Ceramic / copper / graphene bonded body, its manufacturing method, and ceramic / copper / graphene bonded structure

The ceramic/copper/graphene bonded body with an active metal carbide layer and Mg solid solution layer addresses peeling and current flow issues, providing stable heat dissipation and high reliability under thermal cycles.

JP7552282B2Active Publication Date: 2024-09-18MITSUBISHI MATERIALS CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020192559
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-22
Filing Date
2020-11-19
Publication Date
2024-09-18
Estimated Expiration
2040-11-19

AI Technical Summary

Technical Problem

Existing ceramic/copper/graphene bonded structures face issues with peeling and current flow under severe cooling/heating cycles, leading to unreliable thermal conductivity and heat dissipation.

Method used

A ceramic/copper/graphene bonded body with a configuration that includes a copper member, graphene-containing carbonaceous member, and active metal carbide layer, along with a Mg solid solution layer, to enhance bonding strength and suppress current flow, using active metals like Zr, Nb, and Hf for improved thermal cycle reliability.

Benefits of technology

The structure maintains stable heat dissipation characteristics and prevents peeling at the bonding interface, ensuring high reliability under thermal cycles by enhancing bonding strength and thermal conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552282000005
    Figure 0007552282000005
  • Figure 0007552282000006
    Figure 0007552282000006
  • Figure 0007552282000004
    Figure 0007552282000004
Patent Text Reader

Abstract

To provide a ceramic / copper / graphene assembly with excellent cold-heat cycle reliability, in which the copper member and the graphene-containing carbonaceous member are firmly joined, the current flowing through the joined part can be suppressed, and no delamination occurs under cold-heat cycle load.SOLUTION: A ceramic / copper / graphene assembly in which are joined a ceramic member 26, a copper member 21 made of copper or copper alloy, and a graphene-containing carbonaceous member 25 containing graphene aggregates. Along the joined interface between the copper member 21 and the graphene-containing carbonaceous member 25, there is formed on the side of the graphene-containing carbonaceous member 25 an active metal carbide layer 41 that contains carbides of one or more active metals selected from Ti, Zr, Nb, and Hf. Between the active metal carbide layer 41 and the copper member 21 is formed an Mg solid solution layer 42 in which Mg is solid-solved in the matrix phase of Cu.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceramic / copper / graphene bonded structure having a structure in which a ceramic member, a copper member made of copper or a copper alloy, and a graphene-containing carbonaceous member containing graphene aggregates are bonded to each other, a manufacturing method thereof, and a ceramic / copper / graphene bonded structure. [Background technology]

[0002] A graphene-containing carbonaceous material containing graphene aggregates has excellent thermal conductivity and is therefore particularly suitable as a material for forming a heat dissipation member, a heat conduction member, or the like. For example, by forming an insulating layer made of ceramics or the like on the surface of the graphene-containing carbonaceous member containing the above-mentioned graphene aggregates, it becomes possible to use the graphene-containing carbonaceous member as an insulating substrate.

[0003] For example, Patent Document 1 discloses an anisotropic heat conduction element having a structure in which graphene sheets are stacked along a first direction, and an intermediate member (copper plate) joined to an end face of the structure in a second direction intersecting the first direction, with the intermediate member being pressure-bonded to the end face via an insert material containing at least titanium. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-238733 A Summary of the Invention [Problem to be solved by the invention]

[0005] Incidentally, the insulating substrate may be subjected to thermal cycles in the environment in which it is used. In particular, in recent years, the insulating substrate may be used in harsh environments such as engine rooms, and may be subjected to thermal cycles under severe conditions with large temperature differences. In the above-mentioned Patent Document 1, the copper intermediate and the graphene structure are bonded via an insert material containing titanium. However, depending on the bonding conditions, the copper intermediate and the graphene structure may not be bonded firmly, and peeling may occur when subjected to severe thermal cycles.

[0006] Furthermore, when the copper / graphene bonded body of Patent Document 1 is installed in a certain device as a heat dissipation member, the conductive copper intermediate body comes into contact with the device, and therefore, a current may flow into the bonded portion through this intermediate body, which may make it difficult to maintain the bond between the copper intermediate body and the graphene structure.

[0007] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a ceramic / copper / graphene bonded body in which a copper member made of copper or a copper alloy and a graphene-containing carbonaceous member containing graphene aggregates are firmly bonded to each other, the current flowing through the bonded portion can be suppressed, peeling does not occur even when subjected to thermal cycle loads, and the bonded body has excellent thermal cycle reliability, and a manufacturing method thereof. [Means for solving the problem]

[0008] In order to solve such problems and achieve the object, a ceramic / copper / graphene bonded body of the present invention is a ceramic / copper / graphene bonded body having a structure in which a ceramic member, a copper member made of copper or a copper alloy, and a graphene-containing carbonaceous member containing graphene aggregates are bonded together, and is characterized in that at a bonding interface between the copper member and the graphene-containing carbonaceous member, an active metal carbide layer containing carbides of one or more active metals selected from Ti, Zr, Nb and Hf is formed on the graphene-containing carbonaceous member side, and a Mg solid solution layer in which Mg is solid-solved in a Cu matrix is ​​formed between the active metal carbide layer and the copper member.

[0009] In the ceramic / copper / graphene bonded body having this configuration, an active metal carbide layer is formed on the bonding surface of the graphene-containing carbonaceous member at the bonding interface between the copper member and the graphene-containing carbonaceous member, and an Mg solid-solution layer in which Mg is dissolved in a Cu matrix is ​​formed on the bonding surface side of the copper member. As a result, Mg in the Mg solid-solution layer sufficiently reacts with the active metal in the active metal carbide layer, and the copper member is firmly bonded to the graphene-containing carbonaceous material via the active metal carbide layer, so that it is possible to suppress cracks and peeling at the bonding interface during thermal cycle loading. Furthermore, since the ceramic / copper / graphene bonded body having this configuration contains copper as a constituent material, it has a function of efficiently dissipating heat as a heat spreader during a transition period.

[0010] Moreover, in the ceramic / copper / graphene bonded body having this configuration, the copper member having electrical conductivity is covered with the ceramic member. Therefore, when the ceramic / copper / graphene bonded body is brought into contact with a predetermined device, a current is prevented from flowing into the bonded portion through the copper member, and the bond between the copper member and the graphene-containing carbonaceous member can be maintained. Therefore, the ceramic / copper / graphene bonded body having this configuration can maintain stable heat dissipation characteristics while suppressing the occurrence of peeling at the bonded interface due to thermal cycles, thereby achieving high reliability.

