Polyphenylene sulfide resin composition and hollow molded article using same
A PPS resin composition with reinforcing fiber, olefin copolymer, organic silane, and phosphorus oxoacid metal salt addresses moldability and thermal stability issues, ensuring high strength and toughness for blow molding applications.
Patent Information
- Application Number
- JP2020163115
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-26
- Filing Date
- 2020-09-29
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Polyphenylene sulfide (PPS) resin compositions face challenges in blow moldability due to low melt viscosity leading to parison drawdown and insufficient toughness, while increasing fiber reinforcement for strength results in shear viscosity increase and thermal deterioration of epoxy group-containing olefin copolymers, compromising heat aging resistance.
A polyphenylene sulfide resin composition comprising 100 parts by weight of PPS resin, 1 to 200 parts by weight of reinforcing fiber, 1 to 200 parts by weight of olefin copolymer with epoxy groups, 0.01 to 10 parts by weight of organic silane compound, and 0.01 to 5 parts by weight of phosphorus oxoacid metal salt, specifically sodium phosphinate, to maintain high melt viscosity and suppress thermal deterioration.
The composition achieves excellent mechanical strength, toughness, and heat aging resistance, suitable for high-temperature applications, with improved blow moldability and reduced gas generation during molding.
Smart Images

Figure 0007552199000004 
Figure 0007552199000003 
Figure 0007552199000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyphenylene sulfide resin composition having high strength and high toughness and achieving both heat aging resistance and blow moldability, and to a blow molded article using the same. [Background technology]
[0002] As a method for improving fuel economy of automobiles, weight reduction by using resin for ducts and piping in the engine compartment has become widespread, and polyamide-based materials are currently mainly used for these.
[0003] In recent years, due to the rise in operating environment temperatures resulting from the narrowing of engine compartments and exposure to acid through exhaust gas recirculation systems, resin materials need to be designed for use in more severe environments. As a result, attention is being paid to polyphenylene sulfide (hereinafter sometimes abbreviated as PPS) as an engineering plastic with excellent heat resistance, chemical resistance, flame retardancy, and electrical properties.
[0004] On the other hand, since PPS resin has a low melt viscosity, drawdown of the parison occurs in blow molding, which is a suitable molding method for ducts and piping, making it difficult to obtain molded products with little thickness deviation. In addition, lack of toughness is also an issue in practical use. For this reason, the mainstream design is to blend an olefin copolymer containing an epoxy group into PPS resin to increase the melt viscosity and improve the toughness (for example, Patent Document 1).
[0005] However, in recent years, with the development of blow molding technology (e.g., suction blow molding), the degree of freedom in designing molded products has increased, such as by making the diameter and wall thinner, and therefore there are cases in which resin materials are required to have even higher strength and toughness, especially heat aging resistance. For this reason, many studies have been reported on improving the blow moldability and material properties of PPS resin, such as by adding organic silane compounds (e.g., Patent Document 2) and by using fiber reinforcement materials (e.g., Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 3-236930 [Patent Document 2] JP 2011-256387 A [Patent Document 3] JP 2016-183316 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, since the PPS resin compositions described in Patent Documents 2 and 3 both contain an olefin copolymer containing an epoxy group, when the amount of fiber reinforcing material is increased in order to improve strength while maintaining a high melt viscosity capable of suppressing drawdown, a sudden increase in shear viscosity and shear heat generation lead to significant deterioration of the olefin copolymer containing an epoxy group, which has low heat resistance, resulting in problems such as a decrease in mechanical properties, gas generation during molding, and particularly a decrease in heat aging resistance. [Means for solving the problem]
[0008] Therefore, the present inventors conducted intensive research to solve the above-mentioned problems, and as a result, they found that in a composition consisting of a polyphenylene sulfide resin, a fiber reinforcing material, an olefin-based copolymer containing epoxy groups, and an organosilane coupling agent, a phosphorus oxoacid metal salt exhibits several favorable effects, thereby suppressing thermal degradation of the olefin-based copolymer containing epoxy groups and making it possible to achieve both blow moldability and mechanical properties and heat aging resistance.
[0009] That is, the present invention has the following configuration. 1. (A) 100 parts by weight of polyphenylene sulfide resin, (B) 1 to 200 parts by weight of reinforcing fiber, (C) 1 to 200 parts by weight of an olefin copolymer containing an epoxy group, (D) 0.01 to 10 parts by weight of an organic silane compound, and (E) a phosphorus oxoacid metal SaltA polyphenylene sulfide resin composition comprising 0.01 to 5 parts by weight of (E) The phosphorus oxoacid metal salt is sodium phosphinate, and the polyphenylene sulfide resin composition A polyphenylene sulfide resin composition having a flexural strength of 100 MPa or more and 300 MPa or less, as measured in accordance with ISO 178 using an ISO (1A) dumbbell test piece obtained by injection molding. 2. The polyphenylene sulfide resin composition according to item 1, in which the blending amount of the reinforcing fiber (B) is 15% by weight or more and 50% by weight or less, when the total of the polyphenylene sulfide resin (A), the reinforcing fiber (B), and the olefin-based copolymer (C) containing an epoxy group is 100% by weight. 3. The polyphenylene sulfide resin composition according to any one of items 1 to 2, having a melt viscosity measured at a temperature of 300°C and a shear rate of 122 / s of 1000 Pa·s or more and 3000 Pa·s or less. 4. The polyphenylene sulfide resin composition according to any one of items 1 to 3, wherein the weight loss rate (%) when pellets of the resin composition are treated in air at 320° C. for 2 hours is 0.3% or more and 3.0% or less. 5. The polyphenylene sulfide resin composition according to any one of items 1 to 4, wherein the (D) organosilane compound is an alkoxysilane compound having an epoxy group or an isocyanate group. 6. Section 1~ 5 Item 14. A molded article made of the polyphenylene sulfide resin composition according to any one of items 1 to 3. 7. The molded product is a hollow molded product. 6 Item 2. A molded article according to item 1. 8. Section 1~ 5 Item 14. A method for producing a molded article, comprising blow molding the polyphenylene sulfide resin composition according to any one of items 1 to 3. Effect of the Invention
[0010] According to the present invention, a polyphenylene sulfide resin composition having excellent material strength, toughness, and heat aging resistance, as well as excellent blow moldability, can be obtained. The polyphenylene sulfide resin composition having these properties is suitable for molded products such as ducts around automobile engines and thin-walled piping used under high temperature and vibration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will now be described in further detail.
[0012] The (A) polyphenylene sulfide resin (hereinafter sometimes abbreviated as PPS resin) used in the present invention is a polymer having a repeating unit represented by the following structural formula.
[0013] [ka]
[0014] From the viewpoint of heat resistance, it is preferable for the polymer to contain 70 mol % or more, and more preferably 90 mol % or more, of the polymer containing the repeating unit represented by the above structural formula. In addition, about 30 mol % or less of the repeating units of the (A) PPS resin may be composed of repeating units having the following structure.
[0015] [ka]
[0016] Although there is no particular limitation on the melt viscosity of the PPS resin (A) used in the present invention, the higher the melt viscosity, the better in terms of obtaining better toughness. For example, the range of more than 30 Pa·s is preferable, 50 Pa·s or more is more preferable, and 100 Pa·s or more is even more preferable. The upper limit is preferably 600 Pa·s or less from the viewpoint of suppressing thermal degradation of the epoxy-containing olefin-based copolymer due to shear heating.
[0017] The melt viscosity in the present invention is a value measured using a Capillograph manufactured by Toyo Seiki Seisakusho Co., Ltd. under conditions of 310° C. and a shear rate of 1000 / s.
[0018] A method for producing the PPS resin (A) used in the present invention will be described below, but the method is not limited to the method described below as long as the PPS resin (A) having the above structure can be obtained.
[0019] First, the details of the dihaloaromatic compound, sulfidizing agent, polymerization solvent, molecular weight regulator, polymerization aid and polymerization stabilizer used in the production method will be described.
[0020] [Dihaloaromatic compounds] The dihaloaromatic compound refers to a compound having two or more halogen atoms in one molecule.Specific examples of the dihaloaromatic compound include p-dichlorobenzene, m-dichlorobenzene, o-dichlorobenzene, 1,3,5-trichlorobenzene, 1,2,4-trichlorobenzene, 1,2,4,5-tetrachlorobenzene, hexachlorobenzene, 2,5-dichlorotoluene, 2,5-dichloro-p-xylene, 1,4-dibromobenzene, 1,4-diiodobenzene, and 1-methoxy-2,5-dichlorobenzene, and preferably p-dichlorobenzene.
[0021] The amount of the dihaloaromatic compound added, in order to obtain a PPS resin (A) with a viscosity suitable for processing, can be, for example, in the range of 0.9 to 2.0 mol, preferably 0.95 to 1.5 mol, and more preferably 1.005 to 1.2 mol, per mol of the sulfidizing agent.
[0022] [Sulfidizing agent] The sulfidizing agent includes alkali metal sulfides, alkali metal hydrosulfides, and hydrogen sulfide.
[0023] Specific examples of alkali metal sulfides include lithium sulfide, sodium sulfide, potassium sulfide, rubidium sulfide, cesium sulfide, and mixtures of two or more of these, with sodium sulfide being preferred. These alkali metal sulfides can be used as hydrates or aqueous mixtures, or in the anhydrous form.
[0024] Specific examples of the alkali metal hydrosulfide include sodium hydrosulfide, potassium hydrosulfide, lithium hydrosulfide, rubidium hydrosulfide, cesium hydrosulfide, and mixtures of two or more of these, with sodium hydrosulfide being preferred. These alkali metal hydrosulfides can be used as hydrates or aqueous mixtures, or in the anhydrous form.
