Polyethylene resin film
A polyethylene resin film with controlled surface roughness and peak height, using specific density and organic lubricant, addresses blocking and scratch resistance issues, ensuring stable anti-blocking and slipperiness.
Patent Information
- Application Number
- JP2021515939
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-26
- Filing Date
- 2020-04-03
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2040-04-03
AI Technical Summary
Existing polyethylene resin films face issues with blocking, scratch resistance, and stability of anti-blocking properties, leading to contamination, appearance deterioration, and mechanical strength problems when used in laminated films for packaging.
A polyethylene resin film with a specific density range, containing polyethylene resin particles and an organic lubricant, achieving a controlled three-dimensional surface roughness and peak height, enhances scratch resistance and stability.
The film exhibits excellent appearance, heat-sealing properties, stable anti-blocking, and slipperiness, with improved scratch resistance and consistent performance across multiple measurements.
Smart Images

Figure 0007552587000001 
Figure 0007552587000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyethylene resin film, and a laminate and a package using the same. [Background technology]
[0002] In recent years, packaging or containers using films have been used in a wide range of fields due to their convenience, resource conservation, reduced environmental impact, etc. Compared to conventional molded containers and products, films have the advantages of being lightweight, easy to dispose of, and low cost.
[0003] A sealant film is generally used by laminating it with a base film such as a biaxially oriented nylon film, a biaxially oriented ester film, or a biaxially oriented polypropylene film, which has inferior low-temperature heat adhesion to the sealant film. If the sealant film is stored in a roll after lamination with such a base film, blocking occurs between the sealant film and the base film, making it difficult to unwind the laminate film before bag making, or blocking occurs between the sealant films that become the inner surface of the bag during bag making, making it difficult to fill the food. Therefore, a known method is to sprinkle powder such as starch on the surface of the sealant film to avoid the above-mentioned blocking between the sealant film and the substrate, and between sealant films themselves. However, this method not only contaminates the area around the film processing equipment, but also causes problems such as significantly worsening the appearance of the packaged food, powder adhering to the sealant film being directly mixed into the package along with the food, and reducing the heat seal strength.
[0004] In response to this, a polyethylene resin film using inorganic fine powder or inorganic fine particles such as silica in a polyethylene resin has been reported.
[0005] However, this method has the problem that scratches are likely to occur when film surfaces containing inorganic fine powder or inorganic particles such as silica added to the polyethylene resin film are rubbed against each other, and when the sealant fill or the laminate with the base film passes through a laminating machine or bag making machine, the inorganic fine powder or inorganic particles are likely to fall off, causing scratches and foreign matter problems.
[0006] Furthermore, a polyethylene resin film using organic crosslinked particles made of a copolymer mainly composed of an acrylic monomer and a styrene monomer has been reported. However, this method is still not sufficient, although its scratchability is not as bad as that of inorganic particles, and the problem of particles falling off still remains.
[0007] Furthermore, in order to improve the blocking resistance of polyethylene resin films, it has been reported that low-density polyethylene resin or high-density polyethylene resin is added to linear low-density polyethylene resin (see, for example, Patent Documents 1 and 2).
[0008] However, these methods have problems such as deterioration in mechanical strength properties such as tensile strength and transparency, and also poor blocking resistance. Furthermore, a polyethylene resin film has been reported in which particles made of a high molecular weight polyethylene resin are added to a high density polyethylene resin. However, this approach has the problem that it is inferior in mechanical strength properties such as tear strength, heat sealability at low temperatures, and transparency, and that the addition of particles made of polyethylene resin actually makes blocking resistance and slipperiness unstable. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 10-120849 [Patent Document 2] Japanese Patent Application Publication No. 10-87909 Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention aims to provide a polyethylene resin film that is excellent in appearance, heat sealability, stable blocking resistance, stable slipperiness, and also excellent scratch resistance, and also aims to provide a laminate and further a package using the polyethylene resin film. [Means for solving the problem]
[0011] As a result of intensive research, the inventors have found that the above-mentioned problems can be solved by controlling the protrusion height and organic organic lubricant content on the surface of a layer made of a polyethylene-based resin composition containing a polyethylene-based resin having a density in a specific range and particles made of a polyethylene-based resin, thereby achieving the present invention.
[0012] That is, the present invention is a polyethylene resin film having at least one layer A made of a polyethylene resin composition, in which the polyethylene resin composition constituting the layer A satisfies the following 1) to 3), and at least one surface of the layer A satisfies both of the following 4) and 5). 1) Density is 900kg / m 3 More than 935kg / m 3 The polyethylene resin includes the following: 2) Contains particles made of polyethylene resin. 3) The content of organic lubricant is 0.16% by weight or more. 4) The three-dimensional surface roughness SRa is 0.05 to 0.2 μm. 5) The maximum peak height SRmax is 2 to 15 μm.
[0013] Another embodiment is a polyethylene-based resin film having at least one layer A made of a polyethylene-based resin composition, in which the polyethylene-based resin composition constituting the layer A satisfies the following 1) to 3), and at least one surface of the layer A satisfies both of the following 4) and 5). 1) Density is 900kg / m 3 More than 935kg / m 3 The following is the result. 2) Contains particles made of polyethylene resin. 3) The content of organic lubricant is 0.16% by weight or more. 4) The three-dimensional surface roughness SRa is 0.05 to 0.2 μm. 5) The maximum peak height SRmax is 2 to 15 μm.
[0014] 3. The polyethylene resin multilayer film according to claim 1, wherein the particles made of the polyethylene resin have a resin hardness of D70 or less. In this case, it is preferable that the particles made of the polyethylene resin have a viscosity average molecular weight of 1.5 million or more and a melting point peak temperature by DSC of 150° C. or less.
[0015] Furthermore, in this case, it is preferable that the particles made of the polyethylene resin have an average particle size of 5 to 15 μm.
[0016] Furthermore, in this case, it is preferable that the content of the particles made of the polyethylene resin in the polyethylene resin composition constituting the layer A is 0.2 to 2.0% by weight.
[0017] Furthermore, in this case, it is preferable that the blocking value between the surfaces of the layer A is 200 mN / 70 mm or less.
[0018] Furthermore, in this case, it is preferable that the A layer surfaces are set together in a Gakushin abrasion tester manufactured by Yasuda Seiki and abraded 100 times with a load of 200 g, after which the change in haze is 5% or less.
[0019] Furthermore, in this case, a laminate containing any one of the polyethylene resin films described above and a substrate film made of the composition is preferred.
[0020] Furthermore, in this case, a packaging bag including the laminate is preferable. Effect of the Invention
[0021] The present invention can provide a polyethylene-based resin film that is excellent in appearance, heat sealability, stable blocking resistance, stable slipperiness, and particularly scratch resistance. It can also provide a laminate and a package using the polyethylene-based resin film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] (Layer A made of polyethylene resin composition) The layer A in the present invention is made of a polyethylene resin composition, which mainly contains a polyethylene resin and also contains particles made of a polyethylene resin. The polyethylene resin composition preferably contains 50% by weight or more of a polyethylene resin, more preferably 70% by weight or more, and even more preferably 90% by weight or more. (Polyethylene resin) The polyethylene resin in the present invention is any one of a homopolymer of an ethylene monomer, a copolymer of an ethylene monomer and an α-olefin, and a mixture thereof. Examples of the α-olefin include propylene, butene-1, hexene-1, 4-methylpentene-1, octene-1, and decene-1.
