Lithium secondary battery and method for producing the same
The negative electrode-separator composite with controlled air permeability addresses lithium growth issues, enhancing battery performance and safety by suppressing lithium protrusion and applying pressure for uniform growth, thereby improving battery life and safety.
Patent Information
- Application Number
- JP2024527649
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-09-22
- Filing Date
- 2022-09-23
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium secondary batteries face issues with excessive and non-uniform growth of lithium on the side surfaces of the negative electrode, leading to short circuits, reduced battery life, and safety concerns due to lithium melting and leakage.
A negative electrode-separator composite is formed by adhering edges of first and second separators to create a seal with air permeability of 50,000 sec/100 cc or more, housing the negative electrode, which suppresses lithium growth and applies pressure for uniform growth, preventing short circuits and lithium leakage.
The solution effectively minimizes lithium exposure, enhances battery reversibility and life, and prevents side reactions, improving the safety and life characteristics of the lithium secondary battery.
Smart Images

Figure 2024543428000001_ABST
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0187034 filed on December 24, 2021 and Korean Patent Application No. 10-2022-0120348 filed on September 22, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated as part of this specification.
[0002] The present invention relates to a lithium secondary battery comprising a negative electrode-separator composite including a negative electrode and a separator, the negative electrode including a lithium metal layer, the separator including a first separator disposed on one side of the negative electrode and a second separator disposed on the other side of the negative electrode, at least a portion of an edge of the first separator and the second separator are bonded to each other to form a seal portion, the negative electrode is housed inside the separator, and the air permeability of the seal portion is 50,000 sec / 100 cc or more. [Background technology]
[0003] In recent years, electronic products, electronic devices, communication devices, etc. have been rapidly reduced in size and weight, and the need for electric vehicles has become increasingly important in relation to environmental issues. As a result, there is an increasing demand for improved performance of secondary batteries used as power sources for these products. Among them, lithium secondary batteries have attracted considerable attention as high-performance batteries due to their high energy density and high standard electrode potential. Lithium secondary batteries are generally composed of a positive electrode, a negative electrode, an electrolyte, and a separator.
[0004] The negative electrode may be a lithium metal negative electrode, which refers to a negative electrode that is made of a lithium metal layer or has a lithium metal layer disposed on a negative electrode current collector.
[0005] Referring to FIG. 1, when the lithium metal negative electrode 10 is used, lithium is precipitated from the negative electrode 10 during the operation of the battery, and lithium grows (e.g., lithium dendrite) on the surface of the negative electrode. The growth of lithium may occur not only on the wide surface (vertical direction) of the negative electrode facing the positive electrode, but also on the side of the negative electrode (horizontal direction, A direction in FIG. 1). In this case, the size of the negative electrode increases in the horizontal direction during the operation of the battery, and the lithium 10a grown on the side of the negative electrode may grow outside the separator 30, causing a short circuit between the positive electrode 20 and the negative electrode 10. This phenomenon leads to early deterioration and shortening of the life of the battery, and the problem situation is further accelerated as the operating current of the battery increases. Meanwhile, since the lithium 10a grows on the side of the negative electrode without applying an appropriate pressure, the lithium 10a is formed in an uneven shape, the reversibility of the lithium metal negative electrode 10 decreases, and the performance of the battery, especially the life of the battery, decreases due to an increase in side reactions of the electrolyte. In addition, since lithium has a low melting point, when the battery is operated, lithium metal melts and flows out toward the side of the separator 30, which may further increase the likelihood of a short circuit between the positive electrode 20 and the negative electrode 10.
[0006] In order to solve this problem, conventional methods have been tried to reduce the size of the lithium metal anode or to use various electrolytes capable of suppressing the growth of lithium and stabilizing the anode. However, when the size of the lithium metal anode is reduced, there is a problem that the capacity of the battery is reduced. In addition, attempts to use a specific electrolyte to stabilize the anode cannot completely prevent the possibility of short-circuiting between the positive and negative electrodes due to the horizontal growth of lithium in the anode, so there are still problems of reduced battery life and safety. Therefore, a new technology is needed that can suppress the horizontal growth of lithium on the negative electrode. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a lithium secondary battery capable of suppressing excessive and non-uniform growth of lithium on a side surface of a negative electrode including a lithium metal layer.
[0008] Another object of the present invention is to provide a method for producing the lithium secondary battery. [Means for solving the problem]
[0009] According to one embodiment of the present invention, there is provided a lithium secondary battery comprising a negative electrode-separator composite including a negative electrode and a separator, the negative electrode including a lithium metal layer, the separator including a first separator disposed on one side of the negative electrode and a second separator disposed on the other side of the negative electrode, at least a portion of an edge of the first separator and the second separator are bonded to each other to form a seal, the negative electrode is housed inside the separator, and the seal has an air permeability of 50,000 sec / 100 cc or more.
