Coke production method
By adjusting the ash and metal oxide content in a coal blend, the method effectively suppresses coke reaction deterioration, ensuring high strength even with high-metal-content coal, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2023051052
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Existing methods fail to effectively suppress the reaction deterioration of coke caused by catalytic metals originally present in coal, especially when producing ordinary coke, leading to reduced strength after reaction.
A method for producing coke by adjusting the ash and metal oxide content in a coal blend, ensuring that the ash content in briquette coal is higher than in powdered coal, using specific formulas to balance the metal oxide distribution, thereby suppressing reaction deterioration.
This method allows for the production of coke with high strength after reaction, even when using coal with a high content of catalytic metals, expanding the range of usable coal types and reducing reaction deterioration.
Smart Images

Figure 2024140065000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing coke, in which a coal blend containing briquettes produced by briquetting coal and unbriquetted powdered coal is charged into a coke oven and carbonized. [Background technology]
[0002] In order to operate a blast furnace efficiently, it is preferable to use high-strength coke. This is because when coke breaks down in a blast furnace, the resulting powder reduces the permeability of the blast furnace, making efficient operation difficult. Furthermore, coke reacts with CO2 in the blast furnace and becomes porous, making it brittle. In other words, if the amount of coke reacted in the blast furnace increases, the strength of the coke after the reaction decreases, so it is required that the strength after the reaction with CO2 (hereinafter referred to as "post-reaction strength") is high.
[0003] In recent years, there has been a demand to reduce CO2 emissions in response to global warming. For this reason, reducing the amount of coke used in blast furnace operation is important for reducing CO2 emissions in the steel industry. The amount of coke consumed per ton of molten iron produced is called the coke ratio, and it has been reported that the higher the strength of the coke after reaction, the lower the coke ratio.
[0004] As a method for increasing the strength of coke after reaction, a method for reducing the amount of reaction of coke is known to suppress weakening of coke due to reaction with CO2 (hereinafter referred to as "reaction deterioration of coke"). For example, it is known that metal components (ash) present in coke act as catalysts to promote the reaction between the carbonaceous matter of coke and CO2 gas. Therefore, a method is known in which the amount of reaction with CO2 is reduced by reducing the content of catalytic metal components, thereby suppressing the reaction deterioration of coke caused by the reaction. In order to reduce the content of metal components in coke, it is common to use coal with a low content of metal components. However, since the metal components in coal are contained in the inorganic components of coal (components that become ash), it is costly to remove the inorganic components from the mined coal, and coal with a low content of metal components is expensive. In addition, there is also the problem that coal with a low content of metal components has a limited amount of resources.
[0005] As another method to prevent the deterioration of coke due to reaction, a method has been developed to make it difficult for the strength to decrease after the reaction with CO2. This method has been investigated as a technology to obtain coke with high reactivity and high strength. Specifically, a method has been developed in which a metal component that promotes the reaction is added to coal to increase the reactivity with CO2, while suppressing the weakening of the coke caused by the increased reactivity and reinforcing the weakened parts.
[0006] Patent Document 1 discloses a method in which granules of a mixture of catalytic metal and coal are prepared in advance, and then the granules are added to powdered coal and carbonized, thereby promoting a reaction in the part of the granule where the added catalytic metal is concentrated, while not promoting a reaction in the part where the catalytic metal has not been added, thereby maintaining the strength of the coke.
[0007] Patent Document 2 discloses a method of producing granules (pseudo particles) with a core made of a mixture of catalytic metals that promote gasification reactions and a high-strength material (pore wall reinforcement material) arranged on the outside, and then adding the granules to coal and carbonizing them to obtain coke. This method is based on the idea of maintaining the strength of the coke after the reaction by making the core of the granules have a structure that maintains its strength while allowing the gasification reaction to occur mainly in the core of the granules. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2005-232348 A [Patent Document 2] JP 2003-147370 A Summary of the Invention [Problem to be solved by the invention]
[0009] In the prior art, a method has been disclosed in which catalytic metals that promote the gasification reaction of coke are actively added to a coal blend. However, no progress has been made in developing a method for suppressing reaction deterioration caused by catalytic metals originally present in coal, or a method for producing coke that can maintain its strength after the reaction even when coal containing a high content of catalytic metals is used.
