Polyester resin and its manufacturing method
A biodegradable polyester resin is produced using a furandicarboxylic acid-based copolymer with a phosphorus-based stabilizer and complementary dyes to address thermal discoloration and environmental issues, achieving high brightness and efficient production.
Patent Information
- Application Number
- JP2024535968
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-17
- Filing Date
- 2022-11-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The production of polyester resins using terephthalic acid leads to depletion of crude oil resources and environmental pollution due to carbon dioxide emissions, and the replacement with furandicarboxylic acid results in thermal discoloration and low brightness.
A biodegradable polyester resin is produced using a copolymer containing a furandicarboxylic acid compound, a phosphorus-based heat stabilizer with an ester group, and complementary coloring agents like blue and red dyes to suppress thermal discoloration and enhance brightness.
The resin exhibits high brightness and biodegradability while minimizing thermal discoloration, with the phosphorus-based stabilizer controlling polymerization rates and the dyes correcting any discoloration during the manufacturing process.
Smart Images

Figure 2024544394000001 
Figure 2024544394000002 
Figure 2024544394000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester resin and a method for producing the same. [Background technology]
[0002] Polyester resin is a polymer resin that has ester (RO-C(=O)-R') functional groups in its main chain, and is used in a variety of industrial fields for a variety of purposes, including packaging, displays, and insulating materials.
[0003] A representative example of such a resin is polyethylene terephthalate (PET) resin, which is produced by reacting terephthalic acid (TPA) with ethylene glycol (EG).
[0004] However, the main raw material of terephthalic acid is paraxylene, which is produced by refining crude oil. Therefore, the production and use of terephthalic acid leads to the depletion of crude oil resources. In addition, the decomposition of terephthalic acid increases carbon dioxide emissions, which leads to environmental pollution and may cause climate change such as global warming.
[0005] In relation to this, attempts are being made to replace terephthalic acid with 2,5-furandicarboxylic acid (FDCA) during the production of polyester resins. As a biomass-derived material, FDCA can prevent the depletion of crude oil resources and minimize environmental pollution and climate change due to its biodegradability.
[0006] However, furandicarboxylic acid has low thermal stability and causes yellowing or browning during the production process of polyester resin, so when terephthalic acid is replaced with furandicarboxylic acid, it is inevitable to obtain a yellowed or browned polyester resin. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a biodegradable polyester resin that is suppressed from discoloring due to heat, and a method for producing the same. [Means for solving the problem]
[0008] In one embodiment of the present invention, there is provided a polyester resin comprising: a copolymer comprising a diacid residue and a diol residue; a phosphorus-based heat stabilizer; and a color complementing agent, wherein the diacid residue comprises a residue derived from a furandicarboxylic acid compound, the diol residue comprises a residue derived from an alkylene glycol compound, the phosphorus-based heat stabilizer comprises an ester group at a terminal, and the color complementing agent comprises a blue dye and a red dye.
[0009] In another embodiment of the present invention, there is provided a method for producing a polyester resin, the method including the steps of: esterifying a monomer mixture including a diacid component and a diol component; prepolymerizing the esterification reaction product in the presence of a phosphorus-based heat stabilizer and a color complementing agent; and polycondensing the prepolymerized polymer, wherein the diacid component includes a furandicarboxylic acid-based compound, the diol component includes an alkylene glycol-based compound, the phosphorus-based heat stabilizer includes an ester group at a terminal thereof, and the color complementing agent includes a blue dye and a red dye. Effect of the Invention
[0010] According to one embodiment of the present invention, it is possible to provide a polyester resin that exhibits high brightness by suppressing thermal discoloration and by providing complementary colors while exhibiting biodegradability.
[0011] In another embodiment of the present invention, a method can be provided for obtaining a polyester resin that exhibits high brightness by suppressing thermal discoloration during the manufacturing process and compensating for already discolored resin. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] (Definition of terms) Throughout this specification, when a part is said to "comprise" a certain element, this means that it can further include other elements, but not to the exclusion of other elements, unless specifically stated to the contrary.
[0013] To the extent used throughout this specification, the terms "step of" or "step of" do not mean "step for."
[0014] As used herein, the term "moiety" refers to a certain portion or unit derived from a particular compound when the particular compound participates in a chemical reaction and is included in the product of the chemical reaction.
[0015] Specifically, in the polyester resin, the "residue" derived from a furan-based dicarboxylic acid and the "residue" derived from an alkylene glycol refer to a portion derived from a furan-based dicarboxylic acid and a portion derived from an alkylene glycol, respectively.
[0016] The term "alkyl" as used herein, unless otherwise specified, refers to a saturated monovalent aliphatic hydrocarbon group, including straight and branched chains, having the specified number of carbon atoms. An alkyl group typically contains 1 to 20 carbon atoms ("C1-20 alkyl"), preferably 1 to 12 carbon atoms ("C1-12 alkyl"), more preferably 1 to 8 carbon atoms ("C1-8 alkyl"), or 1 to 6 carbon atoms ("C1-6 alkyl"), or 1 to 4 carbon atoms ("C1-4 alkyl"). Examples of alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, iso-butyl, tert-butyl, n-pentyl, isopentyl, neopentyl, n-hexyl, n-heptyl, n-octyl, and the like. An alkyl group can be substituted or unsubstituted. Unless otherwise specified, an alkyl group can be substituted with one or more halogens, up to the total number of hydrogen atoms present on the alkyl residue. Thus, alkyl having 1 to 4 carbon atoms includes halogenated alkyl groups, for example, fluorinated alkyl groups having 1 to 4 carbon atoms, such as trifluoromethyl (-CF3) or difluoroethyl (-CH2CHF2).
[0017] Alkyl groups described herein as optionally substituted are substituted with one or more substituents, which are independently selected unless otherwise specified. The total number of substituents is the same as the total number of hydrogen atoms on the alkyl residue to the extent that such substitution makes chemical sense. Optionally substituted alkyl groups can typically contain 1-6 optional substituents, often 1-5 optional substituents, preferably 1-4 optional substituents, and more preferably 1-3 optional substituents.
[0018] Suitable optional substituents for the alkyl group include, but are not limited to, alkyl of 1 to 8 carbon atoms, alkenyl of 2 to 8 carbon atoms, alkynyl of 2 to 8 carbon atoms, cycloalkyl of 3 to 8 carbon atoms, 3 to 12 membered heterocyclyl, aryl of 6 to 12 carbon atoms, and 5 to 12 membered heteroaryl, halo, =O (oxo), =S (thiono), =N-CN, =N-OR. x , =NRx , -CN, -C(O)R x , -CO2R x , -C(O)NR x R y , -SR x , -SOR x , -SO2R x , -SO2NR x R y , -NO2, -NR x R y , -NR x C(O)R y , -NR x C(O)NR x R y , -NR x C(O)OR x , -NR x SO2R y , -NR x SO2NR x R y , -OR x , -OC(O)R x and -OC(O)NR x R y Each R x and R y are independently hydrogen (H), alkyl having 1 to 8 carbon atoms, acyl having 1 to 8 carbon atoms, alkenyl having 2 to 8 carbon atoms, alkynyl having 2 to 8 carbon atoms, cycloalkyl having 3 to 8 carbon atoms, 3 to 12 membered heterocyclyl, aryl having 6 to 12 carbon atoms, or 5 to 12 membered heteroaryl, or R x and R y can form, together with the N atom to which they are attached, a 3- to 12-membered heterocyclyl or a 5- to 12-membered heteroaryl ring, each of which is optionally O, N, and S(O) q (wherein q is 0 to 2); each R x and R yis optionally substituted with 1 to 3 substituents independently selected from the group consisting of halo, =O, =S, =N-CN, =N-OR', =NR', -CN, -C(O)R', -COR', -C(O)NR'2, -SOR', -SOR', -SONR', -NO2, -NR'2, -NR'C(O)R', -NR'C(O)NR'2, -NR'C(O)OR', -NR'SOR', -NR'SONR'2, -OR', -OC(O)R' and -OC(O)NR'2, wherein each R' is independently selected from hydrogen (H), and each of said alkyl having 1 to 8 carbon atoms, alkenyl having 2 to 8 carbon atoms, alkynyl having 2 to 8 carbon atoms, cycloalkyl having 3 to 8 carbon atoms, 3 to 12 membered heterocyclyl, aryl having 6 to 12 carbon atoms, and heteroaryl having 5 to 12 carbon atoms may be optionally substituted as further defined herein.
