Separator, electrode assembly, cylindrical battery cell, battery pack including the same, and automobile

The tab-less cylindrical battery cell design with a structured non-coated portion and insulating coating layers addresses high resistance and heat generation issues, improving current collection and electrolyte impregnation, thus enhancing safety and performance.

JP2024543432AInactive Publication Date: 2024-11-21LG ENERGY SOLUTION LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024527656
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-12
Filing Date
2022-11-14
Publication Date
2024-11-21
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional cylindrical battery cells face issues with high resistance and heat generation due to concentrated current flow, leading to potential fires, especially when used in electric vehicles, and have problems with electrolyte impregnation asymmetry and heat shrinkage, causing internal short circuits and poor performance.

Method used

A tab-less cylindrical battery cell design with a separation membrane having insulating coating layers on both ends and a structured non-coated portion with segmented electrode tabs to improve current collection efficiency, reduce resistance, and enhance electrolyte impregnation, while preventing short circuits and deformation.

Benefits of technology

The design reduces internal resistance, improves energy density, ensures uniform electrolyte impregnation, and prevents short circuits, enhancing the safety and performance of cylindrical battery cells, particularly in large form factors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543432000001_ABST
    Figure 2024543432000001_ABST
Patent Text Reader

Abstract

A separation membrane is provided, the separation membrane comprising: a porous polymer substrate; and a porous coating layer formed on at least one surface of the porous polymer substrate and including a binder polymer and inorganic particles. The separation membrane further comprises insulating coating layers at both ends of the outermost portion of the separation membrane in a transverse direction (TD), the insulating coating layers having a porous structure including a filler for the insulating coating layer and a binder for the insulating coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a separator, an electrode assembly, a cylindrical battery cell and a battery pack including the same, and a vehicle.

[0002] This application claims priority based on Korean Patent Application No. 10-2021-0156090, filed on November 12, 2021, and the entire contents disclosed in the specification and drawings of that application are incorporated herein by reference. [Background technology]

[0003] Secondary batteries, which are easily applicable to various products and have electrical properties such as high energy density, are widely used not only in portable devices but also in electric vehicles (EVs) and hybrid electric vehicles (HEVs) that are driven by electrical sources.

[0004] Such secondary batteries are attracting attention as a new energy source not only because they have the primary advantage of dramatically reducing the use of fossil fuels, but also because they are environmentally friendly and can improve energy efficiency, as they do not produce any by-products associated with energy use.

[0005] Currently, widely used types of secondary batteries include lithium-ion batteries, lithium polymer batteries, nickel-cadmium batteries, nickel-metal hydride batteries, and nickel-zinc batteries. The operating voltage of such unit secondary battery cells, i.e., unit battery cells, is approximately 2.5V to 4.5V. Therefore, if a higher output voltage is required, a battery pack is constructed by connecting multiple battery cells in series. Alternatively, a battery pack can be constructed by connecting multiple battery cells in parallel depending on the required charge / discharge capacity of the battery pack. Therefore, the number and electrical connection form of battery cells included in the battery pack can be variously set depending on the required output voltage or charge / discharge capacity.

[0006] Known types of secondary batteries include cylindrical, prismatic, and pouch-type secondary batteries. In the case of a cylindrical battery cell, a separator, which is an insulator, is interposed between a positive electrode and a negative electrode, and the separator is wound up to form a jelly-roll-shaped electrode assembly. This jelly-roll-shaped electrode assembly is then inserted into a battery can to form a battery. Strip-shaped electrode tabs may be connected to the uncoated portions of the positive and negative electrodes, electrically connecting the electrode assembly to electrode terminals exposed to the outside. For reference, the positive electrode terminal is a cap plate of a sealed body that seals the opening of the battery can, and the negative electrode terminal is the battery can. However, conventional cylindrical battery cells having this structure have problems such as high resistance, excessive heat generation, and poor current collection efficiency due to current concentration in the strip-shaped electrode tabs connected to the uncoated portions of the positive and / or negative electrodes.

[0007] Resistance and heat generation are not major issues for small cylindrical battery cells with form factors such as 18650 and 21700. However, when the form factor of cylindrical battery cells is increased to be used in electric vehicles, a large amount of heat is generated around the current collecting tabs during the fast charging process, which can cause the cylindrical battery cell to catch fire.

[0008] To solve this problem, a cylindrical battery cell (e.g., a tabless cylindrical battery cell) has been proposed, which has a structure in which positive and negative electrode uncoated areas are located at the upper and lower ends of a jelly roll-type electrode assembly, respectively, and current collecting plates are welded to these uncoated areas to improve current collection efficiency.

[0009] 4 to 6 are diagrams illustrating the manufacturing process of a tabless cylindrical battery cell. Fig. 4 shows the structure of the electrode plate, Fig. 5 shows the electrode plate winding process, and Fig. 6 shows the process of welding a current collector plate to the bent surface area of ​​the non-coated portion.

[0010] 4 to 6, the positive electrode 10 and the negative electrode 11 have a structure in which an active material 21 is coated on a sheet-shaped current collector 20, and include a non-coated portion 22 on one long side along the winding direction X.

[0011] The electrode assembly A is fabricated by sequentially stacking a positive electrode 10 and a negative electrode 11 together with two separators 12, as shown in Fig. 2, and then winding the stack in one direction (X direction). At this time, the non-coated portions of the positive electrode 10 and the negative electrode 11 are arranged in opposite directions.

[0012] After the winding process, the non-coated portion 10a of the positive electrode 10 and the non-coated portion 11a of the negative electrode 11 are bent toward the core side, and then the current collector plates 30 and 31 are welded and joined to the non-coated portions 10a and 11a, respectively.

[0013] The positive electrode non-coated portion 10a and the negative electrode non-coated portion 11a do not have separate electrode tabs attached, and current collecting plates 30 and 31 are connected to external electrode terminals, forming a current path with a large cross-sectional area along the winding axis direction of electrode assembly A (see arrow), which has the advantage of lowering the resistance of the battery. This is because resistance is inversely proportional to the cross-sectional area of ​​the path through which current flows.

[0014] In a table-less cylindrical battery cell, in order to improve the welding characteristics between the non-coated portions 10a, 11a and the current collector plates 30, 31, it is necessary to apply strong pressure to the welding points of the non-coated portions 10a, 11a to bend the non-coated portions 10a, 11a as flat as possible.

[0015] However, when the welded points of the non-coated portions 10a, 11a are bent, the patterns of the non-coated portions 10a, 11a may become irregularly distorted and deformed. In this case, the deformed portions may come into contact with the electrode of the opposite polarity, causing an internal short circuit, or microcracks may be induced in the non-coated portions 10a, 11a. Furthermore, as the non-coated portion 32 adjacent to the core of the electrode assembly A is bent, it may block all or a significant portion of the cavity in the core of the electrode assembly A. This causes problems during the electrolyte injection process. The cavity 33 in the core of the electrode assembly A serves as a passage through which the electrolyte is injected. However, if this passage is blocked, it is difficult to inject the electrolyte. Furthermore, when the electrolyte injector is inserted into the cavity 33, it may interfere with the non-coated portion 32 near the core, causing the non-coated portion 32 to break.

[0016] In addition, the bent portions of the non-coated portions 10a and 11a where the current collector plates 30 and 31 are welded must be overlapped in multiple places without any gaps. This is because sufficient welding strength can be obtained and, even when using cutting-edge technology such as laser welding, it is possible to prevent the laser from penetrating into the electrode assembly A and ablating the separator or active material.

[0017] Furthermore, in a conventional table-less cylindrical battery cell, a positive electrode non-coated area 10a is formed over the entire upper portion of the electrode assembly A. Therefore, when the outer periphery of the upper end of the battery can is pressed into the interior to form a beading portion, the upper peripheral area 34 of the electrode assembly A is subjected to pressure from the battery can. This pressure can cause partial deformation of the electrode assembly A, which can rupture the separator 12 and cause an internal short circuit. If a short circuit occurs inside the battery, heat generation or an explosion can occur.

[0018] Conventional separators incorporate a coating layer containing inorganic particles to improve the thermal shrinkage characteristics of the porous polymer substrate, but these are single-sided inorganic-coated separators, in which the coating layer is applied to only one side of the porous polymer substrate. When such inorganic-coated separators come into contact with the electrode in a jelly roll (J / R), one side is the original sheet and the other is the inorganic (ceramic) coating layer, resulting in asymmetric electrolyte impregnation characteristics. This asymmetry in electrolyte impregnation poses management issues, requiring the anode to be designed to match the separator; impregnating the jelly roll with the electrolyte requires increased pressure / vacuum conditions, which increases costs; and poor performance can occur if the impregnation process is not performed properly.

[0019] In addition, conventional separators with a single-sided inorganic coating have limited heat resistance due to one side of the separator being exposed, resulting in significant shrinkage at temperatures above 130°C. As a result, when subjected to thermal shock (above 130°C), the separator shrinks, causing short circuits in the internal electrodes, and the risk of fire increases when the internal temperature of the cell rises due to abnormal reactions (overcharging, external short circuit).

[0020] Furthermore, even when an inorganic coating layer is applied to the separator's porous polymer substrate, thermal shrinkage of the separator still occurs under high-temperature conditions, resulting in short circuits between the positive and negative electrodes. Furthermore, in the case of unnotched jelly rolls, folding of the foil current collector after assembly can create a closed structure between the inside and outside, hindering the movement of electrolyte to the electrodes within the jelly roll during injection, resulting in uneven electrolyte impregnation characteristics. This is believed to be due to the creation of uneven electrolyte impregnation paths during electrolyte impregnation. Therefore, the decrease in impregnation uniformity increases deviations between batteries, forming an unstable solid electrolyte interface (SEI) layer and increasing resistance dispersion. Summary of the Invention [Problem to be solved by the invention]

[0021] The present invention has been made in light of the background of the prior art as described above, and aims to provide a separator having an improved heat shrinkage rate.

[0022] The present invention has been made in light of the background of the prior art as described above, and another object of the present invention is to provide an electrode assembly having improved electrolyte impregnation characteristics.

[0023] Another technical object of the present invention is to provide an electrode assembly having an improved non-coated portion structure that can alleviate stress applied to the non-coated portions exposed at both ends of the electrode assembly when the non-coated portions are bent.

[0024] Another technical object of the present invention is to provide an electrode assembly in which the electrolyte injection passage is not blocked even when the non-coated portion is bent.

[0025] Another technical object of the present invention is to provide an electrode assembly including a structure capable of preventing contact between the edge of the upper end of the electrode assembly and the inner surface of the battery can when the upper end of the battery can is beaded.

[0026] It is still another technical object of the present invention to provide an electrode assembly having improved energy density and reduced resistance.

[0027] It is still another technical object of the present invention to provide a cylindrical battery cell including an electrode assembly with an improved structure, a battery pack including the same, and a vehicle including the battery pack.

[0028] The technical problems that the present invention aims to solve are not limited to the problems described above, and other problems not mentioned above will be clearly understood by those skilled in the art from the following description of the invention. [Means for solving the problem]

[0029] In order to achieve the above technical objectives, the following separation membranes are provided.

[0030] According to a first embodiment of the present invention, A separation membrane, the separation membrane comprising: a porous polymer substrate; and a porous coating layer formed on at least one surface of the porous polymer substrate, the porous coating layer including a binder polymer and inorganic particles; The separator has an insulating coating layer on each of both ends in a transverse direction (TD) at the outermost side thereof, The separator is characterized in that the insulating coating layer has a porous structure containing a filler for the insulating coating layer and a binder for the insulating coating layer.

[0031] According to a second embodiment of the present invention, in the first embodiment, The width of one insulating coating layer may be 0.1 to 10% of the entire width of the separator.

[0032] According to a third embodiment of the present invention, in the first or second embodiment, The average particle size of the filler for the insulating coating layer may be 10 to 90% of the average particle size of the inorganic filler.

[0033] According to a fourth embodiment of the present invention, in any one of the first to third embodiments, The vertical cross section of the insulating coating layer may have a rectangular, trapezoidal, triangular, parallelogram, semicircular or semi-elliptical structure.

[0034] According to a fifth embodiment of the present invention, A jelly-roll type electrode assembly having a structure in which sheet-shaped first and second electrode plates and a separator interposed therebetween are wound in one direction, The electrode assembly is provided, wherein the separator is the separator of any one of the first to fourth embodiments.

[0035] According to a sixth embodiment of the present invention, a jelly-roll type electrode assembly having a structure in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction; a battery can in which the electrode assembly is housed; and a sealing body that seals an open end of the battery can, A cylindrical battery cell is provided, characterized in that the separator is the separator according to any one of claims 1 to 4.

[0036] According to a seventh embodiment of the present invention, in the sixth embodiment, The cylindrical battery cell may have a form factor ratio of 0.4 or greater.

[0037] According to an eighth embodiment of the present invention, in the sixth or seventh embodiment, The cylindrical battery cell can be a 46110 cell, a 48750 cell, a 48110 cell, a 48800 cell, or a 46800 cell.

[0038] According to the ninth embodiment, in any one of the sixth to eighth embodiments, The cylindrical battery cell may be a battery with a tab-less structure that does not include electrode tabs.

[0039] According to a tenth embodiment of the present invention, in any one of the sixth to ninth embodiments, The positive electrode plate and the negative electrode plate each include an uncoated portion on which an active material layer is not formed, and the uncoated portion of the positive electrode plate and the uncoated portion of the negative electrode plate are located at an upper end and a lower end of the electrode assembly, respectively. Current collecting plates are coupled to the uncoated portion of the positive electrode plate and the uncoated portion of the negative electrode plate, and the current collecting plates may be connected to electrode terminals.

[0040] According to an eleventh embodiment of the present invention, A jelly-roll type electrode assembly having a structure in which sheet-shaped first and second electrode plates and a separator interposed therebetween are wound in one direction, At least one of the first electrode plate and the second electrode plate includes a non-coated portion at an end of a long side where the active material layer is not coated, At least a part of the non-coated portion is used as an electrode tab, the non-coated portion includes a core-side non-coated portion adjacent to a core of the electrode assembly, an outer periphery-side non-coated portion adjacent to an outer periphery surface of the electrode assembly, and an intermediate non-coated portion interposed between the core-side non-coated portion and the outer periphery-side non-coated portion, At least one of the core-side non-coating portion and the outer-periphery-side non-coating portion has a height in the winding axis direction that is relatively smaller than that of the intermediate non-coating portion, At least a portion of the intermediate non-application section is divided into a plurality of segment pieces, The electrode assembly is characterized in that the separator is the separator according to any one of claims 1 to 4.

[0041] An electrode assembly according to one embodiment of the present invention is a jelly-roll type electrode assembly having a structure in which sheet-shaped first and second electrode plates and a separator interposed therebetween are wound in one direction, and at least one of the first and second electrode plates includes a non-coated portion at a long side end where an active material layer is not coated.

[0042] Preferably, at least a portion of the non-coated portion can be used as an electrode tab, and the non-coated portion includes a core-side non-coated portion adjacent to the core of the electrode assembly, an outer-periphery-side non-coated portion adjacent to the outer peripheral surface of the electrode assembly, and an intermediate non-coated portion interposed between the core-side non-coated portion and the outer-periphery-side non-coated portion.

[0043] Preferably, at least one of the core-side non-coated portion and the outer-periphery-side non-coated portion may have a height in the axial direction of winding that is relatively smaller than that of the intermediate non-coated portion.

[0044] According to a twelfth embodiment of the present invention, in the eleventh embodiment, At least a portion of the intermediate non-coating portion may have a height in the winding axial direction that increases stepwise from the core side toward the outer periphery.

[0045] According to an embodiment of the present invention, at least a portion of the middle non-applied portion may be divided into a plurality of segments.

[0046] According to a thirteenth embodiment of the present invention, in the eleventh or twelfth embodiment, Each of the plurality of segment pieces may have a rectangular, trapezoidal, triangular, parallelogram, semicircular or semi-elliptical configuration.

[0047] According to a 14th embodiment of the present invention, in any one of the 11th to 13th embodiments, Each of the plurality of segment pieces has a trapezoidal shape, and the plurality of segment pieces may have a lower interior angle of the trapezoid that increases as the segment pieces move from the core side to the outer periphery side, individually or in groups.

[0048] According to a fifteenth embodiment of the present invention, in any one of the eleventh to fourteenth embodiments, At least one of the height and width in the winding direction of the plurality of segment pieces may increase stepwise from the core side to the outer periphery side, individually or in groups.

[0049] According to a 16th embodiment of the present invention, in any one of the 11th to 15th embodiments, Each of the plurality of segment pieces may satisfy at least one of the following conditions: a width of 1 to 6 mm in the winding direction, a height of 2 to 10 mm in the winding axial direction, and a spacing pitch of 0.05 to 1 mm in the winding direction.

[0050] According to a 17th embodiment of the present invention, in any one of the 11th to 16th embodiments, A predetermined gap may be provided between the lower end of the cutting line of the segment and the active material layer.

[0051] According to an eighteenth embodiment of the present invention, in the seventeenth embodiment, The gap may be 0.2 to 4 mm.

[0052] According to a 19th embodiment of the present invention, in any one of the 11th to 18th embodiments, The plurality of segment pieces form a plurality of segment piece groups as they move from the core side to the outer periphery side, and segment pieces belonging to the same segment piece group may be identical to each other in at least one of width in the winding direction, height in the winding axial direction, and spacing pitch in the winding direction.

[0053] According to a 20th embodiment of the present invention, in any one of the 11th to 19th embodiments, When the winding direction widths of three consecutively adjacent segment groups in the radial direction of the electrode assembly are W1, W2, and W3, respectively, the electrode assembly may include a combination of segment groups in which W3 / W2 is smaller than W2 / W1.

[0054] According to a 21st embodiment of the present invention, in any one of the 19th to 20th embodiments, The segments belonging to the same segment group may have at least one of a width in the winding direction, a height in the winding axial direction, and a spacing pitch in the winding direction that increases stepwise from the core side to the outer periphery side.

[0055] According to a 22nd embodiment of the present invention, in any one of the 19th to 21st embodiments, At least some of the plurality of segment groups may be arranged on the same winding turn of the electrode assembly.

[0056] According to a 23rd embodiment of the present invention, in any one of the 11th to 22nd embodiments, The core-side non-coating portion may not have a segmented structure.

[0057] According to a 24th embodiment of the present invention, in any one of the 11th to 23rd embodiments, The outer peripheral non-coated portion does not need to have a segmented structure.

[0058] According to a 25th embodiment of the present invention, in any one of the 11th to 24th embodiments, The plurality of segment pieces can be folded toward the core and overlapped in multiple layers.

[0059] According to a 26th embodiment of the present invention, in the 25th embodiment, The core of the electrode assembly may have a cavity, which may not be closed by a plurality of segmented pieces bent toward the core.

[0060] According to a 27th embodiment of the present invention, in the 26th embodiment, The radial length R of the core-side non-application portion and the bent length H of the innermost segment piece of the intermediate non-application portion can satisfy the relation H≦R.

[0061] According to a 28th embodiment of the present invention, in any one of the 11th to 27th embodiments, The height of the outer peripheral uncoated portion may decrease stepwise or gradually from the core side to the outer peripheral side.

[0062] According to a 29th embodiment of the present invention, in any one of the 11th to 28th embodiments, The outer non-application portion is divided into a plurality of segment pieces, and the plurality of segment pieces included in the outer non-application portion may be larger than the plurality of segment pieces included in the intermediate non-application portion in at least one of width in the winding direction, height in the winding axial direction, and separation pitch in the winding direction.

[0063] In order to achieve the above technical object, according to the 30th embodiment of the present invention, a jelly-roll type electrode assembly having a structure in which sheet-like first and second electrode plates and a separator interposed therebetween are wound in one direction; a battery can in which the electrode assembly is housed, electrically connected to one of the first electrode plate and the second electrode plate, and having a first polarity; a sealing body that seals the open end of the battery can; a terminal having a second polarity, electrically connected to the remaining one of the first electrode plate and the second electrode plate, and having a surface exposed to the outside; At least one of the first electrode plate and the second electrode plate includes a non-coated portion at a long side end portion where the active material layer is not coated, At least a part of the non-coated portion is used as an electrode tab, the non-coated portion includes a core-side non-coated portion adjacent to a core of the electrode assembly, an outer periphery-side non-coated portion adjacent to an outer periphery surface of the electrode assembly, and an intermediate non-coated portion interposed between the core-side non-coated portion and the outer periphery-side non-coated portion, At least one of the core-side non-coating portion and the outer-periphery-side non-coating portion has a height in the winding axis direction that is relatively smaller than that of the intermediate non-coating portion, At least a portion of the intermediate non-application section is divided into a plurality of segment pieces, The cylindrical battery cell is provided, wherein the separator is the separator described in any one of the first to fourth embodiments.

[0064] A cylindrical battery cell according to one embodiment of the present invention may include: a jelly-roll-type electrode assembly having a structure in which sheet-like first and second electrode plates and a separator interposed therebetween are wound in one direction; a battery can in which the electrode assembly is housed and which is electrically connected to one of the first and second electrode plates and has a first polarity; a sealing body which seals an open end of the battery can; and a terminal which is electrically connected to the remaining one of the first and second electrode plates and has a second polarity, the surface of which is exposed to the outside.

[0065] According to an embodiment of the present invention, at least one of the first electrode plate and the second electrode plate may include a non-coated portion at a long side end portion where the active material layer is not coated.

[0066] According to one embodiment of the present invention, at least a portion of the non-coated portion is used as an electrode tab, and the non-coated portion includes a core-side non-coated portion adjacent to a core of the electrode assembly, an outer-periphery-side non-coated portion adjacent to an outer peripheral surface of the electrode assembly, and an intermediate non-coated portion interposed between the core-side non-coated portion and the outer-periphery-side non-coated portion, and at least one of the core-side non-coated portion and the outer-periphery-side non-coated portion may have a relatively smaller height in the winding axis direction than the intermediate non-coated portion.

[0067] According to a 31st embodiment of the present invention, in the 30th embodiment, The outer non-coated portion may have a height in the axial direction of winding that is relatively smaller than that of the intermediate non-coated portion, the battery can may have a beading portion that is press-fitted inward at an end portion adjacent to an open end, and an inner peripheral surface of the beading portion that faces an upper peripheral edge portion of the electrode assembly and the outer non-coated portion may be spaced apart by a predetermined distance.

[0068] According to a 32nd embodiment of the present invention, in the 30th or 31st embodiment, The press-fit height D1 of the beading portion and the distance D2 from the inner peripheral surface of the battery can to the boundary point between the outer peripheral non-coated portion and the middle non-coated portion can satisfy the relational expression D1≦D2.

[0069] According to a 33rd embodiment of the present invention, in any one of the 30th to 32nd embodiments, The adhesive tape may further include a collecting plate electrically coupled to the middle non-coated portion, and an insulator covering the collecting plate and having a peripheral portion interposed and fixed between an inner peripheral surface of the beading portion and the collecting plate.

