Forward osmosis membrane and its manufacturing method
The forward osmosis membrane with an antimicrobial support grid addresses bacterial contamination issues by using nanoAg and nanoTiO2, maintaining performance and extending its use in complex water environments.
Patent Information
- Application Number
- JP2024536325
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-09
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-02-28
AI Technical Summary
Conventional forward osmosis membranes lack effective antibacterial properties, leading to bacterial growth and contamination, which compromises their performance and longevity in complex water environments.
A forward osmosis membrane with a laminate structure comprising a hydrophilic support grid modified with antimicrobial nanoparticles, such as nanoAg and nanoTiO2, is developed to inhibit bacterial growth and enhance antibacterial efficacy.
The membrane maintains high permeation flux and salt rejection while providing long-lasting antibacterial protection, ensuring effective operation in eutrophic conditions and extending the membrane's service life.
Smart Images

Figure 2024543704000001_ABST
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to Chinese Patent Application No. 202111053419.X, filed on September 9, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to the technical field of polymeric separation membranes and their manufacturing methods, and more particularly to antibacterial forward osmosis membranes and their manufacturing methods. [Background technology]
[0003] The forward osmosis (FO) process is a process in which water is automatically diffused from the low osmotic pressure raw water side to the high osmotic pressure draw liquid side through a selective permeable membrane using the osmotic pressure difference between the draw liquid and the feed liquid as the driving force. This process does not require any external force or energy.
[0004] Unlike pressure-driven membrane separation processes such as ultrafiltration, nanofiltration and reverse osmosis technologies, forward osmosis can be operated at low or no pressure, resulting in low energy consumption during operation. Low pressure operation is characterized by no pressure-induced cake layer formation and low membrane fouling.
[0005] When there is sufficient osmotic pressure difference, high water recovery rates that cannot be achieved by conventional separation membranes can be realized.
[0006] Based on the characteristics of forward osmosis, such as low energy consumption, low membrane fouling, and high rejection, forward osmosis technology has been rapidly developed in recent years as a new membrane separation technology and has attracted attention from researchers both at home and abroad. It is used in the fields of food, medicine, energy, etc., and is particularly expected to be applied in many fields, such as seawater desalination, drinking water treatment, and wastewater treatment.
[0007] An ideal forward osmosis membrane should have good hydrophilicity, high permeation flux, high salt rejection, low internal concentration difference, durability, good antibacterial properties, etc. at the same time. These are also the research directions that have attracted attention in this field in recent years. For example, Chinese Patent Application No. CN201811285404.4 discloses a graphene-added forward osmosis membrane without a support grid, which enhances the strength of the membrane with graphene, improves the water permeation flux, and reduces the polarization of the internal concentration difference while reducing the thickness of the membrane. Chinese Patent Application No. CN201410065806.9 discloses that chitin nanocrystalline particles are added to cellulose triacetate to reduce the polarization of the internal concentration difference, improve hydrophilicity, and reduce the polarization of the internal concentration difference. The technical means disclosed or described in these two patent technologies have antibacterial effects, but they both provide a cellulose triacetate membrane layer of a forward osmosis membrane that is modified by adding graphene material or chitin nanocrystals to the active layer of the forward osmosis membrane. The main issues that are solved are performance issues such as improving water permeation flux and reducing the polarization of internal concentration difference, and the antibacterial effect is not very high.
[0008] In recent years, the understanding of forward osmosis technology has enabled forward osmosis membranes to adapt to more complex water qualities, but in the conventional technologies and products, for example, the forward osmosis membranes disclosed in the above patent documents and patent technologies, due to their insufficient antibacterial efficiency, cannot meet the long-term effective use of forward osmosis membranes in complex and eutrophic water qualities, and in long-term use, eutrophic raw water is prone to a large amount of bacteria growing in the raw water, which is likely to cause problems such as membrane contamination and clogging, affecting the performance of the membrane. At present, it is urgent to provide a comprehensive and high-performance forward osmosis membrane, which is an important factor in improving forward osmosis efficiency. Summary of the Invention
[0009] An object of the present invention is to provide a forward osmosis membrane that can improve the performance of the forward osmosis membrane by inhibiting bacterial growth and improving the antibacterial effect.
