Polyolefin Filament
A polyolefin composition of propylene and butene-1 polymers with specific properties enhances the balance of toughness and elongation in filaments, addressing the limitations of existing technologies for applications like ropes and brushes.
Patent Information
- Application Number
- JP2024532985
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-10
- Filing Date
- 2022-12-05
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyolefin filaments struggle to achieve a balance between toughness and elongation, which is desirable for applications such as ropes, nets, and brushes.
A polyolefin composition comprising 80-95% propylene polymer and 5-20% butene-1 polymer, with specific properties like flexural modulus, melt flow index, and xylene solubility, is used to produce filaments with enhanced elongation at break and reduced stretching ratio.
The filaments exhibit an elongation at break of 90% or more and a stretching ratio of 75 or less, providing improved toughness and elongation, making them suitable for nets, ropes, and brushes.
Smart Images

Figure 2024543592000001 
Figure 2024543592000002 
Figure 2024543592000003
Abstract
Description
[Technical Field]
[0001] The present disclosure relates to polyolefin filaments. [Background technology]
[0002] The term "filament" is commonly used to distinguish fibers in textile and carpet applications.
[0003] Thus, the filaments of the present invention are preferably characterized by a titer of at least 500 denier (hereinafter "den").
[0004] Typical applications for this filament are ropes and yarns for netting, geotextiles and protective netting in the agricultural and building industries.
[0005] According to WO2012049132, filaments, monotapes or drawn tapes with good mechanical properties are obtained from a composition comprising a propylene polymer and up to 95% by weight of a butene-1 polymer. Summary of the Invention [Problem to be solved by the invention]
[0006] However, in many finished products, an improved balance of toughness and elongation is desirable. It has been found that such a goal can be achieved by producing filaments from a polyolefin composition that combines polypropylene with a specific butene-1 polymer.
[0007] Therefore, the present disclosure provides a drawn polyolefin filament comprising a polyolefin composition having an elongation at break EB of 90% or more, preferably 110% or more, more preferably 130% or more, and particularly 90% to 190%, preferably 110% to 190%, more preferably 130% to 185%, and an SR / EB (SR is the draw ratio) of 75 or less, preferably 70 or less, with the lower limit being preferably 30, more preferably 40 in all cases, hereinafter referred to as "polyolefin composition (I)". A) 80 to 95% by weight, preferably 80 to 90% by weight, of a propylene polymer; B) 5 to 20% by weight, preferably 10 to 20% by weight, of a butene-1 polymer having the following characteristics: 1) The flexural modulus is 100 to 800 MPa, preferably 250 to 600 MPa, and more preferably 300 to 600 MPa; 2) Specific MI 10 / MI2 is 20 to 40, preferably 25 to 35, and MI 10 is the melt flow index MI at 190°C and a load of 10 kg, and MI2 is the melt flow index MI at 190°C and a load of 2.16 kg, both measured in accordance with ISO 1133-1:2011. 3) the content of xylene soluble fraction at 0°C based on the total weight of B) is 15% by weight or less, preferably 10% by weight or less, the preferred lower limit being 0.5% by weight in all cases; (2) The amounts of A) and B) refer to the total weight of A) + B), the elongation at break is measured on one filament 7 days after production using a dynamometer with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min, and the flexural modulus is measured 10 days after molding in accordance with standard ISO 178:2010.
[0008] The balance of tenacity and elongation makes the filaments of the present invention particularly useful in the manufacture of nets, ropes and brushes. DETAILED DESCRIPTION OF THE INVENTION
[0009] The polyolefin filaments of the invention preferably have the following additional characteristics, measured on a single filament 7 days after production using a dynamometer with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min: a toughness of at least 1.9, more preferably at least 1.95, in particular between 1.9 and 2.2; and / or -The breaking load must be between 2.5 and 4.5 kg.
[0010] As used herein, the expression "propylene polymer" includes polymers selected from propylene homopolymers, propylene copolymers, especially random copolymers, and mixtures thereof.
[0011] Similarly, as used herein, the expression "butene-1 polymer" includes polymers selected from butene-1 homopolymers, butene-1 copolymers, and mixtures thereof.
[0012] In the polyolefin composition of the present invention, when A) consists of or comprises one or more propylene copolymers, such copolymers may also comprise one or more comonomers, preferably selected from ethylene and CH2=CHR alpha-olefins, where R is a C2-C8 alkyl radical, in particular butene-1, pentene-1, 4-methyl-pentene-1, hexene-1 and octene-1.
[0013] Ethylene, butene-1 and hexene-1 are preferred.
[0014] When B) consists of or comprises one or more butene-1 copolymers, such copolymers may comprise one or more comonomers preferably selected from ethylene, propylene and CH═CHR alpha-olefins, where R is a C-C alkyl radical, in particular pentene-1, 4-methyl-pentene-1, hexene-1 and octene-1. Ethylene, propylene and hexene-1 are preferred. From the above definitions it is clear that the term "copolymer" includes polymers containing two or more types of comonomers.
[0015] In one embodiment, the propylene polymer component A) may have at least one of the following additional features:
[0016] the comonomer content (A) is between 0.5 and 15% by weight, more preferably between 1 and 12% by weight, in the case of copolymers, and in particular between 0.5 and 6% by weight, in the case where the comonomer is ethylene or hexene-1;
[0017] MIL is 0.1 to 400 g / 10 min, in particular 0.5 to 150 g / 10 min or 0.5 to 100 g / 10 min, MIL being the melt flow index at 230 °C and a load of 2.16 kg, measured in accordance with ISO 1133-2:2011;
[0018] The amount of insoluble fraction in xylene at -25°C is 85% by weight or more, more preferably 90% by weight or more, and in particular for propylene homopolymers 95% by weight or more, with an upper limit preferably being 99% for all homopolymers and 96% for all copolymers.
