Nonaqueous electrolyte, nonaqueous electrolyte storage element, and method for producing nonaqueous electrolyte storage element
A nonaqueous electrolyte composition with imide salt, tetrafluoroborate, and phosphate ester addresses capacity retention and thickness issues in nonaqueous electrolyte storage elements by forming a film that suppresses gas generation, thereby improving performance.
Patent Information
- Application Number
- JP2019205796
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-11-13
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-11-13
AI Technical Summary
Nonaqueous electrolyte storage elements using hexafluorophosphate as an electrolyte salt suffer from low capacity retention rates after charge/discharge cycles, while those using imide salts experience thickness increase due to gas generation during charging and discharging.
Incorporating an imide salt, tetrafluoroborate, and phosphate ester into the nonaqueous electrolyte, with a focus on minimizing hexafluorophosphate content, to form a film that suppresses gas generation and maintains electrolyte thickness.
Enhances capacity retention rate and prevents thickness increase in nonaqueous electrolyte storage elements, particularly at high positive electrode potentials, by using a specific electrolyte composition.
Smart Images

Figure 0007552013000003 
Figure 0007552013000002 
Figure 0007552013000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a nonaqueous electrolyte, a nonaqueous electrolyte storage element, and a method for producing a nonaqueous electrolyte storage element. [Background technology]
[0002] Non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, are widely used in electronic devices such as personal computers and communication terminals, automobiles, etc., due to their high energy density. Non-aqueous electrolyte secondary batteries generally have a pair of electrodes electrically isolated by a separator and a non-aqueous electrolyte interposed between the electrodes, and are configured to charge and discharge by transferring ions between the electrodes. In addition, capacitors such as lithium ion capacitors and electric double layer capacitors are also widely used as non-aqueous electrolyte storage elements other than non-aqueous electrolyte secondary batteries.
[0003] In general, the nonaqueous electrolyte of a nonaqueous electrolyte storage element contains a nonaqueous solvent and an electrolyte salt that dissolves in the nonaqueous solvent. As the electrolyte salt, hexafluorophosphates such as LiPF6 and imide salts such as lithium bis(fluorosulfonyl)imide (LiFSI) are widely used (see Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-128052 A [Patent Document 2] JP 2018-101612 A Summary of the Invention [Problem to be solved by the invention]
[0005] A nonaqueous electrolyte storage element having a nonaqueous electrolyte in which a hexafluorophosphate salt is used as the electrolyte salt does not have a sufficient capacity retention rate after charge / discharge cycles, whereas a nonaqueous electrolyte storage element having a nonaqueous electrolyte in which an imide salt is used as the electrolyte salt is prone to an increase in thickness due to gas generation during charge / discharge.
[0006] The present invention has been made in light of the above-mentioned circumstances, and an object of the present invention is to provide a nonaqueous electrolyte that can increase the capacity retention rate and suppress an increase in thickness of a nonaqueous electrolyte storage element after charge-discharge cycles, a nonaqueous electrolyte storage element that has a high capacity retention rate and suppresses an increase in thickness after charge-discharge cycles, and a method for manufacturing such a nonaqueous electrolyte storage element. [Means for solving the problem]
[0007] A non-aqueous electrolyte according to one embodiment of the present invention is a non-aqueous electrolyte for use in an electricity storage element, which contains an imide salt, a tetrafluoroborate, and a phosphate ester.
[0008] A nonaqueous electrolyte electricity storage element according to another embodiment of the present invention is a nonaqueous electrolyte electricity storage element including the nonaqueous electrolyte according to the embodiment of the present invention.
[0009] A method for producing a nonaqueous electrolyte storage element according to another embodiment of the present invention includes preparing a nonaqueous electrolyte containing an imide salt, a tetrafluoroborate salt, and a phosphate ester. Effect of the Invention
[0010] The nonaqueous electrolyte according to one aspect of the present invention can increase the capacity retention rate of a nonaqueous electrolyte storage element after charge-discharge cycles and suppress an increase in thickness. According to the nonaqueous electrolyte storage element according to another aspect of the present invention, the capacity retention rate after charge / discharge cycles is high, and an increase in thickness is suppressed. According to a method for producing a nonaqueous electrolyte storage element according to another aspect of the present invention, it is possible to produce a nonaqueous electrolyte storage element that has a high capacity retention rate after charge / discharge cycles and is suppressed in increase in thickness. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is an external perspective view showing a nonaqueous electrolyte electricity storage element according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an electricity storage device formed by assembling a plurality of nonaqueous electrolyte electricity storage elements according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] First, an outline of the nonaqueous electrolyte, the nonaqueous electrolyte storage element, and the method for producing the nonaqueous electrolyte storage element disclosed in this specification will be described.
[0013] A non-aqueous electrolyte according to one embodiment of the present invention is a non-aqueous electrolyte for use in an electricity storage element, which contains an imide salt, a tetrafluoroborate, and a phosphate ester.
[0014] According to the nonaqueous electrolyte, the capacity retention rate of the nonaqueous electrolyte storage element after the charge-discharge cycle can be increased and the thickness increase can be suppressed. The reason why the nonaqueous electrolyte produces the above effect is unclear, but the following reason is presumed. In the nonaqueous electrolyte, the imide salt is used as the electrolyte salt, so that the capacity retention rate of the nonaqueous electrolyte storage element after the charge-discharge cycle can be increased. This reason is presumed to be because the imide salt is less likely to cause a side reaction that causes a decrease in the capacity of the nonaqueous electrolyte storage element during charging. On the other hand, in a nonaqueous electrolyte storage element using a nonaqueous electrolyte containing a conventional imide salt, the increase in thickness due to gas generation is thought to be caused by the fact that a coating capable of suppressing gas generation is not formed on the electrode surface. For example, when a conventional nonaqueous electrolyte containing hexafluorophosphate is used, a coating containing phosphorus atoms derived from hexafluorophosphate is formed on the electrode surface, which is thought to suppress gas generation and suppress the increase in the thickness of the nonaqueous electrolyte storage element. In contrast, in the nonaqueous electrolyte, by containing a tetrafluoroborate and a phosphate ester in addition to an imide salt, it is presumed that a coating capable of suppressing gas generation is formed due to these, and an increase in the thickness of the nonaqueous electrolyte storage element is suppressed.
[0015] It is preferable that the non-aqueous electrolyte does not substantially contain hexafluorophosphate. Hexafluorophosphate is particularly effective when the positive electrode potential is high (for example, 4.0 V vs. Li / Li + When the nonaqueous electrolyte storage element reaches the above-mentioned temperature, a side reaction that causes a decrease in capacity is likely to occur when the nonaqueous electrolyte storage element is charged. Therefore, when the nonaqueous electrolyte does not substantially contain a hexafluorophosphate, the capacity retention rate after charge-discharge cycles of the nonaqueous electrolyte storage element is increased, and the decrease in capacity can be suppressed especially after charge-discharge cycles in which the positive electrode potential reaches a high potential.
[0016] In the present invention, the non-aqueous electrolyte being "substantially free" of hexafluorophosphate means that the content of hexafluorophosphate is less than 0.15 mol / kg.
[0017] The nonaqueous electrolyte may further contain a chain carbonate. Since the chain carbonate is a solvent with a relatively low boiling point, it is usually likely to cause gas generation. However, even if the nonaqueous electrolyte further contains a chain carbonate, gas generation is suppressed and an increase in the thickness of the nonaqueous electrolyte storage element can be suppressed. Therefore, as a nonaqueous electrolyte according to one embodiment of the present invention, a form containing a chain carbonate is also suitable.
[0018] The non-aqueous electrolyte may further contain a fluorinated cyclic carbonate. Fluorinated cyclic carbonate is easily reductively decomposed at the negative electrode, and is usually a cause of gas generation. However, even if the non-aqueous electrolyte further contains a fluorinated cyclic carbonate, gas generation is suppressed and an increase in the thickness of the non-aqueous electrolyte storage element can be suppressed. Therefore, a non-aqueous electrolyte according to one embodiment of the present invention is also preferably one that contains a fluorinated cyclic carbonate.
[0019] A nonaqueous electrolyte storage element according to another embodiment of the present invention is a nonaqueous electrolyte storage element including the nonaqueous electrolyte according to an embodiment of the present invention. Since the nonaqueous electrolyte storage element uses the nonaqueous electrolyte, the nonaqueous electrolyte storage element has a high capacity retention rate after charge-discharge cycles and is suppressed from increasing in thickness.
