Resin composition, semiconductor wiring layer laminate, and semiconductor device
A curable resin composition with maleimide groups and a photoradical initiator forms a stable inter-wiring insulating layer, addressing copper diffusion issues in semiconductor wiring layers and enhancing insulation reliability.
Patent Information
- Application Number
- JP2022194258
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-01-23
- Filing Date
- 2022-12-05
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2037-09-26
AI Technical Summary
The formation of fine copper wirings in semiconductor wiring layers using the trench method leads to copper diffusion into organic insulating layers, risking short-circuits and compromising insulation reliability due to copper migration.
A resin composition containing a curable resin with maleimide groups and a photoradical polymerization initiator is used to form a wiring interlayer insulating layer that suppresses copper diffusion between adjacent copper wirings, enhancing insulation reliability.
The resin composition effectively prevents copper short-circuits and improves insulation reliability by forming a stable inter-wiring insulating layer with low copper diffusion, maintaining high-frequency characteristics and moisture resistance.
Smart Images

Figure 0007552676000038 
Figure 0007552676000033 
Figure 0007552676000041
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a resin composition, a wiring layer laminate for semiconductor use, and a semiconductor device. [Background technology]
[0002] In order to increase the density and performance of semiconductor packages, a packaging format has been proposed in which chips with different performance are mixed in one package. In this case, a cost-effective high-density interconnect technology between chips is becoming important (for example, see Patent Document 1).
[0003] Non-Patent Documents 1 and 2 describe a package-on-package (PoP) configuration in which a different package is connected by stacking it on top of another package using flip-chip mounting. This PoP configuration is widely adopted for smartphones, tablet terminals, etc.
[0004] Other proposed forms for mounting multiple chips at high density include packaging technology using an organic substrate with high-density wiring, fan-out type packaging technology (FO-WLP: Fan Out-Wafer Level Package) with through mold vias (TMV: Through Mold Via), packaging technology using silicon or glass interposers, packaging technology using through silicon vias (TSV: Through Silicon Via), and packaging technology using chips embedded in a substrate for inter-chip transmission.
[0005] In particular, when semiconductor chips are mounted on a wiring layer for semiconductors and in a FO-WLP, a fine wiring layer is required to electrically connect the semiconductor chips with each other at a high density (for example, see Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2012-529770 [Patent Document 2] US Patent Application Publication No. 2011 / 0221071 [Non-patent literature]
[0007] [Non-Patent Document 1] Jinseong Kim et al., "Application of Through Mold Via (TMV)asPoP Base Package", Electronic Components and Technology Conference (ECTC), p.1089-1092 (2008) [Non-Patent Document 2] SW Yoon et al., "AdvancedLow Profile PoP Solution with Embedded Wafer Level PoP (eWLB-PoP)Technology", ECTC, p.1250-1254(2012) Summary of the Invention [Problem to be solved by the invention]
[0008] A wiring layer (semiconductor wiring layer) for mounting multiple semiconductor chips may be used in build-up substrates, wafer level packages (WLPs), fan-out type PoP bottom packages, etc. For example, when fine wiring having a line width and space width of 5 μm or less is arranged in this wiring layer, the wiring is formed using a trench method. The trench method is a method of forming a metal layer that will become wiring in a trench (groove) formed by a laser or the like on the surface of an organic insulating layer by plating or the like. Therefore, the shape of the wiring formed on the organic insulating layer follows the shape of the groove.
[0009] When forming fine wiring in a wiring layer by the trench method, for example, copper having high conductivity may be used in order to reduce costs and suppress an increase in wiring resistance. When copper wiring is formed, copper may diffuse into the organic insulating layer. In this case, there is a risk of short-circuiting between copper wirings via the diffused copper, which poses a problem in the insulation reliability of the wiring layer.
[0010] An object of the present invention is to provide an inter-wiring insulating layer and a semiconductor device having good insulation reliability, and a resin composition capable of suitably forming the inter-wiring insulating layer. [Means for solving the problem]
[0011] One aspect of the present invention is a resin composition containing a curable resin and a curing agent, which is used to form a wiring interlayer insulating layer in contact with copper wiring. When the wiring interlayer insulating layer formed by this resin composition is interposed between adjacent copper wirings, the diffusion of copper from the copper wiring into the wiring layer laminate is suppressed. Therefore, short circuits between wirings having a copper number via the diffused copper are suppressed, and as a result, the insulation reliability of the wiring layer laminate can be significantly improved.
[0012] The curable resin may have at least two maleimide groups and a divalent hydrocarbon group. The hydrocarbon group may include a chain-like alkylene group having a main chain with 4 or more carbon atoms. The hydrocarbon group may have 8 or more carbon atoms. The curable resin may have a divalent organic group having at least two imide bonds. The divalent organic group may be a group represented by the following formula (I). [ka] In the formula, R 1 represents a tetravalent organic group.
[0013] The hydrocarbon group may be a group represented by formula (II): [ka] In the formula, R2 and R 3 each independently represents an alkylene group; R 4 and R 5 each independently represents an alkyl group.
[0014] The curing agent may include a photoradical polymerization initiator. The resin composition may further include a compound having a (meth)acryloyl group, and may further include a coupling agent.
[0015] The resin composition may further contain a thermoplastic resin. The concentration of chloride ions in the cured product of the resin composition may be 5 ppm or less. The breaking elongation of the cured product of the resin composition may be 5 to 200%. The storage modulus of the cured product of the resin composition at 40°C may be 10 MPa to 5 GPa. The glass transition temperature of the cured product of the resin composition may be 120 to 240°C. The dielectric constant of the cured product of the resin composition at 10 GHz may be 3.0 or less. The dielectric tangent of the cured product of the resin composition at 10 GHz may be 0.005 or less. The 5% weight loss temperature of the cured product of the resin composition may be 300°C or more.
[0016] A cured product of the resin composition may have a moisture absorption rate of 1 mass % or less after being placed in an environment of 130° C. and a relative humidity of 85% for 200 hours.
[0017] Another aspect of the present invention is a wiring layer laminate for semiconductors comprising a plurality of wiring layers including an organic insulating layer, copper wiring provided in the organic insulating layer, and a barrier metal film separating the copper wiring and the organic insulating layer, and a wiring interlayer insulating layer provided between the plurality of wiring layers, wherein a portion of the surface of the copper wiring is exposed on one or both main surfaces of the wiring layer, and the wiring interlayer insulating layer is in contact with the surface of the exposed copper wiring, and the wiring interlayer insulating layer is a layer having a moisture absorption rate of 1 mass % or less after being placed in an environment of 130°C and a relative humidity of 85% for 200 hours.
[0018] The wiring interlayer insulating layer may be a cured product of the resin composition. The organic insulating layer may be a layer formed from a photosensitive insulating resin. The barrier metal film may contain at least one selected from the group consisting of titanium, nickel, palladium, chromium, tantalum, tungsten, and gold. The dielectric constant of the wiring interlayer insulating layer when 10 GHz is applied may be 3.0 or less. The dielectric loss tangent of the wiring interlayer insulating layer when 10 GHz is applied may be 0.005 or less. The 5% weight loss temperature of the wiring interlayer insulating layer may be 300° C. or more.
[0019] Another aspect of the present invention is a semiconductor device including the above-mentioned semiconductor wiring layer laminate and a semiconductor element electrically connected to the copper wiring. Effect of the Invention
[0020] According to the present invention, it is possible to provide a wiring interlayer insulating layer and a semiconductor device having good insulation reliability, and a resin composition capable of suitably forming the wiring interlayer insulating layer. [Brief description of the drawings]
[0021] [Figure 1] 1 is a schematic cross-sectional view of a semiconductor device having a semiconductor wiring layer laminate according to an embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view of a semiconductor wiring layer laminate according to an embodiment of the present invention; [Diagram 3] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 4] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Diagram 5] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 6] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 7] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 8] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 9]1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 10] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 11] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 12] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 13] 1A to 1C are diagrams illustrating a method for manufacturing a semiconductor wiring layer laminate. [Figure 14] FIG. 14(a) is a plan view showing a sample for measurement and evaluation, and FIG. 14(b) is a cross-sectional view taken along line XIVb-XIVb in FIG. 14(a). [Figure 15] 13 is a graph showing the results of a high acceleration life test of Example 3 and Comparative Example 2. [Figure 16] FIG. 16(a) shows a general view photograph of Example 3 after the high acceleration life test, and FIG. 16(b) shows a general view photograph of Comparative Example 2 after the high acceleration life test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, the present embodiment will be described in detail with reference to the drawings. In the following description, the same or corresponding parts are given the same reference numerals, and duplicated descriptions will be omitted. Furthermore, unless otherwise specified, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to the illustrated ratios.
[0023] When terms such as "left", "right", "front", "back", "top", "bottom", "upper", "lower", "first", and "second" are used in the description and claims of this specification, they are intended to be explanatory and do not necessarily mean that they are in this relative position forever. Furthermore, "layer" and "film" include structures that are formed on the entire surface as well as structures that are formed on a part of the surface when observed in a plan view. Furthermore, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. Furthermore, a numerical range indicated using "~" indicates a range that includes the numerical values described before and after "~" as the minimum and maximum values, respectively. Furthermore, in the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage may be replaced with the upper limit or lower limit of a numerical range of another stage.
[0024] The resin composition according to one embodiment contains a curable resin and a curing agent. The curable resin is a compound that is cured by heat or light. That is, the resin composition is a photocurable (photosensitive) resin composition that is cured by light, or a thermosetting resin composition that is cured by heat. The resin composition is suitably used to form a wiring interlayer insulating layer that contacts a copper wiring. In this specification, the copper wiring means a wiring that contains at least copper. The copper wiring may be a wiring made of only copper, or may be a wiring that further contains other components such as nickel, titanium, and palladium in addition to copper.
[0025] In one embodiment (hereinafter referred to as "first embodiment"), the curable resin is a maleimide compound having at least two maleimide groups and a divalent hydrocarbon group (hereinafter also simply referred to as "maleimide compound").
[0026] The maleimide compound has at least two maleimide groups represented by, for example, the following formula (III). [ka]
[0027] The maleimide compound is, for example, a compound represented by the following formula (IV) (bismaleimide compound). [ka] In the formula, X is a divalent linking group containing a divalent hydrocarbon group.
[0028] The divalent hydrocarbon group contained in the linking group represented by X may be either a saturated hydrocarbon group or an unsaturated hydrocarbon group. The divalent hydrocarbon group may be either a chain or a cyclic group, and the chain divalent hydrocarbon group may be either a straight chain or a branched chain. The cyclic unsaturated hydrocarbon group may be an aromatic group. The divalent hydrocarbon group may contain two or more of these groups.
[0029] From the viewpoint of enabling an improvement in the flexibility of the resin composition and the handleability (resistance to tack, cracking, powder falling, etc.) and strength of a film produced from the resin composition, the divalent hydrocarbon group preferably contains a chain-like hydrocarbon group, and more preferably contains a chain-like alkylene group having a main chain with 4 or more carbon atoms.
[0030] A chain-like alkylene group having a main chain of 4 or more carbon atoms is -(CR a R b ) m - (m is an integer of 4 or more, R a and R b each independently represents a hydrogen atom or an alkyl group having less than m carbon atoms. The number of carbon atoms (m) in the main chain of the alkylene group is preferably 4 or more or 6 or more, and preferably 20 or less, 15 or less, or 10 or less.
[0031] The number of carbon atoms of the divalent hydrocarbon group is preferably 8 or more, 10 or more, or 15 or more, from the viewpoint of easily making the molecular structure of the maleimide compound three-dimensional and increasing the free volume of the polymer to lower the density, i.e., to lower the dielectric constant, and is preferably 300 or less, 250 or less, 200 or less, 100 or less, 70 or less, or 50 or less. From the same viewpoint, the number of carbon atoms of the divalent hydrocarbon group may be preferably 8 to 300, 8 to 250, 8 to 200, or 8 to 100. The divalent hydrocarbon group is preferably an alkylene group having 8 to 300, 8 to 250, 8 to 200, or 8 to 100 carbon atoms which may have a branch, more preferably an alkylene group having 10 to 70 carbon atoms which may have a branch, and even more preferably an alkylene group having 15 to 50 carbon atoms which may have a branch.
[0032] In one embodiment, from the viewpoint of more effectively improving high frequency characteristics and HAST (Highly Accelerated Temperature and Humidity Stress Test) resistance, the divalent hydrocarbon group is a group represented by the following formula (II). [ka] In the formula, R 2 and R 3 each independently represents an alkylene group; R 4 and R 5 each independently represents an alkyl group.
[0033] R 2 and R 3 From the viewpoints of further improving flexibility and easiness of synthesis, the number of carbon atoms in the alkylene group represented by R is preferably 4 to 50, more preferably 5 to 25, still more preferably 6 to 10, and particularly preferably 7 to 10. 2 and R 3 The alkylene group represented by the following formula (I) is preferably a chain-like alkylene group having a main chain having 4 or more carbon atoms as described above.
[0034] R 4From the viewpoints of further improving flexibility and easiness of synthesis, the number of carbon atoms in the alkyl group represented by R is preferably 4 to 50, more preferably 5 to 25, still more preferably 6 to 10, and particularly preferably 7 to 10. 5 From the viewpoints of further improving flexibility and ease of synthesis, the alkylene group represented by the following formula (I) preferably has 2 to 50 carbon atoms, more preferably 3 to 25 carbon atoms, further preferably 4 to 10 carbon atoms, and particularly preferably 5 to 8 carbon atoms.
[0035] From the viewpoint of more effectively increasing the high frequency characteristics and the elongation, the maleimide compound preferably has a plurality of divalent hydrocarbon groups. In this case, the plurality of divalent hydrocarbon groups may be the same or different. The maleimide compound preferably has 2 to 40 divalent hydrocarbon groups, more preferably 2 to 20 divalent hydrocarbon groups, and even more preferably 2 to 10 divalent hydrocarbon groups.
[0036] The divalent hydrocarbon group may be, for example, an alkylene group such as a nonylene group, a decylene group, an undecylene group, a dodecylene group, a tetradecylene group, a hexadecylene group, an octadecylene group, a nonadecylene group, an icosilene group, a henicosilene group, a docosilene group, a tricosilene group, a tetracosilene group, a pentacosilene group, a hexacosilene group, a heptacosilene group, an octacosilene group, a nonacosilene group, or a triacontylene group; an arylene group such as a benzylene group, a phenylene group, or a naphthylene group; an arylene alkylene group such as a phenylenemethylene group, a phenyleneethylene group, a benzylpropylene group, a naphthylenemethylene group, or a naphthyleneethylene group; or an arylene dialkylene group such as a phenylenedimethylene group or a phenylenediethylene group.
[0037] The linking group represented by X may consist only of the divalent hydrocarbon group, or may contain other organic groups in addition to the divalent hydrocarbon group. The other organic groups are, for example, divalent organic groups having at least two imide bonds.
[0038] The divalent organic group having at least two imide bonds may be, for example, a group represented by the following formula (I). [ka] In the formula, R 1 represents a tetravalent organic group.
[0039] R 1 From the viewpoint of handleability, the tetravalent organic group represented by the following formula may be a hydrocarbon group. The number of carbon atoms in the hydrocarbon group may be, for example, 1 to 100, 2 to 50, or 4 to 30.
