Rubber composition and tire
A rubber composition with a polymer, polycarboxylic acid, and basic compound forms a network without sulfur, addressing the lack of handling stability in tires, enhancing tire performance through reduced stress concentration and improved responsiveness.
Patent Information
- Application Number
- JP2020017969
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-05
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-02-05
AI Technical Summary
Existing rubber compositions for tires lack sufficient handling stability, and alternative crosslinking methods to sulfur have not been adequately studied to improve this property.
A rubber composition containing a polymer with an epoxy group, polycarboxylic acid, and a basic compound, with specific properties such as a complex modulus E* of 5 MPa or more at 30°C, loss tangent of 0.14 or less at 30°C, and elongation at break of 50% or more, forms a network between polymers without using sulfur, enhancing handling stability.
The composition provides improved handling stability and responsiveness in tires by reducing stress concentration and maintaining good tire wear and responsiveness during sharp turns.
Smart Images

Figure 0007552022000003 
Figure 0007552022000002 
Figure 0007552022000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition and a tire. [Background technology]
[0002] In rubber compositions used in tires, etc., the rubber component is usually crosslinked (vulcanized) with sulfur. In recent years, various crosslinking methods using other than sulfur, such as peroxides, have been studied for the purpose of improving rubber properties (for example, see Patent Document 1), but methods for obtaining good steering stability without using sulfur have not been fully studied. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-052146 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide a rubber composition and a tire that can solve the above problems and improve steering stability. [Means for solving the problem]
[0005] The present invention relates to a rubber composition which contains a polymer having an epoxy group, a polycarboxylic acid, and a basic compound, and which has a complex modulus E* at 30°C of 5 MPa or more, a loss tangent at 30°C of 0.14 or less, and an elongation at break at 0°C of 50% or more.
[0006] It is preferable that the polycarboxylic acid further has a hydroxy group.
[0007] The rubber composition preferably contains silica and / or carbon black.
[0008] The rubber composition preferably has a loss tangent at 30° C. of 0.10 or more.
[0009] The polycarboxylic acid is preferably a compound represented by the following formula (I). HOOC-A-COOH (I) (In the formula, A is a divalent hydrocarbon group having 1 to 10 carbon atoms, which may have a substituent.)
[0010] The present invention also relates to a tire having a tread portion using the above rubber composition, the tire having a negative ratio in the contact patch of the tread portion being less than 40%. Effect of the Invention
[0011] According to the present invention, a rubber composition containing a polymer having an epoxy group, a polycarboxylic acid, and a basic compound has a complex modulus E* of 5 MPa or more at 30°C, a loss tangent of 0.14 or less at 30°C, and a breaking elongation of 50% or more at 0°C, so that a rubber composition and a pneumatic tire having good steering stability can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The rubber composition of the present invention contains a polymer having an epoxy group, a polycarboxylic acid, and a basic compound, and has a complex modulus E* of 5 MPa or more at 30°C, a loss tangent of 0.14 or less at 30°C, and a breaking elongation of 50% or more at 0°C.
[0013] The reason why the above rubber composition provides good steering stability without using sulfur is not clear, but is presumed to be as follows.
[0014] The epoxy group of the polymer and the carboxy group of the polycarboxylic acid can be chemically bonded by using a basic compound as a catalyst. Since the polycarboxylic acid has multiple carboxy groups, it is believed that a network is formed between the polymers via the polycarboxylic acid, thereby crosslinking the polymers.
[0015] In such a network, the distance between polymers is basically determined by the length of the hydrocarbon group in the polycarboxylic acid, so the distance between polymers is kept constant. This makes it difficult for stress concentration to occur, so it is thought that stress can be generated throughout the polymer matrix even when a large input is applied, such as the tire when a car makes a sharp turn.
[0016] In addition, in the above rubber composition, it is believed that by making the complex modulus E* at 30°C to be 5 MPa or more and the loss tangent (tan δ) at 30°C to be 0.14 or less, the responsiveness when operating the steering wheel of a car will be good.
