Acoustic Wave Resonators, Filters and Multiplexers
By employing single crystal lithium tantalate or lithium niobate substrates with comb-shaped electrodes and a structured intermediate and temperature compensation layer, the elastic wave resonator achieves improved temperature characteristics and reduced spurious loss, addressing the limitations of existing resonators.
Patent Information
- Application Number
- JP2023031099
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-03-01
- Publication Date
- 2024-09-18
- Estimated Expiration
- 2039-01-30
AI Technical Summary
Existing surface acoustic wave resonators face insufficient improvements in temperature characteristics and spurious loss, despite bonding a piezoelectric substrate to a support substrate and making its thickness equal to or less than the wavelength of the surface acoustic wave.
The use of a piezoelectric substrate made of single crystal lithium tantalate or lithium niobate, combined with comb-shaped electrodes and a structure that includes an intermediate layer with specific thickness and materials, such as aluminum oxide, and a temperature compensation layer with opposite temperature coefficient of elastic constant, to confine surface acoustic waves and reduce bulk wave propagation.
This configuration enhances the characteristics of the elastic wave resonator by improving temperature stability and reducing spurious loss, resulting in higher Q values and better frequency stability.
Smart Images

Figure 0007553622000007 
Figure 0007553622000009 
Figure 0007553622000010
Abstract
Description
[Technical field]
[0001] The present invention relates to an acoustic wave resonator, a filter, and a multiplexer, and more particularly to an acoustic wave resonator, a filter, and a multiplexer having a pair of comb electrodes. [Background technology]
[0002] Surface acoustic wave resonators are known as acoustic wave resonators used in communication devices such as smartphones. It is known that a piezoelectric substrate forming a surface acoustic wave resonator is attached to a support substrate. It is known that the thickness of the piezoelectric substrate is equal to or less than the wavelength of the surface acoustic wave (e.g., Patent Document 1). It is known that a low acoustic velocity film having a lower acoustic velocity than the piezoelectric substrate is provided between the piezoelectric substrate and the support substrate (e.g., Patent Documents 2 to 4). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-034363 A [Patent Document 2] JP 2015-115870 A [Patent Document 3] U.S. Patent No. 10020796 [Patent Document 4] International Publication No. 2017 / 043427 Summary of the Invention [Problem to be solved by the invention]
[0004] By bonding the piezoelectric substrate to the support substrate, the temperature characteristics of the surface acoustic wave resonator are improved. Furthermore, by making the thickness of the piezoelectric substrate equal to or less than the wavelength of the surface acoustic wave, spurious and loss can be suppressed. However, the improvement in temperature characteristics and the reduction in loss are not sufficient.
[0005] The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to improve the characteristics of an elastic wave resonator. [Means for solving the problem]
[0006] The present invention relates to a piezoelectric substrate which is a single crystal lithium tantalate substrate or a single crystal lithium niobate substrate, a pair of comb-shaped electrodes provided on the piezoelectric substrate and having a plurality of electrode fingers for exciting an elastic wave, the average pitch of the plurality of electrode fingers being 1 / 2 or more of the thickness of the piezoelectric substrate, and an aluminum oxide layer having a thickness of 20 nm or less and provided in contact with the surface of the piezoelectric substrate opposite to the surface on which the pair of comb-shaped electrodes are provided. In layers The elastic wave resonator includes a first layer and a second layer that is provided on a surface of the first layer opposite the piezoelectric substrate and is mainly composed of silicon oxide.
[0007] In the above configuration, the first layer may have a thickness of 2.5 nm or more.
[0008] In the above configuration, the thickness of the first layer is 10 The thickness can be configured to be less than nm.
[0009] In the above configuration, the second layer is provided on a surface opposite to the first layer, The substrate is a sapphire substrate, a spinel substrate, an alumina substrate, a silicon substrate, or a silicon carbide substrate. The device may include a support substrate.
[0015] The present invention is a filter including the above acoustic wave resonator.
[0016] The present invention is a multiplexer including the above filter. Effect of the Invention
[0017] According to the present invention, it is possible to improve the characteristics of an acoustic wave resonator. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a perspective view of an acoustic wave resonator in accordance with a first embodiment. [Diagram 2]FIG. 2(a) is a plan view of the acoustic wave resonator in the first embodiment, and FIG. 2(b) is a cross-sectional view taken along line AA of FIG. 2(a). [Diagram 3] 3(a) to 3(d) are cross-sectional views illustrating a method for manufacturing the acoustic wave resonator in accordance with the first embodiment. [Figure 4] 4(a) to 4(d) are schematic diagrams showing a method for bonding the intermediate layer and the piezoelectric substrate in Example 1. FIG. [Diagram 5] 5(a) and 5(b) are cross-sectional views of acoustic wave resonators according to comparative examples 1 and 2, respectively. [Figure 6] FIG. 6 is a diagram showing the Q value versus frequency in Example 1 and Comparative Examples 1 and 2. In FIG. [Figure 7] 7(a) and 7(b) are cross-sectional views of acoustic wave resonators in simulations A and B. FIG. [Figure 8] 8(a) and 8(b) are diagrams showing the displacement distribution with respect to the position Z in the simulations A and B. FIG. [Figure 9] 9(a) and 9(b) are cross-sectional views illustrating bulk waves. [Figure 10] 10(a) and 10(b) are diagrams showing the maximum Q value versus the thickness T1 of the intermediate layer in Example 1. FIG. [Figure 11] FIG. 11A is a cross-sectional view of an acoustic wave resonator according to a first modification of the first embodiment, and FIG. 11B is a graph showing peak values of unwanted responses versus arithmetic mean roughness Ra. [Figure 12] 12(a) to 12(d) are cross-sectional views of the intermediate layer and the temperature compensation layer of the first embodiment and its second to fourth modifications. [Figure 13] 13(a) to 13(c) are cross-sectional views of the intermediate layer and the temperature compensation layer of Modifications 5 to 7 of Example 1, and FIG. 13(d) is a cross-sectional view of the bonding layer. [Figure 14] FIG. 14(a) is a circuit diagram of a filter in accordance with the second embodiment, and FIG. 14(b) is a circuit diagram of a duplexer in accordance with a first modified example of the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, embodiments of the present invention will be described with reference to the drawings. EXAMPLES
[0020] Fig. 1 is a perspective view of an acoustic wave resonator according to a first embodiment, Fig. 2(a) is a plan view of the acoustic wave resonator in the first embodiment, and Fig. 2(b) is a cross-sectional view taken along line AA of Fig. 2(a). The arrangement direction of the electrode fingers is the X direction, the extension direction of the electrode fingers is the Y direction, and the lamination direction of the support substrate and the piezoelectric substrate is the Z direction. The X direction, the Y direction, and the Z direction do not necessarily correspond to the X-axis direction and the Y-axis direction of the crystal orientation of the piezoelectric substrate. When the piezoelectric substrate is a rotated Y-cut X-propagation substrate, the X direction is the X-axis direction of the crystal orientation.