[0040] The hydrocarbon group may be substituted and may include, for example, a substituted or unsubstituted siloxane group such as those derived from dimethylsiloxane, methylphenylsiloxane, diphenylsiloxane, and the like.
[0041] Examples of the substituent include an alkyl group, an alkenyl group, an alkynyl group, a hydroxyl group, an alkoxy group, a mercapto group, a cycloalkyl group, a substituted cycloalkyl group, a heterocyclic group, a substituted heterocyclic group, an aryl group, a substituted aryl group, a heteroaryl group, a substituted heteroaryl group, an aryloxy group, a substituted aryloxy group, a halogen atom, a haloalkyl group, a cyano group, a nitro group, a nitroso group, an amino group, an amido group, -C(O)H, -C(O)-, -S-, -S(O)2-, -OC(O)-O-, and -C(O)-NR c , -NR c C(O)-N(R c )2, -OC(O)-N(R c 2) may be an acyl group, an oxyacyl group, a carboxyl group, a carbamate group, a sulfonyl group, a sulfonamide group, a sulfuryl group, etc. c represents a hydrogen atom or an alkyl group. One or more of these substituents can be selected according to the purpose, application, etc.
[0042] R 1The tetravalent organic group represented by the formula (I) may be, for example, a tetravalent residue of an acid anhydride having two or more anhydride rings in one molecule, that is, a tetravalent group obtained by removing two acid anhydride groups (-CO(=O)OC(=O)-) from an acid anhydride. Examples of acid anhydrides include compounds described below.
[0043] R 1 From the viewpoint of excellent high frequency characteristics, the organic group represented by the formula (V) is preferably a tetravalent aromatic group, and more preferably a residue obtained by removing two acid anhydride groups from pyromellitic anhydride. The divalent organic group having at least two imide bonds is preferably a group represented by the formula (V) below. [ka]
[0044] From the viewpoint of excellent dielectric properties, the divalent organic group having at least two imide bonds may be a group represented by the following formula (VI) or (VII). [ka] [ka]
[0045] From the viewpoints of excellent high frequency characteristics and excellent compatibility with other resins when the resin composition further contains other resins (particularly high molecular weight thermoplastic elastomer resins), the maleimide compound preferably has a plurality of divalent organic groups having at least two imide bonds. In this case, the divalent organic groups may be the same or different from each other. The maleimide compound preferably has 2 to 40, more preferably 2 to 20, and even more preferably 2 to 10 divalent organic groups.
[0046] More specifically, in one embodiment, the maleimide compound may be, for example, a compound represented by the following formula (VIII) or a compound represented by the following formula (IX). [ka] [ka] In the formula, Z 1 , Z 2 and Z 3 each independently represents the divalent hydrocarbon group described above, R 1 has the same meaning as R1 in formula (I), and n represents an integer of 1 to 10. When n is 2 or more, a plurality of Z 3 may be the same or different from each other.
[0047] The maleimide compound can be used by, for example, purchasing a commercially available product. Examples of commercially available products include BMI-TMH, BMI-1000, BMI-1000H, BMI-1100, BMI-1100H, BMI-2000, BMI-2300, BMI-3000, BMI-3000H, BMI-4000, BMI-5100, BMI-7000, BMI-7000H (all trade names, manufactured by Daiwa Kasei Kogyo Co., Ltd.), BMI, BMI-70, BMI-80 (all trade names, manufactured by K.I. Kasei Co., Ltd.), etc., which are maleimide compounds represented by formula (VIII). Commercially available products include, for example, BMI-1500, BMI-1700, BMI-3000, BMI-5000 and BMI-9000 (all trade names, manufactured by Designer Molecules Inc. (DMI)), which are maleimide compounds represented by formula (IX).
[0048] The molecular weight of the maleimide compound is not particularly limited. The weight average molecular weight Mw of the maleimide compound may be 1000 or more, 1500 or more, or 3000 or more, and may be 30000 or less, 20000 or less, or 15000 or less. The weight average molecular weight Mw of the maleimide compound is preferably 1000 to 30000, more preferably 1500 to 20000, from the viewpoints of solubility in a solvent and compatibility with other components such as monomers and resins.
[0049] The weight-average molecular weight Mw of the maleimide compound can be measured by gel permeation chromatography (GPC) under the following conditions. Pump: L-6200 type [manufactured by Hitachi High-Technologies Corporation] Detector: L-3300 type RI [Hitachi High-Technologies Corporation] Column oven: L-655A-52 [Hitachi High-Technologies Corporation] Guard column and column: TSK Guardcolumn HHR-L + TSKgel G4000HHR + TSKgel G2000HHR [all manufactured by Tosoh Corporation, product names] Column size: 6.0 x 40 mm (guard column), 7.8 x 300 mm (column) Eluent: Tetrahydrofuran Sample concentration: 30mg / 5mL Injection volume: 20μL Measurement temperature: 40℃
[0050] The content of the maleimide compound may be, for example, 50 mass% or more, 65 mass% or more, or 80 mass% or more, and may be 99 mass% or less, 95 mass% or less, or 90 mass% or less, based on the total amount of solids in the resin composition.
[0051] The curing agent according to the first embodiment may contain a photoradical polymerization initiator. That is, in one embodiment, the resin composition contains a maleimide compound and a photoradical polymerization initiator.
[0052] The photoradical polymerization initiator may be, for example, an alkylphenone-based photoradical polymerization initiator, an acylphosphine oxide-based photoradical polymerization initiator, or the like.
[0053] Alkylphenone-based photoradical polymerization initiators can be purchased, for example, from BASF as Irgacure 651, Irgacure 184, DAROCURE 1173, Irgacure 2959, Irgacure 127, DAROCURE MBF, Irgacure 907, Irgacure 369, Irgacure 379 EG, etc. Acylphosphine oxide-based photoradical polymerization initiators can be purchased, for example, from BASF as Irgacure 819, LUCIRINTPO, etc.
[0054] The photoradical polymerization initiator may be other photoradical polymerization initiators available commercially as Irgacure784, IrgacureOXE01, IrgacureOXE02, Irgacure754, and the like, manufactured by BASF.
[0055] As the photoradical polymerization initiator, from the viewpoint of high sensitivity, preferably, Irgacure907, Irgacure369, Irgacure379EG, IrgacureOXE01, and IrgacureOXE02 are preferably used, and from the viewpoint of solubility in a solvent, Irgacure907, Irgacure379EG, and IrgacureOXE02 are more preferably used. These photoradical polymerization initiators may be used alone or in combination of two or more types according to the purpose, application, etc.
[0056] The content of the photoradical polymerization initiator is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the curable resin in order to sufficiently cure the curable resin, and more preferably 1 to 6 parts by mass in order to further reduce the likelihood of unreacted substances remaining.
[0057] The resin composition according to the first embodiment may further contain a compound having a (meth)acryloyl group (hereinafter also referred to as "(meth)acryloyl compound"). That is, in one embodiment, the resin composition contains a maleimide compound, a (meth)acryloyl compound, and a curing agent (photoradical polymerization initiator). Note that a coupling agent having a (meth)acryloyl group, which will be described later, is not included in the (meth)acryloyl compound.
[0058] The (meth)acryloyl compound may be, for example, tricyclodecane dimethanol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, propoxylated ethoxylated bisphenol A (meth)acrylate, dipentaerythritol poly(meth)acrylate, ethoxylated isocyanuric acid tri(meth)acrylate, polyethylene glycol di(meth)acrylate, a silsesquioxane derivative having a (meth)acryloyl group, or the like.
[0059] From the viewpoint of excellent heat resistance, the (meth)acryloyl compound is preferably tricyclodecane dimethanol di(meth)acrylate, ethoxylated bisphenol A di(meth)acrylate, propoxylated ethoxylated bisphenol A (meth)acrylate, or a silsesquioxane derivative having a (meth)acryloyl group, and from the viewpoint of excellent compatibility with the maleimide compound, it is more preferably tricyclodecane dimethanol di(meth)acrylate.
[0060] The content of the (meth)acryloyl compound is preferably 0.1 to 98 parts by mass, when the total of the maleimide compound and the (meth)acryloyl compound is 100 parts by mass, and from the viewpoint of obtaining a good elongation percentage, it is more preferably 2 to 50 parts by mass, and from the viewpoint of achieving both high frequency properties and fine wiring formability, it is even more preferably 5 to 40 parts by mass.
[0061] The resin composition according to the first embodiment may further contain a coupling agent. That is, in one embodiment, the resin composition contains a maleimide compound, a curing agent (photoradical polymerization initiator), and a coupling agent, and in another embodiment, the resin composition contains a maleimide compound, a (meth)acryloyl compound, a curing agent (photoradical polymerization initiator), and a coupling agent.
[0062] The coupling agent may be, for example, a silane coupling agent, which may have, for example, a vinyl group, an epoxy group, a styryl group, an acryloyl group, a methacryloyl group, an amino group, a ureido group, an isocyanate group, an isocyanurate group, or a mercapto group.
[0063] Examples of silane coupling agents having a vinyl group include KBM-1003 and KBE-1003 (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.; the same applies below). Examples of silane coupling agents having an epoxy group include KBM-303, 402, 403, KBE-402, 403, X-12-981S, and X-12-984S. Examples of silane coupling agents having a styryl group include KBM-1403. Examples of silane coupling agents having a methacryloyl group include KBM-502, 503, KBE-502, and 503. Examples of silane coupling agents having an acryloyl group include KBM-5103, X-12-1048, and X-12-1050. Examples of silane coupling agents having an amino group include KBM-602, 603, 903, 573, 575, KBE-903, 9103P, and X-12-972F. Examples of silane coupling agents having an ureido group include KBE-585. Examples of silane coupling agents having an isocyanate group include KBE-9007 and X-12-1159L. Examples of silane coupling agents having an isocyanurate group include KBM-9659. Examples of silane coupling agents having a mercapto group include KBM-802, 803, X-12-1154, and X-12-1156. These may be used alone or in combination of two or more types according to the purpose, application, etc.
[0064] The content of the silane coupling agent is preferably 0.01 to 5 parts by mass relative to 100 parts by mass of the curable resin from the viewpoint of improving adhesion to glass, silica, etc., and more preferably 0.1 to 2 parts by mass from the viewpoint of further reducing the likelihood of unreacted substances remaining.
[0065] The resin composition according to the first embodiment may further contain a thermosetting resin as a curable resin in addition to the maleimide compound. Examples of the thermosetting resin include epoxy resin, phenol resin, cyanate resin, isocyanate resin, benzoxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, dicyclopentadiene resin, silicone resin, triazine resin, and melamine resin. These may be used alone or in combination of two or more. From the viewpoint of heat resistance and electrical insulation, the thermosetting resin is preferably an epoxy resin or a cyanate resin.
[0066] Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, bisphenol A novolac type epoxy resins, bisphenol F novolac type epoxy resins, stilbene type epoxy resins, triazine skeleton-containing epoxy resins, fluorene skeleton-containing epoxy resins, biphenyl type epoxy resins, xylylene type epoxy resins, biphenyl aralkyl type epoxy resins, naphthalene type epoxy resins, dicyclopentadiene type epoxy resins, alicyclic epoxy resins, polyfunctional phenols and diglycidyl ether compounds of polycyclic aromatics such as anthracene, and phosphorus-containing epoxy resins obtained by introducing phosphorus compounds into these. The epoxy resin is a biphenyl aralkyl type epoxy resin or a naphthalene type epoxy resin from the viewpoint of heat resistance and flame retardancy. These may be used alone or in combination of two or more.
[0067] Examples of the cyanate resin include bisphenol-type cyanate resins such as novolac-type cyanate resins, bisphenol A-type cyanate resins, bisphenol E-type cyanate resins, and tetramethylbisphenol F-type cyanate resins, and prepolymers of these partially triazine-converted cyanate resins. These may be used alone or in combination of two or more. From the viewpoints of heat resistance and flame retardancy, the cyanate resin is preferably a novolac-type cyanate resin.
[0068] The resin composition according to the first embodiment may further contain other curing agents as a curing agent in addition to the photoradical polymerization initiator. Examples of other curing agents include aromatic amine compounds such as dicyandiamide, 4,4'-diaminodiphenylmethane, 4,4'-diamino-3,3'-diethyl-diphenylmethane, 4,4'-diaminodiphenylsulfone, phenylenediamine, and xylenediamine, aliphatic amine compounds such as hexamethylenediamine and 2,5-dimethylhexamethylenediamine, and guanamine compounds such as melamine and benzoguanamine. The other curing agent is preferably an aromatic amine compound from the viewpoint of obtaining good reactivity and heat resistance.
[0069] When the resin composition contains a cyanate resin, the resin composition may further contain, as a curing agent, a polyfunctional phenol compound such as phenol novolac, cresol novolac, or aminotriazine novolac resin, or an acid anhydride such as phthalic anhydride, pyromellitic anhydride, maleic anhydride, or maleic anhydride copolymer, etc. These may be used alone or in combination of two or more.
[0070] The resin composition according to the first embodiment may further contain a thermoplastic elastomer. Examples of the thermoplastic elastomer include styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, acrylic elastomers, silicone-based elastomers, and derivatives thereof. Thermoplastic elastomers are composed of hard segment components and soft segment components, and the former generally contributes to heat resistance and strength, while the latter generally contributes to flexibility and toughness. From the viewpoint of further improving heat resistance and insulation reliability, the thermoplastic elastomer is preferably a styrene-based elastomer, an olefin-based elastomer, a polyamide-based elastomer, or a silicone-based elastomer. These can be used alone or in combination of two or more.
[0071] The thermoplastic elastomer may have a reactive functional group at the molecular end or in the molecular chain. Examples of the reactive functional group include an epoxy group, a hydroxyl group, a carboxyl group, an amino group, an amide group, an isocyanato group, an acryloyl group, a methacryloyl group, and a vinyl group. When the thermoplastic elastomer has these reactive functional groups at the molecular end or in the molecular chain, the compatibility with the curable resin is improved, and the internal stress generated during the curing of the resin composition can be more effectively reduced, and as a result, the warpage of the substrate can be significantly reduced. From the viewpoint of adhesion to metal, the reactive functional group is preferably an epoxy group, a hydroxyl group, a carboxyl group, an amino group, or an amide group, and from the viewpoint of further improving heat resistance and insulation reliability, it is more preferably an epoxy group, a hydroxyl group, or an amino group.
[0072] From the viewpoint of effectively achieving low shrinkage and low thermal expansion properties of the cured product, the content of the thermoplastic elastomer is preferably 0.1 to 50 parts by mass, and more preferably 2 to 30 parts by mass, per 100 parts by mass of the total solid content in the resin composition.
[0073] In one embodiment (hereinafter also referred to as "second embodiment"), the resin composition further contains a thermoplastic resin in addition to the curable resin and the curing agent. In this case, the curable resin is preferably a thermosetting resin. That is, the resin composition according to the second embodiment contains a thermoplastic resin, a thermosetting resin, and a curing agent.
[0074] The thermoplastic resin is not particularly limited as long as it is a resin that is softened by heating. The thermoplastic resin may have a reactive functional group at the molecular end or in the molecular chain. Examples of the reactive functional group include an epoxy group, a hydroxyl group, a carboxyl group, an amino group, an amide group, an isocyanato group, an acryloyl group, a methacryloyl group, a vinyl group, and a maleic anhydride group.