[0070] According to a 34th embodiment of the present invention, in the 33rd embodiment, The outermost diameters of the collecting plate and the intermediate non-coated portion are smaller than the smallest inner diameter of the inner surface of the beading portion, and the diameter of the collecting plate may be the same as or larger than the outermost diameter of the intermediate non-coated portion.

[0071] According to a 35th embodiment of the present invention, in the 33rd or 34th embodiment, The current collecting plate may be positioned higher than the beading portion.

[0072] According to a 36th embodiment of the present invention, in any one of the 30th to 35th embodiments, At least a portion of the intermediate non-application portion is bent from the outer periphery toward the core, and a cavity is provided in the core of the electrode assembly, and the cavity does not have to be blocked by the bent structure of the intermediate non-application portion.

[0073] According to a 37th embodiment of the present invention, in the 36th embodiment, The intermediate non-coating portion includes a plurality of segment pieces segmented along the winding direction of the electrode assembly, and the plurality of segment pieces are bent from the outer periphery side to the core side, and the radial length R of the core-side non-coating portion and the bending length H of the segment piece located at the innermost side of the intermediate non-coating portion may satisfy the relational expression H≦R.

[0074] According to a 38th embodiment of the present invention, in the 37th embodiment, Each of the plurality of segment pieces may have a rectangular, trapezoidal, triangular, parallelogram, semicircular or semi-elliptical configuration.

[0075] According to a 39th embodiment of the present invention, in the 37th or 38th embodiment, Each of the plurality of segment pieces may satisfy at least one of the following conditions: a width of 1 to 6 mm in the winding direction, a height of 2 to 10 mm in the winding axial direction, and a spacing pitch of 0.05 to 1 mm in the winding direction.

[0076] According to a 40th embodiment of the present invention, in any one of the 30th to 39th embodiments, A gap may be provided between the lower end of the cutting line of the segment and the active material layer.

[0077] According to a 41st embodiment of the present invention, in the 40th embodiment, The gap may be 0.2 to 4 mm.

[0078] According to a 42nd embodiment of the present invention, in any one of the 37th to 41st embodiments, The plurality of segment pieces are arranged in a plurality of groups, and the segment pieces belonging to each group have the same at least one of the width in the winding direction, the height in the winding axial direction, and the separation pitch in the winding direction, and at least one of the plurality of groups may constitute the same winding turn of the electrode assembly.

[0079] According to a 43rd embodiment of the present invention, in any one of the 37th to 42nd embodiments, When the winding direction widths of three segment groups adjacent to each other in the radial direction of the electrode assembly are W1, W2, and W3, respectively, the electrode assembly may include a combination of segment groups in which W3 / W2 is smaller than W2 / W1.

[0080] According to a 44th embodiment of the present invention, in any one of the 37th to 43rd embodiments, The sealing body may include a cap plate that seals the open end of the battery can, and a gasket that surrounds the periphery of the cap plate and is crimped to the upper end of the battery can, and the terminal having the second polarity may be the cap plate.

[0081] According to a 45th embodiment of the present invention, in any one of the 37th to 44th embodiments, The battery can further includes a current collecting plate electrically connected to the uncoated portion of the second electrode plate having the first polarity and having at least a portion of its edge joined to a side wall of the battery can. In this case, the sealing body may include a non-polar cap plate and a gasket surrounding a peripheral portion of the cap plate and crimped to an upper end of the battery can, and the battery can may include a rivet terminal having the second polarity, electrically connected to the first electrode plate, and insulatively installed in a through-hole formed in a central portion of a closed surface.

[0082] According to a 46th embodiment of the present invention, there is provided a battery pack including at least one cylindrical battery cell according to any one of the 30th to 45th embodiments.

[0083] According to a 47th embodiment of the present invention, there is provided a vehicle including at least one battery pack according to the 46th embodiment. [Effects of the Invention]

[0084] According to one aspect of the present invention, in a separator including a porous coating layer including inorganic particles and a binder polymer on at least one surface of a porous polymer substrate, insulating coating layers are provided on both lateral ends of the outermost surface of the separator, thereby improving the heat resistance and compression resistance of the separator, preventing short circuits within the battery cell, improving the impregnation of the electrolyte into the electrodes within the battery cell, and enhancing the stability of the battery cell.

[0085] According to one aspect of the present invention, the non-coated portions protruding upward and downward of the electrode assembly are used as electrode tabs, thereby reducing the internal resistance of the battery cell and increasing the energy density.

[0086] According to another aspect of the present invention, the structure of the non-coated portion of the electrode assembly is improved to prevent interference between the electrode assembly and the inner surface of the battery can during the process of forming the beading portion of the battery can, thereby preventing a short circuit inside the cylindrical battery cell due to partial deformation of the electrode assembly.

[0087] According to yet another aspect of the present invention, the structure of the non-coated portion of the electrode assembly is improved to prevent the non-coated portion from breaking when bent, and the number of overlapping layers of the non-coated portion is sufficiently increased to improve welding strength.

[0088] According to yet another aspect of the present invention, the structure of the non-coated portion adjacent to the core of the electrode assembly is improved to prevent the cavity in the core of the electrode assembly from being blocked when the non-coated portion is bent, thereby facilitating the process of injecting the electrolyte and the process of welding the battery can and the current collecting plate.

[0089] According to yet another aspect of the present invention, it is possible to provide a cylindrical battery cell having a structure in which internal resistance is low, internal short circuits are prevented, and the welding strength between the current collecting plate and the non-coated portion is improved, as well as a battery pack and a vehicle including the same.

[0090] The present invention also provides various other effects, which will be explained in the respective embodiments, and explanations of effects that can be easily inferred by ordinary skilled artisans will be omitted.

[0091] The following drawings attached to this specification illustrate preferred embodiments of the present invention and, together with the detailed description of the invention, serve to further understand the technical concept of the present invention, so the present invention should not be interpreted as being limited to the matters described in the drawings. [Brief explanation of the drawings]

[0092] [Figure 1] 1 is a schematic diagram of a separation membrane according to an embodiment of the present invention. [Figure 2] 1 is a schematic diagram of a separation membrane according to an embodiment of the present invention. [Figure 3] 1 is a schematic diagram illustrating a manufacturing process of a separator according to an embodiment of the present invention. [Figure 4] 1 is a plan view showing the structure of an electrode plate used in manufacturing a conventional tabless cylindrical battery cell. FIG. [Figure 5] 1A and 1B are diagrams illustrating a winding process of an electrode plate of a conventional tabless cylindrical battery cell. [Figure 6] 10 shows the process of welding a current collecting plate to the bent surface of the non-coated portion in a conventional tabless cylindrical battery cell. [Figure 7] 1 is a plan view showing the structure of an electrode plate according to a first embodiment of the present invention. [Figure 8] FIG. 10 is a plan view showing the structure of an electrode plate according to a second embodiment of the present invention. [Figure 9] FIG. 10 is a plan view showing the structure of an electrode plate according to a third embodiment of the present invention. [Figure 10a] FIG. 10 is a plan view showing the structure of an electrode plate according to a fourth embodiment of the present invention. [Figure 10b] FIG. 10 is an enlarged view showing the segment piece portion in more detail. [Figure 10c] FIG. 10 is an enlarged view showing the segment piece portion in more detail. [Figure 11] 10 is a diagram illustrating the definition of the width, height, and spacing pitch of segment pieces according to an embodiment of the present invention. [Figure 12a] FIG. 10 is a plan view showing the structure of an electrode plate according to a fifth embodiment of the present invention. [Figure 12b] FIG. 10 is an enlarged view showing the segment piece portion in more detail. [Figure 12c] FIG. 10 is an enlarged view showing the segment piece portion in more detail. [Figure 13] 10 is a diagram illustrating the definition of the width, height, and spacing pitch of segment pieces according to an embodiment of the present invention. [Figure 14] FIG. 1 is a cross-sectional view of a jelly-roll type electrode assembly in which the electrode plates of the first embodiment are applied to the first electrode plate (positive electrode plate) and the second electrode plate (negative electrode plate), taken along the Y-axis direction (winding axis direction). [Figure 15] FIG. 10 is a cross-sectional view of a jelly-roll type electrode assembly in which the electrode plates of the second embodiment are applied to the first electrode plate (positive electrode plate) and the second electrode plate (negative electrode plate), taken along the Y-axis direction (winding axis direction). [Figure 16] FIG. 10 is a cross-sectional view of a jelly-roll type electrode assembly in which any one of the electrode plates of the third to fifth embodiments (these modified examples) is applied to the first electrode plate (positive electrode plate) and the second electrode plate (negative electrode plate) along the Y-axis direction (winding axis direction). [Figure 17] 10 is a cross-sectional view of an electrode assembly according to yet another embodiment of the present invention, taken along the Y-axis direction (winding axis direction). [Figure 18]10 is a cross-sectional view of an electrode assembly according to yet another embodiment of the present invention, taken along the Y-axis direction (winding axis direction). [Figure 19] 10 is a cross-sectional view of an electrode assembly according to yet another embodiment of the present invention, taken along the Y-axis direction (winding axis direction). [Figure 20] 2 is a cross-sectional view of a cylindrical battery cell according to an embodiment of the present invention taken along a Y-axis direction. FIG. [Figure 21] FIG. 4 is a cross-sectional view of a cylindrical battery cell according to another embodiment of the present invention taken along the Y-axis direction. [Figure 22] FIG. 10 is a cross-sectional view of a cylindrical battery cell according to yet another embodiment of the present invention taken along the Y-axis direction. [Figure 23] FIG. 10 is a cross-sectional view of a cylindrical battery cell according to yet another embodiment of the present invention taken along the Y axis. [Figure 24] FIG. 10 is a cross-sectional view of a cylindrical battery cell according to yet another embodiment of the present invention taken along the Y axis. [Figure 25] FIG. 10 is a cross-sectional view of a cylindrical battery cell according to yet another embodiment of the present invention taken along the Y axis. [Figure 26] FIG. 10 is a cross-sectional view of a cylindrical battery cell according to yet another embodiment of the present invention taken along the Y axis. [Figure 27] FIG. 10 is a cross-sectional view of a cylindrical battery cell according to yet another embodiment of the present invention taken along the Y axis. [Figure 28] FIG. 10 is a cross-sectional view of a cylindrical battery cell according to yet another embodiment of the present invention taken along the Y axis. [Figure 29] 1 is a diagram illustrating a schematic configuration of a battery pack according to an embodiment of the present invention; [Figure 30] 1 is a schematic diagram of a vehicle including a battery pack according to an embodiment of the present invention. [Figure 31] 1 is a graph showing the compression characteristics of the separation membranes of Example 1 and Comparative Example 1. [Figure 32] 1 is a graph showing the resistance characteristics of cylindrical battery cells having separators according to Example 1 and Comparative Example 1. [Figure 33] 1 is a graph showing the evaluation results of the impregnation amount (impregnation property) of the electrolyte of the positive electrode and the negative electrode of cylindrical battery cells provided with separators of Example 1 and Comparative Example 1. [Figure 34] FIG. 2 is a diagram showing the positions where impregnated samples were collected from the electrode assemblies of Example 1 and Comparative Example 1. [Figure 35] 1 is a graph showing voltage and temperature characteristics of cylindrical battery cells having separators according to Example 1 and Comparative Example 1. DETAILED DESCRIPTION OF THE INVENTION

[0093] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the accompanying drawings. Prior to this, the terms and words used in the specification and claims should not be construed as being limited to their ordinary or dictionary meanings, but should be construed as having meanings and concepts corresponding to the technical ideas of the present invention, in accordance with the principle that the inventor himself can appropriately define the concepts of terms in order to best explain the invention.

[0094] Therefore, it should be understood that the embodiments described in this specification and the configurations shown in the drawings are merely the most preferred embodiment of the present invention and do not represent the entire technical idea of ​​the present invention, and that there may be various equivalents and modifications that can be substituted for them at the time of this application.

[0095] In order to facilitate understanding of the invention, the accompanying drawings may be drawn not to scale but with some components exaggerated. The same reference numerals may be used to refer to the same components in different embodiments.

[0096] According to one aspect of the present invention, A separation membrane, The separator includes a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, the porous coating layer including a binder polymer and inorganic particles; The separator has an insulating coating layer on each of both ends in a transverse direction (TD) at the outermost side thereof, The separator is characterized in that the insulating coating layer has a porous structure containing a filler for the insulating coating layer and a binder for the insulating coating layer.

[0097] 1 and 2 show a separation membrane according to an embodiment of the present invention.

[0098] 1 and 2, a separator according to an embodiment of the present invention comprises a porous coating layer 2 on one side of a porous polymer substrate 1, and an insulating coating layer 3 on each of both outermost ends of the separator. In this case, when a porous coating layer is provided on only one side of the separator porous substrate, the outermost side of the separator is the porous coating layer and one side of the porous polymer substrate (on which no porous coating layer is formed).

[0099] In addition, when the separator porous substrate has porous coating layers on both sides, the outermost surfaces of the separator may be the porous coating layers on both sides, and insulating coating layers may be provided on both lateral ends of the porous coating layers on both sides.

[0100] The porous polymer substrate may be a polyolefin-based porous substrate.

[0101] The polyolefin porous substrate may be in the form of a film or a non-woven web. The porous structure facilitates smooth movement of the electrolyte between the positive and negative electrodes, increases the electrolyte impregnation of the substrate, ensuring excellent ionic conductivity. Furthermore, the increase in the internal resistance of the electrochemical device is prevented, thereby preventing degradation of the performance of the electrochemical device.

[0102] The polyolefin porous substrate used in the present invention can be any planar porous substrate that is commonly used in electrochemical devices, and the material and shape thereof can be selected from a variety of materials depending on the purpose.

[0103] The polyolefin porous substrate may be, but is not limited to, a film or nonwoven web formed from high density polyethylene, low density polyethylene, linear low density polyethylene, ultra-high molecular weight polyethylene, polypropylene, or a mixture of two or more thereof.

[0104] The polyolefin porous substrate may have a thickness of 8 to 30 μm, but this is merely an example, and thicknesses outside this range may be adopted in consideration of mechanical properties and high-rate charge / discharge characteristics of the battery.

[0105] The nonwoven fabric sheet according to the present invention may be formed from polyethylene (PE), polypropylene (PP), or a mixture of two or more thereof. For example, the nonwoven fabric sheet may be produced by fiber spinning. For example, the nonwoven fabric sheet may be produced by blended spinning in which fibers of the material are spun into fiber at or above their melting points using a meltblown method.

[0106] The nonwoven fabric sheet may have an elongation ratio of 200 to 400%, more preferably 300 to 400%. If the elongation ratio is less than 200%, the probability of contact between electrodes increases when a nail penetrates, while if the elongation ratio is greater than 400%, the area around the nail penetration also elongates, making the separator thinner and reducing its barrier properties.

[0107] The nonwoven fabric sheet has a plurality of pores with an average diameter of 0.1 to 10 μm. If the pore size is smaller than 0.1 μm, smooth movement of lithium ions and / or electrolyte solution will be hindered, and if the pore size is larger than 10 μm, it may be difficult to achieve the effect of the present invention, which is to prevent contact between the positive electrode and the negative electrode by stretching the nonwoven fabric sheet when a nail penetrates.

[0108] The nonwoven fabric sheet may have a porosity of 40 to 70%. If the porosity is less than 40%, the lithium ions and / or electrolyte may not move smoothly, and if the porosity is greater than 70%, the effect of the present invention, which is to prevent contact between the positive and negative electrodes by stretching the nonwoven fabric sheet when a nail penetrates it, may not be achieved. The nonwoven fabric sheet produced in this manner may have an air permeability of 1 to 20 seconds / 100 mL.

[0109] The nonwoven fabric sheet may have a thickness of 10 to 20 μm, but this is merely an example and is not intended to be limiting. A nonwoven fabric sheet having a thickness outside this range may also be used depending on the permeability of the nonwoven fabric sheet.

[0110] The nonwoven fabric sheet can be bonded to the separator components placed below the nonwoven fabric sheet by lamination, which can be performed at a temperature of 100 to 150°C. However, if the lamination is performed at a temperature lower than 100°C, the lamination effect is lost, and if the lamination is performed at a temperature higher than 150°C, part of the nonwoven fabric will melt.

[0111] The separator according to one embodiment of the present invention, which is laminated under the above conditions, has improved resistance to nail penetration compared to conventional separators made of nonwoven fabric sheets or separators in which a layer containing inorganic particles is formed on at least one surface of a film or nonwoven fabric sheet.

[0112] In the porous coating layer, inorganic particles are charged and in contact with each other and bound to each other by the binder polymer, thereby forming interstitial volumes between the inorganic particles, and the interstitial volumes between the inorganic particles may become empty spaces to form pores.

[0113] The inorganic particles used to form the porous coating layer are inorganic particles, i.e., particles that are within the operating voltage range (e.g., Li / Li+ Inorganic particles that do not undergo oxidation and / or reduction reactions at a voltage of 0 to 5 V (based on the reference voltage) may be further added. In particular, when inorganic particles having ion transfer ability are used, the ionic conductivity within the electrochemical device can be increased, thereby improving performance. Furthermore, when inorganic particles having a high dielectric constant are used as the inorganic particles, they can contribute to increasing the degree of dissociation of electrolyte salts, such as lithium salts, in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte solution.

[0114] For the reasons mentioned above, the inorganic particles preferably include inorganic particles with a high dielectric constant having a dielectric constant of 5 or more, preferably 10 or more, inorganic particles having lithium ion transfer ability, or a mixture thereof.

[0115] Non-limiting examples of inorganic particles having a dielectric constant of 5 or greater include BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT), PB(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC, or a mixture thereof.

[0116] In particular, the aforementioned BaTiO3, Pb(Zr,Ti)O3 (PZT), and Pb 1-x La x Zr 1-y Ti y O3(PLZT), PB(Mg 1 / 3 Nb 2 / 3Inorganic particles such as )O3-PbTiO3 (PMN-PT) and hafnia (HfO2) not only exhibit high dielectric constants of over 100, but also possess piezoelectricity, which generates a potential difference between the two surfaces when stretched or compressed under a certain pressure, preventing internal short circuits between the electrodes due to external impacts and improving the safety of electrochemical devices. Furthermore, when inorganic particles with high dielectric constants are used in combination with inorganic particles with lithium ion transport capabilities, the synergistic effects of these two materials can be multiplied.

[0117] Inorganic particles with lithium ion transport ability refer to inorganic particles that contain lithium element but have the function of transporting lithium ions without storing lithium. Inorganic particles with lithium ion transport ability can transport and move lithium ions due to a type of defect present inside the particle structure, thereby improving the conductivity of lithium ions in a battery and thereby improving battery performance. Non-limiting examples of inorganic particles with lithium ion transport ability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3,0 <x<2、0<y<3)、リチウムアルミニウムチタンホスフェート(Li x Al y Ti z (PO4)3,0 <x<2、0<y<1、0<z<3)、14Li2O-9Al2O3-38TiO2-39P2O5などのような(LiAlTiP) x O y Glass (0 <x<4、0<y<13)、リチウムランタンチタネート(Li x La y TiO3, 0 <x<2、0<y<3)、Li 3.25 Ge 0.25 P 0.75 Lithium germanium thiophosphate (Li x Ge y P z S w, (0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride such as Li3N (Li x N y , (0 < x < 4, 0 < y < 2), SiS2-based glass such as Li3PO4-Li2S-SiS2 (Li x Si y S z , (0 < x < 3, 0 < y < 2, 0 < z < 4), P2S5-based glass such as LiI-Li2S-P2S5 (Li x P y S z , (0 < x < 3, 0 < y < 3, 0 < z < 7) or mixtures thereof, etc. can be mentioned.

[0118] The size of the inorganic particles in the porous coating layer is not limited, but for the formation of a coating layer with a uniform thickness and an appropriate porosity, it is preferably 0.001 to 10 μm. If it is less than 0.001 μm, the dispersibility of the inorganic particles decreases. If it exceeds 10 μm, the thickness of the porous coating layer increases and the mechanical properties deteriorate, and the probability of internal short circuit during charge and discharge of the battery increases due to too large pore sizes.

[0119] Examples of binder polymers that form the porous coating layer include polyvinylidene fluoride-co-hexafluoropropylene (PVdF), polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene-vinyl acetate copolymer (polyethylene-co-vinyl acetate), polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. The binder polymer may be any one selected from the group consisting of cellulose acetate, cellulose acetate ester ...

[0120] The composition ratio of inorganic particles to binder polymer used in the porous coating layer may be, for example, 50:50 to 99:1 or 70:30 to 95:5. When the inorganic particle to binder polymer content ratio satisfies this range, the thermal stability of the separator can be improved, sufficient space between the inorganic particles can be secured to maintain pore size and porosity, improving final battery performance, and the binder polymer content can be included at a titration level to improve the peel resistance of the porous coating layer. The thickness of the porous coating layer is not particularly limited, but is preferably in the range of 0.01 to 20 μm. The pore size and porosity are also not particularly limited, but are preferably in the range of 0.001 to 10 μm and 10 to 90%. The pore size and porosity mainly depend on the size of the inorganic particles. For example, when inorganic particles with a particle size of 1 μm or less are used, the resulting pores will also be approximately 1 μm or less. Such a pore structure is filled with the electrolyte to be injected later, and the filled electrolyte plays a role of ion transport. When the pore size and porosity satisfy such ranges, the film does not function as a resistance layer and has improved mechanical properties.

[0121] The porous coating layer can be formed by dissolving or dispersing a binder polymer in a dispersion medium, adding inorganic particles to obtain a slurry for forming the porous coating layer, and then coating and drying the slurry on at least one surface of a substrate. The dispersion medium preferably has a solubility index similar to that of the binder polymer to be used and a low boiling point to facilitate uniform mixing and subsequent removal of the dispersion medium. Non-limiting examples of dispersion mediums that can be used include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or a mixture thereof.

[0122] It is preferable to add inorganic particles to a dispersion in which the binder polymer is dispersed in a dispersion medium, and then crush the inorganic particles. In this case, the crushing time is preferably 1 to 20 hours, and the particle size of the crushed inorganic particles is preferably 0.001 to 10 μm, as described above. Conventional crushing methods can be used, and a ball mill method is particularly preferable.

[0123] The binder polymer dispersion liquid containing dispersed inorganic particles is then coated onto at least one surface of a porous polymer substrate under a humidity condition of 10 to 80% and dried. The dispersion liquid can be coated onto the porous polymer substrate using a coating method known in the art. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a combination thereof can be used.

[0124] In addition to the inorganic particles and binder polymer described above as components of the porous coating layer, other additives such as conductive materials may be further included.

[0125] The final separator according to the present invention may have a thickness of 1-100 μm or 5-50 μm. If the thickness is less than 1 μm, the separator may not function properly and mechanical properties may deteriorate, while if the thickness exceeds 100 μm, battery properties may deteriorate during high-rate charge / discharge. The separator may also have a porosity of 40-60% and an air permeability of 150-300 sec / 100 mL.

[0126] According to an embodiment of the present invention, the porous polymer substrate may be polyethylene or polypropylene-based, and the inorganic particles in the porous coating layer may be aluminum oxide or silicon oxide-based coating materials.

