Rubber compositions for dynamic applications, methods for their manufacture, products containing same, and uses thereof - Patents.com
The rubber composition addresses the limitations of existing rubber compositions by forming segmented particles in situ through thermomechanical mixing, enhancing dynamic properties and maintaining static properties, suitable for dynamic applications.
Patent Information
- Application Number
- JP2021519138
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-10-09
- Filing Date
- 2019-10-08
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2039-10-08
AI Technical Summary
Existing rubber compositions for dynamic applications suffer from insufficient mechanical and dynamic properties due to the use of precursor prepolymers, which limit the synthesis of polyurethane-ureas to polar elastomers and result in undesirable Payne effects, particularly at low temperatures and dynamic strains.
A rubber composition is developed by reacting an elastomer with a reinforcing filler and a precursor of a polymer having urethane groups through thermomechanical mixing, followed by crosslinking, to form segmented particles in situ, minimizing Payne effects and maintaining static properties.
The composition achieves improved dynamic properties with reduced Payne effects and retained static properties over a wide temperature range, suitable for anti-vibration supports and elastic joints in vehicles and industrial equipment.
Smart Images

Figure 0007551602000043 
Figure 0007551602000039 
Figure 0007551602000026
Abstract
Description
Detailed Description of the Invention
[0001] The present invention relates to a rubber composition that can be used in mechanical parts with dynamic functions, a process for producing said composition, such parts, and the use of polymers containing urethane groups, which are applied in a non-limiting manner, in particular in mechanical parts selected from anti-vibration supports and elastic joints for electric vehicles or industrial equipment.
[0002] In a known manner, polyurethanes (PU) are obtained by reacting isocyanate (NCO) with alcohol (OH) functional groups to produce urethane functional groups (NHCOO).
[0003] Among polyurethanes typically produced by the reaction of a first precursor consisting of a polyisocyanate, a second precursor consisting of a long-chain polyol, and a polyol-type chain extender, segmented polyurethanes are known. Segmented polyurethanes contain flexible segments formed by the second precursor and rigid segments formed by the first precursor and the chain extender, and there is a mutually immiscible phase separation between these flexible and rigid segments.
[0004] WO-A1-2015 / 032681 relates to mixtures of thermoplastic polyurethanes with rubber, in particular for printing rollers, and in its examples exclusively discloses the in situ production of polyurethane-ureas mixed with nitrile rubber (NBR) by reacting the latter with a previously prepared single prepolymer incorporating two polyisocyanates and a macroglycol precursor together, and with a chain extender of the diamine type.
[0005] The main drawback of the polyurethane-ureas synthesized in the document is the use of precursor prepolymers, which limits the in situ synthesis of polyurethane-ureas to the use of polar elastomers (e.g. NBR) and the fact that the dispersions obtained from the polyurethane-ureas in NBR do not incorporate a minimum amount of reinforcing fillers, resulting in insufficient mechanical and, in particular, dynamic properties for the tested NBR / polyurethane-urea mixtures.
[0006] Non-isocyanate polyurethanes (NIPUs) are also known. They have been developed in recent years to overcome the toxicity and stability problems of isocyanates and therefore to obviate strict regulations regarding their use. These NIPUs are generally prepared by reacting an amine derivative with a cyclic carboxylate salt to produce a polyhydroxyurethane (PHU) according to the following reaction scheme:
[0007] [ka]
[0008] US 9 416 227 B2, for example, discloses the production of non-isocyanate microparticles from polyhydroxyurethanes.
[0009] Traditionally, the reinforcement of elastomers in rubber compositions is achieved by adding fillers (e.g. carbon black and / or silica) to improve the mechanical properties of said compositions, using, on the one hand, the elastomer-filler interaction, on the other hand, the reinforcing-reinforcing interaction, and hydrodynamic effects.
[0010] However, these filler-elastomer and filler-filler interactions give rise to an undesirable phenomenon, usually called the Payne effect, which is reflected by a nonlinearity (i.e. amplitude stiffening) and stiffening, especially at low temperatures, of the crosslinked rubber compositions subjected to dynamic stresses. This stiffening is accompanied by dynamic properties that may prove insufficient for the composition, due to the above-mentioned interactions with the reinforcing fillers used, which are usually related to the complex elastic shear modulus G of the composition at two dynamic strain amplitudes. * It can be evaluated by measuring the ratio of the storage modulus G' to the complexation modulus G * is the formula G * =G'+iG'' is defined as: G': G, also known as storage modulus or elastic modulus * where G' characterizes the stiffness or viscoelastic behavior of the composition (i.e., the energy stored and fully recovered); and G): Also known as the loss modulus, * where G'' characterizes the viscous behavior of the composition (i.e. the energy dissipated in the form of heat; it is noted that the ratio G'' / G' defines the tan δ loss factor).
[0011] This ratio typically corresponds to G' measured by dynamic mechanical analysis (DMA) at low dynamic amplitude to G' measured at high dynamic amplitude, the two moduli G' being measured at the same frequency and at the same temperature (e.g. G'0.5% / G'20%). In known methods, G'0.5% / G'20% is typically 1.80-2.00 for a rubber composition based on polyisoprene (IR) and reinforced with 40 phr (phr: parts by weight per 100 parts of elastomer) of N330 grade carbon black, so that it can be used in dynamic applications. In fact, it is known that in reinforced materials, the viscoelastic behavior starts at small dynamic strain amplitudes, with a substantial decrease in G' with a significant increase in strain.
[0012] In the course of recent research, the Applicant has sought to intensively minimize this Payne effect in crosslinked rubber compositions by minimizing the abovementioned ratio of storage modulus G'0.5% / G'20% so as to be as close as possible to 1.00, so that the storage modulus G' at a maximum strain of 20% is barely reduced below the storage modulus G' at a substantially zero strain of 0.5%, without compromising the static properties of the composition (especially with regard to the secant modulus and stiffness).As a result, it is possible to make these compositions particularly advantageous in dynamic applications.
[0013] An object of the present invention is therefore to propose a novel rubber composition which notably overcomes the above mentioned drawbacks, in particular by improving the dynamic properties of prior art rubber compositions while at the same time preserving the static properties of the prior art rubber compositions.
[0014] Surprisingly, this object is achieved by the applicant precisely by discovering that if an elastomer is reacted by thermomechanical mixing with a reinforcing filler, a precursor of a polymer having urethane groups and a chain extender, and then the product of this reaction is subsequently crosslinked under the specific conditions detailed below, it becomes possible to obtain in the resulting composition a fine and homogeneous dispersion in the elastomer of this polymer having urethane groups, segmented by being formed in situ in an elastomer matrix with minimized Payne effect and preserved static properties, in comparison with crosslinked rubber mixtures based on the same elastomer but not comprising the polymer having urethane groups, but instead having the same reinforcing filler in an amount increased by the amount of said polymer in the composition.
[0015] In other words, the rubber composition according to the invention is based on at least one elastomer, has a polymer having urethane groups dispersed in said at least one elastomer, and a reinforcing filler, said composition comprising the product of an in situ thermomechanical mixing reaction of said at least one elastomer with said reinforcing filler, a precursor of said polymer having urethane groups, and a chain extender.