[0023] The density range of polyethylene resin is 900-935kg / m 3 More preferably, 910 to 933 kg / m 3 More preferably, 910 to 930 kg / m 3 Particularly preferred is a density of 935 kg / m 3The following polyethylene resins have a low heat-seal initiation temperature, are easy to process into bags, and are also excellent in transparency. More importantly, its density is 935kg / m 3 The inventors have found that when the following polyethylene resin is used, the particles made of polyethylene resin make it easy to make the three-dimensional surface roughness SRa of at least one surface of layer A 0.05 μm or more and the maximum peak height SRmax 2 μm or more, and the polyethylene resin film is more likely to have slip properties, blocking resistance, and scratch resistance, so that wrinkles and lumps are less likely to occur during coating, printing, and bag making, and transparency is also easily maintained. In particular, the blocking resistance is stable and does not easily vary between the measured values measured four times. In addition, the density is 900kg / m 3 When the above polyethylene-based resins are used, the particles made of polyethylene-based resin make it easy to control the three-dimensional surface roughness SRa of at least one surface of layer A to 0.2 μm or less and the maximum peak height SRmax to 15 μm or less, making it easy to improve transparency and stiffness.
[0024] Blocking resistance is measured by overlapping the A-layer surfaces of the film on top of each other and subjecting the sample to a heat press (Model SA-303, manufactured by Tester Sangyo Co., Ltd.) with dimensions of 7cm x 7cm, temperature of 50°C, pressure of 18MPa, and time of 15 minutes of pressure treatment. The sample blocked by this pressure treatment and a bar (diameter 6mm, material: aluminum) are attached to an autograph (Model UA-3122, manufactured by Shimadzu Corporation) so that the bar and peeling surface are horizontal, and the force at which the bar peels the blocked part at a speed of 200m / min is measured four times and the average value is used as an index. The density is 935kg / m 3 When the following polyethylene resin was used, not only was there little variation in the measured values from the four measurements, but there was also a tendency for the heat seal initiation temperature to be less likely to increase. It is preferable that the variation in the measured values from the four measurements be at the same level as when inorganic particles are used. The reason why the measured values are unlikely to vary for each measurement sample is that the density is 935 kg / m 3It is believed that when particles made of the following polyethylene and polyethylene-based resin are melt-mixed, changes in particle size due to a decrease in the viscosity average molecular weight of the particles made of polyethylene-based resin and entanglement of molecular chains with polyethylene-based resins other than the particles made of polyethylene-based resin are unlikely to occur, and as a result, the surface protrusions formed are uniform.
[0025] Scratch resistance was determined by placing the A-layer surfaces of polyethylene resin films together in a Yasuda Seiki Gakushin abrasion tester and rubbing 100 times with a load of 200g, and measuring the change in haze. Haze was measured at the center of the film (width x length = 50mm x 180mm) before it was placed on the friction table (points were placed at the edges, and points were placed on both ends that did not affect the haze measurement from the side opposite the friction surface), and then the haze was measured at the same position after rubbing to determine the difference.
[0026] From the viewpoint of film formability, etc., the polyethylene resin preferably has a melt flow rate (hereinafter sometimes referred to as MFR) of about 2.5 to 4.5 g / min. Here, the MFR is measured in accordance with ASTM D1893-67. The polyethylene resin is synthesized by a method known per se.
[0027] When using a polyethylene resin with a low MFR of 2.5 g / 10 min or less, as explained in the density section, the particle size tends to change due to a decrease in the viscosity average molecular weight of the polyethylene resin particles and entanglement of molecular chains with polyethylene resins other than the particles, so care must be taken with the extrusion conditions. When producing films at high speed using a large film-forming machine, an MFR of about 3 to 4 g / 10 min is particularly preferable for film-forming properties.
[0028] From the standpoint of heat resistance and the like, the melting point of the polyethylene resin is preferably 85° C. or higher, more preferably 100° C. or higher, and particularly preferably 110° C. or higher.
[0029] The polyethylene resin may be a single system, but two or more polyethylene resins having different densities within the above density range may be blended. When two or more polyethylene resins having different densities are blended, the average density and blending ratio can be estimated by GPC measurement or density measurement.
[0030] The density as mentioned above is 900-935kg / m 3 The polyethylene resins can be selected according to the application from a variety of options: high-pressure low-density polyethylene (LDPE), which is transparent, flexible, and has excellent average tear strength and tensile strength; linear short-chain branched polyethylene (LLDPE), which is copolymerized with small amounts of butene-1 / hexene-1 / octene-1 and has many short molecular chains in the molecular chain, giving it excellent sealing performance and physical strength; and metallocene-catalyzed linear short-chain branched polyethylene (LLDPE), which has a very sharp molecular weight distribution, uniform comonomer distribution, and excellent tear, tensile, puncture strength, and pinhole resistance. The polyethylene resin used in the sealing layer may be a commercially available product, such as Umerit (registered trademark) 2040FC, 0540F, and 3540FC manufactured by Ube Maruzen Polyethylene Co., Ltd., and Sumikathene (registered trademark) E FV402 and E FV405 manufactured by Sumitomo Chemical Co., Ltd.
[0031] (Particles made of polyethylene resin) The particles made of the polyethylene resin contained in the polyethylene resin composition constituting the A layer preferably have a viscosity average molecular weight of 1.5 million or more, more preferably 1.6 million or more, and even more preferably 1.7 million or more, and preferably 2.5 million or less, more preferably 2.4 million or less, and even more preferably 2.3 million or less. If the viscosity average molecular weight of the particles made of polyethylene-based resin is within this range, it becomes possible to control the average particle diameter of the particles made of polyethylene-based resin, and by using it in combination with a polyethylene-based resin of a specific density, the three-dimensional surface roughness SRa of at least one surface of layer A can be set to 0.05 to 0.2 μm and the maximum peak height SRmax to 2 to 15 μm. The reason for this is believed to be that the difference in molecular weight between the particles made of polyethylene-based resin and polyethylene-based resin other than the particles made of polyethylene-based resin is very large, so the molecules do not mix sufficiently, and even in the film obtained by melt mixing and extrusion, the particles made of polyethylene-based resin easily maintain a shape close to spherical, and aggregation due to fusion or adhesion between particles is unlikely to occur, making it possible to form protrusions with controlled shapes on the film surface. When the viscosity average molecular weight of the particles made of polyethylene resin is 1,500,000 or more, and the temperature during melt mixing with a polyethylene resin other than the particles made of polyethylene resin is higher than the melting point peak of the particles made of polyethylene resin, even under film production conditions of high shear or high draft ratio using a large extruder, decomposition due to heat or shear, fusion and aggregation of the particles made of polyethylene resin, and changes in particle size and shape of the particles made of polyethylene resin due to partial compatibility with polyethylene resins other than the particles made of polyethylene resin are unlikely to occur, so that protrusions with a controlled shape like inorganic particles or organic crosslinked resin particles can be easily formed, and not only does it function sufficiently as an antiblocking agent, but it is also unlikely to affect the appearance such as transparency, the mechanical strength of the film, or the heat sealability. Furthermore, and this is also surprising, it was found that particles made of polyethylene resin with a viscosity average molecular weight of 1.5 million or more have the property of being less likely to aggregate in polyethylene resin, yet are less likely to fall off from the polyethylene resin near the film surface, a characteristic that is not possessed by inorganic particles or organic crosslinked resin particles. When the viscosity average molecular weight is 1.5 million to 2.5 million, it becomes easy to set the average particle size to 5 to 20 μm, and when the sealing layer raw materials are melt-mixed and extruded to form a film, it tends to be easy to form suitable film surface protrusions. Furthermore, when the viscosity average molecular weight of particles made of polyethylene resin is 1.5 million or more, the particles themselves have lubricating properties, which contributes to improved blocking resistance and slippage, and since particles made of polyethylene resin are soft, it is believed that scratch resistance is also improved.
