Separator for electrochemical device and electrochemical device including same

By using a porous polymer substrate and a porous coating with a specific composition on the separator of the electrochemical device, the problem of large dimensional change rate in high temperature and humidity state is solved, and the dimensional stability and durability of the electrochemical device are improved.

CN119096409APending Publication Date: 2024-12-06LG ENERGY SOLUTION LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202480002282.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-01-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing electrochemical devices have a large dimensional change rate under high temperature and humidity conditions, resulting in thermal shrinkage of the electrode and affecting the stability and life of the electrochemical devices.

Method used

The porous coating consisting of a porous polymer substrate and acrylic-based binder, acrylamide-based binder and inorganic particles is used to reduce the heat shrinkage of the partition by controlling the composition and structure of the coating.

Benefits of technology

Under high temperature and humidity conditions, the heat shrinkage rate of the separator is significantly reduced, the dimensional stability and durability of the electrochemical device are improved, and the electrodes are prevented from being exposed due to heat shrinkage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005098012000000181
    Figure BDA0005098012000000181
  • Figure BDA0005098012000000182
    Figure BDA0005098012000000182
  • Figure BDA0005098012000000191
    Figure BDA0005098012000000191
Patent Text Reader

Abstract

The present invention relates to a separator for an electrochemical device comprising a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, in which the porous coating layer comprises an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles, and wherein the porous coating comprises from about 90% to 96% by weight of inorganic particles based on the total weight of the porous coating, and a weight ratio of the acrylic acid-based binder to the acrylamide-based binder is from about 3: 7 to 7: 3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application is based on and claims the benefit of priority from Korean Patent Application No. 10-2023-0038631 filed on March 24, 2023, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference.

[0002] The present disclosure relates to a separator for an electrochemical device and an electrochemical device including the same. Background Art

[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions, and electrochemical devices including lithium secondary batteries have been widely used in recent years due to their high energy density and voltage, long cycle life, and wide use in various applications.

[0004] The lithium secondary battery may include an electrode assembly made of a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode, and the electrode assembly is housed in a housing together with an electrolyte. The separator may include a porous coating comprising a polymer binder and inorganic particles on at least one surface of a porous substrate. The inorganic particles may be connected to other inorganic particles by a polymer binder to form an interstitial volume, and lithium ions may migrate through the interstitial volume. In addition to fixing the inorganic particles, the polymer binder may also provide adhesion to the porous coating, and the porous coating may be adhered to the porous substrate and the electrode, respectively. Summary of the invention

[0005] Technical issues

[0006] The present disclosure provides a separator for an electrochemical device having a reduced dimensional change rate in a high-temperature wet state, a method for manufacturing the separator, and an electrochemical device including the separator.

[0007] Technical Solution

[0008] The present disclosure is directed to obtaining a separator that has dimensional stability under high temperature and wet conditions while keeping the content of polymer binder in the porous coating relatively low.

[0009] According to one aspect of the present disclosure, a separator for an electrochemical device includes: a porous polymer substrate and a porous coating formed on at least one surface of the porous polymer substrate, wherein the porous coating comprises an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles. Based on the total weight of the porous coating, the porous coating comprises about 90 wt % to about 96 wt % of inorganic particles, and the weight ratio of the acrylic acid-based binder to the acrylamide-based binder is about 3:7 to 7:3.

[0010] The acrylamide-based binder may have a weight average molecular weight of about 400,000 to about 1,000,000.

[0011] The porous coating layer may be formed by coating a coating slurry including an acrylic-based binder, an acrylamide-based binder, inorganic particles, a dispersant, and a dispersion medium on the porous polymer substrate, and the pH of the coating slurry may be about 3 to 9.

[0012] The acrylic-based binder may have a repeating unit including one or more monomers selected from acrylic acid and methacrylic acid.

[0013] The acrylamide-based binder may have repeating units containing one or more monomers selected from the group consisting of acrylamide, methacrylamide, N-ethylacrylamide, ethylmethacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-butylacrylamide, and N-butylmethacrylamide.

[0014] The content of the acrylic-based binder in the porous coating layer may be greater than or equal to the content of the acrylamide-based binder.

[0015] According to another aspect of the present disclosure, an electrochemical device is provided, which includes a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, wherein the separator is the separator for an electrochemical device according to one aspect above.

[0016] The electrochemical device may be a lithium secondary battery or a lithium rechargeable battery.

[0017] The electrochemical device may further include an electrolyte including a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed in a weight ratio of about 3:7, or a solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) are mixed in a weight ratio of about 20:5:75.

[0018] Beneficial Effects

[0019] The separator for an electrochemical device according to the present disclosure can provide improved dimensional stability in a dry state and in a wet state in which the electrochemical device is impregnated with an electrolyte solution. For example, the separator can exhibit a dry state heat shrinkage of about 5% or less under high temperature conditions of 200° C. or more, and a wet state heat shrinkage of about 10% or less under high temperature conditions of 130° C. or more, thereby preventing the electrode from being exposed due to thermal shrinkage of the separator. DETAILED DESCRIPTION

[0020] Hereinafter, each feature of the present disclosure will be described in detail to facilitate the practice of those skilled in the art to which the present disclosure belongs. The present disclosure can be implemented in various forms and is not limited or constrained by the embodiments described below.

[0021] As used herein, the term "including" is used to list materials, compositions, devices and methods that can be used in the present disclosure and is not limited to the listed examples.

[0022] As used herein, the words "about," "approximately," and "substantially" are used to mean a range or approximation of a value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent an infringer from taking unfair advantage of the present disclosure where precise or absolute numbers are provided to aid in the understanding of the present disclosure.

[0023] As used herein, the term "electrochemical device" may refer to a primary battery, a secondary battery, or a supercapacitor.

[0024] As used herein, the term “wet state” may refer to a state in which the separator is impregnated with at least a portion of the electrolyte, and the term “dry state” may refer to a dry state in which the separator is not impregnated with the electrolyte.

[0025] As used herein, the term “durability” may mean the ability of a binder to exhibit adhesion or mechanical strength as an inherent property without swelling or deforming when in contact with an electrolyte.

[0026] In an electrode assembly constituting a secondary battery, a separator is a membrane material that isolates two electrodes (positive / negative) to prevent electrical short circuits caused by physical contact, and has an ion-conducting function by providing a channel for ions to move between the two electrodes through an electrolyte contained in micropores.