[0016] According to the present invention, there is provided a composition usable for mechanical components having dynamic functions, in particular selected from anti-vibration supports and elastic joints for electric vehicles or industrial equipment, said composition having a complex shear modulus G that satisfies at least one of the following conditions (i) to (V): * with the ratio of storage modulus G'0.5% / G'20% to σ, G'0.5% and G'20% being measured according to standard ISO 4664 for double shear specimens subjected to shear strains of 0.02% to 50% at the same frequency of 5 Hz and the same temperature T, with dynamic strain amplitudes of 0.5% and 20%, respectively: (i) When T = 100°C, G'0.5% / G'20%≦1.15; (ii) When T = 65°C, G'0.5% / G'20%≦1.40; (iii) When T = 25°C, G'0.5% / G'20%≦1.50; (iv) When T = 0°C, G'0.5% / G'20%≦1.60; (v) When T = -30°C, G'0.5% / G'20% ≤ 2.50.
[0017] As used herein, the term "reinforcing filler" refers to any dispersed filler that is very finely divided in the elastomeric matrix of the composition (i.e., said at least one elastomer) and is capable of reinforcing the composition in particular to give it a secant modulus, a sufficiently high tensile strength and a sufficiently high stiffness; this filler may comprise at least one organic filler (e.g. carbon black) that is sufficiently reinforcing for the application under consideration, and / or at least one inorganic filler (e.g. silica) that is sufficiently reinforcing for the application under consideration.
[0018] The term "product of an in situ thermomechanical mixing reaction" as used herein refers to a mixture produced in a conventional manner by mechanical processing of the aforementioned components, including at least one thermal step during which said at least one elastomer is not only mixed with said reinforcing fillers, said precursors and said chain extenders, but also, preferably, with other additives conventionally used in rubber compositions, such as activator complexes (e.g. zinc oxide and stearic acid) and plasticizers (e.g. oils), with the exception of crosslinking systems (e.g. vulcanization with sulfur and accelerators) that are added to the non-crosslinked mixture obtained after this thermomechanical mixing, and is finally crosslinked in a known manner, as described below, with the aim of obtaining a composition according to the invention.
[0019] It should be noted that the crosslinked rubber composition according to the invention thus obtained forms an entangled network comprising a crosslinked elastomeric network incorporating the hard segments of the polymer containing urethane groups, and an organic reinforcing network comprising the flexible segments of the polymer, which are very finely dispersed in the elastomer and generally uniform, as will be explained below. The Applicant has discovered that this particular entanglement of the flexible and rigid segments, respectively, formed by the polymer thus dispersed, makes it possible to obtain the above-mentioned particularly advantageous conditions (i) to (v), at least one of which is fulfilled for the above-mentioned ratio G'0.5% / G'20%.
[0020] It should also be noted that these conditions (i)-(v) are evidence of a minimization (i.e., a significant reduction) of the Payne effect over a broad temperature range spanning from -30°C to 100°C, as compared to the Payne effect observed for a conventional crosslinked composition that does not include the polymer and that includes the same reinforcing filler in an amount increased by the amount of the polymer in the composition (all other components remaining unchanged).
[0021] It should also be noted that in the rubber composition according to the invention, the polymer containing urethane groups also exerts a reinforcing function on the rubber composition, as a complement to a certain amount of the reinforcing filler which it may partially replace, as demonstrated in the following examples which show that the static secant modulus, tensile strength and hardness properties are substantially preserved.
[0022] Advantageously, the composition of the invention may satisfy at least condition (i), and preferably also (ii), (iii), (iv) and (v), and said test specimen may be subjected to a preliminary mechanical conditioning of 0±4 mm, 50 mm / min, for 8 cycles.
[0023] According to a preferred embodiment of the present invention, the composition comprises 10 to 40 phr (phr: parts by weight per 100 parts of elastomer) of carbon black as reinforcing filler and 10 to 50 phr of said polymer having urethane groups, said composition preferably satisfying the following condition (ia): (ia) When T = 100°C, G'0.5% / G'20%≦1.12.
[0024] More preferably, the composition of the present invention comprises 15 to 30 phr of said carbon black (eg N330 grade) and 15 to 30 phr of said polymer having urethane groups.
[0025] According to another embodiment of the invention, the polymer having urethane groups can be dispersed in the at least one elastomer in the form of nodules having a larger number average transverse dimension (i.e., the diameter if the nodules were generally spherical) of 1 nm to 5 μm, preferably 50 nm to 2 μm, and more preferably 100 nm to 1 μm.
[0026] It should therefore be noted that this dispersion of said polymer in the continuous elastomeric matrix of the composition is advantageously fine and generally uniform, which contributes significantly to obtaining the above-mentioned mechanical properties of the compositions of the invention, including in particular their minimized Payne effect due to the reduction of said ratio G'0.5% / G'20%.
[0027] Generally, the compositions of the invention advantageously comprise: - at least one of the following secant moduli M100, M300, and M400 at strains of 100%, 300%, and 400%, respectively, measured in uniaxial tension according to standard ASTM D 412: M100 ≥ 1.5MPa, M300 ≧ 5.5MPa, and M400 ≥ 9.5MPa; and / or It may also have a tensile strength R / r, measured in uniaxial tension of at least 26 MPa, according to standard ASTM D 412.
[0028] It is noted that these static properties of the composition are advantageously close to those exhibited by a conventional crosslinked composition not including said polymer and including the same reinforcing filler, such as, for example, N330 grade carbon black, but in an amount increased by the amount of said polymer in the composition (all other components remaining unchanged).
[0029] Advantageously, the composition according to the invention may have a Shore A hardness, measured according to standard ASTM D 2240, of at least 48, preferably between 50 and 55.
[0030] Generally, for the composition according to the invention, the at least one elastomer is a rubber, advantageously chosen from diene or non-diene elastomers, excluding silicone rubbers, and the composition comprises a crosslinking system, for example with sulphur, capable of reacting with the product of the in situ thermomechanical mixing reaction, in order to co-crosslink the at least one elastomer and the polymer bearing urethane groups.
[0031] Preferably, said at least one elastomer is a non-polar diene elastomer, more preferably selected from natural rubber (NR), polyisoprene (IR), polybutadiene (BR) and styrene-butadiene copolymer (SBR). It is noted that the use of a non-polar diene elastomer in particular, in contrast to polar diene elastomers such as nitrile rubber (NBR) tested in WO-A1-2015 / 032681, makes it possible to obtain an improved dispersion (both in terms of fineness and uniformity) of the polymer carrying urethane groups in the non-polar elastomer, thus improving the dynamic properties of the composition by minimizing the ratio G'0.5% / G'20% and the Payne effect observed for this composition.
[0032] Also generally, for the composition according to the invention, the polymer containing urethane groups is advantageously a rigid segment, which may be present in the polymer in a mass fraction between 20% and 40%, preferably between 25% and 35%, and which comprises the chain extender and a first of the precursors; and - a flexible segment, comprising a second said precursor, which is a diene polymer having functionalized chain ends, preferably a functionalized polybutadiene, The polymer having urethane groups is co-crosslinked with the at least one elastomer through the double bonds of the second precursor to form a three-dimensional network connected with the at least one elastomer through covalent bonds.
[0033] It should be noted that this particular mass fraction of the rigid segments in the polymer is preferential due to the fact that it contributes to minimizing the ratio G'0.5% / G'20% without compromising the above-mentioned static properties of the composition of the invention.
[0034] It should also be noted that the chemical co-crosslinking according to the invention (for example co-vulcanization for crosslinking with sulfur) of the polymer bearing urethane groups with said at least one elastomer is made possible by the double bonds present in said second precursor, making it possible to better reinforce the composition by covalent bonds and reduce the Payne effect therein, compared to compositions in which the polymer bearing urethane groups is bonded to the elastomer only via weak energetic bonds of the van der Waals type.
[0035] According to a preferred feature of the invention, the first precursor and the second precursor form two separate reactants for the in situ thermomechanical mixing reaction with the at least one elastomer, the reinforcing filler and the chain extender, and the precursors do not form a precursor prepolymer.
