LIQUID DISCHARGE HEAD AND METHOD FOR MANUFACTURING LIQUID DISCHARGE HEAD

By using different materials and thicknesses for the flow path and discharge port forming members, particularly polyetheramide resins, the liquid ejection head's reliability is enhanced by preventing ink penetration and substrate separation.

JP7551296B2Active Publication Date: 2024-09-17CANON KK
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020003024
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-01-10
Publication Date
2024-09-17
Estimated Expiration
2040-01-10

AI Technical Summary

Technical Problem

The use of high-boiling-point solvents in inks leads to increased permeation of the photosensitive resin layer, causing deformation and potential separation of the flow path forming member from the substrate, compromising the reliability of the liquid ejection head.

Method used

The flow path forming member and the discharge port forming member are made of different materials, with the flow path forming member being thicker than the discharge port forming member, and utilizing polyetheramide resin, polyetherimide resin, or polyetheramideimide resin to prevent ink penetration.

Benefits of technology

This design effectively prevents ink penetration, ensuring high reliability by suppressing separation of the flow path forming member from the substrate, even with highly permeable inks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551296000012
    Figure 0007551296000012
  • Figure 0007551296000011
    Figure 0007551296000011
  • Figure 0007551296000010
    Figure 0007551296000010
Patent Text Reader

Abstract

To provide a liquid ejection head in which peeling of a flow passage forming member from a base plate can be suppressed by preventing liquid from penetrating into the flow passage forming member even when highly permeable liquid is used, and which therefore can secure high reliability, and a manufacturing method of a liquid ejection head.SOLUTION: A liquid ejection head is provided, comprising: a base plate; a flow passage forming member provided on a base plate surface of the base plate and forming a liquid flow passage; and an ejection port forming member provided on the flow passage and having an ejection port ejecting liquid. The ejection port forming member and the flow passage forming member are formed of different materials. In a direction perpendicular to the surface of the base plate, a thickness of the flow passage forming member is larger than a thickness of the ejection port forming member. The ejection port forming member is a hardened material of a photosensitive resin composition, and the flow passage forming member contains at least one resin selected from a group comprised of polyether amide resin, polyether imide resin and polyether amide-imide resin.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a liquid ejection head and a method for manufacturing a liquid ejection head. [Background technology]

[0002] A liquid ejection head is used in a liquid ejection device such as an inkjet recording device, and has a flow path forming member and a substrate. The flow path forming member is provided on the substrate and forms a liquid flow path. The substrate has a liquid supply port formed therein, and has energy generating elements on the surface side. The liquid is supplied to the flow path from a liquid supply port, energy is given to the liquid by an energy generating element, and the liquid is ejected from a liquid ejection port of an ejection port forming member provided on the flow path forming member, and lands on a recording medium such as paper. In addition, an inorganic material layer is often provided on the substrate as an insulating layer or a protective layer for covering the energy generating elements, or for various other purposes. On the other hand, it is known to form flow path forming members and other structures on the substrate with an organic material layer. In particular, when the organic material layer is formed with a photosensitive resin, it can be formed with high precision by photolithography.

[0003] For example, in the method of manufacturing a liquid ejection head described in Patent Document 1, a dry film of a photosensitive resin layer that becomes a liquid flow path is formed on a substrate having an inorganic material layer by a lamination method, and exposed to light in the shape of the flow path. Next, a dry film of a photosensitive resin layer that becomes a nozzle portion connecting the ejection port and the flow path and a discharge port is laminated on the photosensitive resin layer that becomes the flow path, and after exposure to light in the shape of the discharge port, the uncured portions of each photosensitive resin layer are removed all at once by development to form the flow path, the nozzle portion, and the discharge port. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-018272 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, for example, as the demands for inkjet image recording become more sophisticated, the performance required for inks also becomes more sophisticated, and there are increasing opportunities to add high-boiling point solvents to inks from the viewpoint of fixation to recorded matter. The ink thus obtained may permeate into a photosensitive resin layer made of an epoxy resin or the like, and may cause deformation of the flow passage forming member. Therefore, when this type of ink is used, in the configuration of Patent Document 1, it is conceivable that deformation of the flow path forming member will progress at a faster pace than with conventionally used ink types, and there is room for improvement in terms of long-term reliability. For example, when the inkjet head is used for a long period of time, the flow path forming member may peel off from the substrate, or the desired ink ejection performance may not be obtained. The present disclosure provides a liquid ejection head and a method for manufacturing a liquid ejection head that can prevent the flow path forming member from peeling off from the substrate by preventing the liquid from penetrating into the flow path forming member even when a highly permeable liquid is used, thereby ensuring high reliability. [Means for solving the problem]

