Liquid ejection head and method for manufacturing the same

A continuous liquid-resistant insulating film in the liquid ejection head design addresses the issue of size and flow resistance by eliminating overlapping portions, ensuring effective liquid resistance and compactness.

JP7551367B2Active Publication Date: 2024-09-17CANON KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020120678
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-14
Publication Date
2024-09-17
Estimated Expiration
2040-07-14

AI Technical Summary

Technical Problem

Existing liquid ejection heads require a large area around the supply port to prevent liquid infiltration, leading to increased size and potential flow resistance due to overlapping film formations.

Method used

A liquid ejection head design with a continuous liquid-resistant insulating film covering both the surface and inner surfaces of the ejection element substrate, eliminating the need for overlapping portions and reducing the distance between the supply port and ejection element, while using materials like SiCN or SiOCN for improved adhesion and liquid resistance.

Benefits of technology

The design suppresses liquid erosion, reduces the head's size, and minimizes flow resistance, enhancing the reliability and efficiency of liquid circulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551367000006
    Figure 0007551367000006
  • Figure 0007551367000001
    Figure 0007551367000001
  • Figure 0007551367000002
    Figure 0007551367000002
Patent Text Reader

Abstract

To inexpensively and compactly configure a liquid discharge head with high reliability which can suppress corrosion caused by liquid.SOLUTION: A liquid discharge head 1 includes: a substrate 10 for a liquid discharge head in which a discharge element 31 is formed to generate discharge energy for discharging liquid; a discharge port formation member 12 which forms a discharge port; and a liquid chamber 23 which is formed between the substrate 10 for the liquid discharge head and the discharge port formation member 12 so as to store liquid discharged from a discharge port 13. The substrate 10 for the liquid discharge head has a substrate 11, an insulation film 37 laminated on the substrate 11 so as to insulate the discharge element 31, communication ports 39 formed in the substrate 11 and the insulation film 37 so as to be communicated with the liquid chamber 23, and a liquid resistant insulation film 38 having adhesion to the discharge port formation member 12. The liquid resistant insulation film 38 has a first portion which covers a surface on a side provided with the discharge port formation member 12 of the insulation film 37 and a part of which comes into contact with the discharge port formation member 12 and a second portion which covers internal surfaces of the communication ports 39 formed in the insulation film 37. The first portion is provided continuously to the second portion.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid ejection head that ejects liquid, and a method for manufacturing a liquid ejection head. [Background technology]

[0002] Some liquid ejection heads are configured such that a liquid chamber is formed by providing an ejection port forming member with an ejection port on one side of a substrate for liquid ejection heads (hereinafter referred to as an ejection element substrate) on which ejection elements are provided, and the liquid in the liquid chamber is ejected from the ejection port by driving the ejection elements. As an ejection element substrate used in this type of liquid ejection head, one in which an interlayer insulating film for insulating the ejection elements and the electric wiring connected thereto is laminated on a silicon substrate is known. A supply port and a liquid flow path for supplying liquid to the liquid chamber are formed in the interlayer insulating film and the silicon substrate. In addition, a liquid-resistant film may be formed on the surface of the ejection element substrate that comes into contact with the liquid in order to suppress erosion by the liquid. In particular, a silicon oxide film (hereinafter referred to as an SiO film) used as an interlayer insulating film may be eroded by the liquid depending on the type of liquid such as ink, so it is desirable to cover the surface that comes into contact with the liquid with a liquid-resistant film.

[0003] Patent Document 1 discloses an ejection element substrate in which the surface of the interlayer insulating film of the ejection element substrate is covered with an insulating film that has good adhesion to an ejection port forming member, while the inner surface of a supply port communicating with the ejection port is covered with a liquid-resistant film using atomic layer deposition (hereinafter referred to as ALD). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-187789 A Summary of the Invention [Problem to be solved by the invention]

[0005] In Patent Document 1, in the manufacture of an ejection element substrate, an insulating film having adhesion to an ejection port forming member and liquid resistance is formed on the surface of an interlayer insulating film provided on a silicon substrate, and then a supply port and a liquid flow path communicating with a liquid chamber are formed. Next, a film having liquid resistance such as TiO (titanium monoxide) is formed on the inner surface of the insulating film and the supply flow path by the ALD method. Furthermore, the film in the area other than the supply port is removed by etching. At this time, etching is performed so that an overlapping portion between the film formed by the ALD method and the insulating film is left with a width of several μm around the opening of the supply port. By forming this overlapping portion, it is possible to suppress the infiltration of liquid such as ink into the interlayer insulating film.

[0006] As described above, in the ejection element substrate disclosed in Patent Document 1, in order to prevent the liquid from penetrating into the interlayer insulating film, it is necessary to form the above-mentioned overlapping films around the supply port. This requires a large area around the supply port, which may increase the area of ​​the entire element substrate.