[0032] The resin hardness of the particles made of polyethylene resin is preferably D70 or less. When the hardness is 70 or less, the laminated layer of the film, for example, the vapor deposition layer, is less likely to be damaged, and the barrier property is less likely to decrease. The hardness is more preferably D68 or less. Furthermore, when the hardness of the particles made of polyethylene resin is D60 or more, the slipperiness is improved and is less likely to deteriorate even when exposed to heat during film processing.
[0033] The particles made of polyethylene-based resins are homopolymers of ethylene monomers, or copolymers of ethylene monomers and α-olefins, or mixtures thereof. Examples of α-olefins include propylene, butene-1, hexene-1, 4-methylpentene-1, octene-1, decene-1, etc.
[0034] The density range of the particles made of polyethylene resin is 930-950kg / m 3 is preferable, and 935 to 945 kg / m 3 More preferably, 937 to 942 kg / m 3 More preferably, the density is 930 kg / m 3 Smaller polyethylene resin particles are soft and have difficulty maintaining their shape during melt extrusion, which reduces blocking resistance. 3 Larger particles made of polyethylene resin are not only harder and more likely to have reduced scratch resistance, but also have reduced affinity with the base polyethylene resin, which may result in reduced resistance to falling off.
[0035] The average particle size of the particles made of the polyethylene resin contained in the polyethylene resin composition constituting the layer A is preferably 5 μm or more, more preferably 6 μm or more, and even more preferably 7 μm or more, and is preferably 20 μm or less, more preferably 17 μm or less, and particularly preferably 15 μm or less. In addition, it is preferable that the film does not contain particles having a particle size of 30 μm or more. Even if the average particle size is 20 μm or less, if the film contains a certain amount of 10% or more particles having a particle size of 30 μm or more, the maximum peak height of the film surface is likely to exceed 15 μm, and if this occurs, the flickering described below will occur when the film surface is visually observed. Furthermore, particles larger than 30 μm are also undesirable because they have the same appearance as gel defects and result in reduced quality.
[0036] By making the average particle size of the polyethylene resin particles 5 μm or more, it is possible to improve the slipperiness and blocking resistance. Furthermore, when the average particle size is 20 μm or less, the three-dimensional surface roughness SRa and maximum protrusion height SRmax of at least one surface of layer A do not become too large, and the number of protrusions increases compared to when the same weight of particles made of polyethylene resin is added, making it easier to obtain sufficient slip properties, blocking resistance, and scratch resistance for film processing.
[0037] Furthermore, the average particle size of particles made of polyethylene resin is less likely to change due to crushing or agglomeration caused by kneading during extrusion than relatively soft inorganic particles such as talc or calcium carbonate, making it easier to control the average particle size (before and after extrusion). By setting the average particle size of particles made of polyethylene resin in the range of 5 to 20 μm, protrusions caused by coarse particles are almost eliminated, and since the hardness of the protrusions themselves is lower than that of inorganic particles, adverse effects on the other side of Layer A or on a coating provided in a layer other than Layer A are suppressed.
[0038] The content of the particles made of polyethylene resin in the polyethylene resin composition constituting the A layer is preferably 0.2% by weight or more, more preferably 0.3% by weight or more, and even more preferably 0.4% by weight or more, based on the polyethylene resin composition. Also, it is preferably 2.0% by weight or less, more preferably 1.5% by weight or less, and even more preferably 1.0% by weight or less. When the amount of the particles made of polyethylene resin added is 0.2% by weight or more, the maximum peak height on at least one side of the A layer surface is within the specified area (0.2 mm 2) is easily set to 2 μm or more, which makes it easier to obtain blocking resistance and slipperiness. Also, if the amount of particles made of polyethylene resin is set to 2.0 wt % or less, the number of protrusions on the surface of layer A is not too large, which makes it easier to improve transparency and low-temperature sealability.
[0039] The polyethylene resin composition constituting the A layer contains an organic lubricant. The film has improved slipperiness and anti-blocking effect, and the film is easier to handle. The reason for this is believed to be that the organic lubricant bleeds out and is present on the film surface, thereby exerting a lubricant effect and a mold release effect. Furthermore, it is preferable to add an organic lubricant having a melting point above room temperature. Examples of organic lubricants include fatty acid amides and fatty acid esters. Specific examples include oleic acid amide, erucic acid amide, behenic acid amide, ethylene bis oleic acid amide, hexamethylene bis oleic acid amide, ethylene bis stearic acid amide, etc. These may be used alone, but it is preferable to use two or more of them in combination, since this makes it possible to maintain lubricity and anti-blocking effects even under harsh environments.
[0040] The lower limit of the content of the organic lubricant in the polyethylene resin composition constituting the A layer is preferably 0.16% by weight or more, preferably 0.18% by weight, more preferably 0.19% by weight, and particularly preferably 0.21% by weight. If it is 0.16% by weight or more, the slipperiness is likely to be stable immediately after film formation. The upper limit is preferably 0.3% by weight, more preferably 0.25% by weight. If it is 0.3% by weight or less, it is not too slippery and is unlikely to whiten over time.
[0041] When inorganic particles are contained in Layer A, the average particle size is preferably sufficiently smaller than that of the particles made of polyethylene resin. Preferably, the average particle size of the inorganic particles is 50% or less of that of the particles made of polyethylene resin, and preferably does not contain coarse particles that are twice or more the average particle size. In the polyethylene resin composition constituting the layer A, the content of inorganic particles is preferably 0.20% by weight or less, more preferably 0.10% by weight or less, even more preferably 0.05% by weight or less, and most preferably 0% by weight. By making the content of inorganic particles 0.20% by weight or less, not only is the residue at the time of incineration reduced, but also it becomes easier to obtain effects similar to those obtained when only particles made of polyethylene resin are added, such as scratch resistance and particles not falling off.
[0042] Even when inorganic particles are added, if the particle size is as described above and the residue when the film is incinerated is 500 ppm or less, the incineration residue can be made extremely small when compared to films containing conventional inorganic particles. The inorganic particles referred to here are inorganic substances generally used as antiblocking agents, such as silica, talc, calcium carbonate, diatomaceous earth, and zeolite.
[0043] When crosslinked organic particles are contained in Layer A, the average particle size is preferably sufficiently smaller than the average particle size of the particles made of polyethylene resin. Preferably, the average particle size of the crosslinked organic particles is 50% or less of the average particle size of the particles made of polyethylene resin, and it is preferable that the crosslinked organic particles contain almost no coarse particles having a particle size of more than twice the average particle size. The content of crosslinked organic particles in the polyethylene resin composition constituting the layer A is preferably equal to or less than the amount of particles made of polyethylene resin from the viewpoints of suppressing die resin buildup and cost. In the polyethylene resin composition constituting layer A, in order to obtain the maximum effect of adding particles made of polyethylene resin, such as scratch resistance and prevention of particle shedding, as in the case of inorganic particles, it is most preferable that the polyethylene resin composition does not contain crosslinked organic particles. The crosslinked organic particles referred to here are organic crosslinked particles typified by polymethyl acrylate resins and the like.
[0044] (Polyethylene resin composition) The density range of the polyethylene resin composition constituting the A layer is 900 to 935 kg / m 3is preferable, and 910 to 933 kg / m 3 More preferably, 910 to 930 kg / m 3 More preferably, 915 to 928 kg / m 3 is particularly preferred, and 915 to 925 kg / m 3 is particularly preferred. 3 Smaller polyethylene resins tend to have poor blocking resistance. Density 935kg / m 3 The following polyethylene resin composition has a low heat seal initiation temperature, is easy to process into bags, and has excellent transparency. More importantly, it has a density of 940 kg / m 3 The inventors have found that when the following polyethylene-based resins are used, the polyethylene-based resin multilayer film is likely to have stable blocking resistance or stable slippage, and that due to the synergistic effect of the organic organic lubricant contained in the polyethylene resin composition constituting layer A and the surface protrusions consisting of polyethylene-based resin particles, the film has extremely excellent scratch resistance.