[0006] The present disclosure relates to A liquid ejection head comprising: a substrate; a flow path forming member provided on the substrate and forming a flow path for liquid; and an ejection port forming member provided on the flow path forming member and having an ejection port for ejecting liquid, the discharge port forming member and the flow path forming member are formed of different materials, a thickness of the flow path forming member is greater than a thickness of the discharge port forming member in a direction perpendicular to the substrate surface; the discharge port forming member is a cured product of a photosensitive resin composition, The present invention relates to a liquid ejection head, wherein the flow path forming member contains at least one resin selected from the group consisting of polyetheramide resins, polyetherimide resins, and polyetheramideimide resins.

[0007] The present disclosure also provides A method for manufacturing a liquid ejection head including: a substrate; a flow path forming member provided on the substrate and forming a flow path for liquid; and an ejection port forming member provided on the flow path forming member and having an ejection port for ejecting liquid, the method comprising the steps of: forming a flow path forming member for forming a liquid flow path on the substrate; forming a discharge port forming member having a discharge port for discharging a liquid on the flow path forming member, the discharge port forming member and the flow path forming member are formed of different materials, a thickness of the flow path forming member is greater than a thickness of the discharge port forming member in a direction perpendicular to the substrate surface; the discharge port forming member is a cured product of a photosensitive resin composition, The present invention relates to a method for producing a liquid ejection head, wherein the flow path forming member contains at least one resin selected from the group consisting of polyetheramide resins, polyetherimide resins, and polyetheramideimide resins. Effect of the Invention

[0008] According to the present disclosure, even when a highly permeable liquid is used, by preventing the liquid from penetrating into the flow path forming member, peeling of the flow path forming member from the substrate can be suppressed, thereby providing a liquid ejection head and a manufacturing method thereof that ensure high reliability. [Brief description of the drawings]

[0009] [Figure 1] 1A is a schematic perspective view showing an example of the configuration of a liquid ejection head, and FIG. 1B is a schematic cross-sectional view taken along line AA' in FIG. [Diagram 2] Schematic cross-sectional view showing an example of a method for producing a resin structure. [Diagram 3] Schematic cross-sectional views showing an example of a manufacturing method for a liquid ejection head [Figure 4] Schematic cross-sectional views showing an example of a manufacturing method for a liquid ejection head [Diagram 5]Schematic cross-sectional views showing an example of a manufacturing method for a liquid ejection head DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, with reference to the drawings, specific examples of the embodiments for carrying out this disclosure will be described. However, the dimensions, materials, shapes, and relative positions of the components described in these embodiments should be appropriately changed depending on the configuration of the member to which the disclosure is applied and various conditions. In other words, it is not intended to limit the scope of this disclosure to the following embodiments. In addition, in this disclosure, the description of "XX or more and YY or less" or "XX to YY" representing a numerical range means a numerical range including the endpoints, that is, the lower limit and the upper limit, unless otherwise specified. Furthermore, when a numerical range is described in stages, the upper and lower limits of each numerical range can be combined in any manner. In the following description, components having the same functions are given the same reference numbers in the drawings, and descriptions thereof may be omitted.

[0011] Fig. 1(A) is a schematic perspective view showing an example of the configuration of a liquid ejection head. Fig. 1(B) is a schematic perspective view of the liquid ejection head as viewed from a plane perpendicular to a substrate, passing through A-A' in Fig. 1(A). FIG. 1 has a substrate 1 on which energy generating elements 2 that generate energy for discharging liquid are formed at a predetermined pitch. The substrate 1 is made of, for example, silicon. Examples of the energy generating element 2 include an electrothermal conversion element and a piezoelectric element. The energy generating element 2 may be provided so as to be in contact with the surface of the substrate 1, or may be provided partially hollow relative to the surface of the substrate 1. A control signal input electrode (not shown) for operating the energy generating element 2 is connected to the energy generating element 2. The substrate 1 is also provided with a supply port 3 for supplying liquid such as ink.