[0075] The thermoplastic resin includes, for example, a resin having a siloxane chain from the viewpoint of suppressing its moisture absorption and dielectric constant. Examples of the thermoplastic resin having a siloxane include a siloxane-containing acrylic resin, a siloxane-containing polyamide resin, a siloxane-containing polyimide, a siloxane-containing polyurethane, a siloxane-modified acrylate, a siloxane-modified epoxy, a silicone resin, and a silicone diamine. From the viewpoint of suppressing outgassing during heating and improving the heat resistance and adhesiveness of the wiring interlayer insulating layer, the thermoplastic resin having a siloxane chain is preferably a polyimide having a siloxane chain (a siloxane-containing polyimide).
[0076] Siloxane-containing polyimides can be synthesized, for example, by reacting a siloxane diamine with a tetracarboxylic dianhydride, or by reacting a siloxane diamine with a bismaleimide.
[0077] The siloxane diamine preferably has a structure represented by the following formula (5). [ka] In the formula, Q 4 and Q 9 each independently represents an alkylene group having 1 to 5 carbon atoms or a phenylene group which may have a substituent; Q 5 , Q 6 , Q 7 and Q 8 each independently represents an alkyl group having 1 to 5 carbon atoms, a phenyl group or a phenoxy group; and d represents an integer of 1 to 5.
[0078] Examples of siloxane diamines in which d in formula (5) is 1 include 1,1,3,3-tetramethyl-1,3-bis(4-aminophenyl)disiloxane, 1,1,3,3-tetraphenoxy-1,3-bis(4-aminoethyl)disiloxane, 1,1,3,3-tetraphenyl-1,3-bis(2-aminoethyl)disiloxane, and 1,1,3,3-tetraphenyl-1,3-bis(3-aminopropane). Examples of the disiloxane include 1,1,3,3-tetramethyl-1,3-bis(2-aminoethyl)disiloxane, 1,1,3,3-tetramethyl-1,3-bis(3-aminopropyl)disiloxane, 1,1,3,3-tetramethyl-1,3-bis(3-aminobutyl)disiloxane, and 1,3-dimethyl-1,3-dimethoxy-1,3-bis(4-aminobutyl)disiloxane.
[0079] Examples of siloxane diamines in which d in formula (5) is 2 include 1,1,3,3,5,5-hexamethyl-1,5-bis(4-aminophenyl)trisiloxane, 1,1,5,5-tetraphenyl-3,3-dimethyl-1,5-bis(3-aminopropyl)trisiloxane, 1,1,5,5-tetraphenyl-3,3-dimethoxy-1,5-bis(4-aminobutyl)trisiloxane, 1,1,5,5-tetraphenyl-3,3-dimethoxy-1,5-bis(5-aminopentyl)trisiloxane, 1,1,5,5-tetramethyl-3,3-dimethoxy-1,5-bis(2 -aminoethyl)trisiloxane, 1,1,5,5-tetramethyl-3,3-dimethoxy-1,5-bis(4-aminobutyl)trisiloxane, 1,1,5,5-tetramethyl-3,3-dimethoxy-1,5-bis(5-aminopentyl)trisiloxane, 1,1,3,3,5,5-hexamethyl-1,5-bis(3-aminopropyl)trisiloxane, 1,1,3,3,5,5-hexaethyl-1,5-bis(3-aminopropyl)trisiloxane, 1,1,3,3,5,5-hexapropyl-1,5-bis(3-aminopropyl)trisiloxane, and the like.
[0080] Commercially available siloxane diamines include, for example, "PAM-E" (amino group equivalent: 130 g / mol) having amino groups at both ends, "KF-8010" (amino group equivalent: 430 g / mol), "X-22-161A" (amino group equivalent: 800 g / mol), "X-22-161B" (amino group equivalent: 1500 g / mol), "KF-8012" (amino group equivalent: 2200 g / mol), "KF-8008" (amino group equivalent: 5700 g / mol), and "X-22- Examples of the siloxane diamine include "BY-16-853U" (amino group equivalent: 460 g / mol), "BY-16-853" (amino group equivalent: 650 g / mol), and "BY-16-853B" (amino group equivalent: 2200 g / mol) (all manufactured by Dow Corning Toray Co., Ltd.). The above-mentioned siloxane diamines may be used alone or in combination of two or more. From the viewpoint of reactivity with maleimide groups, it is preferable to use at least one of "PAM-E", "KF-8010", "X-22-161A", "X-22-161B", "BY-16-853U", and "BY-16-853". From the viewpoint of dielectric properties, it is more preferable to use at least one of "PAM-E", "KF-8010", "X-22-161A", "BY-16-853U", and "BY-16-853". From the viewpoint of compatibility with varnish, it is preferable to use at least one of "KF-8010", "X-22-161A", and "BY-16-853".
[0081] The content of the siloxane component in the siloxane-containing polyimide is not particularly limited, but is, for example, 5 to 50 mass % relative to the total mass of the polyimide from the viewpoints of reactivity and compatibility, preferably 5 to 30 mass % from the viewpoint of heat resistance, and more preferably 10 to 30 mass % from the viewpoint of further reducing the moisture absorption rate of the wiring interlayer insulating layer.
[0082] The other diamine components used as raw materials for polyimide are not particularly limited, and examples thereof include o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether methane, bis(4-amino-3,5-dimethylphenyl)methane, bis(4- Amino-3,5-diisopropylphenyl)methane, 3,3'-diaminodiphenyl difluoromethane, 3,4'-diaminodiphenyl difluoromethane, 4,4'-diaminodiphenyl difluoromethane, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl ketone, 3,4'-diaminodiphenyl ketone, 4,4'-diaminodiphenyl ketone, 2,2-bis(3-aminophenyl)propane, 2,2'-(3,4'-diaminodiphenyl)propane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)hexafluoropropane, 2,2-(3,4'-diaminodiphenyl)hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, 1,3-bis(3-aminophenoxy)benzene, 1, 4-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 3,3'-(1,4-phenylenebis(1-methylethylidene))bisaniline, 3,4'-(1,4-phenylenebis(1-methylethylidene))bisaniline, 4,4'-(1,4-phenylenebis(1-methylethylidene))bisaniline, 2,2-bis(4-(3-aminophenoxy)phenyl)propane, 2,2-bis(4-(3-aminophenoxy)phenyl)hexafluoropropane, 2,Examples of the aromatic diamines include 2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane, bis(4-(3-aminophenoxy)phenyl)sulfide, bis(4-(4-aminophenoxy)phenyl)sulfide, bis(4-(3-aminophenoxy)phenyl)sulfone, bis(4-(4-aminophenoxy)phenyl)sulfone, 3,3'-dihydroxy-4,4'-diaminobiphenyl, and 3,5-diaminobenzoic acid, 1,3-bis(aminomethyl)cyclohexane, 2,2-bis(4-aminophenoxyphenyl)propane, aliphatic ether diamines represented by the following formula (4), aliphatic diamines represented by the following formula (11), and diamines having a carboxyl group and / or a hydroxyl group in the molecule.
[0083] [ka] In the formula, Q 1 , Q 2 and Q 3 each independently represents an alkylene group having 1 to 10 carbon atoms; and b represents an integer of 2 to 80.
[0084] [ka] In the formula, c represents an integer of 5 to 20.
[0085] Examples of the aliphatic ether diamine represented by formula (4) include those represented by the following formula: [ka] In the formula, n represents an integer of 1 or more. and aliphatic ether diamines represented by the following formula (12). [ka] In the formula, e represents an integer of 0 to 80.
[0086] Specific examples of the aliphatic diamine represented by formula (11) include 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 1,7-diaminoheptane, 1,8-diaminooctane, 1,9-diaminononane, 1,10-diaminodecane, 1,11-diaminoundecane, 1,12-diaminododecane, and 1,2-diaminocyclohexane.
[0087] The above diamine components may be used alone or in combination of two or more.
[0088] As a raw material for polyimide, for example, tetracarboxylic dianhydride may be used. The acid anhydride is not particularly limited, and examples thereof include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, and bis(2,3-dicarboxyphenyl)methane dianhydride. , bis(3,4-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, benzene-1,2,3,4-tetracarboxylic dianhydride, 3,4,3',4'-benzophenonetetracarboxylic dianhydride, 2,3,2',3'-benzophenonetetracarboxylic dianhydride, 3,3,3',4'-benzophenonetetracarboxylic dianhydride, 1,2,5,6-naphthalene Tetracarboxylic dianhydrides, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,4,5-naphthalenetetracarboxylic dianhydride, 2,6-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,7-dichloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 2,3,6,7-tetrachloronaphthalene-1,4,5,8-tetracarboxylic dianhydride, phenanthrene-1,8,9,10-tetracarboxylic dianhydride, pyrazine -2,3,5,6-tetracarboxylic dianhydride, thiophene-2,3,5,6-tetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 3,4,3',4'-biphenyltetracarboxylic dianhydride, 2,3,2',3'-biphenyltetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)dimethylsilane dianhydride, bis(3,4-dicarboxyphenyl)methylphenylsilane dianhydride, bis(3,4-dicarboxyphenyl)diphenylsilane dianhydride, 1,4-bis(3,4-dicarboxyphenyldimethylsilyl)benzene dianhydride, 1,3-bis(3,4-dicarboxyphenyl)-1,1,3,3-tetramethyldicyclohexane dianhydride, p-phenylene bis(trimellitate anhydride), ethylene tetracarboxylic dianhydride, 1,2,3,4-butane tetracarboxylic dianhydride, decahydronaphthalene-1,4,5,8-tetracarboxylic dianhydride, 4,8-dimethyl-1,2,3,5,6,7-hexa Hydronaphthalene-1,2,5,6-tetracarboxylic dianhydride, cyclopentane-1,2,3,4-tetracarboxylic dianhydride, pyrrolidine-2,3,4,5-tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, bis(exo-bicyclo[2,2,1]heptane-2,3-dicarboxylic dianhydride, bicyclo-[2,2,2]-oct-7-ene-2,3,5,6-tetracarboxylic dianhydride, 2,2-bi Examples of the dianhydride include bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenyl)phenyl]propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, 2,2-bis[4-(3,4-dicarboxyphenyl)phenyl]hexafluoropropane dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 1,4-bis(2-hydroxyhexafluoroisopropyl)benzene bis(trimellitic anhydride), 1,3-bis(2-hydroxyhexafluoroisopropyl)benzene bis(trimellitic anhydride), 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, tetrahydrofuran-2,3,4,5-tetracarboxylic dianhydride, and tetracarboxylic dianhydride represented by the following formula (7). [ka] In the formula, a represents an integer of 2 to 20.
[0089] The tetracarboxylic dianhydride represented by formula (7) can be synthesized, for example, from trimellitic anhydride monochloride and a corresponding diol. Specific examples of the tetracarboxylic dianhydride represented by formula (7) include 1,2-(ethylene)bis(trimellitate anhydride), 1,3-(trimethylene)bis(trimellitate anhydride), 1,4-(tetramethylene)bis(trimellitate anhydride), 1,5-(pentamethylene)bis(trimellitate anhydride), 1,6-(hexamethylene)bis(trimellitate anhydride), 1,7-(heptamethylene)bis(trimellitate anhydride), and the like. Examples of such anhydrides include 1,8-(octamethylene)bis(trimellitate anhydride), 1,9-(nonamethylene)bis(trimellitate anhydride), 1,10-(decamethylene)bis(trimellitate anhydride), 1,12-(dodecamethylene)bis(trimellitate anhydride), 1,16-(hexadecamethylene)bis(trimellitate anhydride), and 1,18-(octadecamethylene)bis(trimellitate anhydride).
[0090] The tetracarboxylic dianhydride may contain a tetracarboxylic dianhydride represented by the following formula (6) or (8) from the viewpoint of imparting good solubility in a solvent in the resin composition and moisture resistance reliability. [ka] [ka]
[0091] The above-mentioned tetracarboxylic dianhydrides may be used alone or in combination of two or more.
[0092] As a raw material for polyimide, for example, bismaleimide may be used. The bismaleimide is not particularly limited, but examples thereof include bis(4-maleimidophenyl)methane, polyphenylmethane maleimide, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, m-phenylene bismaleimide, and 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane.
[0093] The above-mentioned bismaleimides may be used alone or in combination of two or more. From the viewpoint of high reactivity and further improving dielectric properties and wiring properties, the bismaleimide is preferably at least one of bis(4-maleimidophenyl)methane, bis(4-maleimidophenyl)sulfone, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, and 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane. From the viewpoint of solubility in a solvent, the bismaleimide is preferably at least one of 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, bis(4-maleimidophenyl)methane, and 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane. From the viewpoint of low cost, the bismaleimide is preferably bis(4-maleimidophenyl)methane. From the viewpoint of wireability, the bismaleimide is preferably 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane or "BMI-3000" (trade name) manufactured by Designer Molecules Inc.
[0094] The content of the thermoplastic resin may be 10% by mass to 70% by mass based on the mass of the resin composition (excluding the filler).
[0095] The thermosetting resin is not particularly limited as long as it reacts with the curing agent by heating to cure the resin composition. The thermosetting resin may have a reactive functional group at the molecular end or in the molecular chain. Examples of the reactive functional group include an epoxy group, a hydroxyl group, a carboxyl group, an amino group, an amide group, an isocyanate group, an acryloyl group, a methacryloyl group, a vinyl group, and a maleic anhydride group.
[0096] The thermosetting resin is preferably a thermosetting elastomer selected from styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, acrylic elastomers, and silicone-based elastomers. These thermosetting elastomers are composed of a hard segment component and a soft segment component. In general, the former contributes to the heat resistance and strength of the resin, and the latter contributes to the flexibility and toughness of the resin. The thermosetting elastomer may be used alone or in combination of two or more types. From the viewpoint of further improving the heat resistance and insulation reliability of the wiring interlayer insulating layer, the thermosetting elastomer is preferably at least one of styrene-based elastomers, olefin-based elastomers, polyamide-based elastomers, and silicone-based elastomers, and from the viewpoint of the dielectric properties of the wiring interlayer insulating layer, it is more preferably at least one of styrene-based elastomers and olefin-based elastomers.
[0097] The thermosetting elastomer may have a reactive functional group at the molecular end or in the molecular chain. Examples of the reactive functional group include an epoxy group, a hydroxyl group, a carboxyl group, an amino group, an amide group, an isocyanato group, an acryloyl group, a methacryloyl group, a vinyl group, and a maleic anhydride group. From the viewpoints of compatibility and wireability, the reactive functional group is preferably an epoxy group, an amino group, an acryloyl group, a methacryloyl group, a vinyl group, or a maleic anhydride group, and more preferably an epoxy group, an amino group, or a maleic anhydride group.
[0098] The content of the thermosetting elastomer is, for example, 10% by mass to 70% by mass based on the mass of the resin composition (excluding the filler), and from the viewpoints of dielectric properties and compatibility with the varnish, is preferably 20% by mass to 60% by mass.