[0011] In the ceramic / copper / graphene bonded body of the present invention, it is preferable that the Mg solid solution layer contains a Cu-Mg intermetallic compound phase made of an intermetallic compound containing Cu and Mg. In this case, the Cu-Mg intermetallic compound phase is distributed on the bonding surface side with the active metal carbide layer and is significantly involved in the bonding, thereby increasing the strength of the bond with the active metal carbide layer.

[0012] In the Mg solid solution layer, the active metal carbide thing The boundary between the layer and the Mg solid solution layer CopperWhen the area of ​​a region within a range of a distance of 50 μm toward the member side is A and the area of ​​the Cu—Mg intermetallic compound phase is B, the ratio B / A is preferably 0.3 or less.

[0013] In the ceramic / copper / graphene bonded body of the present invention, it is preferable that the Mg solid solution layer contains a second intermetallic compound phase made of an intermetallic compound containing Cu and the active metal. In this case, the second intermetallic compound phase is distributed on the bonding surface side with the active metal carbide layer and is significantly involved in bonding, thereby increasing the strength of the bond with the active metal carbide layer.

[0014] In the ceramic / copper / graphene bonded body of the present invention, the ceramic member may be made of an oxygen-containing ceramic, and a magnesium oxide layer may be formed on the ceramic member side at the bonding interface between the ceramic member and the copper member. In this case, the formation of the magnesium oxide layer can strengthen the bond between the oxygen-containing ceramic member and the copper member, and can suppress the occurrence of cracks and peeling at the bond interface when subjected to thermal cycle loading.

[0015] In the ceramic / copper / graphene bonded body of the present invention, the ceramic member may be made of a nitrogen-containing ceramic, and an active metal nitride layer containing nitrides of one or more active metals selected from Ti, Zr, Nb, and Hf may be formed on the ceramic member side at the bonding interface between the ceramic member and the copper member. In this case, by forming an active metal nitride layer containing nitrides of one or more active metals selected from Ti, Zr, Nb, and Hf, the bond between the nitrogen-containing ceramic member and the copper member can be strengthened, and cracks and peeling can be suppressed at the bond interface when subjected to thermal cycle loading.

[0016] Furthermore, in the ceramic / copper / graphene bonded body of the present invention, it is preferable that the graphene-containing carbonaceous member includes graphene aggregates formed by depositing single or multiple layers of graphene and flat graphite particles, the flat graphite particles are stacked using the graphene aggregates as a binder such that basal planes of the flat graphite particles are folded over, and the basal planes of the flat graphite particles are oriented in one direction. In this case, it is possible to further improve the thermal conductivity characteristics of the graphene-containing carbonaceous member.

[0017] The method for producing a ceramic / copper / graphene bonded body of the present invention is a method for producing the above-mentioned ceramic / copper / graphene bonded body, and includes a copper / graphene bonding step of bonding the copper member and the graphene-containing carbonaceous member, and a copper / ceramic bonding step of bonding the copper member and the ceramic member, the copper / graphene bonding step including an active metal and Mg arranging step of arranging one or more active metals selected from Ti, Zr, Nb, and Hf, and Mg, between the copper member and the graphene-containing carbonaceous member, a lamination step of laminating the copper member and the graphene-containing carbonaceous member with the active metal and Mg interposed therebetween, and a bonding step of bonding the copper member and the graphene-containing carbonaceous member laminated with the active metal and Mg interposed therebetween by heat treatment in a vacuum atmosphere while applying pressure in a lamination direction, and the active metal and Mg arranging step includes a step of bonding the copper member and the graphene-containing carbonaceous member laminated with the active metal and Mg interposed therebetween by applying pressure in a lamination direction, and 2 The amount of Mg is 14 μmol / cm 2 The present invention is characterized in that:

[0018] According to the method for producing a ceramic / copper / graphene joint having this configuration, in the active metal and Mg arrangement step, the amount of active metal is set to 0.4 μmol / cm 2 or more, and the Mg content is 14 μmol / cm 2 As a result, a sufficient amount of liquid phase necessary for the interface reaction can be obtained, and therefore the copper member and the graphene-containing carbonaceous material can be reliably joined.

[0019] Here, in the method for producing a ceramic / copper / graphene bonded body of the present invention, it is preferable that the pressure load in the bonding step is in the range of 0.049 MPa or more and 1.96 MPa or less, and the heating temperature in the bonding step is in the range of 700°C or more and 950°C or less. In this case, the pressure load in the joining process is set within the range of 0.049 MPa or more and 1.96 MPa or less, and the heating temperature is set within the range of 700°C or more and 950°C or less, so that the liquid phase necessary for the interfacial reaction can be maintained and a uniform interfacial reaction can be promoted.

[0020] In the method for producing a ceramic / copper / graphene bonded body of the present invention, in the copper / ceramic bonding step, it is preferable that one or more active metals selected from Ti, Zr, Nb and Hf and Mg are disposed between the copper member and the ceramic member, and the copper member and the graphene-containing carbonaceous member stacked via the active metal and the Mg are bonded to each other by heat treatment in a vacuum atmosphere while being pressurized in a stacking direction. In this case, one or more active metals selected from Ti, Zr, Nb, and Hf, and Mg are used as bonding materials, which strengthens the bond between the copper member and the ceramic member, thereby making it possible to suppress cracks and peeling at the bonding interface when subjected to thermal cycle loading.

[0021] In the method for producing a ceramic / copper / graphene bonded body of the present invention, in the copper / ceramic bonding step, it is preferable that Mg is disposed between the copper member and the ceramic member, and the copper member and the graphene-containing carbonaceous member stacked via the Mg are bonded to each other by heat treatment in a vacuum atmosphere while being pressurized in a stacking direction. In this case, Mg is used as the bonding material, which strengthens the bond between the copper member and the ceramic member, making it possible to suppress the occurrence of cracks and peeling at the bonding interface when subjected to thermal cycles.

[0022] The ceramic / copper / graphene bonding structure of the present invention is a ceramic / copper / graphene bonding structure having a structure in which a ceramic member, a copper member made of copper or a copper alloy, and a graphene-containing carbonaceous member containing graphene aggregates are bonded together, and is characterized in that at the bonding interface between the copper member and the graphene-containing carbonaceous member, an active metal carbide layer containing carbides of one or more active metals selected from Ti, Zr, Nb and Hf is formed on the graphene-containing carbonaceous member side, and a Mg solid solution layer in which Mg is solid-solved in a Cu matrix is ​​formed between this active metal carbide layer and the copper member.