[0010] Another object of the present invention is to provide a method for producing a forward osmosis membrane, which can improve the performance of the forward osmosis membrane by inhibiting bacterial growth and improving the antibacterial effect.
[0011] In order to achieve the above object, the present invention employs the following technical means. The present invention relates to a forward osmosis membrane. The forward osmosis membrane provided in the present invention has a membrane structure that is laminated in sequence. The laminate includes a hydrophilic support grid and a hydrophilic polymer film layer. The support grid is a non-woven fabric or polyester screen modified with antimicrobial nanoparticles.
[0012] In another preferred embodiment of the present invention, the antibacterial nanoparticles are a mixture of nano Ag and nano TiO2. The mass ratio of the two is 1:1 to 1:5. The average particle size of the nano Ag is 20 nm, and the average particle size of the nano TiO2 is 5-10 nm. Preferably, the mass ratio of the nano Ag and nano TiO2 is 1:2, more preferably, nano Ag is 0.2 wt.% and nano TiO2 is 0.4 wt.%, and the more preferred ratio is the mass ratio to the modified suspension.
[0013] In another preferred embodiment of the present invention, the support grid has a thickness of 30 μm-80 μm and a pore size of 100-200 mesh. The forward osmosis membrane has a thickness of 30 μm-100 μm. Preferably, the support grid has a thickness of 30 μm, 50 μm or 70 μm and a pore size of 100 mesh, 120 mesh or 150 mesh. Preferably, the forward osmosis membrane has a thickness of 30 μm, 50 μm, 70 μm or 100 μm.
[0014] In another preferred embodiment of the present invention, the support grid modified by antibacterial nanoparticles is manufactured by the following method: nano Ag is added to a mass percentage of 0.1-0.5 wt.%, nano TiO2 is added to a mass percentage of 0.2-1 wt.%, and polyvinyl alcohol aqueous solution is added to a mass percentage of 2-8 wt.%, and then ultrasonically dispersed to prepare a modified suspension, and a polyester screen is immersed in the suspension and naturally dried. Preferably, the mass percentage of nano Ag is 0.2 wt.%, the mass percentage of nano TiO2 is 0.4 wt.%, and the polyvinyl alcohol aqueous solution is 4 wt.%.
[0015] In another preferred embodiment of the invention, the hydrophilic polymeric material is at least one of polyacrylonitrile, polyacrylate, polymethyl methacrylate, cellulose acetate, cellulose triacetate, polyvinyl alcohol, polyethylene oxide, and polyvinyl acetate.
[0016] According to another object of the present invention, the present invention also relates to a method for producing a forward osmosis membrane, said method comprising the steps of: (a) manufacturing an antimicrobial modified support grid, said support grid being a hydrophilic nonwoven fabric or polyester screen; (b) preparing a casting solution: mixing a hydrophilic polymer in an aqueous solvent system to prepare a casting solution; (c) pouring the casting solution prepared in step (b) onto the glass plate covered with the antibacterial modified support grid prepared in step (a) to obtain an initial forward osmosis membrane having a specific thickness; (d) treating the outer layer of the initial forward osmosis membrane to remove the solvent and form a dense skin layer on the outer layer of the initial forward osmosis membrane to obtain a second initial forward osmosis membrane; (e) forming a phase separation membrane or an interface membrane on the second initial forward osmosis membrane to obtain the forward osmosis membrane; Includes.
[0017] The antibacterial modified support grid is a polyester screen modified with nano Ag and nano TiO2, which is prepared by the following method: nano Ag and nano TiO2 are placed in an aqueous polyvinyl alcohol solution to prepare a suspension, and a polyester screen is immersed in the suspension, then dried and stored until use.
[0018] The suspension is obtained by the following method: Nano Ag is added to a mass percentage of 0.1-0.5 wt.% and nano TiO2 is added to a mass percentage of 0.2-1 wt.% and a mass percentage of 2-8 wt.% polyvinyl alcohol aqueous solution, and then ultrasonically dispersed. Preferably, the mass percentage of the nano Ag is 0.2 wt.%, the mass percentage of the nano TiO2 is 1 wt.%, and the mass percentage of the polyvinyl alcohol is 4 wt.%. Preferably, the mass percentage of the nano Ag is 0.2 wt.%, and the mass percentage of the nano TiO2 is 0.4 wt.%.