[0012] An inorganic material layer 4 and a protective layer 5 are formed on the surface side of the substrate 1. The substrate 1 may be a silicon substrate made of silicon. The silicon substrate is preferably a single crystal of silicon, and the crystal orientation of the surface is preferably (100). The inorganic material layer 4 may be a silicon oxide (SiO 2 ), silicon nitride (SiN), silicon carbide (SiC), silicon carbonitride (SiCN), silicon carbonate (SiOC), etc. In Fig. 1, the inorganic material layer 4 is used as a heat storage layer or an insulating layer. The protective layer 5 protects the energy generating element and is formed of, for example, Ta or Ir. The inorganic material layer 4 may cover the energy generating element.

[0013] In Fig. 1, the inorganic material layer 4 is formed on almost the entire surface (substrate surface 20) of the substrate 1. A flow path 7 is formed on the inorganic material layer 4 by a flow path forming member 6 that is provided on the substrate surface 20 of the substrate 1 and forms a liquid flow path. Furthermore, a discharge port forming member 10 is formed on the flow path forming member 6 and has a discharge port 8 for discharging liquid. The discharge port forming member 10 has a liquid flow path (nozzle portion 9) that communicates with the discharge port 8. Furthermore, a liquid repellent layer 11 is formed on the discharge port forming member 10 as necessary. In this liquid ejection head, liquid such as ink is supplied from a supply port 3 through a flow path 7, and by applying pressure generated by an energy generating element 2, the liquid is ejected as droplets from an ejection port 8 via a nozzle portion 9.

[0014] Next, a specific example of a manufacturing method for a liquid ejection head will be described with reference to FIGS. FIG. 2 shows an example of a method for producing a resin structure that forms a flow path forming member and contains at least one resin selected from the group consisting of polyetheramide resins, polyetherimide resins, and polyetheramideimide resins. Fig. 3 is a schematic cross-sectional view showing an example of a method for manufacturing a liquid ejection head. Here, an example of a method for manufacturing an inkjet head is shown. Fig. 3 shows a cross-sectional structure of a completed liquid ejection head, as seen from a plane perpendicular to the substrate, similar to Fig. 1(B).

[0015] First, as shown in Fig. 2(a), a film 12 made of polyethylene terephthalate (PET), polyimide, etc. is prepared. Next, as shown in Fig. 2(b), at least one resin (flow path forming member resin 13) selected from the group consisting of polyetheramide resin, polyetherimide resin, and polyetheramideimide resin is applied to the film 12. The application method may be a spin coating method, a slit coating method, etc. After the application of the flow path forming member resin 13, pre-baking is performed to prepare a resin structure having the flow path forming member resin 13.

[0016] At least one resin (flow path forming member resin 13) selected from the group consisting of polyetheramide resin, polyetherimide resin, and polyetheramideimide resin is preferably a thermoplastic resin from the viewpoints of high heat resistance and high adhesion. The weight average molecular weight (Mw) of the polyetheramide resin, polyetherimide resin, and polyetheramideimide resin is preferably 5,000 to 100,000. It is more preferable that the number is 0,000 to 50,000. The weight average molecular weight (Mw) of the polyetheramide resin, polyetherimide resin and polyetheramideimide resin is preferably 100,000 or less from the viewpoints of resolution and solubility in a solvent, while it is preferably 5,000 or more from the viewpoints of coatability and filmability. Polyetheramide resins, polyetherimide resins and polyetheramideimide resins have good processability and low water absorption properties with respect to liquids, and are therefore suitable for use as flow path forming members in liquid ejection heads. The water absorption rate of the polyetheramide resin, polyetherimide resin and polyetheramideimide resin is preferably smaller than the water absorption rate of the cured product of the photosensitive resin composition.

[0017] Here, the flow path forming member is designed to be thicker than the ejection port forming member in the direction perpendicular to the substrate surface 20. This allows for good ejection characteristics, such as reducing droplets other than the main droplet during ejection. In the direction perpendicular to the substrate surface 20, the thickness of the resin 13 for the flow path forming member corresponds to the height of the flow path. The thickness of the resin 13 for the flow path forming member may be appropriately determined according to the ejection design of the liquid ejection head so as to be larger than the thickness of the ejection port forming member, and is preferably set to, for example, 3.0 μm to 25.0 μm. In addition, the thickness of the flow path forming member is more preferably set to 5.0 μm to 24.0 μm.