[0021] 1, 2(a) and 2(b), an intermediate layer 11 is provided on the lower surface of a piezoelectric substrate 12. A temperature compensating layer 13 is provided below the intermediate layer 11. A support substrate 10 is provided below the temperature compensating layer 13. The thicknesses of the support substrate 10, the intermediate layer 11, the piezoelectric substrate 12 and the temperature compensating layer 13 are denoted as T0, T1, T2 and T3, respectively.
[0022] An acoustic wave resonator 20 is provided on a piezoelectric substrate 12. The acoustic wave resonator 20 has an IDT 22 and a reflector 24. The reflectors 24 are provided on both sides of the IDT 22 in the X direction. The IDT 22 and the reflector 24 are formed by a metal film 14 on the piezoelectric substrate 12.
[0023] The IDT 22 includes a pair of comb electrodes 18 facing each other. The comb electrodes 18 include a plurality of electrode fingers 15 and a bus bar 16 to which the plurality of electrode fingers 15 are connected. The region where the electrode fingers 15 of the pair of comb electrodes 18 cross is an intersection region 25. The length of the intersection region 25 is the aperture length. The pair of comb electrodes 18 are provided facing each other such that the electrode fingers 15 are substantially alternated in at least a part of the intersection region 25. The acoustic wave excited by the plurality of electrode fingers 15 in the intersection region 25 propagates mainly in the X direction. The pitch of the electrode fingers 15 of one of the pair of comb electrodes 18 is substantially the wavelength λ of the acoustic wave. The pitch of the electrode fingers 15 of the one comb electrode 18 is the pitch of two electrode fingers 15. The reflector 24 reflects the acoustic wave (surface acoustic wave) excited by the electrode fingers 15 of the IDT 22. As a result, the acoustic wave is confined within the intersection region 25 of the IDT 22.
[0024] The piezoelectric substrate 12 is, for example, a single crystal lithium tantalate (LiTaO3) substrate or a single crystal lithium niobate (LiNbO3) substrate, for example, a rotated Y-cut X-propagation lithium tantalate substrate or a rotated Y-cut X-propagation lithium niobate substrate. The piezoelectric substrate 12 is, for example, a single crystal quartz substrate, a single crystal langasite (La3Ga5SiO 14 ) substrate.
[0025] The support substrate 10 is, for example, a sapphire substrate, a spinel substrate, a silicon substrate, a quartz substrate, a quartz substrate, an alumina substrate, or a silicon carbide substrate. The sapphire substrate is a single crystal Al2O3 substrate, the spinel substrate is a polycrystalline or single crystal MgAl2O3 substrate, the silicon substrate is a single crystal Si substrate, the quartz substrate is a single crystal or amorphous SiO2 substrate, the quartz substrate is a polycrystalline SiO2 substrate, the alumina substrate is a sintered body (sintered ceramics) substrate of Al2O3, and the silicon carbide substrate is a polycrystalline or single crystal SiC substrate. The linear expansion coefficient of the support substrate 10 in the X direction is smaller than the linear expansion coefficient of the piezoelectric substrate 12 in the X direction. This can reduce the frequency temperature dependency of the acoustic wave resonator.
[0026] Temperature compensating layer 13 has a temperature coefficient of elastic constant with an opposite sign to that of piezoelectric substrate 12. For example, the temperature coefficient of elastic constant of piezoelectric substrate 12 is negative, and the temperature coefficient of elastic constant of temperature compensating layer 13 is positive. Temperature compensating layer 13 is, for example, a silicon oxide (SiO2) film with or without an additive element such as fluorine, a tantalum oxide (Ta2O5) film, or glass, and is, for example, an amorphous layer.
[0027] The sound velocity of the shear wave in the intermediate layer 11 is faster than that of the piezoelectric substrate 12. The Young's modulus, Poisson's ratio, density, and shear wave sound velocity of each material are shown in Table 1. The sound velocity V of the shear wave can be calculated by V=√(E / (2ρ(1+γ))) using the Young's modulus E, Poisson's ratio γ, and density ρ. [Table 1]
[0028] In Table 1, LT, Al2O3, SiO2, and SA are single crystal lithium tantalate, polycrystalline aluminum oxide, amorphous silicon oxide, and sapphire (single crystal aluminum oxide), respectively. LN, Si, AlN, SiN, and SiC are single crystal lithium niobate, polycrystalline silicon, polycrystalline aluminum nitride, polycrystalline silicon nitride, and polycrystalline silicon carbide, respectively.