[0127] When using a separator according to an embodiment of the present invention, the porous coating layers on both sides of the porous polymer substrate improve the electrolyte impregnation performance, forming a uniform solid electrolyte interfacial layer and ensuring superior air permeability compared to conventional cross-section inorganic-coated separators. For example, it can be within 120 s / 100 cc. Furthermore, even with inorganic porous coating layers on both sides, it can achieve the same thickness as a conventional single-sided inorganic-coated separator. For example, it can be within 15.0 μm.

[0128] Furthermore, when a separator according to an embodiment of the present invention is used, the separator's stability is improved, ensuring heat resistance and compression resistance. Specifically, the separator can have heat resistance with a thermal shrinkage of 5% or less at 180°C, and can have a puncture strength of 550 gf or more. When core deformation occurs during cycling of a battery using such a separator, the separator can be prevented from being damaged or penetrated at the step.

[0129] The insulating coating layer includes an insulating coating filler and an insulating coating binder.

[0130] The filler for the insulating coating layer may be selected from the inorganic particles contained in the porous coating layer described above, and the binder for the insulating coating layer may be selected from the binder polymers contained in the porous coating layer described above. The filler for the insulating coating layer and the binder for the insulating coating layer may be the same or different from the inorganic particles and the binder polymers contained in the porous coating layer described above, respectively.

[0131] According to one embodiment of the present invention, non-limiting examples of the filler for the insulating coating layer include BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT), PB(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiC, or a mixture thereof.

[0132] According to an embodiment of the present invention, non-limiting examples of the binder for the insulating coating layer include polyvinylidene fluoride-co-hexafluoropropylene (PVdF), polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polybutylacrylate, polyacrylonitrile, and polyvinylpyrrolidone. Examples of binder polymers include any one selected from the group consisting of polyvinyl acetate, ethylene-vinyl acetate copolymer, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, and carboxyl methyl cellulose, or a mixture of two or more of these.

[0133] According to an embodiment of the present invention, the composition ratio of the filler for the insulating coating layer to the binder for the insulating coating layer used in the insulating coating layer may be, for example, 50:50 to 99:1, or 70:30 to 95:5.

[0134] According to one embodiment of the present invention, the average particle size of the filler for the insulating coating layer may be smaller than the average particle size of the inorganic filler. Specifically, the average particle size of the filler for the insulating coating layer may be 10% or more, 20% or more, 30% or more, 40% or more, 50% or more, 50% or less, 60% or less, 70% or less, 80% or less, or 90% or less of the average particle size of the inorganic filler. When the average particle size of the filler for the insulating coating layer is smaller than the average particle size of the inorganic filler or satisfies such a ratio, the packing density of the filler in the insulating coating layer increases, thereby further suppressing thermal shrinkage of the separator.

[0135] According to one embodiment of the present invention, the insulating coating layers formed on both lateral ends of the separator may contact uncoated portions of the electrodes (positive and negative electrodes) in the electrode assembly, and the width of the insulating layer may be adjusted so that the insulating coating layer does not directly contact the active material layers of the electrodes. For example, the width of one insulating coating layer may be 0.1% or more, 0.5% or more, 1% or more, 3% or more, 5% or less, 7% or less, 9% or less, or 10% or less of the total length of the separator in the width direction.

[0136] According to an embodiment of the present invention, the vertical cross section of the insulating coating layer may have a rectangular, trapezoidal, triangular, parallelogram, semicircular, or semi-elliptical structure. Since the insulating coating layer comes into contact with the non-coated area of ​​the electrode, a rectangular, trapezoidal, or parallelogram shape is more preferable to enhance adhesion with the non-coated area.

[0137] FIG. 3 is a schematic diagram illustrating a manufacturing process of a separator according to an embodiment of the present invention.

[0138] Referring to FIG. 3, a method for manufacturing a separator according to an embodiment of the present invention is as follows.

[0139] First, a porous polymer substrate 1 (separator membrane raw material, large unslit raw material) is prepared (step a).

[0140] Then, a binder polymer is dissolved or dispersed in a dispersion medium, and inorganic particles are added to obtain a slurry for forming a porous coating layer. The slurry is then coated on one or both sides of the porous substrate 1 and dried to form a porous coating layer (step b).

[0141] Next, a binder for the insulating coating layer is dissolved or dispersed in a dispersion medium for the insulating coating layer, and a filler for the insulating coating layer is added to obtain a slurry for forming the insulating coating. The slurry is then coated on both lateral ends of the outermost portion of the separator to a predetermined width, and dried to form an insulating coating layer (step c).

[0142] Thereafter, the separator roll on which the insulating coating layer is formed is slit according to a width required for assembling a battery cell, and finally, a separator having a porous coating layer and an insulating coating layer sequentially formed on a porous polymer substrate is manufactured (step d).

[0143] A cylindrical battery cell according to the present invention will now be described.

[0144] A cylindrical battery cell according to the present invention may include a jelly-roll-type electrode assembly having a structure in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode and the negative electrode are wound in one direction; a battery can in which the electrode assembly is housed; and a seal that seals an open end of the battery can.

[0145] Preferably, the cylindrical battery cell according to the present invention may be a large cylindrical battery cell having a form factor ratio (defined as the ratio of the diameter Φ to the height H of a cylindrical battery, i.e., the diameter Φ divided by the height H) of 0.4 or more. Here, the form factor refers to values ​​indicating the diameter and height of a cylindrical battery cell.

[0146] Cylindrical battery cells according to the present invention may be, for example, a 46110 cell (diameter 46 mm, height 110 mm, form factor ratio 0.418), a 48750 cell (diameter 48 mm, height 75 mm, form factor ratio 0.640), a 48110 cell (diameter 48 mm, height 110 mm, form factor ratio 0.418), a 48800 cell (diameter 48 mm, height 80 mm, form factor ratio 0.600), or a 46800 cell (diameter 46 mm, height 80 mm, form factor ratio 0.575). In the form factor numbers, the first two digits indicate the diameter of the cell, the next two digits indicate the height of the cell, and the final digit 0 indicates that the cell has a circular cross section.

[0147] The cylindrical battery cell according to the present invention uses a single particle or pseudo-single particle type positive electrode active material to significantly reduce the amount of gas generation compared to conventional battery cells. As a result, excellent safety can be achieved even in large cylindrical battery cells with a form factor ratio of 0.4 or more.

[0148] Meanwhile, the cylindrical battery cell according to the present invention may preferably be a battery having a tab-less structure that does not include electrode tabs, but is not limited thereto.

[0149] The tabless-structured battery may have a structure in which, for example, each of the positive and negative electrode plates includes an uncoated portion where an active material layer is not formed, the uncoated portion of the positive electrode plate and the uncoated portion of the negative electrode plate are located at the upper and lower ends of the electrode assembly, respectively, current collecting plates are coupled to the uncoated portion of the positive electrode plate and the uncoated portion of the negative electrode plate, and the current collecting plates are connected to electrode terminals.

[0150] The electrode assembly according to an embodiment of the present invention is a jelly-roll type electrode assembly having a structure in which sheet-like first and second electrode plates and a separator interposed therebetween are wound in one direction.

[0151] Preferably, at least one of the first and second electrode plates includes a non-coated portion on a long side edge in the winding direction where the active material is not coated. At least a portion of the non-coated portion is used as an electrode tab. The non-coated portion includes a core-side non-coated portion adjacent to the core of the electrode assembly, an outer-periphery-side non-coated portion adjacent to the outer peripheral surface of the electrode assembly, and an intermediate non-coated portion interposed between the core-side non-coated portion and the outer-periphery-side non-coated portion.

[0152] Preferably, at least one of the core-side non-coated portion and the outer-periphery-side non-coated portion has a height relatively lower than that of the intermediate non-coated portion.

[0153] For ease of explanation, in this specification, the direction along the longitudinal direction of the winding shaft of the electrode assembly wound into a jelly roll is referred to as the axial direction Y. The direction surrounding the winding shaft is referred to as the circumferential direction X. The direction approaching or moving away from the winding shaft is referred to as the radial direction Z. Of these, the direction particularly approaching the winding shaft is referred to as the centripetal direction, and the direction moving away from the winding shaft is referred to as the centrifugal direction.

[0154] First, an electrode assembly according to an embodiment of the present invention will be described.

[0155] The electrode assembly includes a first electrode plate, a second electrode plate, and a separator interposed therebetween, the first electrode plate, the second electrode plate, and the separator being wound in one direction around an axis to form a plurality of winding turns, and the first electrode plate and the second electrode plate each independently include a first side and a second side, the first side and the second side being disposed on opposite sides of each other in the axial direction.

[0156] In one embodiment of the present invention, the first and second electrode plates may be rectangular sheets having an aspect ratio exceeding 1. In this case, the ends of the width of each electrode plate define first and second sides.

[0157] FIG. 7 is a plan view showing the structure of the electrode plate 40 according to the first embodiment of the present invention.

[0158] Referring to Figure 7, the second side portion is a side formed along the lowermost end of the electrode active material portion 42 in the winding axis direction Y, and the first side portion is a side formed along the uppermost end of the non-coated portion 43 in the winding axis direction Y.

[0159] The first and second electrode plates each independently include a first portion, which is an electrode active material portion coated with an electrode active material on at least one surface or both surfaces. The first portion extends a predetermined length from the second side toward the first side. FIG. 4 shows the shape of the electrode plates before being wound into an electrode assembly. Referring to this, the electrode active material portion may have a constant width along the entire length of the electrode plate from the second side toward the beginning of the non-coated portion in the axial direction.

[0160] The second portion is a non-coated portion that is not coated with an electrode active material. The second portion forms an electrode tab and extends from the first side portion toward the second side portion to the electrode active material portion of the first portion.

[0161] In one embodiment of the present invention, at least a portion of the non-application section is divided into a plurality of segments by incision grooves of a predetermined height (not shown).

[0162] The segment has a first end corresponding to the first side. In one embodiment of the present invention, all or at least a portion of the segment is folded radially about an axis at a folding point, which is a point within the segment below the first end, and in this case, one end of the separator may be located between the folding point and the boundary line between the first and second portions. In a more specific embodiment of the present invention, the one end of the separator may be located between the folding point and a reference line or below the reference line.

[0163] In one specific embodiment, the bending point may be a predetermined point between the first end and a reference line.

[0164] In the current collector according to the present invention, the non-coated portion includes a plurality of segments, and the separator may be disposed so that the notched valleys of the cut grooves between the segments are covered and not exposed. The arrangement of the separator will be described in detail below.

[0165] In the present invention, the segment pieces may each have a different height at the first end, the shape of each incision groove may be different, and the height of the notched valley of the incision groove may also be different. That is, the shape and size of the segment pieces and the shape and size of the incision groove may be different from each other.

[0166] Meanwhile, the height of the segment piece may be defined as the axial distance C2, D2 from the notch valley of the incision groove defining the segment piece to the first end of the segment piece. When the heights of the notch valleys of the incision grooves on both sides of the segment piece are different, the height of the segment piece may be defined as the axial distance from the position where the average height of the notch valleys of the incision grooves on both sides is reached to the first end of the segment piece.

[0167] On the other hand, in the present invention, the reference line refers to an imaginary straight line extending in the winding direction X at a height corresponding to the notching valley of the cut groove.

[0168] The first and second electrode plates may each independently include a current collector that is a conductive thin film and an electrode active material layer disposed on one or both surfaces of the current collector, the active material layer forming a first portion of the electrode plate.

[0169] The sheet-like first and second electrode plates may have an aspect ratio exceeding 1. In this case, the non-coated portion may be formed on a long side edge of at least one of the first and second electrode plates in the winding direction, and at least a portion of the non-coated portion may be used as an electrode tab.

[0170] In one embodiment of the present invention, the non-coated portion includes a core-side non-coated portion adjacent to the core of the electrode assembly, an outer-periphery-side non-coated portion adjacent to the outer peripheral surface of the electrode assembly, and an intermediate non-coated portion interposed between the core-side non-coated portion and the outer-periphery-side non-coated portion.

[0171] Preferably, at least one of the core-side non-coated portion and the outer-periphery-side non-coated portion may be relatively lower in height than the intermediate non-coated portion.

[0172] Meanwhile, for convenience of explanation, the term "height" herein may refer to the distance (length) from a predetermined position in the winding direction x to the first side portion in the axial direction. In describing the height of the non-coated portion / notching valley (height) herein, the relative value of the height measured at different positions in the winding direction is more meaningful than the absolute value of the height. Therefore, when measuring the height of the non-coated portion / notching valley, the reference line (zero point) for the height measurement may be omitted. In one embodiment of the present invention, the height of the non-coated portion may be a relative distance at a specific point based on an arbitrary perpendicular line to the winding axial direction. For example, the reference line (zero point) for the height measurement may be the second side portion.

[0173] On the other hand, more specifically, the height of the non-application portion means the distance to the first side in the section where no segment pieces are formed, and in the section where segment pieces are formed, the first side means the position corresponding to the first end of the segment pieces, and the portion that forms the incision groove between the segment pieces is not taken into consideration when measuring the height of the non-application portion in the section where segment pieces are formed.

[0174] The height of the notching valley is measured based on the lowest part of the cutting groove.

[0175] Referring to FIG. 7, the electrode plate 40 of the first embodiment includes a current collector 41 made of metal foil and an active material layer 42. The metal foil may be aluminum or copper, and is appropriately selected depending on the polarity of the electrode plate 40. The active material layer 42 is formed on at least one surface of the current collector 41 and includes an uncoated portion 43 at the end of the long side in the winding direction X. The uncoated portion 43 is an area that is not coated with active material. An insulating coating layer 44 may be formed at the boundary between the active material layer 42 and the uncoated portion 43. The insulating coating layer 44 is formed so that at least a portion of the insulating coating layer 44 overlaps the boundary between the active material layer 42 and the uncoated portion 43. The insulating coating layer 44 includes a polymer resin and may include an inorganic filler such as Al2O3.

[0176] The non-coated portion 43 includes a core-side non-coated portion B1 adjacent to the core side of the electrode assembly, an outer-periphery-side non-coated portion B3 adjacent to the outer-periphery side of the electrode assembly, and an intermediate non-coated portion B2 interposed between the core-side non-coated portion B1 and the outer-periphery-side non-coated portion B3.

[0177] The core-side non-coated region B1, the outer-periphery non-coated region B3, and the middle non-coated region B2 may be defined as the uncoated region adjacent to the core side, the uncoated region adjacent to the outer periphery, and the remaining region excluding these when the electrode plate 40 is wound into a jelly-roll-type electrode assembly, respectively. The boundary between B1 and B2 may be appropriately defined as a point where the height (or change pattern) of the uncoated region substantially changes as one progresses from the core side to the outer periphery of the electrode assembly, or as a predetermined percentage point based on the radius of the electrode assembly (e.g., 5%, 10%, 15% of the radius, etc.). The boundary between B2 and B3 may be defined as a point where the height (or change pattern) of the uncoated region substantially changes as one progresses from the outer periphery to the core side of the electrode assembly, or as a predetermined percentage point based on the radius of the electrode assembly (e.g., 85%, 90%, 95% of the radius, etc.). Once the boundaries between B1 and B2 and between B2 and B3 are identified, the middle non-coated region B2 can be naturally identified. If only the boundary between B1 and B2 is specified, the boundary between B2 and B3 can be appropriately selected as a point near the outer periphery of the electrode assembly. On the other hand, if only the boundary between B2 and B3 is specified, the B1 / B2 boundary can be appropriately selected as a point near the core side of the electrode assembly. In the first embodiment, the height of the non-coated portion 43 is not constant, but there is a relative difference in the winding direction X. That is, the height (length in the Y-axis direction) of the outer periphery non-coated portion B3 is relatively smaller than the core side non-coated portion B1 and the middle non-coated portion B2.

[0178] FIG. 8 is a plan view showing the structure of an electrode plate 45 according to a second embodiment of the present invention.

[0179] Referring to FIG. 8, the electrode plate 45 of the second embodiment differs from the first embodiment only in that the height of the outer non-coating portion B3 gradually decreases as it moves toward the outer periphery, and the remaining configuration is substantially the same.

[0180] In one modification, the outer peripheral non-coating portion B3 can be deformed into a stepped shape (see dotted lines) in which the height decreases stepwise.

[0181] FIG. 9 is a plan view showing the structure of an electrode plate 50 according to a third embodiment of the present invention.

[0182] 9, in the electrode plate 50 of the third embodiment, the heights of the core-side non-coated portion B1 and the outer-periphery-side non-coated portion B3 are relatively smaller than the middle non-coated portion B2, and the heights of the core-side non-coated portion B1 and the outer-periphery-side non-coated portion B3 may be the same or different.

[0183] Preferably, the height of the intermediate non-coated portion B2 may be stepped, increasing stepwise from the core side toward the outer periphery.

[0184] The first to seventh patterns are obtained by dividing the intermediate non-coating portion B2 around the positions where the height of the non-coating portion 43 changes. Preferably, the number of patterns and the height (length in the Y-axis direction) and width (length in the X-axis direction) of each pattern can be adjusted to maximize stress dispersion during the bending process of the non-coating portion 43. The purpose of stress dispersion is to prevent the non-coating portion 43 from breaking.

[0185] Width d of non-coated area B1 on the core side B1 is designed under the condition that when the pattern of the middle non-coated portion B2 is bent toward the core side, the cavity of the electrode assembly core is not blocked.

[0186] As an example, the width d of the core-side non-coating portion B1 B1 can increase in proportion to the bending length of pattern 1. The bending length is the height of the pattern relative to the bending point of the pattern.

[0187] In a specific example, when the electrode plate 60 is used to manufacture an electrode assembly for a cylindrical cell having a form factor of 46800, the width d of the core-side non-coated portion B1 is B1 can be set to 180 to 350 mm depending on the diameter of the electrode assembly core.

[0188] In one embodiment, the width of each pattern can be designed to accommodate the same winding turn of the electrode assembly.

[0189] In one variation, the height of the intermediate non-coated portion B2 may be stepped, increasing and then decreasing as it moves from the core side to the outer periphery side.

[0190] In another modification, the outer peripheral non-coated portion B3 can be modified to have the same structure as in the second embodiment.

[0191] In another variant, the pattern structure applied to the middle non-coated portion B2 can be extended to the outer circumferential non-coated portion B3 (see dotted lines).

[0192] FIG. 10a is a plan view showing the structure of an electrode plate 60 according to a fourth embodiment of the present invention.

[0193] 10a, in the fourth embodiment of the electrode plate 60, the heights of the core-side non-coated portion B1 and the outer-side non-coated portion B3 are smaller than the height of the middle non-coated portion B2. The heights of the core-side non-coated portion B1 and the outer-side non-coated portion B3 may be the same or different.

[0194] Preferably, at least a portion of the middle non-coated portion B2 may include a plurality of segment pieces 61. The height of the plurality of segment pieces 61 may increase stepwise from the core side toward the outer periphery side.

[0195] In the present invention, the segment pieces are bent in whole or at least in part in the radial direction (toward the winding center) of the electrode assembly or in the direction opposite to the radial direction. The bending of the segment pieces may be performed at a position spaced a predetermined height above the notching valley (bottom of the cut groove). In the present invention, the bending point is defined as the point where the inclination of a tangent to a portion of the segment piece that is actually bent toward the center by an external force begins to become 45° or less. The inclination of a tangent refers to the angle between a tangent to the bending point and a plane perpendicular to the winding axis of the electrode assembly. Meanwhile, the bending curve is defined as a line that includes the bending point and is horizontal to the reference line.

[0196] Meanwhile, in the present invention, the heights of the plurality of incision grooves corresponding to the notching valleys may be the same or different from each other.

[0197] When the heights are the same, an imaginary straight line extending the height of the notching valley in the winding direction X is used as the reference line.

[0198] If most of the notch valleys of the incision grooves are located at a specific height and only the heights of some of the notch valleys of the incision grooves are different from the specific height, the reference line may be determined to be a height corresponding to the specific height. For example, if 50% or more of the notch valleys are located at a specific height, the reference line may be determined to be a height corresponding to the heights of these notch valleys. Alternatively, the reference line may be determined based on the height of the notch valley of the incision groove that occupies the longest length in the winding direction. For example, if about two-thirds of the total length occupied by the notch valleys of the incision grooves in the winding direction has a first height, and the height of the notch valley of the incision groove that occupies the remaining one-third of the total length occupied by the notch valleys of the incision grooves in the winding direction is different from the first height, the reference line may be defined as a position corresponding to the first height.

[0199] In addition, if the heights of the notch valleys of the incision grooves are not concentrated at a specific height (if the most frequently occurring in less than 50% of the incision grooves), the reference line may be determined as the average height of the notch valleys of the incision grooves. For example, if the length of the incision grooves with a notch valley height x in the winding direction is 30%, the length of the incision grooves with a notch valley height y in the winding direction is 30%, and the length of the incision grooves with a notch valley height z in the winding direction is 40%, the reference line may be x × 0.3 + y × 0.3 + z × 0.4. The height of the notch valley may be a relative distance at a specific point based on an arbitrary perpendicular line to the winding axis direction. For example, the height of the incision groove may be based on the distance from the second side portion to the incision groove.

[0200] Meanwhile, in one embodiment of the present invention, the bending point may be located approximately 2 mm to 3 mm above the notching valley and may be arranged parallel to the reference line.

[0201] Meanwhile, in one embodiment of the present invention, the reference line may be the same as or different from a line obtained by extending a point having a minimum height in the non-coated portion in the winding direction Y. In a specific embodiment, the reference line may be the same as a line obtained by extending a point having a minimum height in the non-coated portion in the winding direction Y.

[0202] The segments 61 may be laser notched. The segments 61 may be formed by known metal foil cutting processes such as ultrasonic cutting or punching.

[0203] In the fourth embodiment, a predetermined gap is preferably provided between the lower end of the cutting line between the segments 61 and the active material layer 42 to prevent damage to the active material layer 42 and / or the insulating coating layer 44 during bending of the non-coated portion 43. This is because stress concentrates near the lower end of the cutting line when the non-coated portion 43 is bent. The gap is preferably 0.2 to 4 mm. Adjusting the gap within this range prevents damage to the active material layer 42 and / or the insulating coating layer 44 near the lower end of the cutting line due to stress generated during bending of the non-coated portion 43. In addition, the gap prevents damage to the active material layer 42 and / or the insulating coating layer 44 due to tolerances during notching or cutting of the segments 61. Preferably, when the electrode plate 40 is wound into an electrode assembly, at least a portion of the insulating coating layer 44 may be exposed to the outside of the separator. In this case, the insulating coating layer 44 may support the notch valley when the segments 61 are bent.

[0204] The gap between the notched valley of the segment piece and the active material layer may be desirably 1.0 mm or more, which may be even more effective when the electrode is a negative electrode.

[0205] The gap between the notched valley of the segment piece and the active material layer may be more preferably 2.0 mm or more, which may be even more effective when the electrode is a positive electrode.

[0206] A gap smaller than the above range will not fully exhibit the above-mentioned damage prevention effect, and a gap larger than the above range may result in only a decrease in the electrode capacitance without increasing the damage prevention effect.