[0010] According to another embodiment of the present invention, there is provided a method for manufacturing a lithium secondary battery, the method including the steps of: disposing a first separator on one side of a negative electrode including a lithium metal layer, disposing a second separator on the other side of the negative electrode, and bonding at least a portion of an edge of the first separator and the second separator to each other to form a seal, thereby manufacturing a negative electrode-separator composite, wherein the seal has an air permeability of 50,000 sec / 100 cc or more. Effect of the Invention
[0011] According to the present invention, the sealing portion formed by bonding the first separator and the second separator can minimize exposure of the side of the negative electrode including the lithium metal layer, thereby suppressing excessive protrusion of lithium grown during battery operation to the side of the negative electrode, and effectively preventing short circuit between the positive electrode and the negative electrode.
[0012] In addition, when the lithium grows on the side of the negative electrode, the sealing part can apply an appropriate pressure to the side of the negative electrode, thereby allowing the lithium to grow uniformly on the side of the negative electrode, thereby improving the reversibility and lifespan of the negative electrode.
[0013] Furthermore, even if the lithium is partially melted due to heat generated during operation of the battery, the molten lithium can be effectively prevented from escaping to the outside of the negative electrode-separator composite.
[0014] Meanwhile, the sealing portion has a specific air permeability. Therefore, even when the positive electrode contains a positive electrode active material containing elemental sulfur (for example, when the lithium secondary battery is a lithium-sulfur secondary battery), the phenomenon in which lithium polysulfide formed from the positive electrode comes into contact with the negative electrode and causes a side reaction can be suppressed. As a result, the safety and life characteristics of the lithium secondary battery can be improved. [Brief description of the drawings]
[0015] [Figure 1] 1 is a schematic diagram for explaining a problem occurring in a conventional lithium secondary battery. [Diagram 2] 1 is a schematic diagram of a lithium secondary battery according to one embodiment of the present invention; [Diagram 3] 1 is a schematic diagram showing a negative electrode-separator composite included in a lithium secondary battery according to an embodiment of the present invention. [Figure 4] 1A to 1C are schematic diagrams illustrating a method for producing a lithium secondary battery according to an embodiment of the present invention. [Diagram 5] 1A to 1C are schematic diagrams illustrating a method for producing a lithium secondary battery according to an embodiment of the present invention. [Figure 6] 1A to 1C are schematic diagrams illustrating a method for producing a lithium secondary battery according to an embodiment of the present invention. [Figure 7] 1 is a graph showing the capacity per cycle of the lithium secondary batteries of Example 1 and Comparative Examples 1 and 2. [Figure 8]1 is a graph showing the coulombic efficiency per cycle of the lithium secondary batteries of Example 1 and Comparative Examples 1 and 2. [Figure 9] 1 is a photograph showing the negative electrode in the lithium secondary battery of Example 1 after the battery was operated for 240 cycles. [Figure 10] 1 is a photograph showing the negative electrode in the lithium secondary battery of Comparative Example 1 after 60 cycles of operation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will now be described in more detail to aid in understanding the invention. The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a manner that is consistent with the technical idea of the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.
[0017] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. The singular expressions include the plural expressions unless otherwise clearly indicated in the context.
[0018] It should be understood that, as used herein, terms such as "comprises," "comprising," or "having" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, but do not preclude the presence or additional possibility of one or more other features, numbers, steps, components, or combinations thereof.
[0019] In this specification, the air permeability can be measured under the following conditions using an Oken Type Air-permeability & Smoothness Testing Controller manufactured by ASAHI SEIKO.
[0020] Time:6sec(seconds) Value:500 Measure Mode: JIS(sec)
[0021] <Lithium secondary battery> A lithium secondary battery according to an embodiment of the present invention includes a negative electrode-separator composite including a negative electrode and a separator, the negative electrode including a lithium metal layer, the separator including a first separator disposed on one side of the negative electrode and a second separator disposed on the other side of the negative electrode, at least a portion of an edge of each of the first separator and the second separator is bonded to each other to form a seal, the negative electrode is housed inside the separator, and the air permeability of the seal may be 50,000 sec / 100 cc or more.
[0022] (1) Negative electrode-separator composite The lithium secondary battery may include a negative electrode-separator composite. The negative electrode-separator composite may include a negative electrode and a separator.
[0023] 1) Negative electrode The negative electrode may be a lithium metal negative electrode, which in the art may refer to the negative electrode of a lithium metal secondary battery (including a lithium-sulfur secondary battery).
[0024] The negative electrode may include a lithium metal layer. The lithium metal layer may function to store and release lithium. The lithium metal layer may include at least one of lithium metal and a lithium alloy, and may be composed of at least one of lithium metal and a lithium alloy. For example, the lithium metal layer may be composed of lithium metal. The lithium alloy includes an element capable of being alloyed with lithium, and the element may be Si, Sn, C, Pt, Ir, Ni, Cu, Ti, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, Co, or an alloy thereof.