[0017] In addition, when a driver turns the steering wheel of a car, the tire's traveling direction and rotation direction temporarily differ, and it is believed that the input (deformation of the tire) applied to the tire at this time temporarily becomes high frequency. By making the breaking elongation of the above rubber composition at 0°C, which is lower than room temperature, 50% or more, it is believed that tire wear at the moment the steering angle is turned can be suppressed and good responsiveness can be maintained.
[0018] In this specification, the complex modulus E* and tan δ of a rubber composition (after crosslinking) are measured using an Eplexer manufactured by GABO under conditions of a frequency of 10 Hz, an initial strain of 10%, a dynamic strain of 1%, and a temperature of 30°C.
[0019] In this specification, the breaking elongation of the rubber composition (after crosslinking) is measured in accordance with JIS K 6251:2017 by carrying out a tensile test at 0°C using a No. 7 dumbbell-shaped test piece.
[0020] As described above, the complex modulus E* of the rubber composition at 30° C. is 5 MPa or more, preferably 8 MPa or more, more preferably 10 MPa or more, and even more preferably 12 MPa or more, and is preferably 25 MPa or less, more preferably 20 MPa or less, and even more preferably 18 MPa or less. Within the above range, the effect tends to be preferably obtained.
[0021] As described above, the tan δ of the rubber composition at 30° C. is 0.14 or less, preferably 0.13 or less, more preferably 0.12 or less, and preferably 0.05 or more, more preferably 0.08 or more, and even more preferably 0.10 or more. Within the above ranges, the effect tends to be favorably obtained.
[0022] As described above, the breaking elongation of the rubber composition at 0° C. is 50% or more, preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more, and is preferably 800% or less, more preferably 500% or less, and even more preferably 400% or less. Within the above ranges, the effect tends to be preferably obtained.
[0023] The complex modulus E*, tan δ, and elongation at break of the rubber composition can be adjusted by the type and amount of chemicals (particularly rubber components, fillers, softeners, sulfur, vulcanization accelerators, silane coupling agents, and polycarboxylic acids) blended into the rubber composition. For example, the complex modulus E* tends to increase with a decrease in the amount of softener, an increase in the amount of filler, and an increase in the amount of sulfur. Tan δ tends to decrease with the use of a softener that is highly compatible with the rubber component, a decrease in the amount of softener, an increase in the amount of sulfur, an increase in the amount of vulcanization accelerator, and an increase in the amount of silane coupling agents. The elongation at break tends to increase with an increase in the amount of softener, a decrease in the amount of filler, and a decrease in the amount of polycarboxylic acid.
[0024] The following describes the drugs that can be used.
[0025] The rubber composition contains a polymer having an epoxy group (epoxidized polymer).
[0026] The epoxidized polymer is obtained by epoxidizing a polymer by a general method, such as oxidizing the polymer with a peroxide. Examples of the polymer to be epoxidized include thermosetting elastomers such as rubber components, and thermoplastic elastomers such as polyolefins and polystyrene. These may be used alone or in combination of two or more. Among them, from the viewpoint of steering stability when used in tires, thermosetting elastomers are preferred, and rubber components are more preferred.
[0027] Examples of rubber components that can be used in the epoxidized polymer include diene rubbers such as isoprene rubber, butadiene rubber (BR), styrene butadiene rubber (SBR), and styrene isoprene butadiene rubber (SIBR). Examples of isoprene rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. These may be used alone or in combination of two or more. Among these, SBR, BR, and isoprene rubber are preferred, isoprene rubber is more preferred, and NR is even more preferred.
[0028] The epoxidation rate of the epoxidized polymer is preferably 5 mol% or more, more preferably 15 mol% or more, even more preferably 25 mol% or more, particularly preferably 30 mol% or more, and is preferably 80 mol% or less, more preferably 65 mol% or less, even more preferably 50 mol% or less. Within the above ranges, the effect tends to be favorably obtained. The epoxidation rate means the ratio of the number of epoxidized carbon-carbon double bonds to the total number of carbon-carbon double bonds in the polymer before epoxidation, and can be determined, for example, by titration analysis or nuclear magnetic resonance (NMR) analysis.
