Wiring board and semiconductor device

A method for manufacturing flexible wiring boards with embedded layers addresses the need for thinner, foldable electronic components by using a thermosetting resin composition and resin film layer process, ensuring excellent bendability and reflow performance.

JP7552786B2Active Publication Date: 2024-09-18AJINOMOTO CO INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023076799
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-09-18
Estimated Expiration
2035-09-17

Smart Images

  • Figure 0007552786000015
    Figure 0007552786000015
  • Figure 0007552786000023
    Figure 0007552786000023
  • Figure 0007552786000010
    Figure 0007552786000010
Patent Text Reader

Abstract

To provide a flexible wiring board with an embedded wiring layer, and to provide a semiconductor device.SOLUTION: A wiring board with a wiring layer comprises a conductor layer 40, a resin film layer 22, an insulating layer 23, and an embedded wiring layer 14 embedded in the insulating layer. The insulating layer 23 is formed by hardening one or more curing agents selected from an epoxy resin, a phenolic curing agent, a naphtholic curing agent, an active ester curing agent, and a cyanate ester curing agent, and a resin composition layer containing an inorganic filler (excluding one containing a phenoxy resin with a fluorene structure). The resin film layer contains polyimide, polyethylene terephthalate, polyethylene naphthalate, liquid crystal polymer, polyphenylene sulphide, polyetheretherketone, polybenzimidazole, aramid, polyamideimide, or polyetherimide.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a wiring board, and further to a wiring board and a semiconductor device. [Background technology]

[0002] A widely used method for manufacturing wiring boards (printed wiring boards) is the build-up method, in which circuit-forming conductor layers and insulating layers are alternately stacked, and it is known that the insulating layers are formed by curing a resin composition (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-82535 A Summary of the Invention [Problem to be solved by the invention]

[0004] In recent years, electronic devices have been made lighter, thinner, and smaller. Accordingly, there is a demand for flexible wiring boards that can be folded and stored in electronic devices. In addition, in order to enable further thinning of wiring boards, there is a demand for wiring boards that include embedded wiring layers.

[0005] An object of the present invention is to provide a novel method for producing a flexible wiring board having a buried type wiring layer. [Means for solving the problem]

[0006] That is, the present invention includes the following. [1] (1) A step of preparing a substrate with a wiring layer, the substrate having a substrate and a wiring layer provided on at least one surface of the substrate; (2) a step of laminating an adhesive sheet including (i) a thermosetting resin composition layer and (ii) a resin film layer onto a substrate having a wiring layer such that the wiring layer is embedded in the (i) thermosetting resin composition layer, and thermally curing the resulting layer to form an insulating layer; (3) forming a via hole in the insulating layer; (4) forming a conductor layer; and (5) removing the substrate; A method for manufacturing a wiring board comprising: [2] The method according to [1], wherein the adhesive sheet further comprises (iii) a metal foil or a thermosetting resin composition layer, and comprises, in this order, (i) a thermosetting resin composition layer, (ii) a resin film layer, and (iii) a metal foil or a thermosetting resin composition layer. [3] The method according to [1] or [2], wherein the formation of the via hole is carried out by laser irradiation. [4] The method according to any one of [1] to [3], further comprising a step of performing a roughening treatment prior to the step of forming the conductor layer. [5] The method according to any one of [1] to [4], wherein the wiring board is a flexible wiring board. [6] The method according to any one of [1] to [5], wherein the breaking elongation of the adhesive sheet after heat curing is 2% or more. [7] (ii) The method according to any one of [1] to [6], wherein the surface of the resin film layer is corona-treated, plasma-treated, or UV-treated. [8] The method according to any one of [1] to [7], wherein the metal foil is a copper foil. [9] The method according to any one of [1] to [8], wherein the minimum pitch of the wiring pattern is 40 μm or less.

[10] A wiring board comprising a resin film layer, an insulating layer, and an embedded wiring layer embedded in the insulating layer.

[11] The wiring board according to

[10] , which is a flexible wiring board.

[12] The wiring board according to

[10] or

[11] , wherein the thickness of the insulating layer is 2 μm or more.

[13] The wiring board according to any one of

[10] to

[12] , wherein the resin film layer has a thickness of 2 μm or more.

[14] A semiconductor device comprising the wiring board according to any one of

[10] to

[13] . Effect of the Invention

[0007] According to the present invention, a novel method for producing a flexible wiring board having a buried type wiring layer can be provided.

[0008] Furthermore, according to the manufacturing method of the present invention, it is possible to provide a manufacturing method for a wiring board that has excellent bending properties and excellent reflow warpage behavior. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a schematic cross-sectional view for explaining a manufacturing process for a wiring board. [Diagram 2] FIG. 2 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Diagram 3] FIG. 3 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 4] FIG. 4 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Diagram 5] FIG. 5 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 6] FIG. 6 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 7] FIG. 7 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 8] FIG. 8 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 9] FIG. 9 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 10] FIG. 10 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 11] FIG. 11 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 12]FIG. 12 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 13] FIG. 13 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 14] FIG. 14 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 15] FIG. 15 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 16] FIG. 16 is a schematic cross-sectional view for explaining a manufacturing process for a wiring board. [Figure 17] FIG. 17 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 18] FIG. 18 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 19] FIG. 19 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 20] FIG. 20 is a schematic cross-sectional view for explaining a manufacturing process of a wiring board. [Figure 21] FIG. 21 is a schematic cross-sectional view for explaining a wiring board. [Figure 22] FIG. 22 is a schematic cross-sectional view for explaining a wiring board. [Diagram 23] FIG. 23 is a schematic cross-sectional view for explaining a wiring board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Before describing the method for producing a wiring board of the present invention, the adhesive sheet used in the production method will be described.

[0011] [Adhesive sheet] The adhesive sheet includes (i) a thermosetting resin composition layer, and (ii) a resin film layer. The adhesive sheet preferably further includes (iii) a metal foil or a thermosetting resin composition layer. In a preferred embodiment of the adhesive sheet, (i) the thermosetting resin composition layer and (ii) the resin film layer are bonded together, and (ii) the resin film layer and (iii) the metal foil or the thermosetting resin composition layer are bonded together. Each layer constituting the adhesive sheet will be described in detail below.

[0012] <(i) Thermosetting resin composition layer> The adhesive sheet includes a thermosetting resin composition layer (i). As will be described later in detail, when manufacturing a wiring board, the wiring layer is embedded in the thermosetting resin composition layer (i), thereby forming an embedded wiring layer. The thermosetting resin composition constituting the thermosetting resin composition layer (i) is not particularly limited, and it is sufficient that the cured product has sufficient insulation. Examples of such resin compositions include compositions containing a thermosetting resin and a curing agent thereof. As the thermosetting resin, a conventionally known thermosetting resin used when forming an insulating layer of a wiring board can be used, and among them, an epoxy resin is preferable. Therefore, in one embodiment, the thermosetting resin composition includes an epoxy resin (a) and a curing agent (b). The thermosetting resin composition may further include additives such as an inorganic filler (c), a thermoplastic resin (d), a curing accelerator (e), a flame retardant (f), and an organic filler (g), as necessary.

[0013] -(a) Epoxy resin- Examples of epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, etc. The epoxy resins may be used alone or in combination of two or more. The component (a) is preferably at least one selected from bisphenol A type epoxy resins, bisphenol F type epoxy resins, and biphenyl type epoxy resins.

[0014] The epoxy resin preferably contains an epoxy resin having two or more epoxy groups in one molecule. When the non-volatile component of the epoxy resin is 100 mass%, it is preferable that at least 50 mass% of the epoxy resin has two or more epoxy groups in one molecule. Among them, it is preferable to contain an epoxy resin having two or more epoxy groups in one molecule and being liquid at a temperature of 20°C (hereinafter referred to as "liquid epoxy resin") and an epoxy resin having three or more epoxy groups in one molecule and being solid at a temperature of 20°C (hereinafter referred to as "solid epoxy resin"). By using a liquid epoxy resin and a solid epoxy resin in combination as the epoxy resin, a resin composition having excellent flexibility can be obtained. In addition, the breaking strength of the cured product of the resin composition is also improved.

[0015] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, and epoxy resin having a butadiene structure are preferred, and bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, and naphthalene type epoxy resin are more preferred. Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resin) manufactured by DIC Corporation, "828US", "jER828EL" (bisphenol A type epoxy resin), "jER807" (bisphenol F type epoxy resin), "jER152" (phenol novolac type epoxy resin), and "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Corporation, and "ZX1" (bisphenol AF type epoxy resin) manufactured by Nippon Steel & Sumikin Chemical Co., Ltd. Examples of such epoxy resins include "EX-721" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nagase ChemteX Corporation, "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) and "PB-3600" (epoxy resin having a butadiene structure) manufactured by Daicel Corporation, and "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane) manufactured by Nippon Steel Chemical Co., Ltd. These may be used alone or in combination of two or more types.

[0016] As the solid epoxy resin, naphthalene-type tetrafunctional epoxy resin, cresol novolac-type epoxy resin, dicyclopentadiene-type epoxy resin, trisphenol-type epoxy resin, naphthol-type epoxy resin, biphenyl-type epoxy resin, naphthylene ether-type epoxy resin, anthracene-type epoxy resin, bisphenol A-type epoxy resin, and tetraphenylethane-type epoxy resin are preferred, and naphthalene-type tetrafunctional epoxy resin, naphthol-type epoxy resin, and biphenyl-type epoxy resin are more preferred. Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin), "HP-4700", "HP-4710" (naphthalene type tetrafunctional epoxy resin), "N-690" (cresol novolac type epoxy resin), "N-695" (cresol novolac type epoxy resin), "HP-7200" (dicyclopentadiene type epoxy resin), "HP-7200HH", "HP-7200H", "EXA7311", "EXA7311-G3", "EXA7311-G4", "EXA7311-G4S", "HP6000" (naphthylene ether type epoxy resin), and "EPPN-502H" (trisphenol type epoxy resin), "NC7000L" (naphthol novolac type epoxy resin), and "NC30 00H", "NC3000", "NC3000L", "NC3100" (biphenyl type epoxy resin), "ESN475V" (naphthol type epoxy resin) and "ESN485" (naphthol novolac type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd., "YX4000H", "YL6121" (biphenyl type epoxy resin), "YX4000HK" (bixylenol type epoxy resin), "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., "PG-100" and "CG-500" manufactured by Osaka Gas Chemical Co., Ltd., "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., "jER1010" (solid bisphenol A type epoxy resin) and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd., and the like.

[0017] The liquid epoxy resin is preferably an aromatic epoxy resin having two or more epoxy groups in one molecule and being liquid at a temperature of 20° C., and the solid epoxy resin is preferably an aromatic epoxy resin having three or more epoxy groups in one molecule and being solid at a temperature of 20° C. In the present invention, the aromatic epoxy resin means an epoxy resin having an aromatic ring structure in its molecule.

[0018] When liquid epoxy resin and solid epoxy resin are used in combination as epoxy resin, the ratio of the amounts (liquid epoxy resin: solid epoxy resin) is preferably in the range of 1:0.1 to 1:5 by mass. By setting the ratio of the amount of the liquid epoxy resin to the solid epoxy resin in this range, the following effects can be obtained: i) when used in the form of an adhesive sheet, appropriate adhesion is obtained; ii) when used in the form of an adhesive sheet, sufficient flexibility is obtained and handling is improved; and iii) a cured product having sufficient breaking strength can be obtained. From the viewpoint of the above effects i) to iii), the ratio of the amount of the liquid epoxy resin to the solid epoxy resin (liquid epoxy resin: solid epoxy resin) is more preferably in the range of 1:0.3 to 1:4 by mass, and even more preferably in the range of 1:0.6 to 1:3.

[0019] The content of the epoxy resin in the resin composition is preferably 5% by mass or more, more preferably 9% by mass or more, and even more preferably 13% by mass or more, from the viewpoint of obtaining an insulating layer exhibiting good mechanical strength and insulating reliability. The upper limit of the content of the epoxy resin is not particularly limited as long as the effects of the present invention are exhibited, but is preferably 50% by mass or less, more preferably 40% by mass or less.