[0020] The nonaqueous electrolyte storage element further includes a positive electrode having a positive electrode mixture containing phosphorus atoms, and in the X-ray photoelectron spectroscopy spectrum of the surface of the positive electrode mixture, the maximum value of the peak assigned to P2p is preferably at a position of 134 eV or less. By providing such a positive electrode, the capacity retention rate after charge-discharge cycles can be further increased. The reason for this is not clear, but the following is presumed. When a positive electrode mixture is formed from a positive electrode mixture paste containing an oxoacid of phosphorus, a coating containing a component derived from the oxoacid of phosphorus and present at a position where the maximum value of the peak assigned to P2p is at a position of 134 eV or less in the X-ray photoelectron spectroscopy spectrum is formed on the surface of the positive electrode mixture. It is presumed that this coating suppresses the oxidation corrosion of aluminum, which is usually used as a positive electrode substrate, and therefore the capacity retention rate after charge-discharge cycles is increased.
[0021] The sample (positive electrode mixture) used for the measurement of the X-ray photoelectron spectroscopy spectrum is prepared by the following method. The nonaqueous electrolyte storage element is discharged at a current of 0.1 C to the discharge end voltage during normal use to be in a fully discharged state. The fully discharged nonaqueous electrolyte storage element is disassembled to remove the positive electrode, which is thoroughly washed with dimethyl carbonate and then dried under reduced pressure at room temperature. The dried positive electrode is cut into a predetermined size (e.g., 2 x 2 cm), which is used as a sample for the measurement of the X-ray photoelectron spectroscopy spectrum. The operations from disassembling the nonaqueous electrolyte storage element to preparing a sample for the measurement of the X-ray photoelectron spectroscopy spectrum are performed in an argon atmosphere with a dew point of -60°C or less, and the prepared sample is sealed in a transfer vessel and kept in an argon atmosphere with a dew point of -60°C or less, and introduced into the sample chamber of the measurement device for the X-ray photoelectron spectroscopy spectrum. The device and measurement conditions used for the measurement of the X-ray photoelectron spectroscopy spectrum are as follows. Equipment: KRATOS ANALYTICAL's "AXIS NOVA" X-ray source: monochromatic AlKα Acceleration voltage: 15 kV Analysis area: 700μm x 300μm Measurement range: P2p = 145 to 128 eV, C1s = 300 to 272 eV Measurement interval: 0.1 eV Measurement time: P2p = 72.3 seconds / time, C1s = 70.0 seconds / time Accumulation count: P2p = 15 times, C1s = 8 times
[0022] The position of the maximum value of the peak in the above spectrum is determined as follows. First, the position of the peak of C1s attributed to sp2 carbon is set to 284.8 eV, and the binding energies of all the obtained spectra are corrected. Next, the corrected spectrum is subjected to a leveling process by removing the background using a linear method. In the spectrum after the leveling process, the binding energy at which the slope of the tangent to the spectrum peak in the binding energy range of 128 eV to 144 eV is 0 and shows a maximum value is determined as the position of the maximum value of the peak attributed to P2p.
[0023] A method for producing a nonaqueous electrolyte storage element according to another aspect of the present invention includes preparing a nonaqueous electrolyte containing an imide salt, a tetrafluoroborate, and a phosphate ester. The method for producing a nonaqueous electrolyte storage element has a high capacity retention rate after charge-discharge cycles and is suppressed in increase in thickness.
[0024] The manufacturing method preferably further comprises preparing a positive electrode using a positive electrode mixture paste containing a phosphorus oxoacid. By preparing a positive electrode in this manner, as described above, a coating containing a component derived from the phosphorus oxoacid and present at a position where the maximum value of the peak assigned to P2p is 134 eV or less in the X-ray photoelectron spectroscopy spectrum is formed on the surface of the positive electrode mixture, and the capacity retention rate after charge-discharge cycles of the obtained nonaqueous electrolyte storage element is higher.
[0025] A nonaqueous electrolyte, a nonaqueous electrolyte storage element, a method for manufacturing a nonaqueous electrolyte storage element according to one embodiment of the present invention, and other embodiments will be described in detail below. Note that the names of the components (elementary components) used in each embodiment may differ from the names of the components (elementary components) used in the background art.
[0026] <Non-aqueous electrolyte> The non-aqueous electrolyte according to one embodiment of the present invention includes an imide salt, a tetrafluoroborate, and a phosphate ester. The imide salt and the tetrafluoroborate are included in the non-aqueous electrolyte as electrolyte salts. The non-aqueous electrolyte may usually further include a non-aqueous solvent in addition to the imide salt, the tetrafluoroborate, and the phosphate ester. The non-aqueous electrolyte is used as a non-aqueous electrolyte (non-aqueous electrolytic solution) for a storage element.
[0027] (imide salt) The imide salt is contained in the nonaqueous electrolyte as a first electrolyte salt. Examples of the imide salt include lithium imide salt, sodium imide salt, potassium imide salt, magnesium imide salt, and imide salts having an onium ion, with lithium imide salt being preferred.
[0028] The lithium imide salt may be, for example, Lithium sulfonylimide salts such as LiN(SO2F)2 (lithium bis(fluorosulfonyl)imide: LiFSI), LiN(CF3SO2)2 (lithium bis(trifluoromethanesulfonyl)imide: LiTFSI), LiN(C2F5SO2)2 (lithium bis(pentafluoroethanesulfonyl)imide: LiBETI), LiN(C4F9SO2)2 (lithium bis(nonafluorobutanesulfonyl)imide), CF3-SO2-N-SO2-N-SO2CF3Li, FSO2-N-SO2-C4F9Li, CF3-SO2-N-SO2-C4F9Li, CF3-SO2-N-SO2-CF2-SO2-N-SO2-CF3Li2, CF3-SO2-N-SO2-CF2-SO3Li2, CF3-SO2-N-SO2-CF2-SO2-C(-SO2CF3)2Li2; Examples include lithium phosphonylimide salts such as LiN(POF2)2 (lithium bis(difluorophosphonyl)imide: LiDFPI). The lithium imide salts can be used alone or in combination of two or more.
[0029] The lithium imide salt preferably contains a fluorine atom, and specifically, for example, it is preferable that the lithium imide salt contains a fluorosulfonyl group, a difluorophosphonyl group, a fluoroalkyl group, or the like.
[0030] In addition, the imide salt is preferably a bis(fluorosulfonyl)imide salt such as LiFSI. Bis(fluorosulfonyl)imide salts have a higher corrosion potential for aluminum, which is used as a material for general positive electrode substrates, compared to, for example, LiTFSI. Therefore, by using a bis(fluorosulfonyl)imide salt, corrosion of the positive electrode substrate, etc. is suppressed, and the capacity retention rate of the nonaqueous electrolyte storage element after charge-discharge cycles can be further increased.
[0031] The content of the imide salt in the non-aqueous electrolyte is preferably 0.2 mol / kg or more and 5.0 mol / kg or less, more preferably 0.4 mol / kg or more and 3.0 mol / kg or less. The lower limit of the content of the imide salt may be more preferably 0.6 mol / kg. The upper limit of the content of the imide salt may be more preferably 2.0 mol / kg, even more preferably 1.2 mol / kg. By making the content of the imide salt equal to or more than the lower limit, the capacity retention rate of the non-aqueous electrolyte storage element after the charge-discharge cycle can be further increased. On the other hand, by making the content of the imide salt equal to or less than the upper limit, the increase in the thickness of the non-aqueous electrolyte storage element also tends to be suppressed.
[0032] Furthermore, in the nonaqueous electrolyte according to one embodiment of the present invention, the effect of the present invention of increasing the capacity retention rate of a nonaqueous electrolyte storage element after charge-discharge cycles can be exhibited even if the imide salt is not at a high concentration, for example, much higher than 1.0 mol / kg. Therefore, the nonaqueous electrolyte can also be suitably used as a design in which the imide salt is in a non-high concentration range, which can improve undesirable points of nonaqueous electrolytes or nonaqueous electrolyte storage elements using a high concentration of imide salt, such as high viscosity and high internal resistance.