[0010] The method disclosed in Patent Document 1 is a technology that can maintain the post-reaction strength of coke even when the catalytic metal content is high, but is characterized by the fact that the catalytic metal is actively added to coal to make the catalytic metal concentrated. For this reason, it cannot be applied to the production of normal coke when coal that originally contains a high content of catalytic metal is used. And, it cannot be confirmed whether the method disclosed in Patent Document 1 can reduce the reaction deterioration of coke caused by the catalytic metal originally present in the coal. In addition, in the examples of Patent Document 1, there are also some examples where the post-reaction strength is lower than the normal coke strength when the catalytic metal is not added. This suggests that the coke strength may not be maintained when the catalytic metal is added. In other words, it is suggested that the method of Patent Document 1, which aims to produce a highly reactive coke, cannot be directly applied to solve the problem of reaction deterioration when producing normal coke.
[0011] The method disclosed in Patent Document 2 is based on the technical idea of suppressing the decrease in strength after reaction caused by increased reaction by using a high-strength raw material, which makes it unsuitable for use in normal coke production using coal that originally contains a large amount of catalytic metals.
[0012] On the other hand, if coal pulverized by a normal method (powdered coal) is simply carbonized without using the methods disclosed in Patent Documents 1 and 2, the reaction deterioration of the coke is significantly affected by the catalytic metals contained in the coal, making it difficult to suppress the reaction deterioration.
[0013] The present invention has been made in consideration of the above circumstances, and has an object to provide a coke production method that can suppress the reactive deterioration of coke caused by metal oxides originally present in coal. [Means for solving the problem]
[0014] The gist and configuration of the present invention to solve the above problems are as follows. [1] A method for producing coke by carbonizing a coal blend containing molded coal and powdered coal, the method comprising: determining an ash content in the molded coal and a metal content or a metal oxide content in the ash content of the molded coal; determining an ash content in the powdered coal and a metal content or a metal oxide content in the ash content of the powdered coal; and calculating a CAsh value from the determined ash content and the determined metal content or the determined metal oxide content in the molded coal. bq (mass%), and CAsh calculated from the ash content and the metal content or the metal oxide content in the obtained powder coal p The method for producing coke comprises carbonizing a blended coal in which the metal content or the metal oxide content in the molded coal and the powdered coal is adjusted so that (mass%) satisfies the following formula (1): CAsh bq (mass%)>CAsh p (mass%)...(1) Here, CAsh bq (% by mass) is calculated using the following formula (6), and CAsh p (% by mass) is calculated according to the following formula (4): CAsh bq (mass%)=Ash bq (mass%)×(a×Na2O bq (mass%)+b×K2O bq (mass%)+c×CaO bq (mass%)+d×MgO bq (mass%)+e×Fe2O 3bq (mass%)) / 100 (6) CAsh p (mass%)=Ash p (mass%)×(a×Na2O p (mass%)+b×K2O p (mass%)+c×CaO p (mass%)+d×MgO p (mass%)+e×Fe2O 3p (mass%)) / 100 (4) Ash bq (% by mass) is the ash content in the briquettes, Ash p(mass%) is the ash content in the powdered coal, NaO bq (% by mass) is the Na2O content in the ash of the molded coal, p (mass%) is the Na2O content in the ash of the powdered coal, bq (% by mass) is the K2O content in the ash of the briquettes, p (mass%) is the K2O content in the ash of the powdered coal, CaO bq (% by mass) is the CaO content in the ash of the molded coal, CaO p (mass%) is the CaO content in the ash of the powdered coal, MgO bq (% by mass) is the MgO content in the ash of the molded coal, MgO p (mass%) is the MgO content in the ash of the powdered coal, FeO 3bq (% by mass) indicates the Fe2O3 content in the ash of the molded coal, and a, b, c, d, and e indicate the ash content of the powdered coal, the Na2O, K2O, CaO, MgO in the ash, and the post-reaction strength or reactivity of the coke after carbonization of the powdered coal as the objective variable. 、 This is a coefficient determined by multiple regression analysis using the Fe2O3 content as an explanatory variable. Effect of the Invention
[0015] According to the present invention, it is possible to suppress the reactive deterioration of coke caused by metal oxides originally present in coal. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a graph showing the results of coke reactivity and post-reaction strength versus the limestone content. [Diagram 2] FIG. 1 shows the correlation between CAshp and post-reaction intensity. [Diagram 3] FIG. 1 shows the relationship between ΔCAsh value and reactivity (CRI) or post-reaction strength (CSR). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the present invention will be described through embodiments of the present invention.