[0007] An object of the present invention is to provide a highly reliable liquid ejection head that is capable of suppressing erosion by liquid while suppressing an increase in size. [Means for solving the problem]

[0008] The present invention provides a liquid ejection head including a substrate for a liquid ejection head provided with ejection elements that generate ejection energy for liquid, an ejection port forming member in which ejection ports for ejecting liquid are formed, and a liquid chamber formed between the substrate for the liquid ejection head and the ejection port forming member and containing liquid to be ejected from the ejection ports, the substrate for the liquid ejection head including a substrate, an insulating film laminated on the substrate and insulating the ejection elements, a cavitation-resistant layer covering a position of the insulating film where the ejection elements are provided; a liquid-resistant insulating film having a communication port formed in the substrate and the insulating film so as to communicate with the liquid chamber, and having adhesion to the ejection port forming member; The liquid-resistant insulating film is a first portion that covers a surface of the insulating film on which the ejection port forming member is provided and has a portion that contacts the ejection port forming member; and a second portion that covers an inner surface of the communication port formed in the insulating film; and a third portion covering a part of the cavitation-resistant layer.It is characterized by: Effect of the Invention

[0009] According to the present invention, it is possible to provide a highly reliable liquid ejection head that is capable of suppressing erosion by liquid while suppressing an increase in size. [Brief description of the drawings]

[0010] [Figure 1] 1 is a cross-sectional perspective view that illustrates a liquid ejection head according to an embodiment of the present invention; [Diagram 2] 2A and 2B are a partial cross-sectional view and a partial plan view of the liquid ejection head shown in FIG. [Diagram 3] 5A to 5C are partial cross-sectional views illustrating a manufacturing method of a liquid ejection head in a comparative example. [Figure 4] 4A and 4B are a partial cross-sectional view and a partial plan view of a liquid ejection head in a comparative example. [Diagram 5] 3A to 3C are partial cross-sectional views illustrating a manufacturing method of the liquid ejection head in the first embodiment. [Figure 6] FIG. 11 is a partial cross-sectional view showing a liquid ejection head in a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] (Embodiment) Hereinafter, embodiments of the present invention will be described with reference to the drawings. However, the following description is not intended to limit the scope of the present invention.

[0012] FIG. 1 is a cross-sectional perspective view that shows a schematic diagram of a liquid ejection head 1 according to an embodiment of the present invention. The liquid ejection head 1 includes a substrate for a liquid ejection head (hereinafter, also referred to as an ejection element substrate) 10 and an ejection port forming member 12 provided on the front side (upper side in FIG. 1) of the ejection element substrate 10. The ejection element substrate 10 includes a substrate 11 made of Si (silicon) and a cover plate 20 provided on the rear side (lower side in FIG. 1) of the substrate 11. On the front side of the substrate 11, ejection elements 31 as ejection elements that generate ejection energy for ejecting liquid, electric wiring (not shown) connected to the ejection elements 31, an interlayer insulating film (not shown in FIG. 1), and the like are formed. In addition, the ejection port forming member 12 has four ejection port arrays 14 corresponding to each ink color. The arrangement direction of the multiple ejection ports 13 that constitute the ejection port array 14, i.e., the direction in which the ejection port array extends (Y direction), is also referred to as the "ejection port array direction".

[0013] As shown in FIG. 1, the ejection elements 31 are disposed at positions facing the ejection ports 13. The ejection elements 31 are constituted by heat generating elements for foaming liquid by thermal energy. The ejection port forming member 12 defines a pressure chamber (liquid chamber) 23 having the ejection element 31 therein between the ejection port forming member 12 and the substrate 11. The pressure chamber 23 contains the liquid to be ejected from the ejection port 13. The ejection elements 31 are electrically connected to the electrode pad section 16 by electrical wiring (not shown) provided on the ejection element substrate 10. The electrode pad section 16 is connected to a wiring substrate (not shown) provided outside the ejection element substrate 10. The ejection elements 31 generate heat based on a pulse signal input from the outside via the wiring substrate, and boil the liquid in the pressure chamber 23. The liquid is ejected from the ejection port 13 by pressure applied to the liquid when boiling.

[0014] The liquid supply flow path 18a and the liquid recovery flow path 18b formed in the ejection element substrate 10 are flow paths extending in the ejection port array direction (Y direction). The liquid supply flow path 18a and the liquid recovery flow path 18b are respectively connected to the pressure chamber 23 via an independent supply port 39a and an independent recovery port 39b (see FIG. 2). The pressure chamber 23 is connected to the ejection port 13.

[0015] Fig. 2(a) is a cross-sectional view of the liquid ejection head substrate (ejection element substrate) 10 shown in Fig. 1 taken along line IIa-IIa, and shows the peripheral configuration of the ejection element 31 disposed at a position facing the ejection port 13. Fig. 2(b) is a plan view of the peripheral configuration of the ejection element 31 as viewed from the front surface side (ejection port 13 side).

[0016] The configuration of the discharge element substrate 10 in this embodiment will be described below with reference to FIG. 2(a) and FIG. 2(b). An interlayer insulating film (insulating film) 37 is formed on the surface side (upper surface side in FIG. 2(a)) of the substrate 11. A circuit composed of electrical wiring such as AL (aluminum) is provided in this interlayer insulating film 37. Discharge elements 31 formed of a cermet material such as TaSiN (tantalum silicon nitride) or WSiN (tungsten silicon nitride) are formed on the surface side of the interlayer insulating film 37. The discharge elements 31 are electrically connected to the electrical wiring provided in the interlayer insulating film 37 by electrode plugs (not shown) made of tungsten. Furthermore, an insulating protective film (not shown) made of SiN (silicon nitride) or SiCN (silicon carbonitride) or a laminate thereof is formed so as to cover the discharge elements 31. An anti-cavitation layer 35 having a top layer made of a material such as Ta (tantalum) or Ir (iridium) is formed on the surface of the insulating protective film.

