Method for estimating the inert factor coefficient of coal and the surface destructive strength of coke
The method uses solvent extraction to determine the inert factor coefficient, addressing inaccuracies in estimating coke strength from inferior quality coal blends, particularly for coals with volatile content below 30% by mass, by correcting void filling degrees and improving prediction accuracy.
Patent Information
- Application Number
- JP2020149901
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-06
- Filing Date
- 2020-09-07
- Publication Date
- 2024-09-19
- Estimated Expiration
- 2040-09-07
AI Technical Summary
Existing methods for estimating the surface fracture strength of coke produced using inferior quality coal blends are inaccurate due to the non-additive nature of expansion specific volumes, particularly for coals with volatile content below 30% by mass, leading to insufficient prediction of coke strength.
A method involving solvent extraction to determine the inert factor coefficient, which correlates with the solvent extraction rate, is used to estimate the surface fracture strength of coke blends containing inferior quality coal, accounting for different volatile content ranges and heating rates.
This method allows for precise estimation of coke surface fracture strength by correcting void filling degrees, improving accuracy across varying blending ratios of inferior quality coal, thereby enhancing the prediction of coke strength in blast furnaces.
Smart Images

Figure 0007553785000013 
Figure 0007553785000015 
Figure 0007553785000018
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for estimating the inert factor coefficient of coal and a method for estimating coke strength when low-quality coal is used as part of a coal blend. [Background technology]
[0002] In order to ensure the permeability of blast furnaces and ensure stable operation, the coke used in blast furnaces is required to have high strength quality. In the coal for producing such coke, high-quality coal is in a state of depletion in terms of resources, while low-quality coal is abundant. Therefore, it is desirable to increase the blending ratio of cheap low-quality coal.
[0003] When the blending ratio of low-quality coal is increased, the expansion and bonding of coal particles becomes insufficient, resulting in a decrease in coke strength. Therefore, it is important to accurately predict in advance the coke strength when low-quality coal is blended.
[0004] As a representative method for estimating coke strength, Patent Document 1 discloses a method in which the void filling degree at the time of coal softening and melting is calculated from the expansion specific volume SV at the time of coal softening and the charging bulk density BD, and the surface fracture strength of the coke is estimated from the void filling degree. The surface breaking strength is the 6mm index (DI) of drum strength. 150 6), that is, the percentage of the mass of coke on the sieve (particle size over 6 mm) sieved through a 6 mm sieve after the drum has been rotated 150 times to the total mass of charged coke. In the following, the surface destruction strength is defined as DI 150 Sometimes it is written as 6.
[0005] Coal is broadly classified into two categories based on its total expansion rate: coal with a total expansion rate of over 0% and inferior coal with a total expansion rate of 0%. Coal with a total expansion rate of over 0% is further classified into two categories: high-rank coal, whose resolidification temperature, as measured by the fluidity test method of JIS M8801, is 470°C or higher, and low-rank coal, whose resolidification temperature is below 470°C.
[0006] When estimating the surface fracture strength of coke from a coal blend containing inferior quality coal based on the void filling degree, the weighted average of the measured values of each coal in the coal blend is used as the expansion specific volume. However, when the blending ratio of low-quality coal increases, additivity does not hold for the expansion specific volume of coal, so the method disclosed in Patent Document 1 may not be able to estimate the surface fracture strength with sufficient accuracy.
[0007] In order to estimate the strength of coke produced when a coal blend containing these coals is carbonized, the concept of the inhibition of expansion property of low-rank coal or inferior quality coal compared to high-rank coal is important, and it has been made clear, for example in Patent Document 2, that this inhibition of expansion property can be quantified by an index called the inert factor (inert coefficient). However, Patent Document 2 targets coal that expands when heated at a heating rate of 3.0°C / min using an apparatus specified in JIS M8801, and does not disclose any estimation of coke strength when blending inferior coal with a total expansion rate of 0%.
[0008] In contrast, Patent Document 3 discloses a method for estimating the surface rupture strength of coke produced by using inferior coal with a total expansion coefficient of 0% as part of a coal blend, in which an inert factor related to the surface rupture strength of high-rank coal is calculated using the value of the specific volume of the inferior coal measured at a heating rate of 3°C / min or more during rapid heating, and this is used to experimentally obtain a correlation line between the specific volume of the inferior coal measured at rapid heating and the inert factor coefficient to calculate an estimate of the surface rupture strength of high-rank coal, and this estimate and the estimate of the surface rupture strength of the inferior coal are used to calculate a weighted average based on the blending ratio of high-rank coal to inferior coal in the coal blend, thereby estimating the surface rupture strength of the coke. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Patent No. 3971563 [Patent Document 2] Japanese Patent Application Publication No. 9-255965 [Patent Document 3] JP 2016-69469 A Summary of the Invention [Problem to be solved by the invention]
[0010] Patent Document 3 makes it possible to estimate the inert factor coefficient of inferior coal with a volatile content of 30% by mass or more, but does not disclose an estimation of the inert factor coefficient of inferior coal with a volatile content of less than 30% by mass. Therefore, the present invention aims to estimate the inert factor coefficient of inferior coal with a total expansion coefficient TD of 0% in a simple manner, even when the coal contains inferior coal with a volatile content VM of less than 30% by mass, and to use this value to estimate the surface fracture strength of coke made from a coal blend containing inferior coal. [Means for solving the problem]
[0011] It was found that there is a certain correlation between the solvent extraction rate of low-quality coal and the inert factor coefficient.