[0018] In order to achieve the above object, the inventors have focused on the molded coal blending method. The molded coal blending method is a method in which a binder is blended and mixed with a part of the coal that is the raw material of the coke, and then the molded coal is mechanically compacted to form molded coal, and the molded coal is charged into a coke oven together with unmolded powdered coal (hereinafter referred to as "powdered coal") and carbonized. By adopting the molded coal blending method, the cold strength of the coke can be maintained even when a large amount of relatively inexpensive, low-caking, non-slightly caking coal that is unsuitable for coke production is used. This effect is achieved by molding a part of the coal in advance, thereby reducing the distance between coal particles in the molded coal, and even coal particles with low caking properties are bonded to each other. The molded coal blending method is similar to the methods disclosed in Patent Documents 1 and 2 in that a part of the coal is agglomerated and then carbonized, but in the methods disclosed in Patent Documents 1 and 2, agglomerates are obtained by pseudo-particle formation or granulation, and no compaction is performed. Since the gas diffusion state in the agglomerates differs between granulation and compaction, it is thought that the reactivity after coke formation also differs. However, the impact of this difference in reactivity has not been investigated in the past.
[0019] Therefore, the inventors of the present invention have conducted extensive research into the effects of the catalytic metal content in the briquettes and powdered coal on the strength and reactivity of coke after the reaction, which is produced by blending coal produced by the briquettes blending method. As a result, it was found that when the metal is contained in the briquettes, the effect of increasing the reactivity of the coke and the effect of decreasing the strength after the reaction are both smaller than when the metal is contained in the powdered coal. The present invention is based on this discovery.
[0020] <Reactivity and post-reaction strength of coke when catalytic metals are added in large amounts to molded coal> We investigated the effect of Ca, an example of a catalytic metal that promotes the reactivity of coke, on the reactivity of coke when it is included in molded coal and pulverized coal. In the investigation, limestone (CaCO3) was used as Ca, and molded coal and pulverized coal containing limestone at various ratios were prepared, and the effect of Ca on the reactivity and post-reaction strength of the coke obtained by carbonization of these was investigated.
[0021] The powdered coal was prepared by mixing several brands of coal. The quality of the powdered coal was the same as that of raw coal generally used in coke production, that is, Ro = 1.02 (%), logMF = 2.40 (logddpm), and Ash = 9.5 (mass%). The particle size of the powdered coal was adjusted so that the proportion of powdered coal with a particle size of less than 3 (mm) was 80 (mass%) and the proportion of powdered coal with a particle size of 3 (mm) to 10 (mm) was 20 (mass%) for air-dried coal. The moisture content of the powdered coal was adjusted to 8 (mass%) and subjected to the carbonization test. Here, Ro is the average maximum reflectance of the vitrinite of the coal obtained by the method of JIS M8816:1992, logMF is the common logarithm of the Gieseler maximum fluidity MF obtained by the method of JIS M8801:2008, and Ash is the ash content of the coal obtained by the method of JIS M8812:2006.