[0036] In other words, contrary to the use of precursor prepolymers in the examples of WO-A1-2015 / 032681, which limit the dispersion of the polyurethane-urea in the NBR polar elastomer by sacrificing the quality of this dispersion, the two precursors according to the invention are preferably added separately to the elastomer in order to carry out the thermomechanical mixing.
[0037] It should be noted that this separate reaction of the at least one elastomer with the two precursors added separately contributes to improving the quality of the dispersion obtained from the polymer with urethane groups in an elastomer matrix, both in terms of fineness and homogeneity.
[0038] More preferably, said chain extender has a molar mass equal to or less than 700 g / mol, preferably less than 600 g / mol.
[0039] It is also noted that said chain extenders are advantageously characterized by a short chain.
[0040] According to a first embodiment of the invention, the polymer containing urethane groups belongs to the family of polyurethanes (PU) obtained from isocyanate compounds, excluding polyurethane-ureas such as those synthesized in the examples of WO-A1-2015 / 032681.
[0041] According to this first embodiment of the invention: said first precursor may be a polyisocyanate having a functionality greater than 2, preferably chosen from monomers or prepolymers based on 4,4'-methylenebis(phenylisocyanate), isophorone diisocyanate, hexamethylene diisocyanate and 4,4'-diphenylmethylene diisocyanate; said second precursor may be a diol-functionalized diene polymer having a functionality greater than 2, preferably a non-hydrogenated hydroxytelechelic polybutadiene having a number average molecular weight between 1000 and 3000 g / mol and a functionality greater than or equal to 2.2; said chain extender may be a polyol chosen from diols and triols (short-chain polyols) having a molar mass less than or equal to 300 g / mol, and preferably chosen from cyclohexanedimethanol, isosorbide and glycerol.
[0042] According to a preferred embodiment of the first aspect of the present invention: said at least one elastomer is advantageously a non-polar diene elastomer, preferably chosen from natural rubber (NR), polyisoprene (IR), polybutadiene (BR) and styrene-butadiene copolymers (SBR); - the reinforcing filler comprises carbon black (for example grade N330) present in the composition in an amount ranging from 15 to 30 phr (phr: parts by weight per 100 parts of elastomer); said polymer containing urethane groups is advantageously present in the composition in an amount ranging from 15 to 30 phr, and The total amount of said carbon black and said polymer having urethane groups in said composition is advantageously between 35 and 55 phr.
[0043] According to a preferred embodiment of the first embodiment of the invention, the composition satisfies the following condition (ia): (ia) When T = 100°C, G'0.5% / G'20%≦1.12.
[0044] According to a second embodiment of the invention, the polymer containing urethane groups belongs to the family of polyhydroxyurethanes obtained without isocyanates (NIPU).
[0045] According to this second embodiment of the invention: said first precursor may be a polyamine chosen from diamines and triamines, preferably chosen from 1,3-cyclohexanebis(methylamine), xylylenediamine, 2,2′-(ethylenedioxy)bis(ethylamine) and tris(2-aminoethyl)amine; said second precursor is a diene polymer functionalized with cyclocarbonate chain ends, preferably a polybutadiene functionalized with two carbonate end rings, each of which is 5 or 6 members, said chain extenders are cyclic carbonates having a molar mass less than or equal to 500 g / mol (i.e. short chain) and may preferably be chosen from cyclohexane biscarbonate, resorcinol biscarbonate, glycerol tricarbonate and phloroglucinol tricarbonate.
[0046] According to a preferred embodiment of this second embodiment of the invention: said at least one elastomer is advantageously a non-polar diene elastomer, preferably chosen from natural rubber (NR), polyisoprene (IR), polybutadiene (BR) and styrene-butadiene copolymers (SBR); - the reinforcing filler comprises carbon black (for example N330 grade) present in the rubber composition in an amount of 15 to 30 phr (phr: parts by weight per 100 parts of elastomer); the polymer having urethane groups is present in the rubber composition in an amount of 15 to 30 phr; The total amount of the carbon black and the polymer having a urethane group in the rubber composition is 35 to 55 phr.
[0047] According to this preferred embodiment of the second embodiment of the present invention, the rubber composition may advantageously satisfy at least one of the following (ia) to (va), preferably all of the following (ia) to (va): (ia) When T = 100°C, G'0.5% / G'20%≦1.12; (ii-a) When T = 65°C, G'0.5% / G'20%≦1.20; (iii-a) When T = 25°C, G'0.5% / G'20%≦1.30; (iv-a) When T = 0°C, G'0.5% / G'20%≦1.40; (va)When T = -30°C, G'0.5% / G'20%≦1.50.
[0048] According to this preferential example of the second embodiment, the rubber composition more advantageously satisfies at least one of the following conditions (ib) to (vb), and preferably also all of the following conditions (ib) to (vb): (ib) When T = 100°C, G'0.5% / G'20%≦1.10; (ii-b) When T = 65°C, G'0.5% / G'20%≦1.15; (iii-b) When T = 25°C, G'0.5% / G'20%≦1.20; (iv-b) When T = 0°C, G'0.5% / G'20%≦1.25; (vb) When T = -30°C, G'0.5% / G'20%≦1.40.
[0049] The mechanical member with dynamic function according to the invention is selected from anti-vibration supports and in particular elastic joints for electric vehicles or industrial equipment, said member comprising at least one elastic member made of the rubber composition defined above, adapted to be subjected to dynamic stresses.
[0050] The process according to the invention for producing the rubber composition defined above comprises the following steps: a) forming a non-crosslinked mixture comprising the polymer having urethane groups dispersed in the at least one elastomer via the thermomechanical mixing reaction of the reinforcing filler, the precursor and the chain extender, the reaction being preferably carried out in an internal mixer at a maximum temperature of 130° C. to 180° C.; b) adding a crosslinking system to the crosslinkable mixture thus obtained, accompanied by mechanical processing of said mixture, preferably carried out in an open mill at a maximum temperature of less than 80° C., then c) crosslinking the crosslinkable mixture by vulcanization in a press at a temperature between 130°C and 180°C, preferably by compression molding, in which the polymer bearing urethane groups is chemically co-crosslinked with the at least one elastomer, forming covalent bonds with said elastomer.
[0051] It should be noted that this chemical co-crosslinking makes it possible to satisfactorily toughen the resulting composition while minimizing the Payne effect of the composition, and that this co-crosslinking is made possible by the double bonds carried by said second precursor and by the use of a functionality of more than two for each of the first and second precursors.
[0052] It should also be noted that the thermomechanical mixing of step a) can include at least one thermal step, the minimum temperature of which can be reached and the maximum temperature of which can be between 130° C. and 180° C., preferably between 140° C. and 170° C. Suitable mixing times vary proportionally as a function of the operating conditions adopted by the person skilled in the art, in particular the temperature selected, as well as the nature and volume of the components subjected to the thermomechanical work.
[0053] Preferably, said at least one elastomer, said polymer having urethane groups, is segmented into rigid segments comprising said chain extender and said first precursor, and flexible segments comprising said second precursor, forming said first precursor and second precursor, which are added separately in step a).
[0054] It should be noted that the initial introduction of the at least one elastomer, preferably a non-polar diene elastomer, into the internal mixer makes it possible to sufficiently plasticize this elastomer and facilitate the incorporation of the other components that are subsequently added into the elastomer matrix.
[0055] More preferably, the total mass fraction of the first precursor and the chain extender in the polymer having a urethane group formed in step a) is 20% to 40%, and preferably 25% to 35%.
