Highly heat-resistant and chemically-resistant polyimide powder using glass fiber powder and its manufacturing method
By polymerizing dianhydride and diamine monomers with glass fiber powder in a mixed solvent, the polyimide powder achieves high heat resistance and chemical stability, addressing the limitations of conventional polyimides in insulation and processing.
Patent Information
- Application Number
- JP2024534378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-08
- Filing Date
- 2022-12-07
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2042-12-07
AI Technical Summary
Conventional polyimide powders face challenges in maintaining insulation properties and stability at high temperatures of 800°C, and when using ceramic or metal materials, they become difficult to process or exhibit low insulation properties.
A method involving the polymerization of dianhydride and diamine monomers with glass fiber powder in a mixed organic solvent, followed by heat treatment, to produce a polyimide powder that maintains insulation and chemical resistance at high temperatures, using a mixed solvent of aprotic and protic solvents to enhance moldability and processability.
The resulting polyimide powder exhibits high heat resistance up to 800°C, maintains insulation properties, and demonstrates excellent chemical resistance to acids and bases, with improved moldability and processability.
Smart Images

Figure 2024545151000001 
Figure 2024545151000002 
Figure 2024545151000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a highly heat-resistant and chemically resistant polyimide powder utilizing glass fiber powder and a method for producing the same. [Background technology]
[0002] Generally, polyimide (PI) is a polymer of imide monomer formed by solution polymerization of dianhydride and diamine or diisocyanate, and has excellent mechanical properties such as strength, chemical resistance, weather resistance, and heat resistance based on the chemical stability of the imide ring. In addition, polyimide is in the spotlight as a high-performance polymer material that can be applied to a wide range of industrial fields such as electronics, communications, and optics due to its excellent electrical properties such as insulation properties and low dielectric constant.
[0003] On the other hand, although conventional polyimides have excellent insulating properties and heat resistance as described above, there is a problem that their stability decreases at high temperatures of about 800° C. When ceramic materials among inorganic materials are used to improve the high temperature stability of such conventional polyimide powders, there is a problem that processing is difficult, and when used with metal materials among inorganic materials, there is a problem that it is difficult to use them as insulating materials due to their low insulating properties.
[0004] Therefore, research is being conducted into a method for producing a highly heat-resistant polyimide powder that can maintain insulation properties and ensure stability at high temperatures of up to 800° C. Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to solve the problems and technical issues of the prior art as described above.
[0006] The present invention provides a highly heat-resistant polyimide powder that can maintain insulation properties and ensure stability at high temperatures of around 800° C., and a method for producing the same.
[0007] The present invention also provides a chemically resistant polyimide powder that can ensure stability against acids and / or bases, and a method for producing the same. [Means for solving the problem]
[0008] The present invention relates to a polyimide powder and a method for producing the same.
[0009] The polyimide powder according to the present invention has a dianhydride monomer component and a diamine monomer component as polymerized units.
[0010] As mentioned above, conventional polyimides have excellent insulating properties and heat resistance, but have problems in that their stability or chemical resistance decreases at high temperatures of around 800° C. When ceramic materials, among inorganic materials, are used to ensure the high-temperature stability of such conventional polyimide powders, there is a problem that processing is difficult, and when used with metal materials, among inorganic materials, there is a problem that it is difficult to use as an insulating material due to its low insulating properties.
[0011] The present invention provides a chemical-resistant polyimide powder having high heat resistance, acid and alkali resistance, and the ability to maintain insulation and ensure stability at high temperatures of up to 800°C by polymerizing a dianhydride monomer component, a diamine monomer component and a glass fiber powder.
[0012] A method for preparing a polyimide powder according to an embodiment of the present invention includes the steps of: solution-polymerizing a dianhydride monomer and a diamine monomer in an organic solvent containing glass fibers to prepare a polyamic acid solution; heating the polyamic acid solution to prepare a polyimide mixture; and filtering and drying a precipitate present in the mixture to obtain a polyimide powder.
[0013] In the past, polyimide powders were produced by dispersing a dianhydride monomer and a diamine monomer in an aqueous solvent to produce a dispersion, and then heat-treating the dispersion. However, when a dispersion was produced by further adding glass fiber powder to an aqueous solvent as in the past, there was a problem that the glass fiber powder aggregated in the dispersion, decreasing dispersibility.