[0019] the flexural modulus is higher than 200 MPa, more preferably higher than 400 MPa, the upper limit being preferably 2000 MPa in all cases.
[0020] Both the propylene homopolymers and propylene copolymers are known in the art and commercially available.
[0021] Examples of commercially available propylene homopolymers and copolymers are the polymer products sold under the trademark Moplen by LyondellBasell Industries.
[0022] They can be produced by using Ziegler-Natta catalysts or metallocene-based catalyst systems in the polymerization process.
[0023] Typically, Ziegler-Natta catalysts comprise the reaction product of an organometallic compound from Groups 1, 2, or 13 of the Periodic Table of the Elements with a transition metal compound from Groups 4 to 10 of the Periodic Table of the Elements (new notation). In particular, the transition metal compound can be selected from compounds of Ti, V, Zr, Cr, and Hf, preferably supported on MgCl2.
[0024] Particularly preferred catalysts comprise the reaction product of said organometallic compound of Group 1, 2 or 13 of the Periodic Table of the Elements with a solid catalyst component comprising a Ti compound and an electron donor compound supported on MgCl2.
[0025] Preferred organometallic compounds are aluminum alkyl compounds.
[0026] Thus, preferred Ziegler-Natta catalysts are those comprising the reaction product of: 1) a solid catalyst component comprising a Ti compound, preferably a halogenated Ti compound, in particular TiCl4, and an electron donor (internal electron donor) supported on MgCl2; 2) an aluminum alkyl compound (cocatalyst), and optionally, 3) Electron donor compounds (external electron donors).
[0027] The solid catalyst component (1) contains as electron donors compounds generally chosen from ethers, ketones, lactones, compounds containing N, P and / or S atoms, and mono- and dicarboxylic acid esters.
[0028] Catalysts having the above properties are well known in the patent literature. Particularly advantageous are the catalysts described in US Pat. No. 4,399,054 and EP 45977.
[0029] Among the internal electron donor compounds, phthalic acid esters, preferably diisobutyl phthalate, and succinic acid esters are particularly suitable.
[0030] Other internal electron donors are particularly suitable, such as 1,3-diethers, as set out in published European patent applications EP-A-361 493 and 728769.
[0031] As cocatalyst (2), it is preferred to use trialkylaluminum compounds such as Al-triethyl, Al-triisobutyl and Al-tri-n-butyl.
[0032] Electron donor compounds (3) that can be used as external electron donors include aromatic acid esters (such as alkyl benzoates), heterocyclic compounds (such as 2,2,6,6-tetramethylpiperidine and 2,6-diisopropylpiperidine), and especially silicon compounds containing at least one Si—OR bond (where R is a hydrocarbon radical).
[0033] Useful silicon compounds include (tert-butyl)2Si(OCH3)2, (cyclohexyl)(methyl)Si(OCH3)2, (phenyl)2Si(OCH3)2, and (cyclopentyl)2Si(OCH3)2.
[0034] The above 1,3 diethers are also suitable as external electron donors. When the internal electron donor is one of the above 1,3-diethers, the external electron donor can be omitted.
[0035] By preliminarily contacting the catalyst with a small amount of olefin (prepolymerization), maintaining it in suspension in a hydrocarbon solvent, and polymerizing it at a temperature of room temperature to 60°C, it is possible to produce a polymerization amount of 0.5 to 3 times the weight of the catalyst.
[0036] This operation can also be carried out in liquid monomer, producing polymer in amounts up to 1000 times the weight of the catalyst.
[0037] Preferred examples of metallocene-based catalyst systems are disclosed in US Pat. No. 20060020096 and WO 98040419.
[0038] The polymerization conditions used with the above catalysts are also generally well known.
[0039] The polymerization can be carried out in one stage or in two or more stages under different polymerization conditions.
[0040] It can occur in the liquid phase (e.g., using liquid propylene as a diluent), the gas phase, or the liquid-gas phase
[0041] Conventional molecular weight regulators known in the art, such as chain transfer agents (e.g., hydrogen or ZnEt2), can be used.
[0042] The polymerization temperature is preferably 40 to 120°C, and more preferably 50 to 80°C.
[0043] The polymerization pressure may be atmospheric or higher.
[0044] When polymerizing in liquid propylene, the pressure is competitive with the vapor pressure of liquid propylene at the operating temperature used, and may be modified by the vapor pressure of small amounts of inert diluent used to provide the catalyst mixture, any monomer overpressure, and hydrogen used as a molecular weight regulator.
[0045] In particular, the propylene polymer A) can be produced by a polymerization process carried out in a gas-phase polymerization reactor comprising at least two interconnected polymerization zones, as shown in European Patent Application No. 782587.
[0046] In particular, the process is carried out in first and second interconnected polymerization zones, into which propylene and optional comonomers are fed in the presence of a catalyst system and from which the polymer produced is discharged. In the process, growing polymer particles flow upward under fast fluidization conditions through one of the polymerization zones (the riser), exit the riser into another (second) polymerization zone (the downcomer), through which they flow downward in dense form, leave the downcomer under the action of gravity, and are reintroduced into the riser, thus establishing a polymer circulation between the riser and the downcomer.
[0047] In the downcomer, the density of the solids reaches a high value, approaching the bulk density of the polymer. A positive pressure increase is thus achieved in the direction of flow, allowing the polymer to be reintroduced into the riser without the aid of special mechanical means. In this way, a "loop" circulation is established, which depends on the pressure balance between the two polymerization zones and the head loss introduced into the system.
