Wafer manufacturing method, acoustic wave device and manufacturing method thereof

By forming a bonding layer of aluminum nitride oxide and activating it with rare gas elements, the bonding strength between the substrate and piezoelectric substrate is enhanced, improving the reliability of acoustic wave devices.

JP7551371B2Active Publication Date: 2024-09-17TAIYO YUDEN KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020121523
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-15
Publication Date
2024-09-17
Estimated Expiration
2040-07-15

AI Technical Summary

Technical Problem

The bonding strength between the support substrate and the piezoelectric substrate in acoustic wave devices is insufficient, which affects the reliability of the device.

Method used

A bonding layer containing aluminum nitride oxide is formed on the surfaces of the substrate and piezoelectric substrate, and activated using rare gas element atoms or ions to enhance bonding strength, with the process involving reactive sputtering using an aluminum or aluminum alloy target and gases like nitrogen and oxygen.

Benefits of technology

The improved bonding strength between the substrate and piezoelectric substrate enhances the reliability and durability of the acoustic wave device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551371000004
    Figure 0007551371000004
  • Figure 0007551371000005
    Figure 0007551371000005
  • Figure 0007551371000003
    Figure 0007551371000003
Patent Text Reader

Abstract

To provide a manufacturing method of a wafer, an elastic wave device, and a manufacturing method of the same that can improve the bonding strength between a substrate 17 and a piezoelectric substrate 14.SOLUTION: The manufacturing method of a wafer includes the steps of forming a junction layer 13, mainly composed of aluminum nitride oxide, on at least one of a first surface of a substrate 17, which has a support substrate 10, and a second surface of a piezoelectric substrate 14, and activating a surface of the junction layer 13, and bonding the first surface of the substrate 17 and the second surface of the piezoelectric substrate 14 through the junction layer 13.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a wafer, an acoustic wave device, and a method for manufacturing the same, for example, to a method for manufacturing a wafer including a piezoelectric substrate, an acoustic wave device, and a method for manufacturing the same. [Background technology]

[0002] A surface acoustic wave device having an IDT (Interdigital Transducer) with a pair of comb electrodes on a piezoelectric substrate is known as an acoustic wave device used in communication devices such as smartphones. The surface acoustic wave device is used as a bandpass filter in a circuit that processes wireless signals in a frequency band of, for example, 45 MHz to 2 GHz.

[0003] It is known to activate the surfaces of a support substrate and a piezoelectric substrate, and then bond the support substrate and the piezoelectric substrate (for example, Patent Document 1). It is known to provide a hard layer between the support substrate and the piezoelectric substrate (for example, Patent Document 2). It is known to provide an aluminum oxynitride film at the bonding interface between a base substrate and a semiconductor substrate (for example, Patent Document 3). It is known to form a silicon oxide film and a bonding layer on a piezoelectric substrate, activate the surfaces of the bonding layer and the support substrate, and then bond the bonding layer to the support substrate (Patent Document 4). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2004-343359 A [Patent Document 2] JP 2008-028980 A [Patent Document 3] JP 2012-160713 A [Patent Document 4] International Publication No. 2017 / 163722 Summary of the Invention [Problem to be solved by the invention]

[0005] In Patent Document 4, the bonding strength between the support substrate and the piezoelectric substrate is improved by using aluminum nitride, alumina, etc. as a bonding layer. However, the bonding strength between the support substrate and the piezoelectric substrate is not sufficient.

[0006] The present invention has been made in consideration of the above-mentioned problems, and has an object to improve the bonding strength between a substrate and a piezoelectric substrate. [Means for solving the problem]

[0007] The present invention is a method for manufacturing a wafer, comprising the steps of forming a bonding layer primarily composed of aluminum oxide nitride on at least one of a first surface of a substrate having a support substrate and a second surface of a piezoelectric substrate, activating a surface of the bonding layer, and bonding the first surface and the second surface via the bonding layer.

[0008] In the above-described structure, the step of activating the surface of the bonding layer can include a step of irradiating the bonding layer with atoms or ions of a rare gas element.

[0009] In the above configuration, the substrate has the first surface and is provided with an intermediate layer mainly composed of silicon oxide, and the step of forming the bonding layer can be configured to include a step of forming the bonding layer in contact with the first surface.

[0010] In the above configuration, after the step of bonding the first surface and the second surface, the bonding layer can be in contact with the substrate and the piezoelectric substrate.

[0011] In the above-described structure, the step of forming the bonding layer can include a step of forming the bonding layer by a reactive sputtering method using an aluminum or aluminum alloy target, oxygen gas, and nitrogen gas.

[0012] In the above configuration, the piezoelectric substrate may be a lithium tantalate substrate or a lithium niobate substrate.

[0013] The above-described configuration may include, after the bonding step, a step of polishing or grinding the piezoelectric substrate to thin the piezoelectric substrate.