[0014] In the method for producing a polyimide powder according to an embodiment of the present invention, a dianhydride monomer, a diamine monomer, and glass fibers are dispersed in a mixed organic solvent to form a polymerization solution (varnish), which is then heat-treated to produce a polyimide powder, so that the dispersibility of the glass fibers can be good.
[0015] In one embodiment, the glass fiber is not particularly limited in shape, but may be in the form of chopped strands or a powder obtained by pulverizing the chopped strands. In particular, taking into consideration dispersibility, the diameter may be 5 μm or more, 7 μm or more, or 9 μm or more, and the powder may be 18 μm or less, 15 μm or less, or 12 μm or less.
[0016] The type of glass fiber is not particularly limited, but glass fiber having a high acid resistance, base resistance, and electrical resistance can be used.
[0017] The content of the glass fiber in the organic solvent may be, for example, 5 to 90 parts by weight, 6 to 70 parts by weight, 7 to 60 parts by weight, 8 to 55 parts by weight, or 10 to 50 parts by weight, based on 100 parts by weight of the dianhydride monomer and the diamine monomer in total. If the content of the glass fiber is too low, it is difficult to ensure stability or chemical resistance at a high temperature of 800° C., and if the content is too high, mechanical properties such as tensile strength and elongation may decrease.
[0018] The organic solvent of the present invention may be a mixed solvent of an aprotic solvent and a protic solvent. The mixed solvent has the advantage of being superior in moldability and processability compared to the case where an aprotic solvent or a protic solvent is used alone.
[0019] Without being bound by theory, it is believed that in the case of aprotic solvents, it acts as a kind of imidization catalyst, and in the case of protic solvents, it acts to grow the molecular weight.
[0020] The aprotic solvent is not particularly limited, and may be one or more selected from the group consisting of toluene, xylene, naphtha, anisole, cresol, ethylbenzene, propylbenzene, chlorobenzene, dichlorobenzene, trichlorobenzene, biphenyl, terphenyl, diphenyl ether, diphenyl sulfide, acetophenone, chlorinated biphenyl, and chlorinated diphenyl ether. The protic solvent is not particularly limited, and may be one or more selected from the group consisting of N-methyl-pyrrolidone (NMP), N,N'-dimethylformamide (DMF), N,N'-diethylformamide (DEF), N,N'-dimethylacetamide (DMAc), dimethylpropanamide (DMPA), N,N-diethylacetamide (DEAc), 3-methoxy-N,N-dimethylpropanamide (KJCMPA), and gamma-butyrolactone (GBL).
[0021] The mixed solvent may contain 10-90wt% aprotic solvent and 10-90wt% protic solvent, for example, 20-80wt% aprotic solvent and 20-80wt% protic solvent. If the content of the aprotic solvent is too low, imidization is not sufficiently performed in the heating process, so moldability is not ensured and the intrinsic viscosity (IV) is low, while if the content is too high, the molecular weight of the polymerization liquid is formed too slowly (the chain is too small), so that moldability is not ensured when molding the molded product.
[0022] The step of preparing the polyamic acid solution may be carried out at 50 to 100°C, for example, 60 to 90°C, 65 to 85°C, or 70 to 80°C, and the step of preparing the polyimide mixture may be carried out at 160 to 200°C, for example, 170 to 190°C, or 175 to 185°C.
[0023] If the heating temperature is lower than the above range, mechanical properties such as elongation and tensile strength may decrease, and breakage may occur during molding, resulting in a decrease in yield and processability. Also, if the heating temperature is higher than the above range, the color of the powder may become dark and the particle size may increase.
[0024] The step of preparing the polyamic acid solution and / or the step of preparing the polyimide mixed solution may be carried out under pressurized conditions, for example, at 1 to 10 bar. In particular, in one embodiment of the present invention, the dianhydride monomer, the diamine monomer, and the glass fiber powder are dispersed in a mixed solvent and polymerized, so that the polymerization reaction may be carried out under normal pressure or a pressurized condition of 1 to 3 bar. Pressurization may be achieved by injecting an inert gas into the reactor or by using water vapor generated in the reactor. The inert gas may be nitrogen, argon, helium, neon, or the like.