[0019] The term "alkoxy" as used herein, unless otherwise specified, refers to a monovalent -O-alkyl group in which the alkyl portion has the specified number of carbon atoms. An alkoxy group typically has 1 to 8 carbon atoms ("C1-8 alkoxy"), or 1 to 6 carbon atoms ("C1-6 alkoxy"), or 1 to 4 carbon atoms ("C1-4 alkoxy"). For example, an alkoxy having 1 to 4 carbon atoms includes methoxy (-OCH3), ethoxy (-OCH2CH3), isopropoxy (-OCH(CH3)2), tert-butyloxy (-OC(CH3)3), and the like. The alkoxy group may be substituted or unsubstituted on the alkyl portion with the same groups as are applicable for the alkyl and described herein. In particular, an alkoxy group may be optionally substituted with one or more halo atoms, in particular one or more fluoro atoms, up to the total number of hydrogen atoms present on the alkyl portion. Such groups are referred to as "haloalkoxy" groups having the specified number of carbon atoms and substituted with one or more halo substituents, e.g., when fluorinated, more specifically as "fluoroalkoxy" groups; typically, such groups contain 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, often 1 or 2 carbon atoms, and 1, 2 or 3 halo atoms (i.e., a "C1-6 haloalkoxy," a "C1-4 haloalkoxy," or a "C1-2 haloalkoxy"). More specifically, a fluorinated alkyl group can typically be specifically referred to as a fluoroalkoxy group substituted with 1, 2 or 3 fluoro atoms, e.g., a C1-6, C1-4, or C1-2 fluoroalkoxy group. Thus, C1-4 fluoroalkoxy includes trifluoromethyloxy (-OCF3), difluoromethyloxy (-OCF2H), fluoromethyloxy (-OCFH2), difluoroethyloxy (-OCH2CF2H), and the like.
[0020] As used herein, the term "divalent aliphatic hydrocarbon (i.e., alkylene)" refers to a divalent hydrocarbyl group having a specified number of carbon atoms that can link two other groups together, unless otherwise specified. Often, alkylene is defined as -(CH2)n - (where n is 1 to 8, preferably n is 1 to 4). In certain cases, alkylene can also be substituted with other groups and can include at least one degree of unsubstitution (i.e., alkenylene or alkynylene residue) or ring. The open valences of an alkylene do not have to be at opposite ends of the chain. Thus, branched alkylene groups, such as -CH(Me)-, -CH2CH(Me)-, and -C(Me)2-, are also included within the scope of the term "alkylene", as are cyclic groups, such as cyclopropane-1,1-diyl, and unsaturated groups, such as ethylene (-CH=CH-) or propylene (-CH2-CH=CH-). The alkylene groups are as appropriate for alkyl and are unsubstituted or substituted with the same groups as described herein.
[0021] As used herein, the terms "optionally substituted" and "substituted or unsubstituted" are used interchangeably to indicate that the particular group being described may have no non-hydrogen substituents (i.e., unsubstituted) or that the group may have one or more non-hydrogen substituents (i.e., substituted). Unless otherwise specified, the total number of substituents that may be present is equal to the number of H atoms present in the unsubstituted form of the group being described. When any substituent is attached through a double bond (e.g., an oxo (=O) substituent), the group occupies an available valence and the total number of other substituents contained therein is reduced by two. When any substituent is independently selected from a list of alternatives, the selected groups may be the same or different. It will be understood that throughout this specification, the number and nature of any substituent is limited to the extent that such substitution satisfies chemical sense.
[0022] In this specification, the CIE1976 L*a*b* color system corresponds to a color space defined by the CIE (International Commission on Illumination) and currently standardized worldwide.
[0023] In this CIE 1976 L*a*b* color space, the L* value represents lightness in CIE, ranging from 0 to 100, with 0 representing perfect black and 100 representing perfect white. a* represents the leaning towards either red or green, and if this value is positive, i.e. "+", it is red; if it is negative, i.e. "-", it is green. b* represents the leaning towards either yellow or blue, and if this value is positive, i.e. "+", it is yellow; if it is negative, i.e. "-", it is blue.
[0024] Based on the above definitions, the implementation of the present invention will be described in detail. However, these are merely presented as examples and do not limit the present invention, and the present invention is defined only by the scope of the claims below.
[0025] (polyester resin) In one embodiment of the present invention, there is provided a polyester resin comprising: a copolymer including a diacid residue and a diol residue; a phosphorus-based heat stabilizer; and a color complementing agent, wherein the diacid residue includes a residue derived from a furandicarboxylic acid compound, the diol residue includes a residue derived from an alkylene glycol compound, the phosphorus-based heat stabilizer includes an ester group at a terminal, and the color complementing agent includes a blue dye and a red dye.
[0026] The polyester resin of the embodiment can be produced by a series of steps of producing a polyester resin by subjecting a diacid component containing an aromatic dicarboxylic acid and a diol component containing an aliphatic diol to an esterification reaction, a prepolymerization reaction, and a polycondensation reaction.
[0027] The furandicarboxylic acid compounds are derived from environmentally friendly raw materials produced from biomass such as wood and corn, and can be completely decomposed (i.e., biodegraded) by microorganisms under certain conditions.
[0028] Therefore, by using the furandicarboxylic acid compound instead of terephthalic acid as a raw material for polyester resin, it is possible to prevent the depletion of crude oil resources. In addition, polyester resins produced using the furandicarboxylic acid compound as a raw material are biodegradable, and can contribute to preventing environmental pollution, climate change, etc.
[0029] However, the furandicarboxylic acid-based compounds have low thermal stability, and polyester resins produced using them generally turn yellow or brown and exhibit low brightness.
[0030] However, the polyester resin of the embodiment may exhibit relatively high brightness while being produced from the furandicarboxylic acid-based compound, and may be inhibited from yellowing or browning.
[0031] The color characteristics of the polyester resin of one embodiment may be due to additives provided during its manufacturing process.
[0032] Specifically, the polyester resin of the embodiment may be prepared in the presence of a phosphorus-based heat stabilizer having an ester group at its terminal. Among heat stabilizers, the phosphorus-based heat stabilizer having an ester group at its terminal may minimize thermal discoloration during the preparation process of the polyester resin.
[0033] In addition, the polyester resin of the embodiment may be manufactured in the presence of a color complementing agent containing a blue dye and a red dye. Among the color complementing agents, the color complementing agent containing a blue dye and a red dye can correct the color of the resin even if discoloration has already occurred during the manufacturing process of the polyester resin. The color complementing agent containing a blue dye and a red dye also serves as a catalyst during the manufacturing process of the polyester resin, improving the reaction rate and shortening the heat exposure time of the polyester resin.
[0034] Meanwhile, most of the phosphorus-based heat stabilizer having an ester group at its terminal and the color complementing agent including the blue dye and the red dye remain, except for the amount that is lost during the process of producing the polyester resin of the embodiment. Therefore, the polyester resin of the embodiment includes the phosphorus-based heat stabilizer having an ester group at its terminal and the blue dye and the red dye.
[0035] Overall, the polyester resin of the embodiment exhibits biodegradability, while being able to exhibit high brightness by suppressing thermal discoloration during the manufacturing process and by providing complementary colors.
[0036] The polyester resin of the embodiment will be described in detail below.
[0037] <Phosphorus-based heat stabilizer containing an ester group at the end> Phosphorus-based heat stabilizers that do not have an ester group at the end, such as triphenylphosphate and phosphoric acid, as well as non-phosphorus-based heat stabilizers, have a drawback in that they slow down the polymerization reaction rate.
[0038] In contrast, a phosphorus-based heat stabilizer having an ester group at its end has the advantage of being able to appropriately control the polymerization reaction rate and minimizing thermal discoloration during the process of producing the polyester resin of the embodiment.
[0039] The phosphorus-based heat stabilizer containing an ester group at its terminal is represented by the following chemical formula 1:
[0040] [Chemical formula 1] JPEG2024544394000001.jpg3875
[0041] In the above Chemical Formula 1, R1 is the same or different and is a substituted or unsubstituted alkyl having 1 to 10 carbon atoms; R2 is a substituted or unsubstituted alkyl having 1 to 10 carbon atoms.
[0042] Specifically, the phosphorus-based heat stabilizer containing an ester group at its terminal may be trimethyl phosphonoacetate, triethyl phosphonoacetate, or a combination thereof.