[0033] On the other hand, in the nonaqueous electrolyte according to one embodiment of the present invention, even if the imide salt is at a high concentration, for example, exceeding 2.0 mol / kg, the effect of the present invention of increasing the capacity retention rate of a nonaqueous electrolyte storage element after charge-discharge cycles can be exhibited. Therefore, since the nonaqueous electrolyte can realize a state in which the content of nonaqueous solvent that is not solvated in the electrolyte salt containing the imide salt is very small or absent, the nonaqueous electrolyte can be suitably used as a design in which the imide salt is in a high concentration range, which can improve undesirable points of nonaqueous electrolytes or nonaqueous electrolyte storage elements using a low concentration imide salt, such as a low corrosion potential of aluminum.
[0034] (Tetrafluoroborate) The tetrafluoroborate is contained in the nonaqueous electrolyte as a second electrolyte salt, and although it is not clear, it is presumed that the inclusion of the tetrafluoroborate together with the phosphate ester in the nonaqueous electrolyte forms a coating containing phosphorus atoms capable of suppressing gas generation.
[0035] Examples of the tetrafluoroborate include alkali metal salts of tetrafluoroboric acid such as LiBF4 (lithium tetrafluoroborate), NaBF4 (sodium tetrafluoroborate), and KBF4 (potassium tetrafluoroborate), Mg(BF4)2 (magnesium tetrafluoroborate), and tetrafluoroborates having onium ions, with LIBF4 being preferred. One or more of the tetrafluoroborates can be used.
[0036] The content of the tetrafluoroborate in the non-aqueous electrolyte is preferably 0.05 mol / kg or more and 1.50 mol / kg or less, more preferably 0.10 mol / kg or more and 1.00 mol / kg or less. The lower limit of the content of the tetrafluoroborate may be more preferably 0.15 mol / kg or 0.25 mol / kg. The upper limit of the content of the tetrafluoroborate may be more preferably 0.75 mol / kg or 0.50 mol / kg. By making the content of the tetrafluoroborate to be equal to or more than the lower limit, the increase in the thickness of the non-aqueous electrolyte storage element can be more sufficiently suppressed. On the other hand, by making the content of the tetrafluoroborate to be equal to or less than the upper limit, the capacity retention rate after the charge-discharge cycle of the non-aqueous electrolyte storage element tends to be increased.
[0037] (Hexafluorophosphate) The non-aqueous electrolyte is preferably substantially free of hexafluorophosphate (LiPF6, etc.), which is a type of electrolyte salt. In this case, the non-aqueous electrolyte can increase the capacity retention rate of the non-aqueous electrolyte storage element, particularly after charge-discharge cycles in which the positive electrode potential reaches a high potential. The content of hexafluorophosphate in the non-aqueous electrolyte is preferably less than 0.15 mol / kg, more preferably less than 0.10 mol / kg, even more preferably less than 0.05 mol / kg, and even more preferably less than 0.01 mol / kg. Furthermore, it may be substantially 0 mol / kg or 0 mol / kg.
[0038] (Other electrolyte salts, etc.) The non-aqueous electrolyte may or may not further contain other electrolyte salts, such as lithium salts, sodium salts, potassium salts, magnesium salts, onium salts, and the like, other than imide salts and tetrafluoroborates.
[0039] The total content of imide salt and tetrafluoroborate in the total electrolyte salt in the non-aqueous electrolyte is preferably 80 mol% or more, more preferably 90 mol% or more, and even more preferably 99 mol% or more. When the electrolyte salt in the non-aqueous electrolyte is substantially composed of only imide salt and tetrafluoroborate, the effect of the present invention may be more fully achieved. In addition, the molar ratio of imide salt and tetrafluoroborate in the electrolyte in the non-aqueous electrolyte (imide salt: tetrafluoroborate) is not particularly limited, but is preferably 10:90 or more and 90:10 or less, more preferably 20:80 or more and 80:20 or less, and even more preferably 50:50 or more and 75:25 or less.
[0040] The total electrolyte salt content in the nonaqueous electrolyte is preferably 0.5 mol / kg to 5.0 mol / kg, more preferably 0.7 mol / kg to 2.0 mol / kg, and even more preferably 0.9 mol / kg to 1.2 mol / kg.
[0041] (phosphate ester) The non-aqueous electrolyte contains a phosphoric acid ester. It is presumed that when a non-aqueous electrolyte containing a phosphoric acid ester is used, a coating containing phosphorus derived from the phosphoric acid ester is formed on the electrode surface. It is presumed that this coating can suppress gas generation and suppress an increase in the thickness of the non-aqueous electrolyte storage element.
[0042] Phosphate esters are O=P(OR 1 )(OR 2 )(OR 3 )(R 1 , R 2 and R 3 are each independently a hydrocarbon group or a fluorinated hydrocarbon group.
[0043] R 1 , R 2 and R 3 The hydrocarbon group represented by the formula (1) may be either an aliphatic hydrocarbon group or an aromatic hydrocarbon group. Examples of the aliphatic hydrocarbon group include alkyl groups such as methyl, ethyl, n-propyl, i-propyl, n-butyl, and n-pentyl groups, alkenyl groups such as ethenyl (vinyl), 1-propenyl, and 2-propenyl (allyl) groups, alkynyl groups such as ethynyl and propynyl groups, and cycloalkyl groups such as cyclohexyl groups. Examples of the aromatic hydrocarbon group include phenyl and tolyl groups.
[0044] R 1 , R 2 and R 3 Examples of the fluorinated hydrocarbon group represented by the formula (I) include the above-mentioned hydrocarbon groups in which some or all of the hydrogen atoms have been substituted with fluorine atoms.
[0045] R 1 , R 2 and R 3 As the alkyl group, an aliphatic hydrocarbon group and a fluorinated aliphatic hydrocarbon group are preferable, and an alkyl group, an alkenyl group, a fluoroalkyl group and a fluoroalkenyl group are more preferable.
[0046] R 1 , R 2 and R 3 The number of carbon atoms may be, for example, 1 or more and 12 or less, preferably 1 or more and 6 or less, and more preferably 2 or more and 4 or less.
[0047] R 1 , R 2 and R 3 When R is a fluorinated hydrocarbon group, 1 , R 2 and R 3 The number of fluorines contained in the group is preferably 1 or more and 12 or less, and more preferably 2 or more and 8 or less.
[0048] Examples of phosphate esters include O=P(OCH3)3, O=P(OCH2CH3)3, O=P(OCH2CFH2)3, O=P(OCH2CF2H)3, O=P(OCH2CF3)3, O=P(OCH3)2(OCH2CF3), O=P(OCH3)(OCH2CF3)2, O=P(OCH2CH3)2(OCH2CF3), O=P(OCH2CH3)(OCH2CF3)2, O=P(OCH2CH2CH3)3, O=P(OCH2CF2CF2H)3, O=P(OCH2CF2CF3)3, O=P(OCH2CH=CH2)3, O=P(OCH(CH3)2), O=P(OCH(CF3)2), and O=P(OC(CH3)3).
[0049] The content of the phosphoric acid ester relative to all components other than the electrolyte salt in the nonaqueous electrolyte is preferably 1% by volume or more and 60% by volume or less, more preferably 3% by volume or more and 50% by volume or less, and even more preferably 5% by volume or more and 40% by volume or less. The lower limit of the content of the phosphoric acid ester may be more preferably 10%, 15% by volume or 20% by volume. The upper limit of the content of the phosphoric acid ester may be more preferably 30%, 25% by volume or 20% by volume. The content of the phosphoric acid ester relative to the total of the phosphoric acid ester and the nonaqueous solvent in the nonaqueous electrolyte is also preferably within the above numerical range. By setting the content of the phosphoric acid ester to the above lower limit or more, a sufficient coating is formed, and the increase in the thickness of the nonaqueous electrolyte storage element can be more sufficiently suppressed. On the other hand, by setting the content of the phosphoric acid ester to the above upper limit or less, the capacity retention rate after the charge-discharge cycle of the nonaqueous electrolyte storage element tends to increase.
[0050] (Non-aqueous solvent) As the non-aqueous solvent, a known non-aqueous solvent that is usually used as a non-aqueous solvent for a general non-aqueous electrolyte storage element can be used. Examples of the non-aqueous solvent include carbonates (cyclic carbonates and chain carbonates), esters, ethers, amides, sulfones, lactones, and nitriles. Among these, carbonates are preferred. The carbonate may be a carbonate that does not have a substituent, or a carbonate that has a substituent. Examples of the substituent include a hydroxyl group and a halogen atom. One or more types of non-aqueous solvents can be used.