[0023] In the ceramic / copper / graphene bonding structure having this configuration, an active metal carbide layer is formed on the bonding surface of the graphene-containing carbonaceous member at the bonding interface between the copper member and the graphene-containing carbonaceous member, and an Mg solid solution layer in which Mg is dissolved in a Cu matrix is ​​formed on the bonding surface side of the copper member. As a result, Mg in the Mg solid solution layer sufficiently reacts with the active metal in the active metal carbide layer, and the copper member is firmly bonded to the graphene-containing carbonaceous material via this active metal carbide layer, so that it is possible to suppress cracks and peeling at the bonding interface during thermal cycle loading. Furthermore, since the ceramic / copper / graphene bonding structure having this configuration contains copper as a constituent material, it has a function of efficiently dissipating heat as a heat spreader during a transition period.

[0024] Moreover, in the ceramic / copper / graphene bonding structure having this configuration, the copper member having electrical conductivity is covered with the ceramic member. Therefore, when the structure is brought into contact with a specific device, the flow of current into the bonding portion through the copper member is suppressed, and the bond between the copper member and the graphene-containing carbonaceous member can be maintained. Therefore, this ceramic / copper / graphene bonding structure can maintain stable heat dissipation characteristics while suppressing the occurrence of peeling at the bonding interface due to thermal cycles, thereby achieving high reliability. Effect of the Invention

[0025] According to the present invention, a copper / graphene bonded body in which a copper member made of copper or a copper alloy and a graphene-containing carbonaceous member containing graphene aggregates are firmly bonded to each other, a current flowing through a bonded portion can be suppressed, and peeling does not occur even when subjected to a thermal cycle load, thereby providing an excellent thermal cycle reliability; and a manufacturing method thereof can be provided. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a schematic explanatory diagram of a power module using a ceramic / copper / graphene bonded body (insulating substrate) according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic explanatory diagram of a ceramic / copper / graphene bonded body (insulating substrate) according to an embodiment of the present invention. [Diagram 3] FIG. 2 is an enlarged schematic view of a bonding interface between a copper member and a graphene-containing carbonaceous member and a bonding interface between a copper member and a ceramic member in a ceramic / copper / graphene bonded body (insulating substrate) according to an embodiment of the present invention. [Figure 4] FIG. 1 is a flow diagram showing an example of a method for producing a ceramic / copper / graphene bonded body (insulating substrate) according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, embodiments of the present invention will be described with reference to the attached drawings. Note that the following embodiments are specifically described to better understand the gist of the invention, and do not limit the present invention unless otherwise specified. In addition, the drawings used in the following description may show essential parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0028] First, a ceramic / copper / graphene bonded body (ceramic / copper / graphene bonded structure) according to an embodiment of the present invention will be described with reference to FIGS. 1 to 4. FIG. The ceramic / copper / graphene bonded body in this embodiment is an insulating substrate 20 having a structure in which a ceramic member, a copper member made of copper or a copper alloy, and a graphene-containing carbonaceous member containing graphene aggregates are bonded together.

[0029] First, a power module using a ceramic / copper / graphene bonded body (insulating substrate 20) according to this embodiment will be described. The power module 1 shown in FIG. 1 includes an insulating circuit board 10, a semiconductor element 3 joined to one surface side (upper side in FIG. 1) of the insulating circuit board 10 via a solder layer 2, and a heat sink 31 disposed on the other surface side (lower side in FIG. 1) of the insulating circuit board 10.

[0030] Insulating circuit board 10 comprises an insulating layer (insulating substrate 20), a circuit layer 12 disposed on one surface (the upper surface in FIG. 1) of the insulating layer, and a metal layer 13 disposed on the other surface (the lower surface in FIG. 1) of the insulating layer. The insulating layer prevents electrical connection between the circuit layer 12 and the metal layer 13, and is made of an insulating substrate 20 in this embodiment.

[0031] The circuit layer 12 is formed by bonding a metal plate having excellent conductivity to one surface of an insulating layer (insulating substrate 20). In this embodiment, a copper plate made of copper or a copper alloy, specifically a rolled plate of oxygen-free copper, is used as the metal plate constituting the circuit layer 12. A circuit pattern is formed on this circuit layer 12, and one surface thereof (the upper surface in FIG. 1) serves as a mounting surface on which a semiconductor element 3 is mounted. The thickness of the metal plate (copper plate) that becomes the circuit layer 12 is set within the range of 0.1 mm to 1.0 mm, and is set to 0.6 mm in this embodiment. There is no particular limitation on the method for joining the metal plate (copper plate) that will become the circuit layer 12 and the insulating substrate 20, and they can be joined using an active metal brazing material or the like.

[0032] The metal layer 13 is formed by joining a metal plate having excellent thermal conductivity to the other surface of the insulating layer (insulating substrate 20). In this embodiment, the metal plate constituting the metal layer 13 is a copper plate made of copper or a copper alloy, specifically, a rolled plate of oxygen-free copper. The thickness of the metal plate (copper plate) that becomes the metal layer 13 is set within the range of 0.1 mm to 1.0 mm, and is set to 0.6 mm in this embodiment. There is no particular limitation on the method for joining the metal plate (copper plate) that will become the metal layer 13 and the insulating substrate 20, and they can be joined using an active metal brazing material or the like.

[0033] The heat sink 31 is for cooling the insulating circuit board 10 described above, and has a structure in which a plurality of flow paths 32 are provided for circulating a cooling medium (for example, cooling water). This heat sink 31 is preferably made of a material with good thermal conductivity, such as aluminum or an aluminum alloy, copper or a copper alloy, and in this embodiment, is made of 2N aluminum with a purity of 99 mass % or more. In this embodiment, the metal layer 13 of the insulating circuit board 10 and the heat sink 31 are bonded by solid-state diffusion bonding.

[0034] The semiconductor element 3 is made of a semiconductor material such as Si or SiC, and is mounted on the circuit layer 12 via a solder layer 2 made of a solder material such as Sn-Ag, Sn-In, or Sn-Ag-Cu.

[0035] The insulating substrate 20 of this embodiment constituting the insulating layer has a structure in which a ceramic plate 26 made of a ceramic member, a copper plate 21 made of a copper member made of copper or a copper alloy, and a carbon plate 25 made of a graphene-containing carbonaceous member containing graphene aggregates are laminated together, as shown in Fig. 2. The copper plates 21 are bonded to both main surfaces of the carbon plate 25, respectively. Here, an example of insulating substrate 20 is shown in which ceramic plate 26, copper plate 21, carbon plate 25, copper plate 21, and ceramic plate 26 are stacked in this order, but there is no limit to the number of layers as long as the outermost layer (end) in the stacking direction is ceramic plate 26 and the order of ceramic plate 26, copper plate 21, and carbon plate 25 is maintained.