[0029] When the epoxidized polymer is a rubber component (e.g., epoxidized natural rubber (ENR)), the content of the epoxidized polymer in 100% by mass of the rubber component is preferably 50% by mass or more, more preferably 65% by mass or more, even more preferably 80% by mass or more, particularly preferably 90% by mass or more, and may be 100% by mass. Within the above range, the effect tends to be preferably obtained.
[0030] When the epoxidized polymer is not a rubber component (for example, when it is an epoxidized polyethylene), the content of the epoxidized polymer relative to 100 parts by mass of the rubber component is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, even more preferably 40 parts by mass or less. Within the above ranges, the effects tend to be favorably obtained.
[0031] The rubber composition contains a polycarboxylic acid. The polycarboxylic acid is a carboxylic acid having a plurality of carboxy groups, and a compound represented by the following formula (I) can be suitably used. Since this compound has carboxy groups at both ends, it is possible to form a strong network between polymers, and it is believed that better steering stability can be obtained. In addition, an effect of improving fuel efficiency (low heat generation) is also expected. HOOC-A-COOH (I) (In the formula, A is a divalent hydrocarbon group having 1 to 10 carbon atoms, which may have a substituent.)
[0032] The hydrocarbon group of A may have 1 to 10 carbon atoms, preferably 2 or more, and preferably 6 or less, more preferably 4 or less, and further preferably 3 or less.
[0033] Examples of the hydrocarbon group for A include an alkylene group, an alkenylene group, a cycloalkylene group, and an arylene group, and an alkylene group is preferred. Furthermore, examples of the alkylene group include linear alkylene groups such as a methylene group, an ethylene group, an n-propylene group, an n-butylene group, and a hexylene group, and branched alkylene groups such as an isopropylene group, an isobutylene group, and a 2-methylpropylene group. Of these, linear alkylene groups are preferred, with an ethylene group and an n-propylene group being more preferred, and an ethylene group being even more preferred.
[0034] The hydrocarbon group of A may have a substituent. Examples of the substituent include a hydroxy group, a carboxy group, an alkoxy group, and an amino group. These may be one type or two or more types. Among them, a hydroxy group is preferable. In this way, when the polycarboxylic acid further has a hydroxy group, that is, when the polycarboxylic acid is a hydroxy acid having a carboxy group and a hydroxy group, it is considered that the stability of the intermediate formed during the reaction between the epoxy group in the epoxidized polymer and the carboxy group of the polycarboxylic acid is improved, and the strength of the network between the polymers is improved. In addition, an effect of improving fuel efficiency (low heat generation) is also expected.
[0035] Specific examples of polycarboxylic acids include dicarboxylic acids such as malic acid, tartaric acid, and suberic acid, tricarboxylic acids such as citric acid, and hexacarboxylic acids such as mellitic acid. These may be used alone or in combination of two or more. Among them, dicarboxylic acids are preferred, and dicarboxylic acids further having a hydroxyl group such as malic acid and tartaric acid are more preferred.
[0036] The content of the polycarboxylic acid is preferably 1 part by mass or more, more preferably 3 parts by mass or more, even more preferably 6 parts by mass or more, particularly preferably 7 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 12 parts by mass or less, relative to 100 parts by mass of the epoxidized polymer. Within the above ranges, the effect tends to be preferably obtained.
[0037] The rubber composition contains a basic compound. As the basic compound, an imidazole compound can be suitably used. The imidazole compound is a compound having an imidazole ring, and is preferably a compound represented by the following formula (II). [ka] (In the formula, R 1 , R 2 , R 3 , R 4 R may be the same or different and represents a hydrogen atom or a hydrocarbon group.3 , R 4 may be bonded to each other to form a ring structure.
[0038] R 1 , R 2 , R 3 , R 4 Examples of the hydrocarbon group include an alkyl group having 1 to 20 carbon atoms (preferably 2 to 12 carbon atoms), a cycloalkyl group having 5 to 24 carbon atoms (preferably 5 to 8 carbon atoms), an aryl group having 6 to 30 carbon atoms (preferably 6 to 24 carbon atoms), and an aralkyl group having 7 to 25 carbon atoms (preferably 7 to 13 carbon atoms).
