Iron-copper alloy having a mesh structure and its manufacturing method
An iron-copper alloy with a network structure, produced by specific manufacturing processes, addresses the limitations of existing alloys by enhancing hardness, tensile strength, and thermal conductivity, enabling its use in mold materials and cooling applications.
Patent Information
- Application Number
- JP2024519953
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-09
- Filing Date
- 2022-04-22
- Publication Date
- 2024-12-06
AI Technical Summary
Existing iron-copper alloys have low mechanical properties such as hardness and thermal conductivity, making them unsuitable for applications requiring heat dissipation and cooling, while beryllium-copper alloys are expensive and difficult to melt and cast.
An iron-copper alloy with a network structure formed by copper, containing 65 to 85% iron and 15 to 35% copper, is produced through melting, casting, natural cooling, heat treatment, and rapid quenching to achieve high hardness, tensile strength, and thermal conductivity.
The alloy achieves high Rockwell hardness of 30HRC or more, tensile strength of 700N/mm² or more, and thermal conductivity of 90W/m·K or more, making it suitable for mold materials and cooling machine components.
Smart Images

Figure 2024545388000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an iron-copper alloy having a network structure and a manufacturing method thereof. In one embodiment, the present invention relates to a high-hardness iron-copper alloy that contains an appropriate amount of copper (Cu) in iron (Fe), has a network structure formed by copper (Cu) in the alloy structure, and has high hardness while improving tensile strength and thermal conductivity, and a manufacturing method thereof. [Background technology]
[0002] Aluminum alloys are used for various purposes in various industrial fields due to their excellent light weight, thermal conductivity, and ductility. Aluminum alloys have particularly high thermal conductivity and can quickly cool heat. As a result, aluminum alloys can minimize deformation and warping of molded products, and are effectively used as mold materials for injection molding and die casting.
[0003] For example, technologies relating to aluminum alloys for die casting are disclosed in Patent Documents 1 and 2. Aluminum alloys are based on aluminum (A1) with small amounts of silicon (Si), iron (Fe), manganese (Mn), magnesium (Mg), etc. added, and aluminum-silicon-magnesium (Al-Si-Mg) type alloys are widely used as materials for die casting dies.
[0004] However, aluminum alloys have low mechanical properties such as hardness (wear resistance) and tensile strength. In recent years, beryllium-copper (Be-Cu) alloys, which have good thermal conductivity and excellent mechanical properties such as hardness and tensile strength, have been attracting attention as mold materials. For example, Patent Documents 3 to 5 disclose techniques related to beryllium-copper (Be-Cu) alloys.
[0005] However, beryllium-copper alloys have problems in that melt casting is difficult, and the raw materials beryllium (Be) and copper (Cu) themselves are expensive, making them less economical. As a result, beryllium-copper alloys are limited to use in expensive, high-end products, and are less versatile.
[0006] On the other hand, iron-copper (Fe-Cu) alloys are easier to melt cast than beryllium-copper alloys, and are also advantageous in terms of economy. For example, Patent Document 6 discloses iron-copper alloys produced using a melt casting method. However, conventional iron-copper alloys have poorer mechanical properties than beryllium-copper alloys, particularly poor hardness and thermal conductivity, making them difficult to apply to machine parts that require heat dissipation or cooling. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Republic of Korea Patent Publication No. 10-2015-0046014 [Patent Document 2] Republic of Korea Patent No. 10-1606525 [Patent Document 3] Japanese Patent Publication No. 2003-003246 [Patent Document 4] Republic of Korea Patent Publication No. 110-2012-0048287 [Patent Document 5] Republic of Korea Patent Publication No. 10-2015-0053814 [Patent Document 6] Japanese Patent Application Publication No. 5-331572 Summary of the Invention [Problem to be solved by the invention]
[0008] The present invention aims to provide a high-hardness iron-copper alloy, which is an inexpensive iron-copper (Fe-Cu) alloy that can replace beryllium-copper (Be-Cu) alloy and has improved tensile strength and thermal conductivity while maintaining high hardness, and a method for producing the same. [Means for solving the problem]
[0009] In order to achieve the above object, the present invention provides an iron-copper alloy containing 65 to 85 atomic % of iron and 15 to 35 atomic % of copper, the alloy structure having a network structure formed by copper.
