Method for plasma etching layers based on III-N materials - Patents.com

Pulsed bias voltage plasma treatment for etching III-N materials addresses material degradation and etch depth control issues, enhancing etching efficiency and quality for microelectronic devices.

JP2024543935APending Publication Date: 2024-11-26COMMISSARIAT A LENERGIE ATOMIQUE ET AUX ENERGIES ALTERNATIVES +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024531684
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-29
Filing Date
2022-11-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Current etching methods for III-N materials, such as GaN and AlGaN, cause material degradation and poor etch depth control, leading to reduced device performance in microelectronic devices like transistors and diodes.

Method used

A method involving chlorine-based plasma treatment with pulsed bias voltage application to the substrate, combining chlorination and ion bombardment, with a duty cycle of 10% to 80%, to etch III-N layers, reducing ion bombardment energy and enhancing etching rate while minimizing material damage.

Benefits of technology

The method significantly reduces etching duration and maintains the quality of III-N layers, suitable for industrial production, achieving similar performance to existing methods in a fraction of the time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024543935000001_ABST
    Figure 2024543935000001_ABST
Patent Text Reader

Abstract

The object of the invention relates to a method for etching at least a portion (10c) of a layer (10) based on III-N material, comprising a step of exposing at least a portion of a top surface (10a) of the III-N layer (10) to a plasma treatment (20) with a chlorine-based bias voltage pulsing, the plasma treatment (20) being configured to have a duty cycle comprised between 20% and 80%, in which a first non-zero polarization bias Vbias-substrate1 is applied to the substrate (1) during Ton and a second polarization bias |Vbias-substrate2| less than |Vbias-substrate1| or no polarization bias is applied during Toff to etch the portion (10c) of the III-N layer (10), such that the duration of the etching is significantly reduced and a sufficient quality of the III-N layer (10) for the operation of a microelectronic device such as a transistor or diode is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention generally relates to the incorporation of layers based on III-N materials, such as gallium nitride (GaN) and aluminum gallium nitride (AlGaN) and their derivatives, into microelectronic devices. An advantageous application of the present invention is the fabrication of devices, such as transistors or diodes, that incorporate one or more layers of III-N materials. [Background technology]

[0002] The trend and increasing demand for reducing energy waste is driving microelectronic device manufacturers to improve the efficiency and performance of their power conversion systems. Currently, conversion circuits are made from silicon, and much research has been done to develop architectures to improve efficiency and conductivity. However, these devices are reaching the theoretical limits of silicon, and new solutions must be developed.

[0003] AlGaN / GaN heterostructures, formed by a layer of aluminum gallium nitride on a layer of gallium nitride, are showing great promise for the development of power electronics and diodes due to their electrical properties that allow the formation of a two-dimensional electron gas. AlGaN / GaN heterostructures are competitive with Si and SiC in terms of device size, voltage handling, carrier mobility, and series resistance.

[0004] Nevertheless, the practical use of this AlGaN / GaN heterostructure in devices such as transistors or diodes poses major problems that need to be addressed in order to fully exploit the performance of these GaN-based materials. More generally, these problems arise in the case of III-V and especially III-N materials. In particular, the etching steps for device structuring are critical and are known to degrade the electrical properties of the channel.

[0005] These etching steps are related to, for example, opening up the passivation layer on top of the AlGaN / GaN heterostructure to form contacts for diodes or to form gates or contacts for transistors, for example HEMTs (High Electron Mobility Transistors).

[0006] AlGaN and GaN etching is typically performed by plasma etching with chlorinated chemistry in an inductively coupled plasma (ICP) reactor.

[0007] These solutions have many drawbacks. In particular, ion bombardment during plasma etching typically degrades the material of the layers and patterns being supported. In addition, etch depth control is performed at a time when no stop layer is present, requiring stable process performance to achieve the exact target depth.

[0008] All these defects degrade the III-N layers and reduce the device performance.

[0009] Cyclic etching techniques have been proposed to limit these drawbacks. For example, the atomic layer etching (ALE) cycle for etching GaN layers consists of two steps that are repeated consecutively: A first self-limiting step to chlorinate the GaN layer using Cl2 and BCl3 plasma treatment to chemically modify the top part of the GaN to be etched; A subsequent second step consists of etching this chlorinated portion selectively with respect to unmodified GaN by an Ar-based plasma applying a small bias voltage to the substrate, typically less than 90V in absolute value.

[0010] Although this technique improves post-etch thickness control and reduces surface damage, it has the drawback of requiring long processing times, which do not meet industrial requirements for productivity. [Prior art documents] [Patent documents]

[0011] [Patent Document 1] EP3023799A1 Summary of the Invention [Problem to be solved by the invention]

[0012] The object of the present invention is therefore to propose a solution that makes it possible to etch layers of III-N materials such as GaN or AlGaN, limiting or even eliminating the drawbacks of these known solutions. In particular, one object is to reduce the duration of etching the III-N layers while limiting damage to the III-N layers.

[0013] Other objects, features, and advantages of the present invention will become apparent from the following description and the accompanying drawings, and it will be understood that other advantages may also be incorporated. [Means for solving the problem]

[0014] To achieve these objectives, according to one embodiment, the invention relates to a method for etching at least a portion of a layer based on a III-N material, comprising: Providing a substrate comprising at least one layer based on III-N materials, which layer constitutes a top surface, called "III-N layer"; performing at least one etching cycle comprising exposing at least a portion of the top surface to a chlorine-based plasma treatment with a plasma potential Vplasma, the plasma treatment being performed using bias voltage pulsing and configured to have a duty cycle DC=Ton / (Ton+Toff) comprised between 10% and 80%; During at least a portion of the Ton time frame, a first non-zero bias voltage, referred to as Vbias-substrate1, is applied to the substrate, preferably the first Vbias-substrate1 having an absolute value |Vbias-substrate1| of 100V or greater; During the Toff time frame, a second bias voltage, called Vbias-substrate2, is applied to the substrate, such that Vbias-substrate2 has an absolute value |Vbias-substrate2| that is less than |Vbias-substrate1| or no bias voltage is applied to the substrate; Vbias-substrate1 and Vbias-substrate2 provide a method, independent of Vplasma, to etch the portion of the III-N layer extending from the portion of the top surface.

[0015] In this method, the chlorination and plasma treatment of the III-N layer are carried out simultaneously to etch the III-N layer. During Ton, the etching of the III-N layer combines the chlorination of the III-N layer with the ion bombardment of the III-N layer. During Toff, the ion bombardment of the top surface is reduced and preferentially no significant bombardment occurs on the top surface of the III-N layer. This value of the bias voltage applied to the substrate increases the etching rate of the III-N layer. On the other hand, the pulse Vbias-substrate allows to lower the average energy of the ion bombardment of the III-N layer and thus reduces the damage that may occur. Synergistically, the duration of the etching is significantly reduced compared to the pure ALE cycle, resulting in a sufficient quality of the III-N layer for the operation of microelectronic devices such as transistors or diodes.