[0017] In addition, on the ejection element substrate 10, an independent supply port 39a and an independent recovery port 39b are formed on both sides of the ejection element 31 as communication ports communicating with the pressure chamber 23. The independent supply port 39a provided on one side of the ejection element 31 communicates with a liquid supply flow path 18a formed from the back side of the substrate 11 (the lower side in FIG. 2(a)). In addition, the independent recovery port 39b provided on the other side of the ejection element 31 communicates with a liquid recovery flow path 18b formed from the back side of the substrate 11. In the following description, when there is no need to particularly distinguish between the independent supply port 39a and the independent recovery port 39b, they will be collectively referred to as the independent port 39. In addition, when there is no need to distinguish between the liquid supply flow path 18a and the liquid recovery flow path 18b, they will be collectively referred to as the liquid flow path 18.

[0018] The independent opening 39 includes an opening 391 formed in an interlayer insulating film 37 provided on the substrate 11, and an opening 392 formed in the substrate 11. These openings 391, 392 are each formed by dry etching performed from the front surface side of the substrate 11.

[0019] Further, on the surface of the discharge element substrate 10, a discharge port forming member 12 made of resin is provided in a state of being in close contact with the surface (upper surface in FIG. 2(a)) of the discharge element substrate 10. Between this discharge port forming member 12 and the surface of the discharge element substrate 10, a pressure chamber 23 communicating with an independent port 39 is formed.

[0020] In the liquid ejection head 1 having the ejection element substrate 10 and the ejection orifice forming member 12 as described above, it is necessary that the ejection element substrate 10 and the ejection orifice forming member 12 are well adhered to each other. It is also necessary to suppress the interlayer insulating film 37 in the independent port 39 from dissolving due to contact with a liquid such as ink. Therefore, in this embodiment, the surface of the ejection element substrate 10 except for the upper part of the ejection element 31 and the electrode pad part 16 (see FIG. 1) and the inner surface of the independent port 39 formed by the interlayer insulating film 37 are covered with a continuous liquid-resistant insulating film 38 (coating film). Therefore, the ejection orifice forming member 12 is in direct contact with the liquid-resistant insulating film 38. Note that the part of the liquid-resistant insulating film 38 that covers the surface of the interlayer insulating film 37 on the side where the ejection orifice forming member 12 is provided and that comes into contact with the ejection orifice forming member 12 is also referred to as the first part of the liquid-resistant insulating film 38. In addition, a portion of the liquid-resistant insulating film 38 that covers the inner surface of the independent port 39 formed in the interlayer insulating film 37 is also referred to as a second portion of the liquid-resistant insulating film 38. The liquid-resistant insulating film 38 has a first portion and a second portion that are provided continuously.

[0021] In this embodiment, the liquid-resistant insulating film 38 is made of SiCN (silicon carbonitride), SiOCN (silicon oxynitride), SiOC (silicon oxycarbide), or a laminated film of these materials. This makes it possible to protect the interlayer insulating film 37 from liquids including ink. Furthermore, since SiCN, SiOCN, and SiOC have good adhesion to the ejection port forming member 12, the liquid-resistant insulating film 38 also serves as an adhesion improving layer.

[0022] In this embodiment, the liquid-resistant insulating film 38 contains carbon atoms (C), which allows the liquid-resistant insulating film 38 to have liquid resistance. From the viewpoint of liquid resistance, the liquid-resistant insulating film 38 preferably contains 5 atom % or more of carbon atoms (C). The liquid-resistant insulating film 38 preferably has higher liquid resistance to liquids such as ink than the interlayer insulating film 37.

[0023] In this embodiment, if the liquid-resistant insulating film 38 is a silicon compound such as SiCN, SiOCN, or SiOC, it can have adhesion to the ejection port formation member 12 formed of a resin.

[0024] Therefore, in this embodiment, the manufacturing process can be simplified compared to the comparative example described later in which the adhesion improving layer formed on the surface of the interlayer insulating film and the liquid-resistant film formed in the independent port are formed separately. Also, in the comparative example described later, it is necessary to form an overlapping portion where the liquid-resistant film and the adhesion improving film overlap in the peripheral portion of the independent port, which is a factor that increases the distance between the independent port and the ejection element 31. In contrast, in this embodiment, since the liquid-resistant insulating film is formed continuously, an overlapping portion like the comparative example is not required. Therefore, in this embodiment, it is possible to shorten the distance between the independent port and the ejection element 31 compared to the comparative example, and it is possible to miniaturize the liquid ejection head 1. Also, with the shortening of the distance between the independent port 39 and the ejection element 31, it is possible to reduce the flow resistance of the liquid in the liquid ejection head 1. Furthermore, since it is not necessary to consider the formation of the overlapping portion, the degree of freedom in designing the liquid ejection head 1 is improved.

