Evaluation method for hot working process

A method using a rod-shaped test piece with controlled temperature and strain simulates hot working processes, enabling efficient evaluation and optimization of manufacturing parameters for hot worked products in smaller facilities.

JP2025002230APending Publication Date: 2025-01-09DAIDO STEEL CO LTD

Patent Information

Application Number
JP2023102265
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-22
Publication Date
2025-01-09

AI Technical Summary

Technical Problem

Existing methods for evaluating hot working processes in manufacturing hot worked products are inefficient and require repeated prototype production and small-scale demonstration experiments due to the complex relationship between material structure and physical properties, making it difficult to predict and optimize the manufacturing process accurately.

Method used

A method using a rod-shaped test piece with a metal structure mimicking a part of the ingot, subjected to temperature and strain control, is evaluated in a smaller experimental facility to simulate the hot working process, including unidirectional solidification and hot pressing to analyze metallographic structure and mechanical strength.

Benefits of technology

Enables efficient evaluation of hot working processes using small-scale experimental equipment, allowing for accurate prediction of material properties and optimization of manufacturing parameters, reducing costs and time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2025002230000001_ABST
    Figure 2025002230000001_ABST
Patent Text Reader

Abstract

To provide an evaluation method using an experimental facility smaller than a manufacturing facility for actual products, as an evaluation method of a hot working process in a manufacturing method for hot-worked products provided by hot-working ingots.SOLUTION: There is provided an evaluation method for a hot working process in a manufacturing method for hot worked products provided via the hot working process of hot-working an ingot until generating prescribed cumulative equivalent plastic strain while controlling the temperature. When evaluating the hot working process by analyzing a worked test piece obtained by a working simulation process in which a rod-like test piece made to have a metal structure simulating a portion of an ingot, is pressed from the side to elongate it in the longitudinal direction, the working simulation process involves temperature control, and heating control and strain control corresponding to a prescribed cumulative equivalent plastic strain.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating a hot working step in a manufacturing method of a hot worked product obtained by hot working an ingot. [Background technology]

[0002] The manufacturing process of plastically processed products is a fusion of two technologies: "creative technology," which creates a shape by plastic deformation, and "quality creation technology," which creates a material so that it has the desired physical and / or chemical properties (physical properties). The former "creative technology" is mainly a hot processing process such as forging, and can be simulated by numerical analysis using the finite element method. On the other hand, "quality creation technology" is greatly affected by the plastic processing in addition to the material structure (metal structure) of the ingot, and the relationship between the material structure and the physical properties is complex, making it difficult to perform a highly accurate computer simulation. As a result, prototypes and small-scale demonstration experiments are repeated. Therefore, methods have been proposed for producing test pieces that mimic the material structure of the ingot to be used in small-scale demonstration experiments.

[0003] For example, Patent Document 1 discloses a method of reproducing the solidification structure of a large ingot produced by electroslag remelting (ESR) or vacuum arc remelting (VAR) using a small test device. In this method, it is said that by arranging the crucible (refractory container) vertically, the cooling device becomes the bottom surface, and the mold cooling (cooling from the side) of ESR or VAR can be reproduced by the heating zone surrounding the crucible. In addition, as an example simulating VAR, a cooling device is arranged on the bottom surface to perform forced cooling to reproduce the rapid cooling state near the water-cooled surface plate of the actual ingot, and the zone heating is adjusted so that the time from the bottom to the top of the crucible heated to the molten metal temperature is shortened. It is said that this method can obtain a directional solidification structure similar to that of an ingot obtained by VAR. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 8-334483 Summary of the Invention [Problem to be solved by the invention]

[0005] In order to create a manufacturing plan for a plastic processed product, it is necessary to evaluate the relationship between the manufacturing process and the material structure. Here too, if it is possible to evaluate (predict) the manufacturing process using experimental equipment that is smaller than the manufacturing equipment used to manufacture the actual product, it will be possible to create a manufacturing plan at low cost and in a short time. It may also be possible to experimentally clarify the relationship between the material structure and physical properties (especially mechanical properties).