[0027] The porous coating formed on one side of the separator contains a polymer binder and inorganic particles, and can prevent thermal shrinkage of the porous polymer substrate. The separator including the porous coating exhibits good dimensional stability in a dry state without an electrolyte, but in a wet state in which the separator is impregnated with an electrolyte, the adhesion of the polymer binder may be reduced due to the expansion and swelling of the polymer binder due to the electrolyte, or due to the separator being exposed to a temperature of about 130°C or higher (depending on the operating conditions of the lithium secondary battery including the separator). That is, due to the reduced adhesion of the porous coating, the separator tends to shrink significantly under these high temperature wet conditions. For example, a cylindrical battery in which an electrode assembly is wound and inserted into a housing using tension applied to the electrode assembly requires lower adhesion between the electrode and the separator than a pouch-type battery, and therefore contains less polymer binder, resulting in lower dimensional stability in a wet state.

[0028] The present disclosure provides a separator having improved dimensional stability under high temperature and wet conditions while keeping the content of polymer binder in the porous coating relatively low.

[0029] According to one embodiment of the present disclosure, a separator for an electrochemical device includes a porous polymer substrate and a porous coating formed on at least one surface of the porous polymer substrate, wherein the porous coating comprises an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles. Based on the total weight of the porous coating, the porous coating comprises about 90 wt % to 96 wt % of inorganic particles, and the weight ratio of the acrylic acid-based binder to the acrylamide-based binder is about 3:7 to 7:3.

[0030] The porous polymer substrate can be a porous film having a plurality of pores that electrically insulates the positive electrode and the negative electrode to prevent short circuits. For example, when the electrochemical device is a lithium secondary battery, the porous polymer substrate can be an ion-conducting barrier that allows lithium ions to pass while blocking electrical contact between the positive electrode and the negative electrode. At least a portion of the pores can form a three-dimensional network that communicates with the surface and interior of the porous polymer substrate, and a fluid can pass through the porous polymer substrate via the pores.

[0031] The porous polymer substrate can be a material that is physically and chemically stable to an electrolyte that is an organic solvent. Examples of porous polymer substrates include resins, such as polyolefins (e.g., polyethylene, polypropylene, and polybutylene), polyvinyl chloride, polyethylene terephthalate, polycycloolefins, polyethersulfones, polyamides, polyimides, polyimide amides, nylons, polytetrafluoroethylene, and copolymers or mixtures thereof, but are not limited thereto. For example, a polyolefin-based resin can be used. A polyolefin-based resin is suitable for manufacturing an electrochemical device with a higher energy density because it can be processed into a relatively small thickness and is easily coated with a slurry.

[0032] The porous polymer substrate may have a monolayer or multilayer structure. The porous polymer substrate may include two or more polymer resin layers with different melting points (Tm) to provide shutdown capability during high temperature runaway of the battery. For example, the porous polymer substrate may include a polypropylene layer with a relatively high melting point and a polyethylene layer with a relatively low melting point. The porous polymer substrate may be a three-layer structure in which polypropylene, polyethylene, and polypropylene are laminated in this order. When the temperature of the battery rises above a predetermined temperature, the polyethylene layer melts and closes the pores, thereby preventing thermal runaway of the battery.

[0033] The thickness of the porous polymer substrate may be about 1 μm or more and 100 μm or less. For example, the thickness of the porous polymer substrate may be about 10 μm or more and 90 μm or less, 20 μm or more and 80 μm or less, 30 μm or more and 70 μm or less, or 40 μm or more and 60 μm or less. For example, the thickness of the polymer substrate may be 1 μm or more and 30 μm or less. For example, the thickness of the polymer substrate may be about 5 μm or more and 15 μm or less, or 8 μm or more and 13 μm or less. When the thickness of the porous polymer substrate is adjusted within the above range, the amount of active material contained in the electrochemical device may be increased by minimizing the volume of the electrochemical device while electrically insulating the positive and negative electrodes.

[0034] The porous polymer substrate may include pores having an average diameter of about 0.01 μm or more and 1 μm or less. For example, the size of the pores included in the porous polymer substrate may be about 0.01 μm or more and 0.09 μm or less, 0.02 μm or more and 0.08 μm or less, 0.03 μm or more and 0.07 μm or less, or 0.04 μm or more and 0.06 μm or less. For example, the size of the pores may be about 0.02 μm or more and 0.06 μm or less. When the pore size of the porous polymer substrate is adjusted within the above range, the permeability and ionic conductivity of the entire separator prepared may be controlled.

[0035] The permeability of porous polymer substrate can be about 10 seconds / 100cc or more and 100 seconds / 100cc or less. For example, the permeability of porous polymer substrate can be 10 seconds / 100cc or more and 90 seconds / 100cc or less, 20 seconds / 100cc or more and 80 seconds / 100cc or less, 30 seconds / 100cc or more and 70 seconds / 100cc or less, or 40 seconds / 100cc or more and 60 seconds / 100cc or less. For example, the permeability of porous polymer substrate can be about 50 seconds / 100cc or more and 70 seconds / 100cc or less. When the permeability of porous polymer substrate is within the above range, the permeability of the separator prepared can be set in the range suitable for ensuring the output characteristics and cycle characteristics of electrochemical device.

[0036] Permeability (seconds / 100cc) means the time (in seconds) it takes for 100cc of air to pass through a predetermined area of ​​a porous polymer substrate or separator at a constant pressure. Permeability can be measured using a Gurley air permeability tester according to ASTM D726-58, ASTM D726-94, or JIS-P8117. For example, a 4110N instrument from Gurley can be used to measure the permeability of 100cc of air at 0.304 kPa air or 1.215 kN / m2 The pressure of water passing through 1 square inch (or 6.54 cm 2 For example, the time it takes for 100cc of air to pass through a 1 square inch sample at room temperature under a constant pressure of 4.8 inches of water can be measured using an ASAHI SEIKO EG01-55-1MR instrument.

[0037] The porosity of the porous polymer substrate can be about 10 volume % or more and 60 volume % or less. For example, the porosity of the porous polymer substrate can be about 15 volume % or more and 55 volume % or less, 20 volume % or more and 50 volume % or less, 25 volume % or more and 45 volume % or less, or 30 volume % or more and 40 volume % or less. For example, the porosity of the porous polymer substrate can be about 30 volume % or more and 50 volume % or less. When the porosity of the porous polymer substrate is within the above range, the ionic conductivity of the prepared separator can be set within a range suitable for ensuring the output characteristics and cycle characteristics of the electrochemical device.