[0048] Generally, high-speed fluidization conditions in the riser are established by feeding a gas mixture containing the relevant monomers into the riser. The gas mixture is preferably fed below the point of reintroduction of the polymer into the riser, if necessary by using a gas distribution means. The velocity of the transport gas into the riser is higher than the transport velocity under operating conditions, preferably 2 to 15 m / s.
[0049] Typically, the polymer and gas mixture leaving the riser is conveyed to a solid / gas separation zone. Solid / gas separation can be accomplished using conventional separation means. From the separation zone, the polymer enters the downcomer. The gaseous mixture leaving the separation zone is compressed, cooled, and transferred to the riser, optionally with the addition of make-up monomer and / or molecular weight regulator. Transfer can be accomplished using a gaseous mixture recycle line.
[0050] Control of polymer circulation between the two polymerization zones can be achieved by metering the amount of polymer exiting the downcomer using any suitable means for controlling the flow of solids, such as a mechanical valve.
[0051] The process can be carried out under an operating pressure of 0.5 to 10 MPa, preferably 1.5 to 6 MPa.
[0052] Optionally, an inert gas such as nitrogen or an aliphatic hydrocarbon may be maintained in the polymerization zone in an amount such that the sum of the partial pressures of the inert gas is preferably 5 to 80% of the total pressure of the gas.
[0053] The catalyst can be fed to the riser at any point in the riser. However, it can also be fed at any point in the downcomer. The catalyst can be in any physical state, so that either solid or liquid catalyst can be used.
[0054] The butene-1 polymers component B) are known to those skilled in the art and are commercially available, as shown in the examples.
[0055] The butene-1 polymer component B) is preferably a highly isotactic linear polymer.
[0056] In particular, the butene-1 polymer component B) operates at 150.91 MHz 13 It has an isotacticity of 90 to 99%, more preferably 93 to 99%, and most preferably 95 to 99%, as measured by C-NMR as mmmm pentads / total pentads or as the amount by weight of xylene insolubles at 0°C.
[0057] The butene-1 polymer component B) preferably has an MI2 value of 0.05 to 50 g / 10 min, more preferably 0.1 to 10 g / 10 min.
[0058] Butene-1 polymer component B) MI 10The value is preferably 1 to 100 g / 10 minutes, more preferably 2 to 50 g / 10 minutes.
[0059] In one embodiment, the butene-1 polymer component B) may be a homopolymer.
[0060] In a further embodiment, the butene-1 polymer B) may be a copolymer having a comonomer content, in particular a copolymerized ethylene content, of 0.5 to 10 mol %, preferably 0.7 to 9 mol %.
[0061] In a further embodiment, the butene-1 polymer component B) may be a butene-1 polymer composition comprising: B1) butene-1 homopolymers or copolymers of butene-1 with at least one comonomer selected from ethylene, propylene, CH═CHR olefins as defined above and mixtures thereof, the copolymerized comonomer content being less than or equal to 2 mol %; B2) copolymers of butene-1 with at least one comonomer selected from ethylene, propylene, the CH═CHR olefins defined above and mixtures thereof, having a copolymerized comonomer content of 3 to 25 mol %, The composition has a total copolymerizable comonomer content, as the sum of B1)+B2), of 0.5 to 18 mol %, preferably 0.7 to 15 mol %.
[0062] The relative amounts of B1) and B2) may range from 10% to 50% by weight of B1), in particular from 15% to 45% by weight, and from 90% to 50% by weight, in particular from 85% to 55% by weight, said amounts referring to the sum of B1)+B2).
[0063] In one embodiment, the butene-1 polymer component B) may have at least one of the following additional characteristics: Mw is the weight-average molar mass as measured by gel permeation chromatography, Mn is the number-average molar mass as measured by gel permeation chromatography, and the molecular weight distribution Mw / Mn is greater than or equal to 4, preferably greater than or equal to 5, with an upper limit of preferably 10; the melting point TmII, measured by DSC (differential scanning calorimetry) in a second heating run at a scanning rate of 10°C / min, is not more than 125°C, preferably not more than 120°C, the lower limit being preferably in all cases 75°C; -X-ray crystallinity is 25-65%.
[0064] Optionally, the butene-1 polymer component B) may have at least one of the following further additional characteristics: an intrinsic viscosity (IV) measured in tetrahydronaphthalene (THN) at -135°C of not more than 5 dL / g, preferably not more than 3 dL / g, the lower limit being preferably 0.4 dL / g in all cases; ii) Mw is 100,000 g / mol or more, in particular 100,000 to 650,000 g / mol; - the melting point Tml measured by DSC at a scanning rate of 10°C / min is 95°C to 135°C; -Density: 885-925kg / m 3 , preferably 900 to 920 kg / m 3 , especially 912-920 kg / m 3 That is.
[0065] The butene-1 polymer component B) can be obtained using known processes and polymerization catalysts.
[0066] For example, to prepare butene-1 polymer component B), TiCl3-based Ziegler-Natta catalysts and aluminum derivatives such as aluminum halides as cocatalysts, as well as the above-mentioned MgCl2-supported catalyst systems, can be used.
[0067] When using the above supported catalyst systems, other examples of internal electron donor compounds include 3,3-dimethyldiethyl or diisobutyl glutarate.
[0068] Preferred examples of external electron donor compounds are cyclohexyltrimethoxysilane, t-butyltrimethoxysilane, diisopropyltrimethoxysilane and thexyltrimethoxysilane. Particularly preferably, hexyltrimethoxysilane is used.