[0207] The boundary between the non-coated region where the active material layer is not coated and the region where the active material layer is coated may be covered with an insulating layer, and in this case, a predetermined gap may also be provided between the notched valley of the segment and the insulating layer.

[0208] Such a gap may be between 0.2 mm and 1.5 mm.

[0209] A gap smaller than the above range will not fully exhibit the above-mentioned damage prevention effect, and a gap larger than the above range will not increase the damage prevention effect and may result in a reduced bending support effect for the segment pieces of the insulating coating layer.

[0210] The plurality of segment pieces 61 may be arranged into a plurality of segment piece groups from the core side to the outer periphery side. The width, height and spacing pitch of the segment pieces belonging to the same segment piece group may be substantially the same.

[0211] 10a and 12a, a separator SP may be provided in contact with the active material layer 42 and / or the insulating coating layer 44 of the electrode plate 60 of the fourth embodiment to form an electrode assembly.

[0212] 10b, 10c, 11, 12b and 12c, the position where the end of the separator is located on the non-coated portion of the electrode plate in the electrode assembly according to an embodiment of the present invention will be described.

[0213] The position where the end of the separator is located on the non-coated portion of the electrode plate in the electrode assembly of the present invention will be described in more detail with reference to FIGS. 7b, 7c, 8, 9b and 9c.

[0214] In one embodiment of the present invention, the non-application portion may include a plurality of segments, and the depths of the notch valleys between the segments may be the same. In this case, a line extending from a point corresponding to the depth of the notch valley is defined as a reference line.

[0215] In this case, the reference line may correspond to a line connecting the smallest height of the core-side non-coated portion, the outer periphery-side non-coated portion, and the middle non-coated portion to both ends of the non-coated portion.

[0216] In the present invention, the widthwise end SL of the separator is located between the bending point and the reference line DL or is located from the reference line toward the inside of the electrode assembly. Here, the outside of the electrode assembly refers to the direction from the active material layer of the electrode plate toward the non-coated portion, i.e., toward the first side, and the inside refers to the opposite direction to the outside, i.e., toward the second side.

[0217] In one embodiment of the present invention, the electrode assembly may have a surface region formed at the upper or lower end in the winding axis direction by adjacent winding turn segments continuously overlapping in the radial direction or in opposite directions among the folded segments. In this case, when the shortest distance between the maximum height (highest point) in the winding axis direction of the surface region and the reference line is defined as the height HS of the surface region, the widthwise end of the separator may be positioned toward the outside of the electrode assembly or toward the inside of the electrode assembly within 90% of the height HS of the surface region relative to the reference line.

[0218] According to one embodiment of the present invention, by controlling the widthwise edge of the separator to be positioned close to the reference line, the electrolyte flows into the electrode assembly along the notch valley (empty space), which is advantageous for impregnation. Specifically, when the electrolyte is introduced into the electrode assembly, it moves into the cut grooves between the segments, and then further impregnates the notch valley, i.e., the end of the separator located close to the reference line, and ultimately impregnates into the active material layer of the electrode. As a result, the electrolyte impregnation uniformity within the electrode assembly is improved.

[0219] The more the widthwise end of the separator moves toward the outside of the jelly roll, i.e., toward the outside of the electrode assembly, the more negatively it affects the welding characteristics. On the other hand, the more the widthwise end of the separator moves toward the inside of the jelly roll, i.e., toward the inside of the electrode assembly, the greater the risk of short-circuiting between the positive and negative electrodes, which can be problematic.

[0220] Therefore, the widthwise end of the separator of the present invention is controlled to be positioned toward the outside of the electrode assembly relative to the reference line, or toward the inside of the electrode assembly relative to the reference line, and more preferably, to be positioned at 90% or less of the height HS of the surface area.

[0221] Meanwhile, in one embodiment of the present invention, if the segment having the smallest height among the folded segments among the plurality of segments is defined as the smallest folded segment, the widthwise end of the separator may be positioned toward the outside (first side) of the electrode assembly within less than 50%, within 40%, within 30%, within 20%, or within 10% of the height Ha of the smallest folded segment from the reference line. Preferably, it may be positioned toward the outside of the electrode assembly within 30%. In this case, the separator may be positioned so that the notched valley of the incision groove between the segments is covered by the separator and not exposed.

[0222] If the separator is positioned closer to the first end of the segment than this range, the separator may be damaged by heat when the segment is later welded. According to yet another embodiment, the widthwise end of the separator may be positioned toward the inside (second side) of the electrode assembly within 30%, 20%, or 10% of the height Ha of the smallest bent segment from the reference line. If the separator is positioned below the reference line in this manner, all or at least a portion of the notching valley may be exposed and not covered by the separator.

[0223] 7b, 7c, 9b, or 9c, the first group of segments may be the smallest bent segments, and one widthwise end of the separator may be located toward the outside (first side) of the electrode assembly within 30% or less of the height Ha of the smallest bent segment from the reference line, or the widthwise end of the separator may be located toward the inside (second side) of the electrode assembly within 30% of the height Ha of the smallest bent segment from the reference line. More specifically, the first group of segments may be the smallest bent segments, and one widthwise end of the separator may be located toward the outside (first side) of the electrode assembly within 30% of the height Ha of the smallest bent segment from the reference line. Referring to FIG. 7b or 9b, when one side end of the separator is positioned above the reference line, one side end of the separator is located between Hb. Here, the maximum length of Hb is less than 50% of the height (length) of the smallest folded segment. On the other hand, when one end of the separation membrane is located below the DL, the maximum length of Hb is 30% of the height of the smallest folded segment.

[0224] That is, in the present invention, the segment serving as a reference for arranging the separation membrane may refer to the segment having the smallest height among the folded segments, which is referred to as the minimum folded segment.

[0225] In a specific embodiment of the present invention, the minimum bent segment may be 2 mm or more, and in this case, the height of the minimum bent segment is higher than the height of the bent point. If the height of the segment is less than 2 mm, the segment may not be folded smoothly due to interference between the separator and the segment. For this reason, the minimum bent segment may be determined from among the segment segments having a height of 2 mm or more.

[0226] According to one embodiment of the present invention, in the minimum bent segment piece, the height A from the reference line to the bend line based on the bend line may be equal to or longer than the length from the bend line to the height B of the segment piece. Alternatively, in the minimum bent segment piece, the height A from the reference line to the bend line based on the bend line may be equal to or shorter than the length from the bend line to the height B of the segment piece.

[0227] In one embodiment of the present invention, the electrode assembly may further include a segment (segment A) having a height smaller than that of the minimum bent segment. In this case, segment A is not bent. In a specific embodiment, segment A may be disposed closer to the core than the other segments among the plurality of segments.

[0228] In an embodiment of the present invention, the electrode assembly may not include a segment having a height smaller than that of the smallest bent segment, and the smallest bent segment may be the smallest segment.

[0229] According to one embodiment of the present invention, the widthwise end of the separator may be located outside the electrode assembly within 1.5 mm from the reference line, or the widthwise end of the separator may be located inside the electrode assembly within 1.5 mm from the reference line.

[0230] FIG. 11 is a diagram illustrating the definition of the width, height, and spacing pitch of the segment pieces 61 according to an embodiment of the present invention.

[0231] 11, the width C1, height C2, and spacing pitch C3 of the segment pieces 61 are designed to prevent tearing of the non-coated portion 43 during bending and to increase the number of overlapping layers of the non-coated portion 43 to improve weld strength, while also preventing abnormal deformation of the non-coated portion 43. Abnormal deformation refers to the non-coated portion below the bending point C4 being unable to maintain a straight state and being crushed and deformed irregularly.

[0232] According to one embodiment of the present invention, the width C1 of the segment 61 may be adjusted within a range of 1 to 6 mm. If C1 is less than 1 mm, when the segment 61 is bent toward the core, a non-overlapping region or space (gap) that is insufficient to ensure sufficient welding strength is generated. On the other hand, if C1 exceeds 6 mm, the non-coated portion 43 near the bending point C4 may be torn due to stress when the segment 61 is bent. Furthermore, the height of the segment 61 may be adjusted within a range of 2 to 10 mm. If C2 is less than 2 mm, when the segment 61 is bent toward the core, a non-overlapping region or space (gap) that is insufficient to ensure sufficient welding strength is generated. On the other hand, if C2 exceeds 10 mm, it is difficult to manufacture an electrode plate while maintaining uniform flatness of the non-coated portion in the winding direction X. In other words, the height of the non-coated portion increases, resulting in waviness.

[0233] Furthermore, the spacing pitch C3 of the segment pieces 61 can be adjusted within a range of 0.05 to 1 mm. If C3 is less than 0.05 mm, the non-coated portion 43 near the bending point C4 may break due to stress when the segment pieces 61 are bent. On the other hand, if C3 exceeds 1 mm, regions or spaces (gaps) may be generated where the segment pieces 61 do not overlap each other to an extent that sufficient welding strength can be ensured when the segment pieces 61 are bent.

[0234] In one embodiment of the present invention, the corners of the two segments may be connected in a straight line, i.e., the bottom of the incision groove may be formed as a flat, straight line extending in the winding direction X. A rounded reinforcement may be added to the corner.

[0235] The radius r of the round reinforcement portion may be 0.02 mm or more. If the radius is greater than this, the stress dispersion effect can be reliably achieved. The radius of the round reinforcement portion may be 0.1 mm or less. If the radius is greater than 0.1 mm, the stress dispersion effect will not be further increased, and the space near the bottom of the cut groove will be reduced, which may hinder the impregnation of the electrolyte.

[0236] Referring further to FIG. 10a, the width d of the core-side non-coated portion B1 B1is designed under the condition that when the segment piece 61 of the middle non-coating portion B2 is bent toward the core, the cavity of the core of the electrode assembly is not blocked.

[0237] For example, the width d of the core-side non-coated portion B1 B1 can increase in proportion to the folded length of the segment pieces 61 of group 1.

[0238] In a specific example, when the electrode plate 60 is used to manufacture an electrode assembly for a cylindrical cell having a form factor of 46800, the width d of the core-side uncoated portion B1 is B1 can be set to 180 to 350 mm depending on the diameter of the electrode assembly core.

[0239] In one embodiment, the width of each segment group can be designed to accommodate the same winding turn of the electrode assembly.

[0240] In one variant, the width and / or height and / or spacing pitch of the segment pieces 61 belonging to the same segment piece group may increase or decrease gradually and / or stepwise and / or irregularly within the group.

[0241] The first to seventh groups are merely examples of segment groups. The number of groups and the number of segment pieces 61 included in each group can be adjusted so that the segment pieces 61 are overlapped in multiple layers to maximize stress distribution during the bending process of the non-coated portion 43 and ensure sufficient welding strength.

[0242] In another variation, the height of the outer peripheral non-coating portion B3 may decrease gradually or stepwise, as in the first and second embodiments. Furthermore, the segmented structure of the intermediate non-coating portion B2 may extend to the outer peripheral non-coating portion B3 (see dotted lines). In this case, the outer peripheral non-coating portion B3 may also include multiple segmented pieces, similar to the intermediate non-coating portion B2. In this case, the segmented pieces of the outer peripheral non-coating portion B3 may have a width and / or height and / or spacing pitch greater than those of the intermediate non-coating portion B2.

[0243] In a specific example, when the electrode plate 60 is used to manufacture an electrode assembly for a cylindrical cell having a form factor of 46800, the segment pieces may be formed in eight groups. Here, the segment pieces of the first to seventh groups may be formed in the middle non-coated portion B2, and the segment piece of the eighth group may be formed in the outer peripheral non-coated portion B3 as in the above-described modification.

[0244] In a specific example, the width d of the core-side non-coating portion B1 B1 The width of the first group may be 35 to 40% of the width of the core-side non-application portion B1. The width of the second group may be 130 to 150% of the width of the first group. The width of the third group may be 120 to 135% of the width of the second group. The width of the fourth group may be 85 to 90% of the width of the third group. The width of the fifth group may be 120 to 130% of the width of the fourth group. The width of the sixth group may be 100 to 120% of the width of the fifth group. The width of the seventh group may be 90 to 120% of the width of the sixth group. The width of the eighth group may be 115 to 130% of the width of the seventh group.

[0245] The reason why the widths of the first to eighth groups do not show a constant increase or decrease pattern is that although the width of the segments gradually increases from the first to eighth groups, the number of segments included in a group is limited to an integer. Therefore, the number of segments may decrease in a particular segment group. Therefore, the width of the group may show an irregular change as it moves from the core side to the outer periphery, as shown in the example above.

[0246] That is, when the widths in the winding direction of each of three segment groups adjacent to each other in the radial direction of the electrode assembly are W1, W2, and W3, the electrode assembly may include a combination of segment groups in which W3 / W2 is smaller than W2 / W1.

[0247] In the specific example, this applies to groups 4 to 6. The ratio of the width of group 5 to group 4 is 120 to 130%, and the ratio of the width of group 6 to group 5 is 100 to 120%, which is smaller than 120 to 130%.

[0248] FIG. 12a is a plan view showing the structure of an electrode plate 70 according to a fifth embodiment of the present invention.

[0249] Referring to FIG. 12a, the electrode plate 70 of the fifth embodiment is substantially identical in configuration to the fourth embodiment (or modified example), except that the shape of the segment 61' has been changed from a square to a trapezoid compared to the fourth embodiment.

[0250] FIG. 13 shows the definition of the width, height and spacing pitch of the trapezoidal segment pieces 61'.

[0251] Referring to FIG. 13, the width D1, height D2, and spacing pitch D3 of the segment piece 61' are designed to prevent the non-coated portion 43 from tearing near the bending point D4 when the non-coated portion 43 is bent, and to prevent abnormal deformation of the non-coated portion 43 while sufficiently increasing the number of overlapping layers of the non-coated portion 43 to ensure sufficient welding strength.

[0252] Preferably, the width D1 of the segment 61' can be adjusted within a range of 1 to 6 mm. If D1 is less than 1 mm, when the segment 61' is bent toward the core, a region or space (gap) where the segment 61' does not overlap to a degree sufficient to ensure welding strength may be generated. On the other hand, if D1 exceeds 6 mm, the non-coated portion 43 near the bending point D4 may be torn due to stress when the segment 61' is bent. In addition, the height of the segment 61' can be adjusted within a range of 2 to 10 mm. If D2 is less than 2 mm, when the segment 61' is bent toward the core, a region or space (gap) where the segment 61' does not overlap to a degree sufficient to ensure welding strength may be generated. On the other hand, if D2 exceeds 10 mm, it is difficult to manufacture an electrode plate while maintaining uniform flatness of the non-coated portion 43 in the winding direction. Furthermore, the spacing pitch D3 between the segments 61' can be adjusted within a range of 0.05 to 1 mm. If D3 is less than 0.05 mm, the non-coated portion 43 near the bending point D4 may break due to stress when the segments 61' are bent. On the other hand, if D3 exceeds 1 mm, when the segments 61' are bent, regions or spaces (gaps) may be generated where the segments 61' do not overlap each other to an extent that sufficient welding strength can be ensured.

[0253] When the segments are trapezoidal, the separation pitch D3 can be defined as the distance between the corners of two adjacent segments 61'. The corners of the two adjacent segments can be connected in a straight line. That is, the bottom of the cut groove can have a flat, straight line shape extending in the winding direction X.

[0254] The corners may further be provided with rounded reinforcement portions, thereby eliminating stress concentration that may occur at the corners.

[0255] The radius r of the round reinforcing portion may be 0.02 mm or more, which can reliably achieve the effect of stress dispersion.

[0256] The radius of the round reinforcing portion may be 0.1 mm or less. If the radius exceeds 0.1 mm, the effect of stress dispersion will not be further increased, and the space near the bottom of the cut groove may be reduced, which may hinder the impregnation of the electrolyte.

[0257] The separation pitches C3 and D3 may be determined in relation to the widths C1 and D1 of the adjacent segments 61 and 61' that define the separation pitches C3 and D3, measured in the winding direction. For example, it is desirable that the separation pitch between the segments increases as the width of the segments increases in the winding direction. This allows for uniform distribution of the electrolyte impregnation along the winding direction of the electrode assembly.

[0258] The width of the segments in the winding direction may be set to gradually increase from the core side to the outer periphery of the electrode assembly. The width of the segments in the winding direction may increase gradually or stepwise from the core side to the outer periphery of the electrode assembly. For example, the widths C1 and D1 of the segments in the winding direction may be within a range of 1 to 6 mm, decreasing toward the core side and increasing toward the outer periphery.

[0259] Accordingly, the spacing pitches C3 and D3 may also be within a range of 0.5 to 1 mm, and may increase gradually or stepwise from the core side to the outer periphery side of the electrode assembly.

[0260] In the fifth embodiment, the lower interior angle θ of the trapezoid of the plurality of segments 61′ may increase from the core side toward the outer periphery. As the radius of the electrode assembly 70 increases, the curvature increases. If the lower interior angle θ of the segments 61′ increases as the radius of the electrode assembly increases, stresses generated in the radial and circumferential directions when the segments 61′ are bent can be alleviated. Furthermore, as the lower interior angle θ increases, the overlapping area and number of overlapping layers with the inner segments 61′ also increase when the segments 61′ are bent, ensuring uniform welding strength in the radial and circumferential directions and forming flat bent surfaces.

[0261] In one example, when the electrode plate 70 is used to manufacture an electrode assembly for a cylindrical cell having a form factor of 46800, as the radius of the electrode assembly 70 increases from 4 mm to 22 mm, the interior angle of the segment piece 61' may increase stepwise in the range of 60° to 85°.

[0262] In one variant, the height of the outer peripheral non-coating portion B3 may decrease gradually or stepwise, as in the first and second embodiments. Furthermore, the segmented structure of the intermediate non-coating portion B2 may extend to the outer peripheral non-coating portion B3 (see dotted lines). In this case, the outer peripheral non-coating portion B3 may also include multiple segmented pieces, similar to the intermediate non-coating portion B2. In this case, the segmented pieces of the outer peripheral non-coating portion B3 may have a width and / or height and / or spacing pitch greater than those of the intermediate non-coating portion B2.

[0263] When the intermediate non-application portion B2 includes multiple segment pieces 60, 60' as in the fourth and fifth embodiments, the shape of each segment piece 60, 60' can be changed to a triangle, semicircle, semi-ellipse, parallelogram, etc.

[0264] The shapes of the segments 60, 60' may also be varied depending on the region of the middle non-application portion B2. For example, a round shape (e.g., semicircular, semi-elliptical, etc.) that is advantageous for stress dispersion may be applied to the section where stress is concentrated, and a polygonal shape (e.g., quadrilateral, trapezoid, parallelogram, etc.) with the largest area may be applied to the section where stress is relatively low.

[0265] In the fourth and fifth embodiments, the segmented structure of the middle non-coating portion B2 can also be applied to the core-side non-coating portion B1. However, if a segmented structure is applied to the core-side non-coating portion B1, when the segment pieces 60, 60' of the middle non-coating portion B2 are bent along the curvature radius of the core, a reverse forming phenomenon may occur, in which the end of the core-side non-coating portion B1 is warped toward the outer periphery. Therefore, it is preferable that the core-side non-coating portion B1 does not have a segmented structure, or if a segmented structure is applied, the width, height, and / or spacing of the segment pieces 60, 60' be adjusted to a level that prevents reverse forming, taking into account the curvature radius of the core.

[0266] The height of the segment pieces where this reverse molding can occur may be less than about 3 mm. Also, if the height of the segment pieces is less than 2 mm, interference occurs between the segment pieces and the separator film, making bending difficult. Also, if the height of the segment pieces is less than 4 mm, the welding process of the segment pieces may not be smooth. Therefore, taking bending into consideration, the minimum height H of the segment pieces is set. min may be 2 mm or more, or 3 mm or more, or 4 mm or more, or 5 mm or more, whereby the height of the smallest folded segment may be 2 mm or more, or 3 mm or more, or 4 mm or more, or 5 mm or more.

[0267] Therefore, the minimum height H that can be bent in the non-coated area is based on the reference line DL. min If the end SL in the width direction of the separation membrane is within a range of ±30% (based on the reference line) of the height Ha of the smallest bent segment among the segment pieces having a height of 2 mm, 3 mm, 4 mm, or 5 mm (as mentioned above), impregnation can be significantly improved. In other words, when determining the smallest segment piece that defines the position of the end SL in the width direction of the separation membrane, segment pieces that may cause reverse molding or segment pieces that are not bent may be excluded.

[0268] In other words, the minimum height Ha of the bendable segment in the non-application portion and the minimum height H that can be bent are determined based on the reference line DL. min The largest height max(Ha,H min When the end SL in the width direction of the separation membrane is within a range of ±30% of the above value, the impregnation property can be significantly improved.

[0269] In other words, the minimum height H at which the bend can be made is determined based on the reference line DL. min When the end SL in the width direction of the separator is within a range of ±30% of the reference line DL, the impregnation of the electrolyte can be significantly improved. This can be in the range of the reference line DL ±1.5 mm, the reference line DL ±1.2 mm, the reference line DL ±0.9 mm, or the reference line DL ±0.6 mm.

[0270] Alternatively, the end position of the separation membrane in the width direction may be in the range of DL ± 0.3 Ha and in the range of DL ± 1.5 mm, or the end position of the separation membrane in the width direction may be in the range of DL ± 0.3 Ha and in the range of DL ± 1.2 mm, or the end position of the separation membrane in the width direction may be in the range of DL ± 0.3 Ha and in the range of DL ± 0.9 mm, or the end position of the separation membrane in the width direction may be in the range of DL ± 0.3 Ha and in the range of DL ± 0.6 mm.

[0271] The electrode plate structure of the above-described embodiment (variant) may be applied to at least one of a first electrode plate and a second electrode plate having different polarities included in a jelly roll-type electrode assembly. Furthermore, when the electrode structure of the embodiment (variant) is applied to one of the first electrode plate and the second electrode plate, a conventional electrode plate structure may be applied to the other. Furthermore, the electrode plate structures applied to the first electrode plate and the second electrode plate may not be identical to each other, but may be different.

[0272] In one example, when the first electrode plate and the second negative electrode are a positive electrode plate and a negative electrode plate, respectively, any one of the embodiments (variant examples) may be applied to the first electrode plate, and a conventional electrode plate structure (see FIG. 1) may be applied to the second electrode plate.

[0273] In another example, when the first electrode plate and the second negative electrode plate are a positive electrode plate and a negative electrode plate, respectively, any one of the embodiments (variants) may be selectively applied to the first electrode plate, and any one of the embodiments (variants) may be selectively applied to the second electrode plate.

[0274] In the present invention, the positive electrode active material coated on the positive electrode plate and the negative electrode active material coated on the negative electrode plate may be any active material known in the art without any limitation.