[0010] The present invention also provides an iron-copper alloy containing 68 to 80 atomic % of iron and 20 to 32 atomic % of copper, having a network structure formed by copper in the alloy structure, and having the following physical properties (a) to (c):
[0011] (a) Rockwell hardness: 30HRC or more (b) Tensile strength: 700N / mm 2 End (c) Thermal conductivity: 90 W / m K or more
[0012] The present invention also provides a melting step of feeding iron and copper into a melting furnace and melting them to form a molten metal so that the iron-copper alloy contains 65 to 85 atomic % of iron and 15 to 35 atomic % of copper; casting step of pouring the molten metal into a casting flask to form a casting; a cooling step of naturally cooling the casting at room temperature; A heat treatment step of placing the naturally cooled casting in a heat treatment furnace and heat treating it at a temperature of 945°C to 980°C; and a quenching step of immersing the heat-treated casting in a cooling medium immediately after the heat treatment to rapidly cool it; The present invention provides a method for producing an iron-copper alloy having a mesh structure formed by copper in the alloy structure, comprising:
[0013] According to one embodiment, the heat treatment process can be carried out by placing the naturally cooled casting into a heat treatment furnace and then increasing the temperature in the heat treatment furnace to 945°C to 980°C at a rate of 2°C / min to 15°C / min. Effect of the Invention
[0014] According to the present invention, an inexpensive iron-copper (Fe-Cu) alloy that can replace beryllium-copper (Be-Cu) alloy is provided. Specifically, according to the present invention, the alloy is an amorphous alloy in which an appropriate amount of copper (Cu) is molten and alloyed with iron (Fe), and has a network structure in the alloy structure, which has the effect of improving at least hardness, tensile strength, and thermal conductivity, etc., compared to conventional iron-copper (Fe-Cu) alloys. In addition, according to the present invention, the mechanical properties and thermal conductivity are improved, and the alloy can be used not only as a mold material but also as a cooling machine part, etc. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic cutaway view of an Fe—Cu alloy for explaining the network structure according to the present invention. [Diagram 2] FIG. 2 is a SEM photograph of an Fe—Cu alloy produced according to an embodiment of the present invention, taken before heat treatment. [Diagram 3] FIG. 3 is a SEM photograph of an Fe—Cu alloy produced according to an embodiment of the present invention, which is a highly magnified microstructure photograph after heat treatment and quenching. [Figure 4] FIG. 4 is a SEM photograph of an Fe—Cu alloy produced according to a comparative example of the present invention, which is a highly magnified microstructure photograph after heat treatment and quenching. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention provides an iron-copper alloy that is an iron-based alloy mainly composed of iron (Fe), contains iron (Fe) and copper (Cu) in appropriate amounts, has a network structure formed within the alloy structure, and has improved at least mechanical properties and thermal properties. The present invention also provides a method for manufacturing such an iron-copper alloy.
[0017] The iron-copper alloy according to the present invention contains iron (Fe) and copper (Cu), and is an iron-based alloy with a higher content of iron (Fe) than copper (Cu), and contains 65-85 atomic % of iron (Fe) and 15-35 atomic % of copper based on the total of iron (Fe) and copper (Cu). The content unit "atomic %" used in the present invention is based on the total atomic content of iron (Fe) and copper (Cu) (the total of Fe and Cu is 100 atomic %), which can also be expressed as "volume %" as is well known in the art. That is, in the present invention, it can be expressed as atomic % = volume %.