[0045] The polyethylene resin composition preferably has a melt flow rate (hereinafter sometimes referred to as MFR) of about 2.5 to 4.5 g / min from the viewpoint of film formability, etc. The MFR was measured in accordance with ASTM D1893-67.
[0046] (Multi-layer structure) The polyethylene resin film of the present invention may have a multi-layer structure. In the case of a multi-layer structure, in addition to the layer A, one or more other layers may be provided. As a specific method for forming the multilayer structure in this way, a general multilayering device (such as a multilayer feed block, a static mixer, or a multilayer multi-manifold) can be used. For example, a method can be used in which thermoplastic resins discharged from different flow paths using two or more extruders are laminated in multiple layers using a field block, a static mixer, a multi-manifold die, etc. It is also possible to use only one extruder and introduce the above-mentioned multi-layering device into the melt line from the extruder to the T-die.
[0047] In the case of a three-layer structure, it is recommended that the other layers be an intermediate layer (layer B) and a laminate layer (layer C), in that order. In this case, the outermost layers are layers A and C, respectively.
[0048] The polyethylene resin used in the intermediate layer (B layer) and laminate layer (C layer) may be, for example, one or a mixture of two or more selected from ethylene-α-olefin copolymers and high-pressure polyethylene. The ethylene-α-olefin copolymer is a copolymer of ethylene and an α-olefin having 4 to 18 carbon atoms, and examples of the α-olefin include butene-1, hexene-1, 4-methylpentene-1, octene-1, and decene-1. Films obtained from these polyethylene resins have excellent heat seal strength, hot tack properties, impurity sealability, and impact resistance. The polyethylene resins may be mixed with other resins, such as ethylene-vinyl acetate copolymers and ethylene-acrylate copolymers, to the extent that these properties are not impaired.
[0049] In this case, the polyethylene resins used in the intermediate layer (B layer) and the laminate layer (C layer) may be the same or different. Also, particles made of polyethylene resin may be added or not added, but it is preferable not to add them because the presence of large particles such as coarse particles in the laminate layer tends to cause lamination lifting.
[0050] In this case, it is preferable that the average density of the polyethylene resin composition constituting each layer of the film is Layer A≦Intermediate layer (Layer B)≦Laminate layer (Layer C). The organic lubricant contained therein does not easily migrate to layers with high density, and is therefore effective in maintaining the slipperiness of Layer A after lamination and in maintaining the laminate strength over time.
[0051] In this case, the lower limit of the density of the polyethylene resin composition constituting the intermediate layer (B layer) is preferably 900 kg / m 3 and more preferably 920 kg / m 3and more preferably 930 kg / m 3 If it is less than the above, the strength will be weak and it may be difficult to process. The upper limit of the density of the intermediate layer (B layer) is preferably 960 kg / m 3 and more preferably 940 kg / m 3 and more preferably 935 kg / m 3 It is.
[0052] The polyethylene resin composition constituting the intermediate layer (B layer) of the polyethylene resin film of the present invention may contain the above-mentioned organic organic lubricant, and the lower limit of the organic organic lubricant is preferably 100 ppm. If the amount is less than the above, the slipperiness may be deteriorated. The upper limit of the organic lubricant in the polyethylene resin composition constituting the intermediate layer is preferably 2000 ppm, more preferably 1500 ppm. If the upper limit is exceeded, the lubricant becomes too slippery, which may cause misalignment during winding or whitening over time.
[0053] The recovered resin may be blended in the intermediate layer (layer B) of the film of the present invention to an extent that does not impair the quality of the recovered resin.
[0054] In the present invention, it is preferable to subject the laminate layer (layer C) surface of the polyethylene resin film described above to actinic ray treatment such as corona treatment, which improves the laminate strength.
[0055] When the polyethylene resin film of the present invention is two-layered, it is preferable that layer A is a sealing layer and the other layer is a laminate layer (layer C).
[0056] (Three-dimensional surface roughness SRa) The three-dimensional surface roughness SRa of the seal layer of the polyethylene-based resin multilayer film of the present invention is preferably 0.05 μm or more. When SRa is 0.05 μm or more, the film has excellent slip properties and blocking resistance. SRa is more preferably 0.07 μm or more, and particularly preferably 0.1 μm or more. The three-dimensional surface roughness SRa of the seal layer of the polyethylene-based resin multilayer film of the present invention is preferably 0.2 μm or less. When SRa is 0.2 μm or less, transparency is less likely to decrease. SRa is more preferably 0.18 μm or less, and particularly preferably 0.16 μm or less. The measurement method is the method described in the examples. (Maximum protrusion height SRmax) The maximum projection height of at least one surface of the A layer of the polyethylene resin film of the present invention must be 2 μm or more and 15 μm or less. If the maximum projection height SRmax exceeds 15 μm, it is not preferable because it causes a defective appearance. The measurement method is the method described in the examples.
[0057] (Heat seal start temperature) The upper limit of the heat seal initiation temperature of the polyethylene resin film of the laminate obtained by laminating a biaxially oriented nylon film (15 μm) and a polyethylene resin film is preferably 140° C., more preferably 130° C. If the temperature exceeds the above range, sealing processing may become difficult.
[0058] (attained heat seal strength) The lower limit of the heat seal strength attained by the polyethylene resin film of the laminate obtained by laminating a biaxially oriented nylon film (15 μm) and a polyethylene resin film at 150° C. is preferably 30 N / 15 mm, more preferably 35 N / 15 mm. If it is less than the above, the bag may be easily torn after bag formation. The upper limit of the heat seal strength at 150°C of the polyethylene resin film of the laminate obtained by laminating a biaxially oriented nylon film (15 μm) and a polyethylene resin film is preferably almost the same as the breaking strength of the laminated nylon. When the breaking strength is the same as that of the nylon, it means that the lamination strength is sufficiently high and the peel strength of the seal interface is sufficiently high. The measurement method is the method described in the examples.
[0059] (Blocking strength) The blocking strength of the polyethylene resin film in the laminate obtained by laminating a biaxially oriented nylon film (15 μm) and a polyethylene resin film is preferably as small as possible, more preferably 200 mN / 70 mm or less, and even more preferably 150 mN / 70 mm. If it exceeds the above range, the powder-free property and the opening property of the bagged product cannot be sufficiently obtained. The measurement method is the method described in the Examples.
[0060] (Coefficient of friction) The lower limit of the static friction coefficient of the polyethylene resin film in the laminate obtained by laminating a biaxially oriented nylon film (15 μm) and a polyethylene resin film is preferably 0.05, more preferably 0.08. If it is less than the above, the film may slip too much during winding, which may cause winding misalignment. The upper limit of the static friction coefficient after lamination is preferably 0.70, more preferably 0.5. If it exceeds the upper limit, the opening property after bag making and the filling property of the contents become poor, and loss during processing may increase. The measurement is carried out according to the method described in the Examples.
[0061] (Hayes) The lower limit of the haze of the polyethylene resin film of the present invention is preferably 3%, more preferably 4%, and further preferably 5%. If it is less than the above, the antiblocking agent may not be present on the surface sufficiently, which may cause blocking. The upper limit of the haze is preferably 18%, more preferably 16%, and even more preferably 13%. If it exceeds the above range, it may become difficult to visually confirm the contents. The measurement method is the method described in the examples.
[0062] (Flickering) It is preferable that the polyethylene resin film of the present invention exhibits almost no flickering or exhibits fine flickering that is uniform and not particularly bothersome. The measurement method is the method described in the Examples. In the so-called non-powder type, which has blocking resistance without sprinkling powder such as starch on the film surface, conventionally, inorganic particles with an average particle size of about 10 μm have been added, but these often contain coarse particles and are prone to flickering and poor transparency.