[0025] The lithium metal layer may be a sheet or foil. The lithium metal layer itself may constitute the negative electrode. Alternatively, the negative electrode may further include a negative electrode current collector, and the lithium metal or lithium alloy may be deposited or coated on the negative electrode current collector by a dry process, or particulate metal and alloy may be deposited or coated on the negative electrode current collector by a wet process. The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, aluminum-cadmium alloy, etc. may be used. In addition, various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric body with or without fine unevenness on the surface may be used. The negative electrode may be in the form of a rectangular sheet and may have a predetermined thickness.
[0026] Meanwhile, the negative electrode may further include a negative electrode tab. The negative electrode tab is connected to an external electric wire to allow a current to flow between the negative electrode and the outside. The negative electrode tab may protrude from a side surface of the negative electrode.
[0027] 2) Separator FIG. 2 is a schematic diagram illustrating a lithium secondary battery according to one embodiment of the present invention, and FIG. 3 is a schematic diagram showing a cross section B-B' of the negative electrode-separator composite 100 shown in FIG. 2.
[0028] 2 and 3, the negative electrode-separator composite 100 may include a negative electrode 110 and a separator 120, and the separator 120 may be disposed on the negative electrode 110. The separator 120 may include a first separator 121 and a second separator 122.
[0029] The first separator 121 may be disposed on one surface of the negative electrode 110, and the second separator 122 may be disposed on another surface of the negative electrode 110 opposite to the one surface.
[0030] The first separator 121 and the second separator 122 may each include a porous substrate. The porous substrate may be any porous substrate typically used in electrochemical devices, such as, but not limited to, a polyolefin-based porous membrane or nonwoven fabric.
[0031] Examples of the polyolefin-based porous membrane include membranes formed from polyolefin-based polymers such as polyethylene (e.g., high density polyethylene, linear low density polyethylene, low density polyethylene, ultra-high molecular weight polyethylene), polypropylene, polybutylene, and polypentene, either alone or in combination.
[0032] Examples of the nonwoven fabric include polyolefin-based nonwoven fabrics, and nonwoven fabrics formed from polymers such as polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyether ether ketone, polyether sulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalate, either alone or in combination. The nonwoven fabric may include a nonwoven fabric made of high-melting glass fiber or ceramic material. The structure of the nonwoven fabric may be a spunbonded or meltblown nonwoven fabric made of long fibers.
[0033] The thickness of the porous substrate is not particularly limited, but may be 1 to 100 μm, and preferably 5 to 50 μm. The size of the pores present in the porous substrate and the porosity are not particularly limited, and may be 0.001 to 50 μm and 10 to 95%, respectively.
[0034] In some cases, each of the first separator and the second separator may include an adhesive layer (not shown) disposed on the porous substrate. The adhesive layer may be located between the negative electrode and the separator and may include an adhesive binder. This allows the negative electrode and the separator to be stably contacted, thereby improving the stability of the negative electrode-separator composite.
[0035] Meanwhile, in some cases, the separator (the first separator and the second separator, respectively) may further include a coating layer (not shown) disposed on the porous substrate. The coating layer may be made of inorganic particles, or inorganic particles and a binder. The coating layer may improve the thermal stability of the separator.
[0036] The coating layer may include pores. The pores may have a size that makes it difficult for lithium polysulfide to pass through. Specifically, the pores may have a particle size of 0.1 nm to 1,000 nm, specifically 0.5 nm to 500 nm. This can prevent lithium polysulfide formed from the positive electrode from reaching the negative electrode when the positive electrode includes a positive electrode active material containing elemental sulfur (in the case of a lithium-sulfur secondary battery), and can prevent side reactions caused by lithium polysulfide, thereby improving the life characteristics and efficiency of the battery.
[0037] At least a portion of edge portions 121' and 122' of the first separator 121 and the second separator 122 may be bonded to each other to form a seal portion 120a. The edge portions 121' and 122' refer to regions of the first separator 121 and the second separator 122 that are not in contact with the negative electrode 110. The edge portions 121' and 122' may be formed side by side on four side surfaces of the negative electrode 110.
[0038] The sealing part 120a can minimize exposure of the side of the negative electrode 110 including the lithium metal layer. This can prevent the lithium grown during the operation of the battery from excessively protruding from the side of the negative electrode 110, effectively preventing a short circuit between the positive electrode 200 and the negative electrode 110. Even if the lithium grows on the side of the negative electrode 110, the sealing part 120a can apply an appropriate pressure to the side of the negative electrode 110, so that the lithium can grow uniformly on the side of the negative electrode 110, thereby improving the reversibility and life of the negative electrode 110. Furthermore, even if the lithium partially melts due to heat generated during the operation of the battery, the melted lithium can be effectively prevented from escaping to the outside of the negative electrode-separator composite 100. This can improve the life characteristics of the lithium secondary battery.