[0014] The present invention is a method for manufacturing an acoustic wave device, comprising the steps of forming a wafer using the above-described wafer manufacturing method, and forming an electrode on a surface of the piezoelectric substrate of the wafer opposite to the second surface.

[0015] The present invention relates to a support substrate and a Single crystal a piezoelectric substrate; an intermediate layer mainly composed of silicon oxide provided between the support substrate and the piezoelectric substrate; and a piezoelectric substrate and an intermediate layer provided between the piezoelectric substrate and the intermediate layer. ,before a bonding layer in contact with the intermediate layer and containing aluminum oxide nitride as a main component; an amorphous layer provided between the piezoelectric substrate and the bonding layer, the amorphous layer containing constituent elements of the piezoelectric substrate and the bonding layer and a rare gas element; The piezoelectric substrate is provided on a surface opposite to the bonding layer. , a comb-shaped electrode having a plurality of electrode fingers and an electrode. Effect of the Invention

[0016] According to the present invention, the bonding strength between the substrate and the piezoelectric substrate can be improved. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1(a) is a plan view of an acoustic wave resonator in accordance with a first embodiment, and FIG. 1(b) is a cross-sectional view taken along line AA of FIG. 1(a). [Diagram 2] 2(a) to 2(c) are cross-sectional views (part 1) illustrating a method for manufacturing the acoustic wave resonator in accordance with the first embodiment. [Diagram 3] 3(a) to 3(c) are cross-sectional views (part 2) illustrating the method for manufacturing the acoustic wave resonator in accordance with the first embodiment. [Figure 4] 4(a) to 4(c) are schematic diagrams showing a method for bonding substrates in the first embodiment. [Diagram 5] 5(a) and 5(b) are schematic diagrams of the wafers of Example 1 and Comparative Example 1, respectively, observed from above. [Figure 6] FIG. 6(a) is a diagram showing the XPS spectrum of nitrogen 1s in Experiment 2, FIG. 6(b) is a diagram showing the Al-NOx bond, and FIG. 6(c) is a diagram showing Ox-Al-N. [Figure 7] 7(a) to 7(c) are cross-sectional views illustrating a method for manufacturing an acoustic wave resonator according to a first modification of the first embodiment. [Figure 8] 8(a) to 8(c) are cross-sectional views illustrating a method for manufacturing an acoustic wave resonator according to a second modification of the first embodiment. [Figure 9] 9(a) to 9(c) are cross-sectional views illustrating a method for manufacturing an acoustic wave resonator according to a third modification of the first embodiment. [Figure 10] FIG. 10(a) is a circuit diagram of a filter in accordance with the second embodiment, and FIG. 10(b) is a circuit diagram of a duplexer in accordance with a first modified example of the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, embodiments of the present invention will be described with reference to the drawings. EXAMPLES

[0019] Fig. 1(a) is a plan view of an acoustic wave resonator according to a first embodiment, and Fig. 1(b) is a cross-sectional view taken along line AA of Fig. 1(a). The arrangement direction of the electrode fingers is the X direction, the extension direction of the electrode fingers is the Y direction, and the lamination direction of the support substrate and the piezoelectric substrate is the Z direction. The X direction, Y direction, and Z direction do not necessarily correspond to the X-axis direction and Y-axis direction of the crystal orientation of the piezoelectric substrate. When the piezoelectric substrate is a rotated Y-cut X-propagation substrate, the X direction is the X-axis direction of the crystal orientation.

[0020] 1(a) and 1(b), a piezoelectric substrate 14 is bonded onto a substrate 17 via a bonding layer 13. The substrate 17 includes a support substrate 10, a boundary layer 11, and a temperature compensation film 12. The temperature compensation film 12 is provided between the support substrate 10 and the piezoelectric substrate 14, and the boundary layer 11 is provided between the support substrate 10 and the temperature compensation film 12. The thicknesses of the support substrate 10, the boundary layer 11, the temperature compensation film 12, the bonding layer 13, and the piezoelectric substrate 14 are defined as T0, T1, T2, T3, and T4, respectively.

[0021] An acoustic wave resonator 26 is provided on the piezoelectric substrate 14. The acoustic wave resonator 26 has an IDT 22 and a reflector 24. The reflectors 24 are provided on both sides of the IDT 22 in the X direction. The IDT 22 and the reflector 24 are formed by the metal film 16 on the piezoelectric substrate 14.

[0022] The IDT 22 includes a pair of comb electrodes 20 facing each other. The comb electrodes 20 include a plurality of electrode fingers 18 and a bus bar 19 to which the plurality of electrode fingers 18 are connected. The region where the electrode fingers 18 of the pair of comb electrodes 20 intersect is an intersection region 25. The length of the intersection region 25 is the aperture length. The pair of comb electrodes 20 are provided facing each other such that the electrode fingers 18 are substantially alternated in at least a part of the intersection region 25. The acoustic wave excited by the plurality of electrode fingers 18 in the intersection region 25 propagates mainly in the X direction. The pitch of the electrode fingers 18 of one of the pair of comb electrodes 20 is substantially the wavelength λ of the acoustic wave. If the pitch of the plurality of electrode fingers 18 (the pitch between the centers of the electrode fingers 18) is D, the pitch of the electrode fingers 18 of one comb electrode 20 is the pitch D of two electrode fingers 18. The reflector 24 reflects the acoustic wave (surface acoustic wave) excited by the electrode fingers 18 of the IDT 22. As a result, the acoustic wave is confined within the intersection region 25 of the IDT 22.

