Plateable polymeric compositions for use at high frequencies - Patents.com
A plateable polymer composition with thermotropic liquid crystal polymers and noble metal catalysts addresses the limitations of traditional LDS in MIDs by providing low dielectric loss and mechanical strength, enabling efficient conductive element formation in high-frequency electronic components.
Patent Information
- Application Number
- JP2024531502
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-01
- Filing Date
- 2022-11-21
- Publication Date
- 2024-11-26
AI Technical Summary
Existing molded interconnect devices (MIDs) face limitations in forming conductive elements without traditional laser direct structuring (LDS) processes, which can be hindered by spinel crystals and environmental concerns related to heavy metals like copper and chromium.
A plateable polymer composition comprising a thermotropic liquid crystal polymer with noble metal catalysts and controlled dielectric properties, allowing for conductive element formation without LDS, with low dielectric loss tangent and dielectric constant, and minimal heavy metal content.
The polymer composition enables efficient conductive element formation with low dielectric loss, excellent melt processability, thermal stability, and mechanical strength, suitable for high-frequency applications in electronic components.
Smart Images

Figure 2024543929000001_ABST
Abstract
Description
[Technical field]
[0001] Related Applications
[0001] This application claims priority to U.S. Provisional Patent Application No. 63 / 284,831, having a filing date of December 1, 2021, which is incorporated by reference herein. [Background technology]
[0002] To form various electronic components, especially those used at high frequencies, molded interconnect devices (MIDs) are often formed that include a plastic substrate on which conductive elements or paths are formed. Such MID devices are thus three-dimensional molded parts with integrated printed conductors or circuit layouts. MIDs are typically formed using a laser direct structuring ("LDS") process in which a computer-controlled laser beam moves over the plastic substrate to activate its surface where the conductive paths are to be located. Various materials have been proposed to form the plastic substrate of laser direct structured devices. For example, one such material is a blend of polycarbonate, acrylonitrile butadiene styrene, and copper chromite. In the laser direct structuring process, the copper chromite cracks open, releasing metal atoms that can act as nuclei for crystal growth in a subsequent electroless copper plating process. Despite its advantages, one of the limitations of laser direct structuring materials is that spinel crystals tend to adversely affect the performance of the composition under certain circumstances. Furthermore, due to potential environmental concerns, it is increasingly desirable to minimize the use of heavy metals such as copper and chromium. Thus, there is currently a need for molded interconnect devices in which conductive elements can be easily formed without using traditional LDS processes. Summary of the Invention [Means for solving the problem]
[0003]
[0003] In accordance with one embodiment of the present invention, a plateable polymeric composition is disclosed. The polymeric composition comprises a precious metal catalyst distributed within a polymeric matrix comprising at least one highly naphthenic thermotropic liquid crystalline polymer comprising repeat units derived from naphthenic hydroxycarboxylic acids and / or dicarboxylic acids in an amount of about 10 mol.% or greater. The polymeric composition exhibits a dielectric loss tangent of about 0.01 or less determined at a frequency of 2 GHz.
[0004]
[0004] Other features and aspects of the present invention are set forth in greater detail below.
[0005] A full and enabling disclosure of the present invention, including the best mode thereof, to one of ordinary skill in the art, is set forth more particularly in the remainder of the specification, including reference to the accompanying drawings. [Brief description of the drawings]
[0005] [Figure 1]
[0006] FIG. 1 is a front and rear perspective view, respectively, of one embodiment of an electronic component that can utilize the antenna system. [Diagram 2] FIG. 2 is a front and rear perspective view, respectively, of one embodiment of an electronic component that can utilize the antenna system. [Diagram 3]
[0007] FIG. 3 is a top view of an exemplary inverted-F antenna resonating element of one embodiment of an antenna system. [Figure 4]
[0008] FIG. 4 is a top view of an exemplary monopole antenna resonating element of one embodiment of the antenna system. [Diagram 5]
[0009] FIG. 5 is a top view of an exemplary slot antenna resonating element of one embodiment of an antenna system. [Figure 6]
[0010] FIG. 6 is a top view of an exemplary patch antenna resonating element of one embodiment of the antenna system. [Figure 7]
[0011] FIG. 7 is a top view of an exemplary multi-branch inverted-F antenna resonating element of one embodiment of an antenna system. [Figure 8]
[0012] FIG. 8 illustrates a 5G antenna system including a base station, one or more relay stations, one or more user computing devices, and one or more Wi-Fi repeaters, in accordance with an embodiment of the present disclosure. [Figure 9A]
[0013] FIG. 9A illustrates a top-down view of an exemplary user computing device including a 5G antenna in accordance with an embodiment of the present disclosure. [Figure 9B]
[0014] FIG. 9B is a diagram illustrating a side elevation view of the example user computing device of FIG. 9A including a 5G antenna according to an embodiment of the present disclosure. [Figure 10]
[0015] FIG. 10 illustrates an expanded view of a portion of the user computing device of FIG. 9A. [Figure 11]
[0016] FIG. 11 is a diagram illustrating a side elevation view of a coplanar waveguide antenna array configuration according to an embodiment of the present disclosure. [Figure 12A]
[0017] FIG. 12A is a diagram illustrating an antenna array for a massive multiple-input multiple-output configuration according to an embodiment of the present disclosure. [Figure 12B]
[0018] FIG. 12B illustrates an antenna array formed by laser direct structuring according to an embodiment of the present disclosure. [Figure 12C]
[0019] FIG. 12C is a diagram illustrating an example antenna configuration according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0006]
[0020] It will be understood by those skilled in the art that this discussion is a description of exemplary embodiments only, and is not intended to limit the broader aspects of the invention.
[0021] In general, the present invention relates to a plateable polymeric composition comprising a precious metal catalyst distributed within a polymeric matrix comprising at least one thermotropic liquid crystal polymer. By selectively controlling various aspects of the composition, the inventors have discovered that the resulting composition can maintain a low dielectric loss tangent, as determined by a split post resonator method, of about 0.01 or less, in some embodiments about 0.009 or less, in some embodiments about 0.008 or less, and in some embodiments about 0.0001 to about 0.007, over typical 5G frequencies (e.g., 2GHz). The composition may also exhibit a low dielectric constant, for example, as determined by a split post resonator method, of about 5 or less, in some embodiments about 4.5 or less, in some embodiments about 0.1 to about 4.4, in some embodiments about 1 to about 4.2, in some embodiments about 1.5 to about 4, in some embodiments about 2 to about 3.9, and in some embodiments about 3.5 to about 3.9, over typical 5G frequencies (e.g., 2GHz). Notably, the inventors have also surprisingly discovered that the dielectric constant and dielectric loss tangent can be maintained within the above-mentioned ranges even when exposed to various temperatures, such as temperatures from about -30°C to about 100°C. For example, when subjected to the thermal cycle test described herein, the ratio of the dielectric constant after thermal cycling to the initial dielectric constant may be about 0.8 or more, in some embodiments about 0.9 or more, and in some embodiments about 0.95 to about 1.1. Similarly, the ratio of the dielectric loss tangent after exposure to high temperatures to the initial dielectric loss tangent may be about 1.3 or less, in some embodiments about 1.2 or less, in some embodiments about 1.1 or less, in some embodiments about 1.0 or less, in some embodiments about 0.95 or less, in some embodiments about 0.1 to about 0.95, and in some embodiments about 0.2 to about 0.9. The change in dielectric loss tangent (i.e., initial dielectric loss tangent minus dielectric loss tangent after thermal cycling) may also be in the range of about -0.1 to about 0.1, in some embodiments about -0.05 to about 0.01, and in some embodiments about -0.001 to 0.
[0007]
[0022] The polymeric composition may also be readily plated without the use of a laser direct structuring system. In this manner, the polymeric composition may be beneficially formed without the use of copper chromite (CuCr2O4) as a laser activatable additive, such that the resulting polymeric composition may generally be free of chromium and / or copper. For example, chromium may be present in the composition in an amount of about 2,000 parts per million ("ppm") or less, in some embodiments about 1,500 ppm or less, in some embodiments about 1,000 ppm or less, and in some embodiments about 0.001 to about 500 ppm, while copper is generally present in the composition in an amount of about 1,000 ppm or less, in some embodiments about 750 ppm or less, in some embodiments about 500 ppm or less, and in some embodiments about 0.001 to about 100 ppm. The copper and chromium content may be determined using known techniques, such as x-ray fluoroscopy (e.g., an Innov-X Systems Model a-2000 x-ray fluorescence spectrometer equipped with a Si-PiN diode detector). Of course, apart from copper chromite, the polymer composition may also generally be free of other types of conventional laser activatable additives, such as spinel crystals having the formula AB2O4, where A is a metal cation having a valence of two (e.g., cadmium, chromium, manganese, nickel, zinc, copper, cobalt, iron, magnesium, tin, titanium, etc.) and B is a metal cation having a valence of three (e.g., chromium, iron, aluminum, nickel, manganese, or tin) (e.g., MgAl2O4, ZnAl2O4, FeAl2O4, CuFe2O4, MnFe2O4, NiFe2O4, TiFe2O4, FeCr2O4, or MgCr2O4). The polymer composition may be free of such spinel crystals (i.e., 0 wt.%), or such crystals may be present only in minor concentrations, such as amounts of about 1 wt.% or less, in some embodiments about 0.5 wt.% or less, and in some embodiments, about 0.001 wt.% to about 0.2 wt.%.