[0025] The liquid ejection head 1 in this embodiment has a configuration used in a liquid ejection device that employs a liquid circulation system. That is, the liquid supply flow path 18a and the liquid recovery flow path 18b of the liquid ejection head 1 are connected to the device-side supply flow path and the device-side recovery flow path provided in the liquid ejection device, respectively. The liquid in the liquid storage section of the liquid ejection device is supplied to the liquid supply flow path 18a of the liquid ejection head 1 via the device-side supply flow path, and the liquid that flows into the liquid supply flow path 18a flows into the pressure chamber 23 via the independent supply port 39a. A part of the liquid that flows into the pressure chamber 23 is ejected from the ejection port 13 by driving the ejection element 31, and the remaining liquid returns to the liquid storage section via the independent recovery port 39b, the liquid recovery flow path 18b, and the device-side recovery flow path. In this way, according to a liquid ejection device of a liquid circulation system that ejects liquid while circulating the liquid, it is possible to suppress the settling of coloring materials and the like contained in the liquid, and it is possible to maintain good liquid ejection performance. Furthermore, in the above-described embodiment, the distance L1 from the independent supply port 39a to the ejection element 31 and the distance L1 from the independent recovery port 39b to the ejection element 31 are shortened. This reduces the flow resistance when the liquid flows from the independent supply port 39a to the independent recovery port 39b, making it possible to realize smooth liquid circulation.

[0026] Next, the configuration and manufacturing method of the liquid ejection head 1 of this embodiment will be described in more detail in Examples 1 and 2. In the following description, in order to clarify the features of this embodiment, a comparative example of this embodiment will be described first, and then each example will be described.

[0027] (Comparative Example) The configuration and manufacturing method of a liquid ejection head 100 in a comparative example to this embodiment will be described with reference to Fig. 3 and Fig. 4. Fig. 3(a) to Fig. 3(e) are cross-sectional views showing the manufacturing method of this comparative example. Fig. 4(a) is a partial cross-sectional view of the liquid ejection head in this comparative example, and Fig. 4(b) is a plan view.

[0028] 3(a) shows a state in which an interlayer insulating film 37 and ejection elements 31 are formed on a substrate 11, and an anti-cavitation layer 35 is further formed in a position facing the ejection elements 31. Here, the process up to forming the laminated structure shown in FIG. 3(a) will be described.

[0029] An interlayer insulating film 37 made of SiO (silicon oxide) and having a thickness of 1 to 2 μm was formed on the substrate 11 on which drive elements (not shown) for driving the ejection elements 31 and wiring (not shown) for driving the drive elements were formed. Next, a part of the interlayer insulating film 37 was opened using a dry etching method to form a through hole. Next, an electrode plug (not shown) was formed using tungsten so as to fill the through hole. The electrode plug serves to electrically connect the drive elements in the lower layer and the ejection elements 31 formed in the upper layer.

[0030] Thereafter, the ejection element 31 was formed from a cermet material made of TaSiN. At this time, the ejection element 31 was formed to have a thickness of 15 nm and a size in the planar direction of 15 μm. Photolithography and a dry etching method using chlorine were used to form the ejection element 31. Next, an insulating protective film (not shown) made of SiN was formed to a thickness of 200 nm by using a plasma CVD method so as to cover the ejection element 31. Here, the thickness of the insulating protective film was set to 200 nm from the viewpoint of insulation. However, the thickness of the protective layer needs to be 100 nm or more, and further, from the viewpoint of thermal conduction to the liquid, it is sufficient that the protective layer is formed to a thickness of 100 nm or more and 500 nm or less.

[0031] Next, a cavitation-resistant layer 35 was formed on the insulating protective film. This cavitation-resistant layer was formed by sequentially stacking three layers, a Ta layer, an Ir layer, and a Ta layer, from the surface side of the substrate 11 (the upper surface side in the figure). These three layers were formed in the entire surface area of ​​the substrate 11 with thicknesses of 30 nm, 50 nm, and 50 nm, respectively, from the substrate side, using a sputtering method. The thickness of the Ir layer may be any thickness that satisfies cavitation resistance, and is preferably 20 nm or more. Furthermore, taking into account the viewpoint of processability, the thickness of the Ir layer is more preferably 20 nm or more and 300 nm or less. The Ta layer located on the surface side of the substrate 11 is disposed to ensure adhesion, and is preferably 20 nm or more. Furthermore, taking into account the viewpoint of processability, the thickness of the Ta layer located on the surface side of the substrate 11 is more preferably 20 nm or more and 300 nm or less.

[0032] After that, a patterning process was carried out on the cavitation-resistant layer 35. In this patterning process, of the cavitation-resistant layer formed over the entire surface of the substrate 11, the cavitation-resistant layer located on the ejection elements 31 was left, and the cavitation-resistant layer existing in other positions was removed by dry etching. As a result, the layered structure shown in FIG. 3(a) was formed.

[0033] Next, an adhesion improving layer 36 having adhesion to the discharge port forming member 12 was formed on the entire surface of the interlayer insulating film 37 by a CVD method to a thickness of 150 nm (see FIG. 3(b)). In this comparative example, a SiOCN film was used as the adhesion improving layer, but a film such as SiC or SiCN may also be used. Next, the adhesion improving layer 36 on the discharge element 31 was removed by a dry etching method, and the Ta layer located at the outermost surface of the above-mentioned three layers constituting the cavitation-resistant layer 35 was removed so that the Ir film appeared on the outermost surface. In addition, an opening was formed at the location where the electrode pad portion was to be formed, and an Au pad portion (not shown) electrically connected to the discharge element 31 was formed in the formed opening.