[0039] The sealing portion 120a may be formed so that the remaining portion of the negative electrode 110, excluding the negative electrode tab (not shown), is not exposed to the outside of the separator 120. That is, the edges of the first separator 121 and the second separator 122 may be bonded to each other while surrounding the four sides of the negative electrode, and the sealing portion 120a may be present while surrounding the four sides of the negative electrode 110, but the sealing portion 120a may not be formed only in the area of the first separator 121 and the second separator 122 that contacts the negative electrode tab. When the negative electrode-separator composite 100 having the above-mentioned configuration is formed, it is possible to more effectively prevent a short circuit between the positive electrode 200 and the negative electrode 110 by suppressing lithium that grows during battery operation from excessively protruding to the side of the negative electrode. It is possible to more effectively suppress the escape of molten lithium to the outside of the negative electrode-separator composite 100. As a result, it is possible to more effectively improve the life characteristics of the lithium secondary battery. On the other hand, the "negative electrode tab" and the "first separator and / or second separator" may be in contact with each other by being adhered to each other, or may be separated from each other.
[0040] The air permeability of the seal part 120a may be 50,000sec / 100cc or more, specifically 65,000sec / 100cc to 100,000sec / 100cc, more specifically 80,000sec / 100cc to 100,000sec / 100cc. If the air permeability is less than 50,000sec / 100cc, the grown lithium may pass through the seal part 120a and be present outside the separator, so that the stability of the battery may be reduced. In addition, if the air permeability is less than 50,000sec / 100cc, when the positive electrode contains a positive electrode active material containing sulfur element (in the case of a lithium-sulfur secondary battery), lithium polysulfide formed from the positive electrode may pass through the seal part 120a and cause a side reaction with the negative electrode. This may reduce the life characteristics of the battery.
[0041] That is, controlling the air permeability of the sealing part 120a to 50,000 sec / 100 cc or more is a very important factor in improving the life characteristics of the battery. Also, the air permeability range can be derived by contacting the negative electrode with the first separator and the second separator and then heat fusing them with an appropriate level of heat before manufacturing an electrode assembly including all of the negative electrode, the separator, and the positive electrode.
[0042] If the positive electrode contains a positive electrode active material containing elemental sulfur, and a positive electrode-separator composite is manufactured by contacting separators arranged on both sides of the positive electrode, rather than a negative electrode-separator composite, the high air permeability (50,000 sec / 100 cc or more) of the seal part of the positive electrode-separator composite prevents lithium polysulfide from escaping from the inside of the positive electrode-separator composite, causing the viscosity of the electrolyte near the positive electrode to become excessively high, resulting in a decrease in the driving capacity of the battery. In the present invention, the negative electrode-separator composite is formed on the negative electrode, not on the positive electrode, so the above-mentioned problems do not occur.
[0043] 3) Positive electrode The positive electrode may include a positive electrode active material. Specifically, the positive electrode may include a positive electrode active material layer, and the positive electrode active material may be included in the positive electrode active material layer. The positive electrode active material layer may constitute a positive electrode by itself, or alternatively, a positive electrode may be configured in a state in which the positive electrode active material layer is disposed on a positive electrode current collector.
[0044] The positive electrode active material may be a commonly used positive electrode active material. Specifically, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2) or lithium nickel oxide (LiNiO2) or a compound substituted with one or more transition metals; a lithium iron oxide such as LiFe3O4; 1+a M b O 2+c The M may be at least one element selected from the group consisting of Ni, Co, Mn, Fe, P, Al, Mg, Ca, Zr, Zn, Ti, Ru, Nb, W, B, Si, Na, K, Mo, and V, and may be within the range of -0.2≦a≦0.2, 0 <b≦2、0≦c≦2であってもよい。
[0045] The positive electrode active material may include a sulfur-based compound containing elemental sulfur. The sulfur-based compound may include inorganic sulfur (S8), Li2S n1 (n1≧1), disulfide compounds, organic sulfur compounds, and carbon-sulfur polymers (C2S x ) n2 , x=2.5 to 50, n2≧2). Preferably, inorganic sulfur (S8) may be used.
[0046] The sulfur-based compound alone does not have electrical conductivity, and is therefore used in combination with a conductive material. Preferably, the positive electrode active material may be a sulfur-carbon composite.
[0047] In the sulfur-carbon composite, carbon is a porous carbon material that provides a skeleton to which sulfur, a positive electrode active material, can be uniformly and stably fixed, and compensates for the electrical conductivity of sulfur to facilitate an electrochemical reaction.