[0056] According to another embodiment of the present invention, In order to reduce the Payne effect of the composition at all temperatures T between -30°C and 100°C in comparison with a rubber mixture based on the at least one elastomer that does not have the polymer having urethane groups and has the reinforcing filler in the composition and a phr of the reinforcing filler equal to the total phr of the polymer having urethane groups, the Payne effect is reduced by the complex shear modulus G * is determined by the ratio G'0.5% / G'20% of the storage coefficient G' to A polymer having urethane groups is used, dispersed in a rubber composition based on at least one elastomer, via an in situ thermomechanical mixing reaction of at least one elastomer, a reinforcing filler, a precursor of said polymer and a chain extender.
[0057] According to this use of the invention, In comparison with the rubber composition not having the polymer having urethane groups and having a phr of the carbon black equal to the total phr of the composition having the polymer and the carbon black, In order to reduce the ratio G'0.5% / G'20% to more than 40% and, additionally, also maintain the Shore A hardness of the composition within 15%, a rubber composition having 10 to 50 phr of the polymer having urethane groups and 10 to 40 phr of carbon black as reinforcing filler (phr: parts by weight per 100 parts of elastomer) can be advantageously used.
[0058] Other characteristics, advantages and details of the invention will become apparent from reading the following description of some embodiments of the invention, given by way of non-limiting example with reference to the accompanying drawings, in which: BRIEF DESCRIPTION OF THE DRAWINGS [Regarding one embodiment of the present invention (PU)] FIG. 1 is a graph showing the secant elastic moduli M100, M300 and M400, Shore A hardness and the ratio G'0.5% / G'20% at 100° C. of an unreinforced rubber composition, a known mixture reinforced with 40 phr of carbon black, a rubber composition not in accordance with the invention that is not reinforced (i.e. does not contain rigid segments (hereinafter RS)) and has 40 phr of PU without chain extenders, and a rubber composition not in accordance with the invention that does not contain RS and has 20 phr of PU and 20 phr of carbon black, FIG. 2 is a graph illustrating the effect of adding a glycerol chain extender to M100, M300 and M400, the tensile strength R / r, Shore A hardness and G'0.5% / G'20% at 100° C. for said known mixture reinforced with 40 phr of carbon black, another known mixture reinforced with 20 phr of carbon black, said compound not according to the invention and a composition I1 according to the invention having 20 phr of PU with 30% by weight of RS and 20 phr of carbon black, FIG. 2a is a graph showing the influence of the functionality and degree of unsaturation of the second precursor on M100, M300 and M400 and R / r for a known mixture with 40 phr of carbon black, two mixtures not according to the invention comprising 20 phr of carbon black and 20 phr of PU derived from a first precursor according to the invention but from a second precursor not according to the invention, and a composition I1′ according to the invention comprising 20 phr of carbon black and 20 phr of PU derived from said first precursor but from a second precursor according to the invention, FIG. 3 is a graph showing the effect of various chain extenders on M100, M300 and M400, tensile strength R / r, Shore A hardness and G'0.5% / G'20% at 100° C. for a known mixture reinforced with 40 phr carbon black, another known mixture reinforced with 20 phr carbon black and three compositions according to the invention I2, I3 and I1 with 30% by mass of RS, 20 phr of three PUs each with CDM, isosorbide and glycerol chain extenders (see schematic formula) and 20 phr of carbon black, for the same polyisocyanate (Suprasec 2015) and polyol (polyBd R20 LM) precursors as in composition I1; FIG. 4 is a graph showing the effect of various polyisocyanate precursors on M100, M300 and M400, R / r, Shore A hardness and G'0.5% / G'20% at 100° C. for a known mixture reinforced with 40 phr carbon black, another known mixture reinforced with 20 phr carbon black, the polyisocyanate Suprasec 2015 and three other compositions according to inventions I4, I5 and I6 with 20 phr carbon black and three other PUs, but obtained with IPDI, HDI and 4,4'-MDI polyisocyanates, respectively (see schematic formula), with the same CHDM chain extender and polyol precursor (polyBd R20 LM); FIG. 5 is a graph showing the ratio G'0.5% / G'20% obtained at various temperatures ranging from −30° C. to 100° C. for known mixtures reinforced with 40 phr of carbon black and for compositions I1, I2, I3, I4, I5 and I6, 6, 7, 8, 9, and 10 are atomic force microscopy (AFM) images obtained in the "tapping" mode for compositions I2, I3, I1, I4, and I5, where for each composition the left image is a topographical map and the right image is a phase image; [Regarding the second embodiment of the present invention (NIPU)] FIG. 11 is a graph showing the effect of various cyclic carbonate (hereafter abbreviated CC) chain extenders on M100, M300, and M400, R / r, Shore A, and G'0.5% / G'20% at 100° C., for the same first polyamine precursor (1,3-cyclohexanebis(methylamine), abbreviated CHMA), and the same second polycyclocarbonate precursor (cyclocarbonate-terminated polybutadiene), for a known mixture reinforced with 40 phr of carbon black, another known mixture reinforced with 20 phr of carbon black, and four compositions according to compositions I7, I8, I9, and I10 having 20 phr of five NIPUs and 20 phr of carbon black, obtained with CyclohexanebisCC, ResorcinolbisCC, GlycerolTriCC, and PhloroglucinolTriCC extenders (see schematic formulas), respectively; FIG. 12 is a graph showing the effect of various polyamine precursors on M100, M300 and M400, R / r, Shore A and G'0.5% / G'20% at 100° C. for the known mixture reinforced with 40 phr of carbon black, the known mixture reinforced with 20 phr of carbon black, composition I10 having CHMA extender, and three other compositions according to the invention I11, I12 and I13 having 20 phr of three NIPUs, 20 phr of carbon black, obtained with polyamines, xylylenediamine, EDEA and TAEA (see schematic formula), respectively, with the same phloroglucinol tri-CC chain extender and the same polycyclocarbonate second precursor (cyclocarbonate terminated polybutadiene); FIG. 13 is a graph showing the G'0.5% / G'20% obtained at various temperatures ranging from −30° C. to 100° C. for known mixtures having 40 phr carbon black and compositions I7, I8, I9, I10, I11, I12, and I13; and 14, 15, 16, 17, 18, 19, and 20 are atomic force microscope (AFM) images obtained in the "tapping" mode for compositions I7, I8, I9, I10, I11, I12, and I13, respectively, where the image on the left is a topographical map and the image on the right is a phase map for each composition.
[0059] In all these examples of mixtures and compositions thus presented, the elastomeric matrix used is the same synthetic polyisoprene, known as IR Nipol 2200, and N330 carbon black is used as reinforcing filler, the components of which are identified in the following table (expressed in phr: parts by weight per 100 parts of IR):
[0060] In a first embodiment of the invention, illustrated in FIGS. 1 to 10, the PU was obtained in situ with the following first and second precursors according to the invention for compositions I1, I2 and I3:
[0061] [ka]
[0062] The PUs for compositions I4, I5 and I6 according to the invention were obtained with the same secondary precursor PolyBd R20 LM, but with different primary precursors IPDI, HDI and 4,4'-MDI having the formula shown in FIG. 4.
[0063] In a second embodiment of the invention shown in Figures 11 to 20, NIPUs were obtained in situ with the following first and second precursors for compositions I7, I8, I9, and I10 according to the invention.
[0064] -1,3-cyclohexanebis(methylamine) (abbreviated as cyclohexamine or CHMA in the table below) and -Cyclocarbonate-terminated polybutadiene (abbreviated as PolyBd-CC).