[0034] Next, independent ports 39 (independent supply port 39a, independent recovery port 39b) were formed by dry etching on the surface (upper surface in the figure) of interlayer insulating film 37 and substrate 11. Furthermore, liquid flow paths 18 (liquid supply flow path 18a, liquid recovery flow path 18b) communicating with independent ports 39 (independent supply port 39a, independent recovery port 39b) were formed by dry etching on the rear surface of substrate 11 (see FIG. 3(c)).

[0035] Thereafter, a TiO (titanium monoxide) film 40 having resistance to liquids such as ink was formed to a thickness of 100 nm on the exposed portions of the substrate 11 and the interlayer insulating film 37 by using the ALD method. That is, the TiO film 40 was formed on the back surface of the substrate 11, the inner surface of the liquid flow path 18, the inner surface of the independent port 39, and the surface of the interlayer insulating film 37.

[0036] Here, the TiO film 40 formed on the substrate 11 and the interlayer insulating film 37 was removed by wet etching using buffered hydrofluoric acid, leaving the TiO film 40 formed on the inner surface of the independent port 39 and the inner surface of the liquid flow path 18. At this time, in order to reliably leave the TiO film 40 formed on the inner surface of the independent port 39, wet etching was performed so that the TiO film 40 overlaps the adhesion improving layer 36 formed on the surface of the interlayer insulating film 37 at a distance of 5 μm, forming an overlapping portion 40a. This state is shown in FIG. 3(d). From the viewpoint of adhesion between the adhesion improving layer 36 and the TiO film 40 and from the viewpoint of manufacturing tolerance, it is necessary to form the overlapping portion 40a with a distance of 5 μm as described above in the TiO film 40. In this manner, the ejection element substrate 10 was formed.

[0037] Thereafter, as shown in FIG. 3(e), the discharge port forming member 12 was provided on the discharge element substrate 10. For the discharge port forming member 12 used in this comparative example and the first and second examples described below, a laminated film in which multiple negative photosensitive resin layers were laminated was used. Specifically, multiple resin layers were formed on a film, and then the film was attached to a base material having an uneven surface, and the discharge port forming member 12 was formed by performing exposure and development. In particular, a resin layer containing polyol was used for the negative photosensitive resin layer that directly contacts the discharge element substrate 10. This resin layer has good adhesion to silicon compounds such as SiOCN used in this comparative example and the examples. On the other hand, it does not have good adhesion to films such as metals and metal oxide films, and peeling may occur at the interface when immersed in ink at high temperatures. Therefore, in this comparative example, the discharge port forming member 12 and the TiO film 40 are not in direct contact with each other. As described above, the liquid discharge head 100 in the comparative example was produced.

[0038] As shown in FIGS. 4(a) and 4(b), in the comparative example, an overlapping portion 40a is formed around the opening of the independent port 39 on the surface (top surface in the figure) of the ejection element substrate 10. Since a distance of 5 μm is required for this overlapping portion 40a as described above, it is necessary to form the independent port 39 at a position taking this distance into consideration. As a result, the distance L2 from the independent port 39 to the ejection element 31 becomes large, which leads to an increase in the size of the ejection element substrate 10, and in turn, an increase in the size of the liquid ejection head 1. In addition, the increase in distance L2 may increase the flow resistance of the liquid, and the manufacturing process may become complicated in order to form the overlapping portion.

[0039] (First Example) Next, a first embodiment of the present invention will be described. Below, a manufacturing method of the liquid ejection head 1 shown in Fig. 2(a) and Fig. 2(b) will be described step by step based on the manufacturing steps shown in Fig. 5(a) to Fig. 5(e). Fig. 5(a) is a cross-sectional view showing a state in which a patterning process of the cavitation-resistant layer 35 is performed on the substrate 11. The steps up to the patterning process of this cavitation-resistant layer 35 are the same as those in Comparative Example 1, so a description thereof will be omitted.

[0040] 1 is formed (not shown in FIG. 4). After that, dry etching is performed only on the interlayer insulating film 37 from the front surface side (upper surface side in the figure) of the interlayer insulating film 37 to form an opening 391 corresponding to a part of the independent port 39 (independent supply port 39a and independent recovery port 39b) shown in FIG. 2 (see FIG. 5(b)).

[0041] After forming the opening 391 of the independent port 39, as shown in FIG. 5(c), a continuous liquid-resistant insulating film 38 was formed on the surface of the interlayer insulating film 37 (upper surface in FIG. 5) and the entire inner surface (side surface and bottom surface) of the opening 391 by using a plasma CVD method. In this embodiment, a SiOCN film was formed as the liquid-resistant insulating film 38 to a thickness of 150 nm on the surface of the interlayer insulating film 37. At this time, a film of 100 nm or more was formed on the inner surface (side surface and bottom surface) of the opening 391 of the independent port 39, continuous with the SiOCN film formed on the surface of the interlayer insulating film 37. This makes it possible to protect the interlayer insulating film 37 from liquids such as ink. That is, it is possible to suppress contact between the interlayer insulating film 37 and liquid and suppress elution of the interlayer insulating film 37. The liquid-resistant insulating film 38 may be formed of a SiCN film, a SiOC film, or a laminated film thereof. In addition, the liquid-resistant insulating film 38 made of a SiOCN film, a SiCN film, a SiOC film, or a laminated film thereof has good adhesion to the resin constituting the ejection port forming member 12, and therefore also serves as an adhesion improving layer. Therefore, there is no need to newly form an adhesion improving layer in a separate process.