[0018] Specific manufacturing methods are described below, but are not limited to these. As shown in FIG. 3(a), a substrate 1 having energy generating elements 2 on its front surface (substrate surface 20 side) is prepared. 3(b), an inorganic material layer 4 is formed on the front surface side (on the substrate surface) of the substrate 1 so as to cover the energy generating elements 2. In addition, a protective layer 5 is formed above the energy generating elements 2. The inorganic material layer 4 and the protective layer 5 are patterned as necessary. 3(c), a supply port 3 is formed through the substrate to supply ink. The supply port 3 is formed at a desired position by wet etching using an alkaline etching solution such as TMAH (tetramethylammonium hydroxide) or dry etching such as reactive ion etching. 3(d), the resin structure having the flow path forming member resin 13 described in FIG. 2 is transferred onto the inorganic material layer 4 of the substrate 1 on which the energy generating elements 2 and the supply port 3 are arranged, by a lamination method to form a film. Thereafter, the film 12 is peeled off from the resin structure having the flow path forming member resin 13 by a peeling tape or the like. In the case of a substrate in which the supply port 3 is not arranged, the resin 13 for flow path forming members may be applied by spin coating or slit coating to form a film without using the resin structure.

[0019] Next, as shown in FIG. 3(e), a mask resist 14 is applied onto the flow path forming member resin 13, and is pattern-exposed through a flow path forming mask 15 having a flow path pattern, and developed to form an etching mask. 3(f), patterning is performed with oxygen plasma or the like to form a flow path forming member 6 and a flow path 7 of the liquid ejection head. The etching mask that is no longer necessary is removed with a remover or the like.

[0020] Next, as shown in FIG. 3(g), a photosensitive resin composition 16 is applied to a film made of PET, polyimide or the like, and then transferred onto the flow path forming member 6 by a lamination method to form a film. The photosensitive resin composition 16 that becomes the discharge port forming member 10 preferably contains a cationic polymerization type epoxy resin, taking into consideration the adhesion to the flow path forming member 6, mechanical strength, resolution, and the like.

[0021] The discharge port forming member may be made of at least one resin selected from the group consisting of polyetheramide resin, polyetherimide resin, and polyetheramideimide resin, which is the same as the flow path forming member. However, when a non-photosensitive resin is used, the resolution may be poor because the processing is performed by dry etching through a mask resist. Therefore, it is preferable to use a photosensitive resin composition containing a cationic polymerization type epoxy resin for the discharge port forming member. The photosensitive resin composition preferably contains a cationic polymerization type epoxy resin in view of the adhesion performance and mechanical strength of the cured product, the reactivity as a photolithography material, the resolution, and the like. Here, the epoxy resin is preferably a thermosetting resin having reactive epoxy groups at its terminals. Moreover, the photosensitive resin composition more preferably contains a cationically polymerizable epoxy resin having two or more epoxy groups in one molecule. Furthermore, the cationic polymerization type epoxy resin is preferably a photo-cationic polymerization type epoxy resin. In this case, the photosensitive resin composition preferably contains a photo-acid generator. Specific examples of photocationic polymerization type epoxy resins include resin compositions containing bisphenol A and F type epoxy resins; phenol novolac type epoxy resins; cresol novolac type epoxy resins; and polyfunctional epoxy resins having a norbornene skeleton, a terpene skeleton, a dicyclopentadiene skeleton, an oxycyclohexane skeleton, or the like. The photosensitive resin composition is preferably a negative composition, which becomes less soluble in a developer when exposed to light, and the exposed portion remains after development.

[0022] When the photosensitive resin composition contains a cationic polymerization type epoxy resin having two or more epoxy groups in one molecule, the cured product is three-dimensionally crosslinked, making it suitable for obtaining desired properties. Examples of the photoacid generator or photopolymerization initiator include a sulfonic acid compound, a diazomethane compound, a sulfonium salt compound, an iodonium salt compound, and a disulfone compound.

[0023] Two or more types of photoacid generators or photopolymerization initiators can be mixed and used. Furthermore, the photosensitive resin composition can contain a silane coupling agent for the purpose of improving adhesion performance. In addition, in order to improve pattern resolution and adjust sensitivity (exposure dose required for curing), the photosensitive resin composition can contain a sensitizer such as anthracene compounds, a basic substance such as amines, or an acid generator that generates weakly acidic (pKa=-1.5 to 3.0) toluenesulfonic acid.