[0065] NIPUs for compositions I11, I12, and I13 were obtained with the same second precursor, but with different first precursors, xylylenediamine, EDEA, and TAEA, having the formulas shown in FIG.
[0066] Regarding the steps used to obtain all of the compositions I1 to I13 according to the invention, the following experimental protocol was followed.
[0067] Polyisoprene / polymer mixtures with urethane groups (PU or NIPU) were prepared using a Haake internal mixer for a thermomechanical mixing process, followed by a Polymix open roll mill for incorporating a crosslinking system into the resulting mixture.
[0068] The elastomer was first introduced into the internal mixer to facilitate plasticization and the incorporation of the other ingredients. The nominal temperature was then 55°C and the rotor speed was 45 rpm. After mixing for 1.5 minutes, the activator complex consisting of stearic acid and ZnO (Silox 3C), oil (Plaxolene 50) and N330 carbon black were added. After 1 minute, the first and second precursors were introduced into the internal mixer. As the two precursors were liquid, the mechanical mixing torque was significantly reduced upon their incorporation and it was necessary to wait for the purification of the PU or NIPU to increase the mechanical torque again. The material was then heated by increasing the rotor speed present in the Haake mixer and the mixture was collected when it reached 150°C.
[0069] The crosslinking system was then added to the Polymix open mill and the roller temperature was set at 40° C. The vulcanization of the resulting crosslinkable composition was then carried out by compression molding under a hydraulic press at 150° C.
[0070] For the measurement of the static properties of the compositions, including the secant modulus M100, M300 and M400, the tensile strength R / r (shown successively from left to right for each material in the attached graph) and the Shore A hardness, uniaxial tensile tests were carried out according to ISO 37: with an Instron 5565 dynamometer at 23° C., a force cell of 10 kN, a processing speed of 500 mm / min. The dumbbell specimens used were of the H2 type (working length=25 mm, width=4 mm, thickness=2 mm).
[0071] For the determination of the dynamic properties of the compositions and in particular the ratio G'0.5% / G'20%, which indicates the Payne effect for different rubber mixtures and compositions, the process was carried out at different temperatures (-30, 0, 25, 65 and 100 °C) using a Metravib DMA+1000 machine. To do this, 1 / 2 QC double shear specimens were used. The specimens were subjected to shear strains ranging from 0.02% to 50% at a frequency of 5 Hz. A preliminary mechanical conditioning (0 ± 4 mm, 50 mm / min, 8 cycles) was carried out. Their storage modulus G' was measured according to the standard ISO 4664 of 2005 (validated in 2011).
[0072] [Table 1]
[0073] [Table 2]
[0074] [Table 3]
[0075] [Table 4]
[0076] [Table 5]
[0077] [Table 6]
[0078] [Table 7]
[0079] [Table 8]
[0080] [Table 9]
[0081] [Table 10]
[0082] [Table 11]
[0083] As can be seen in FIG. 1, the unreinforced mixture with 40 phr of in situ synthesized PU has improved modulus compared to the mixture without unreinforced PU, but does not reach the modulus criteria of the mixture with 40 phr of carbon black. However, the Payne effect of the unreinforced mixture with 40 phr of PU is greatly reduced compared to the Payne effect of the mixture with 40 phr of carbon black instead of PU. A non-inventive composition with "mixed reinforcement" of in situ synthesized carbon black + PU without RS can have a Payne effect comparable to the unreinforced mixture with 40 phr of PU, while at the same time having better static properties than said unreinforced mixture (see G'0.5% / G'20% of 1.05, much less than 1.94 equivalent to the mixture with 40 phr of carbon black).
[0084] As can be seen in Figure 2, the addition of chain extenders allows a further improvement of the static properties through the formation of rigid segments (RS) in the in situ synthesized PU, by notably increasing the elastic modulus and hardness of the composition. At a RS mass content of 30%, composition I1 reveals that it achieves the same level of hardness as the reference mixture (loaded with 40 phr carbon black) and, in addition, shows a very reduced Payne effect (G'0.5% / G'20% of 1.08) compared to the reference mixture.
[0085] As can be seen in Figure 3, the choice of the structure of the selected chain extender and therefore of the properties of the rigid elements obtained in the elastomeric matrix makes it possible to modify the mechanical properties of compositions I1, I2 and I3, for the same polyisocyanate (Suprasec 2015) and the same 30% RS mass, while having a hardness close to or identical to that of the reference mixture, and also a low Payne effect (see that the ratio G'0.5% / G'20% at 100 °C is always less than 1.12 or even less than 1.10).
[0086] As can be seen in Figure 4, by choosing the structure of the polyisocyanate (identical to the CHDM chain extender), it is also possible to modify the mechanical properties of compositions I2, I4, I5 and I6. The Payne effect at 100°C remains low for I2, I4, I5 and I6 (see the ratio G'0.5% / G'20% being less than or equal to 1.12), which is much lower compared to the Payne effect of the reference mixture.
[0087] As can be seen in FIG. 5, which shows the dynamic properties measured at various temperatures (−30° C., 0° C., 25° C., 65° C., and 100° C.) for compositions I1 to I6, the Payne effect is significantly reduced for these compositions I1 to I6 compared to the reference mixture.
[0088] In conclusion, the above results show that the dynamic properties of the compositions according to the first embodiment of the invention are significantly improved compared to the prior art represented by the reference mixture (containing 40 phr carbon black and no PU), which advantageously allows these compositions to be used in dynamic applications and in a wide temperature range extending from -30°C to 100°C.
[0089] 6 to 10 show that the PU obtained in situ as described above is very finely and relatively uniformly dispersed in the polyisoprene in the form of nodules having large number-average transverse dimensions ranging from 50 nm to 2 μm, or even 100 nm to 1 μm, which contributes to obtaining the above-mentioned mechanical properties of the composition of the invention, including in particular a minimized Payne effect.
[0090] In summary, this chemical reinforcement of the elastomeric matrix with an entangled PU network allows compositions I1 to I6 to maintain their mechanical properties (elastic modulus and hardness) compared to the reference blend, while at the same time minimizing their nonlinearity (dynamic stiffness) compared to the reference blend.
[0091] The effect of the functionality and ethylenic unsaturation of the second precursor on the mechanical properties obtained for the composition was further studied by using the same specific masterbatch, the formula of which is that of the non-reinforced control rubber mixture detailed in Table 1 above, to prepare the following: - A known control rubber mix reinforced with 40 phr of N330 carbon black added to the masterbatch; a composition I1' according to the invention comprising, in addition to the masterbatch, 20 phr of N330 carbon black and 20 phr of PU derived from a first MDI precursor "Suprasec 2015", a hydroxytelechelic polybutadiene (Mn=2800 g / mol, functionality=2.5) known as "PolyBd-OH R45 HTLO" as a second precursor and the abovementioned CHDM as chain extender; - rubber mixture No. 1 not according to the invention, containing, in addition to the masterbatch, 20 phr of N330 carbon black and 20 phr of PU derived from a first MDI precursor "Suprasec 2015", CHDM as chain extender and a hydroxytelechelic polybutadiene "Krasol LBH 2000" (with Mn=2100 g / mol and functionality equal to 1.9) as a second precursor; and - rubber mixture No. 2 not according to the invention, comprising, in addition to the masterbatch, 20 phr of N330 carbon black and 20 phr of PU derived from a first MDI precursor "Suprasec 2015", CHDM as chain extender and a hydrogenated hydroxytelechelic polybutadiene "Krasol HLBH-P 2000" (Mn=2100 g / mol and functionality equal to 1.9) as a second precursor.