[0042] In this embodiment, in the liquid-resistant insulating film 38 formation process, a SiOCN film having a thickness of 150 nm was formed on the surface of the interlayer insulating film 37, but the liquid-resistant insulating film 38 formation process is not necessarily limited to this embodiment. The liquid-resistant insulating film 38 formation process may be performed so that a SiOCN film having a thickness of 100 nm or more is formed inside the independent port 39. In addition, the liquid-resistant insulating film 38 was formed using the plasma CVD method, but a film formation method such as the ALD method may also be used. If the SiOCN film forming the liquid-resistant insulating film 38 contains carbon atoms (C) of 5 atom % or more, the film loss (thickness reduction) of the liquid-resistant insulating film 38 due to contact with liquid can be significantly reduced. In this embodiment, the carbon atom (C) content was set to 10 atom %. In this manner, in this embodiment, a continuous liquid-resistant insulating film 38 covering the surface of the interlayer insulating film 37 and the inner surface of the independent port 39 was formed.

[0043] Next, as shown in FIG. 5(d), the liquid-resistant insulating film (SiOCN film) 38 formed above the ejection elements 31 and the Ta film located at the outermost layer of the three layers constituting the cavitation-resistant layer 35 were removed by dry etching. This exposed the Ir layer of the cavitation-resistant layer 35. This dry etching was performed using a chlorine-based gas under low bias conditions. This allows the etching to be stopped at the position where the Ir layer is exposed. Therefore, it becomes possible to etch the SiOCN film and the Ta film continuously.

[0044] 5(d), the SiOCN film formed on the bottom surface of the opening 391 constituting part of the independent port 39 (independent supply port 39a, independent recovery port 39b) and the opening 392 formed by the substrate 11 in the independent port 39 were etched from the front surface side (upper surface side in the figure). Furthermore, dry etching was performed from the rear surface side (lower surface side in the figure) of the substrate 11 to form the liquid flow path 18 (liquid supply flow path 18a, liquid recovery flow path 18b) communicating with the independent port 39. In this manner, the ejection element substrate 10 was produced.

[0045] Next, the ejection port forming member 12 was provided on the surface (upper surface in the figure) of the ejection element substrate 10 by the same method as in the comparative example, and a pressure chamber 23 communicating with an independent port 39 was formed between the ejection element substrate 10 and the ejection port forming member 12. A liquid-resistant insulating film 38 having good adhesion to the ejection port forming member 12 was formed on the outermost surface of the ejection element substrate 10. Therefore, when providing the ejection port forming member 12, it is not necessary to particularly consider the adhesion with the ejection element substrate 10, and the ejection port forming member 12 may be formed in a required location. In addition, since it is not necessary to form an overlapping portion of 5 μm on the surface of the ejection element substrate 10 as in the comparative example, it is possible to shorten the distance L1 between the ejection element 31 and the independent port compared to the distance L2 in the comparative example. Therefore, it is possible to configure the liquid ejection head 1 in a small size, and it is possible to reduce the flow resistance of the liquid in the liquid ejection head 1, and it is possible to increase the fluidity of the liquid.

[0046] (Second Example) Next, a second embodiment of the present invention will be described. In the above-mentioned first embodiment, only the interlayer insulating film 37 of the ejection element substrate 10, which is easily eluted by contact with liquid such as ink, is covered with a liquid-resistant insulating film 38 such as a SiOCN film. In contrast, the second embodiment has a configuration in which the inner surfaces of the liquid flow paths 18 (liquid supply flow paths 18a, liquid recovery flow paths 18b) formed in the substrate 11 are also covered with a film having liquid resistance.

[0047] Fig. 6 is a cross-sectional view showing a liquid ejection head 1A in the second embodiment. In this embodiment, similarly to the first embodiment, the processes shown in Fig. 5(a) to Fig. 5(d) were performed. That is, a continuous liquid-resistant insulating film 38 was formed on the surface of the interlayer insulating film 37 and on the inner surface of the opening 391 which is a part of the independent port 39 by using a plasma CVD method. Thereafter, the liquid-resistant insulating film 38 and the substrate 11 in the opening 391 were etched from the surface side of the interlayer insulating film 37 to form the independent port 39 (independent supply port 39a, independent recovery port 39b), and further, the liquid flow path 18 was formed from the rear surface side of the substrate by dry etching.

[0048] The above completes the process up to FIG. 5(d). Next, in this embodiment, a TiO film 41 having liquid resistance was formed to a thickness of 100 nm on the front and back surfaces of the substrate 11, including the independent port 39 and the liquid flow path 18, by using the ALD method. Then, the TiO film 41 formed on the surface of the interlayer insulating film 37 was removed by using an etch-back method from the front side of the interlayer insulating film 37, and the liquid-resistant insulating film 38 was exposed on the surface of the interlayer insulating film 37. At this time, since the TiO film formed in the independent port 39 and the liquid flow path 18 is difficult to etch, the TiO film 41 remains without being removed as shown in FIG. 6. Also, by removing the TiO film 41 by etch-back, it is possible to adopt the same layout design as in the first embodiment. As a result, the formation of the ejection element substrate 10A in this embodiment is completed.