[0023] The piezoelectric substrate 14 is a single crystal lithium tantalate (LiTaO3) substrate or a single crystal lithium niobate (LiNbO3) substrate, for example a rotated Y-cut X-propagation lithium tantalate substrate or a rotated Y-cut X-propagation lithium niobate substrate.

[0024] The support substrate 10 is, for example, a silicon substrate, a sapphire substrate, an alumina substrate, a spinel substrate, a quartz substrate, or a silicon nitride substrate. The silicon substrate is a single crystal or polycrystalline Si substrate, the sapphire substrate is a single crystal Al2O3 substrate, the alumina substrate is a polycrystalline or amorphous Al2O3 substrate, the spinel substrate is a polycrystalline MgAl2O4 substrate, the quartz substrate is a single crystal SiO2 substrate, and the silicon nitride substrate is a polycrystalline or amorphous SiN substrate. The linear expansion coefficient of the support substrate 10 in the X direction is smaller than the linear expansion coefficient of the piezoelectric substrate 14 in the X direction. This makes it possible to reduce the frequency temperature dependency of the acoustic wave resonator.

[0025] The temperature compensation film 12 has a temperature coefficient of elastic constant with the opposite sign to that of the piezoelectric substrate 14. For example, the temperature coefficient of the elastic constant of the piezoelectric substrate 14 is negative, and the temperature coefficient of the elastic constant of the temperature compensation film 12 is positive. The temperature compensation film 12 is, for example, a silicon oxide (SiO2) film with no additives or with an additive element such as fluorine, and is, for example, amorphous. This makes it possible to reduce the frequency temperature coefficient of the elastic wave resonator. When the temperature compensation film 12 is a silicon oxide film, the sound velocity of the bulk wave propagating through the temperature compensation film 12 is slower than the sound velocity of the bulk propagating through the piezoelectric substrate 14.

[0026] The boundary layer 11 is, for example, polycrystalline or amorphous, and is an aluminum oxide film, a silicon nitride film, or an aluminum nitride film. The sound velocity of the bulk wave propagating through the boundary layer 11 is faster than the sound velocity of the bulk wave propagating through the temperature compensation film 12. As a result, the elastic wave is confined within the piezoelectric substrate 14 and the temperature compensation film 12.

[0027] The bonding layer 13 is a layer that bonds the temperature compensation film 12 and the piezoelectric substrate 14, and is a polycrystalline or amorphous aluminum oxide nitride (AlON) film. The aluminum oxide nitride film is mainly composed of aluminum, nitrogen, and oxygen. The concentrations of aluminum, nitrogen, and oxygen are each, for example, 5 atomic % to 60 atomic %.

[0028] In order to make the energy of the elastic wave exist to some extent in the temperature compensation film 12, the thickness T4 of the piezoelectric substrate 14 is, for example, 1λ or less. In order to confine the elastic wave in the piezoelectric substrate 14 and the temperature compensation film 12, the thickness T2 of the temperature compensation film 12 is, for example, 1λ or less. The distance between the lower surface of the temperature compensation film 12 and the upper surface of the piezoelectric substrate 14 is, for example, 2λ or less. In order to confine the elastic wave in the piezoelectric substrate 14 and the temperature compensation film 12, the thickness T1 of the boundary layer 11 is, for example, 1λ or more. In order for the support substrate 10 to support other layers, the thickness T0 of the support substrate 10 is, for example, 50 μm or more. The thickness T3 of the bonding layer 13 is, for example, 5 nm or more to function as a bonding layer, and is 100 nm or less to not reflect the elastic wave.

[0029] The metal film 16 is a film mainly composed of, for example, aluminum (Al), copper (Cu) or molybdenum (Mo). Here, "mainly composed of a certain material" means that the material contains impurities, either intentionally or unintentionally, for example, 50 atomic % or more of a certain material, or 80 atomic % or more of the material. An adhesive film such as a titanium (Ti) film or a chromium (Cr) film may be provided between the electrode fingers 18 and the piezoelectric substrate 14. The adhesive film is thinner than the electrode fingers 18. An insulating film may be provided to cover the electrode fingers 18. The insulating film functions as a protective film or a temperature compensation film.