[0099] Examples of the curing agent include peroxides, imidazoles and derivatives thereof, organic phosphorus compounds, secondary amines, tertiary amines, quaternary ammonium salts, etc. From the viewpoint of reactivity, the curing agent is preferably at least one of peroxides, phosphorus, and imidazoles, and from the viewpoint of good self-polymerization of the maleimide group, it is more preferably a peroxide.
[0100] The content of the curing agent may vary depending on the type of catalyst and resin, or the application to which the resin composition is applied. For example, when the curing agent is a peroxide-based agent, the content of the curing agent is preferably 0.1% by mass to 10% by mass based on the mass of the resin composition (excluding the filler), and from the viewpoint of dielectric properties and film handling properties, is more preferably 0.5% by mass to 5% by mass, and even more preferably 0.75% by mass to 3% by mass.
[0101] The resin composition according to the second embodiment may contain an epoxy resin as a thermosetting resin. The epoxy resin preferably contains at least two or more epoxy groups in the molecule. From the viewpoint of curability and cured product properties, the epoxy resin is more preferably a phenol glycidyl ether type epoxy resin. Examples of such resins include glycidyl ether of bisphenol A type (or AD type, S type, F type), glycidyl ether of water-added bisphenol A type, glycidyl ether of ethylene oxide adduct bisphenol A type, glycidyl ether of propylene oxide adduct bisphenol A type, glycidyl ether of phenol novolac resin, glycidyl ether of cresol novolac resin, glycidyl ether of bisphenol A novolac resin, glycidyl ether of naphthalene resin, trifunctional (or tetrafunctional) glycidyl ether, glycidyl ether of dicyclopentadiene phenol resin, glycidyl ester of dimer acid, trifunctional (or tetrafunctional) glycidyl amine, glycidyl amine of naphthalene resin, and the like. The epoxy resin may be used alone or in combination of two or more kinds.
[0102] The resin composition according to the second embodiment may contain a (meth)acrylate compound. Examples of the (meth)acrylate compound include diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, trimethylolpropane diacrylate, trimethylolpropane triacrylate, trimethylolpropane dimethacrylate, trimethylolpropane trimethacrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, pentaerythritol trimeth ...acrylate, pentaerythritol trimethacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pentaerythritol triacrylate, pen Examples of the monomer unit include taerythritol tetramethacrylate, dipentaerythritol hexaacrylate, dipentaerythritol hexamethacrylate, styrene, divinylbenzene, 4-vinyltoluene, 4-vinylpyridine, N-vinylpyrrolidone, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 1,3-acryloyloxy-2-hydroxypropane, 1,2-methacryloyloxy-2-hydroxypropane, methylenebisacrylamide, N,N-dimethylacrylamide, N-methylolacrylamide, triacrylate of tris(β-hydroxyethyl)isocyanurate, a compound represented by the following formula (13), urethane acrylate or urethane methacrylate, urea acrylate, isocyanuric acid-modified di / triacrylate and methacrylate, and the like. [ka] In the formula, R 41 and R 42 each independently represents a hydrogen atom or a methyl group, and f and g each independently represent an integer of 1 or greater.
[0103] The resin composition according to the second embodiment may further contain an adhesion aid, such as a silane coupling agent, a triazole-based compound, or a tetrazole-based compound.
[0104] As the silane coupling agent, a compound having a nitrogen atom is preferably used in order to improve adhesion with metal. Examples of the silane coupling agent include N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, and 3-isocyanatepropyltriethoxysilane. The content of the silane coupling agent is preferably 0.1 parts by mass to 20 parts by mass based on the total amount of solids in the resin composition from the viewpoints of the effect of addition, heat resistance, and production cost.
[0105] Examples of triazole compounds include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenyl]benzotriazole, phenol], 6-(2-benzotriazolyl)-4-tert-octyl-6'-tert-butyl-4'-methyl-2,2'-methylenebisphenol, 1,2,3-benzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]benzotriazole, carboxybenzotriazole, 1-[N,N-bis(2-ethylhexyl)aminomethyl]methylbenzotriazole, 2,2'-[[(methyl-1H-benzotriazol-1-yl)methyl]imino]bisethanol, and the like.
[0106] Examples of tetrazole compounds include 1H-tetrazole, 5-amino-1H-tetrazole, 5-methyl-1H-tetrazole, 5-phenyl-1H-tetrazole, 1-methyl-5-ethyl-1H-tetrazole, 1-methyl-5-mercapto-1H-tetrazole, 1-phenyl-5-mercapto-1H-tetrazole, 1-(2-dimethylaminoethyl)-5-mercapto-1H-tetrazole, 2-methoxy-5-(5-trifluoromethyl-1H-tetrazol-1-yl)-benzaldehyde, 4,5-di(5-tetrazolyl)-[1,2,3]triazole, and 1-methyl-5-benzoyl-1H-tetrazole.
[0107] The content of the triazole-based compound and the tetrazole-based compound is preferably 0.1 to 20 parts by mass based on the total solid content in the resin composition, from the viewpoints of the effect of the addition, heat resistance, and production costs.
[0108] The above silane coupling agents, triazole-based compounds, and tetrazole-based compounds may be used alone or in combination.
[0109] The resin composition according to the second embodiment may further contain an ion trapping agent. By adsorbing ionic impurities in the resin composition with the ion trapping agent, the insulation reliability of the wiring interlayer insulating layer during moisture absorption can be further improved. Examples of the ion trapping agent include triazine thiol compounds, phenol-based reducing agents, and inorganic compounds such as powdered bismuth, antimony, magnesium, aluminum, zirconium, calcium, titanium, and tin, as well as mixtures thereof. Triazine thiol compounds and phenol-based reducing agents are compounds known as copper damage inhibitors for preventing copper from being ionized and dissolved.
[0110] Examples of the ion scavenger include inorganic ion scavenger (manufactured by Toagosei Co., Ltd., product names: IXE-300 (antimony-based), IXE-500 (bismuth-based), IXE-600 (antimony and bismuth mixed system), IXE-700 (magnesium and aluminum mixed system), IXE-800 (zirconium-based), and IXE-1100 (calcium-based)). The ion scavenger may be used alone or in combination of two or more. The content of the ion scavenger is preferably 0.01 to 10 parts by mass based on the total solid content in the resin composition, from the viewpoints of the effect of addition, heat resistance, production costs, and the like.
[0111] Hereinafter, matters common to the first and second embodiments will be described. The resin composition may further contain a filler from the viewpoint of imparting low moisture absorption and low moisture permeability. The filler may be an inorganic filler made of an inorganic material, or an organic filler made of an organic material. These fillers are preferably insulating fillers.
[0112] Examples of inorganic fillers include alumina, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, calcium silicate, magnesium silicate, calcium oxide, magnesium oxide, aluminum oxide, aluminum nitride, crystalline silica, amorphous silica, boron nitride, titania, glass, iron oxide, ceramics, etc. Examples of organic fillers include carbon, rubber-based fillers, etc. Fillers can be used without particular restrictions regardless of type, shape, etc.
[0113] The filler may be used according to the desired function. For example, the inorganic filler is added for the purpose of imparting thermal conductivity, low thermal expansion, low moisture absorption, etc. to the wiring interlayer insulating layer. The organic filler is added for the purpose of imparting toughness, etc. to the wiring interlayer insulating layer. The filler may contain at least one of an inorganic filler and an organic filler, and one type of filler may be used alone or in combination of two or more types. The filler is preferably an inorganic filler from the viewpoint of imparting thermal conductivity, low moisture absorption characteristics, insulation, etc. required for the wiring interlayer insulating layer, and is more preferably at least one of a silica filler and an alumina filler from the viewpoint of good dispersibility in the resin varnish and the viewpoint of imparting high adhesive strength when heated.
[0114] The average particle size of the filler is, for example, 10 μm or less, and the maximum particle size of the filler is, for example, 30 μm or less. It is preferable that the average particle size of the filler is 5 μm or less, and the maximum particle size of the filler is 20 μm or less. By having an average particle size of 10 μm or less and a maximum particle size of 30 μm or less, the effect of improving the fracture toughness of the wiring interlayer insulating layer can be favorably exhibited, and the occurrence of a decrease and variation in the adhesive strength of the wiring interlayer insulating layer can be suppressed, and the surface of the wiring interlayer insulating layer can be roughened and the adhesive strength can be suppressed from decreasing. There is no particular limit to the lower limit of the average particle size and the lower limit of the maximum particle size of the filler, but both may be 0.001 μm or more.
[0115] The average particle size and maximum particle size of the filler can be measured, for example, by measuring the particle size of about 20 fillers using a scanning electron microscope (SEM). The measurement method using SEM can be, for example, by preparing a sample by heat-curing (preferably at 150 to 180°C for 1 to 10 hours) a resin composition containing the filler, cutting the center of the sample, and observing the cross section with an SEM. In this case, it is preferable that the probability of the presence of fillers with a particle size of 30 μm or less in the cross section is 80% or more of all fillers.
[0116] The content of the filler is appropriately determined depending on the characteristics or functions to be imparted. The content of the filler is, for example, preferably 1% by mass to 70% by mass, or 2% by mass to 60% by mass, more preferably 5% by mass to 50% by mass, based on the mass of the resin composition. By increasing the content of the filler, the elastic modulus of the wiring interlayer insulating layer is increased. This effectively improves the dicing property (cutting property by a dicer blade), the wire bonding property (ultrasonic efficiency), and the adhesive strength during heating. From the viewpoint of suppressing the decrease in thermocompression bonding property, the content of the filler is preferably equal to or less than the upper limit value described above. The optimal content of the filler may be determined to balance the required properties. The mixing and kneading of the filler may be performed by appropriately combining a dispersing machine such as a normal stirrer, a mortar mill, a three-roll mill, or a ball mill.
[0117] The resin composition may further contain an antioxidant from the viewpoints of storage stability, prevention of electromigration, and prevention of corrosion of the metal conductor circuit. The antioxidant is not particularly limited, and examples thereof include benzophenone-based, benzoate-based, hindered amine-based, benzotriazole-based, and phenol-based antioxidants. The content of the antioxidant is preferably 0.01 to 10 parts by mass with respect to 100 parts by mass of the resin component from the viewpoints of the effect of addition, heat resistance, cost, and the like.
[0118] The resin composition may further contain a catalyst to further promote curing. Examples of the catalyst include peroxides, imidazole compounds, organic phosphorus compounds, secondary amines, tertiary amines, and quaternary ammonium salts. These may be used alone or in combination of two or more. From the viewpoint of reactivity, the catalyst is preferably at least one selected from the group consisting of peroxides, imidazole compounds, and organic phosphorus compounds, and more preferably a peroxide from the viewpoint of contributing to the self-polymerization of the maleimide group and the reaction between the maleimide group and the acryloyl group.
[0119] The resin composition may further contain a flame retardant. The flame retardant is not particularly limited, but may be a halogen-containing flame retardant such as a bromine-based flame retardant or a chlorine-based flame retardant, a phosphorus-based flame retardant such as triphenyl phosphate, tricresyl phosphate, tris-dichloropropyl phosphate, a phosphoric acid ester compound, or red phosphorus, a nitrogen-based flame retardant such as guanidine sulfamate, melamine sulfate, melamine polyphosphate, or melamine cyanurate, a phosphazene-based flame retardant such as cyclophosphazene or polyphosphazene, or an inorganic flame retardant such as antimony trioxide. These flame retardants may be used alone or in combination of two or more.
[0120] The resin composition may further contain an ultraviolet absorbing agent. The ultraviolet absorbing agent is not particularly limited, but may be, for example, a benzotriazole-based ultraviolet absorbing agent.
[0121] The resin composition may further contain a fluorescent whitening agent. The fluorescent whitening agent is not particularly limited, but examples thereof include stilbene derivatives.
[0122] From the viewpoint of ease of handling, the resin composition is preferably in the form of a film. The resin composition may be in the form of a varnish (liquid) in which each component is dissolved or uniformly dispersed in a solvent.
[0123] The preparation means and conditions of the varnish are not particularly limited. For example, the main components in the predetermined amounts are thoroughly and uniformly stirred and mixed by a mixer or the like, then kneaded using a mixing roll, an extruder, a kneader, a roll, an extruder, or the like, and the kneaded product obtained is further cooled and pulverized. The kneading method is not particularly limited.
[0124] When the resin composition is a varnish, the solvent may be, for example, an organic solvent. The organic solvent is not particularly limited, but may be, for example, alcohols such as methanol, ethanol, butanol, butyl cellosolve, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and cyclopentanone; aromatic hydrocarbons such as toluene, xylene, mesitylene, and limonene; esters such as methoxyethyl acetate, ethoxyethyl acetate, butoxyethyl acetate, and ethyl acetate; and nitrogen-containing solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. These may be used alone or in combination of two or more. In terms of solubility, the organic solvent is preferably toluene, xylene, cyclohexanone, cyclopentanone, limonene, or mesitylene, and more preferably cyclopentanone, limonene, or mesitylene in terms of low toxicity.
[0125] The organic solvent is preferably used in an amount such that the solid content of the resin composition in the varnish is 5 to 90 mass %, and more preferably in an amount such that the solid content is 10 to 60 mass %, in order to maintain good handleability and coatability of the varnish.
[0126] The cured product of the resin composition preferably has a moisture absorption rate of 1 mass % or less after being placed in an atmosphere at 130° C. and a relative humidity of 85% for 200 hours.
[0127] The moisture absorption rate of the cured resin composition after being placed in an environment of 130°C and 85% relative humidity for 200 hours can be measured by the following procedure. A 10 μm thick curable film of the resin composition is laminated on a silicon wafer at 100°C, and the curable film is cured by heating at 180°C for 2 hours in that state. A sample, which is a laminate of a silicon wafer and a cured film of the resin composition, is left to stand for 200 hours in a thermohygrostat (EHS-221MD manufactured by Espec Corp.) at 130°C and 85% relative humidity. Thereafter, the temperature in the thermohygrostat is lowered to 50°C, and the sample is taken out, and the cured film is scraped off from the silicon wafer. The weight loss rate of the obtained cured sample due to heating is measured using a differential thermal thermogravimetry simultaneous analyzer (manufactured by SII Nanotechnology, product name "TG / DTA6300") under the conditions of a heating rate of 10°C / min, nitrogen flow (400mL / min), and temperature of 25 to 150°C. The mass loss rate when heated to 150° C. (ratio to the mass of the cured sample before measurement) is recorded as the moisture absorption rate (mass %).
[0128] The concentration of chloride ions in the cured product of the resin composition is preferably 5 ppm or less from the viewpoint of insulation reliability, and more preferably 3 ppm or less from the viewpoint of suppressing discoloration of copper wiring. The concentration of chloride ions can be measured by the following procedure. 1 g of the cured product sample and 10 g of ultrapure water as an extracting solution are placed in a heat-resistant container made of Teflon (registered trademark) and heated at 130°C for 5 hours. The extracting solution is then filtered and analyzed by ion chromatography. In the obtained chromatogram, the peak detected at elution times of 0 to 30 minutes is regarded as the total amount of eluted material, and the mass of chloride ions in the cured product sample is determined from the peak area of chloride ions at around 9.6 minutes. The ratio of the determined mass of chloride ions to the mass of the cured product sample is calculated as the concentration (ppm) of chloride ions in the cured product. The conditions for the ion chromatography are as follows: Equipment: Dionex ISC-2000 Detector: Electrical conductivity detector Column: AS20 (4mmφ×200mm) Column temperature: 30℃ ·Flow rate: 1.0ml / min ·Injection volume: 25μl Gradient settings: KOH concentration was set to 5 mM at 0 min, 5 mM at 5 min, 30 mM at 15 min, and 55 mM at 20 min.