[0063] (Scratch resistance) A laminate obtained by laminating a biaxially oriented nylon film (15 μm) and a polyethylene resin film has a haze change of preferably 3% or less, more preferably 2% or less, even more preferably 1% or less, and particularly preferably 0.5% or less, even after the polyethylene resin film surfaces are rubbed together. The measurement method is the method described in the Examples. Conventional non-powder types, which have blocking resistance without sprinkling powder such as starch on the film surface, have included inorganic particles with an average particle size of about 10 μm. However, because inorganic particles are much harder than polyethylene resin, scratch resistance tends to be poor even when a sufficient amount of organic lubricant is present on the film surface.
[0064] (Young's Modulus) The lower limit of the Young's modulus (MD) of the polyethylene resin film of the present invention is preferably 60 MPa, more preferably 70 MPa. If it is less than the above, the stiffness may be too weak and processing may be difficult. The upper limit of the Young's modulus (MD) is preferably 600 MPa, more preferably 500 MPa.
[0065] The lower limit of the Young's modulus (TD) of the polyethylene resin film of the present invention is preferably 60 MPa, more preferably 70 MPa. If it is less than the above, the film may be too weak and difficult to process. The upper limit of the Young's modulus (TD) is preferably 600 MPa, more preferably 500 MPa.
[0066] (Laminate) The polyethylene resin multilayer film of the present invention can also be used as a packaging film or a packaging sheet in a laminate configuration in which at least one other base film is further laminated. The base film is not particularly limited, and may be appropriately selected and used depending on the intended use of the laminate, such as polyolefin films such as polyethylene and polypropylene, styrene-based resin films, polyester films such as polyethylene terephthalate and polybutylene terephthalate, polyamide films such as nylon 6 and nylon 6,6, or stretched films thereof, laminated films of polyolefin films and resin films having gas barrier properties such as polyamide films or ethylene-vinyl alcohol copolymer films, and, if necessary, metal foils such as aluminum, or vapor-deposited films or papers on which aluminum, silica, etc. are vapor-deposited. The base film may be used not only as one type, but also as a combination of two or more types laminated together.
[0067] In this case, it is preferable that the substrate film is adjacent to the laminate layer side of the polyethylene-based resin multi-layer film.
[0068] As a method for laminating the polyethylene-based resin multilayer film on the above-mentioned substrate film, a method of dry laminating the substrate film and the polyethylene-based resin multilayer film can be adopted. In that case, the structure can be polyethylene-based resin multilayer film / adhesive layer / other substrate film. For the adhesive layer, an anchor coating agent such as a urethane-based or isocyanate-based adhesive is used, or a modified polyolefin such as an unsaturated carboxylic acid grafted polyolefin is used as an adhesive resin, thereby enabling adjacent layers to be firmly bonded.
[0069] There is no particular limit to the thickness of the laminate, but when the laminate is used as a film for a lid or the like, it is preferably 10 to 200 μm, and when it is used as a sheet for cups or trays, it is preferably 200 to 1000 μm.
[0070] (packaging) A container can be manufactured by placing the seal layer surfaces of the sealant films of the laminate facing each other, or placing the seal layer surface of the sealant film layer of the laminate facing another base film, and then heat sealing at least a part of the periphery from the laminate side to form a desired container shape. Also, by heat sealing the entire periphery, a sealed bag-like container can be manufactured. If the molding process of this bag-like container is combined with a filling process of the contents, that is, the bottom and sides of the bag-like container are heat sealed, the contents are filled, and then the top is heat sealed, a package can be manufactured. Therefore, this laminate can be used in an automatic packaging device for solid, powder, or liquid materials such as snacks.
[0071] In addition, a container with the contents packaged therein can also be obtained by filling a container formed into a cup shape by vacuum forming or pressure forming, a container obtained by injection molding or blow molding, or a container formed from a paper base material with the contents, and then covering it with the laminate of the present invention as a lid material and heat sealing it. EXAMPLES
[0072] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not particularly limited by the following examples. The measured values of each item in the detailed description of the present invention and the examples were measured by the following methods.
[0073] Hereinafter, embodiments of the present invention will be described in detail. (1) Measurement method for particles made of polyethylene resin For the particles made of polyethylene resin, the physical properties of the raw material resin before processing were measured. Even after film formation, it is possible to completely dissolve the particles in decane and then separate the high molecular weight fraction using GPC or the like to separate the particles made of polyethylene resin and measure them.
[0074] (2) Viscosity average molecular weight of particles made of polyethylene resin Measurements were performed in accordance with ASTM-D4020.
[0075] (3) Average particle size of particles made of polyethylene resin The average particle size of the particles made of polyethylene resin before use was measured as follows. The particles were dispersed in ion-exchanged water stirred at a specified rotation speed (approximately 5000 rpm) using a high-speed stirrer, and the dispersion was added to isotone (physiological saline) and further dispersed using an ultrasonic disperser. The particle size distribution was then determined using the Cole counter method, and the average particle size was calculated.
[0076] (4) Particle size distribution of polyethylene resin particles The proportion of particles of polyethylene resin having a particle size of 30 μm or more before use was calculated from the particle size distribution obtained by the Coal Counter method.
[0077] (5) Melting point of particles made of polyethylene resin The melting point of the polyethylene resin particles before use was measured using a differential scanning calorimeter (DSC) manufactured by SII with a sample weight of 10 mg and a heating rate of 10°C / min. The melting endothermic peak temperature detected here was taken as the melting point.
[0078] (6) Density, MFR, and melting point of polyethylene resin other than particles made of polyethylene resin The raw materials before film formation were each measured by the following methods. The polyethylene resin forming the layer containing the particles made of polyethylene resin can be measured in the same manner after checking the layer structure with an electron microscope or the like for the entire layer if it is a single layer, or for a laminate, scraping off the surface to a thickness less than the surface layer, and removing the solvent from the filtered solution obtained in (1) above. When scraping off from a laminate, it can be done by laminating it on a PET film or the like and scraping off the surface layer with a razor or the like.
[0079] (density) The measurement was performed by the density gradient tube method according to JIS-K7112.
[0080] (Melt flow rate: MFR) (g / 10 min) The measurement was performed at a temperature of 190°C in accordance with JIS-K7210.
[0081] (Melting Point) Using a differential scanning calorimeter (DSC) manufactured by SII, measurements were performed with a sample weight of 10 mg and a heating rate of 10° C. / min. The melting endothermic peak temperature detected here was taken as the melting point.
[0082] (7) Content (wt%) of inorganic particles in the resin composition The content of the inorganic particles in the resin composition was calculated from the amount added in the raw material resin composition before processing. Even after forming the film, it is possible to separate and measure the inorganic particles by dissolving the film in decane as a solvent at a temperature at which the film completely dissolves, and then filtering the residue through a filter with a filtration accuracy of 1 to 2 μm.
[0083] (8) Residue amount after incineration of film (ppm) Approximately 30 g of film was weighed on a precision balance to the first decimal place (rounded off to the second decimal place). The crucible was pre-baked at 700°C for 1 hour, and after it had cooled to below 100°C, it was seasoned in a glass desiccator until it reached room temperature, and the weight of the crucible was then measured. The film was then placed in the crucible and incinerated in an electric furnace at 700°C for 2 hours, and after the heater was turned off, it was transferred to a glass desiccator after it had cooled to about 100°C and seasoned for 30 minutes until it reached room temperature. The difference in the crucible weight before and after incineration was then divided by the weight of the film to calculate the amount of residue.