[0012] The gist of the present invention, which was made based on such findings, is as follows. [1] A solvent extraction rate measurement step of solvent-extracting a predetermined weight of coal and determining a solvent extraction rate (α), which is the ratio of the amount of solvent extraction to the weight of the coal; an αi-fi correlation acquisition step of performing the solvent extraction rate measurement step for a plurality of different coals to obtain a relationship (αi-fi correlation) between the solvent extraction rate (αi) of the coal and the inert factor coefficient (fi) of the coal; an inert factor coefficient estimation step of measuring the solvent extraction rate of an unknown coal by carrying out the solvent extraction rate measurement step for the unknown coal, and calculating an inert factor coefficient f' of the unknown coal using α' and the αi-fi correlation; A method for estimating the inert factor coefficient of coal, comprising: [2] The coal is a low-quality coal having a total expansion coefficient of 0%; The method for estimating an inert factor coefficient of coal according to [1], wherein the inert factor coefficient is the inert factor coefficient of a coal blend obtained by blending the inferior quality coal with high-rank coal having a total expansion coefficient of more than 0% and a resolidification temperature of 470°C or higher as measured by the fluidity test method of JIS M8801, or with low-rank coal having a total expansion coefficient of more than 0% and a resolidification temperature of less than 470°C as measured by the fluidity test method of JIS M8801. [3] The method for estimating the inert factor coefficient of coal according to [1] or [2], characterized in that the solvent is a mixed solvent of carbon disulfide and N-methyl-2-pyrrolidone. [4] A method for estimating the surface fracture strength of blast furnace coke produced by using inferior coal as part of a coal blend, comprising: The blended coal is composed of high-rank coal, which has a total expansion rate of more than 0% and a coal resolidification temperature of 470°C or higher as measured by the fluidity test method of JIS M8801, and low-quality coal, which has a total expansion rate of 0%. In order to estimate the surface fracture strength of coke produced from a coal blend to be used in an actual coke oven, the necessary relationships are first obtained by the following procedures (A) to (B): (A) Using various coal blends, a relationship (a1) between the void filling degree, which is expressed by the product (SV × BD) of the expansion specific volume SV of the actually measured coal blend and the charging bulk density BD, and the surface fracture strength of the resulting coke is obtained; (B) Classify inferior coal with a total expansion rate of 0% into low VM inferior coal with a volatile matter VM of more than 10% by mass and less than 30% by mass, and high VM inferior coal with a VM of 30% by mass or more, and obtain the relationship between the expansion index of the low VM inferior coal and the high VM inferior coal and the inert factor coefficient (f) in the inert factor (IF) in the following formula (1) as follows: (B1) A high VM inferior coal is heated at a predetermined heating rate S1 higher than 3°C / min, and the high rate heating expansion specific volume SV'(H) is measured as an expansion index; (B2) The relationship (b2) between the measured high-speed heating expansion specific volume SV' (H) of the high VM inferior coal and the inferior coal inert factor coefficient (f) is obtained. (B3) Measure the solvent extraction rate (α) of low VM inferior coal with a solvent, (B4) The relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f) is determined. Next, to estimate the surface fracture strength of blast furnace coke produced from the blended coal to be used in an actual coke oven, steps (C) to (H) are carried out. (C) Determine the void filling rate of the high-rank coal in the blended coal to be used; (D) Determine the void filling degree of inferior coal in the blended coal to be used; (E) When the inferior coal in the coal blend used is a high VM inferior coal, the rapid heating expansion specific volume SV'(E) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained SV'(E) and the above (b2), (F) When the inferior coal in the coal blend used is a low VM inferior coal, the solvent extraction rate (α) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained solvent extraction rate (α) and the above (b3), (G) Calculate the inert factor (IF) according to the blending ratio of low-quality coal, and calculate the corrected void filling ratio of high-rank coal from the product of the void filling ratio of the high-rank coal calculated in (C) above and the IF; (H) calculating a weighted average of the corrected void filling degree of the high-rank coal calculated in (G) and the void filling degree of the low-rank coal calculated in (D) based on the blending ratio of the high-rank coal and the low-rank coal in the coal blend used to calculate the void filling degree of the coal blend, and calculating an estimated value of the surface fracture strength of the coke from the relationship in (a1), wherein: IF = 1.00 - fx (1) Here, the method for estimating the surface fracture strength of coke is characterized in that IF: inert factor [-], f: inert factor coefficient [-], and x: blending ratio of low-quality coal [mass%]. [5] A method for estimating the surface fracture strength of blast furnace coke produced by using low-quality coal as part of a coal blend, comprising: The blended coal is composed of high-rank coal, which has a total expansion rate of more than 0% and a coal resolidification temperature of 470°C or higher as measured by the fluidity test method of JIS M8801, and low-quality coal, which has a total expansion rate of 0%. In order to estimate the surface fracture strength of coke produced from a coal blend to be used in an actual coke oven, the necessary relationships are first obtained by the following procedures (A) to (B): (A) Using various coal blends, a relationship (a1) between the void filling degree, which is expressed by the product (SV × BD) of the expansion specific volume SV of the actually measured coal blend and the charging bulk density BD, and the surface fracture strength of the resulting coke is obtained; (B) Classify inferior coal with a total expansion rate of 0% into low VM inferior coal with a volatile matter VM of more than 10% by mass and less than 30% by mass, and high VM inferior coal with a VM of 30% by mass or more, and obtain the relationship between the expansion index of the low VM inferior coal and the high VM inferior coal and the inert factor coefficient (f) in the inert factor (IF) in the following formula (1) as follows: (B1) Measure the solvent extraction rate (α) of high VM inferior coal by solvent, (B2) Determine the relationship (b2') between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f), (B3) Measure the solvent extraction rate (α) of low VM inferior coal with a solvent, (B4) The relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f) is determined. Next, to estimate the surface fracture strength of blast furnace coke produced from the blended coal to be used in an actual coke oven, steps (C) to (H) are carried out. (C) Determine the void filling rate of the high-rank coal in the blended coal to be used; (D) Determine the void filling degree of inferior coal in the blended coal to be used; (E) When the inferior coal in the coal blend used is a high VM inferior coal, the solvent extraction rate (α) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained solvent extraction rate (α) and the above (b2'), (F) When the inferior coal in the coal blend used is a low VM inferior coal, the solvent extraction rate (α) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained solvent extraction rate (α) and the above (b3), (G) Calculate the inert factor (IF) according to the blending ratio of low-quality coal, and calculate the corrected void filling ratio of high-rank coal from the product of the void filling ratio of the high-rank coal calculated in (C) above and the IF; (H) calculating a weighted average of the corrected void filling degree of the high-rank coal calculated in (G) and the void filling degree of the low-rank coal calculated in (D) based on the blending ratio of the high-rank coal and the low-rank coal in the coal blend used to calculate the void filling degree of the coal blend, and calculating an estimated value of the surface fracture strength of the coke from the relationship in (a1), wherein: IF = 1.00 - fx (1) Here, the method for estimating the surface fracture strength of coke is characterized in that IF: inert factor [-], f: inert factor coefficient [-], and x: blending ratio of low-quality coal [mass%]. [6] The relationship (b2) between the inert factor coefficient (f) and the high-rate heating expansion specific volume SV' (E) of the high-VM inferior coal is the expansion specific volume [cm 3 / g] is used, the relationship (b2) between the inert factor coefficient (f) of the low VM inferior coal and the solvent extraction rate (α) of the low VM inferior coal is expressed by the following formula (b3): f=d1SV' 4 -d2SV' 3 +d3SV' 2 -d4SV'+d5···(b2) f=a1α 2 +a2α+a3···(b3) where f is the inert factor coefficient [-], SV' is the expansion specific volume SV' (H) [cm measured at 12°C / min 3 / g], α: solvent extraction rate [%], and d1 to d5 and a1 to a3 are constants that can be experimentally determined. [7] The relationship (b2') between the inert factor coefficient (f) of the high VM inferior coal and the solvent extraction rate (α) of the high VM inferior coal is expressed by the following formula (b2'), and the relationship (b3) between the inert factor coefficient (f) of the low VM inferior coal and the solvent extraction rate (α) is expressed by the following formula (b3): f=a 1’ α 2 +a 2’ α+a 3’ (b2') f=a1α 2 +a2α+a3···(b3) where f is the inert factor coefficient [-], α is the solvent extraction rate [%], and a 1’ ~a 3’ and a1 to a3 are constants that can be experimentally determined. [8] The blended coal further contains low-rank coal having a total expansion rate of more than 0% and a coal resolidification temperature of less than 470°C as measured by the fluidity test method of JIS M8801, and (B) above is replaced with the following (B') and (G) above is replaced with the following (G'): (B') Classify inferior coal with a total expansion coefficient of 0% into low VM inferior coal with a volatile matter VM of more than 10% by mass and less than 30% by mass, and high VM inferior coal with a VM of 30% by mass or more, and determine in advance the relationship between the expansion index of low VM inferior coal, high VM inferior coal, and low coal rank coal and the inert factor coefficient (f) in the inert factor (IF) in the above formula (1) as follows, (B1) When high VM inferior coal is heated at a predetermined heating rate S1 higher than 3 ° C / min, the high rate heating expansion specific volume SV' (H) is measured as an expansion index, (B2) The relationship (b2) between the measured expansion specific volume SV' (H) of the high VM inferior coal and the inferior coal inert factor coefficient (f) is obtained. (B3) Measure the solvent extraction rate (α) of low VM inferior coal with a solvent, (B4) The relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f) is determined. (B5) The low-rank coal inert factor coefficient (f) is set to 0.0057; (G') calculating an inert factor (IF) corresponding to the blending ratio of low-quality coal and low-coalification coal using the inert factor coefficient (f) calculated in (E) and / or (F) above according to the expansion specific volume of the low-quality coal used and the inert factor coefficient (f) of low-coalification coal determined in (B5) above, and calculating a corrected void filling degree of high-coalification coal from the product of the void filling degree of the high-coalification coal calculated in (C) above and the IF; The method for estimating the surface fracture strength of coke according to [4] or [6], characterized in that: [9] The blended coal further contains low-rank coal having a total expansion rate of more than 0% and a coal resolidification temperature of less than 470°C as measured by the fluidity test method of JIS M8801, and (B) above is replaced with the following (B') and (G) above is replaced with the following (G'): (B') Classify inferior coal with a total expansion coefficient of 0% into low VM inferior coal with a volatile matter VM of more than 10% by mass and less than 30% by mass, and high VM inferior coal with a VM of 30% by mass or more, and determine in advance the relationship between the expansion index of low VM inferior coal, high VM inferior coal, and low coal rank coal and the inert factor coefficient (f) in the inert factor (IF) in the above formula (1) as follows, (B1) Measure the solvent extraction rate (α) of high VM inferior coal by solvent, (B2) Determine the relationship (b2') between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f), (B3) Measure the solvent extraction rate (α) of low VM inferior coal with a solvent, (B4) The relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f) is determined. (B5) The low-rank coal inert factor coefficient (f) is set to 0.0057; (G') calculating an inert factor (IF) corresponding to the blending ratio of low-quality coal and low-coalification coal using the inert factor coefficient (f) calculated in (E) and / or (F) above according to the expansion specific volume of the low-quality coal used and the inert factor coefficient (f) of low-coalification coal determined in (B5) above, and calculating a corrected void filling degree of high-coalification coal from the product of the void filling degree of the high-coalification coal calculated in (C) above and the IF; The method for estimating the surface fracture strength of coke according to [5] or [7], characterized in that:
[10] The method for estimating the surface fracture strength of coke according to any one of [4] to [9], wherein the solvent is a mixed solvent of carbon disulfide and N-methyl-2-pyrrolidone.