[0049] Next, by using the same method as in the comparative example, an ejection port forming member 12 was provided on the surface of the ejection element substrate 10A, and a pressure chamber 23 communicating with the independent port 39 was formed between the ejection element substrate 10A and the ejection port forming member 12. Through the above steps, the liquid ejection head 1A in the second embodiment was completed.

[0050] In this embodiment, as in the first embodiment, it is possible to reduce the distance between the independent port 39 and the ejection element 31, thereby making it possible to miniaturize the liquid ejection head 1A. Furthermore, according to this embodiment, it is possible to protect not only the interlayer insulating film 37 but also the substrate 11 from liquid, making it possible to manufacture a more reliable liquid ejection head 1A.

[0051] Furthermore, in the second embodiment, by adding the step of depositing a TiO41 film by the ALD method and etching it back, it is possible to cover the substrate 11 with a liquid-resistant film, making it possible to manufacture a more reliable liquid ejection head 1A.

[0052] (Comparison between the first and second examples and the comparative example) Here, the first and second embodiments are compared with the comparative example. As shown in FIG. 4(b), in the comparative example, it is necessary to provide an overlapping portion 40a of the liquid-resistant film (TiO film 40) of about 5 μm around the independent port 39 on the front side of the ejection element substrate 10. In contrast, in the first and second embodiments, as shown in FIG. 2 and FIG. 6, it is not necessary to provide an overlapping portion of the liquid-resistant film around the independent port 39. For this reason, in this embodiment, the width (5 μm) of the overlapping portion 40a required in the comparative example is deleted, and the formation position of the independent port 39 is moved closer to the ejection element 31 by that amount. That is, the distance L1 between the ejection element 31 and the independent port 39 in this embodiment is shorter than the distance L2 between the ejection element 31 and the independent port 39 in the comparative example by at least the width (5 μm) of the overlapping portion 40a. For this reason, it is possible to reduce the size of the liquid ejection head 1A and reduce the flow resistance of the liquid compared to the comparative example.

[0053] In addition, in the comparative example, the interlayer insulating film 37 is protected by two types of films, the adhesion improving layer 36 and the TiO film 40, whereas in the first embodiment, the liquid is protected by only one type of liquid-resistant insulating film 38. This simplifies the manufacturing process and reduces manufacturing costs.

[0054] Furthermore, in the second embodiment, by forming the TiO film 41 by the ALD method and etching it back, it becomes possible to protect the substrate 11 from the liquid by the TiO film 41, and a liquid ejection head with higher reliability can be manufactured.

[0055] (Other embodiments) In the above embodiment and example, an independent supply port 39a and an independent recovery port 39b are formed on both sides of each ejection element 31, and the remaining liquid that is supplied from the independent supply port 39a to the pressure chamber 23 and not ejected from the ejection port 13 is recovered from the independent recovery port 39b. However, the present invention is not limited to such a configuration. The present invention is also applicable to a liquid ejection head that employs a configuration in which liquid is supplied to the pressure chamber from two independent ports provided on both sides of the ejection element. Furthermore, the present invention is also applicable to a liquid ejection head that employs a configuration in which an independent port communicating with the pressure chamber is formed only on one side of the ejection element, and liquid is supplied to the pressure chamber from one independent port. [Explanation of symbols]

[0056] 1 Liquid ejection head 10. Liquid ejection head substrate 11 Substrate 12 Discharge port forming member 23 Pressure chamber (liquid chamber) 31 Discharge element 37 Interlayer insulating film (insulating film) 38 Liquid-resistant insulating film 39 Independent port (communicating port)

Claims

1. A liquid ejection head including a substrate for a liquid ejection head provided with ejection elements that generate ejection energy for liquid, an ejection port forming member in which an ejection port for ejecting liquid is formed, and a liquid chamber formed between the substrate for the liquid ejection head and the ejection port forming member for containing liquid to be ejected from the ejection port, The liquid ejection head substrate is A substrate; an insulating film laminated on the substrate and insulating the ejection elements; a cavitation-resistant layer covering a position of the insulating film where the ejection elements are provided; a communication port formed in the substrate and the insulating film so as to communicate with the liquid chamber; a liquid-resistant insulating film having adhesion to the ejection port forming member; Equipped with A liquid ejection head characterized in that the liquid-resistant insulating film covers the surface of the insulating film on which the ejection port forming member is provided, and is continuously provided over a first portion that is in contact with the ejection port forming member, a second portion that covers the inner surface of the communication port formed in the insulating film, and a third portion that covers part of the cavitation-resistant layer.

2. A liquid ejection head as described in claim 1, characterized in that the communication port includes a first opening formed in the insulating film and a second opening communicating with a liquid flow path formed in the substrate, and the liquid-resistant insulating film is formed on the inner surface of the first opening.

3. 3. The liquid ejection head according to claim 1, wherein the liquid-resistant insulating film is an insulating film containing carbon atoms.

4. 4. The liquid ejection head according to claim 1, wherein the liquid-resistant insulating film is an insulating film containing carbon atoms in an amount of 5 atom % or more.

5. 5. A liquid ejection head according to claim 1, wherein the liquid-resistant insulating film is formed of a SiCN (silicon carbonitride) film, a SiOCN (silicon oxynitride) film, a SiOC (silicon oxycarbide) film, or a laminated film thereof.