[0025] In addition, an alkali metal sulfide prepared in situ in the reaction system from an alkali metal hydrosulfide and an alkali metal hydroxide can also be used. Alternatively, an alkali metal sulfide can be prepared from an alkali metal hydrosulfide and an alkali metal hydroxide, and then transferred to a polymerization tank for use.
[0026] Alternatively, an alkali metal sulfide prepared in situ in the reaction system from an alkali metal hydroxide such as lithium hydroxide or sodium hydroxide and hydrogen sulfide can be used.Alkaline metal sulfides can be prepared from an alkali metal hydroxide such as lithium hydroxide or sodium hydroxide and hydrogen sulfide, and then transferred to a polymerization tank for use.
[0027] When a part of the sulfidizing agent is lost before the start of the polymerization reaction due to a dehydration operation or the like, the amount of the charged sulfidizing agent means the remaining amount obtained by subtracting the lost amount from the actual charged amount.
[0028] In addition, it is possible to use an alkali metal hydroxide and / or an alkaline earth metal hydroxide together with the sulfidizing agent. Specific examples of the alkali metal hydroxide include, for example, sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, cesium hydroxide, and mixtures of two or more of these. Specific examples of the alkaline earth metal hydroxide include, for example, calcium hydroxide, strontium hydroxide, barium hydroxide, etc., and among these, sodium hydroxide is preferably used.
[0029] When an alkali metal hydrosulfide is used as the sulfidizing agent, it is particularly preferable to use an alkali metal hydroxide simultaneously. The amount of the alkali metal hydroxide used is, for example, in the range of 0.95 to 1.20 mol, preferably 1.00 to 1.15 mol, and more preferably 1.005 to 1.100 mol per mol of the alkali metal hydrosulfide.
[0030] [Polymerization solvent] As the polymerization solvent, it is preferable to use an organic polar solvent. Specific examples include N-alkylpyrrolidones such as N-methyl-2-pyrrolidone and N-ethyl-2-pyrrolidone, caprolactams such as N-methyl-ε-caprolactam, aprotic organic solvents such as 1,3-dimethyl-2-imidazolidinone, N,N-dimethylacetamide, N,N-dimethylformamide, hexamethylphosphoric triamide, dimethylsulfone, and tetramethylene sulfoxide, and mixtures thereof, all of which are preferably used because of their high reaction stability. Among these, N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as NMP) is particularly preferably used.
[0031] The amount of the organic polar solvent used is selected from the range of 2.0 to 10 moles, preferably 2.25 to 6.0 moles, and more preferably 2.5 to 5.5 moles, per mole of the sulfidizing agent.
[0032] [Molecular weight regulator] A monohalogen compound (which does not necessarily have to be an aromatic compound) can be used in combination with the polyhalogenated aromatic compound in order to form reactive terminals in the resulting PPS resin (A) or to adjust the polymerization reaction or molecular weight.
[0033] [Polymerization aid] In order to obtain a PPS resin (A) with a relatively high degree of polymerization in a short time, it is also a preferred embodiment to use a polymerization aid. Here, the polymerization aid means a substance that has the effect of increasing the viscosity of the resulting PPS resin (A). Specific examples of such polymerization aids include organic carboxylates, water, alkali metal chlorides, organic sulfonates, alkali metal sulfates, alkaline earth metal oxides, alkali metal phosphates, and alkaline earth metal phosphates. These can be used alone or in combination of two or more. Among these, organic carboxylates, water, and alkali metal chlorides are preferred, and alkali metal carboxylates are more preferred as organic carboxylates, and lithium chloride is more preferred as alkali metal chlorides.
[0034] The above alkali metal carboxylate has the general formula R(COOM) n (wherein R is an alkyl group, a cycloalkyl group, an aryl group, an alkylaryl group, or an arylalkyl group having 1 to 20 carbon atoms; M is an alkali metal selected from lithium, sodium, potassium, rubidium, and cesium; and n is an integer of 1 to 3). The alkali metal carboxylate can also be used as a hydrate, anhydride, or an aqueous solution. Specific examples of the alkali metal carboxylate include lithium acetate, sodium acetate, potassium acetate, sodium propionate, lithium valerate, sodium benzoate, sodium phenylacetate, potassium p-toluate, and mixtures thereof.
[0035] The alkali metal carboxylate may be formed by adding and reacting an organic acid with one or more compounds selected from the group consisting of alkali metal hydroxides, alkali metal carbonates, and alkali metal bicarbonates in approximately equal chemical equivalents. Among the above alkali metal carboxylates, lithium salts have high solubility in the reaction system and have a large auxiliary effect, but are expensive, while potassium, rubidium, and cesium salts are considered to have insufficient solubility in the reaction system. Therefore, sodium acetate, which is inexpensive and has moderate solubility in the polymerization system, is most preferably used.
[0036] When these alkali metal carboxylates are used as polymerization aids, the amount used is usually in the range of 0.01 mol to 2 mol per mol of the charged alkali metal sulfide. In terms of obtaining a higher degree of polymerization, the amount used is preferably in the range of 0.1 mol to 0.6 mol, and more preferably in the range of 0.2 mol to 0.5 mol.
[0037] When water is used as a polymerization aid, the amount added is usually in the range of 0.3 mol to 15 mol per mol of the charged alkali metal sulfide, and in terms of obtaining a higher degree of polymerization, the range of 0.6 mol to 10 mol is preferable, and the range of 1 mol to 5 mol is more preferable.
[0038] Of course, two or more of these polymerization aids can be used in combination. For example, when an alkali metal carboxylate and water are used in combination, a higher molecular weight can be achieved with a smaller amount of each.
[0039] There is no particular designation for the timing of addition of these polymerization aids, and they may be added at any time during the pre-step, at the start of polymerization, or during the polymerization, as described below, or may be added in several portions, but when an alkali metal carboxylate is used as the polymerization aid, it is more preferable to add it at the start of the pre-step or at the start of polymerization, because it is easy to add it. When water is used as the polymerization aid, it is effective to add it during the polymerization reaction after the dihalo aromatic compound is charged.
[0040] [Polymerization stabilizer] A polymerization stabilizer can be used to stabilize the polymerization reaction system and suppress side reactions. The polymerization stabilizer contributes to the stabilization of the polymerization reaction system and suppresses undesirable side reactions. One of the indicators of side reactions is the generation of thiophenol, and the addition of a polymerization stabilizer can suppress the generation of thiophenol. Specific examples of polymerization stabilizers include compounds such as alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, and alkaline earth metal carbonates. Among them, alkali metal hydroxides such as sodium hydroxide, potassium hydroxide, and lithium hydroxide are preferred. The above-mentioned alkali metal carboxylates also act as polymerization stabilizers, and therefore are included in the polymerization stabilizers. In addition, when an alkali metal hydrosulfide is used as a sulfidizing agent, it is particularly preferable to use an alkali metal hydroxide at the same time, as mentioned above, but an excess of an alkali metal hydroxide relative to the sulfidizing agent can also serve as a polymerization stabilizer.
[0041] These polymerization stabilizers can be used alone or in combination of two or more. The polymerization stabilizer is preferably used in a ratio of usually 0.02 mol to 0.2 mol, preferably 0.03 mol to 0.1 mol, more preferably 0.04 mol to 0.09 mol, per mol of the charged alkali metal sulfide. If this ratio is too small, the stabilizing effect is insufficient, and conversely, if it is too large, there is an economic disadvantage and the polymer yield tends to decrease.
[0042] The timing of adding the polymerization stabilizer is not particularly specified, and it may be added at any time during the pre-step described below, at the start of polymerization, or during the polymerization, or may be added in several divided portions. However, it is more preferable to add it simultaneously at the start of the pre-step or at the start of polymerization from the viewpoint of ease.
[0043] Next, a preferred method for producing the PPS resin (A) used in the present invention will be specifically described in order, including a pre-process, a polymerization reaction process, a recovery process, and a post-treatment process, although the method is not limited to this method.
[0044] [Pre-process] In the production process for (A) PPS resin, the sulfidizing agent is usually used in the form of a hydrate. It is preferable to heat a mixture containing an organic polar solvent and a sulfidizing agent and remove excess water from the system before adding a dihalo aromatic compound.
[0045] As described above, the sulfidizing agent may be prepared in situ in the reaction system from an alkali metal hydrosulfide and an alkali metal hydroxide, or in a tank separate from the polymerization tank. There is no particular restriction on this method, but a preferable method is to add an alkali metal hydrosulfide and an alkali metal hydroxide to an organic polar solvent in an inert gas atmosphere at room temperature to 150°C, preferably room temperature to 100°C, and then heat the mixture to at least 150°C or higher, preferably 180 to 260°C, under normal pressure or reduced pressure, to distill off water. A polymerization aid may be added at this stage. Toluene or the like may be added to promote the distillation of water.
[0046] In the polymerization reaction, the amount of water in the polymerization system is preferably 0.3 to 10.0 mol per 1 mol of the charged sulfidizing agent. Here, the amount of water in the polymerization system is the amount of water charged to the polymerization system minus the amount of water removed from the polymerization system. The charged water may be in any form such as water, an aqueous solution, or crystal water.
[0047] [Polymerization reaction process] (A) PPS resin is produced by reacting a sulfidizing agent with a dihaloaromatic compound in an organic polar solvent at a temperature range of 200° C. or higher and lower than 290° C.