[0019] The support grid has a thickness of 30 μm-80 μm and a pore size of 100-200 mesh. The forward osmosis membrane has a thickness of 30 μm-100 μm. Preferably, the support grid has a thickness of 30 μm, 50 μm or 70 μm and a pore size of 100 mesh, 120 mesh or 150 mesh. Preferably, the forward osmosis membrane has a thickness of 30 μm, 50 μm, 70 μm or 100 μm.
[0020] The hydrophilic polymer material is at least one of polyacrylonitrile, polyacrylate, polymethylmethacrylate, cellulose acetate, cellulose triacetate, polyvinyl alcohol, polyethylene oxide, and polyvinyl acetate. The solvent system includes a mixture of 1,4-dioxane, acetone, methanol, and lactic acid. The weight percentage of the hydrophilic polymer is 8-15 wt.%, the weight percentage of 1,4-dioxane is 30-60 wt.%, the weight percentage of acetone is 5-20 wt.%, the weight percentage of methanol is 5-10 wt.%, and the weight percentage of lactic acid is 6-8 wt.%.
[0021] The method further includes the steps of: (b-1) The casting liquid obtained in step (b) is degassed. The step (c) further comprises pouring the degassed casting liquid from step (b-1) onto a glass plate on which an antibacterial modified hydrophilic support grid is laid, and using a film applicator to produce an initial forward osmosis membrane having a specific thickness. In the outer layer treatment and solvent removal step (d), the resulting initial forward osmosis membrane is left standing in air to volatilize the solvent and form a dense skin layer on the outer layer. In the step (e), the second initial forward osmosis membrane is immersed in deionized water to cause gelation and phase separation to occur, forming a membrane. (f) The forward osmosis membrane obtained in step (e) is immersed in deionized water to remove residual organic solvents. (g) Remove the forward osmosis membrane, rinse with deionized water, and store in a solution of sodium metabisulfite until use.
[0022] The hydrophilic support grid is a polyester screen, which is used after being pre-washed. In the pre-washing step, the polyester screen is immersed in 10% sodium hydroxide and 2% hydrochloric acid for 1 hour to remove impurities adsorbed on the surface, and then rinsed with deionized water, dried and stored. The initial forward osmosis membrane produced by the film applicator has a thickness of 30 μm-100 μm.
[0023] In step (b) of the preparation method, the mixing conditions are 30-50°C temperature, 12-48h stirring to mix uniformly, preferably 40°C temperature, 24h stirring. The defoaming method is 12-36h standing to defoam thoroughly, or ultrasonic wave assisted defoaming, preferably 24h standing. The conditions for standing in air are 30-90s standing in an environment with a temperature of 25°C or less and a humidity of 90% or more to form a dense skin layer, preferably 60s standing in an environment with a temperature of 25°C and a humidity of 90%. In step (f) of the preparation method, before immersing the membrane in deionized water, the membrane is placed in a water bath of 40-50°C for 5-20 minutes for heat treatment, and then placed in deionized water to remove residual organic solvent, the immersion time is 12-36h, preferably 24h. In step (g) of the preparation method, the concentration of sodium metabisulfite is 0.5-2%, preferably 1%.