[0038] Porosity refers to the ratio of the volume of the pores to the total volume of the porous polymer substrate. Porosity can be measured by methods known in the art. For example, porosity can be measured by Brunauer Emmett Teller (BET) measurement using nitrogen adsorption, capillary flow porometer, or water or mercury permeation method.

[0039] The porous coating layer is formed on at least one surface of the porous polymer substrate and includes a polymer binder and inorganic particles, and the polymer particles may include an acrylic-based binder and an acrylamide-based binder.

[0040] The porous coating can be formed by coating at least one surface of a porous polymer substrate with a coating slurry comprising an acrylic acid-based binder, an acrylamide-based binder, inorganic particles, a dispersant, and a dispersion medium. For example, the separator can be prepared by applying the coating slurry to at least one surface of the porous polymer substrate and then drying to remove the dispersion medium. Since the inorganic particles contained in the porous coating are connected by an acrylic acid-based binder and an acrylamide-based binder to form an interstitial volume, the porous coating adheres to the porous polymer substrate while allowing lithium ions to pass through the interstitial volume, thereby preventing thermal shrinkage of the porous polymer substrate.

[0041] The coating slurry can include a dispersion medium for dissolving or dispersing at least a portion of an acrylic acid-based binder or an acrylamide-based binder and dispersing inorganic particles. By controlling the type and content of the dispersion medium, a coating slurry in which a polymer binder and inorganic particles are uniformly dispersed can be used. The example of the dispersion medium includes water, ethanol, acetone, isopropyl alcohol (IPA), dimethylacetamide (DMAc), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), acetonitrile, and a combination thereof. The dispersion medium of the above type can be used to form a porous coating in which inorganic particles are uniformly dispersed.

[0042] The coating slurry may contain a dispersant for maintaining uniform dispersion of an acrylic acid-based binder, an acrylamide-based binder, and inorganic particles. Examples of dispersants include one or more selected from the following: oil-soluble polyamines, oil-soluble amine compounds, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid, pyrogallic acid, and polyacrylic acid. For example, the dispersant may be a polymer dispersant based on polyacrylic acid. By using the above-mentioned type of dispersant, the stability of the coating slurry can be improved, and the uniformity of the porous coating formed by the coating slurry can be ensured.

[0043] Based on the total weight of the coating slurry, the dispersant may be included in an amount of about 0.01 wt % or more and 5 wt % or less. For example, the content of the dispersant may be 0.1 wt % or more and 4 wt % or less, 0.5 wt % or more and 3 wt % or less, or 1 wt % or more and 2 wt % or less. For example, the content of the dispersant may be about 3 wt % or more and 5 wt % or less. When the content of the dispersant is adjusted within the above range, uniform dispersion and stability of the polymer binder and inorganic particles contained in the coating slurry may be achieved.

[0044] The pH of the coating slurry containing the dispersant can be about 3 to 9. For example, the pH of the coating slurry can be about 3.5 or more and 8.5 or less, 4.0 or more and 8.0 or less, 4.5 or more and 7.5 or less, 5.0 or more and 7.0 or less, or 5.5 or more and 6.5 or less. For example, the pH of the coating slurry can be about 5.5 to 8.5, or about 6.0 to 8.0. The pH of the coating slurry can be adjusted by changing the type or physical properties of the dispersant. For example, the dispersant can be a polymer dispersant based on polyacrylic acid, and the pH of the coating slurry can be adjusted by adjusting the degree of substitution of the polymer dispersant based on polyacrylic acid. For example, the pH of the coating slurry can be adjusted by controlling the -COOH in the polymer dispersant based on polyacrylic acid to be replaced by -COOH - Na +When the pH of the coating slurry is adjusted within the above range, the cohesion with the inorganic particles is improved by uniform dispersion of the polymer binder, especially the acrylic-based binder, contained in the coating slurry, thereby reducing the thermal shrinkage of the porous coating layer and the separator provided with the porous coating layer.

[0045] The viscosity of the coating slurry containing a dispersant can be about 10cps or more and 500cps or less. For example, the viscosity of the coating slurry can be 50cps or more and 450cps or less, 100cps or more and 400cps or less, 150cps or more and 350cps or less, or 200cps or more and 300cps or less. For example, the viscosity of the coating slurry can be about 10cps or more and 100cps or less, or about 10cps or more and 50cps or less. When the viscosity of the coating slurry exceeds 500cps, agglomerates with an average particle size (D99) of about 100 μm are formed, which makes it difficult to manufacture a separator by continuously applying on a porous polymer substrate, making it difficult to ensure productivity.

[0046] The coating slurry may also include additives such as surfactants, defoamers, flame retardants and wetting agents. Based on the gross weight of the coating slurry, the additive may be included in an amount of about 0 wt % or more and 10 wt % or less. For example, the content of the additive is about 0.01 wt % or more and 9 wt % or less, 0.1 wt % or more and 8 wt % or less, 1 wt % or more and 7 wt % or less, 2 wt % or more and 6 wt % or less, or 3 wt % or more and 5 wt % or less. For example, the content of the additive may be about 1 wt % or more and 5 wt % or less. When the content of the additive is adjusted within the above range, the dimensional stability and flame retardancy of the porous coating formed by the coating slurry can be ensured.

[0047] After forming the porous coating, the dispersion medium contained in the coating slurry can be removed by drying or heating. For example, the porous coating can contain 5ppm or less dispersion medium. For example, the porous coating can be composed of an acrylic acid-based binder, an acrylamide-based binder, inorganic particles and a dispersant. In the process of removing the dispersion medium, a plurality of holes can be formed on the surface and inside of the porous coating. The hole can include the gap volume formed by connecting adjacent inorganic particles through an acrylic acid-based binder, an acrylamide-based binder or the two, and can have a structure in which a three-dimensional network is formed to allow fluid to pass.