[0043] For example, a phosphorus-based heat stabilizer containing a terminal ester group can be triethyl phosphonoacetate, as shown in the examples below.
[0044] The polyester resin of the embodiment may contain the heat stabilizer having an ester group at its terminal in an amount of 1 to 50 ppm based on the weight of the copolymer, which can minimize thermal discoloration of the polyester resin.
[0045] Specifically, 1 g of the polyester resin of the embodiment is frozen under liquid nitrogen for 10 minutes and then pulverized. 100 ml of n-hexane is added per 1 g of the pulverized polyester resin, and Soxhlet extraction is performed for 6 hours to finally concentrate or dilute the resin to 50 to 250 ml. 10 to 50 μg of Fluoranthene-d10 is added as an internal standard substance, and then GC / MS analysis is performed. The remaining amount of the heat stabilizer in the polyester resin of the embodiment can be confirmed by calculating the relative ratio to the internal standard substance.
[0046] For example, the heat stabilizer having an ester group at its end may be present within a range of 1 ppm or more, 5 ppm or more, 10 ppm or more, or 15 ppm or more, and 50 ppm or less, 40 ppm or less, 30 ppm or less, or 25 ppm or less, based on the weight of the polyester resin of one embodiment.
[0047] <Color complement> The color complementing agent is a material that compensates for the color of the resin that has been thermally discolored during the process of producing the polyester resin of the embodiment and also acts as a catalyst, and may include a blue dye and a red dye.
[0048] The blue dye is not particularly limited as long as it exhibits a blue hue, and may be an anthraquinone-based blue dye, a phthalocyanine-based blue dye, or a combination thereof.
[0049] For example, as an anthraquinone blue dye, 3,3'-[(9,10-dihydro-9,10-dioxo-1,4-anthrylene)diimino]bis[N-cyclohexyl-2,4,6-trimethylbenzenesulphonamide] (product name: Solvent Blue 45, CAS NO. 23552-74-1) represented by the following chemical formula 2-1 can be used:
[0050] [Chemical formula 2-1] JPEG2024544394000002.jpg129127
[0051] The red dye is not particularly limited as long as it exhibits a red hue, and may be a perinone red dye, an azo red dye, or a combination thereof.
[0052] For example, as a perinone red dye, 8,9,10,11-Tetrachloro-12H-isoindolo[2,1-a]perimidin-12-one (product name: Solvent Red 135, CAS No. 20749-68-2) represented by the following chemical formula 3-1 can be used:
[0053] [Chemical formula 3-1] JPEG2024544394000003.jpg7899
[0054] The polyester resin of the embodiment may contain the blue dye in an amount of 1 to 150 ppm and the red dye in an amount of 1 to 100 ppm based on the weight of the copolymer.
[0055] Here, 1 g of the polyester resin is frozen under liquid nitrogen for 10 minutes and then pulverized. 100 ml of n-hexane is added per 1 g of the pulverized polyester resin, and Soxhlet extraction is performed for 6 hours to finally concentrate or dilute the resin to 50 to 250 ml. 10 to 50 μg of Fluoranthene-d10 is added as an internal standard substance, and then GC / MS analysis is performed to confirm the remaining amounts of the blue dye and the red dye in the polyester resin by calculating the relative ratio to the internal standard substance.
[0056] Specifically, the polyester resin of the embodiment may contain the blue dye in an amount of 1 ppm or more, 2 ppm or more, 5 ppm or more, or 10 ppm or more, and 150 ppm or less, 140 ppm or less, 130 ppm or less, 120 ppm or less, or 100 ppm or less, based on the weight of the copolymer.
[0057] As the content of the blue dye increases within the above range, the polyester resin of the embodiment has a decreased L* value according to the CIE1976 L*a*b* color system, a* value is roughly the same, and a* value is increased.
[0058] In addition, the polyester resin of the embodiment may contain the red dye in an amount of 1 ppm or more, 10 ppm or more, 20 ppm or more, or 30 ppm or more, and 100 ppm or less, 80 ppm or less, 70 ppm or less, 60 ppm or less, or 50 ppm or less, based on the weight of the copolymer.
[0059] As the content of the red dye increases within the above range, the polyester resin of the embodiment has a decreased L* value, a similar b* value, and an increased a* value according to the CIE1976 L*a*b* color system.
[0060] Depending on the purpose, the amount of each dye added during the process of producing the polyester resin of the embodiment can be adjusted to control the final content (residual amount) of each dye and the color properties of the resin.
[0061] The color complementing agent may contain the blue dye and the red dye in a weight ratio (blue:red) of 1:9 to 9:1 or 1:4 to 4:1.
[0062] When the blue dye and the red dye are mixed together in this manner, the yellowed or browned color of the polyester resin can be effectively corrected and its brightness can be increased.
[0063] <Copolymer> The copolymer contains a residue derived from a furandicarboxylic acid compound (hereinafter, "a residue derived from a furandicarboxylic acid compound") among diacid residues, and exhibits excellent biodegradability due to the furandicarboxylic acid compound.
[0064] The furandicarboxylic acid compound is represented by the following formula 1A:
[0065] [Chemical formula 1A] JPEG2024544394000004.jpg36133
[0066] In the above Chemical Formula 1, L1 and L2 each independently represent a single bond or a substituted or unsubstituted alkylene having 1 to 10 carbon atoms.
[0067] For example, the furandicarboxylic acid compound is 2,5-furandicarboxylic acid, and in this case, L1 and L2 in Chemical Formula 1 may all be single bonds.
[0068] The residue derived from a furandicarboxylic acid compound is represented by the following chemical formula 1-1:
[0069] [Chemical formula 1-1] JPEG2024544394000005.jpg36122
[0070] In the above chemical formula 1-1, L1 and L2 each independently represent a single bond or a substituted or unsubstituted alkylene having 1 to 10 carbon atoms; * indicates the bonding position.
[0071] For example, when the furandicarboxylic acid compound is 2,5-furandicarboxylic acid, L1 and L2 in Chemical Formula 1-1 may all be single bonds.
[0072] The copolymer contains a residue derived from an alkylene glycol compound (hereinafter, "alkylene glycol compound-derived residue") among diacid residues, and exhibits excellent compatibility and elongation properties due to the alkylene glycol compound-derived residue.
[0073] The alkylene glycol compound is represented by the following Chemical Formula 2:
[0074] [Chemical formula 2] JPEG2024544394000006.jpg1760
[0075] In the above chemical formula 2, L3 and L4 are each independently a substituted or unsubstituted alkylene having 1 to 10 carbon atoms.
[0076] For example, the alkylene glycol compound may be ethylene glycol or 1,4-butanediol, in which case L3 in Formula 2 may be a C1 alkylene (i.e., methylene), and R4 may be a C1 alkylene (i.e., methylene) or a C3 alkylene (i.e., propylene).
[0077] The alkylene glycol compound-derived residue is represented by the following chemical formula 2-1A:
[0078] [Chemical formula 2-1A] JPEG2024544394000007.jpg1780
[0079] In the above chemical formula 2-1, R3 and R4 are each independently a substituted or unsubstituted alkylene having 1 to 10 carbon atoms; * indicates the bonding position.
[0080] For example, when the alkylene glycol compound is ethylene glycol or 1,4-butanediol, R3 in Formula 2-1 can be a C1 alkylene (i.e., methylene), and R4 can be a C1 alkylene (i.e., methylene) or a C3 alkylene (i.e., propylene).
[0081] The molar ratio of the furandicarboxylic acid compound-derived residue and the alkylene glycol compound-derived residue in the copolymer may be 9:1 to 1:9, 8:2 to 2:8, or 1:1 to 1:2. Within this range, the effects of the furandicarboxylic acid compound-derived residue and the alkylene glycol compound-derived residue can be harmoniously achieved.
[0082] The copolymer may further include at least one of a diacid residue and a diol residue, in addition to the residue derived from the furandicarboxylic acid compound and the residue derived from the alkylene glycol compound.
[0083] The additional diacid residue may be derived from an aromatic dicarboxylic acid, an aliphatic dicarboxylic acid, or a mixture thereof, excluding the furandicarboxylic acid-based compound.
[0084] The additional diol residue may be derived from an aromatic diol, an aliphatic diol, or a mixture thereof.