[0036] The graphene-containing carbonaceous member constituting the carbon plate 25 preferably includes graphene aggregates formed by deposition of single or multiple layers of graphene and flat graphite particles, and the flat graphite particles are preferably laminated with the graphene aggregates as a binder so that the basal surfaces of the flat graphite particles are folded over. The basal surfaces of the flat graphite particles are preferably oriented in one direction.

[0037] The flat graphite particles have a basal surface on which the hexagonal carbon mesh plane appears and an edge surface on which the end of the hexagonal carbon mesh plane appears. As the flat graphite particles, flake graphite, flaky graphite, amorphous graphite, flaky graphite, kish graphite, pyrolytic graphite, highly oriented pyrolytic graphite, etc. can be used. Here, the average particle size of the graphite particles as viewed from the basal plane is preferably in the range of 10 μm to 1000 μm, more preferably in the range of 50 μm to 800 μm. By setting the average particle size of the graphite particles within the above range, the thermal conductivity is improved. Furthermore, the thickness of the graphite particles is preferably in the range of 1 μm to 50 μm, and more preferably in the range of 1 μm to 20 μm. By setting the thickness of the graphite particles within the above range, the orientation of the graphite particles can be appropriately adjusted. Furthermore, by adjusting the thickness of the graphite particles to within the range of 1 / 1000 to 1 / 2 of the particle size as viewed from the basal plane, excellent thermal conductivity and the orientation of the graphite particles can be appropriately adjusted.

[0038] The graphene aggregate is formed by depositing single-layer or multi-layer graphene, and the number of layers of the multi-layer graphene is, for example, not more than 100, and preferably not more than 50. This graphene aggregate can be produced, for example, by dropping a graphene dispersion in which single-layer or multi-layer graphene is dispersed in a solvent containing a lower alcohol or water onto a filter paper, and depositing the graphene aggregate while separating the solvent. Here, the average particle size of the graphene aggregates is preferably within a range of 1 μm to 1000 μm. By setting the average particle size of the graphene aggregates within the above range, the thermal conductivity is improved. Furthermore, the thickness of the graphene aggregates is preferably within a range of 0.05 μm or more and less than 50 μm. By setting the thickness of the graphene aggregates within the above range, the strength of the carbonaceous member is ensured.

[0039] 3 shows an enlarged schematic diagram of a bonding interface between a copper plate 21 made of a copper member made of copper or a copper alloy and a carbon plate 25 made of a graphene-containing carbonaceous material, and a bonding interface between the copper plate 21 and a ceramic plate 26. As shown in FIG. 3, at the bonding interface 40 between the copper plate 21 made of a copper member and the carbon plate 25 made of a graphene-containing carbonaceous material, an active metal carbide layer 41 containing one or two types of active metal carbides is formed on the bonding surface of the carbon plate 25. The copper plate 21 contains simple metals such as Mg and Cu, and intermetallic compounds (IMCs) such as Cu-Mg and Cu-Ti, and in particular, at the joint interface 40, an Mg solid solution layer 42 in which Mg is dissolved in a Cu matrix is ​​formed between the copper plate 21 and the active metal carbide layer 41. The Mg solid solution layer 42 may contain a Cu-Mg intermetallic compound phase made of an intermetallic compound containing Cu and Mg, or a second intermetallic compound phase made of an intermetallic compound containing Cu and an active metal.

[0040] This Cu-Mg intermetallic compound phase is composed of a Cu2Mg phase and / or a CuMg2 phase. In the Mg solid solution layer 42, in a cross section along the lamination direction of the copper member and the graphene-containing carbonaceous member, the area of ​​a region within a distance of 50 μm from the boundary surface 40a with the active metal carbide layer 41 toward the copper member side is defined as A (μm 2 ), and the area of ​​the Cu-Mg intermetallic compound phase is B (μm 2 ), the ratio B / A is preferably 0.3 or less, more preferably 0.25 or less, and most preferably 0.15 or less. There are also cases where the Mg solid solution layer 42 does not contain a Cu-Mg intermetallic compound phase, that is, where the ratio B / A is zero.

[0041] The active metal carbide layer 41 is formed by a reaction between the active metal contained in the bonding material interposed between the copper plate 21 and the carbon plate 25 and the carbon contained in the carbon plate 25 during bonding. The active metal constituting the active metal carbide layer 41 may be, for example, one or more selected from Ti, Zr, Hf, and Nb. In this embodiment, the active metal is Ti, and the active metal carbide layer 41 is made of titanium carbide (Ti-C).

[0042] Here, if the thickness t1 of the active metal carbide layer 41 is less than 0.05 μm, the reaction between the active metal and carbon may be insufficient, and the bonding strength between the copper plate 21 and the carbon plate 25 via the active metal carbide layer 41 may be insufficient. On the other hand, if the thickness t1 of the active metal carbide layer 41 exceeds 1.5 μm, cracks may occur in the active metal carbide layer 41 when subjected to a thermal cycle load. Therefore, in this embodiment, it is preferable to set the thickness t1 of the active metal carbide layer 41 within the range of 0.05 μm to 1.5 μm. The lower limit of the thickness t1 of the active metal carbide layer 41 is more preferably 0.1 μm or more, and even more preferably 0.25 μm or more. On the other hand, the upper limit of the thickness t1 of the active metal carbide layer 41 is more preferably 1.2 μm or less, and even more preferably 1.0 μm or less.

[0043] The ceramic plate 26 is bonded to the copper plate 21 via a compound layer 43. The compound layer 43 is a layer formed by reacting one or more active metals selected from Ti, Zr, Nb, and Hf, or Mg, as a bonding material, with the constituent elements of the ceramic plate 26. As the ceramic plate 26, for example, oxides such as Al2O3 and Zr-added Al2O3, nitrides such as AlN and Si3N4, and those containing SiAlON are used.

[0044] When the ceramic plate 26 is mainly composed of an oxide, it is preferable to use Mg as the bonding material, in which case the main element constituting the compound layer 43 is MgO. When the ceramic plate 26 is mainly composed of a nitride, it is preferable to use Ti as the bonding material, in which case the main element constituting the compound layer 43 is TiN.