[11] A method for estimating the surface fracture strength of coke described in any one of [4] to
[10] , characterized in that the oxygen content of the low VM poor-quality coal is more than 2 mass% and less than 7 mass%, and the oxygen content of the high VM poor-quality coal is 7 mass% or more. Effect of the Invention
[0013] According to the present invention, the inert factor coefficient, which is the coefficient at which inferior coal with a volatile matter VM of less than 30 mass% inhibits the expansibility of high-rank coal and / or low-rank coal, can be estimated by a simple method called solvent extraction, and the surface fracture strength of coke can be estimated using this value. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a diagram showing the relationship between the blending ratio of inferior coal, which is the basis for deriving the inert factor coefficient, and the obtained expansion specific volume. [Diagram 2] FIG. 2 is a diagram showing the relationship between the blending ratio of inferior coal, which is the basis for deriving the inert factor coefficient, and the inert factor obtained from FIG. 1. [Diagram 3] FIG. 1 is a graph showing an example of the relationship between the SV value and the inert factor coefficient of inferior coal measured at a heating rate of 12° C. / min. [Figure 4] FIG. 1 is a graph showing an example of the relationship between the solvent extraction rate of low VM inferior coal and the inert factor coefficient of a coal blend in which the low VM inferior coal is blended with high-rank coal. [Diagram 5] FIG. 1 is a diagram showing an example of the relationship between the corrected void filling rate and the surface breakdown strength according to the present invention. [Figure 6] FIG. 2 is a diagram showing an example of the relationship between the amount of oxygen and the amount of volatile matter in inferior coal. [Figure 7] FIG. 1 is a diagram for comparing the estimated and actually measured values of surface fracture strength with respect to the blending ratio of inferior coal in Example 1. [Figure 8] FIG. 11 is a diagram for comparing the estimated and actually measured values of the surface breakdown strength for Example 2. [Figure 9] FIG. 1 is a diagram showing an example of the relationship between the solvent extraction rate of low-VM inferior coal and the inert factor coefficient of a coal blend containing the low-VM inferior coal and low-coalification coal. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <First embodiment> In a first embodiment of the present invention, the surface fracture strength of coke produced using a coal blend containing high-rank coal, which has a total expansion coefficient of more than 0% and a coal resolidification temperature of 470°C or higher as measured by the fluidity test method of JIS M8801, and low-quality coal, which has a total expansion coefficient of 0%, is estimated based on a weighted average value of the void filling degree at the time of softening of the high-rank coal, which is calculated from the product (SV×BD×IF) of the expansion specific volume SV, the charging bulk density BD, and the inert factor (IF) of the blended high-rank coal, and the void filling degree of the low-quality coal, based on a relationship between the void filling degree and the surface fracture strength, which is calculated from the expansion specific volume value of the blended coal actually measured in advance. Inferior coal with a total expansion rate of 0% is classified into low VM inferior coal with a volatile matter VM of more than 10% by mass but less than 30% by mass, and high VM inferior coal with a VM of 30% by mass or more. The relationship between the expansion index of high VM inferior coal and the inert factor coefficient (f) in the inert factor (IF) and the relationship between the solvent extraction rate of low VM inferior coal and the inert factor coefficient are determined in advance, and the surface fracture strength of coke is estimated using the inert factor coefficient (f) of low VM inferior coal and / or high VM inferior coal depending on the blend of coal to be estimated.
[0016] The inventors investigated the effect of inferior coal with a total expansion coefficient TD of 0% and a volatile matter VM of less than 30% by mass on the expansion of high-rank coal. As a result, for inferior coal with a volatile matter VM of less than 30% by mass, as in Patent Document 3, no specific correlation was found between the expansion specific volume (SV') and the inert factor coefficient, measured by heating at a rate of 12°C / min, which is faster than the heating rate (3°C / min) specified in JIS M8801. Therefore, the extraction rate of low-quality coal (a, b, c, d) with a volatile matter VM of less than 30 mass% was measured using a mixed solvent of equal volumes of carbon disulfide and N-methyl-2-pyrrolidone, and a significant correlation was found between the measured value and the inert factor coefficient. The experiments that yielded these findings are described below.
[0017] First, similarly to Patent Document 3, the expansion specific volume of a coal blend in which high-rank coal was blended with low-VM inferior-quality coal was measured at the above-mentioned heating rate (3°C / min). From the results, the inert factor was calculated for each blending ratio, and the inert coefficient for each brand of low-VM inferior-quality coal was calculated from the relationship between the blending ratio and the inert factor.
[0018] Low VM inferior coals A to G with a volatile content VM of less than 30 mass% and high coal rank coal with the properties shown in Table 1 were used, and these were crushed to 1.5 mm or less (100 mass%). After that, 0 to 40 mass% of low VM inferior coal was blended with the high coal rank coal, and the bulk density was 0.90 g / cm 3 The high-rank coal and the blended coal were packed into a reaction tube so that the expansion specific volumes of the high-rank coal and the blended coal were measured by increasing the temperature in a heating furnace at a rate of 3° C. / min. The extraction of low VM poor quality coal with a carbon disulfide / N-methyl-2-pyrrolidone mixed solvent was carried out as follows. After crushing low VM inferior coal to 0.15 mm or less (100% by mass), 0.5 g was collected, mixed with 50 mL of a carbon disulfide / N-methyl-2-pyrrolidone mixed solvent, and ultrasonic vibration was applied. Then, solid-liquid separation was performed by centrifugation and filtration, the extraction residue was washed with acetone, and dried under reduced pressure at 80°C for 12 hours to obtain a solid powder, which was then weighed and the solvent extraction rate of the low VM inferior coal was measured from the difference from the weight of 0.5 g before the extraction operation. The above-mentioned conditions for solvent extraction of coal, including the coal particle size, coal weight, solvent amount, and drying conditions for the extraction residue, are examples of optimal conditions, but the conditions for solvent extraction of coal for estimating the inert factor of the present invention are not limited to the above. The measurement of the solvent extraction rate of each coal may be performed under the same solvent extraction conditions. The mixing ratio (volume ratio) of carbon disulfide and N-methyl-2-pyrrolidone is preferably in the range of 4:6 to 6:4. As other solvents, dimethylammonium-dimethylcarbamate, which is an ionic liquid, a mixed solvent of toluene and N-methyl-2-pyrrolidone, 1-methylnaphthalene, etc. may be used.