[0051] The nonaqueous solvent may contain a chain carbonate. Even if the nonaqueous electrolyte contains a chain carbonate that is generally considered to be a cause of gas generation, gas generation is suppressed and an increase in the thickness of the nonaqueous electrolyte storage element can be suppressed.
[0052] Examples of the chain carbonate include diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diphenyl carbonate, methyl trifluoroethyl carbonate (MFEC), and bis(trifluoroethyl) carbonate (FDEC).
[0053] As the chain carbonate, a fluorinated chain carbonate such as MFEC or FDEC is preferable because it can suppress side reactions during charging and discharging in which the positive electrode potential reaches a high potential.
[0054] The content of the chain carbonate in the non-aqueous electrolyte relative to all components other than the electrolyte salt is preferably 20% by volume to 80% by volume, more preferably 30% by volume to 70% by volume. The content of the chain carbonate in the non-aqueous electrolyte relative to the total of the phosphate ester and the non-aqueous solvent is also preferably within the above numerical range. The content of the chain carbonate in the non-aqueous solvent is preferably 20% by volume to 90% by volume, more preferably 50% by volume to 90% by volume.
[0055] The non-aqueous solvent may contain a cyclic carbonate. Examples of the cyclic carbonate include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), vinylene carbonate (VC), vinylethylene carbonate (VEC), chloroethylene carbonate, fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), fluoromethylethylene carbonate, trifluoroethylethylene carbonate, styrene carbonate, catechol carbonate, 1-phenylvinylene carbonate, and 1,2-diphenylvinylene carbonate.
[0056] As the cyclic carbonate, fluorinated cyclic carbonates such as FEC and DFEC are preferred because they can suppress side reactions during charging and discharging in which the positive electrode potential reaches a high potential, etc. On the other hand, even when the nonaqueous electrolyte contains a fluorinated cyclic carbonate that is generally considered to be a cause of gas generation, gas generation is suppressed and an increase in the thickness of the nonaqueous electrolyte storage element can be suppressed.
[0057] The content of the cyclic carbonate in the non-aqueous electrolyte relative to all components other than the electrolyte salt is preferably 5% by volume to 50% by volume, more preferably 10% by volume to 40% by volume. The content of the cyclic carbonate in the non-aqueous electrolyte relative to the total of the phosphate ester and the non-aqueous solvent is also preferably within the above numerical range. The content of the cyclic carbonate in the non-aqueous solvent is preferably 10% by volume to 60% by volume, more preferably 15% by volume to 45% by volume.
[0058] The non-aqueous solvent preferably contains a chain carbonate and a cyclic carbonate. When the chain carbonate and the cyclic carbonate are used in combination, the volume ratio of the chain carbonate to the cyclic carbonate (chain carbonate:cyclic carbonate) is not particularly limited, but is preferably, for example, 50:50 or more and 90:10 or less.
[0059] The content of carbonate in the non-aqueous solvent (the total content of chain carbonate and cyclic carbonate) may be preferably 50% by volume or more, more preferably 90% by volume or more, and even more preferably 99% by volume or more or substantially 100% by volume. In this way, when carbonate is the main non-aqueous solvent, the effects of the present invention may be more fully exhibited.
[0060] The lower limit of the total content of the fluorinated solvent in the non-aqueous solvent is preferably 50% by volume, more preferably 90% by volume, and even more preferably 99% by volume. The fluorinated solvent refers to a solvent (non-aqueous solvent) having a fluorine atom in the molecule, such as a fluorinated carbonate (a fluorinated chain carbonate and a fluorinated cyclic carbonate). By setting the total content of the fluorinated solvent to the above lower limit or more, the capacity retention rate can be further increased, especially after the charge-discharge cycle in which the positive electrode potential reaches a high potential.
[0061] The non-aqueous electrolyte may contain other additives, but the upper limit of the content of components other than the electrolyte salt, the phosphate ester, and the non-aqueous solvent in the non-aqueous electrolyte may be preferably 20% by mass, more preferably 5% by mass, even more preferably 2% by mass, and even more preferably 1% by mass or 0.1% by mass.
[0062] <Non-aqueous electrolyte electricity storage element> The nonaqueous electrolyte storage element according to one embodiment of the present invention has a positive electrode, a negative electrode, and a nonaqueous electrolyte. The nonaqueous electrolyte storage element may further have a separator. Hereinafter, a nonaqueous electrolyte secondary battery (hereinafter, also simply referred to as a "secondary battery") will be described as an example of a nonaqueous electrolyte storage element. The positive electrode and the negative electrode are usually stacked or wound alternately through a separator to form an electrode body. That is, the electrode body is usually composed of a positive electrode, a negative electrode, and a separator. This electrode body is stored in a container, and the container is filled with a nonaqueous electrolyte. The nonaqueous electrolyte is interposed between the positive electrode and the negative electrode. In addition, as the container, a known metal container, a resin container, etc. that are usually used as a container for a secondary battery can be used.
[0063] (positive electrode) The positive electrode has a positive electrode substrate and a positive electrode active material layer disposed on the positive electrode substrate directly or via an intermediate layer.
[0064] The positive electrode substrate has electrical conductivity. Here, the term "electrically conductive" means that the volume resistivity measured in accordance with JIS-H-0505 (1975) is 10 7"Non-conductive" means that the volume resistivity is 10 7 It means that the resistance is more than Ω·cm. As the material of the substrate, metals such as aluminum, titanium, tantalum, stainless steel, etc. or their alloys are used. Among these, aluminum and aluminum alloys are preferred because of the balance between high conductivity and cost. In addition, when the positive electrode substrate is aluminum or an aluminum alloy, the addition of phosphorus oxoacid to the positive electrode mixture can suppress the decrease in the capacity retention rate due to the oxidation corrosion of the aluminum of the positive electrode substrate. Examples of the form of the positive electrode substrate include foil and vapor deposition film, and foil is preferred from the viewpoint of cost. In other words, aluminum foil is preferred as the positive electrode substrate. In addition, examples of aluminum or aluminum alloys include A1085P, A3003P, etc. specified in JIS-H-4000 (2014).
[0065] The average thickness of the positive electrode substrate is preferably 3 μm or more and 50 μm or less, more preferably 5 μm or more and 40 μm or less, even more preferably 8 μm or more and 30 μm or less, and particularly preferably 10 μm or more and 25 μm or less. By setting the average thickness of the positive electrode substrate within the above range, it is possible to increase the strength of the positive electrode substrate while increasing the energy density per volume of the secondary battery. The "average thickness" refers to the value obtained by dividing the punched mass when a substrate of a predetermined area is punched out by the true density and punched area of the substrate. The "average thickness" is also defined in the same way when used for other members, etc.
[0066] The intermediate layer is a coating layer on the surface of the positive electrode substrate, and contains conductive particles such as carbon particles to reduce the contact resistance between the positive electrode substrate and the positive electrode active material layer. The configuration of the intermediate layer is not particularly limited, and can be formed, for example, from a composition containing a resin binder and conductive particles.
[0067] The positive electrode active material layer is a layer formed from a positive electrode mixture. The positive electrode mixture contains a positive electrode active material. The positive electrode mixture preferably contains phosphorus atoms, and further contains optional components such as a conductive agent, a binder, a thickener, a filler, and a dispersant as necessary. When the positive electrode mixture contains phosphorus atoms, it is preferable that the maximum value of the peak assigned to P2p is present at a position of 134 eV or less in the X-ray photoelectron spectroscopy spectrum of the surface of the positive electrode mixture (positive electrode active material layer). The positive electrode active material layer is usually formed on the surface of the positive electrode substrate by coating and drying a positive electrode mixture paste containing a positive electrode active material and the like. The positive electrode mixture paste preferably contains an oxoacid of phosphorus. In the secondary battery, a part or all of the oxoacid of phosphorus may be modified. It is also presumed that the phosphorus atoms are present in a coating film formed on the surface of the positive electrode active material layer. It is presumed that the presence of phosphorus atoms derived from phosphorus oxoacid in the coating film formed on the surface of the positive electrode active material layer causes the maximum value of the peak assigned to P2p to be located at a position of 134 eV or less in the X-ray photoelectron spectroscopy spectrum of the positive electrode mixture (positive electrode active material layer) surface.
