Water-Based UV-Curable Coating Composition

A water-based UV-curable coating with polyurethane resin and PDMS-(meth)acrylate oligomer addresses the challenge of stain resistance in 3C coatings, providing simple preparation and effective stain resistance while maintaining mechanical properties.

JP2024543264AActive Publication Date: 2024-11-20PPG COATINGS TIANJIN
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024531276
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-24
Filing Date
2022-11-23
Publication Date
2024-11-20
Estimated Expiration
2042-11-23

AI Technical Summary

Technical Problem

Existing 3C coatings for computers, communications equipment, and consumer electronics, such as those made of polycarbonate (PC), polycarbonate + acrylonitrile/butadiene/styrene copolymer (PC+ABS), polycarbonate + carbon fiber (PC+CF), and polycarbonate + glass fiber (PC+GF), suffer from poor stain resistance and require complex and costly preparation of PDMS-modified polyurethane resins to improve this property.

Method used

A water-based UV-curable coating composition comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer is developed, offering simple preparation and effective stain resistance while maintaining mechanical properties.

Benefits of technology

The coating composition achieves excellent stain resistance and meets mechanical appearance requirements, demonstrating improved performance in 3C coatings without compromising other properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543264000008
    Figure 2024543264000008
  • Figure 2024543264000001
    Figure 2024543264000001
  • Figure 2024543264000002
    Figure 2024543264000002
Patent Text Reader

Abstract

A water-based UV-curable coating composition is disclosed, comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer. Also disclosed is a use of the water-based UV-curable coating composition for coating a substrate, and a substrate at least partially coated with the water-based UV-curable coating composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of coatings, specifically water-based UV-curable coatings. [Background technology]

[0002] In 3C coatings, including coatings for computers, communication devices, and home appliances, water-based UV-curable coatings for plastics such as polycarbonate (PC), polycarbonate + acrylonitrile / butadiene / styrene copolymer (PC+ABS), polycarbonate + carbon fiber (PC+CF), and polycarbonate + glass fiber (PC+GF) generally have relatively poor stain resistance. In order to improve stain resistance, those skilled in the art have conducted extensive research. At present, a widely used method is to prepare a polydimethylsiloxane (PDMS) modified polyurethane resin, and then formulate a water-based UV coating based on the modified polyurethane resin.

[0003] However, the preparation of PDMS modified polyurethane resins that meet application scenarios requires a lot of research efforts and costs. Moreover, it is also difficult in the art to design and balance the formulations based on the prepared PDMS modified polyurethane resins so that the coatings have stain resistance without degrading other performances. Summary of the Invention [Problem to be solved by the invention]

[0004] Thus, there is an urgent practical need and potential commercial value to obtain water-based UV-curable coatings that have both stain resistance and other mechanical and aesthetic properties in a simple and convenient manner. [Means for solving the problem]

[0005] The present inventors have conducted a great deal of research and developed a water-based UV curable coating composition which has the advantages of simple preparation and stain resistance, and at the same time can meet the various mechanical properties and appearance requirements of 3C coatings.

[0006] The present invention provides a water-based UV-curable coating composition comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer.

[0007] The present invention further provides a coated substrate comprising a substrate and an aqueous UV-curable coating composition deposited on at least a portion of the substrate, the aqueous UV-curable coating composition comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer.

[0008] The present invention further provides the use of the water-based UV-curable coating composition for coating a substrate, wherein the water-based UV-curable coating composition comprises a polyurethane resin and a PDMS-(meth)acrylate oligomer.

[0009] The features and advantages of the present invention are particularly presented in the following detailed description of the embodiments. [Brief description of the drawings]

[0010] [Figure 1] 1 shows the results of a water-based UV curable coating according to the present invention and a comparative coating in a stain resistance test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] As used herein, unless expressly stated otherwise, numbers used in the specification and claims, e.g., numbers expressing values, ranges, contents, or percentages, are to be understood as being modified in all respects by the term "about," even if this term is not expressly designated. Thus, unless indicated to the contrary, all numerical parameters set forth in the description and claims herein are approximations and may vary depending upon the properties obtained by the present invention.