[0024] The thickness of the ejection port forming member in the direction perpendicular to the substrate surface 20 may be appropriately determined depending on the ejection design of the liquid ejection head, but is preferably set to, for example, 3.0 μm to 25.0 μm from the viewpoint of mechanical strength, etc. Furthermore, the thickness of the ejection port forming member is more preferably set to 4.5 μm to 20.0 μm.

[0025] Next, as shown in FIG. 3(h), a liquid-repellent layer 11 is formed on the photosensitive resin composition 16. By forming the liquid-repellent layer 11 on the discharge port forming member, it is possible to reduce the water absorption of the discharge port forming member. The liquid-repellent layer 11 is required to have liquid repellency against liquids such as ink, and is preferably made of a perfluoroalkyl composition or a perfluoropolyether composition having cationic polymerization. In the present disclosure, the thickness of the liquid-repellent layer is not included in the thickness of the discharge port forming member. In general, it is known that in perfluoroalkyl compositions and perfluoropolyether compositions, fluorinated alkyl chains segregate at the interface between the composition and air upon baking treatment after application, making it possible to increase the liquid repellency of the surface of the composition.

[0026] Next, as shown in FIG. 3(i), a discharge port forming mask 17 having a discharge port pattern is used. The photosensitive resin composition 16 and the liquid repellent layer 11 are then exposed to pattern light. The exposed areas are then cured by a heat treatment (Post Exposure Bake) to form the discharge port forming member 10. The discharge port forming mask 17 is a substrate made of a material such as glass or quartz that transmits light of the exposure wavelength, on which a light-shielding film such as a chrome film is formed in accordance with the discharge port pattern. As the exposure device, a projection exposure device having a single wavelength light source such as an i-line exposure stepper or a KrF stepper, or a broad wavelength light source of a mercury lamp such as the mask aligner MPA-600Super (product name, manufactured by Canon) can be used.

[0027] Next, as shown in Fig. 3(j), the photosensitive resin composition 16 and the uncured portion of the liquid repellent layer 11 are developed with a developer to remove them all at once, forming the discharge port 8 and the nozzle portion 9, and then heat treatment is performed as necessary to complete the liquid discharge head. Examples of the developer include PGMEA (propylene glycol monomethyl ether acetate), MIBK (methyl isobutyl ketone), and xylene. If necessary, a rinse treatment using IPA (isopropyl alcohol) or the like may be performed. EXAMPLES

[0028] Hereinafter, the present disclosure will be described in detail with reference to examples and comparative examples, but the present disclosure is not limited to the configurations embodied in these examples. Furthermore, "parts" used in the examples and comparative examples means "parts by mass" unless otherwise specified.

[0029] <Example 1> First, as shown in FIG. 4(a), a PET film 12 having a thickness of 100 μm was prepared. Next, as shown in FIG. 4(b), a polyetheramide resin, HIMAL HL-1200CH (product name) manufactured by Hitachi Chemical (13 in FIG. 4(b)), was applied onto the PET film 12 by spin coating, and baked at 120° C. for 20 minutes to volatilize the solvent, forming a 5.0 μm film. Next, as shown in FIG. 4(c), a substrate 1 made of silicon having energy generating elements 2 made of TaSiN on its front surface side (substrate surface 20 side) was prepared. Next, as shown in Fig. 4(d), SiCN was deposited by plasma CVD as an inorganic material layer 4 to a thickness of 0.3 µm on the front surface of the substrate 1 so as to cover the energy generating elements 2. Then, Ta was formed by sputtering to a thickness of 0.25 µm as a protective layer 5. Furthermore, the inorganic material layer 4 and the protective layer 5 were patterned by photolithography and reactive ion etching.

[0030] Next, the supply port 3 was formed as shown in FIG. 4(e). The supply port 3 was formed by forming an etching mask having an opening using a positive photosensitive resin made of THMP-iP5700HP (manufactured by Tokyo Ohka Kogyo Co., Ltd.) and performing reactive ion etching through the opening of the etching mask. The reactive ion etching was performed by the Bosch process using an ICP etching device (manufactured by Alcatel, model number: 8E). After the supply port 3 was formed, the etching mask was removed using a stripping solution.