[0016] The method disclosed in this disclosure shows superior results compared to known ALE techniques. The sequence of cycles in the embodiments of the disclosure allows the substrate surface to be modified to a certain depth during chlorination, and then the modified layer to be selectively removed by an argon-based plasma treatment without affecting the underlying material. To achieve this, the energy applied during the Ar plasma treatment must be carefully selected.

[0017] FIG. 1 shows the etch volume per cycle (EPC) for the ALE cycle as a function of the removal energy E, e.g., ion energy. For example, as shown in FIG. 1, different energy regimes are observed. In regime I, the bombardment energy is insufficient to completely remove the modified layer. Thus, removal is partial. The energy is also too low to disrupt the underlying unmodified material, thus not causing degradation. In regime II, the bombardment energy is sufficient to remove the entire modified layer. Thus, removal is complete, and the thickness removed per cycle corresponds to the thickness modified during the first stage. However, the ion energy is again too low to damage the underlying unmodified material, thus the removal step is selective and self-limiting. The third regime corresponds to an energy range in which the bombardment has enough energy to disrupt the unmodified material. Within this range, removal of the modified layer is complete, but the underlying material is also damaged. Thus, the removal step is no longer selective. In addition, if the energy E is increased too much, the material will degrade further, thereby changing its electrical properties.

[0018] It is therefore clear that to achieve the desired quality of the underlying material by the ALE cycle, the energy level must be carefully controlled to be high enough to remove the modified layers, but low enough to avoid damage to the unmodified III-N layers. The energy window is therefore narrow, thereby resulting in a long etching period. Overall, the etching duration using ALE alone is too long for practical industrial production.

[0019] The embodiments of the present disclosure solve this problem by limiting the average energy of the ions by applying a pulsed bias voltage to the substrate. Thus, each ion has a high enough energy to increase the etch rate of the III-N layers, due in part to the polarization bias voltage applied to the substrate, and also limits the average ion bombardment energy. In addition to increasing the etch rate, damage to the material layer is limited.

[0020] The average energy of the ions can be further limited according to the duty cycle of the plasma treatment. During the development of the invention, it was found that a duty cycle of 10% to 80% corresponds to a range in which a sufficiently good compromise is found between the performance of the microelectronic device with the etched III-N layer and the industrial requirements in terms of productivity, more specifically the duration of the etching of the III-N layer.

[0021] This method is completely different from existing solutions using plasmas whose source is operated in a pulsed manner. Plasma treatments with source pulsing reduce the electron temperature in the plasma by constant ion bombardment. Plasma treatments, in which pulsing of a bias voltage is applied to the substrate, make it possible to modulate the ion bombardment on the top surface of the III-N layer.

[0022] The objects, features and advantages of the present invention will become more apparent from the following detailed description of embodiments of the present invention, illustrated by the accompanying drawings. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 illustrates the three forms of energy in the ALE cycle. [Diagram 2] FIG. 2 is a cross-sectional view of a substrate comprising III-N layers according to one embodiment. [Diagram 3] 3 is a cross-sectional view of the substrate of FIG. 2 after deposition of a mask. [Figure 4]FIG. 13 illustrates the RF bias power of the plasma when the bias voltage Vbias-substrate is pulsed during plasma processing. [Figure 5A] 4 is a cross-sectional view of the substrate of FIG. 3 during an etching cycle according to one embodiment. [Figure 5B] 5B is a cross-sectional view of the substrate of FIG. 3 during an etching cycle according to an alternative embodiment to or complementary to the embodiment of FIG. 5A. [Figure 5C] 5B is a cross-sectional view of the substrate of FIG. 3 during etching prior to the etching cycle shown in FIG. 5A. [Figure 6] FIG. 5C is a cross-sectional view of the substrate of FIG. 5B after removing the mask. [Figure 7] FIG. 5C is a cross-sectional view of a microelectronic device obtained after filling the etched openings in the III-N layers as illustrated by FIGS. 5A and 5B. [Figure 8] FIG. 1 is a schematic diagram of an example reactor. [Figure 9A] FIG. 13 illustrates the measurement of Rsheet according to one embodiment. [Figure 9B] FIG. 13 illustrates the measurement of Rsheet according to one embodiment. [Figure 10] FIG. 1 is a diagram of Rsheet measurements. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The figures are given as examples and are not limiting of the present invention. The figures are schematic representations in principle intended to facilitate understanding of the present invention, and therefore are not necessarily to scale in actual applications. More specifically, the relative thicknesses of the various layers and films are not representative of reality.

[0025] Before discussing and describing embodiments of the present invention in detail, the following describes optional features that may be combined or used alternatively.

[0026] According to some embodiments, the applied |Vbias-substrate1| is between 20 V and 800 V, preferably between 100 V and 800 V, preferably between 100 V and 500 V. In some embodiments, the applied |Vbias-substrate1| is between 20 V and 350 V, preferably between 150 V and 350 V, during at least a portion of the Ton time frame, preferably for all Ton time frames of at least one etch cycle. These Vbias-substrate values ​​allow for more efficient etching while maintaining good surface quality of the III-N layer, making them suitable for industrial production applications.

[0027] According to one embodiment, |Vbias-substrate2| is essentially equal to or less than 0.5*|Vbias-substrate1|, and preferably is essentially less than 0.2*|Vbias-substrate1|.

[0028] According to one embodiment, |Vbias-substrate1| > 2*|Vbias-substrate2|, preferably |Vbias-substrate1| > 5*|Vbias-substrate2|, and more preferably |Vbias-substrate1| > 10*|Vbias-substrate2|, during at least a portion of the Ton timeframe, and preferably for at least all Ton timeframes of at least one etch cycle.

[0029] According to one embodiment, the duty cycle is comprised between 20% and 70%. In some embodiments, the duty cycle is about 50%. Controlling the duty cycle percentage further improves the trade-off between industrial requirements on the performance and productivity of microelectronic devices comprising etched III-N layers, more specifically the duration of etching of III-N layers.

[0030] According to one embodiment, the at least one etching cycle has a duration such that the etched portion of the at least one III-N layer has a thickness comprised between 20 nm and 3 μm, particularly when the substrate is to be implemented into a transistor, e.g. a HEMT.

[0031] According to one embodiment, the at least one etching cycle has a duration such that the etched portion of the at least one III-N layer has a thickness comprised between 100 nm and 5 μm, in particular when the substrate is to be mounted on an LED, e.g. a μm-LED.

[0032] When the method includes multiple etching cycles, the total duration of all cycles, i.e., the sum of the durations of each cycle, is selected such that the etched portion of at least one III-N layer has a thickness as given above.