[0025] If the pressure conditions are lower than the above range, mechanical properties such as elongation and tensile strength may decrease, and breakage may occur during molding, resulting in a decrease in yield and processability.If the pressure conditions are higher than the above range, the color of the powder may become dark and the particle size may increase.
[0026] The reaction time in the step of preparing the polyamic acid solution and / or the step of preparing the polyimide mixture may be 1 to 20 hours, for example, 1 to 10 hours, 1 to 8 hours, 1 to 6 hours, or 1 to 4 hours.
[0027] If the reaction time is shorter than the above range, the reaction yield may decrease, mechanical properties such as elongation and tensile strength may decrease, and breakage may occur during molding, resulting in a decrease in yield and processability. Also, if the reaction time is longer than the above range, the color of the powder may become dark and the particle size may increase.
[0028] The step of obtaining the polyimide powder includes filtering and drying a precipitate present in the mixture to obtain the polyimide powder.
[0029] The method of filtering and drying is not particularly limited, and may be, for example, vacuum drying or oven drying.
[0030] The dianhydride monomer is not particularly limited as long as it can react with the diamine monomer to form a polyimide. For example, the dianhydride monomer according to the present invention may include at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA) and p-phenylenebis(trimellitate anhydride) (TAHQ).
[0031] The diamine monomer is not particularly limited as long as it can react with the dianhydride monomer to form a polyimide. For example, the diamine monomer according to the present invention may include at least one selected from the group consisting of 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenyl ether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine (M-TOLIDINE), 2,2-bis(trifluoromethyl)benzidine (TFDB), 1,4-bisaminophenoxybenzene (TPE-Q), bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).
[0032] In this case, the molar ratio (b / a) indicating the number of moles (b) of the diamine monomer component to the number of moles (a) of the dianhydride monomer component is not more than 1. For example, the upper limit of the molar ratio (b / a) of the diamine monomer component to the dianhydride monomer component may be 0.99 or less, 0.98 or less, 0.97 or less, 0.96 or less, or 0.95 or less, and the lower limit of the molar ratio may be 0.9 or more, 0.91 or more, 0.92 or more, 0.93 or more, or 0.94 or more, and specifically, the molar ratio of the diamine monomer component to the dianhydride monomer component may be 0.9 to 0.99, 0.93 to 0.99, 0.94 to 0.99, 0.95 to 0.99, 0.95 to 0.98, or 0.96 to 0.98.
[0033] For example, in the present invention, the number of moles of the diamine monomer component is smaller than the number of moles of the dianhydride monomer component. Although polyimide can be produced by stoichiometrically reacting the dianhydride monomer and the diamine monomer in a 1:1 ratio, the reaction proceeds mainly in the presence of a solvent and / or a catalyst. In this case, since a side reaction between the functional group of the solvent or catalyst and the diamine may occur, the diamine is generally added in an excess amount or the dianhydride and the diamine are added in equal molar amounts.
[0034] The solid content in the mixed solvent may be 1 to 30 wt %. The solid content may refer to a dianhydride monomer component and a diamine monomer component. For example, the solid content in the mixed solvent may be 1 to 20% or 10 to 20%. By having the above solid content, the intrinsic viscosity of the polyimide powder can be adjusted to have suitable processability.
[0035] In particular, in the method for producing polyimide powder according to one embodiment of the present invention, a dianhydride monomer component, a diamine monomer component, and a glass fiber powder are dispersed in a mixed solvent to form a polymerization solution (varnish), which is then heat-treated to produce polyimide powder. Since the intrinsic viscosity of the polyimide powder is higher (>0.9 dL / g) than that of conventional aqueous polymerization methods, the polyimide powder has excellent moldability and processability.
[0036] A polyimide powder according to another embodiment of the present invention includes a polyimide metric having polymerized units derived from a dianhydride monomer and a diamine monomer, and glass fibers dispersed within the polyimide metric, and satisfies one or more of the following conditions:
[0037] a) After being left at 800°C for 25 hours, the weight loss rate measured is 35% or less, and the surface resistance is 10 14 Ω / cm 2 More than; b) A weight loss of 2.6% or less, measured after immersion for 168 hours in an acidic aqueous solution having a pH of 5 or less; or c) The weight loss measured after immersion for 168 hours in an alkaline aqueous solution having a pH of 9 or more is 15% or less.