[0019] The relationship between the expansion specific volume measured for coal blends with different blend ratios of coal G and the blend ratio of coal G is shown in Figure 1. As shown in Figure 1, the actual measured values are below the weighted average line, which indicates that inferior coal inhibits the expansion of high-rank coal. In addition, for G coal, the inert factor at each blend ratio was calculated as the ratio (measured result / calculated value) of the expansion specific volume of high-rank coal (measured result) to the weighted average expansion specific volume (calculated value). The results are shown in Figure 2.
[0020] The inert factor (IF) is defined by the following formula (1). IF = 1.00 - fx (1) Here, IF is the inert factor [-], f is the inert factor coefficient [-], and x is the blending ratio of low-quality coal [mass%].
[0021] As shown in Figure 2, for G coal, there is a relationship between the blending ratio of low-quality coal and the inert factor. y=-0.0113x+1 From the absolute value of the slope of the line, the inert factor coefficient was obtained as 0.0113.
[0022] The inert factor coefficients for the other coals A to F were similarly determined. Table 2 shows the SV' values (SV 12°C / min) and inert factor coefficients measured at a heating rate of 12°C / min for coals A to G. In the following Tables 1 and 2, the data on volatile matter, ash content, total expansion coefficient, and SV12°C / min for coals A to F shown in Tables 1 and 2 of Patent Document 3 are cited as data for coals H to M.
[0023] [Table 1]
[0024] [Table 2]
[0025] FIG. 3 shows the relationship between the expansion specific volume SV' of inferior coal measured at a heating rate of 12° C. / min and the inert factor coefficient calculated as described above. From Figure 3, it can be seen that for inferior coal, even though the high-speed heating expansion specific volume value is the same, the inert factor coefficient can take two different values depending on the VM value. It was confirmed that for high-VM inferior coal with a VM of 30 mass% or more, the following relationship exists between SV12°C / min (SV') and the inert factor coefficient (f). f=0.088SV' 4 -0.656SV' 3 +1.820SV' 2 -2.239SV'+1.036
[0026] In contrast, for low-VM inferior coal with a VM of less than 10 to 30% by mass, even when measured at 12°C / min, no significant correlation was obtained between SV12°C / min (SV') and the inert factor coefficient (f) in the region with small expansion specific volume. Therefore, we attempted to measure the extraction rate using a mixed solvent of equal volumes of carbon disulfide and N-methyl-2-pyrrolidone. The results are shown in Table 3 and FIG. [Table 3]
[0027] Figure 4 shows that there is a clear relationship between the solvent extraction rate α and the inert factor coefficient, which is expressed by the following quadratic equation. f=-0.000013344α 2 -0.000211935α+0.013162819 ···(2)
[0028] In the present invention, based on the results of the above investigation, inferior coal is classified into high VM inferior coal with a VM of 30% by mass or more and low VM inferior coal with a VM of more than 10% by mass and less than 30% by mass. For high VM inferior coal, the inert factor coefficient is calculated from the expansion specific volume measured at a heating rate S1 of more than 3°C / min. For low VM inferior coal, the solvent extraction rate is measured to calculate the inert factor coefficient. The calculated inert factor coefficient is used to calculate an inert factor IF according to the brand and blending ratio of the inferior coal to be blended. A corrected void filling degree of the high-rank coal is calculated from the product of this IF and the void filling degree of the high-rank coal. This corrected void filling degree and the void filling degree of the inferior coal are then weighted and averaged with the blending ratio of the high-rank coal and the inferior coal in the coal blend used. An estimated value is obtained from the relationship between the void filling degree and surface fracture strength calculated in advance. The following describes the requirements and preferred requirements of the present invention.
[0029] (Target blended coal) There are the following types of coal: High-rank coal: Coal with a total expansion rate of over 0% and a resolidification temperature of 470°C or higher as measured by the fluidity test method of JIS M8801. Low rank coal: Coal with a total expansion rate of more than 0% and a coal resolidification temperature of less than 470°C as measured according to the JIS M8801 fluidity test method. Low-quality coal: Coal with a total expansion rate of 0% The present invention is directed to estimating the surface fracture strength of coke produced from a coal blend containing the above-mentioned high-coalification coal and low-quality coal, but can also be applied to cases where the blend further contains the above-mentioned low-coalification coal.
[0030] (Advance preparation) In the present invention, (A) the relationship between the void filling degree of a coal blend and coke strength, and (B) the relationships between the solvent extraction rate of low VM inferior coal and the expansion specific volume of high VM inferior coal, and the inert factor coefficient (f) in the inert factor (IF) in the following formula (1) are primarily determined in advance. Below, (A) and (B) will be explained in order.
[0031] (A) Determine the relationship between void filling degree and coke strength. The expansion specific volume SV of the coal blend was measured, and the void filling degree SV×BD was calculated from the product of the expansion specific volume SV and the bulk density BD. The coal blend was also carbonized in a test coke oven to produce a coke with a surface fracture strength of 100%. The void filling degree of the coal blend and the surface fracture strength DI of the coke were calculated. 150 The relationship between the expansion specific volume SV and 6 is obtained in advance. The obtained relationship is called (a1). An example is shown in Figure 5. Incidentally, the properties of the coal blend used here are not particularly specified, and various coals can be used. In addition, when obtaining the relationship in Figure 5, it is necessary to change the void filling degree SV x BD. The expansion specific volume SV can be changed by selecting coal with different properties, and the bulk density BD can be changed by adjusting the coal particle size, etc.
[0032] The expansion specific volume SV is measured as follows. First, powdered coal is charged to a specified density (0.80 [dry, g / cm) in a thin tube specified in JIS M8801. 3 ]) to a height of 60 mm, then a piston was inserted on top of the coal blend in the capillary tube, and with the piston inserted, the capillary tube was heated from 300°C to 600°C at a heating rate of 3.0±0.1°C / min, and the height of the coal blend after heating was completed was measured. In this study, the load applied by the piston to the coal was approximately 110 g. The height of the blended coal after heating was taken as L [mm]. The expansion specific volume [cm 3 / g] was calculated. Expansion specific volume=L / (60×0.8)
[0033] (B) Next, the inferior coal with a total expansion coefficient of 0% is classified into low VM inferior coal with a volatile matter VM of more than 10 mass% and less than 30 mass%, and high VM inferior coal with a VM of 30 mass% or more. The relationship between the expansion index of the low VM inferior coal and the high VM inferior coal and the inert factor coefficient (f) in the inert factor (IF) in the following formula (1) is calculated by the following steps (B1) to (B3). IF = 1.00 - fx (1) Here, IF is the inert factor [-], f is the inert factor coefficient [-], and x is the blending ratio of low-quality coal [%]. In addition, when it was impossible to actually measure the expansion specific volume (heating rate: 3°C / min) SV of inferior quality coal, the reciprocal of the bulk density 0.80 was used.