[0069] Alternatively, the butene-1 polymer component B) can be obtained by polymerizing the monomers in the presence of a metallocene catalyst system obtained by contacting: stereorigid metallocene compounds, alumoxanes or compounds capable of forming alkylmetallocene cations, and optionally -organoaluminum compounds.
[0070] The polymerization process can be carried out with said catalyst in the liquid phase, optionally in the presence of an inert hydrocarbon solvent, or in the gas phase, using a fluidized bed or by operating a mechanically stirred gas phase reactor.
[0071] The hydrocarbon solvent may be either aromatic (such as toluene) or aliphatic (such as propane, hexane, heptane, isobutane, cyclohexane, and 2,2,4-trimethylpentane, isododecane, etc.).
[0072] Preferably, the polymerization process is carried out by using liquid butene-1 as the polymerization medium.
[0073] The polymerization temperature may be between 20°C and 150°C, particularly between 50°C and 90°C, for example between 65°C and 82°C.
[0074] To control the molecular weight, molecular weight regulators, especially hydrogen, are provided to the polymerization environment.
[0075] Mw / Mn values of 4 or greater and MI as previously defined10 / MI2 ratio の値は Generally, it is believed that the molecular weight distribution (MWD) will be broad.
[0076] Broad molecular weight butene-1 polymers can be obtained in several ways. One way is to use a catalyst capable of producing substantially broad MWD polymers when (co)polymerizing butene-1. Another possibility is to mechanically blend butene-1 polymers with sufficiently different molecular weights using conventional mixing equipment.
[0077] It is also possible to carry out a multi-stage polymerization process in which butene-1 polymers of different molecular weights are produced sequentially in two or more reactors under different reaction conditions, such as the concentration of molecular weight regulator fed to each reactor.
[0078] It is also possible to feed different amounts of monomer to each reactor.
[0079] In particular, when the butene-1 polymer component B) contains the two components B1) and B2) described above, the polymerization process can be carried out in two or more reactors connected in series, with components B1) and B2) being prepared separately in subsequent stages, each stage, except the first, operating in the presence of the polymer formed and the catalyst used in the previous stage.
[0080] The catalyst may be added to only the first reactor, or may be added to multiple reactors.
[0081] The above polymer components can achieve high MI values directly during polymerization, or by subsequent chemical treatment (chemical visbreaking).
[0082] Chemical visbreaking of polymers is carried out in the presence of a free radical initiator such as a peroxide.
[0083] The peroxides most conveniently used in polymer visbreaking processes preferably have a decomposition temperature in the range of 150° C. to 250° C. Commercially available peroxides include, for example, dibutyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne, and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane.
[0084] The amount of peroxide required for the visbreaking process is preferably in the range of 0.001 to 0.5% by weight of the polymer, more preferably 0.001 to 0.2%.
[0085] The polyolefin composition (I) is obtained by melt-mixing the components, and the mixing temperature in the mixer is usually 180 to 310°C, preferably 190 to 280°C, and more preferably 200 to 250°C.
[0086] All known devices and techniques can be used for this purpose.
[0087] Useful melt mixing devices in this context are in particular extruders or kneaders, with twin-screw extruders being particularly preferred. It is also possible to premix the components at room temperature in a mixing device and then feed the mixture thus obtained directly into the device used to produce the filaments.
[0088] During the preparation of the polyolefin composition (I), in addition to the main components A) and B) and other optional components, additives commonly used in the art, such as stabilizers (against heat, light, and UV rays), plasticizers, acid inhibitors, antistatic agents, water repellents, and pigments, may also be introduced.
[0089] The filaments of the present invention comprise at least 70% by weight of polyolefin composition (I), more preferably at least 80% by weight, especially at least 90% or 95% by weight of polyolefin composition (I), relative to the total weight of the filament or fiber, the upper limit being in all cases 100% by weight.
[0090] The filaments of the present invention are typically characterized by a cross-section that is rounded (circular, elliptical, lenticular, or more complex such as multilobal) or angular, such as rectangular.
[0091] A filament having a rounded cross section is also called a "monofilament," and a filament having an angular, especially rectangular, cross section is also called a "tape." Therefore, the definition of "filament" in the present invention includes said monofilaments and tapes.
[0092] The thickness of the tape is preferably 0.03 to 1 mm, and the width is preferably 2 to 20 mm.
[0093] As mentioned above, the filaments are preferably characterized by a titer of 500 den or greater.
[0094] The titer of the filament is particularly preferably 800 den or more, especially 1000 or 1300 or more, with the upper limit being preferably 7000 den for monofilaments and 25000 den for tapes.
[0095] As described above, the filaments are drawn, and it is particularly preferable that the draw ratio is 3:1 to 4.5:1.
[0096] All of the filaments can be used in bundle or reel form for the production of a variety of finished products.
[0097] The polyolefin filaments or fibers of the present invention can be produced using processes and equipment well known in the relevant art.
[0098] Generally, the process for producing polyolefin filaments includes the following steps: (a) Melting the polyolefin composition (I) and other polymeric components, if present. (b) Spinning filaments or extruding precursor films or tapes. (c) stretching the filaments or precursor film or tape if not previously stretched, and / or cutting the precursor film or tape and stretching the resulting filaments.
[0099] The melting step (a) and the spinning or extrusion step (b) are generally carried out continuously in succession by using a single-screw or twin-screw extruder equipped with an appropriate spinning or extrusion head. Thus, the aforementioned melt mixing step can also be carried out in the same spinning or extrusion device.
[0100] The spinning head is equipped with a number of holes that have the same shape as the cross section of the filament (monofilament or tape).
[0101] A film extrusion head is typically a flat or annular die commonly used in the production of film.