[0033] According to one embodiment, the plasma process in which pulsing of bias voltage is applied to the substrate is configured to have a frequency F=1 / (Ton+Toff). In some embodiments, the frequency F is between 100 Hz and 5 kHz, preferably between 150 Hz and 1 kHz. In some embodiments, the frequency F is set according to the above ranges to accommodate certain process or equipment constraints.

[0034] In some embodiments, the etching method may include multiple etching cycles, with |Vbias-substrate1| varying between the etching cycles. In some embodiments, |Vbias-substrate1| of at least one etching cycle is strictly lower than |Vbias-substrate1| of the previous etching cycle. The etching rate may be enhanced, especially for the top of the III-N layer, when the applied |Vbias-substrate1| is greater than 100V, as compared to existing ALF solutions. Also, decreasing Vbias-substrate as multiple cycles proceed reduces further damage to the III-N layer as the desired etching level is approached.

[0035] According to this embodiment, the plasma may be based on the same compound during several etching cycles: for all etching cycles, the plasma may be based on Cl2, preferentially a combination of Cl2 and CBCl3.

[0036] According to one embodiment, |Vbias-substrate1| is essentially equal to or less than 100 V during at least some other cycles within the group of all multiple cycles, further limiting damage induced on the III-N layers in some cases.

[0037] According to one embodiment, the method comprises, prior to at least one etching cycle, a pre-etching cycle on said portion of the III-N layer, exposing at least a portion of the upper surface to a chlorine-based plasma treatment with a plasma potential V; applying a non-zero bias voltage, preferably a non-pulsing bias voltage Vbias-substrate to the substrate during said plasma treatment, where Vbias-substrate is independent of Vplasma, and preferentially |Vbias-substrate| is 100 V or higher during at least a portion of the previous etching cycle.

[0038] A plasma process in which a non-pulsing bias voltage is applied to the substrate is faster than a plasma process with bias pulsing, but causes more damage to the layer being etched. This is particularly useful when etching a thin portion of the III-N layer, where a fast first etching step can be used to etch most of the layer, and the etching can be terminated by limiting the damage to the III-N layer. According to one embodiment, prior to at least one etching cycle, the top surface of the III-N layer is covered by a mask.

[0039] According to one embodiment, the source of plasma has a power comprised between 100W and 2000W, preferentially between 300W and 1000W.

[0040] According to one embodiment, the plasma treatment with bias pulsing is carried out in a reaction chamber, the pressure inside the reaction chamber is less than 250 mTorr, preferentially less than 90 mTorr, for example comprised between 2 mTorr and 250 mTorr, in some examples between 2 mTorr and 90 mTorr, in some examples between 2 mTorr and 20 mTorr, during at least one etching cycle. The pressure influences the residence time of the species and the directionality of the ions. A pressure below 90 mTorr limits the risk of ion deflection and therefore improves the uniformity of the etched surface. When the pressure is below 20 mTorr, the plasma is more highly ionized. The effect of the plasma treatment with bias voltage pulses is enhanced compared to using higher pressures.

[0041] According to one embodiment, the plasma treatment with bias pulsing is carried out in a reaction chamber, and the temperature of the reaction chamber, more specifically the temperature of the chamber walls and the sample holder (equivalent to the substrate temperature), is between 20°C and 80°C. In some examples, the temperature of the reaction chamber is between 30°C and 60°C for at least one etching cycle. This temperature affects the sticking coefficient and dynamic reaction rate of the species during etching. This temperature range enhances the etching rate of the III-N layers.

[0042] According to one embodiment, the plasma treatment with bias pulsing is preferentially based on Cl2 combined with BCl3. The etching of III-N layers is mainly due to the presence of chlorine radicals and is driven by ion bombardment. Cl2 is sufficient to etch III-N materials except for oxides. Bl3 further provides less reactive chlorine compared to Cl2 and is able to etch oxides. The role of Bl3 is to act as a micromask during the chlorine etch, etching any surface oxides that increase roughness and to capture traces of oxygen contained in the plasma so that oxidation of the surface being etched is limited.

[0043] According to another embodiment, the plasma treatment with bias pulsing is based on BCl3, preferentially in combination with Cl2. As mentioned above, BCl3 promotes the etching of the III-N layer and avoids increasing the roughness of the III-N layer. According to one embodiment, the III-N material comprises a chemical element selected from the group consisting of aluminum and gallium, for example selected from the group consisting of AlGaN, GaN, AlN, InGaN, AlInGaN.

[0044] According to one embodiment, the substrate is incorporated into transistors for power electronics, such as HEMT transistors.

[0045] According to one embodiment, the substrate incorporates a light emitting diode.

[0046] According to one embodiment, the plasma treatment with bias pulsing is fluorine-free for at least one etching cycle, and preferentially for all etching cycles.

[0047] According to one embodiment, the plasma power supply is turned on during essentially the entire etch cycle. Similarly, the plasma power supply is not pulsed.

[0048] For the purposes of the present invention, the thickness of a layer is measured in a direction perpendicular to the surface along which the layer has its greatest extension. In the figures, the thickness is measured in the vertical direction. Similarly, when two elements are shown to be aligned with each other, this means that the two elements are both located on the same line perpendicular to the main plane of extension of the layer, i.e., on the same line oriented vertically in the figures.

[0049] It is to be clarified that in the context of the present invention, the terms "on," "above," "overlying," "underlying," "facing," and their equivalents do not necessarily mean "in contact with." Thus, for example, depositing, transferring, bonding, assembling, or applying a first layer to a second layer does not necessarily mean that the two layers are in direct contact with each other, but rather that the first layer at least partially overlies the second layer, either by being in direct contact with the second layer or by being separated from the second layer by at least one other layer or element.

[0050] III-N materials are materials that contain at least one chemical element from column III of the periodic table and nitrogen (N).

[0051] A substrate, film, or layer "based on" material A means a substrate, film, or layer that comprises only material A or that comprises material A and possibly other materials. Thus, in the present description, a layer based on III-N materials may be a layer that consists exclusively of III-N materials or a layer that comprises III-N materials and other elements.

[0052] According to one embodiment, in the context of the present invention, a layer based on a III-N material is a GaN or AlN based material, for example AlGaN (or Al x Ga (1-x) N, where x is 0 to 1), GaN, AlN, InGaN, and AlInGaN.

[0053] The GaN-based layer may be a layer consisting exclusively of GaN. Alternatively, the GaN-based layer may consist of GaN and one or more elements from columns III or V of the periodic table of the elements, typically AlGaN, InGaN, or AlInGaN, or other elements that may be present unintentionally, possibly resulting from unwanted implants, for example.

[0054] According to one embodiment, the III-N material layer is doped. The doping can be performed with at least one of the following species: Mg, Si, P, O, Ca, C.

[0055] A layer may also be composed of several sublayers of the same material or of different materials respectively. A layer based on III-N materials may therefore comprise a stack of several layers based on one III-N material or on different III-N materials. In particular, a GaN-based layer may be a stack of GaN-based layers. For example, the stack may comprise an AlGaN layer located on a layer made of GaN and preferably in direct contact with this layer.