[0008]
[0023] It was previously believed that plateable polymer compositions having low dielectric loss tangents also did not have a melt viscosity low enough to flow easily into a mold cavity to form small parts. However, in contrast to conventional belief, it has been found that polymer compositions have excellent melt processability. For example, polymer compositions generally have a melt processability of 1,000 s according to ISO 11443:2021. -1 and at a temperature about 15° C. above the melt temperature of the polymer composition.
[0009]
[0024] The polymeric composition also has excellent thermal properties. The melting temperature of the composition may be, for example, about 280°C to about 400°C, in some embodiments about 300°C to about 380°C, and in some embodiments about 320°C to about 370°C. Even at such melting temperatures, the ratio of the deflection temperature under load ("DTUL"), a measure of short-term heat resistance, to the melting temperature may still remain relatively high. For example, the ratio may range from about 0.5 to about 1.00, in some embodiments about 0.6 to about 0.95, and in some embodiments about 0.65 to about 0.85. Specific DTUL values may be, for example, about 200°C or higher, in some embodiments about 220°C or higher, in some embodiments about 230°C to about 300°C, and in some embodiments about 240°C to about 280°C. Such high DTUL values may, among other things, enable the use of fast and reliable surface attachment processes for mating the structure with other parts of the electrical component.
[0010]
[0025] The polymer composition may also have a high impact strength, useful in forming thin layers. The composition may have, for example, an impact strength of about 0.5 kJ / m2, determined at a temperature of 23° C. according to ISO Test No. ISO 179-1:2010. 2 In some embodiments, about 1 to about 60 kJ / m 2 and in some embodiments, from about 2 to about 50 kJ / m 2and in some embodiments, from about 5 to about 45 kJ / m 2 The composition may have a notched Charpy impact strength of about 20 to about 500 MPa, in some embodiments about 50 to about 400 MPa, in some embodiments about 70 to about 350 MPa; a tensile break strain of about 0.4% or more, in some embodiments about 0.5% to about 10%, in some embodiments about 0.6% to about 3.5%; and / or a tensile modulus of about 5,000 MPa to about 20,000 MPa, in some embodiments about 8,000 MPa to about 20,000 MPa, in some embodiments about 10,000 MPa to about 20,000 MPa. Tensile properties may be determined at a temperature of 23° C. according to ISO Test No. 527:2019. The polymeric composition may also exhibit a flexural strength of about 20 to about 500 MPa, in some embodiments about 50 to about 400 MPa, and in some embodiments about 100 to about 350 MPa; a flexural elongation of about 0.4% or greater, in some embodiments about 0.5% to about 10%, and in some embodiments about 0.6% to about 3.5%; and / or a flexural modulus of about 5,000 MPa to about 20,000 MPa, in some embodiments about 8,000 MPa to about 20,000 MPa, and in some embodiments about 10,000 MPa to about 15,000 MPa. Flexural properties may be determined at a temperature of 23° C. in accordance with 178:2019.
[0011]
[0026] As a result of the above-mentioned properties, the polymer composition can be easily formed into a substrate onto which one or more conductive elements can then be plated. Due to the beneficial properties of the polymer composition, the resulting substrate may have a very small size, such as a thickness of about 5 millimeters or less, in some embodiments about 4 millimeters or less, in some embodiments about 2 millimeters or less, and in some embodiments about 0.1 to about 1 millimeter. If desired, the conductive element may be an antenna (e.g., an antenna resonating element), whereby the resulting part is an antenna system that may be utilized in a wide variety of different electronic components, such as mobile phones, in-vehicle devices, and the like.
[0012]
[0027] Various embodiments of the invention will now be described in more detail. I. Polymer Composition A. Polymer Matrix
[0028] The polymer matrix includes one or more thermotropic liquid crystal polymers. Liquid crystal polymers generally have a rod-like structure and are classified as "thermotropic" as long as they are capable of exhibiting crystalline behavior in the molten state (e.g., in a thermotropic nematic state). Liquid crystal polymers utilized in the polymer composition typically have a melting temperature of about 280°C to about 400°C, in some embodiments about 300°C to about 380°C, and in some embodiments about 320°C to about 370°C. The melting temperature may be determined as known in the art using, for example, differential scanning calorimetry ("DSC") as determined by ISO 11357-3:2018. Such polymers may be formed from one or more types of repeating units as known in the art. Liquid crystal polymers may, for example, generally be represented by the following formula (I):
[0013] [ka]
[0014] (In the formula, Ring B is a substituted or unsubstituted 6-membered aryl group (e.g., 1,4-phenylene or 1,3-phenylene), a substituted or unsubstituted 6-membered aryl group fused with a substituted or unsubstituted 5- or 6-membered aryl group (e.g., 2,6-naphthalene), or a substituted or unsubstituted 6-membered aryl group linked to a substituted or unsubstituted 5- or 6-membered aryl group (e.g., 4,4-biphenylene); Y1 and Y2 are independently O, C(O), NH, C(O)HN, or NHC(O). The aromatic ester may contain one or more aromatic ester repeat units represented by:
[0015]
[0029] Typically, at least one of Y1 and Y2 is C(O). Examples of such aromatic ester repeat units include, for example, aromatic dicarboxylic acid repeat units (Y1 and Y2 in formula I are C(O)), aromatic hydroxycarboxylic acid repeat units (Y1 in formula I is O and Y2 is C(O)), and various combinations thereof.
[0016]
[0030] For example, aromatic hydroxycarboxylic acid repeat units derived from aromatic hydroxycarboxylic acids such as 4-hydroxybenzoic acid, 4-hydroxy-4'-biphenylcarboxylic acid, 2-hydroxy-6-naphthoic acid, 2-hydroxy-5-naphthoic acid, 3-hydroxy-2-naphthoic acid, 2-hydroxy-3-naphthoic acid, 4'-hydroxyphenyl-4-benzoic acid, 3'-hydroxyphenyl-4-benzoic acid, 4'-hydroxyphenyl-3-benzoic acid, and the like, as well as alkyl, alkoxy, aryl, and halogen substituted versions thereof, and combinations thereof, may be utilized. Particularly suitable aromatic hydroxycarboxylic acids are 4-hydroxybenzoic acid ("HBA") and 6-hydroxy-2-naphthoic acid (HNA). When utilized, repeat units derived from hydroxycarboxylic acids (e.g., HBA and / or HNA) typically comprise from about 20 mol.% to about 85 mol.%, in some embodiments from about 30 mol.% to about 80 mol.%, and in some embodiments, from about 40 mol.% to 75 mol.% of the polymer.
[0017]
[0031] Aromatic dicarboxylic acid repeat units derived from aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, diphenylether-4,4'-dicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 4,4'-dicarboxybiphenyl, bis(4-carboxyphenyl)ether, bis(4-carboxyphenyl)butane, bis(4-carboxyphenyl)ethane, bis(3-carboxyphenyl)ether, bis(3-carboxyphenyl)ethane, and the like, as well as alkyl, alkoxy, aryl, and halogen substituted versions thereof, and combinations thereof, may also be utilized. Particularly suitable aromatic dicarboxylic acids can include, for example, terephthalic acid ("TA"), isophthalic acid ("IA"), and 2,6-naphthalenedicarboxylic acid ("NDA"). When utilized, repeat units derived from aromatic dicarboxylic acids (e.g., IA, TA and / or NDA) typically comprise from about 1 mol.% to about 50 mol.%, in some embodiments from about 5 mol.% to about 40 mol.%, and in some embodiments, from about 10 mol.% to about 35 mol.% of the polymer.
[0018]
[0032] Other repeat units can also be utilized in the polymer. For example, in certain embodiments, repeat units derived from aromatic diols such as hydroquinone, resorcinol, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 4,4'-dihydroxybiphenyl (or 4,4'-biphenol), 3,3'-dihydroxybiphenyl, 3,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl ether, bis(4-hydroxyphenyl)ethane, and the like, as well as alkyl, alkoxy, aryl, and halogen substituted versions thereof, and combinations thereof, may be utilized. Particularly suitable aromatic diols can include, for example, hydroquinone ("HQ") and 4,4'-biphenol ("BP"). When utilized, repeat units derived from aromatic diols (e.g., HQ and / or BP) typically comprise from about 1 mol.% to about 50 mol.%, in some embodiments from about 5 mol.% to about 40 mol.%, and in some embodiments from about 10 mol.% to about 35 mol.% of the polymer. Repeat units such as those derived from aromatic amides (e.g., acetaminophen ("APAP")), and / or aromatic amines (e.g., 4-aminophenol ("AP"), 3-aminophenol, 1,4-phenylenediamine, 1,3-phenylenediamine, etc.) may also be utilized. When utilized, repeat units derived from aromatic amides (e.g., APAP) and / or aromatic amines (e.g., AP) typically comprise from about 0.1 mol.% to about 20 mol.%, in some embodiments from about 0.5 mol.% to about 15 mol.%, and in some embodiments from about 1 mol.% to about 10% of the polymer. It should also be understood that various other monomeric repeat units may be incorporated into the polymer. For example, in certain embodiments, a polymer may contain one or more repeat units derived from non-aromatic monomers, such as aliphatic or alicyclic hydroxycarboxylic acids, dicarboxylic acids, diols, amides, amines, etc. Of course, in other embodiments, the polymer may be "fully aromatic" in that it does not include repeat units derived from non-aromatic (e.g., aliphatic or alicyclic) monomers.