[0034] The inert factor and the inert factor coefficient are determined as follows. First, the expansion specific volumes of high-rank coal and low-quality coal alone are measured as described above, and the expansion specific volume of a coal blend of high-rank coal and low-quality coal is measured as described above, and the inert factor is calculated based on the deviation from the weighted average expansion specific volume of the coal blend (see Figures 1 and 2). Then, a linear relationship expressed by the above formula (1) is found between the blending ratio of low-quality coal and the inert factor, and the inert factor coefficient is calculated from that formula. In the example shown in FIG. 2, the following equation is used as the linear equation: y=-0.0113x+1 In addition, an example in which the inert factor coefficient (f) was calculated as 0.0113 is shown.
[0035] (B1) The rapid heating expansion specific volume SV'(H) of high VM inferior quality coal when it is heated at a predetermined heating rate S1 higher than 3°C / min, and the rapid heating expansion specific volume SV'(L) of low VM inferior quality coal when it is heated at a predetermined heating rate S2 higher than the heating rate S1 are measured as expansion indexes. The specified heating rate S1 higher than 3°C / min is set to a heating rate or higher at which expansibility appears for multiple high VM inferior quality coals used to determine the "relationship between the high rate heating expansion specific volume SV'(H) of high VM inferior quality coal and the inert factor coefficient (f) of inferior quality coal" in (B2), and is not particularly limited, but an example of this is a heating rate of 12°C / min or higher. (B2) The relationship (b2) between the high rate heating expansion specific volume SV' (H) and the inert factor coefficient (f) of each of the measured high VM inferior coals is determined. It was confirmed that there is a correlation between the inert factor coefficient (f) measured at a heating rate of 3°C / min and the expansion specific volume (SV') measured at a heating rate of 12°C / min, as expressed by the following formula (b2). For high VM inferior coal, by measuring the expansion specific volume (SV') at a heating rate of 12°C / min, it is possible to obtain a relationship with the inert factor coefficient (f). f=d1SV' 4 -d2SV' 3 +d3SV' 2 -d4SV'+d5···(b2) where f is the inert factor coefficient [-], SV' is the expansion specific volume SV' (H) [cm measured at a heating rate of 12°C / min 3 / g]. d1 to d5 are coefficients obtained experimentally, and in Figure 3, d1 = 0.088, d2 = 0.656, d3 = 1.820, d4 = 2.239, and d5 = 1.036.
[0036] (B3) Calculate the solvent extraction rate of low VM inferior coal.
[0037] (B4) Next, determine the relationship (b3) between the solvent extraction rate (α) and the inert factor coefficient (f). For low VM poor quality coal, the extraction rate (α) can be measured using a mixed solvent of equal volumes of carbon disulfide and N-methyl-2-pyrrolidone, giving a correlation with the inert factor coefficient (f). f=a1α 2 +a2α+a3···(b3) Here, f is the inert factor coefficient [-], and α is the solvent extraction rate (%). a1 to a3 are coefficients obtained experimentally, and in the example of FIG. 4, a1 = 0.000013344, a2 = -0.000211935, and a3 = 0.013162819.
[0038] (Estimation of surface destruction strength) The surface fracture strength of blast furnace coke produced from a coal blend to be used in an actual coke oven is estimated by the following steps (C) to (H). (C) The void filling degree, which is expressed as the product of the expansion specific volume and the charging bulk density of the high rank coal in the coal blend used, is calculated. When there is more than one high-rank coal, the SV of the high-rank coal is the weighted average value.
[0039] (D) The void filling degree of the inferior coal, which is expressed by the product of the expansion specific volume of the inferior coal in the coal blend used and the charging bulk density, is calculated. When there is more than one inferior quality coal, the SV of the inferior quality coal is calculated using the weighted average value.
[0040] (E) When the inferior coal in the coal blend used is high VM inferior coal, the expansion specific volume SV'(H) is calculated, and the inert factor coefficient (f) is calculated from the relationship between the calculated SV'(H) and the above (b4).
[0041] (F) When the inferior coal in the coal blend used is a low VM inferior coal, the solvent extraction rate (α) is calculated, and the inert factor coefficient (f) is calculated according to the relationship between the calculated solvent extraction rate (α) and the inert factor coefficient (f).
[0042] (G) Using the inert factor coefficient (f) determined in (E) and / or (F) above according to the expansion specific volume SV' (H) and / or solvent extraction rate (α) of the inferior coal, determine the inert factor (IF) corresponding to the blending ratio of the inferior coal, and determine the corrected void filling ratio of the high-rank coal from the product of the void filling ratio of the high-rank coal determined in (C) above and the IF. When multiple inferior-rank coals are blended, the IF determined as the weighted average based on the blending amounts of all inferior-rank coals is used.
[0043] (H) The corrected void filling degree of the high-rank coal calculated in (G) above and the void filling degree of the low-rank coal calculated in (D) above are weighted and averaged with the blending ratio of the high-rank coal and the low-rank coal in the coal blend used, and an estimate of the surface fracture strength of the coke is obtained from the relationship in (a1) above.
[0044] <Second embodiment> The method for estimating coke surface fracture strength according to the second embodiment of the present invention will be described below with respect to differences from the first embodiment. In this embodiment, the inert factor coefficients of not only low VM inferior coal but also high VM inferior coal are estimated based on the solvent extraction rate of each coal. That is, (B1) and (B2) in the first embodiment are replaced as follows. (B1) Measure the solvent extraction rate (α) of high VM inferior coal by solvent, (B2) Determine the relationship (b2') between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f), (B3) Measure the solvent extraction rate (α) of low VM inferior coal with a solvent, (B4) The relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f) is determined. The method for measuring the solvent extraction rate is as described above. In addition, the relationship (b2') between the inert factor coefficient (f) of high VM inferior coal and the solvent extraction rate (α) of the high VM inferior coal is expressed by the following formula (b2'), and the relationship (b3) between the inert factor coefficient (f) of the low VM inferior coal and the solvent extraction rate (α) is expressed by the following formula (b3). f=a 1’ α 2 +a 2’ α+a 3’ (b2') f=a1α 2 +a2α+a3···(b3) Here, f is the inert factor coefficient [-], and α is the solvent extraction rate [%]. 1’ ~a 3’ and a1 to a3 are constants that are experimentally determined. Furthermore, (E) and (F) in the first embodiment are replaced as follows. (E) When the inferior coal in the coal blend used is a high VM inferior coal, the solvent extraction rate (α) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained solvent extraction rate (α) and the above (b2'). (F) When the inferior coal in the coal blend used is a low VM inferior coal, the solvent extraction rate (α) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained solvent extraction rate (α) and the above (b3). The other procedures of this embodiment are similar to those of the first embodiment.
[0045] By using the above-mentioned procedures, the present invention is capable of accurately estimating the surface fracture strength of a coal blend in which high-rank coal is blended with lower-quality coal, etc.; however, the inventors further investigated the reason why the correlation between the rapid heating specific volume of lower-quality coal and the inert factor coefficient varies depending on the VM value. As a result, it was found that the volatile matter in coal is correlated with the oxygen content, that inferior coal with a high oxygen content has an oxygen expansion inhibitory effect on high-rank coal, and that inferior coal with a low oxygen content has a small oxygen expansion inhibitory effect on high-rank coal, and that the relationship between the rapid heating expansion specific volume and the inert factor coefficient differs depending on the VM range.
[0046] Therefore, the oxygen content of the low VM inferior coals A to F was measured and the relationship with the VM value was examined. For the high VM inferior coal, the data on oxygen content and VM value disclosed in Japanese Patent No. 4691212 was used. The obtained results are shown in Figure 6. From these results, it was confirmed that high VM inferior coal is coal with an oxygen content of 7 mass% or more, and low VM inferior coal is coal with an oxygen content of 2 mass% or more and less than 7 mass%. This also shows that it is possible to distinguish between low VM and high VM inferior coals based on the oxygen content.