[0020] In the present invention, the content of each component in the resin composition is a value when the non-volatile components in the resin composition are taken as 100 mass %, unless otherwise specified.

[0021] The epoxy equivalent of the epoxy resin is preferably 50 to 5000, more preferably 50 to 3000, even more preferably 80 to 2000, and even more preferably 110 to 1000. Within this range, the crosslink density of the cured product is sufficient, and an insulating layer with small surface roughness can be obtained. The epoxy equivalent can be measured according to JIS K7236, and is the mass of a resin containing one equivalent of an epoxy group.

[0022] The weight average molecular weight of the epoxy resin is preferably 100 to 5000, more preferably 250 to 3000, and further preferably 400 to 1500. Here, the weight average molecular weight of the epoxy resin is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).

[0023] -(b) Hardener- The curing agent is not particularly limited as long as it has the function of curing the epoxy resin, and examples thereof include phenol-based curing agents, naphthol-based curing agents, active ester-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, and carbodiimide-based curing agents. The curing agent may be used alone or in combination of two or more. The (b) component is preferably one or more selected from phenol-based curing agents, naphthol-based curing agents, active ester-based curing agents, and cyanate ester-based curing agents.

[0024] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferred. Also, from the viewpoint of adhesion to the wiring layer, a nitrogen-containing phenol-based curing agent is preferred, and a triazine skeleton-containing phenol-based curing agent is more preferred. Among them, from the viewpoint of highly satisfying heat resistance, water resistance, and adhesion to the wiring layer, a triazine skeleton-containing phenol novolac curing agent is preferred.

[0025] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN375", and "SN395" manufactured by Nippon Steel & Sumitomo Metal Corporation, and "LA7052", "LA7054", "LA3018", and "EXB-9500" manufactured by DIC Corporation.

[0026] From the viewpoint of obtaining an insulating layer having excellent adhesion to the wiring layer, an active ester-based curing agent is also preferred. The active ester-based curing agent is not particularly limited, but generally, a compound having two or more highly reactive ester groups in one molecule, such as phenol esters, thiophenol esters, N-hydroxyamine esters, and esters of heterocyclic hydroxy compounds, is preferably used. The active ester-based curing agent is preferably one obtained by a condensation reaction between a carboxylic acid compound and / or a thiocarboxylic acid compound and a hydroxy compound and / or a thiol compound. In particular, from the viewpoint of improving heat resistance, an active ester-based curing agent obtained from a carboxylic acid compound and a hydroxy compound is preferred, and an active ester-based curing agent obtained from a carboxylic acid compound and a phenol compound and / or a naphthol compound is more preferred. Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyromellitic acid. Examples of phenol compounds or naphthol compounds include hydroquinone, resorcin, bisphenol A, bisphenol F, bisphenol S, phenolphthaline, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucin, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, etc. Here, the term "dicyclopentadiene-type diphenol compounds" refers to diphenol compounds obtained by condensing one molecule of dicyclopentadiene with two molecules of phenol.

[0027] Specifically, active ester compounds containing a dicyclopentadiene-type diphenol structure, active ester compounds containing a naphthalene structure, active ester compounds containing an acetylated product of phenol novolac, and active ester compounds containing a benzoylated product of phenol novolac are preferred, and among these, active ester compounds containing a naphthalene structure and active ester compounds containing a dicyclopentadiene-type diphenol structure are more preferred. The "dicyclopentadiene-type diphenol structure" refers to a divalent structural unit consisting of phenylene-dicyclopentylene-phenylene.

[0028] Commercially available active ester curing agents include "EXB9451", "EXB9460", "EXB9460S", and "HPC-8000-65T" (manufactured by DIC Corporation) as active ester compounds containing a dicyclopentadiene-type diphenol structure, "EXB9416-70BK" (manufactured by DIC Corporation) as an active ester compound containing a naphthalene structure, "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester compound containing an acetylated product of phenol novolac, Examples of active ester compounds containing benzoyl derivatives of phenol novolac include "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "DC808" (manufactured by Mitsubishi Chemical Corporation) is an active ester-based curing agent which is an acetylated derivative of phenol novolac, and "YLH1026" (manufactured by Mitsubishi Chemical Corporation), "YLH1030" (manufactured by Mitsubishi Chemical Corporation), and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) are active ester-based curing agents which are benzoyl derivatives of phenol novolac.

[0029] Specific examples of benzoxazine-based curing agents include "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industries Co., Ltd.

[0030] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (both of which are phenol novolac-type multifunctional cyanate ester resins), "BA230" and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan Co., Ltd.

[0031] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.

[0032] The ratio of the amount of epoxy resin to the curing agent is preferably 1:0.01 to 1:2, more preferably 1:0.015 to 1:1.5, and even more preferably 1:0.02 to 1:1, in terms of the ratio of [total number of epoxy groups in the epoxy resin] to [total number of reactive groups in the curing agent]. Here, the reactive groups in the curing agent are active hydroxyl groups, active ester groups, etc., and vary depending on the type of curing agent. The total number of epoxy groups in the epoxy resin is the value obtained by dividing the solid content mass of each epoxy resin by the epoxy equivalent, and the total number of reactive groups in the curing agent is the value obtained by dividing the solid content mass of each curing agent by the reactive group ...

[0033] In one embodiment, the thermosetting resin composition includes the above-mentioned (a) epoxy resin and (b) curing agent. The thermosetting resin composition preferably includes (a) a mixture of a liquid epoxy resin and a solid epoxy resin as the epoxy resin (the mass ratio of the liquid epoxy resin:solid epoxy resin is preferably 1:0.1 to 1:5, more preferably 1:0.3 to 1:4, and even more preferably 1:0.6 to 1:3), and (b) one or more types selected from the group consisting of a phenol-based curing agent, a naphthol-based curing agent, an active ester-based curing agent, and a cyanate ester-based curing agent (preferably one or more types selected from the group consisting of an active ester-based curing agent and a cyanate ester-based curing agent).

[0034] The content of the curing agent in the thermosetting resin composition is not particularly limited, but is preferably 30% by mass or less, more preferably 25% by mass or less, and further preferably 20% by mass or less. There is no particular lower limit, but it is preferably 2% by mass or more.

[0035] -(c) Inorganic filler- The material of the inorganic filler is not particularly limited, and examples thereof include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Moreover, as the silica, spherical silica is preferred. The inorganic filler may be used alone or in combination of two or more.

[0036] From the viewpoint of good embeddability, the average particle size of the inorganic filler is preferably 2 μm or less, more preferably 1 μm or less, even more preferably 0.8 μm or less, and even more preferably 0.6 μm or less. The lower limit of the average particle size is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more. Examples of commercially available inorganic fillers having such an average particle size include "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd., "UFP-30" manufactured by Denki Kagaku Kogyo Co., Ltd., "Silfill NSS-3N", "Silfill NSS-4N", and "Silfill NSS-5N" manufactured by Tokuyama Co., Ltd., and "SOC2" and "SOC1" manufactured by Admatechs Co., Ltd.

[0037] The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, a particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample is preferably an inorganic filler dispersed in water using ultrasonic waves. The "LA-500" manufactured by Horiba, Ltd. can be used as a laser diffraction / scattering particle size distribution measuring device.

[0038] From the viewpoint of improving moisture resistance and dispersibility, the inorganic filler is preferably treated with one or more surface treatment agents such as an aminosilane coupling agent, an epoxysilane coupling agent, a mercaptosilane coupling agent, a silane coupling agent, an organosilazane compound, and a titanate coupling agent. Examples of commercially available surface treatment agents include "KBM403" (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM803" (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBE903" (3-aminopropyltriethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., "SZ-31" (hexamethyldisilazane) manufactured by Shin-Etsu Chemical Co., Ltd., "KBM103" (phenyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., and "KBM-4803" (long-chain epoxy type silane coupling agent) manufactured by Shin-Etsu Chemical Co., Ltd.

[0039] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin varnish or the melt viscosity in the form of a sheet, it is more preferable that the melt viscosity is 1 mg / m 2 Less than 0.8 mg / m is preferred. 2Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0040] The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0041] The content of the inorganic filler in the thermosetting resin composition is preferably 20% by mass or more, more preferably 30% by mass or more, from the viewpoint of obtaining an insulating layer with a low thermal expansion coefficient. The upper limit of the content of the inorganic filler in the thermosetting resin composition is preferably 85% by mass or less, more preferably 80% by mass or less, from the viewpoint of the mechanical strength, particularly elongation, of the insulating layer.

[0042] -(d)Thermoplastic resin- Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polybutadiene resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polycarbonate resin, polyetheretherketone resin, and polyester resin, and phenoxy resin is preferable. The thermoplastic resin may be used alone or in combination of two or more kinds.

[0043] The polystyrene-equivalent weight average molecular weight of the thermoplastic resin is preferably in the range of 8,000 to 70,000, more preferably in the range of 10,000 to 60,000, and even more preferably in the range of 20,000 to 60,000. The polystyrene-equivalent weight average molecular weight of the thermoplastic resin is measured by gel permeation chromatography (GPC). Specifically, the polystyrene-equivalent weight average molecular weight of the thermoplastic resin is measured at a column temperature of 40°C using a measuring device LC-9A / RID-6A manufactured by Shimadzu Corporation, a column Shodex K-800P / K-804L / K-804L manufactured by Showa Denko K.K., and chloroform or the like as a mobile phase, and can be calculated using a calibration curve of standard polystyrene.

[0044] Examples of the phenoxy resin include phenoxy resins having one or more skeletons selected from the group consisting of bisphenol A skeleton, bisphenol F skeleton, bisphenol S skeleton, bisphenolacetophenone skeleton, novolac skeleton, biphenyl skeleton, fluorene skeleton, dicyclopentadiene skeleton, norbornene skeleton, naphthalene skeleton, anthracene skeleton, adamantane skeleton, terpene skeleton, and trimethylcyclohexane skeleton. The terminal of the phenoxy resin may be any functional group such as a phenolic hydroxyl group or an epoxy group. The phenoxy resin may be used alone or in combination of two or more. Specific examples of phenoxy resins include "1256" and "4250" (both of which are phenoxy resins containing a bisphenol A skeleton), "YX8100" (phenoxy resin containing a bisphenol S skeleton), and "YX6954" (phenoxy resin containing a bisphenol acetophenone skeleton), all manufactured by Mitsubishi Chemical Corporation. Other examples include "FX280" and "FX293" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "YX6954BH30", "YX7553", "YX7553BH30", "YL7769BH30", "YL6794", "YL7213", "YL7290", and "YL7482" manufactured by Mitsubishi Chemical Corporation.

[0045] Examples of polyvinyl acetal resins include polyvinyl formal resins and polyvinyl butyral resins, and polyvinyl butyral resins are preferred.Specific examples of polyvinyl acetal resins include "Denka Butyral 4000-2", "Denka Butyral 5000-A", "Denka Butyral 6000-C", and "Denka Butyral 6000-EP" manufactured by Denki Kagaku Kogyo Co., Ltd., and S-LEC BH series, BX series (e.g. BX-5Z), KS series (e.g. KS-1), BL series, and BM series manufactured by Sekisui Chemical Co., Ltd.

[0046] Specific examples of polyimide resins include "Rikacoat SN20" and "Rikacoat PN20" manufactured by New Japan Chemical Co., Ltd. Specific examples of polyimide resins also include modified polyimides such as linear polyimides obtained by reacting bifunctional hydroxyl-terminated polybutadiene, a diisocyanate compound, and a tetrabasic acid anhydride (polyimides described in JP-A-2006-37083), and polysiloxane skeleton-containing polyimides (polyimides described in JP-A-2002-12667 and JP-A-2000-319386, etc.).

[0047] Specific examples of polyamide-imide resins include "Viromax HR11NN" and "Viromax HR16NN" manufactured by Toyobo Co., Ltd. Specific examples of polyamide-imide resins also include modified polyamide-imides such as "KS9100" and "KS9300" (polysiloxane skeleton-containing polyamide-imide) manufactured by Hitachi Chemical Co., Ltd.