[0092] Composition I1' and the three mixtures mentioned above were prepared with 1.6 equivalents of vulcanizing agent (see Table 1) as the crosslinking system and PU with 30% rigid segment RS as described above for compositions I1 to I6. Table 12 below summarizes the formulas used as the masterbatch raw materials for I1' and mixtures No. 1 and No. 2.
[0093] [Table 12]
[0094] As can be seen in FIG. 2a, the second precursor Krasol LBH 2000 gives a significantly lower tensile modulus for mixture No. 1 than that of composition I1', the molecular weight Mn of Kurasol LBH 2000 being lower than that of PolyBd R45 HTLO, while the second polyol precursor of mixture No. 1 (just like the first precursor) has a functionality greater than 2. Lower mechanical properties were in fact obtained for mixture No. 1, despite having short flexible segments. The PU formed is linear. The linearity of the PU formed demonstrates the positive effect of the functionality 2.5 of the second polyol precursor, which through its double bonds chemically co-crosslinks the PU formed by the elastomeric matrix of composition I1', giving said PU a three-dimensional structure that better reinforces the composition.
[0095] It can also be seen in Figure 2a that the second hydrogenated precursor Krasol HLBH-P 2000, which does not have double bonds, gives to Mix No. 2 even poorer mechanical properties compared to those of Mix No. 1. In particular, the absence of double bonds in the second precursor opposes the co-vulcanization of the PU with polyisoprene (the PU formed in Mix No. 2 is also linear) and therefore leads to poor reinforcement of the second precursor due to the lack of covalent bonds between the PU and the elastomeric matrix of the mixture.
[0096] The Payne effect obtained for known mixtures with 40 phr of N330 was measured at 100° C. as indicated above for mixtures No. 1 and No. 2 for composition I1′ (see Table 13 below).
[0097] [Table 13]
[0098] As can be seen in Table 13, the Payne effect is higher for mixtures No. 1 and No. 2, each incorporating linear PU. In fact, during dynamic stress, it is easier to break the low energy bonds between the chains of linear PU in mixtures No. 1 and No. 2 than to break the three-dimensional network of the co-crosslinked PU in composition I1'.
[0099] The intrinsic properties of the second precursor (particularly its functionality and its double bonds) are therefore decisive for generating the desired mechanical properties of the composition.
[0100] [Second embodiment of the present invention (NIPU)]
[0101] [Table 14]
[0102] [Table 15]
[0103] [Table 16]
[0104] [Table 17]
[0105] [Table 18]
[0106] [Table 19]
[0107] [Table 20]
[0108] As seen in FIG. 11, the addition of in situ synthesized NIPU also allows for reinforcement of the elastomeric matrix, as particularly shown by the elastic modulus of the IR / NIPU blend, which is greater than the elastic modulus of the blend reinforced with 20 phr of carbon black alone.
[0109] Furthermore, by selecting the structure of the chain extender (with the first polyamine precursor 1,3-cyclohexanebis(methylamine)), it is possible to modify the mechanical properties of compositions I7 to I10 in order to obtain hardness close to that of the reference mixture (with 40 phr of carbon black and no NIPU).
[0110] The Payne effect at 100° C. for each of compositions I7 to I10 is very low (see the ratio being ≦1.05), regardless of the chain extender used.
[0111] As can be seen in Figure 12, the choice of polyamine used (the same phloroglucinol Tri-CC chain extender) also influences the mechanical properties of compositions I10 to I13, making it possible to give them variable hardness (from 48 to 52 Shore A). In all cases, the Payne effect at 100°C is always very reduced compared to the reference mixture (see the ratio is below 1.09 or even 1.06).
[0112] As can be seen in FIG. 13, which shows the dynamic properties of compositions I7 to I13 measured at various temperatures (−30° C., 0° C., 25° C., 65° C., and 100° C.), the Payne effect is significantly reduced in compositions I7 to I13 compared to the reference mixture.
[0113] In conclusion, the above results demonstrate that the dynamic properties of the composition according to this second embodiment of the invention are significantly improved compared to the prior art represented by the reference mixture (with 40 phr carbon black and no NIPU), thereby advantageously allowing said composition to be used in dynamic applications over a wide temperature range extending from -30°C to 100°C.
[0114] 14 to 20 show that the NIPU thus obtained in situ are very finely and relatively uniformly dispersed in the polyisoprene in the form of nodules having large number-average transverse dimensions between 50 nm and 2 μm, or even between 100 nm and 1 μm, which contributes to obtaining the above-mentioned mechanical properties of the composition of the invention, including in particular the minimized Payne effect.
[0115] In summary, the chemical reinforcement of the elastomer matrix with such an entangled NIPU network structure thus makes it possible to maintain the mechanical properties (elastic modulus and hardness) of compositions I7 to I13 relative to the reference mixture, while at the same time minimizing the nonlinearity (dynamic properties) relative to the reference mixture. [Brief description of the drawings]
[0116] [Figure 1] 1 is a graph showing the secant elastic moduli M100, M300 and M400, Shore A hardness and the ratio G'0.5% / G'20% at 100°C of an unreinforced rubber composition, a known mixture reinforced with 40 phr of carbon black, a rubber composition not in accordance with the invention that is not reinforced (i.e. does not contain rigid segments (hereinafter indicated as RS)) and has 40 phr of PU without chain extenders, and a rubber composition not in accordance with the invention that has 20 phr of PU and 20 phr of carbon black without RS. [Diagram 2]1 is a graph illustrating the effect of adding a glycerol chain extender to M100, M300 and M400, the tensile strength R / r, the Shore A hardness and G'0.5% / G'20% at 100°C for said known mixture reinforced with 40 phr of carbon black, another known mixture reinforced with 20 phr of carbon black, said compound not according to the invention and a composition I1 according to the invention having 20 phr of PU with 30% by weight of RS and 20 phr of carbon black. [Figure 2a] FIG. 2 is a graph showing the influence of the functionality and degree of unsaturation of the second precursor on M100, M300 and M400 and R / r for a known mixture with 40 phr of carbon black, two mixtures not according to the invention comprising 20 phr of carbon black and 20 phr of PU derived from a first precursor according to the invention but from a second precursor not according to the invention, and a composition I1′ according to the invention comprising 20 phr of carbon black and 20 phr of PU derived from said first precursor but from a second precursor of the invention. [Diagram 3] 1 is a graph showing the effect of various chain extenders on M100, M300 and M400, tensile strength R / r, Shore A hardness and G'0.5% / G'20% at 100°C for a known mixture reinforced with 40 phr of carbon black, another known mixture reinforced with 20 phr of carbon black and three compositions according to the invention I2, I3 and I1 having 30% by mass of RS and 20 phr of three PUs, each with CDM, isosorbide and glycerol chain extenders (see schematic), and 20 phr of carbon black, for the same polyisocyanate (Suprasec 2015) and polyol (polyBd R20 LM) precursors as in composition I1. [Figure 4]1 is a graph showing the influence of various polyisocyanate precursors on M100, M300 and M400, R / r, Shore A hardness and G'0.5% / G'20% at 100°C for a known mixture reinforced with 40 phr carbon black, another known mixture reinforced with 20 phr carbon black, the polyisocyanate Suprasec 2015 and three other compositions according to inventions I4, I5 and I6 having 20 phr carbon black and three other PUs but obtained with IPDI, HDI and 4,4'-MDI polyisocyanates respectively (see schematic formula), with the same CHDM chain extender and polyol