[0012] Notwithstanding that the numerical ranges and parameters reciting the broad scope of the invention are approximations, the numerical values ​​recited in the specific examples are to be reported as precisely as possible. Any numerical value, however, inherently contains certain errors which are necessarily the result of the standard deviation found in its corresponding measuring method.

[0013] Additionally, it is to be understood that any numerical range recited herein is intended to encompass all subranges subsumed therein. For example, a range "1 to 10" is intended to include all subranges between (and including) the minimum value of 1 and the recited maximum value of 10, i.e., having a minimum value of 1 or greater and a maximum value of 10 or less.

[0014] In this application, the use of the singular includes the plural and the use of the plural includes the singular, unless expressly stated otherwise. Additionally, in this application, the use of "or" means "and / or," unless expressly stated otherwise, although in some cases "and / or" may be explicitly used. Additionally, in this application, the use of "a" or "an" means "at least a / an," unless expressly stated otherwise. For example, "a" polymer, "a" coating, etc., refers to one or more of any of these items. Additionally, as one of ordinary skill in the art will recognize, feature(s) of one embodiment can be used with other embodiments, even if not expressly stated otherwise.

[0015] In this application, the term "comprising" and similar terms are meant to include, but not be limited to, without excluding any modifications or additions. Additionally, although the present invention describes coating compositions and / or methods having "comprising" or similar terms, those coating compositions etc. may also be described as "consisting essentially of" or "consisting of".

[0016] As used herein, the term "water-based" means that the solvent in the coating composition comprises at least 50% water by weight. The coating composition according to the present invention is a low-VOC coating composition. As used herein, the term "VOC (volatile organic compound)(s)" refers to any organic compound having a boiling point of 250°C (482°F) or less measured at standard atmospheric pressure of 101.3 kPa. Organic solvents are often the main source of VOCs. The coating composition according to the present invention has a VOC content of less than 200 g / L, which meets the national standard that water-based coatings should have a VOC of less than 420 g / L. The VOC value can be determined by measuring the content of various organic compound components in the coating by gas chromatography and then adding up the contents of the various components.

[0017] As used herein, "UV curable" means that the material in the coating composition cures to form a film after exposure to ultraviolet (UV) light. As used herein, the term "cured / curing / curable" refers to the process in which the material is "set" to form an irreversible crosslinked network that no longer flows, melts, or dissolves. As used herein, the term "cured / curing" can be used interchangeably with "crosslinked / crosslinking."

[0018] The water-based UV curable coating composition according to the present invention can be used as a "topcoat". "Topcoat" refers to the outermost coating in a multi-layer coating system. When the water-based UV curable coating composition according to the present invention is used as a topcoat, it can be used in combination with any primer / basecoat as long as they are compatible with each other. Alternatively, the water-based UV curable coating composition according to the present invention can be applied directly to the surface of a substrate without prior application of any primer / basecoat.

[0019] The present invention provides a water-based UV-curable coating composition comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer.

[0020] The polyurethane resin used in the aqueous UV curable coating composition according to the present invention refers to a polymer having repeating units containing carbamate functional groups. The polyurethane can include carbamate-linked organic units selected from the group consisting of simple diols, polyester diols, polyether diols, and / or polycarbonate diols.

[0021] Suitably, the polyurethane resin can comprise a (meth)acrylate-functionalized polyurethane resin. A (meth)acrylate-functionalized polyurethane resin refers to a polyurethane resin that comprises a (meth)acrylate-based functional group bonded thereto. Suitably, the polyurethane resin can comprise 30% to 100% by weight of a (meth)acrylate-functionalized polyurethane resin, for example, at least 40% by weight, for example, at least 50% by weight of a (meth)acrylate-functionalized polyurethane resin, and / or up to 90% by weight, for example, up to 80% by weight of a (meth)acrylate-functionalized polyurethane resin, based on the total weight of the resin. Suitably, the polyurethane resin can comprise a (meth)acrylate-functionalized polyurethane resin and a different polyurethane resin, the different polyurethane resin not comprising a (meth)acrylate-based functional group.