[0048] When starting the polymerization reaction process, the organic polar solvent, the sulfidizing agent, and the dihalo aromatic compound are mixed, desirably in an inert gas atmosphere, at a temperature range of room temperature to 240° C., preferably 100° C. to 230° C. A polymerization aid may be added at this stage. The order of charging these raw materials may be random, or they may be charged simultaneously.
[0049] The mixture is usually heated to a temperature in the range of 200° C. or higher and lower than 290° C. There are no particular limitations on the heating rate, but a rate of 0.01° C. / min to 5° C. / min is usually selected, and a range of 0.1° C. / min to 3° C. / min is more preferable.
[0050] In general, the temperature is finally raised to a temperature of 250° C. or higher and lower than 290° C., and the reaction is carried out at that temperature for usually 0.25 to 50 hours, preferably 0.5 to 20 hours.
[0051] In order to obtain a higher degree of polymerization, it is effective to react at 200° C. to 260° C. for a certain period of time before the final temperature is reached, and then to raise the temperature to 270° C. or more and less than 290° C. In this case, the reaction time at 200° C. to 260° C. is usually selected within the range of 0.25 hours to 20 hours, and preferably 0.25 hours to 10 hours.
[0052] In order to obtain a polymer with a higher degree of polymerization, it may be effective to carry out the polymerization in multiple stages. When carrying out the polymerization in multiple stages, it is effective that the conversion rate of the dihaloaromatic compound in the system at 245°C is 40 mol% or more, preferably 60 mol%.
[0053] The conversion rate of dihaloaromatic compounds (abbreviated as DHA here) is a value calculated by the following formula: The amount of remaining DHA can usually be determined by gas chromatography. (a) When the dihaloaromatic compound is added in excess of the alkali metal sulfide in terms of molar ratio Conversion rate = [DHA charge amount (mol) - DHA remaining amount (mol)] / [DHA charge amount (mol) - DHA excess amount (mol)] (b) Cases other than (a) above Conversion rate = [charged amount of DHA (mol) - remaining amount of DHA (mol)] / [charged amount of DHA (mol)].
[0054] [Recovery process] In the method for producing the (A) PPS resin, after the polymerization is completed, a solid matter is recovered from the polymerization reaction product containing the polymer, the solvent, etc. As the recovery method, any known method may be adopted.
[0055] For example, after the polymerization reaction is completed, the polymer particles may be collected by gradually cooling. The cooling speed is not particularly limited, but is usually about 0.1°C / min to 3°C / min. It is not necessary to cool at the same speed throughout the entire cooling process, and a method of gradually cooling at a speed of 0.1°C / min to 1°C / min until the polymer particles crystallize and precipitate, and then at a speed of 1°C / min or more may be used.
[0056] It is also preferred to carry out the above recovery under rapid cooling conditions, and a preferred recovery method is the flash method. In the flash method, the polymerization reaction product is subjected to high temperature and high pressure (usually 250°C or higher, 8 kg / cm 2 The method is to flash the polymer from the above state into an atmosphere of normal pressure or reduced pressure, recover the solvent, and recover the polymer in powder form at the same time. Flashing here means to eject the polymerization reaction product from a nozzle. Specific examples of the flashing atmosphere include nitrogen or water vapor at normal pressure, and the temperature is usually selected in the range of 150°C to 250°C.
[0057] [Post-processing process] The (A) PPS resin may be produced through the above-mentioned polymerization and recovery steps, and then may be subjected to an acid treatment, hot water treatment, washing with an organic solvent, or an alkali metal or alkaline earth metal treatment.
[0058] The acid treatment is carried out as follows: There are no particular limitations on the acid used in the acid treatment of the (A) PPS resin so long as it does not have the effect of decomposing the (A) PPS resin, and examples of the acid include acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, silicic acid, carbonic acid, and propylic acid, and among these, acetic acid and hydrochloric acid are more preferably used, but acids such as nitric acid that decompose and deteriorate the (A) PPS resin are undesirable.
[0059] The acid treatment may be carried out by immersing the PPS resin (A) in an acid or an aqueous solution of an acid, and may be carried out with appropriate stirring or heating, if necessary. For example, when acetic acid is used, a sufficient effect can be obtained by immersing the PPS resin powder in an aqueous solution of pH 4 heated to 80°C to 200°C and stirring for 30 minutes. The pH after the treatment may be 4 or higher, for example, about pH 4 to 8. The PPS resin (A) that has been subjected to the acid treatment is preferably washed several times with water or warm water to remove the remaining acid or salt. The water used for washing is preferably distilled water or deionized water, so as not to impair the effect of the preferable chemical modification of the PPS resin (A) by the acid treatment.
[0060] The hot water treatment is carried out as follows: When treating the (A) PPS resin with hot water, the temperature of the hot water is preferably 100° C. or higher, more preferably 120° C. or higher, still more preferably 150° C. or higher, and particularly preferably 170° C. or higher. If the temperature is less than 100° C., the desired chemical modification effect of the (A) PPS resin is small, which is not preferred.
[0061] In order to achieve the desired chemical modification effect of the (A) PPS resin by hot water washing, it is preferable that the water used is distilled water or deionized water. There are no particular limitations on the procedure for the hot water treatment, and it can be carried out by adding a specified amount of (A) PPS resin to a specified amount of water, heating and stirring in a pressure vessel, or by continuous hot water treatment. The ratio of (A) PPS resin to water is preferably higher, but a bath ratio of 200 g or less of (A) PPS resin to 1 liter of water is usually selected.
[0062] In addition, since decomposition of the terminal groups is undesirable, it is desirable to carry out the treatment in an inert atmosphere to avoid this. Furthermore, after this hot water treatment, the (A) PPS resin is preferably washed several times with warm water to remove any remaining components.
[0063] When washing with an organic solvent, the procedure is as follows. The organic solvent used for washing the (A) PPS resin is not particularly limited as long as it does not have the action of decomposing the (A) PPS resin, and examples thereof include nitrogen-containing polar solvents such as N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, 1,3-dimethylimidazolidinone, hexamethylphosphoramide, and piperazinones, sulfoxide-sulfone solvents such as dimethyl sulfoxide, dimethyl sulfone, and sulfolane, ketone solvents such as acetone, methyl ethyl ketone, diethyl ketone, and acetophenone, dimethyl ether, dipropyl ether, dioxane, tetrahydrofuran, and the like. Examples of the organic solvent include ether solvents such as hydrofuran, halogen-based solvents such as chloroform, methylene chloride, trichloroethylene, ethylene dichloride, perchloroethylene, monochloroethane, dichloroethane, tetrachloroethane, perchloroethane, and chlorobenzene, alcohol-phenol solvents such as methanol, ethanol, propanol, butanol, pentanol, ethylene glycol, propylene glycol, phenol, cresol, polyethylene glycol, and polypropylene glycol, and aromatic hydrocarbon solvents such as benzene, toluene, and xylene. Among these organic solvents, N-methyl-2-pyrrolidone, acetone, dimethylformamide, and chloroform are particularly preferred. These organic solvents are used alone or in combination of two or more.
[0064] The method of washing with an organic solvent includes immersing the PPS resin (A) in the organic solvent, and stirring or heating can be performed as necessary. There is no particular restriction on the washing temperature when washing the PPS resin (A) with an organic solvent, and any temperature between room temperature and about 300°C can be selected. The higher the washing temperature, the higher the washing efficiency tends to be, but usually a washing temperature between room temperature and 150°C is sufficient to obtain the desired effect. Washing can also be performed under pressure in a pressure vessel at a temperature above the boiling point of the organic solvent. There is also no particular restriction on the washing time. Although it depends on the washing conditions, in the case of batch washing, washing for 5 minutes or more usually obtains the desired effect. Continuous washing is also possible.
[0065] Examples of the method of alkali metal treatment or alkaline earth metal treatment include a method of adding an alkali metal salt or an alkaline earth metal salt before, during, or after the previous step, a method of adding an alkali metal salt or an alkaline earth metal salt into a polymerization vessel before, during, or after the polymerization step, or a method of adding an alkali metal salt or an alkaline earth metal salt at the beginning, middle, or end of the washing step. The easiest method among them is a method of adding an alkali metal salt or an alkaline earth metal salt after removing residual oligomers and residual salts by washing with an organic solvent or washing with warm or hot water. The alkali metal or alkaline earth metal is preferably introduced into the PPS resin in the form of an alkali metal ion or an alkaline earth metal ion such as an acetate, hydroxide, or carbonate. It is also preferable to remove excess alkali metal salt or alkaline earth metal salt by washing with warm water or the like. The alkali metal ion concentration and alkaline earth metal ion concentration when introducing the above alkali metal and alkaline earth metal are preferably 0.001 mmol or more per 1 g of PPS, and more preferably 0.01 mmol or more. The temperature is preferably 50° C. or more, more preferably 75° C. or more, and particularly preferably 90° C. or more. There is no particular upper limit to the temperature, but from the viewpoint of operability, 280° C. or less is usually preferred. The bath ratio (weight of cleaning solution relative to the weight of dry PPS) is preferably 0.5 or more, more preferably 3 or more, and even more preferably 5 or more.
[0066] In the present invention, from the viewpoint of obtaining a polyphenylene sulfide resin composition excellent in toughness, a method in which residual oligomers and residual salts are removed by repeatedly washing with an organic solvent and with warm water of about 80° C. or the above-mentioned hot water several times, and then the method in which the resin is treated with an acid or an alkali metal salt or an alkaline earth metal salt is treated is preferred, and in particular a method in which the resin is treated with an alkali metal salt or an alkaline earth metal salt is more preferred.