[0019]
[0033] Although not required, at least one liquid crystal polymer is utilized in a polymer matrix that is a "high naphthenic" polymer to the extent that it contains a relatively high content of repeat units derived from naphthenic hydroxycarboxylic acids and naphthenic dicarboxylic acids, such as NDA, HNA, or a combination thereof. That is, the total amount of repeat units derived from naphthenic hydroxycarboxylic acids and / or dicarboxylic acids (e.g., NDA, HNA, or a combination of HNA and NDA) is typically about 10 mol.% or more of the polymer, in some embodiments about 15 mol.% or more, in some embodiments about 20 mol.% to about 80 mol.%, in some embodiments about 30 mol.% to about 70 mol.%, in some embodiments about 40 mol.% to about 60 mol.%. In contrast to many conventional "low naphthenic" polymers, it is believed that the resulting "high naphthenic" polymers can exhibit good thermal and mechanical properties.
[0020]
[0034] In a particular embodiment, for example, the liquid crystal polymer may contain repeat units derived from HNA in an amount of 20 mol.% to about 80 mol.%, in some embodiments, about 30 mol.% to about 70 mol.%, and in some embodiments, about 40 mol.% to about 60 mol.%. The liquid crystal polymer may also contain various other monomers. For example, the polymer may contain repeat units derived from HBA in an amount of about 0.1 mol.% to about 15 mol.%, in some embodiments, about 0.5 mol.% to about 10 mol.%, and in some embodiments, about 1 mol.% to about 5 mol.%. When utilized, the molar ratio of repeat units derived from HBA to repeat units derived from HNA may be selectively controlled within a particular range to help achieve desired properties, for example, about 5 to about 40, in some embodiments, about 10 to about 35, and in some embodiments, about 20 to about 30. The polymer may also include repeat units derived from aromatic dicarboxylic acids (e.g., IA and / or TA) in an amount of about 10 mol.% to about 40 mol.%, in some embodiments about 20 mol.% to about 30 mol.%; and / or aromatic diols (e.g., BP and / or HQ) in an amount of about 10 mol.% to about 40 mol.%, in some embodiments about 20 mol.% to about 30 mol.%. However, in some cases, it may be desirable to minimize the presence of such monomers in the polymer to help achieve desired properties. For example, the total amount of repeat units derived from aromatic dicarboxylic acids (e.g., IA and / or TA) and / or aromatic diols (e.g., BP and / or HQ) may be about 5 mol.% or less, in some embodiments about 4 mol.% or less, in some embodiments about 0.1 mol.% to about 3 mol.% of the polymer.
[0021]
[0035] Regardless of the specific components and properties of the polymer, the liquid crystal polymer can be prepared by first introducing aromatic monomers used to form the ester repeat units (e.g., aromatic hydroxycarboxylic acids, aromatic dicarboxylic acids, etc.) and / or other repeat units (e.g., aromatic diols, aromatic amides, aromatic amines, etc.) into a reaction vessel to initiate a polycondensation reaction. The specific conditions and steps utilized in such reactions are well known and may be described in more detail in U.S. Pat. No. 4,161,470 to Calundann, U.S. Pat. No. 5,616,680 to Linstid, III et al., U.S. Pat. No. 6,114,492 to Linstid, III et al., U.S. Pat. No. 6,514,611 to Shepherd et al., and WO 2004 / 058851 to Waggoner. The vessel utilized in the reaction is not particularly limited, but it is typically desirable to utilize one commonly used for reactions of highly viscous fluids. Examples of such reaction vessels include agitation tank-type apparatuses having agitators equipped with agitation blades of various shapes, such as anchor type, multi-stage type, spiral ribbon type, screw shaft type, and modified shapes thereof. Further examples of such reaction vessels include mixing apparatuses commonly used for resin kneading, such as kneaders, roll mills, and Banbury mixers.
[0022]
[0036] If desired, the reaction can proceed by acetylation of the monomer as known in the art. This can be accomplished by adding an acetylating agent (e.g., acetic anhydride) to the monomer. Acetylation is generally initiated at a temperature of about 90° C. In the early stages of acetylation, reflux may be utilized to maintain the vapor phase temperature below the point where the acetic acid by-product and anhydride begin to distill. The temperature during acetylation typically ranges from 90° C. to 150° C., in some embodiments from about 110° C. to about 150° C. If reflux is used, the vapor phase temperature typically exceeds the boiling point of acetic acid, but remains low enough to retain residual acetic anhydride. For example, acetic anhydride vaporizes at a temperature of about 140° C. Thus, it is particularly desirable to provide the reactor with a vapor phase reflux at a temperature of about 110° C. to about 130° C. An excess of acetic anhydride can be utilized to ensure a substantially complete reaction. The amount of excess anhydride will vary depending on the particular acetylation conditions utilized, including the presence or absence of reflux. It is not uncommon to use an excess of about 1 to about 10 mole percent acetic anhydride, based on the total moles of reactant hydroxyl groups present.
[0023]
[0037] Acetylation may be carried out in a separate reaction vessel or in situ in the polymerization reaction vessel. If a separate reaction vessel is utilized, one or more of the monomers may be introduced into the acetylation reactor and then transferred to the polymerization reactor. Similarly, one or more of the monomers may be introduced directly into the reaction vessel without prior acetylation.
[0024]
[0038] In addition to the monomer and optional acetylating agent, other components that help promote polymerization may also be included in the reaction mixture. For example, catalysts such as metal salt catalysts (e.g., magnesium acetate, tin(I) acetate, tetrabutyl titanate, lead acetate, sodium acetate, potassium acetate, etc.) and organic compound catalysts (e.g., N-methylimidazole) can be optionally utilized. Such catalysts are typically used in amounts of about 50 to about 500 parts per million based on the total weight of the repeat unit precursor. When separate reactors are utilized, it is typically desirable to apply the catalyst to the acetylation reactor rather than the polymerization reactor, although this is by no means required.
[0025]
[0039] The reaction mixture is generally heated to an elevated temperature in a polymerization reactor vessel to initiate melt polycondensation of the reactants. The polycondensation may be carried out within a temperature range of, for example, about 200°C to about 400°C. For example, one suitable technique for forming aromatic polyesters may include charging the precursor monomers and acetic anhydride to a reactor, heating the mixture to a temperature of about 90°C to about 150°C to acetylate the hydroxyl groups of the monomers (e.g., to form acetoxy), and then increasing the temperature to about 200°C to about 400°C to carry out melt polycondensation. As the final polymerization temperature is approached, the volatile by-products of the reaction (e.g., acetic acid) can also be removed, thereby making it easier to achieve the desired molecular weight. The reaction mixture is generally subjected to stirring during polymerization to ensure good heat and mass transfer, and thus good material homogeneity. The rotation speed of the stirrer may vary over the course of the reaction, but typically ranges from about 10 to about 100 revolutions per minute ("rpm"), and in some embodiments, from about 20 to about 80 rpm. To increase the molecular weight of the melt, the polymerization reaction may be carried out under a vacuum, the application of which facilitates the removal of volatile materials formed in the final stages of polycondensation. The vacuum may be created by application of suction pressures, such as within the range of about 5 to about 30 pounds per square inch ("psi"), and in some embodiments, about 10 to about 20 psi.
[0026]
[0040] After melt polymerization, the molten polymer may be discharged from the reactor through an extrusion orifice, typically with a die of the desired shape, and cooled and collected. Generally, the melt is discharged through a perforated die to form strands that are captured in a water bath, pelletized, and dried. In some embodiments, the melt-polymerized polymer may also be subjected to a subsequent solid-state polymerization process to further increase its molecular weight. The solid-state polymerization may be carried out in the presence of a gas (e.g., air, an inert gas, etc.). Suitable inert gases may include, for example, nitrogen, helium, argon, neon, krypton, xenon, etc., and combinations thereof. The solid-state polymerization reaction vessel may be of virtually any design that allows the polymer to be maintained at the desired solid-state polymerization temperature for the desired residence time. Examples of such vessels may have fixed beds, stationary beds, moving beds, fluidized beds, etc. The temperature at which the solid-state polymerization is carried out may vary, but is typically in the range of about 200°C to about 400°C. The polymerization time will, of course, vary based on the temperature and the target molecular weight. In most cases, however, the solid state polymerization time is from about 2 hours to about 12 hours, and in some embodiments, from about 4 hours to about 10 hours.
[0027]
[0041] The total amount of liquid crystal polymer utilized in the polymer composition is typically about 50 wt.% to about 99 wt.%, in some embodiments about 60 wt.% to about 98 wt.%, and in some embodiments about 70 wt.% to about 95 wt.% of the total polymer composition. In certain embodiments, all of the liquid crystal polymers are "high naphthenic" polymers as described above. However, in other embodiments, "low naphthenic" liquid crystal polymers can also be utilized in the composition, in which the total amount of repeat units derived from naphthenic hydroxycarboxylic acids and / or dicarboxylic acids (e.g., NDA, HNA, or a combination of HNA and NDA) is less than 10 mol.%, in some embodiments about 8 mol.% or less, in some embodiments about 6 mol.% or less, and in some embodiments about 1 mol.% to about 5 mol.% of the polymer. When utilized, it is generally desirable that such low naphthenic polymers are present in relatively low amounts. For example, when utilized, the low naphthene liquid crystalline polymer typically comprises from about 1 wt.% to about 50 wt.%, in some embodiments from about 10 wt.% to about 45 wt.%, in some embodiments from about 20 wt.% to about 40 wt.%, and in some embodiments from about 0.5 wt.% to about 45 wt.%, in some embodiments from about 2 wt.% to about 35 wt.%, and in some embodiments from about 5 wt.% to about 25 wt.% of the total amount of liquid crystalline polymer in the composition. In contrast, the high naphthene liquid crystalline polymer typically comprises from about 50 wt.% to about 99 wt.%, in some embodiments from about 55 wt.% to about 95 wt.%, in some embodiments from about 60 wt.% to about 90 wt.%, and in some embodiments from about 25 wt.% to about 65 wt.%, in some embodiments from about 30 wt.% to about 60 wt.%, and in some embodiments from about 35 wt.% to about 55 wt.% of the total amount of liquid crystalline polymer in the composition.