[0045] Next, a method for producing the ceramic / copper / graphene bonded body (insulating substrate 20) according to this embodiment will be described with reference to a flow diagram shown in FIG.

[0046] (Carbon plate formation process S01) First, the above-mentioned flat graphite particles and graphene aggregates are weighed to have a predetermined compounding ratio, and then mixed using an existing mixer such as a ball mill. The mixture thus obtained is filled into a mold having a given shape and pressed to obtain a molded product. Heating may be performed during the pressing. The resulting molded body is then cut to obtain the carbon plate 25.

[0047] The pressure during molding is preferably in the range of 20 MPa to 1000 MPa, more preferably in the range of 100 MPa to 300 MPa. The temperature during molding is preferably in the range of 50° C. to 300° C. The pressurization time is preferably in the range of 0.5 minutes to 10 minutes.

[0048] (First active metal and Mg arrangement step S02) Next, a copper plate 21 made of copper or a copper alloy is prepared, the joining surface of this copper plate 21 is placed opposite the joining surface of the carbon plate 25 obtained in the previous step, and one or more active metals selected from Ti, Zr, Nb, and Hf, and Mg are placed between the two plates as joining materials. When the copper plate 21 is replaced with a plate of a different material, Cu is further placed as a joining material. The active metal and Mg can be placed by sputtering, (co)evaporation, foil material, or paste application (hydrides of active metal and Mg can also be used).

[0049] The amount of active metal to be placed between the copper plate 21 and the carbon plate 25 as a bonding material is 0.4 μmol / cm 2 The amount of Mg is 14 μmol / cm 2 Preferably, the amount of active metal is 0.4 μmol / cm 2 More than 47.0μmol / cm 2 The Cu content is within the range of 4 μmol / cm 2 More than 350μmol / cm 2 The Mg content is within the range of 14 μmol / cm 2 More than 180μmol / cm 2 It is within the following range.

[0050] (First lamination process S03) Next, the copper plates 21 are laminated (bonded) to both main surfaces of the carbon plate 25 via a bonding material.

[0051] (First joining process S04) Next, the carbon plate 25 and the copper plate 21 laminated with the bonding material therebetween are pressed in the lamination direction and heated, and then cooled, thereby bonding the carbon plate 25, the copper plate 21, and the ceramic plate 26 together. Here, the heating temperature is preferably within a range of 700°C or more and 950°C or less. The holding time at the heating temperature is preferably within a range of 10 minutes or more and 180 minutes or less. Furthermore, the pressing pressure is preferably within a range of 0.049 MPa or more and 1.96 MPa or less. Furthermore, the atmosphere during bonding is preferably a non-oxidizing atmosphere.

[0052] In this first bonding process S04, the active metal (Ti in this embodiment) contained in the bonding material reacts with the carbon contained in the carbon plate 25 at the bonding interface between the carbon plate 25 and the copper plate 21, thereby forming an active metal carbide layer 41 on the bonding surface of the carbon plate 25. Then, a part of Cu, Mg, and the active metal contained in the bonding material is absorbed into the copper plate 21, and further, the Cu and Mg contained in the bonding material react with each other, so that an Mg solid solution layer 42 in which Mg is dissolved in a Cu matrix is ​​formed between the copper plate 21 and the active metal carbide layer 41. The Mg solid solution layer 42 may contain a Cu-Mg intermetallic compound phase made of an intermetallic compound containing Cu and Mg, or may contain a second intermetallic compound phase made of an intermetallic compound containing Cu and an active metal.

[0053] (Second active metal and Mg arrangement step S05) Next, a ceramic plate 26 is prepared, the bonding surface of this ceramic plate 26 is placed opposite the bonding surface of the copper plate 25, and at least one material consisting of one or more active metals selected from Ti, Zr, Nb, and Hf, and Mg is placed between the two plates. The active metal and Mg can be placed by sputtering, (co)evaporation, foil material, or paste application (hydrides of the active metal and Mg can also be used).

[0054] When one or more active metals selected from Ti, Zr, Nb, and Hf are disposed between the copper plate 21 and the ceramic plate 25 as a bonding material, the amount of the active metal to be disposed is 0.4 μmol / cm 2 More than 47.0μmol / cm 2 It is preferable that the amount of Mg to be placed between the copper plate 21 and the ceramic plate 25 as a bonding material is within the following range. 2 More than 180μmol / cm 2 It is preferable to set it within the following range.

[0055] (Second lamination step S06) Next, a ceramic plate 26 is laminated via a bonding material onto each of the two copper plates 21 laminated onto the carbon plate 25. In this case, the bonding surface of the copper plate 21 becomes the main surface opposite to the carbon plate 25.

[0056] (Second bonding process S07) Next, the copper plate 21 and the ceramic plate 26 laminated with the bonding material therebetween are pressed in the lamination direction and heated, and then cooled, thereby bonding the copper plate 21 and the ceramic plate 26 together. Here, the heating temperature is preferably within a range of 700°C to 950°C. The holding time at the heating temperature is preferably within a range of 10 minutes to 90 minutes. The applied pressure is preferably within a range of 0.049 MPa to 1.96 MPa. The atmosphere during bonding is preferably a non-oxidizing atmosphere.

[0057] In the second bonding step S07, oxygen or nitrogen constituting the ceramic plate 26 reacts with elements of the bonding material at the bonding interface between the copper plate 21 and the ceramic plate 26, forming an oxide layer or a nitride layer.

[0058] When the ceramic plate 26 contains oxides such as Al2O3 and Zr-added Al2O3, and the bonding material between the copper plate 21 and the ceramic plate 26 is Mg, the bonding step S04 causes Mg to react with oxygen contained in the ceramic plate 26, and an MgO layer (compound layer 43) is formed at the bonding interface between the copper plate 21 and the ceramic plate 26.

[0059] When the ceramic plate 26 contains a nitride such as AlN or Si3N4, and the bonding material between the copper plate 21 and the ceramic plate 26 is Ti, the bonding step S04 causes Ti to react with the nitrogen contained in the ceramic plate 26, and a TiN layer (compound layer 43) is formed at the bonding interface between the copper plate 21 and the ceramic plate 26.

[0060] When the ceramic plate 26 contains SiAlON and the bonding material between the copper plate 21 and the ceramic plate 26 is Ti, the bonding step S04 causes Ti to react with the nitrogen contained in the ceramic plate 26, and a TiN layer (compound layer 43) is formed at the bonding interface between the copper plate 21 and the ceramic plate 26.