[0102] If a precursor film or tape is obtained in step (b), it is cut into tapes of the desired size in step (c) and processed. If the precursor film or tape is subjected to a drawing process, the final filament does not need to be subjected to a drawing process.
[0103] The melting step (a) and the spinning / extrusion step (b) are usually carried out at a temperature predetermined in the melt mixing step, ie, 180 to 310°C, preferably 190 to 280°C, more preferably 200 to 250°C.
[0104] Typical spinning conditions are as follows: -The temperature inside the extruder head is 200-300°C. - The winding speed of the primary web (unstretched) is 1 to 50 m / min.
[0105] The film extrusion conditions were as follows: -The temperature inside the extruder head is 200-300°C. - Output value is 20-1000 kg / hour (for industrial plants).
[0106] The filaments or precursor film obtained in step (b) are typically cooled, for example using one or more chill rolls or by immersion in water at a temperature between 5 and 40°C.
[0107] To perform the drawing process, the filament (monofilament or tape) or precursor tape is preheated to a temperature of 40° C. to 120° C. to 140° C. Heating can be achieved, for example, by using a hot air oven, a boiling water bath, a heated roll, or by irradiation or other known means.
[0108] Drawing can be achieved by passing the precursor tape or filament through a series of rollers having different rotational speeds, and the preferred range of draw ratios thus achieved is a predefined range.
[0109] The draw ratio is the ratio of the fast speed of the rollers in the drawing unit to the speed of the rollers in the take-off unit (primary speed). As mentioned above, in the take-off unit, the slow moving tape or filament is heated before being drawn at a faster speed. Thus, dividing the value of such ratio, eg, 3 for 3:1, 4.5 for 4.5:1, by the elongation at break gives the SR / EB value. Example
[0110] Examples and advantages of the various embodiments, compositions, and methods provided herein are disclosed in the following examples, which are merely illustrative and are not intended to limit the scope of the appended claims in any way.
[0111] The following analytical methods are used to evaluate the polymer composition and filament properties.
[0112] density
[0113] Measured at 23°C according to ISO 1183-1:2012.
[0114] Melt Flow Index
[0115] Measured at 190°C and a specified load in accordance with ISO 1133-12012-03.
[0116] Intrinsic viscosity (IV)
[0117] The sample was dissolved in tetrahydronaphthalene at 135°C and then injected into a capillary viscometer. The viscometer tube (Ubbelohde type) was surrounded by a cylindrical glass jacket, which allowed for temperature control by a circulating thermostatically controlled liquid. The time it took to pass down the meniscus was measured by an optoelectronic device.
[0118] When the meniscus passes in front of the upper ramp, a counter with a quartz oscillator is started. When the meniscus passes the lower ramp, the counter is stopped and the flow time is recorded. This is converted to intrinsic viscosity using Huggins' equation (Huggins, M.L., J. Am. Chem. Soc., 1942, 64, 2716; Chem. Soc., 1942, 64, 2716), provided that the flow time of the pure solvent under the same experimental conditions (same viscometer and same temperature) is known. [η] was measured using a single polymer solution.
[0119] Molecular weight distribution measurement
[0120] Molar mass distributions and the resulting average Mn, Mw, Mz, and Mw / Mn were determined using a PolymerChar GPC-IR instrument. The instrument was equipped with a column set consisting of four PLgel Olexis mixed-bed columns (Polymer Laboratories) and an IR5 infrared detector (PolymerChar). The column dimensions were 300 x 7.5 mm, with a particle size of 13 μm. The mobile phase flow rate was maintained at 1.0 mL / min. All measurements were performed at 150 °C. The solution concentration was 2.0 mg / mL (at 150 °C), and 0.3 g / L of 2,6-ditert-butyl-p-cresol was added to prevent decomposition. A universal calibration curve was obtained for GPC calculations using 12 polystyrene (PS) standard samples (peak molecular weight range 266–1,220,000) provided by PolymerChar. A third-order polynomial fit was used to interpolate the experimental data and obtain the relevant calibration curve. Data acquisition and processing were performed using Empower 3 (Waters). The Mark-Houwink relationship was used to determine the molecular weight distribution and associated average molecular weight. K values were calculated as K for PS and polybutene (PB), respectively. PS =1.21×10 -4 dL / g and K PB =1.78×10 -4 dL / g, while for PS (0.706) and for PB (0.725) Mark-Houwink indexes were used.
[0121] In the case of butene / ethylene copolymers, as far as data evaluation is concerned, for each sample the composition was assumed to be constant over the entire range of molecular weights, and the K values of the Mark-Houwink relationship were calculated using linear combinations as reported below.
[0122]
number
[0123] where K EB is the copolymer constant. K PE (4.06×10 -4 , dL / g) and KPB (1.78×10 -4 dL / g) is a constant for polyethylene (PE) and PB. x E and x B is the relative weight amount of ethylene and butene, and x E +x B = 1. The Mark-Howink exponent α = 0.725 was used for all butene / ethylene copolymers, independent of their composition. Final processing data processing was modified for all samples to include fractions up to 1000 in terms of molecular weight equivalent. Fractions below 1000 were examined via GC.
[0124] Comonomer Content
[0125] Propylene Polymer A)
[0126] For propylene copolymers, the comonomer content was determined by infrared spectroscopy by collecting IR spectra of the sample and air background using a Fourier transform infrared spectrometer (FTIR). The instrument data collection parameters were as follows: -Purge time: minimum 30 seconds. -Collection time: Minimum 3 minutes. -Apodization: Happ-Genzel. -Resolution: 2cm -1 .