[0067] In addition, the (A) PPS resin can also be used after being subjected to a thermal oxidative crosslinking treatment in which, after completion of polymerization, it is heated in an oxygen atmosphere or heated with the addition of a crosslinking agent such as a peroxide to increase the molecular weight.
[0068] When dry heat treatment is performed for the purpose of increasing the molecular weight by thermal oxidation crosslinking, the temperature is preferably 160°C to 260°C, more preferably 170°C to 250°C. The oxygen concentration is desirably 5% by volume or more, more desirably 8% by volume or more. There is no particular upper limit to the oxygen concentration, but the limit is about 50% by volume. The treatment time is preferably 0.5 hours to 100 hours, more preferably 1 hour to 50 hours, and even more preferably 2 hours to 25 hours. The heat treatment device may be a normal hot air dryer or a rotary type or a heating device with stirring blades, but in order to treat efficiently and more uniformly, it is more preferable to use a rotary type or a heating device with stirring blades.
[0069] Dry heat treatment can also be performed to suppress thermal oxidative crosslinking and remove volatiles. The temperature is preferably 130°C to 250°C, more preferably 160°C to 250°C. In this case, the oxygen concentration is preferably less than 5% by volume, and even more preferably less than 2% by volume. The treatment time is preferably 0.5 hours to 50 hours, more preferably 1 hour to 20 hours, and even more preferably 1 hour to 10 hours. The heat treatment device may be a normal hot air dryer or a rotary or stirring blade-equipped heating device, but in the case of efficient and more uniform treatment, it is more preferable to use a rotary or stirring blade-equipped heating device.
[0070] However, from the viewpoint of exhibiting excellent toughness, the (A) PPS resin of the present invention is preferably a substantially linear PPS resin that has not been subjected to high molecular weight by thermal oxidation crosslinking treatment, or a semi-crosslinked PPS resin that has been lightly oxidative crosslinked. On the other hand, a PPS resin that has been subjected to thermal oxidation crosslinking treatment is preferable from the viewpoint of suppressing creep strain to a small value, and it is possible to use the resin by mixing it with a linear PPS resin as appropriate. In addition, in the present invention, a plurality of (A) PPS resins having different melt viscosities may be used by mixing them.
[0071] Examples of the reinforcing fibers (B) used in the present invention include glass fibers, carbon fibers, carbon nanotubes, carbon nanohorns, potassium titanate whiskers, zinc oxide whiskers, calcium carbonate whiskers, wollastonite whiskers, aluminum borate whiskers, aramid fibers, alumina fibers, silicon carbide fibers, ceramic fibers, asbestos fibers, gypsum fibers, and metal fibers. Glass fibers are preferred in terms of the balance between the effect of improving the mechanical strength of the resin composition and cost.
[0072] It is also preferable to pre-treat the surfaces of the (B) reinforcing fibers with a coupling agent such as an isocyanate compound, an organosilane compound, an organotitanate compound, an organoborane compound, or an epoxy compound, from the viewpoints of improving the bundling ability of the (B) reinforcing fibers, their dispersibility during resin blending, and the adhesion between the glass fibers and the resin.
[0073] The shape of the (B) reinforcing fiber cannot be generally defined because it varies depending on the type of fiber used, but the fiber diameter is preferably 1 to 50 μm, more preferably 3 to 30 μm, and even more preferably 5 to 20 μm. The length is preferably 30 μm to 10 mm, and more preferably 50 μm to 5 mm. By setting the fiber cross-sectional diameter and fiber length within the above ranges, the mechanical strength of the resin composition can be improved, which is preferable.
[0074] From the viewpoint of obtaining a strength improving effect, the blending amount of the (B) reinforcing fiber must be in the range of 1 to 200 parts by weight relative to 100 parts by weight of the (A) polyphenylene sulfide resin, and is preferably 10 parts by weight or more, more preferably 30 parts by weight or more, and particularly preferably 50 parts by weight or more. The upper limit of the blending amount is preferably 150 parts by weight or less, more preferably 120 parts by weight or less. If the blending amount of the (B) reinforcing fiber is less than 1 part by weight, excellent mechanical strength cannot be obtained, and if it exceeds 200 parts by weight, the melt viscosity increases significantly, which leads to a decrease in moldability and toughness, which is not preferable.
[0075] The epoxy group-containing olefin copolymer (C) used in the present invention includes olefin copolymers having glycidyl esters, glycidyl ethers, glycidyl diamines, etc. in the side chains, and olefin copolymers having double bonds in which the double bond portions are epoxy-oxidized. Among these, olefin copolymers in which a monomer having an epoxy group is copolymerized are preferred, and in particular, olefin copolymers whose main components are an α-olefin and a glycidyl ester of an α,β-unsaturated acid are preferably used.
[0076] Specific examples of such α-olefins include ethylene, propylene, butene-1, 4-methylpentene-1, hexene-1, decene-1, octene-1, etc., of which ethylene is preferred, and two or more of these can be used simultaneously.
[0077] On the other hand, the glycidyl ester of an α,β-unsaturated acid is represented by the general formula
[0078] [ka]
[0079] (wherein R represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms), and specific examples thereof include glycidyl acrylate, glycidyl methacrylate, and glycidyl ethacrylate, with glycidyl methacrylate being preferred.
[0080] Such an olefin-based copolymer having as its main components an α-olefin and a glycidyl ester of an α,β-unsaturated acid may be any of a random, block, and graft copolymers of the above-mentioned α-olefin and the glycidyl ester of an α,β-unsaturated acid.
[0081] The copolymerization amount of the glycidyl ester of α,β-unsaturated acid in the olefin-based copolymer mainly composed of α-olefin and glycidyl ester of α,β-unsaturated acid is preferably 0.5 to 40% by weight from the viewpoint of the effect on the target effect, polymerizability, gelation, heat resistance, fluidity, strength, etc. The lower limit is preferably 1.0% by weight or more from the viewpoint of obtaining sufficient melt viscosity and toughness improvement effect, more preferably 3.0% by weight or more, and particularly preferably 5.0% by weight or more. The upper limit is preferably 20% by weight or less from the viewpoint of suppressing excessive reaction and the associated shear heat generation, more preferably 15% by weight or less, and particularly preferably 10% by weight or less.
[0082] In the present invention, as the olefin copolymer containing an epoxy group, an olefin copolymer containing an epoxy group, which contains, as an essential component, in addition to an α-olefin (1) and a glycidyl ester of an α,β-unsaturated acid (2), a monomer (3) represented by the following general formula, is also preferably used.
[0083] [ka]
[0084] (where R 1 represents hydrogen or an alkyl group having 1 to 5 carbon atoms, and X represents -COOR 2 a group selected from the group consisting of a -CN group, an aromatic group, and R 2 represents an alkyl group having 1 to 10 carbon atoms.
[0085] The details of the α-olefin (1) and the glycidyl ester of α,β-unsaturated acid (2) used in such an olefin copolymer are the same as those in the above-mentioned (C) olefin copolymer containing an epoxy group.
[0086] On the other hand, specific examples of the monomer (3) include α,β-unsaturated carboxylic acid alkyl esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, t-butyl acrylate, isobutyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, t-butyl methacrylate, and isobutyl methacrylate, acrylonitrile, styrene, α-methylstyrene, styrene in which the aromatic ring is substituted with an alkyl group, and acrylonitrile-styrene copolymers, and two or more of these can be used simultaneously.
[0087] Such an olefin copolymer containing an epoxy group may be any of the copolymerization modes, such as a random copolymer, block copolymer, or graft copolymer of an α-olefin (1), a glycidyl ester of an α,β-unsaturated acid (2), and a monomer (3), or a copolymer obtained by copolymerizing these copolymers. It may also be a copolymer in which two or more copolymerization modes are combined, such as a random copolymer of an α-olefin (1) and a glycidyl ester of an α,β-unsaturated acid (2) that is graft copolymerized with a monomer (3).
[0088] The copolymerization ratio of the olefin copolymer containing an epoxy group is preferably selected in the range of α-olefin (1) / glycidyl ester of α,β-unsaturated acid (2)=60% by weight to 99% by weight / 40% by weight to 1% by weight from the viewpoint of the effect on the intended effect, the polymerizability, gelation, heat resistance, fluidity, and strength. The copolymerization ratio of the monomer (3) is preferably selected in the range of 5% by weight to 60% by weight of the monomer (3) relative to the total amount of α-olefin (1) and glycidyl ester of α,β-unsaturated acid (2) of 95% by weight to 40% by weight. It is also possible to adjust the melt viscosity and toughness of the polyphenylene sulfide resin composition by using these olefin copolymers containing an epoxy group with different copolymerization ratios in combination.
[0089] The blending amount of the epoxy group-containing olefin copolymer (C) depends on the copolymerization amount of the glycidyl ester of α,β-unsaturated acid in the olefin copolymer mainly composed of α-olefin and glycidyl ester of α,β-unsaturated acid, so it cannot be generally specified. However, from the viewpoint of obtaining excellent toughness and melt viscosity suitable for blow molding, the blending amount is required to be in the range of 1 to 200 parts by weight relative to 100 parts by weight of the polyphenylene sulfide resin (A), preferably 5 parts by weight or more, and more preferably 10 parts by weight or more. The upper limit of the blending amount is preferably 150 parts by weight or less, more preferably 100 parts by weight or less, and particularly preferably 70 parts by weight or less. If the epoxy group-containing olefin copolymer (C) is less than 1 part by weight, excellent toughness and blow moldability cannot be obtained, and if it exceeds 200 parts by weight, the melt viscosity increases significantly, which leads to gel formation and a decrease in toughness, which is not preferable.