[0048] The porous carbon material may be generally prepared by carbonizing various carbon precursors. The porous carbon material may include pores having different sizes, and the average diameter of the pores may be in the range of 1-200 nm, and the porosity or void ratio may be in the range of 10-90% of the total volume of the porous material. If the average diameter of the pores is less than the above range, the size of the pores is merely at the molecular level, and impregnation with sulfur is not possible. Conversely, if the average diameter of the pores exceeds the above range, the mechanical strength of the porous carbon is weakened, making it unsuitable for use in the manufacturing process of an electrode.
[0049] The shape of the porous carbon material may be spherical, rod-like, needle-like, plate-like, tubular, or bulk-like, and any shape that is commonly used in lithium-sulfur batteries may be used without limitation.
[0050] The porous carbon material may be any material commonly used in the art that has a porous structure or a high specific surface area. For example, the porous carbon material may be one or more selected from the group consisting of graphite, graphene, carbon black such as denka black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, carbon nanotubes (CNTs) such as single-walled carbon nanotubes (SWCNTs) and multi-walled carbon nanotubes (MWCNTs), carbon fibers such as graphite nanofibers (GNFs), carbon nanofibers (CNFs), and activated carbon fibers (ACFs), natural graphite, artificial graphite, expanded graphite, and activated carbon, but is not limited thereto. Preferably, the porous carbon material may be carbon nanotubes.
[0051] The sulfur-carbon composite may contain 60 to 90 parts by weight, preferably 65 to 85 parts by weight, and more preferably 70 to 80 parts by weight of sulfur based on 100 parts by weight of the sulfur-carbon composite. If the sulfur content is less than the above range, the content of the porous carbon material in the sulfur-carbon composite is relatively high, which increases the specific surface area and increases the content of the binder during the preparation of the slurry. Such an increase in the amount of binder used may ultimately increase the surface resistance of the positive electrode and act as an insulator that prevents electron pass, thereby reducing the performance of the battery. On the other hand, if the sulfur content exceeds the above range, sulfur or sulfur compounds that cannot be bonded to the porous carbon material may aggregate with each other or re-dissolve on the surface of the porous carbon material, making it difficult to receive electrons and unable to participate in the electrochemical reaction, which may cause a loss of capacity in the battery.
[0052] The positive electrode active material may further include one or more additives selected from transition metal elements, group 2 elements, group 3 elements, sulfur compounds of these elements, and alloys of these elements and sulfur. The transition metal elements may include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Os, Ir, Pt, Au, or Hg, the group 2 elements may include Al, Ga, In, Ti, and the group 3 elements may include Ge, Sn, Pb, and the like.
[0053] The positive electrode active material may be contained in the positive electrode active material layer in an amount of 50% by weight to 99% by weight, specifically 60% by weight to 90% by weight, more specifically 65% by weight to 85% by weight. If the content of the positive electrode active material is less than the above range, it is difficult to fully exert the electrochemical reaction of the positive electrode, and conversely, if it exceeds the above range, there is a problem that the content of the conductive material and the binder described below is relatively insufficient, so that the resistance of the positive electrode increases and the physical properties of the positive electrode are deteriorated.
[0054] The positive electrode may further include a positive electrode conductive material, which electrically connects the electrolyte and the positive electrode active material and serves as a path through which electrons move from a current collector to the positive electrode active material. Any material having porosity and conductivity may be used. For example, the positive electrode conductive material may be a carbon-based material having porosity, and examples of such carbon-based materials include carbon black, graphite, graphene, activated carbon, and carbon fiber; metallic fibers such as metal mesh; metallic powders such as copper, silver, nickel, and aluminum; and organic conductive materials such as polyphenylene derivatives. The conductive materials may be used alone or in combination.
[0055] The positive electrode conductive material may be contained in the positive electrode active material layer in an amount of 1 wt% to 10 wt%, specifically 4 wt% to 7 wt%. If the content of the conductive material is less than the above range, the amount of sulfur in the positive electrode that cannot react increases, which ultimately leads to a decrease in capacity. On the other hand, if the content exceeds the above range, it has a negative effect on the high-efficiency discharge characteristics and the charge / discharge cycle life, so it is preferable to determine the appropriate content within the above range.
[0056] The positive electrode may further include a positive electrode binder, which further enhances the binding strength between the components constituting the positive electrode and between the components and the current collector, and may be any binder known in the art. For example, the positive electrode binder may be one or a mixture or copolymer of two or more selected from the group consisting of fluororesin-based binders including polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); rubber-based binders including styrene butadiene rubber (SBR), acrylonitrile butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders; polyolefin-based binders including polyethylene and polypropylene; polyimide-based binders; polyester-based binders; and silane-based binders.