[0056] The term "dielectric" refers to a material whose electrical conductivity is low enough to act as an electrical insulator in a given application.

[0057] When gas mixtures are expressed as percentages, these percentages correspond to a fraction of the total flow rate of gases introduced into the reactor, so for example, if a gas mixture intended to form a plasma contains x% of Gas A, this means that the introduction rate of Gas A corresponds to x% of the total flow rate of gases introduced into the reactor to form the plasma.

[0058] Microelectronic devices refer to any type of device made by microelectronic means, including in particular purely electronic devices as well as micromechanical or electromechanical devices (MEMS, NEMS, etc.) and optical or optoelectronic devices (MOEMS, LEDs, etc.).

[0059] This may be a device intended to perform an electronic, optical, or mechanical function, etc. The device may be an intermediate product intended to create another microelectronic device.

[0060] For the purposes of this invention, a "HEMT" is a high electron mobility field effect transistor, sometimes referred to as a heterostructure field effect transistor. Such transistors contain a superposition of two semiconductor layers, each with a different band gap, that form a quantum well at the interface of the semiconductor layers. Electrons are confined in this quantum well, forming a two-dimensional electron gas. Due to their high voltage and temperature capabilities, the materials for these transistors are chosen to have wide energy band gaps.

[0061] The term "step" does not necessarily imply that actions taken during a step are performed simultaneously or consecutively, unless otherwise stated. In particular, some actions of a first step may be followed by actions relating to a different step, and other actions of the first step may be repeated at a later time. Thus, the term step does not necessarily imply a single, inseparable action in time and in the sequence of method phases.

[0062] A parameter that is "substantially equal to / less than / greater than" a given value is defined as equal to / less than / greater than a given value within ±10% of the given value. A parameter that is "substantially between" two given values ​​means that the parameter is at least equal to the smaller given value within ±10% of that value and at most equal to the larger given value within ±10% of that value.

[0063] In the following, this method will be described according to a specific embodiment with reference to FIGS.

[0064] In a preliminary step, a substrate 1 is prepared, comprising at least one layer 10 based on III-N material, as shown, for example, in FIG. 2. Typically, this material is based on GaN. This layer 100 can be formed in a single layer. This layer 100 can also be formed in a stack of layers 100, 101, 102, as will be further explained below. The layer 100 can be located on other layers, typically on a support 13 or on a growth substrate (not shown in FIGS. 3-6). Intermediate layers 11, 12 may be arranged between the support layer 13 and the layer 10. According to an embodiment, the III-N layer 10 is intended to form the active layer of a transistor. The substrate 1 comprising the III-N layer 10 can therefore either be a stack in which the III-N layer is one of the deposited layers on the support layer 13, or a stack comprising only the III-N layer. In this case, this layer can be self-supporting, i.e. it supports its own weight.

[0065] According to one embodiment, a mask 14 may be deposited covering layer 10 in order to etch only a certain portion 10c (e.g., as shown in FIG. 5A) or to etch several separate portions 10c of layer 10. However, the presence of this mask 14 is not essential to perform the steps described below.

[0066] According to an example that can be illustrated by FIG. 3, the mask 14 is arranged in direct contact with the upper surface 10a of the layer 10. The mask 14 is formed, for example, by lithography of a layer deposited or transferred onto the layer 10. In some embodiments, the mask 14 is a hard mask. The mask 14 is, for example, a Si x N ywhere x and y are non-zero positive numbers. Examples of materials for forming the hard mask 14 include SiN, Si3N4, SiOCN, SiCBN and derivatives thereof, photoresists, such as carbon photoresists, and combinations thereof. The mask 14 has openings 140 as shown in FIG. 3. Each opening is defined by straight lateral walls from which the portion 10c of the III-N layer 10 is etched. The mask 14 can be lifted off the III-N layer 10 after the portion 10c of the layer 10 is etched, as shown by FIG. 6.

[0067] Example of an Etching Cycle The method includes at least one etching cycle as described below. During one etching cycle, a portion 10b (in some embodiments, several portions 10b of the upper surface 10a of the III-N layer) is exposed to a plasma treatment 20 using bias pulsing. During the plasma treatment, a non-zero polarization bias voltage (Vbias-substrate1) is applied to the substrate 1, as shown by Figures 4 and 5A.

[0068] The portion 10b of the upper surface 10a is exposed to a plasma treatment 20 using bias pulsing from a chlorine-based gas mixture. According to one embodiment, the gas mixture includes boron trichloride (BCl3) or chlorine (Cl2). In some embodiments, boron trichloride (BCl3) is mixed with chlorine (Cl2). The chlorine-based plasma may be based on a chemistry that includes only one or several chemical species that include the element Cl, and possibly one or more other species, e.g., one or more inert gases.

[0069] The plasma treatment 20 using bias pulsing can be obtained by intermittently or periodically operating a bias voltage Vbias-substrate1 applied to the substrate 1 such that ion bombardment is performed on the exposed portion of the upper surface. An example of an apparatus that can be used is described below with reference to FIG. 8. As shown in FIG. 4, in some embodiments, a bias voltage (Vbias-substrate1) is applied to the substrate 1 for a number of times Ton, such as Ton(n) and Ton(n+1), where two successive times Ton(n) and Ton(n+1) are separated by a time Toff. In some embodiments, Toff can vary within an etching cycle. In some embodiments, Toff is constant for a given cycle, and in some instances, constant for each cycle. In some embodiments, successive Ton are constant for a given cycle, and in some examples, constant for each cycle.

[0070] In particular, it is possible to adjust the characteristics of the plasma process 20 using bias pulsing by the duty cycle DC=Ton / (Ton+Toff). In the duty cycle DC, Ton is the time frame during which the bias voltage (Vbias-substrate1) is applied to the substrate 1 during a pulse period, and Toff is the time frame during a pulse period during which the bias voltage applied to the substrate (Vbias-substrate2) is lower than the bias voltage applied during Ton (Vbias-substrate1), and in some examples, the bias voltage during Toff is at a minimum value similar to Vplasma. With reference to FIG. 4, a pulse period is equal to one iteration Ton and Toff. An etching cycle includes several iterations Ton and Toff.

[0071] For example, DC20% means that the ion bombardment is increased for 20% of the pulse period and reduced, preferably deactivated, for the remainder of the pulse period. The dose received by the substrate is proportional to the duty cycle. The plasma potential Vplasma can be non-zero during essentially all of the etching cycle. According to one embodiment, the plasma power supply is activated during essentially all of the etching cycle.