[0061] Through the above steps, the ceramic / copper / graphene bonded body (insulating substrate 20) of this embodiment is manufactured.

[0062] In the above embodiment, the carbon plate 25 and the copper plate 21 are joined together, and then the copper plate 21 and the ceramic plate 26 are joined together. However, the carbon plate 25, the copper plate 21, and the ceramic plate 26 may be joined together at the same time. Specifically, first, one or more active metals selected from Ti, Zr, Nb, and Hf, and Mg are arranged as bonding materials on one surface of the carbon plate 25, and the copper plate 21 is laminated on the arranged active metals and Mg. Furthermore, one or more active metals selected from Ti, Zr, Nb, and Hf, and Mg are arranged as bonding materials on the copper plate 21, and the ceramic plate 26 is laminated on the arranged active metals and Mg. When the copper plate 21 and the ceramic plate 26 are laminated on the other surface of the carbon plate 25, the carbon plate 25, the copper plate 21 and the ceramic plate 26 are laminated in the same manner. The active metal and Mg can be deposited by sputtering, (co)evaporation, application of a foil, or a paste (hydrides of the active metal and Mg can also be used).

[0063] Next, the carbon plate 25, the copper plate 21 and the ceramic plate 26 are pressed together in the stacking direction and heated, and then cooled, thereby bonding the carbon plate 25, the copper plate 21 and the ceramic plate 26 together. Here, the heating temperature is preferably within a range of 700°C or more and 950°C or less. The holding time at the heating temperature is preferably within a range of 10 minutes or more and 180 minutes or less. Furthermore, the pressing pressure is preferably within a range of 0.049 MPa or more and 1.96 MPa or less. Furthermore, the atmosphere during bonding is preferably a non-oxidizing atmosphere.

[0064] As described above, according to the ceramic / copper / graphene bonded body (insulating substrate 20) of the present embodiment, at the bonding interface between the copper member (copper plate 21) and the graphene-containing carbonaceous member (carbon plate 25), an active metal carbide layer 41 is formed on the bonding surface of the graphene-containing carbonaceous member, and an Mg solid solution layer 42 in which Mg is dissolved in a Cu matrix is ​​formed on the bonding surface side of the copper member. As a result, Mg in the Mg solid solution layer 42 sufficiently reacts with the active metal in the active metal carbide layer 41, and the copper member is firmly bonded to the graphene-containing carbonaceous material via the active metal carbide layer 41, so that it is possible to suppress the occurrence of cracks and peeling at the bonding interface during thermal cycle loading. Furthermore, since the ceramic / copper / graphene bonded body of the present embodiment contains copper as a constituent material, it has a function of efficiently dissipating heat as a heat spreader during a transition period.

[0065] Moreover, in the ceramic / copper / graphene bonded body of the present embodiment, the copper member having conductivity is covered with the ceramic member. Therefore, when the ceramic / copper / graphene bonded body is brought into contact with a predetermined device, a current is prevented from flowing into the bonded portion through the copper member, and the bond between the copper member and the graphene-containing carbonaceous member can be maintained. Therefore, the ceramic / copper / graphene bonded body of the present embodiment can maintain stable heat dissipation characteristics while suppressing the occurrence of peeling at the bonded interface due to thermal cycles, and can achieve high reliability.

[0066] In the ceramic / copper / graphene bonded body of this embodiment, it is preferable that the Mg solid solution layer contains a Cu-Mg intermetallic compound phase consisting of an intermetallic compound containing Cu and Mg. In this case, the Cu-Mg intermetallic compound phase is distributed on the bonding surface side with the active metal carbide layer and is greatly involved in bonding, thereby increasing the strength of bonding with the active metal carbide layer.

[0067] In the ceramic / copper / graphene bonded body of this embodiment, the Mg solid solution layer preferably contains a second intermetallic compound phase made of an intermetallic compound containing Cu and an active metal. In this case, the second intermetallic compound phase is distributed on the bonding surface side with the active metal carbide layer and is greatly involved in bonding, thereby increasing the strength of bonding with the active metal carbide layer.

[0068] In the ceramic / copper / graphene bonded body of the present embodiment, the ceramic member may be made of an oxygen-containing ceramic, and a magnesium oxide layer may be formed on the ceramic member side at the bonding interface between the ceramic member and the copper member. In this case, the magnesium oxide layer can strengthen the bonding between the oxygen-containing ceramic member and the copper member, and can suppress the occurrence of cracks and peeling at the bonding interface when subjected to thermal cycle loading.

[0069] In the ceramic / copper / graphene bonded body of the present embodiment, the ceramic member may be made of a nitrogen-containing ceramic, and an active metal nitride layer containing one or more nitrides of active metals selected from Ti, Zr, Nb, and Hf may be formed on the ceramic member side at the bonding interface between the ceramic member and the copper member. In this case, the active metal nitride layer containing one or more nitrides of active metals selected from Ti, Zr, Nb, and Hf is formed, thereby strengthening the bond between the nitrogen-containing ceramic member and the copper member, and suppressing the occurrence of cracks and peeling at the bonding interface during thermal cycle loading.

[0070] Furthermore, in the ceramic / copper / graphene bonded body of the present embodiment, the graphene-containing carbonaceous member preferably includes graphene aggregates formed by deposition of single or multiple layers of graphene and flat graphite particles, the flat graphite particles are laminated with the graphene aggregates as a binder such that the basal planes of the flat graphite particles are folded over, and the basal planes of the flat graphite particles are oriented in one direction. In this case, it is possible to further improve the thermal conductivity characteristics of the graphene-containing carbonaceous member.

[0071] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. For example, in the present embodiment, a power module is configured by mounting a semiconductor element (power semiconductor element) on the circuit layer of an insulating circuit board, but the present invention is not limited to this. For example, an LED module may be configured by mounting an LED element on an insulating circuit board, or a thermoelectric module may be configured by mounting a thermoelectric element on the circuit layer of an insulating circuit board.

[0072] In the present embodiment, as shown in FIG. 1, the insulating substrate 20 of the present embodiment is described as being applied as an insulating layer of the insulating circuit board 10. However, the present invention is not limited to this, and there is no particular limitation on the method of using the ceramic / copper / graphene bonded body of the present invention. EXAMPLES

[0073] The following describes confirmation experiments (Invention Examples 1 to 8, 11 to 19, and Comparative Examples 1 to 3) conducted to confirm the effectiveness of the present invention.