[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a method for evaluating a hot working step in a manufacturing method of a hot worked product obtained by hot working an ingot, using experimental equipment that is smaller than the manufacturing equipment for the actual product. [Means for solving the problem]

[0007] The method according to the present invention is a method for evaluating a hot working process in a manufacturing method for a hot worked product, which is provided through a hot working process in which a cast ingot is hot worked while controlling the temperature until it reaches a predetermined accumulated equivalent plastic strain, and is characterized in that, in evaluating the hot working process, a processed test piece obtained through a processing simulation process in which a rod-shaped test piece made to have a metal structure simulating a portion of the ingot is pressed from the side to elongate it in the longitudinal direction is analyzed and the processing simulation process performs the temperature control and heating control and strain control corresponding to the predetermined accumulated equivalent plastic strain.

[0008] According to this feature, it is possible to evaluate the hot working process using a small test piece simulating a part of an ingot even in an experimental facility smaller than the manufacturing facility for an actual product.

[0009] In the above-mentioned invention, at least the metal structure and mechanical strength of the processed test piece may be analyzed, and the temperature control and the accumulated equivalent plastic strain in the hot working process may be evaluated. According to this feature, by analyzing the metal structure and mechanical strength, the hot working process can be evaluated even in a small-scale experimental facility.

[0010] In the above-mentioned invention, the rod-shaped test piece may be characterized in that it is unidirectionally solidified to give the metal structure. Also, the rod-shaped test piece may be characterized in that it is produced by melting an alloy in a crucible placed inside a heating furnace, moving the crucible vertically at a predetermined speed, and pulling it out of the heating furnace to unidirectionally solidify it to give the metal structure. With this feature, the hot working process can be evaluated more easily even in a small-scale experimental facility.

[0011] The alloy ingot produced in the crucible may be cut to obtain the rod-shaped test piece by cutting the outer periphery of the ingot over an area ratio of 80% or more of the cross section perpendicular to the longitudinal direction. This feature makes it possible to use small-scale experimental equipment including the crucible and to evaluate the hot working process while maintaining a high yield of test pieces.

[0012] In the above-mentioned invention, the hot-worked product may be made of a precipitation-hardened Ni alloy. In addition, in the processing simulation process, the heating control may be performed at a temperature of 980°C or higher, and the strain control may be performed so that the accumulated equivalent plastic strain is 5 or more. According to this feature, it is possible to evaluate the hot working process of a precipitation-hardened Ni alloy that can be used for a large hot-worked product using a small-scale experimental facility. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a flow diagram of an evaluation method for a hot working process. [Diagram 2] FIG. 2 is a side cross-sectional view of a directional solidification apparatus used for casting ingots for test pieces. [Diagram 3]FIG. 2 is a side view of a main part of a hot working reproduction test device used in a test piece working simulation process. [Figure 4] FIG. 1(a) is a top view showing a simulated part, and FIG. 1(b) is a graph showing the temperature and strain history during hot working. [Diagram 5] 1 is a graph showing the relationship between the cooling rate during casting of a test piece ingot and SDAS. [Figure 6] 1A is a structural photograph of a longitudinal cross section of a test specimen ingot, and FIG. 1B is an enlarged photograph of the same. [Figure 7] 1 is a bar graph showing the 0.2% proof stress and tensile strength in tensile tests at (a) room temperature and (b) elevated temperatures, expressed as the ratio of the worked test piece to the hot worked (rolled) product. [Figure 8] The grain sizes of the processed test pieces and hot-processed (rolled) products and micrographs taken at the time of measurement. [Figure 9] 1 is a bar graph showing the 0.2% proof stress and tensile strength in tensile tests at (a) room temperature and (b) elevated temperatures, expressed as the ratio of the worked test piece to the hot worked (forged) product. [Figure 10] The grain sizes of processed test pieces and hot-processed (forged) products and micrographs taken at the time of measurement. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] A method for evaluating a hot working process will be described as one embodiment of the present invention.