[0024] In the forward osmosis membrane and the manufacturing method thereof provided by the present invention, the support grid layer of the membrane is completely covered with antibacterial nanoparticles, particularly a mixture of nano Ag and nano TiO2, so that the strength, water permeation flux, and salt rejection rate of the forward osmosis membrane are not reduced, and an effective, long-lasting, and comprehensive antibacterial effect is provided. In the present invention, the support grid of the forward osmosis membrane is antibacterial modified with antibacterial nanoparticles, particularly a mixture of nano Ag and nano TiO2, so that the growth of bacteria on the forward osmosis membrane is inhibited, the forward osmosis property is improved, and the safety of the entire purification and filtration system is improved. The antibacterial forward osmosis membrane of the present invention can be applied to the filtration and purification of complex water sources, especially the purification and filtration of water sources where bacteria are likely to grow due to eutrophication. In addition, the safety of nano silver has been commercially recognized, and the material is widely used in baby products such as tableware and baby bottles. [Brief description of the drawings]
[0025] [Figure 1] 1 is a flow chart of a manufacturing process for a forward osmosis membrane of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] In order to further explain the technical means and effects for achieving the object of the present invention, the forward osmosis membrane and its manufacturing method of the present invention, its specific embodiment, structure, manufacturing method, features and functions are described below with reference to the drawings and preferred examples. The present invention will be further described in the following examples, but the following examples are merely for explaining the present invention and are not intended to limit the present invention.
[0027] Figure 1 is a flow chart of the manufacturing process of the forward osmosis membrane of the present invention. The specific process is as follows: 1. Preparation of antibacterial support grid: The support grid is a hydrophilic nonwoven fabric or polyester screen. In the present invention, more preferably, a polyester screen modified with nano Ag and nano TiO2 is prepared. Nano Ag and nano TiO2 are put into a polyvinyl alcohol aqueous solution, and a suspension is prepared by ultrasonic dispersion. The support grid is immersed in the suspension, then air-dried, and stored until use. 2. Preparation of casting liquid: Mix hydrophilic polymer material and organic solvent system uniformly. In the present invention, the hydrophilic polymer material is further added to the water-soluble organic solvent system mixed liquid, and after stirring at a temperature of 30°C-50°C for 12-48 hours, a uniform casting liquid is obtained. In the present invention, more preferably, cellulose triacetate is added to a mixed liquid of 1,4-dioxane, acetone, methanol and lactic acid, and after stirring at a temperature of 40°C for 24 hours, a uniform casting liquid is obtained. 3. Degassing: The casting liquid obtained in step 2 is left to stand for 12-36 hours to be thoroughly degassed or ultrasonic degassing is used to assist the degassing. In the present invention, it is more preferable to leave the casting liquid to stand for 24 hours to be thoroughly degassed. 4. Preparation of initial forward osmosis membrane: The completely degassed casting liquid is poured onto a glass plate on which the prepared antibacterial support grid is laid, and an initial forward osmosis membrane with a specific thickness is prepared using a film applicator. 5. Film formation: The film obtained in step 4 is left to stand in air for a few seconds under a given temperature and humidity environment to form a dense skin layer, and then immersed in deionized water to gel and cause phase separation to form a film. In the present invention, it is preferable to leave it to stand in air at a temperature of 25°C or less and a humidity of 90% or more for 30 to 90 seconds. 6. Optimization treatment: The membrane obtained in step 5 is placed in a 40-50°C water bath for heat treatment for 5-20 minutes, and then immersed in deionized water for 24 hours to remove residual organic solvents, thus obtaining a further optimized forward osmosis membrane. 7. Storage until use: Take out the forward osmosis membrane, rinse with deionized water, then place in a 0.5-2% sodium metabisulfite solution, preferably a 1% sodium metabisulfite solution, and store until use. Decide whether to store until use as needed.
[0028] The method for producing the forward osmosis membrane provided by the present invention will be further described below. Preparation of nano Ag / TiO2 modified polyester screen: Nano Ag is added at a mass percentage of 0.1-0.5 wt.%, nano TiO2 is added at a mass percentage of 0.2-1 wt.%, and polyvinyl alcohol aqueous solution at a mass percentage of 2-8 wt.% is added, and ultrasonic dispersion is performed to prepare a suspension. A polyester screen is immersed in the suspension, then naturally dried and stored until use. Produced casting liquid: Cellulose triacetate is added at a mass percentage of 8-15 wt.% to a mixture of acetone mass percentage of 5-20 wt.%, methanol mass percentage of 5-10 wt.%, lactic acid mass percentage of 6-8 wt.%, and the remaining part of 1,4-dioxane, and stirred at a temperature of 40°C for 24 hours to obtain a uniform casting liquid. The obtained casting liquid is left to stand for 24 hours and thoroughly degassed or assisted by ultrasonic degassing. The completely degassed casting liquid is poured onto a glass plate covered with the prepared modified polyester screen, and a film applicator is used to prepare an initial forward osmosis membrane of 30-100 μm. The membrane obtained in the previous step is left in air for 60-90 seconds in an environment of 25°C and 90% humidity to form a dense skin layer, and then immersed in deionized water to gel, and phase separation occurs to form a membrane. The thickness of the modified polyester screen is 30 μm-80 μm, and preferably 30 μm, 50 μm, or 70 μm.