[0275] The positive electrode active material is a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; 1+x Mn 2-xO4 (where x is 0 to 0.33), lithium manganese oxides (LiMnO2) such as LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, and Cu2V2O7; and the chemical formula LiNi 1-x M x O2 (where M=Co, Mn, Al, Cu, Fe, Mg, B, or Ga, and x=0.01 to 0.3); 2-x M x Examples of the lithium intercalation material include, but are not limited to, lithium manganese composite oxides represented by LiMnO2 (where M=Co, Ni, Fe, Cr, Zn, or Ta, and x=0.01 to 0.1) or Li2Mn3MO8 (where M=Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which part of the lithium in the chemical formula is replaced with an alkaline earth metal ion; disulfide compounds; Fe2(MoO4)3, or composite oxides formed by a combination thereof.

[0276] In the present invention, the positive electrode active material is in the form of a single particle consisting of one primary particle or a pseudo-single particle which is an aggregate of 10 or less primary particles.

[0277] Conventionally, positive electrode active materials for battery cells have typically been spherical secondary particles formed by agglomeration of tens to hundreds of primary particles. However, such positive electrode active materials in the form of secondary particles formed by agglomeration of many primary particles are prone to particle cracking, in which the primary particles separate during the rolling process used to manufacture the positive electrode, and to internal cracking during charge and discharge. Particle cracking or internal cracking of the positive electrode active material increases the contact area with the electrolyte, leading to increased gas generation due to side reactions with the electrolyte. Increased gas generation within a cylindrical battery cell increases the internal pressure of the battery, potentially leading to a battery explosion. In particular, increasing the volume of a cylindrical battery cell increases the amount of active material within the battery, significantly increasing the amount of gas generation, further increasing the risk of battery fire and / or explosion.

[0278] In contrast, positive electrode active materials in the form of single particles consisting of one primary particle or pseudo-single particles consisting of an aggregate of 10 or fewer primary particles have higher particle strength than existing positive electrode active materials in the form of secondary particles consisting of an aggregate of tens to hundreds of primary particles, and therefore hardly ever undergo particle cracking during rolling. Furthermore, in the case of positive electrode active materials in the form of single particles or pseudo-single particles, the number of primary particles constituting the particle is small, so there is little change due to volume expansion and contraction of the primary particles during charge and discharge, and therefore the occurrence of cracks within the particles is also significantly reduced.

[0279] Therefore, when a positive electrode active material made of monoparticles or quasi-monoparticles is used as in the present invention, the amount of gas generation due to particle cracking and internal cracking can be significantly reduced, thereby achieving excellent safety even in large cylindrical battery cells. In the present invention, only monoparticle or quasi-monoparticle positive electrode active materials are used as the positive electrode active material, and secondary particle positive electrode active materials are not used. This is because the inclusion of secondary particle positive electrode active materials reduces the gas generation suppression effect, thereby preventing sufficient safety when applied to large cylindrical battery cells.

[0280] On the other hand, the positive electrode active material in the form of a single particle or pseudo-single particle according to the present invention has an average particle diameter D 50 The average particle size D of the positive electrode active material may be 5 μm or less, preferably 1 μm to 5 μm, and more preferably 2 μm to 5 μm. 50 When the value of the resistance satisfies the above range, the increase in the resistance can be minimized.

[0281] A positive electrode active material in the form of a single particle or quasi-single particle has a problem that the lithium mobility is lower than that of a positive electrode active material in the form of a secondary particle because there are fewer interfaces between primary particles, which serve as paths for lithium ions to move within the particles, resulting in increased resistance. This increase in resistance becomes more pronounced as the particle size increases, and the increased resistance adversely affects capacity and output characteristics. Therefore, the average particle size D 50 The company applied small single particle or pseudo-single particle positive electrode active material with a particle size of 5 μm or less to minimize the distance that lithium ions travel inside the particle, thereby suppressing the increase in resistance.

[0282] The positive electrode active material may have a primary particle size of 0.5 μm to 5 μm, preferably 1 μm to 5 μm, and more preferably 2 μm to 5 μm. When the average particle size of the primary particles is within this range, a single-particle or quasi-single-particle positive electrode active material with excellent electrochemical properties can be formed. If the average particle size of the primary particles is too small, the number of agglomerates of the primary particles forming the positive electrode active material increases, reducing the effect of suppressing particle cracking during rolling. If the average particle size of the primary particles is too large, the lithium diffusion path within the primary particles becomes longer, increasing resistance and potentially deteriorating output characteristics.

[0283] In the present invention, the positive electrode active material preferably has a unimodal particle size distribution. Conventionally, bimodal positive electrode active materials, which combine a large-particle positive electrode active material with a small-particle positive electrode active material, have been used to improve the electrode density of the positive electrode active material layer. However, as described above, in the case of a single-particle or quasi-single-particle positive electrode active material, increasing particle size significantly increases the lithium migration path and resistance. Therefore, when large-particle particles are mixed, the capacity and output characteristics may be reduced. Therefore, it is preferable to use a positive electrode active material with a unimodal particle size distribution.

[0284] Meanwhile, the positive electrode active material may include a lithium nickel-based oxide, specifically, a lithium nickel-based oxide represented by the following Chemical Formula 1:

[0285] [Chemical formula 1] Li a Ni b Co c M 1 d M 2 e O2 In the above Chemical Formula 1, M 1 is Mn, Al or a combination thereof, and may desirably be Mn or Mn and Al.

[0286] Said M 2 is at least one selected from the group consisting of Zr, W, Y, Ba, Ca, Ti, Mg, Ta and Nb, preferably at least one selected from the group consisting of Zr, Y, Mg and Ti, more preferably Zr, Y or a combination thereof. 2 Although the elements are not essential, when contained in an appropriate amount, they can play a role in promoting grain growth during firing or in stably forming a crystal structure.

[0287] The a represents the molar ratio of lithium in the lithium nickel-based oxide, and can be 0.8 ≦ a ≦ 1.2, 0.85 ≦ a ≦ 1.15, or 0.9 ≦ a ≦ 1.2. When the molar ratio of lithium satisfies the above range, the crystal structure of the lithium nickel-based oxide can be stably formed.

[0288] The b represents the molar ratio of nickel in the total metal excluding lithium in the lithium nickel-based oxide, and can be 0.8 ≦ b < 1, 0.82 ≦ b < 1, or 0.83 ≦ b < 1. When the molar ratio of nickel satisfies the above range, it shows a high energy density and enables the realization of a high capacity.

[0289] The c represents the molar ratio of cobalt in the total metal excluding lithium in the lithium nickel-based oxide, and can be 0 < c < 0.2, 0 < c < 0.18, or 0.01 ≦ c ≦ 0.17. When the molar ratio of cobalt satisfies the above range, good resistance characteristics and output characteristics can be realized.

[0290] The d represents the molar ratio of the M 1 element in the total metal excluding lithium in the lithium nickel-based oxide, and can be 0 < d < 0.2, 0 < d < 0.18, or 0.01 ≦ d ≦ 0.17. When the molar ratio of the M 1 element satisfies the above range, the structural stability of the positive electrode active material is excellently shown.

[0291] The e represents the molar ratio of the M 2 element in the total metal excluding lithium in the lithium nickel-based oxide, and can be 0 ≦ e ≦ 0.1 or 0 ≦ e ≦ 0.05.

[0292] On the other hand, the positive electrode active material according to the present invention may further include a coating layer containing one or more coating elements selected from the group consisting of Al, Ti, W, B, F, P, Mg, Ni, Co, Fe, Cr, V, Cu, Ca, Zn, Zr, Nb, Mo, Sr, Sb, Bi, Si, and S on the surface of the lithium nickel-based oxide particles as required. Desirably, the coating element can be Al, B, Co, or a combination thereof.

[0293] When a coating layer is present on the surface of the lithium nickel-based oxide particles, the coating layer inhibits contact between the electrolyte and the lithium composite transition metal oxide, thereby reducing the elution of the transition metal and gas generation due to side reactions with the electrolyte.

[0294] The positive electrode active material may be contained in an amount of 80 to 99 wt %, preferably 85 to 99 wt %, and more preferably 90 to 99 wt %, based on the total weight of the positive electrode active material layer.

[0295] The positive electrode current collector has a thickness of, for example, 3 to 500 μm. There are no particular limitations on the positive electrode current collector, as long as it does not induce chemical changes in the battery and is conductive. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. The electrode current collector may have fine irregularities on its surface to enhance the adhesive strength of the positive electrode active material, and may be in various forms, such as a film, sheet, foil, net, porous material, foam, or nonwoven fabric.

[0296] A conductive material may be further mixed with the positive electrode active material particles. The conductive material may be added in an amount of, for example, 1 to 50 wt % based on the total weight of the mixture containing the positive electrode active material. There are no particular limitations on the conductive material, as long as it does not induce chemical changes in the battery and has high conductivity. Examples of the conductive material include graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0297] The negative electrode is fabricated by coating and drying negative electrode active material particles on a negative electrode current collector, and may further contain components such as the aforementioned conductive material, binder, solvent, etc. as required.

[0298] The negative electrode current collector has, for example, a thickness of 3 to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, those surface-treated with carbon, nickel, titanium, silver, etc. on the surface of copper or stainless steel, aluminum-cadmium alloy, etc. can be used. Also, similar to the positive electrode current collector, fine irregularities may be formed on the surface to strengthen the binding force of the negative electrode active material, and it can be used in various forms such as films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc.

[0299] The negative electrode active material is, for example, carbon such as graphitizable carbon, graphite-based carbon; Li x Fe2O3 (0 ≦ x ≦ 1), Li x WO2 (0 ≦ x ≦ 1), Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1 elements, Group 2 elements, Group 3 elements of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8) metal composite oxides; lithium metal; lithium alloys; silicon-based alloys; tin-based alloys; oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials, etc. can be used.

[0300] The binder polymer usable in the electrode is a component that assists in binding between the electrode active material particles and the conductive material and between the electrode current collector, and is added in an amount of, for example, 1 to 50 wt % based on the total weight of the mixture including the electrode active material. Examples of such binder polymers include polyvinylidene fluoride-co-hexafluoropropylene (PVdF), polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, ethylene-vinyl acetate copolymer (polyethylene-co-vinyl acetate), polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. The binder polymer may be any one selected from the group consisting of cellulose acetate, cellulose acetate ester ...

[0301] Non-limiting examples of solvents used in the manufacture of the electrode include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or mixtures thereof. Such solvents provide a titration level of viscosity so that a slurry coating layer can be formed at a desired level on the surface of the electrode current collector.

[0302] The negative electrode includes a current collector and a negative electrode active material layer located on at least one surface of the current collector and including a negative electrode active material, a binder polymer, and a conductive material. The negative electrode active material includes a lower layer region in surface contact with the current collector and an upper layer region in surface contact with the lower layer region and extending to a surface of the negative electrode active material layer. The lower layer region and the upper layer region may each independently include at least one of graphite and a silicon-based compound as a negative electrode active material layer.

[0303] The lower layer region may contain natural graphite as the negative electrode active material, and the upper layer region may contain artificial graphite as the negative electrode active material.

[0304] The lower layer region and the upper layer region may each independently further include a silicon-based compound as a negative electrode active material.

[0305] The silicon-based compound may include at least one of SiOx (0≦x≦2) and SiC.

[0306] According to an embodiment of the present invention, the negative electrode may be manufactured by coating a lower layer slurry containing a lower layer negative electrode active material on a current collector and drying the slurry to form a lower layer region, and then coating an upper layer slurry containing an upper layer negative electrode active material on the lower layer region and drying the slurry to form an upper layer region.

[0307] According to an embodiment of the present invention, the negative electrode may include a step of preparing a lower layer slurry containing a negative electrode active material for a lower layer and an upper layer slurry containing a negative electrode active material for an upper layer; coating one surface of a negative electrode current collector with the lower layer slurry, and simultaneously or after a predetermined time lag, coating the upper layer slurry on the lower layer slurry; and drying the coated lower layer slurry and upper layer slurry simultaneously to form an active material layer.

[0308] In the latter method, a mixed region (intermixing) where different types of active materials are mixed may exist at the contact portion of the lower layer region and the upper layer region in the negative electrode. This is because, when an active material layer is formed by simultaneously or successively coating a lower layer slurry containing a lower layer negative electrode active material and an upper layer slurry containing an upper layer negative electrode active material on a current collector and then simultaneously drying them, a predetermined mixed region is generated at the interface where the lower layer slurry and the upper layer slurry come into contact before drying, and this mixed region is formed in the form of a mixed region layer when the slurry is subsequently dried.

[0309] In the active material layer of the negative electrode according to an embodiment of the present invention, the weight ratio (or the ratio of the load amount per unit area) of the upper layer region to the lower layer region may be 20:80 to 50:50, specifically 25:75 to 50:50.

[0310] The thicknesses of the lower and upper regions of the negative electrode active material layer of the present invention may not be exactly the same as the thicknesses of the coated lower layer slurry and the coated upper layer slurry, but the thickness ratio of the lower and upper regions of the negative electrode active material layer finally obtained after the drying or optional rolling process may be the same as the thickness ratio of the coated lower layer slurry and the coated upper layer slurry.

[0311] The first slurry is coated, and the second slurry is coated on top of the first slurry simultaneously or after a predetermined time lag. According to one embodiment of the present invention, the predetermined time lag may be 0.6 seconds or less, or 0.02 to 0.6 seconds, or 0.02 to 0.06 seconds, or 0.02 to 0.03 seconds. Since the time lag between the first and second slurries is due to the coating equipment, it is more preferable to coat the first and second slurries simultaneously. The method of coating the second slurry on top of the first slurry may use an apparatus such as a double slot die.

[0312] The step of forming the active material layer may further include a step of rolling the active material layer after the drying step. In this case, the rolling may be performed by a method commonly used in the art, such as roll pressing, at a pressure of 1 to 20 MPa and a temperature of 15 to 30°C.

[0313] The step of simultaneously drying the coated lower layer slurry and upper layer slurry to form the active material layer may be performed by a method commonly used in the art using a device that combines a hot air dryer and an infrared dryer.

[0314] The weight % of the first binder polymer in the solid content of the lower layer slurry may be the same as or greater than the weight % of the second binder polymer in the solid content of the upper layer slurry. According to one embodiment of the present invention, the weight % of the first binder polymer in the solid content of the lower layer slurry is 1.0 to 4.2 times, 1.5 to 3.6 times, or 1.5 to 3 times greater than the weight % of the second binder polymer in the solid content of the upper layer slurry.

[0315] In this case, when the weight percentage of the first binder in the coated lower layer slurry and the weight percentage of the second binder in the coated upper layer slurry satisfy this range, the binder in the lower layer region does not become too small, so detachment of the electrode layer does not occur, and the binder in the upper layer region does not become too large, so the resistance of the upper layer of the electrode decreases, which may result in advantageous fast charging performance.

[0316] The weight percentage of the first binder polymer in the solid content of the lower layer slurry may be 2 to 30 weight percent, or 5 to 20 weight percent, or 5 to 20 weight percent, and the weight percentage of the second binder polymer in the solid content of the upper layer slurry may be 0.5 to 20 weight percent, or 1 to 15 weight percent, or 1 to 10 weight percent, or 2 to 5 weight percent.

[0317] The total proportion (wt %) of the first binder polymer and the second binder polymer in the total solid content of the lower layer slurry and the upper layer slurry may be 2 to 20 wt %, or 5 to 15 wt %.

[0318] Hereinafter, the structure of an electrode assembly according to an embodiment of the present invention will be described in detail.

[0319] FIG. 14 is a cross-sectional view of a jelly-roll type electrode assembly 80 in which the electrode plate 40 of the first embodiment is applied to the first electrode plate (positive electrode plate) and the second electrode plate (negative electrode plate), taken along the Y-axis direction (winding axis direction).

[0320] The electrode assembly 80 can be manufactured by the winding method described in Fig. 2. For ease of explanation, the protruding structure of the non-coated portions 43a, 43b extending outward from the separator is shown in detail, and the winding structure of the first electrode plate, the second electrode plate, and the separator is not shown. The non-coated portion 43a protruding upward extends from the first electrode plate, and the non-coated portion 43b protruding downward extends from the second electrode plate.

[0321] The varying heights of the non-coated portions 43a, 43b are shown only schematically. That is, the heights of the non-coated portions 43a, 43b may vary irregularly depending on where the cross section is cut. For example, when the side portions of the trapezoidal segments 61, 61' are cut, the height of the non-coated portions in the cross section will be lower than the height of the segments 61, 61'. Therefore, it is understood that the height of the non-coated portions 43a, 43b in the drawings showing the cross section of the electrode assembly corresponds to the average height of the non-coated portions included in each winding turn (C2 in FIG. 11, D2 in FIG. 13).

[0322] Referring to Figure 14, the non-coated portion 43a of the first electrode plate includes a core-side non-coated portion B1 adjacent to the core of the electrode assembly 80, an outer-periphery-side non-coated portion B3 adjacent to the outer peripheral surface of the electrode assembly 80, and an intermediate non-coated portion B2 interposed between the core-side non-coated portion B1 and the outer-periphery-side non-coated portion B3.

[0323] The height (length in the Y-axis direction) of the outer peripheral non-coated portion B3 is relatively smaller than the height of the middle non-coated portion B2, which prevents the outer peripheral non-coated portion B3 from being pressed by the beading portion of the battery can, thereby preventing an internal short circuit from occurring.

[0324] The lower non-coating portion 43b has the same structure as the upper non-coating portion 43a. In one variation, the lower non-coating portion 43b may have a conventional electrode plate structure or the electrode plate structure of another embodiment (variation).

[0325] Ends 81 of the upper non-coated portion 43a and the lower non-coated portion 43b may be bent from the outer periphery toward the core of the electrode assembly 80. In this case, the outer periphery non-coated portion B3 may not be substantially bent.

[0326] FIG. 15 is a cross-sectional view of a jelly-roll type electrode assembly 90 in which the electrode plate 45 of the second embodiment is applied to the first electrode plate (positive electrode plate) and the second electrode plate (negative electrode plate), taken along the Y-axis direction (winding axis direction).

[0327] Referring to Figure 15, the non-coated portion 43a of the first electrode plate includes a core-side non-coated portion B1 adjacent to the core of the electrode assembly 90, an outer-periphery-side non-coated portion B3 adjacent to the outer periphery upper surface of the electrode assembly 90, and an intermediate non-coated portion B2 interposed between the core-side non-coated portion B1 and the outer-periphery-side non-coated portion B3.

[0328] The height of the outer non-coated portion B3 is relatively smaller than the height of the intermediate non-coated portion B2, and decreases gradually or in steps from the core side to the outer periphery side, thereby preventing the outer non-coated portion B3 from being pressed by the beading portion of the battery can and causing an internal short circuit.

[0329] The lower non-coating portion 43b has the same structure as the upper non-coating portion 43a. In one variation, the lower non-coating portion 43b may have a conventional electrode plate structure or an electrode plate structure of another embodiment (variation).

[0330] Ends 91 of the upper non-coated portion 43a and the lower non-coated portion 43b may be bent from the outer periphery toward the core of the electrode assembly 90. In this case, the outermost portion 92 of the outer periphery non-coated portion B3 may not be substantially bent.

[0331] FIG. 16 is a cross-sectional view of a jelly-roll type electrode assembly 100 in which any one of the electrode plates 50, 60, and 70 of the third to fifth embodiments (modifications thereof) is used as the first electrode plate (positive electrode plate) and the second electrode plate (negative electrode plate) along the Y-axis direction (winding axis direction).

[0332] Referring to Figure 16, the non-coated portion 43a of the first electrode plate includes a core-side non-coated portion B1 adjacent to the core of the electrode assembly 100, an outer-periphery-side non-coated portion B3 adjacent to the outer peripheral surface of the electrode assembly 100, and an intermediate non-coated portion B2 interposed between the core-side non-coated portion B1 and the outer-periphery-side non-coated portion B3.

[0333] The height of the core-side non-coating portion B1 is relatively smaller than the height of the middle non-coating portion B2. The height H is equal to or smaller than the bending length of the innermost non-coating portion 43a in the middle non-coating portion B2 or the radial length R of the core-side non-coating portion B1. The bending length H corresponds to the height of the non-coating portion 43a based on the point where the non-coating portion 43a is bent (C4 in FIG. 11, D4 in FIG. 13).

[0334] Therefore, even if the middle non-coated portion B2 is bent, the bent portion does not block the cavity 102 in the core of the electrode assembly 100. If the cavity 102 is not blocked, the electrolyte injection process is not difficult and the efficiency of the electrolyte injection is improved. In addition, a welding jig can be inserted through the cavity 102 to easily perform the welding process between the negative electrode current collecting plate and the battery can.

[0335] The height of the outer non-coated portion B3 is relatively smaller than the height of the middle non-coated portion B2, which prevents the outer non-coated portion B3 from being pressed by the beading portion and causing an internal short circuit.

[0336] In one variation, the height of the outer peripheral non-coated portion B3 may decrease gradually or in steps, unlike that shown in Figure 16. Also, in Figure 16, the height of the middle non-coated portion B2 is the same at a portion on the outer peripheral side, but the height of the middle non-coated portion B2 may increase gradually or in steps from the boundary between the core side non-coated portion B1 and the middle non-coated portion B2 to the boundary between the middle non-coated portion B2 and the outer peripheral non-coated portion B3.

[0337] The lower non-coating portion 43b has the same structure as the upper non-coating portion 43a. In one variation, the lower non-coating portion 43b may have a conventional electrode plate structure or an electrode plate structure of another embodiment (variation).

[0338] The ends 101 of the upper non-coated portion 43a and the lower non-coated portion 43b may be bent from the outer periphery side to the core side of the electrode assembly 100. At this time, the core-side non-coated portion B1 and the outer periphery-side non-coated portion B3 are not substantially bent.

[0339] When the middle non-coated portion B2 includes multiple segments, bending stress is alleviated, preventing tearing or abnormal deformation of the non-coated portion 43a near the bending point. Also, when the width and / or height and / or spacing pitch of the segments are adjusted within the ranges of the above-mentioned embodiments, the segments are folded toward the core, overlapping each other to an extent that sufficient welding strength is ensured, and no holes (gaps) are formed on the folded surface (surface viewed from the Y axis).

[0340] FIG. 17 is a cross-sectional view of an electrode assembly 110 according to yet another embodiment of the present invention, taken along the Y-axis (winding axis) direction.

[0341] Referring to Figure 17, the electrode assembly 110 is substantially identical in configuration to the electrode assembly 100 of Figure 16, except that the height of the outer non-coated portion B3 is substantially the same as the height of the outermost portion of the middle non-coated portion B2.

[0342] The outer peripheral non-coating portion B3 may include a plurality of segment pieces. The configuration relating to the plurality of segment pieces is substantially the same as that of the fourth embodiment and the fifth embodiment (modified examples).

[0343] In the electrode assembly 110, the height of the core-side non-coating portion B1 is relatively smaller than the height of the middle non-coating portion B2. In addition, the bending length H of the innermost non-coating portion of the middle non-coating portion B2 is equal to or smaller than the radial length R of the core-side non-coating portion B1.

[0344] Therefore, even if the middle non-coated portion B2 is bent, the bent portion does not block the cavity 112 in the core of the electrode assembly 110. If the cavity 112 is not blocked, the electrolyte injection process is easy and the efficiency of the electrolyte injection is improved. In addition, a welding jig can be inserted through the cavity 112 to easily perform the welding process between the negative electrode current collecting plate and the battery can.