6. 6. The liquid ejection head according to claim 1, wherein the ejection port forming member is made of a resin.

7. 7. The liquid ejection head according to claim 1, wherein the ejection port forming member is made of a laminated film in which a plurality of negative photosensitive resin layers are laminated.

8. 8. The liquid ejection head according to claim 7, wherein the resin layer in contact with the liquid-resistant insulating film, among the resin layers constituting the laminated film, contains a polyol.

9. 3. The liquid ejection head according to claim 2, wherein the first opening and the second opening are formed on at least one side of the ejection element.

10. the first opening and the second opening are formed on both sides of the ejection element, the first opening and the second opening formed on one side of the ejection element constitute a supply port for supplying liquid to the liquid chamber, 10. The liquid ejection head according to claim 9, wherein the first opening and the second opening formed on the other side of the ejection element constitute a recovery port for recovering the liquid from the liquid chamber.

11. 11. The liquid ejection head according to claim 10, wherein a second liquid-resistant insulating film is formed on an inner surface of the second opening and an inner surface of the liquid flow path.

12. The liquid ejection head according to claim 11 , wherein the second liquid-resistant insulating film covers the liquid-resistant insulating film formed on the inner surface of the first opening.

13. A liquid ejection head as described in claim 11 or 12, characterized in that the liquid-resistant insulating film is formed of a SiCN (silicon carbonitride) film, a SiOCN (silicon oxynitride) film, a SiOC (silicon oxycarbide) film or a laminated film thereof, and the second liquid-resistant insulating film is formed of a TiO (titanium monoxide) film.

14. A liquid ejection head described in any one of claims 1 to 13, wherein at least a portion of the cavitation-resistant layer is exposed from the liquid-resistant insulating film.

15. A liquid ejection head including a substrate for a liquid ejection head provided with ejection elements that generate ejection energy for liquid, an ejection port forming member in which an ejection port for ejecting liquid is formed, and a liquid chamber formed between the substrate for the liquid ejection head and the ejection port forming member for containing liquid to be ejected from the ejection port, The liquid ejection head substrate is A substrate; an insulating film laminated on the substrate and insulating the ejection elements; a cavitation-resistant layer covering a position of the insulating film where the ejection elements are provided; a communication port formed in the substrate and the insulating film so as to communicate with the liquid chamber; A liquid ejection head comprising a coating film continuously provided on a first portion covering the surface of the insulating film on which the ejection port forming member is provided and a portion of which is in contact with the ejection port forming member, a second portion covering the inner surface of the communication port formed in the insulating film, and a third portion covering a portion of the cavitation-resistant layer, the coating film being formed of a silicon compound containing carbon atoms.

16. 16. The liquid ejection head according to claim 15, wherein the coating film contains carbon atoms in an amount of 5 atom % or more.

17. 17. The liquid ejection head according to claim 15, wherein the coating film is formed of a SiCN (silicon carbonitride) film, a SiOCN (silicon oxycarbonitride) film, a SiOC (silicon oxycarbide) film, or a laminated film thereof.

18. A liquid ejection head described in any one of claims 15 to 17, wherein at least a portion of the cavitation-resistant layer is exposed from the coating film.

19. 19. The liquid ejection head according to claim 1, wherein the ejection port forming member is made of a resin.

20. A liquid ejection head as described in any one of claims 1 to 19, wherein the insulating film is provided with a circuit constituted by electrical wiring.

21. A liquid ejection head described in any one of claims 1 to 20, wherein the ejection element is a heating element for foaming the liquid by thermal energy.

22. A liquid ejection head described in any one of claims 1 to 21, wherein the cavitation-resistant layer includes an Ir layer.

23. A method for manufacturing a liquid ejection head including a substrate for a liquid ejection head on which ejection elements that generate ejection energy for liquid are formed, an ejection port forming member on which ejection ports for ejecting liquid are formed, and a liquid chamber formed between the substrate for the liquid ejection head and the ejection port forming member for containing liquid to be ejected from the ejection ports, comprising: laminating an insulating film on a substrate; forming the ejection elements and a cavitation-resistant layer covering the ejection elements on a surface of the insulating film; forming an opening in the insulating film at a side of the ejection element; a liquid-resistant insulating film forming step of forming a liquid-resistant insulating film having adhesion to the discharge port forming member so as to continuously cover a surface of the insulating film on which the discharge port forming member is provided, a part of the cavitation-resistant layer, and an inner surface of the opening; providing the ejection port forming member so as to be in contact with a portion of the liquid-resistant insulating film; A method for manufacturing a liquid ejection head, comprising:

24. A method for manufacturing a liquid ejection head as described in claim 23, wherein in the liquid-resistant insulating film formation process, the liquid-resistant insulating film is formed so that at least a portion of the cavitation-resistant layer is exposed from the liquid-resistant insulating film.

Citation Information

Patent Citations

  • Ink-jet printer head and production method therefor

    JP2001270121A

  • Etching method and method of manufacturing liquid discharge head substrate

    JP2016037625A

  • Method for manufacturing liquid discharge head and liquid discharge head

    JP2018138375A

  • Substrate junction body, method for manufacturing substrate junction body, liquid discharge head, and method for manufacturing liquid discharge head

    JP2018171911A

  • Method for producing laminate and method for producing liquid discharge head

    JP2018187789A