[0029] The forward osmosis membrane obtained by forming the gel phase separation membrane is placed in a water bath at 40-50°C for heat treatment for 5-15 minutes, and then immersed in deionized water for 24 hours to remove residual organic solvents.
[0030] The antibacterial forward osmosis membrane of the present invention has a membrane permeation flux of 8-13 L / (m2) when 0.5 mol / L sodium chloride and 0.01 mol / L magnesium sulfate are used as the draw and feed liquids, respectively. 2 *h), the magnesium sulfate inhibition rate is higher than 97%, the antibacterial rate is higher than 90%, and the antibacterial rate in the antibacterial durability test is higher than 90%.
[0031] The present invention will now be further described with reference to specific examples.
[0032] Example 1 1. A polyester screen with a thickness of 30 μm and a pore size of 100 mesh was immersed in 2% hydrochloric acid and 10% sodium hydroxide for 1 hour to remove impurities adsorbed on the surface, then rinsed with deionized water, dried, and stored until use. 2. Preparation of nano-Ag and nano-TiO2 modified polyester screen: Nano-Ag at 0.2 wt.% and nano-TiO2 at 0.4 wt.% were added to a polyvinyl alcohol aqueous solution at 4 wt.% by mass, and ultrasonically dispersed to prepare a suspension. A polyester screen was immersed in this suspension, then naturally dried and stored until use. 3. Cellulose triacetate (mass percentage: 13 wt.%) was added to a mixture of 1,4-dioxane (mass percentage: 54 wt.%), acetone (mass percentage: 19 wt.%), methanol (mass percentage: 8 wt.%), and lactic acid (mass percentage: 6 wt.%), and stirred at a temperature of 40°C for 24 hours to prepare a uniform casting liquid. 4. The cast liquid obtained in step 3 was allowed to stand for 24 hours and then thoroughly degassed or assisted by ultrasonic degassing. 5. The completely degassed casting liquid was poured onto a glass plate covered with the prepared modified polyester screen having a thickness of 30 μm, and an initial forward osmosis membrane having a thickness of 50 μm was prepared using a film applicator. 6. The membrane obtained in step 5 was left to stand in air at 25°C and 90% humidity for 30 seconds to form a dense skin layer, and was then immersed in deionized water, causing gelation and phase separation to form a membrane. 7. The membrane obtained in step 6 was placed in a water bath at 50°C for 15 min for heat treatment, and then immersed in deionized water for 24 h to remove residual organic solvents.
[0033] Membrane performance The forward osmosis membrane produced in the above steps has a thickness of 50 μm. When 0.5 mol / L sodium chloride and 0.01 mol / L magnesium sulfate are used as the draw and feed liquids, respectively, the membrane permeation flux is 12.5 L / (m 2 *h), the magnesium sulfate blocking rate was 97.8%, and the antibacterial rate was 95%. In the antibacterial durability test, the antibacterial rate was 93%. Specific performance tests are shown in Table 1.