[0048] The thickness of the porous coating layer may be about 1 μm or more and 15 μm or less. For example, the thickness of the porous coating layer may be about 2 μm or more and 14 μm or less, 3 μm or more and 13 μm or less, 4 μm or more and 12 μm or less, 5 μm or more and 11 μm or less, 6 μm or more and 10 μm or less, or 7 μm or more and 9 μm or less. For example, the thickness of the porous coating layer may be about 1 μm or more and 5 μm or less. For example, the thickness of the porous coating layer may be about 1.5 μm or more and 3.5 μm or less. When the thickness of the porous coating layer is adjusted within the above range, the shrinkage of the porous polymer substrate may be minimized and stable adhesion to the porous polymer substrate may be achieved.

[0049] The acrylic-based binder can bind the inorganic particles contained in the porous coating and improve the adhesion of the porous coating to the porous polymer substrate. The acrylic-based binder can have a repeating unit containing one or more monomers selected from acrylic acid and methacrylic acid. For example, the acrylic-based binder can be polyacrylic acid (PAA).

[0050] When an acrylic-based binder is included in the coating slurry, dispersibility may be determined by the pH concentration of the coating slurry. When the pH of the coating slurry is 3 to 9, binding of the inorganic particles through the acrylic-based binder and resulting dimensional stability of the porous coating layer may be ensured.

[0051] The weight average molecular weight (Mw) of the acrylic-based binder can be about 50,000 or more and 400,000 or less. For example, the weight average molecular weight of the acrylic-based binder can be about 100,000 or more and 350,000 or less, 150,000 or more and 300,000 or less, or 200,000 or more and 250,000 or less. For example, the weight average molecular weight of the acrylic-based binder can be about 100,000 or more and 200,000 or less. When the weight average molecular weight of the acrylic-based binder is adjusted within the above range, the dense agglomeration of the inorganic particles can be achieved by uniformly mixing with the inorganic particles in the porous coating, thereby reducing the thermal shrinkage of the separator.

[0052] In the present disclosure, the weight average molecular weight of the polymer binder can be measured by gel permeation chromatography (GPC) (PL GPC220, Agilent Technologies). For example, the weight average molecular weight can be determined by using trichlorobenzene (TCB) as a solvent in a PL Olexis (Polymer Laboratories) column (column temperature: 160°C), and using an Agilent high temperature RI detector (using cubic function correction, reference: polystyrene) under the conditions of a sample concentration of 1.0 mg / mL, a flow rate of 1.0 mL / min, and an injection volume of 200 μl.

[0053] The binder based on acrylamide can be included in the porous coating to give the porous coating tolerance to electrolyte. The binder based on acrylamide can have a repeating unit containing one or more monomers selected from the following: acrylamide, methacrylamide, N-ethylacrylamide, ethylmethacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-butylacrylamide and N-butylmethacrylamide. Butylacrylamide can refer to sec-butylacrylamide and tert-butylacrylamide, and butylmethacrylamide can refer to sec-butylmethacrylamide and tert-butylmethacrylamide. For example, the binder based on acrylamide can be polyacrylamide (PAM).

[0054] The weight average molecular weight (Mw) of the acrylamide-based binder can be about 400,000 or more and 1,000,000 or less. For example, the weight average molecular weight of the acrylamide-based binder can be 450,000 or more and 950,000 or less, 500,000 or more and 900,000 or less, 550,000 or more and 850,000 or less, 600,000 or more and 800,000 or less, or 650,000 or more and 750,000 or less. For example, the weight average molecular weight of the acrylamide-based binder can be about 400,000 or more and 900,000 or less. When the weight average molecular weight of the acrylamide-based binder is within the above range, the viscosity of the coating slurry will not exceed 500cps to form a porous coating, thereby reducing the thermal shrinkage of the separator.

[0055] The porous coating layer may include an acrylic-based binder and an acrylamide-based binder in a weight ratio of about 3:7 to 7:3. For example, the porous coating layer may include an acrylic-based binder and an acrylamide-based binder in a weight ratio of about 4:6 to 6:4, preferably 4.5:5.5 to 5.5:4.5. For example, the content of the acrylic-based binder of the porous coating layer may be greater than or equal to the content of the acrylamide-based binder while satisfying the above range. For example, the porous coating layer may include an acrylic-based binder and an acrylamide-based binder in a weight ratio of about 6:4 to 5:5.

[0056] Acrylic acid-based binders can interact with inorganic particles more easily than acrylamide-based binders, thereby contributing to the formation of the above-mentioned gap volume. For example, acrylic acid-based binders can show electrostatic attraction or hydrogen bond formation to inorganic particles via carboxyl groups. Acrylamide-based binders show a larger modulus than acrylic acid-based binders, which can help ensure the durability of the separator by maintaining the structure of the porous coating even in the wet state of the separator impregnated with electrolyte. When the content of acrylic acid-based binders and acrylamide-based binders is adjusted within the above range, the gap volume formation of acrylic acid-based binders and the structural stability of the porous coating by acrylamide-based binders can be ensured at the same time. The thermal shrinkage of the separator with a porous coating that meets the above range in a wet state can be reduced. When the content of acrylic acid-based binders exceeds the above range, the structural stability of the porous coating may be reduced in a wet state, thereby causing rapid thermal shrinkage. When the content of acrylamide-based binders exceeds the above range, the combination of inorganic particles may be insufficient in a dry state, thereby causing rapid thermal shrinkage.

[0057] The porous coating layer contains an acrylic acid-based binder and an acrylamide-based binder separately, but does not contain a copolymer of an acrylic acid-based binder and an acrylamide-based binder. Compared with the use of a copolymer, the use of a mixture of an acrylic acid-based binder and an acrylamide-based binder facilitates the adjustment of the weight average molecular weight and content ratio of a single binder, making it easy to simultaneously achieve the above-mentioned advantages based on the weight average molecular weight range and the advantages based on the content range.

[0058] Based on the total weight of the porous coating, the porous coating may include about 90% to 96% by weight of inorganic particles. For example, based on the total weight of the porous coating, the content of the inorganic particles may be about 90.5% by weight or more and 95.5% by weight or less, 91.0% by weight or more and 95.0% by weight or less, 91.5% by weight or more and 94.5% by weight or less, 92.0% by weight or more and 94.0% by weight or less, or 92.5% by weight or more and 93.5% by weight or less. For example, based on the total weight of the porous coating, the content of the inorganic particles may be about 93% by weight or more and 96% by weight or less. Since within the above range, the separator has a mechanical strength suitable for cylindrical batteries, a separator with reduced thermal shrinkage in a wet state can be manufactured. At the same time, even if the content of the inorganic particles based on the total weight of the porous coating deviates from the above range to a certain extent within the error range, for example, even if the content of the inorganic particles is slightly less than 90% by weight or slightly more than 96% by weight, it still does not deviate from the spirit of the present disclosure.

