery capacity and performance.
Patent Information
- Application Number
- JP2024535208
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-13
- Filing Date
- 2022-12-13
- Publication Date
- 2024-11-15
AI Technical Summary
Multilayer coated battery separators (MCS) face issues with uneven adhesion on both sides, leading to reduced adhesion at spots where ceramic particles protrude from the adhesive layer, and the need for improved adhesion uniformity across both sides.
A double-sided coated battery separator design with distinct adhesive coating formulations on each side, where the second coating includes a ceramic and adhesive layer, and the adhesive layer of the second coating is more adhesive than the first, ensuring uniform adhesion and minimizing protrusion of ceramic particles.
The solution enhances adhesion uniformity and stability, allowing for better electrode attachment, reducing electrical resistance, and improving battery performance by accommodating more separators and electrodes in the same space.
Smart Images

Figure 2024542854000001_ABST
Abstract
Description
[Technical field]
[0001] Related Application Data This application claims priority under Article 8 of the Patent Cooperation Treaty and 35 U.S.C. § 119(e) to U.S. Provisional Patent Application No. 63 / 288,823, filed December 13, 2021, which is incorporated herein by reference in its entirety.
[0002] This application is directed to a double-sided coated battery separator, and in particular to an adhesive double-sided coated battery separator. This application is also directed to a secondary battery including the double-sided coated battery separator. [Background technology]
[0003] A multi-layer coated separator (MCS) includes two or more layers of coating on at least one side of a battery separator. For example, an MCS may include a two-layer coating on at least one side, with the first layer of coating formed closest to the separator surface being a ceramic layer. An adhesive layer may be formed on top of the ceramic layer. Thinner adhesive coatings are preferred as they contribute less to the overall thickness of the coated separator, and thinner battery separators are preferred from a battery capacity standpoint. The thinner the separator, the more separators, electrodes, etc. that can be accommodated in the same space, leading to higher capacity. However, if a thin adhesive is formed, ceramic particles from the lower ceramic layer may protrude from the adhesive layer, causing reduced adhesion at those spots. Figure 1 shows ceramic particles of a ceramic coating protruding from an adhesive layer in an MCS.
[0004] If the adhesion on one side of a double sided coated battery separator is very different from the adhesion on the other side, the battery separator may stick to one electrode better than the other. This is not preferred. It is preferred that the adhesion on both sides is equal or nearly equal.
[0005] Therefore, a MCS with improved adhesion is desirable. Summary of the Invention [Problem to be solved by the invention]
[0006] The battery separator as described hereinabove. For example, the battery separator as described herein may provide improved adhesion. [Means for solving the problem]
[0007] In one aspect, a double-sided coated battery separator includes a first coating on one side of the separator and a second coating on a second side of the separator. In some embodiments, the first coating may be a single or multi-layer coating including one or more coating layers. The outermost coating layer of the first coating is an adhesive coating layer. The second coating of the double-sided coated battery separator may be a multi-layer coating having two or more layers. The second coating may include a ceramic coating layer and an adhesive coating layer on top of the ceramic coating layer. The adhesive coating layer is the outermost layer of the second coating. In a preferred embodiment, the adhesive coating layer of the first coating and the adhesive coating layer of the second coating are formed from different coating formulations. In a particularly preferred embodiment, the coating formulation used to form the adhesive coating layer of the second coating is more adhesive than the one used to form the adhesive coating layer of the first coating. For example, the formulation may be more adhesive at 5 N / m, more adhesive at 7 N / m, or more adhesive at 10 N / m.
[0008] In some preferred embodiments, the adherent coating layer of the first or second coating has a thickness of 1 micron or less.
[0009] In some preferred embodiments, the coating formulation used to form the adherent coating of the first or second coating comprises PVDF, a binder, and water as a solvent. In some embodiments, the coating formulation may further comprise less than 10%, or less than 5%, of nanoceramics.
[0010] In another aspect, a secondary battery is described that includes the double-sided coated battery separator disclosed herein. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram of a double-sided coated battery separator according to some embodiments described herein. [Diagram 2] FIG. 2 is a schematic diagram of a double-sided coated battery separator according to some embodiments described herein. [Diagram 3] FIG. 3 is a schematic diagram of a secondary battery according to some embodiments described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Thus, the embodiments described herein may be more readily understood by reference to the following detailed description, examples, and figures. However, the elements, devices, and methods described herein are not limited to the specific embodiments depicted in the detailed description, examples, and figures. It should be recognized that the illustrative embodiments herein are merely illustrative of the principles of the present invention. Numerous modifications and adaptations will be readily apparent to those skilled in the art without departing from the spirit and scope of the present invention.