[0057] The positive electrode binder may be included in the positive electrode active material layer in an amount of 1 wt % to 10 wt %. If the content of the positive electrode binder is less than the range, the physical properties of the positive electrode may be deteriorated, and the positive electrode active material and the positive electrode conductive material may fall off, and if the content exceeds the range, the ratio of the positive electrode active material and the positive electrode conductive material in the positive electrode may relatively decrease, and the battery capacity may decrease. Therefore, it is preferable to determine the appropriate content within the above range.
[0058] 6, the positive electrode 200 may be in contact with the negative electrode-separator composite 100. Specifically, the separator 120 may be located between the positive electrode 200 and the negative electrode 110.
[0059] 4) Electrolytes The lithium secondary battery may further include an electrolyte. Examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries, but are not limited to these.
[0060] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt. Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0061] In particular, ethylene carbonate and propylene carbonate, which are cyclic carbonates among the carbonate-based organic solvents, can be preferably used as high-viscosity organic solvents, because they have a high dielectric constant and dissociate lithium salts well. When such cyclic carbonates are mixed in an appropriate ratio with linear carbonates having low viscosity and low dielectric constant, such as dimethyl carbonate and diethyl carbonate, an electrolyte having high electrical conductivity can be prepared, and therefore such a mixture can be used even more preferably.
[0062] The metal salt may be a lithium salt, which is a substance that is easily dissolved in the non-aqueous electrolyte solution. For example, the anion of the lithium salt may be F - , Cl - , I - , NO3 - , N(CN)2 -, BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.
[0063] In addition to the components of the electrolyte, the electrolyte may further include one or more additives such as a haloalkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride, in order to improve the life characteristics of the battery, suppress a decrease in the battery capacity, and improve the discharge capacity of the battery.
[0064] <Method of manufacturing lithium secondary battery> A method for manufacturing a lithium secondary battery according to another embodiment of the present invention includes the steps of disposing a first separator on one side of a negative electrode including a lithium metal layer and disposing a second separator on the other side of the negative electrode, and bonding at least a portion of an edge of the first separator and the second separator to each other to form a seal, thereby manufacturing a negative electrode-separator composite, wherein the air permeability of the seal may be 50,000 sec / 100 cc or more.
[0065] The lithium metal layer, the negative electrode, the first separator, the second separator, the sealing portion, the negative electrode-separator composite, the sealing portion, and the lithium secondary battery are similar to the lithium metal layer, the negative electrode, the first separator, the second separator, the sealing portion, the negative electrode-separator composite, the sealing portion, and the lithium secondary battery of the above-mentioned embodiment, and therefore detailed description thereof will be omitted.
[0066] 4, a first separator 121 may be disposed on one side of the negative electrode 110, and a second separator 122 may be disposed on the other side of the negative electrode 110. Since the width of the first separator 121 and the second separator 122 is wider than the width of the negative electrode 110, the first separator 121 and the second separator 122 may each include an edge that does not contact the negative electrode 110.
[0067] Referring to FIG. 5, in the step of manufacturing a negative electrode-separator composite by bonding at least a portion of each edge of the first separator 121 and the second separator 122 to each other to form a sealing portion 120a, the sealing portion 120a may be formed by heat-sealing at least a portion of each edge of the first separator 121 and the second separator 122 to each other.
[0068] The heat fusion may be performed at a temperature of 110°C to 140°C, specifically 120°C to 135°C, more specifically 125°C to 135°C. When the above range is satisfied, the pores of the seal part 120a may be effectively closed, specifically, the air permeability of the seal part 120a may be 50,000sec / 100cc or more. As a result, even when a positive electrode active material containing a sulfur element is used as the positive electrode active material, lithium polysulfide formed from the positive electrode is less likely to pass through the seal part 120a, and the lithium polysulfide can be effectively prevented from causing a side reaction at the negative electrode.
[0069] The heat sealing may include applying a pressure of 100 psi to 300 psi, specifically 120 psi to 250 psi, more specifically 150 psi to 200 psi. When this range is satisfied, pores in the sealed portion can be uniformly closed.
[0070] 6, the method may further include a step of contacting the negative electrode-separator composite 100 with a positive electrode 200. The positive electrode is the same as the positive electrode introduced in the above-mentioned embodiment, and therefore a description of the positive electrode will be omitted.
[0071] The method for manufacturing the lithium secondary battery is different from a method in which an electrode assembly including a negative electrode, a positive electrode, a first separator, and a second separator is manufactured, and then the first separator is brought into contact with the second separator. Specifically, the method for manufacturing the lithium secondary battery of the present invention may first manufacture a negative electrode-separator composite using a negative electrode, a first separator, and a second separator, and then bring the positive electrode into contact with the negative electrode-separator composite.
[0072] In this way, when the edges of the first separator and the second separator are at least partially bonded to form a seal before the electrode assembly is manufactured, the negative electrode and the first separator (or the second separator) are more closely attached to each other to form a negative electrode-separator composite. This effectively reduces the space (so-called death space) between the negative electrode and the first separator (or the second separator) in the negative electrode-separator composite, and more effectively inhibits the growth of lithium in the horizontal direction of the negative electrode.