[0068] The positive electrode active material may be a lithium transition metal composite oxide or a polyanion compound. The lithium transition metal composite oxide may be, for example, Li x MO y (M represents at least one transition metal) x CoO2, Li x NiO2, Li x MnO3, Li x Ni α Co 1-α O2, Li x Ni α Co β Al 1-α-β O2, Li x Ni α Mn β Co 1-α-β O2, Li 1+x (Ni α Mn β Co 1-α-β ) 1-x Li with spinel crystal structure such as O2 xMn2O4, Li x Ni α Mn 2-α O4, etc. Also, examples of polyanion compounds include Li w Me x (XO y ) z (Me represents at least one type of transition metal, and X represents, for example, P, Si, B, V, etc.) polyanion compounds (LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4, Li3V2(PO4)3, Li2MnSiO4, Li2CoPO4F, etc.) in the above formula. The elements or polyanions in these compounds may be partially substituted with other elements or anion species. In the positive electrode active material layer, one of these compounds may be used alone, or two or more of them may be used in combination.
[0069] The positive electrode active material is a secondary battery with a positive electrode potential of 4.0 V vs. Li / Li at the end of charge voltage during normal use. + The above, and further 4.2V vs. Li / Li + or above 4.4V vs. Li / Li + In the secondary battery, the maximum potential of the positive electrode is preferably 4.0 V vs. Li / Li. + Even when used in excess of the above range, the capacity retention rate after charge / discharge cycles is high and the increase in thickness can be suppressed. + By using a positive electrode active material that can satisfy the above requirements, a secondary battery can be obtained in which the energy density is increased, the capacity retention rate after charge / discharge cycles is high, and an increase in thickness is suppressed.
[0070] The positive electrode potential at the end of charge voltage during normal use is 4.0V vs. Li / Li + Examples of the positive electrode active material that can satisfy the above conditions include lithium transition metal composite oxides, and lithium transition metal composite oxides having an α-NaFeO2 type crystal structure and containing at least one of nickel, manganese, and cobalt are preferred. 1+x (Ni α Mnβ Co 1-α-β ) 1-x O2 (0≦x<1, 0≦α≦1, 0≦β≦1, 0≦1-α-β≦1). In the above formula, x is preferably more than 0 and 0.5 or less.
[0071] Here, "normal use" refers to the case where the secondary battery is used under the recommended or specified charging and discharging conditions for the secondary battery. With regard to charging conditions, if a charger for the secondary battery is provided, normal use refers to the case where the secondary battery is used using the charger.
[0072] The lower limit of the content of the lithium transition metal composite oxide in the total positive electrode active material is preferably 50% by mass, more preferably 90% by mass, and even more preferably 99% by mass. The positive electrode active material may be substantially composed of only the lithium transition metal composite oxide. Increasing the content of the lithium transition metal composite oxide in this way can increase the energy density.
[0073] The positive electrode active material is usually a particle (powder). The average particle size of the positive electrode active material is preferably, for example, 0.1 μm or more and 20 μm or less. By setting the average particle size of the positive electrode active material to the above lower limit or more, the positive electrode active material can be easily manufactured or handled. By setting the average particle size of the positive electrode active material to the above upper limit or less, the electronic conductivity of the positive electrode active material layer is improved. In addition, when a composite of the positive electrode active material and another material is used, the average particle size of the composite is taken as the average particle size of the positive electrode active material. "Average particle size" means a value at which the volume-based cumulative distribution calculated in accordance with JIS-Z-8819-2 (2001) is 50% based on the particle size distribution measured by a laser diffraction / scattering method for a diluted solution obtained by diluting particles with a solvent in accordance with JIS-Z-8825 (2013).
[0074] In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, etc. are used. Examples of the pulverization method include a method using a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, or a sieve. During pulverization, wet pulverization in the presence of water or an organic solvent such as hexane can also be used. As a classification method, a sieve, an air classifier, etc. are used as necessary for both the dry and wet methods.
[0075] The content of the positive electrode active material in the positive electrode active material layer can be, for example, from 80% by mass to 98% by mass, and is preferably 90% by mass or more.
[0076] In the X-ray photoelectron spectroscopy spectrum of the positive electrode mixture (positive electrode active material layer) surface, the upper limit of the position of the maximum value of the peak assigned to P2p is preferably 134.0 eV, more preferably 133.5 eV, while the lower limit of the position of the maximum value of this peak may be 130 eV or 132 eV.
[0077] The conductive agent is not particularly limited as long as it is a conductive material that does not adversely affect the performance of the secondary battery. Examples of such conductive agents include natural or artificial graphite, carbon black such as furnace black, acetylene black, and ketjen black, metals, conductive ceramics, etc., and acetylene black is preferred. The conductive agent may be in the form of powder, fiber, etc.
[0078] Examples of binders include thermoplastic resins such as fluororesins (polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), etc.), polyethylene, polypropylene, and polyimide; elastomers such as ethylene-propylene-diene rubber (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), and fluororubber; and polysaccharide polymers.
[0079] Examples of the thickener include polysaccharide polymers such as carboxymethyl cellulose (CMC), methyl cellulose, etc. In addition, when the thickener has a functional group that reacts with lithium, it is preferable to deactivate this functional group in advance by methylation or the like.
[0080] The filler is not particularly limited as long as it does not adversely affect the performance of the electricity storage device. Examples of the main component of the filler include polyolefins such as polypropylene and polyethylene, silica, alumina, zeolite, and glass.
[0081] The positive electrode active material layer (positive electrode mixture) may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the positive electrode active material, conductive agent, binder, thickener, and filler.
[0082] (Negative electrode) The negative electrode has a negative electrode substrate and a negative electrode active material layer disposed on the negative electrode substrate directly or via an intermediate layer, which may have the same structure as the intermediate layer of the positive electrode.
[0083] The negative electrode substrate can have the same structure as the positive electrode substrate, but the material is a metal such as copper, nickel, stainless steel, nickel-plated steel, or an alloy thereof, and copper or a copper alloy is preferred. That is, the negative electrode substrate is preferably a copper foil. Examples of the copper foil include rolled copper foil and electrolytic copper foil.
[0084] The average thickness of the negative electrode substrate is preferably 2 μm to 35 μm, more preferably 3 μm to 30 μm, further preferably 4 μm to 25 μm, and particularly preferably 5 μm to 20 μm. By setting the average thickness of the negative electrode substrate within the above range, it is possible to increase the strength of the negative electrode substrate and to increase the energy density per volume of the secondary battery.
[0085] The negative electrode active material layer is formed from a negative electrode mixture containing a negative electrode active material. The negative electrode mixture forming the negative electrode active material layer contains optional components such as a conductive agent, a binder, a thickener, a filler, a dispersant, etc. as necessary. The optional components such as the conductive agent, the binder, the thickener, the filler, the dispersant, etc. can be the same as those of the positive electrode active material layer.
[0086] The negative electrode active material layer (negative electrode mixture) may contain typical nonmetallic elements such as B, N, P, F, Cl, Br, and I, typical metallic elements such as Li, Na, Mg, Al, K, Ca, Zn, Ga, Ge, Sn, Sr, and Ba, and transition metallic elements such as Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Mo, Zr, Nb, and W as components other than the negative electrode active material, conductive agent, binder, thickener, and filler.
[0087] The negative electrode active material can be appropriately selected from known negative electrode active materials. A material capable of absorbing and releasing lithium ions is usually used as the negative electrode active material for lithium ion secondary batteries. Examples of the negative electrode active material include metal Li; metals or semimetals such as Si and Sn; metal oxides or semimetal oxides such as Si oxide, Ti oxide, and Sn oxide; Li4Ti5O 12 Examples of the material include titanium-containing oxides such as LiTiO2 and TiNb2O7; polyphosphate compounds; silicon carbide; and carbon materials such as graphite and non-graphitic carbon (easily graphitized carbon or non-graphitizable carbon). Among these materials, graphite and non-graphitic carbon are preferred. In the negative electrode active material layer, one of these materials may be used alone, or two or more of them may be used in combination.
[0088] "Graphite" refers to graphite that has an average lattice spacing (d 002 ) is 0.33 nm or more and less than 0.34 nm. Examples of graphite include natural graphite and artificial graphite. Artificial graphite is preferred from the viewpoint of availability of materials with stable physical properties.
[0089] "Non-graphitic carbon" refers to carbon that has an average lattice spacing (d002 ) is 0.34 nm or more and 0.42 nm or less. Examples of non-graphitizable carbon include non-graphitizable carbon and graphitizable carbon. Examples of non-graphitizable carbon include resin-derived materials, petroleum pitch or petroleum pitch-derived materials, petroleum coke or petroleum coke-derived materials, plant-derived materials, and alcohol-derived materials.