[0031] Next, as shown in Fig. 4(f), a polyetheramide resin layer (13 in Fig. 4(f)) was formed. Specifically, the PET film having the polyetheramide resin produced in Fig. 4(b) was transferred to the substrate 1 on which the energy generating elements 2 and the supply port 3 were arranged, while applying heat of 70°C and pressure using a lamination method. Thereafter, the PET film 12 was peeled off from the polyetheramide resin with a peeling tape (not shown). Next, as shown in FIG. 4(g), THMP-iP5700HP (manufactured by Tokyo Ohka Kogyo Co., Ltd.) is applied as a mask resist 14 from above the resin 13 for flow path formation members made of polyether amide resin, and pattern exposure is performed through a flow path formation mask 15 having a flow path pattern, and a development is performed. An etching mask was formed by imaging.

[0032] Next, as shown in Fig. 4(h), reactive ion etching was performed through the openings in the etching mask using an ICP etching device (manufactured by Alcatel, model number: 8E) to form a flow path forming member 6 and a flow path 7 of the liquid ejection head. After the flow path 7 was formed, the etching mask was removed using a stripping liquid. Next, as shown in FIG. 4(i), a photosensitive resin composition 16 was formed. First, a photosensitive resin composition 16 made of the composition materials shown in Table 1 below was applied onto a PET film having a thickness of 100 μm, and baked at 90° C. for 20 minutes to volatilize the solvent, forming a film having a thickness of 4.5 μm. Next, the photosensitive resin composition 16 was transferred and laminated onto the flow path forming member 6 made of the polyetheramide resin 13 while applying heat of 50° C. by using a lamination method.

[0033] [Table 1] In the table, jER157S70: Mitsubishi Chemical Corporation CPI-410S: San-Apro A-187: Momentive Performance Materials PGMEA: 2-Methoxy-1-methylethyl acetate

[0034] Next, a liquid-repellent layer 11 was formed as shown in Fig. 4(j). A condensate of a composition consisting of a compound represented by the following formula (1), glycidylpropyltriethoxysilane, and methyltriethoxysilane was diluted with 2-butanol and ethanol to form a fluorine-containing compound for forming the liquid-repellent layer. The fluorine-containing compound was applied onto the photosensitive resin composition 16 by a slit coating method, and heat-treated at 70°C for 3 minutes to volatilize the dilution solvent, thereby forming a liquid-repellent layer 11 with a thickness of 0.5 µm on the photosensitive resin composition 16.

[0035] [ka] (In formula (1), t is an integer of 3 to 10.)

[0036] Next, as shown in FIG. 4( k ), the photosensitive resin composition 16 and the liquid repellent layer 11 are exposed to light at 1100 J / m using an i-line exposure stepper (Canon, product name: i5) through a discharge port forming mask 17 having a discharge port pattern. 2 The exposed portion was then cured by performing a heat treatment at 90° C. for 5 minutes to form a discharge port forming member 10. Next, as shown in FIG. 4(l), the photosensitive resin composition 16 and the uncured portion of the liquid repellent layer 11 are removed by pressing. The resin was removed by developing with propylene glycol monomethyl ether acetate (PGMEA) for 10 minutes, thereby forming the ejection port 8 and the nozzle portion 9, which were then cured at 200° C. to obtain the liquid ejection head.

[0037] <Example 2> A liquid ejection head was produced in the same manner as in Example 1, except that a polyetheramideimide resin, HIMAL HL-1210CH (product name) manufactured by Hitachi Chemical Co., Ltd., was used for the flow path forming member.

[0038] <Comparative Example 1> A liquid ejection head was produced in the same manner as in the example, except that a flow path forming member was formed using a photosensitive resin composition made of the composition materials shown in Table 2 below.

[0039] First, as shown in FIG. 5(a), a PET film 12 having a thickness of 100 μm was prepared. Next, as shown in FIG. 5(b), a photosensitive resin composition 18 consisting of the composition materials shown in Table 2 below was applied onto a 100 μm-thick PET film 12, and baked at 90° C. for 20 minutes to volatilize the solvent, thereby forming a 5.0 μm-thick film. Next, in the same manner as in Example 1, a substrate having a supply port 3 was produced as shown in FIGS.