[0039] Also, R 4 , R 5 When they are bonded to form a ring structure, R 4 , R 5 and the carbon atom of the imidazole ring, may be, for example, an aromatic ring, a heterocyclic ring, or an aliphatic ring having 5 to 12 carbon atoms.
[0040] In terms of the strength of the network between polymers, R 1 , R 2 , R 3 , R 4 It is preferable that at least one of R is an alkyl group. 1 , R 2 , R 3 , R 4 It is more preferable that one of R is an alkyl group and the other three are hydrogen atoms. 1 is an alkyl group, R 2 , R 3 , R 4 It is more preferable that is a hydrogen atom.
[0041] Specific examples of the imidazole compound include imidazole, 1-butylimidazole, 1-propylimidazole, 1-ethylimidazole, 1-methylimidazole, 1,2-dimethylimidazole, 1-decyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. These may be used alone or in combination of two or more. Among them, 1-butylimidazole, 1-propylimidazole, 1-ethylimidazole, and 1-methylimidazole are preferred, and 1-butylimidazole is more preferred.
[0042] The content of the basic compound is preferably 0.05 molar equivalent or more, more preferably 0.15 molar equivalent or more, even more preferably 0.25 molar equivalent or more, and is preferably 3 molar equivalent or less, more preferably 2 molar equivalent or less, even more preferably 1 molar equivalent or less, relative to the carboxyl group in the polycarboxylic acid. When the content is within the above range, the effect tends to be preferably obtained.
[0043] The rubber composition preferably contains silica and / or carbon black as a reinforcing material, which can increase the strength of the network formed between the polymers.
[0044] Examples of silica include dry process silica (anhydrous silica), wet process silica (hydrated silica), etc. Among these, wet process silica is preferred because it has a large number of silanol groups.
[0045] The amount of silica per 100 parts by mass of the rubber component is preferably 5 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 35 parts by mass, and particularly preferably 45 parts by mass, and is preferably 150 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 80 parts by mass or less.
[0046] The nitrogen adsorption specific surface area (N2SA) of the silica is preferably 30 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 150m 2 / g or more, particularly preferably 175m 2 / g or more, and preferably 300m 2 / g or less, more preferably 250m 2 / g or less, more preferably 200m 2 / g or less. The nitrogen adsorption specific surface area of silica is a value measured by the BET method in accordance with ASTM D3037-81.
[0047] As the silica, for example, products manufactured by Degussa, Rhodia, Tosoh Silica Co., Ltd., Solvay Japan Co., Ltd., Tokuyama Corporation, etc. can be used.
[0048] Silica is preferably used in combination with a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl, mercapto-based compounds such as 3-mercaptopropyltrimethoxysilane and 2-mercaptoethyltriethoxysilane; vinyl-based compounds such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based compounds such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based compounds such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based compounds such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based compounds such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. As commercially available products, for example, products from Degussa, Momentive, Shin-Etsu Silicone Co., Ltd., Tokyo Chemical Industry Co., Ltd., Azumax Co., Ltd., Toray Dow Corning Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. Among them, sulfide-based and mercapto-based silane coupling agents are preferred.
[0049] The content of the silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, and even more preferably 8 parts by mass or more, relative to 100 parts by mass of silica, and is preferably 20 parts by mass or less, and more preferably 15 parts by mass or less.
[0050] Examples of carbon black include, but are not limited to, GPF, FEF, HAF, ISAF, SAF, etc. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shin-Nichika Carbon Co., Ltd., Columbia Carbon Co., Ltd., etc.
[0051] The amount of carbon black, based on 100 parts by mass of the rubber component, is preferably 5 parts by mass or more, preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and is preferably 70 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less.