[0047] In addition, just as the inert factor coefficient when low-quality coal is blended with high-quality coal can be calculated from the solvent extraction rate of low-quality coal, the inert factor coefficient when low-quality coal is blended with low-quality coal can also be calculated from the solvent extraction rate of low-quality coal. That is, the expansion specific volumes of low-quality coal and low-quality coal alone are measured as described above, and the expansion specific volume of a coal blend in which low-quality coal is blended with low-quality coal is measured as described above, and the inert factor is calculated based on the deviation from the weighted average expansion specific volume of the coal blend. More specifically, the inert factor at each blending ratio is calculated as the ratio (measured result / calculated value) of the expansion specific volume of the coal blend (measured result) to the expansion specific volume (calculated value) by the weighted average. Then, a linear relationship expressed by the above formula (1) is found between the blending ratio of low-quality coal and the inert factor, and the inert factor coefficient is calculated from the formula. The inert factor coefficient is calculated for multiple different low-quality coals according to the above method. Next, the solvent extraction rate (α) is measured for each inferior coal according to the method described above. Then, the correlation between the solvent extraction rate and the inert factor coefficient is obtained. Here, the inferior coal may be either low VM or high VM. In this way, the relationship between the solvent extraction rate and the inert factor coefficient as shown in FIG. 4 or formula (b3) is obtained. Therefore, by measuring the solvent extraction rate of the inferior coal to be measured, the inert factor coefficient for the blend of this inferior coal with a low-rank coal can be estimated. Figure 9 shows the relationship between the solvent extraction rate obtained for inferior coals a to d listed in Table 3 and the inert factor coefficient when blended with low-rank coal. The low-rank coal used had a total expansion rate of 60 volume %, a resolidification temperature of 462°C, an ash content of 8.7 mass %, and a volatile matter content of 37.6 mass %. Figure 9 shows a clear relationship between the solvent extraction rate α and the inert factor coefficient, which is expressed by the following quadratic equation. f=-0.00002425α 2 +0.00008552α+0.01379491 EXAMPLES
[0048] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to the contents of these examples.
[0049] Example 1 Strength was estimated when two types of coal were blended: high-rank coal and low-VM inferior coal (Coal G in Table 1 was used). Table 5 shows the measured coke strength values for coke made by varying the blending amount of low-VM inferior coal. The high-rank coal used had the following properties: total expansion coefficient of 124% by volume, resolidification temperature of 496°C, ash content of 11.0% by mass, and volatile matter of 23.6% by mass. The estimation was based on the void filling degree of the coal blend (the product of the measured SV and bulk density of the coal blend) and the surface destruction strength DI. 150 The relationship between the two shown in FIG. 5 was obtained by previously determining the relationship between the actual measured values of 6.
[0050] The coal used was crushed to 90% by mass of 3.0 mm or less and mixed as shown in Table 5. The bulk density of the coal charged in the actual machine was 0.80 g / cm. 3 After packing the mixture at an equivalent bulk density, it was carbonized in a test coke oven (Nomura et al., 2004 Fuel 38 1771-1776) with a furnace temperature equivalent to 1250°C of an actual oven.
[0051] [Table 5]
[0052] Since coal G is a low-VM, inferior coal with a VM of <30, the inert factor coefficient was estimated using solvent extraction. Since coal G has an extraction rate of 6.3%, the inert factor coefficient (f) was calculated as 0.0113 from the previously calculated relationship (b2) in Figure 4. Next, the inert factor IF was calculated from formula (1), and the void filling ratio of high-rank coal (SV*BD*IF) and that of inferior coal (SV*BD) were calculated by setting the expansion specific volume (heating rate: 3°C / min) SV of high-rank coal to 2.15, the expansion specific volume (heating rate: 3°C / min) SV of low-VM inferior coal to 1.25, and the bulk density to 0.80. Note that since it is impossible to actually measure the expansion specific volume (heating rate: 3°C / min) SV of low-VM inferior coal, the reciprocal of the bulk density of 0.80 was used. The weighted average value of the void filling degree of the coal blend was derived based on the blending ratio of high-rank coal and low-rank coal, and the surface fracture strength of the coke was estimated using the correlation in Figure 5. The calculated values and the coke surface fracture strength DI of the blended coal obtained from Figure 5 150 The estimated values of 6 are shown in Table 6. Comparing Tables 5 and 6, it can be seen that according to the method of the present invention, the blending ratio of low-quality coal can be accurately estimated from 0 volume % to 30 volume %.
[0053] [Table 6]
[0054] Next, as Comparative Example 1, the method disclosed in Patent Document 2 (JP Patent Publication No. 9-255965) was used to estimate coke strength while keeping the inert factor coefficients of all low VM inferior coal constant. The results are shown in Table 7 and Figure 7. The inert factor coefficient was set to 0.0057. A comparison of Tables 5 and 7 shows that in Comparative Example 1, when the blending ratio of inferior coal was 30 volume %, the surface fracture strength of the coke was overestimated. In addition, as Comparative Example 2, the inert factor coefficient estimation method for high VM poor quality coal disclosed in Patent Document 3 (JP Patent Publication No. 2016-69469) was applied to low VM poor quality coal, and (f=0.088SV' 4 -0.656SV' 3 +1.820SV' 2 The results of estimating the strength of coke using the inert factor coefficient when applying the inert factor coefficient f = 0.088SV' + 1.036 to low VM poor quality coal are shown in Table 8. 4 -0.656SV'3 +1.820SV' 2 When the inert factor coefficient is applied, −2.239SV′+1.036), the inert factor coefficient is 0.0239. Comparing Tables 5 and 8, it can be seen that in Comparative Example 2, when the blending ratio of low-quality coal is 30 volume %, the surface fracture strength of the coke is underestimated. From Tables 7 and 8 and FIG. 7, it can be seen that the estimation method of the present invention improves the estimation accuracy of the coke surface breakdown strength compared to the conventional estimation methods of Comparative Example 1 and Comparative Example 2.
[0055] [Table 7]
[0056] [Table 8]
[0057] Example 2 Strength was estimated when three types of coal - high-rank coal, low-rank coal, and inferior quality coal (Coal G in Table 1) - were blended in the proportions shown in Table 9. The high-rank coal used had the same properties as those in Example 1. The low-rank coal used had a total expansion rate of 26% by volume, a resolidification temperature of 460°C, an ash content of 8.8% by mass, and a volatile matter content of 35.5% by mass. The coal was carbonized in the same manner as in Example 1. Table 9 shows the coke surface fracture strength DI of the prepared coke. 150 The actual measured values of 6 are also shown.
[0058] [Table 9]
[0059] Since coal G is a low-VM, inferior coal with a VM of <30, the inert factor coefficient was estimated using solvent extraction. Since coal G has an extraction rate of 6.3%, the inert factor coefficient (f) was calculated as 0.0113 from the previously calculated relationship (b2) in Figure 4. Next, the inert factor IF was calculated from formula (1), and the expansion specific volume (heating rate: 3°C / min) SV of high-rank coal was set to 1.79, the expansion specific volume (heating rate: 3°C / min) SV of low-rank coal was set to 1.30, the expansion specific volume (heating rate: 3°C / min) SV of low-VM inferior coal was set to 1.25, and the bulk density was set to 0.80. The corrected space filling ratio (SV*BD*IF) of high-rank coal and the space filling ratio (SV*BD) of low-rank coal and inferior coal were calculated. Note that since it is impossible to actually measure the expansion specific volume (heating rate: 3°C / min) SV of low-VM inferior coal, the reciprocal of the bulk density of 0.80 was used. The weighted average value of the space filling degree of the coal blend was then derived based on the blending ratio of high-rank coal, low-rank coal, and inferior quality coal, and the surface fracture strength of the coke was estimated using the correlation in Figure 5.