[0085] The content of the additional residue in the polyester resin containing the additional residue can be controlled to 1 to 20 mol % based on the total 100 mol %. When the additional residue is contained in this range, the mechanical properties and heat resistance of the polyester resin can be further improved.
[0086] The copolymer may be a random copolymer or a block copolymer. Specifically, the copolymer does not include additional residues and is represented by the following formula 4:
[0087] [Chemical formula 4] JPEG2024544394000008.jpg33129
[0088] In the above Chemical Formula 4, the definitions of each substituent are as described above.
[0089] For example, the copolymer is represented by the following formula 4-1:
[0090] [Chemical formula 4-1] JPEG2024544394000009.jpg52153
[0091] Specifically, the copolymer represented by the chemical formula 4-1 corresponds to poly(ethylene furandicarboxylate) (PEF) in which the residue derived from a furandicarboxylic acid compound is a residue derived from furandicarboxylic acid, the residue derived from an ethylene glycol compound is a residue derived from ethylene glycol, and the molar ratio of the ethylene glycol-derived residue to the ethylene glycol-derived residue is 1:1.
[0092] <Number average molecular weight (Mn) and molecular weight distribution (MWD) of polyester resin> The polyester resin may have a number average molecular weight (Mn) of 20,000 g / mol or more, 21,000 g / mol or more, 22,000 g / mol or more, 23,000 g / mol or more, 24,000 g / mol or more, or 25,000 g / mol or more, but may be 30,000 g / mol or less, 29,000 g / mol or less, or 27,000 g / mol or less.
[0093] If the number average molecular weight of the polyester resin is less than 20,000 g / mol, it is difficult to process the polyester resin into a film for use as a packaging material, and the desired modulus cannot be achieved. On the other hand, if the number average molecular weight of the polyester resin is more than 30,000 g / mol, the viscosity becomes high, leading to low productivity and low yield.
[0094] The polyester resin may have a ratio of weight average molecular weight (Mw) / number average molecular weight (Mn), i.e., a molecular weight distribution (MWD), of 1 or more, 1.2 or more, 1.4 or more, or 1.5 or more, and 2.5 or less, 2 or less, 1.9 or less, or 1.8 or less.
[0095] If the molecular weight distribution of the polyester resin is less than 1, process control becomes difficult, resulting in a high defect rate and high process costs. On the other hand, if the molecular weight distribution of the polyester resin of the embodiment exceeds 2.5, the non-uniform molecular weight distribution may cause defects during product manufacturing.
[0096] <Color characteristics of polyester resin> The polyester resin of the embodiment may have an L* value of 92 to 97, an a* value of 2 or less, and a b* value of 3 or less according to the CIE1976 L*a*b* color system.
[0097] The color characteristics according to the CIE1976 L*a*b* color system can be measured in a solution state by dissolving a chip in a specific solvent at a specific concentration, rather than using a commonly known chip colorimeter. Specifically, 2 g of the polyester resin can be dissolved in 20 ml of hexafluoroisopropanol (HFIP) solvent at a concentration of 0.1 g / ml, and then measured using a solution colorimeter according to the CIE1976 L*a*b* color system.
[0098] The a* value of 2 or less and the b* value of 3 or less mean that thermal denaturation such as yellowing or browning is suppressed, and the L* value of 92 to 97 means high brightness.
[0099] Specifically, the higher the L* value is in the range of 92 or more, the closer the color to white it can be expressed. However, depending on the use, purpose, etc. of the product to which the polyester resin of the embodiment is applied, the lightness can be controlled within a range of the L* value being 92 or more, 92.5 or more, or 93 or more, and 97 or less, or 96 or less.
[0100] In the case of the a* value, the smaller the value is within a range of 2 or less, the lighter the red color and the darker the green color. However, depending on the use and purpose of the product to which the polyester resin of the embodiment is applied, the a* value can be controlled to a degree of red and green within a range of 2 or less, 1.6 or less, 1.2 or less, or 1 or less, and -3 or more, -2.5 or more, -2 or more, or -1 or more.
[0101] In the case of the b* value, the yellow color may become lighter and the blue color may become darker as the value becomes smaller within a range of 3 or less. However, depending on the use and purpose of the product to which the polyester resin of the embodiment is applied, the degree of yellow and blue may be controlled within a range of 3 or less, 2.7 or less, 2.5 or less, or 2 or less, and -5 or more, -4 or more, -3 or more, -2 or more, or -1 or more.
[0102] Although a more detailed description will be given later, the color characteristics of the polyester resin of one embodiment can be adjusted during the manufacturing process by the phosphorus-based heat stabilizer having an ester group at its terminal; and the color complementing agent including the blue dye and red dye.
[0103] <Physical properties of polyester> The polyester resin according to one embodiment of the present invention has a change in intrinsic viscosity (ΔIV 12 ) may be 0.15 (but greater than 0) dl / g.
[0104] [Formula 1] △IV 12 =IV1-IV2
[0105] In the above formula 1, IV1 is the intrinsic viscosity at 25°C, and IV2 is the intrinsic viscosity at 35°C.
[0106] The change in intrinsic viscosity according to the above formula (ΔIV 12 If the modulus is less than the lower limit, it is difficult to process the film for use as a packaging material, and the desired modulus cannot be achieved. Conversely, if the modulus is greater than the upper limit, the viscosity becomes high, leading to low productivity and low yield.
[0107] Specifically, the polyester resin of the embodiment has a change in intrinsic viscosity (ΔIV 12 ) may be 0.05 dl / g or more, 0.1 dl / g or more, or 0.14 dl / g or more, and 0.4 dl / g or less, 0.3 dl / g or less, 0.2 dl / g or less, or 0.15 dl / g or less.
[0108] The polyester resin of the embodiment may have an intrinsic viscosity at 25° C. of 0.1 to 2 dl / g, specifically 0.2 to 1.5 dl / g, more specifically 0.4 to 1 dl / g, for example, 0.6 to 0.8 dl / g.
[0109] The polyester resin of the embodiment may have an intrinsic viscosity at 35° C. of 0.1 to 2 dl / g, specifically 0.2 to 1.5 dl / g, more specifically 0.3 to 1 dl / g, for example 0.4 to 0.6 dl / g.
[0110] If the intrinsic viscosity measured at each of the above temperatures is below the lower limit, it is difficult to process the film for use as a packaging material, and the desired modulus cannot be achieved.In contrast, if the intrinsic viscosity is above the upper limit, the viscosity becomes high, resulting in low productivity and low yield.
[0111] The polyester resin may have a glass transition temperature (Tg) of 50 to 100°C, specifically 70 to 95°C, for example 80 to 90°C.
[0112] If the glass transition temperature is less than 50° C., the polyester resin cannot have physical properties or thermal stability at room temperature, and there is a limit to the film processing process of the polyester resin for use as a packaging material. In contrast, in order for the glass transition temperature to exceed 100° C., the density of the molecular structure must be high, and in this case, the crystallinity of the polyester resin also increases, resulting in a decrease in transparency.
[0113] (Method of producing polyester resin) In another embodiment of the present invention, there is provided a method for producing a polyester resin, the method comprising the steps of: esterifying a monomer mixture including a diacid component and a diol component; prepolymerizing the esterification reaction product in the presence of a phosphorus-based heat stabilizer and a color complementing agent; and polycondensing the prepolymerized polymer, wherein the diacid component includes a furandicarboxylic acid-based compound, the diol component includes an alkylene glycol-based compound, the phosphorus-based heat stabilizer includes an ester group at a terminal thereof, and the color complementing agent includes a blue dye and a red dye.
[0114] The phosphorus-based heat stabilizer having an ester group at its end minimizes thermal discoloration during the process of manufacturing the polyester resin, and even if discoloration has already occurred, the color complementing agent containing the blue dye and the red dye can correct the color of the polyester resin. In addition, the color complementing agent containing the blue dye and the red dye also acts as a catalyst during the process of manufacturing the polyester resin, improving the reaction rate and shortening the time that the polyester resin is exposed to heat.
[0115] Therefore, the polyester resin of the embodiment described above can be obtained by the manufacturing method of the embodiment.
[0116] Hereinafter, the description overlapping with the above will be omitted, and each step of the manufacturing method will be described in detail.
[0117] <Esterification reaction> First, in the manufacturing method according to the embodiment, a monomer mixture including a diacid component and a diol component is subjected to an esterification reaction, and oligomers having a low degree of polymerization may be formed at this stage.