[0034] Example 2 1. A polyester screen with a thickness of 50 μm and a pore size of 100 mesh was immersed in 2% hydrochloric acid and 10% sodium hydroxide for 1 hour to remove impurities adsorbed on the surface, then rinsed with deionized water, dried, and stored until use. 2. Preparation of nano-Ag and nano-TiO2 modified polyester screen: Nano-Ag at 0.2 wt.% and nano-TiO2 at 0.4 wt.% were added to a polyvinyl alcohol aqueous solution at 4 wt.% by mass, and ultrasonically dispersed to prepare a suspension. A polyester screen was immersed in this suspension, then naturally dried and stored until use. 3. Cellulose triacetate (mass percentage: 13 wt.%) was added to a mixture of 1,4-dioxane (mass percentage: 54 wt.%), acetone (mass percentage: 19 wt.%), methanol (mass percentage: 8 wt.%), and lactic acid (mass percentage: 6 wt.%), and stirred at a temperature of 40°C for 24 hours to prepare a uniform casting liquid. 4. The resulting casting liquid was allowed to stand for 24 hours and then thoroughly degassed or assisted by ultrasonic degassing. 5. The completely degassed casting liquid was poured onto a glass plate covered with the prepared modified polyester screen having a thickness of 50 μm, and an initial forward osmosis membrane having a thickness of 70 μm was prepared using a film applicator. 6. The membrane obtained in step 5 was left to stand in air at 25°C and 90% humidity for 60 seconds to form a dense skin layer, and was then immersed in deionized water, causing gelation and phase separation to form a membrane. 7. The membrane obtained in step 6 was placed in a water bath at 45°C for 20 min for heat treatment, and then immersed in deionized water for 24 h to remove residual organic solvents.
[0035] Membrane performance The forward osmosis membrane produced in the above steps has a thickness of 70 μm. When 0.5 mol / L sodium chloride and 0.01 mol / L magnesium sulfate are used as the draw and feed liquids, respectively, the membrane permeation flux is 11.0 L / (m 2 *h), the magnesium sulfate blocking rate was 98.1%, and the antibacterial rate was 94%. In the antibacterial durability test, the antibacterial rate was 92%. Specific performance tests are shown in Table 1.
[0036] Example 3 1. A polyester screen with a thickness of 50 μm and a pore size of 100 mesh was immersed in 2% hydrochloric acid and 10% sodium hydroxide for 1 hour to remove impurities adsorbed on the surface, then rinsed with deionized water, dried, and stored until use. 2. Preparation of nano-Ag and nano-TiO2 modified polyester screen: Nano-Ag at 0.2 wt.% and nano-TiO2 at 0.4 wt.% were added to a polyvinyl alcohol aqueous solution at 4 wt.% by mass, and ultrasonically dispersed to prepare a suspension. A polyester screen was immersed in this suspension, then naturally dried and stored until use. 3. Cellulose triacetate (mass percentage: 10 wt.%) was added to a mixture of 1,4-dioxane (mass percentage: 57 wt.%), acetone (mass percentage: 19 wt.%), methanol (mass percentage: 8 wt.%), and lactic acid (mass percentage: 6 wt.%), and stirred at a temperature of 40°C for 24 hours to prepare a uniform casting liquid. 4. The resulting casting liquid was allowed to stand for 24 hours and then thoroughly degassed or assisted by ultrasonic degassing. 5. The completely degassed casting liquid was poured onto a glass plate covered with the prepared modified polyester screen having a thickness of 50 μm, and an initial forward osmosis membrane having a thickness of 100 μm was prepared using a film applicator. 6. The membrane obtained in step 5 was left to stand in air at 25°C and 90% humidity for 80 seconds to form a dense skin layer, and was then immersed in deionized water, causing gelation and phase separation to form a membrane. 7. The membrane obtained in step 6 was placed in a 40°C water bath for heat treatment for 15 min, and then immersed in deionized water for 24 h to remove residual organic solvents.
[0037] Membrane performance The forward osmosis membrane produced in the above steps has a thickness of 100 μm. When 0.5 mol / L sodium chloride and 0.01 mol / L magnesium sulfate are used as the draw and feed liquids, respectively, the membrane permeation flux is 10.5 L / (m 2 *h), the magnesium sulfate blocking rate was 98.2%, and the antibacterial rate was 95%. In the antibacterial durability test, the antibacterial rate was 93%. Specific performance tests are shown in Table 1.
[0038] Table 1: Performance evaluation of membranes using 0.5 mol / L sodium chloride and 0.01 mol / L magnesium sulfate as draw and feed liquids, respectively.