[0090] In the present invention, excellent toughness can be obtained by using an unmodified olefin copolymer together with the above-mentioned (C) olefin copolymer containing an epoxy group.
[0091] Specific examples of unmodified olefin copolymers include ethylene-propylene copolymers, ethylene-butene copolymers, ethylene-hexene copolymers, ethylene-octene copolymers, polybutene, ethylene-propylene-diene copolymers, styrene-butadiene copolymers, polybutadiene, butadiene-acrylonitrile copolymers, polyisoprene, butene-isoprene copolymers, and SBS, SIS, SEBS, SEPS, etc. Among these, from the viewpoint of compatibility with the olefin copolymer containing the epoxy group (C), ethylene-propylene copolymers, ethylene-butene copolymers, ethylene-hexene copolymers, ethylene-octene copolymers, and ethylene-propylene-diene copolymers are particularly preferred.
[0092] The amount of the unmodified olefin copolymer is preferably in the range of 1 to 200 parts by weight of the total of the epoxy group-containing olefin copolymer (C) and the unmodified olefin copolymer per 100 parts by weight of the polyphenylene sulfide resin (A). The lower limit of the amount is preferably 5 parts by weight or more, more preferably 10 parts by weight or more. The upper limit of the amount is preferably 150 parts by weight or less, more preferably 100 parts by weight or less, and particularly preferably 70 parts by weight or less, of the total of the epoxy group-containing olefin copolymer (C) and the unmodified olefin copolymer. By making the total of the epoxy group-containing olefin copolymer (C) and the unmodified olefin copolymer 1 part by weight or more, toughness and blow moldability can be obtained, and when it is 200 parts by weight or less, the coarse dispersion of the unmodified olefin copolymer is suppressed, and toughness can be maintained.
[0093] When the total of (A) polyphenylene sulfide resin, (B) reinforcing fiber, and (C) olefin-based copolymer containing epoxy groups is taken as 100% by weight, the blending amount of (B) reinforcing fiber is preferably 15% by weight or more from the viewpoint of obtaining sufficient mechanical strength, more preferably 20% by weight or more from the viewpoint of obtaining practical strength in a thin-walled molded product, particularly preferably 25% by weight or more from the viewpoint of increasing the rigidity of the parison to suppress drawdown and obtain uniformity in thickness, and particularly preferably 30% by weight or more. By making it 15% by weight or more, sufficient mechanical strength can be obtained. In addition, the upper limit is preferably 70% by weight or less, more preferably 60% by weight or less, and particularly preferably 50% by weight or less from the viewpoint of obtaining an excellent appearance of the molded product, and most preferably 40% by weight or less. By making it 70% by weight or less, shear heat generation due to an increase in melt viscosity caused by the significant entanglement of (B) reinforcing fiber can be suppressed, and thermal decomposition of the polymer can be suppressed.
[0094] In the polyphenylene sulfide resin composition of the present invention, it is essential to add an organic silane compound (D) from the viewpoint of obtaining excellent toughness and excellent blow moldability by adjusting the melt viscosity. The above effect is the same as that of the olefin copolymer containing an epoxy group (C), but it is advantageous in that it does not cause a decrease in mechanical strength. The organic silane compound (D) preferably has at least one functional group selected from an epoxy group, an isocyanate group, an amino group, a hydroxyl group, a mercapto group, a ureido group, and an alkoxy group. Among them, an alkoxysilane compound having an epoxy group or an isocyanate group is preferred from the viewpoint of reactivity with the polyphenylene sulfide resin (A), the reinforcing fiber (B), and the olefin copolymer containing an epoxy group (C).Specific examples include isocyanate-modified silicone, epoxy-modified silicone, amino-modified silicone, carbinol-modified silicone, carboxyl-modified silicone, mercapto-modified silicone, ureido-modified silicone, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropylmethyl Preferred examples of the silane include diethoxysilane, N-phenylaminomethyltrimethoxysilane, N-phenylaminopropyltrimethoxysilane, dimethoxymethyl-3-piperazinopropylsilane, 3-piperazinopropyltrimethoxysilane, 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, 3-isocyanatepropylmethyldimethoxysilane, 3-isocyanatepropylmethyldiethoxysilane, 3-isocyanatepropylethyldimethoxysilane, 3-hydroxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptomethyldimethoxysilane, γ-ureidopropyltrimethoxysilane, etc. Among them, from the viewpoint of reactivity and handling, 3-isocyanatepropyltriethoxysilane, 3-aminopropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane are preferred. The organosilane compounds (D) can be used alone or in the form of a mixture of two or more kinds.
[0095] The blending amount of the (D) organosilane compound must be 0.01 to 10 parts by weight, preferably 0.1 to 5 parts by weight, and more preferably 0.3 to 3 parts by weight, based on 100 parts by weight of the (A) polyphenylene sulfide resin. If the blending amount of the (D) organosilane compound exceeds 10 parts by weight, the melt viscosity increases significantly, which is undesirable since it leads to the formation of a gelled product and a decrease in toughness, and if it is less than 0.01 part by weight, sufficient blow moldability is not obtained, which is undesirable.
[0096] In the polyphenylene sulfide resin composition of the present invention, it is essential to incorporate (E) a phosphorus oxoacid metal salt from the viewpoints of suppressing thermal degradation of (C) the olefin-based copolymer containing epoxy groups, suppressing gas generation during molding, and obtaining excellent mechanical strength, toughness, and heat aging resistance.
[0097] The (E) phosphorus oxoacid metal salt can suppress the thermal oxidation of the (C) epoxy group-containing olefin copolymer by a known reducing action. In addition, the present inventors have newly discovered that the (E) phosphorus oxoacid metal salt suppresses the shear heat generation during melt kneading in a resin composition consisting of (A) polyphenylene sulfide resin, (B) reinforcing fiber, (C) epoxy group-containing olefin copolymer, and (D) organosilane compound while maintaining the same melt viscosity. This action makes it possible to suppress the shear heat generation and the thermal deterioration of the (C) epoxy group-containing olefin copolymer even if the amount of the (B) reinforcing fiber is increased while maintaining a high melt viscosity that allows blow molding, and can suppress gas generation during molding, as well as obtain a polyphenylene sulfide resin composition having excellent mechanical strength, toughness, and especially heat aging resistance. The mechanism by which this action occurs is unclear, but it is presumed to control the reactivity of the (B) reinforcing fiber.
[0098] The (E) phosphorus oxoacid metal salt is preferably a metal salt of an acid selected from phosphorous acid, phosphoric acid, phosphinic acid, phosphonic acid, diphosphoric acid, and triphosphoric acid, and more preferably a metal salt of phosphinic acid.Specific examples include potassium phosphinate, sodium phosphinate, calcium phosphinate, aluminum phosphinate, aluminum diethylphosphinate, zinc phosphinate, and magnesium phosphinate.Among these, from the viewpoints of phosphorus concentration and handling, a metal salt of phosphinic acid is preferred, and sodium phosphinate is more preferred.
[0099] These (E) phosphorus oxoacid metal salts can be used alone or in the form of a mixture of two or more kinds.
[0100] The blending amount of the (E) phosphorus oxoacid metal salt must be 0.01 to 5 parts by weight per 100 parts by weight of the (A) polyphenylene sulfide resin, and is preferably 0.05 parts by weight or more, and more preferably 0.1 parts by weight or more. The upper limit of the blending amount is preferably 3 parts by weight or less, and more preferably 1 part by weight or less. If the blending amount of the (E) phosphorus oxoacid metal salt exceeds 5 parts by weight, it may cause a large amount of gas generation, and if it is less than 0.01 part by weight, a sufficient shear heat generation suppression effect cannot be obtained.
[0101] In the present invention, additives, other thermoplastic resins, fillers, etc. may be blended as necessary within the limits that do not impair the properties.
[0102] Additives that can be blended include phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, plasticizers such as organophosphorus compounds, crystal nucleating agents such as organophosphorus compounds, polyether ether ketone, montanic acid waxes, metal soaps such as lithium stearate and aluminum stearate, release agents such as ethylenediamine-stearic acid-sebacic acid polycondensates and silicone compounds, as well as other conventional additives such as water, lubricants, UV inhibitors, colorants, and foaming agents.
[0103] The amount of the additive added is preferably 0.1 to 10 parts by weight, and more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the polyphenylene sulfide resin (A).
[0104] Other thermoplastic resins include polyketone resins, polyarylate resins, liquid crystal polymers, polyether ketone resins, polythioether ketone resins, polyether ether ketone resins, polyether sulfone resins, polyethylene tetrafluoride resins, and ethylene tetrafluoroethylene copolymers.
[0105] In addition, as the filler, fullerene, talc, wollastonite, zeolite, sericite, mica, kaolin, clay, pyrophyllite, silica, bentonite, asbestos, silicate such as alumina silicate, metal compounds such as silicon oxide, magnesium oxide, alumina, zirconium oxide, titanium oxide, iron oxide, carbonates such as calcium carbonate, magnesium carbonate, dolomite, sulfates such as calcium sulfate, barium sulfate, hydroxides such as calcium hydroxide, magnesium hydroxide, aluminum hydroxide, glass beads, glass flakes, glass powder, ceramic beads, boron nitride, silicon carbide, carbon black, and non-fibrous fillers such as silica and graphite are used, and these inorganic fillers may be hollow, and two or more types may be used in combination. In addition, these inorganic fillers may be pretreated with a coupling agent such as an isocyanate compound, an organic silane compound, an organic titanate compound, an organic borane compound, and an epoxy compound before use. Among these, calcium carbonate, silica and carbon black are preferred from the viewpoints of corrosion prevention, lubricant and electrical conductivity.