[0038] The glass fiber powder may be contained in an amount of 0.01 to 90 parts by weight, preferably 0.1 to 50 parts by weight, based on 100 parts by weight of the polyimide powder. The glass fiber powder may be contained during polymerization of the polyimide powder, or may be additionally mixed into the polyimide powder.
[0039] The polyimide powder may have a weight loss rate of 35% or less, for example, 34% or less, 33% or less, 10% to 35%, 15% to 34%, or 18% to 32%, measured after standing at 800° C. for 25 hours. If the weight loss rate is 35% or more, the high-temperature heat resistance may be insufficient.
[0040] The polyimide powder has a surface resistivity of 10 14 Ω / cm 2 For example, the polyimide powder according to the present invention may have a surface resistance as measured by ASTM D257 of 10 14 Ω / cm 2 or more, and the upper limit of the surface resistance is 10 15 Ω / cm 2 The surface resistance may be 10 14 Ω / cm 2 If it is less than this, the insulating properties may be insufficient.
[0041] The polyimide powder may have a weight loss rate of 2.6% or less, for example, 2.5% or less, 0.5 to 2.6%, or 1 to 2.5%, measured after immersion for 168 hours in an acidic aqueous solution having a pH of 5 or less. The acidic aqueous solution having a pH of 5 or less is not particularly limited, but for example, a 45 to 55 wt % hydrofluoric acid aqueous solution can be used. The measurement temperature or pressure is not particularly limited, but the measurement can be performed at room temperature or normal pressure.
[0042] The polyimide powder may have a weight loss rate of 15% or less, for example, 13% or less, 1 to 11%, or 2 to 10%, measured after immersion for 168 hours in an alkaline aqueous solution having a pH of 9 or more. The alkaline aqueous solution having a pH of 9 or more is not particularly limited, but for example, a 20 to 30 wt% ammonia aqueous solution can be used. The measurement temperature or pressure is not particularly limited, but the measurement can be performed at room temperature or normal pressure.
[0043] The dianhydride monomer of the polyimide powder may include at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA), and p-phenylenebis(trimellitate anhydride) (TAHQ).
[0044] The diamine monomer of the polyimide powder may include at least one selected from the group consisting of 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenylether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine (M-TOLIDINE), 2,2-bis(trifluoromethyl)benzidine (TFDB), 1,4-bisaminophenoxybenzene (TPE-Q), bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).
[0045] The present invention also provides a method for producing a polyimide molded product, comprising the step of compressing and molding the polyimide powder described above.
[0046] The pressure molding step may be performed at a pressure of 30 to 1000 MPa, and the pressure molding step may be performed at 200 to 500°C. The pressure molding step may further include a step of sintering the polyimide powder, which is pressure molded at room temperature, at 200 to 500°C. If the pressure is lower than the above range, the moldability of the powder during molding may be insufficient, and if it is higher, the processability of the molded product may be reduced. If the temperature is lower than the above range, the moldability may be significantly reduced since the molecular fluidity is not ensured, and if it is higher, some parts may be oxidized due to overheating.
[0047] The present invention also provides a molded article produced using the polyimide powder. The polyimide powder produced according to the present invention can be molded into a molded article by various molding methods, for example, compression molding, injection molding, slush molding, blow molding, extrusion molding, or spinning methods. The form of the molded article is not limited, and may be a film, sheet, pellet, tube, belt, injection molded article, or extrusion molded article.
[0048] The polyimide powder prepared according to the present invention can be used in a variety of fields, including electrical / electronic, semiconductor, display, automotive, medical, battery and aerospace applications. Effect of the Invention
[0049] According to the present application, it is possible to produce a highly heat-resistant polyimide powder that can maintain insulation properties and ensure stability at high temperatures of up to 800°C.
[0050] The polyimide powder of the present application has a surface resistance of 10 14 Ω / cm 2 Since the insulating property can be maintained, the insulating property can be increased to the above level.
[0051] Furthermore, the polyimide powder of the present application contains glass fiber powder as a filler, and unlike other fillers, it is able to maintain insulation properties and ensure stability at high temperatures of around 800°C.