[0090] Here, the "discharged state" refers to a state in which the open circuit voltage is 0.7 V or more in a single-electrode battery using a negative electrode containing a carbon material as a negative electrode active material as a working electrode and metallic Li as a counter electrode. Since the potential of the metallic Li counter electrode in the open circuit state is approximately equal to the redox potential of Li, the open circuit voltage in the single-electrode battery is approximately equal to the potential of the negative electrode containing the carbon material relative to the redox potential of Li. In other words, the open circuit voltage of 0.7 V or more in the single-electrode battery means that lithium ions capable of being absorbed and released during charging and discharging are sufficiently released from the carbon material, which is the negative electrode active material.
[0091] "Non-graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.36 nm or more and 0.42 nm or less.
[0092] "Graphitizable carbon" means the above d 002 This refers to carbon materials with a particle size of 0.34 nm or more and less than 0.36 nm.
[0093] The negative electrode active material is usually a particle (powder). The average particle size of the negative electrode active material can be, for example, 1 μnm or more and 100 μm or less. When the negative electrode active material is, for example, a carbon material, the average particle size may be preferably 1 μm or more and 100 μm or less. When the negative electrode active material is a metal, a semi-metal, a metal oxide, a semi-metal oxide, a titanium-containing oxide, a polyphosphate compound, or the like, the average particle size may be preferably 1 nm or more and 1 μm or less. By setting the average particle size of the negative electrode active material to the above lower limit or more, the production or handling of the negative electrode active material becomes easy. By setting the average particle size of the negative electrode active material to the above upper limit or less, the electronic conductivity of the active material layer is improved. In order to obtain powder with a predetermined particle size, a pulverizer, a classifier, or the like is used. The pulverization method and the powder classification method can be selected, for example, from the methods exemplified for the positive electrode.
[0094] The content of the negative electrode active material in the negative electrode active material layer is preferably 60% by mass to 99% by mass, more preferably 90% by mass to 98% by mass. By setting the content of the negative electrode active material in the above range, both high energy density and manufacturability of the negative electrode active material layer can be achieved.
[0095] (Separator) The separator may be made of a material such as woven fabric, nonwoven fabric, or porous resin film. Among these, a porous resin film is preferred from the viewpoint of strength, and a nonwoven fabric is preferred from the viewpoint of nonaqueous electrolyte retention. As the main component of the separator, a polyolefin such as polyethylene or polypropylene is preferred from the viewpoint of strength, and a polyimide or aramid is preferred from the viewpoint of resistance to oxidation and decomposition. These resins may also be combined.
[0096] An inorganic insulating layer may be disposed between the separator and the electrode (usually, the positive electrode). This inorganic insulating layer is a porous layer also called a heat-resistant layer. A separator having an inorganic insulating layer formed on one or both surfaces of a porous resin film may also be used. The inorganic insulating layer is usually composed of inorganic insulating particles and a binder, and may contain other components. As the inorganic insulating particles, Al2O3, SiO2, aluminosilicate, etc. are preferable.
[0097] (Non-aqueous electrolyte) The non-aqueous electrolyte used in the secondary battery is the non-aqueous electrolyte according to one embodiment of the present invention described above.
[0098] (Maximum potential of positive electrode, etc.) The secondary battery has a maximum positive electrode potential of 4.0 V vs. Li / Li + Even after the charge-discharge cycle of 4.0V vs. Li / Li, the capacity retention rate is high and the increase in thickness is suppressed. + The lower limit of the maximum potential of the positive electrode of the secondary battery is 4.0 V vs. Li / Li. + is preferred, 4.2V vs. Li / Li + is more preferable, 4.4V vs. Li / Li + is more preferable, 4.6V vs. Li / Li + It is even more preferable that the maximum potential of the positive electrode is high. This high maximum potential of the positive electrode can increase the energy density. The upper limit of the maximum potential of the positive electrode is, for example, 5.4 V vs. Li / Li + 5.0V vs. Li / Li + may be also possible.
[0099] The maximum potential of the positive electrode is preferably the positive electrode potential at the end of charge voltage of the secondary battery during normal use. In general, when the positive electrode potential frequently reaches a high potential due to repeated charging and discharging, the capacity is likely to decrease and the thickness is likely to increase. Therefore, when the maximum potential of the positive electrode frequently reaches, for example, 4.0 V vs. Li / Li due to repeated charging and discharging, + In the above cases, the effect of improving the capacity retention rate of the secondary battery after charge / discharge cycles and the effect of suppressing an increase in thickness are more significantly exhibited.
[0100] <Method of Manufacturing Nonaqueous Electrolyte Storage Element> The nonaqueous electrolyte storage element is preferably produced by the following method: That is, the method for producing a nonaqueous electrolyte storage element according to one embodiment of the present invention includes preparing a nonaqueous electrolyte containing an imide salt, a tetrafluoroborate, and a phosphate ester (nonaqueous electrolyte preparation step).
[0101] The manufacturing method preferably further includes the step of producing a positive electrode using the positive electrode mixture paste (positive electrode producing step). In this case, the positive electrode mixture paste preferably contains an oxoacid of phosphorus.
[0102] (Non-aqueous electrolyte preparation process) In this step, the imide salt, the tetrafluoroborate, and the phosphate ester, as well as other components as necessary, are mixed to prepare the non-aqueous electrolyte, and it is preferable that the hexafluorophosphate is not substantially mixed.
[0103] (Positive electrode manufacturing process) The positive electrode mixture paste usually contains a positive electrode active material and a binder in addition to the phosphorus oxoacid, which is a preferred component, and further contains other components as necessary. The positive electrode mixture paste can be obtained by mixing these components. By applying this positive electrode mixture paste to the surface of the positive electrode substrate and drying it, a positive electrode is obtained in which the maximum value of the peak assigned to P2p is present at a position of 134 eV or less in the X-ray photoelectron spectroscopy spectrum of the positive electrode mixture.
[0104] The phosphorus oxoacid refers to a compound having a structure in which a hydroxyl group (-OH) and an oxy group (=O) are bonded to a phosphorus atom. Examples of the phosphorus oxoacid include phosphoric acid (H3PO4), phosphonic acid (H3PO3), phosphinic acid (H3PO2), pyrophosphoric acid (H4P2O7), and polyphosphoric acid. Among these, phosphoric acid and phosphonic acid are preferred, and phosphonic acid is more preferred. The phosphorus oxoacid forms a coating containing phosphorus atoms on the positive electrode.
[0105] The content (addition amount) of the phosphorus oxoacid in the positive electrode mixture paste is preferably 0.05 parts by mass to 5 parts by mass, more preferably 0.1 parts by mass to 3 parts by mass, and even more preferably 0.3 parts by mass to 2 parts by mass, relative to 100 parts by mass of the positive electrode active material. By setting the content of the phosphorus oxoacid within the above range, the capacity retention rate after charge-discharge cycles of the nonaqueous electrolyte storage element can be further increased.
[0106] The positive electrode mixture paste usually uses an organic solvent as a dispersion medium, such as polar solvents such as N-methyl-2-pyrrolidone (NMP), acetone, and ethanol, and non-polar solvents such as xylene, toluene, and cyclohexane.
[0107] The method for applying the positive electrode mixture paste is not particularly limited, and may be a known method such as roller coating, screen coating, or spin coating.
[0108] The manufacturing method may include other steps included in a manufacturing method of a normal nonaqueous electrolyte storage element in addition to the nonaqueous electrolyte preparation step and the positive electrode preparation step. The manufacturing method may include, for example, preparing a negative electrode, forming an electrode body in which the positive electrode and the negative electrode are alternately stacked by stacking or rolling them with a separator interposed therebetween, housing the positive electrode and the negative electrode (electrode body) in a container, and injecting the nonaqueous electrolyte into the container. Usually, the electrode body is housed in a container, and then the nonaqueous electrolyte is injected into the container, but this order may be reversed. After these steps, the injection port is sealed to obtain a nonaqueous electrolyte storage element.
[0109] <Other embodiments> The present invention is not limited to the above embodiment, and can be embodied in various modified and improved forms in addition to the above embodiment. For example, the positive electrode or negative electrode does not need to have an intermediate layer. In addition, the positive electrode of the nonaqueous electrolyte storage element does not need to have a clear layer formed by the positive electrode mixture. For example, the positive electrode may have a structure in which the positive electrode mixture is supported on a mesh-shaped positive electrode base material.