[0106] The amount of any of the above other components added is undesirable if it exceeds 20% by weight of the entire composition since the inherent properties are impaired, and it is advisable to add no more than 10% by weight, preferably no more than 5% by weight.
[0107] The melt viscosity of the polyphenylene sulfide resin composition of the present invention is preferably 1000 Pa·s or more, more preferably 1300 Pa·s or more, from the viewpoint of suppressing drawdown during blow molding. Also, from the viewpoint of obtaining a uniform wall thickness of the blow molded product, it is particularly preferable that it is 1500 Pa·s or more. The upper limit is preferably 3000 Pa·s or less, more preferably 2500 Pa·s or less, from the viewpoint of maintaining melt fluidity. By setting the melt viscosity to 1000 Pa·s or more, molding defects such as the occurrence of drawdown and loss of uniformity in wall thickness can be suppressed.
[0108] The melt viscosity of the polyphenylene sulfide resin composition of the present invention can be increased, for example, by selecting a high-viscosity polyphenylene sulfide resin (A) or by increasing the blending amounts of (B) reinforcing fiber, (C) olefin copolymer containing an epoxy group, and (D) organic silane compound. The melt viscosity of the resin composition of the present invention is a value measured using a Capillograph manufactured by Toyo Seiki Seisakusho Co., Ltd. under conditions of 300°C and a shear rate of 122 / s.
[0109] The weight loss rate of the polyphenylene sulfide resin composition of the present invention is preferably 3.0% by weight or less, more preferably 2.5% by weight or less, from the viewpoint of suppressing void inclusion in the molded product, and particularly preferably 2.0% by weight or less, most preferably 1.5% by weight or less, from the viewpoint of suppressing the decrease in strength of a thin-walled molded product due to void inclusion. The weight loss rate of the resin composition in the present invention is the ratio of the weight change before and after drying treatment to the weight before drying treatment when pellets of the resin composition are treated in air at 320°C for 2 hours. In other words, the weight loss rate is also an index representing the amount of gas generated from the resin composition. The method of making the weight loss rate of the polyphenylene sulfide resin composition 3.0% by weight or less is not particularly limited as long as such a resin composition can be obtained, but for example, a method of suppressing the shear heat generation during melt-kneading of the polyphenylene sulfide resin composition to lower the resin temperature, and a method of suppressing the thermal degradation of the olefin copolymer containing an epoxy group (C) by adding an antioxidant can be mentioned.
[0110] The polyphenylene sulfide resin composition of the present invention must have a bending strength of 100 MPa or more and 300 MPa or less, measured according to ISO178 on an ISO dumbbell test piece (1A) obtained by injection molding. From the viewpoint of obtaining practical strength in a thinner molded product, it is preferably 150 MPa or more, more preferably 200 MPa or more. If the bending strength exceeds 300 MPa, it becomes difficult to achieve compatibility with blow moldability, which is not preferable. The bending strength of the polyphenylene sulfide resin composition can be increased by increasing the blending amount of (B) reinforcing fiber. Furthermore, from the viewpoint of obtaining durability in a high-temperature environment, it is preferable that the ISO dumbbell test piece (1A) has a bending strength of 100 MPa or more and 300 MPa or less after being treated at 180°C for 500 hours. In order to suppress the decrease in bending strength after heat treatment at 180°C for 500 hours, for example, it is preferable to suppress the shear heat generation during melt kneading of the polyphenylene sulfide resin composition to lower the resin temperature, and to add an antioxidant to suppress the thermal deterioration of the epoxy group-containing olefin copolymer (C). Furthermore, from the viewpoint of obtaining durability in an environment where the composition is in contact with a coolant mainly composed of ethylene glycol used to cool automobile engines and motors, it is preferable that the ISO dumbbell test piece (1A) has a bending strength of 100 MPa or more and 300 MPa or less after being treated for 500 hours at 150°C in a liquid obtained by mixing LLC (Toyota Super Long Life Coolant (product number 08889-01005) manufactured by Toyota Motor Corporation) and ion-exchanged water at a weight ratio of 1:1. In order to suppress the decrease in bending strength after heat treatment at 150°C for 500 hours in LLC, for example, it is preferable to make the chemical bond formed between the polyphenylene sulfide resin (A) and the reinforcing fiber (B) a bond with higher hydrolysis resistance.
[0111] The polyphenylene sulfide resin composition of the present invention preferably has a tensile elongation at break of 3.0% or more and 20.0% or less, as measured according to ISO527-1 and -2 on an ISO dumbbell test piece (1A) obtained by injection molding. From the viewpoint of obtaining practical toughness in a thinner molded product, the tensile elongation at break is preferably 3.5% or more, more preferably 4.0% or more, and particularly preferably 4.5% or more. The tensile elongation at break of the polyphenylene sulfide resin composition can be increased by increasing the blending amount of (C) an olefin copolymer containing an epoxy group or (D) an organic silane compound. Furthermore, from the viewpoint of obtaining durability in a high-temperature environment, it is preferable that the ISO dumbbell test piece (1A) has a tensile elongation at break of 3.0% or more and 20.0% or less after being treated at 180°C for 500 hours. In order to suppress the decrease in the tensile elongation at break after heat treatment at 180°C for 500 hours, for example, it is preferable to suppress the shear heat generation during melt-kneading of the polyphenylene sulfide resin composition to lower the resin temperature, and to add an antioxidant to suppress the thermal deterioration of the epoxy group-containing olefin copolymer (C). Furthermore, from the viewpoint of obtaining durability in an environment where the composition comes into contact with a coolant mainly composed of ethylene glycol used to cool automobile engines and motors, it is preferable that the ISO (1A) dumbbell test piece has a tensile elongation of 3.0% or more and 20.0% or less after being treated at 150°C for 500 hours in a mixture of LLC (Toyota Super Long Life Coolant (product number 08889-01005) manufactured by Toyota Motor Corporation) and ion-exchanged water in a weight ratio of 1:1. In order to suppress a decrease in the tensile elongation at break after heat treatment in LLC at 150°C for 500 hours, it is preferable that the chemical bond formed between the (A) polyphenylene sulfide resin and the (B) reinforcing fibers be a bond with higher hydrolysis resistance, for example.
[0112] The method for producing the polyphenylene sulfide resin composition of the present invention is not particularly limited, and a representative example thereof includes a method in which raw materials are supplied to a commonly known melt kneader such as a single-screw or twin-screw extruder, a Banbury mixer, a kneader, or a mixing roll, and melt kneaded so that the resin temperature is the melting peak temperature of the polyphenylene sulfide resin (A) +5°C to 100°C. Among these, melt kneading using a twin-screw extruder is preferred.
[0113] The ratio (L / D) of the screw length L (mm) to the screw diameter D (mm) of the twin-screw extruder is desirably 10 or more, more preferably 20 or more, and even more preferably 30 or more. The upper limit of L / D of the twin-screw extruder is usually 60. If L / D is less than 10, kneading tends to be insufficient, making it difficult to obtain sufficient melt viscosity and toughness.
[0114] In this case, the order of mixing the raw materials is not particularly limited, and any method may be used, such as a method of mixing all the raw materials and then melt-kneading them by the above method, a method of mixing some of the raw materials and then melt-kneading them by the above method, and then further mixing and melt-kneading the remaining raw materials, or a method of mixing some of the raw materials and then using a side feeder to mix the remaining raw materials halfway through melt-kneading them with an extruder. From the viewpoint of obtaining sufficient material strength, it is preferable to mix the (B) reinforcing fiber using a side feeder.
[0115] It is also preferable to suppress gelation of the extrusion gut due to overreaction of (A) polyphenylene sulfide resin, (B) reinforcing fiber, (C) olefin copolymer containing epoxy groups, and (D) organic silane compound, and the associated decrease in toughness. To achieve this, it is preferable to use a stirring screw with a notch. Here, the "notch" refers to a part of the screw flight that is cut off. A stirring screw with a notch can increase the resin filling rate. When the molten resin passes through the kneading section to which the stirring screw is connected, it is easily affected by the extruder cylinder temperature. By using a stirring screw with a notch, the molten resin that is heated by shear during kneading is efficiently cooled, making it possible to lower the resin temperature during kneading. In addition, a stirring screw with a notch can perform kneading mainly by stirring and stirring, unlike the conventional method of grinding the resin, and therefore it is possible to further suppress thermal deterioration of the resin due to heat generation.
[0116] From the viewpoint of improving the cooling efficiency of the molten resin by filling with resin and improving the kneading property, the stirring screw having the notches is preferably a stirring screw having a screw pitch length in the range of 0.1D to 0.3D, where D (mm) is the screw diameter, and having 10 to 15 notches per pitch. Here, the "screw pitch length" refers to the screw length between the screw crests when the screw rotates 360 degrees.
[0117] For stirring screws having notches, the notches are preferably introduced so as to occupy 3% or more of the total length L (mm) of the screw, more preferably 5% or more, with the upper limit being preferably 20% or less, and more preferably 15% or less.
[0118] The cylinder temperature of the extruder depends on the melting point of the (A) polyphenylene sulfide resin used and cannot be generally determined, but a preferable range is, for example, 280° C. or more and 320° C. or less.
[0119] From the viewpoint of suppressing thermal degradation of the (C) epoxy group-containing olefin copolymer, the resin temperature during melt kneading is preferably 350° C. or less, more preferably 340° C. or less, and particularly preferably 330° C. or less. The resin temperature during melt kneading in the present invention is a temperature measured by a thermometer provided on the die head of the extruder.