[0073] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same. The battery module and the battery pack include the lithium secondary battery having high capacity, high rate characteristics, and high cycle characteristics, and therefore can be used as a power source for medium to large devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.
[0074] Below, preferred examples are presented to aid in understanding the present invention. However, the following examples are merely illustrative of the present description, and it will be apparent to those skilled in the art that various changes and modifications are possible within the scope and technical spirit of the present description. It goes without saying that such changes and modifications fall within the scope of the appended claims.
[0075] Examples and Comparative Examples Example 1: Manufacture of a lithium secondary battery (1) Manufacturing of negative electrode-separator composite A 16 μm thick polyethylene porous film (porosity 68%) was used as the first separator and the second separator. The first separator was placed on one side of a negative electrode made of a 80 μm thick lithium metal layer (lithium foil), and the second separator was placed on the other side of the negative electrode (located in the opposite direction to the one side). The horizontal and vertical lengths of the first separator were 1 mm larger than the horizontal and vertical lengths of the negative electrode, and the horizontal and vertical lengths of the second separator were 1 mm larger than the horizontal and vertical lengths of the negative electrode.
[0076] Thereafter, except for the point where the negative electrode tab contacts the first separator and the second separator, the portion where the first separator does not contact the negative electrode (the edge of the first separator) and the portion where the second separator does not contact the negative electrode (the edge of the second separator) were bonded to form a seal along the four sides of the negative electrode. The bonding was performed by heat sealing at a temperature of 130° C. and a pressure of 170 psi. The seal was formed surrounding the four sides of the negative electrode, and the air permeability of the seal was 89,000 sec / 100 cc. The air permeability was measured using an Oken Type Air-permeability & Smoothness Testing Controller device from ASAHI SEIKO under the conditions of Time: 6 sec, Value: 500, and Measure Mode: JIS (sec).
[0077] (2) Manufacturing of positive electrodes A positive electrode slurry composition was prepared by mixing sulfur-carbon composite (S:C=75:25) as a positive electrode active material, styrene-butadiene rubber and carboxymethyl cellulose (SBR:CMC=7:3) as a positive electrode binder with deionized water (DI water) as a solvent. The positive electrode slurry composition was applied to both sides of an aluminum current collector, dried at 80°C, and rolled (roll pressed) to form a positive electrode active material layer (loading amount: 2.7 mAh / cm 2 The sulfur-carbon composite was contained in the positive electrode active material layer at 96 wt %, and the positive electrode binder was contained in the positive electrode active material layer at 4 wt %.
[0078] (3) Manufacture of lithium secondary batteries After preparing eight negative electrode-separator composites and seven positive electrodes, the negative electrode-separator composites and the positive electrodes were alternately stacked with the separator between them to separate the negative electrodes and the positive electrodes to prepare an electrode assembly. The electrode assembly was then placed in a battery case, and an electrolyte (a mixture of 1M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 1 wt% lithium nitrate (LiNO3) dissolved in an organic solvent consisting of 1,3-dioxolane and dimethyl ether (DOL:DME=1:1 (volume ratio))) was injected into the battery case, and the battery case was sealed to prepare a lithium secondary battery (lithium-sulfur secondary battery).
[0079] Comparative Example 1: Manufacture of lithium secondary battery A total of 14 polyethylene porous films having a thickness of 16 μm were prepared as separators, and eight negative electrodes and seven positive electrodes were prepared as in Example 1. The negative electrodes and the positive electrodes were alternately stacked, and a separator was disposed between the negative electrodes and the positive electrodes to form an electrode assembly. That is, the separators were not bonded to each other and sealed, so there was no seal portion as in Example 1.
[0080] Thereafter, the electrode assembly was placed in a battery case, and an electrolyte (a mixture of 1 M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and 1 wt % lithium nitrate (LiNO3) dissolved in an organic solvent consisting of 1,3-dioxolane and dimethyl ether (DOL:DME = 1:1 (volume ratio))) was injected into the battery case, and the battery case was then sealed to manufacture a lithium secondary battery (lithium-sulfur secondary battery). Unlike Example 1, the lithium secondary battery of Comparative Example 1 does not include a negative electrode-separator composite including a seal portion.
[0081] Comparative Example 2: Manufacture of lithium secondary battery A lithium secondary battery was manufactured in the same manner as in Example 1, except that a temperature of 100°C was used as the bonding temperature when bonding the separator. The seal was formed surrounding the four sides of the negative electrode, and the air permeability of the seal was 3,000 sec / 100 cc. The air permeability was measured using an Oken Type Air-permeability & Smoothness Testing Controller from ASAHI SEIKO under the conditions of Time: 6 sec, Value: 500, and Measure Mode: JIS (sec).