[0028] B. Precious Metal Catalyst
[0042] As indicated above, the polymer composition includes a precious metal catalyst, which may serve to facilitate the subsequent plating of the composition. The precious metal catalyst typically includes a precious metal component, such as one selected from Groups IB, VIIA and VIIIA of the Periodic Table (IUPAC Table), which generally have an atomic weight of at least 100. Examples of such precious metal components include palladium, ruthenium, rhodium, iridium, platinum, and alloys or combinations of any of the foregoing. Palladium is particularly preferred. To help improve the physical strength of the catalyst, the precious metal component is also typically supported by a matrix material, such as an inorganic metal oxide. Suitable inorganic metal oxides for this purpose include, for example, silica, alumina, silica-alumina, magnesia, silica-magnesia, silica-zirconia, silica-thoria, silica-beryllia, silica-titania, silica-alumina-thoria, silica-alumina-zirconia, silica-alumina-magnesia, silica-magnesia-zirconia, halloysite, kaolinite, illite, montmorillonite, vermiculite, palygorskite, pyrophyllite, calcium silicate, aluminum silicate, wollastonite, and the like. Natural and / or synthetic silicate minerals such as kaolinite are particularly suitable. The matrix material may be a mixture of simple or complex ions of the selected metal component (e.g., Pd(NH3)4 2+ The precious metal component may be combined with the matrix material in a variety of ways, such as by impregnation or ion exchange (or both), using a solution of the complex cation, such as ZnO, Fe, FeNb, FeNbO ...
[0029]
[0043] The total amount of catalyst utilized in the polymeric composition is generally such that the precious metal component comprises from about 0.1 parts by weight to about 6 parts by weight, in some embodiments from about 0.2 parts by weight to about 4 parts by weight, and in some embodiments from about 0.5 parts by weight to about 2.5 parts by weight per 100 parts by weight of the polymeric matrix. For example, the precious metal component may comprise from about 0.1 wt.% to about 5 wt.%, in some embodiments from about 0.2 wt.% to about 3 wt.%, and in some embodiments from about 0.4 wt.% to about 1.5 wt.% of the polymeric composition. Thus, the actual amount of catalyst utilized in the composition will depend on the amount of precious metal component utilized in the catalyst. Typically, the precious metal component comprises from about 0.01 wt.% to about 3 wt.%, in some embodiments from about 0.05 wt.% to about 1 wt.%, and in some embodiments from about 0.1 wt.% to about 0.8 wt.% of the catalyst. In such embodiments, the catalyst comprises from about 0.5 parts by weight to about 20 parts by weight, in some embodiments from about 1 part by weight to about 15 parts by weight, and in some embodiments from about 2 parts by weight to about 10 parts by weight, per 100 parts by weight of the polymer matrix. For example, the catalyst may comprise from about 0.1 wt.% to about 15 wt.%, in some embodiments from about 0.5 wt.% to about 10 wt.%, and in some embodiments from about 1 wt.% to about 6 wt.% of the polymer composition.
[0030] C. Optional Additives i. Mineral Fillers
[0044] The polymeric composition may optionally include one or more mineral fillers distributed within the polymeric matrix. When utilized, such mineral fillers typically comprise from about 1 part by weight to about 60 parts by weight, in some embodiments from about 5 parts by weight to about 50 parts by weight, and in some embodiments from about 15 parts by weight to about 35 parts by weight per 100 parts by weight of the polymeric matrix. For example, the mineral filler may comprise from about 1 wt.% to about 50 wt.%, in some embodiments from about 5 wt.% to about 40 wt.%, and in some embodiments from about 10 wt.% to about 30 wt.% of the polymeric composition. The nature of the mineral fillers utilized in the polymeric composition may vary, such as mineral particles, mineral fibers (or "whiskers"), and the like, and blends thereof. Typically, the mineral fillers utilized in the polymeric composition have a particular hardness value to help improve the mechanical strength, adhesive strength, and surface properties of the composition. For example, the hardness value may be about 2.0 or greater, in some embodiments about 2.5 or greater, in some embodiments about 3.0 or greater, in some embodiments about 3.0 to about 11.0, in some embodiments about 3.5 to about 11.0, and in some embodiments about 4.5 to about 6.5 on the Mohs hardness scale.
[0031]
[0045] Any of a variety of different types of mineral particles may generally be utilized in the polymer compositions, such as those formed from natural and / or synthetic silicate minerals, such as talc, mica, silica (e.g., amorphous silica), alumina, halloysite, kaolinite, illite, montmorillonite, vermiculite, palygorskite, pyrophyllite, calcium silicate, aluminum silicate, wollastonite, and the like; sulfates; carbonates; phosphates; fluorides, borates, and the like. Particularly preferred are particles having the desired hardness values, such as calcium carbonate (CaCO3, Mohs hardness 3.0), copper hydroxide carbonate (Cu2CO3(OH)2, Mohs hardness 4.0); calcium fluoride (CaFl2, Mohs hardness 4.0); calcium pyrophosphate ((Ca2P2O7, Mohs hardness 5.0), dicalcium phosphate anhydrous (CaHPO4, Mohs hardness 3.5), hydrated aluminum phosphate (AlPO4·2H2O, Mohs hardness 4.5); silica (SiO2, Mohs hardness 5.0); hardness 5.0-6.0), potassium aluminum silicate (KAlSi3O8, Mohs hardness 6), copper silicate (CuSiO3·H2O, Mohs hardness 5.0); calcium borosilicate hydroxide (Ca2B5SiO9(OH)5, Mohs hardness 3.5); alumina (AlO2, Mohs hardness 10.0); calcium sulfate (CaSO4, Mohs hardness 3.5), barium sulfate (BaSO4, Mohs hardness 3-3.5), mica (Mohs hardness 2.5-5.3), and combinations thereof.
[0032]
[0046] In certain embodiments, it may be desirable to utilize mineral fillers that are "flaky" to improve the surface and mechanical properties of the composition. In such embodiments, the particles generally have a relatively high aspect ratio (e.g., average diameter divided by average thickness), such as about 4 or more, in some embodiments about 10 or more, and in some embodiments, about 40 to about 250. The average diameter of the particles may range, for example, from about 5 micrometers to about 200 micrometers, in some embodiments from about 8 micrometers to about 150 micrometers, and in some embodiments, from about 10 micrometers to about 100 micrometers, as determined using laser diffraction techniques, for example, according to ISO 13320:2009 (e.g., using a Horiba LA-960 particle size distribution analyzer). The average thickness may similarly be about 2 micrometers or less, in some embodiments from about 5 nanometers to about 1 micrometer, and in some embodiments, from about 20 nanometers to about 500 nanometers. The flake particles are typically formed from natural and / or synthetic silicate minerals such as mica, halloysite, kaolinite, illite, montmorillonite, vermiculite, palygorskite, pyrophyllite, calcium silicate, aluminum silicate, wollastonite, and the like. For example, mica is particularly suitable. Any form of mica can generally be utilized, such as muscovite (KAl2(AlSi3)O 10 (OH)2), biotite (K(Mg,Fe)3(AlSi3)O 10 (OH)2), phlogopite (KMg3(AlSi3)O 10 (OH)2), red mica (K(Li,Al) 2-3 (AlSi3)O 10 (OH)2), glauconite (K,Na)(Al,Mg,Fe)2(Si,Al)4O 10 (OH)2). Muscovite micas are particularly suitable for use in polymer compositions.
[0033]
[0047] Of course, in other embodiments, the mineral particles may have a shape that is generally granular or nodular in nature. In such embodiments, the particles may have a median size (e.g., diameter) of about 0.5 to about 20 micrometers, in some embodiments about 1 to about 15 micrometers, in some embodiments about 1.5 to about 10 micrometers, and in some embodiments about 2 to about 8 micrometers, as determined using laser diffraction techniques (e.g., using a Horiba LA-960 particle size distribution analyzer) according to, for example, ISO 13320:2009. Examples of such granular particles include, for example, barium sulfate. Mineral fibers may also be utilized, such as those derived from silicates, such as neosilicates, sorosilicates, inosilicates (e.g., calcium inosilicates such as wollastonite; calcium magnesium inosilicates such as tremolite; calcium magnesium iron inosilicates such as yangtite; magnesium iron inosilicates such as anthophyllite, etc.), phyllosilicates (e.g., aluminum phyllosilicates such as palygorskite), tectosilicates, etc.; sulfates, such as calcium sulfate (e.g., dehydrated or anhydrous gypsum); mineral wools (e.g., rock or slag wool), etc. Particularly suitable are fibers having the desired hardness values, including fibers derived from inosilicates, such as wollastonite (Mohs hardness 4.5-5.0), available from Nyco Minerals under the trade name Nyglos® (e.g., Nyglos® 4W or Nyglos® 8). The mineral fibers may have a median width (e.g., diameter) of about 1 to about 35 micrometers, in some embodiments about 2 to about 20 micrometers, in some embodiments about 3 to about 15 micrometers, and in some embodiments about 7 to about 12 micrometers. The mineral fibers may also have a narrow size distribution, i.e., at least about 60% by volume of the fibers, in some embodiments at least about 70% by volume of the fibers, and in some embodiments at least about 80% by volume of the fibers may have a size within the above-mentioned ranges.In addition to having the size characteristics described above, the mineral fibers may also have a relatively high aspect ratio (average length divided by median width) to help further improve the mechanical properties and surface quality of the resulting polymer composition. For example, the mineral fibers may have an aspect ratio of about 2 to about 100, in some embodiments about 2 to about 50, in some embodiments about 3 to about 20, and in some embodiments about 4 to about 15. The volume average length of such mineral fibers may range, for example, from about 1 to about 200 micrometers, in some embodiments about 2 to about 150 micrometers, in some embodiments about 5 to about 100 micrometers, and in some embodiments about 10 to about 50 micrometers.