[0052] The nitrogen adsorption specific surface area (N2SA) of the carbon black is preferably 80 m 2 / g or more, more preferably 100m 2 / g or more, more preferably 110m 2 / g or more, and preferably 160m 2 / g or less, more preferably 140m 2 / g or less, more preferably 125m 2 / g or less. The nitrogen adsorption specific surface area of carbon black is a value measured in accordance with JIS K6217-2:2001.
[0053] As described above, in the rubber composition, a sufficient crosslinked structure is obtained without using sulfur because a network is formed by the epoxy groups in the epoxidized polymer and the carboxyl groups in the polycarboxylic acid, and therefore the amount of sulfur and chemicals that assist crosslinking (vulcanization) by sulfur (e.g., vulcanization accelerator, stearic acid, zinc oxide) used can be reduced.
[0054] The amount of sulfur per 100 parts by mass of the rubber component is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, further preferably 0.1 parts by mass or less, and may be 0 part by mass.
[0055] The content of the vulcanization accelerator per 100 parts by mass of the rubber component is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, further preferably 0.1 parts by mass or less, and may be 0 part by mass.
[0056] The amount of stearic acid per 100 parts by mass of the rubber component is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, further preferably 0.1 parts by mass or less, and may be 0 part by mass.
[0057] The amount of zinc oxide per 100 parts by mass of the rubber component is preferably 1 part by mass or less, more preferably 0.5 parts by mass or less, further preferably 0.1 parts by mass or less, and may be 0 part by mass.
[0058] The rubber composition may contain oil. Examples of the oil include process oil, vegetable oil, and mixtures thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. These may be used alone or in combination of two or more. Among them, process oil is preferred, and aromatic process oil is particularly preferred.
[0059] The oil content, per 100 parts by mass of the rubber component, is preferably at least 2 parts by mass, more preferably at least 5 parts by mass, and even more preferably at least 7 parts by mass, and is preferably at most 50 parts by mass, more preferably at most 30 parts by mass, and even more preferably at most 20 parts by mass. The oil content includes the amount of oil (extending oil) contained in the rubber (oil-extended rubber).
[0060] The rubber composition may contain a resin. The resin is not particularly limited as long as it is one that is commonly used in the tire industry, and examples thereof include rosin-based resins, coumarone-indene resins, α-methylstyrene-based resins, terpene-based resins, pt-butylphenol acetylene resins, acrylic resins, C5 resins, C9 resins, etc. Commercially available products include those from Maruzen Petrochemical Co., Ltd., Sumitomo Bakelite Co., Ltd., Yasuhara Chemical Co., Ltd., Tosoh Corporation, Rutgers Chemicals, BASF, Arizona Chemical Company, Nitto Chemical Co., Ltd., Nippon Shokubai Co., Ltd., JXTG Nippon Oil & Energy Co., Ltd., Arakawa Chemical Industries Co., Ltd., Taoka Chemical Co., Ltd., Toagosei Co., Ltd., etc. These may be used alone or in combination of two or more kinds.
[0061] The resin content per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and preferably 30 parts by mass or less, more preferably 20 parts by mass or less.
[0062] The rubber composition may contain a wax. The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene, etc. These may be used alone or in combination of two or more. Among them, petroleum waxes are preferred, and paraffin wax is more preferred.
[0063] As the wax, for example, products available from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. can be used.
[0064] The amount of the wax per 100 parts by mass of the rubber component is preferably 0.3 part by mass or more, more preferably 0.5 part by mass or more, and is preferably 20 parts by mass or less, more preferably 10 parts by mass or less.
[0065] The rubber composition may contain an antioxidant. Examples of the antioxidant include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di-2-naphthyl-p-phenylenediamine. Examples of the antioxidant include p-phenylenediamine antioxidants such as quinolinone; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. These antioxidants may be used alone or in combination of two or more. Among them, p-phenylenediamine antioxidants and quinoline antioxidants are preferred.
[0066] As the antioxidant, for example, products available from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Industry Co., Ltd., Flexis, etc. can be used.
[0067] The amount of the antioxidant per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less.
[0068] The rubber composition may further contain other compounding agents (such as organic crosslinking agents) that are generally used in the tire industry in addition to the above components. The content of these compounding agents is preferably 0.1 to 200 parts by mass per 100 parts by mass of the rubber component.