[0029] As shown in Table 1, when a lithium tantalate substrate or a lithium niobate substrate is used as piezoelectric substrate 12, if a silicon oxide film is used as temperature compensating layer 13, the sound velocity of shear waves in temperature compensating layer 13 will be slower than that of shear waves in piezoelectric substrate 12. If an aluminum oxide layer, silicon layer, aluminum nitride layer, silicon nitride layer, or silicon carbide layer is used as intermediate layer 11, the sound velocity of shear waves in intermediate layer 11 will be faster than that of shear waves in piezoelectric substrate 12.
[0030] The metal film 14 is a film mainly composed of, for example, Al (aluminum) or Cu (copper), and is, for example, an Al film or a Cu film. An adhesive film such as a Ti (titanium) film or a Cr (chromium) film may be provided between the electrode fingers 15 and the piezoelectric substrate 12. The adhesive film is thinner than the electrode fingers 15. An insulating film may be provided so as to cover the electrode fingers 15. The insulating film functions as a protective film or a temperature compensation layer.
[0031] The thickness T0 is, for example, 50 μm to 500 μm. The thickness T1 is, for example, 2.5 nm to 15 nm. The thickness T2 is, for example, 0.1 μm to 5 μm, and is, for example, equal to or less than the wavelength λ of the elastic wave. The thickness T3 is, for example, 0.1 μm to 5 μm, and is, for example, equal to or less than λ. The wavelength λ of the elastic wave is, for example, 1 μm to 6 μm. When two electrode fingers 15 are considered as one pair, the number of pairs is, for example, 20 pairs to 300 pairs. The duty ratio of the IDT 22 is the thickness of the electrode finger 15 / the pitch of the electrode finger 15, and is, for example, 30% to 70%. The aperture length of the IDT 22 is, for example, 10λ to 50λ.
[0032] [Production method of Example 1] 3(a) to 3(d) are cross-sectional views showing a manufacturing method of the acoustic wave resonator according to Example 1. As shown in Fig. 3(a), a temperature compensating layer 13 is formed on a supporting substrate 10. An intermediate layer 11 is formed on the temperature compensating layer 13. The temperature compensating layer 13 and the intermediate layer 11 are formed by, for example, a sputtering method, a vacuum deposition method, or a CVD (Chemical Vapor Deposition) method.
[0033] 3(b), the lower surface of the piezoelectric substrate 12 is irradiated with ions 54. This activates the lower surface of the piezoelectric substrate 12. The upper surface of the intermediate layer 11 is irradiated with ions 54. This activates the upper surface of the intermediate layer 11.
[0034] As shown in Fig. 3(c), the upper surface of the intermediate layer 11 and the lower surface of the piezoelectric substrate 12 are bonded at room temperature. This bonds the intermediate layer 11 and the piezoelectric substrate 12. As shown in Fig. 3(d), the upper surface of the piezoelectric substrate 12 is flattened to make the piezoelectric substrate 12 have a desired thickness. Thereafter, a metal film 14 and the like are formed.
[0035] A method for attaching the lower surface of the piezoelectric substrate 12 to the upper surface of the intermediate layer 11 in Fig. 3(b) to Fig. 3(d) will be described in detail. Fig. 4(a) to Fig. 4(d) are schematic diagrams showing a method for bonding the intermediate layer and the piezoelectric substrate in Example 1. As shown in Fig. 4(a), the intermediate layer 11 is a polycrystalline layer in which atoms 50a of the elements constituting the intermediate layer 11 are regularly arranged. A natural oxide film 11c is formed on the upper surface of the intermediate layer 11. The natural oxide film 11c is composed of atoms 50a and oxygen.
[0036] 4(b), the piezoelectric substrate 12 is a single crystal substrate, and atoms 52a of the elements constituting the piezoelectric substrate 12 are regularly arranged. A native oxide film 12c is formed on the lower surface of the piezoelectric substrate 12. The native oxide film 12c is composed of atoms 52a and oxygen.
[0037] As shown in Figures 4(a) and 4(b), in a vacuum, the upper surface of the intermediate layer 11 and the lower surface of the piezoelectric substrate 12 are irradiated with ions 54 and the like. The ions 54 are, for example, ions of an inert element (for example, a rare gas element) such as Ar (argon) ions. The ions 54 and the like are irradiated as an ion beam, a neutralized beam, or plasma. This activates the upper surface of the intermediate layer 11 and the lower surface of the piezoelectric substrate 12. When Ar ions are used, for example, the current of the Ar ions is set to 25 mA to 200 mA, and the irradiation time of the Ar ions is set to about 30 seconds to 120 seconds.
[0038] As shown in FIG. 4(c), an amorphous layer 11b is formed on the upper surface of the intermediate layer 11. The amorphous layer 11b contains atoms 50a and ions 54 of the constituent elements of the intermediate layer 11. As a result, the intermediate layer 11 contains a polycrystalline layer 11a and an amorphous layer 11b on the polycrystalline layer 11a. An amorphous layer 12b is formed on the lower surface of the piezoelectric substrate 12. The amorphous layer 12b contains atoms 52a and ions 54 of the constituent elements of the piezoelectric substrate 12. As a result, the piezoelectric substrate 12 contains a single crystal layer 12a and an amorphous layer 12b below the single crystal layer 12a. Unbonded bonds are formed (i.e., activated) on the surfaces of the amorphous layers 11b and 12b.