[0013] In addition, all ranges disclosed herein should be understood to encompass any and all subranges subsumed therein. For example, a range stated as "from 1.0 to 10.0" should be considered to encompass any and all subranges beginning with a minimum value equal to or greater than 1.0 and ending with a maximum value equal to or less than 10.0, such as from 1.0 to 5.3, or from 4.7 to 10.0, or from 3.6 to 7.9.
[0014] All ranges disclosed herein should also be considered to include the endpoints of the range unless expressly stated otherwise. For example, a range "between 5 and 10" or "from 5 to 10" or "5-10" should generally be considered to include the endpoints 5 and 10.
[0015] Further, when the phrase "up to" is used in connection with an amount or quantity, it should be understood that the amount is at least a detectable amount or quantity. For example, a material present in an amount "up to" a particular amount may be present from a detectable amount up to and including the particular amount.
[0016] Additionally, in any disclosed embodiment, the terms "substantially," "approximately," and "about" may be substituted with "within [a percentage] of" that specified, where that percentage includes 0.1, 1, 5, and 10 percent.
[0017] Many different arrangements of the various components and / or steps depicted and described, as well as those not shown, are possible without departing from the scope of the following claims. The embodiments of the present technology have been described with intent to be illustrative rather than restrictive. Alternative embodiments will become apparent with reference to this disclosure. Alternative ways of carrying out the foregoing may be accomplished without departing from the scope of the following claims. Certain features and subcombinations are of utility and may be used without reference to other features and subcombinations and are contemplated within the scope of the claims.
[0018] The present application is directed to a double-sided coated battery separator having a first coating on one side of the battery separator and a second coating on the opposite side of the battery separator. Each coating may have one, two, three, four, or more coating layers. The outermost coating layer of each of the first and second coatings is an adhesive coating layer. In a preferred embodiment, the outermost adhesive coating layer is formed using a different coating formulation. One of the coating formulations forms a coating that is more adhesive than the other. For example, one of the coating formulations may form a coating that is more 5 N / m, more 7 N / m, or more 10 N / m adhesive. FIG. 1 includes an embodiment as described herein in which each of the first and second coatings includes one coating layer. The one coating layer is an adhesive coating layer that is the outermost layer of the first and second coatings. FIG. 2 includes an embodiment in which the second coating includes two coating layers and the first coating includes one coating layer. The outermost coating layer of each coating is an adhesive coating layer.
[0019] In some particularly preferred embodiments, a double-sided coated battery separator such as that shown in FIG. 2 is described. The double-sided coated battery separator includes a first coating having at least one coating layer and a second coating having at least two coating layers. Each of the first and second coatings may include more coating layers. In a preferred embodiment, the outermost coating layer of the first coating is an adhesive coating layer, and the second coating includes at least a ceramic coating layer and an adhesive coating layer on top of the ceramic coating layer. The adhesive coating layer on top of the ceramic coating layer is the outermost coating layer of the second coating (i.e., the layer that does not have any additional layers formed on top). In a particularly preferred embodiment, the adhesive coating layer on top of the ceramic coating layer is formed using a coating formulation that is more adhesive than the coating formulation used to form the other outermost adhesive coating layer. For example, the coating formulation may form a coating that is more adhesive than 5 N / m, more than 7 N / m, or more than 10 N / m.
[0020] In some preferred embodiments, the outermost adhesive coating layer may be thin. For example, they may have a thickness of less than 2 microns, less than 1.5 microns, less than 1 micron, less than 0.9 microns, less than 0.8 microns, less than 0.7 microns, less than 0.6 microns, less than 0.5 microns, less than 0.4 microns, less than 0.3 microns, less than 0.2 microns, or less than 0.1 microns. Due to the fact that the ceramic particles of the ceramic coating layer may protrude from the adhesive coating layer as shown in FIG. 2, a thin adhesive coating layer may exhibit reduced adhesion when formed on top of a ceramic coating layer. This results in areas of the adhesive coating layer having reduced adhesion. Forming the adhesive coating layer with a more adhesive coating formulation may alleviate this problem.