[0040] Next, as shown in Fig. 5(f), the PET film having the photosensitive resin composition 18 prepared in Fig. 5(b) was transferred to the substrate 1 on which the energy generating element 2 and the supply port 3 were arranged by applying heat of 70°C and pressure using a lamination method. After that, the PET film 12 was peeled off from the photosensitive resin composition 18 with a peeling tape (not shown). Next, as shown in FIG. 5( g ), the photosensitive resin composition 18 is exposed through a flow path forming mask 19 having a flow path pattern, using an i-line exposure stepper (Canon, product name: i5) at 4000 J / m 2 The exposed portion was then cured by performing a heat treatment at 90° C. for 5 minutes, thereby forming a side wall that would become the flow path forming member 6. Next, as shown in FIG. 5(h), the uncured portion of the photosensitive resin composition 18 was removed by developing with 2-methoxy-1-methylethyl acetate (PGMEA) for 10 minutes, thereby forming a flow path forming member 6 and a flow path 7. Next, as shown in FIG. 5(i), a photosensitive resin composition 16 was formed. First, photosensitive resin composition 16 made of the composition materials shown in Table 1 above was applied onto a PET film having a thickness of 100 μm, and baked at 90° C. for 20 minutes to volatilize the solvent, forming a film having a thickness of 4.5 μm. Next, the photosensitive resin composition 16 was transferred and laminated onto the flow path forming member 6 made of the photosensitive resin composition 18 by using a lamination method while applying heat of 50°C. The rest of FIG. 5(j) to (l) are the same as in the embodiment.

[0041] [Table 2] In the table, TECHMORE VG3101: Printec SP-172: Adeka Optomer SP-172 manufactured by ADEKA A-187: Momentive Performance Materials PGMEA: 2-Methoxy-1-methylethyl acetate

[0042] [evaluation] <Water absorption rate> The water absorption rates of the cured products of the resin and the photosensitive resin composition described in Examples 1 and 2 and Comparative Example 1 were evaluated by the following method. First, a silicon substrate was coated with HIMAL HL-1200CH (trade name: polyetheramide resin) manufactured by Hitachi Chemical Co., Ltd. and HIMAL HL-1210CH (trade name: polyetheramideimide resin) manufactured by Hitachi Chemical Co., Ltd., which were used in Examples 1 and 2. After coating, the substrate was baked at 120° C. for 20 minutes to volatilize the solvent, and a film of 5 μm was formed. Next, the cured product of the photosensitive resin composition used in Comparative Example 1 was subjected to exposure and heat treatment under the same conditions as in the method for forming the flow path forming member of Comparative Example 1, to produce a cured product of photosensitive resin composition 18. Thereafter, the substrate on which the cured product of each resin was formed was immersed in pure water at 70°C for one day, and the change in mass of the cured product of each resin before and after immersion in pure water was measured using a mass spectrometer (manufactured by Metryx, product name: Mentor The water absorption was measured using a 100% cellulose acetate sintered body (OCS23). The results of the water absorption measurement are shown in Table 3. The cured products prepared in Examples 1 and 2 had significantly lower water absorption than the Comparative Example.

[0043] [Table 3]

[0044] <Ink resistance> The inks shown in Table 4 below were filled into the flow paths of the liquid ejection heads produced in Examples 1 and 2, and Comparative Example 1, and the heads were left in an oven at 70° C. for 90 days.

[0045] [Table 4]

[0046] The bonding state between the inorganic material layer 4 and the flow path forming member 6 after standing was observed with a metallurgical microscope and evaluated according to the following criteria. Table 5 shows the evaluation results of ink resistance. In the liquid ejection heads produced in Examples 1 and 2, peeling occurred between the inorganic material layer and the flow path forming member. In contrast, in the comparative example, partial peeling was observed between the inorganic material layer and the flow path forming member. (Evaluation Criteria) A: Even after storage at 70° C. for 90 days, no peeling occurred between the inorganic material layer 4 and the flow path forming member 6 . B: After storage at 70° C. for 90 days, peeling occurred between the inorganic material layer 4 and the flow path forming member 6, which was not observed when the liquid ejection head was completed.

[0047] [Table 5]

[0048] <Printing evaluation> The liquid ejection heads produced in the examples and comparative examples were filled with the same ink as that used in the ink resistance evaluation, and were stored at 70° C. for 90 days, after which a printing evaluation was performed. The results of the printing evaluation are shown in Table 6. In the liquid ejection heads produced in Examples 1 and 2, the print evaluation was good, whereas in the comparative example, partial peeling occurred between the inorganic material layer and the flow path forming member, and a decrease in print quality was observed.