[0120] The polyphenylene sulfide resin composition of the present invention can be applied to various molding methods, such as extrusion molding, injection molding, hollow molding, calendar molding, compression molding, vacuum molding, foam molding, blow molding, and rotational molding. In particular, the polyphenylene sulfide resin composition of the present invention is useful for blow molding applications because it can suppress drawdown during molding and obtain molded products with little thickness deviation. Examples of blow molding include extrusion blow molding and injection blow molding, and examples of blow molding include multi-layer blow such as direct blow and exchange blow, multi-dimensional blow such as suction blow, injection blow, and injection stretch blow. In addition, air can be used as the air used to blow up the parison during blow molding, and in terms of suppressing thermal oxidation deterioration, it is preferable to use an inert gas such as nitrogen or helium, and nitrogen is particularly preferable in terms of cost.
[0121] Applications of molded products obtained by extrusion molding or blow molding include round bars, square bars, sheets, films, tubes, pipes, etc., and more specific applications include electrical insulating materials for water heater motors, air conditioner motors, drive motors, etc., film capacitors, speaker diaphragms, recording magnetic tapes, printed circuit board materials, printed circuit board peripheral parts, semiconductor packages, semiconductor carrier trays, process / release films, protective films, automotive film sensors, insulating tapes for wire cables, insulating washers in lithium ion batteries, tubes for hot water, cooling water, and chemicals, automotive fuel tubes, hot water piping, chemical piping in chemical plants, etc., piping for ultrapure water and ultrahigh purity solvents, automotive piping, automotive cooling piping, piping pipes for freon and supercritical carbon dioxide refrigerants, and workpiece retaining rings for polishing equipment. Other examples include coated molded articles for windings of motor coils in hybrid cars, electric cars, railways, and power generation facilities, wire harnesses and control wires such as heat-resistant electric cables for home appliances and flat cables used for wiring inside cars, and coated molded articles for windings of signal transformers or on-board transformers for communication, transmission, high frequency, audio, measurement, etc. Among these, the polyphenylene sulfide resin composition of the present invention is useful as various pipes and ducts for fuel-related, exhaust, intake, and cooling systems of automobiles exposed to high-temperature environments, such as hybrid cars, electric cars, and automobiles equipped with turbo mechanisms, taking advantage of its excellent characteristics of heat aging resistance and chemical resistance.
[0122] In addition, the polyphenylene sulfide resin composition of the present invention can be used to design molded articles that are thin while maintaining their strength, taking advantage of its characteristics of high strength, high toughness, and excellent heat aging resistance, and can be used to reduce the weight and diameter of molded articles.
[0123] Applications of molded products obtained by injection molding include generators, electric motors, transformers, current transformers, voltage regulators, rectifiers, inverters, relays, power contacts, switches, circuit breakers, knife switches, multi-pole rods, electrical component cabinets and other electrical equipment parts, sensors, LED lamps, connectors, sockets, resistors, relay cases, small switches, coil bobbins, capacitors, variable capacitor cases, optical pickups, oscillators, various terminal boards, transformers, plugs, printed circuit boards, tuners, speakers, microphones, headphones, small motors, magnetic head bases, power modules, semiconductors, liquid crystal displays, FDD carriages, FDD chassis, and motor brush holders. electronic components such as parabolic antennas, and computer-related components; home and office electrical appliances such as VTR parts, television parts, irons, hair dryers, rice cooker parts, microwave oven parts, audio parts, audio equipment parts such as laser discs (registered trademark) and compact discs, lighting parts, refrigerator parts, air conditioner parts, typewriter parts, word processor parts, and other components; office computer-related parts, telephone-related parts, facsimile-related parts, copier-related parts, cleaning tools, motor parts, lighters, typewriters, and other machinery-related parts; microscopes, binoculars, cameras, watches, and other optical and precision machinery-related parts;Alternator terminals, alternator connectors, IC regulators, potentiometer bases for light dimmers, various valves such as exhaust gas valves, automotive cooling piping, various pipes and ducts for fuel, exhaust systems and intake systems, turbo ducts, air intake nozzle snorkels, intake manifolds, fuel pumps, engine coolant joints, carburetor main bodies, carburetor spacers, exhaust gas sensors, coolant sensors, oil temperature sensors, brake pad wear sensors, throttle position sensors, crankshaft position sensors, air flow meters, brake pad wear sensors, thermostat bases for air conditioners, heating hot air flow control valves, radiator motors Examples of the materials used include brush holders for motors, water pump impellers, turbine vanes, wiper motor-related parts, distributors, starter switches, starter relays, transmission wire harnesses, windshield washer nozzles, air conditioner panel switch boards, coils for fuel-related electromagnetic valves, fuse connectors, horn terminals, electrical component insulating plates, step motor rotors, lamp sockets, lamp reflectors, lamp housings, brake pistons, solenoid bobbins, engine oil filters, ignition device cases and other automobile and vehicle-related parts, gaskets for primary or secondary batteries in mobile phones, notebook computers, video cameras, hybrid cars, electric cars, etc.; EXAMPLES
[0124] The effects of the present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Basic evaluations in each example and comparative example were carried out by the following methods.
[0125] (1) Melt viscosity measurement The resin composition pellets obtained in each of the Examples and Comparative Examples were measured using a Capillograph manufactured by Toyo Seiki Seisakusho Co., Ltd. under conditions of a test temperature of 300° C., a shear rate of 122 / s, a capillary length of 10 mm, and a capillary diameter of 1 mm.
[0126] (2) Measurement of generated gas volume 10 g of the resin composition pellets obtained in each Example and Comparative Example were weighed into an aluminum cup, treated for 2 hours in an Espec PHH202 hot air dryer heated to 320° C., and allowed to cool at room temperature. The weight was then measured, and the weight loss rate (%), which is the ratio of the weight change before and after the drying treatment to the weight before the drying treatment, was determined as the amount of generated gas.
[0127] (3) Injection molding The resin composition pellets obtained in each of the Examples and Comparative Examples were injection molded into ISO (1A) dumbbell test pieces using an injection molding machine SE75-DUZ manufactured by Sumitomo Heavy Industries, with a cylinder temperature of 310°C and a mold temperature of 140°C.
[0128] (4) Initial mechanical properties The tensile properties of the ISO (1A) dumbbell test pieces injection molded under the conditions described in (3) were evaluated at 23°C using an autograph AG-Xplus 20kN testing machine in accordance with ISO 527-1, -2, with a support distance of 114 mm and a tensile speed of 5 mm / min. Next, the bending properties were evaluated according to ISO178 at a support distance of 64 mm and a speed of 2 mm / min.
[0129] (5) Mechanical properties after heat treatment at 180℃ for 500 hours The ISO (1A) dumbbell test pieces injection molded under the conditions described in (3) were treated for 500 hours in an Espec PHH202 hot air dryer heated to 180°C, and then allowed to cool at room temperature for 24 hours.
[0130] Next, the tensile properties and bending properties were evaluated in the same manner as described in (4).
[0131] (6) Mechanical properties after LLC treatment at 150℃ for 500 hours The ISO (1A) dumbbell test pieces injection molded under the conditions described in (3) were immersed in an autoclave filled with a mixture of LLC (Toyota Super Long Life Coolant (product number 08889-01005) manufactured by Toyota Motor Corporation) and ion-exchanged water in a weight ratio of 1:1, and then treated for 500 hours in an ESPEC PHH202 hot air dryer heated to 150°C, and then allowed to cool at room temperature for 24 hours.
[0132] Next, the tensile properties and bending properties were evaluated in the same manner as described in (4).
[0133] (7) Blow molding The resin composition pellets obtained in each of the Examples and Comparative Examples were subjected to a blow molding machine, and a hollow molded body having a wall thickness of 3 mm, φ40 mm and a length of 200 mm and a thin-walled hollow molded body having a wall thickness of 1 mm, φ40 mm and a length of 200 mm were molded at a cylinder temperature of 320°C.
[0134] (8) Thickness uniformity evaluation For the blow molded hollow molded bodies and thin-walled hollow molded bodies, the thicknesses were measured at five arbitrary points on the circumference of the upper part (30 mm from the upper end) and lower part (30 mm from the lower end) of the molded products, and the wall thickness uniformity was calculated using the following formula. Thickness uniformity = ((average thickness of the bottom 5 points - average thickness of the top 5 points) / (average thickness of the top 5 points)) x 100 (%)
[0135] (9) Repeated pressure test The blow molded hollow molded bodies and thin-walled hollow molded bodies were subjected to a pressurization operation of introducing compressed air to increase the internal pressure from 0 MPa to 1 MPa 1,000 times, and were evaluated as follows according to the number of times that pressure leakage occurred. ◎: No pressure leakage even after 1000 cycles ○: 300 times or more to less than 1000 times ×: Less than 300 times
[0136] The raw materials used in each of the examples and comparative examples are shown below.
[0137] [Reference Example 1] (A) Polyphenylene sulfide resin A 70-liter autoclave equipped with a stirrer and a bottom plug valve was charged with 8.27 kg (70.00 mol) of 47.5% sodium hydrosulfide, 2.94 kg (70.63 mol) of 96% sodium hydroxide, 11.45 kg (115.50 mol) of N-methyl-2-pyrrolidone (NMP), 1.89 kg (23.1 mol) of sodium acetate, and 5.50 kg of ion-exchanged water. The mixture was gradually heated to 245°C over about 3 hours while passing nitrogen through it at normal pressure. After distilling out 9.77 kg of water and 0.28 kg of NMP, the reaction vessel was cooled to 200°C. The amount of water remaining in the system per mole of charged alkali metal sulfide was 1.06 mol, including the water consumed in the hydrolysis of NMP. The amount of hydrogen sulfide scattered was 0.02 mol per mole of charged alkali metal sulfide.