[0021] Battery Separator The battery separator of the double-sided coated battery separator described herein is not limited in any way and any battery separator capable of being used in a secondary battery, e.g., a lithium ion battery, may be used. In some preferred embodiments, the battery separator may comprise, consist of, or consist essentially of a polyolefin. The battery separator may be nanoporous, microporous, mesoporous, or macroporous. The battery separator may be a monolayer, bilayer, trilayer, or multilayer battery separator. In some preferred embodiments, the battery separator may be formed by a dry process that does not use a solvent or oil. In some embodiments, the dry process may be a dry stretch process where a polymer is extruded and stretched to form pores. The stretching may be uniaxial, biaxial, or multiaxial. In other embodiments, the battery separator may be formed by a wet process that includes the use of a solvent or oil to form pores.
[0022] First Coating The first coating may be a single layer coating, a two layer coating, a three layer coating, a four layer coating, or a five layer coating. In some embodiments, the first coating may have more than five coating layers. In a preferred embodiment, the outermost coating layer of the first coating is an adhesive coating layer. In one preferred embodiment, the first coating is a single layer coating, and the single layer is an adhesive coating layer.
[0023] The adhesive coating is not very limited. In some embodiments, the adhesive coating may include an adhesive polymer. The adhesive polymer may be one or more selected from polyvinylidene fluoride (PVDF) homopolymer, PVDF copolymer, PEO, acrylic polymer, and PVA. For example, the PVDF copolymer may be a PVDF-HFP copolymer.
[0024] In some embodiments, the adhesive coating layer may be formed using a coating formulation that uses an organic solvent or water as the solvent. In embodiments where water is used as the solvent, a small amount of alcohol or another water-soluble solvent may be added.
[0025] In some preferred embodiments, the adhesive polymer may be water insoluble. One example of an adhesive polymer that is water insoluble is PVDF.
[0026] In some preferred embodiments, the adherent coating layer may be formed using a coating formulation that includes less than 10%, less than 9%, less than 8%, less than 7%, less than 6%, or less than 5% nanoceramics. The nanoceramics may have an average particle size of less than about 500 nm, less than 450 nm, less than 400 nm, less than 350 nm, less than 300 nm, less than 250 nm, less than 225 nm, less than 200 nm, less than 175 nm, less than 150 nm, less than 125 nm, or smaller. Nanoceramics may include iron oxide, silicon dioxide (SiO2), aluminum oxide (Al2O3), boehmite (Al(O)OH), zirconium dioxide (ZrO2), titanium dioxide (TiO2), barium sulfate (BaSO4), barium titanate (BaTiO3), aluminum nitride, silicon nitride, calcium fluoride, barium fluoride, zeolite, apatite, kaolin, mullite, spinel, karanite, mica, tin dioxide (SnO2), indium tin oxide, oxides of transition metals, graphite, carbon, metals, and any combination thereof.
[0027] In some preferred embodiments, the adhesive coating layer may have a thickness of less than 2 nm, less than 1.9 nm, less than 1.8 nm, less than 1.7 nm, less than 1.6 nm, less than 1.5 nm, less than 1.4 nm, less than 1.3 nm, less than 1.2 nm, less than 1.1 nm, less than 1.0 nm, less than 0.9 nm, less than 0.8 nm, less than 0.7 nm, less than 0.6 nm, less than 0.5 nm, less than 0.4 nm, less than 0.3 nm, less than 0.2 nm, or less than 0.1 nm. In embodiments where the first coating comprises only a single layer which is an adhesive coating layer, the total thickness of the first coating is preferably less than 2 nm, less than 1.9 nm, less than 1.8 nm, less than 1.7 nm, less than 1.6 nm, less than 1.5 nm, less than 1.4 nm, less than 1.3 nm, less than 1.2 nm, less than 1.1 nm, less than 1.0 nm, less than 0.9 nm, less than 0.8 nm, less than 0.7 nm, less than 0.6 nm, less than 0.5 nm, less than 0.4 nm, less than 0.3 nm, less than 0.2 nm, or less than 0.1 nm.
[0028] Second Coating The second coating may be a single layer coating, a two layer coating, a three layer coating, a four layer coating, or a five layer coating. In some embodiments, the second coating may have more than five coating layers. In a preferred embodiment, the outermost coating layer of the second coating is an adhesive coating layer. In some particularly preferred embodiments, the second coating is a two layer coating including a ceramic coating layer and an adhesive coating layer on top of the ceramic coating layer. The ceramic coating layer may be directly formed on the surface of the battery separator, or may be one or more intervening layers between the ceramic coating layer and the surface of the battery separator.