[0345] In one variation, the structure in which the height of the intermediate non-coated portion B2 increases gradually or in steps from the core side toward the outer periphery side may be extended to the outer periphery non-coated portion B3. In this case, the height of the non-coated portion 43a may increase gradually or in steps from the boundary between the core side non-coated portion B1 and the intermediate non-coated portion B2 to the outermost surface of the electrode assembly 110.

[0346] The lower non-coating portion 43b has the same structure as the upper non-coating portion 43a. In one variation, the lower non-coating portion 43b may have a conventional electrode plate structure or the electrode plate structure of another embodiment (variation).

[0347] The ends 111 of the upper non-coated portion 43a and the lower non-coated portion 43b may be bent from the outer periphery side to the core side of the electrode assembly 110. At this time, the core-side non-coated portion B1 is not substantially bent.

[0348] When the middle non-coated portion B2 and the outer peripheral non-coated portion B3 include multiple segments, bending stress is alleviated, preventing tearing or abnormal deformation of the non-coated portions 43a, 43b near the bending points. Furthermore, when the width and / or height and / or spacing pitch of the segments are adjusted within the ranges of the above-mentioned embodiments, the segments are overlapped to an extent that sufficient welding strength is ensured as they are bent toward the core, preventing holes (gaps) from forming on the bending surface (surface viewed from the Y axis).

[0349] FIG. 18 is a cross-sectional view of an electrode assembly 120 according to yet another embodiment of the present invention, taken along the Y-axis (winding axis) direction.

[0350] Referring to FIG. 18, the electrode assembly 120 differs from the electrode assembly 100 of FIG. 16 in that the height of the intermediate non-coated portion B2 increases or decreases gradually or stepwise, but the remaining configuration is substantially the same.

[0351] The height of the middle non-coating portion B2 can be changed by adjusting the height of the step pattern (see FIG. 9) or segment pieces (see FIG. 10a or 12a) included in the middle non-coating portion B2.

[0352] In the electrode assembly 120, the height of the core-side non-coating portion B1 is relatively smaller than the height of the middle non-coating portion B2. In addition, the bending length H of the innermost non-coating portion of the middle non-coating portion B2 is equal to or smaller than the radial length R of the core-side non-coating portion B1.

[0353] Therefore, even if the middle non-coated portion B2 is bent toward the core side, the bent portion does not block the cavity 122 in the core of the electrode assembly 120. If the cavity 122 is not blocked, the electrolyte injection process becomes easier and the efficiency of electrolyte injection improves. In addition, a welding jig can be inserted through the cavity 122 to easily perform the welding process between the negative electrode current collecting plate and the battery can.

[0354] In addition, the height of the outer non-coated portion B3 is relatively smaller than the height of the middle non-coated portion B2. This prevents the outer non-coated portion B3 from being pressed by the beading of the battery can, causing an internal short circuit. In one example, the height of the outer non-coated portion B3 may decrease gradually or in steps toward the outer periphery.

[0355] The lower non-coating portion 43b has the same structure as the upper non-coating portion 43a. In a modified example, the lower non-coating portion 43b may have a conventional electrode plate structure or an electrode plate structure of another embodiment (modified example).

[0356] The ends 121 of the upper non-coated portion 43a and the lower non-coated portion 43b may be bent from the outer periphery side to the core side of the electrode assembly 120. At this time, the core-side non-coated portion B1 and the outer periphery-side non-coated portion B3 are not substantially bent.

[0357] When the middle non-coated portion B2 includes multiple segments, bending stress is alleviated, thereby preventing tearing or abnormal deformation of the non-coated portions 43a, 43b. Furthermore, when the width and / or height and / or spacing pitch of the segments are adjusted within the ranges of the above-mentioned embodiments, the segments are folded toward the core and overlapped to an extent that sufficient welding strength is ensured, and no holes (gaps) are formed on the folded surface (surface viewed from the Y axis).

[0358] FIG. 19 is a cross-sectional view of an electrode assembly 130 according to yet another embodiment of the present invention, taken along the Y-axis direction (winding axis direction).

[0359] Referring to FIG. 19, the electrode assembly 130 differs from the electrode assembly 120 of FIG. 18 in that the height of the outer non-coated portion B3 has a pattern in which the height gradually or stepwise decreases from the boundary between the outer non-coated portion B3 and the middle non-coated portion B2 toward the outermost surface of the electrode assembly 130; the remaining configurations are substantially identical.

[0360] The height change of the outer non-coated portion B3 can be realized by extending the stepped pattern (see FIG. 9) included in the middle non-coated portion B2 to the outer non-coated portion B3 and gradually or stepwise decreasing the height of the pattern toward the outer periphery. In another variation, the height change of the outer non-coated portion B3 can be realized by extending the segmented piece structure of the middle non-coated portion B2 to the outer non-coated portion B3 and gradually or stepwise decreasing the height of the segmented piece toward the outer periphery.

[0361] In the electrode assembly 130, the height of the core-side non-coating portion B1 is relatively smaller than the height of the middle non-coating portion B2. In addition, the bending length H of the innermost non-coating portion of the middle non-coating portion B2 is equal to or smaller than the radial length R of the core-side non-coating portion B1.

[0362] Therefore, even if the middle non-coated portion B2 is bent toward the core, the bent portion does not block the cavity 132 in the core of the electrode assembly 120. When the cavity 132 is not blocked, the electrolyte injection process becomes easier and the efficiency of electrolyte injection improves. In addition, a welding jig can be inserted through the cavity 132 to easily weld the negative electrode current collecting plate to the battery can.

[0363] The lower non-coating portion 43b has the same structure as the upper non-coating portion 43a. In one variation, the lower non-coating portion 43b may have a conventional electrode plate structure or an electrode plate structure of another embodiment (variation).

[0364] The ends 131 of the upper non-coated portion 43a and the lower non-coated portion 43b may be bent from the outer periphery side to the core side of the electrode assembly 130. At this time, the core-side non-coated portion B1 is not substantially bent.

[0365] When the middle non-coated portion B2 and the outer peripheral non-coated portion B3 include multiple segments, bending stress is alleviated, preventing tearing or abnormal deformation of the non-coated portions 43a, 43b near the bending points. Furthermore, when the width and / or height and / or spacing pitch of the segments are adjusted within the numerical ranges of the above-mentioned embodiments, the segments are bent toward the core and overlapped to an extent that sufficient welding strength is ensured, and no holes (gaps) are formed on the bending surface (surface viewed from the Y axis).

[0366] Various electrode assembly structures according to embodiments of the present invention are applicable to jelly-roll type cylindrical battery cells.

[0367] Desirably, the cylindrical battery cell may be, for example, a cylindrical battery cell having a form factor ratio (defined as the diameter divided by the height of the cylindrical battery cell, i.e., the ratio of the diameter Φ to the height H) of greater than about 0.4.

[0368] Here, the form factor refers to values ​​indicating the diameter and height of a cylindrical battery cell. Cylindrical battery cells according to an embodiment of the present invention may be, for example, 46110 cells, 48750 cells, 48110 cells, 48800 cells, and 46800 cells. In the numerical value indicating the form factor, the first two digits indicate the diameter of the cell, the next two digits indicate the height of the battery, and the last digit 0 indicates that the cross section of the cell is circular.

[0369] When an electrode assembly having a tabless structure is applied to a cylindrical battery cell with a form factor ratio exceeding 0.4, bending the non-coated portion can easily cause the non-coated portion to break due to the large radial stress applied. Furthermore, when welding a current collecting plate to the bent surface of the non-coated portion, the number of overlapping layers of the non-coated portion must be increased to ensure sufficient welding strength and reduce resistance. These requirements can be met by the electrode plate and electrode assembly according to an embodiment (variant) of the present invention.

[0370] A battery cell according to one embodiment of the present invention may be a substantially cylindrical cell having a diameter of about 46 mm, a height of about 110 mm, and a form factor ratio of 0.418.

[0371] Another example battery cell may be a cylindrical battery cell that is approximately cylindrical, with a diameter of about 48 mm, a height of about 75 mm, and a form factor ratio of 0.640.

[0372] In yet another embodiment, the battery cell may be a cylindrical battery cell that is approximately cylindrical, with a diameter of about 48 mm, a height of about 110 mm, and a form factor ratio of 0.436.

[0373] In yet another embodiment, the battery cell may be a cylindrical battery cell that is approximately cylindrical, with a diameter of about 48 mm, a height of about 80 mm, and a form factor ratio of 0.600.

[0374] In yet another embodiment, the battery cell may be a cylindrical battery cell that is approximately cylindrical, with a diameter of about 46 mm, a height of about 80 mm, and a form factor ratio of 0.575.

[0375] Conventionally, battery cells with a form factor ratio of approximately 0.4 or less have been used. For example, 18650 cells and 21700 cells have been used. 18650 cells have a diameter of approximately 18 mm, a height of approximately 65 mm, and a form factor ratio of 0.277. 21700 cells have a diameter of approximately 21 mm, a height of approximately 70 mm, and a form factor ratio of 0.300.

[0376] Hereinafter, a cylindrical battery cell according to an embodiment of the present invention will be described in detail.

[0377] FIG. 20 is a cross-sectional view of a cylindrical battery cell 140 according to an embodiment of the present invention taken along the Y-axis direction.

[0378] Referring to FIG. 20, a cylindrical battery cell 140 according to one embodiment of the present invention includes an electrode assembly 141 including a first electrode plate, a separator, and a second electrode plate, a battery can 142 that houses the electrode assembly 141, and a seal 143 that seals the open end of the battery can 142.

[0379] The battery can 142 is a cylindrical container with an opening at the top. The battery can 142 is made of a conductive metal material such as aluminum or steel. The battery can 142 accommodates the electrode assembly 10 in the inner space through the opening at the top, along with the electrolyte.

[0380] The electrolyte is A + B - The salt may have the structure: + Li + , Na + , K. + or a combination thereof. - is F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 -, AlO4 - , AlCl4 - , PF6 - , SbF6 - , AsF6 - , BF2C2O4 - , BC4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , C4F9SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN- and (CF3CF2SO2)2N - The anion comprises one or more anions selected from the group consisting of:

[0381] Alternatively, the electrolyte may be dissolved in an organic solvent, such as propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone, or a mixture thereof.

[0382] The electrode assembly 141 may have a jelly roll shape. As shown in Fig. 5, the electrode assembly 141 may be manufactured by sequentially stacking a lower separator, a first electrode plate, an upper separator, and a second electrode plate at least once, and winding the stack around a winding center C.

[0383] The first and second electrode plates have opposite polarities. That is, when one has a positive polarity, the other has a negative polarity. At least one of the first and second electrode plates may have an electrode plate structure according to the above-described embodiment (variant). The other of the first and second electrode plates may have a conventional electrode plate structure or an electrode plate structure according to the embodiment (variant).

[0384] An uncoated portion 146a of the first electrode plate and an uncoated portion 146b of the second electrode plate protrude from the upper and lower portions of the electrode assembly 141, respectively. The first electrode plate has the electrode plate structure of the first embodiment (variant). Therefore, in the uncoated portion 146a of the first electrode plate, the height of the outer peripheral uncoated portion B3 is smaller than the height of the uncoated portions of other portions. The outer peripheral uncoated portion B3 is spaced a predetermined distance from the inner circumferential surface of the battery can 142, particularly the beading portion 147. Therefore, the outer peripheral uncoated portion B3 of the first electrode plate does not come into contact with the battery can 142, which is electrically connected to the second electrode plate, thereby preventing an internal short circuit of the battery cell 140.

[0385] The non-coated portions 146b of the second electrode plate have the same height. In a modified example, the non-coated portions 146b of the second electrode plate may have the same structure as the non-coated portions 146a of the first electrode plate. In another modified example, the non-coated portions 146b of the second electrode plate may selectively have the structure of the non-coated portions of the electrode plate according to the embodiment (modified example).

[0386] The sealing body 143 may include an upper plate 143a, a first gasket 143b that provides airtightness between the upper plate 143a and the battery can 142 and has insulating properties, and a connecting plate 143c that is electrically and mechanically coupled to the upper plate 143a.

[0387] The cap plate 143a is a component made of a conductive metal material and covers the upper opening of the battery can 142. The cap plate 143a is electrically connected to the uncoated portion 146a of the first electrode plate and is electrically insulated from the battery can 142 by a first gasket 143b. Therefore, the cap plate 143a can function as a first electrode terminal of the cylindrical battery cell 140.

[0388] The cap plate 143a is mounted on a beading portion 147 formed on the battery can 142 and fixed by a crimping portion 148. A first gasket 143b may be interposed between the cap plate 143a and the crimping portion 148 to ensure airtightness of the battery can 142 and to provide electrical insulation between the battery can 142 and the cap plate 143a. The cap plate 143a may have a protrusion 143d formed to protrude upward from the center thereof.

[0389] The battery can 142 is electrically connected to the non-coated portion 146b of the second electrode plate. Therefore, the battery can 142 has the same polarity as the second electrode plate. If the second electrode plate has a negative polarity, the battery can 142 also has a negative polarity.

[0390] The battery can 142 has a beading portion 147 and a crimping portion 148 at its upper end. The beading portion 147 is formed by press-fitting around the outer periphery of the battery can 142. The beading portion 147 prevents the electrode assembly 141 housed inside the battery can 142 from slipping out of the upper opening of the battery can 142 and may function as a support portion on which the sealing body 143 is mounted.

[0391] The inner circumferential surface of the beading portion 147 is spaced a predetermined distance from the outer circumferential non-coated portion B3 of the first electrode plate. More specifically, the lower end of the inner circumferential surface of the beading portion 147 is spaced a predetermined distance from the outer circumferential non-coated portion B3 of the first electrode plate. In addition, because the height of the outer circumferential non-coated portion B3 is low, the outer circumferential non-coated portion B3 is not substantially affected when the battery can 12 is press-fitted from the outside to form the beading portion 147. Therefore, the outer circumferential non-coated portion B3 is not compressed by other components such as the beading portion 147, which prevents partial deformation of the electrode assembly 141 and prevents short circuits inside the cylindrical battery cell 140.

[0392] Preferably, the relationship D1≦D2 may be satisfied by defining the press-fit depth of the beading portion 147 as D1 and the radial length from the inner circumferential surface of the battery can 142 to the boundary between the outer non-coated portion B3 and the middle non-coated portion B2 as D2. In this case, damage to the outer non-coated portion B3 is substantially prevented when the battery can 142 is press-fit to form the beading portion 147.

[0393] The crimping portion 148 is formed on the upper portion of the beading portion 147. The crimping portion 148 has a curved shape that extends to surround the outer circumferential surface of the cap plate 143a disposed on the beading portion 147 and a portion of the upper surface of the cap plate 143a.

[0394] The cylindrical battery cell 140 may further include a first current collecting plate 144 and / or a second current collecting plate 145 and / or an insulator 146 .

[0395] The first current collecting plate 144 is connected to the upper part of the electrode assembly 141. The first current collecting plate 144 is made of a conductive metal material such as aluminum, copper, or nickel, and is electrically connected to the uncoated portion 146a of the first electrode plate. A lead 149 may be connected to the first current collecting plate 144. The lead 149 may extend upward from the electrode assembly 141 and be connected to the connection plate 143c, or may be directly connected to the lower surface of the cap plate 143a. The lead 149 may be connected to other components by welding.

[0396] Preferably, the first current collecting plate 144 may be integrally formed with the lead 149. In this case, the lead 149 may be in the form of a long plate extending outward from the center of the first current collecting plate 144.

[0397] The first current collecting plate 144 may have a plurality of radially formed projections and recesses (not shown) on its lower surface. When the radial projections and recesses are provided, the first current collecting plate 144 may be pressed against the first electrode plate to press the projections and recesses into the non-coated portion 146a.

[0398] The first current collecting plate 144 is bonded to an end of the uncoated portion 146a of the first electrode plate. The uncoated portion 146a and the first current collecting plate 144 may be bonded together by, for example, laser welding. Laser welding may be performed by partially melting the base material of the current collecting plate. In a modified example, the first current collecting plate 144 and the uncoated portion 146a may be welded together using solder. In this case, the solder may have a lower melting point than the first current collecting plate 144 and the uncoated portion 146a. Laser welding may be replaced by resistance welding, ultrasonic welding, etc.

[0399] A second current collecting plate 145 may be coupled to the lower surface of the electrode assembly 141. One surface of the second current collecting plate 145 may be coupled to the uncoated portion 146b of the second electrode plate by welding, and the other surface may be coupled to the inner bottom surface of the battery can 142 by welding. The coupling structure between the second current collecting plate 145 and the uncoated portion 146b of the second electrode plate may be substantially the same as the coupling structure between the first current collecting plate 144 and the uncoated portion 146a of the first electrode plate.

[0400] The non-coated portions 146a, 146b are not limited to the structure shown in the figure, and therefore, the non-coated portions 146a, 146b may selectively have not only the structure of a conventional non-coated portion but also the structure of a non-coated portion of an electrode plate according to an embodiment (variant).

[0401] The insulator 146 may cover the first current collecting plate 144. By covering the first current collecting plate 144 with the upper surface of the first current collecting plate 144, the insulator 146 may prevent direct contact between the first current collecting plate 144 and the inner peripheral surface of the battery can 142.

[0402] The insulator 146 has lead holes 151 through which the leads 149 extending upward from the first current collecting plate 144 are drawn out. The leads 149 are drawn upward from the lead holes 151 and coupled to the lower surface of the connection plate 143c or the lower surface of the cap plate 143a.

[0403] The peripheral region of the insulator 146 may be interposed between the first current collecting plate 144 and the beading portion 147 to fix the combination of the electrode assembly 141 and the first current collecting plate 144. This limits the movement of the combination of the electrode assembly 141 and the first current collecting plate 144 in the height direction of the battery cell 140, thereby improving the assembly stability of the battery cell 140.

[0404] The insulator 146 may be made of an insulating polymer resin. In one example, the insulator 146 may be made of polyethylene, polypropylene, polyimide, or polybutylene terephthalate.

[0405] The battery can 142 may further include a vent portion 152 formed on its bottom surface. The vent portion 152 is a region on the bottom surface of the battery can 142 that is thinner than the surrounding region. The vent portion 152 is structurally weaker than the surrounding region. Therefore, if an abnormality occurs in the cylindrical battery cell 140 and the internal pressure increases above a certain level, the vent portion 152 may burst, thereby releasing gas generated inside the battery can 142 to the outside.

[0406] The vent portion 152 may be formed continuously or discontinuously in a circle on the bottom surface of the battery can 142. In a variation, the vent portion 152 may be formed in a linear pattern or other patterns.

[0407] FIG. 21 is a cross-sectional view of a cylindrical battery cell 150 according to another embodiment of the present invention, taken along the Y-axis direction.

[0408] Referring to FIG. 21, the cylindrical battery cell 150 is substantially identical in configuration to the cylindrical battery cell 140 of FIG. 20, except that the electrode plate structure of the second embodiment (variant) is adopted for the uncoated portion 146a of the first electrode plate.

[0409] 21, the non-coated portion 146a of the first electrode plate may have a shape in which the height of the outer non-coated portion B3 decreases gradually or in steps as it progresses toward the inner circumferential surface of the battery can 142. Preferably, an imaginary line connecting the uppermost ends of the outer non-coated portion B3 may have the same or similar shape as the inner circumferential surface of the beading portion 147.

[0410] The outer peripheral non-coated portion B3 forms an inclined surface. Therefore, when the battery can 142 is press-fitted to form the beading portion 147, the outer peripheral non-coated portion B3 can be prevented from being pressed and damaged by the beading portion 147. Furthermore, the outer peripheral non-coated portion B3 can be prevented from coming into contact with a battery can 142 of opposite polarity, thereby preventing an internal short circuit.

[0411] The remaining configuration of the cylindrical battery cell 150 is substantially the same as that of the previously described embodiment (variant).

[0412] The non-coated portions 146a, 146b are not limited to the structure shown in the figure, and thus the non-coated portions 146a, 146b can selectively have not only the structure of a conventional non-coated portion but also the structure of a non-coated portion of an electrode plate according to an embodiment (variant).

[0413] FIG. 22 is a cross-sectional view of a cylindrical battery cell 160 according to yet another embodiment of the present invention, taken along the Y-axis direction.

[0414] Referring to FIG. 22, a cylindrical battery cell 160 differs from the cylindrical battery cells 140 and 150 described above in that the lead 149 connected to the first current collecting plate 144 is directly connected to the cap plate 143a of the sealed body 143 through the lead hole 151 of the insulator 146, and the insulator 146 and the first current collecting plate 144 are in close contact with the lower surface of the cap plate 143a, but the remaining configurations are substantially the same.

[0415] In the cylindrical battery cell 160, the diameter of the first current collecting plate 144 and the outermost diameter of the middle uncoated portion B2 are smaller than the smallest inner diameter of the battery can 142. In addition, the diameter of the first current collecting plate 144 may be the same as or larger than the outermost diameter of the middle uncoated portion B2.

[0416] Specifically, the minimum inner diameter of the battery can 142 may be the inner diameter of the battery can 142 at the position where the beading portion 147 is formed. In this case, the outermost diameters of the first current collecting plate 144 and the middle non-coated portion B2 are smaller than the inner diameter of the battery can 142 at the position where the beading portion 147 is formed. In addition, the diameter of the first current collecting plate 144 may be the same as or larger than the outermost diameter of the middle non-coated portion B2. The peripheral region of the insulator 146 may be bent downward and interposed between the outer peripheral non-coated portion B3 and the beading portion 147 to fix the combination of the electrode assembly 141 and the first current collecting plate 144.

[0417] Preferably, the insulator 146 includes a portion that covers the outer peripheral non-coated portion B3 and a portion that covers the first current collecting plate 144, and the portion connecting these two portions may both have a curved shape according to the curved shape of the beading portion 147. The insulator 146 may insulate the outer peripheral non-coated portion B3 from the inner peripheral surface of the beading portion 147, and may also insulate the first current collecting plate 144 from the inner peripheral surface of the beading portion 147.

[0418] The first current collecting plate 144 may be positioned higher than the lower end of the beading portion 147 and may be coupled to the core-side non-coated portion B1 and the middle non-coated portion B2. In this case, the press-fit depth D1 of the beading portion 147 is equal to or smaller than the distance D2 from the inner circumferential surface of the battery can 142 to the boundary between the outer circumferential non-coated portion B3 and the middle non-coated portion B2. Therefore, the core-side non-coated portion B1, the middle non-coated portion B2, and the first current collecting plate 144 coupled thereto may be positioned higher than the lower end of the beading portion 147. The lower end of the beading portion 147 refers to a bending point B between the beading portion 147 and the portion of the battery can 142 that houses the electrode assembly 141.