[0129] The dielectric constant of the wiring interlayer insulating layer (cured product of the resin composition) at 10 GHz is preferably 3.6 or less, 3.2 or less, or 3.0 or less in terms of suppressing crosstalk between wiring layers, and more preferably 2.8 or less in terms of improving the reliability of electrical signals. The dielectric constant may be 1.0 or more. The dielectric constant can be measured using a test piece obtained by cutting a 300 μm thick cured product obtained by curing the resin composition by heating at 180° C. for 2 hours into a length of 60 mm and a width of 2 mm and vacuum drying at 30° C. for 6 hours.
[0130] The dielectric loss tangent of the wiring interlayer insulating layer (cured product of the resin composition) at 10 GHz is preferably 0.012 or less, 0.008 or less, or 0.005 or less. The dielectric loss tangent may be 0.0001 or more. The dielectric loss tangent can be calculated from the resonance frequency and the unloaded Q value obtained at 10 GHz. The measurement temperature is 25°C. As a measuring device for the dielectric constant and the dielectric loss tangent, for example, a vector network analyzer (manufactured by Keysight Technologies Inc., product name: E8364B) and a 10 GHz resonator (manufactured by Kanto Electronics Application Development Co., Ltd., product name: CP531) can be used, and the program CPMA-V2 can be used.
[0131] The glass transition temperature of the cured product of the resin composition is preferably 120°C or higher from the viewpoint of suppressing cracks during temperature cycling, and more preferably 140°C or higher from the viewpoint of reducing stress on wiring. The glass transition temperature of the cured product of the resin composition is preferably 240°C or lower from the viewpoint of enabling lamination at low temperatures, and more preferably 220°C or lower from the viewpoint of suppressing cure shrinkage. The glass transition temperature of the cured product of the resin composition may be 120 to 240°C, 120 to 220°C, 140 to 240°C, or 140 to 220°C.
[0132] The glass transition temperature of the cured resin composition is measured using a sample prepared by cutting a 300 μm thick cured product obtained by curing the resin composition by heating at 180° C. for 2 hours into a length of 30 mm and a width of 4 mm. The measurement is performed using a dynamic viscoelasticity measuring device manufactured by UBM, with a chuck distance of 20 mm, a frequency of 10 Hz, and a heating rate of 5° C. / min in the temperature range of 40 to 260° C., and the temperature at which tan δ is maximum is recorded as the glass transition temperature.
[0133] The breaking elongation of the cured resin composition is, for example, 5% or more from the viewpoint of reducing warpage of the wiring interlayer insulating layer. From the viewpoint of relaxing stress on the copper wiring, the breaking elongation is preferably 10% or more. From the viewpoint of improving the temperature cycle reliability of the wiring layer laminate, the breaking elongation is more preferably 15% or more. The breaking elongation may be 200% or less. The breaking elongation of the cured resin composition may be 5 to 200%, 10 to 200%, or 15 to 200%. The breaking elongation can be measured using a sample prepared by cutting a 300 μm thick cured product obtained by curing the resin composition by heating at 180° C. for 2 hours into a length of 30 mm and a width of 5 mm. The breaking elongation is measured using a small tabletop testing machine (manufactured by Shimadzu Corporation, product name: EZ-S) at a feed rate of 5 mm / min.
[0134] From the viewpoint of heat resistance reliability, the 5% weight loss temperature of the cured resin composition is, for example, 300° C. or higher. The 5% weight loss temperature of the first wiring interlayer insulating layer 17 can be measured using a thermogravimetric and differential thermal analyzer (manufactured by Hitachi High-Tech Science Corporation, product name: TG / DTA6300) under conditions of a heating rate of 10° C. / min and a nitrogen flow of 400 ml / min, using a 300 μm-thick cured sample obtained by curing the resin composition by heating at 180° C. for 2 hours.
[0135] The cured product of the resin composition may have a storage modulus at 40° C. of 10 MPa to 5 GPa.
[0136] 1 is a schematic cross-sectional view of a semiconductor package having a semiconductor wiring layer laminate according to one embodiment. The semiconductor wiring layer laminate of the present disclosure is preferably used in a package form requiring an interposer for mounting different types of chips together.
[0137] As shown in FIG. 1, the semiconductor package 100 is a semiconductor device including a substrate 1, a wiring layer laminate 10 provided on the substrate 1, and semiconductor chips 2A and 2B mounted on the wiring layer laminate 10. The semiconductor chips 2A and 2B are fixed on the wiring layer laminate 10 by corresponding underfills 3A and 3B, respectively, and are electrically connected to each other via surface wiring (not shown) provided in the wiring layer laminate 10. The substrate 1 is a sealed body formed by sealing the semiconductor chips 2C and 2D and the electrodes 5A and 5B with an insulating material 4. The semiconductor chips 2C and 2D in the substrate 1 can be connected to an external device via the electrodes exposed from the insulating material 4. The electrodes 5A and 5B function as, for example, conductive paths for electrically connecting the wiring layer laminate 10 and the external device to each other.
[0138] Each of the semiconductor chips 2A to 2D is, for example, a graphic processing unit (GPU), a volatile memory such as a dynamic random access memory (DRAM) or a static random access memory (SRAM), a non-volatile memory such as a flash memory, an RF chip, a silicon photonics chip, a micro electro mechanical system (MEMS), a sensor chip, or the like. The semiconductor chips 2A to 2D may have a TSV. For example, a semiconductor element stacked on each of the semiconductor chips 2A to 2D can be used. In this case, the semiconductor element stacked using the TSV can be used. The thickness of the semiconductor chips 2A and 2B is, for example, 200 μm or less. From the viewpoint of thinning the semiconductor package 100, the thickness of the semiconductor chips 2A and 2B is preferably 100 μm or less. Moreover, from the viewpoint of ease of handling, the thickness of the semiconductor chips 2A and 2B is more preferably 30 μm or more. Each of the semiconductor chips 2A to 2D is electrically connected to any of the wirings in the wiring layer stack 10.
[0139] The underfills 3A and 3B are, for example, a capillary underfill (CUF), a molded underfill (MUF), a paste underfill (NCP), a film underfill (NCF), or a photosensitive underfill. The underfills 3A and 3B are each composed mainly of a liquid curing resin (for example, an epoxy resin). The insulating material 4 is, for example, a curing resin having insulating properties.
[0140] Next, the wiring layer laminate 10 according to this embodiment will be described in detail with reference to Fig. 2. The wiring layer laminate 10 is a wiring board on which a semiconductor element or the like is mounted. The shape of the wiring layer laminate 10 corresponds to the shape of a substrate 11 described later, and may be a wafer shape (approximately circular in a plan view) or a panel shape (approximately rectangular in a plan view).
[0141] The wiring layer laminate 10 provided on the substrate 11 shown in FIG. 2 includes a plurality of wiring layers 41, 42 each including organic insulating layers 21, 22, copper wirings 13, 14 embedded in the organic insulating layers 21, 22, and barrier metal films 15, 16 provided between the copper wirings 13, 14 and the organic insulating layers 21, 22, wiring interlayer insulating layers 17, 18 adjacent to the wiring layers 41, 42, and through wirings 19 penetrating the organic insulating layers 21, 22 and the wiring interlayer insulating layers 17, 18. The organic insulating layers 21, 22 and the wiring interlayer insulating layers 17, 18 are alternately laminated on the substrate 11. A part of the surface of the copper wirings 13, 14 is exposed on one main surface side of the wiring layers 41, 42, and the wiring interlayer insulating layers 17, 18 are in contact with the surface of the exposed copper wirings 13, 14. The wiring interlayer insulating layers 17, 18 are a cured product of the curable resin composition according to the above embodiment. The organic insulating layers 21 and 22 may be layers formed from a photosensitive insulating resin. The copper wiring may be exposed on both main surfaces of the wiring layer, and an insulating layer between wiring layers may be in contact with the surfaces of the exposed copper wiring.
[0142] The substrate 11 is a support that supports the wiring layer laminate 10. The shape of the substrate 11 in a plan view is, for example, circular or rectangular. If the substrate 11 is circular, it has a diameter of, for example, 200 mm to 450 mm. If the substrate 11 is rectangular, one side of the substrate 11 is, for example, 300 mm to 700 mm.
[0143] The substrate 11 is, for example, a silicon substrate, a glass substrate, or a peelable copper foil. The substrate 11 may be, for example, a build-up substrate, a substrate for wafer-level packaging, a coreless substrate, a substrate produced by thermally curing a sealing material, or a substrate in which a chip is sealed or embedded. When a silicon substrate or a glass substrate is used as the substrate 11, a temporary fixing layer (not shown) for temporarily fixing the wiring layer laminate 10 and the substrate 11 may be provided. In this case, the substrate 11 can be easily peeled off from the wiring layer laminate 10 by removing the temporary fixing layer. The peelable copper foil is a laminate in which a support, a peeling layer, and a copper foil are stacked in this order. In the peelable copper foil, the support corresponds to the substrate 11, and the copper foil can form a part of the through wiring 19.
[0144] The organic insulating layer 21 (first organic insulating layer) includes a third organic insulating layer 23 located on the substrate 11 side and a fourth organic insulating layer 24 located on the second organic insulating layer 22 side. The first organic insulating layer 21 has a plurality of grooves 21a (first grooves) in which corresponding copper wirings 13 are arranged. The fourth organic insulating layer 24 is provided with a plurality of openings corresponding to the grooves 21a. The surfaces of the third organic insulating layer 23 exposed by these openings form the bottom surfaces of the inner surfaces of the grooves 21a. The side surfaces of the grooves 21a are formed by the fourth organic insulating layer 24.
[0145] The third organic insulating layer 23 and the fourth organic insulating layer 24 each have a thickness of, for example, 0.5 μm to 10 μm. Therefore, the first organic insulating layer 21 has a thickness of, for example, 1 μm to 20 μm. When the first organic insulating layer 21 has a thickness of 1 μm or more, the first organic insulating layer 21 contributes to stress relaxation of the wiring layer laminate 10, and the temperature cycle resistance of the wiring layer laminate 10 can be improved. When the first organic insulating layer 21 has a thickness of 20 μm or less, warping of the wiring layer laminate 10 is suppressed, and, for example, when the wiring layer laminate 10 is ground, the wiring and the like can be easily exposed. From the viewpoint of forming the copper wiring 13 having a width of 3 μm or less by performing exposure and development, the thickness of the first organic insulating layer 21 is preferably 15 μm or less, and more preferably 10 μm or less.
[0146] The grooves 21a are provided on the surface of the first organic insulating layer 21 opposite to the substrate 11. In a cross section along a direction perpendicular to the extension direction of the grooves 21a, each of the grooves 21a has a substantially rectangular shape. Therefore, the inner surface of the grooves 21a has a side surface and a bottom surface. The grooves 21a have a predetermined line width L and space width S. Each of the line width L and space width S is, for example, 0.5 μm to 10 μm, preferably 0.5 μm to 5 μm, and more preferably 2 μm to 5 μm. From the viewpoint of realizing high-density transmission of the wiring layer laminate 10, the line width L is preferably 1 μm to 5 μm. The line width L and space width S may be set to be the same as each other, or may be set to be different from each other. The line width L corresponds to the width of the grooves 21a in a direction perpendicular to the extension direction of the grooves 21a in a plan view. The space width S corresponds to the distance between adjacent grooves 21a. The depth of the groove portion 21a corresponds to the thickness of the fourth organic insulating layer 24, for example.
[0147] The organic insulating layer 22 (second organic insulating layer) is laminated on the first organic insulating layer 21 with the wiring interlayer insulating layer 17 (first wiring interlayer insulating layer) sandwiched therebetween. The second organic insulating layer 22 has a plurality of grooves 22a (second grooves) in which the corresponding copper wirings 14 are disposed.
[0148] The thickness of each of the second organic insulating layers 22 is, for example, 1 μm to 10 μm. When the thickness of the second organic insulating layer 22 is 1 μm or more, the second organic insulating layer 22 contributes to stress relaxation of the wiring layer laminate 10, and the temperature cycle resistance of the wiring layer laminate 10 can be improved. When the thickness of the second organic insulating layer 22 is 10 μm or less, warping of the wiring layer laminate 10 is suppressed, and, for example, when the wiring layer laminate 10 is ground, the wiring and the like can be easily exposed. A part of the second organic insulating layer 22 is provided with a plurality of openings corresponding to the grooves 22a. The surfaces of the first wiring interlayer insulating layer 17 exposed by these openings constitute the bottom surfaces of the inner surfaces of the grooves 22a. Each side surface of the grooves 22a is constituted by the second organic insulating layer 22. In this embodiment, the line width and space width of the plurality of grooves 22a are the same as the line width L and space width S of the grooves 21a.
[0149] The first organic insulating layer 21 in which the groove portion 21a is formed and the second organic insulating layer 22 in which the groove portion 22a is provided may each be hardened by a heat treatment. The heat treatment is carried out, for example, using an oven. From the viewpoint of reducing the residual stress of the wiring layer laminate 10, it is preferable to carry out the heat treatment at, for example, 200° C. or less. From the viewpoint of production efficiency, it is preferable to set the heat treatment time to less than 3 hours.
[0150] As described above, the copper wirings 13 are provided in the corresponding grooves 21a and function as conductive paths inside the wiring layer laminate 10. For this reason, the width of the copper wirings 13 approximately matches the line width L of the grooves 21a, and the distance between adjacent copper wirings 13 approximately matches the space width S of the grooves 21a.
[0151] As described above, the copper wiring 14 is provided in the corresponding groove portion 22a and functions as a conductive path inside the wiring layer laminate 10. Therefore, the width of the copper wiring 13 is approximately the same as the line width of the groove portion 22a, and the interval between adjacent copper wirings 14 is approximately the same as the space width of the groove portion 22a. The copper wiring 14 contains the same metal material as the copper wiring 13.
[0152] The barrier metal film 15 (first barrier metal film) is a metal film provided so as to separate the copper wiring 13 from the first organic insulating layer 21 (i.e., the inner surface of the groove portion 21a). The first barrier metal film 15 is a film for preventing the diffusion of copper from the copper wiring 13 to the first organic insulating layer 21, and is formed along the inner surface of the groove portion 21a. For this reason, the first barrier metal film 15 contains a metal material that is difficult to diffuse into the organic insulating layer (for example, titanium, chromium, tungsten, palladium, nickel, gold, tantalum, or an alloy containing these). The first barrier metal film 15 may contain one or more types of metal. From the viewpoint of adhesion to the inner surface of the groove portion 21a, the first barrier metal film 15 is preferably a titanium film or an alloy film containing titanium. When the first barrier metal film 15 is formed by sputtering, the first barrier metal film 15 is preferably a titanium film, a tantalum film, a tungsten film, a chromium film, or an alloy film containing at least one of titanium, tantalum, tungsten, and chromium.