[0034] ii. Glass fiber
[0048] One beneficial aspect of the present invention is that good dielectric properties can be achieved without adversely affecting the mechanical properties of the resulting part. To help ensure that such properties are maintained, it is generally desirable for the polymer composition to remain substantially free of traditional fibrous fillers, such as glass fibers. Thus, if utilized, glass fibers typically comprise no more than about 10 wt.%, in some embodiments no more than about 5 wt.%, and in some embodiments, from about 0.001 wt.% to about 3 wt.% of the polymer composition.
[0035] iii. Optional Additives
[0049] A wide variety of other additional additives may also be included in the polymer composition, such as lubricants, conductive fillers (e.g., carbon fiber, graphite, etc.), thermally conductive fillers (e.g., carbon black, graphite, boron nitride, etc.), pigments, antioxidants, stabilizers, surfactants, waxes, flame retardants, anti-sag additives, nucleating agents (e.g., boron nitride), tribological agents (e.g., fluoropolymers), antistatic fillers (e.g., carbon black, carbon nanotubes, carbon fiber, graphite, ionic liquids, etc.), and other materials added to improve properties and processability. For example, lubricants that can withstand the processing conditions of liquid crystal polymers without substantial degradation can be utilized in the polymer composition. Examples of such lubricants include fatty acid esters, salts thereof, esters, fatty acid amides, organophosphate esters, and hydrocarbon waxes of the type typically used as lubricants in the processing of engineering plastic materials, including mixtures thereof. Suitable fatty acids typically have a backbone carbon chain of about 12 to about 60 carbon atoms, such as myristic acid, palmitic acid, stearic acid, arachic acid, montanic acid, octadecinic acid, parinaric acid, etc. Suitable esters include fatty acid esters, fatty alcohol esters, wax esters, glycerol esters, glycol esters, and complex esters. Fatty acid amides include fatty acid primary amides, fatty acid secondary amides, methylene and ethylene bisamides, and alkanolamides, such as palmitic acid amide, stearic acid amide, oleic acid amide, N,N'-ethylene bisstearamide, etc. Also suitable are metal salts of fatty acids, such as calcium stearate, zinc stearate, magnesium stearate, etc.; hydrocarbon waxes, including paraffin wax, polyolefin and oxidized polyolefin waxes, and microcrystalline waxes. Particularly suitable lubricants are stearic acids, salts or amides, such as pentaerythritol tetrastearate, calcium stearate, or N,N'-ethylenebisstearamide.If utilized, the lubricant typically comprises from about 0.05 wt.% to about 1.5 wt.%, and in some embodiments from about 0.1 wt.% to about 0.5 wt.% (by weight) of the polymer composition.
[0036] II. formation
[0050] The components used to form the polymer composition may be combined together using any of a variety of different techniques, as known in the art. In one particular embodiment, for example, the liquid crystal polymer, the precious metal catalyst, and any other additives are melt processed as a mixture in an extruder to form the polymer composition. The mixture may be melt kneaded in a single or multiple screw extruder at a temperature of about 250°C to about 450°C. In one embodiment, the mixture may be melt processed in an extruder that includes multiple temperature zones. The temperature of the individual zones is typically set within a range of about -60°C to about 25°C relative to the melt temperature of the liquid crystal polymer. By way of example, the mixture may be melt processed using a twin screw extruder, such as a Leistritz 18mm co-rotating fully intermeshing twin screw extruder. The mixture may be melt processed using a versatile screw design. In one embodiment, the mixture containing all of the components may be fed by a volumetric feeder to a feed port in the first barrel. In another embodiment, different components may be added at different addition points in the extruder, as is known. For example, the liquid crystal polymer may be applied at a feed port and certain additives (e.g., precious metal catalysts) may be fed at the same or different temperature zones downstream therefrom. Regardless, the resulting mixture may be melted, mixed, and then extruded through a die. The extruded polymer composition may then be quenched in a water bath to solidify, pelletized in a pelletizer, and then dried.
[0037] III. Molded Interconnect Devices
[0051] In certain embodiments, the polymer composition may be utilized to mold interconnect devices. For example, the device may include a substrate comprising the polymer composition of the present invention and one or more conductive elements plated thereon. The substrate may be formed using a variety of different molding techniques. Suitable techniques may include, for example, injection molding, low pressure injection molding, extrusion compression molding, gas injection molding, foam injection molding, low pressure gas injection molding, low pressure foam injection molding, gas extrusion compression molding, foam extrusion compression molding, extrusion molding, foam extrusion molding, compression molding, foam compression molding, gas compression molding, insert molding, pin insert molding, and the like. For example, an injection molding system may be utilized that includes a mold into which the polymer composition can be injected. The time in the injector may be controlled and optimized to prevent pre-solidification of the polymer matrix. Once the cycle time is reached and the barrel is full for ejection, a piston may be used to inject the composition into the mold cavity. Compression molding systems may also be utilized. Similar to injection molding, the shaping of the polymer composition into the desired article also occurs in a mold. The composition may be placed into a compression mold using any known technique, for example by being picked up by an automated robotic arm. The temperature of the mold may be maintained at or above the solidification temperature of the polymer matrix for a desired time to allow solidification. The molded product may then be solidified by bringing it to a temperature below that of the melting temperature. The resulting product may be demolded. The cycle time of each molding process may be adjusted to suit the polymer matrix, achieve sufficient bonding, and improve the productivity of the overall process.
[0038]
[0052] The conductive elements may be deposited on the substrate using any of a variety of known plating techniques, such as electrolytic plating, electroless plating, digital printing, aerosol jet printing, and the like. The conductive elements may include one or more of a variety of conductive materials, such as metals, e.g., gold, silver, nickel, aluminum, copper, and mixtures or alloys thereof. In one embodiment, for example, the conductive elements may include copper and / or nickel (e.g., pure or alloys thereof). If desired, a seed layer may be formed on the substrate first to facilitate the plating process. Methods for forming the desired interconnect pattern may vary as known to those skilled in the art. For example, in certain cases, a pattern may first be formed on the surface of the substrate based on the desired circuit interconnect pattern. This may be accomplished using a variety of known techniques, such as laser ablation or patterning, plasma etching, ultraviolet light treatment, acid etching, and the like. After formation, the resulting interconnect pattern may be plated with the desired conductive elements. However, in other cases, the surface of the substrate (e.g., the entire surface) may be plated and then ablated using techniques such as those mentioned above to form the desired interconnect pattern. In one embodiment, for example, the plated surface may be laser ablated to form the desired interconnect pattern.
[0039]
[0053] Regardless of the method utilized, the method by which the surface is plated may also be selected based on techniques known in the art. In one embodiment, for example, the surface of the substrate may be contacted with an activation solution containing a precious metal, such as palladium, platinum, iridium, rhodium, and mixtures thereof. Palladium is particularly preferred. The presence of a precious metal catalyst in the polymer composition allows the activation solution to exhibit good adhesion to the substrate for the subsequent plating operation. Of course, in certain cases, the precious metal catalyst itself may function as an activator so that a subsequent solution is not required. In any case, after the optional activation step, a first metal layer may be formed thereon on the substrate, such as by electroless and / or electrolytic plating. Electroless plating may occur by an autocatalytic reaction in which the metal deposited on the surface acts as a catalyst for further deposition. Typically, nickel and / or copper are electrolessly plated on the surface of the substrate. Electroless nickel plating may be achieved, for example, using a solution containing a nickel salt (e.g., nickel sulfate). Electrolytic plating may also be utilized in which the substrate is contacted with a metal solution and subjected to an electric current to initiate deposition of the metal. If desired, the substrate surface may be roughened prior to plating using various known techniques, such as laser ablation, plasma etching, ultraviolet treatment, fluorination, etc. Among other things, such roughening helps to facilitate plating in the desired interconnect pattern. In addition, the substrate may also be subjected to one or more additional steps to form a final metal coating layer. For example, a second metal layer may be electrolytically deposited on the first metal layer (e.g., electrolytically and / or electrolessly plated copper and / or nickel). The second metal layer may include, for example, copper or nickel. In certain embodiments, one or more additional metal layers, such as copper and / or nickel, may also be electrolytically deposited on the second metal layer.