[0072] During Ton, a bias voltage Vbias-substrate, called Vbias-substrate1, is applied to the substrate 1 so that the III-N layer is exposed to ion bombardment. During Toff, a bias voltage Vbias-substrate, called Vbias-substrate2, is applied to the substrate 1 so that the III-N layer is exposed to reduced ion bombardment compared to during Ton. For example, |Vbias-substrate2| is lower than |Vbias-substrate1|, preferably |Vbias-substrate2|≦0.5*|Vbias-substrate1|, more preferably |Vbias-substrate2|≦0.2*|Vbias-substrate1|.

[0073] In some embodiments, a non-zero bias voltage Vbias-substrate1 is applied to the substrate 1 during Ton, with an absolute value |Vbias-substrate1| equal to or greater than 100 V during at least a portion of the etch cycle. In some embodiments, the absolute value |Vbias-substrate1| is between 100 V and 350 V. When |Vbias-substrate1| is equal to or greater than 100 V, it is possible to increase the ion bombardment during Ton and thus increase the etch rate, while limiting damage due to bias voltage pulsing.

[0074] During Toff, in some embodiments, no voltage bias is applied to the substrate, i.e. Vbias-substrate2 is switched off or equal to zero. For this purpose, the polarization device 312 (described further below) can be deactivated during Toff. Ion bombardment is thus minimized. Preferably |Vbias-substrate2|=0. During Toff, theoretically |Vbias-substrate2|=0V, i.e. no Vbias-substrate is spontaneously applied to the substrate 1 by the polarization device 312 during Toff, and a residual Vbias-substrate2 may still be applied to the substrate due to seizing phenomena in the plasma. The voltage at the substrate 1 may in this case be similar to Vplasma. In this condition, the ions in the chamber may still be energized and slight ion bombardment occurs on the substrate 1, but the energy of the ions is significantly reduced since Vplasma is generally lower than 20V. The plasma potential during Toff is generally lower than 20V, more specifically, approximately equal to 15V during Toff.

[0075] In what follows, it is considered, without limitation, that no Vbias-substrate is applied to substrate 1 during Toff. Further references to Vbias-substrate relate to the bias voltage Vbias-substrate1 applied during Ton, unless otherwise specified.

[0076] Vbias-substrate can vary over an etch cycle (pulsing between Ton and Toff), for example, Vbias-substrate can decrease or remain constant along an etch cycle. In some embodiments, |Vbias-substrate| is constant during Ton and exceeds 100V for at least a portion of the cycle, so that |Vbias-substrate| is greater than 100V. In some embodiments, the average of Vbias-substrate exceeds 100V in absolute value over at least a portion of the cycle.

[0077] The plasma is partially operated with a plasma potential Vplasma set by the plasma source 30, which controls the plasma density and therefore the amount of ions. When bias pulsing is activated, Vbias-substrate during Ton increases the energy of the ions while the exposed portion 10b of the upper surface 10a is bombarded with ions. The higher voltage provided by Vbias-substrate causes the ions to be more highly energized (compared to an ion plasma with Vplasma only) and therefore a higher etch rate into the exposed portion 10b (i.e., ions move faster towards the exposed portion 10b during Ton). Since the ion bombardment is mainly activated, preferably only during Ton, the average energy of the ions striking the exposed portion 10b is reduced. The average energy of the ion bombardment is lowered, limiting the degradation of the layer to be etched. The degradation and the etch rate are proportional to the duty cycle and therefore to the time Ton during which ion bombardment occurs on the exposed portion 10b. During Ton and Toff, the plasma density may remain constant, and therefore the number of ions impinging on the surface to be etched may remain constant. According to some embodiments, the plasma treatment with bias pulsing allows for an increased etching rate of the III-N layer compared to ALE, compared to steady-state etching at high voltages (e.g., 150V-300V). Thus, the damage that may occur to the III-N layer is significantly reduced. Overall, the method in the present disclosure significantly reduces the etching duration while the degradation level of the layer to be etched remains comparable, obtaining sufficient quality of the III-N layer for the operation of the microelectronic device, such as a transistor or diode, in which the substrate is integrated.

[0078] According to one embodiment, the RF plasma source is also pulsed, i.e., the plasma source is operated intermittently. These pulsings can be synchronous. Pulsing both the plasma source and Vbias-substrate provides the advantages described above.

[0079] According to one example, the duty cycle is comprised between 10% and 80%, in some examples between 20% and 70%, and in some examples essentially equal to 50%. Adjusting the duty cycle percentage can improve the tradeoff between the quality of the III-N layer after etching and the time required to complete the etching of the III-N layer.

[0080] According to one embodiment, the etching cycle is performed such that the etched portion of the III-N layer 10 has a thickness d measured essentially perpendicular to the main extension plane of the III-N layer, as shown in FIG. 10c In some embodiments, the thickness d 10c can be between 20 nm and 3 μm, especially when the substrate is implemented into a transistor, such as a HEMT. In some embodiments, the thickness d 10c can be 100 nm to 5 μm when the substrate is mounted on an LED, e.g., μm-LED. In some embodiments, only one etch cycle is required to achieve the desired thickness for portion 10c. In some embodiments, multiple etch cycles can be used to achieve the desired thickness. When multiple etch cycles are used, the total duration of the multiple cycles can be determined based on the desired etch thickness. Whether the method includes one etch cycle or multiple etch cycles for the same etch thickness, embodiments of the present disclosure allow for a significant reduction in the number of cycles and duration of the method compared to existing ALE techniques. Additionally, because the number of cycles is reduced (compared to existing ALE techniques), some steps, such as reactor purging steps, are eliminated, which further reduces the overall production time.

[0081] Non-limiting examples of parameters used in embodiments of the present disclosure are described below.

[0082] For example, successive etching cycles may be performed as shown by FIG. 5B and FIG. 5A. In each cycle, the portion 10b of the upper surface 10a may be exposed to a plasma treatment 20 using chlorine-based bias pulsing, while a bias voltage Vbias-substrate is applied to the substrate 1. The Vbias-substrate V1, V2 may vary between cycles, preferably between each cycle. Thus, the ion energy may be adapted (or changed) between different cycles, respectively. In some embodiments, the Vbias-substrate of at least one etching cycle is strictly lower than the Vbias-substrate of the previous etching cycle. In some embodiments, the Vbias-substrate of the successive etching cycles is gradually lower. For example, if V2 in FIG. 5B is followed by V1 in FIG. 5A, V1 may be lower than V2 (i.e., V2>V1), etc. Each Vbias-substrate may be strictly lower than the Vbias-substrate applied in the previous etching cycle. Vbias-substrate may be reduced in each subsequent cycle. This allows for a faster etch rate but a stronger impact at the beginning and a more precise etch but a weaker impact at the end. Thus, when the desired etch level is reached, the damage induced to the III-N layers can be limited. Vbias-substrate can be 100V or less during at least some of the cycles, especially for the last cycle.

[0083] Each etching cycle is performed, for example, in an etching reactor, for example, an inductively coupled plasma (ICP) reactor as described below. The ICP reactor may be a reactive ion etching (RIE) ICP reactor.