[0074] As disclosed in this embodiment, flat graphite particles and graphene aggregates were mixed at a predetermined mixing ratio and molded under pressure and heat to obtain a molded body having a structure in which flat graphite particles are laminated with the graphene aggregates as a binder so that the basal planes of the flat graphite particles are folded over each other. The obtained molded body was cut out to obtain a carbon plate (40 mm x 40 mm x 1.0 mm thick).

[0075] Mg and active metal were placed on one side of this carbon plate in the amounts of Mg and active metal shown in Tables 1 and 2, a copper plate (37 mm x 37 mm x 0.3 mm thick) was laminated on top of the placed Mg and active metal, and Mg and active metal were further placed on top of the copper plate in the amounts of Mg and active metal shown in Tables 1 and 2, a ceramic plate (made of silicon nitride, 37 mm x 37 mm x 0.3 mm thick) was laminated on top of the placed Mg and active metal, and the carbon plate, copper plate, and ceramic plate were joined under the conditions shown in Tables 1 and 2. The amount of Mg and the amount of active metal placed on one surface of the carbon plate were the same as the amount of Mg and the amount of active metal placed on the copper plate. Note that Mg and the active metal were deposited by co-evaporation. Here, the bonded interface between the carbon plate and the copper plate was observed to confirm the presence or absence of an active metal carbide layer, a Cu-Mg intermetallic compound phase, an active metal compound phase, and an Mg solid solution layer.

[0076] (with or without active metal carbide layer) The bonded interface between the copper plate and the carbon plate was observed at a cross section along the lamination direction of the obtained bonded body using a scanning transmission electron microscope (Titan ChemiSTEM (with EDS detector) manufactured by FEI) at a magnification of 20,000 to 120,000 times and an acceleration voltage of 200 kV. Mapping was performed using energy dispersive X-ray analysis (NSS7 manufactured by Thermo Scientific). An electron diffraction pattern was obtained by irradiating an electron beam narrowed to about 1 nm in the area where the active metal and C overlap (NBD (nanobeam diffraction) method). If this electron diffraction pattern was an intermetallic compound of the active metal and C, the active metal carbide layer was judged to be "present."

[0077] (Presence or absence of Cu-Mg intermetallic compound phase) In the cross section along the lamination direction of the obtained bonded body, the bonding interface between the copper plate and the carbon plate was observed using an electron beam microanalyzer (JXA-8539F manufactured by JEOL Ltd.) at a magnification of 2000 times and an acceleration voltage of 15 kV, and the elemental map of Mg was obtained in the region (400 μm × 600 μm) (hereinafter referred to as the observation region) including the bonding interface. The presence or absence of the Cu-Mg intermetallic compound phase was confirmed by determining the region where the Cu concentration was 5 atomic % or more and the Mg concentration was 30 atomic % or more and 70 atomic % or less in the average of five points of quantitative analysis in the region where the presence of Mg was confirmed. Note that the concentration here is the concentration when the total amount of Cu and Mg is 100 atomic %. In addition, in the joints of Examples 11 to 19 of the present invention, the active metal carbide in the observation area was thing The boundary between the layer and the Mg solid solution layer Copper The area of ​​the region within a distance of 50 μm toward the component side is defined as A, and the area of ​​the active metal carbide in the observation region is thing The ratio B / A was measured, where B is the area of ​​the Cu-Mg intermetallic compound phase in a region within a distance of 50 μm from the boundary between the layer and the Mg solid solution layer toward the copper member side.

[0078] (Presence or absence of active metal compound phase) The bonding interface between the copper plate and the ceramic substrate was observed using an electron beam microanalyzer (JXA-8539F manufactured by JEOL Ltd.) at a magnification of 2000 times and an acceleration voltage of 15 kV, and an elemental map of the active metal in the region (400 μm × 600 μm) including the bonding interface was obtained. In the region where the presence of the active metal was confirmed, the average of five points of quantitative analysis was determined to be a Cu-active intermetallic compound phase, and the presence or absence of the active metal compound phase was confirmed and indicated as the presence or absence of a second intermetallic compound phase. The concentration here is the concentration when the total amount of Cu and active metal is 100 atomic %.

[0079] (Presence or absence of Mg solid solution phase) The area (400μm×600μm) including the bonding interface between the copper plate and the ceramic substrate was observed with an electron beam microanalyzer (JXA-8539F manufactured by JEOL Ltd.) at a magnification of 2000 times and an accelerating voltage of 15kV. Quantitative analysis was performed at 10μm intervals from the ceramic substrate surface toward the copper plate side, at a range of 10 to 20 points depending on the thickness of the copper plate, and the presence or absence of the Mg solid solution phase was confirmed by defining the area with a Mg concentration of 0.01 atomic % to 6.9 atomic % as the Mg solid solution phase.

[0080] The resulting joined bodies of Examples 1 to 8 of the present invention and Comparative Examples 1 to 3 were subjected to 2000 thermal cycles of -40°C for 5 minutes and 150°C for 5 minutes. Further, a heating test was carried out on the obtained bonded bodies of Examples 11 to 19 of the present invention in a vacuum atmosphere, in which heating at 400° C. for 30 minutes and cooling to room temperature (25° C.) were repeated 10 times. Then, the initial bonded area and non-bonded area between the carbon plate and the copper plate were measured using an ultrasonic flaw detector (FineSAT200 manufactured by Hitachi Power Solutions Co., Ltd.) for these bonded bodies, and the bonding rate of the interface between the carbon plate and the copper plate was calculated using the following formula. (Bonding rate)=[{(Initial bonding area)-(Non-bonding area)} / (Initial bonding area)]×100 The initial bonded area here means the area of ​​the parts that should have been bonded. The non-bonded area means the part that should have been bonded but is not actually bonded, that is, the area of ​​the peeled part. In the image obtained by binarizing the ultrasonic inspection image, the peeling is shown as a white part in the bonded part, so the area of ​​this white part was taken as the non-bonded area (peeled area).

[0081] [Table 1]

[0082] [Table 2]

[0083] In Comparative Example 1, the amount of Mg was small, so the liquid phase generated at the interface was small, and the active metal carbide layer was not sufficiently generated. In Comparative Example 2, the amount of active metal was small, so the active metal carbide layer was not sufficiently generated. In Comparative Example 3, the amount of Mg was small, so the liquid phase generated at the interface was small, and furthermore, the amount of active metal was small, so the active metal carbide layer was not sufficiently generated. Therefore, the bonding rate between the copper plate and the carbon plate is low, less than 55%, in the initial stage, and after the thermal cycle load, it drops to about 0-2%, indicating that the bonding is almost completely eliminated.