[0018] The iron-copper alloy according to the present invention does not contain any metal elements other than iron (Fe) and copper (Cu) except for unavoidable ones. The iron-copper alloy according to the present invention may contain unavoidable impurities. The unavoidable impurities are those contained in the raw materials themselves, or those that are unavoidably introduced from the outside during the melting process, etc., and may include, for example, metal elements such as aluminum (A1) and nickel (Ni) and nonmetal elements such as carbon (C) and oxygen (O), but such impurities are contained in extremely small amounts. The impurities are based on the entire alloy composition (the sum of Fe + Cu + impurities), and may be unavoidably contained in extremely small amounts, for example, 0.5 atomic % or less, 0.2 atomic % or less, 0.1 atomic % or less, 0.05 atomic % or less, or 0.01 atomic % or less.
[0019] The iron-copper alloy according to the present invention has at least high mechanical and thermal properties due to the appropriate content of iron (Fe) and copper (Cu) and the network structure formed in the alloy structure. Specifically, the iron-copper alloy according to the present invention has high hardness, tensile strength, thermal diffusion rate, and thermal conductivity compared to conventional iron-copper alloys, and does not contain segregation or cracks.
[0020] Hereinafter, a method for producing an iron-copper alloy according to the present invention will be described together with an embodiment of the iron-copper alloy according to the present invention. The method described below can easily realize the production of the iron-copper alloy according to the present invention. However, the iron-copper alloy according to the present invention is not limited to the one produced by the method described below.
[0021] The method for producing an iron-copper alloy according to the present invention (hereinafter, abbreviated as "production method") includes a melting process for forming a molten iron-copper alloy in a melting furnace, a casting process for pouring the molten iron-copper alloy into a casting flask for casting, and a cooling process for naturally cooling the casting at room temperature. According to a preferred embodiment, the production method according to the present invention further includes a heat treatment process for heat treating the naturally cooled casting; and a quenching process for quenching the heat treated casting. An embodiment of each process will be described as follows.
[0022] [1] Melting process The alloy raw material of iron and copper is put into a melting furnace and melted. In this case, high-purity pure iron can be used as the iron, and high-purity electrolytic copper can be used as the copper. The melting furnace is not particularly limited, and for example, a melting furnace for ordinary ceramic materials can be used. The melting furnace can preferably be a high-frequency induction heat melting furnace capable of rapid melting through rapid heating. The melting furnace is preferably maintained at a temperature at which iron and copper can be melted. For example, it is preferable to quickly heat the melting furnace through high-frequency induction heat and maintain it at about 1520°C to 1650°C to melt the iron and copper. In this melting process, stirring is performed. After the iron and copper are completely melted, the molten metal temperature can be stabilized by maintaining it at, for example, 1450°C to 1520°C and leaving it. By such stabilization, the iron and copper can be homogenized.
[0023] In this melting process, iron and copper are charged into a melting furnace and melted to form a molten metal so that the final iron-copper alloy contains 65-85 atomic % (or volume %) of iron and 15-35 atomic % (or volume %) of copper based on the total amount. Specifically, when the total amount of iron and copper charged into the melting furnace is 65-85 volume % of iron and 15-35 volume % of copper (i.e., the volume ratio of iron:copper=65-85:15-35), the alloy composition can be obtained as described above. At this time, if the copper content is less than 15 atomic %, a mesh structure is not formed, and mechanical properties and thermal properties may become poor. In addition, if the copper content is less than 15 atomic %, cracks may occur when the alloy is subjected to high-temperature heat treatment at 860°C or more after melt casting. In addition, if the copper content exceeds 35 atomic %, a complete mesh structure is difficult to form, and mechanical properties may be poor. As a result, in an embodiment of the present invention, when the copper content is 15 to 35 atomic %, no cracks occur even when a high-temperature heat treatment of 860°C or higher is performed after molten casting, and the material has high mechanical properties and thermal characteristics.
[0024] According to a preferred embodiment of the present invention, in the melting process, it is preferable to feed iron and copper into a melting furnace and melt them to form a molten metal so that the final iron-copper alloy contains 68-80 atomic % of iron and 20-32 atomic % of copper. That is, it is preferable to feed the total amount of iron and copper into the melting furnace with 68-80 volume % of iron and 20-32 volume % of copper, so that the alloy has an alloy composition containing 68-80 atomic % of iron and 20-32 atomic % of copper. When the alloy has such an alloy composition, a complete network structure is formed in the alloy structure, and the alloy has excellent mechanical properties and thermal properties.