[0022] The polyurethane resin suitable for the present invention has a glass transition temperature (T g ), for example, T from 0℃ to 100℃ g For example, T of 20℃ to 80℃ g T g can be determined by dynamic mechanical analysis (DMA) using a TA Instruments Q800 instrument with the following parameters: frequency of 10 Hz, amplitude of 5 mm, and temperature range of -100°C to 250°C. g is determined as the peak of the tan δ curve according to ASTM D7028.

[0023] Suitably, the polyurethane resin for this application may be in the form of an aqueous dispersion having a solids content of about 30% to 60% by weight, the term "solids content" referring to the percentage of the mass remaining after evaporation of the solution in the mass of the original dispersion.

[0024] Based on the total weight of the aqueous UV curable coating composition, the polyurethane resin can be present in the composition in an amount of about 10 wt% or more, such as about 20 wt% or more, such as about 25 wt% or more, and / or about 70 wt% or less, such as about 50 wt% or less, such as about 45 wt% or less. Based on the total weight of the aqueous UV curable coating composition, the polyurethane resin can be present in a range of about 10 wt% to 70 wt%, such as about 20 wt% to 50 wt%, such as about 25 wt% to 45 wt%, or any other combination of these endpoints.

[0025] The PDMS-(meth)acrylate oligomer used in the water-based UV-curable coating composition according to the present invention refers to an oligomer comprising a PDMS portion and a (meth)acrylate portion. The PDMS portion comprises polydimethylsiloxane. The (meth)acrylate portion can comprise one or more (meth)acrylate units.

[0026] Preferably, the PDMS-(meth)acrylate oligomer is water-dispersible. "Water-dispersible" means that the oligomer contains hydrophilic groups and can be uniformly dispersed in water or aqueous solvents without phase separation or similar phenomena. Preferably, the PDMS-(meth)acrylate oligomer contains polyoxyethylene and / or polyoxypropylene block moieties. Preferably, the PDMS-(meth)acrylate oligomer contains the structure (PDMS-polyoxyethylene and / or polyoxypropylene-(meth)acrylate). Preferably, the PDMS-(meth)acrylate oligomer contains linear and / or branched structures. As used herein, the term "linear" means that the oligomeric chain is substantially linear. As used herein, the term "branched" means that the oligomeric chain contains side chain(s) attached to the backbone or otherwise covalently attached side chains.

[0027] The PDMS-(meth)acrylate oligomers suitable for the present invention have a number average molecular weight (M n ) is ≦10,000, for example, M n ≦8,000, for example, M n is ≦6,000. n can be determined by gel permeation chromatography using suitable standards, e.g., polystyrene standards.

[0028] Based on the total weight of the aqueous UV curable coating composition, the PDMS-(meth)acrylate oligomer can be present in the composition in an amount of about 0.1 wt% or more, such as about 0.5 wt% or more, such as about 1 wt% or more, and / or about 10 wt% or less, such as about 8 wt% or less, such as about 6 wt% or less. Based on the total weight of the aqueous UV curable coating composition, the PDMS-(meth)acrylate oligomer can be present in the composition in an amount of about 0.1 wt% to 10 wt%, such as about 0.5 wt% to 8 wt%, such as about 1 wt% to 6 wt%, or any other combination range using these endpoints.

[0029] In the aqueous UV curable coating composition of the present invention, the polyurethane resin and the PDMS-(meth)acrylate oligomer can constitute at least 60% by weight, preferably at least 80% by weight, such as at least 95% by weight, or even 100% by weight of the total solid weight of the composition. In the aqueous UV curable coating composition of the present invention, the polyurethane resin can constitute at least 30% by weight, such as at least 40% by weight, such as at least 50% by weight, preferably at least 60% by weight, such as at least 70% by weight, such as at least 80% by weight, such as at least 90% by weight, at least 95% by weight, or at least 98% by weight of the total solid weight of the composition. Here, "total solid weight" refers to the total weight of the coating composition after removal of the solvent.

[0030] Suitably, in the aqueous UV curable coating composition of the present invention, the weight ratio of polyurethane resin to PDMS-(meth)acrylate oligomer may be about 40:1 to 300:1, such as about 50:1 to 250:1, for example, about 80:1 to 150:1.