[0048] A specific example of the polyethersulfone resin is "PES5003P" manufactured by Sumitomo Chemical Co., Ltd.

[0049] Specific examples of polysulfone resins include polysulfones "P1700" and "P3500" manufactured by Solvay Advanced Polymers, Inc.

[0050] Among them, the thermoplastic resin is preferably a phenoxy resin or a polyvinyl acetal resin. Therefore, in a preferred embodiment, the thermoplastic resin includes one or more selected from the group consisting of a phenoxy resin and a polyvinyl acetal resin.

[0051] When the thermosetting resin composition contains a thermoplastic resin, the content of the thermoplastic resin is preferably 0.5% by mass to 60% by mass, more preferably 3% by mass to 50% by mass, and further preferably 5% by mass to 40% by mass.

[0052] -(e) Curing accelerator- Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, guanidine-based curing accelerators, and metal-based curing accelerators, and phosphorus-based curing accelerators, amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are preferred, and amine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators are more preferred. The curing accelerator may be used alone or in combination of two or more.

[0053] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.

[0054] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, with 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene being preferred.

[0055] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.

[0056] As the imidazole-based curing accelerator, a commercially available product may be used, for example, "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0057] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of such biguanide include o-[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide. Of these, dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred.

[0058] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0059] The content of the curing accelerator in the thermosetting resin composition is not particularly limited, but is preferably 0.01% by mass to 3% by mass when the total amount of non-volatile components of the epoxy resin and the curing agent is taken as 100% by mass.

[0060] -(f) Flame retardants- Examples of the flame retardant include organic phosphorus flame retardants, organic nitrogen-containing phosphorus compounds, nitrogen compounds, silicone flame retardants, metal hydroxides, etc. The flame retardants may be used alone or in combination of two or more.

[0061] As the flame retardant, a commercially available product may be used, for example, "HCA-HQ" manufactured by Sanko Co., Ltd.

[0062] When the thermosetting resin composition contains a flame retardant, the content of the flame retardant is not particularly limited, but is preferably 0.5% by mass to 20% by mass, more preferably 0.5% by mass to 15% by mass, and even more preferably 0.5% by mass to 10% by mass.

[0063] -(g)Organic filler- The thermosetting resin composition may contain any organic filler that can be used in forming an insulating layer for a printed wiring board, such as rubber particles, polyamide fine particles, silicone particles, and the like.

[0064] As the rubber particles, commercially available products may be used, for example, "EXL-2655" manufactured by Dow Chemical Japan Ltd., and "AC3816N" manufactured by Ganz Chemical Co., Ltd.

[0065] When the thermosetting resin composition contains an organic filler, the content of the organic filler is preferably 0.1 mass % to 20 mass %, more preferably 0.2 mass % to 10 mass %, and even more preferably 0.3 mass % to 5 mass %, or 0.5 mass % to 3 mass %.

[0066] -Other ingredients- The thermosetting resin composition may further contain other additives as necessary. Examples of such other additives include organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds, as well as resin additives such as thickeners, defoamers, leveling agents, adhesion promoters, and colorants.

[0067] From the viewpoint of producing a flexible wiring board, the thermosetting resin composition preferably further contains a polyimide resin having a polybutadiene structure, a urethane structure, an imide structure in the molecule, and a phenol structure at the molecular end. When the polyimide resin is contained, the content is preferably 10% by mass to 85% by mass, more preferably 15% by mass to 50% by mass, and further preferably 20% by mass to 30% by mass.

[0068] For details of the polyimide, reference can be made to the description in International Publication No. 2008 / 153208, the contents of which are incorporated herein by reference.

[0069] From the viewpoint of thinning the wiring board, the thickness of the thermosetting resin composition layer is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, even more preferably 40 μm or less or 20 μm or less. The lower limit of the thickness of the thermosetting resin composition layer is not particularly limited, but is preferably 2 μm or more, more preferably 5 μm or more.

[0070] From the viewpoint of obtaining good wiring embeddability, the minimum melt viscosity of the thermosetting resin composition layer in the adhesive sheet is preferably 9000 poise (900 Pa·s) or less, more preferably 8000 poise (800 Pa·s) or less, even more preferably 4000 poise (400 Pa·s) or less, 3500 poise (350 Pa·s) or less, or even more preferably 3000 poise (300 Pa·s) or less. The lower limit of the minimum melt viscosity is preferably 100 poise (10 Pa·s) or more, more preferably 200 poise (20 Pa·s) or more, even more preferably 250 poise (25 Pa·s) or more.

[0071] The minimum melt viscosity of the thermosetting resin composition layer refers to the minimum viscosity exhibited by the thermosetting resin composition layer when the resin of the thermosetting resin composition layer is melted. In detail, when the thermosetting resin composition layer is heated at a constant heating rate to melt the resin, the melt viscosity decreases with increasing temperature in the initial stage, and then increases with increasing temperature beyond a certain level. The minimum melt viscosity refers to the melt viscosity at such a minimum point. The minimum melt viscosity of the thermosetting resin composition layer can be measured by a dynamic viscoelasticity method, and can be measured, for example, according to the method described in <Measurement of the minimum melt viscosity of the thermosetting resin composition layer> described later.

[0072] <(ii) Resin Film Layer> The adhesive sheet includes (ii) a resin film layer. In the present invention, by using an adhesive sheet including a resin film layer, it becomes possible to manufacture a flexible wiring board.

[0073] The resin film layer is not particularly limited as long as it can be bent to produce a flexible wiring board, and examples of the material include polyimide, polyethylene terephthalate, polyethylene naphthalate, liquid crystal polymer, polyphenylene sulfide, polyether ether ketone, polybenzimidazole, aramid, polyamideimide, polyetherimide, and the like.

[0074] The glass transition temperature of the resin film layer is preferably 150°C or higher, more preferably 170°C or higher, and even more preferably 200°C or higher or 250°C or higher. The upper limit is not particularly limited, but is generally 500°C or lower. The glass transition temperature of the resin film layer can be measured according to the method described in JIS K 7179, specifically, by using thermomechanical analysis (TMA), dynamic mechanical analysis (DMA), etc. Examples of thermomechanical analysis (TMA) include TMA-SS6100 (manufactured by Seiko Instruments Inc.) and TMA-8310 (manufactured by Rigaku Corporation), and examples of dynamic mechanical analysis (DMA) include DMS-6100 (manufactured by Seiko Instruments Inc.). In addition, when the glass transition temperature is higher than the decomposition temperature and the glass transition temperature is not actually observed, the decomposition temperature can be used as a standard instead of the glass transition temperature. The decomposition temperature is defined as the temperature at which the mass loss rate is 5% when measured according to the method described in JIS K 7120.

[0075] The linear thermal expansion coefficient of the resin film layer is preferably 40 ppm / ° C. or less, more preferably 30 ppm / ° C. or less, and even more preferably 20 ppm / ° C. or less, 15 ppm / ° C. or less, 10 ppm / ° C. or less, or 5 ppm / ° C. or less. From a practical standpoint, the lower limit is preferably −20 ppm / ° C. or more, more preferably −15 ppm / ° C. or more, and even more preferably −10 ppm / ° C. or more.

[0076] The surface of the resin film layer may be corona-treated, plasma-treated, or UV-treated. In a preferred embodiment, (i) the surface of the resin film layer on the side to be bonded to the thermosetting resin composition layer is corona-treated, plasma-treated, or UV-treated. By using such a resin film layer, the adhesion between the resin film layer and the thermosetting resin composition layer can be increased. The treatment conditions for the corona treatment, plasma treatment, or UV treatment may be appropriately determined depending on the material of the resin film layer, etc. In addition, (iii) the surface of the resin film layer on the side to be bonded to the thermosetting resin composition layer may be corona-treated, plasma-treated, or UV-treated.

[0077] The resin film layer may be a commercially available product, for example, "Upilex" manufactured by Ube Industries, Ltd., "Kapton" manufactured by DuPont-Toray Co., Ltd., "Pomilan" manufactured by Arakawa Chemical Industries, Ltd., "Apical" manufactured by Kaneka Corporation, aramid films such as "Mictron" manufactured by Toray Industries, Inc. and "Aramica" manufactured by Asahi Chemical Industry Co., Ltd., liquid crystal polymer films such as "Vexstar" manufactured by Kuraray Co., Ltd. and "Viac" manufactured by Japan Gore-Tex Co., Ltd., and polyether ether ketone such as "Sumilite FS-1100C".

[0078] From the viewpoint of thinning the wiring board, the thickness of the resin film layer is preferably 100 μm or less, more preferably 80 μm or less, further preferably 60 μm or less, 40 μm or less, or 20 μm or less. The lower limit of the thickness of the resin film layer is not particularly limited, but from the viewpoint of mechanical strength of the wiring board, it is preferably 1 μm or more, more preferably 2 μm or more.

[0079] <(iii) Metal foil or thermosetting resin composition layer> The adhesive sheet may further include (iii) a metal foil or a thermosetting resin composition layer. The adhesive sheet preferably includes (i) a thermosetting resin composition layer, (ii) a resin film layer, and (iii) a metal foil or a thermosetting resin composition layer in this order.

[0080] Examples of the metal foil include copper foil and aluminum foil, and copper foil is preferred. The copper foil may be a foil made of a single metal such as copper, or a foil made of an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.). The metal foil may be a laminated foil in which two or more metal foils are laminated.

[0081] The metal foil may have an adhesive layer on the side that is bonded to the resin film layer (ii). The adhesive layer is not particularly limited, and any known adhesive or pressure-sensitive adhesive may be used.

[0082] The thermosetting resin composition layer is the same as the above (i) thermosetting resin composition layer, and the preferred range is also the same.

[0083] (iii) From the viewpoint of thinning the wiring board, the thickness of the metal foil or the thermosetting resin composition layer is preferably 100 μm or less, more preferably 80 μm or less, and even more preferably 60 μm or less, 40 μm or less, 20 μm or less, or 10 μm or less. The lower limit of the thickness is not particularly limited, but can usually be 1 μm or more, 2 μm or more, 3 μm or more, etc.

[0084] The adhesive sheet may include other layers in addition to the above layers (i) to (iii). For example, the adhesive sheet may have a protective film layer, which will be described later, on the outermost surface.

[0085] <Method of manufacturing adhesive sheet> The manufacturing method of the adhesive sheet is not particularly limited as long as an adhesive sheet containing the above-mentioned (i) thermosetting resin composition layer and (ii) resin film layer in order can be obtained. Hereinafter, an example of a manufacturing method of an adhesive sheet in which the adhesive sheet contains the layer (iii) and the layer (iii) is a thermosetting resin composition layer is shown. First, a resin varnish is prepared by dissolving the thermosetting resin composition for the thermosetting resin composition layer (i) in an organic solvent, and this resin varnish is applied to a protective film described later using a die coater or the like. The applied resin varnish is dried to form the thermosetting resin composition layer (i) to obtain a laminate 1. Next, the resin film layer (ii) is laminated on the thermosetting resin composition layer (i) of the laminate 1 to obtain a laminate 2. Separately, a resin varnish is prepared by dissolving the thermosetting resin composition for the thermosetting resin composition layer (iii) in an organic solvent, and this resin varnish is applied to a protective film described later using a die coater or the like. The applied resin varnish is dried to form the thermosetting resin composition layer (iii) to obtain a laminate 3. An adhesive sheet is obtained by laminating the laminate 2 and the laminate 3 so that the (ii) resin film layer and the (iii) thermosetting resin composition layer are bonded to each other. When producing an adhesive sheet in which the (iii) layer is a metal foil, a laminate 3' in which the (ii) resin film layer and the (iii) metal foil are laminated may be used. An adhesive sheet is obtained by laminating the laminate 1 and the laminate 3' so that the (i) thermosetting resin composition layer and the (ii) resin film layer are bonded to each other.