[0118] Specific components constituting each of the diacid component and the diol component are as described above.
[0119] The monomer mixture in the esterification reaction step may include 100 to 200 moles of the alkylene glycol compound based on 100 moles of the furandicarboxylic acid compound.
[0120] If the alkylene glycol compound is used in an amount of more than 200 moles based on 100 moles of the furan dicarboxylic acid compound, the viscosity increase rate during the polycondensation reaction slows down and the color of the polymer deteriorates. On the other hand, if the alkylene glycol compound is used in an amount of less than 100 moles, the clear point cannot be confirmed and the end point of the esterification reaction cannot be confirmed.
[0121] On the other hand, taking into consideration the amount of material lost or unreacted during the esterification reaction, the amount of the reactants may be used in excess of about 120% of the desired copolymer composition. Therefore, by adjusting the molar ratio of the reactants within the above range, a copolymer in which the content of each residue is controlled within the above range can be formed.
[0122] Specifically, based on 100 moles of the furan dicarboxylic acid compound, the alkylene glycol compound may be included in an amount of 100 moles or more, 110 moles or more, 115 moles or more, or 120 moles or more, and 200 moles or less, 190 moles or less, 180 moles or less, or 150 moles or less.
[0123] The esterification reaction may be carried out in a nitrogen (N2) atmosphere at a temperature range of 180 to 220° C. and a pressure of 1 to 5.5 atm for 1 to 5 hours.
[0124] The esterification reaction conditions can be appropriately adjusted depending on the blending ratio of the raw materials, the specific properties of the desired polyester composition, and the like.
[0125] For example, the esterification reaction may be carried out at a temperature range of 180°C or more, 182°C or more, 184°C or more, or 185°C or more, and 220°C or less, 210°C or less, 200°C or less, or 195°C or less.
[0126] The esterification reaction may be carried out at 1 atm or more and 5.5 atm or less, 5 atm or less, 3 atm or less, or 1.5 atm or less.
[0127] The esterification reaction may be carried out for 1 hour or more, 1.5 hours or more, or 2 hours or more, but not exceeding 5 hours, not exceeding 4 hours, or not exceeding 3 hours.
[0128] If the temperature, pressure, reaction time, etc. of the esterification reaction are below the respective ranges, the reaction yield may be low or the reaction may not occur sufficiently, and the properties of the polyester finally produced may be deteriorated.If the temperature, pressure, reaction time, etc. of the esterification reaction are above the respective ranges, the appearance of the polyester produced may be likely to be yellow, or a depolymerization reaction may occur, and the polyester resin may not be synthesized by the above production method.
[0129] The transesterification reaction may be carried out in a batch or continuous manner, and each raw material may be added separately. For example, the alkylene glycol may be mixed with the furan-based dicarboxylic acid and added in the form of a slurry.
[0130] The esterification reaction may be carried out in the presence of an esterification catalyst including a titanium (Ti)-based compound, a tin (Sn)-based compound, an antimony (Sb)-based compound, etc. In particular, the esterification catalyst can improve the reaction rate from the early stage of the reaction and shorten the time that the polyester resin is exposed to heat.
[0131] The tin (Sn)-based compound may be, for example, dibutyltin oxide.
[0132] The esterification catalyst can be used in an amount of 1 ppm to 100 ppm based on the central atom of the polyester to be synthesized. If the content of the esterification catalyst is too small, the efficiency of the esterification reaction may not be significantly improved, and the amount of reactants that do not participate in the reaction may increase significantly. In addition, if the content of the esterification catalyst is too high, the appearance properties of the polyester to be produced may be deteriorated.
[0133] Meanwhile, the monomer mixture may further include at least one of a diacid component and a diol component in addition to the furan-based dicarboxylic acid and the alkylene glycol.
[0134] When the monomer mixture further includes the diacid component, the polyester resin may include the diacid residue described above. When the monomer mixture further includes the diol component, the polyester resin may include the diol residue described above.
[0135] The diol component includes an aromatic diol and an aliphatic diol.
[0136] The aromatic diol may include an aromatic diol compound having a carbon number of 8 to 40, for example, a carbon number of 8 to 33. Examples of such aromatic diol compounds include polyoxyethylene-(2.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.2)-polyoxyethylene-(2.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxyethylene-(2.3)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(6)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.3)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.4)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(3.3 ... Examples of bisphenol A derivatives to which ethylene oxide and / or propylene oxide have been added include polyoxyethylene-(n)-2,2-bis(4-hydroxyphenyl)propane, polyoxyethylene-(3.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxyethylene-(6)-2,2-bis(4-hydroxyphenyl)propane, etc. include polyoxyethylene-(n)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(n)-polyoxyethylene-(n)-2,2-bis(4-hydroxyphenyl)propane, etc., where n denotes the number of polyoxyethylene or polyoxypropylene units.
[0137] The aliphatic diol may include an aliphatic diol compound having 2 to 20 carbon atoms, for example, 2 to 12 carbon atoms. Examples of such aliphatic diol compounds include linear, branched, or cyclic aliphatic diol components such as ethylene glycol, diethylene glycol, triethylene glycol, propanediol (1,2-propanediol, 1,3-propanediol, etc.), 1,4-butanediol, pentanediol, hexanediol (1,6-hexanediol, etc.), neopentyl glycol (2,2-dimethyl-1,3-propanediol), 1,2-cyclohexanediol, 1,4-cyclohexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, and tetramethylcyclobutanediol.
[0138] The aromatic dicarboxylic acid component may be an aromatic dicarboxylic acid having 8 to 20 carbon atoms, preferably 8 to 14 carbon atoms, or a mixture thereof. Examples of the aromatic dicarboxylic acid may include isophthalic acid, naphthalenedicarboxylic acid such as 2,6-naphthalenedicarboxylic acid, diphenyldicarboxylic acid, 4,4'-stilbene dicarboxylic acid, 2,5-furandicarboxylic acid, and 2,5-thiophenedicarboxylic acid.
[0139] <Preliminary Polymerization> In one embodiment, the method comprises prepolymerizing the esterification reaction product in the presence of a phosphorus-based heat stabilizer having an ester group at a terminal thereof and a color complementing agent having a blue dye and a red dye to produce an oligomer having a higher degree of polymerization than the esterification reaction product.
[0140] Specifically, water is generated during the reaction of the diacid component and the diol component, and the esterification reaction is terminated when the diacid component is completely dissolved and the clear point is reached. If the phosphorus-based heat stabilizer having an ester group at its terminal and the color complementing agent including the blue dye and the red dye are added in the esterification reaction step, the clear point cannot be accurately determined, so in the manufacturing method of the embodiment, the additives are added in the prepolymerization step.
[0141] During the prepolymerization, the heat stabilizer can be used in an amount of 1 to 50 ppm, the blue dye can be used in an amount of 1 to 150 ppm, and the red dye can be used in an amount of 1 to 100 ppm, based on the weight of the esterification reaction product.
[0142] When the heat stabilizer is used in the above range, thermal discoloration during the prepolymerization and polycondensation reactions is minimized, and when the color complementing agent is used in the above range, it not only corrects the discolored resin color during the prepolymerization and polycondensation reactions, but also effectively plays a role as a catalyst for the polycondensation reaction, minimizing heat exposure.
[0143] Moreover, when the above-mentioned ranges are satisfied, it is possible to obtain a polyester resin in which the heat stabilizer and color complementing agent remain within the above-mentioned ranges.
[0144] For example, the phosphorus-based heat stabilizer having an ester group at its terminal can be used in an amount of 1 ppm or more, 5 ppm or more, 10 ppm or more, or 15 ppm or more, and 50 ppm or less, 40 ppm or less, 30 ppm or less, or 25 ppm or less, based on the weight of the esterification reaction product.
[0145] In addition, the blue dye can be used in an amount of 1 ppm or more, 2 ppm or more, 5 ppm or more, or 10 ppm or more and 150 ppm or less, 140 ppm or less, 130 ppm or less, 120 ppm or less, or 100 ppm or less, based on the weight of the esterification reaction product.
[0146] In addition, the red dye can be used in an amount of 1 ppm or more, 10 ppm or more, 20 ppm or more, or 30 ppm or more, and 100 ppm or less, 80 ppm or less, 70 ppm or less, 60 ppm or less, or 50 ppm or less, based on the weight of the esterification reaction product.
[0147] The pre-polymerization can be carried out under temperature controlled conditions (thermal pre-condensation).