[0031] The aqueous UV curable coating composition according to the present invention may further comprise a polyisocyanate. The polyisocyanate may consist of the following monomers: hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and / or dicyclohexylmethane-4,4'-diisocyanate (HMDI). Preferably, the polyisocyanate may comprise the following multimers (at least trimers): hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), and / or dicyclohexylmethane-4,4'-diisocyanate (HMDI). For example, the polyisocyanate may comprise HDI trimer and / or IPDI trimer.

[0032] Based on the total weight of the aqueous UV-curable coating composition, the polyisocyanate can be present in the composition in an amount of about 1% to 10% by weight, such as about 2% to 6% by weight.

[0033] The aqueous UV curable coating composition according to the present invention may further comprise a surfactant. Preferably, the surfactant used in the present invention comprises a non-ionic surfactant having wetting and defoaming properties. Generally, the matting agent may be present in the composition in an amount of about 0% to 2% by weight, based on the total weight of the aqueous UV curable coating composition.

[0034] The water-based UV-curable coating composition according to the present invention may further comprise a matting agent. The matting agent comprises an inorganic matting agent and / or an organic matting agent. Preferably, the inorganic matting agent comprises a silica-based matting agent. The silica-based matting agent may comprise silica with or without surface treatment. The organic matting agent comprises a polymethylurea (PUM)-based matting agent. Generally, based on the total weight of the water-based UV-curable coating composition, the matting agent may be present in the composition in an amount of about 0% to 5% by weight, for example, about 1% to 4% by weight.

[0035] The aqueous UV curable coating composition according to the present invention may further comprise a photoinitiator. The photoinitiator may decompose under UV irradiation and cause polymerization of the polymerizable oligomer and / or monomer to form a three-dimensional network structure. Generally, based on the total weight of the aqueous UV curable coating composition, the photoinitiator may be present in the composition in an amount of about 1% to 5% by weight.

[0036] The aqueous UV-curable coating composition according to the present invention may further comprise a substrate wetting agent. The wetting agent may improve the surface tension and permeability of the coating composition, better wet the coating layer, and improve the adhesion of the coating. Preferably, the wetting agent comprises an organosilicon-based and / or poly(meth)acrylate-based wetting agent. Generally, based on the total weight of the aqueous UV-curable coating composition, the substrate wetting agent may be present in the composition in an amount of about 0% to 2% by weight.

[0037] The aqueous UV-curable coating composition according to the present invention may further comprise a thickener. The thickener may improve the viscosity of the coating, improve the wet film thickness, and protect the coating from settling and phase separation. Preferably, the thickener comprises an alkali-soluble anionic thickener and an associative thickener. Generally, based on the total weight of the aqueous UV-curable coating composition, the thickener may be present in the composition in an amount of about 0% to 5% by weight.

[0038] The aqueous UV curable coating composition according to the present invention may further comprise an organic solvent. The organic solvent may reduce the surface tension of the composition and increase the evaporation rate. Preferably, the organic solvent comprises an alcohol such as butanol, isopropanol, 2-butoxyethanol, etc. In general, based on the total weight of the aqueous UV curable coating composition, the organic solvent may be present in the composition in an amount of about 0% to 5% by weight.

[0039] The aqueous UV-curable coating composition according to the present invention may further comprise 40 to 70% by weight of water.

[0040] The water-based UV-curable coating composition according to the present invention may further comprise (meth)acrylate resins and / or polyester resins, or other film-forming materials. The water-based UV-curable coating composition according to the present invention may further comprise one or more additional auxiliary components (additives), including, but not limited to: rheological aids to improve flow and leveling properties and reduce defects; preservatives to protect the coating from mildew; pH adjusters to control pH and stabilize the coating; waxes to increase scratch resistance and improve hand feel; pigments to impart color, fill and / or abrasion resistance to the coating, and the like. When present, each type of auxiliary component is present in an amount of at most about 5% by weight, based on the total weight of the water-based UV-curable coating composition.

[0041] The aqueous UV-curable coating composition according to the present invention can be prepared by uniformly mixing the composition containing the polyurethane resin and the PDMS-(meth)acrylate oligomer at room temperature. As used herein, "room temperature" refers to a temperature of 20°C to 30°C, for example 22°C.