[0086] Examples of the organic solvent include ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone, acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate, carbitols such as cellosolve and butyl carbitol, aromatic hydrocarbons such as toluene and xylene, and amide solvents such as dimethylformamide, dimethylacetamide (DMAc), and N-methylpyrrolidone. The organic solvents may be used alone or in combination of two or more.

[0087] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of organic solvent in the thermosetting resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of organic solvent is used, a thermosetting resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 15 minutes.

[0088] A protective film can be further laminated on the surface of the (i) thermosetting resin composition layer that is not bonded to the (ii) resin film layer (i.e., the surface opposite to the resin film layer) and the surface of the (ii) resin film layer that is not bonded to the (i) thermosetting resin composition layer (i.e., the surface opposite to the thermosetting resin composition layer). In addition, when the adhesive sheet includes a (iii) metal foil or a thermosetting resin composition layer, a protective film can be further laminated on the surface of the (iii) metal foil or the (ii) thermosetting resin composition layer that is not bonded to the (ii) resin film layer (i.e., the surface opposite to the resin film layer) and the surface of the (i) thermosetting resin composition layer that is not bonded to the (ii) resin film layer. By laminating a protective film, it is possible to prevent adhesion of dirt and the like and scratches on the surfaces of the (i) and (ii) layers (the (i) and (iii) layers when the (iii) layer is included). The adhesive sheet can be stored by rolling up in a roll. When the adhesive sheet has a protective film, it can be used by peeling off the protective film.

[0089] The protective film is preferably a film made of a plastic material.

[0090] Examples of plastic materials include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polyolefins such as polyethylene and polypropylene, polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate, polyethylene naphthalate, and polypropylene are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0091] The protective film may be subjected to a matte treatment or corona treatment on the surface that is to be joined to (i) the thermosetting resin composition layer or (ii) the resin film layer (in the case where (iii) a metal foil or a thermosetting resin composition layer is included, the (i) thermosetting resin composition layer or (iii) metal foil or thermosetting resin composition layer).

[0092] In addition, as the protective film, a support with a release layer having a release layer on the surface to be bonded to (i) a thermosetting resin composition layer or (ii) a resin film layer (when a layer (iii) is included, (iii) a metal foil or a thermosetting resin composition layer) may be used. Examples of the release agent used in the release layer of the support with a release layer include one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. As the support with a release layer, a commercially available product may be used, and examples thereof include "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, and "Lumirror T6AM" manufactured by Toray Industries, Inc., which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0093] The thickness of the protective film is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0094] For the adhesive sheet, the description in JP 2014-187091 A can be referred to, the contents of which are incorporated herein by reference.

[0095] The adhesive sheet of the present invention exhibits good embeddability. In one embodiment, when laminated on a substrate with a wiring layer, the adhesive sheet can be laminated on the wiring layer without voids. The embeddability can be measured according to the method described in "(2-2) Observation of embeddability" in the Examples below.

[0096] Since the adhesive sheet has a resin film layer, it exhibits the property of being bendable even after heat curing. The breaking elongation of the adhesive sheet after heat curing is preferably 2% or more, more preferably 3% or more, and even more preferably 5% or more. There is no particular upper limit, but it is 10% or less. The breaking elongation can be measured according to the method described below in <Measurement of breaking elongation>. Since the wiring board of the present invention is manufactured using such an adhesive sheet, it can be a flexible wiring board. The breaking elongation of the adhesive sheet after heat curing means the breaking elongation of the (i) thermosetting resin composition layer of the adhesive sheet.

[0097] [Manufacturing method of wiring board] The method for producing a wiring board of the present invention comprises the steps of: (1) preparing a substrate with a wiring layer, the substrate having a substrate and a wiring layer provided on at least one surface of the substrate; (2) a step of laminating an adhesive sheet including (i) a thermosetting resin composition layer and (ii) a resin film layer onto a substrate having a wiring layer such that the wiring layer is embedded in the (i) thermosetting resin composition layer, and thermally curing the resulting layer to form an insulating layer; (3) forming a via hole in the insulating layer; (4) forming a conductor layer; and (5) a step of removing the base material.

[0098] Hereinafter, a method for producing a wiring board in which the adhesive sheet includes (iii) a metal foil or a thermosetting resin composition layer, and the (iii) metal foil or thermosetting resin composition layer is a thermosetting resin composition layer, will be described as a first embodiment, and a method for producing a wiring board in which the (iii) layer of the adhesive sheet is a metal foil will be described as a second embodiment; however, the present invention is not limited thereto.

[0099] 1. First embodiment <Process (1)> Step (1) is a step of preparing a substrate with a wiring layer, which has a substrate and a wiring layer provided on at least one surface of the substrate. As shown in an example in Fig. 1, substrate with a wiring layer 10 has a first metal layer 12 and a second metal layer 13, which are parts of substrate 11, on both surfaces of substrate 11, and has a wiring layer 14 on the surface of one of the second metal layers 13 opposite to the surface on the substrate 11 side.

[0100] The details of step (1) are as follows: a dry film (photosensitive resist film) is laminated on a substrate, and a patterned dry film is formed by exposing and developing the film under predetermined conditions using a photomask. The developed patterned dry film is used as a plating mask to form a wiring layer by electrolytic plating, and then the patterned dry film is peeled off.

[0101] There are no particular limitations on the material used for the first and second metal layers. In a preferred embodiment, the first and second metal layers are preferably made of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, more preferably copper, from the standpoints of cost, ease of etching and peeling, etc.

[0102] The substrate is not particularly limited as long as it can carry out steps (1) to (5). Examples of the substrate include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate, and a metal layer such as a copper foil may be formed on the substrate surface.

[0103] The dry film is not particularly limited as long as it is a photosensitive dry film made of a photoresist composition, and for example, a dry film of novolac resin, acrylic resin, etc. can be used. A commercially available product may be used as the dry film, and for example, "ALPHO 20A263" manufactured by Nikko Materials Co., Ltd., which is a dry film with a PET film, can be used. The dry film may be laminated on one side of the substrate, or may be laminated on both sides of the substrate as in the second embodiment described later.

[0104] The lamination conditions for the substrate and the dry film are the same as those for laminating the adhesive sheet in the wiring layer so as to be embedded in the wiring layer in step (2) described below, and the preferred ranges are also the same.

[0105] After laminating the dry film on the substrate, the dry film is exposed and developed under prescribed conditions using a photomask to form a desired pattern.

[0106] The line (circuit width) / space (width between circuits) ratio of the wiring layer is not particularly limited, but is preferably 20 / 20 μm or less (i.e., pitch is 40 μm or less), more preferably 15 / 15 μm or less (pitch is 30 μm or less), and even more preferably 10 / 10 μm or less (pitch is 20 μm or less). The lower limit of the line / space ratio of the wiring layer is not particularly limited, but is preferably 0.5 / 0.5 μm or more, and more preferably 1 / 1 μm or more. The pitch does not need to be the same throughout the wiring layer.

[0107] The minimum pitch of the wiring layer may be 40 μm or less, 30 μm or less, or 20 μm or less.

[0108] After forming the pattern of the dry film, a wiring layer is formed and the dry film is peeled off. Here, the wiring layer can be formed by a plating method using the dry film with the desired pattern formed thereon as a plating mask.

[0109] The conductive material used for the wiring layer is not particularly limited. In a preferred embodiment, the wiring layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The wiring layer may be a single metal layer or an alloy layer, and examples of the alloy layer include those formed from an alloy of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among them, from the viewpoints of versatility, cost, ease of patterning, etc. of wiring layer formation, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy, copper-nickel alloy, copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver or copper, or an alloy layer of nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0110] The thickness of the wiring layer depends on the desired design of the wiring board, but is preferably 3 μm to 35 μm, more preferably 5 μm to 30 μm, and even more preferably 10 to 20 μm, or 15 μm.

[0111] After the wiring layer is formed, the dry film is peeled off. The dry film can be peeled off using an alkaline peeling solution such as a sodium hydroxide solution. If necessary, the unnecessary wiring pattern can be removed by etching or the like to form a desired wiring pattern. The pitch of the wiring layer to be formed is as described above.

[0112] <Process (2)> Step (2) is a step of laminating an adhesive sheet on a substrate with a wiring layer so that the wiring layer is embedded in the (i) thermosetting resin composition layer, and thermally curing the adhesive sheet to form an insulating layer. Since the adhesive sheet of the present invention exhibits good embedding properties, it can be laminated on a substrate with a wiring layer without voids. As shown in an example in FIG. 2, the wiring layer 14 of the substrate with a wiring layer obtained in the above-mentioned step (1) is laminated so as to be embedded in the (i) thermosetting resin composition layer 21 of the adhesive sheet 20, and the (i) thermosetting resin composition layer of the adhesive sheet 20 is thermally cured. The adhesive sheet 20 is formed by laminating the (i) thermosetting resin composition layer 21, (ii) resin film layer 22, and (iii) metal foil or thermosetting resin composition layer 23 in this order. That is, the adhesive sheet 20 has at least a three-layer structure. The adhesive sheet 20 may also be provided with (iii) a protective film 24 on the surface of the metal foil or thermosetting resin composition layer 23 opposite to the surface on which the resin film layer 22 is provided.

[0113] Although the adhesive sheet 20 used in the first embodiment has a three-layer structure, the adhesive sheet 20 is not limited to this, and for example, an adhesive sheet 20 having a two-layer structure in which (i) a thermosetting resin composition layer and (ii) a resin film layer are laminated in this order may be used. In this case, the layer 23 (iii) in the figure is omitted.

[0114] First, as an example shown in FIG. 2, (i) the thermosetting resin composition layer 21 of the adhesive sheet 20 is laminated on the substrate with the wiring layer so that the wiring layer 14 is embedded.

[0115] The wiring layer and the adhesive sheet can be laminated, for example, by thermocompression bonding the adhesive sheet to the wiring layer from the layer (iii) side after removing the protective film of the adhesive sheet. Examples of the member for thermocompression bonding the adhesive sheet to the wiring layer (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression bonding member not directly onto the adhesive sheet, but via an elastic material such as heat-resistant rubber so that the adhesive sheet can sufficiently follow the surface irregularities of the wiring layer.

[0116] The wiring layer and the adhesive sheet may be laminated by a vacuum lamination method after removing the protective film of the adhesive sheet. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably 30 seconds to 300 seconds. The lamination is preferably performed under reduced pressure conditions of 13hPa or less.

[0117] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Nikko Materials Co., Ltd., a vacuum pressure laminator manufactured by Meiki Co., Ltd., and a vacuum applicator manufactured by Nichigo-Morton Co., Ltd.

[0118] After lamination, the laminated adhesive sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the layer (iii). The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0119] After the wiring layer is laminated on the substrate with the wiring layer so as to be embedded in the (i) thermosetting resin composition layer, the (i) thermosetting resin composition layer is thermally cured to form an insulating layer. The thermal curing conditions for the (i) thermosetting resin composition layer are not particularly limited, and conditions that are usually adopted when forming an insulating layer for a wiring board may be used. In the first embodiment, when the (iii) layer is present, the (iii) layer also becomes an insulating layer.

[0120] For example, the thermal curing conditions for the thermosetting resin composition layer vary depending on the type of thermosetting resin composition, but the curing temperature can be in the range of 120°C to 240°C (preferably in the range of 150°C to 220°C, more preferably in the range of 170°C to 200°C), and the curing time can be in the range of 5 minutes to 120 minutes (preferably in the range of 10 minutes to 100 minutes, more preferably in the range of 15 minutes to 90 minutes).

[0121] Before the thermosetting resin composition layer is thermally cured, the thermosetting resin composition layer may be preheated at a temperature lower than the curing temperature. For example, before the thermosetting resin composition layer is thermally cured, the thermosetting resin composition layer may be preheated at a temperature of 50° C. or more and less than 120° C. (preferably 60° C. or more and 110° C. or less, more preferably 70° C. or more and 100° C. or less) for 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes).

[0122] The protective film of the adhesive sheet may be peeled off after laminating the adhesive sheet on the substrate with the wiring layer and heat curing it, or before laminating the adhesive sheet on the substrate with the wiring layer. Also, the protective film may be peeled off after step (3) and before the roughening treatment step.