precursor (polyBd R20 LM). [Diagram 5] 1 is a graph showing the ratio G'0.5% / G'20% obtained at various temperatures ranging from -30°C to 100°C for a known mixture reinforced with 40 phr of carbon black and for compositions I1, I2, I3, I4, I5 and I6. [Figure 6] FIG. 2: Atomic Force Microscopy (AFM) images obtained with the "tapping" method for composition I2, the image on the left is a topographic image and the image on the right is a phase image. [Figure 7] FIG. 2 shows atomic force microscope (AFM) images obtained by the “tapping” method for composition I3, where the image on the left is a topographical image and the image on the right is a phase image. [Figure 8] FIG. 2 shows atomic force microscope (AFM) images obtained by the "tapping" method for composition I1, where the image on the left is a topographical image and the image on the right is a phase image. [Figure 9] FIG. 2 shows atomic force microscope (AFM) images obtained by the “tapping” method for composition I4, where the image on the left is a topographical image and the image on the right is a phase image. [Figure 10] FIG. 2 shows atomic force microscope (AFM) images obtained by the “tapping” method for composition I5, where the image on the left is a topographical image and the image on the right is a phase image. [Figure 11]1 is a graph showing the effect of various cyclic carbonate (hereafter abbreviated CC) chain extenders on M100, M300 and M400, R / r, Shore A and G'0.5% / G'20% at 100°C for the same first polyamine precursor (1,3-cyclohexanebis(methylamine), abbreviated CHMA) and the same second polycyclocarbonate precursor (cyclocarbonate terminated polybutadiene) for a known mixture reinforced with 40 phr of carbon black, another known mixture reinforced with 20 phr of carbon black, and four compositions according to compositions I7, I8, I9 and I10 having 20 phr of five NIPUs and 20 phr of carbon black, obtained with CyclohexanebisCC, ResorcinolbisCC, GlyceroltriCC and PhloroglucinoltriCC extenders (see schematic formulas), respectively. [Figure 12] 1 is a graph showing the effect of various polyamine precursors on M100, M300 and M400, R / r, Shore A and G'0.5% / G'20% at 100°C, with the same phloroglucinol tri-CC chain extender and the same polycyclocarbonate second precursor (cyclocarbonate terminated polybutadiene), for a known mixture reinforced with 40 phr of carbon black, a known mixture reinforced with 20 phr of carbon black, composition I10 with CHMA extender, and three other compositions according to the invention I11, I12 and I13 with 20 phr of three NIPUs, 20 phr of carbon black, obtained respectively with polyamines, xylylenediamine, EDEA and TAEA (see schematic formula). [Figure 13] 1 is a graph showing the G'0.5% / G'20% obtained at various temperatures ranging from -30°C to 100°C for known mixtures having 40 phr carbon black and compositions I7, I8, I9, I10, I11, I12, and I13. [Figure 14] FIG. 2 Atomic force microscope (AFM) images obtained in the "tapping" mode for composition I7, the image on the left is a topographical image and the image on the right is a phase image. [Figure 15] FIG. 2: Atomic force microscope (AFM) images obtained in the "tapping" mode for composition I8, the image on the left is a topographical image and the image on the right is a phase image. [Figure 16] FIG. 2: Atomic force microscope (AFM) images obtained in the "tapping" mode for composition I9, the image on the left is a topographical image and the image on the right is a phase image. [Figure 17] FIG. 2 shows atomic force microscopy (AFM) images obtained in the "tapping" mode for composition I10, where the image on the left is a topographical image and the image on the right is a phase image. [Figure 18] FIG. 2 Atomic force microscope (AFM) images obtained in the "tapping" mode for composition I11, the image on the left is a topographical image and the image on the right is a phase image. [Figure 19] FIG. 2 Atomic force microscope (AFM) images obtained in the "tapping" mode for composition I12, the image on the left is a topographical image and the image on the right is a phase image. [Figure 20] FIG. 2 Atomic force microscope (AFM) images obtained in the "tapping" mode for composition I13, the image on the left is a topographical image and the image on the right is a phase image.
Claims
1. A rubber composition usable for mechanical members having dynamic functions selected from anti-vibration supports and elastic joints for electric vehicles or industrial equipment, The rubber composition is based on at least one elastomer and comprises: - reinforcing fillers, and a polymer containing urethane groups dispersed in said at least one elastomer, the rubber composition comprises a product of a thermomechanical mixing reaction of the at least one elastomer having the reinforcing filler, a precursor of the polymer having urethane groups, and a chain extender; The rubber composition has a complex shear modulus G * The ratio of the storage modulus to the storage modulus is G'0.5% / G'20%, The G'0.5% and G'20% are measured according to standard ISO 4664 on double shear specimens subjected to shear strains of 0.02% to 50% at the same frequency of 5 Hz and at the same temperature T at dynamic strain amplitudes of 0.5% and 20%, respectively, of the rubber composition: (i) When T = 100 ° C., G'0.5% / G'20% ≦ 1.15; (ii) when T = 65 ° C., G'0.5% / G'20% ≦ 1.40; (iii) when T = 25 ° C., G'0.5% / G'20% ≦ 1.50; (iv) when T = 0 ° C., G'0.5% / G'20% ≦ 1.60; (v) When T = -30°C, G'0.5% / G'20% < 2.
50.
2. The rubber composition satisfies at least condition (i), 2. The rubber composition of claim 1, wherein the test specimen is subjected to a preliminary mechanical conditioning of 0±4 mm, 50 mm / min for 8 cycles.
3. The rubber composition of claim 2, wherein the rubber composition also satisfies conditions (ii), (iii), (iv) and (v).
4. The rubber composition according to any one of claims 1 to 3, comprising 10 to 40 phr (phr: parts by weight per 100 parts of elastomer) of carbon black as a reinforcing filler, and 10 to 50 phr of the polymer having a urethane group.
5. The rubber composition according to claim 4, further satisfying the following condition (i-a): (i-a) When T = 100°C, G'0.5% / G'20%≦1.
12.
6. 6. The rubber composition according to claim 4, wherein the rubber composition comprises 15 to 30 phr of the carbon black and 15 to 30 phr of the polymer having a urethane group.
7. 7. The rubber composition according to claim 1, wherein the polymer having urethane groups is dispersed in the at least one elastomer in the form of nodules having a maximum number average transverse dimension of 1 nm to 5 μm.
8. 8. The rubber composition of claim 7, wherein the polymer having urethane groups is dispersed in the at least one elastomer in the form of nodules having a maximum number average transverse dimension of from 50 nm to 2 μm.
9. The rubber composition comprises: at least one of the secant moduli M100, M300 and M400 at strains of 100%, 300% and 400%, respectively, measured in uniaxial tension according to standard ASTM D 412: M100≧1.5MPa, M300≧5.5 MPa, and M400≧9.5MPa; and / or - tensile strength R / r, measured in uniaxial tension of at least 26 MPa according to standard ASTM D 412 The rubber composition according to any one of claims 1 to 8, wherein
10. A rubber composition according to any one of the preceding claims, wherein said rubber composition has a Shore A hardness, measured according to standard ASTM D 2240, of at least 48.
11. the at least one elastomer is a rubber selected from diene or non-diene elastomers, excluding silicone rubbers; The rubber composition comprises a crosslinking system, The rubber composition according to any one of claims 1 to 10, wherein the crosslinking system is capable of reacting with the product of the thermomechanical mixing reaction to co-crosslink the at least one elastomer and the polymer bearing urethane groups.
12. The rubber composition of claim 11 , wherein the crosslinking system comprises sulfur.
13. 13. The rubber composition according to claim 11 or 12, wherein said at least one elastomer is a non-polar diene elastomer.