[0084] In some embodiments, each step in the cycle is performed in the same etch reactor, which reduces the number of steps and the overall process time, and also eliminates the need to remove layer 10 from the device, which is more likely to cause contamination.

[0085] Non-limiting examples of parameters used in embodiments of the present disclosure are described below.

[0086] Additional pre-etch step According to the example shown in FIG. 5C, the method includes a pre-etch step before the above-described etch cycle, in which the portion 10b of the upper surface 10a is exposed to a chlorine-based plasma 22 treatment. A non-zero and non-pulsing Vbias-substrate V3 may be applied to the substrate 1 during the plasma 22 treatment. In some embodiments, the Vbias-substrate V3 may be essentially equal to or different from the Vbias-substrate of the subsequent etch cycle. For example, the Vbias-substrate V3 during the pre-etch is higher than the Vbias-substrate of the subsequent etch cycle. In some embodiments, the Vbias-substrate V3 during the pre-etch is 100V or more during at least a portion of the pre-etch cycle. A plasma treatment with a non-pulsing bias is faster than a plasma treatment with a pulsed bias, but causes increased damage to the layer being etched. A prior plasma treatment with a non-pulsing bias is particularly useful for etching thick portions of the III-N layers, where a fast first etch step can be used to etch most of the layer, and the etch can be terminated by limiting damage to the III-N layers.

[0087] This pre-etch step can replace or complement the successive etch cycles described above. For example, two successive etch cycles can be performed with a plasma treatment with bias pulsing, with Vbias-substrate V1=200V and V2=90V, respectively. Two successive etch cycles can be performed with a plasma treatment with a non-pulsed plasma, with Vbias-substrate V1=200V, and bias pulsing, with Vbias-substrate V2=90V.

[0088] Example of subsequent steps after a prior etch cycle 6 shows the result after an etching cycle through the mask 14, after the mask 14 has been removed. The portion 10c of the III-N layer 10 is now at a thickness d from the upper surface 10a. 10c It is etched up to

[0089] The etched portions 10c form openings in the III-N layer 10, which may for example be filled with one or more materials to form functional parts of a microelectronic device.

[0090] 7, etched portions 10c may be filled with a conductive material to form electrical contacts, e.g., grid 15. Although not shown, other etched portions, such as shallower etched portions that extend only through layers 101 and 102, may be filled to form sources and drains. In this example, layer 100 forms the active layer of a transistor.

[0091] Of course, numerous other microelectronic devices may be formed from the etched portions 10c of the III-N layer 10, such as LEDs and, more specifically, LEDs emitting in the μm wavelength range (μm-LEDs).

[0092] Example of the device FIG. 8 illustrates an exemplary ICP plasma reactor 3 that can be used to practice embodiments of the present disclosure.

[0093] According to one embodiment, the reactor 3 includes a plasma source 30. The plasma potential Vplasma can be set by a coil 300 or a power supply 301 coupled to an antenna located outside the chamber 31. Typically, an alternating current flows through the coil 300, inducing a magnetic field inside the chamber 31. A gas mixture is introduced into the chamber 31 through a duct 303, as represented by the arrows on the top of the reactor. This magnetic flux variation inductively generates an RF electric field, and thus an electromagnetic field, which serves to initiate and maintain the plasma in the chamber 31. The plasma density and dissociation coefficient are typically controlled by the RF power introduced into the coil. In an ICP reactor, the plasma potential Vplasma is offset from the substrate 1. The plasma is ignited below the quartz window 302 by a planar coil 300 above the quartz window 302.

[0094] The reaction chamber 31 may include an interior defined by an outer wall 310, within which the substrate 1 is disposed.

[0095] The reaction chamber 31 may include a sample holder 311, which may also be called a tray. The substrate 1 may be placed on the sample holder 311 by its backside. The front side of the substrate 1 is exposed to the species present in the reaction chamber 31. The tray 311 is preferentially electrically conductive. The reactor 3 also includes a pump 313 to control the pressure in the reaction chamber 31 synergistically with the flow rate of the introduced gas and to extract the species present in the reaction chamber 31.

[0096] Advantageously, the reactor 3 includes a polarization device 312 configured to apply a polarization bias voltage Vbias-substrate to the tray 311, for example via a radio frequency power generator. This voltage may be applied eventually to the substrate 1, at least on the side facing the plate 311, regardless of whether this side is conductive or not. This polarization device 312 is different from the plasma source 30, and more specifically from the plasma power supply 301. Vbias-substrate increases the ion energy at the substrate 1. In the absence of Vbias-substrate, at zero voltage, the ion energy is similar to Vplasma. Thus, the efficiency of ion bombardment on the III-N layer 10 can be better controlled than with a non-remote plasma source 30, or for example with a remote source that is not associated with the application of Vbias-substrate by the substrate polarization device 312. In addition, the use of the remote source 30 avoids direct contact of the plasma with the substrate 1 in the formation zone of the plasma. Such contact may damage the substrate 1. The use of an offset plasma source also minimizes the directionality of the plasma process, which may facilitate the fabrication of three-dimensional structures, especially nanostructures.

[0097] The polarization device 312 and plasma power supply 301 are configured to apply Vbias-substrate to the tray 311 independent of the plasma potential Vplasma. Vbias-substrate and Vplasma are independent of each other. Vbias-substrate and Vplasma are controlled independently of each other. Thus, the polarization device 312 is distinct from an impedance matching unit that may be associated with the sample holder 311.

[0098] Example of experimental parameters Non-limiting examples of parameters used in the etch cycle are now described. In some embodiments, the same or similar parameters can be applied to the pre-etch with non-pulsing bias plasma process, apart from the frequency not being applied to the non-pulsing bias plasma process. In some embodiments, the bias pulsing plasma process 20 is configured to have a pulse frequency F=1 / (Ton+Toff), where F can be between 100 Hz and 1 kHz, and in some cases, between 150 Hz and 1 kHz. For example, the pulse frequency can be set by a polarization device or bias RF generator 312.

[0099] In some embodiments, the power of the generating source may be comprised essentially between 100W and 2000W, and in some implementations between 300W and 1000W.

[0100] In some embodiments, the flow rate of the gas species can range from 30 sccm to 1500 sccm, hi some implementations, the flow rate can be from 50 sccm to 500 sccm.

[0101] In some embodiments, the introduced gas species can be Cl2 combined with BCl3. Preferably, the amount of Cl2 introduced is greater than the amount of BCl3 introduced. For example, the Cl2 flow rate is greater than the BCl3 flow rate. Similarly, the gas mixture intended to form the plasma includes more Cl2 than BCl3. In some embodiments, the ratio of Cl2 to BCl3 may be varied, such as 100% Cl2 and 0% BCl3 or 0% Cl2 and 100% BCl3. In some embodiments, the introduced gas species may be diluted with a neutral gas, such as Ar or He. In some embodiments, the introduced gas species may be diluted with other reactive gases, such as N2 and O2.