[0153] The thickness of the first barrier metal film 15 is less than half the width of the groove portion 21a and less than the depth of the groove portion 21a. From the viewpoint of preventing electrical conduction between the copper wirings 13 and suppressing an increase in the resistance of the copper wiring 13, the thickness of the first barrier metal film 15 is, for example, 0.001 μm to 0.5 μm. From the viewpoint of preventing the diffusion of metal materials in the copper wiring 13, the thickness of the first barrier metal film 15 is preferably 0.01 μm to 0.5 μm. From the viewpoint of flatness of the first barrier metal film 15 and increasing the amount of current flowing through the copper wiring 13, the thickness of the first barrier metal film 15 is preferably 0.001 μm to 0.3 μm. From the above, the thickness of the first barrier metal film 15 is most preferably 0.01 μm to 0.3 μm.
[0154] The second barrier metal film 16 is a metal film provided so as to separate the copper wiring 14 from the second organic insulating layer 22 (i.e., the inner surface of the groove 22a). The second barrier metal film 16 is a film for preventing diffusion of copper from the copper wiring 14 to the second organic insulating layer 22, and is formed along the inner surface of the groove 22a. For this reason, the second barrier metal film 16 contains a metal material that is difficult to diffuse into the organic insulating layer, similar to the first barrier metal film 15. The thickness of the second barrier metal film 16 is less than half the width of the groove 22a and less than the depth of the groove 22a, similar to the first barrier metal film 15. Therefore, the thickness of the second barrier metal film 16 is, for example, 0.001 μm to 0.5 μm, preferably 0.01 μm to 0.5 μm or 0.001 μm to 0.3 μm, and most preferably 0.01 μm to 0.3 μm.
[0155] The first wiring interlayer insulating layer 17 is an insulating film for preventing diffusion of copper from the copper wiring 13 to the first organic insulating layer 21 and the second organic insulating layer 22. The first wiring interlayer insulating layer 17 is provided between the wiring layer 41 (first wiring layer) and the wiring layer 42 (second wiring layer) so as to separate the copper wiring 13 from the second organic insulating layer 22. The first wiring interlayer insulating layer 17 is in contact with the surface of the copper wiring 13 exposed on the main surface of the first wiring layer 41 opposite to the substrate 11. From the viewpoint of making the wiring layer laminate 10 thin, the thickness of the first wiring interlayer insulating layer 17 is, for example, 50 μm or less. From the viewpoint of preventing electrical conduction between the copper wirings 13, the thickness of the first wiring interlayer insulating layer 17 is, for example, 1 μm or more, and preferably 10 μm or more. The thickness of the first wiring interlayer insulating layer 17 is preferably 30 μm or less from the viewpoint of surface smoothness of the first wiring interlayer insulating layer 17. Details of the materials contained in the first wiring interlayer insulating layer 17 and other properties of the first wiring interlayer insulating layer 17 will be described later.
[0156] The second wiring interlayer insulating layer 18 is an insulating film for preventing diffusion of copper from the copper wiring 14 to the second organic insulating layer 22. The second wiring interlayer insulating layer 18 is provided on the second wiring layer 42 while being in contact with the surface of the copper wiring 14 exposed on the main surface of the second wiring layer 42 opposite to the substrate 11. The second wiring interlayer insulating layer 18 contains the same material as the first wiring interlayer insulating layer 17, and has the same characteristics as the first wiring interlayer insulating layer 17.
[0157] The through wiring 19 is a wiring embedded in a via 31 that penetrates the wiring layers 41 and 42 and the wiring interlayer insulating layers 17 and 18, and functions as a connection terminal to an external device.
[0158] Next, a method for manufacturing the wiring layer laminate 10 according to this embodiment will be described with reference to Figs. 3 to 10. The wiring layer laminate 10 formed by the manufacturing method described below is particularly suitable for a form requiring miniaturization and a large number of pins, for example. Fig. 4(b) is an enlarged view of a main part of Fig. 4(a). Similarly, Fig. 5(b), Fig. 6(b), Fig. 7(b), Fig. 8(b), Fig. 9(b), Fig. 10(b), Fig. 11(b), and Fig. 12(b) are enlarged views of a main part of the corresponding drawing.
[0159] First, as a first step, as shown in Fig. 3(a), a bottom 19a of the through wiring is formed on the substrate 11. The bottom 19a of the through wiring is formed by patterning a metal film formed on the substrate 11. In the first step, the metal film is formed by, for example, a coating method, a physical vapor deposition method (PVD method) such as vacuum deposition or sputtering, a printing method or a spray method using a metal paste, or various plating methods. In this embodiment, a copper foil is used as the metal film.
[0160] When a temporary fixing layer (not shown) is provided between the substrate 11 and the bottom 19a of the through wiring, the temporary fixing layer contains, for example, a resin containing a non-polar component such as polyimide, polybenzoxazole, silicon, or fluorine, a resin containing a component that expands in volume or foams when heated or exposed to UV (ultraviolet light), a resin containing a component that undergoes a crosslinking reaction when heated or exposed to UV, or a resin that generates heat when exposed to light. Examples of a method for forming the temporary fixing layer include spin coating, spray coating, and lamination. From the viewpoint of achieving a high degree of both ease of handling and carrier peelability, it is preferable that the temporary fixing layer is easily peeled off by an external stimulus such as light or heat. From the viewpoint of being peelable so that the temporary fixing layer does not remain in the semiconductor wiring layer laminate 10 to be manufactured later, it is most preferable that the temporary fixing layer contains a resin that expands in volume when heated.
[0161] When a temporary fixing layer is provided between the substrate 11 and the bottom 19a of the through wiring, the bottom 19a of the through wiring may be formed from the copper foil of the peelable copper foil. In this case, the substrate 11 corresponds to the support of the peelable copper foil, and the temporary fixing layer corresponds to the peeling layer of the peelable copper foil.
[0162] 3(b), a third organic insulating layer 23 is formed on the substrate 11 so as to cover the bottom 19a of the through wiring. In the second step, for example, the third organic insulating layer 23 can be formed by attaching a photosensitive insulating resin film to the substrate 11. If necessary, the photosensitive insulating resin film is subjected to an exposure process, a development process, a curing process, and the like.
[0163] 3(c), a fourth organic insulating layer 24 is formed on the third organic insulating layer 23 to form the first organic insulating layer 21. In the third step, similar to the second step, a film containing a photosensitive insulating resin is attached to the third organic insulating layer 23 to form the fourth organic insulating layer. If necessary, the film of the photosensitive insulating resin is subjected to an exposure process, a development process, a curing process, and the like.
[0164] Next, as a fourth step, as shown in Fig. 4(a) and (b), a plurality of grooves 21a are formed in the first organic insulating layer 21. In the fourth step, the plurality of grooves 21a are formed by, for example, laser ablation, photolithography, or imprinting. From the viewpoint of miniaturization of the grooves 21a and the formation cost, it is preferable to apply photolithography. For example, the plurality of grooves 21a can be formed by performing an exposure process and a development process on the photosensitive insulating resin used to form the fourth organic insulating layer 24.
[0165] The method of exposing the photosensitive insulating resin by the photolithography can be a known projection exposure method, contact exposure method, direct drawing exposure method, etc. In addition, in order to develop the photosensitive insulating resin, for example, an alkaline aqueous solution of sodium carbonate, tetramethylammonium hydroxide (TMAH), etc. may be used.
[0166] In the fourth step, after forming the multiple grooves 21a, the first organic insulating layer 21 may be further heated and cured. In this case, for example, the heating temperature is set to 100 to 200° C. and the heating time is set to 30 minutes to 3 hours, to heat and cure the first organic insulating layer 21.
[0167] Next, as a fifth step, as shown in FIGS. 5(a) and 5(b), a first barrier metal film 15 is formed on the first organic insulating layer 21 so as to cover the inner surface of the groove portion 21a. In the fifth step, the first barrier metal film 15 is formed by, for example, a coating method, a PVD method, a printing method or a spray method using a metal paste, or various plating methods. In the case of the coating method, the first barrier metal film 15 is formed by coating a complex of palladium or nickel on the first organic insulating layer 21 and then heating it. In the case of using a metal paste, the first barrier metal film 15 is formed by coating a paste containing metal particles such as nickel or palladium on the first organic insulating layer 21 and then sintering it. In this embodiment, the first barrier metal film 15 is formed by sputtering, which is one of the PVD methods.
[0168] Next, as a sixth step, as shown in Figs. 6(a) and (b), a copper layer 13A for forming copper wiring is formed on the first barrier metal film 15 so as to fill the groove portion 21a. In the sixth step, the copper layer 13A is formed, for example, by a method using a metal paste or a plating method using the first barrier metal film 15 as a seed layer. The thickness of the copper layer 13A is preferably, for example, 0.5 to 3 times the thickness of the first organic insulating layer 21. When the thickness of the copper layer 13A is 0.5 times or more, there is a tendency that the increase in the surface roughness of the copper wiring 13 formed in a later process can be suppressed. Also, when the thickness of the copper layer 13A is 3 times or less, there is a tendency that the warping of the copper layer 13A is suppressed and that the copper layer 13A adheres well to the first organic insulating layer 21.
[0169] Next, as a seventh step, as shown in FIGS. 7(a) and 7(b), the copper layer 13A is thinned so that the first organic insulating layer 21 is exposed. In the seventh step, the copper layer 13A is thinned so that the first organic insulating layer 21 is exposed, and the first barrier metal film 15 is thinned so that the first organic insulating layer 21 is exposed. This thinning process exposes the first organic insulating layer 21 and thins the copper layer 13A, forming the copper wiring 13 embedded in the groove 21a. This thinning process may be a planarization process of the combined surface of the first organic insulating layer 21 and the copper wiring 13. In this case, the target portions of the copper layer 13A and the first barrier metal film 15 are removed by CMP or flycutting, and the surface of the first organic insulating layer 21 is polished or ground to be planarized.
[0170] When CMP is used in the seventh step, the following slurries are used: a slurry containing alumina, which is generally used for polishing resins; a slurry containing hydrogen peroxide and silica, which is used for polishing the first barrier metal film 15; and a slurry containing hydrogen peroxide and ammonium persulfate, which is used for polishing the copper layer 13A. From the viewpoint of reducing costs and suppressing the increase in surface roughness, it is preferable to grind the first organic insulating layer 21, the first barrier metal film 15, and the copper layer 13A using a slurry containing alumina. When CMP is used, the cost tends to be high. In addition, when the first organic insulating layer 21, the first barrier metal film 15, and the copper layer 13A (copper wiring 13) are planarized simultaneously, dishing occurs in the copper wiring 13 due to differences in polishing speed, and as a result, the planarity of the surface of the first organic insulating layer 21 and the copper wiring 13 tends to be significantly impaired. For this reason, it is more preferable to grind the first organic insulating layer 21, the first barrier metal film 15, and the copper layer 13A (copper wiring 13) by a flycut method using a surface planer.
[0171] 8(a) and (b), in an eighth step, a first wiring interlayer insulating layer 17 is formed so as to cover the copper wiring 13 in the groove portion 21a. In the eighth step, the first wiring interlayer insulating layer 17 is formed by, for example, spin coating, spray coating, bar coating, curtain coating, a printing method, or lamination. From the viewpoint of ease of handling, it is preferable to form the first wiring interlayer insulating layer 17 using a film-like resin composition. Also, from the viewpoint of the film thickness uniformity of the first wiring interlayer insulating layer 17 and the ability to accommodate larger sizes, it is preferable to form the first wiring interlayer insulating layer 17 by lamination. When forming the first wiring interlayer insulating layer 17 by lamination, a film-like resin composition is attached to the first organic insulating layer 21, as in the second and third steps. In this case, it is preferable to set the temperature to 150° C. or less from the viewpoint of reducing residual stress, and it is preferable to set the temperature to 60° C. or more from the viewpoint of suppressing voids.
[0172] In the eighth step, the first wiring interlayer insulating layer 17 is preferably formed on the copper wiring 13 as well as on a portion of the first barrier metal film 15 that contacts the side surface of the groove portion 21a. In this case, a portion of the copper wiring 13 (the side surface and bottom surface of the copper wiring 13 that face the inner surface of the groove portion 21a) is covered with the first barrier metal film 15, and the other portion of the copper wiring 13 (the upper surface of the copper wiring 13) is covered with the first wiring interlayer insulating layer 17. The copper wiring 13 is covered without any gaps by the first barrier metal film 15 and the first wiring interlayer insulating layer 17.
[0173] Next, as a ninth step, as shown in FIGS. 9(a) and 9(b), a second organic insulating layer 22 having grooves 22a is formed on the first wiring interlayer insulating layer 17. In the ninth step, a photosensitive insulating resin film is first attached to the first wiring interlayer insulating layer 17 in the same manner as in the third step. Then, a plurality of grooves 22a are formed in the attached photosensitive insulating resin film. In the ninth step, the grooves 22a are formed by the same method as the grooves 21a described in the fourth step. In the ninth step, from the viewpoint of preventing the diffusion of copper constituting the copper wiring 13, it is preferable not to perform a development process on the second organic insulating layer 22.
[0174] 10(a) and 10(b), a second barrier metal film 16 and a copper layer 14A for forming copper wiring are sequentially formed on the second organic insulating layer. In the tenth step, the second barrier metal film 16 is first formed on the second organic insulating layer 22 so as to cover the inner surface of the groove 22a by the same method as in the fifth step. Then, the copper layer 14A is formed on the second barrier metal film 16 so as to fill the groove 22a by the same method as in the sixth step.
[0175] 11(a) and (b), in the 11th step, the copper layer 14A is thinned so as to expose the second organic insulating layer 22. In the 11th step, the portion of the copper layer 14A outside the groove portion 22a and the portion of the second barrier metal film 16 that does not cover the groove portion 22a are mechanically or chemically removed in the same manner as in the 7th step. This exposes the second organic insulating layer 22 and thins the copper layer 14A, forming the copper wiring 14 embedded in the groove portion 22a.
[0176] Next, as a twelfth step, as shown in FIGS. 12(a) and 12(b), a second wiring interlayer insulating layer 18 is formed so as to cover the copper wiring 14 in the groove portion 22a. In the twelfth step, the second wiring interlayer insulating layer 18 is formed on the second organic insulating layer 22 by the same method as in the eighth step. In the twelfth step, the second wiring interlayer insulating layer 18 is preferably formed on the copper wiring 14 as well as on the portion of the second barrier metal film 16 that contacts the side surface of the groove portion 22a. In this case, each side surface and bottom surface of the copper wiring 14 are covered by the second barrier metal film 16, and the top surface of the copper wiring 14 is covered by the second wiring interlayer insulating layer 18. The copper wiring 14 is covered without any gaps by the second barrier metal film 16 and the second wiring interlayer insulating layer 18.
[0177] Next, as a thirteenth step, as shown in Fig. 13(a), a via 31 is formed penetrating the first organic insulating layer 21, the first wiring interlayer insulating layer 17, the second organic insulating layer 22, and the second wiring interlayer insulating layer 18. For example, a laser is used to form the via 31. Examples of the laser include a carbon dioxide laser, a UV laser, a YAG laser, and an excimer laser. After the via 31 is formed, it is preferable to clean the inside of the via 31 by a known method such as a desmear process.