[0069] The rubber composition can be produced, for example, by kneading the components using a rubber kneading device such as an open roll or a Banbury mixer, and then press-molding the resulting kneaded mixture.
[0070] Regarding the kneading conditions for kneading each component, the kneading temperature is usually 100 to 180° C., preferably 120 to 170° C., and the kneading time is usually 1 to 30 minutes, preferably 2 to 10 minutes. Regarding the conditions for press molding (vulcanization) the kneaded product obtained by kneading, the temperature is usually 140 to 190° C., preferably 150 to 185° C., and the kneading time is usually 1 to 60 minutes, preferably 5 to 30 minutes.
[0071] The rubber composition can be used (as a rubber composition for tires) for tire components such as treads (cap treads), sidewalls, base treads, undertreads, clinches, bead apex, breaker cushion rubber, carcass cord covering rubber, insulation, chafers, inner liners, and the like, as well as side reinforcing layers of run-flat tires, and is particularly suitable for treads (cap treads).
[0072] The tire (pneumatic tire or the like) of the present invention is produced by a conventional method using the above rubber composition. That is, the rubber composition is extruded in an unvulcanized state to match the shape of the tread, and molded together with other tire components in a tire building machine by a normal method to form an unvulcanized tire. The unvulcanized tire is then heated and pressurized in a vulcanizer to obtain a tire.
[0073] The tire has a tread portion using the rubber composition, but it is sufficient that at least a part of the tread portion is made of the rubber composition, and the entire tread portion may be made of the rubber composition. Moreover, the rubber composition may be used not only in the tread portion but also in tire components other than the tread portion.
[0074] In the tire, the negative ratio in the contact area of the tread portion is preferably less than 40%, more preferably 35% or less, even more preferably 30% or less, particularly preferably 25% or less, and is preferably 5% or more, more preferably 10% or more, and even more preferably 15% or more. Within the above ranges, the effect tends to be preferably obtained. The negative ratio in the contact patch of the tread portion is the ratio of the total groove area in the contact patch to the total area of the contact patch.
[0075] The above-mentioned tires can be used as passenger car tires, large passenger car tires, large SUV tires, heavy load tires such as trucks and buses, light truck tires, motorcycle tires, racing tires (high performance tires), etc. They can also be used as all-season tires, summer tires, studless tires (winter tires), etc. EXAMPLES
[0076] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.
[0077] ENR50: ENR manufactured by Kunpuran Gasri (epoxidation ratio: 50 mol%) ENR25: ENR manufactured by Kunpuran Gasri (epoxidation ratio: 25 mol%) 1-Butylimidazole: 1-Butylimidazole manufactured by Tokyo Chemical Industry Co., Ltd. Malic acid: Malic acid manufactured by Fuso Chemical Co., Ltd. Tartaric acid: Tartaric acid manufactured by Fuso Chemical Industry Co., Ltd. Suberic acid: Suberic acid manufactured by Tokyo Chemical Industry Co., Ltd. Silica: Ultrasil VN3 (N2SA175m) from Evonik Degussa 2 / g) Silane coupling agent: Si69 (bis(3-triethoxysilylpropyl)tetrasulfide) from Evonik Degussa Anti-aging agent: Ozonone 6C (N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine) manufactured by Seiko Chemical Co., Ltd. Peroxide crosslinking agent: Percumyl (registered trademark) D-40 manufactured by NOF Corporation
[0078] Examples and Comparative Examples According to the compounding recipe shown in Table 1, chemicals other than sulfur and the vulcanization accelerator were kneaded for 5 minutes at 150° C. using a 1.7 L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. The resulting kneaded product was press molded in a 2 mm thick mold at 170° C. for 10 minutes to obtain a crosslinked rubber composition (sheet).