[0040] IV. Antenna Systems
[0054] The molded interconnect device may be particularly suitable for use in antenna systems. In such embodiments, the plated conductive element may be an antenna element (e.g., an antenna resonating element). The conductive elements may form a variety of different types of antennas, such as patch antenna elements, inverted-F antenna elements, closed and open slot antenna elements, loop antenna elements, antennas having resonating elements formed from monopoles, dipoles, planar inverted-F antenna elements, hybrids of these designs, and the like. The resulting antenna system may be utilized in a variety of different electronic components. By way of example, the antenna system may be formed in electronic components such as desktop computers, portable computers, handheld electronic devices, vehicle mounted equipment, and the like. In one preferred configuration, the antenna system is formed within the housing of a relatively compact portable electronic component having a relatively small amount of available interior space. Examples of suitable portable electronic components include mobile phones, laptop computers, small portable computers (e.g., ultraportable computers, netbook computers, and tablet computers), wristwatch devices, pendant devices, headphone and earphone devices, media players with wireless communication capabilities, handheld computers (sometimes referred to as personal digital assistants), remote controllers, global positioning system (GPS) devices, handheld gaming devices, and the like. The antenna may be integrated with other parts of the handheld device, such as the camera module, speaker or battery cover.
[0041]
[0055] One particularly suitable electronic component shown in Figures 1-2 is a handheld device 10 with cellular telephone functionality. As shown in Figure 1, the device 10 may have a housing 12 formed from plastic, metal, other suitable dielectric material, other suitable conductive material, or a combination of such materials. A display 14, such as a touch screen display, may be provided on the front side of the device 10. The device 10 may also have a speaker port 40 and other input / output ports. One or more buttons 38 and other user input devices may be used to collect user input. As shown in Figure 2, an antenna system 26 is also provided on a rear side 42 of the device 10, although it should be understood that the antenna system may generally be positioned at any desired location on the device. The antenna system may be electrically connected to other components within the electronic device using any of a variety of known techniques. Referring again to Figures 1-2, for example, the housing 12 or a portion of the housing 12 may serve as a conductive ground plane for the antenna system 26. This is more particularly shown in Figure 3, which shows antenna system 26 being powered by a radio frequency source 52 at a positive antenna feed terminal 54 and a ground antenna feed terminal 56. Positive antenna feed terminal 54 may be coupled to an antenna resonating element 58, and ground antenna feed terminal 56 may be coupled to a ground element 60. Resonating element 58 may have a main arm 46 and a shorting branch 48 connecting main arm 46 to ground 60.
[0042]
[0056] Various other configurations for electrically connecting the antenna system are also contemplated. For example, in FIG. 4, the antenna system is based on a monopole antenna configuration, with the resonating element 58 having a serpentine serpentine shape. In such an embodiment, the feed terminal 54 may be connected to one end of the resonating element 58, and the ground feed terminal 56 may be coupled to the housing 12 or another suitable ground plane element. In another embodiment shown in FIG. 5, the conductive antenna element 62 is configured to define a closed slot 64 and an open slot 66. The antenna formed from the structure 62 may be fed using the positive antenna feed terminal 54 and the ground antenna feed terminal 56. In this type of arrangement, the slots 64 and 66 serve as antenna resonating elements for the antenna element 26. The size of the slots 64 and 66 may be configured so that the antenna element 26 operates in a desired communication band (e.g., 2.4 GHz and 5 GHz, etc.). Another possible configuration of the antenna system 26 is shown in FIG. 6. In this embodiment, antenna element 26 has a patch antenna resonating element 68 and may be fed using positive antenna feed terminal 54 and ground antenna feed terminal 56. Ground 60 may be coupled to housing 12 or other suitable ground plane element of device 10. FIG. 7 illustrates yet another exemplary configuration that may be used for antenna elements of antenna system 26. As shown, antenna resonating element 58 has two main arms 46A and 46B. Arm 46A is shorter than arm 46B and is therefore associated with a higher operating frequency than arm 46A. By using two or more separate resonating element structures of different sizes, antenna resonating element 58 may be configured to cover a wider bandwidth or more than a single communications band of interest.
[0043]
[0057] In certain embodiments of the present invention, the polymeric compositions may be particularly well suited for radio frequency antennas and antenna arrays for use in base stations, repeaters (e.g., "femtocells"), relay stations, terminals, user devices, and / or other suitable components of 5G systems. As used herein, "5G" generally refers to high speed data communication via radio frequency signals. 5G networks and systems can communicate data at much faster rates than previous generation data communication standards (e.g., "4G," "LTE"). For example, as used herein, "5G frequencies" may refer to frequencies of 1.5 GHz or higher, in some embodiments about 2.0 GHz or higher, in some embodiments about 2.5 GHz or higher, in some embodiments about 3.0 GHz or higher, in some embodiments about 3 GHz to about 300 GHz or higher, in some embodiments about 4 GHz to about 80 GHz, in some embodiments about 5 GHz to about 80 GHz, in some embodiments about 20 GHz to about 80 GHz, and in some embodiments about 28 GHz to about 60 GHz. Various standards and specifications have been published that quantify the requirements for 5G communications. As an example, the International Telecommunications Union (ITU) published the International Mobile Telecommunications-2020 ("IMT-2020") standard in 2015. The IMT-2020 standard specifies various data transmission criteria for 5G (e.g., downlink and uplink data rates, latency, etc.). The IMT-2020 standard defines uplink and downlink peak data rates as the minimum data rates for uploading and downloading data that a 5G system must support. The IMT-2020 standard specifies a downlink peak data rate requirement of 20 Gbit / s, and an uplink peak data rate of 10 Gbit / s. As another example, the 3G LTE standard specifies a 5G LTE standard for 5G LTE. rdThe Third Generation Partnership Project (3GPP) recently announced a new standard for 5G, referred to as "5G NR." In 2018, 3GPP published "Release 15," which defines "Phase 1" for the standardization of 5G NR. 3GPP defines the 5G frequency bands as "Frequency Range 1" (FR1), which generally includes sub-6 GHz frequencies, and "Frequency Range 2" (FR2), as frequency bands in the range of 20-60 GHz. The antenna systems described herein may meet or be certified as "5G" under standards published by 3GPP, such as Release 15 (2018), and / or the IMT-2020 standard.
[0044]
[0058] To achieve high-speed data communication at high frequencies, antenna elements and arrays may utilize small feature sizes / spacings (e.g., fine pitch technology) that can improve antenna performance. For example, the feature size (spacing between antenna elements, width of antenna elements), etc., generally depends on the wavelength ("λ") of the desired transmit and / or receive radio frequency propagating through the substrate dielectric on which the antenna elements are formed (e.g., nλ / 4, where n is an integer). Additionally, beamforming and / or beamsteering may be utilized to facilitate transmission and reception across multiple frequency ranges or channels (e.g., multiple-input multiple-output (MIMO), massive MIMO).
[0045]
[0059] High frequency 5G antenna elements can have various configurations. For example, 5G antenna elements may be or include coplanar waveguide elements, patch arrays (e.g., mesh-grid patch arrays), other suitable 5G antenna configurations. Antenna elements may be configured to provide MIMO, massive MIMO functionality, beam steering, and the like. As used herein, "massive" MIMO functionality generally refers to providing a large number of transmit and receive channels by an antenna array, for example, 8 transmit (Tx) and 8 receive (Rx) channels (abbreviated as 8x8). Massive MIMO functionality may be provided at 8x8, 12x12, 16x16, 32x32, 64x64, or more.
[0046]
[0060] The antenna elements can have a variety of configurations and arrangements and can be fabricated using a variety of manufacturing techniques. As an example, the antenna elements and / or associated elements (e.g., ground elements, feedlines, etc.) can utilize fine pitch technology. Fine pitch technology generally refers to small or fine spacing between its components or leads. For example, the feature size / dimension and / or spacing between antenna elements (or between antenna elements and a ground plane) can be about 5,000 micrometers or less, in some embodiments about 3,000 micrometers or less, in some embodiments 1,500 micrometers or less, in some embodiments 750 micrometers or less (e.g., center-to-center spacing of 1.5 mm or less), 650 micrometers or less, in some embodiments 550 micrometers or less, in some embodiments 450 micrometers or less, in some embodiments 350 micrometers or less, in some embodiments 250 micrometers or less, in some embodiments 150 micrometers or less, in some embodiments 100 micrometers or less, and in some embodiments 50 micrometers or less. However, it should be understood that smaller and / or larger feature sizes and / or spacings may be utilized within the scope of the present disclosure.
[0047]
[0061] As a result of such small feature sizes, the antenna system can be implemented with a large number of antenna elements in a small footprint. For example, the antenna array may have an average antenna element density of more than 10 antenna elements per square centimeter, in some embodiments more than 50 antenna elements per square centimeter, in some embodiments more than 200 antenna elements per square centimeter, in some embodiments more than 1,000 antenna elements per square centimeter, in some embodiments more than 3,000 antenna elements per square centimeter, and in some embodiments more than about 5,000 antenna elements per square centimeter. Such a dense arrangement of antenna elements can provide a larger number of channels for MIMO functionality per unit area of antenna area. For example, the number of channels may correspond to (e.g., be equal to or proportional to) the number of antenna elements.