[0084] (9) Filter pressure increase (film forming processability) The resin composition used in the sealing layer of Comparative Example 1 was passed through a Naslon sintered filter with a filtration accuracy of 120 μm at a resin temperature of 230° C. using a Troughton testing machine, and discharged into a filtration area of 81π square millimeters at a discharge rate of 1 kg / hour for 5 hours. The amount of pressure rise (ΔMPa) was used as the standard (△), and the results were classified into the following categories: ◎, ○, △, ×. ⊚: The amount of pressure increase is 5% or less than that at the start of extrusion. ◯: The amount of pressure increase is 10% or less than that at the start of extrusion. △: The amount of pressure increase is 15% or less than that at the start of extrusion. ×: The amount of pressure increase is 20% or less than that at the start of extrusion.
[0085] (10) Lip stains (film forming processability) The resin composition used for the sealing layer was extruded at 230°C for 5 hours using an extruder with a strand die (2 holes, 5 mm diameter). The lip stains were visually observed and classified as ◎, ○, △, or × using the result as the standard (△). ◎: Almost no lip stains can be seen. ○: Lip stains are slightly observed. △: Lip stains are clearly visible. ×: The lip stain grew and streak-like depressions appeared in the strands.
[0086] (11) Three-dimensional surface roughness SRa In accordance with JIS B0601-1994, a contact surface roughness tester (Kosaka Laboratory, Model ET4000A) was used to measure 100 arbitrary measurement points of 1 mm x 0.2 mm on a 3 cm x 3 cm square film piece, with a low cutoff of λs = 0.08 mm, a length of 1000 μm, and a pitch of 2 μm. From the obtained cross-sectional curve, the three-dimensional surface roughness SRa of the seal layer surface of the polyethylene resin multilayer film was calculated using the three-dimensional surface roughness analysis program TDA-22 in accordance with JIS B0601-1994. Measurements were performed using the above method (n=3), and the average value of the three-dimensional surface roughness SRx was calculated.
[0087] (12) Maximum projection height SRmax In accordance with JIS B0601-1994, a contact surface roughness tester (Kosaka Laboratory, Model ET4000A) was used to measure 100 arbitrary measurement points of 1 mm x 0.2 mm on a 3 cm x 3 cm square film piece, with a low cutoff of λs = 0.08 mm, a length of 1000 μm, and a pitch of 2 μm. From the obtained cross-sectional curve, the three-dimensional surface roughness analysis program TDA-22 was used to calculate the maximum projection height SRmax in accordance with JIS B0601-1994. Measurements were carried out using the above method (n=3), and the average value of the maximum projection height SRmax was calculated.
[0088] (13) Heat seal initiation temperature (℃) A dry lamination adhesive (TM569, CAT-10L) made by Toyo-Morton was applied to the corona surface of a nylon film (Toyobo biaxially oriented nylon film: N1100, 15 μm) at a solid content of 3 g / m 2 The adhesive was applied so that the adhesive would be applied to the sample, and the solvent was removed by volatilization in an oven at 80°C. The corona surface of the polyethylene resin film and the adhesive-coated surface were nipped and laminated on a temperature-controlled roll at 60°C. The laminated film was aged at 40°C for 2 days. The laminated sample was heat-sealed at a width of 10 mm at 10°C intervals with a sealing pressure of 0.1 MPa, a sealing time of 0.5 seconds, and a sealing temperature of 90 to 160°C. The heat-sealed sample was cut into strips with a heat seal width of 15 mm and set in an autograph (Shimadzu Corporation, model: UA-3122). The maximum strength of the peeled seal surface at a speed of 200 mm / min was measured with n number 3, and the heat seal strength and heat seal temperature at each temperature were plotted. The heat seal temperature at 4.9 N / 15 mm was read from a graph connecting each plot with a straight line and was taken as the heat seal start temperature.
[0089] (14) Heat seal strength achieved (N / 15mm) A dry lamination adhesive (TM569, CAT-10L) made by Toyo-Morton was applied to the corona surface of a nylon film (Toyobo biaxially oriented nylon film: N1100, 15 μm) at a solid content of 3 g / m 2The adhesive was applied so that the adhesive would be applied to the sample, and the solvent was removed by volatilization in an oven at 80°C. The corona surface of the polyethylene resin film and the adhesive-coated surface were then nipped and laminated on a temperature-controlled roll at 60°C. The laminated film was aged at 40°C for 2 days. The laminated sample was heat-sealed at 10°C intervals to a width of 10 mm with a sealing pressure of 0.1 MPa, a sealing time of 0.5 seconds, and a sealing temperature of 120 to 190°C. The heat-sealed sample was cut into strips with a heat seal width of 15 mm and set in an autograph (Shimadzu Corporation, model: UA-3122). The maximum strength of the peeled seal surface at a speed of 200 mm / min was measured with n number 3, and the heat seal strength with the highest average value was taken as the achieved seal strength.
[0090] (15) Blocking strength (mN / 70mm) A laminate film with a nylon film (biaxially oriented nylon film: N1100, 15 μm, manufactured by Toyobo) was prepared as follows. Apply Toyo Morton dry laminating adhesive (TM569, CAT-10L) to the corona surface of the nylon film at a solid content of 3 g / m 2 After the solvent was removed by volatilization in an oven at 80°C, the corona surface of the polyethylene resin film and the adhesive-coated surface were nipped and laminated on a temperature-controlled roll at 60°C. The laminated film was aged at 40°C for 2 days. A sample (10cm x 15cm) with the A layer surfaces overlapping is placed in a heat press (Tester Sangyo Co., Ltd., model: SA-303) so that the edge of an aluminum plate (2mm thick) measuring 7cm x 7cm is aligned with the center of the sample width (10cm) and 1cm inside in the length direction (15cm), and pressure treatment is performed at a temperature of 50°C, a gauge pressure of 18MPa, and a time of 15 minutes. The sample blocked by this pressure treatment and a bar (diameter 6 mm, material: aluminum) were attached to an autograph (Shimadzu Corporation, model: UA-3122) and the force at which the bar peeled off the blocked portion at a speed of 200 m / min was measured. In this case, it is assumed that the bar and the peeled surface are horizontal. The same sample was measured four times and the average value was displayed.
[0091] (16) Coefficient of static friction A laminate film with a nylon film (biaxially oriented nylon film: N1100, 15 μm, manufactured by Toyobo) was prepared as follows. Apply Toyo Morton dry laminating adhesive (TM569, CAT-10L) to the corona surface of the nylon film at a solid content of 3 g / m 2 After the solvent was removed by volatilization in an oven at 80°C, the corona surface of the polyethylene resin film and the adhesive-coated surface were nipped and laminated on a temperature-controlled roll at 60°C. The laminated laminated film was aged at 40°C for two days. The static friction coefficient between the polyethylene resin film surfaces of the laminated film was measured in an environment of 23°C and 65% RH in accordance with JIS-K-7125.
[0092] (17) Hayes Only the polyethylene resin film was measured using a direct reading haze meter manufactured by Toyo Seiki Seisakusho Co., Ltd. in accordance with JIS-K-7105. Haze (%) = [Td (diffuse transmittance %) / Tt (total light transmittance %)] x 100
[0093] (18) Flickering Only the polyethylene resin film was visually observed, and the flickering sensation was classified into the following categories: ◎, ◯, △, ×. : Almost no bright spots are noticeable. ○: There are small bright spots, but they are uniform and not particularly noticeable. △: There are some bright spots and a foreign body sensation is felt. ×: Bright spots are present all over the surface, impairing transparency.
[0094] (19) Scratch resistance (mechanical evaluation) The scratch resistance was evaluated by placing the sealing surfaces of the films together in a Yasuda Seiki Gakushin-type friction tester (friction tester type II, flat friction element 20 x 20 mm, test piece base flat type, sliding arc length 100 mm) so that the surfaces with polyethylene resin particles were aligned, and judging by the change in haze after 40 frictions with a load of 200 g. The haze was measured by measuring the haze at the center of the friction base of the film (width x length = 30 mm x 180 mm, 50 x 50 mm for flat friction element) before setting it on the friction base, and measuring the haze at the same position before and after friction to determine the difference.