[0060] Next, as Comparative Example 3, the method disclosed in Patent Document 2 (JP Patent Publication 9-255965 A) was used to estimate the coke strength by setting the inert factor coefficients of all low VM inferior coals to a constant value. The inert factor coefficient was set to 0.0057. In addition, as Comparative Example 4, the inert factor coefficient estimation method for high VM poor quality coal disclosed in Patent Document 3 (JP Patent Publication No. 2016-69469) was applied to low VM poor quality coal to obtain the formula (f=0.088SV' 4 -0.656SV' 3 +1.820SV' 2 The inert factor coefficient was used to estimate coke strength when the inert factor (-2.239SV'+1.036) was applied to low VM inferior coal. For G coal (f=0.088SV' 4 -0.656SV' 3 +1.820SV' 2 -2.239SV'+1.036), the inert factor coefficient is 0.0239.
[0061] The coke surface fracture strength DI of the blended coal obtained from the calculated values during the estimation and Figure 5 for the present invention and the comparative example 150 The estimated values for 6 are shown in Table 10. The actual measurements and the estimated values are shown in Figure 8. From Table 10 and FIG. 8, it can be seen that the estimation method of the present invention improves the estimation accuracy of the coke surface breakdown strength compared to the conventional estimation methods of Comparative Example 3 and Comparative Example 4.
[0062] [Table 10]
Claims
1. a solvent extraction rate measuring step of solvent-extracting a predetermined weight of coal and determining a solvent extraction rate (α) which is a ratio of the amount of the solvent extraction to the weight of the coal; an αi-fi correlation acquisition step of performing the solvent extraction rate measurement step for a plurality of different coals and determining a relationship (αi-fi correlation) between the solvent extraction rate (αi) of the coal and the inert factor coefficient (fi) of the coal; The solvent extraction rate measurement step is carried out for an unknown coal to measure the solvent extraction rate (α') of the unknown coal, and an inert factor coefficient f' of the unknown coal is calculated using α' and the αi-fi correlation; an inert factor coefficient estimation step, wherein the solvent is a mixed solvent obtained by mixing carbon disulfide and N-methyl-2-pyrrolidone, and the mixing ratio (volume ratio) of carbon disulfide to N-methyl-2-pyrrolidone is in the range of 4:6 to 6:4; A method for estimating the inert factor coefficient of coal, comprising:
2. The coal is a low-quality coal having a total expansion coefficient of 0%, 2. The method for estimating an inert factor coefficient of coal according to claim 1, wherein the inert factor coefficient is an inert factor coefficient of a coal blend obtained by blending the inferior quality coal with high-rank coal having a total expansion coefficient of more than 0% and a resolidification temperature of 470°C or higher as measured by the fluidity test method of JIS M8801, or with low-rank coal having a total expansion coefficient of more than 0% and a resolidification temperature of less than 470°C as measured by the fluidity test method of JIS M8801.
3. A method for estimating the surface fracture strength of blast furnace coke produced by using low-quality coal as a part of a coal blend, comprising: The blended coal is composed of high-rank coal, which has a total expansion rate of more than 0% and a coal resolidification temperature of 470°C or higher as measured by the fluidity test method of JIS M8801, and low-quality coal, which has a total expansion rate of 0%. In order to estimate the surface fracture strength of coke produced from a coal blend to be used in an actual coke oven, the necessary relationships are obtained in advance by the following procedures (A) to (B): (A) Using various coal blends, a relationship (a1) between the void filling degree, which is represented by the product (SV×BD) of the expansion specific volume SV and the charging bulk density BD of the actually measured coal blends, and the surface fracture strength of the resulting coke is obtained; (B) Classify inferior coals having a total expansion coefficient of 0% into low VM inferior coals having a volatile matter VM of more than 10% by mass and less than 30% by mass, and high VM inferior coals having a VM of 30% by mass or more, and obtain the relationship between the expansion indexes of the low VM inferior coals and the high VM inferior coals and the inert factor coefficient (f) in the inert factor (IF) in the following formula (1) as follows: (B1) High VM poor quality coal is heated at a predetermined heating rate S higher than 3 ° C / min 1 The rapid heating expansion specific volume SV'(H) when the temperature was raised at (B2) determining the relationship (b2) between the measured high-rate heating expansion specific volume SV' (H) of the high VM inferior coal and the inferior coal inert factor coefficient (f); (B3) Measure the solvent extraction rate (α) of low VM poor quality coal with a solvent; (B4) determining the relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f); Next, in order to estimate the surface fracture strength of blast furnace coke produced from the blended coal to be used in an actual coke oven, steps (C) to (H) are carried out; (C) determining the void filling degree of the high-rank coal in the blended coal to be used; (D) determining the void filling degree of inferior coal in the blended coal to be used; (E) When the inferior coal in the coal blend used is a high VM inferior coal, the rapid heating expansion specific volume SV'(E) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained SV'(E) and (b2); (F) When the inferior coal in the coal blend used is a low VM inferior coal, the solvent extraction rate (α) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained solvent extraction rate (α) and the above (b3); (G) calculating an inert factor (IF) according to the blending ratio of low-quality coal, and calculating a corrected void filling ratio of the high-coalification coal from the product of the void filling ratio of the high-coalification coal calculated in (C) and the IF; (H) The corrected void filling degree of the high-rank coal obtained in (G) and the void filling degree of the low-rank coal obtained in (D) are weighted and averaged with the blending ratio of the high-rank coal and the low-rank coal in the coal blend to obtain the void filling degree of the coal blend, and an estimated value of the surface fracture strength of the coke is obtained from the relationship in (a1), where IF=1.00-fx (1) Here, IF is the inert factor [-], f is the inert factor coefficient [-], and x is the blending ratio of inferior coal [mass%]. The method for estimating the surface fracture strength of coke, wherein the solvent is a mixed solvent of carbon disulfide and N-methyl-2-pyrrolidone, and the mixing ratio (volume ratio) of carbon disulfide to N-methyl-2-pyrrolidone is in the range of 4:6 to 6:
4.