[0048]
[0062] 8, an embodiment of a 5G antenna system 100 is shown that includes a base station 102, one or more relay stations 104, one or more user computing devices 106, one or more Wi-Fi repeaters 108 (e.g., “femtocells”), and / or other suitable antenna components for a 5G antenna system 100. The relay stations 104 may be configured to facilitate communication with the base station 102 by the user computing devices 106 and / or other relay stations 104 by relaying or “repeat” signals between the base station 102 and the user computing devices 106 and / or the relay stations 104. The base station 102 may include a MIMO antenna array 110 configured to receive and / or transmit radio frequency signals 112 to and / or from the relay stations 104, the Wi-Fi repeaters 108, and / or directly to the user computing devices 106. The user computing devices 106 are not necessarily limited by the present invention and include devices such as 5G smartphones.
[0049]
[0063] The MIMO antenna array 110 may utilize beam steering to focus or direct the radio frequency signals 112 relative to the relay station 104. For example, the MIMO antenna array 110 may be configured to adjust an elevation angle 114 relative to the XY plane, and / or a heading angle 116 defined in the ZY plane and relative to the Z direction. Similarly, one or more of the relay station 104, user computing device 106, and Wi-Fi repeater 108 may utilize beam steering to improve reception and / or transmission capabilities for the MIMO antenna array 110 by directionally tuning the sensitivity and / or power transmission of the devices 104, 106, 108 with respect to the MIMO antenna array 110 of the base station 102 (e.g., by adjusting one or both of the relative elevation angles and / or relative azimuth angles of the respective devices).
[0050]
[0064] 9A and 9B show top and side elevation views, respectively, of an exemplary user computing device 106. The user computing device 106 may include one or more antenna elements 200, 202 (e.g., arranged as a respective antenna array). With reference to FIG. 9A, the antenna elements 200, 202 may be configured to perform beam steering in the XY plane (as illustrated by arrows 204, 206 and corresponding to the relative azimuth angles). With reference to FIG. 9B, the antenna elements 200, 202 may be configured to perform beam steering in the ZY plane (as illustrated by arrows 204, 206).
[0051]
[0065] FIG. 10 shows a simplified schematic diagram of multiple antenna arrays 302 connected (e.g., with a front-end module) using respective feed lines 304. The antenna array 302 may be attached to a side 306 of a substrate 308, which may be formed from the polymer composition of the present invention. The antenna array 302 may include multiple vertically connected elements (e.g., as a mesh grid array). Thus, the antenna array 302 may extend generally parallel to the side 306 of the substrate 308. Shielding may optionally be provided on the side 306 of the substrate 308 such that the antenna array 302 is located outside of the shielding for the substrate 308. The vertical spacing distances between the vertically connected elements of the antenna array 302 may correspond to the "feature size" of the antenna array 302. Thus, in some embodiments, these spacing distances may be relatively small (e.g., less than about 750 micrometers) such that the antenna array 302 is a "fine pitch" antenna array 302.
[0052]
[0066] FIG. 11 shows a side elevation view of a configuration of a coplanar waveguide antenna 400. One or more coplanar ground layers 402 may be arranged parallel to the antenna elements 404 (e.g., patch antenna elements). Another ground layer 406 may be spaced apart from the antenna elements 404 by a substrate 408, which may be formed from the polymer composition of the present invention. One or more additional antenna elements 410 may be spaced apart from the antenna elements 404 by a second layer or substrate 412, which may also be formed from the polymer composition of the present invention. The dimensions "G" and "W" may correspond to the "feature size" of the antenna 400. The "G" dimension may correspond to the distance between the antenna elements 404 and the coplanar ground layer 406. The "W" dimension may correspond to the width (e.g., line width) of the antenna elements 404. Thus, in some embodiments, the dimensions "G" and "W" may be relatively small (e.g., less than about 750 micrometers) such that the antenna 400 is a "fine pitch" antenna 400.
[0053]
[0067] FIG. 12A illustrates an antenna array 500 according to another aspect of the disclosure. The antenna array 500 may include a substrate 510, which may be formed from the polymer composition of the present invention, and a plurality of antenna elements 520 formed thereon. The plurality of antenna elements 520 may be approximately equally sized in the X and / or Y directions (e.g., square or rectangular). The plurality of antenna elements 520 may be approximately evenly spaced apart in the X and / or Y directions. The dimensions of and / or spacing between the antenna elements 520 may correspond to the "feature size" of the antenna array 500. Thus, in some embodiments, the dimensions and / or spacing may be relatively small (e.g., less than about 750 micrometers) such that the antenna array is a "fine pitch" antenna array. As indicated by the ovals 522, the number of columns of antenna elements 520 illustrated in FIG. 12 is provided by way of example only. Similarly, the number of rows of antenna elements 520 is provided by way of example only.
[0054]
[0068] The tuned antenna array 500 may be used, for example, in a base station (e.g., as described above with respect to FIG. 8) to provide massive MIMO functionality. More specifically, the radio frequency interactions between the various elements may be controlled or tuned to provide multiple transmit and / or receive channels. The transmit power and / or receive sensitivity may be directionally controlled to focus or direct the radio frequency signal, for example, as described with respect to the radio frequency signal 112 of FIG. 8. The tuned antenna array 500 may provide a large number of antenna elements 522 in a small footprint. For example, the tuned antenna 500 may have an average antenna element density of 1,000 antenna elements per square centimeter or more. Such a compact arrangement of antenna elements may increase the number of channels for MIMO functionality per unit area. For example, the number of channels may correspond to (e.g., be equal to or proportional to) the number of antenna elements.
[0055]
[0069] FIG. 12B illustrates an antenna array 540 formed by laser direct structuring, which may optionally be utilized to form antenna elements. The antenna array 540 may include a plurality of antenna elements 542 and a plurality of feed lines 544 connecting the antenna elements 542 (e.g., with other antenna elements 542, a front-end module, or other suitable components). The antenna elements 542 may have respective widths "w" and spacing distances "S1" and "S2" therebetween (e.g., in the X- and Y-directions, respectively). These dimensions may be selected to achieve 5G radio frequency communications at a desired 5G frequency. More particularly, the dimensions may be selected to tune the antenna array 540 to transmit and / or receive data using radio frequency signals that are within the 5G frequency spectrum. The dimensions may be selected based on material properties of the substrate. For example, one or more of "w", "S1", or "S2" may correspond to a multiple of the propagation wavelength ("λ") of the desired frequency through the substrate material (e.g., nλ / 4, where n is an integer).
[0056]
[0070] As an example, λ is:
[0057]
number
[0058] (c is the speed of light in a vacuum, and ε R where f is the dielectric constant of the substrate (or surrounding material) and f is the desired frequency.
[0071] 12C illustrates an exemplary antenna configuration 560 according to an embodiment of the present disclosure. The antenna configuration 560 may include a plurality of antenna elements 562 arranged on parallel long sides of a substrate 564, which may be formed from a polymer composition of the present invention. The various antenna elements 562 may have respective lengths "L" (and spacing distances therebetween) that tune the antenna configuration 560 for reception and / or transmission at a desired frequency and / or frequency range. More particularly, such dimensions may be selected based on the propagation wavelength λ at a desired frequency of the substrate material, for example, as described above with reference to FIG. 12B.
[0059]
[0072] 13A-13C show simplified flow diagrams of a laser direct structuring manufacturing process that may be used to form antenna elements and / or arrays according to aspects of the present disclosure. With reference to FIG. 13A, a substrate 600 may be formed from the polymer composition of the present invention using any desired technique (e.g., injection molding). In certain embodiments, as shown in FIG. 13B, a laser 602 may be used to activate the laser activatable additive to form a circuit pattern 604 that may include one or more of the antenna elements and / or arrays. For example, the laser may melt conductive particles in the polymer composition to form the circuit pattern 604. With reference to FIG. 13C, the substrate 600 may be immersed in an electroless copper bath to plate the circuit pattern 604 to form the antenna elements, element arrays, other components, and / or conductive lines therebetween.
[0060]
[0073] The invention may be better understood with reference to the following examples. EXAMPLES
[0061] Test Method
[0074] Melt viscosity: Melt viscosity (Pa s) was measured at a shear rate of 400 s using a Dynisco LCR7001 capillary rheometer. -1 or 1,000s -1and 15°C above the melt temperature (e.g., about 325°C) according to ISO11443:2021. The rheometer orifice (die) may have a diameter of 1 mm, a length of 20 mm, an L / D ratio of 20.1, and an entrance angle of 180°. The barrel diameter may be 9.55mm+0.005mm and the rod length may be 233.4mm.
[0062]
[0075] Melting temperature: Melting temperature ("Tm") can be determined by differential scanning calorimetry ("DSC") as known in the art. Melting temperature is the differential scanning calorimetry (DSC) peak melting temperature as determined by ISO11357-3:2018. For the DSC procedure, samples were heated and cooled at 20°C per minute as described in ISO standard 10350, using DSC measurements performed on a TA Q2000 Instrument.
[0063]
[0076] Deflection Temperature Under Load ("DTUL"): Deflection temperature under load may be determined in accordance with ISO 75-2:2013 (technically equivalent to ASTM D648). More specifically, a test specimen sample having a length of 80 mm, a thickness of 10 mm, and a width of 4 mm may be subjected to an edgewise three-point bending test with a prescribed load (maximum outer fiber stress) of 1.8 megapascals. The specimen may be lowered into a silicone oil bath with a temperature increase of 2°C per minute until it deflects 0.25 mm (0.32 mm for ISO Test No. 75-2:2013).
[0064]
[0077] Tensile modulus, tensile stress and tensile elongation: Tensile properties may be tested according to ISO 527:2019 (technically equivalent to ASTM D638). Modulus and strength measurements may be performed on identical test specimen samples having a length of 80 mm, a thickness of 10 mm, and a width of 4 mm. The test temperature may be 23°C and the test speed may be 1 or 5 mm / min.