[0030] The wavelength λ of the elastic wave is, for example, 1 μm to 6 μm. When two electrode fingers 18 are considered as one pair, the number of pairs is, for example, 20 to 300 pairs. The duty ratio of the IDT 22 is a value obtained by dividing the thickness of the electrode fingers 18 by the pitch of the electrode fingers 18, and is, for example, 30% to 70%. The aperture length of the IDT 22 is, for example, 10λ to 50λ.

[0031] [Production method of Example 1] 2(a) to 3(c) are cross-sectional views showing a method for manufacturing the acoustic wave resonator according to the embodiment 1. As shown in Fig. 2(a), a boundary layer 11 and a temperature compensation film 12 are formed on a support substrate 10 by, for example, a chemical vapor deposition (CVD) method, a sputtering method, or a vacuum deposition method. In this way, a substrate 17 including the support substrate 10, the boundary layer 11, and the temperature compensation film 12 is formed.

[0032] As shown in FIG. 2(b), a bonding layer 13 is formed on the temperature compensation film 12. A reactive sputtering method is used to form the bonding layer 13. In the reactive sputtering method, the support substrate 10 is placed in the chamber of a sputtering device. A target made of aluminum or an aluminum alloy is placed facing the support substrate 10. In addition to the argon (Ar) gas in the chamber, nitrogen (N2) gas and oxygen (O2) gas are introduced. By applying high-frequency power, aluminum atoms sputtered from the target react with the nitrogen and oxygen and are deposited on the support substrate 10.

[0033] 2(c), atoms, ions, or the like are irradiated onto the upper surface of the bonding layer 13 and the lower surface of the piezoelectric substrate 14 (arrow 55), thereby activating the upper surface of the bonding layer 13 and the lower surface of the piezoelectric substrate 14.

[0034] As shown in Fig. 3(a), the upper surface of the bonding layer 13 is brought into contact with the lower surface of the piezoelectric substrate 14, and the upper surface of the bonding layer 13 is directly bonded to the lower surface of the piezoelectric substrate 14 at room temperature. As shown in Fig. 3(b), the upper surface of the piezoelectric substrate 14 is planarized using, for example, a chemical mechanical polishing (CMP) method. This results in a thickness of the piezoelectric substrate 14 of T4. A wafer 28 is completed in which the piezoelectric substrate 14 is laminated on the support substrate 10. As shown in Fig. 3(c), a metal film 16 is formed on the piezoelectric substrate 14, thereby forming an IDT 22 and a reflector 24 on the piezoelectric substrate 14.

[0035] 4(a) to 4(c) are schematic diagrams showing a method for bonding substrates in Example 1. As shown in FIG. 4(a), bonding layer 13 has bonding layer 13a and amorphous layer 13b. Bonding layer 13a is amorphous aluminum oxide nitride, and has atoms 50, which are aluminum atoms, nitrogen atoms, and oxygen atoms. Atoms 54 or ions are irradiated onto the upper surface of bonding layer 13 in a vacuum, as indicated by arrow 55. The region irradiated with atoms 54 or ions is amorphous layer 13b, and has atoms 50 and irradiated atoms 54.

[0036] As shown in FIG. 4(b), the piezoelectric substrate 14 has a piezoelectric layer 14a and an amorphous layer 14b. The piezoelectric substrate 14a is a single crystal piezoelectric substrate, and in the case of a lithium tantalate substrate, it has atoms 52 which are tantalum atoms, lithium atoms, and oxygen atoms, and in the case of a lithium niobate substrate, it has atoms which are niobium atoms, lithium atoms, and oxygen atoms. As indicated by arrow 55, atoms 54 or ions are irradiated onto the lower surface of the piezoelectric substrate 14 in a vacuum. The region irradiated with the atoms 54 or ions is the amorphous layer 14b, and has atoms 52 and the irradiated atoms 54.

[0037] In Fig. 4(a) and Fig. 4(b), the atoms 54 are inert elements (e.g., rare gas elements) such as argon (Ar), xenon (Xe), or krypton (Kr). The atoms 54 or ions are irradiated as an ion beam, a neutralized beam, or plasma. As a result, unbonded dangling bonds are formed on the upper surface of the amorphous layer 13b and the lower surface of the amorphous layer 14b (i.e., the upper surface of the amorphous layer 13b and the lower surface of the amorphous layer 14b are activated). When argon ions are used, for example, a surface activated bonding (SAB) device may be used.

[0038] As shown in FIG. 4(c), while maintaining a vacuum, the support substrate 10 and the piezoelectric substrate 14 are pressed as indicated by the arrow 56 to bond the amorphous layers 13b and 14b together. At this time, the dangling bonds formed on the surfaces of the amorphous layers 13b and 14b bond together to form a strong bond. This bonds the bonding layer 13 and the piezoelectric substrate 14 together. This bonding is performed at room temperature (for example, 100° C. or lower and −20° C. or higher, preferably 80° C. or lower and 0° C. or higher), so that thermal stress can be suppressed. Whether or not bonding is performed at room temperature can be confirmed by checking the temperature dependency of the residual stress. In other words, the residual stress is smallest at the bonding temperature.