[0039] As shown in Fig. 4(d), when the amorphous layers 11b and 12b are bonded together while maintaining a vacuum, the dangling bonds are bonded to each other, forming a strong bond. This bonds the intermediate layer 11 and the piezoelectric substrate 12. This bonding is performed at room temperature (for example, 100°C or lower and -20°C or higher, preferably 80°C or lower and 0°C or higher), so that thermal stress can be suppressed. Whether or not bonding is performed at room temperature can be confirmed by checking the temperature dependence of the residual stress. In other words, the residual stress is smallest at the bonding temperature.
[0040] In this way, when the intermediate layer 11 and the piezoelectric substrate 12 are bonded, when the intermediate layer 11 is an aluminum oxide film, the amorphous layer 11b is mainly composed of Al (aluminum) and O (oxygen) and contains Ar. When the piezoelectric substrate 12 is a lithium tantalate substrate, the amorphous layer 12b is mainly composed of Ta (tantalum), Li (lithium) and oxygen and contains Ar. The amorphous layer 11b contains almost no elements other than the elements of the piezoelectric substrate 12 among the elements of the intermediate layer 11. For example, the amorphous layer 11b contains almost no Ta and Li. The amorphous layer 12b contains almost no elements other than the elements of the intermediate layer 11 among the elements of the piezoelectric substrate 12. For example, the amorphous layer 12b contains almost no Al.
[0041] The thickness of the amorphous layers 11b and 12b is preferably greater than 0 nm, and more preferably equal to or greater than 1 nm. This can improve the bonding between the intermediate layer 11 and the piezoelectric substrate 12. The thickness of the amorphous layers 11b and 12b is preferably equal to or less than 10 nm, and more preferably equal to or less than 5 nm. This can suppress deterioration of the characteristics of the acoustic wave resonator. The polycrystalline layer 11a, the amorphous layers 11b and 12b, and the single crystal layer 12a can be observed using a TEM (Transmission Electron Microscope) method.
[0042] [Explanation of the reason for providing a temperature compensation layer] The following describes the reason why the temperature coefficient of frequency in the first embodiment is close to 0. The temperature coefficient of frequency (TCF) of acoustic wave resonator 20 is expressed by the following equation. TCF=TCV-CTE TCV (Temperature Coefficient of Velocity) is the temperature coefficient of sound velocity. CTE (Coefficient of Thermal Expansion) is the linear expansion coefficient. The linear expansion coefficient in the X-axis direction of the X-propagation lithium tantalate substrate used as the piezoelectric substrate 12 is approximately 16 ppm / K. The linear expansion coefficient of the C-axis (axis parallel to the X-axis) of the sapphire substrate used as the support substrate 10 is approximately 7.7 ppm / K. Therefore, when the thickness of the piezoelectric substrate 12 is reduced, the CTE of the acoustic wave resonator 20 approaches the CTE of the support substrate 10. However, it does not become smaller than the CTE of the support substrate 10.
[0043] Generally, the linear expansion coefficient is positive regardless of the material. Furthermore, the TCV of the material generally used for the piezoelectric substrate 12 is negative. This results in a negative TCF. Therefore, a material having a positive TCV is used for the temperature compensating layer 13. This allows the positive TCV of the temperature compensating layer 13 to compensate for the negative TCV of the piezoelectric substrate 12 and the CTE of the support substrate 10. This allows the TCF to be close to zero.
[0044] [Explanation of the reason for establishing a middle class] [experiment] Elastic wave resonators of Example 1 and Comparative Examples 1 and 2 were fabricated. Fig. 5(a) and Fig. 5(b) are cross-sectional views of the elastic wave resonators according to Comparative Examples 1 and 2, respectively. As shown in Fig. 5(a), in Comparative Example 1, a temperature compensating layer 13 is provided below a piezoelectric substrate 12, and an intermediate layer 11 is provided below the temperature compensating layer 13. A support substrate 10 is provided below the intermediate layer 11. Room temperature bonding is performed between the temperature compensating layer 13 and the intermediate layer 11. The other configurations are the same as those of Example 1.
[0045] 5(b), in Comparative Example 2, a temperature compensating layer 13 is provided under a piezoelectric substrate 12, and a support substrate 10 is provided under the temperature compensating layer 13. The temperature compensating layer 13 includes temperature compensating layers 13a and 13b, and an intermediate layer 11 is provided between the temperature compensating layers 13a and 13b. The temperature compensating layer 13a and the intermediate layer 11 are bonded at room temperature. The other configurations are the same as those of Example 1.
[0046] The conditions for fabricating the elastic wave resonator are as follows. Elastic wave wavelength λ: 5μm IDT22 pairs: 100 pairs Opening length: 20λ Duty ratio: 50% The wavelength λ of the acoustic wave is approximately twice the average pitch of the electrode fingers 15 of the IDT 22 .
[0047] Piezoelectric substrate 12: 42° rotated Y-cut X-propagation lithium tantalate substrate with a thickness T2 of 2 μm (0.4 λ) Intermediate layer 11: polycrystalline aluminum oxide layer with a thickness T1 of 10 nm Temperature compensation layer 13: Silicon oxide film with a thickness T3 of 2 μm (0.4 λ) Support substrate 10: Single crystal sapphire substrate with a thickness T0 of 500 μm
[0048] 6 is a diagram showing the Q value versus frequency in Example 1 and Comparative Examples 1 and 2. The resonant frequency and anti-resonant frequency of the fabricated acoustic wave resonator are approximately 760 MHz and approximately 790 MHz, respectively. As shown in FIG. 6, Example 1 has a higher Q value than Comparative Examples 1 and 2.