[0065]
[0078] Flexural modulus, flexural stress and flexural elongation: Flexural properties may be tested according to ISO178:2019 (technically equivalent to ASTM D790). The test may be performed with a support span of 64 mm. The test may be performed on the central section of an uncut ISO 3167 multipurpose bar. The test temperature may be 23°C and the test speed may be 2 mm / min.
[0066]
[0079] Charpy Impact Strength: Charpy properties may be tested according to ISO179-1:2010 (technically equivalent to ASTM D256-10, Method B). The test may be performed using a Type 1 specimen size (80 mm length, 10 mm width and 4 mm thickness). When testing notched impact strength, the notch may be a Type A notch (0.25 mm bottom radius). The specimen may be cut from the center of a utility bar using a single tooth milling machine. The test temperature may be 23°C.
[0067]
[0080] Permittivity ("Dk") and dissipation factor ("Df"): The permittivity (or specific static permittivity) and dissipation factor are determined by Baker-Jarvis et al., IEEE Trans. on Dielectric and Electrical Insulation, 5(4), p. 571 (1998) and Krupka et al., Proc. th It is determined using the known split-post dielectric resonator technique as described in International Conference on Dielectric Materials: Measurements and Applications, IEEE Conference Publication No. 430 (September 1996). More specifically, a plaque specimen with size 80 mm x 90 mm x 3 mm, or a disk with diameter 101.6 mm and thickness 3 mm, was inserted between two fixed dielectric resonators. The resonators measured the dielectric constant components in the plane of the specimen. Five specimens were tested and the average value was recorded. Split-post resonators may also be used to make dielectric measurements in the low gigahertz region, such as 2 GHz.
[0068]
[0081] Thermal cycling test: The specimen is placed in a temperature controlled chamber and heated / cooled in the temperature range of -30℃ to 100℃. First, the specimen is heated until it reaches a temperature of 100℃, at which point it is immediately cooled. Once the temperature reaches -30℃, the specimen is immediately heated again until it reaches 100℃. 23 heating / cooling cycles may be performed over a 3-hour period.
[0069] Examples 1-2
[0082] Examples 1-2 are formed from various combinations of liquid crystal polymer (LCP1), mica, and precious metal catalyst (0.25% palladium on kaolin). LCP1 is formed from 48% HNA, 25% BP, 25% TA, and 2% HBA. Compounding was performed using an 18mm single screw extruder. Parts were injection molded and samples were molded into plaques (60mmx60mm).
[0070] [Table 1]
[0071]
[0083] Examples 1-2 were tested for thermal and mechanical properties and the results are shown in Table 2 below.
[0072] [Table 2]
[0073]
[0084] These and other modifications and variations of the present invention may be practiced by those skilled in the art without departing from the spirit and scope of the present invention. In addition, it should be understood that aspects of the various embodiments may be interchanged both in whole or in part. Furthermore, those skilled in the art will appreciate that the foregoing description is for illustrative purposes only and is not intended to limit the present invention as further described in such appended claims.
Claims
1. 1. A platable polymer composition comprising a precious metal catalyst distributed within a polymer matrix comprising at least one highly naphthenic thermotropic liquid crystalline polymer comprising repeat units derived from naphthenic hydroxycarboxylic acids and / or dicarboxylic acids in an amount of about 10 mol. % or greater, said polymer composition exhibiting a dielectric loss tangent of about 0.01 or less determined at a frequency of 2 GHz.
2. 10. The plateable polymeric composition of claim 1, exhibiting a dielectric constant of about 5 or less at a frequency of 2 GHz.
3. 1,000s -1 10. The plateable polymeric composition of claim 1, exhibiting a melt viscosity of about 0.1 to about 50 Pa·s determined at a shear rate of about 0.1 to about 50 Pa·s and at a temperature about 15° C. above the melting temperature of said polymeric composition.
4. The plateable polymeric composition of claim 1 having a melting temperature of about 280°C to about 400°C.
5. 10. The plateable polymeric composition of claim 1, exhibiting a deflection temperature under load of about 200°C or greater, determined at 1.8 MPa.
6. 10. The platable polymer composition of claim 1, wherein the liquid crystalline polymer comprises from about 50 wt.% to about 99 wt.% of the polymer composition.
7. 10. The plateable polymer composition of claim 1, wherein the highly naphthenic thermotropic liquid crystalline polymer comprises repeat units derived from one or more aromatic dicarboxylic acids, one or more aromatic hydroxycarboxylic acids, or a combination thereof.
8. 2. The plateable polymer composition of claim 1, wherein the aromatic hydroxycarboxylic acid comprises 4-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, or a combination thereof.
9. The plateable polymeric composition of claim 7, wherein the aromatic dicarboxylic acid comprises terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, or a combination thereof.
10. 8. The plateable polymer composition of claim 7, wherein the highly naphthenic thermotropic liquid crystalline polymer further comprises repeat units derived from one or more aromatic diols.
11. The plateable polymer composition of claim 10, wherein the aromatic diol comprises hydroquinone, 4,4'-biphenol, or a combination thereof.
12. The platable polymer composition of claim 1 , wherein said thermotropic liquid crystalline polymer is wholly aromatic.
13. 2. The platable polymer composition of claim 1, wherein the liquid crystalline polymer comprises repeat units derived from 6-hydroxy-2-naphthoic acid in an amount of about 30 mol. % or greater.
14. 14. The plateable polymer composition of claim 13, wherein the liquid crystalline polymer comprises repeat units derived from 6-hydroxy-2-naphthoic acid and 4-hydroxybenzoic acid in a molar ratio of about 5 to about 40.
15. The platable polymeric composition of claim 1 further comprising a mineral filler.
16. 16. The plateable polymeric composition of claim 15, wherein said mineral filler has a hardness value of about 2 or greater.
17. 16. The plateable polymeric composition of claim 15, wherein said mineral filler is in the form of flake-like particles having an aspect ratio of about 4 or greater.
18. The plateable polymeric composition of claim 15 , wherein the particulate filler comprises mica.
19. The platable polymer composition of claim 1, wherein said mineral filler comprises from about 1 to about 60 parts by weight per 100 parts by weight of said polymer matrix.
20. 10. The plateable polymer composition of claim 1, wherein the catalyst comprises a precious metal component comprising palladium, iridium, ruthenium, platinum, rhodium, or alloys or combinations thereof.
21. The plateable polymeric composition of claim 1 , wherein the catalyst comprises a precious metal component comprising palladium.
22. The plateable polymer composition of claim 1 , wherein the catalyst comprises a precious metal component supported by a matrix material.
23. The plateable polymeric composition of claim 22 , wherein the material comprises a silicate.
24. The platable polymer composition of claim 1, wherein the catalyst comprises a precious metal component comprising from about 0.1 parts by weight to about 6 parts by weight per 100 parts by weight of the polymer matrix.
25. The plateable polymer composition of claim 1, wherein the catalyst comprises from about 0.5 to about 20 parts by weight per 100 parts by weight of the polymer matrix.
26. The platable polymeric composition of claim 1 which is glass fiber free.
27. The platable polymeric composition of claim 1 which is free of laser activatable additives.
28. 13. A molded interconnect device comprising a substrate having a surface having at least one conductive element plated thereon, said substrate comprising the polymer composition of claim 1.
29. 30. The molded interconnect device of claim 28, wherein the conductive elements comprise copper, nickel, or a combination thereof.
30. 30. A method for forming a molded interconnect device according to claim 28, comprising forming an interconnect pattern on a surface of the substrate and then plating the patterned surface of the substrate.
31. 30. The method for forming a molded interconnect device of claim 28, comprising plating a surface of the substrate and thereafter forming an interconnect pattern on the plated surface of the substrate.
32. The method of claim 30 , wherein the interconnect pattern is formed by a method including laser ablation.
33. 31. The method of claim 30, wherein the plating step comprises electroless plating, electrolytic plating, or a combination thereof.
34. 30. An antenna system including the molded interconnect device of claim 28, wherein the conductive element is an antenna element configured to transmit and / or receive radio frequency signals.
35. 35. The antenna system of claim 34, wherein the radio frequency signal is a 5G signal.
36. 35. The antenna system of claim 34, wherein said antenna elements have a feature size of less than about 5,000 micrometers.
37. 35. The antenna system of claim 34, wherein a plurality of antenna elements are formed on a surface of the substrate.
38. 38. The antenna system of claim 37, wherein said antenna elements are spaced apart by a spacing distance of less than about 3,000 micrometers.
39. 38. The antenna system of claim 37, wherein said antenna elements include at least 16 antenna elements.
40. 38. The antenna system of claim 37, wherein the antenna elements are arranged in an array.
41. 41. The antenna system of claim 40, wherein the array is configured for at least eight transmit channels and at least eight receive channels.
42. 41. The antenna system of claim 40, wherein said array has an average antenna element density of greater than 10 antenna elements per square centimeter.
Citation Information
Patent Citations
Catalyst filler for electroless metal plating, resin composition for electroless metal plating and composite formed article
JP1996283952A
Method of manufacturing plastics mold circuit board that can be gold wire bonded
JP1997223857A
Polymer composition and film for use in 5g applications
WO2021050221A1
Liquid crystalline polymer composition
WO2021050222A1
Circuit board for use at 5g frequencies
WO2021061305A1