[0102] In some embodiments, the pressure in the reaction chamber 31 may be essentially comprised between 2 mTorr and 250 mTorr, in some examples between 5 mTorr and 90 mTorr, and in some examples between 5 mTorr and 20 mTorr, where 1 Torr = 1 = mmHg ≈ 133,322 Pa. In some embodiments, the pressure in the reaction chamber 31 may be adjusted as a function of the introduction gas flow rate and the suction by the pump 313.

[0103] In some embodiments, the wafer temperature of the reaction chamber 31 may be comprised essentially between 20° C. and 80° C., and in some examples between 30° C. and 60° C. The temperature of the reaction chamber may be the temperature of the walls 310 and / or the temperature of the sample holder 311.

[0104] In some embodiments, the absolute value of Vbias-substrate is essentially comprised between 20 V and 800 V. In some examples, it is comprised between 20 V and 350 V, in some examples, it is comprised between 100 V and 500 V, and in some examples, it is comprised between 150 V and 350 V. This parameter primarily determines the energy of each ion during plasma processing using bias pulsing.

[0105] The duration of each etching cycle can be adapted depending on the desired thickness to be etched.

[0106] In some cases, a stabilization step may be performed before any plasma processing step, e.g., before each plasma processing step, to stabilize the gases, pressure, and temperature. This stabilization phase may be performed for a duration of several seconds.

[0107] Material Examples 2, III-N layer 10 comprises multiple layers, each based on a III-N material. In this non-limiting example, layer 10 comprises a layer 100 of GaN, a layer 101 of AlN, and a layer 102 of AlGaN, disposed successively from support 13. According to another embodiment, layer 10 comprises a layer 100 of GaN and a layer 102 of AlGaN, disposed successively from support 13 without an intermediate layer of AlN.

[0108] In some embodiments, a buffer layer 11 may be disposed between layer 10 and support 13, as shown, for example, in FIG.

[0109] Although not shown, in some embodiments, an oxide layer may be disposed on top of layer 10. For example, an oxide layer may be disposed in direct contact with top surface 10a.

[0110] Non-limiting embodiments and characterization by Rsheet measurements Standard electrical characterization techniques (van der Pauw and transmission line methods) require suitable structures and therefore lithographic processes. Aiming to characterize the etched III-N layer 10 after etching without the need for stacking time-consuming and costly steps, the four-point probe method is used to characterize the layer resistance Rsheet of the III-N layer without lithographic steps. The layer resistance is also called Rsheet, expressed in Ω / □ and also denoted Q / sq. The layer resistance is measured, for example, by the known four-point probe method. An example of this known method is described, for example, in patent application EP 3023799 A1, published on March 25, 2016, and named by C. Leroux and J. LEHMANN as inventors.

[0111] In general, this electrical characterization can be used to evaluate the electrical degradation induced by different etching processes, especially in this context after etching of the III-N layer 10. An example of the four-probe method is now described.

[0112] According to some embodiments, the measurement is performed in two stages, as shown in Figures 9A and 9B. After aligning the four metal chips 40 and placing them at equal distances from each other, for example within 1 mm from each other, a potential difference is created with the two-dimensional electron gas 100a of the III-N layer 10, hereafter referred to as 2DEG. To do this, a stack short circuit is performed between each chip 40 and the substrate 1. As shown in Figure 9A, for each chip, a voltage of 120 V is applied between the chip 40 and the substrate 1. This creates a vertical short circuit in a direction essentially perpendicular to the main extension plane of the III-N layer. The vertical short circuit contacts the 2DEG, which extends along a plane essentially parallel to the main extension plane of the III-N layer. After the contact with the 2DEG is made, a measurement can be performed. As shown in Figure 9B, a current I of the order of milliamps is applied to chip 40 number 1, crosses the 2DEG, and emerges from chip 40 number 4, which is connected to ground. Chips 2 and 3 are used to measure the voltage V of the 2DEG while the current I passes through.

[0113] Determination of Rsheet in the square, i.e. the resistance in the 2DEG, is possible by applying the following formula, which is obtained by assuming collinear measurements on a semi-infinite thin film:

[0114]

number

[0115] If V is the measured voltage, I is the applied current, and F is the form factor. In a thin film configuration, the form factor is

[0116]

number

[0117] is given by:

[0118] For example, the equipment used to perform this measurement is a SUMMIT1200 semi-automated probe system available from CASCADE Microtech operating in conjunction with a 4156C parameter analyzer available from Agilent. An HP Basic program allows for automation of the short circuit and measurement.

[0119] Before each series of measurements, the instrument is preferably tested on a reference plate with known Rsheet to determine the measurement deviation. If the deviation is too large, the positioning of the chip and its condition are checked until the Rsheet measurement is acceptable. The standard deviation of the measurements is on the order of a few percent.

[0120] Some embodiments will now be described by way of non-limiting examples: The substrate shown in Figure 2 and described above was etched according to different conditions detailed in the following samples. 50: exposed to a continuous plasma treatment (sometimes called steady state etching) based on Cl2 / BCl3 with a 1:1 ratio and applying a non-pulsing Vbias-substrate of 237V. 51: Exposed to a plasma treatment with bias pulsing based on Cl2 / BCl3 with a ratio of 1:1, F=200Hz and DC=20%, applying a Vbias-substrate of 237V. 52: Exposed to a plasma treatment with bias pulsing based on Cl2 / BCl3 with a ratio of 1:1, F=200Hz and DC=50%, applying a Vbias-substrate of 237V. 53: Exposed to a plasma treatment using a bias pulsing treatment based on Cl2 / BCl3 with a ratio of 1:1, F=200Hz and DC=90%, applying a Vbias-substrate of 237V. 54:42 cycles of ALE. During the chlorination phase of each ALE cycle, the plasma consists of Cl2 / BCl3 with a ratio of 19:1 and no bias RF is applied. During the ion bombardment phase of the ALE cycle, the plasma consists of argon and a bias voltage of 50 V is applied to sputter the chlorinated material.

[0121] The R measurements 6 for these samples are presented in FIG. 10 relative to the unetched substrate according to the following formula:

[0122]

number

[0123] The table below summarizes the relative Rsheet, etch rate, and duration of methods for etching a 70 nm III-N layer.

[0124] [Table 1]

[0125] FIG. 10 and the above table show the advantage of etching by plasma treatment with Vbias-substrate bias pulsing. Continuous plasma treatment 50 (steady state, high voltage etch) induces an Rsheet of 52%, while ALF etching (sample 54) limits the damage by only 32% Rsheet. However, ALE etching is very long in duration and does not meet the industrial standard of less than 2 minutes etching step. As shown in the above table, similar Rsheet values ​​were achieved using plasma treatment with bias pulsing (e.g. compare sample 54 with sample 52). Etching of III-N layer by bias pulsing using application of Vbias-substrate with DC=50% achieved similar degradation of III-N layer as with ALE etching, but with a much shorter duration (40 seconds) for the same etch thickness (70 nm).