[0015] In summary, this is a method for evaluating the hot working process in the manufacturing process of large hot-worked products that are made into products through casting and hot working, in which a specific location (referred to as the "reference location") in the hot-worked product is selected, and a rod-shaped test piece is prepared that has a metal structure simulating a portion of the ingot after casting that will provide the reference location (referred to as the "reference corresponding location"). A hot pressing test is performed on this test piece to obtain physical property data, which will be used to evaluate the manufacturing parameters of the hot working process in the manufacture of the actual product. The details will be explained further.

[0016] As shown in FIG. 1, first, a test piece is prepared (S1: test piece preparation step).

[0017] In the preparation of test pieces, first, an ingot for the test piece is cast. Here, the ingot for the test piece to be cast is prepared so as to obtain a metal structure simulating the metal structure of a reference corresponding portion, which is a portion of the ingot before hot working of a large hot-worked product (hereinafter simply referred to as a hot-worked product) that is an actual product. The reference corresponding portion is a portion of the ingot before hot working (hereinafter simply referred to as an ingot) that provides the reference portion, which is a portion of the hot-worked product.

[0018] For example, the cooling rate during solidification varies depending on the position of the reference corresponding portion in the ingot, and the metal structure obtained varies for each reference corresponding portion. Therefore, the ingot for the test piece is solidified by controlling the temperature of a molten metal made of an alloy with a predetermined composition so as to obtain a metal structure simulating the reference corresponding portion. For example, the cooling rate is adjusted to prepare the ingot for the test piece so as to have microsegregation corresponding to the metal structure of the reference corresponding portion. In addition, when the composition of the alloy is significantly different depending on the position of the reference corresponding portion due to the influence of macrosegregation in the ingot, the composition of the molten metal for obtaining the ingot for the test piece is also prepared to correspond to the significant difference.

[0019] It is assumed that the component composition and metal structure of the reference corresponding part of the ingot are known from past investigations, but values ​​obtained by numerical analysis of the cooling rate, etc. may be used. In other words, the cooling rate of the reference corresponding part is obtained by numerical analysis, and then the cooling rate during casting of the ingot for the test piece is adjusted to this cooling rate or multiplied by a predetermined coefficient. This also makes it possible to cast an ingot for the test piece having a metal structure simulating the reference corresponding part.

[0020] In order to obtain such a metal structure, it is preferable to cast the ingot for test piece by unidirectional solidification in the longitudinal direction, for example. By unidirectional solidification, the cooling rate can be adjusted to correspond to the cooling rate of the reference corresponding part, and a metal structure simulating the reference corresponding part can be easily generated. For example, by slowing the cooling rate, the growth of dendrites as microsegregation can be promoted, or by increasing the cooling rate, the growth of dendrites can be suppressed. In other words, the solidification forms of the part close to the surface layer or the central part of the ingot can be simulated, and microsegregation simulating each of them can be obtained. As described above, by adjusting the cooling rate and performing unidirectional solidification, the ingot for test piece can be given a solidification similar to the solidification of the reference corresponding part of the ingot, and an equivalent metal structure can be generated.

[0021] It is also preferable that the ingot for the test piece is made to have uniform microsegregation throughout. Whether the microsegregation is uniform or not can be determined, for example, by the secondary dendrite arm spacing (SDAS) of the ingot for the test piece. In general, the SDAS ([center SDAS]) of the center where the cooling rate is slow is wide, and the SDAS ([surface SDAS]) of the vicinity of the surface where the cooling rate is fast is narrow. Therefore, for example, by setting [surface SDAS] / [center SDAS]×100% to 90% or more, it can be determined that the microsegregation is uniform. It may also be determined by the cooling rate of the center and the vicinity of the surface of the ingot for the test piece during casting. For example, it can be determined that uniform microsegregation has been obtained by setting [cooling rate of the center] / [cooling rate of the surface layer]×100% to 90% or more. In this case, the cooling rate can be obtained by simulation or the like, but it is preferable to calculate it based on the obtained SDAS.