[0025] FIG. 1 is a perspective cutaway view illustrating an Fe-Cu alloy according to the present invention, which is a schematic diagram of an alloy structure for explaining a mesh structure. Referring to FIG. 1, the mesh structure (10) of the present invention is formed of copper (Cu), which is formed overall on the surface and inside of the alloy and has a three-dimensional structure. In the present invention, "formed of copper (Cu)" means copper-rich. According to the present invention, the mesh structure (10) improves the mechanical properties (hardness, tensile strength, etc.) of the alloy, which in particular increases the thermal diffusion rate of the alloy, thereby significantly improving thermal conductivity.
[0026] As shown in FIG. 1, the mesh structure (10) is formed by connecting linear copper-rich wires (12) in a mesh-like manner within the alloy structure. The mesh structure (10) has, for example, a cage-shaped three-dimensional mesh structure, which is mainly composed of copper (Cu). Specifically, the copper-rich wires (12) are mainly composed of copper (Cu). In one embodiment, the copper-rich wires (12) contain copper (Cu) and iron (Fe), with the copper (Cu) content being higher than the iron (Fe). The copper-rich wires (12) may contain, for example, 60 atomic % or more, 70 atomic % or more, or 80 atomic % or more of copper (Cu), with the remainder being composed of iron (Fe). In addition, the copper-rich wires (12) have a thickness of micrometers (μm), which may be, for example, 0.1 μm to 30 μm. Such copper-rich wires (12) act as fast tunnels for fast heat diffusion, which at least increases the heat diffusion rate of the alloy.
[0027] [2] Casting process The molten metal is poured into the flask to form an alloy casting having a desired shape. This casting process is a conventional process. The flask is not particularly limited, and it can have the shape of an ingot or a cast piece, or in some cases the shape of an actual application product (such as a machine part). In addition, the flask can have a cooling function as in the conventional case.
[0028] [3] Cooling process The casting is naturally cooled at room temperature. This cooling step can be carried out by leaving the casting at room temperature, for example, while it is housed in a casting flask. In the present invention, room temperature is, for example, a temperature of 5°C to 30°C, and a specific example is room temperature of about 15°C to 25°C.
[0029] [4] Heat treatment process The naturally cooled casting is heat treated. The heat treatment can be performed by placing the naturally cooled casting in a heat treatment furnace, raising the temperature in the heat treatment furnace to a high temperature, and maintaining the high temperature for a predetermined period of time. The heat treatment can be performed in an air atmosphere or an inert (non-oxidizing) atmosphere. There are no particular limitations on the heat treatment furnace as long as it can apply high heat to the casting, and for example, an electric furnace (heating furnace) equipped with an electric heating wire can be used.
[0030] The heat treatment is preferably performed at a temperature of 945°C to 980°C. Specifically, the heat treatment may be performed by placing the naturally cooled casting into a heat treatment furnace, increasing the temperature in the heat treatment furnace to 945°C to 980°C at a heating rate of 2°C / min to 15°C / min, and then maintaining the temperature at 945°C to 980°C for a predetermined period of time. When the heat treatment is performed in this temperature range, the mechanical properties and thermal properties of the alloy are improved. When the heat treatment temperature is less than 945°C or exceeds 980°C, the degree of improvement in the mechanical properties and thermal properties may decrease. In consideration of this, it is more preferable to perform the heat treatment at a temperature of 950°C to 970°C. In addition, the heat treatment may be performed for an appropriate time depending on the thickness of the casting, and for example, it is preferable to perform the heat treatment for about 30 to 90 minutes per 25 mm thickness of the casting. For example, when the thickness of the casting is 50 mm, it is preferable to perform the heat treatment for about 1 to 3 hours.