[0138] After that, it was cooled to 200°C, 10.42 kg (70.86 mol) of p-dichlorobenzene and 9.37 kg (94.50 mol) of NMP were added, the reaction vessel was sealed under nitrogen gas, and the temperature was raised from 200°C to 270°C at a rate of 0.6°C / min while stirring at 240 rpm, and the reaction was carried out at 270°C for 140 minutes. Then, 2.40 kg (133 mol) of water was injected while cooling from 270°C to 250°C over 15 minutes. Then, it was gradually cooled from 250°C to 220°C over 75 minutes, and then quenched to near room temperature and the contents were removed.
[0139] The contents were diluted with about 35 liters of NMP, stirred at 85°C for 30 minutes as a slurry, and filtered through an 80 mesh wire mesh (opening 0.175 mm) to obtain a solid. The obtained solid was washed and filtered with about 35 liters of NMP in the same manner. The obtained solid was diluted with 70 liters of ion-exchanged water, stirred at 70°C for 30 minutes, and filtered through an 80 mesh wire mesh to recover the solid. This operation was repeated three times in total. The obtained solid and 32 g of acetic acid were diluted with 70 liters of ion-exchanged water, stirred at 70°C for 30 minutes, filtered through an 80 mesh wire mesh, and the obtained solid was further diluted with 70 liters of ion-exchanged water, stirred at 70°C for 30 minutes, and filtered through an 80 mesh wire mesh to recover the solid. The solid thus obtained was dried at 120°C under a nitrogen stream to obtain a dried PPS.
[0140] [Other ingredients] (B) Reinforcing fiber: Glass fiber (T-747H manufactured by Nippon Electric Glass Co., Ltd.), 3 mm long, average fiber diameter 10.5 μm (C) Olefin copolymer containing epoxy groups: ethylene-glycidyl methacrylate copolymer (Sumitomo Chemical's "Bondfast" E). Amount of glycidyl methacrylate copolymerized: 12 wt% Unmodified olefin copolymer: Ethylene-1-butene copolymer (Mitsui Chemicals "Tafmer" A4085) Polyamide: Nylon 66 with a relative viscosity of 3.0 (Toray's "Amilan") (D) Organic silane compound-1: 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane (Shin-Etsu Silicone: KBM303) (D) Organic silane compound-2: 3-isocyanate propyl triethoxysilane (Shin-Etsu Silicone: KBE9007N) (E) Phosphorus oxoacid metal salt: Sodium phosphinate monohydrate (Wako Pure Chemical Industries, Ltd.) Phenolic antioxidant: 3,9-bis{2-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane (ADEKA "Adekastab" AO80) Phosphorus-based antioxidant: 3,9-bis(2,6-di-t-butyl-4-methylphenoxy)2,4,8,10-tetraoxa-3,9-diphosphapyro[5.5]undecane (ADEKA "ADEKA STAB" PEP36)
[0141] [Examples 1 to 4, Comparative Examples 1 to 6] The raw materials were dry-blended in the ratios shown in Table 1, and then melt-kneaded at a cylinder temperature of 280°C and a screw rotation speed of 300 rpm using a Japan Steel Works TEX30α twin-screw extruder (L / D=45, two kneading sections) equipped with a vacuum vent, and pelletized using a strand cutter.
[0142] The pellets were then dried overnight at 130°C and injection molded, and the test pieces obtained were subjected to various physical property evaluations. The pellets were then dried overnight at 130°C and direct blow molded as described above to obtain a hollow molded product with a wall thickness of 3 mm and a thin-walled hollow molded product with a wall thickness of 1 mm. The hollow molded products were then subjected to a pressure cycle test.
[0143] [Table 1]
[0144] The results of the Examples and Comparative Examples in Table 1 above will be compared and explained. As shown in Examples 1 to 4, (A) polyphenylene sulfide resin, (B) reinforcing fiber, (C) olefin-based copolymer containing epoxy groups, (D) organosilane compound, and (E) phosphorus oxoacid metal salt were melt-kneaded, and the resulting composition maintained a high melt viscosity capable of suppressing drawdown, while exhibiting a small amount of gas generation and excellent initial mechanical properties. In addition, the mechanical properties showed excellent heat aging resistance after treatment at 180°C for 500 hours.
[0145] In particular, in Examples 2 to 4, since a large amount of (B) reinforcing fiber was blended, excellent bending strength was obtained, and as a result, no pressure leakage was observed even in a repeated pressure test of a thin-walled hollow molded product with a wall thickness of 1 mm.
[0146] In Comparative Example 1, the melt viscosity was lower than in Example 1, and drawdown was observed during blow molding of a thin-walled hollow molded product with a wall thickness of 1 mm, and a thin-walled hollow molded product with an uneven wall thickness was obtained that was not worthy of a pressure cycle test. In Comparative Example 2, compared to Example 1, the phosphorus oxoacid metal salt (E) was not added, so the reactive extrusion control was insufficient and the resin temperature during melt kneading increased significantly. As a result, an increase in the amount of gas generated, a decrease in initial mechanical properties, and a significant decrease in the tensile elongation at break and bending strength after 500 hours of treatment at 180°C were observed. As a result, although a thin-walled hollow molded product was obtained, the molded product had many voids, and pressure leakage was observed in less than 300 cycles in the pressure cycle test.
[0147] In Comparative Example 3, the melt viscosity was lower than that in Example 2, so that drawdown was observed even during blow molding of a hollow molded product with a wall thickness of 3 mm, and a hollow molded product was obtained with an uneven wall thickness that was not worthy of a pressure cycle test. In Comparative Example 4, since (E) the phosphorus oxoacid metal salt was not added, the reactive extrusion control was insufficient and the resin temperature during melt kneading increased significantly. As a result, an increase in the amount of gas generated, a decrease in initial mechanical properties, and a significant decrease in the tensile elongation at break and bending strength after 500 hours of treatment at 180°C were observed. As a result, although a thin-walled hollow molded product was obtained, the molded product had many voids, and pressure leakage was observed in less than 300 cycles in the pressure cycle test.
[0148] In Comparative Example 5, compared to Example 2, a phenol-based antioxidant and a phosphorus-based antioxidant were added instead of the phosphorus oxoacid metal salt (E). However, the reactive extrusion was not well controlled, and the result was similar to that of Comparative Example 4. As a result, although a thin-walled hollow molded product was obtained, the molded product had many voids, and pressure leakage was observed within 300 cycles in a pressure cycle test.
[0149] In Comparative Example 6, a polyamide was melt-kneaded instead of the olefin copolymer containing epoxy groups (C), and a decrease in melt viscosity was observed. As a result, drawdown was observed even during blow molding of a hollow molded article with a wall thickness of 3 mm, and the obtained hollow molded article had an uneven wall thickness and was not worthy of a pressure cycle test. It is clear that the olefin copolymer containing epoxy groups (C) is essential for applying a polyphenylene sulfide resin composition to blow molding.
Claims
1. A polyphenylene sulfide resin composition comprising 100 parts by weight of (A) polyphenylene sulfide resin, 1 to 200 parts by weight of (B) reinforcing fiber, 1 to 200 parts by weight of (C) an olefin copolymer containing an epoxy group, 0.01 to 10 parts by weight of (D) an organosilane compound, and 0.01 to 5 parts by weight of (E) a metal salt of a phosphorus oxoacid, wherein the metal salt of a phosphorus oxoacid (E) is sodium phosphinate, and the polyphenylene sulfide resin composition has a flexural strength of 100 MPa or more and 300 MPa or less, as measured in accordance with ISO 178 using an ISO (1A) dumbbell test piece obtained by injection molding the polyphenylene sulfide resin composition.
2. 2. The polyphenylene sulfide resin composition according to claim 1, wherein the blending amount of the reinforcing fiber (B) is 15% by weight or more and 50% by weight or less when the total amount of the polyphenylene sulfide resin (A), the reinforcing fiber (B), and the olefin-based copolymer (C) containing an epoxy group is 100% by weight.
3. The polyphenylene sulfide resin composition according to any one of claims 1 to 2, having a melt viscosity measured at a temperature of 300°C and a shear rate of 122 / s of 1000 Pa·s or more and 3000 Pa·s or less.
4. 4. The polyphenylene sulfide resin composition according to claim 1, wherein the weight loss rate (%) of the resin composition when pellets are treated in air at 320° C. for 2 hours is 0.3% or more and 3.0% or less.
5. The polyphenylene sulfide resin composition according to any one of claims 1 to 4, wherein the (D) organic silane compound is an alkoxysilane compound having an epoxy group or an isocyanate group.
6. A molded article comprising the polyphenylene sulfide resin composition according to any one of claims 1 to 5.
7. The molded article according to claim 6, which is a hollow molded article.
8. A method for producing a molded article, comprising blow molding the polyphenylene sulfide resin composition according to any one of claims 1 to 5.
Citation Information
Patent Citations
Blow hollow molded product
JP1991236930A
Polyphenylene sulfide resin composition for laser welding, and composite molded product using it
JP2005015792A
Blow molded article and process for making the same
JP2011256387A
Long fiber reinforced polyarylene sulfide resin composition, molded article and manufacturing method therefor
JP2016183316A
Polyphenylene sulfide resin compositions
WO2004108827A1