[0022] In addition, since deformation occurs due to hot working from the ingot to the hot worked product, it is also preferable to obtain a reference corresponding portion (position) of the ingot that corresponds to a reference portion of the hot worked product by numerical analysis.

[0023] For example, referring to FIG. 2 as well, the above-mentioned test piece ingot can be obtained by a unidirectional solidification apparatus 10. The unidirectional solidification apparatus 10 includes a bottomed, substantially cylindrical crucible 1. The crucible 1 contains a molten alloy 2 in which an alloy having a predetermined composition is melted. A slag 3 for heat retention is further appropriately placed above the molten alloy 2. The crucible 1 is contained in a refractory container 5, and the gap between the crucible 1 and the container 5 is filled with backsand 4. The crucible 1 and the container 5 are then placed in a heating furnace 6 using a substantially cylindrical susceptor (heating body). This allows the molten alloy 2 to be heated together with the crucible 1 and the temperature to be controlled. Thermocouples (not shown) are placed at a plurality of positions at different heights around the crucible 1, allowing temperature measurement for temperature control.

[0024] In the unidirectional solidification apparatus 10, the molten alloy 2 is heated by the heating furnace 6, while the crucible 1 is moved vertically downward at a predetermined speed, so that the molten alloy 2 can be drawn from the inside to the outside of the heating furnace 6. By unidirectionally solidifying the molten alloy 2 while adjusting the drawing speed, for example, dendrite arms are generated while being controlled to obtain an ingot for a test piece having a metal structure with uniform microsegregation. Here, the drawing speed is determined so as to correspond to the cooling speed of a reference corresponding portion of the ingot, thereby obtaining a metal structure simulating the reference corresponding portion.

[0025] Then, the obtained ingot for test piece is machined to cut out a test piece. At this time, the dimensions of the ingot for test piece are preferably such that the area of ​​the cross section in the direction perpendicular to the longitudinal direction of the test piece is 80% or more of the same area of ​​the ingot for test piece. In other words, the shape of the ingot for test piece is preferably close to the shape of a test piece with a set size used for the pressing process described later, so that a high yield can be maintained. For example, when a test piece is obtained by skin scraping to remove the black skin, if 10% of the radius of the ingot for test piece is removed from the outer periphery, the cross-sectional area of ​​the test piece is 81% of the cross-sectional area of ​​the ingot for test piece. In addition, by increasing the yield, the amount of molten metal used for the ingot for test piece can be minimized, and macrosegregation can be suppressed, which also contributes to obtaining a uniform metal structure. In addition, the machining to cut out the test piece may be performed after the obtained ingot for test piece is heat treated.

[0026] Next, the test piece is subjected to a pressing process in which the test piece is pressed from the side so as to be elongated in the longitudinal direction while controlling the temperature, which is equivalent to hot working such as hot forging and hot rolling to obtain a hot worked product (S2: processing simulation process). In the hot working process of the hot worked product, the ingot is hot worked while controlling the temperature until a predetermined accumulated equivalent plastic strain is reached. Therefore, in the processing simulation process of the test piece, heating control and strain control corresponding to the temperature control and the predetermined accumulated equivalent plastic strain are performed.

[0027] 3, in the processing simulation step (S2), it is preferable to use a hot processing reproduction test device 20 that can simultaneously perform temperature control and pressing while holding a test piece. The hot processing reproduction test device 20 includes an upper anvil 11a and a lower anvil 11b for pressing the test piece 21 from above and below, a pair of chuck jigs 12 for holding the test piece 21, a saddle coil 13 for heating the test piece 21, and a two-color thermometer (not shown) for measuring the temperature of the test piece 21.