[0123] The thickness of the insulating layer is similar to the thickness of the (i) thermosetting resin composition layer or the thickness of the (iii) layer, and the preferred range is also similar.

[0124] <Process (3)> Step (3) is a step of forming a via hole in the insulating layer. The via hole is preferably formed by laser irradiation. In detail, as shown in FIG. 3, in step (3), after peeling off the protective film 24, laser irradiation is performed from the surface side of the adhesive sheet 20 to form a via hole 31 that penetrates the insulating layer 23, the resin film layer 22, and the insulating layer 21 to expose the wiring layer 14. Alternatively, before peeling off the protective film 24, laser irradiation is performed from the surface side of the adhesive sheet to form a via hole 31 that penetrates the protective film 24, the insulating layer 23, the resin film layer 22, and the insulating layer 21 to expose the wiring layer 14, and the protective film 24 may be peeled off after the via hole 31 is formed.

[0125] This laser irradiation can be carried out using any suitable laser processing machine that uses a carbon dioxide gas laser, a YAG laser, an excimer laser, or the like as a light source. Examples of laser processing machines that can be used include the CO 2 Examples include the laser processing machine "LC-2k212 / 2C," the 605GTWIII(-P) manufactured by Mitsubishi Electric Corporation, and the laser processing machine manufactured by Panasonic Welding Systems Co., Ltd.

[0126] The conditions for the laser irradiation are not particularly limited, and the laser irradiation can be carried out by any suitable process according to a conventional method depending on the selected means.

[0127] The shape of the via hole, i.e., the shape of the outline of the opening when viewed in the extension direction, is not particularly limited, but is generally circular (approximately circular). Hereinafter, the "diameter" of the via hole refers to the diameter of the outline of the opening when viewed in the extension direction. In this specification, the top diameter refers to the diameter of the outline of the via hole on the insulating layer 23 side, and the bottom diameter refers to the diameter of the outline of the via hole on the wiring layer 14 side.

[0128] It is preferable to form the via hole so that the top diameter r1 of the via hole is 120 μm or less, and more preferably 90 μm or less.

[0129] The via hole is preferably formed so that the top diameter r1 of the via hole is larger than the bottom diameter r2 of the via hole 31.

[0130] This improves the filling of the via holes and suppresses the occurrence of voids, thereby improving the reliability of the electrical connection by the filled vias, which will be described later.

[0131] After the via holes are formed, a so-called desmear process, which is a process for removing smears from within the via holes, may be performed. When the step (4) described below is performed by a plating process, the via holes may be subjected to, for example, a wet desmear process, and when the step (4) is performed by a sputtering process, a dry desmear process such as a plasma treatment process may be performed. The desmear process may also serve as a roughening process.

[0132] The method may include a step of performing a roughening treatment before the step (5) of forming a conductor layer. The roughening treatment is performed on the via holes and the adhesive sheet, and the procedure and conditions of the roughening treatment are not particularly limited. For example, known procedures and conditions that are usually used when forming an insulating layer of a multilayer printed wiring board can be adopted. An example of a dry roughening treatment is a plasma treatment, and an example of a wet roughening treatment is a method in which a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid are performed in this order.

[0133] In the wet roughening treatment, for example, the insulating layer 23 can be roughened by performing a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order. The swelling liquid is not particularly limited, but examples thereof include an alkaline solution, a surfactant solution, and the like, and is preferably an alkaline solution, and as the alkaline solution, a sodium hydroxide solution or a potassium hydroxide solution is more preferable. Examples of commercially available swelling liquids include Swelling Dip Securigans P and Swelling Dip Securigans SBU manufactured by Atotech Japan Co., Ltd.

[0134] The swelling treatment using a swelling liquid is not particularly limited, but can be performed by, for example, immersing the insulating layer 23 in a swelling liquid at 30°C to 90°C for 1 to 20 minutes. From the viewpoint of suppressing the swelling of the resin of the insulating layer 23 to an appropriate level, it is preferable to immerse the insulating layer 23 in a swelling liquid at 40°C to 80°C for 5 to 15 seconds. The oxidizing agent is not particularly limited, but for example, an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide can be used. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer 23 in an oxidizing agent solution heated to 60°C to 80°C for 10 to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as Concentrate Compact P and Dosing Solution Securigans P, both manufactured by Atotech Japan Co., Ltd. Furthermore, the neutralizing solution is preferably an acidic aqueous solution, and an example of a commercially available product is Reduction Solution Securigans P, both manufactured by Atotech Japan Co., Ltd.

[0135] The treatment with the neutralizing solution can be carried out by immersing the surface that has been roughened with an oxidizing solution in a neutralizing solution at 30° C. to 80° C. for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing solution is immersed in a neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes is preferred.

[0136] <Process (4)> Step (4) is a step of forming a conductor layer. The conductor material constituting the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer can be formed from the same conductor material as that used for the wiring pattern, and is preferably made of copper.

[0137] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0138] The thickness of the conductor layer depends on the desired design of the wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.

[0139] The conductor layer can be formed by any suitable method known in the art, such as plating, sputtering, vapor deposition, etc., and is preferably formed by plating. In a preferred embodiment, for example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a known technique such as a semi-additive method or a full-additive method.

[0140] In detail, a plating seed layer is formed by electroless plating on the surface of the insulating layer 23 (or on the surface of the resin film layer 22 if layer (iii) is not present). Next, a mask pattern is formed on the formed plating seed layer to expose a portion of the plating seed layer corresponding to the desired wiring pattern. After that, an electric field plating layer is formed on the exposed plating seed layer by electrolytic plating, and the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like, and a conductor layer having a desired wiring pattern can be formed.

[0141] As shown in FIG. 4 as an example, a plating seed layer 41 is formed to be bonded to the exposed surface of the insulating layer 23 (when the layer (iii) does not exist, the surface of the resin film layer 22, and the same applies below). First, an alkaline cleaning is performed to clean the surface of the insulating layer 23 and adjust the charge. Next, a soft etching process is performed to clean the inside of the via hole 31. Specifically, an etchant such as an aqueous solution of sodium peroxodisulfate with sulfuric acid may be used under any suitable conditions. Next, a pre-dip process is performed to adjust the charge of the surface of the insulating layer 23 in order to apply Pd (palladium) to the surface of the insulating layer 23. Next, Pd, which is an activator, is applied to the surface, and the Pd applied to the insulating layer 23 is reduced. Next, copper (Cu) is precipitated on the surface of the insulating layer 23 to form a plating seed layer 41. At this time, the plating seed layer 41 is formed so as to cover the inside of the via hole 31, that is, the side wall and the wiring pattern 14 exposed from the via hole 31.

[0142] 5, after forming the plating seed layer 41, a mask pattern 50 is formed to expose a part of the plating seed layer 41. The mask pattern 50 can be formed, for example, by bonding a dry film to the plating seed layer 41 and performing exposure, development, and washing under predetermined conditions.

[0143] The dry film that can be used in step (4) is the same as the above-mentioned dry film, and the preferred range is also the same.

[0144] As shown in an example in FIG. 6, an electrolytic plating layer 42 is formed on an exposed plating seed layer 41 by electrolytic plating under conditions that fill the via hole 31, and the via hole is also embedded by electrolytic plating to form a filled via 61.

[0145] As shown in an example in FIG. 7, the mask pattern is then peeled off and removed, and flash etching is performed under any suitable conditions to remove only the exposed plating seed layer 41, thereby forming a patterned conductor layer 40.

[0146] The conductor layer may include not only linear wiring but also, for example, electrode pads (lands) on which external terminals can be mounted, etc. The conductor layer may also be composed of only electrode pads.

[0147] Alternatively, the conductor layer may be formed by forming a plating seed layer, forming an electrolytic plating layer and a filled via without using a mask pattern, and then performing patterning by etching.

[0148] <Process (5)> Step (5) is a step of removing the base material to form the wiring board of the present invention, as shown in an example in Fig. 8. The method of removing the base material is not particularly limited. In a preferred embodiment, the base material is peeled off from the wiring board at the interface between the first and second metal layers, and the second metal layer is etched away with, for example, an aqueous solution of copper chloride.

[0149] If necessary, the substrate may be peeled off while the conductor layer 23 is protected with a protective film. The protective film may be the same as the protective film used in the adhesive sheet, and the preferred range is also the same.

[0150] By such a manufacturing method of the present invention, a wiring board in which the wiring layer 14 is embedded in the insulating layer 21 can be manufactured. Furthermore, by including at least one resin film layer 22, a flexible wiring board can be obtained. Furthermore, the formation of the insulating layer and the conductor layer in steps (2) to (4) may be repeated to form a multilayer wiring board, if necessary. When manufacturing a multilayer wiring board, at least one adhesive sheet having a resin film layer may be used. That is, even if the wiring board of the present invention is a multilayer wiring board, it is sufficient that it has at least one resin film layer. Flexible means that the wiring board can be bent at least once without cracking or changing the resistance value.

[0151] 2. Second embodiment The second embodiment is a method for manufacturing a wiring board when the layer (iii) of the adhesive sheet is a metal foil. In the drawings used in the following description, the same components as those in the first embodiment are denoted by the same reference numerals, and duplicated descriptions may be omitted.

[0152] Step (1) is a step of preparing a substrate with a wiring layer, which has a substrate and a wiring layer provided on one surface of the substrate, as shown in an example in Fig. 9. The method of forming the wiring layer 14 is the same as in the first embodiment.

[0153] In step (2), an adhesive sheet is laminated on a substrate with a wiring layer so that the wiring layer is embedded in the thermosetting resin composition layer (i), and then thermally cured. As shown in an example in FIG. 10, the wiring layer 14 of the substrate with a wiring layer obtained in the above-mentioned step (1) is laminated so that it is embedded in the thermosetting resin composition layer (i) of the adhesive sheet 20, and the thermosetting resin composition layer (i) of the adhesive sheet 20 is thermally cured. The adhesive sheet 20 is formed by laminating the thermosetting resin composition layer (i), the resin film layer (ii), and the metal foil 25 in this order. The adhesive sheet 20 may also include a protective film 24 on the surface of the metal foil (iii) 25 opposite to the surface having the resin film layer 22.

[0154] 11, it is preferable that laser irradiation is performed from the side of the thermally cured adhesive sheet 20 to form via holes 31 in the thermally cured adhesive sheet 20. After completion of the step (3), a roughening treatment is performed.

[0155] Step (4) is a step of forming a conductor layer. In the second embodiment, since the layer (iii) of the adhesive sheet is a metal foil, it is preferable to form a conductor layer having a desired wiring pattern by a conventionally known technique such as a subtractive method.

[0156] In a preferred embodiment of step (4), an etching resist pattern is first formed on the surface of the metal foil, which exposes a part of the metal foil corresponding to the desired wiring pattern. The etching resist pattern can be formed, for example, by bonding an etching resist film to the metal foil and exposing and developing it under predetermined conditions.

[0157] After forming the etching resist pattern, the exposed metal foil portion is removed by etching or the like, and then the etching resist pattern is peeled off and removed, thereby forming the conductor layer 43 having the desired wiring pattern.

[0158] As the etching resist film, the same ones as the above-mentioned dry film can be used, and the preferred ranges are also the same.

[0159] Step (5), an example of which is shown in FIG. 12, is a step of removing the base material to form the wiring board of the present invention.

[0160] 3. Third embodiment In the first and second embodiments, a wiring board is manufactured from a substrate with a wiring layer having a wiring layer on one side, but in the third embodiment, a wiring board is manufactured from a substrate with a wiring layer having wiring layers on both sides of the substrate, and is similar to the first and second embodiments. In each figure used in the following description, similar components are denoted by the same reference numerals, and duplicated descriptions may be omitted.