[0059] The inorganic particles may be electrochemically stable. The inorganic particles are not particularly limited as long as they are within the operating voltage range of the electrochemical device (e.g., based on Li / Li + In particular, the use of inorganic particles with a high dielectric constant can help increase the dissociation of electrolyte salts (e.g., lithium salts) in liquid electrolytes, thereby improving the ionic conductivity of the electrolyte. For the above reasons, the inorganic particles may include high dielectric constant inorganic particles having a dielectric constant of about 5 or greater, such as about 10 or greater. Non-limiting examples of inorganic particles having a dielectric constant of 5 or greater include BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT,0 <x<1,0<y<1)、Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnium dioxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, Al(OH)3, SiC, AlOOH, TiO2, and mixtures thereof.

[0060] In addition, inorganic particles having lithium ion transfer capability (i.e., inorganic particles containing elemental lithium but not storing lithium and having the ability to transfer lithium ions) may be used as inorganic particles. Non-limiting examples of inorganic particles having lithium ion transfer capability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y(PO4)3, where 0 < x < 2 and 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, where 0 < x < 2, 0 < y < 1, and 0 < z < 3), (LiAlTiP) x O y series glasses (0 < x < 4, 0 < y < 13) such as 14Li2O - 9Al2O3 - 38TiO2 - 39P2O5, lithium lanthanum titanate (Li x La y TiO3, where 0 < x < 2 and 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , where 0 < x < 4, 0 < y < 1, 0 < z < 1, and 0 < w < 5) such as Li 3.25 Ge 0.25 P 0.75 S4, lithium nitride (Li x N y , where 0 < x < 4 and 0 < y < 2) such as Li3N, SiS2 series glasses (Li x Si y S z , where 0 < x < 3, 0 < y < 2, and 0 < z < 4) such as Li3PO4 - Li2S - SiS2, and P2S5 series glasses (Li x P y S z , where 0 < x < 3, 0 < y < 3, and 0 < z < 7) such as LiI - Li2S - P2S5, or a mixture of two or more of them.

[0061] In addition, inorganic particles with flame retardancy can be used to impart flame retardant properties to the separator or prevent a rapid increase in temperature inside the electrochemical element. Non - limiting examples of inorganic particles with flame retardancy include Sb2O3, Sb2O4, Sb2O5, SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, Zn2SnO4, ZnSnO3, ZnSn(OH)6, ZrO2, Y2O3, SiO2, Al2O3, AlOOH, Al(OH)3, SiC, TiO2, H3BO3, HBO2, and mixtures thereof.

[0062] The average particle size (D50) of the inorganic particles can be about 50nm or more and 5,000nm or less. For example, the average particle size (D50) of the inorganic particles can be about 100nm or more and 4,500nm or less, 200nm or more and 4,000nm or less, 300nm or more and 3,000nm or less, 400nm or more and 2,000nm or less, or 500nm or more and 1,000nm or less. When the average particle size of the inorganic particles is less than about 50nm, due to the increase in specific surface area, an additional polymer binder for bonding between the inorganic particles is required, which is disadvantageous in terms of resistance. When the average particle size of the inorganic particles exceeds 5,000nm, the uniformity of the surface of the coating may be reduced, and damage to the porous polymer substrate or the electrode may occur during lamination.

[0063] The aspect ratio of the inorganic particles can be about 1 or more and 2 or less. For example, the aspect ratio of the inorganic particles can be about 1.1 or more and 1.9 or less, 1.2 or more and 1.8 or less, 1.3 or more and 1.7 or less, or 1.4 or more and 1.6 or less. When the aspect ratio of the inorganic particles is adjusted within the above range, a porous coating can be formed that promotes the migration of the polymer binder via the pores between the inorganic particles and ultimately includes a gap volume that allows lithium ions to migrate.

[0064] The BET specific surface area of ​​the inorganic particles can be about 5 m 2 / g or more and 25m 2 / g or less. For example, the BET specific surface area of ​​the inorganic particles can be about 6m 2 / g or more and 24m 2 / g or less, 7m 2 / g or more and 23m 2 / g or less, 8m 2 / g or more and 22m 2 / g or less, 9m 2 / g or more and 21m 2 / g or less, 10m 2 / g or more and 20m 2 / g or less, 11m 2 / g or more and 19m 2 / g or less, 12m 2 / g or more and 18m 2 / g or less, 13m 2 / g or more and 17m 2 / g or less, or 14m 2 / g or more and 26m 2When the BET specific surface area of ​​the inorganic particles is adjusted within the above range, migration of the polymer binder through the pores between the inorganic particles can be controlled.

[0065] The permeability of the separator for electrochemical device can be about 50 seconds / 100cc or more and 150 seconds / 100cc or less. For example, the permeability of the separator can be about 60 seconds / 100cc or more and 140 seconds / 100cc or less, 70 seconds / 100cc or more and 130 seconds / 100cc or less, 80 seconds / 100cc or more and 120 seconds / 100cc or less, or 90 seconds / 100cc or more and 110 seconds / 100cc or less. For example, the permeability of the separator can be about 100 seconds / 100cc or more and 120 seconds / 100cc or less. When the permeability of the separator is within the above range, the output, stability and cycle characteristics of the electrochemical device can be ensured.

[0066] The thermal shrinkage of the separator for an electrochemical device may be about 10% or less. For example, the dry thermal shrinkage of the separator may be about 5% or less, and the wet thermal shrinkage may be 10% or less. For example, the dry thermal shrinkage may be a dimensional change rate based on exposure to 200°C for 30 minutes, and the wet thermal shrinkage may be a dimensional change rate based on exposure to 135°C for 30 minutes while the separator is immersed in an electrolyte solution. For example, the dry thermal shrinkage of the separator may be about 5% or less in both the MD direction and the TD direction, and the wet thermal shrinkage may be about 10% or less in both the MD direction and the TD direction.

[0067] When a battery is manufactured using a separator for an electrochemical device, the resistance of the battery may be about 0.5 ohms or more and 1.5 ohms or less. For example, the resistance of the battery may be about 0.6 ohms or more and 1.4 ohms or less, 0.7 ohms or more and 1.3 ohms or less, 0.8 ohms or more and 1.2 ohms or less, or 0.9 ohms or more and 1.1 ohms or less. For example, the resistance of the battery may be about 0.6 ohms or more and 0.8 ohms or less.