[0148] Specifically, the prepolymerization can be performed including: a step of increasing the temperature to a temperature range of 220 to 280° C. or 220 to 260° C.; and a step of maintaining the reached temperature and prepolymerizing the esterification reaction product.
[0149] In addition, after the pressure is reduced until the pressure during the temperature increase reaches 0 to 1 atm or 0 to 0.5 atm, the ultimate pressure can be maintained while the ultimate temperature is maintained.
[0150] The prepolymerization conditions can be appropriately adjusted depending on the blending ratio of the raw materials, the amounts of the heat stabilizer and the color toner used, and the specific properties of the desired polyester composition.
[0151] If the temperature, pressure, reaction time, etc. during the prepolymerization are below the respective ranges, the reaction yield may be low or the reaction may not occur sufficiently, and the properties of the polyester finally produced may be deteriorated.If the temperature, pressure, reaction time, etc. during the prepolymerization are above the respective ranges, the appearance of the polyester produced may be likely to be yellow or a depolymerization reaction may occur, and the polyester resin may not be synthesized by the above production method.
[0152] <Polycondensation reaction> In the above-mentioned production method, after the prepolymerization, the prepolymerized polymer is subjected to a polycondensation reaction.
[0153] The poly-condensation reaction can be carried out at a temperature in the range of 220 to 280° C. or 220 to 260° C. and under a pressure of 1 torr or less, or 0.4 to 0.8 torr or less, for 2 to 6 hours.
[0154] If the temperature, pressure, reaction time, etc. during the polycondensation are below the respective ranges, glycol, which is a by-product of the polycondensation reaction, cannot be effectively removed from the system, and the intrinsic viscosity of the final reaction product is low, resulting in poor physical properties of the polyester produced. On the other hand, if the temperature, pressure, reaction time, etc. during the polycondensation are above the respective ranges, the appearance of the polyester produced may be yellowed or a depolymerization reaction may occur, resulting in no polyester being synthesized.
[0155] In the polycondensation, a polycondensation reaction catalyst can be used.
[0156] The polycondensation catalyst may be added to the product of the esterification reaction before the start of the polycondensation reaction, may be added to a mixture containing the diol component and the dicarboxylic acid component before the esterification reaction, or may be added during the esterification reaction step.
[0157] The polycondensation catalyst may be a titanium-based compound, a germanium-based compound, an antimony-based compound, an aluminum-based compound, a tin-based compound, or a mixture thereof.
[0158] Examples of the titanium-based compound include tetraethyl titanate, acetyl tripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, polybutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, titanium lactate, triethanolamine titanate, acetylacetonate titanate, ethyl acetoacetic ester titanate, isostearyl titanate, titanium dioxide, titanium dioxide / silicon dioxide copolymer, and titanium dioxide / zirconium dioxide copolymer.
[0159] Examples of the germanium-based compound include germanium dioxide (GeO2), germanium tetrachloride (GeCl4), germanium ethyleneglycoxide, germanium acetate, copolymers using these, and mixtures thereof. <Mode for carrying out the invention>
[0160] The present invention will now be described with reference to examples. However, the following examples are merely illustrative of the present invention, and the scope of the present invention is not limited to these examples.
[0161] <Example 1-1> 5.5 mol of 2,5-furandicarboxylic acid (FDCA) and 9.9 mol of ethylene glycol (EG) were added to the hopper of a 2L autoclave reactor. Then, dibutyltin oxide, a type of tin-based catalyst, was added in an amount of 50 ppm based on tin, and the FDCA and EG were esterified at a temperature of 190°C under normal pressure (1 atm) in a nitrogen atmosphere for 2 to 3 hours. This reaction produced oligomers consisting of FDCA-derived residues and EG-derived residues.
[0162] After the esterification reaction was completed, a PC64 catalyst (Tyzor (registered trademark) PC64), which is a type of titanium chelate catalyst, was added as a polycondensation catalyst in an amount of 100 ppm based on tin, and 20 ppm of triethyl phosphonoacetate (TEPA) was added as a thermal stabilizer. After adding the polycondensation catalyst and the thermal stabilizer, the mixture was stirred for 30 minutes, and 100 ppm of Solvent Blue 45 dye as a blue dye and 30 ppm of Solvent Red 135 as a red dye were added. The mixture was further stirred for 15 minutes, and the temperature in the reactor was raised for 1 hour to reach a temperature range of 220 to 240°C, and then the pressure was gradually reduced for 1 hour using a vacuum pump until the pressure inside the reactor reached 1 atm to 0 atm, thereby performing prepolymerization.
[0163] Thereafter, the reaction was carried out for 2 to 6 hours at a temperature range of 220 to 240°C under high vacuum of 0.8 torr or less, and when the load transmitted to the torque meter of the autoclave reached a desired load, the autoclave was drained to obtain a polyester resin of Example 1-1.
[0164] <Examples 1-2, 1-3 and 1-5> Polyester resins of Examples 1-2, 1-3 and 1-5 were produced in the same manner as in Example 1-1, except that the amount of Solvent Blue 45 added was changed according to Table 1 below.
[0165] <Examples 1-4 and 1-6> The polyester resins of Examples 1-4 and 1-6 were prepared in the same manner as in Example 1-1, except that the amounts of Solvent Blue 45 and Solvent Red 135 were changed. Here, the amounts of Solvent Blue 45 and Solvent Red 135 are shown in Table 1 below.
[0166] <Example 2-1> 5.5 mol of 2,5-furandicarboxylic acid (FDCA) and 9.9 mol of ethylene glycol (EG) were added to the hopper of a 2L autoclave reactor. Then, dibutyltin oxide, a type of tin-based catalyst, was added in an amount of 50 ppm based on tin, and the FDCA and EG were esterified at a temperature of 190°C under normal pressure (1 atm) in a nitrogen atmosphere for 2 to 3 hours. This reaction produced oligomers consisting of FDCA-derived residues and EG-derived residues.
[0167] After the esterification reaction was completed, a PC64 catalyst (Tyzor (registered trademark) PC64), which is a type of titanium chelate catalyst, was added as a polycondensation catalyst in an amount of 100 ppm based on tin, and 20 ppm of triethyl phosphonoacetate (TEPA) was added as a thermal stabilizer. After adding the polycondensation catalyst and the thermal stabilizer, the mixture was stirred for 30 minutes, and 100 ppm of Global PRT Blue dye and 30 ppm of Global PRT Red dye were added. After stirring for another 15 minutes, the temperature inside the reactor was raised for 1 hour to reach a temperature range of 220 to 240°C, and the pressure was gradually reduced using a vacuum pump for 1 hour until the pressure inside the reactor reached 1 atm to 0 atm, thereby performing prepolymerization.
[0168] Thereafter, the reaction was carried out for 2 to 6 hours at a temperature range of 220 to 240°C under high vacuum of 0.8 torr or less, and when the load transmitted to the torque meter of the autoclave reached a desired load, the autoclave was drained to obtain the polyester resin of Example 2-1.
[0169] <Examples 2-2, 2-3 and 2-5> The polyester resins of Examples 2-2, 2-3 and 2-5 were produced in the same manner as in Example 2-1, except that the amount of Global PRT Blue added was changed, where the content of Global PRT Blue was as shown in Table 1 below.
[0170] <Examples 2-4 and 2-6> The polyester resins of Examples 2-4 and 2-6 were produced in the same manner as in Example 1-1, except that the amounts of Global PRT Blue and Global PRT Red were changed, as shown in Table 1 below.
[0171] <Comparative Example 1-1> A polyester resin of Comparative Example 1-1 was prepared in the same manner as in Example 1-1, except that the heat stabilizer, the blue dye and the red dye were not added.
[0172] <Comparative Example 2-1> The blue and red dyes were not added, and triphenyl phosphate (TPP) was added as a heat stabilizer instead of triethyl phosphonoacetate (TEPA). The amount of triphenyl phosphate added is shown in Table 1 below.
[0173] Except for this, a polyester resin of Comparative Example 2-1 was produced in the same manner as in Example 1-1.
[0174] <Comparative Example 2-2> The blue and red dyes were not added, and phosphoric acid (PA) was added instead of triethyl phosphonoacetate (TEPA) as a thermal stabilizer. The amount of phosphoric acid added is shown in Table 1 below.
[0175] Except for this, a polyester resin of Comparative Example 2-2 was produced in the same manner as in Example 1-1.