[0028] The test piece 21 has handles 22 welded to both longitudinal end faces for holding it in the chuck jig 12. That is, the chuck jig 12 can hold the test piece 21 by gripping the handles 22 at both ends of the test piece 21. The chuck jig 12 is designed to rotate the test piece 21 around a rotation axis parallel to the longitudinal direction and hold it at a predetermined angle. This allows the rotation of the test piece 21 around the rotation axis and the holding angle to be controlled, and the test piece 21 can be heated uniformly in the circumferential direction even when heated by the saddle coil 13. In addition, by rotating the test piece 21, it is possible to control the pressure from above and below so that the pressure is applied from any angle around the axis.

[0029] Furthermore, the saddle coil 13 is shaped like a spiral coil with a large central opening, with both ends bent downward, and is disposed so as to straddle the test piece 21. This allows the saddle coil 1 to control the temperature by high-frequency heating of the test piece 21 without interfering with the pressing of the test piece 21 by the upper anvil 11a and the lower anvil 11b.

[0030] As described above, in the processing simulation step (S2), the test piece 21 is pressed, and by using the hot processing reproduction test device 20 that heats and presses the test piece in the same device, the conditions of the pressing can be easily adjusted. For example, it is relatively easy and preferable to perform pressing while simulating the processing history in hot processing of a reference portion of a hot-worked product. Here, the test piece is pressed by performing heating control and strain control corresponding to the processing history including the temperature control and accumulated equivalent plastic strain given to the reference corresponding portion of the ingot by the hot processing step to obtain a hot-worked product.

[0031] For example, when evaluating the hot working process of a hot worked product made of a precipitation strengthened Ni alloy, which is often used in hot worked products, the test piece is a Ni alloy with the same composition. When such a Ni alloy is used, it is preferable to perform press working while maintaining high deformability by dissolving precipitates while controlling the temperature in a temperature range of, for example, 800°C or higher, preferably 980°C or higher, as in the hot working process of such a hot worked product. In addition, when such a hot worked product is a bar steel by rolling, and a cumulative equivalent plastic strain of 3 or more is given, it is also preferable to control the strain in the working simulation process (S2) so as to give an equivalent cumulative equivalent plastic strain of 3 or more. Similarly, when a cumulative equivalent plastic strain of 5 or more is given to a hot worked product, it is also preferable to give an equivalent cumulative equivalent plastic strain of 5 or more in the working simulation process (S2).

[0032] For example, as shown in FIG. 4(a), a cylindrical ingot 30 is assumed to have a reference corresponding portion 31 near the surface and a reference corresponding portion 32 near the center. In this case, when hot working is performed by pressing from the periphery and rolling, the reference corresponding portion 31 near the surface has a large processing strain (including accumulated equivalent plastic strain) and the temperature drops quickly, as shown in FIG. 4(b). On the other hand, the reference corresponding portion 32 near the center has a small processing strain and the temperature drops slowly. In the processing simulation step (S2) of the test piece 21, the difference in processing history due to the reference corresponding portion that results in such temperature and processing strain is taken into consideration. In other words, the pressing processing of the test piece corresponding to each of the reference corresponding portions 31 and 32 is performed individually so that the temperature control and strain control given to the test piece are different in accordance with the difference in processing history. The history of temperature and processing strain imparted to each reference corresponding portion of the hot-worked product in the hot-working process may be based on empirical rules based on past manufacturing results, but it is also preferable to determine it by numerical analysis using the finite element method.

[0033] It is also preferable that the pressing process in the processing simulation step (S2) includes a step of rotating the test piece 21 around the rotation axis and pressing the side of the test piece 21 at each predetermined rotation angle. This makes it possible to give the test piece 21 a complex processing history that is similar to the processing history including temperature control and accumulated equivalent plastic strain in the hot processing step in the reference corresponding portion of the hot-worked product.