[0095] (20) Scratch resistance (visual evaluation) A laminate film with a nylon film (biaxially oriented nylon film: N1100, 15 μm, manufactured by Toyobo) was prepared as follows. Apply Toyo Morton dry laminating adhesive (TM569, CAT-10L) to the corona surface of the nylon film at a solid content of 3 g / m 2 The adhesive was applied so that the adhesive layer was evenly distributed, and the solvent was removed by volatilization in an oven at 80°C. The corona surface of the polyethylene resin film and the adhesive-coated surface were then nipped and laminated on a temperature-controlled roll at 60°C. The laminated film was aged at 40°C for two days. The polyethylene resin film surfaces of the laminated film thus prepared were pinched with fingers so that they overlapped, and rubbed 10 times. The film was then visually inspected and classified as ◎, ○, △, or × for susceptibility to scratching. ◎: Almost no scratches. ○: Thin streak-like scratches occur, but whitening does not occur. △: Thin, dense streaks and partial whitening are observed. ×: The rubbed area turns almost white.
[0096] Next, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to the following examples. The following raw materials were used in the examples and comparative examples. (Polyethylene resin) (1) Ube Maruzen Polyethylene Co., Ltd. Yumerit (registered trademark) 0540F (metallocene-based linear low-density polyethylene, density 904 kg / m 3, MFR4.0g / 10min, melting point 111℃) (2) Sumitomo Chemical Co., Ltd. Sumikathene (registered trademark) E FV402 (metallocene catalyst-based LLDPE, density: 913 kg / m 3 , MFR: 3.8g / 10min, Melting point: 115℃) (3) Sumitomo Chemical Co., Ltd. Sumikathene (registered trademark) E FV405 (metallocene catalyst-based LLDPE, density: 923 kg / m 3 , MFR: 3.8g / 10min, Melting point: 118℃) (4) Sumitomo Chemical Co., Ltd. Sumikathene (registered trademark) E FV407 (metallocene catalyst-based LLDPE, density: 930 kg / m 3 , MFR: 3.2g / 10min, Melting point: 124℃) (5) Ube Maruzen Polyethylene Co., Ltd. Yumerit (registered trademark) 3540FC (metallocene catalyst-based LLDPE, density: 931 kg / m 3 , MFR: 3.6g / 10min, Melting point: 123℃) (6) Ube Maruzen Polyethylene Co., Ltd. Yumerit (registered trademark) 4540F (metallocene catalyst-based LLDPE, density: 944 kg / m 3 , MFR: 4.0g / 10min, Melting point: 128℃)
[0097] (Particles made of polyethylene resin) (1) Mipelon PM200 (average particle size 10 μm, melting point 136°C, density 940 kg / m) manufactured by Mitsui Chemicals, Inc. 3 , viscosity average molecular weight 1.8 million, percentage of particles with a diameter of more than 30 μm is 0%, resin hardness D65, ultra-high molecular weight polyethylene particles) (2) Mipelon XM221U (average particle size 25 μm, melting point 136, density 940 kg / m) manufactured by Mitsui Chemicals, Inc. 3 , viscosity average molecular weight 2 million, percentage of particles with a diameter of more than 30 μm is 25%, resin hardness D65, ultra-high molecular weight polyethylene particles)
[0098] (Inorganic particles) (1) Grefco. Inc., Dicalite WF (diatomaceous earth, processed to an average particle size of 5 μm using a pin mill) (2) Shin-Etsu Silicone's KMP-130-10 (spherical silica particles, average particle size 10 μm) was used as a 15% MB based on Sumitomo Chemical's FV402.
[0099] (Masterbatch) (1) Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd. was mixed with Mipelon PM200 to prepare a master batch (1) containing 15% by weight of Mipelon PM200. (2) Mipelon XM221U was mixed with Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd. to prepare a master batch (2) containing 15% by weight of Mipelon XM221U. (3) Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd. was mixed with Dicalite WF manufactured by Grefco. Inc. to prepare a master batch (3) containing 20% by weight of Dicalite WF manufactured by Grefco. Inc. (4) Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd. was mixed with KMP-130-10 manufactured by Shin-Etsu Silicones Co., Ltd. to prepare a master batch (4) containing 15% by weight of KMP-130-10 manufactured by Shin-Etsu Silicones Co., Ltd. (5) Erucamide was mixed with Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical to prepare a master batch (5) containing 4% by weight of erucamide. (6) Ethylene bis oleamide was mixed with Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical to prepare a master batch (6) containing 2% by weight of ethylene bis oleamide.
[0100] Example 1 [Sealing layer composition] A composition for a sealing layer was prepared using a mixture of 86.25% by weight of Umerit (registered trademark) 0540F manufactured by Ube Maruzen Polyethylene Co., Ltd., 4% by weight of master batch (1), 1.25% by weight of master batch (5), and 8.5% by weight of master batch (6). [Laminate layer composition] The laminate layer composition was prepared using only FV402 manufactured by Sumitomo Chemical Co., Ltd. [Composition for intermediate layer] A composition for an intermediate layer was prepared using a mixture of 99.4% by weight of FV402 manufactured by Sumitomo Chemical Co., Ltd., 0.5% by weight of master batch (5), and 0.1% by weight of master batch (6). The laminate layer composition, intermediate layer composition, and seal layer composition were melt-extruded at 240°C using an extruder with a T-die in the order of laminate layer composition, intermediate layer composition, and seal layer composition, and the thickness ratio of the laminate layer, intermediate layer, and seal layer was 8:34:8. Thereafter, the laminate layer surface was subjected to a corona discharge treatment. Then, the laminate layer was wound up on a roll at a speed of 150 m / min to obtain a polyethylene resin multilayer film having a thickness of 50 μm and a wet tension of 45 mN / m on the treated surface.
[0101] Example 2 In the sealing layer, 86% by weight of Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd., 4% by weight of masterbatch (1), 1.50% by weight of masterbatch (5), and 8.5% by weight of masterbatch (6) were mixed, A polyethylene resin multilayer film and a vapor-deposited film were obtained in the same manner as in Example 1, except that in the laminate layer, Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd. was used alone.
[0102] Example 3 A polyethylene resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that in the seal layer, 87.75% by weight of Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., 4% by weight of masterbatch (1), 1.25% by weight of masterbatch (5), and 7% by weight of masterbatch (6) were mixed, in the intermediate layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., and in the laminate layer, only Sumikathene (registered trademark) E FV407 manufactured by Sumitomo Chemical Co., Ltd. was changed.
[0103] Example 4 A polyethylene resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that in the seal layer, 84.75% by weight of Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., 8% by weight of masterbatch (1), 1.25% by weight of masterbatch (5), and 6% by weight of masterbatch (6) were mixed, in the intermediate layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., and in the laminate layer, only Sumikathene (registered trademark) E FV407 manufactured by Sumitomo Chemical Co., Ltd. was changed.
[0104] Example 5 In the sealing layer, 86.75% by weight of Umerit (registered trademark) 3540F manufactured by Ube Maruzen Polyethylene Co., Ltd., 4% by weight of masterbatch (1), 1.75% by weight of masterbatch (5), and 7.5% by weight of masterbatch (6) were mixed, In the middle layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Yumerit (registered trademark) 3540F manufactured by Ube Maruzen Polyethylene Co., Ltd. A polyethylene resin multilayer film and a vapor-deposited film were obtained in the same manner as in Example 1, except that in the laminate layer, only Umerit (registered trademark) 3540F manufactured by Ube Maruzen Polyethylene Co., Ltd. was used.