[0176] <Comparative Example 2-3> The blue dye and the red dye were not added, and triethyl phosphonoacetate (TEPA) was added as a heat stabilizer. The amount of triethyl phosphonoacetate added is shown in Table 1 below.
[0177] Except for this, a polyester resin of Comparative Example 2-3 was produced in the same manner as in Example 1-1.
[0178] <Comparative Example 3-1> No heat stabilizer or red dye was added, but instead, a blue dye, Solvent Blue 45, was added. The amount of Solvent Blue 45 added is shown in Table 1 below.
[0179] Except for this, a polyester resin of Comparative Example 3-1 was produced in the same manner as in Example 1-1.
[0180] <Comparative Example 3-2> No heat stabilizer or red dye was added, but the blue dye Global PRT Blue was added. The amount of Global PRT Blue added is shown in Table 1 below.
[0181] Except for this, a polyester resin of Comparative Example 3-2 was produced in the same manner as in Example 1-1.
[0182] <Comparative Example 3-3> No heat stabilizer or blue dye was added, but a red dye, Solvent Red 135, was added. The amount of Solvent Red 135 added is shown in Table 1 below.
[0183] Except for this, a polyester resin of Comparative Example 3-3 was produced in the same manner as in Example 1-1.
[0184] <Comparative Example 3-4> No heat stabilizer or blue dye was added, but the red dye Global PRT Red was added. The amount of Global PRT Red added is shown in Table 1 below.
[0185] Except for this, a polyester resin of Comparative Example 3-4 was produced in the same manner as in Example 1-1.
[0186] <Comparative Example 4-1> No heat stabilizer was added, but a blue dye, Solvent Blue 45, and a red dye, Solvent Red 135, were added. The amounts of Solvent Blue 45 and Solvent Red 135 added are shown in Table 1 below.
[0187] Except for this, a polyester resin of Comparative Example 4-1 was produced in the same manner as in Example 1-1.
[0188] <Comparative Example 4-2> No heat stabilizer was added, but the blue dye Global PRT Blue and the red dye Global PRT Red were added. The amounts of Global PRT Blue and Global PRT Red added are shown in Table 1 below.
[0189] Except for this, a polyester resin of Comparative Example 4-2 was produced in the same manner as in Example 1-1.
[0190] [Table 1]
[0191] <Test Example 1: Copolymer Residue Composition> For each polyester resin sample of the Examples and Comparative Examples, the copolymer residue composition, and the number average molecular weight (Mn) and molecular weight distribution (MWD) of the polyester resin containing the same were evaluated by the following methods, and the evaluation results are shown in Table 2 below.
[0192] (1) Copolymer Residue Composition: The copolymer residue composition (mol%) contained in the polyester resin sample was confirmed by dissolving the sample in CDCl3 solvent at a concentration of 3 mg / mL and then measuring the 1H-NMR spectrum obtained at 25°C using a nuclear magnetic resonance apparatus (JEOL, 600 MHz FT-NMR).
[0193] (2) Number average molecular weight (Mn) and molecular weight distribution (MWD) of polyester resin: Gel permeation chromatography (GPC) was used to measure Mw and Mn, and the molecular weight distribution ("Mw / Mn") was calculated.
[0194] Specifically, the analysis was performed using a TSKgel guardcolumn SuperAW-H + 2 × TSKgel SuperAWM-H (6.0 × 150 mm) column and a Tosoh HLC-8420 GPC apparatus. The evaluation temperature was 40 °C, HFIP + 0.01 N NaTFA was used as the developing solvent, and the flow rate was 0.3 mL / min.
[0195] Samples, including polyester resin samples, were prepared to a concentration of 3 mg / 10 mL and then delivered in 10 μL volumes. Calibration curves generated using PMMA standards were used to derive Mw and Mn values and determine the molecular weight distribution ("Mw / Mn").
[0196] [Table 2] JPEG2024544394000012.jpg25170
[0197] From Table 2 above, it can be seen that the final copolymer residue composition and the weight properties of the polyester resin containing the same are the same in all the examples and comparative examples. This is because the raw material blend for producing the copolymer is the same in all the examples and comparative examples. Meanwhile, it can be seen that the molecular weight distribution is low, at 2 or less, when a phosphorus-based heat stabilizer is used in all the examples and comparative examples, and particularly when triethyl phosphonoacetate is used (Comparative Examples 2-3 and 2-4, Examples 1-1 to 1-5, and Examples 2-1 to 2-6).
[0198] <Test Example 2: Residual Amount of Additives in Polyester Resin> For each of the polyester resin samples of the Examples and Comparative Examples, the amount of remaining additives was evaluated by the following method, and the evaluation results are shown in Table 3 below.
[0199] 1g of polyester sample was frozen under liquid nitrogen for 10 minutes. The sample was pulverized using a grinder, and then 100ml of n-hexane was added per 1g of sample, and Soxhlet extraction was performed for 6 hours. The sample was concentrated or diluted to a final volume of 50-250ml, and 10-50μg of an internal standard (Fluoranthene-d10) was added, followed by GC / MS analysis. The relative content of the heat stabilizer, blue dye, and red dye relative to the internal standard was calculated to confirm the remaining amount in the sample.
[0200] [Table 3] JPEG2024544394000014.jpg25170
[0201] From Table 3 above, it can be seen that most of the heat stabilizer and color complement remained in all examples and comparative examples. The decrease in the remaining amount relative to the input amount is presumed to be due to loss during the reaction.
[0202] <Test Example 3: Color properties of polyester resin> For each of the polyester resin samples of the Examples and Comparative Examples, the color characteristics were evaluated by the following method, and the evaluation results are shown in Table 4 below.
[0203] Using a Konica Minolta CM-3700A color difference meter, the L*, a*, and b* values were measured under the following conditions. Specifically, 2 g of a polyester resin sample was dissolved in 20 ml of hexafluoroisopropanol (HFIP) (0.1 g / ml in HFIP). The color difference of the sample solution was measured using a quartz cell dedicated to solution color difference meter measurements using the Konica Minolta CM-3700A product.
[0204] [Table 4]
[0205] According to Table 4 above, when triethyl phosphonoacetate is used as the phosphorus-based heat stabilizer and red and blue dyes are used as complementary colorants (Examples 1-1 to 1-6 and Examples 2-1 to 2-6), the L* value of the final polyester resin according to the CIE1976 L*a*b* color system is 92 to 97, the a* value is 2 or less, and the b* value is 3 or less. Meanwhile, it can be seen that the color properties of the final polyester resin can be adjusted according to the type and amount of each of the red and blue dyes, while using triethyl phosphonoacetate as the phosphorus-based heat stabilizer and red and blue dyes as complementary colorants.
[0206] <Test Example 4: Physical properties of polyester resin> For each of the polyester resin samples of Example 1 and Comparative Example, the intrinsic viscosity and glass transition temperature were evaluated by the following methods, and the evaluation results are shown in Table 5 below.
[0207] 1) Intrinsic viscosity (IV): 0.5 g of a polyester resin sample was dissolved in 10 ml of a 1:1 solution of phenol:tetrachloroethane, and the IV was measured at 25°C and 35°C using an Ostwald viscometer.
[0208] 2) Glass transition temperature (Tg): The glass transition temperature of the polyester resin sample was measured using a DSC manufactured by TA Instruments under the conditions of N2, 20 psi, and room temperature to 300°C at 20°C / min.
[0209] [Table 5] JPEG2024544394000017.jpg36170
[0210] According to Table 5 above, when a red dye was used as a color complement (Comparative Examples 3-3 and 3-4, Comparative Examples 4-1 and 4-2, Examples 1-1 to 1-6, and Examples 2-1 to 2-6), the intrinsic viscosity (IV1) at 25°C, the intrinsic viscosity (IV2) at 35°C, and the change in intrinsic viscosity (IV1-IV2) of the final polyester resin were significantly decreased, and the glass transition temperature was significantly increased. On the other hand, it can be seen that even when a red dye is used, the intrinsic viscosity and glass transition temperature of the final polyester resin can be adjusted depending on the type, amount, etc. of the red dye.
[0211] <Test Example 5: Physical properties of film containing polyester resin> For each of the polyester resin samples of Example 1 and Comparative Example, the physical properties after film production were evaluated by the following methods, and the evaluation results are shown in Table 6 below.