[0084] In contrast, the ceramic / copper / graphene joints of Inventive Examples 1 to 8 and 11 to 19 have an active metal carbide layer and an Mg solid solution layer at the joint, and therefore the bonding rate between the copper plate and the carbon plate is high and exceeds 95%, and does not fall below 90% even when subjected to a thermal cycle load or heating test similar to those of Comparative Examples 1 to 3. These results show that the ceramic / copper / graphene joints of Inventive Examples 1 to 8 and 11 to 19 have sufficient strength to suppress peeling during a thermal cycle load, and thus achieve high reliability. [Explanation of symbols]

[0085] 20 Insulating substrate (ceramics / copper / graphene composite) 21 Copper plate (copper material) 25 Carbon plate (graphene-containing carbonaceous material) 26 Ceramic plate (ceramic component) 40 Joint interface 40a Boundary surface 41 Active metal carbide layer 42 Mg solid solution layer 43 Compound layer

Claims

1. A ceramic / copper / graphene bonded body having a structure in which a ceramic member, a copper member made of copper or a copper alloy, and a graphene-containing carbonaceous member containing graphene aggregates are bonded to each other, at a joining interface between the copper member and the graphene-containing carbonaceous member, an active metal carbide layer containing a carbide of one or more active metals selected from Ti, Zr, Nb, and Hf is formed on the graphene-containing carbonaceous member side, A ceramic / copper / graphene joint, characterized in that an Mg solid solution layer, in which Mg is dissolved in a Cu matrix, is formed between the active metal carbide layer and the copper member.

2. 2. The ceramic / copper / graphene joint according to claim 1, wherein the Mg solid solution layer contains a Cu-Mg intermetallic compound phase made of an intermetallic compound containing Cu and Mg.

3. 3. The ceramic / copper / graphene joint according to claim 2, wherein, when an area of ​​a region in the Mg solid solution layer within a distance of 50 μm from a boundary between the active metal carbide layer and the Mg solid solution layer toward the copper member is defined as A and an area of ​​the Cu-Mg intermetallic compound phase is defined as B, a ratio B / A is 0.3 or less.

4. 4. The ceramic / copper / graphene joined body according to claim 1, wherein the Mg solid solution layer has a second intermetallic compound phase made of an intermetallic compound containing Cu and the active metal.

5. 5. The ceramic / copper / graphene joined body according to claim 1, wherein the ceramic member is made of an oxygen-containing ceramic, and a magnesium oxide layer is formed on the ceramic member side at a joining interface between the ceramic member and the copper member.

6. 5. The ceramic / copper / graphene bonded body according to claim 1, wherein the ceramic member is made of a nitrogen-containing ceramic, and an active metal nitride layer containing nitrides of one or more active metals selected from Ti, Zr, Nb, and Hf is formed on the ceramic member side at a bonding interface between the ceramic member and the copper member.

7. 7. The ceramic / copper / graphene joint according to claim 1, wherein the graphene-containing carbonaceous member includes graphene aggregates formed by depositing single or multiple layers of graphene and flat graphite particles, the flat graphite particles are stacked using the graphene aggregates as a binder such that basal planes of the flat graphite particles are folded over, and the basal planes of the flat graphite particles are oriented in one direction.

8. 8. A method for producing a ceramic / copper / graphene bonded body according to claim 1, comprising: a copper / graphene bonding step of bonding the copper member and the graphene-containing carbonaceous member; and a copper / ceramic bonding step of bonding the copper member and the ceramic member, The copper / graphene bonding step includes an active metal and Mg arranging step of arranging one or more active metals selected from Ti, Zr, Nb, and Hf, and Mg, between the copper member and the graphene-containing carbonaceous member; a lamination step of laminating the copper member and the graphene-containing carbonaceous member with the active metal and Mg interposed therebetween; and a bonding step of bonding the copper member and the graphene-containing carbonaceous member laminated with the active metal and Mg interposed therebetween by heat treatment in a vacuum atmosphere while applying pressure in a lamination direction, In the active metal and Mg arrangement step, the amount of active metal is 0.4 μmol / cm 2 The amount of Mg is 14 μmol / cm 2 The above is a method for producing a ceramic / copper / graphene bonded body.

9. The pressure load in the joining step is in the range of 0.049 MPa or more and 1.96 MPa or less, 9. The method for producing a ceramic / copper / graphene bonded body according to claim 8, wherein a heating temperature in the bonding step is within a range of 700° C. or more and 950° C. or less.

10. 10. The method for producing a ceramic / copper / graphene bonded body according to claim 8 or 9, wherein in the copper / ceramic bonding step, one or more active metals selected from Ti, Zr, Nb, and Hf and Mg are disposed between the copper member and the ceramic member, and the copper member and the graphene-containing carbonaceous member stacked via the active metal and Mg are bonded to each other by heat treatment in a vacuum atmosphere while being pressurized in a stacking direction.

11. 10. The method for producing a ceramic / copper / graphene bonded body according to claim 8 or 9, wherein in the copper / ceramic joining step, Mg is disposed between the copper member and the ceramic member, and the copper member and the graphene-containing carbonaceous member stacked via the Mg are joined by being heat-treated in a vacuum atmosphere in a state in which the copper member and the graphene-containing carbonaceous member are pressurized in a stacking direction.

12. A ceramic / copper / graphene bonding structure in which a ceramic member, a copper member made of copper or a copper alloy, and a graphene-containing carbonaceous member containing graphene aggregates are bonded to each other, at a joining interface between the copper member and the graphene-containing carbonaceous member, an active metal carbide layer containing a carbide of one or more active metals selected from Ti, Zr, Nb, and Hf is formed on the graphene-containing carbonaceous member side, A ceramic / copper / graphene bonding structure, characterized in that an Mg solid solution layer, in which Mg is dissolved in a Cu matrix, is formed between the active metal carbide layer and the copper member.

Citation Information

Patent Citations

  • Copper and graphene composite coating on surface of integrated circuit ceramic circuit board and preparation method of copper and graphene composite coating

    CN108715992A

  • Brazing filler metal for joining of copper and ceramics or carbon-based copper compound material and method for joining the same

    JP2005305526A

  • Anisotropic thermally-conductive element and manufacturing method thereof

    JP2012238733A

  • Copper-ceramic bonded body, insulating circuit board, method for manufacturing copper-ceramic bonded body, and method for manufacturing insulating circuit board

    JP2018140929A

  • Composite heat transfer member and method of manufacturing the same

    JP2019096858A