[0034] Finally, the test piece 21 is pressed to obtain a processed test piece, which is then cooled and used to perform analysis and evaluate the hot working process of the hot worked product (S3: evaluation process). If necessary, the processed test piece is machined into a test piece for measuring physical properties, and structure observation and mechanical testing are performed.

[0035] In the analysis of the processed test piece, for example, the component composition, metal structure, mechanical strength, etc. are investigated and measured to obtain physical property data. At this time, a combination is obtained that links the processing history, including at least the temperature control and accumulated equivalent plastic strain of the hot processing process corresponding to the simulated processing process of the test piece, with the physical property data. The processing history may also include the history of other things that affect the physical properties during the manufacturing process, such as heat treatment. Then, the hot processing process is evaluated based on the physical property data corresponding to the reference part of the hot processed product corresponding to such processing history. In other words, a processed test piece is manufactured by giving a processing history corresponding to the reference part of the hot processed product, and its physical properties are investigated and measured, and this is obtained as the physical property data corresponding to the physical properties of the reference part.

[0036] Then, the processing history of the hot working process is judged to be valid or not depending on whether the physical property data is a predetermined physical property. In other words, it is judged whether at least the temperature control and the accumulated equivalent plastic strain included in the processing history are valid or not. It may also be judged whether other manufacturing parameters included in the processing history are valid or not. Alternatively, it may be judged whether at least the temperature control and the accumulated equivalent plastic strain of the hot working process are valid or not depending on whether the predicted physical property matches the specifications of the hot worked product by predicting the physical property of the reference part from the physical property data. Note that the processed test piece does not completely reproduce the processing history of the reference part of the hot worked product, and may be processed under conditions that have differences with respect to the processing history of the hot worked product. Therefore, in consideration of such differences, the obtained physical property may be multiplied by a coefficient, or the physical property used as the standard for judgment may be given a range.

[0037] In addition, it is also preferable to heat-treat the test piece 21 to prepare a processed test piece in a process before and / or after the processing simulation process (S2) so as to match the manufacturing process of the hot-worked product. In other words, it is preferable to give the processing history of the test piece closer to the processing history of the hot-worked product.

[0038] [Manufacturing test] Next, the results of a test in which the physical properties of the hot-worked product produced by the hot-working process to be evaluated and test pieces produced by the above-mentioned method were compared will be described.

[0039] First, we investigated the ingots for obtaining hot-worked products and the ingots for test pieces produced corresponding to them. The ingots for obtaining hot-worked products were φ440mm×H1500mm ingots made of precipitation-strengthened Ni alloy (alloy equivalent to Alloy718) melted by vacuum arc remelting (VAR).

[0040] On the other hand, the ingot for the test piece was obtained as follows. 700 g of Ni alloy having the same composition as above was charged into the crucible 1 (see FIG. 2) of the unidirectional solidification device 10, heated to 1450°C, and held at the same temperature. 30 g of Al2O3 was further charged from the top as slag 3 for heat retention, and the temperature was held isothermal for another 10 minutes. While maintaining the current flow to the heater of the heating furnace 6 at a constant current, the crucible 1 was pulled down at a predetermined speed, and the ingot for the test piece was obtained after being cooled and solidified. The dimensions of the ingot for the test piece were determined by the inner dimensions of the crucible 1, and here, they were set to φ30 mm × H120 mm. The withdrawal speed (predetermined speed) of the crucible 1 was set to five speeds: 0.3, 0.6, 1.2, 3.0, and 15 mm / min, and the cooling speed during solidification was calculated for each speed using JMatPro (registered trademark) ver. 11 (manufactured by Sente Software). The cooling speed was determined within the solid-liquid range (1365 to 1160 ° C) obtained by the Scheil equation. Furthermore, a cross section (longitudinal cross section) parallel to the dendrite growth direction (longitudinal direction) of the obtained ingot for test piece was observed with an electron probe microanalyzer (EPMA) to determine the secondary dendrite arm spacing (SDAS). The SDAS was also determined in the same manner for the reference corresponding portion of the ingot.