[0039] The amorphous layer 13b is mainly composed of aluminum, nitrogen, and oxygen, which are the constituent elements of the bonding layer 13, which is an aluminum oxynitride film, and contains an element for surface activation (e.g., argon). The amorphous layer 14b is mainly composed of the constituent elements of the piezoelectric substrate 14 and contains an element for surface activation (e.g., argon). When the piezoelectric substrate 14 is a lithium tantalate substrate, the amorphous layer 14b is mainly composed of tantalum, lithium, and oxygen, and contains an element for surface activation (e.g., argon). When the piezoelectric substrate 14 is a lithium niobate substrate, the amorphous layer 14b is mainly composed of niobium, lithium, and oxygen, and contains an element for surface activation (e.g., argon).

[0040] The total thickness of the amorphous layers 13b and 14b is preferably greater than 0 nm, and more preferably 0.5 nm or more. This can improve the bonding between the bonding layer 13 and the piezoelectric substrate 14. The total thickness of the amorphous layers 13b and 14b is preferably 10 nm or less, and more preferably 5 nm or less. This can suppress deterioration of the characteristics of the acoustic wave resonator.

[0041] [Experiment 1] A wafer was produced in which a piezoelectric substrate 14 was bonded onto a support substrate 10. The production conditions were as follows. Support substrate 10: sapphire substrate with thickness T0 of 500 μm Boundary layer 11: Aluminum oxide (Al2O3) film with thickness T1 of 1.35 μm Temperature compensation film 12: Silicon oxide (SiO2) film with a thickness T2 of 0.3 μm Bonding layer 13: Example 1: Aluminum oxynitride film (AlON) film with thickness T3 of 20 nm Comparative Example 1: Aluminum oxide (Al2O3) film with thickness T3 of 10 nm Piezoelectric substrate 14: Lithium tantalate substrate with a thickness T4 of 0.6 μm Wafer size: 4 inches

[0042] In FIG. 2(a), the boundary layer 11 and the temperature compensation film 12 were formed by the CVD method. In FIG. 2(b), the bonding layer 13 was formed by reactive sputtering using an aluminum target and argon gas to which nitrogen gas and oxygen gas were introduced. In FIG. 2(c), the thickness of the piezoelectric substrate 14 was 180 μm. In FIG. 3(b), the upper surface of the piezoelectric substrate 14 was polished using the CMP method. In this way, the wafers 28 of Example 1 and Comparative Example 1 were produced. Three wafers 28 of Example 1 and one wafer 28 of Comparative Example 1 were produced.

[0043] After the piezoelectric substrate 14 was polished to a thickness T4, the wafer was observed from above. Figures 5(a) and 5(b) are schematic diagrams of the wafers of Example 1 and Comparative Example 1 observed from above, respectively. As shown in Figure 5(a), in Example 1, no peeling of the piezoelectric substrate 14 was observed in any of the three wafers 28. As shown in Figure 5(b), in Comparative Example 1, peeling 30 of the piezoelectric substrate 14 was observed around the periphery of the wafer 28.

[0044] [Experiment 2] An aluminum oxide nitride film having a thickness of 200 nm was formed on a silicon substrate having a thickness of 525 μm using the same film formation conditions as those for the bonding layer 13 in Example 1 of Experiment 1. The binding energy of nitrogen N at 1s was evaluated using XPS (X-ray Photoelectron Spectroscopy). Figure 6(a) is a diagram showing the XPS spectrum of nitrogen 1s in Experiment 2. The solid line indicates the XPS spectrum at a depth of about 20 nm from the surface, and the dashed line indicates the XPS spectrum at a depth of about 200 nm from the surface.

[0045] As shown in Figure 6(a), the solid and dashed spectra are almost the same, and the nitrogen in the aluminum oxide nitride film is in almost the same bond state regardless of the depth. The Ox-Al-N bond peak was observed, and the Al-NOx peak was hardly observed. Figure 6(b) shows the Al-NOx bond, and Figure 6(c) shows the Ox-Al-N bond. As shown in Figure 6(b), in the Al-NOx bond, there is an ON bond in addition to the Al-O bond and the Al-N bond. As shown in Figure 6(c), in the Ox-Al-N bond, the Al-O bond and the Al-N bond are predominant.

[0046] In Fig. 6(a), the Ox-Al-N bond is the main bond, which indicates that in the bonding layer 13, the main bonds are Al-O bonds and Al-N bonds, and there are almost no ON bonds. In addition, the atomic composition ratio of aluminum, nitrogen, and oxygen, Al:N:O, was approximately 4:2:4. This indicates that the bonding layer 13 is an AlON film, not Al2O3 and AlN.