[0082] Experimental Example 1: Evaluation of discharge capacity per cycle and coulombic efficiency of lithium secondary batteries The lithium secondary batteries of Example 1 and Comparative Examples 1 and 2 were charged and discharged at 25° C., and the discharge capacity and coulombic efficiency per cycle are shown in graphs (FIGS. 7 and 8). Each cycle was charged at 0.2 C (charged to 2.5 V) and discharged at 2.0 C (discharged to 1.7 V) (CC mode).
[0083] FIG. 7 shows the discharge capacity per cycle, and FIG. 8 shows the coulombic efficiency (the ratio of the discharge capacity to the charge capacity of 100%) per cycle. 7 and 8, it can be seen that the lithium secondary battery of Example 1 has a superior discharge capacity per cycle and coulombic efficiency as compared with the lithium secondary batteries of Comparative Examples 1 and 2.
[0084] Experimental example 2: Confirmation of whether lithium grows unevenly A test of Experimental Example 1 was carried out on Example 1 and Comparative Example 1, and changes in the negative electrode in the battery of Example 1 and the negative electrode in the battery of Comparative Example 1 were confirmed.
[0085] Specifically, Fig. 9 is a photograph of the negative electrode in the battery of Example 1 after 240 cycles, and Fig. 10 is a photograph of the negative electrode in the battery of Comparative Example 1 after 60 cycles. The dotted line in the photograph indicates the original size of the negative electrode before the battery was operated (in Comparative Example 1, the cell stopped operating after 60 cycles due to a voltage drop, so it was only possible to check the negative electrode at 60 cycles).
[0086] 9, the anode used in the battery of Example 1 maintained its initial size even after 240 cycles, whereas FIG 10 shows that the anode used in the battery of Comparative Example 1 had increased in size after only 60 cycles due to uneven lithium growth on the side of the anode. [Explanation of symbols]
[0087] 100: Negative electrode-separator composite 110: Negative electrode 120: Separator 121: First separator 122: Second separator 121': Edge of first separator 122': Edge of second separator 120a: Seal part 200: Positive electrode
Claims
1. a negative electrode-separator composite including a negative electrode and a separator; the negative electrode comprises a lithium metal layer; the separator includes a first separator disposed on one surface of the negative electrode and a second separator disposed on the other surface of the negative electrode; The first separator and the second separator, with the negative electrode housed therein, have at least a portion of an edge of the first separator and the second separator bonded to each other to form a seal portion; a sealing portion having an air permeability of 50,000 sec / 100 cc or more in a horizontal direction of the negative electrode;
2. 2. The lithium secondary battery according to claim 1, wherein the air permeability of the sealing portion is 65,000 sec / 100 cc to 100,000 sec / 100 cc.
3. the negative electrode includes a negative electrode tab; The lithium secondary battery of claim 1 , wherein the sealing portion is formed such that a remaining portion of the negative electrode excluding the negative electrode tab is not exposed to the outside of the separator.
4. The lithium secondary battery of claim 1 , wherein the negative electrode-separator composite further comprises an adhesive layer located between the negative electrode and the separator and including an adhesive binder.
5. The lithium secondary battery of claim 1 , wherein the separator further comprises a coating layer including pores having an average diameter of 0.1 nm to 1,000 nm.
6. The lithium secondary battery further includes a positive electrode including a positive electrode active material, 2. The lithium secondary battery according to claim 1, wherein the separator is located between the positive electrode and the negative electrode.
7. The positive electrode active material is inorganic sulfur (S 8 ), Li 2 S n1 (n1≧1), disulfide compounds, organic sulfur compounds, and carbon-sulfur polymers ((C 2 S x ) n2 7. The lithium secondary battery according to claim 6, comprising one or more selected from the group consisting of: x = 2.5 to 50, n2 ≧ 2.
8. disposing a first separator on one side of the negative electrode including the lithium metal layer and a second separator on the other side of the negative electrode; forming a seal portion by bonding at least a portion of an edge portion of the first separator and the second separator to each other to produce a negative electrode-separator composite; Including, The sealing portion has an air permeability of 50,000 sec / 100 cc or more.
9. The method of claim 8 , wherein the seal portion is formed by heat-sealing at least a portion of an edge of the first separator and the second separator to each other.
10. The method for producing a lithium secondary battery according to claim 9, wherein the heat fusion is performed at a temperature of 110°C to 140°C.
11. The method for producing a lithium secondary battery according to claim 8, further comprising the step of contacting the negative electrode-separator composite with a positive electrode.
Citation Information
Patent Citations
Nonaqueous electrolyte battery
JP1988202859A
Nonaqueous electrolyte secondary battery
JP1998027597A
Electric storage device and method of manufacturing the same
JP2010199282A
Electrode for secondary battery
JP2010212213A
Electrochemical device
JP2011258798A