[0042] The present invention further provides a use of the aqueous UV curable coating composition for coating a substrate, the aqueous UV curable coating composition comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer. As used herein, the term "substrate" refers to a material having a rough or smooth surface, with or without a coating. The substrate includes a plastic substrate. Suitable substrates include, but are not limited to, polycarbonate, polycarbonate + acrylonitrile / butadiene / styrene copolymer, polycarbonate + carbon fiber, and / or polycarbonate + glass fiber. The substrate may be a substrate for use in a vehicle display screen, a mobile phone PET protective film, a computer display screen, a keyboard, and / or a laptop housing.

[0043] The present invention further provides a substrate coated with an aqueous UV-curable coating composition comprising a substrate and an aqueous UV-curable coating composition deposited on at least a portion of the substrate, where the aqueous UV-curable coating composition comprises a polyurethane resin and a PDMS-(meth)acrylate oligomer.

[0044] The coating composition of the present invention can be coated by any standard method known in the art, such as spraying, dipping, roller coating, brush coating, etc., and then cured under UV radiation to form a coating film. For example, the coating composition can be baked at 50°C to 70°C for about 10 to 15 minutes to evaporate the solvent and water, followed by curing under UV radiation at 800 to 1,200 mJ / cm. 2 UV energy of 100-200mW / m2 This coating generally has a film thickness in the range of 15-20 μm. EXAMPLES

[0045] The following examples are provided to further illustrate the invention but should not be construed as limiting the invention to the details thereof. All parts and percentages in the following examples are by weight unless otherwise indicated.

[0046] Examples 1 to 4: Water-based UV curable coating compositions according to the present invention, Ex-1, Ex-2, Ex-3 and Ex-4, were prepared according to the ingredients and amounts listed in the following Table 1. Specifically, the ingredients listed in the table were placed in a container under stirring and mixed for about 30 minutes, and then the resulting mixture was sieved through a 200 mesh device. [Table 1]

[0047] Comparative Examples 1 to 4: Comparative water-based UV curable coating compositions, CE-1, CE-2, CE-3, and CE-4, were prepared according to the ingredients and amounts listed in Table 2 below. Specifically, the ingredients listed in the table were placed in a container under stirring and mixed for about 30 minutes, and then the resulting mixture was sieved through a 200 mesh device. [Table 2]

[0048] Performance Test: First, the aqueous UV-curable coating compositions Ex-1, Ex-2, Ex-3, and Ex-4 according to the present invention, and the aqueous UV-curable coating compositions CE-1, CE-2, CE-3, and CE-4 according to the comparative examples were applied to a polycarbonate substrate, baked at about 60° C. for about 10 minutes, and then irradiated with 1,000 mJ / cm 2of UV energy and 120mW / cm 2 The specimen was exposed to UV radiation having an optical radiation intensity of 100 nm.

[0049] The coated substrates were subjected to various performance tests as follows:

[0050] 1-VOC Herein, the VOC content (water-free, g / L) of the water-based UV curable coating compositions according to the present invention, Ex-1, Ex-2, Ex-3 and Ex-4, was calculated in the following manner.

[0051] For 1 g of the composition, the mass m of each component in the composition i , the mass of water in the composition m w , and the density ρ of the composition s were measured, respectively.

[0052] The calculation was made according to the following formula:

number

[0053] 2-Gloss The gloss of the resulting coatings was measured at 60° using a commercial glossmeter BYK Micro-Gloss. [Table 4]

[0054] 3-Water contact angle The water contact angles of the coatings were measured using a commercially available optical contact angle meter. [Table 5]

[0055] 4-Stain resistance In the present invention, the stain resistance of the coating was evaluated by drawing a mark on the coating with a red oil-based Sharpie pen, then drying at room temperature for 15 minutes, wiping the mark five times with a dry paper towel, and evaluating the stain resistance of the coating according to the state of the mark after wiping. Specifically, the stain resistance was rated (scored) from 0 to 10, with 0 representing the worst, i.e., no change in the red mark, and 10 representing the best, i.e., no red mark was left. [Table 6]

[0056] The stain resistance test results of the water-based UV curable coating compositions according to the present invention, Ex-1, Ex-2, Ex-3, Ex-4, and the comparative water-based UV curable coating compositions, CE-1, CE-2, CE-3 and CE-4, are also shown in FIG.