[0178] Next, as a 14th step, as shown in FIG. 13(b), a metal material is filled into the via 31 to form an intra-via conductive portion 19b, thereby forming a through wiring 19 having a bottom portion 19a and an intra-via conductive portion 19b. In the 14th step, the intra-via conductive portion 19b is formed, for example, by a PVD method or various plating methods. Examples of the metal material include copper, nickel, and tin. Through the above steps, the wiring layer laminate 10 shown in FIG. 2 is manufactured. If a temporary fixing layer is provided, the wiring layer laminate 10 may be peeled off from the substrate 11.
[0179] In the wiring layer laminate 10 formed by the manufacturing method described above, the moisture absorption rate of the wiring interlayer insulating layer after being left in an environment of 130°C and 85% relative humidity for two hours is 1 mass% or less, so that the amount of moisture contained in the wiring interlayer insulating layer is extremely small. This makes it possible to effectively suppress the diffusion of copper into the wiring interlayer insulating layer caused by the reaction between copper and water in the wiring interlayer insulating layer. As a result, the insulation properties of the wiring interlayer insulating layer are well maintained and short circuits between copper wirings are suppressed, so that the insulation reliability of the wiring layer laminate 10 can be effectively improved.
[0180] By mounting a plurality of semiconductor chips on the wiring layer laminate 10 according to this embodiment, a semiconductor device in which semiconductor chips are integrated can be provided with a high yield.
[0181] The present disclosure is not limited to the above-described embodiment, and may be modified as appropriate without departing from the spirit of the present disclosure. For example, a resin layer containing a photosensitive insulating resin, an insulating layer between wiring layers, a build-up material, or the like may be formed between the first organic insulating layer 21 and the substrate 1.
[0182] On the first wiring interlayer insulating layer 17, a resin layer containing a photosensitive insulating resin, a wiring interlayer insulating layer, a build-up material, an underfill, or the like may be formed in place of the second organic insulating layer 22 and the copper wiring 14, or a copper wiring or bump, etc. may be formed. Also, the first wiring interlayer insulating layer 17 may be provided with a via for embedding a metal material for connecting the copper wirings 13 and 14.
[0183] A resin layer containing a photosensitive insulating resin, a wiring interlayer insulating layer, a build-up material, an underfill, or the like may be formed on the second wiring interlayer insulating layer 18, or a copper wiring, bump, or the like may be formed. Also, the second wiring interlayer insulating layer 18 may be provided with a via for embedding a metal material that connects the copper wiring 14 to a semiconductor chip, or the like. EXAMPLES
[0184] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples.
[0185] Example 1 The measurement and evaluation samples shown in Fig. 14(a) and (b) were prepared as follows. First, a 3 μm-thick photosensitive insulating resin film 52 was attached to a 150 mm-thick silicon wafer 51. This photosensitive insulating resin film 52 was formed as follows. First, a cresol novolac resin (manufactured by Asahi Organic Chemicals Co., Ltd., product name: TR-4020G, 100 parts by mass), 1,3,4,6-tetrakis(methoxymethyl)glycoluril (30 parts by mass), trimethylolpropane triglycidyl ether (40 parts by mass), triarylsulfonium salt (manufactured by San-Apro Co., Ltd., product name: CPI-310B, 8 parts by mass), and methyl ethyl ketone (100 parts by mass) were mixed to obtain a photosensitive insulating resin. Next, the obtained photosensitive insulating resin was applied to a polyethylene terephthalate film (manufactured by Teijin DuPont Films, product name: A-53) and dried in an oven at 90° C. for 10 minutes to obtain a photosensitive insulating resin film 52 having a thickness of 3 μm.
[0186] Next, the photosensitive insulating resin film 52 attached to the silicon wafer 51 was subjected to exposure treatment, heating treatment, development treatment, and heat curing treatment in order. Next, a photosensitive insulating resin film 53 having a thickness of 3 μm, which was formed in the same manner as the film 52, was attached to the photosensitive insulating resin film 52. Next, the attached photosensitive insulating resin film 53 was exposed through a photomask, and then subjected to heating treatment, development treatment, and heat curing treatment in order. In this way, the photosensitive insulating resin film 53 was patterned to form a first groove portion 53a and a second groove portion 53b having a comb-like shape so as to interlock with each other, a first connection portion 53c connecting the first groove portions 53a, and a second connection portion 53d connecting the second groove portions 53b. The width of the first groove portion 53a and the width of the second groove portion 53b were each set to 5 μm. These widths correspond to the line width L of the wiring described later. Moreover, the distance (space width S) between adjacent first groove portion 53a and second groove portion 53b was set to 5 μm, and the length of each groove was set to 1 mm.
[0187] Next, a barrier metal film 54 containing titanium and having a thickness of 0.05 μm was formed on the photosensitive insulating resin film 53 by sputtering. Next, a copper layer was formed by electrolytic plating using the barrier metal film 54 as a seed layer to fill the first groove 53a, the second groove 53b, the first connection portion 53c, and the second connection portion 53d. Next, a part of the copper layer and a part of the barrier metal film 54 that does not cover the inner surfaces of the first groove 53a, the second groove 53b, the first connection portion 53c, and the second connection portion 53d were ground by a fly-cut method using a surface planer. As a result, a first wiring 55a buried in the first groove 53a, a second wiring 55b buried in the second groove 53b, a first connection wiring 55c buried in the first connection portion 53c, and a second connection wiring 55d buried in the second connection portion 53d were formed. An automatic surface planer (manufactured by Disco Corporation, product name "DAS8930") was used as the surface planer. In addition, in the grinding by the flycut method, the feed rate was set to 1 mm / s, and the spindle rotation speed was set to 2000 min -1 was set to.
[0188] Next, a 10 μm thick curable film was attached so as to expose at least a part of the first connection wiring 55c and a part of the second connection wiring 55d, and the curable film was thermally cured to form the wiring interlayer insulating layer 57. The curable film was attached so as to fill at least the first wiring 55a and the second wiring 55b. Material A described below was used as the curable film.
[0189] <Material A> First, in order to synthesize a thermoplastic resin having a siloxane chain, 25 g of "BMI-3000" (manufactured by Designer Molecules Inc., product name), 25 g of 2,2-bis(4-(4-maleimidophenoxy)phenyl)propane (manufactured by Daiwa Kasei Kogyo Co., Ltd., product name: BMI-4000), and 150 g of toluene were placed in a flask and stirred for 20 minutes. Next, 16.4 g of silicone diamine (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF-8010) was placed in the flask and heated to 130°C using an oil bath. The mixture was stirred for 3 hours from the start of reflux to react, and then cooled to room temperature by air cooling to form a thermoplastic resin having a solid silicone chain. Next, 50 g of a thermosetting elastomer (manufactured by Asahi Kasei Corporation, product name: Tuftec M1911) dissolved in toluene was mixed with 50 g of the above-mentioned thermoplastic resin having a silicone chain in solid content, and 2 g of a curing agent (manufactured by NOF Corporation, product name: Perhexine 25B). This mixture was stirred for 30 minutes to uniformly disperse, thereby forming a varnish of a resin composition for forming an insulating layer between wiring layers, the non-volatile content of which was adjusted to 20%. The obtained varnish of the resin composition was applied to a PET film (thickness 38 μm, product name: NR-1) that had been subjected to a release treatment using a tabletop coater. The thickness of the coating film was adjusted to 10 μm after drying using an applicator. Next, the coating film of the resin composition was dried by heating at 130° C. for 10 minutes, and a curable film (material A) was formed on the PET film. Then, the PET film was removed, and the curable film (material A) was used to form the insulating layer between wiring layers 57. The wiring interlayer insulating layer 57 of Example 1 (cured product of material A) had a moisture absorption rate of 1.0 mass % or less, a chloride ion concentration of 3 ppm or less, a breaking elongation of 150%, and a storage modulus at 40° C. of 60 MPa.
[0190] Returning to FIG. 14, a 3 μm-thick photosensitive insulating resin film 58 formed in the same manner as the photosensitive insulating resin film 52 was attached to the wiring interlayer insulating layer 57. Then, the photosensitive insulating resin film was subjected to an exposure process, a development process, and a thermal curing process. In this manner, the measurement evaluation sample 50 shown in FIGS. 14(a) and (b) was formed. In this measurement evaluation sample 50, the first wirings 55a are connected to each other by a first connection wiring 55c, and the first wirings 55a are covered by the barrier metal film 54 and the wiring interlayer insulating layer 57. The second wirings 55b are connected to each other by a second connection wiring 55d, and the second wirings 55b are also covered by the barrier metal film 54 and the wiring interlayer insulating layer 57.
[0191] In order to confirm the insulation reliability of the above-mentioned measurement and evaluation sample 50, a highly accelerated stress test (HAST) was carried out as described below. In this test, a voltage of 3.3 V was applied to the first connection wiring 55c and the second connection wiring 55d under conditions of 85% humidity and 130°C, and the sample was left to stand for a predetermined time. This allowed the change in insulation between the first wiring 55a and the second wiring 55b over time to be measured. In this test, the resistance value between the first wiring 55a and the second wiring 55b was found to be 1×10 200 hours after the start of the test. 6 If it is more than 1×10 Ω, it is rated A, and if it is less than 1×10 Ω within 200 hours from the start of the test, 6 If it was less than Ω, it was rated as B. The results of the high acceleration life test of Example 1 are shown in Table 1 below.
[0192] Example 2 The measurement and evaluation sample 50 was formed in the same manner as in Example 1, except that the line width L and the space width S were set to 3 μm, and the above-mentioned high acceleration life test was performed. The results of the high acceleration life test of Example 2 are shown in Table 1 below.
[0193] Example 3 The measurement and evaluation sample 50 was formed in the same manner as in Example 1, except that the line width L and the space width S were set to 2 μm, and the above-mentioned high acceleration life test was performed. The results of the high acceleration life test of Example 3 are shown in Table 1 below.
[0194] Example 4 A measurement evaluation sample 50 was formed in the same manner as in Example 2, except that the following material B was used as the curable film for forming the wiring interlayer insulating layer 57. The above-mentioned high acceleration life test was performed on this measurement evaluation sample 50. The results of the high acceleration life test of Example 4 are shown in Table 1 below.
[0195] <Material B> First, in order to synthesize a thermoplastic resin having a siloxane chain, 8.17 g of 1,4-butanediol bis(3-aminopropyl)ether (manufactured by Tokyo Chemical Industry Co., Ltd., product name: B-12), 21.65 g of polyoxypropylenediamine (manufactured by BASF Japan Ltd., product name: D-400), 8.6 g of silicone diamine (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KF-8010), and 250 g of NMP (N-methyl-2-pyrrolidone) solvent were added to a 500 ml flask equipped with a stirrer, a thermometer, and a nitrogen replacement device (nitrogen inlet tube), and the diamine was dissolved in the solvent by stirring. Next, a reflux condenser with a water receiver was attached to the flask, and the temperature was raised to 180°C while blowing in nitrogen gas, and then the temperature was maintained at 180°C for 5 hours, and the reaction was carried out while removing water. The solution thus obtained was cooled to room temperature. Next, 50 g of polybutadiene resin (manufactured by CRAY VALLEY, product name: Ricon130MA8) dissolved in NMP in solid content, 50 g of the above-mentioned thermoplastic resin having a siloxane chain in solid content, 2 g of a curing agent (manufactured by NOF Corporation, product name: Perhexine 25B), and 1 g of G8009L (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name) were mixed and stirred for 30 minutes to uniformly disperse, forming a varnish of a resin composition for forming an insulating layer between wiring layers. The obtained varnish of the resin composition was applied onto a release-treated PET film (thickness 38 μm, product name: NR-1) using a tabletop coater. The film thickness of the coating film of the resin composition was adjusted to 10 μm after drying using an applicator. Next, the coating film of the resin composition was dried by heating at 120° C. for 20 minutes to form a curable film (material B) on the PET film. Then, the PET film was removed, and the curable film (material B) was used to form the wiring interlayer insulating layer 57. The wiring interlayer insulating layer 57 (cured product of material B) of Example 4 had a moisture absorption rate of 1.0 mass % or less, a chloride ion concentration of 3 ppm or less, an elongation at break of 70%, and a storage modulus at 40° C. of 180 MPa.
[0196] Example 5 The measurement and evaluation sample 50 was formed in the same manner as in Example 4, except that the line width L and the space width S were set to 2 μm, and the above-mentioned high acceleration life test was performed. The results of the high acceleration life test of Example 5 are shown in Table 1 below.
[0197] Example 6 A measurement evaluation sample 50 was formed in the same manner as in Example 2, except that the following material C was used as the curable film for forming the wiring interlayer insulating layer 57. The above-mentioned high acceleration life test was performed on this measurement evaluation sample 50. The results of the high acceleration life test of Example 6 are shown in Table 1 below.
[0198] <Material C> First, in order to synthesize a thermoplastic resin, 10.3 g of 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 4.1 g of 1,4-butanediol bis(3-aminopropyl)ether (manufactured by Tokyo Chemical Industry Co., Ltd., product name: B-12), and 101 g of NMP were added to a flask equipped with a stirrer, a thermometer, and a nitrogen replacement device. Next, 20.5 g of 1,2-(ethylene)bis(trimellitate anhydride) was added to the flask and stirred at room temperature for 1 hour. Next, a reflux condenser with a water receiver was attached to the flask, and the temperature was raised to 180°C while blowing in nitrogen gas, and then the temperature was maintained at 180°C for 5 hours, and the reaction was carried out while removing water. The solution thus obtained was cooled to room temperature. Next, 50 g of polybutadiene resin (manufactured by CRAY VALLEY, product name: Ricon130MA8) dissolved in NMP in solid content, 50 g of the above thermoplastic resin in solid content, 2 g of hardener (manufactured by NOF Corporation, product name: Perhexine 25B), 10 g of epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name: NC3000H) dissolved in NMP in solid content, 1 g of G8009L (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., product name), and 70 g of silica slurry [manufactured by Admatechs; product name: SC2050-KNK] in solid content were mixed and stirred for 30 minutes to uniformly disperse, forming a varnish of a resin composition for forming an insulating layer between wiring layers. The obtained varnish of the resin composition was applied onto a release-treated PET film (thickness 38 μm, product name: NR-1) using a bench coater. The film thickness of the coating film of the resin composition was adjusted to 10 μm after drying using an applicator. Next, the coating of the resin composition was dried by heating at 120°C for 20 minutes to form a curable film (material C) on the PET film. Then, the PET film was removed, and the curable film (material C) was used to form the wiring interlayer insulating layer 57. The wiring interlayer insulating layer 57 (cured product of material C) of Example 6 had a moisture absorption rate of 1.0 mass% or less, a chloride ion concentration of 5 ppm or less, an elongation at break of 3%, and a storage modulus at 40°C of 11 GPa.
[0199] Comparative Example 1 A measurement and evaluation sample 50 was formed in the same manner as in Example 1, except that the wiring interlayer insulating layer 57 was formed using the following material D. However, the attached material D was exposed to light with a high-precision parallel exposure machine (manufactured by ORC Manufacturing Co., Ltd., product name: EXM-1172-B-∞) at a dose of 500 mJ / cm. 2 After the exposure treatment, a thermal curing treatment was carried out. The above-mentioned high acceleration life test was carried out on this measurement and evaluation sample 50. The results of the high acceleration life test of Comparative Example 1 are shown in Table 1 below.