[0419] Because the core-side non-coated portion B1 and the middle non-coated portion B2 occupy the radially inner space of the beading portion 147, the space between the electrode assembly 141 and the cap plate 143a can be minimized. In addition, the connection plate 143c, which was previously located in the space between the electrode assembly 141 and the cap plate 143a, is omitted. As a result, the lead 149 of the first electrode plate 144 can be directly coupled to the underside of the cap plate 143a. This structure reduces the space within the battery cell, and energy density can be maximized by the reduced space.

[0420] In the cylindrical battery cell 160, the first current collecting plate 144 and the second current collecting plate 145 may be welded to the ends of the non-coated portions 146a and 146b, respectively, in the same manner as in the above-described embodiment.

[0421] The non-coated portions 146a, 146b are not limited to the structure shown in the figure, and therefore, the non-coated portions 146a, 146b may selectively have not only the structure of a conventional non-coated portion but also the structure of a non-coated portion of an electrode plate according to an embodiment (variant).

[0422] FIG. 23 is a cross-sectional view of a cylindrical battery cell 170 according to yet another embodiment of the present invention taken along the Y axis.

[0423] Referring to FIG. 23, the cylindrical battery cell 170 has substantially the same electrode assembly structure as the cylindrical battery cell 140 shown in FIG. 20, but differs in that the remaining structure except for the electrode assembly has been changed.

[0424] Specifically, the cylindrical battery cell 170 includes a battery can 171 having a rivet terminal 172 penetrating therethrough. The rivet terminal 172 is provided on the closed surface (top surface in the drawing) of the battery can 171. The rivet terminal 172 is riveted into the through-hole of the battery can 171 with a second insulating gasket 173 interposed therebetween. The rivet terminal 172 is exposed to the outside in the direction opposite to the direction of gravity.

[0425] The rivet terminal 172 includes a terminal exposure portion 172a and a terminal insertion portion 172b. The terminal exposure portion 172a is exposed to the outside of the closed surface of the battery can 171. The terminal exposure portion 172a may be located approximately at the center of the closed surface of the battery can 171. The maximum diameter of the terminal exposure portion 172a may be larger than the maximum diameter of the through-hole formed in the battery can 171. The terminal insertion portion 172b may penetrate approximately the center of the closed surface of the battery can 171 to be electrically connected to the uncoated portion 146a of the first electrode plate. The terminal insertion portion 172b may be rivet-connected to the inner surface of the battery can 171. That is, an end of the terminal insertion portion 172b may be bent toward the inner surface of the battery can 171. The maximum diameter of the end of the terminal insertion portion 172b may be larger than the maximum diameter of the through-hole in the battery can 171.

[0426] The lower end surface of the terminal insertion portion 172b may be welded to the first current collecting plate 144 connected to the uncoated portion 146a of the first electrode plate. An insulating cap 174 made of an insulating material may be interposed between the first current collecting plate 144 and the inner surface of the battery can 171. The insulating cap 174 covers the upper portion of the first current collecting plate 144 and the upper edge of the electrode assembly 141. This prevents the outer peripheral uncoated portion B3 of the electrode assembly 141 from coming into contact with the inner surface of the battery can 171 having the opposite polarity, causing a short circuit. The terminal insertion portion 172b of the rivet terminal 172 may be welded to the first current collecting plate 144 through the insulating cap 174.

[0427] The second gasket 173 is interposed between the battery can 171 and the rivet terminal 172 to prevent electrical contact between the battery can 171 and the rivet terminal 172, which have opposite polarities. As a result, the upper surface of the battery can 171, which has a substantially flat shape, can function as a second electrode terminal of the cylindrical battery cell 170.

[0428] The second gasket 173 includes a gasket exposing portion 173a and a gasket inserting portion 173b. The gasket exposing portion 173a is interposed between the terminal exposing portion 172a of the rivet terminal 172 and the battery can 171. The gasket inserting portion 173b is interposed between the terminal inserting portion 172b of the rivet terminal 172 and the battery can 171. The gasket inserting portion 173b may be deformed during riveting of the terminal inserting portion 172b, thereby adhering closely to the inner surface of the battery can 171. The second gasket 173 may be made of, for example, an insulating polymer resin.

[0429] The gasket exposing portion 173a of the second gasket 173 may extend to cover the outer peripheral surface of the terminal exposing portion 172a of the rivet terminal 172. When the second gasket 173 covers the outer peripheral surface of the rivet terminal 172, it is possible to prevent a short circuit from occurring during the process of connecting an electrical connection part, such as a bus bar, to the upper surface of the battery can 171 and / or the rivet terminal 172. Although not shown, the gasket exposing portion 173a may extend to cover not only the outer peripheral surface of the terminal exposing portion 172a but also a portion of the upper surface.

[0430] When the second gasket 173 is made of a polymer resin, the second gasket 173 can be bonded to the battery can 171 and the rivet terminal 172 by thermal welding. In this case, the airtightness at the bonding interface between the second gasket 173 and the rivet terminal 172 and at the bonding interface between the second gasket 173 and the battery can 171 can be strengthened. Meanwhile, when the gasket exposed portion 173a of the second gasket 173 has a shape that extends to the upper surface of the terminal exposed portion 172a, the rivet terminal 172 can be bonded integrally to the second gasket 173 by insert injection.

[0431] The remaining area 175 on the top surface of the battery can 171 excluding the area occupied by the rivet terminal 172 and the second gasket 173 becomes a second electrode terminal having a polarity opposite to that of the rivet terminal 172 .

[0432] The second current collecting plate 176 is coupled to the lower part of the electrode assembly 141. The second current collecting plate 176 is made of a conductive metal material such as aluminum, steel, copper, or nickel, and is electrically connected to the non-coated portion 146b of the second electrode plate.

[0433] Preferably, the second current collecting plate 176 is electrically connected to the battery can 171. To this end, the second current collecting plate 176 may be fixed with at least a portion of its peripheral edge interposed between the inner surface of the battery can 171 and the first gasket 178b. In one example, at least a portion of the peripheral edge of the second current collecting plate 176 may be fixed to the beading portion 178b by welding while being supported by the lower end surface of the beading portion 180 formed on the lower end surface of the battery can 171. In a modified example, at least a portion of the peripheral edge of the second current collecting plate 176 may be directly welded to the inner wall surface of the battery can 171.

[0434] The second current collecting plate 176 may have a plurality of projections and recesses (not shown) formed radially on the surface facing the non-coated portion 146b. When the projections and recesses are formed, the second current collecting plate 176 may be pressed against the non-coated portion 146b to press the projections and recesses into the non-coated portion 146b.

[0435] Preferably, the end of the second current collecting plate 176 and the uncoated portion 146b may be joined by welding, for example, laser welding.

[0436] The sealing body 178 that seals the lower open end of the battery can 171 includes a cap plate 178a and a first gasket 178b. The first gasket 178b electrically isolates the cap plate 178a from the battery can 171. A crimping portion 181 secures the periphery of the cap plate 178a and the first gasket 178b together. The cap plate 178a is provided with a vent portion 179. The configuration of the vent portion 179 is substantially the same as that of the above-described embodiment (variant).

[0437] Preferably, the cap plate 178a is made of a conductive metal material. However, the cap plate 178a does not have electrical polarity because the first gasket 178b is interposed between the cap plate 178a and the battery can 171. The seal 178 seals the open end of the lower part of the battery can 171 and functions to discharge gas when the internal pressure of the battery cell 170 increases above a critical value.

[0438] Preferably, the rivet terminal 172 electrically connected to the uncoated portion 146a of the first electrode plate is used as the first electrode terminal. Furthermore, a portion 175 of the upper surface of the battery can 171, excluding the rivet terminal 172, electrically connected to the uncoated portion 146b of the second electrode plate via the second current collecting plate 176 is used as a second electrode terminal having a polarity opposite to that of the first electrode terminal. When two electrode terminals are located on the upper portion of the cylindrical battery cell 170, electrical connection components such as bus bars can be disposed on only one side of the cylindrical battery cell 170. This simplifies the battery pack structure and improves energy density. Furthermore, the portion 175 used as the second electrode terminal has a substantially flat shape, ensuring a sufficient bonding area for bonding electrical connection components such as bus bars. This allows the cylindrical battery cell 170 to reduce resistance at the bonding locations of the electrical connection components to a desired level.

[0439] Meanwhile, the structure of the electrode assembly 141 and the structure of the non-application portion are not limited to those shown in the drawings, and can be replaced with the structures of the above-described embodiment (variations).

[0440] FIG. 24 is a cross-sectional view of a cylindrical battery cell 180 according to yet another embodiment of the present invention taken along the Y axis.

[0441] Referring to FIG. 24, the cylindrical battery cell 180 has substantially the same structure as the cylindrical battery cell 150 shown in FIG. 21 in terms of the electrode assembly 141, and the remaining configurations except for the electrode assembly 141 are substantially the same as the cylindrical battery cell 170 shown in FIG. 23.

[0442] Therefore, the configurations of the embodiments (variations) relating to the cylindrical battery cells 150 and 170 can be similarly applied to the cylindrical battery cell 180.

[0443] Furthermore, the structure of the electrode assembly 141 and the structure of the non-coating portion are not limited to those shown in the drawings, and can be replaced with the structures of the above-described embodiment (variations).

[0444] FIG. 25 is a cross-sectional view of a cylindrical battery cell 190 according to yet another embodiment of the present invention taken along the Y axis.

[0445] Referring to FIG. 25, a cylindrical battery cell 190 includes the electrode assembly 110 shown in FIG. 17, and the remaining configuration, excluding the electrode assembly 110, is substantially identical to the cylindrical battery cell 140 shown in FIG. 20.

[0446] 25, the non-coated portions 146a and 146b of the electrode assembly 110 are bent from the outer periphery toward the core. At this time, the core-side non-coated portion B1 is not substantially bent because it is lower in height than the other portions. The first current collecting plate 144 may be welded to the bent surface of the non-coated portion 146a, and the second current collecting plate 145 may be welded to the bent surface of the non-coated portion 146b. The bent surfaces may be formed at the top and bottom of the electrode assembly 110 by overlapping the non-coated portions 146a and 146b when they are bent.

[0447] The height of the core-side non-coating portion B1 is relatively smaller than that of other portions of the electrode assembly 110. Also, as shown in Fig. 17, the bending length H of the innermost non-coating portion of the middle non-coating portion B2 is equal to or smaller than the radial length R of the core-side non-coating portion B1.

[0448] Therefore, even if the non-coating portion 46a is bent toward the core side, the cavity 112 of the core of the electrode assembly 110 can be opened upward without being closed (see the dotted circle).

[0449] If the cavity 112 is not blocked, the process of injecting the electrolyte becomes easier, improving the efficiency of injecting the electrolyte. In addition, the process of welding the second current collecting plate 145 and the battery can 142 can be easily performed by inserting a welding jig through the cavity 112.

[0450] If the non-coated portions 146a, 146b have a segmented structure, by adjusting the width and / or height and / or spacing pitch of the segments to satisfy the numerical range of the above-mentioned embodiment, when the segments are bent, the segments are overlapped to an extent that sufficient welding strength can be ensured, and no space (gap) is formed at the bent surface.

[0451] The structure of the non-application portions 146a and 146b may be modified as desired to the structure of the above-described embodiment (variation) different from that shown in the figure. Note that there is no restriction on applying the structure of a conventional non-application portion to either one of the non-application portions 146a and 146b.

[0452] FIG. 26 is a cross-sectional view of a cylindrical battery cell 200 according to yet another embodiment of the present invention taken along the Y axis.

[0453] Referring to FIG. 26, a cylindrical battery cell 200 includes the electrode assembly 110 shown in FIG. 17, and the remaining configuration except for the electrode assembly 110 is substantially the same as the cylindrical battery cell 180 shown in FIG. 25.

[0454] 26, the non-coated portions 146a, 146b of the electrode assembly 110 are bent from the outer periphery toward the core. At this time, the core-side non-coated portion B1 is not substantially bent because it is lower in height than the other portions. The first current collecting plate 144 may be welded to the bent surface of the non-coated portion 146a, and the second current collecting plate 176 may be welded to the bent surface of the non-coated portion 146b.

[0455] The height of the core-side non-coating portion B1 is relatively lower than the other portions of the electrode assembly 110. Also, as shown in Fig. 17, the bending length H of the innermost non-coating portion of the middle non-coating portion B2 is equal to or smaller than the radial length R of the core-side non-coating portion B1.

[0456] Therefore, even if the non-coating portions 146a and 146b are bent toward the core side, the cavity 112 of the core of the electrode assembly 110 can be opened upward without being closed (see the dotted circle).

[0457] If cavity 112 is not blocked, the process of injecting the electrolyte becomes easier, improving the efficiency of injecting the electrolyte. Also, a welding jig can be inserted through cavity 112 to easily weld second current collecting plate 176 and battery can 171 together.

[0458] When the non-coated portions 146a, 146b have a segmented structure, if the width and / or height and / or spacing pitch of the segments are adjusted to satisfy the numerical range of the above-mentioned embodiment, when the segments are bent, the segments are overlapped to an extent that sufficient welding strength is ensured, and no space (gap) is formed at the bent surface.

[0459] The structure of the non-application portions 146a and 146b may be modified as desired to the structure of the above-described embodiment (variation) different from that shown in the figure. Note that there is no restriction on applying the structure of a conventional non-application portion to either one of the non-application portions 146a and 146b.

[0460] FIG. 27 is a cross-sectional view of a cylindrical battery cell 210 according to yet another embodiment of the present invention taken along the Y axis.

[0461] Referring to FIG. 27, a cylindrical battery cell 210 includes the electrode assembly 100 shown in FIG. 16, and the remaining configuration except for the electrode assembly 100 is substantially the same as the cylindrical battery cell 140 shown in FIG. 20.

[0462] Preferably, the non-coated portions 146a and 146b of the electrode assembly 100 are bent from the outer periphery toward the core. In this case, the core-side non-coated portion B1 and the outer periphery-side non-coated portion B3 of the non-coated portion 146a are not substantially bent because they are lower in height than the other portions. The same applies to the non-coated portion 146b. The first current collecting plate 144 may be welded to the bent surface of the non-coated portion 146a, and the second current collecting plate 145 may be welded to the bent surface of the non-coated portion 146b.

[0463] The height of the core-side non-coating portion B1 is relatively lower than that of the intermediate non-coating portion B2. As shown in Figure 16, the bent length H of the innermost non-coating portion of the intermediate non-coating portion B2 is equal to or smaller than the radial length R of the core-side non-coating portion B1.

[0464] Therefore, even if the non-application portions 146a and 146b are bent toward the core side, the cavity 102 of the core of the electrode assembly 100 can be opened upward without being closed (see the dotted circle).

[0465] If the cavity 102 is not blocked, the process of injecting the electrolyte becomes easier, improving the efficiency of injecting the electrolyte. In addition, the process of welding the second current collecting plate 145 and the battery can 142 can be easily performed by inserting a welding jig through the cavity.

[0466] Furthermore, the height of the outer peripheral non-coating portion B3 is relatively lower than that of the intermediate non-coating portion B2. Therefore, when the non-coating portion 146a is bent, the outer peripheral non-coating portion B3 is not substantially bent. Furthermore, since the outer peripheral non-coating portion B3 is sufficiently separated from the beading portion 147, the problem of the outer peripheral non-coating portion B3 being damaged during the process of press-fitting the beading portion 147 is solved.

[0467] When the non-coated portions 146a, 146b have a segmented structure, if the width and / or height and / or spacing pitch of the segments are adjusted to satisfy the numerical range of the above-mentioned embodiment, when the segments are bent, the segments are overlapped to an extent that sufficient welding strength is ensured, and no space (gap) is formed at the bent surface.

[0468] The structure of the non-application portions 146a and 146b may be modified as desired to the structure of the above-described embodiment (variation) different from that shown in the figure. Note that there is no restriction on applying the structure of a conventional non-application portion to either one of the non-application portions 146a and 146b.

[0469] FIG. 28 is a cross-sectional view of a cylindrical battery cell 220 according to yet another embodiment of the present invention taken along the Y axis.

[0470] Referring to FIG. 28, a cylindrical battery cell 220 includes the electrode assembly 100 shown in FIG. 17, and the remaining configuration except for the electrode assembly 100 is substantially the same as the cylindrical battery cell 180 shown in FIG. 24.

[0471] Preferably, the non-coated portions 146a, 146b of the electrode assembly 100 are bent from the outer periphery toward the core. At this time, the core-side non-coated portion B1 of the non-coated portion 146a is not substantially bent because it is lower in height than the other portions. The same applies to the non-coated portion 146b. The first current collecting plate 144 may be welded to the bent surface of the non-coated portion 146a, and the second current collecting plate 176 may be welded to the bent surface of the non-coated portion 146b.

[0472] In the electrode assembly 100, the height of the core-side non-coating portion B1 is relatively lower than that of the middle non-coating portion B2. Also, as shown in Fig. 16, the bending length H of the innermost non-coating portion in the middle non-coating portion B2 is equal to or smaller than the radial length R of the core-side non-coating portion B1.

[0473] Therefore, even if the non-coated portion 146a is bent toward the core side, the cavity 102 of the core of the electrode assembly 100 can be opened upward without being closed (see the dotted circle).

[0474] When the cavity 102 is not blocked, the process of injecting the electrolyte becomes easier, improving the efficiency of injecting the electrolyte. In addition, the process of welding the second current collecting plate 176 and the battery can 171 can be easily performed by inserting a welding jig through the cavity 102.

[0475] Furthermore, the height of outer peripheral non-coating portion B3 of non-coating portion 146a is relatively smaller than that of intermediate non-coating portion B2. As a result, when non-coating portion 146a is bent, outer peripheral non-coating portion B3 is not substantially bent. The same is true for non-coating portion 146b.

[0476] When the non-coated portions 146a, 146b have a segmented structure, if the width and / or height and / or spacing pitch of the segments are adjusted to satisfy the numerical range of the above-mentioned embodiment, when the segments are bent, the segments are overlapped to an extent that sufficient welding strength is ensured, and no space (gap) is formed at the bent surface.

[0477] The structure of the non-application portions 146a and 146b may be modified as desired to the structure of the above-described embodiment (variation) different from that shown in the figure. Note that there is no restriction on applying the structure of a conventional non-application portion to either one of the non-application portions 146a and 146b.

[0478] The cylindrical battery cells according to the above-described embodiments (variations) can be used to manufacture a battery pack.

[0479] FIG. 29 is a diagram schematically illustrating the configuration of a battery pack according to an embodiment of the present invention.

[0480] 29, a battery pack 300 according to an embodiment of the present invention includes an assembly of electrically connected cylindrical battery cells 301 and a pack housing 302 that accommodates the assembly. The cylindrical battery cells 301 may be any one of the battery cells according to the above-described embodiments (variants). For ease of illustration, components such as bus bars for electrically connecting the cylindrical battery cells 301, a cooling unit, and external terminals are omitted from the drawings.

[0481] The battery pack 300 may be installed in a vehicle. For example, the vehicle may be an electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle. The vehicle may include a four-wheeled vehicle or a two-wheeled vehicle.

[0482] FIG. 30 is a diagram illustrating a vehicle including the battery pack 300 of FIG.

[0483] 30, a vehicle V according to an embodiment of the present invention includes a battery pack 300 according to an embodiment of the present invention. The vehicle V operates by receiving power from the battery pack 300 according to an embodiment of the present invention.

[0484] According to the present invention, the non-coated portions protruding upward and downward from the electrode assembly are used as electrode tabs, thereby reducing the internal resistance of the cylindrical battery cell and increasing the energy density.

[0485] According to another aspect of the present invention, the structure of the non-coated portion of the electrode assembly is improved to prevent interference between the electrode assembly and the inner surface of the battery can during the process of forming a beading portion of the battery can, thereby preventing an internal short circuit in a cylindrical battery cell due to partial deformation of the electrode assembly.

[0486] In addition, according to another aspect of the present invention, by improving the structure of the non-coated portion of the electrode assembly, it is possible to prevent the non-coated portion from tearing near the bending point when the non-coated portion is bent, and to sufficiently increase the number of overlapping layers of the non-coated portion, thereby improving the welding strength.

[0487] According to yet another aspect of the present invention, by improving the structure of the non-coated portion adjacent to the core of the electrode assembly, it is possible to prevent the cavity in the core of the electrode assembly from being blocked when the non-coated portion is bent, and to facilitate the steps of injecting the electrolyte and welding the battery can and the current collecting plate.

[0488] According to yet another aspect of the present invention, it is possible to provide a cylindrical battery cell having a structure in which internal resistance is low, internal short circuits are prevented, and the welding strength between the current collecting plate and the non-coated portion is improved, as well as a battery pack and a vehicle including the same.

[0489] Although the present invention has been described above with reference to limited embodiments and drawings, the present invention is not limited thereto, and it is of course possible for a person skilled in the art to which the present invention pertains to make various modifications and variations within the technical spirit of the present invention and the equivalent scope of the claims set forth below.

[0490] Example 1 (1) Separation membrane manufacturing Approximately 5 wt% of polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP) polymer was added to tetrahydrofuran (THF) and dissolved at 50°C for approximately 12 hours to prepare a polymer solution. BaTiO powder with a diameter of approximately 400 nm was added to this polymer solution at a total solids content of 20 wt% and dispersed to prepare a mixed solution (BaTiO / PVdF-HFP = 80:20 (weight ratio)). The mixed solution was coated on both sides of a porous polymer substrate made of polypropylene using a doctor blade method. After coating, the THF was dried to form a porous coating layer on both sides of the porous polymer substrate.

[0491] Then, 80 parts by weight of Al2O3 as a filler for the insulating coating layer, 20 parts by weight of polyvinylidene fluoride (PVdF) as a binder for the insulating coating layer, and tetrahydrofuran as a solvent (dispersion medium) were added to prepare a composition for the insulating coating layer with a solid content of 20 wt%. The prepared composition for the insulating coating layer was coated on both ends of the porous coating layers formed on both sides of the porous polymer substrate and dried to produce a separator with an insulating coating layer.

[0492] The insulation width was 1.25 mm and the height was 0.3 μm. The porous polymer substrate had a thickness of 10 μm, and the porous coating layer had a thickness of 1.5 μm on each side. Measurements using a porosimeter revealed that the pore size and porosity of the resulting separator were 0.4 μm and 60%, respectively.

[0493] (2) Preparation of the current collector 1) Preparation of the positive electrode current collector As shown in Table 1 below, a metal thin film (15 μm thick) for a current collector made of aluminum material including a non-coated portion where the segment pieces of the first and second groups would be formed was prepared.

[0494] The metal thin film had a length in the winding direction from the core to the outer periphery (B1 + B2 + B3) of 4,000 mm, and a width in the winding axial direction of 75 mm. The metal thin film was divided into regions: B1 was the core-side non-coated region, B3 was the outer-periphery-side non-coated region, and B2, between the core-side non-coated region B1 and the outer-side non-coated region B3, was the intermediate non-coated region. The length of B1 was 350 mm, the length of B2 was 3,500 mm, and the length of B3 was 150 mm.

[0495] In the width direction of the metal thin film, a predetermined width from the second side portion to the inside is made into a positive electrode active material portion, and the remainder is made into a first part of the non-coated portion, and the core side non-coated portion and the outer peripheral side non-coated portion have a smaller height in the winding axis direction than the intermediate non-coated portion.