[0049] [Table 6]

[0050] As described above, according to the present disclosure, even when ink with high permeability is used, it is possible to prevent the ink from penetrating into the flow path forming member, thereby suppressing peeling of the flow path forming member from the substrate, thereby providing a liquid ejection head that ensures high reliability. [Explanation of symbols]

[0051] 1: substrate, 2: energy generating element, 3: supply port, 4: inorganic material layer, 5: protective layer, 6: flow path forming member, 7: flow path, 8: discharge port, 9: nozzle portion, 10: discharge port forming member, 11: liquid repellent layer, 12: film, 13: resin for flow path forming member, 14: mask resist, 15: flow path forming mask, 16: photosensitive resin composition, 17: discharge port forming mask, 18: photosensitive resin composition, 19: flow path forming mask, 20: substrate surface

Claims

1. A liquid ejection head including a substrate, a flow path forming member provided on a substrate surface of the substrate to form a flow path for liquid, and an ejection port forming member provided on the flow path forming member and having an ejection port for ejecting liquid, the discharge port forming member and the flow path forming member are formed of different materials, a thickness of the flow path forming member is greater than a thickness of the discharge port forming member in a direction perpendicular to the substrate surface; the discharge port forming member is a cured product of a photosensitive resin composition, A liquid ejection head, wherein the flow path forming member contains at least one resin selected from the group consisting of polyetherimide resins and polyetheramideimide resins.

2. The liquid ejection head according to claim 1 , wherein the polyetherimide resin and the polyetheramide-imide resin are thermoplastic resins.

3. 3. The liquid ejection head according to claim 1, wherein the polyetherimide resin and the polyetheramideimide resin have a weight average molecular weight of 5,000 to 100,000.

4. 4. The liquid ejection head according to claim 1, wherein the photosensitive resin composition contains a cationic polymerization type epoxy resin.

5. 5. The liquid ejection head according to claim 1, wherein the photosensitive resin composition contains a cationic polymerization type epoxy resin having two or more epoxy groups in one molecule.

6. 6. The liquid ejection head according to claim 1, wherein the photosensitive resin composition is a negative composition.

7. 7. The liquid ejection head according to claim 1, wherein the photosensitive resin composition contains a photoacid generator.

8. The water absorption rate of the polyetherimide resin and the polyetheramide-imide resin is 8. The liquid ejection head according to claim 1, which has a water absorption rate lower than that of a cured product of the photosensitive resin composition.

9. 9. The liquid ejection head according to claim 1, further comprising a liquid repellent layer formed on said ejection port forming member.

10. A method for manufacturing a liquid ejection head including: a substrate; a flow path forming member provided on a substrate surface of the substrate to form a flow path for liquid; and an ejection port forming member provided on the flow path forming member and having an ejection port for ejecting liquid, the method comprising the steps of: forming a flow path forming member for forming a liquid flow path on the substrate; forming a discharge port forming member having a discharge port for discharging a liquid on the flow path forming member, the discharge port forming member and the flow path forming member are formed of different materials, a thickness of the flow path forming member is greater than a thickness of the discharge port forming member in a direction perpendicular to the substrate surface; the discharge port forming member is a cured product of a photosensitive resin composition, A method for manufacturing a liquid ejection head, wherein the flow path forming member contains at least one resin selected from the group consisting of polyetherimide resins and polyetheramideimide resins.

11. A liquid ejection head as described in claim 1, wherein the flow path forming member contains polyetheramide imide resin.

12. A method for manufacturing a liquid ejection head as described in claim 10, wherein the flow path forming member contains polyetheramide imide resin.

Citation Information

Patent Citations

  • Ink jet recording head

    JP1994099578A

  • Ink-jet recording head and manufacture thereof

    JP1997131867A

  • Photosensitive resin composition, inkjet recording head obtained by using the same and manufacturing method thereof

    JP2005008652A

  • Nozzle plate, method for manufacturing nozzle plate, droplet discharge head, method for manufacturing droplet discharge head, and droplet discharge device

    JP2010280229A

  • Substrate for liquid ejection head, liquid ejection head, and method for manufacturing the same

    JP2011126102A