[0039] [Table 1]
[0040] As can be seen from Table 1, the forward osmosis membrane of the present invention equipped with an antibacterial support grid has high antibacterial properties, and after immersion in eutrophic raw water for 10 days and subsequent testing after simple rinsing, the antibacterial properties were still maintained at 90% or more, and the membrane permeation flux and salt rejection were not affected. Conventional forward osmosis membranes made of cellulose triacetate and forward osmosis membranes of conventional products do not have antibacterial properties, so as the immersion time increases, the membrane performance is significantly reduced due to the proliferation of organisms.
[0041] In the examples of the present invention, the concentrations of sodium hydroxide, hydrochloric acid and sodium metabisulfite are calculated by mass ratio.
[0042] In the forward osmosis membrane and the manufacturing method thereof provided in the present invention, the invented forward osmosis membrane is a forward osmosis membrane with an antibacterial modified support grid, which can inhibit bacterial growth under environmental conditions of eutrophic raw water, improve the permeability of the forward osmosis membrane, enable the forward osmosis membrane to be effectively used for a long period of time, extend the service life of the forward osmosis membrane system, and reduce the operating cost.
[0043] Although the present invention has been described herein with reference to specific embodiments, it will be apparent that various modifications and changes can be made thereto without departing from the spirit and scope of the present invention. Accordingly, the present specification and drawings are to be regarded as illustrative rather than restrictive.
Claims
1. A forward osmosis membrane, The forward osmosis membrane has a sequentially laminated membrane structure, the laminate including a hydrophilic support grid and a hydrophilic polymer film layer, the support grid being a non-woven fabric or polyester screen modified with antibacterial nanoparticles, the support grid being modified with antibacterial nanoparticles in the following manner: nano Ag in a mass percentage of 0.1-0.5 wt. %, nano TiO 2 The nano Ag particles were added to a polyvinyl alcohol aqueous solution having a mass percentage of 2-8 wt. % and dispersed ultrasonically to obtain a suspension. A support grid was immersed in the suspension and then dried. The average particle size of the nano Ag particles was 20 nm, and the nano TiO 2 The average particle size of the forward osmosis membrane is 5-10 nm, and the feed liquid is 0.5 mol / L sodium chloride and 0.01 mol / L magnesium sulfate, respectively. The permeation flux of the membrane is 8-13 L / (m 2 *h), which has a magnesium sulfate rejection rate of more than 97%, an antibacterial rate of more than 90%, and when immersed in eutrophic raw water for 10 days, rinsed off, and then subsequently tested, the antibacterial activity still remains at 90% or more.
2. The nano Ag and nano TiO 2 The forward osmosis membrane according to claim 1, characterized in that the mass ratio of
3. 3. The forward osmosis membrane of claim 2, wherein the thickness of the support grid is 30 μm-80 μm and the pore size is 100-200 mesh, and the thickness of the forward osmosis membrane is 50 μm-100 μm.
4. 4. The forward osmosis membrane of claim 3, wherein the support grid has a thickness of 30 μm, 50 μm or 70 μm, a pore size of 100 mesh, 120 mesh or 150 mesh, and the forward osmosis membrane has a thickness of 50 μm, 70 μm or 100 μm.
5. 5. The forward osmosis membrane according to claim 1, wherein the hydrophilic polymer material is at least one of polyacrylonitrile, polyacrylate, polymethyl methacrylate, cellulose acetate, cellulose triacetate, polyvinyl alcohol, polyethylene oxide, and polyvinyl acetate.