[0049] Thus, the reason why the Q value is improved by providing the intermediate layer 11 between the temperature compensating layer 13 and the piezoelectric substrate 12 is, for example, as follows. The IDT 22 excites a surface acoustic wave in the piezoelectric substrate 12. For example, when the piezoelectric substrate 12 is a 40°-48° rotated Y-cut X-propagation lithium tantalate substrate, the IDT 22 mainly excites an SH (Shear Horizontal) wave. The SH wave is a wave that is parallel to the surface of the piezoelectric substrate 12 and displaces in a direction perpendicular to the propagation direction of the SH wave. In order for the TCV of the temperature compensating layer 13 to compensate for the negative TCV of the piezoelectric substrate 12 and the -CTE of the support substrate 10, it is required that the displacement of the surface acoustic wave is distributed within the temperature compensating layer 13.
[0050] Therefore, the displacement distribution at the resonant frequency in the substrate was simulated. Figures 7(a) and 7(b) are cross-sectional views of the elastic wave resonators in simulations A and B. As shown in Figure 7(a), in simulation A, the substrate is only a 42° rotated Y-cut X-propagation lithium tantalate substrate as the piezoelectric substrate 12, and the support substrate 10 and the temperature compensation layer 13 are not provided. As shown in Figure 7(b), in simulation B, the substrate is a sapphire substrate as the support substrate 10 and a 42° rotated Y-cut X-propagation lithium tantalate substrate as the piezoelectric substrate 12, and the temperature compensation layer 13 and the intermediate layer 11 are not provided. The thickness T2 of the piezoelectric substrate 12 is about 0.7λ. In both simulations A and B, the surface of the piezoelectric substrate 12 that is in contact with the electrode fingers 15 is set to 0, and the depth direction of the substrate is set to position Z.
[0051] 8(a) and 8(b) are diagrams showing the displacement distribution with respect to the position Z in the simulations A and B. On the top of FIG. 8(a) and FIG. 8(b), double-headed arrows are shown indicating the range of the piezoelectric substrate 12 and the support substrate 10. As shown in FIG. 8(a), in the simulation A, most of the displacement falls within Z / λ of 2 or less. In particular, most of the displacement distribution falls within Z / λ of 1.5 or less. This indicates that the surface acoustic wave propagates in the range from the surface of the piezoelectric substrate 12 to about 2λ (particularly 1.5λ). As shown in FIG. 8(b), in the simulation B, most of the displacement falls within Z / λ of 1 or less. In particular, almost no displacement is distributed within the support substrate 10. This is because the sound velocity of the transverse wave in the support substrate 10 is high.
[0052] As shown in the above simulation, the surface acoustic wave propagates near the substrate surface. Therefore, by thinning the piezoelectric substrate 12 and providing the temperature compensating layer 13 under the piezoelectric substrate 12, the displacement of the surface acoustic wave is distributed in the temperature compensating layer 13, and the TCF can be made close to 0. The thickness T2 of the piezoelectric substrate 12 is preferably equal to or less than the wavelength λ of the acoustic wave, more preferably equal to or less than 0.9λ, and even more preferably equal to or less than 0.8λ. In order to propagate the surface acoustic wave, the thickness T2 of the piezoelectric substrate 12 is preferably equal to or more than 0.1λ, and more preferably equal to or more than 0.2λ.
[0053] Next, the bulk wave will be described. FIG. 9(a) and FIG. 9(b) are cross-sectional views for explaining the bulk wave. As shown in FIG. 9(a), the temperature compensating layer 13 is provided between the piezoelectric substrate 12 and the support substrate 10. The IDT 22 excites a surface acoustic wave 52 such as an SH wave on the surface of the piezoelectric substrate 12. The thickness T4 where the displacement of the surface acoustic wave 52 exists is about 2λ. When the IDT 22 excites the surface acoustic wave 52, the IDT 22 emits a bulk wave 58 in the piezoelectric substrate 12. The bulk wave 58 is 1 / 10 the size of the surface acoustic wave 52 in the main mode. The thickness where the bulk wave 58 exists is about 10λ. The thickness T2 of the piezoelectric substrate 12 is smaller than the thickness T4. As a result, the displacement of the surface acoustic wave 52 is distributed in both the piezoelectric substrate 12 and the temperature compensating layer 13. Therefore, the TCF can be suppressed. However, in addition to the surface acoustic wave 52, the bulk wave 58 also propagates in the temperature compensating layer 13. As a result, the energy of the surface acoustic wave 52 is lost as a bulk wave 58. This increases the loss of the acoustic wave resonator.
[0054] 9(b), in the first embodiment, intermediate layer 11, through which the sound velocity of shear waves is high, is provided between piezoelectric substrate 12 and temperature compensating layer 13. This makes it easier for bulk waves 58 to be confined within piezoelectric substrate 12, and reduces the energy of bulk waves 58a propagating through temperature compensating layer 13. This is believed to improve the Q value of the acoustic wave resonator.
[0055] 10(a) and 10(b) are diagrams showing the maximum Q value versus thickness T1 of the intermediate layer in Example 1. FIG. 10(a) shows an elastic wave resonator with a resonant frequency of about 600 MHz, fabricated under the same conditions as FIG. 6. Note that the Q value does not match that of FIG. 6, since the elastic wave resonator is not the same as that of FIG. 6. FIG. 10(b) shows an elastic wave resonator with a resonant frequency of about 2.5 GHz. Thicknesses T2 and T3 are set to 0.4λ.