[0057] It can be seen that the water-based UV curable coating composition provided by the present invention has excellent stain resistance. At the same time, the water-based UV curable coating composition according to the present invention can meet other requirements of appearance and mechanical properties.

[0058] While particular embodiments of the present invention have been illustrated and described, it would be obvious to those skilled in the art that many other changes and modifications can be made without departing from the spirit and scope of the invention. It is therefore intended that the appended claims cover all such changes and modifications that are within the scope of this invention.

Claims

1. A water-based UV-curable coating composition comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer.

2. The coating composition of claim 1, wherein the PDMS-(meth)acrylate oligomer is water-dispersible.

3. The coating composition of claim 1 or 2, wherein the PDMS-(meth)acrylate oligomer comprises polyoxyethylene and / or polyoxypropylene block moieties.

4. The coating composition according to any one of claims 1 to 3, wherein the PDMS-(meth)acrylate oligomer comprises a structure of (PDMS-polyoxyethylene and / or polyoxypropylene-(meth)acrylate).

5. The coating composition of any one of claims 1 to 4, wherein the PDMS-(meth)acrylate oligomer comprises a linear or branched structure.

6. The coating composition of any one of claims 1 to 5, wherein the PDMS-(meth)acrylate oligomer has a number average molecular weight of ≦10,000.

7. The coating composition of any one of claims 1 to 6, wherein the composition comprises less than 10 wt% of the PDMS-(meth)acrylate oligomer, based on the total weight of the composition.

8. The coating composition of any one of claims 1 to 7, wherein the polyurethane resin comprises a (meth)acrylate-functionalized polyurethane resin.

9. The coating composition of any one of claims 1 to 8, wherein the polyurethane resin comprises 30 to 100 weight percent of a (meth)acrylate-functionalized polyurethane resin, based on the total weight of the polyurethane resin.

10. The coating composition according to any one of claims 1 to 9, wherein the polyurethane resin has a glass transition temperature of from -30°C to 110°C.

11. The coating composition of any one of claims 1 to 10, wherein the polyurethane resin comprises at least 30% by weight of the total solids weight of the composition.

12. The coating composition of any one of claims 1 to 11, wherein the polyurethane resin and the PDMS-(meth)acrylate oligomer constitute at least 80% by weight of the total solids weight of the composition.

13. The coating composition of any one of claims 1 to 12, wherein the weight ratio of the polyurethane resin to the PDMS-(meth)acrylate oligomer is comprised between 40:1 and 300:

1.

14. The coating composition of any one of claims 1 to 13, having a VOC content, measured without water, of less than 200 g / L.

15. 1. A coated substrate comprising a substrate and an aqueous UV curable coating composition deposited on at least a portion of the substrate, the aqueous UV curable coating composition comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer.

16. 16. The coated substrate of claim 15, wherein the substrate comprises polycarbonate, polycarbonate + acrylonitrile / butadiene / styrene copolymer, polycarbonate + carbon fiber, and / or polycarbonate + fiberglass.

17. 17. The coated substrate of claim 15 or 16, wherein the substrate is for use in a vehicle display screen, a mobile phone PET protective film, a computer display screen, a keyboard, and / or a laptop housing.

18. 1. Use of an aqueous UV curable coating composition for coating a substrate, said aqueous UV curable coating composition comprising a polyurethane resin and a PDMS-(meth)acrylate oligomer.

19. 20. The use according to claim 18, wherein the substrate comprises polycarbonate, polycarbonate + acrylonitrile / butadiene / styrene copolymer, polycarbonate + carbon fibre, and / or polycarbonate + glass fibre.

20. 20. The use according to claim 18 or 19, wherein the substrate is a substrate for use in vehicle display screens, mobile phone PET protective films, computer display screens, keyboards and / or laptop housings.

Citation Information

Patent Citations

  • Polyurethane emulsion, preparation method of the polyurethane emulsion, nanometer color paste, preparation method of the nanometer color paste, ultraviolet light-cured coating composition and preparation method of the ultraviolet light-cured coating composition

    CN102618020A

  • Radiation-curing surface control aid, its manufacturing method and application

    JP2015531806A