[0105] Example 6 A polyethylene resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that in the seal layer, 86.75% by weight of Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., 4% by weight of masterbatch (1), 0.5% by weight of masterbatch (3), 1.25% by weight of masterbatch (5), and 7.5% by weight of masterbatch (6) were mixed, in the intermediate layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., and in the laminate layer, only Sumikathene (registered trademark) E FV407 manufactured by Sumitomo Chemical Co., Ltd. was changed.
[0106] Example 7 A polyethylene resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that in the seal layer, 87.25% by weight of Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., 4% by weight of masterbatch (1), 1.25% by weight of masterbatch (5), and 7.5% by weight of masterbatch (6) were mixed, in the intermediate layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., and in the laminate layer, only Sumikathene (registered trademark) E FV407 manufactured by Sumitomo Chemical Co., Ltd. was changed.
[0107] The polyethylene resin films obtained in Examples 1 to 7 contained almost no inorganic particles larger than the particle size of the polyethylene resin particles, and therefore had excellent scratch resistance, low-temperature heat sealability, blocking resistance, slipperiness, and appearance. Moreover, the film had excellent processability in film formation, with very little residue when incinerated and almost no eye tar or filter pressure buildup.
[0108] Comparative Example 1 A polyethylene resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that in the seal layer, 82.25% by weight of Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., 2.5% by weight of masterbatch (3), 8% by weight of masterbatch (4), 1.25% by weight of masterbatch (5), and 6% by weight of masterbatch (6) were mixed, in the intermediate layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., and in the laminate layer, only Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd. was used. The film obtained in Comparative Example 1 had excellent blocking resistance and slipperiness, but had a slight flickering sensation, a large amount of inorganic residue after incineration, and was particularly poor in scratch resistance and slightly poor in film-forming processability.
[0109] Comparative Example 2 A polyethylene resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that in the seal layer, 90.25% by weight of Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., 2.5% by weight of masterbatch (3), 1.25% by weight of masterbatch (5), and 6% by weight of masterbatch (6) were mixed, in the intermediate layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., and in the laminate layer, only Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd. was used. The film obtained in Comparative Example 2 had relatively little residue and was excellent in terms of flickering, but was poor in blocking resistance, scratch resistance, and slipperiness.
[0110] Comparative Example 3 A polyethylene resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that in the seal layer, 87.75% by weight of Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., 1% by weight of masterbatch (1), 2.5% by weight of masterbatch (3), 1.25% by weight of masterbatch (5), and 7.5% by weight of masterbatch (6) were mixed, in the intermediate layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., and in the laminate layer, only Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd. was used. The film obtained in Comparative Example 3 had relatively few residues and was slightly superior in scratch resistance, but had few protrusions and was inferior in blocking resistance.
[0111] Comparative Example 4 In the sealing layer, 87.25% by weight of Umerit (registered trademark) 4540F manufactured by Ube Maruzen Polyethylene Co., Ltd., 4% by weight of masterbatch (1), 1.25% by weight of masterbatch (5), and 7.5% by weight of masterbatch (6) were mixed, In the middle layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Yumerit (registered trademark) 4540F manufactured by Ube Maruzen Polyethylene Co., Ltd. A polyethylene resin multilayer film and a vapor-deposited film were obtained in the same manner as in Example 1, except that in the laminate layer, only Umerit (registered trademark) 4540F manufactured by Ube Maruzen Polyethylene Co., Ltd. was used. The film obtained in Comparative Example 4 had relatively little residue and excellent scratch resistance, but the high resin density caused the surface protrusions made of polyethylene particles to be unstable, and the blocking resistance and slip properties were insufficient and there was a large variation.
[0112] Comparative Example 5 A polyethylene resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that in the seal layer, 87.25% by weight of Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., 4% by weight of masterbatch (2), 1.25% by weight of masterbatch (5), and 7.5% by weight of masterbatch (6) were mixed, in the intermediate layer, Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd. was changed to Sumikathene (registered trademark) E FV405 manufactured by Sumitomo Chemical Co., Ltd., and in the laminate layer, only Sumikathene (registered trademark) E FV407 manufactured by Sumitomo Chemical Co., Ltd. was changed. The film obtained in Comparative Example 5 had little residue and excellent scratch resistance, but because the particle diameter was large even though a large amount was added, the protrusion density was low and the blocking resistance and flickering sensation were poor.
[0113] Comparative Example 6 A polyethylene-based resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 1, except that a composition for the sealing layer was prepared using a mixture of 86.25% by weight of Umerit (registered trademark) 0540F manufactured by Ube Maruzen Polyethylene Co., Ltd., 4% by weight of masterbatch (1), 1.25% by weight of masterbatch (5), and 5.0% by weight of masterbatch (6).
[0114] Comparative Example 7 A polyethylene-based resin multilayer film and a vapor deposition film were obtained in the same manner as in Example 2, except that a composition for the sealing layer was prepared by mixing 95.90% by weight of Sumikathene (registered trademark) E FV402 manufactured by Sumitomo Chemical Co., Ltd., 4% by weight of masterbatch (1), 1.25% by weight of masterbatch (5), and 5.0% by weight of masterbatch (6).
[0115] The results are shown in Tables 1 and 2.
[0116] [Table 1]
[0117] [Table 2]
[0118] The polyethylene resin film of the present invention has been described above based on several examples. However, the present invention is not limited to the configurations described in the above examples, and the configuration can be appropriately changed within the scope of the gist of the present invention, such as by appropriately combining the configurations described in each example. [Industrial Applicability]
[0119] The polyethylene resin film of the present invention has excellent properties and can be suitably used as a film for a wide range of applications, such as food packaging.
Claims
1. The present invention has at least a layer A made of a polyethylene-based resin composition, and the polyethylene-based resin composition constituting the layer A satisfies the following 1) to 3), and at least one surface of the layer A satisfies both of the following 4) and 5). 1) Density is 900 kg / m3 or more and 935 kg / m3 or more 3 The polyethylene resin includes the following: 2) It contains particles made of a polyethylene resin having an average particle size of 5 to 20 μm. 3) The content of the organic lubricant is 0.16% by weight or more. 4) The three-dimensional surface roughness SRa is 0.05 to 0.2 μm. 5) The maximum peak height SRmax is 2 to 15 μm.
2. 2. The polyethylene resin multilayer film according to claim 1, wherein the particles made of the polyethylene resin have a resin hardness of D70 or less.
3. 3. The polyethylene resin film according to claim 1, wherein the particles made of the polyethylene resin have a viscosity average molecular weight of 1,500,000 or more.
4. 3. The polyethylene resin film according to claim 1, wherein the content of the polyethylene resin particles in the polyethylene resin composition constituting the layer A is 0.2 to 2.0% by mass.
5. 3. The polyethylene resin film according to claim 1, wherein the blocking value between the surfaces of the layer A is 200 mN / 70 mm or less.
6. 3. The polyethylene resin film according to claim 1, wherein the change in haze after 100 abrasion cycles at a load of 200 g when the A layer surfaces are placed against each other in a Gakushin abrasion tester manufactured by Yasuda Seiki is 3% or less.
7. A laminate comprising the polyethylene resin film according to any one of claims 1 to 6 and a substrate film made of a thermoplastic resin composition.
8. A packaging bag comprising the laminate according to claim 7.
Citation Information
Patent Citations
Polyolefin resin composition and film
JP1998045959A
Sealant film for retort
JP1998087909A
Toughened propylene polymer hardly exhibiting white fracture disposition
JP1998120849A
Low odored polyethylene-based resin laminated film, its manufacturing method and vessel made of low odored polyethylene-based resin laminated film
JP2006069096A
Linear polyethylene film
JP2013095066A