4. A method for estimating the surface fracture strength of blast furnace coke produced by using low-quality coal as a part of a coal blend, comprising: The blended coal is composed of high-rank coal, which has a total expansion rate of more than 0% and a coal resolidification temperature of 470°C or higher as measured by the fluidity test method of JIS M8801, and low-quality coal, which has a total expansion rate of 0%. In order to estimate the surface fracture strength of coke produced from a coal blend to be used in an actual coke oven, the necessary relationships are obtained in advance by the following procedures (A) to (B): (A) Using various coal blends, a relationship (a1) between the void filling degree, which is represented by the product (SV×BD) of the expansion specific volume SV and the charging bulk density BD of the actually measured coal blends, and the surface fracture strength of the resulting coke is obtained; (B) Classify inferior coals having a total expansion coefficient of 0% into low VM inferior coals having a volatile matter VM of more than 10% by mass and less than 30% by mass, and high VM inferior coals having a VM of 30% by mass or more, and obtain the relationship between the expansion indexes of the low VM inferior coals and the high VM inferior coals and the inert factor coefficient (f) in the inert factor (IF) in the following formula (1) as follows: (B1) Measure the solvent extraction rate (α) of high VM poor quality coal with a solvent; (B2) determining the relationship (b2') between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f); (B3) Measure the solvent extraction rate (α) of low VM poor quality coal with a solvent; (B4) determining the relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f); Next, in order to estimate the surface fracture strength of blast furnace coke produced from the blended coal to be used in an actual coke oven, steps (C) to (H) are carried out; (C) determining the void filling degree of the high-rank coal in the blended coal to be used; (D) determining the void filling degree of inferior coal in the blended coal to be used; (E) When the inferior coal in the coal blend used is a high VM inferior coal, the solvent extraction rate (α) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained solvent extraction rate (α) and the above (b2'); (F) When the inferior coal in the coal blend used is a low VM inferior coal, the solvent extraction rate (α) is measured, and the inert factor coefficient (f) is calculated from the relationship between the obtained solvent extraction rate (α) and the above (b3); (G) calculating an inert factor (IF) according to the blending ratio of low-quality coal, and calculating a corrected void filling ratio of the high-coalification coal from the product of the void filling ratio of the high-coalification coal calculated in (C) and the IF; (H) calculating a weighted average of the corrected void filling degree of the high-rank coal calculated in (G) and the void filling degree of the low-rank coal calculated in (D) based on the blending ratio of the high-rank coal and the low-rank coal in the coal blend used to calculate the void filling degree of the coal blend, and calculating an estimated value of the surface fracture strength of the coke from the relationship in (a1), IF=1.00-fx...(1) Here, IF is the inert factor [-], f is the inert factor coefficient [-], and x is the blending ratio of inferior coal [mass%]. The method for estimating the surface fracture strength of coke, wherein the solvent is a mixed solvent of carbon disulfide and N-methyl-2-pyrrolidone, and the mixing ratio (volume ratio) of carbon disulfide to N-methyl-2-pyrrolidone is in the range of 4:6 to 6:
4.
5. The relationship (b2) between the inert factor coefficient (f) and the high-rate heating expansion specific volume SV' (E) of the high VM inferior coal is the expansion specific volume [cm 3 / g], the relationship (b3) between the inert factor coefficient (f) of the low VM poor quality coal and the solvent extraction rate (α) of the low VM poor quality coal is represented by the following formula (b3): <h2 style=";text-align:left;direction:ltr">f=d<h2 style=";text-align:left;direction:ltr"> 1 <h2 style=";text-align:left;direction:ltr"> 55'<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> -d<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> 55'<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> +d<h2 style=";text-align:left;direction:ltr"> 3 <h2 style=";text-align:left;direction:ltr"> 55'<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> -d<h2 style=";text-align:left;direction:ltr"> 4 <h2 style=";text-align:left;direction:ltr"> 5V'+d<h2 style=";text-align:left;direction:ltr"> 5 <h2 style=";text-align:left;direction:ltr">・・・(b2) f=a 1 a 2 +a 2 a+a 3 ・・・(b3) where f is the inert factor coefficient [-], SV' is the expansion specific volume SV' (H) [cm measured at 12°C / min 3 / g], α: solvent extraction rate [%], d 1 ~d 5 and a 1 ~a 3 4. The method for estimating the surface breakdown strength of coke according to claim 3, characterized in that: is a constant which can be experimentally determined.
6. The relationship (b2') between the inert factor coefficient (f) of the high VM poor-quality coal and the solvent extraction rate (α) of the high VM poor-quality coal is expressed by the following formula (b2'), and the relationship (b3) between the inert factor coefficient (f) of the low VM poor-quality coal and the solvent extraction rate (α) is expressed by the following formula (b3): f=a 1’ α 2 +a 2’ α+a 3’ ・・・(b2’) f=a 1 a 2 +a 2 a+a 3 ・・・(b3) Here, f is the inert factor coefficient [-], α is the solvent extraction rate [%], and a 1’ ~a 3’ and a 1 ~a 3 5. The method for estimating the surface breakdown strength of coke according to claim 4, characterized in that: is a constant that can be experimentally determined.
7. The blended coal further contains low-rank coal having a total expansion rate of more than 0% and a resolidification temperature of less than 470° C. as measured by the fluidity test method of JIS M8801, and (B) is replaced with the following (B') and (G) is replaced with the following (G'), (B') Classify inferior coals having a total expansion coefficient of 0% into low VM inferior coals having a volatile matter VM of more than 10% by mass and less than 30% by mass, and high VM inferior coals having a VM of 30% by mass or more, and determine in advance the relationship between the expansion indexes of the low VM inferior coals, high VM inferior coals, and low rank coals and the inert factor coefficient (f) in the inert factor (IF) in the above formula (1) as follows: (B1) High VM poor quality coal is heated at a predetermined heating rate S higher than 3 ° C / min 1 The rapid heating expansion specific volume SV'(H) when the temperature was raised at (B2) determining the relationship (b2) between the measured expansion specific volume SV' (H) of the high VM inferior coal and the inferior coal inert factor coefficient (f); (B3) Measure the solvent extraction rate (α) of low VM poor quality coal with a solvent; (B4) determining the relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f); (B5) The low-rank coal inert factor coefficient (f) is set to 0.0057; (G') calculating an inert factor (IF) corresponding to the blending ratio of low-quality coal and low-coalification coal using the inert factor coefficient (f) calculated in (E) and / or (F) above according to the expansion specific volume of the low-quality coal used and the inert factor coefficient (f) of the low-coalification coal defined in (B5) above, and calculating a corrected void filling degree of the high-coalification coal from the product of the void filling degree of the high-coalification coal calculated in (C) above and the IF; The method for estimating the surface fracture strength of coke according to claim 3 or 5, characterized in that
8. The blended coal further contains low-rank coal having a total expansion rate of more than 0% and a resolidification temperature of less than 470° C. as measured by the fluidity test method of JIS M8801, and (B) is replaced with the following (B') and (G) is replaced with the following (G'), (B') Classify inferior coals having a total expansion coefficient of 0% into low VM inferior coals having a volatile matter VM of more than 10% by mass and less than 30% by mass, and high VM inferior coals having a VM of 30% by mass or more, and determine in advance the relationship between the expansion indexes of the low VM inferior coals, high VM inferior coals, and low rank coals and the inert factor coefficient (f) in the inert factor (IF) in the above formula (1) as follows: (B1) Measure the solvent extraction rate (α) of high VM poor quality coal with a solvent; (B2) determining the relationship (b2') between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f); (B3) Measure the solvent extraction rate (α) of low VM poor quality coal with a solvent; (B4) determining the relationship (b3) between the measured solvent extraction rate (α) and the inferior coal inert factor coefficient (f); (B5) The low-rank coal inert factor coefficient (f) is set to 0.0057; (G') calculating an inert factor (IF) corresponding to the blending ratio of low-quality coal and low-coalification coal using the inert factor coefficient (f) calculated in (E) and / or (F) above according to the expansion specific volume of the low-quality coal used and the inert factor coefficient (f) of the low-coalification coal defined in (B5) above, and calculating a corrected void filling degree of the high-coalification coal from the product of the void filling degree of the high-coalification coal calculated in (C) above and the IF; The method for estimating the surface fracture strength of coke according to claim 4 or 6, characterized in that
9. The method for estimating the surface fracture strength of coke according to any one of claims 3 to 8, characterized in that the oxygen content of the low VM inferior coal is more than 2 mass% and less than 7 mass%, and the oxygen content of the high VM inferior coal is 7 mass% or more.
Citation Information
Patent Citations
Method of determining dilatation of coal, method of estimating specific volume of coal, method of determining degree of space filling, and method of coal blending
CN102348977A
Method for estimating specific volume of coal blend
JP1997255965A
Method for estimating coke strength
JP2005194358A
Estimation of specific volume of coal blend
JP2015214593A
Estimation method for coke strength
JP2016069469A