[0052] In addition, the polyimide powder according to the present application has a mass change rate of 1.0% to 2.6% when measured when immersed in a hydrofluoric acid solution, and a mass change rate of 2.0% to 10.0% when measured when immersed in ammonia water, and thus has superior chemical resistance compared to conventional polyimide powders.
[0053] However, the effects of the present invention are not limited to those mentioned above, and other effects not mentioned will be clearly understood by those skilled in the art from the following description. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0054] The present invention will be described in more detail below with reference to examples according to the present invention and comparative examples not according to the present invention, but the scope of the present invention is not limited to the following examples. EXAMPLES
[0055] <Example 1> A polyamic acid solution was prepared by sequentially adding 900g of a mixed solvent of 30wt% m-xylene and 70wt% NMP (N-methylpyrrolidone), 46g ODA, 10g of glass fiber powder, 40g PMDA, and 14g ODPA to a glass reactor and stirring at 75°C for 2 hours. The completed polyamic acid solution was heated at 180°C for 2 hours at normal pressure to prepare a polyimide mixed solution. The powder precipitated in the mixed solution was filtered and washed with ethanol, and then dried for 24 hours to prepare a polyimide powder. The prepared powder was pressure molded at >50MPa and >300°C to prepare a molded product.
[0056] <Example 2> A molded article was produced in the same manner as in Example 1, except that 15 g of glass fiber powder was used.
[0057] <Example 3> A molded article was produced in the same manner as in Example 1, except that 20 g of glass fiber powder was used.
[0058] <Example 4> A molded article was produced in the same manner as in Example 1, except that 30 g of glass fiber powder was used.
[0059] <Example 5> A molded article was produced in the same manner as in Example 1, except that 40 g of glass fiber powder was used.
[0060] <Example 6> A molded article was produced in the same manner as in Example 1, except that 50 g of glass fiber powder was used.
[0061] <Comparative Examples 1 to 5> As shown in Table 1 below, polyimide powder was prepared in the same manner as in Example 1, except that the filler components were different.
[0062] Specifically, Comparative Example 1 is a case where no filler was added, and Comparative Examples 2 to 5 are cases where various fillers that are conventionally added were added.
[0063] <Experimental Example> The physical properties of the prepared polyimide powder were measured using the following methods, and the results are shown in Table 1 below.
[0064] Experimental Example 1 - Measurement of weight loss rate To analyze the weight loss rate, a compression molded test piece (5mm x 5mm x 5mm regular hexahedron shape) of polyimide powder was used to measure the weight loss rate (%) at 800℃ using a thermogravimetric analyzer (TGA). Specifically, the weight loss rate was compared after leaving the specimen at 800℃ for 25 hours under 0.61Mpa air pressure.
[0065] % weight loss = (initial weight - weight after exposure) / initial weight x 100
[0066] Experimental Example 2: Measurement of surface resistance To measure the surface resistance, compression molded test pieces of polyimide powder were used, and the surface resistance of the examples and comparative examples was measured according to the standard ASTM D257. Specifically, the surface resistance was measured according to the ASTM-D257 measurement method under the conditions of 55% RH, 23°C, and an applied voltage of 500V, and the measurement equipment was a 4-point probe meter (CMT-SR 1000N, AIT).
[0067] [Table 1]
[0068] Referring to Table 1, in the case of Examples 2, 4, 5 and 6 in which the polyimide powder having the dianhydride monomer component and the diamine monomer component as polymerization units according to the present invention further contains glass fiber powder, the surface resistance is 10 14 Ω / cm 2The 800°C weight loss rate (%) is 18.1% to 31.5%, which shows that the insulation properties are maintained and stability at high temperatures of 800°C is ensured. In particular, in the case of Example 6, when the content of the glass fiber powder is 50wt%, the 800°C weight loss rate (%) is 18.1%, which shows that the molded product has excellent high heat resistance. As a result, in the cases of Examples 2, 4, 5 and 6 of the present invention, the molded product standard is 10 14 Ω / cm 2 As described above, it is possible to reduce the 800°C weight loss rate (%), and therefore it is possible to maintain the insulation properties and ensure stability at high temperatures of 800°C.