[0127] Sample Production
[0128] A thick sheet was obtained by pressing approximately 1 g of sample between two sheets of aluminum foil using a hydraulic press. If uniformity is an issue, a minimum of two pressing operations is suggested. A small portion was cut from this sheet to form a membrane. The recommended film thickness range is 0.02–0.05 cm (8–20 mils).
[0129] Press temperature: 180±10℃ (356℃), approximately 10kg / cm 2(142.2 PSI) pressure was applied for approximately 1 minute. The pressure was then released and the sample was removed from the press and allowed to cool to room temperature.
[0130] Spectra of pressed films of the polymer were recorded as absorbance versus wavenumber (cm -1 The following measurements were used to calculate the ethylene and butene-1 content: - 4482~3950cm, used for spectroscopic normalization of film thickness -1 Area of the combined absorption band (At). -750-700 cm after appropriate successive spectroscopic subtraction of the spectrum of isotactic unadditive polypropylene in the presence of ethylene. -1 and, in the presence of butene-1, the area of the absorption band between 800 and 690 cm -1 Reference spectra of butene-1-propylene random copolymers in the range of In the presence of -butene-1, the spectrum of isotactic unadditive polypropylene is at 769 cm after appropriate spectral subtraction of two successive spectra. -1 (maximum) of the absorption band height (DC4), and in the presence of ethylene, 800–690 cm -1 Reference spectra of ethylene-propylene random copolymers in the range of
[0131] To calculate the ethylene and butene-1 content, calibration lines for ethylene and butene-1 are required, obtained using samples of known amounts of ethylene and butene-1.
[0132] Butene-1 Polymer B)
[0133] The comonomer content of the butene-1 polymer was measured via FT-IR.
[0134] Spectrum of pressed polymer films (cm -1 ) was recorded as absorbance versus wavenumber. The following measurements were used to calculate the ethylene content: a) 4482–3950 cm, used for spectroscopic normalization of film thickness-1 The area of the combined absorption band (A t ), b) The spectrum of the polymer sample and the subtraction coefficient (FCR) of the digital subtraction between the absorption bands due to the arrangement of methylene groups (CH2 locking) BEE and BEB (B: butene unit, E: ethylene unit). C2 )vibration) c) Area of the remaining band after subtracting the C2PB spectrum (A C2,block)。 It is derived from the arrangement of methylene groups EEE (CH2 rocking vibration).
[0135] Device
[0136] A Fourier transform infrared spectrometer (FTIR) can be used to perform the spectroscopic measurements reported above.
[0137] A hydraulic press (Carver or equivalent) with platens heatable to 200°C is used.
[0138] method
[0139] (BEB+BEE) sequence calibration
[0140] %(BEB+BEE)wt vs. FCR C2 / A t The calibration line is obtained by plotting the slope G r and intercept I r is calculated by linear regression.
[0141] EEE sequence calibration
[0142] %(EEE)wt vs. A C2、ブロック / A t The calibration line is obtained by plotting the slope G H and intercept I H is calculated by linear regression.
[0143] Sample preparation
[0144] A thick sheet was obtained by pressing approximately 1.5 g of sample between two sheets of aluminum foil using a hydraulic press. If uniformity is an issue, it is recommended to perform at least two pressing operations. A small portion of this sheet was cut out to form a membrane. The recommended membrane thickness is 0.1 to 0.3 mm.
[0145] The press temperature is 140°C (10°C).
[0146] Because the change in crystalline phase occurs over time, it is suggested to collect IR spectra of sample films immediately after casting.
[0147] procedure
[0148] The data collection parameters of the instrument are as follows: Purge time: 30 seconds minimum. Collection time: Minimum 3 minutes. Apodization: Happ-Genzel. Resolution: 2cm -1 . IR spectra of the samples were collected against an air background.
[0149] calculation The weight concentration of the BEE+BEB sequence of ethylene units was calculated.
number
number
[0150]
number
[0151] X-ray crystallinity determination
[0152] X-ray crystallinity was measured using an X-ray powder diffraction analyzer (XDPD) capable of collecting spectra between diffraction angles 2θ = 5° and 2θ = 35° every 6 seconds with a step size of 0.1° using Cu-Kα1 radiation with a fixed slit.
[0153] The samples were press-molded diskettes with thicknesses of approximately 1.5-2.5 mm and diameters of 2.5-4.0 cm. The diskettes were aged at room temperature (23°C) for 96 hours.
[0154] After this preparation, the specimen was inserted into the XRPD sample holder. XRPD spectra of the sample were collected from diffraction angles 2θ = 5° to 2θ = 35° with a step size of 0.1° using a counting time of 6 seconds, and the XRPD instrument was adjusted to collect a final spectrum at the end.
[0155] Define Ta as the total area between the spectral profile and the baseline, expressed in counts / sec·2θ, and Aa as the total amorphous area, expressed in counts / sec·2θ, where Ca is the total crystalline area, expressed in counts / sec·2θ. The spectra or diffraction patterns were analyzed by the following procedure. 1) Define an appropriate linear baseline for the entire spectrum and calculate the total area (Ta) between the spectral contour and the baseline; 2) defining an appropriate amorphous profile along the entire spectrum that separates amorphous regions from crystalline regions based on a phase model; 3) Calculate the amorphous area (Aa), which is the area between the amorphous contour and the baseline; 4) Calculate the crystalline area (Ca) as the area between the spectral contour and the amorphous contour, e.g., Ca = Ta - Aa; 5) Calculate the crystallinity (%Cr) of the sample using the following formula:
number
[0156] Xylene soluble and insoluble fractions at 25°C (XS-25°C)
[0157] 2.5 g of polymer was dissolved in 250 ml of xylene with stirring at 135 °C. After 20 min, the solution was cooled to 25 °C with stirring and then allowed to stand for 30 min. The precipitate was filtered through filter paper, the solution was evaporated in a nitrogen stream, and the residue was dried under vacuum at 80 °C until a constant weight was reached. The weight percentages of soluble (xylene soluble - XS) and insoluble polymer at room temperature (25 °C) were calculated accordingly.