[0029] The ceramic coating is not limited and any ceramic coating suitable for use in secondary batteries, e.g., lithium ion batteries, may be used. The ceramic coating may provide heat resistance, block dendrites, among others. The ceramic may include iron oxide, silicon dioxide (SiO2), aluminum oxide (Al2O3), boehmite (Al(O)OH), zirconium dioxide (ZrO2), titanium dioxide (TiO2), barium sulfate (BaSO4), barium titanate (BaTiO3), aluminum nitride, silicon nitride, calcium fluoride, barium fluoride, zeolite, apatite, kaolin, mullite, spinel, karanite, mica, tin dioxide (SnO2), indium tin oxide, oxides of transition metals, graphite, carbon, metals, and any combination thereof. The thickness of the ceramic coating may be less than 5 microns, less than 4 microns, less than 3 microns, less than 2 microns, less than 1 micron, or less than 0.5 microns.
[0030] The adhesive coating layer of the second coating may be similar to that used to form the first coating, but the coating formulation used to form the adhesive coating layer of the second coating is preferably different from the coating formulation used to form the adhesive coating layer of the first coating. For example, the coating formulation may include a different adhesive polymer.
[0031] In some preferred embodiments, the adhesive coating layer may have a thickness of less than 2 nm, less than 1.9 nm, less than 1.8 nm, less than 1.7 nm, less than 1.6 nm, less than 1.5 nm, less than 1.4 nm, less than 1.3 nm, less than 1.2 nm, less than 1.1 nm, less than 1.0 nm, less than 0.9 nm, less than 0.8 nm, less than 0.7 nm, less than 0.6 nm, less than 0.5 nm, less than 0.4 nm, less than 0.3 nm, less than 0.2 nm, or less than 0.1 nm.
[0032] In the embodiment where the adhesive coating layer is the outermost layer of the second coating and the adhesive coating layer is formed on top of the ceramic coating layer, it is preferred that the coating formulation used to form the adhesive coating layer of the second coating is different from the coating formulation used to form the outermost adhesive coating layer of the first coating. The coating formulation used for the second coating, in preferred embodiments, forms a coating that is more adhesive than the coating formulation used for the first coating. Preferably, the coating formulation forms a coating that is at least 5 N / m, at least 6 N / m, at least 7 N / m, at least 8 N / m, at least 9 N / m, or at least 10 N / m adhesive. This is tested by applying each coating formulation separately directly to the same type of substrate and forming layers of the same thickness. The adhesion of the formulations may then be tested using the methods described herein.
[0033] In some embodiments, the adhesive coating of the second coating may be a discontinuous layer or a continuous layer. In some preferred embodiments, the adhesive coating of the second coating may be discontinuous. For example, the adhesive layer may be formed using spray coating or dot pattern coating. The use of a discontinuous adhesive layer may have the benefit of lowering electrical resistance after heat compression to be useful for high power applications, reducing moisture content, and also providing cost savings.
[0034] secondary battery The secondary battery may include a double-sided coated battery separator as described hereinbefore. In some embodiments, the double-sided coated battery separator may include a ceramic coating layer, which may be present on the side of the battery separator closest to the anode. See FIG. 3. EXAMPLES
[0035] Adhesion Test Prepare the sample: Coat the formulation used for the outermost adhesive layer of the first coating directly onto a polyolefin battery separator (1). Coat the formulation used for the outermost adhesive layer of the second coating directly onto the same type of polyolefin battery separator (2). Cut 1 inch by 7 inch coated separator specimens (1 and 2). Cut 1 inch by 1 inch electrode material using the same material for each separator. Place a 1 inch by 1 inch electrode on top of the 1 inch by 7 inch specimen. The 1 inch by 1 inch electrode must be placed at one end of the 1 inch by 7 inch specimen and not in the center.
[0036] The sample, including the separator and top electrode, is placed into a paper pouch slightly larger than the size of the electrode material, approximately 2 inches by 2 inches.
[0037] heating: Using the heat gloves, place the pouch containing the sample in the black square (electrode material) onto the bottom plate of the heat press as shown above. Clamp the top plate for 10 seconds. Remove the top plate of the heat press.
[0038] test: Cut a 1 inch by 1 inch piece of double-sided tape and place it on top of the steel plate. Remove the heated sample from the pouch and place the sample on the steel plate so that the electrode side of the sample is in contact with the tape.
[0039] A roller is used to adhere the sample to the steel plate.
[0040] The finished sample is inserted into the bottom of the Chatillon roller grips and the test is run through.