[0031] [5] Rapid cooling process The heat-treated casting is quenched. Quenching is carried out immediately after the heat treatment, specifically within 5 minutes after the heat treatment. Quenching is carried out by quenching the heat-treated casting in a cooling medium. Once this quenching is completed, an alloy with a complete mesh structure (10) and excellent mechanical and thermal properties is obtained. If the heat-treated casting is allowed to cool (gradual natural cooling) without quenching, the mesh structure (10) will be eliminated and the mechanical and thermal properties may deteriorate.
[0032] In the present invention, quenching is performed by baking in a cooling medium immediately after heat treatment, and the cooling medium used here can be selected from liquids having a temperature of 30° C. or less. The cooling medium can be selected from, for example, water and oil, and these can be at room temperature.
[0033] According to the manufacturing method of the present invention described above, an iron-copper alloy is manufactured that is a homogeneous amorphous iron-copper alloy free from segregation or cracks and has improved at least mechanical properties (hardness, tensile strength, etc.) and thermal properties (thermal conductivity, etc.).
[0034] According to a preferred embodiment, the iron-copper alloy according to the present invention contains 68-80 atomic % of iron and 20-32 atomic % of copper. When the alloy has such an alloy composition, properties such as hardness, tensile strength, and thermal conductivity are effectively improved. In addition, the iron-copper alloy according to the present invention preferably has the following physical properties (a) to (c). When the alloy has the following physical properties (a) to (c), the alloy can be usefully used not only as a mold material for injection molding and die casting, but also as a cooling machine part that requires heat dissipation or cooling.
[0035] (a) Rockwell hardness: 30HRC or more (b) Tensile strength: 700N / mm 2 End (c) Thermal conductivity of 90 W / m K or more
[0036] Rockwell hardness, tensile strength and thermal conductivity are measured according to conventional methods. Rockwell hardness may be measured according to KSB0806, and tensile strength may be measured according to KSB0801. Thermal conductivity may be measured at room temperature (20°C to 25°C), for example, according to ASTM E1461 (Laser flash: Thru-plane). The iron-copper alloy according to the present invention has, for example, a Rockwell hardness of 30 to 48HRC, a thermal conductivity of 700 to 750N / mm 2 and a thermal conductivity of 90 to 120 W / m·K.
[0037] Hereinafter, examples and comparative examples of the present invention will be described. The following examples are provided for illustrative purposes to help understand the present invention, and are not intended to limit the technical scope of the present invention. In addition, the following comparative examples do not represent prior art, and are provided merely for comparison with the examples.
[0038] [Example 1] <Melting / Casting / Cooling> Iron (pure iron with a purity of about 99.9% by weight) and copper (electrolytic copper with a purity of about 99.9% by weight) were initially put into a melting furnace (high-frequency induction thermal melting furnace) in a volume ratio of 1:1, and the melting furnace's power output was increased while stirring to quickly melt the mixture. During the melting process, a deoxidizer was intermittently added to the melting furnace to deoxidize it. After confirming that the added iron and copper had completely melted by visual observation, iron was added to the melting furnace in small batches while continuing to stir, and the molten metal temperature was maintained within the range of about 1500°C to 1550°C to completely melt the added iron. Next, the power was cut off, and the molten metal was left in the melting furnace for a predetermined time so that the alloy structure could be stabilized. After that, the molten metal was removed from the melting furnace and poured into a casting frame, and then gradually cooled naturally at room temperature (about 25°C) to obtain an Fe-Cu alloy ingot.
[0039] <Quenching / Quenching> The naturally cooled ingot (width x length x thickness = about 50 mm x 25 mm x 25 mm) was put into a heat treatment furnace (electric furnace with heating wires) prepared in advance, and then heated at a heating rate of 5 ° C / min. The heat treatment temperature was set to 845 ° C by a temperature controller. At this time, the temperature inside the heat treatment furnace was maintained in the range of about 840 to 850 ° C. The ingot was heat treated for about 1 hour in the above temperature range. The heat-treated ingot was immersed in a water tank containing water (cooling medium) at about 17 ° C immediately after the heat treatment (within 1 minute after being removed from the heat treatment furnace) and quenched. After quenching in the water tank for a sufficient time and quenching, the ingot was removed from the water tank, and an alloy sample according to this embodiment in which the heat treatment / quenching process was completed was manufactured.