[0056] As shown in Figures 10(a) and 10(b), when the thickness T1 of the intermediate layer 11 is 10 nm or less, the Q value remains almost unchanged, but as T1 becomes thicker, the Q value decreases. T1 is preferably 20 nm or less, more preferably 15 nm or less, and even more preferably 10 nm or less. This makes it possible to suppress the decrease in the Q value. If T1 is too thin, the effect of improving the Q value of the intermediate layer 11 decreases. Therefore, T1 is preferably 2.5 nm or more, and more preferably 3 nm or more.
[0057] 10(a) and 10(b), the preferable thickness T1 does not depend on the resonant frequency (i.e., the wavelength of the elastic wave). Therefore, even if the resonant frequency of the elastic wave resonator is 1000 MHz or 800 MHz or less, the thickness of intermediate layer 11 may be 20 nm or less.
[0058] The acoustic velocity of the transverse wave in the support substrate 10 is set to be faster than that in the piezoelectric substrate 12. This allows the bulk wave 58 to be confined within the piezoelectric substrate 12 and the temperature compensating layer 13. If the total thickness T1+T2+T3 of the piezoelectric substrate 12, intermediate layer 11, and temperature compensating layer 13 is large, the bulk wave 58 propagates through the temperature compensating layer 13, resulting in large loss. T1+T2+T3 may be within a range in which the surface acoustic wave 52 is distributed in the temperature compensating layer 13. Therefore, from the results of Figures 9(a) and 9(b), T1+T2+T3 is preferably 2λ or less, more preferably 1.5λ or less. This allows the loss of the acoustic wave resonator to be suppressed.
[0059] [Modification 1 of Example 1] Fig. 11(a) is a cross-sectional view of an acoustic wave resonator according to a first modification of the first embodiment. As shown in Fig. 11(a), the interface between the support substrate 10 and the temperature compensating layer 13 is roughened surface 56. A plurality of convex portions and a plurality of concave portions are provided on the roughened surface 56. The roughened surface 56 is formed by grinding the upper surface of the support substrate 10 with a grinder. The roughened surface 56 may also be formed by irradiating the upper surface of the support substrate 10 with atoms or ions.
[0060] FIG. 11(b) is a diagram showing the peak value of the unwanted response versus the arithmetic mean roughness Ra. The arithmetic mean roughness Ra is the arithmetic mean roughness (center line average roughness) of the interface between the support substrate 10 and the temperature compensation layer 13. The peak value of the unwanted response indicates the magnitude of the unwanted response caused by the bulk wave. As shown in FIG. 11(b), as Ra increases, the unwanted response decreases. This is because reflection of the bulk wave 58 on the rough surface is suppressed. Ra is preferably 0.02λ or more, and more preferably 0.04λ or more.
[0061] [Modification 2-4 of Example 1] 12(a) to 12(d) are cross-sectional views of the intermediate layer and the temperature compensation layer of Example 1 and its Modifications 2 to 4. As shown in FIG. 12(a), in Example 1, intermediate layer 11 and piezoelectric substrate 12 are bonded at room temperature. For this reason, intermediate layer 11 includes polycrystalline layer 11a and amorphous layer 11b, and piezoelectric substrate 12 includes single crystal layer 12a and amorphous layer 12b. Since amorphous layer 12b has low piezoelectricity, if amorphous layer 12b is thick, the characteristics of the acoustic wave resonator are deteriorated. Therefore, it is preferable that amorphous layer 12b is thinner than amorphous layer 11b.
[0062] The main components of the amorphous layer 11b are the main constituent elements of the polycrystalline layer 11a, and the main components of the amorphous layer 12b are the main constituent elements of the single crystal layer 12a. Thus, the amorphous layer 11b is a part of the intermediate layer 11, and the amorphous layer 12b is a part of the piezoelectric substrate 12. Thus, in the case of FIG. 12(a), the intermediate layer 11 is provided in contact with the piezoelectric substrate 12.
[0063] As shown in FIG. 12(b), in the second modification of the first embodiment, the temperature compensating layer 13 and the intermediate layer 11 are bonded at room temperature. Therefore, the intermediate layer 11 includes a polycrystalline layer 11a and an amorphous layer 11b, and the temperature compensating layer 13 includes a temperature compensating layer 13a that does not contain an element for activation (e.g., Ar) and an amorphous layer 13c that contains an element for activation. The temperature compensating layer 13a is a polycrystalline layer or an amorphous layer. The amorphous layer 11b contains almost no elements other than the elements of the intermediate layer 11 among the constituent elements of the temperature compensating layer 13. For example, when the intermediate layer 11 is an aluminum oxide layer and the temperature compensating layer 13 is a silicon oxide film, the amorphous layer 11b contains almost no Si.
[0064] As shown in Fig. 12(c), in the third modification of the first embodiment, the temperature compensating layers 13a and 13b are bonded at room temperature. Therefore, the temperature compensating layer 13 includes the temperature compensating layers 13a and 13b that do not contain an element for activation (e.g., Ar) and the amorphous layers 13c and 13d that contain an element for activation. The amorphous layers 13c and 13d are bonded at room temperature. The temperature compensating layers 13a and 13b are polycrystalline layers or amorphous layers.
[0065] As shown in FIG. 12(d), in the fourth modification of the first embodiment, the temperature compensating layer 13 and the support substrate 10 are bonded at room temperature. For this reason, the temperature compensating layer 13 includes a temperature compensating layer 13a that does not contain an element for activation (e.g., Ar) and an amorphous layer 13c that contains an element for activation. The support substrate 10 includes a support substrate 10a that does not contain an element for activation and an amorphous layer 10b that contains an element for activation. The amorphous layers 13c and 10b are bonded at room temperature. The support substrate 10a is a single crystal substrate, a polycrystalline substrate, or an amorphous substrate.