[0110] In the above embodiment, the nonaqueous electrolyte storage element is mainly a nonaqueous electrolyte secondary battery, but the nonaqueous electrolyte storage element may be another type of nonaqueous electrolyte storage element, such as a capacitor (electric double layer capacitor, lithium ion capacitor, etc.).
[0111] FIG. 1 is a schematic diagram of a rectangular nonaqueous electrolyte storage element 1, which is one embodiment of the nonaqueous electrolyte storage element according to the present invention. The figure is a see-through view of the inside of a container. In the nonaqueous electrolyte storage element 1 shown in FIG. 1, an electrode body 2 is housed in a container 3. The electrode body 2 is formed by winding a positive electrode having a positive electrode mixture and a negative electrode having a negative electrode mixture with a separator interposed therebetween. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 41, and the negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 51. A nonaqueous electrolyte is poured into the container 3.
[0112] The configuration of the nonaqueous electrolyte storage element according to the present invention is not particularly limited, and examples thereof include a cylindrical battery, a prismatic battery (rectangular battery), and a flat battery. The present invention can also be realized as an electricity storage device including a plurality of the nonaqueous electrolyte storage elements. One embodiment of the electricity storage device is shown in FIG. 2. In FIG. 2, an electricity storage device 30 includes a plurality of electricity storage units 20. Each electricity storage unit 20 includes a plurality of nonaqueous electrolyte storage elements 1. The electricity storage device 30 can be mounted as a power source for automobiles such as electric vehicles (EVs), hybrid vehicles (HEVs), and plug-in hybrid vehicles (PHEVs). EXAMPLES
[0113] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0114] (Preparation of lithium-excess positive electrode active material) 17.7 g of nickel sulfate hexahydrate and 32.5 g of manganese sulfate pentahydrate were weighed, and the total amount was dissolved in 200 mL of ion-exchanged water to prepare a 1.0 mol / L sulfate aqueous solution with a molar ratio of Ni:Mn of 33.3:66.7. Meanwhile, 750 mL of ion-exchanged water was poured into a 2 L reaction vessel, and CO2 gas was bubbled for 30 min to dissolve CO2 in the ion-exchanged water. The temperature of the reaction vessel was set to 50°C (±2°C), and the sulfate aqueous solution was dripped at a rate of 2 mL / min while stirring the reaction vessel at a rotation speed of 700 rpm using a paddle blade equipped with a stirring motor. Here, the pH in the reaction vessel was controlled to always be kept at 7.9 (±0.05) by appropriately dripping an aqueous solution containing 1.0 M sodium carbonate from the start to the end of the drip. After the dripping was completed, stirring in the reaction vessel was continued for another 5 h. After stirring was stopped, the mixture was allowed to stand for 12 hours or more. Next, the coprecipitated carbonate particles formed in the reaction tank were separated using a suction filter, and sodium ions attached to the particles were washed off using ion-exchanged water. The particles were then dried in an air atmosphere at normal pressure and 80°C for 20 hours using an electric furnace. After that, the particles were ground in an agate mortar for several minutes to make the particle size uniform. In this way, the coprecipitated carbonate precursor was produced.
[0115] 1.2 g of lithium carbonate was added to 2.8 g of the coprecipitated carbonate precursor, and mixed thoroughly using an agate mortar to prepare a mixed powder with a molar ratio of Li:(Ni,Mn) of 1.35:1. Using a pellet molding machine, the mixture was molded at a pressure of 40 MPa to obtain a pellet with a diameter of 25 mm. The amount of the mixed powder used for pellet molding was determined by converting it so that the mass of the expected final product was 2.5 g. One pellet was placed on the lid of an alumina crucible with a total length of about 50 mm, placed in a box-type electric furnace (model number: AMF20), and heated from room temperature to a temperature of 890°C over 10 hours in an air atmosphere under normal pressure, and fired at the temperature after the temperature increase for 9 hours. The internal dimensions of the box-type electric furnace were 10 cm long, 20 cm wide, and 30 cm deep, with heating wires spaced 20 cm apart in the width direction. After firing, the heater was turned off and the alumina crucible was left in the furnace with the lid on and cooled naturally. As a result, the temperature of the furnace dropped to about 200°C after 5 hours, but the temperature drop rate thereafter was somewhat slow. After a day and night, it was confirmed that the temperature of the furnace was below 100°C, and the pellets were taken out and crushed in an agate mortar for several minutes to make the particle size uniform. In this way, the lithium-excess positive electrode active material Li 1.35 Ni 0.315 Mn 0.685 O2 was produced.
[0116] (Aluminum treatment of lithium-excess positive electrode active material) Aluminum sulfate hydrate and ion-exchanged water were mixed in a 300 mL Erlenmeyer flask to prepare an aluminum sulfate aqueous solution with an aluminum sulfate concentration of 0.5 mol / L. The aluminum sulfate aqueous solution was stirred at 25°C and 400 rpm using a stirrer, and 5.0 g of the lithium-excess positive electrode active material was added. After adding the lithium-excess positive electrode active material, the lithium-excess positive electrode active material was collected on a filter paper by suction filtration 30 seconds later. This lithium-excess type positive electrode active material was dried in air at normal pressure and 80° C. for 20 hours using a dryer to obtain an aluminum-treated lithium-excess type positive electrode active material.
[0117] (Heat treatment of aluminum-treated lithium-rich positive electrode active material) The above aluminum-treated lithium-excess type positive electrode active material was placed on the lid of an alumina crucible, which was then placed in a box-type electric furnace (model number: AMF20) and heat-treated in air under conditions of a temperature increase rate of 5°C / min, a heat treatment temperature of 400°C, and a holding time of 4 hours, thereby obtaining an aluminum-coated lithium-excess type positive electrode active material.
[0118] (Preparation of positive electrode) A positive electrode mixture paste was prepared containing the above-mentioned aluminum-coated lithium-excess positive electrode active material: acetylene black (AB): polyvinylidene fluoride (PVDF): phosphonic acid (H3PO3) in a ratio of 93.5: 4.5: 1.5: 0.5 (solid equivalent), and N-methylpyrrolidone (NMP) as a dispersion medium. This positive electrode paste was applied to one side of an aluminum foil, which is a positive electrode substrate. The positive electrode mixture paste was then dried at 100°C for 1 h to remove the NMP in the positive electrode mixture paste, thereby forming a positive electrode active material layer. The positive electrode mixture paste was also applied to the opposite side of the aluminum foil in the same manner and dried. The positive electrode active material layer formed on this opposite side was peeled off after drying. In this way, a positive electrode was obtained.
[0119] (Preparation of negative electrode) A negative electrode was fabricated using graphite as the negative electrode active material.
[0120] [Example 1] (Preparation of non-aqueous electrolyte) Fluoroethylene carbonate (FEC), methyl trifluoroethyl carbonate (MFEC), and tris(2,2,2-trifluoroethyl)phosphate (TFEP:O=P(OCH2CF3)3) were mixed in a volume ratio of 30:65:5. Furthermore, lithium bis(fluorosulfonyl)imide (LiFSI) was dissolved as an electrolyte salt at a concentration of 0.75 mol / kg, and lithium tetrafluoroborate (LiBF4) was dissolved at a concentration of 0.25 mol / kg to prepare the nonaqueous electrolyte of Example 1.
[0121] (Fabrication of non-aqueous electrolyte storage element) The positive electrode and the negative electrode were laminated with a separator made of a microporous polyolefin film interposed therebetween to prepare an electrode assembly. The electrode assembly was placed in a container made of a metal resin composite film, and the nonaqueous electrolyte of Example 1 was poured into the container, which was then sealed by thermal welding to obtain a nonaqueous electrolyte storage element (laminate-type nonaqueous electrolyte secondary battery) of Example 1.
[0122] [Examples 2 to 9, Comparative Examples 1 to 8] The nonaqueous electrolytes and nonaqueous electrolyte storage elements of Examples 2 to 9 and Comparative Examples 1 to 8 were obtained in the same manner as in Example 1, except that the compositions of the nonaqueous electrolytes were as shown in Table 1.