[0041] As shown in Fig. 5, the SDAS decreases monotonically with respect to the calculated cooling rate. In other words, it was found that the SDAS can be controlled by the cooling rate of the molten alloy when producing the ingot for the test piece, and further by the speed at which the crucible 1 is withdrawn. This makes it possible to make the SDAS of the ingot for the test piece equal to the SDAS of the ingot for the hot worked product, for example.

[0042] As shown in Fig. 6(a), it was observed that a uniform metal structure was obtained in the cross-sectional structure of the ingot for the test piece when the drawing speed was 0.6 mm / min. As shown in Fig. 6(b), it was also observed that the primary dendrite arms extended in the vertical direction, which was the solidification direction.

[0043] Next, similarly manufactured ingots for test pieces were pressed using the hot working reproduction test device 20 to obtain processed test pieces, which were then subjected to mechanical testing. The results are then compared with the results of the mechanical testing of the hot worked products.

[0044] First, a comparison between a rolled product produced by rolling as a hot worked product and a processed test piece produced corresponding to the rolled product will be described.

[0045] Here, a test piece ingot having dimensions that allow cutting out a test piece of φ50 mm × L170 mm was used. The material was a Ni alloy equivalent to Alloy 718. In addition, the calculation of [Surface SDAS] / [Center SDAS] × 100% for this test piece ingot was 128.2 (μm) / 127.7 (μm) × 100% = 100.4%. In other words, this test piece ingot had a uniform microsegregation metal structure. The hot-worked products (rolled products) were also made of the same Ni alloy, and were round bars with two different diameters, large and small, manufactured by hot working and heat treatment. The reference parts were the centers of the hot-worked products of each diameter.

[0046] The ingots for the test specimens were machined into round bars of φ50 mm × L170 mm after soaking (homogenization heat treatment) to prepare the test specimens, and handles were welded to both longitudinal ends. The test specimens with the handles attached were pressed using a hot processing reproduction test device 20 to obtain a processing history including temperature control and accumulated equivalent plastic strain equivalent to that of the reference part of the hot processing product. In the pressing process, the sides were pressed from two directions at every 90 degree rotation angle to form a square bar with a cross section of 15 mm × 15 mm and a length of 270 mm. Then, the test specimens were solution heat treated to prepare processed test specimens. Test specimens for mechanical testing were cut out from the processed test specimens and subjected to mechanical testing. Grain size measurements were also performed.

[0047] As shown in Figure 7, tensile tests were performed at room temperature (RT) and at high temperature at 650°C. As a result, the ratios of the 0.2% proof stress and tensile strength of the processed test pieces to the hot-worked products are shown in the figure. For both small and large round bars, and at both room and high temperatures, the ratios were all within the range of 0.95 to 1.05. In other words, the 0.2% proof stress and tensile strength of the processed test pieces to the hot-worked products by rolling were close to each other, within ±5%.

[0048] In addition, as shown in Fig. 8, the average grain size in the processed test pieces was close to that of the two hot-processed products, large and small, and the grain size numbers were similar. In other words, the metal structure of the test pieces after pressing was equivalent to that of the rolled product after hot processing.

[0049] Next, a comparison will be made between a forged product produced by free forging as a hot worked product and a processed test piece produced corresponding to the forged product.

[0050] Here, the forged products were round bars of one diameter, and Ni alloy equivalent to Alloy718 (hereafter referred to as Alloy718) and Ni alloy equivalent to Alloy706 (hereafter referred to as Alloy706) were used as materials. The high-temperature tensile test was performed at 650°C for Alloy718, the same as above, but at 400°C for Alloy706. The rest was the same as in the case of the rolled products.