[0047] When a silicon oxide film such as the temperature compensation film 12 is directly bonded to the piezoelectric substrate 14 using a surface activation method, the bonding strength is weakened. This is believed to be because the surface of the silicon oxide film is difficult to activate (i.e., dangling bonds are difficult to form). Therefore, by using an aluminum oxide film as the bonding layer 13 on the temperature compensation film 12 as in Comparative Example 1, the surface of the bonding layer 13 is easily activated, and the bonding strength between the temperature compensation film 12 and the piezoelectric substrate 14 can be improved. However, as in Comparative Example 1 of Experiment 1, the bonding strength between the temperature compensation film 12 and the piezoelectric substrate 14 is not sufficient. Therefore, an aluminum nitride oxide film is used as the bonding layer 13. This allows the bonding strength between the temperature compensation film 12 and the piezoelectric substrate 14 to be improved as in Experiment 1.

[0048] In Experiment 1, the reason why the bonding strength between the temperature compensation film 12 and the piezoelectric substrate 14 is improved by using an aluminum oxynitride film as the bonding layer 13 is not clear, but it may be considered as follows, for example. When aluminum oxide or aluminum nitride is used as the bonding layer 13, Al-O bonds are stable in Al2O3. Furthermore, Al-N bonds are stable in AlN. Therefore, even if the surface of the bonding layer 13 is activated, few dangling bonds are generated. On the other hand, when aluminum oxynitride is used as the bonding layer 13, the Al-O bonds and Al-N bonds in the bonding layer 13 are not as stable as the Al-O bonds in Al2O3 and the Al-N bonds in AlN, and when the surface of the bonding layer 13 is activated, few dangling bonds are generated even if the surface of the bonding layer 13 is activated. More dangling bonds are generated from Al2O3 and AlN. This is thought to improve the bonding strength between the bonding layer 13 and the piezoelectric substrate 14.

[0049] [Modification 1 of Example 1] 7(a) to 7(c) are cross-sectional views showing a method for manufacturing an acoustic wave resonator according to a first modification of the first embodiment. As shown in FIG. 7(a), a bonding layer 13c is formed on the upper surface of the temperature compensation film 12. A bonding layer 13d is formed on the lower surface of the piezoelectric substrate 14. The surfaces of the bonding layers 13c and 13d are activated as indicated by the arrows 55. As shown in FIG. 7(b), the bonding layers 13c and 13d are brought into contact with each other to be directly bonded. The bonding layers 13c and 13d form a bonding layer 13. As shown in FIG. 7(c), the piezoelectric substrate 14 is thinned, and then a metal film 16 is formed on the piezoelectric substrate 14. This forms an acoustic wave resonator having an IDT 22 and a reflector 24. As in the first modification of the first embodiment, the bonding layers 13c and 13d may be formed on both the upper surface of the temperature compensation film 12 and the lower surface of the piezoelectric substrate 14. The other configurations are the same as those of the first embodiment, and will not be described.

[0050] [Modification 2 of Example 1] 8(a) to 8(c) are cross-sectional views showing a method for manufacturing an acoustic wave resonator according to the second modification of the first embodiment. As shown in FIG. 8(a), the substrate 17 includes a support substrate 10 and an insulating layer 15 provided on the support substrate 10. The insulating layer 15 is, for example, an aluminum oxide film. A bonding layer 13 is formed on the lower surface of the piezoelectric substrate 14. As shown by the arrow 55, the surfaces of the insulating layer 15 and the bonding layer 13 are activated. As shown in FIG. 8(b), the bonding layer 13 and the insulating layer 15 are directly bonded by contacting each other. As shown in FIG. 8(c), the piezoelectric substrate 14 is thinned, and then a metal film 16 is formed on the piezoelectric substrate 14. This forms an acoustic wave resonator having an IDT 22 and a reflector 24. As in the second modification of the first embodiment, the bonding layer 13 may be formed on the lower surface of the piezoelectric substrate 14, and may not be formed on the upper surface of the substrate 17. When the insulating layer 15 is mainly composed of silicon oxide, the surface is less likely to be activated as described below. Therefore, when the bonding layer 13 is not formed on the upper surface of the insulating layer 15, it is preferable that the main component of the insulating layer 15 is not silicon oxide. The other configurations are the same as those in the first embodiment, and therefore the description will be omitted.

[0051] [Modification 3 of Example 1] 9(a) to 9(c) are cross-sectional views showing a method for manufacturing an acoustic wave resonator according to the third modification of the first embodiment. As shown in FIG. 9(a), the substrate 17 is a support substrate 10. A bonding layer 13 is formed on the upper surface of the support substrate 10. The surfaces of the bonding layer 13 and the piezoelectric substrate 14 are activated as indicated by the arrow 55. As shown in FIG. 9(b), the bonding layer 13 and the piezoelectric substrate 14 are brought into contact with each other to be directly bonded to each other. As shown in FIG. 9(c), the piezoelectric substrate 14 is thinned, and then a metal film 16 is formed on the piezoelectric substrate 14. This forms an acoustic wave resonator having an IDT 22 and a reflector 24. As in the third modification of the first embodiment, the substrate 17 is a support substrate 10, and the support substrate 10 and the piezoelectric substrate 14 may be bonded to each other only via the bonding layer 13. In FIG. 9(a), the bonding layer 13 may be formed on at least one of the upper surface of the support substrate 10 and the lower surface of the piezoelectric substrate 14. The other configurations are the same as those of the first embodiment, and therefore will not be described.