[0158] The weight percent of polymer that is insoluble in xylene at room temperature (25°C) is considered the isotactic index of the polymer. This value corresponds substantially to the isotactic index determined by extraction with boiling n-heptane, which by definition constitutes the isotactic index of propylene polymers.
[0159] Fractions soluble and insoluble in xylene at 0°C (XS-0°C)
[0160] A 2.5 g polymer sample was dissolved in 250 ml of xylene at 135 °C with stirring. After 30 minutes, the solution was cooled to 100 °C with stirring and then cooled to 0 °C in a water and ice bath. The solution was then left in the water and ice bath for 1 hour. The precipitate was filtered with filter paper. During filtration, the flask was left in an ice-water bath to keep the internal temperature of the flask as close to 0 °C as possible. An aliquot of the solution was evaporated in a stream of nitrogen gas, and the residue was dried at 80 °C under vacuum until a constant weight was reached. The weight difference between the two residues should be less than 3%. Otherwise, the test should be repeated. The weight percentage of the polymer solubles was calculated from the average weight of the residue (xylene solubles at 0 °C = XS0 °C). The insoluble fraction in o-xylene at 0 °C (xylene insolubles at 0 °C = XI%0 °C) was calculated as follows:
[0161]
number
[0162] Melting and crystallization temperatures of butene-1 polymers (B) determined by differential scanning calorimetry (DSC)
[0163] Differential scanning calorimetry (DSC) data were obtained using a Perkin Elmer DSC-7 instrument using weighed samples (5–10 mg) sealed in aluminum pans.
[0164] To determine the melting temperature of polybutene-1 crystalline form I (TmI), the sample was heated to 200 °C at a scanning rate equivalent to 10 °C / min, held at 200 °C for 5 minutes, and then cooled to 20 °C at a cooling rate of 10 °C / min. The sample was then stored at room temperature for 10 days. After 10 days, the sample was subjected to DSC, cooled to -20 °C, and then heated to 200 °C at a scanning rate equivalent to 10 °C / min. In this heating procedure, the highest temperature peak of the thermogram was used as the melting temperature (TmI).
[0165] Melting temperature and crystallization temperature T of polybutene-1 crystalline form II (TmII) c To determine the crystallization temperature (T), the sample was heated to 200 °C at a scanning rate equivalent to 10 °C / min and held at 200 °C for 5 min to completely melt all crystallites and cancel the thermal history of the sample. Subsequently, the peak temperature was cooled to -20 °C at a scanning rate equivalent to 10 °C / min. c ) and the area was taken as the crystallization enthalpy. After standing at -20 °C for 5 min, the sample was heated a second time to 200 °C at a scan rate equivalent to 10 °C / min. In this second heating run, the peak temperature was taken as the melting temperature (TmII) of polybutene-1 crystalline form II, and the area was taken as the melting enthalpy (ΔHfII).
[0166] NMR analysis of chain structure
[0167] 13 C NMR spectra were acquired on a Bruker AV-600 spectrometer equipped with a cryoprobe, operating at 120 °C and 150.91 MHz in Fourier transform mode.
[0168] T βδ Carbon peak (CJ Carman, RA Harrington and CE Wilkes, Macromolecules, 10, 3 ,536 (1977)) was used as the internal standard at 37.24 ppm. Samples were dissolved in 1,1,2,2-tetrachloroethane d2 at 120 °C at a concentration of 8% wt / v. Each spectrum was 1 H- 13 The data was acquired using a 90° pulse, a 15-second delay between pulses, and CPD to remove C coupling. Approximately 512 transients were stored in 32,000 data points using a 9000 Hz spectral window.
[0169] Kakugo [M. Kakugo, Y. Naito, K. Mizunuma and T. Miyatake, <Polymer>, 16, 4 Based on [J.C. Randall, Macromol. Chem. Phys., C30, 211 (1989)] and Randall [J.C. Randall, Macromol. Chem. Phys., C30, 211 (1982)], the following terms are used to assign values to the spectrum and evaluate the ternary distribution and composition:
[0170]
number
[0171] [Table 1]
[0172] As a first approximation, mmmm was calculated using 2B2 carbons as follows:
[0173] [Table 2]
[0174]
number
[0175] Filament toughness, elongation at break, and breaking load
[0176] Titer in denier is commonly used to measure the size of fibers or filaments in textiles and is defined as the weight (in grams) of 9000m of filament or tape. On a laboratory scale, the actual titer value (in denier) is determined by multiplying the weight of 100m of filament or tape by 90.
[0177] Toughness, elongation at break and load at break are measured on a single filament 7 days after manufacture using a dynamometer such as LLOYDRX-Plus with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min. The load cell provides the force at break (grams or kilograms) and the elongation at break (%) is calculated as follows:
number
[0178] The tenacity (at break) is obtained by dividing the breaking load (grams) by the strength (denier).
[0179] Flexural modulus
[0180] Measurements were taken 10 days after molding according to standard ISO 178:2010.
[0181] Example 1 and Comparative Examples 1 to 5
[0182] The following materials were used to produce the polyolefin composition (I):
[0183] Propylene Polymer A)
[0184] A propylene homopolymer having the properties set out in Table 1 below.
[0185] It is available on the market under the trademark MoplenHP556E sold by LyondellBasell.