[0068] According to another embodiment of the present disclosure, the electrochemical device includes a positive electrode, a negative electrode and a separator between the positive electrode and the negative electrode, wherein the separator is the separator of the above embodiment. The electrochemical device can be manufactured by inserting an electrode assembly including a positive electrode, a negative electrode and a separator between the positive electrode and the negative electrode into a housing or a bag, and sealing the housing or the bag. Before the housing or the bag is sealed, the electrode assembly can be impregnated with an electrolyte solution by injecting an electrolyte solution. The shape of the housing or the bag is not limited. For example, the electrochemical device can be a cylindrical, prismatic, coin-shaped or pouch-shaped lithium secondary battery.

[0069] The positive electrode and the negative electrode can be coated by applying an electrode active material on at least one surface of each current collector and drying. The current collector can be a material having conductivity and not causing chemical changes in the electrochemical device. Examples of current collectors for the positive electrode include aluminum, nickel, titanium, fired carbon, and stainless steel; and aluminum or stainless steel subjected to surface treatment with carbon, nickel, titanium, or silver, but are not limited thereto. Examples of current collectors for the negative electrode include copper, nickel, titanium, fired carbon, and stainless steel; and copper or stainless steel subjected to surface treatment with carbon, nickel, titanium, or silver, but are not limited thereto. The current collector can be in various forms, such as thin metal plates, films, foils, meshes, porous materials, or foams.

[0070] The positive electrode includes a positive electrode current collector and a positive electrode active material layer containing a positive electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The positive electrode active material includes layered compounds such as lithium manganese composite oxides (e.g., LiMn2O4 and LiMnO2), lithium cobalt oxide (LiCoO2), and lithium nickel oxide (LiNiO2), or compounds substituted with one or more transition metal elements; lithium manganese oxides represented by the formula Li 1+x Mn 2-x O4 (where x is from 0 to 0.33), LiMnO3, LiMn2O3, or LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; Ni-site type lithium nickel oxides represented by the formula LiNi 1-x M x O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B, or Ga, and x = 0.01 to 0.3); lithium manganese composite oxides represented by the formula LiMn 1-x M x O2 (where M = Co, Ni, Fe, Cr, Zn, or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu, or Zn); LiMn2O4 in which some Li in the formula is replaced by alkaline earth metal ions; disulfide compounds; Fe2(MoO4)3, and these can be used alone or as a mixture of two or more of them.

[0071] The negative electrode includes a negative electrode current collector and a negative electrode active material layer containing a negative electrode active material, a conductive material, and a binder resin on at least one surface of the current collector. The negative electrode active material in the negative electrode includes carbon such as lithium metal oxides, hard carbon, and graphite carbon; silicon-based materials such as Li x Fe2O3 (0 ≤ x ≤ 1), Li x WO2 (0 ≤ x ≤ 1), Si, SiO x (0 < x < 2), SiC, and Si alloys; metal composite oxides such as Snx Me 1-x Me' y O z (Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of Group 1, Group 2 and Group 3 of the periodic table, halogens; 0 < x ≤ 1; 1 ≤ y ≤ 3; 1 ≤ z ≤ 8); lithium metal; lithium alloy; tin-based alloy; metal oxides such as SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4 and Bi2O5; conductive polymers such as polyacetylene; Li-Co-Ni-based materials; and titanium oxides, which may be used alone or in a mixture of two or more of them.

[0072] The conductive material may be any one of the conductive materials selected from the following or a mixture of two or more conductive materials: graphite, carbon black, carbon fiber or metal fiber, metal powder, conductive whisker, conductive metal oxide, carbon nanotube, activated carbon and polyphenylene derivative. The carbon nanotube has a cylindrical graphite sheet with a diameter of nanometer size and an sp 2 bonding structure, and exhibits conductor or semiconductor characteristics depending on the rolling angle and structure of the graphite sheet. The carbon nanotube can be classified into single-walled carbon nanotube (SWCNT), double-walled carbon nanotube (DWCNT) and multi-walled carbon nanotube (MWCNT) based on the number of bonds constituting its wall, and the carbon nanotube can be appropriately selected based on the application of the dispersion. For example, the conductive material may be one selected from the following: natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate and titanium oxide, or a mixture of two or more of them.

[0073] The binder resin that can be used herein can be any binder resin commonly used for the electrode of electrochemical device. Non-limiting examples of binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, poly(methyl methacrylate), poly(ethylhexyl acrylate), poly(butyl acrylate), polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan and carboxymethyl cellulose, but are not limited thereto.

[0074] The electrolyte can be prepared by making a + B - A salt of the structure of is obtained by dissolving or dissociating in an organic solvent, wherein A + Including alkali metal cations such as Li + 、Na + or K + , or a combination thereof, and B - Including anions such as PF6 - 、BF4 - , Cl - Br - ,I - 、ClO4 - 、AsF6 - 、CH3CO2 - CF3SO3 - 、N(CF3SO2)2 - or C(CF2SO2)3 - , or a combination thereof, the organic solvent being, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), γ-butyrolactone, or a mixture thereof.

[0075] For example, the electrolyte may include a solvent having a weight ratio of EC / EMC of about 3 / 7, or a solvent having a weight ratio of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) of about 20 / 5 / 75, which may maximize the dimensional stability of the separator according to the above embodiment.

[0076] The electrochemical device including the electrode assembly can be a lithium secondary (rechargeable) battery. The battery can be used as a unit cell, and can be used as a battery module including a unit cell, a battery pack including a battery module, and a device including a battery pack as a power source. Examples of the device include devices such as computers, mobile phones, and power tools; electric vehicles powered by electric motors, including electric vehicles (EV), hybrid electric vehicles (HEV), and plug-in hybrid electric vehicles (PHEV); electric two-wheeled vehicles, including electric bicycles (E-bike) and electric scooters (E-scooters); electric golf carts, etc.; and medium to large devices, such as power storage systems; and the like.

[0077] Another embodiment of the present invention provides a method for preparing a separator for an electrochemical device, the method comprising forming a porous coating layer comprising an acrylic acid-based binder, an acrylamide-based binder and inorganic particles on at least one surface of a porous polymer substrate. The contents overlapping with those described in the separator for an electrochemical device are replaced by the description of the aforementioned embodiment.