[0069] On the other hand, when no filler was added (Comparative Example 1) and when conventional fillers were added (Comparative Examples 2 to 5), the surface resistance was low, resulting in poor insulation, and the 800°C weight loss rate (%) increased, resulting in poor high-temperature stability.
[0070] In addition, the method for producing polyimide powder according to the present application involves mixing glass fibers during in-situ polymerization, so the polyimide powder has excellent dispersibility, and the glass fibers act as seeds to produce a more uniform powder.
[0071] In addition, since the polyimide powder according to the present application contains an aromatic chain and further contains glass fiber powder as a filler, it may have better heat resistance than conventional polyimide powders.
[0072] Experimental Example 2: Measurement of chemical resistance (weight loss rate) To analyze chemical resistance, polyimide molded products were processed into 5mm x 5mm x 5mm regular hexahedron test pieces. The regular hexahedron test pieces were immersed in a 49% hydrofluoric acid solution for 168 hours. The appearance change and weight loss rate after immersion were measured.
[0073] Using the same method, a regular hexahedral test piece was immersed in 25-28% ammonia water for 168 hours, and the appearance change and weight loss rate before and after immersion were measured.
[0074] [Table 2]
[0075] Referring to Table 2, in the case of Examples 1, 3, 4 and 6, which include glass fiber powder dispersed in polyimide metric having polymerization units derived from dianhydride monomer and diamine monomer as in the present invention, the weight loss rate measured when immersed in a hydrofluoric acid solution was 1.0% to 2.6%, and the weight loss rate measured when immersed in an ammonia aqueous solution was 2.0% to 10.0%, indicating that the chemical resistance is excellent.
[0076] On the other hand, when no filler was added (Comparative Example 1), the weight loss rate measured when immersed in a hydrofluoric acid solution and an ammonia solution was high, indicating that the chemical resistance was low.
[0077] Table 3 below shows the experimental results comparing the intrinsic viscosity (IV), moldability, and processability of an embodiment using a mixed solvent of an aprotic solvent and a protic solvent according to one embodiment of the present invention and comparative examples using an aprotic solvent alone or a protic solvent alone.
[0078] Specifically, Comparative Example 6 is a case where m-cresol was used alone, and Comparative Example 7 is a case where NMP was used alone, but is otherwise the same as Example 1. Example 7 is a case where a 50 / 50 wt% mixed solution of m-cresol / NMP was used, Example 8 is a case where a 30 / 70 wt% mixed solution of m-cresol / NMP was used, and Example 9 is a case where a 70 / 30 wt% mixed solution of m-cresol / NMP was used, but is otherwise the same as Example 1.
[0079] [Table 3]
[0080] As shown in Table 3, in the cases of Comparative Examples 6 and 7 in which a protic solvent or an aprotic solvent was used alone, the intrinsic viscosity (IV) was low, and it was difficult to ensure moldability and processability.
[0081] On the other hand, in the case of Examples 7 to 9 in which a mixed solvent of a protic solvent and an aprotic solvent was used as in the embodiment of the present invention, it can be seen that the intrinsic viscosity (IV) was high and the moldability and processability were all excellent.
[0082] The present invention described above is not limited to the above-described embodiments, since various substitutions and modifications can be made by those having ordinary skill in the art to which the present invention pertains without departing from the technical spirit of the present invention.
Claims
1. preparing a polyamic acid solution by solution polymerizing a dianhydride monomer and a diamine monomer in an organic solvent containing glass fibers; heating the polyamic acid solution to prepare a polyimide mixture; and and filtering and drying the precipitate present in the mixture to obtain a polyimide powder.
2. 2. The method of claim 1, wherein the content of the glass fiber contained in the organic solvent is 5 to 90 parts by weight based on 100 parts by weight of the dianhydride monomer and the diamine monomer combined.
3. 2. The method for producing a polyimide powder according to claim 1, wherein the organic solvent is a mixed solvent of an aprotic solvent and a protic solvent.