6. 1. A method for producing a forward osmosis membrane, the method comprising: (a) Preparation of antibacterial modified support grid: The support grid is a hydrophilic nonwoven fabric or polyester screen, and the antibacterial modified support grid is made of nano Ag, nano TiO 2 A modified support grid was fabricated by the following method: nano Ag with a mass percentage of 0.1-0.5 wt. %, nano TiO 2 % by weight in an aqueous polyvinyl alcohol solution having a weight percentage of 2-8 wt. %, and ultrasonically dispersing the mixture to prepare a suspension, and then immersing a support grid in the suspension and drying it; (b) preparing a casting solution: mixing a hydrophilic polymer in an aqueous solvent system to prepare a casting solution; (c) pouring the casting liquid prepared in step (b) onto the glass plate covered with the antibacterial modified support grid prepared in step (a) to obtain an initial forward osmosis membrane with a specific thickness; (d) treating the outer layer of the initial forward osmosis membrane to remove the solvent and form a dense skin layer on the outer layer of the initial forward osmosis membrane to obtain a second initial forward osmosis membrane; (e) forming a phase separation membrane or an interface membrane on the second initial forward osmosis membrane to obtain the forward osmosis membrane; Including, The average particle size of the nano Ag is 20 nm, and the nano TiO 2 The average particle size of the forward osmosis membrane is 5-10 nm, and when 0.5 mol / L sodium chloride and 0.01 mol / L magnesium sulfate are used as the draw liquid and feed liquid, respectively, the membrane permeation flux is 8-13 L / (m 2 *h), the inhibition rate of magnesium sulfate is higher than 97%, the antibacterial rate is higher than 90%, and when the product is immersed in eutrophic raw water for 10 days, washed off, and then tested, the antibacterial activity is still maintained at 90% or more.
7. The method of claim 6, wherein the thickness of the support grid is 30μm-80μm, the pore size is 100-200 mesh, and the thickness of the forward osmosis membrane is 50μm-100μm.
8. 8. The method of claim 7, wherein the support grid has a thickness of 30 μm, 50 μm or 70 μm, a pore size of 100 mesh, 120 mesh or 150 mesh, and a forward osmosis membrane has a thickness of 50 μm, 70 μm or 100 μm.
9. 9. The method according to claim 6, wherein the hydrophilic polymer material is at least one of polyacrylonitrile, polyacrylate, polymethyl methacrylate, cellulose acetate, cellulose triacetate, polyvinyl alcohol, polyethylene oxide, and polyvinyl acetate.
10. The method further includes the steps of: (b-1) Degassing the cast liquid obtained in step (b); The step (c) further comprises pouring the degassed casting liquid from the step (b-1) onto a glass plate on which a hydrophilic support grid is laid, and using a film applicator to prepare an initial forward osmosis membrane having a specific thickness; In the outer layer treatment and solvent removal step (d), the initial forward osmosis membrane is left standing in the air to volatilize the solvent and form a dense skin layer on the outer layer; In the step (e), the second initial forward osmosis membrane is immersed in deionized water to gel and undergo phase separation to form a membrane; (f) immersing the forward osmosis membrane obtained in step (e) in deionized water to remove residual organic solvent; The method of claim 6, further comprising the steps of: (g) removing the forward osmosis membrane, rinsing it with deionized water, and storing it in a solution of sodium metabisulfite until use.
11. The hydrophilic support grid is a polyester screen having a thickness of 30 μm, 50 μm or 70 μm and a pore size of 100 mesh, 120 mesh or 150 mesh, and is used after being pre-cleaned, in which the polyester screen is immersed in 10% sodium hydroxide or 2% hydrochloric acid for 1 hour to remove impurities adsorbed on the surface, and then rinsed with deionized water, dried and stored, and the initial forward osmosis membrane produced by the film applicator has a thickness of 30 μm to 100 μm.
12. The method according to claim 11, characterized in that in step (b) of the preparation method, the mixing conditions are to mix uniformly at a temperature of 30-50°C for 12-48 hours by stirring, the degassing method is to leave the mixture for 12-36 hours to fully degas or to assist degassing with ultrasonic waves, and the conditions for leaving the mixture in air are to leave the mixture for 30-90 seconds at a temperature of 25°C or less and a humidity of 90% or more to form a dense skin layer, in step (f) of the preparation method, before the membrane is immersed in deionized water, the membrane is placed in a water bath at 40-50°C for 5-20 minutes for heat treatment, and then placed in deionized water for 12-36 hours to remove residual organic solvent, and in step (g) of the preparation method, the concentration of sodium metabisulfite is 0.5-2%.
Citation Information
Patent Citations
Spacer used for separating membrane supporting body and separating membrane in lamination
JP2001340734A
Method for reducing fouling on a surface
JP2018512275A
A forward osmosis membrane
WO2012102678A1