[0052] According to the first embodiment and its modified examples, as shown in FIG. 2(b), FIG. 7(a), FIG. 8(a), and FIG. 9(a), a bonding layer 13 mainly made of aluminum oxynitride is formed on at least one of the upper surface (first surface) of the substrate 17 having the support substrate 10 and the lower surface (second surface) of the piezoelectric substrate 14. As shown in FIG. 2(c), FIG. 7(a), FIG. 8(a), and FIG. 9(a), the surface of the bonding layer 13 is activated. As shown in FIG. 3(a), FIG. 7(b), FIG. 8(b), and FIG. 9(b), the upper surface of the substrate 17 and the lower surface of the piezoelectric substrate 14 are bonded via the bonding layer 13. In this way, by using aluminum oxynitride as the bonding layer 13, the bonding strength between the substrate 17 and the piezoelectric substrate 14 can be improved.

[0053] The term "mainly composed of aluminum oxynitride" means that it has Al-O bonds and Al-N bonds to such an extent that the bonding strength between the substrate 17 and the piezoelectric substrate 14 is improved, and may contain impurities intentionally or unintentionally. In order to improve the bonding strength between the substrate 17 and the piezoelectric substrate 14, the bonding layer 13 preferably contains aluminum, nitrogen, and oxygen in total of 80 atomic % or more, and preferably 90 atomic %. The bonding layer 13 preferably contains aluminum, nitrogen, and oxygen in total of 5 atomic % to 80 atomic %, and preferably 10 atomic % to 70 atomic %. Surface activation may not be performed on the surfaces of the upper surface of the substrate 17 and the lower surface of the piezoelectric substrate 14 on which the bonding layer 13 is not provided.

[0054] After the substrate 17 and the piezoelectric substrate 14 are bonded together, the bonding layer 13 comes into contact with the substrate 17 and the piezoelectric substrate 14. This makes it possible to improve the bonding strength between the substrate 17 and the piezoelectric substrate 14.

[0055] As in the first embodiment and its first modified example, the substrate 17 includes a temperature compensation film 12 (intermediate layer). The temperature compensation film 12 has the upper surface of the substrate 17 and is mainly composed of silicon oxide. The inventors have found through their experience that a layer mainly composed of silicon oxide is less likely to have dangling bonds even if the surface is activated. Therefore, a bonding layer 13 is formed in contact with the upper surface of the temperature compensation film 12. This can improve the bonding strength between the temperature compensation film 12 and the piezoelectric substrate 14.

[0056] The temperature compensation film 12 mainly contains silicon oxide. This means that it contains silicon and oxygen to the extent that it can function as the temperature compensation film 12, and impurities may be intentionally or unintentionally contained. The temperature compensation film 12 may contain, for example, fluorine. To function as the temperature compensation film 12, the temperature compensation film 12 preferably contains, for example, 50 atomic % or more of silicon and oxygen in total, and more preferably contains 80 atomic %. Furthermore, the temperature compensation film 12 preferably contains, for example, 10 atomic % to 90 atomic % each of silicon and oxygen, and more preferably contains 20 atomic % to 80 atomic % each of silicon and oxygen.

[0057] 3(c), 7(c), 8(c), and 9(c), electrodes such as the IDT 22 and the reflector 24 are formed on the top surface (the surface opposite to the second surface) of the piezoelectric substrate 14 of the wafer 28 manufactured in this manner. This makes it possible to manufacture an acoustic wave device in which the bonding strength between the substrate 17 and the piezoelectric substrate 14 is improved.

[0058] In the acoustic wave device manufactured in this manner, the temperature compensation film 12 is provided between the support substrate 10 and the piezoelectric substrate 14, and is mainly composed of silicon oxide. The bonding layer 13 is provided between the piezoelectric substrate 14 and the temperature compensation film 12, and is mainly composed of aluminum oxynitride in contact with the piezoelectric substrate 14 and the temperature compensation film 12. Electrodes such as the comb electrode 20 are provided on the upper surface of the piezoelectric substrate 14 (the surface opposite to the bonding layer 13).

[0059] The step of activating the surface of the bonding layer 13 preferably includes a step of irradiating the bonding layer 13 with atoms or ions of a rare gas element. This allows the surface of the bonding layer 13 to be activated.

[0060] In the process of forming the aluminum oxide nitride film as the bonding layer 13, the aluminum oxide nitride film is formed by reactive sputtering using an aluminum or aluminum alloy target, oxygen gas, and nitrogen gas. This makes it possible to form the bonding layer 13 having Al-N bonds and Al-O bonds. This makes it possible to improve the bonding strength between the substrate 17 and the piezoelectric substrate 14.