[0161] Step (1) is a step of preparing a substrate with a wiring layer having a substrate and wiring layers provided on both sides of the substrate, as shown in Fig. 13 as an example. The method of forming the wiring layer 14 is the same as in the first and second embodiments, and the wiring layers provided on both sides of the substrate may be simultaneously formed to prepare a substrate with a wiring layer, or one wiring layer may be formed first and then the other wiring layer to prepare a substrate with a wiring layer. Moreover, each wiring layer may have the same pattern or different patterns.

[0162] Step (2) is a step of laminating adhesive sheets on both sides of the substrate with a wiring layer so that the wiring layers are embedded in the (i) thermosetting resin composition layer, and then thermally curing the adhesive sheets, as shown in an example in Fig. 14. The two adhesive sheets used may be the same adhesive sheet or different adhesive sheets.

[0163] In step (3), it is preferable to form via holes in the heat-cured adhesive sheet by irradiating both sides of the substrate with the wiring layer with a laser from the heat-cured adhesive sheet side, as shown in an example in Fig. 15. The via holes may be formed simultaneously, or one via hole may be formed first and then the other via hole.

[0164] Before the step (4), a step of performing a roughening treatment on both surfaces of the substrate with the wiring layer may be included, and the surfaces of the two insulating layers 23 are roughened. The roughening treatments may be performed simultaneously, or one of the surfaces may be roughened after the other surface.

[0165] In step (4), a conductor layer is formed on both sides of the substrate with the wiring layer. As shown in FIG. 16, a plating seed layer 41 is formed on the insulating layer 23 after the roughening treatment. After the plating seed layer 41 is formed, as shown in FIG. 17, a mask pattern 50 is formed to expose a part of the plating seed layer 41. As shown in FIG. 18, an electric field plating layer 42 is formed on the exposed plating seed layer 41, and the via hole is filled by electric field plating to form a filled via 61. As shown in FIG. 19, the mask pattern is removed and a conductor layer is formed. The details of the formation of the conductor layer can be performed in the same manner as in the first embodiment. In addition, the two conductor layers may be formed simultaneously, or one conductor layer may be formed and then the other conductor layer may be formed.

[0166] When the layer (iii) of the adhesive sheet is a metal foil, the conductor layer may be formed in the same manner as in the second embodiment. Alternatively, one conductor layer may be formed in the same manner as in the first embodiment, and the other conductor layer may be formed in the same manner as in the second embodiment.

[0167] Step (5) is a step of removing the base material to form the wiring board of the present invention, as shown in an example in Figure 20. In the third embodiment, it becomes possible to simultaneously manufacture two types of wiring boards.

[0168] [Wiring board] The wiring board of the present invention is characterized by comprising a resin film layer, an insulating layer, and a buried wiring layer embedded in the insulating layer. Note that descriptions that overlap with the above content may be omitted.

[0169] The wiring board of the present invention can be manufactured by the method for manufacturing a wiring board of the present invention, which includes the above steps (1) to (5). As described above, the wiring board of the present invention has an embedded wiring layer 14, an insulating layer 21, and a resin film layer 22 laminated in this order, as shown in Fig. 8 and Fig. 20 as an example. An insulating layer 23 and a conductor layer 40 are provided on the surface of the resin film layer 22 that is not bonded to the insulating layer (i.e., on the surface opposite to the resin film layer 22). The embedded wiring layer 14 is bonded to the conductor layer 40 through a filled via 61. Alternatively, as shown in Fig. 12 as an example, the conductor layer 43 and the embedded wiring layer 14 may be bonded to each other.

[0170] The embedded wiring layer refers to a wiring layer (wiring layer 14) that is embedded in the insulating layer 21 as long as it is possible to provide a conductive connection with components such as a semiconductor chip. The embedded wiring layer is usually embedded in the insulating layer so that the protruding height on the surface opposite to the side on which the adhesive sheet is laminated is substantially 0 (zero), usually -1 μm to +1 μm.

[0171] The wiring board of the present invention may be a multilayer wiring board, and in this case, the resin film layer 22 bonded to the insulating layer 21 may be at least one layer. The resin film layer 22 may be provided on the surface of the insulating layer 21 that is not bonded to the embedded wiring layer 14, as shown in FIG. 21, or may be provided on the surface of the insulating layer 21 that is bonded to the electrolytic plating layer, as shown in FIG. 22. In addition, as shown in FIG. 23, two or more resin film layers 22 may be provided. Note that the wiring board shown in FIG. 21 and FIG. 22 is obtained by using an adhesive sheet having a two-layer thermosetting resin composition layer as an adhesive sheet other than the adhesive sheet having the resin film layer 22, and thus has an embodiment in which the insulating layer 21 and the insulating layer 23 are laminated, but the wiring board may be obtained by using an adhesive sheet having a one-layer thermosetting resin composition layer as an adhesive sheet other than the adhesive sheet having the resin film layer 22, and only the insulating layer 21 (or the insulating layer 23) is provided.

[0172] 21 to 23 show a multilayer wiring board manufactured using an adhesive sheet further including layer (iii) where layer (iii) is a thermosetting resin composition layer, but the multilayer wiring board may be manufactured using an adhesive sheet where layer (iii) is a metal foil, or may be a multilayer wiring board manufactured using an adhesive sheet that does not include layer (iii), i.e., an adhesive sheet including (i) a thermosetting resin composition layer and (ii) a resin film layer.

[0173] The wiring board obtained by the wiring board manufacturing method of the present invention exhibits good foldability. In one embodiment, no abnormality such as cracks occurs on both sides of the bent portion after a bending test. This bending test can be measured, for example, according to the method described in <Bending test (cracks)> below. In one embodiment, the change in resistance value after the bending test is 50% or less. The change in resistance value after the bending test can be measured, for example, according to the method described in <Bending test (resistance change)> below.

[0174] The wiring board obtained by the method for producing a wiring board of the present invention exhibits good reflow behavior. In one embodiment, the reflow warpage behavior is 50 μm or less. The reflow warpage behavior can be measured, for example, according to the method described in <Evaluation of reflow warpage behavior>.

[0175] [Semiconductor Devices] The semiconductor device of the present invention is characterized by including the wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the wiring board of the present invention.

[0176] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft).

[0177] The semiconductor device of the present invention can be manufactured by mounting a component (semiconductor chip) on a conductive portion of a printed wiring board. The "conductive portion" refers to a portion of a printed wiring board that transmits an electric signal, and the portion may be either on the surface or embedded. The semiconductor chip is not particularly limited as long as it is an electric circuit element made of semiconductor material.

[0178] The method of mounting the semiconductor chip when manufacturing the semiconductor device of the present invention is not particularly limited as long as the semiconductor chip functions effectively, but specific examples include a wire bonding mounting method, a flip chip mounting method, a mounting method using a bumpless buildup layer (BBUL), a mounting method using an anisotropic conductive film (ACF), a mounting method using a non-conductive film (NCF), etc. Here, the "mounting method using a bumpless buildup layer (BBUL)" refers to "a mounting method in which a semiconductor chip is directly embedded in a recess in a printed wiring board and the semiconductor chip is connected to the wiring on the printed wiring board." EXAMPLES

[0179] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the following description, "parts" and "%" mean "parts by mass" and "% by mass", respectively, unless otherwise specified. The thickness of each layer of the adhesive sheet was measured using a contact type layer thickness meter (manufactured by Mitutoyo Corporation, MCD-25MJ).

[0180] <Preparation of evaluation board> (1) A step of preparing a substrate having a wiring layer, the substrate having a substrate and a wiring layer provided on at least one surface of the substrate. (1-1) Lamination of dry film onto base material (core substrate) As the core substrate, a glass cloth-based epoxy resin double-sided copper-clad laminate (layer structure: Mitsui Mining & Smelting Co., Ltd. Microthin MT-Ex (copper foil thickness 3 μm / carrier copper foil 18 μm), Panasonic Corporation "R1515A" substrate (thickness 0.2 mm), Mitsui Mining & Smelting Co., Ltd. Microthin MT-Ex (carrier copper foil 18 μm / thickness 3 μm copper foil)) was prepared. A dry film with a PET film (Hitachi Chemical Co., Ltd., high resolution type, thickness 15 μm) was laminated on both sides of the 3 μm thick copper foil side of the laminate using a batch type vacuum pressure laminator (Nikko Materials Co., Ltd. 2-stage build-up laminator "CVP700"). The dry film was laminated by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at a temperature of 70 ° C and a pressure of 0.1 MPa for 20 seconds.

[0181] (1-2) Pattern formation A glass mask (photomask) with the pattern shown below formed on it was placed on the PET film, which is the protective layer of the dry film, and exposed to a UV lamp with an irradiation intensity of 150 mJ / cm 2 After UV irradiation, the PET film of the dry film was peeled off, and a 1% aqueous sodium carbonate solution at 30°C was sprayed at a spray pressure of 0.15 MPa for 30 seconds.Then, the dry film was washed with water and developed (patterned).

[0182] Glass mask wiring pattern: L / S=10μm / 10μm, i.e. a comb-tooth pattern (wiring length 10mm, 16 lines) with a wiring pitch of 20μm is formed at 10mm intervals.

[0183] (1-3) Formation of wiring layers After developing the dry film, electrolytic copper plating was performed to a thickness of 8 μm to form a wiring layer. Next, a 3% sodium hydroxide solution at 50°C was sprayed at a spray pressure of 0.2 MPa, and the dry film was peeled off, followed by rinsing with water and drying at 150°C for 30 minutes.

[0184] (2) A step of laminating an adhesive sheet onto a substrate having a wiring layer so that the wiring layer is embedded in the (i) thermosetting resin composition layer, and then thermally curing the adhesive sheet. (2-1) Lamination of adhesive sheets The protective film (a release PET film having a thickness of 25 μm in Example 1, and a protective film having a thickness of 20 μm in Examples 2-3 and Comparative Examples 1-2) of the adhesive sheet prepared in the Examples and Comparative Examples was peeled off, and the thermosetting resin composition layer was embedded and laminated on both sides of the wiring pattern so that it was bonded to the wiring pattern using a batch-type vacuum pressure laminator (a two-stage build-up laminator "CVP700" manufactured by Nikko Materials Co., Ltd.). The lamination was performed by reducing the pressure for 30 seconds to 13 hPa or less, and then pressing at 110°C and a pressure of 0.74 MPa for 30 seconds. Next, the laminated adhesive sheet was heat-pressed at atmospheric pressure, 110°C, and a pressure of 0.5 MPa for 60 seconds to smooth it. This is referred to as evaluation substrate A.

[0185] (2-2) Observation of embeddability The surface of the thermosetting resin composition layer of evaluation substrate A was observed with a micro microscope ("VH-5500" manufactured by Keyence Corporation). Those that were free of voids and embedded in the wiring pattern were marked with "O" and those that had voids were marked with "X".

[0186] (2-3) Thermal curing of the thermosetting resin composition layer After lamination of the adhesive sheet, the thermosetting resin composition layer was thermally cured at 100°C for 30 minutes, and then at 170°C (170°C with 38 μm of release PET attached in Example 1 and Comparative Example 1) or 180°C (180°C with the release PET peeled off in Example 2 and Comparative Example 2) for 30 minutes to form insulating layers on both sides of the wiring layer.

[0187] (3) Forming via holes in the insulating layer In Example 1 and Comparative Example 1, a laser was irradiated from above the release PET or carrier copper foil, and in Example 2, Example 3, and Comparative Example 2, a laser was irradiated from above the insulating layer under the following conditions to form a via hole in the insulating layer directly above a 150 μm square wiring layer that would serve as the land for the wiring layer.

[0188] The via hole formation process was carried out under different conditions as shown below.

[0189] (A) Mitsubishi Electric Corporation CO 2 Using the laser processing machine "605GTWIII(-P)", a laser was irradiated from above the release PET side to form a via hole with a top diameter of 30μm in the insulating layer. The laser irradiation conditions were mask diameter 1mm, pulse width 16μs, energy 0.20mJ / shot, number of shots 2, and burst mode (10kHz). (B) Via Mechanics CO 2 Using the laser processing machine "LC-2k212 / 2C," a laser was irradiated from above the insulating layer to form a via hole with a top diameter of 50 μm in the insulating layer. The laser irradiation conditions were a mask diameter of 3 mm, a pulse width of 4 μs, a power of 0.8 W, a shot count of 3, and the operation was performed in cycle mode (2 kHz). (C) Mitsubishi Electric Corporation CO 2Using the laser processing machine "605GTWIII(-P)", a laser was irradiated from above the 3μm thick copper foil after peeling off the carrier copper foil, forming a via hole with a top diameter of 45μm in the insulating layer. The laser irradiation conditions were mask diameter of 1.5mm, pulse width of 16μs, energy of 0.36mJ / shot, number of shots of 3, and burst mode (10kHz).