[0212] 1) Transmittance First, a biaxially stretched film of a polyester resin sample was produced. Specifically, the polyester resin sample was melted at a temperature of 180 to 260° C. in an extruder.
[0213] The melt was extruded through a die to form a sheet and then quenched. The sheet thus obtained was stretched 3.0 times in the machine direction (MD) and then 3.7 times in the transverse direction (TD). In order to impart dimensional stability to the stretched film, the film was heat-set at 120 to 160°C under tension to obtain a biaxially stretched film.
[0214] The polyester film thus produced was cut into a size of 10 cm x 10 cm (longitudinal length x horizontal length) to prepare a test piece. The parallel transmittance and diffuse transmittance of the test piece were measured by the ASTM D1003-97 measurement method using a Minolta CM-3600A measuring device. The transmittance is defined as the combined value of the parallel transmittance and diffuse transmittance. Therefore, the transmittance was calculated from the parallel transmittance and diffuse transmittance of the test piece.
[0215] 2) Tensile strength, elongation and elastic modulus The polyester resin sample was extruded at 220~260℃ using a Microcompounder extruder at a screw speed of 100~120rpm to produce ASTM D638-V Type test specimens. The produced mechanical property test specimens were mounted using a vice grip under a universal testing machine UTM 5566A (Instron). The sample was stretched at a speed of 5mm / min at room temperature until it broke. The strength at the point where the sample broke was taken as the tensile strength, the length stretched was taken as the elongation, and the slope of the load against the initial deformation was taken as the tensile modulus.
[0216] [Table 6]
[0217] According to Table 6 above, when a color complementing agent is used (Comparative Examples 2-1 to 2-4, Comparative Examples 3-1 to 3-4, Comparative Examples 4-1 and 4-2, Examples 1-1 to 1-6, and Examples 2-1 to 2-6), the transmittance, tensile strength, elongation, and elastic modulus of the film are at roughly similar levels.
Claims
1. Copolymers containing diacid and diol residues; Phosphorus-based heat stabilizers; and Contains color complementing agents, the diacid residue comprises a residue derived from a furandicarboxylic acid compound, The diol residue includes a residue derived from an alkylene glycol compound, The phosphorus-based heat stabilizer contains an ester group at a terminal thereof, The color complementing agent comprises a blue dye and a red dye.
2. The phosphorus-based heat stabilizer having an ester group at its terminal is represented by the following chemical formula 1: [Chemical formula 1] In the above Chemical Formula 1, R 1 are the same or different and are substituted or unsubstituted alkyl having 1 to 10 carbon atoms; R 2 is a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms.
3. The polyester resin according to claim 2, wherein the phosphorus-based heat stabilizer having an ester group at its terminal is trimethyl phosphonoacetate, triethyl phosphonoacetate, or a combination thereof.
4. The polyester resin is 1 g of the polyester resin is frozen under liquid nitrogen for 10 minutes, pulverized, and subjected to Soxhlet extraction for 6 hours by adding 100 ml of n-hexane per 1 g of the pulverized polyester resin, and then concentrated or diluted to a final volume of 50 to 250 ml. 10 to 50 μg of fluoranthene-d10 is added as an internal standard substance, and then GC / MS analysis is performed to confirm the remaining amount of the heat stabilizer having an ester group at its end in the polyester resin by calculating the relative ratio to the internal standard substance.
4. The polyester resin according to claim 3, further comprising 1 to 50 ppm of the heat stabilizer having an ester group at its terminal, based on the weight of the copolymer.
5. 2. The polyester resin of claim 1, wherein the blue dye is an anthraquinone-based blue dye, a phthalocyanine-based blue dye, or a combination thereof.
6. The polyester resin is 1 g of the polyester resin is frozen under liquid nitrogen for 10 minutes, pulverized, and 100 ml of n-hexane is added per 1 g of the pulverized polyester resin, followed by Soxhlet extraction for 6 hours. The resulting mixture is concentrated or diluted to a final volume of 50 to 250 ml, and 10 to 50 μg of fluoranthene-d10 is added as an internal standard. The remaining amount of the blue dye in the polyester resin is then confirmed by calculating the relative ratio to the internal standard.
6. The polyester resin of claim 5, comprising 1 to 150 ppm of said blue dye, based on the weight of said copolymer.
7. 2. The polyester resin of claim 1, wherein the red dye is a perinone red dye, an azo red dye, or a combination thereof.
8. The polyester resin is 1 g of the polyester resin is frozen under liquid nitrogen for 10 minutes, pulverized, and 100 ml of n-hexane is added per 1 g of the pulverized polyester resin, followed by Soxhlet extraction for 6 hours to concentrate or dilute to a final volume of 50 to 250 ml. 10 to 50 μg of fluoranthene-d10 is added as an internal standard, and then GC / MS analysis is performed to confirm the remaining amount of the red dye in the polyester resin by calculating the relative ratio to the internal standard.
8. The polyester resin according to claim 7, comprising 1 to 100 ppm of said red dye based on the weight of said copolymer.
9. The color complementing agent is 2. The polyester resin of claim 1, comprising said blue dye and said red dye in a weight ratio (blue:red) of 1:9 to 9:
1.
10. The polyester resin according to claim 1, wherein the polyester resin has a number average molecular weight of 20,000 to 30,000 g / mol.
11. The polyester resin according to claim 1 , wherein the polyester resin has a molecular weight distribution of 2.5 or less (but greater than 0).
12. The polyester resin is The polyester resin according to claim 1, wherein, when 2 g of the polyester resin is dissolved in 20 ml of hexafluoroisopropanol (HFIP) solvent having a concentration of 0.1 g / ml and then measured using a solution colorimeter according to the CIE 1976 L*a*b* color system, the L* value is 92 to 97, the a* value is 2 or less, and the b* value is 3 or less.
13. The polyester resin is The change in intrinsic viscosity (ΔIV) according to the following formula 1 12 2. The polyester resin of claim 1, wherein the molecular weight of the polyester resin is 0.4 (but greater than 0) dl / g. [Formula 1] △IV 12 = IV 1 -IV 2 In the above formula 1, IV 1 is the intrinsic viscosity at 25°C, and IV 2 is the intrinsic viscosity at 35°C.
14. The polyester resin according to claim 1, wherein the polyester resin has a glass transition temperature (Tg) of 50 to 100°C.
15. subjecting a monomer mixture comprising a diacid component and a diol component to an esterification reaction; prepolymerizing the esterification reaction product in the presence of a phosphorus-based thermal stabilizer and a color-stimulating agent; and The prepolymerized polymer is subjected to a polycondensation reaction, the diacid component comprises a furandicarboxylic acid compound, The diol component includes an alkylene glycol compound, The phosphorus-based heat stabilizer contains an ester group at a terminal thereof, The method for producing a polyester resin, wherein the color complementing agent comprises a blue dye and a red dye.
16. The method for producing a polyester resin according to claim 15, wherein the monomer mixture contains 100 to 200 moles of the alkylene glycol compound based on 100 moles of the furan dicarboxylic acid compound.
17. The method for producing a polyester resin according to claim 15, wherein the esterification reaction is carried out at a temperature range of 180 to 220°C.
18. The esterification reaction is carried out using nitrogen (N 2 The method for producing a polyester resin according to claim 15, wherein the method is carried out under an atmosphere of
19. The method for producing a polyester resin according to claim 15, wherein the esterification reaction is carried out under a pressure of 1 to 5.5 atm.
20. During the prepolymerization, 16. The method for producing a polyester resin according to claim 15, wherein the phosphorus-based heat stabilizer having an ester group at its terminal is used in an amount of 1 to 50 ppm, the blue dye is used in an amount of 1 to 150 ppm, and the red dye is used in an amount of 1 to 100 ppm, based on the weight of the esterification reaction product.
21. The prepolymerization is increasing the temperature until a temperature range of 220-280° C. is reached; and The method for producing a polyester resin according to claim 15, further comprising a step of maintaining the reached temperature and prepolymerizing the esterification reaction product.
22. The pressure during the temperature increase is reduced until it reaches 0 to 1 atm; The method for producing a polyester resin according to claim 21, wherein the ultimate pressure is also maintained while the ultimate temperature is maintained.
23. The method for producing a polyester resin according to claim 15, wherein the polycondensation reaction is carried out at a temperature range of 220 to 280°C.
24. The method for producing a polyester resin according to claim 15, wherein the polycondensation reaction is carried out for 2 to 8 hours.