[0126] The above table also shows the etch rate of each sample to etch 70 nm of GaN. As shown in samples 51, 52, and 53, the etch duration is kept below 2 minutes, which is compatible with industrial processes. In comparison, the ALE method takes 10 minutes to etch 70 nm (or even 20 minutes if you take into account the full stabilization steps between each step of the ALE cycle).

[0127] The present invention is not limited to the examples described above. Numerous other embodiments are possible, for example by combining features already described without departing from the scope of the present disclosure. Furthermore, features described in connection with one aspect of the invention may be combined with another aspect of the invention.

[0128] For example, in the above examples, the top layer is based on GaN. Nevertheless, the invention also extends to embodiments in which the top layer is a layer based on other III-N materials. The III-N material based layer may include at least one from the group consisting of indium, gallium, and aluminum. For example, the III-N layer may be GaN, AlGaN, AlN, InGaN, or AlInGaN. Thus, all of the above examples, features, steps, and technical advantages with reference to GaN-based layers are applicable to structures based on any of the III-N materials.

[0129] Moreover, in the examples described above, the structure is a layer. Nevertheless, all of the above examples, features, steps, and technical advantages referring to the structure forming a layer are applicable to the structure forming a point structure without forming a layer, for example, a three-dimensional relief. The structure may be a nanostructure or may comprise a plurality of nanostructures. The second layer may be a nanostructure or may comprise a plurality of nanostructures. [Explanation of symbols]

[0130] 1 Board 3. Reactor 10 III-N layer 10a top surface 10b Exposed area 10c Etched part 11, 12 layers 13 Support 14 Mask 15 Grid 20 Plasma processing using bias pulsing 22 Plasma 30 Plasma Source 31 Chamber 40 Metal Chip 100, 101, 102 layers 100a Two-dimensional electron gas 300 coils 301 Power supply 302 Quartz window 303 Duct 310 Exterior Wall 311 Sample Holder 312 Polarization Device 313 Pump d 10c Thickness V1, V2, V3 Vbias-substrate

Claims

1. A method for etching at least a portion (10c) of a layer (10) based on a III-N material, comprising: Providing a substrate having an upper surface and at least one layer based on a III-N material, referred to as a "III-N layer"; performing at least one etching cycle comprising exposing at least a portion of the top surface to a chlorine-based plasma treatment with a plasma potential Vplasma, the plasma treatment being performed with bias voltage pulsing and configured to have a duty cycle DC=Ton / (Ton+Toff) comprised between 10% and 80%; a first non-zero bias voltage, referred to as Vbias-substrate1, is applied to the substrate during at least a portion of the Ton time frame, the first Vbias-substrate1 having an absolute value |Vbias-substrate1| of 100V or greater; During a Toff time frame, a second bias voltage, called Vbias-substrate2, is applied to the substrate, such that Vbias-substrate2 has an absolute value |Vbias-substrate2| that is less than |Vbias-substrate1| or no bias voltage is applied to the substrate (1); The method, wherein Vbias-substrate1 and Vbias-substrate2 are independent of Vplasma to etch the portion (10c) of the III-N layer (10) extending from the portion (10b) of the top surface (10a).

2. 2. The method of claim 1, wherein |Vbias-substrate1| is configured between 100V and 800V, preferentially between 150V and 350V, during at least a portion of the Ton time frame.

3. 3. The method of claim 1 or 2, wherein |Vbias-substrate1|>2*|Vbias-subrate2|, preferably |Vbias-substrate1|>5*|Vbias-subrate2|, and more preferably |Vbias-substrate1|>10*|Vbias-subrate2|, during at least a portion of the Ton time frame.

4. The method according to any one of claims 1 to 3, wherein the duty cycle is comprised between 20% and 70%.

5. 5. The method according to any one of claims 1 to 4, wherein the at least one etching cycle has a duration such that the etched portion (10c) of the at least one III-N layer (10) has a thickness (d10c) comprised between 20 nm and 3 μm.

6. The method according to any one of claims 1 to 5, wherein the plasma treatment (20) using bias pulsing is configured to have a frequency F=1 / (Ton+Toff) comprised between 100 Hz and 5 kHz.

7. The method of any one of claims 1 to 6, wherein the method comprises a plurality of etching cycles, and |Vbias-substrate1| varies between the etching cycles.

8. The method of any one of claims 1 to 7, wherein |Vbias-substrate1| is less than or equal to 100V during at least some other cycles of the plurality of cycles.

9. Prior to the at least one etching cycle, a prior etching cycle is included for the portion (10c'') of the III-N layer (10), the prior etching cycle comprising: exposing said at least a portion (10b) of said upper surface (10a) to a chlorine-based plasma (23) treatment with a plasma potential Vplasma; applying a non-zero and non-pulsing bias voltage Vbias-substrate to the substrate during the plasma (23) treatment, Vbias-substrate being independent of Vplasma.

10. The method according to any one of claims 1 to 9, wherein prior to said at least one etching cycle, said top surface (10a) of said III-N layer (10) is covered by a mask (14).

11. 11. The method according to any one of claims 1 to 10, wherein the plasma treatment (20) using a bias pulsing treatment is carried out in a reaction chamber (31), the pressure inside the reaction chamber (31) being comprised between 2 mTorr and 250 mTorr during the at least one etching cycle.

12. The method according to any one of claims 1 to 11, wherein said plasma treatment (20) using a bias pulsing treatment is carried out in a reaction chamber (31), the temperature of which is comprised between 20°C and 80°C, preferentially between 30°C and 60°C, during said at least one etching cycle.

13. The plasma treatment (20) using a bias pulsing treatment is preferentially performed using BCl 3 Cl combined with 2 The method according to any one of claims 1 to 12, which is based on

14. 14. The method of claim 1, wherein the III-N material comprises a chemical element selected from the group consisting of aluminum and gallium, for example, the III-N material is selected from the group consisting of AlGaN, GaN, AlN, InGaN, and AlInGaN.

15. 15. The method according to any one of the preceding claims, wherein the substrate (1) is integrated into a transistor, preferentially a HEMT transistor, for power electronic devices.

16. 15. The method according to any one of the preceding claims, wherein the substrate (1) is integrated into a light emitting diode.

Citation Information

Patent Citations

  • Method and apparatus for anisotropic tungsten etching

    JP2016139792A

  • ATOMIC LAYER ETCHING OF GaN AND OTHER III-V MATERIALS

    JP2017022368A

  • Method for etching high-k dielectric using pulsed bias power

    US20140256149A1

  • Method for measuring the resistance of a coated conductive layer

    EP3023799A1