[0190] (3-1) Roughening treatment process After the via holes were formed, if any release PET was attached, it was peeled off, and the structure provided with the via holes was subjected to a desmear treatment, which was a wet desmear treatment as described below.

[0191] Wet desmear process: The circuit board with via holes was immersed in a swelling liquid (Atotech Japan's "Swelling Dip Securigant P", an aqueous solution of diethylene glycol monobutyl ether and sodium hydroxide) at 60°C for 3 minutes, then in an oxidizing agent solution (Atotech Japan's "Concentrate Compact CP", an aqueous solution of potassium permanganate at approximately 6% and sodium hydroxide at approximately 4%) at 80°C for 8 minutes, and finally in a neutralizing solution (Atotech Japan's "Reduction Solution Securigant P", an aqueous solution of sulfuric acid) at 40°C for 5 minutes, and then dried at 80°C for 15 minutes.

[0192] (4) Forming a conductor layer (4-1) Electroless plating process In order to form a conductive layer on the surface of the evaluation board, a plating process including the following steps 1 to 6 (copper plating process using a chemical solution manufactured by Atotech Japan KK) was carried out to form the conductive layer.

[0193] 1. Alkaline cleaning (cleaning the surface of the insulating layer with via holes and adjusting the charge) The plate was washed at 60° C. for 5 minutes using Cleaning Cleaner Securiganth 902 (trade name). 2. Soft etching (cleaning inside the via hole) The mixture was treated with an aqueous solution of sulfuric acid and sodium peroxodisulfate at 30° C. for 1 minute. 3. Pre-dip (adjusting the charge on the surface of the insulating layer for Pd deposition) Pre. Dip Neoganth B (trade name) was used and treated at room temperature for 1 minute. 4. Adding an activator (adding Pd to the surface of the insulating layer) The cells were treated with Activator Neoganth 834 (trade name) at 35° C. for 5 minutes. 5. Reduction (reducing Pd added to the insulating layer) The mixture was treated with Reducer Neoganth WA (trade name) and Reducer Acceralator 810 mod. (trade name) at 30° C. for 5 minutes. 6. Electroless copper plating process (Cu is deposited on the surface of the insulating layer (Pd surface)) The substrate was treated for 20 minutes at 35° C. using a mixture of Basic Solution Printganth MSK-DK (trade name), Copper solution Printganth MSK (trade name), Stabilizer Printganth MSK-DK (trade name), and Reducer Cu (trade name). The thickness of the electroless copper plating layer formed was 0.8 μm.

[0194] (4-2) Electrolytic plating process Next, an electrolytic copper plating process was performed using a chemical solution manufactured by Atotech Japan Co., Ltd. under conditions in which copper was filled into the via holes. After that, a land pattern with a diameter of 100 μm corresponding to the via holes was formed as a resist pattern for patterning by etching (parts without via connections were also formed on the entire surface at a pitch of 400 μm), and a conductor layer having a conductor pattern with a thickness of 10 μm was formed on the surface of the insulating layer using this land pattern. Next, an annealing treatment was performed at 190° C. for 60 minutes.

[0195] (5) Removing the base material After laminating an adhesive PET film (50 μm thick) on the entire surface of the substrate with wiring layer on which the conductor layer was formed, the 3 μm thick copper foil of the Microthin MT-Ex copper foil of the core substrate and the 18 μm thick carrier foil were peeled off at the interface, and the core substrate was separated. Next, while the surface on which the conductor layer was formed was protected with the adhesive PET film, the 3 μm copper foil was etched off with a copper chloride aqueous solution, washed with water, and then dried at 110°C for 30 minutes. After that, the adhesive PET film was peeled off, and a wiring board with an L / S=10 / 10 μm comb tooth pattern embedded on one side was produced. The obtained wiring board is called "evaluation board B".

[0196] <Bending test (crack)> Evaluation board B was cut into a test piece with a width of 15 mm and a length of 110 mm, and was folded 20 times in the vertical direction to the center of the comb tooth pattern using an MIT test device (MIT folding fatigue tester "MIT-DA" manufactured by Toyo Seiki Seisakusho Co., Ltd.) under the measurement conditions of a load of 2.5 N, a folding angle of 90 degrees, a folding radius of 1.0 mm, and a folding speed of 175 times / min. The folded parts were observed with a micro microscope ("VH-5500" manufactured by Keyence Corporation). Those without abnormalities such as cracks on both sides were marked with "○", and those with abnormalities were marked with "×".

[0197] <Bending test (resistance change)> Furthermore, the insulation resistance value (Ω) of the substrate with an L / S=10 / 10 μm comb pattern (wiring length 10 mm, 16 lines) embedded in the bent portion was measured using an electrochemical migration tester ("ECM-100" manufactured by J-RAS Co., Ltd.) The insulation resistance value (Ω) was evaluated according to the following evaluation criteria. Evaluation criteria: ○: The change in resistance value after bending is 50% or less ×: The change in resistance value after bending exceeds 50%.

[0198] <Evaluation of reflow warpage behavior> Evaluation board B was cut into five 30 mm square pieces, and then passed through a reflow device ("HAS-6116" manufactured by Nippon Antom Co., Ltd.) that reproduces a solder reflow temperature of a peak temperature of 260°C (reflow temperature profile conforming to IPC / JEDEC J-STD-020C) once. Next, using a shadow moire device ("TherMoire AXP" manufactured by Akrometrix), the bottom surface of evaluation board B was heated with a reflow temperature profile conforming to IPC / JEDEC J-STD-020C (peak temperature 260°C), and the displacement of a 5 mm square part in the center of the board was measured. The measurements were performed on the five pieces, and the average value was calculated and evaluated according to the following evaluation criteria. Evaluation criteria: ○: Displacement is 50μm or less ×: Displacement exceeds 50 μm

[0199] <Measurement of Minimum Melt Viscosity of Thermosetting Resin Composition Layer> Only the thermosetting resin composition layer was peeled off from each of the Examples and Comparative Examples, and compressed in a mold to prepare a pellet for measurement (diameter 18 mm, 1.2 to 1.3 g).

[0200] Using the measurement pellets, a dynamic viscoelasticity measuring device (Rheosol-G3000, manufactured by UBM Corp.) was used to measure the dynamic viscoelasticity of 1 g of the sample thermosetting resin composition layer under the measurement conditions of a measurement temperature interval of 2.5°C, a vibration frequency of 1 Hz, and a strain of 1 deg, by heating the sample from a starting temperature of 60°C to 200°C at a heating rate of 5°C / min using parallel plates with a diameter of 18 mm, and calculating the minimum melt viscosity (poise).

[0201] <Measurement of breaking elongation> The adhesive sheets having only the 30 μm-thick thermosetting resin composition layer produced in the adhesive sheets 1 to 3 were heated at 190° C. for 90 minutes to thermally cure the thermosetting resin composition layer, and then the release PET film ("PET501010" (thickness 50 μm) manufactured by Lintec Corporation) was peeled off. The obtained cured product (thickness 30 μm) was cut into a dumbbell shape, and the tensile strength of the test piece was measured using a tensile tester RTC-1250A manufactured by Orientec Corporation in accordance with JIS K 7127 to determine the breaking elongation at 23° C. This operation was performed five times, and the average value of the top three points was calculated, which was 5.5% for Example 1 and 3.1% for both Examples 2 and 3.

[0202] <Preparation of Adhesive Sheet 1 Used in Example 1> (1) Preparation of resin varnish 1 9 parts of bisphenol type epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical Co., Ltd., a 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent 169), 6 parts of crystalline bifunctional epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent approximately 185), 15 parts of biphenyl type epoxy resin ("NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 288), and 15 parts of phenoxy resin ("YX6954BH30" manufactured by Mitsubishi Chemical Co., Ltd., a 1:1 solution of MEK (methyl ethyl ketone) and cyclohexanone with a solid content of 30 mass%) were dissolved in 10 parts of solvent naphtha by heating with stirring. The heated and dissolved material was cooled to room temperature, and 10 parts of a triazine skeleton-containing phenol-based hardener (DIC Corporation's "LA-7054", a MEK solution with a hydroxyl equivalent of 125 and a solid content of 60%), 10 parts of a naphthalene-type hardener (Nippon Steel Chemical Co., Ltd.'s "SN-485", a MEK solution with a hydroxyl equivalent of 215 and a solid content of 60%), 15 parts of a polyvinyl acetal resin (Sekisui Chemical Co., Ltd.'s "BX-5Z", a 1:1 solution of ethanol and toluene with a solid content of 15% by mass), 0.2 parts of a hardening accelerator (4-dimethylaminopyridine (DMAP), a MEK solution with a solid content of 5% by mass), and 0.2 parts of an imidazole-based hardener were added. The mixture was prepared by mixing 0.1 parts of an accelerator ("P200-H50" manufactured by Mitsubishi Chemical Corporation, a propylene glycol monomethyl ether solution with a solid content of 50% by mass), 3 parts of a flame retardant ("HCA-HQ" manufactured by Sanko Co., Ltd., 10-(2,5-dihydroxyphenyl)-10-hydro-9-oxa-10-phosphaphenanthrene-10-oxide, average particle size 2 μm), and spherical silica (average particle size 0.5 μm, "SOC2" manufactured by Admatechs Co., Ltd., carbon amount per unit area 0.39 mg / m) surface-treated with a phenylaminosilane coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.). 2 ) were mixed, uniformly dispersed in a high-speed rotating mixer, and filtered through a cartridge filter ("SHP050" manufactured by ROKITECHNO) to prepare Resin Varnish 1.

[0203] (2) Preparation of resin varnish 2 9 parts of bisphenol type epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical Co., Ltd., a 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent 169), 6 parts of crystalline bifunctional epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent approximately 185), 15 parts of biphenyl type epoxy resin ("NC3000H" manufactured by Nippon Kayaku Co., Ltd., epoxy equivalent 288), and 15 parts of phenoxy resin ("YX6954BH30" manufactured by Mitsubishi Chemical Co., Ltd., a 1:1 solution of MEK (methyl ethyl ketone) and cyclohexanone with a solid content of 30 mass%) were dissolved in 10 parts of solvent naphtha by heating with stirring. The heated solution was cooled to room temperature, and 10 parts of a triazine skeleton-containing phenolic hardener (DIC Corporation's "LA-7054", a MEK solution with a hydroxyl equivalent of 125 and a solid content of 60%), 10 parts of a naphthalene type hardener (Nippon Steel Chemical Co., Ltd.'s "SN-485", a MEK solution with a hydroxyl equivalent of 215 and a solid content of 60%), 15 parts of a polyvinyl acetal resin (Sekisui Chemical Co., Ltd.'s "KS-1", a 1:1 solution of ethanol and toluene with a solid content of 15% by mass), and a curing accelerator (4-dimethylaminopyridine (DMAP), a MEK solution with a solid content of 5% by mass). ), 0.4 parts of an imidazole-based curing accelerator ("P200-H50" manufactured by Mitsubishi Chemical Corporation, a propylene glycol monomethyl ether solution with a solid content of 50% by mass), and 2 parts of rubber particles (AC3816N manufactured by Ganz Chemical Co., Ltd.) were allowed to swell in 8 parts of solvent naphtha at room temperature for 12 hours, and spherical silica (average particle size 0.24 μm, "SOC1" manufactured by Admatechs Co., Ltd., carbon amount per unit area 0.36 mg / m) surface-treated with a phenylaminosilane-based coupling agent ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.) was used. 2 ) were mixed, uniformly dispersed in a high-speed rotating mixer, and filtered through a cartridge filter ("SHP030" manufactured by ROKITECHNO) to prepare Resin Varnish 2.