[0066] Since no amorphous layer 11b is formed on the piezoelectric substrate 12, it is preferable to perform room temperature bonding between the lower surface of the intermediate layer 11 and the upper surface of the temperature compensating layer 13, the interface between the temperature compensating layers 13a and 13b, or the lower surface of the temperature compensating layer 13 and the upper surface of the supporting substrate 10, as in variants 2 to 4 of Example 1.
[0067] [Modifications 5-7 of Example 1] 13(a) to 13(c) are cross-sectional views of the intermediate layer and the temperature compensating layer of the fifth to seventh modifications of the first embodiment, and FIG. 13(d) is a cross-sectional view of the bonding layer. As shown in FIG. 13(a), in the fifth modification of the first embodiment, a bonding layer 28 is provided between the temperature compensating layer 13 and the intermediate layer 11. As shown in FIG. 13(b), in the sixth modification of the first embodiment, a bonding layer 28 is provided between the temperature compensating layers 13a and 13b. As shown in FIG. 13(c), in the seventh modification of the first embodiment, a bonding layer 28 is provided between the support substrate 10 and the temperature compensating layer 13. The other configurations are the same as those of the first embodiment, and therefore will not be described.
[0068] As shown in FIG. 13(d), the bonding layer 28 includes bonding layers 28a and 28b and amorphous layers 18c and 18d. The bonding layers 28a and 28b do not contain an element for activation, and the amorphous layers 18c and 28d contain an element for activation. The bonding layers 28a and 28b are, for example, silicon layers. It is difficult to bond a silicon oxide film by a surface activation method. In such a case, the bonding layers 28a and 28b may be formed on the surface of the silicon oxide film, and the bonding layers 28a and 28b may be bonded by a surface activation method. The bonding layer 28 may be a titanium layer or a nickel layer other than a silicon layer. The bonding layer 28 may be bonded to the piezoelectric substrate 12 and the support substrate 10 by a method other than the surface activation method.
[0069] In order to bond at a location far from the piezoelectric substrate 12, it is preferable that the bonding layer 28 be provided between the lower surface of the intermediate layer 11 and the upper surface of the support substrate 10, as in the fifth to seventh modified examples of the first embodiment.
[0070] According to the first embodiment, the pair of comb electrodes 18 includes a plurality of electrode fingers 15 that excite an acoustic wave, and the average pitch (i.e., λ / 2) of the plurality of electrode fingers 15 is equal to or greater than ½ of the thickness T2 of the piezoelectric substrate 12. The intermediate layer 11 (first layer) is provided in contact with the surface of the piezoelectric substrate 12 opposite to the surface on which the comb electrodes 18 are provided, and has a transverse wave acoustic velocity faster than the transverse wave acoustic velocity of the piezoelectric substrate 12. The temperature compensating layer 13 (second layer) is provided on the surface of the intermediate layer 11 opposite to the piezoelectric substrate, and the sign of the temperature coefficient of the elastic constant of the temperature compensating layer 13 is opposite to the sign of the temperature coefficient of the elastic constant of the piezoelectric substrate 12, and the transverse wave acoustic velocity of the temperature compensating layer 13 is slower than the transverse wave acoustic velocity of the piezoelectric substrate 12.
[0071] By setting thickness T2 of piezoelectric substrate 12 to be equal to or less than twice the average pitch of electrode fingers 15 (i.e., equal to or less than the wavelength λ of the elastic wave), surface acoustic waves 52 are distributed in temperature compensating layer 13. This improves the temperature characteristics of elastic wave resonator 20 as described in FIGS. 8(a) and 8(b). However, if the sound velocity of the transverse wave in temperature compensating layer 13 is slower than that of the piezoelectric substrate 12, loss in elastic wave resonator 20 increases. Thus, by providing intermediate layer 11, loss in elastic wave resonator 20 can be suppressed as described in FIGS. 9(a) and 9(b). The average pitch of electrode fingers 15 can be calculated by dividing the length of elastic wave resonator 20 in the X direction by the number of electrode fingers 15.
[0072] The thickness of intermediate layer 11 is preferably 2.5 nm or more. This allows the loss in acoustic wave resonator 20 to be further suppressed. The thickness of intermediate layer 11 is 20 nm or less. This allows the loss in acoustic wave resonator 20 to be further suppressed, as shown in Figures 10(a) and 10(b). Intermediate layer 11 is preferably made of a material that has no piezoelectricity. This allows the acoustic wave to be confined by piezoelectric substrate 12. In addition, intermediate layer 11 is preferably made of a material with low conductivity. This allows the acoustic wave to be confined by piezoelectric substrate 12.
[0073] The linear expansion coefficient of the support substrate 10 is smaller than the linear expansion coefficient of the piezoelectric substrate 12 in the X direction. This can further improve the temperature characteristics of the elastic wave resonator 20. The linear expansion coefficient of the support substrate 10 is preferably ⅔ or less, more preferably ½ or less, of the linear expansion coefficient of the piezoelectric substrate 12 in the X direction. In order to confine the bulk waves 58 in the piezoelectric substrate 12, the intermediate layer 11, and the temperature compensation layer 13. The sound velocity of the transverse waves of the support substrate 10 is preferably faster than the sound velocity of the transverse waves of the piezoelectric substrate 12, and preferably faster than the sound velocity of the transverse waves of the intermediate layer 11. The flexural strength of the support substrate 10 is preferably greater than the flexural strength of the piezoelectric substrate 12. This can improve the impact resistance.