[0496] 2) Preparation of negative electrode current collector A negative electrode current collector was prepared in the same manner as the positive electrode current collector, except that a copper thin film (thickness 10 μm) was used as the current collector material and the width along the winding axis direction was 80 mm.

[0497] [Table 1]

[0498] (3) Manufacturing of the negative electrode Natural graphite with an average particle size D50 of 11 μm, carbon black, carboxymethyl cellulose (CMC), and styrene butadiene rubber (SBR) were mixed with water in a weight ratio of 94:1.5:2:2.5 to prepare a negative electrode active material layer slurry with a concentration of 50 wt% of the remaining components (excluding water). The slurry was then applied to the negative electrode active material portion on the surface of the copper current collector prepared above using a slot die at a running speed of 40 m / min. The width of the negative electrode active material portion was 70 mm based on the winding axis direction, and the width of the non-coated portion was 10 mm. The negative electrode active material loading amount was 16 mg / cm based on the electrode area. 2 The copper thin film coated with the negative electrode active material layer slurry was dried by passing it through a 60 m long hot air oven, and the oven temperature was controlled to maintain 130°C. Then, a target thickness of 180 μm was achieved, and a negative electrode with a density of 3.45 g / cc was obtained by roll pressing.

[0499] Thereafter, the middle non-coated section was notched with a laser to form a plurality of segments, each segment being divided according to the conditions in Table 1. At this time, the lower ends of the notched valleys of each segment were adjusted to have substantially the same height.

[0500] (4) Manufacturing of the positive electrode Li(Ni) as the positive electrode active material 0.6 Mn 0.2 Co 0.2 A cathode slurry was prepared by adding 02 (NCM-622), carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder to water as a dispersion medium in a weight ratio of 96:2:2. The slurry was coated on the surface of the aluminum current collector prepared above, and the cathode was fabricated by drying and rolling under the same conditions as the anode. The cathode had a width of 65 mm in the direction of the winding axis, and a width of 10 mm in the non-coated area. In this case, the positive electrode active material layer was formed to have an NP ratio of 1.18 (118%, approximately 27.7 cm ) of the battery, taking into account the theoretical discharge capacity of the NMC622. 2 ) was adjusted.

[0501] Next, the middle non-coated section was notched with a laser to form a plurality of segment pieces, each divided according to the conditions in Table 1. At this time, the lower ends of the notched valleys of each segment piece were adjusted to have substantially the same height.

[0502] (5) Preparation of electrode assembly The prepared anode / separator / cathode were stacked in this order and wound up to fabricate a jelly roll-type electrode assembly. The widthwise end of the separator was positioned at 30% (1.5 mm) of the height of the smallest folded segment (first group) based on the reference line and toward the outside of the electrode assembly.

[0503] (6) Cylindrical battery cell manufacturing (4680 type) The exposed upper and lower segments of the electrode assembly (groups 1 through 7) were folded toward the core, and then positive and negative current collectors were welded to the upper and lower bent surfaces, respectively. A cylindrical cell was then fabricated, as shown in Figure 28. Specifically, the electrode assembly with the welded positive and negative current collectors was inserted into a battery housing with pre-installed external terminals. The positive and negative current collectors were welded to the external terminals, and the peripheral edge of the negative current collector was welded to the beading. The battery housing was then placed in the chamber of an electrolyte injection device and stood upright with its opening facing counter to gravity. A nonaqueous electrolyte was then prepared by dissolving LiPF6 to a concentration of 1.0 M in an organic solvent mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and diethyl carbonate (DEC) in a 1:2:1 (volume ratio). After that, the electrolyte was injected through the opening of the battery housing, the chamber pressure was increased to 800 kPa for 20 seconds and maintained for 150 seconds, and the chamber pressure was then reduced to -90 kPa for another 20 seconds, maintaining a substantial vacuum state for 20 seconds. After the electrolyte impregnation process was completed, the opening of the battery housing was sealed with a sealant using a gasket to complete the fabrication of the cylindrical cell.

[0504] Comparative Example 1 (1) Separation membrane manufacturing A polymer solution was prepared by adding approximately 5 wt% polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP) to tetrahydrofuran (THF) and dissolving it at 50°C for at least 12 hours. BaTiO powder with a particle size of approximately 400 nm was added to the polymer solution at a total solids content of 20 wt% and dispersed to prepare a mixed solution (BaTiO / PVdF-HFP = 80:20 (weight ratio)). The mixed solution was coated on both sides of a porous polymer substrate made of polypropylene using a doctor blade method. After coating, the THF was dried to form porous coating layers on both sides of the porous polymer substrate, thereby producing a separator.

[0505] The thickness of the porous polymer substrate was 10 μm, and the thickness of the porous coating layer was 1.5 μm on each side. The pore size and porosity of the prepared separator were measured using a porosimeter and found to be 0.4 μm and 60%, respectively.

[0506] A current collector, a positive electrode, a negative electrode, and a cylindrical battery cell were manufactured in the same manner as in Example 1, except that the separator manufactured in Comparative Example 1 was used.

[0507] Evaluation of separators and cylindrical battery cells (1) Evaluation of the compression characteristics of separation membranes The compression characteristics of the separators prepared in Example 1 and Comparative Example 1 were evaluated by the following method.

[0508] Four sheets of A4 paper measuring 70 mm x 100 mm, two sheets of Haze PET measuring 50 mm x 50 mm, and one sheet of Haze PET were prepared, and three or more 50 mm x 50 mm separator membranes were punched out using a punching machine.

[0509] The thickness of the punched separator membrane before compression was measured. Three sheets were stacked, and then measurements were taken at a 3x3 point on the inner side, 10 cm from the periphery. The prepared separator membrane roll, PET film, and A4 paper were stacked in order. Starting from the top, two sheets of A4 paper, one sheet of haze PET film, one separator membrane roll, two sheets of haze PET film, and two sheets of A4 paper were stacked in this order.

[0510] The laminated sample was pressed using a hot press under conditions of 2,000 kgf (7.8 MPa), 70°C, and 10 seconds. The thickness of the separator after compression was measured using the same method as before compression to confirm the change in thickness.

[0511] The evaluation results of the compression characteristics of the separators prepared in Example 1 and Comparative Example 1 are shown in FIG.

[0512] 31, it can be seen that the separator of Example 1, which has an insulating coating layer on both ends of the porous coating layer, has an improved compressibility of about 1% compared to the separator of Comparative Example 1, which does not have an insulating coating layer. This is thought to be due to the force supported by the insulating coating layers coated on both ends of the separator when the separator is compressed.

[0513] (2) Evaluation of the resistance characteristics of cylindrical battery cells The resistance characteristics of the cylindrical battery cells manufactured in Example 1 and Comparative Example 1 according to the SOC were evaluated by the following method.

[0514] By applying charge and discharge currents alternately for 10 seconds, and taking into account the voltage drop / rise caused by each current, the slope can be calculated using Ohm's law, which is defined as DCIR (direct current internal resistance), i.e., internal resistance.

[0515] The resistance characteristics of the cylindrical battery cells manufactured in Example 1 and Comparative Example 1 are shown in FIG.

[0516] 32, it can be seen that the cylindrical battery cell including the separator of Example 1, which has insulating coating layers on both ends of the porous coating layer, exhibits a lower resistance value than the cylindrical battery cell including the separator of Comparative Example 1, which does not have an insulating coating layer. This is believed to be due to smoother movement of lithium ions when current is applied due to improved electrolyte impregnation.

[0517] (3) Evaluation of the amount of electrolyte impregnation (impregnation) The impregnated amount (impregnation ability) of the electrolyte of the cylindrical battery cells manufactured in Example 1 and Comparative Example 1 was evaluated by the following method, and the results are shown in FIG.

[0518] The cylindrical battery cells manufactured in Example 1 and Comparative Example 1 were disassembled to obtain the positive and negative electrodes, respectively. Then, a total of 9 points were cut at 10 cm intervals on the negative and positive electrodes. 2 Samples of the appropriate size were obtained by cutting out samples. The nine samples were taken from the area adjacent to the core of the electrode assembly when the electrode was unfolded: three samples (#1 to #3) from the area adjacent to the outer periphery of the electrode assembly when the electrode was unfolded, three samples (#7 to #9) from the area adjacent to the outer periphery of the electrode assembly, and three samples (#4 to #6) from the center of the electrode relative to the winding direction. Three samples were taken from each sample area, one each at the bottom, center, and top of the active material layer along the winding axis. Samples #1, #4, and #7 are near one end of the electrode in the width direction, and samples #3, #6, and #9 are near the other end of the electrode in the width direction. Samples #2, #5, and #8 represent intermediate portions. The sampled areas can be seen in Figure 34. Note that Figure 34 simply shows the sampled areas based on Figure 10, and the shapes and values ​​other than the sampled areas refer to Table 1.

[0519] The impregnation of the electrolyte was determined from the difference in weight between the control sample and the collected sample. The control sample was prepared identically to the electrodes used in Example 1 and Comparative Example 1 and was obtained from the same collection positions on the positive and negative electrodes that were not impregnated with the electrolyte.

[0520] In the electrode assembly of Example 1, the average impregnated amount of electrolyte in each of the #1 to #9 positive electrode portions was 21.3 mg, while in the electrode assembly of Comparative Example 1, the average impregnated amount of electrolyte in each of the #1 to #9 positive electrode portions was 18.3 mg. Furthermore, in the electrode assembly of Example 1, the average impregnated amount of electrolyte in each of the #1 to #9 negative electrode portions was 31.3 mg, while in the electrode assembly of Comparative Example 1, the average impregnated amount of electrolyte in each of the #1 to #9 negative electrode portions was 27.7 mg. It was confirmed that the impregnated amount of electrolyte in Example 1 was higher than that in Comparative Example 1. This is likely due to the fact that the application of insulating coating layers in addition to the porous coating layers formed on both sides of the separator's porous polymer substrate widened the area in which the electrolyte was absorbed. Furthermore, since the electrolyte was injected from top to bottom into the cylindrical battery cell, the electrolyte was first absorbed by the insulating coating layers, improving impregnation and increasing the impregnated amount.

[0521] (4) Evaluation of voltage and temperature characteristics of cylindrical battery cells The voltage and temperature characteristics according to SOC of the cylindrical battery cells having the separators of Example 1 and Comparative Example 1 were evaluated by the following method.

[0522] When discharging, if the current rate (C-rate) is changed, heat is generated in the cell, and the heat generation characteristics can be confirmed by comparing the temperature of the heat generated at this time.

[0523] FIG. 35 shows the evaluation results of voltage and temperature characteristics according to SOC of the cylindrical battery cells having the separators of Example 1 and Comparative Example 1.

[0524] Referring to FIG. 35, when the same current rate is applied, the separator of the present invention exhibits lower heat generation characteristics than conventional separators when discharged at current rates of 0.5C, 1.0C, 2.0C, and 3.0C. This is believed to be due to the previously lower internal resistance (DC-IR) and improved impregnation.

Claims

1. A separation membrane, The separator includes a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, the porous coating layer including a binder polymer and inorganic particles. An insulating coating layer is provided on each of both ends of the outermost lateral direction (TD) of the separator, The separator, wherein the insulating coating layer has a porous structure containing a filler for the insulating coating layer and a binder for the insulating coating layer.

2. 2. The separator according to claim 1, wherein the width of one of the insulating coating layers is 0.1% to 10% of the entire length of the separator in the width direction.

3. 2. The separator according to claim 1, wherein the average particle size of the filler for the insulating coating layer is 10% to 90% of the average particle size of the inorganic filler.

4. The separator according to claim 1 , wherein the vertical cross-sectional shape of the insulating coating layer has a rectangular, trapezoidal, triangular, parallelogrammatic, semicircular or semi-elliptical structure.

5. A jelly-roll type electrode assembly having a structure in which a sheet-like first electrode plate, a second electrode plate and a separator interposed therebetween are wound in one direction, 5. An electrode assembly, wherein the separator is the separator according to claim 1.

6. a jelly-roll type electrode assembly having a structure in which a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate are wound in one direction; a battery can in which the electrode assembly is housed; and a sealing body that seals an open end of the battery can, A cylindrical battery cell, characterized in that the separator is the separator according to any one of claims 1 to 4.

7. 7. The cylindrical battery cell of claim 6, wherein the cylindrical battery cell has a form factor ratio of 0.4 or greater.

8. 8. The cylindrical battery cell of claim 7, wherein the cylindrical battery cell is a 46110 cell, a 48750 cell, a 48110 cell, a 48800 cell, or a 46800 cell.

9. 7. The cylindrical battery cell according to claim 6, wherein the cylindrical battery cell is a battery having a tabless structure that does not include an electrode tab.

10. The positive electrode plate and the negative electrode plate each include a non-coated portion on which an active material layer is not formed, A positive electrode non-coated portion and a negative electrode non-coated portion are located at an upper end and a lower end of the electrode assembly, respectively; A current collecting plate is coupled to the non-coated portion of the positive electrode plate and the non-coated portion of the negative electrode plate, 7. The cylindrical battery cell according to claim 6, wherein the current collecting plate is connected to an electrode terminal.

11. A jelly-roll type electrode assembly having a structure in which a sheet-like first electrode plate, a second electrode plate and a separator interposed therebetween are wound in one direction, At least one of the first electrode plate and the second electrode plate includes a non-coated portion at an end of a long side where an active material layer is not coated, At least a part of the non-coated portion is used as an electrode tab, the non-coated portion includes a core-side non-coated portion adjacent to a core of the electrode assembly, an outer periphery-side non-coated portion adjacent to an outer periphery surface of the electrode assembly, and an intermediate non-coated portion interposed between the core-side non-coated portion and the outer periphery-side non-coated portion, At least one of the core-side non-coated portion and the outer-periphery-side non-coated portion has a height in the winding axial direction that is relatively smaller than that of the intermediate non-coated portion, At least a portion of the intermediate non-applied portion is divided into a plurality of segment pieces, An electrode assembly, wherein the separator is the separator according to claim 1 .

12. The electrode assembly according to claim 11, wherein the height of at least a portion of the intermediate non-coated portion in the winding axial direction increases stepwise from the core side to the outer periphery side.

13. The electrode assembly of claim 11, wherein each of the plurality of segment pieces has a rectangular, trapezoidal, triangular, parallelogrammatic, semicircular or semi-elliptical structure.

14. Each of the plurality of segment pieces is trapezoidal; The electrode assembly of claim 11, wherein the plurality of segment pieces are each configured such that a lower interior angle of the trapezoid increases from a core side to an outer periphery side, individually or in groups.

15. 12. The electrode assembly of claim 11, wherein at least one of a height in a winding axial direction and a width in a winding direction of the plurality of segment pieces increases stepwise from a core side to an outer periphery side, individually or in groups.

16. The electrode assembly of claim 11, wherein each of the plurality of segment pieces satisfies at least one of the following conditions: a width condition of 1 to 6 mm in a winding direction, a height condition of 2 to 10 mm in a winding axial direction, and a spacing condition of 0.05 to 1 mm in the winding direction.

17. The electrode assembly of claim 11, wherein a predetermined gap is provided between a lower end of the cutting line of the segment and the active material layer.

18. The electrode assembly according to claim 17, wherein the gap is between 0.2 mm and 4 mm.

19. The electrode assembly of claim 11, characterized in that the plurality of segment pieces form a plurality of segment piece groups as they proceed from the core side to the outer periphery side, and the segment pieces belonging to the same segment piece group have at least one of the width in the winding direction, the height in the winding axial direction, and the separation pitch in the winding direction that are the same as each other.

20. The electrode assembly according to claim 11, further comprising a combination of segment groups in which W3 / W2 is smaller than W2 / W1, where W1, W2, and W3 are widths in the winding direction for each of three segment groups that are consecutively adjacent in the radial direction of the electrode assembly.

21. The electrode assembly of claim 19, characterized in that the segments belonging to the same segment group have at least one of a width in the winding direction, a height in the winding axial direction, and a separation pitch in the winding direction that gradually increases as they move from the core side to the outer periphery side.

22. 20. The electrode assembly of claim 19, wherein at least some of the plurality of segment groups are disposed on the same winding turn of the electrode assembly.

23. The electrode assembly according to claim 11 , wherein the core-side non-coated portion does not have a segmented structure.

24. The electrode assembly according to claim 11 , wherein the outer peripheral non-coated portion does not have a segmented structure.

25. The electrode assembly according to claim 11, wherein the plurality of segment pieces are folded toward the core to overlap each other in multiple layers.

26. A cavity is provided in the core of the electrode assembly, 26. The electrode assembly of claim 25, wherein the cavity is not closed by a plurality of segment pieces folded toward the core.

27. 27. The electrode assembly according to claim 26, wherein a radial length R of the core-side non-coated portion and a bending length H of the innermost segment piece of the intermediate non-coated portion satisfy a relational expression H≦R.

28. The electrode assembly according to claim 11, wherein the height of the outer peripheral non-coated portion decreases stepwise or gradually from the core side to the outer peripheral side.

29. The outer peripheral non-coated portion is divided into a plurality of segments, The electrode assembly of claim 11, wherein the plurality of segment pieces included in the outer non-coating portion are larger than the plurality of segment pieces included in the middle non-coating portion in at least one of a width in the winding direction, a height in the winding axial direction, and a separation pitch in the winding direction.

30. a jelly-roll type electrode assembly having a structure in which a sheet-like first electrode plate, a sheet-like second electrode plate, and a separator interposed therebetween are wound in one direction; a battery can in which the electrode assembly is housed and which is electrically connected to one of the first electrode plate and the second electrode plate and has a first polarity; a sealing body that seals an open end of the battery can; a terminal having a second polarity, electrically connected to the first electrode plate and the remaining one of the second electrode plates and having a surface exposed to the outside; At least one of the first electrode plate and the second electrode plate includes a non-coated portion at a long side end portion where an active material layer is not coated, At least a part of the non-coated portion is used as an electrode tab, the non-coated portion includes a core-side non-coated portion adjacent to a core of the electrode assembly, an outer periphery-side non-coated portion adjacent to an outer periphery surface of the electrode assembly, and an intermediate non-coated portion interposed between the core-side non-coated portion and the outer periphery-side non-coated portion, At least one of the core-side non-coating portion and the outer-periphery-side non-coating portion has a height in the winding axial direction that is relatively smaller than that of the intermediate non-coating portion, At least a portion of the intermediate non-applied portion is divided into a plurality of segment pieces, A cylindrical battery cell, characterized in that the separator is the separator according to any one of claims 1 to 4.

31. the outer peripheral non-coating portion has a height in the winding axial direction that is relatively smaller than that of the intermediate non-coating portion, the battery can has a beading portion pressed inward at an end portion adjacent to the open end, The cylindrical battery cell according to claim 30, wherein an inner circumferential surface of the beading portion facing an upper peripheral edge of the electrode assembly and the outer circumferential uncoated portion are spaced apart by a predetermined distance.

32. 32. The cylindrical battery cell according to claim 31, wherein a press-in height D1 of the beading portion and a distance D2 from an inner peripheral surface of the battery can to a boundary point between the outer peripheral uncoated portion and the middle uncoated portion satisfy a relational formula D1≦D2.

33. a current collecting plate electrically coupled to the intermediate uncoated portion; 32. The cylindrical battery cell according to claim 31, further comprising: an insulator covering the current collecting plate, the insulator having a peripheral portion interposed and fixed between an inner peripheral surface of the beading portion and the current collecting plate.

34. 34. The cylindrical battery cell according to claim 33, wherein an outermost diameter of the current collecting plate and the intermediate uncoated portion is smaller than a minimum inner diameter of an inner circumferential surface of the beading portion, and a diameter of the current collecting plate is the same as or larger than the outermost diameter of the intermediate uncoated portion.

35. The current collecting plate is The cylindrical battery cell according to claim 33 , wherein the cylindrical battery cell is located higher than the beading portion.

36. At least a portion of the intermediate non-coated portion is bent from the outer periphery side to the core side, The electrode assembly has a core having a cavity therein, The cylindrical battery cell according to claim 30 , wherein the cavity is not closed by a folded structure of the middle uncoated portion.

37. the intermediate non-coating portion includes a plurality of segment pieces segmented along a winding direction of the electrode assembly, The plurality of segment pieces are bent from the outer periphery side to the core side, 37. The cylindrical battery cell according to claim 36, wherein a radial length R of the core-side non-coated portion and a bending length H of the segment piece located at the innermost side of the middle non-coated portion satisfy a relationship H≦R.

38. 38. The cylindrical battery cell according to claim 37, wherein each of the plurality of segment pieces has a rectangular, trapezoidal, triangular, parallelogrammatic, semicircular, or semi-elliptical structure.

39. 38. The cylindrical battery cell of claim 37, wherein each of the plurality of segment pieces satisfies at least one of the following conditions: a width condition of 1 mm to 6 mm in a winding direction, a height condition of 2 mm to 10 mm in a winding axial direction, and a spacing condition of 0.05 mm to 1 mm in the winding direction.

40. The cylindrical battery cell according to claim 30 , wherein a gap is provided between a lower end of the cutting line of the segment piece and the active material layer.

41. 41. The cylindrical battery cell according to claim 40, wherein the gap is between 0.2 mm and 4 mm.

42. The plurality of segment pieces constitute a plurality of groups, The segments belonging to each group are identical in at least one of the width in the winding direction, the height in the winding axis direction, and the separation pitch in the winding direction, 38. The cylindrical battery cell according to claim 37, wherein at least one of the plurality of groups constitutes the same wound turn of the electrode assembly.

43. The plurality of segment pieces constitute a plurality of groups, 38. The cylindrical battery cell according to claim 37, comprising a combination of segment groups in which W3 / W2 is smaller than W2 / W1, where W1, W2, and W3 are widths in the winding direction for each of three segment groups that are consecutively adjacent in the radial direction of the electrode assembly.

44. the sealing body includes a cap plate that seals an open end of the battery can, and a gasket that surrounds a peripheral portion of the cap plate and is crimped to an upper end of the battery can, 31. The cylindrical battery cell as claimed in claim 30, wherein the terminal having the second polarity is the cap plate.

45. a current collecting plate electrically connected to the non-coated portion of the second electrode plate having the first polarity and having at least a portion of an edge connected to a side wall of the battery can; the sealing body includes a non-polarized cap plate and a gasket that surrounds a periphery of the cap plate and is crimped to an upper end of the battery can, 31. The cylindrical battery cell according to claim 30, wherein the battery can includes a rivet terminal insulatively installed in a through-hole formed in a center of a closed surface, electrically connected to the first electrode plate, and having the second polarity.

46. A battery pack comprising at least one battery cell according to claim 30.

47. 47. A motor vehicle comprising at least one battery pack according to claim 46.

Citation Information

Patent Citations

  • Secondary battery

    JP2006012834A

  • Separator for electrochemical element and electrochemical element including the same

    JP2021513190A

  • Electrode assembly and secondary battery comprising the same

    KR1020170111721A

  • Method for predicting solubility and method for screening solvent using thereof