[0200] <Material D> Material D is a film having a thickness of 10 μm, formed from the same photosensitive insulating resin as the photosensitive insulating resin film 52, etc. The cured product of material D had a moisture absorption rate of 2.0 mass % and a chloride ion concentration of 8.6 ppm.
[0201] Comparative Example 2 Except for setting the line width L and space width S to 2 μm, the measurement and evaluation sample 50 was formed in the same manner as in Comparative Example 1, and the above-mentioned high acceleration life test was performed. The results of the high acceleration life test of Comparative Example 2 are shown in Table 1 below.
[0202] Comparative Example 3 A measurement and evaluation sample 50 was formed in the same manner as in Comparative Example 1, except that the wiring interlayer insulating layer 57 was formed using the following material E, and the line width L and space width S were set to 3 μm. The above-mentioned high acceleration life test was performed on this measurement and evaluation sample 50. The results of the high acceleration life test of Comparative Example 3 are shown in Table 1 below.
[0203] <Material E> FZ-2700GA (product name, manufactured by Hitachi Chemical Co., Ltd.) was used as material E. The cured product of material E had a moisture absorption rate of 1.3 mass % and a chloride ion concentration of 6.3 ppm.
[0204] Comparative Example 4 A measurement evaluation sample 50 was formed in the same manner as in Comparative Example 1, except that the following material F was used as a curable film for forming the wiring interlayer insulating layer 57, and the line width L and space width S were set to 3 μm. The above-mentioned high acceleration life test was performed on this measurement evaluation sample 50. The results of the high acceleration life test of Comparative Example 4 are shown in Table 1 below.
[0205] <Material F> First, in order to synthesize a thermoplastic resin, 2.16 g of 5,5'-methylene-bis(anthranilic acid), 15.13 g of aliphatic ether diamine (manufactured by BASF Japan Ltd., product name: D-400), 1.63 g of 1,1,3,3-tetramethyl-1,3-bis(4-aminophenyl)disiloxane (manufactured by Shin-Etsu Chemical Co., Ltd., product name: LP-7100), and 115 g of NMP were mixed in a flask equipped with a stirrer, a thermometer, and a nitrogen replacement device. Next, 16.51 g of oxydiphthalic anhydride (ODPA) was added to the flask, and the mixture was stirred at room temperature for 1 hour. Then, the temperature was raised to 180°C while blowing nitrogen gas into the flask, and the temperature was maintained at 180°C for 5 hours, and the reaction was carried out while removing water. The solution thus obtained was cooled to room temperature. 30 g of epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name: NC3000H) dissolved in NMP was mixed with 50 g of the above thermoplastic resin in solid content, and 1 g of 2P4MHZ (manufactured by Shikoku Kasei Kogyo Co., Ltd., product name) as a curing agent, and the mixture was stirred for 30 minutes to uniformly disperse the mixture, forming a varnish of the resin composition. The obtained varnish of the resin composition was applied to a release-treated PET film (thickness 38 μm, product name: NR-1) using a tabletop coater. The coating film of the resin composition was adjusted to 10 μm after drying using an applicator. Next, the coating film of the resin composition was dried by heating at 120° C. for 20 minutes to form a curable film (material F) on the PET film. Then, the PET film was removed, and the curable film (material F) was used to form a wiring interlayer insulating layer. The wiring interlayer insulating layer (cured product of material F) of Comparative Example 4 had a moisture absorption rate of 1.2 mass% and a chloride ion concentration of 5 ppm or less.
[0206] [Table 1]
[0207] In Table 1 above, when the moisture absorption rate of the wiring interlayer insulating layer 57 is 1.0 mass % or less, it is indicated as "Y", and when the moisture absorption rate of the wiring interlayer insulating layer 57 exceeds 1.0 mass %, it is indicated as "N". As can be seen from Table 1, the results of the high acceleration life test of Examples 1 to 6 were all rated A, while the results of the high acceleration life test of Comparative Examples 1 to 4 were all rated B. These results show that the insulation reliability of the measurement evaluation sample 50 differs greatly depending on the presence or absence of the wiring interlayer insulating layer 57 having a moisture absorption rate of 1.0 mass % or less.
[0208] Fig. 15 is a graph showing the results of high acceleration life tests of Example 3 and Comparative Example 2. In Fig. 13, the horizontal axis indicates time, and the vertical axis indicates the resistance value between the first wiring 55a and the second wiring 55b. In Fig. 15, data 61 is the test result of Example 3, and data 62 is the test result of Comparative Example 2.
[0209] As shown in FIG. 15, in Example 3, even after 300 hours had passed since the start of the test, the resistance between the first wiring 55a and the second wiring 55b was 1×10 7 On the other hand, in Comparative Example 2, the resistance value suddenly decreased to 1×10 7 It became less than Ω.
[0210] Fig. 16(a) is a diagram showing the observation of the measurement and evaluation sample 50 of Example 3 after the high acceleration life test, and Fig. 16(b) is a diagram showing the observation of the measurement and evaluation sample 50 of Comparative Example 2 after the high acceleration life test. As shown in Fig. 16(b), in Comparative Example 2, it was confirmed that at least the first wiring 55a and the second wiring 55b were corroded due to some factor. On the other hand, as shown in Fig. 16(b), in Example 3, no obvious corrosion was confirmed in the wiring, etc.
[0211] (Examples 7 to 13) The following components were mixed together to obtain the composition shown in Table 1, and stirred at 25° C. for 30 minutes or more, and then filtered through a #200 nylon mesh (mesh opening: 75 μm) to obtain a resin composition (varnish).
[0212] Component (A-1): Maleimide compound represented by the following formula (mixture of n = 1 to 10, weight average molecular weight: about 15,000 to 20,000) [ka]
[0213] Component (A-2): A mixture of maleimide compounds represented by the following formula: [ka] [ka]
[0214] Component (B): Compound having a (meth)acryloyl group (manufactured by Shin-Nakamura Chemical Co., Ltd., product name: A-DCP) Component (C): Photoradical polymerization initiator (manufactured by BASF, product name: Irgacure907) Component (D-1): silane coupling agent having an epoxy group (manufactured by Shin-Etsu Chemical Co., Ltd., product name: X-12-984S) Component (D-2): silane coupling agent having an epoxy group (manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-403)
[0215] The resin composition (varnish) of each example was evaluated as follows, and the results are shown in Table 2.
[0216] <Dielectric properties (dielectric constant: Dk, dielectric tangent: Df) evaluation> To evaluate the dielectric properties, the varnish was applied to copper foil using a tabletop coater and dried to a thickness of 50μm after drying to obtain a resin film (semi-cured). The obtained resin film (semi-cured) was then irradiated with UV at 2000mJ / cm2. Resin films were similarly formed and laminated on the prepared resin film, until the resin film had a thickness of 300μm. The copper foil support was then removed by physical peeling or etching to obtain a resin film for evaluation. The resin film was cut into a length of 60 mm, width of 2 mm, and thickness of 0.3 mm, and used as a test piece to measure the dielectric properties by the cavity resonator perturbation method. The measuring device used was the Agilent Technologies Vector Network Analyzer E8364B, the cavity resonator was the Kanto Electronics Application Development Co., Ltd. CP531 (10 GHz band resonator), and the measurement program was CPMA-V2. The conditions were a frequency of 10 GHz and a measurement temperature of 25°C.
[0217] <Moisture absorption rate measurement> The varnish was applied to a wafer (6 inch diameter, 400 μm thick) using a spin coater and dried at 90°C for 5 minutes to form a resin layer. 2 After being exposed to light and cured, the sample was heated at 180°C for 1 hour to prepare a sample. The sample was left to stand for 200 hours in a thermo-hygrostat (manufactured by Espec Corporation, product name: EHS-221MD) set at a relative humidity of 85% and 130°C. The temperature in the thermo-hygrostat was then lowered to 50°C, after which the sample was taken out and a part of the resin was scraped off from the silicon wafer. The scraped off part of the resin was measured using a thermogravimetry and differential thermal analyzer (manufactured by Hitachi High-Tech Science Corporation, product name: TG / DTA6300) under the conditions of a heating rate of 10°C / min, a nitrogen flow of 400mL / min, and a temperature range of 25°C to 150°C. The weight loss rate at 150°C was calculated as the moisture absorption rate.
[0218] <Measurement of elongation rate> A sample obtained by cutting a resin film produced by the same method as described above into a length of 30 mm and a width of 5 mm was measured for elongation at break when measured at a feed rate of 5 mm / min using a small benchtop tester (manufactured by Shimadzu Corporation, product name: EZ-S).
[0219] <Evaluation of Fine Wiring Formability> A varnish was applied by spin coating on a silicon wafer (6-inch diameter, 400 μm thick), and heated and dried at 90 °C for 5 minutes to form a resin film on the silicon wafer. At that time, the spin coating conditions were adjusted so that the film thickness of the resin after drying would be 5 μm. Next, a negative-type pattern mask with Line / Space (L / S (μm / μm)) of 200 / 200, 100 / 100, 80 / 80, 60 / 60, 50 / 50, 40 / 40, 30 / 30, 20 / 20, 10 / 10, 7 / 7, 5 / 5, 4 / 4, 3 / 3 and a via diameter of 50, 40, 30, 20, 10, 7, 5, 4, 3 μm was placed, and exposed using a high-precision parallel exposure machine (manufactured by OAK Corporation, product name: EXM-1172-B-∞) at 1000 mJ / cm 2 and exposed. Further, additional heating was performed under the conditions of 100 °C for 1 minute to obtain a sample. The obtained sample was immersed in cyclopentanone at room temperature for 60 seconds while shaking, then rinsed with cyclopentanone and then immersed in isopropyl alcohol at room temperature for 5 seconds. Thereafter, isopropyl alcohol was volatilized by blowing compressed air or the like. The fine wiring formability was confirmed with a metal microscope for peeling of the resin film from the wafer, cracking of the resin film, presence or absence of roughness at the pattern edges, and presence or absence of residues at the bottom of the pattern where the resin was developed. Table 2 shows the minimum L / S and via diameter for which these defects could not be confirmed.
[0220] <b-HAST Resistance> A pattern was formed in the same manner as in the above high-acceleration life test. Next, it was plated up by electroless / electrolytic copper plating or the like, and the surface was planarized by CMP. The mask size was adjusted so that L / S (μm / μm) would be 3 / 3 and 5 / 5. Next, varnish was laminated on the obtained wiring by spin coating and dried at 90°C for 5 minutes. When spin coating, polyimide tape was attached to the 55c and 55d parts of the wiring to prevent the resin from being coated, and the polyimide tape was peeled off after UV curing. The spin coating conditions were adjusted so that the thickness of the resin film was 5 μm. The UV was 1000 mJ / cm 2 After irradiation, the resin film was cured by heating at 180°C for 1 hour. Note that between the substrate wafer (6 inch diameter, 400 μm thickness) and the wiring layer, there is a resin layer that was prepared in exactly the same way except for forming the pattern. A voltage of 3.3 V was applied to the first connection wiring 55c and the second connection wiring 55d of the obtained wiring under conditions of 85% humidity and 130° C., and the wiring was left to stand for a predetermined time. In this way, the change in the insulation between the first wiring 55a and the second wiring 55b over time was measured. In this test, the resistance value between the first wiring 55a and the second wiring 55b was 1×10 for more than 300 hours. 6 Those that were Ω or higher were rated as "A" (b-HAST resistant), and those that were not were rated as "B" (b-HAST not resistant).
[0221] [Table 2] [Explanation of symbols]
[0222] 1...substrate, 2A to 2D...semiconductor chip, 3A, 3B...underfill, 4...insulating material, 10...semiconductor wiring layer laminate, 11...substrate, 13...copper wiring, 13A...copper layer, 14...copper wiring, 14A...copper layer, 15, 16...barrier metal film, 17, 18...interlayer insulating layer, 21...organic insulating layer, 21a...groove, 22...organic insulating layer, 22a...groove, 100...semiconductor package, L...line width, S...space width.
Claims
1. A material comprising a PET film and a curable film formed from a resin composition, The curable film is used to form an insulating layer between wiring layers in contact with fine copper wiring having a line width and space width of 5 μm or less, The resin composition contains a curable resin and a coupling agent, and does not contain an inorganic filler; The curable resin contains a compound represented by the following formula (VIII): 【Chemistry 1】 [In the formula, Z 1 represents a divalent hydrocarbon group containing a chain-like alkylene group having a main chain having 4 or more carbon atoms.] a moisture absorption rate of a cured product of the resin composition after being placed in an environment of 130° C. and a relative humidity of 85% for 200 hours is 1% by mass or less; A material, in which the concentration of chloride ions in a cured product of the resin composition is 5 ppm or less (excluding the case where the resin composition contains a compound having a maleimide group, a divalent group having at least two imide bonds, and a saturated or unsaturated divalent hydrocarbon group).
2. The material according to claim 1 , wherein the hydrocarbon group has 8 or more carbon atoms.
3. The resin composition further contains a curing agent, The material of claim 1 or 2, wherein the hardener comprises a photoradical polymerization initiator.
4. The material according to any one of claims 1 to 3, wherein the resin composition further contains a compound having a (meth)acryloyl group.
5. The material according to any one of claims 1 to 4, wherein the resin composition further contains a thermoplastic resin.
6. The material according to any one of claims 1 to 5, wherein the breaking elongation of the cured product of the resin composition is 5 to 200%.
7. The material according to any one of claims 1 to 6, wherein the storage modulus of the cured product of the resin composition at 40 ° C. is 10 MPa to 5 GPa.
8. The material according to any one of claims 1 to 7, wherein the glass transition temperature of the cured product of the resin composition is 120 to 240 ° C.
9. The material according to any one of claims 1 to 8, wherein the cured product of the resin composition has a dielectric constant of 3.0 or less at 10 GHz.
10. The material according to any one of claims 1 to 9, wherein the dielectric tangent at 10 GHz of the cured product of the resin composition is 0.005 or less.
11. The material according to any one of claims 1 to 10, wherein the 5% weight loss temperature of the cured product of the resin composition is 300°C or higher.
12. A plurality of wiring layers including an organic insulating layer, fine copper wiring having a line width and a space width of 5 μm or less provided in the organic insulating layer, and a barrier metal film separating the copper wiring and the organic insulating layer; an inter-wiring layer insulating layer provided between the plurality of wiring layers; Equipped with a part of a surface of the copper wiring is exposed on one or both main surfaces of the wiring layer, and the wiring interlayer insulating layer is in contact with the exposed surface of the copper wiring; The wiring layer laminate for semiconductor use, wherein the wiring interlayer insulating layer is a cured product of the curable film according to any one of claims 1 to 11.
Citation Information
Patent Citations
Low thermal expansion polyimide and electrical device using same
JP1987184025A
Adhesive composition and adhesive sheet for semiconductor device
JP2007091794A
Composite body, method of manufacturing the same, and semiconductor device
JP2010258415A
Circuit board and method for manufacturing the same
JP2011003884A
A multi-chip package and a method for providing die-to-die interconnects for a multi-chip package.
JP2012529770A