[0078] The step of forming the porous coating layer includes preparing a coating slurry comprising an acrylic acid-based binder and an acrylamide-based binder as polymer binders, inorganic particles, a dispersant, and a dispersion medium, applying the coating slurry to a porous polymer substrate, and then drying. For example, the coating slurry can be prepared by first mixing an acrylamide-based binder, inorganic particles, a dispersant, and a dispersion medium, and then adding an acrylic acid-based binder to prevent aggregation and precipitation of the acrylamide-based binder and the acrylic acid-based binder.

[0079] The step of forming the porous coating layer may further include subjecting at least one surface of the porous polymer substrate to a corona discharge treatment before applying the coating slurry to the porous polymer substrate. The step of subjecting at least one surface of the porous polymer substrate to a corona discharge treatment can prevent the bonding force between the porous polymer substrate surface and the coating surface from being reduced at high temperatures, and prevent the bonding force between the polymer substrate surface and the coating surface from being reduced due to the electrolyte.

[0080] At least one surface of the porous polymer substrate can be subjected to corona discharge treatment in air at a voltage of 0.1 kV or more and 10 kV or less. For example, the corona discharge treatment can be carried out at the following voltages: 0.2 kV or more and 9 kV or less, 0.3 kV or more and 8 kV or less, 0.4 kV or more and 7 kV or less, 0.5 kV or more and 6 kV or less, 0.6 kV or more and 5 kV or less, 0.7 kV or more and 4 kV or less, 0.8 kV or more and 3 kV or less, 0.9 kV or more and 2 kV or less, or 1.0 kV or more and 2 kV or less. For example, the corona discharge treatment can be carried out in air at a voltage of 1.8 kV. When the applied voltage of the corona discharge treatment is adjusted within the above range, a suitable number of functional groups can be formed on the surface of the polymer substrate, and the damage to the surface of the polymer substrate can be prevented.

[0081] The step of forming the porous coating layer may include applying the coating slurry to the porous polymer substrate to form the coating layer. For example, the coating layer may be formed by, but is not limited to, a rod coater, a wire rod coater, a roller coater, a spray coater, a spin coater, an inkjet coater, a screen coater, a reverse coater, a gravure coater, a knife coater, a slot die coater, a hot melt coater, a comma coater, and a direct metering coater. For example, the step of forming the coating layer may include using a rod coater or a slot die coater to simultaneously coat two surfaces of the porous polymer substrate with the coating slurry.

[0082] The step of forming a porous coating may include applying a coating slurry to a porous polymer substrate, followed by drying or heating the coating to evaporate the dispersion medium contained in the coating. The removal of the dispersion medium may be performed at a temperature that allows only the dispersion medium contained in the coating to evaporate without modifying the polymer binder contained in the coating. For example, the removal of the dispersion medium may be achieved by heating the coating to a predetermined temperature, but ensuring that the temperature of the coating surface does not exceed 60°C. When the coating is heated under the above conditions, the thermal energy may be first used to heat the dispersion medium and change the phase, and may not be used to modify the polymer binder.

[0083] Hereinafter, the present disclosure will be described in more detail with reference to specific embodiments and experimental examples. The following embodiments and experimental examples merely illustrate the present disclosure, and the present disclosure is not limited to the following embodiments and experimental examples.

[0084] Example 1

[0085] Preparation of coating slurry

[0086] In a 250 mL wide-mouth round bottle at room temperature (25°C), 5.4 g of an acrylamide-based binder (polyacrylamide, Mw: 900,000) (solid content 10%) and 30 g of Al2O3 as inorganic particles (particle size: 500 nm) were added to 67 mL of water, beads were further added, and the bottle was shaken to mix.

[0087] 2.1 g of an acrylic acid-based binder (polyacrylic acid, Mw: 350,000) (solid content 25%) and 1.1 g of a polyacrylic acid-based polymer dispersant (solid content 42%) were added to the bottle and stirred twice with a vibrator (a total of 2 hours), and then 0.2 g of a wetting agent (solid content 100%) was added and stirred with a vibrator for another 15 minutes to prepare a slurry.

[0088] The slurry was filtered to remove any lumps and a coating slurry having a solids content of 30% and a pH of 7.0 was prepared.

[0089] Preparation of porous polymer substrates

[0090] A polyethylene film having a size of 20 cm×30 cm and a thickness of 10 μm was used as the porous polymer substrate.

[0091] Preparation of separators

[0092] The coating slurry was coated on both surfaces of a polyethylene film using a bar coater to form a coating layer having a thickness of 1.5 μm.

[0093] The process of applying an air volume to the polyethylene film having the coating layer formed thereon and removing the dispersion medium was repeated five times to prepare a separator having a total thickness of 13 μm.

[0094] Comparative Example 1

[0095] A separator was prepared in the same manner as in Example 1, except that a polyacrylic acid-based polymer dispersant (solid content 25%) having a substitution degree different from that of the dispersant of Example 1 was used to adjust the pH of the coating slurry to 2.5 when preparing the coating slurry.

[0096] Example 2

[0097] A separator was prepared in the same manner as in Example 1, except that polyacrylamide (Mw: 400,000, solid content 15%) was used as an acrylamide-based binder when preparing the coating slurry.

[0098] Comparative Example 2

[0099] A separator was prepared in the same manner as in Example 1, except that polyacrylamide (Mw: 1,200,000, solid content 5%) was used as an acrylamide-based binder when preparing the coating slurry.

[0100] Example 3

[0101] A separator was prepared in the same manner as in Example 1, except that 3 g of polyacrylic acid (solid content 25%) and 0.32 g of polyacrylamide (solid content 10%) were used in preparing the coating slurry.

[0102] Example 4

[0103] A separator was prepared in the same manner as in Example 1, except that 1.3 g of polyacrylic acid (solid content 25%) and 7.6 g of polyacrylamide (solid content 10%) were used in preparing the coating slurry.

[0104] Comparative Example 3

[0105] A separator was prepared in the same manner as in Example 1, except that 4.3 g of polyacrylic acid (solid content 25%) was used and the acrylamide-based binder was not used when preparing the coating slurry.

[0106] Comparative Example 4

[0107] A separator was prepared in the same manner as in Example 1, except that, in preparing the coating slurry, 11 g of polyacrylamide (solid content 10%) was used and no acrylic-based binder was used.