[0074] The total thickness T1+T2+T3 of piezoelectric substrate 12, intermediate layer 11 and temperature compensating layer 13 is equal to or less than four times (2λ) the pitch of electrode fingers 15. This makes it possible to suppress loss in acoustic wave resonator 20 due to bulk waves 58.
[0075] The arithmetic mean roughness Ra of the interface between the supporting substrate 10 and the temperature compensation layer 13 is equal to or greater than 0.01 times (0.02λ) the average pitch of the electrode fingers 15. This makes it possible to suppress unwanted responses caused by bulk waves 58, as shown in FIG. 11(b).
[0076] Intermediate layer 11 and temperature compensating layer 13 are in contact with each other. This can further improve the temperature characteristics of acoustic wave resonator 20.
[0077] When the acoustic waves excited mainly by the pair of comb electrodes 18 are SH waves, bulk waves 58 are likely to be excited.
[0078] In particular, the piezoelectric substrate 12 is a lithium tantalate substrate or a lithium niobate substrate, the intermediate layer 11 is a layer mainly composed of aluminum oxide, and the temperature compensating layer 13 is a layer mainly composed of silicon oxide. This allows the CTE of the acoustic wave resonator 20 to be small. The temperature compensating layer 13 is provided, and the thickness T2 of the piezoelectric substrate 12 is made smaller than λ. This allows the surface acoustic wave 52 to be distributed within the temperature compensating layer 13, so that the TCF can be made closer to 0. However, the loss due to the bulk wave increases. Therefore, the intermediate layer 11 having a thickness T1 of 2.5 nm or more and 20 nm or less is provided. This allows the Q value of the acoustic wave resonator 20 to be improved.
[0079] "The intermediate layer 11 is mainly composed of aluminum oxide" means that the intermediate layer 11 contains impurities that are added intentionally or unintentionally other than aluminum oxide, and for example, the total atomic concentration of aluminum and oxygen in the intermediate layer 11 is 50% or more, and 80% or more. "The temperature compensating layer 13 is mainly composed of silicon oxide" means that the temperature compensating layer 13 contains impurities that are added intentionally or unintentionally other than silicon oxide, and for example, the total atomic concentration of silicon and oxygen in the temperature compensating layer 13 is 50% or more, and 80% or more. EXAMPLES
[0080] FIG. 14(a) is a circuit diagram of a filter according to a second embodiment. As shown in FIG. 14(a), one or more series resonators S1 to S3 are connected in series between an input terminal Tin and an output terminal Tout. One or more parallel resonators P1 and P2 are connected in parallel between the input terminal Tin and the output terminal Tout. The acoustic wave resonator of the first embodiment can be used for at least one of the one or more series resonators S1 to S3 and the one or more parallel resonators P1 and P2. The number of resonators of the ladder filter can be set as appropriate. The filter may be a multimode filter.
[0081] [Modification 1 of Example 2] FIG. 14(b) is a circuit diagram of a duplexer according to a first modified example of the second embodiment. As shown in FIG. 14(b), a transmission filter 40 is connected between a common terminal Ant and a transmission terminal Tx. A reception filter 42 is connected between the common terminal Ant and a reception terminal Rx. The transmission filter 40 passes a signal in a transmission band among high-frequency signals input from the transmission terminal Tx to the common terminal Ant as a transmission signal, and suppresses signals of other frequencies. The reception filter 42 passes a signal in a reception band among high-frequency signals input from the common terminal Ant to the reception terminal Rx as a reception signal, and suppresses signals of other frequencies. At least one of the transmission filter 40 and the reception filter 42 can be the filter of the second embodiment.
[0082] Although a duplexer has been described as an example of a multiplexer, a triplexer or a quadplexer may also be used.
[0083] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0084] 10 Support substrate 11 Middle Class 12 Piezoelectric substrate 13 Temperature compensation layer 15 Electrode finger 18 Comb-shaped electrode 20. Elastic Wave Resonator 22 IDT
Claims
1. a piezoelectric substrate which is a single crystal lithium tantalate substrate or a single crystal lithium niobate substrate; a pair of comb-shaped electrodes provided on the piezoelectric substrate, the comb-shaped electrodes including a plurality of electrode fingers for exciting an elastic wave, the average pitch of the plurality of electrode fingers being equal to or greater than half the thickness of the piezoelectric substrate; a first layer that is an aluminum oxide layer and has a thickness of 20 nm or less and is provided in contact with a surface of the piezoelectric substrate opposite to the surface on which the pair of comb electrodes are provided; a second layer, the second layer being provided on a surface of the first layer opposite to the piezoelectric substrate and containing silicon oxide as a main component; An elastic wave resonator comprising:
2. 2. The acoustic wave resonator according to claim 1, wherein the first layer has a thickness of 2.5 nm or more.
3. 2. The acoustic wave resonator according to claim 1, wherein the first layer has a thickness of 10 nm or less.
4. 4. The elastic wave resonator according to claim 1, further comprising a support substrate, the support substrate being a sapphire substrate, a spinel substrate, an alumina substrate, a silicon substrate or a silicon carbide substrate, provided on a surface of the second layer opposite to the first layer.
5. A filter comprising the acoustic wave resonator according to claim 1 .
6. A multiplexer including a filter according to claim 5.
Citation Information
Patent Citations
Surface acoustic wave element
JP2001185975A
Surface acoustic wave device
JP2001196896A
Surface acoustic wave element, manufacturing method of surface acoustic wave element, and electronic apparatus
JP2005065050A
Acoustic wave device
JP2015115870A
Elastic wave device and module
JP2017034363A