[0061] As shown in Fig. 3(b), the piezoelectric substrate 14 is polished or ground to reduce its thickness. At this time, the substrate 17 and the piezoelectric substrate 14 are likely to peel off from each other, as shown in Fig. 4(b). Therefore, it is preferable that the bonding layer 13 contains aluminum oxynitride as a main component. EXAMPLES

[0062] FIG. 10(a) is a circuit diagram of a filter according to a second embodiment. As shown in FIG. 10(a), one or more series resonators S1 to S3 are connected in series between an input terminal Tin and an output terminal Tout. One or more parallel resonators P1 and P2 are connected in parallel between the input terminal Tin and the output terminal Tout. The acoustic wave resonators according to the first embodiment and its modified examples can be used for at least one of the one or more series resonators S1 to S3 and the one or more parallel resonators P1 and P2. The number of resonators of the ladder filter can be set as appropriate. The filter may be a multimode filter.

[0063] [Modification 1 of Example 2] FIG. 10(b) is a circuit diagram of a duplexer according to a first modified example of the second embodiment. As shown in FIG. 10(b), a transmission filter 40 is connected between a common terminal Ant and a transmission terminal Tx. A reception filter 42 is connected between the common terminal Ant and a reception terminal Rx. The transmission filter 40 passes a signal in a transmission band among high-frequency signals input from the transmission terminal Tx to the common terminal Ant as a transmission signal, and suppresses signals of other frequencies. The reception filter 42 passes a signal in a reception band among high-frequency signals input from the common terminal Ant to the reception terminal Rx as a reception signal, and suppresses signals of other frequencies. At least one of the transmission filter 40 and the reception filter 42 can be the filter of the second embodiment.

[0064] Although a duplexer has been described as an example of a multiplexer, a triplexer or a quadplexer may also be used.

[0065] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0066] 10 Support substrate 11 Boundary layer 12 Temperature compensation membrane 13, 13c, 13d bonding layer 14 Piezoelectric substrate 15 Insulating layer 17 Substrate 20 comb electrode 22 IDT 26 Elastic Wave Resonator 28 Wafers

Claims

1. forming a bonding layer mainly made of aluminum oxynitride on at least one of a first surface of a substrate having a support substrate and a second surface of a piezoelectric substrate; activating a surface of the bonding layer; bonding the first surface and the second surface via the bonding layer; A method for manufacturing a wafer comprising the steps of:

2. The method for manufacturing a wafer according to claim 1 , wherein the step of activating the surface of the bonding layer includes the step of irradiating the bonding layer with atoms or ions of a rare gas element.

3. the substrate has the first surface and includes an intermediate layer mainly composed of silicon oxide; The method for manufacturing a wafer according to claim 1 , wherein the step of forming the bonding layer includes the step of forming the bonding layer in contact with the first surface.

4. The method for manufacturing a wafer according to claim 1 , wherein after the step of bonding the first surface and the second surface, the bonding layer contacts the substrate and the piezoelectric substrate.

5. 5. The method for manufacturing a wafer according to claim 1, wherein the step of forming the bonding layer includes a step of forming the bonding layer by using a reactive sputtering method using an aluminum or aluminum alloy target, oxygen gas, and nitrogen gas.

6. 6. The method for manufacturing a wafer according to claim 1, wherein the piezoelectric substrate is a lithium tantalate substrate or a lithium niobate substrate.

7. The method for manufacturing a wafer according to claim 1 , further comprising the step of thinning the piezoelectric substrate by polishing or grinding the piezoelectric substrate after the bonding step.

8. forming a wafer by using the wafer manufacturing method according to any one of claims 1 to 7; forming an electrode on a surface of the piezoelectric substrate of the wafer opposite the second surface; A method for manufacturing an acoustic wave device comprising the steps of:

9. A support substrate; a single crystal piezoelectric substrate provided on the support substrate; an intermediate layer mainly composed of silicon oxide, the intermediate layer being provided between the support substrate and the piezoelectric substrate; a bonding layer provided between the piezoelectric substrate and the intermediate layer, in contact with the intermediate layer, and containing aluminum oxynitride as a main component; an amorphous layer provided between the piezoelectric substrate and the bonding layer, the amorphous layer containing constituent elements of the piezoelectric substrate and the bonding layer and a rare gas element; an interdigital electrode having a plurality of electrode fingers, the interdigital electrode being provided on a surface of the piezoelectric substrate opposite the bonding layer;

Citation Information

Patent Citations

  • Method of manufacturing surface acoustic wave element

    JP2004343359A

  • Acoustic wave device, and method for manufacturing the same

    JP2008028980A

  • Manufacturing method for SOI substrate

    JP2012160713A

  • Thin film piezoelectric resonator and method for manufacturing the same

    WO2008032543A1

  • Bonding method

    WO2017163722A1