[0040] [Examples 2 to 6] The alloy test pieces in this embodiment were made by changing the temperature during the heat treatment compared to the above-mentioned Example 1. Specifically, the heat treatment temperature was changed for each Example for an Fe-Cu alloy ingot having the same alloy composition as Example 1. This is shown in [Table 1].
[0041] [Examples 7 to 11] The alloy test pieces of this embodiment were prepared by changing the Cu content of the composite composition and the temperature during heat treatment in comparison with Example 1. The specific Cu content and heat treatment temperature in each embodiment are shown in Table 1.
[0042] [Comparative Examples 1 to 10] Compared to Example 1, one or more of the Cu content in the synthetic composition, the temperature during heat treatment, the heat treatment method, and the cooling method after heat treatment were changed and used as alloy samples in this comparative example. This is as shown in [Table 1]. In [Table 1], the slow cooling in Comparative Example 8 and Comparative Example 9 is natural cooling in which the heat-treated ingot was gradually cooled to room temperature (about 25°C). Also, in [Table 1], the "quenching (950)" in Comparative Example 10 is a heat treatment performed by immersing the ingot in oil maintained at a temperature of about 950°C for one hour.
[0043] The Fe-Cu alloy test pieces according to the examples and comparative examples obtained as described above were subjected to component analysis, crack, network structure and physical property evaluation as follows, and the results are shown in Table 1. The Cu content shown in Table 1 is the at% of Cu (the remainder is Fe) based on the total of Fe and Cu atoms being 100 (=Fe+Cu) as determined by the component analysis described below, and this does not take into account unavoidable impurities such as extremely small amounts of metal elements (metals other than Fe and Cu), C and O.
[0044] <Component analysis> The alloy sample whose weight was measured was placed in a glass beaker, and 10 mL of aqua regia (aqueous solution of hydrochloric acid and sulfuric acid) was added to dissolve it. After that, Fe and Cu were quantified and converted into the concentration in the sample by inductively coupled plasma atomic emission spectrometry (ICP-AES) under the following measurement conditions.
[0045] * ICP-AES measurement conditions -Measuring device: Perkin Elmer Optima 5300DV -Measurement wavelength: 238.204nm (Fe), 327.393nm (Cu) -Quantification method: Internal standard method
[0046] <Crack> After the heat treatment and quenching, the alloy samples were subjected to surface observation at high magnification. If cracks occurred, they were rated as "occurred", and if no cracks were present, they were rated as "absent". The results are shown in Table 1.
[0047] <Mesh structure> The alloy test pieces after heat treatment and quenching were observed with a SEM (scanning electron microscope). When a complete mesh structure was observed, it was rated as "Good", when it was difficult to determine a complete mesh structure and lumps or breaks were observed, it was rated as "Good", and when no mesh structure was observed, it was rated as "Poor". The results are shown in Table 1.
[0048] Fig. 2 is a photograph of the Fe-Cu alloy according to Example 4 before heat treatment, and Fig. 3 is a highly magnified microscopic photograph of the Fe-Cu alloy according to Example 4 after heat treatment and quenching. And Fig. 4 is a highly magnified microscopic photograph of the Fe-Cu alloy according to Comparative Example 7 after heat treatment and quenching. To explain the evaluation of the network structure in detail, when a complete network structure is clearly visible as in Fig. 3 and Cu forms a network structure with a substantially constant thickness, it is marked as "◯", when it is difficult to see a complete network structure as in Fig. 4 and parts where Cu is solidified are observed, it is marked as "△", and when no network structure is observed at all, it is marked as "X".