[0204] (3) Preparation of adhesive sheet 1 A resin varnish 1 was uniformly applied onto the release surface of a release-treated polyethylene terephthalate film (hereinafter abbreviated as release PET) ("AL5" manufactured by Lintec Corporation, thickness 25 μm) so that the thickness of the thermosetting resin composition layer 1 after drying would be 10 μm. The resin varnish 1 was then dried at 80 to 120°C (average 100°C) for 2.5 minutes to form a thermosetting resin composition layer 1. After that, a polyimide film ("Kapton 20EN" manufactured by Toray DuPont Co., Ltd., thickness 5 μm, with double-sided plasma treatment) was bonded to the thermosetting resin composition layer 1 using a heated roll to produce an adhesive sheet (1-1).

[0205] On the other hand, a resin varnish 2 was uniformly applied onto the release surface of a release PET ("AL5" manufactured by Lintec Corporation, thickness 38 μm) so that the thickness of the thermosetting resin composition layer 2 after drying would be 3 μm, and the resin varnish 2 was dried at 80 to 120°C (average 100°C) for 2 minutes to form a thermosetting resin composition layer 2. After that, the polyimide film surface of the adhesive sheet (1-1) was bonded to the thermosetting resin composition layer 2 with a hot roll to obtain an adhesive sheet 1 having a configuration of release PET (25 μm) / thermosetting resin composition layer 1 (10 μm) / polyimide film (5 μm) / thermosetting resin composition layer 2 (3 μm) / release PET (38 μm).

[0206] <Preparation of Adhesive Sheet 2 Used in Example 2> (1) Preparation of resin varnish 3 50 parts of polymer resin A prepared as follows, 3 parts of bisphenol type epoxy resin ("ZX1059" manufactured by Nippon Steel Chemical Co., Ltd., 1:1 mixture of bisphenol A type and bisphenol F type, epoxy equivalent 169), 3 parts of crystalline bifunctional epoxy resin ("YX4000HK" manufactured by Mitsubishi Chemical Co., Ltd., epoxy equivalent approximately 185), and 3 parts of naphthalene type epoxy resin ("HP4032SS" manufactured by DIC Corporation, epoxy equivalent approximately 144) were dissolved in 25 parts of solvent naphtha by heating with stirring. The heated and dissolved material was cooled to room temperature, and 4 parts of an active ester compound (DIC Corporation's "HPC8000-65T", a toluene solution with a weight average molecular weight of about 2700 and an active group equivalent of about 223 and a non-volatile content of 65% by mass), 0.4 parts of a curing accelerator (4-dimethylaminopyridine (DMAP), a MEK solution with a solid content of 5% by mass), 0.3 parts of an imidazole curing accelerator (Mitsubishi Chemical Corporation's "P200-H50", a propylene glycol monomethyl ether solution with a solid content of 50% by mass), and spherical silica (average particle size 0.5 μm, Admatechs Corporation's "SOC2", carbon amount per unit area 0.39 mg / m) surface-treated with a phenylaminosilane coupling agent (Shin-Etsu Chemical Co., Ltd.'s "KBM573"). 2 ) were mixed, uniformly dispersed in a high-speed rotating mixer, and filtered through a cartridge filter ("SHP050" manufactured by ROKITECHNO) to prepare Resin Varnish 3.

[0207] -Preparation of polymer resin A- In a reaction vessel, 50 g of G-3000 (bifunctional hydroxyl group-terminated polybutadiene, number average molecular weight = 5047 (number average molecular weight converted into polystyrene by GPC method), hydroxyl group equivalent: 1798 g / eq., solid content 100 mass%: manufactured by Nippon Soda Co., Ltd.), 23.5 g of Ipzole 150 (aromatic hydrocarbon-based mixed solvent: manufactured by Idemitsu Petrochemical Co., Ltd.), and 0.005 g of dibutyltin laurate were mixed and dissolved uniformly. When the mixture became uniform, the temperature was raised to 50°C, and 4.8 g of toluene-2,4-diisocyanate (isocyanate group equivalent: 87.08 g / eq.) was added while further stirring, and the reaction was carried out for about 3 hours. Next, the reaction mixture was cooled to room temperature, and 8.96 g of benzophenonetetracarboxylic dianhydride (acid anhydride equivalent: 161.1 g / eq.), 0.07 g of triethylenediamine, and 40.4 g of ethyl diglycol acetate (manufactured by Daicel Chemical Industries, Ltd.) were added thereto, and the temperature was raised to 130° C. with stirring, and the reaction was carried out for about 4 hours. -1 The disappearance of the NCO peak was confirmed. The disappearance of the NCO peak was regarded as the end point of the reaction, and the reaction mixture was cooled to room temperature and filtered through a 100 mesh filter cloth to obtain a polymer resin A having an imide skeleton, a urethane skeleton, and a butadiene skeleton. Viscosity: 7.5Pa s (25℃, E-type viscometer) Acid value: 16.9mgKOH / g Solid content: 50% by mass Number average molecular weight: 13723 (polystyrene equivalent by GPC method) Glass transition temperature: -10℃ (measured by DSC method) Polybutadiene structural portion content: 50 / (50+4.8+8.96)×100=78.4% by mass.

[0208] (2) Preparation of adhesive sheet 2 A polyimide film ("Apical 10NPI" manufactured by Kaneka Corporation, 10 μm thick, corona-treated on both sides) was immersed in the resin varnish 3, squeezed so that the thickness of the thermosetting resin composition layer after drying was 10 μm on each side, and dried at 80 to 120°C (average 100°C) for 3 minutes to form a thermosetting resin composition layer 3. After that, a release PET ("AL5" manufactured by Lintec Corporation, 38 μm thick) was attached to one resin surface, and a protective film (polypropylene film, "Alphan MA-430" manufactured by Oji F-Tex Co., Ltd., 20 μm thick) was attached to the other surface with a hot roll to obtain an adhesive sheet 2 having a configuration of release PET (38 μm) / thermosetting resin composition layer 3 (10 μm) / polyimide film (10 μm) / thermosetting resin composition layer 3 (10 μm) / protective film (20 μm).

[0209] <Preparation of Adhesive Sheet 3 Used in Example 3> On the polyimide film surface of a two-layer single-sided copper-clad polyimide film (manufactured by Arisawa Seisakusho Co., Ltd., a 12.5 μm thick polyimide film was formed on the upper surface of a 3 μm thick copper foil of Microsin MT-Ex (18 μm thick carrier copper foil / 3 μm thick copper foil) manufactured by Mitsui Mining & Smelting Co., Ltd.), a resin varnish 3 was uniformly applied so that the thickness of the thermosetting resin composition layer 3 after drying would be 10 μm, and the resin varnish 3 was dried at 80 to 120 ° C (average 100 ° C) for 2.5 minutes to form a thermosetting resin composition layer 3, and then a protective film (polypropylene film, Oji F-Tex Co., Ltd.'s "Alphan MA-430", thickness 20 μm) was bonded to the thermosetting resin composition layer 3 so as to be joined, and an adhesive sheet 3 having a configuration of copper foil (18 μm carrier foil / 3 μm copper foil) / polyimide film (12.5 μm) / thermosetting resin composition layer 3 (10 μm) / protective film (20 μm) was obtained.

[0210] <Preparation of Adhesive Sheet 4 Used in Comparative Example 1> Resin varnish 1 was uniformly applied onto the release surface of release PET ("AL5" manufactured by Lintec Corporation, thickness 38 μm) so that the thickness of the thermosetting resin composition layer 1 after drying would be 18 μm, and the resin varnish was dried at 80 to 120°C (average 100°C) for 3 minutes to form the thermosetting resin composition layer 1. After that, a protective film (polypropylene film, "Alphan MA-430" manufactured by Oji F-Tex Co., Ltd., thickness 20 μm) was bonded to the thermosetting resin composition layer 1 so as to be joined to the thermosetting resin composition layer 1, and an adhesive sheet 4 having a configuration of release PET (38 μm) / thermosetting resin composition layer 1 (18 μm) / protective film (20 μm) was obtained.

[0211] <Preparation of Adhesive Sheet 5 Used in Comparative Example 2> A resin varnish 3 was uniformly applied onto the release surface of a release PET ("AL5" manufactured by Lintec Corporation, thickness 38 μm) so that the thermosetting resin composition layer 3 would have a thickness of 30 μm after drying, and the resin varnish was dried at 80 to 120°C (average 100°C) for 4 minutes to form a thermosetting resin composition layer 3. After that, a protective film (polypropylene film, "Alphan MA-430" manufactured by Oji F-Tex Co., Ltd., thickness 20 μm) was attached so as to be bonded to the thermosetting resin composition layer 3, and an adhesive sheet 5 having a configuration of release PET (38 μm) / thermosetting resin composition layer 3 (30 μm) / protective film (20 μm) was obtained.

[0212] [Table 1]

[0213] [Table 2] 1) Of the two-layer, single-sided copper-clad polyimide film, the copper foil portion was designated as layer (iii) (thickness is the total value), and the polyimide film portion was designated as the resin film layer (layer (ii)). [Explanation of symbols]

[0214] 10 Substrate with wiring layer 11 Base material (core substrate) 12 1st metal layer 13 Second metal layer 14 Wiring layer (buried wiring layer) 20 Adhesive Sheet 21 (i) Thermosetting resin composition layer (insulating layer) 22 (ii) Resin film layer 23 (iii) Thermosetting resin composition layer (insulating layer) 24 Protective Film 25 (iii) Metal foil 31 Beer Hall 40 Conductor Layer 41 Plating seed layer 42 Electroplating layer 43 Conductor Layer 50 Mask Patterns 61 Filled Via

Claims

1. The insulating layer includes a resin film layer, an insulating layer, and a buried wiring layer buried in the insulating layer, A buried wiring layer, an insulating layer, and a resin film layer are laminated in this order, the insulating layer is formed by curing a resin composition layer (excluding those containing a phenoxy resin having a fluorene structure) containing (a) an epoxy resin, (b) one or more curing agents selected from a phenol-based curing agent, a naphthol-based curing agent, an active ester-based curing agent, and a cyanate ester-based curing agent, and (c) an inorganic filler; the resin film layer contains polyimide, polyethylene terephthalate, polyethylene naphthalate, a liquid crystal polymer, polyphenylene sulfide, polyether ether ketone, polybenzimidazole, aramid, polyamideimide, or polyetherimide; The change in resistance value after a bending test at a bending angle of 90 degrees is 50% or less compared to before the bending test, The resin film layer and the resin composition layer have a breaking elongation at 23°C of 2% or more and 10% or less, as measured in accordance with JIS K 7127 for a cured product obtained by heating an adhesive sheet including a resin film layer and a 30 μm-thick resin composition layer at 190°C for 90 minutes. wiring board.

2. The wiring board of claim 1 which is a flexible wiring board.

3. 3. The wiring board according to claim 1, wherein the insulating layer has a thickness of 2 μm or more.

4. The wiring board according to any one of claims 1 to 3, wherein the resin film layer has a thickness of 2 µm or more.

5. A wiring board described in any one of claims 1 to 4, wherein the embedded wiring layer is embedded in the insulating layer so that the protrusion height is -1 μm to +1 μm.

6. A wiring board described in any one of claims 1 to 5, comprising a second insulating layer and a conductor layer, in that order, on a surface of the resin film layer that is not laminated with the insulating layer, and the embedded wiring layer is joined to the conductor layer via a filled via.

7. A semiconductor device comprising the wiring board according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Thermocompression-bondable, high-precision circuit connector

    JP1995014571U

  • Flexible substrate, multilayer flexible substrate, and manufacturing method therefor

    JP2005303274A

  • Resin composition for printed circuit board, insulating layer with supporting substrate, laminate, and printed circuit board

    JP2009144052A

  • Resin composition

    JP2014015608A

  • Curable resin composition

    JP2014201698A