14. The rubber composition of claim 13, wherein said at least one elastomer is selected from natural rubber (NR), polyisoprene (IR), polybutadiene (BR) and styrene-butadiene copolymer (SBR).
15. The polymer having a urethane group is a rigid segment present in said polymer at a mass fraction between 20% and 40% and comprising a first precursor contained in said chain extender and said precursor; and - a flexible segment, comprising a second precursor contained in said precursor, which is a diene polymer having functionalized chain ends; The polymer having urethane groups is co-crosslinked with the at least one elastomer through the double bonds of the second precursor to form a three-dimensional network connected with the at least one elastomer through covalent bonds. The rubber composition according to any one of claims 1 to 14.
16. 16. The rubber composition of claim 15, wherein the rigid segment is present in the polymer at a mass fraction of 25% to 35% and the second precursor of the flexible segment is a functionalized polybutadiene.
17. the first precursor and the second precursor form two separate reactants for the thermomechanical mixing reaction with the at least one elastomer, the reinforcing filler, and the chain extender; 17. The rubber composition according to claim 15 or 16, wherein the first precursor and the second precursor do not form a precursor prepolymer.
18. The rubber composition according to any one of claims 15 to 17, wherein the chain extender has a molar mass of less than or equal to 700 g / mol.
19. The rubber composition according to any one of claims 15 to 18, wherein the polymer having urethane groups belongs to the family of polyurethanes obtained from isocyanate compounds, excluding polyurethane-ureas.
20. said first precursor is a polyisocyanate with a functionality greater than 2, - said second precursor is a diol-functionalized diene polymer having a functionality greater than 2; A rubber composition according to claim 19, wherein said chain extender is a polyol chosen from diols and triols having a molar mass of less than or equal to 300 g / mol.
21. said first precursor is selected from monomers or prepolymers based on 4,4'-methylenebis(phenylisocyanate), isophorone diisocyanate, hexamethylene diisocyanate and 4,4'-diphenylmethylene diisocyanate; said second precursor is a non-hydrogenated hydroxytelechelic polybutadiene having a number average molecular weight between 1000 and 3000 g / mol and a functionality greater than or equal to 2.2; A rubber composition according to claim 20, wherein said chain extenders are chosen from cyclohexanedimethanol, isosorbide and glycerol.
22. said at least one elastomer is a non-polar diene elastomer and is selected from natural rubber (NR), polyisoprene (IR), polybutadiene (BR) and styrene-butadiene copolymers (SBR); said reinforcing filler comprises carbon black present in said rubber composition in an amount ranging from 15 to 30 phr (phr: parts by weight per 100 parts of elastomer); the polymer containing urethane groups is present in the rubber composition in an amount of from 15 to 30 phr, and The rubber composition according to any one of claims 19 to 21, wherein the total amount of the carbon black and the polymer having urethane groups in the rubber composition is 35 to 55 phr.
23. The rubber composition according to claim 22, wherein the rubber composition satisfies the following condition (i-a): (i-a) When T = 100°C, G'0.5% / G'20%≦1.
12.
24. A rubber composition according to any one of claims 15 to 18, wherein the polymer containing urethane groups belongs to the family of polyhydroxyurethanes obtained without isocyanates.
25. said first precursor is a polyamine chosen from diamines and triamines, said second precursor is a diene polymer functionalized with cyclocarbonate chain ends, A rubber composition according to claim 24, wherein said chain extender is a cyclic carbonate having a molar mass less than or equal to 500 g / mol.
26. said first precursor is selected from 1,3-cyclohexanebis(methylamine), xylylenediamine, 2,2′-(ethylenedioxy)bis(ethylamine) and tris(2-aminoethyl)amine; said second precursor is a polybutadiene functionalized with two carbonate end rings, each of which is 5 or 6 members; A rubber composition according to claim 25, wherein said chain extenders are selected from cyclohexane biscarbonate, resorcinol biscarbonate, glycerol tricarbonate and phloroglucinol tricarbonate.
27. said at least one elastomer is a non-polar diene elastomer and is selected from natural rubber (NR), polyisoprene (IR), polybutadiene (BR) and styrene-butadiene copolymer (SBR); said reinforcing filler comprises carbon black present in said rubber composition in an amount ranging from 15 to 30 phr (phr: parts by weight per 100 parts of elastomer); said polymer containing urethane groups is present in said rubber composition in an amount of from 15 to 30 phr; The rubber composition according to any one of claims 24 to 26, wherein the total amount of the carbon black and the polymer having urethane groups in the rubber composition is 35 to 55 phr.
28. The rubber composition according to claim 27, wherein the rubber composition satisfies at least one of the following conditions (ia) to (va): (i-a) When T = 100 ° C., G'0.5% / G'20% ≦ 1.12, (ii-a) when T = 65 ° C, G'0.5% / G'20% ≦ 1.20; (iii-a) when T = 25 ° C., G'0.5% / G'20% ≦ 1.30; (iv-a) when T = 0 ° C., G'0.5% / G'20% ≦ 1.40; (va) When T = -30°C, G'0.5% / G'20% ≦ 1.
50.
29. The rubber composition according to claim 28, further satisfying at least one of the following conditions (ib) to (vb): (i-b) When T = 100 ° C., G'0.5% / G'20% ≦ 1.10, (ii-b) when T = 65 ° C, G'0.5% / G'20% ≦ 1.15; (iii-b) when T = 25 ° C., G'0.5% / G'20% ≦ 1.20; (iv-b) when T = 0 ° C., G'0.5% / G'20% ≦ 1.25; (v−b) When T=−30° C., G′0.5% / G′20%≦1.
40.
30. A mechanical member having a dynamic function selected from anti-vibration supports and elastic joints for electric vehicles or industrial equipment, The mechanical member includes at least one elastic member made of a rubber composition configured to be subjected to dynamic stress; A mechanical member, wherein the rubber composition is the rubber composition according to any one of claims 1 to 29.
31. A method for producing the rubber composition according to any one of claims 1 to 14, comprising the steps of: a) forming a non-crosslinked mixture comprising said polymer having urethane groups dispersed in said at least one elastomer via said thermomechanical mixing reaction of said reinforcing filler, said precursor, and said chain extender; b) adding a crosslinking system to the crosslinkable mixture obtained as above, followed by mechanical processing of said mixture, c) crosslinking the crosslinkable mixture by vulcanization in a press at a temperature between 130°C and 180°C, the polymer having urethane groups being chemically co-crosslinked with the at least one elastomer to form covalent bonds with said elastomer.
32. In step a), the reaction is carried out in an internal mixer at a maximum temperature of 130° C. to 180° C., In step b), the mechanical processing of the crosslinkable mixture is carried out in an open mill at a maximum temperature of less than 80° C., and The method for producing a rubber composition according to claim 31 , wherein in step c) the crosslinking of the crosslinkable mixture is carried out by compression molding.
33. 33. The method according to claim 31 or 32, wherein the at least one elastomer, the polymer having urethane groups, is segmented into rigid segments having the chain extender and the first precursor, and flexible segments having the second precursor, after which the precursors form a first precursor and a second precursor which are added separately in step a).
34. The method according to claim 33, wherein the total mass fraction of the first precursor and the chain extender in the polymer having urethane groups formed in step a) is 20% to 40%.
Citation Information
Patent Citations
Composition of polyurethane and rubbery elastomer
JP2001254012A
Thermoplastic vulcanizates obtained from dynamically vulcanized tpu / non-polar rubber compounds
JP2003506550A
Blends from thermoplastic polyurethanes and rubbers and methods for making them
JP2016529376A