[0049] <Physical Properties> The physical properties were evaluated for the alloy test pieces after heat treatment and quenching. The hardness was evaluated by Rockwell Hardness (HRC) according to KSB0806, and the tensile strength was evaluated according to KSB0801. The thermal conductivity was evaluated according to ASTM E1461 (Laser flash: Thru-plane) after measuring the density, specific heat, and thermal diffusion coefficient of the alloy sample as a method for measuring the thermal conductivity of metal samples.
[0050] [Table 1] [Table 1]
[0051] In the present invention, many experiments were conducted to examine the effects of the Fe and Cu contents in the alloy composition, the heat treatment conditions after melt casting, and the cooling conditions after heat treatment on the Fe-Cu alloy. For example, the alloy composition was finely divided into Cu contents in the range of 5-50 at%, and the heat treatment temperature was increased from 600°C to 1100°C in 10°C increments. The above examples and comparative examples are only a few of the many experimental examples of the present invention.
[0052] According to the experimental study of the present invention, it was found that the structure, mechanical properties, and thermal properties of the Fe-Cu alloy vary depending on the Cu content in the alloy composition, the heat treatment temperature, and the cooling method after heat treatment (quenching or gradual release). In particular, it was found that a mesh structure formed by Cu was observed under specific Cu content and heat treatment conditions, and that such a mesh structure significantly improves at least the hardness and thermal conductivity. This is explained below with reference to [Table 1].
[0053] Referring to [Table 1], first, it was found whether or not a mesh structure exists depending on the Cu content. Specifically, when the Cu content is less than 15 at% (Comparative Examples 1 to 5), no mesh structure appears in the alloy structure. Also, when the Cu content is less than 15 at%, cracks occur when heat-treated at a temperature of 860°C or higher (Comparative Examples 2 to 5). This is considered to be because the Fe structure is not finely divided and segregates. On the other hand, when the Cu content exceeds 35 at% (Comparative Examples 6 and 7), a mesh structure appears, but it is difficult to see this as a complete mesh structure. Specifically, as shown in FIG. 4 (photograph of alloy test piece of Comparative Example 7: Cu content 40.24 at%), the shape and thickness of the copper-rich wire are not uniform, making it difficult to see a complete mesh structure, and the aggregation phenomenon of Cu and Fe occurs in places.
[0054] On the other hand, when the Cu content was about 20 to 32 at% (Examples 1 to 11), a complete mesh structure was clearly observed. Also, as shown in Figure 3 (photograph of alloy test piece of Example 4: Cu content 20.12 at%), it was found that the copper-rich wires forming the mesh structure had a nearly constant thickness in micrometers (μm). And, as shown in [Table 1], it was found that the thermal conductivity as well as hardness and tensile strength were highly evaluated.
[0055] It was also found that the mechanical properties and thermal properties differ depending on the heat treatment temperature. For example, comparing Examples 1 to 6, it was found that when heat treatment was performed under the same conditions at a temperature of about 950°C to 980°C (Examples 4 and 5), the best results were observed in all properties including hardness, tensile strength, and thermal conductivity. In particular, hardness and tensile strength did not continuously increase in proportion to the increase in heat treatment temperature. From these results, it was found that the optimal heat treatment temperature was about 945°C to 980°C.
[0056] It was also found that rapid cooling is preferable for cooling after heat treatment. For example, when Example 4 (rapid cooling) is compared with Comparative Example 9 (slow cooling), it was found that when slow cooling was performed under all the same conditions (Comparative Example 9), no mesh structure was formed and the mechanical properties and thermal characteristics were inferior. This is believed to be because the mesh structure formed in the early stages in the alloy structure disappeared during the gradual cooling process.
[0057] In addition, it was found that the mechanical and thermal properties differ depending on the heat treatment method. Comparing Example 4 (heat treatment in a heat treatment furnace) and Comparative Example 10 (heat treatment in a quenching furnace), it was found that when quenching heat treatment was performed under the same conditions (Comparative Example 10), a complete mesh structure did not appear, and hardness and thermal conductivity decreased.