[0079] In Comparative Example 4 using a peroxide crosslinking agent, a process of kneading chemicals other than the peroxide crosslinking agent for 5 minutes at 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd., and a process of kneading the peroxide crosslinking agent for 4 minutes at 80°C using an open roll were carried out in that order, and the kneaded mixture was press molded in a 2 mm thick mold at 170°C for 10 minutes to obtain a crosslinked rubber composition (sheet).
[0080] The prepared rubber compositions were evaluated by the following methods, and the results are shown in Tables 1 and 2.
[0081] (Elongation at break) In accordance with JIS K 6251:2017, a tensile test was carried out at 0°C using a No. 7 dumbbell-shaped test piece made of the above rubber composition, and the breaking elongation (%) was measured.
[0082] (Viscoelasticity measurement (30℃E*, 30℃tanδ)) The complex elastic modulus E* and tan δ of the rubber composition were measured under conditions of a frequency of 10 Hz, an initial strain of 10%, a dynamic strain of 1%, and a temperature of 30° C. using an Iplexer manufactured by GABO Corporation.
[0083] (Handling performance) A computer simulation was performed by inputting the breaking elongation, complex modulus E*, and tan δ obtained above as the physical properties of the tread portion, and the reaction force at the moment when a steering angle was made with respect to the road surface while traveling at 80 km / h with a tire having the negative rate in Table 2 was calculated taking into account the influence of wear, and the result was expressed as an index with Comparative Example 10 being set to 100. A higher index indicates better handling performance (steering stability).
[0084] [Table 1]
[0085] [Table 2]
[0086] As can be seen from Table 2, the Examples had better steering stability than the Comparative Examples.
Claims
1. The rubber composition includes a rubber component including a polymer having an epoxy group, a polycarboxylic acid, and a basic compound, The polycarboxylic acid further has a hydroxy group, the content of the polycarboxylic acid is 1 to 12 parts by mass based on 100 parts by mass of the polymer having an epoxy group, Complex elastic modulus E* at 30°C is 5 to 25 MPa, Loss tangent at 30°C is 0.05 to 0.14, A rubber composition having a breaking elongation at 0°C of 50 to 400%.
2. The rubber composition according to claim 1, which contains silica and / or carbon black.
3. The nitrogen adsorption specific surface area of the silica is 30 m 2 / g or more 300m 2 The rubber composition according to claim 2, wherein the elastic modulus is 0.1 to 1.0 g / g or less.
4. The carbon black has a nitrogen adsorption specific surface area of 80 m 2 / g or more 160m 2 The rubber composition according to claim 2 or 3, wherein the elastic modulus is not more than 1 / g.
5. The rubber composition according to any one of claims 1 to 4, which has a loss tangent at 30°C of 0.10 or more.
6. The rubber composition according to any one of claims 1 to 5, wherein the polycarboxylic acid is a compound represented by the following formula (I): HOOC-A-COOH (I) (In the formula, A is a divalent hydrocarbon group having 1 to 10 carbon atoms, which may have a substituent.)
7. The rubber composition according to any one of claims 1 to 6, wherein the content of the polymer having an epoxy group is 50% by mass or more and 100% by mass or less based on 100% by mass of the rubber component.
8. 8. The rubber composition according to claim 1, wherein the content of the basic compound is 0.05 to 3 molar equivalents based on the carboxyl group in the polycarboxylic acid.
9. The rubber composition according to any one of claims 1 to 8, further comprising a silane coupling agent.
10. The rubber composition according to any one of claims 1 to 9, further comprising an antioxidant.
11. A tire having a tread portion using the rubber composition according to any one of claims 1 to 10, The tire has a negative ratio within the contact patch of the tread portion of less than 40%.
Citation Information
Patent Citations
Rubber composition for tire and pneumatic tire
JP2011052146A
A tire containing a rubber composition containing an epoxy elastomer crosslinked with a polycarboxylic acid
JP2016501940A
A tire containing a rubber composition containing an epoxy elastomer crosslinked with a polycarboxylic acid
JP2016501941A
Tire containing rubber composition containing epoxide polymer crosslinked with polycarboxylic acid
JP2016506430A
A tire comprising a rubber composition containing an olefinic epoxide elastomer crosslinked by a polycarboxylic acid