[0108] Experimental Example 1. Determination of the characteristics of the separator according to the characteristics of the coating slurry

[0109] The properties of the separators prepared according to Example 1 and Comparative Example 1 were determined and shown in Table 1 below.

[0110] Determination of improvement in dry heat shrinkage

[0111] The separators of the embodiments and comparative examples were each prepared into a sample with a size of 5 cm×5 cm. After being stored in a convection oven at 200° C. for 30 minutes, the heat shrinkage in the machine direction (MD) and the transverse direction (TD) was calculated according to [(length of the initial sample-length after storage at 200° C. for 0.5 hours) / (length of the initial sample)]×100(%).

[0112] Determination of improvement in wet heat shrinkage

[0113] The separators of Examples and Comparative Examples were prepared into test pieces having a size of 5 cm×5 cm and inserted into an aluminum bag having a size of 7 cm×10 cm in size. The bag was filled with 1 g or less of an electrolyte solution and sealed.

[0114] Electrolyte 1 was used, which contained a solvent including a mixture of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) in a weight ratio of 3 / 7 and 2 wt % of vinylene carbonate (VC) and 1 M lithium salt LiPF6 as additives.

[0115] Electrolyte 2 was used, and the electrolyte 2 contained a solvent containing a mixture of ethylene carbonate (EC) / ethyl methyl carbonate (EMC) / dimethyl carbonate (DMC) in a weight ratio of about 20 / 5 / 75. After the sealed bag was stored in a convection oven at 135° C. for 30 minutes, the separator was taken out, and the heat shrinkage in the machine direction (MD) and the transverse direction (TD) was calculated according to [(length of the initial sample-length after storage at 135° C. for 0.5 hours) / (length of the initial sample)]×100(%).

[0116] [Table 1]

[0117]

[0118] Experimental Example 2. Determination of separator properties according to the molecular weight of acrylamide-based binder

[0119] Conditions for separators prepared according to Examples 1 to 2 and Comparative Example 2 were determined and properties of each separator were determined and shown in the following Table 2. The method for determining each property was the same as in the aforementioned Experimental Example.

[0120] [Table 2]

[0121]

[0122] Experimental Example 3. Determination of characteristics of separator according to weight ratio of acrylic acid-based binder and acrylamide-based binder

[0123] Conditions of the separators prepared according to Examples 1, 3 and 4 and Comparative Examples 3 and 4 were determined and the characteristics of each separator were determined and shown in the following Table 3. The method for determining each characteristic was the same as that of the aforementioned Experimental Examples.

[0124] [Table 3]

[0125]

[0126] From the foregoing, it will be understood that, for illustrative purposes, various embodiments of the present disclosure are described herein, and various modifications may be made without departing from the scope and spirit of the present disclosure. Therefore, the various embodiments disclosed herein are not intended to be limiting, with the true scope and spirit being indicated by the appended claims.

Claims

1. A separator for an electrochemical device, comprising: a porous polymer substrate; and forming a porous coating layer on at least one surface of the porous polymer substrate, wherein the porous coating comprises an acrylic acid-based binder, an acrylamide-based binder and inorganic particles, The porous coating layer comprises 90 wt % to 96 wt % of the inorganic particles based on the total weight of the porous coating layer, and A weight ratio of the acrylic-based binder to the acrylamide-based binder is 3:7 to 7:

3. 2 . The separator according to claim 1 , wherein the acrylamide-based binder has a weight average molecular weight of 400,000 to 1,000,000.

3. The separator according to claim 1, wherein the porous coating layer is formed by coating a coating slurry comprising the acrylic-based binder, the acrylamide-based binder, the inorganic particles, a dispersant, and a dispersion medium on the porous polymer substrate, and The pH of the coating slurry is 3 to 9. The separator according to claim 1 , wherein the acrylic-based binder comprises a repeating unit containing one or more monomers selected from acrylic acid and methacrylic acid.

5. The separator according to claim 1, wherein the acrylamide-based binder comprises repeating units containing one or more monomers selected from the group consisting of acrylamide, methacrylamide, N-ethylacrylamide, ethylmethacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-butylacrylamide, and N-butylmethacrylamide. 6 . The separator according to claim 1 , wherein a content of the acrylic-based binder in the porous coating layer is greater than or equal to a content of the acrylamide-based binder.

7. An electrochemical device comprising: positive electrode; negative electrode; and A separator disposed between the positive electrode and the negative electrode, wherein the separator comprises a porous polymer substrate and a porous coating layer formed on at least one surface of the porous polymer substrate, The porous coating layer comprises an acrylic acid-based binder, an acrylamide-based binder and inorganic particles, The porous coating layer comprises 90 wt % to 96 wt % of the inorganic particles based on the total weight of the porous coating layer, and A weight ratio of the acrylic-based binder to the acrylamide-based binder is 3:7 to 7:

3.

8. The electrochemical device according to claim 7, further comprising: An electrolyte comprising a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) are mixed at a weight ratio of 3:7, or a solvent in which ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) are mixed at a weight ratio of 20:5:

75. 9 . The electrochemical device according to claim 7 , wherein the acrylamide-based binder has a weight average molecular weight of 400,000 to 1,000,000.

10. The electrochemical device according to claim 7, wherein the porous coating layer is formed by coating a coating slurry comprising the acrylic-based binder, the acrylamide-based binder, the inorganic particles, a dispersant, and a dispersion medium on the porous polymer substrate, and The pH of the coating slurry is 3 to 9. 11 . The electrochemical device according to claim 7 , wherein the acrylic-based binder comprises a repeating unit containing one or more monomers selected from acrylic acid and methacrylic acid.

12. The electrochemical device of claim 7, wherein the acrylamide-based binder comprises repeating units containing one or more monomers selected from the group consisting of acrylamide, methacrylamide, N-ethylacrylamide, ethylmethacrylamide, N-propylacrylamide, N-isopropylacrylamide, N-isopropylmethacrylamide, N-butylacrylamide, and N-butylmethacrylamide. 13 . The electrochemical device according to claim 7 , wherein a content of the acrylic acid-based binder in the porous coating layer is greater than or equal to a content of the acrylamide-based binder.

Citation Information

Cited By

  • High-temperature-resistant diaphragm for lithium battery as well as preparation method and application of high-temperature-resistant diaphragm

    CN119921053A