[0058] To summarize the above results, it was found that when the Cu content is within the range of about 20-32 at% (the remainder is Fe), heat treatment is performed in a heat treatment furnace (electric furnace) at a temperature range of 945°C to 980°C (preferably 950°C to 970°C), and the material is quenched after heat treatment (quenched in a cooling medium), the material has a perfect mesh structure without cracks and has excellent mechanical properties and thermal characteristics. Specifically, the mechanical properties and thermal characteristics are a Rockwell hardness of at least 30HRC and a Rockwell hardness of at least 700N / mm 2 It was found that the alloy had a tensile strength of at least 30 HRC and a thermal conductivity of at least 90 W / m K. The iron-copper (Fe-Cu) alloy of the present invention, which has such properties, can of course be used as a substitute for beryllium-copper (Be-Cu) alloy, and since it has a high hardness of at least 30 HRC and a high thermal conductivity of at least 90 W / m K, it can also be usefully used as a cooling machine part.
Claims
1. A melting step of feeding iron and copper into a melting furnace and melting them to form a molten metal so that the iron-copper alloy contains 65-85 atomic % iron and 15-35 atomic % copper; casting step of pouring the molten metal into a casting flask to form a casting; and A cooling step of naturally cooling the casting at room temperature is included. A method for producing an iron-copper alloy, in which no cracks are generated when the cooled casting is heat treated at 860°C or higher.
2. A melting step of feeding iron and copper into a melting furnace and melting them to form a molten metal so that the iron-copper alloy contains 65-85 atomic % iron and 15-35 atomic % copper; casting step of pouring the molten metal into a casting flask to form a casting; a cooling step of naturally cooling the casting at room temperature; A heat treatment step of placing the naturally cooled casting in a heat treatment furnace and heat treating it at a temperature of 945°C to 980°C; and The method includes a quenching step in which the heat-treated casting is quenched in a cooling medium immediately after the heat treatment, and the method includes the steps of: producing an iron-copper alloy having a mesh structure formed by copper in the alloy structure;
3. The method for producing an iron-copper alloy according to claim 2, wherein the heat treatment step is performed by placing the naturally cooled casting in a heat treatment furnace and then increasing the temperature in the heat treatment furnace to 945°C to 980°C at a rate of 2°C / min to 15°C / min.
4. In iron-copper alloys, The iron-copper alloy is produced by the method for producing the iron-copper alloy according to claim 2, 68-80 atomic % iron; and Contains 20 to 32 atomic percent copper; The alloy structure has a mesh structure formed by copper, The following (a) to (c) (a) Rockwell hardness: 30HRC or higher (b) Tensile strength: 700 N / mm 2 End (c) Thermal conductivity: 90 W / m K or more An iron-copper alloy having the physical properties described above.
5. In iron-copper alloys, 65 to 85 atomic percent iron; and Contains 15 to 35 atomic percent copper; An iron-copper alloy having a mesh structure formed by copper in the alloy structure.
6. The iron-copper alloy is 68-80 atomic % iron; and Contains 20 to 32 atomic percent copper; The following (a) to (c) (a) Rockwell hardness: 30HRC or higher (b) Tensile strength: 700 N / mm 2 End (c) Thermal conductivity: 90 W / m K or more The iron-copper alloy according to claim 5, having physical properties of
7. The mesh structure is formed by connecting copper-rich lines in a mesh shape, The iron-copper alloy according to any one of claims 4 to 6, wherein the copper-rich wire has a thickness of 0.1 μm to 30 μm.
Citation Information
Patent Citations
Copper-iron alloy
JP1993331572A
Cu-Be BASED AMORPHOUS ALLOY
JP2003003246A
Aluminum alloy for die casting having excellent corrosion resistance
KR101606525B1
Highly heat conductive aluminum alloy for die casting, aluminum alloy die cast product using same, and heatsink using same
KR1020150046014A
Cu-Be ALLOY AND METHOD FOR PRODUCING SAME
KR1020150053814A