[0186] Butene-1 Polymer B)
[0187] Butene-1 homopolymers produced with Ziegler-Natta catalysts in liquid monomer polymerizations have the properties listed in Table 1 below. It is available on the market under the trademark ToppylPB 0110M, sold by LyondellBasell. Table I [Table 3]
[0188] Preparation of polyolefin composition (I) and filament spinning
[0189] Components A) and B), including a conventional stabilizing additive composition, were dry mixed in a drum blender for 15 minutes and then spun into filaments of round cross section.
[0190] The equipment used was a Leonard+ gear pump extruder with a diameter of 25 mm and a length of 27 L / D. The die had 10 circular holes and a diameter of 1.2 mm.
[0191] The main process conditions are as follows: Temperature profile:-Cylinder 180-185-190-195℃; -Pump 200℃ - Adapter 205℃ -Head die 210℃ Melting temperature: 212+ / -3℃ Output used: approx. 4 kg / h Cooling water bath: 21+ / -1℃ Stretching oven set: 106+ / -2℃ (hot air) Annealing oven set: 106+ / -2℃ (hot air) Annealing coefficient: average -5.0% (slow).
[0192] The properties of the resulting filaments are listed for all examples in Table II. Table II [Table 4] Table II continued [Table 5]
Claims
1. A stretched polyolefin filament comprising a polyolefin composition (I), wherein the elongation at break EB is 90% or more, preferably 110% or more, more preferably 130% or more, particularly 90% to 190%, preferably 110% to 190%, more preferably 130 to 185%, and SR / EB (SR is a stretch ratio) is 75 or less, preferably 70 or less, with the lower limit being preferably 30 in all cases, more preferably 40; A) 80 to 95% by weight, preferably 80 to 90% by weight, of a propylene polymer; B) 5 to 20% by weight, preferably 10 to 20% by weight, of a butene-1 polymer having the following characteristics: 1) the flexural modulus is 100 to 800 MPa, more preferably 250 to 600 MPa, and most preferably 300 to 600 MPa; 2) Ratio MI 10 / M.I. 2 is 20 to 40, preferably 25 to 35, and MI 10 is the melt flow index MI at 190° C. and a load of 10 kg, and MI 2 is the melt flow index MI at 190°C and a load of 2.16 kg, both of which are measured in accordance with ISO 1133-1:2011; 3) the content of xylene soluble fraction at 0° C. based on the total weight of B) is not more than 15% by weight, preferably not more than 10% by weight, the preferred lower limit being 0.5% by weight in all cases; (2) The amount of A) and B) refers to the total weight of A)+B), EB is measured on one filament 7 days after production using a dynamometer with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min, and flexural modulus is measured 10 days after molding according to standard ISO 178:2010 for oriented polyolefin filaments.
2. 2. The drawn polyolefin filament according to claim 1, having a titer of at least 800 Den.
3. 3. The drawn polyolefin filament according to claim 1 or 2, which is a monofilament.
4. The drawn polyolefin filament according to claim 1 or 2, wherein the SR is from 3:1 to 4.5:
1.
5. 3. The drawn polyolefin filament according to claim 1 or 2, further having the following characteristics measured on one filament 7 days after production using a dynamometer with a clamping distance of 250 mm and an applied elongation rate of 250 mm / min: a toughness of at least 1.9, preferably at least 1.95, in particular between 1.9 and 2.2; and / or - The load at break is 2.5 to 4.5 kg.
6. 3. The drawn polyolefin filament according to claim 1 or 2, wherein the butene-1 polymer B) is selected from butene-1 homopolymers and butene-1 copolymers, and mixtures thereof, having a comonomer content, in particular a copolymerized ethylene content, of 0.5 mol % to 10 mol %, preferably 0.7 mol % to 9 mol %.
7. 3. The drawn polyolefin filament according to claim 1 or 2, wherein said butene-1 polymer B) has a molecular weight distribution Mw / Mn greater than or equal to 4, preferably greater than or equal to 5, the upper limit being in all cases preferably 10, Mw being the weight average molar mass measured by gel permeation chromatography, Mn being the number average molar mass measured by gel permeation chromatography.
8. 3. The drawn polyolefin filament according to claim 1 or 2, wherein said butene-1 polymer B) has one or more of the following additional characteristics: the melting point TmII, measured by DSC (differential scanning calorimetry) in a second heating run at a scanning rate of 10° C. / min, is not more than 125° C., preferably not more than 120° C., the lower limit being in all cases preferably 75° C. - X-ray crystallinity is 25-65% The intrinsic viscosity (I.V.) measured in tetrahydronaphthalene (THN) at -135°C is not more than 5 dl / g, preferably not more than 3 dl / g, the lower limit being preferably 0.4 dl / g in all cases. ii) Mw is 100,000 g / mol or more, in particular 100,000 to 650,000 g / mol. The melting point Tml measured by DSC at a scanning rate of 10°C / min is 95°C to 135°C. - Density is 885-925 kg / m 3 , preferably 900 to 920 kg / m 3 , especially 912 to 920 kg / m 3 To be
9. 3. The drawn polyolefin filament according to claim 1 or 2, wherein the propylene polymer A) is selected from propylene homopolymers, propylene copolymers and mixtures thereof, the amount of xylene insoluble fraction at 25° C. being 85% by weight or more, more preferably 90% by weight or more, in particular for propylene homopolymers 95% by weight or more, the upper limit being preferably 99% for all homopolymers and 96% for all copolymers.
10. 2. An article comprising the drawn polyolefin filaments according to any one of the preceding claims.
11. 11. The article of claim 10 in the form of a net, rope or brush.