4. The aprotic solvent is at least one selected from the group consisting of toluene, xylene, naphtha, anisole, cresol, ethylbenzene, propylbenzene, chlorobenzene, dichlorobenzene, trichlorobenzene, biphenyl, terphenyl, diphenyl ether, diphenyl sulfide, acetophenone, chlorinated biphenyl, and chlorinated diphenyl ether; 4. The method of claim 3, wherein the protic solvent is at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), N,N'-dimethylformamide (DMF), N,N'-diethylformamide (DEF), N,N'-dimethylacetamide (DMAc), dimethylpropanamide (DMPA), N,N-diethylacetamide (DEAc), 3-methoxy-N,N-dimethylpropanamide (KJCMPA), and gamma-butyrolactone (GBL).
5. 4. The method for producing a polyimide powder according to claim 3, wherein the mixed solvent contains 10 to 90 wt % of an aprotic solvent and 10 to 90 wt % of a protic solvent.
6. 2. The method of claim 1, wherein the step of preparing the polyamic acid solution is performed at a temperature of 50 to 100.degree.
7. 2. The method of claim 1, wherein the step of preparing the polyimide mixture is performed at a temperature of 140 to 200.degree.
8. 2. The method of claim 1, wherein the dianhydride monomer comprises at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA), and p-phenylenebis(trimellitate anhydride) (TAHQ).
9. 2. The method of claim 1, wherein the diamine monomer comprises at least one selected from the group consisting of 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenyl ether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine (M-TOLIDINE), 2,2-bis(trifluoromethyl)benzidine (TFDB), 1,4-bisaminophenoxybenzene (TPE-Q), bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).
10. polyimide metric having polymerized units derived from dianhydride and diamine monomers; and glass fibers dispersed within said polyimide metric; A polyimide powder characterized by satisfying one or more of the following conditions: a) After standing at 800° C. for 25 hours, the weight loss rate measured is 35% or less, and the surface resistance is 10 14 Ω / cm 2 The above; b) a weight loss of 2.6% or less, measured after immersion for 168 hours in an acidic aqueous solution having a pH of 5 or less; or c) A weight loss of less than 15% measured after immersion for 168 hours in an alkaline aqueous solution having a pH of 9 or more.
11. The polyimide powder according to claim 10, comprising 0.01 to 90 parts by weight of glass fiber powder per 100 parts by weight of the polyimide powder.
12. 11. The polyimide powder according to claim 10, wherein the dianhydride monomer comprises at least one selected from the group consisting of pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4-biphenyltetracarboxylic dianhydride (a-BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), oxydiphthalic dianhydride (ODPA), 4,4-(hexafluoroisopropylidene)diphthalic anhydride (6-FDA), and p-phenylenebis(trimellitate anhydride) (TAHQ).
13. 11. The polyimide powder according to claim 10, wherein the diamine monomer comprises at least one selected from the group consisting of 1,4-diaminobenzene (PPD), 1,3-diaminobenzene (MPD), 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenyl ether (ODA), 4,4'-methylenediamine (MDA), 4,4-diaminobenzanilide (4,4-DABA), N,N-bis(4-aminophenyl)benzene-1,4-dicarboxamide (BPTPA), 2,2-dimethylbenzidine (M-TOLIDINE), 2,2-bis(trifluoromethyl)benzidine (TFDB), 1,4-bisaminophenoxybenzene (TPE-Q), bisaminophenoxybenzene (TPE-R), 2,2-bisaminophenoxyphenylpropane (BAPP), and 2,2-bisaminophenoxyphenylhexafluoropropane (HFBAPP).
14. A method for producing a polyimide molded product, comprising the step of compressing and molding the polyimide powder according to claim 10.
15. The method for producing a polyimide molded product according to claim 14, wherein the pressure molding is performed at a pressure of 30 to 1,000 MPa.
16. The method for producing a polyimide molded product according to claim 14, wherein the pressure molding is performed at 200 to 500° C.
17. The method for producing a polyimide molded product according to claim 14, further comprising the step of sintering the pressed polyimide powder at 200 to 500° C.
18. A polyimide molded product produced by the method according to any one of claims 14 to 17.
Citation Information
Patent Citations
Preparation method of aerospace low-resistivity polyimide composite material
CN103725001A
Polyimide resin composition
JP1986095067A
Polyimide powder and production thereof
JP1986281150A
Polyimide powder containing inorganic powder and production thereof
JP1988081160A
Polyimide molded article
JP2001354782A