[0051] As shown in Figure 9, the results of the tensile test show the ratios of the 0.2% proof stress and tensile strength of the processed test pieces to the hot-worked products. For both Alloy706 and Alloy718, and at both room temperature and high temperature, the ratios were all within the range of 0.95 to 1.05. In other words, the 0.2% proof stress and tensile strength of the processed test pieces to the hot-worked products by forging were close to each other, within ±5%.

[0052] In addition, as shown in Fig. 10, the average grain size of the processed test piece was close to that of the hot-worked products made of the two Ni alloys. In other words, the metal structure of the test piece after pressing was equivalent to that of the forged product after hot working.

[0053] As described above, according to the method for evaluating the hot working process of this embodiment, a test piece is used that has a metal structure simulating a part of an ingot to reflect the casting process, and therefore, it has been shown that the hot working process can be easily evaluated using experimental equipment smaller than the manufacturing equipment for the actual product. For the evaluation of the hot working process, for example, the manufacturing parameters of the hot working process in the hot working product can be evaluated using physical property data obtained by analyzing a processed test piece produced by pressing the test piece. This makes it possible to determine the manufacturing parameters. Furthermore, at least in the above-mentioned manufacturing test, physical properties close to those of the hot working product could be obtained from the processed test piece. In other words, it can be said that it is also possible to predict the physical properties of the reference portion of the hot working product from the physical property data obtained by pressing the test piece.

[0054] Although the representative embodiments of the present invention and modified examples based thereon have been described above, the present invention is not necessarily limited to these, and a person skilled in the art will be able to find various alternative embodiments and modified examples without departing from the spirit of the present invention or the scope of the appended claims. [Explanation of symbols]

[0055] 1 crucible 2 Molten alloy 6 Furnace 10 Unidirectional solidification equipment 20. Hot working simulation test equipment 21 Test Pieces

Claims

1. A method for evaluating a hot working process in a manufacturing method of a hot worked product, the hot working process being a step of hot working an ingot until a predetermined accumulated equivalent plastic strain is reached while controlling the temperature, comprising the steps of: In order to evaluate the hot working process, a processed test piece obtained by a processing simulation process in which a rod-shaped test piece having a metal structure simulating a part of the ingot is pressed from the side to be elongated in the longitudinal direction is analyzed, The method for evaluating a hot working process, wherein the working simulation process includes performing the temperature control and heating control and strain control corresponding to the predetermined accumulated equivalent plastic strain.

2. 2. The method for evaluating a hot working process according to claim 1, further comprising the steps of: analyzing at least the metal structure and mechanical strength of the worked test piece; and evaluating the temperature control and the accumulated equivalent plastic strain in the hot working process.

3. 2. The method for evaluating a hot working process according to claim 1, wherein the rod-shaped test piece is provided with the metal structure by unidirectional solidification.

4. The method for evaluating a hot working process according to claim 3, characterized in that the rod-shaped test piece is prepared by melting an alloy in a crucible placed inside a heating furnace, moving the crucible vertically at a predetermined speed, and pulling the alloy out of the heating furnace to solidify it in one direction to give the metal structure.

5. The method for evaluating a hot working process according to claim 4, characterized in that the outer periphery of the alloy ingot produced in the crucible is machined over an area ratio of 80% or more of the cross section perpendicular to the longitudinal direction to form the rod-shaped test piece.

6. 6. The method for evaluating a hot working process according to claim 1, wherein the hot worked product is made of a precipitation strengthened Ni alloy.

7. 7. The method for evaluating a hot working process according to claim 6, wherein in the working simulation process, the heating control is performed at a temperature of 800° C. or higher, and the strain control is performed so that the accumulated equivalent plastic strain is 3 or more.

Citation Information

Patent Citations

  • Solidification simulation device and method therefor