[0123] The non-aqueous solvents and phosphate esters in the table represent the following compounds. FEC: Fluoroethylene carbonate MFEC: Methyl trifluoroethyl carbonate TFEP: Tris(2,2,2-trifluoroethyl) phosphate (O=P(OCH2CF3)3) TEP: Triethyl phosphate (O=P(OCH2CH3)3) TAP: Triallyl phosphate (O=P(OCH2CH=CH2)3) HFiP: Tris(1,1,1,3,3,3-hexafluoro-2-propyl) phosphate (O=P(OCH(CF3)2)3) BTP: Bis(2,2,2-trifluoroethyl) phosphite (O=PH(OCH2CF3)2)
[0124] [evaluation] (Initial charge / discharge) The obtained nonaqueous electrolyte storage elements were initially charged and discharged under the following conditions: They were charged at a constant current of 0.1 C to 4.6 V at 25° C., and then charged at a constant voltage of 4.6 V. The charge was terminated when the charge current reached 0.05 C. After a 10-minute pause after charging, they were discharged at a constant current of 0.1 C to 2.0 V at 25° C.
[0125] (X-ray photoelectron spectroscopy measurement) The nonaqueous electrolyte storage elements of Example 1 and Comparative Example 8 in a fully discharged state after initial charging and discharging were disassembled in an argon atmosphere with a dew point of -60 ° C. or less to take out the positive electrode, and the positive electrode was washed with dimethyl carbonate and then dried under reduced pressure at room temperature. The obtained positive electrode was sealed in a transfer vessel in an argon atmosphere, introduced into a sample chamber of an X-ray photoelectron spectroscopy measurement device, and X-ray photoelectron spectroscopy was performed on the surface of the positive electrode mixture (positive electrode active material layer) of the positive electrode under the above-mentioned conditions. From the obtained spectrum, the position of the maximum value of the peak attributed to P2p was obtained by the above-mentioned method. In the positive electrode mixtures of Example 1 and Comparative Example 8, the maximum value of the peak attributed to P2p was between 133 eV and 134 eV. In addition, in the positive electrode mixture of Example 1 containing a phosphate ester, the maximum value of the peak attributed to P2p derived from the phosphate ester was also confirmed near 134.5 eV. On the other hand, in the positive electrode mixture of Comparative Example 8 in which LiPF6 was used as the electrolyte salt, the maximum value of the peak assigned to P2p derived from LiPF6 was confirmed also near 136 eV.
[0126] (Charge-discharge cycle test) After the initial charge and discharge, each nonaqueous electrolyte storage element was stored in a thermostatic chamber at 45°C for 2 hours, and then charged to 4.6V at a constant current of 0.25C, and then charged to a constant voltage of 4.6V. The charge was terminated when the charge current reached 0.05C. The positive electrode potential (= maximum potential of the positive electrode) at the end of charge was 4.7V vs. Li / Li. + After charging, the battery was allowed to rest for 10 minutes, and then discharged at a constant current of 0.25C to 2.0V. After discharging, the battery was allowed to rest for 10 minutes. This cycle of charging, discharging, and resting was counted as one cycle, and this cycle was repeated 25 times. The charging, discharging, and resting were all performed in a thermostatic chamber at 45°C.
[0127] (Capacity maintenance rate) For each nonaqueous electrolyte storage element, the discharge capacity at the 25th cycle relative to the discharge capacity at the 1st cycle in the charge-discharge cycle test is shown as the capacity retention rate (%) in Table 1. A capacity retention rate of 93.0% or more was evaluated as "A," and a capacity retention rate of less than 93.0% was evaluated as "B."
[0128] (Thickness increase) Before and after the charge-discharge cycle test, the thickness of the gas reservoir (the edge of the container excluding the heat-welded portion where the electrode body is not present) in each nonaqueous electrolyte storage element was measured with a vernier caliper. The increase in thickness (mm) of the gas reservoir after the charge-discharge cycle test compared to the thickness before the charge-discharge cycle test is shown in Table 1. A thickness increase of less than 1.50 mm was rated as "A," and a thickness increase of 1.50 mm or more was rated as "B."
[0129] [Table 1]
[0130] As shown in Table 1, each of the nonaqueous electrolyte storage elements of Examples 1 to 9, which used a nonaqueous electrolyte containing an imide salt, a tetrafluoroborate, and a phosphate, had a high capacity retention rate and a small thickness increase.
[0131] In contrast, the nonaqueous electrolyte storage element of Comparative Example 1, which uses a nonaqueous electrolyte containing LiPF6, which is a hexafluorophosphate salt, as the electrolyte salt, and which does not contain an imide salt or a tetrafluoroborate salt, has a low capacity retention rate. The nonaqueous electrolyte storage elements of Comparative Examples 2 to 6, which use a nonaqueous electrolyte containing an imide salt as the electrolyte salt, have a higher capacity retention rate than Comparative Example 1. However, Comparative Example 2, in which the nonaqueous electrolyte does not contain a tetrafluoroborate salt or a phosphate salt, and Comparative Examples 3 to 6, in which the nonaqueous electrolyte contains a phosphate salt but does not contain a tetrafluoroborate salt, all have a large thickness increase. In each of the nonaqueous electrolyte storage elements of Comparative Examples 2 to 6, although gas generation is easily caused by using an imide salt as the electrolyte salt, it is considered that a coating capable of suppressing such gas generation is not formed because the element does not contain a phosphate salt or a tetrafluoroborate salt. Furthermore, the nonaqueous electrolyte storage element of Comparative Example 7, in which BTP, which is a phosphite salt, is used instead of a phosphate salt, has a low capacity retention rate and a large thickness increase. In addition, the nonaqueous electrolyte storage elements of Comparative Example 8, which use LiPF6 similarly containing phosphorus atoms instead of phosphate ester, also have low capacity retention rates and large thickness increase due to the use of LiPF6. Comparative Example 8 uses LiPF6 containing an amount of phosphorus atoms in an amount approximately equimolar to the amount of phosphorus atoms in the phosphate ester of Example 1. These results show that the presence of both phosphate ester and tetrafluoroborate in the nonaqueous electrolyte can suppress the generation of gas that is likely to occur when an imide salt is used, thereby exerting the effect of suppressing the increase in thickness of the nonaqueous electrolyte storage element. [Industrial Applicability]
[0132] The present invention can be applied to nonaqueous electrolyte electricity storage elements used as power sources for electronic devices such as personal computers and communication terminals, and automobiles. [Explanation of symbols]
[0133] 1. Non-aqueous electrolyte storage element 2 Electrode body 3 containers 4 Positive terminal 41 Positive lead 5 Negative terminal 51 Negative lead 20 Energy Storage Unit 30 Energy storage device
Claims
1. A non-aqueous electrolyte for an electric storage element, comprising one or more imide salts selected from the group consisting of lithium imide salts, sodium imide salts, potassium imide salts, and magnesium imide salts, a tetrafluoroborate, and a phosphate, and substantially no hexafluorophosphate.
2. The nonaqueous electrolyte according to claim 1 , further comprising a chain carbonate.
3. The nonaqueous electrolyte according to claim 1 or 2, further comprising a fluorinated cyclic carbonate.
4. A nonaqueous electrolyte storage element comprising the nonaqueous electrolyte according to claim 1 .
5. Further comprising a positive electrode having a positive electrode mixture containing a phosphorus atom; 5. The nonaqueous electrolyte storage element according to claim 4, wherein in an X-ray photoelectron spectroscopy spectrum of the positive electrode mixture surface, a maximum value of a peak assigned to P2p is present at a position of 134 eV or less.
6. A method for producing a nonaqueous electrolyte storage element, comprising: preparing a nonaqueous electrolyte solution that contains one or more imide salts selected from the group consisting of lithium imide salts, sodium imide salts, potassium imide salts, and magnesium imide salts, a tetrafluoroborate, and a phosphate ester, and is substantially free of hexafluorophosphate.
7. The method for producing a nonaqueous electrolyte storage element according to claim 6 , further comprising: preparing a positive electrode using a positive electrode mixture paste containing an oxoacid of phosphorus.
Citation Information
Patent Citations
Electricity storage element
JP2015128052A
Gel polymer electrolyte and lithium secondary battery containing the same
JP2015537352A
Nonaqueous electrolyte for power storage device, nonaqueous electrolyte power storage device, and method for manufacturing the same
JP2017208215A
Nonaqueous electrolyte and nonaqueous electrolyte power storage device
JP2018101612A
Lithium secondary battery
JP2019169426A