Claims
1. 1. A double-sided coated battery separator, comprising: a first coating on one side of the battery separator including at least one coating layer, an outermost coating layer of the first coating being an adhesive coating layer; a second coating on an opposite side of the battery separator, the second coating including at least two coating layers, one coating layer of the second coating being a ceramic coating layer and an outermost coating layer of the second coating being an adhesive coating layer; Including, the adhesive coating layer of the first coating and the adhesive coating layer of the second coating are formed using different coating formulations; Battery separator coated on both sides.
2. 10. The double sided coated battery separator of claim 1, wherein a coating formulation used to form said adhesive coating layer of said second coating is more adhesive than a coating formulation used to form said adhesive coating layer of said first coating.
3. 3. The double sided coated battery separator of claim 2, wherein the coating formulation used to form the adhesive coating layer of the second coating has an adhesion greater than 5 N / m.
4. 3. The double sided coated battery separator of claim 2, wherein the coating formulation used to form the adhesive coating layer of the second coating has an adhesion greater than 7 N / m.
5. 3. The double sided coated battery separator of claim 2, wherein the coating formulation used to form the adhesive coating layer of the second coating has an adhesion greater than 10 N / m.
6. 10. The double sided coated battery separator of claim 1, wherein said outermost coating layer of said second coating is an adhesive coating layer having a thickness of 1 micron or less.
7. 10. The double sided coated battery separator of claim 1, wherein said outermost coating layer of said first coating is an adhesive coating layer having a thickness of 1 micron or less.
8. 7. The double sided coated battery separator of claim 6, wherein said outermost coating layer of said first coating is an adherent coating layer having a thickness of 1 micron or less.
9. 7. The double sided coated battery separator of claim 6, wherein the coating formulation used to form the adhesive coating layer of the second coating comprises PVDF, a binder, and water as a solvent.
10. 9. The double sided coated battery separator of claim 8, wherein the coating formulation used to form the adhesive coating layer of the second coating comprises PVDF, a binder, and water as a solvent.
11. 7. The double sided coated battery separator of claim 6, wherein the coating formulation used to form the adherent coating layer of the second coating comprises PVDF, a binder, less than 10% nanoceramic, and water as a solvent.
12. 10. The double sided coated battery separator of claim 8, wherein the coating formulation used to form the adherent coating layer of the second coating comprises PVDF, a binder, less than 10% nanoceramic, and water as a solvent.
13. 7. The double sided coated battery separator of claim 6, wherein the coating formulation used to form the adherent coating layer of the second coating comprises PVDF, a binder, less than 5% nanoceramic, and water as a solvent.
14. 10. The double sided coated battery separator of claim 8, wherein the coating formulation used to form the adherent coating layer of the second coating comprises PVDF, a binder, less than 5% nanoceramic, and water as a solvent.
15. 13. A secondary battery comprising the double-sided coated battery separator of claim 1.
16. A double-sided coated membrane, a first coating on one side of the membrane comprising at least one coating layer, the first coating having an outermost coating layer being an adhesive coating layer; a second coating on the opposite side of the membrane comprising at least two coating layers, one coating layer of the second coating being a ceramic coating layer and an outermost coating layer of the second coating being an adhesive coating layer; and Including, the adhesive coating layer of the first coating and the adhesive coating layer of the second coating are formed using different coating formulations; Membrane coated on both sides.
17. 17. The double-sided coated membrane of claim 16, wherein a coating formulation used to form the adhesive coating layer of the second coating is more adhesive than a coating formulation used to form the adhesive coating layer of the first coating.
18. 17. The double-sided coated membrane of claim 16, wherein the adhesive coating layer of the second coating is continuous or discontinuous.
19. 20. The double-sided coated membrane of claim 18, wherein the adhesive coating layer of the second coating is continuous.
20. 20. The double-sided coated membrane of claim 18, wherein the adhesive coating layer of the second coating is discontinuous.
21. 10. The double sided coated battery separator of claim 1, wherein said adhesive coating layer of said second coating is continuous or discontinuous.
22. 22. The double-sided coated membrane of claim 21, wherein the adhesive coating layer of the second coating is continuous.
23. 22. The double-sided coated membrane of claim 21, wherein the adhesive coating layer of the second coating is discontinuous.
24. 10. The double sided coated battery separator of claim 1, wherein said adhesive coating layer of said second coating is a spray coating or a dot pattern coating.
25. 22. The double-sided coated membrane of claim 21, wherein the adhesive coating layer of the second coating is a spray coating or a dot pattern coating.