[0022] Here, "ash" is generally defined as the residue after coal is burned, and its amount is determined by the method of "JIS M8812:2006" and the corresponding national and international standards. Coal contains mineral matter, which is sometimes called gangue. When coal is burned, this mineral matter is decomposed and oxidized to produce oxides, and the oxidation products of the mineral matter that remain without being volatilized are the main components of ash. Metal components in coal are contained in both the mineral matter and the organic matter of coal, and most of the metal components become metal oxides when burned (also called incineration). Since almost no metal components in coal are lost during carbonization, metal components derived from coal remain in the coke. It is known that some metal components remaining in the coke have a catalytic effect that promotes the reaction of coke with gases such as CO2 (coke gasification reaction). To quantify the metal components in coal or coke, it is difficult to quantify minerals that exist in various forms, so it is common to quantify the content of metal oxides generated by the combustion (ashing) process. The amount of metal oxide in ash may be determined by measuring the content of the metal oxide itself, or by measuring the content of the metal itself and determining the amount of the oxide when the metal is oxidized. In the present invention, the amount of metal oxide contained in ash was used as an index of the amount of metal components in coal, and its effect on the gasification reaction of coke was investigated.
[0023] The molded coal was produced by the following procedure. The coal used for producing the molded coal was a blended coal for molded coal adjusted to Ro = 0.92 (%), logMF = 2.4 (logddpm), and Ash = 9.5 (mass%). The blended coal for molded coal was adjusted so that the ratio of powdered coal with a particle size of less than 2 (mm) was 100 (mass%). The limestone to be mixed with the blended coal for molded coal was adjusted so that the ratio of limestone with a particle size of less than 1 (mm) was 100 (mass%). Then, the blended coal and limestone were mixed in a predetermined ratio, and then binders (2 (mass%) of coal tar pitch, 3.6 (mass%) of soft pitch, and 2.4 (mass%) of asphalt pitch relative to 100 (mass%) of coal) were added (externally added), and the mixture was thoroughly mixed in a kneader to obtain a kneaded product. The mixture was then molded in a high-pressure molding machine equipped with a 6cc egg-shaped mold.
[0024] The limestone content in the blended coal, which is a combination of briquettes and powdered coal, was varied from 0 to 9 (mass%), and a level in which limestone was blended only in the powdered coal and a level in which limestone was blended only in the briquettes were set. The blending ratio of briquettes to powdered coal was set at 80 (mass%) and 20 (mass%) of powdered coal. The blended coal, which is a combination of powdered coal and briquettes, was set at a bulk density of 830 (kg-dry / m 3 The mixture was charged into a SUS can so that the coke had a particle size of 19-21 mm, and then cooled under a nitrogen atmosphere to obtain coke. The resulting coke was adjusted to have a particle size of 19-21 mm and subjected to a CO2 reactivity test (CRI) and a CO2 post-reaction strength test (CSR). The CO2 reactivity test (CRI) and CO2 post-reaction strength test (CSR) were measured using a method conforming to ISO18894:2006. Here, the results obtained from the CO2 reactivity test correspond to the "reactivity" of the coke. And the results obtained from the CO2 post-reaction strength test correspond to the "post-reaction strength" of the coke.
[0025] Figure 1 shows the results of coke reactivity and post-reaction strength as a function of limestone content. As shown in Figure 1, when limestone is added to pulverized coal, the reactivity increases (see Figure 1(a)) and the post-reaction strength decreases (see Figure 1(b)) as the limestone content increases, in line with conventional knowledge. On the other hand, when limestone is added to molded coal, there is almost no increase in reactivity or decrease in post-reaction strength, even if the limestone content is increased.
[0026] Here, in the method of adding catalytic metals such as Ca to the granulated material (Patent Document 1), the reactivity showed a tendency to increase with the inclusion of catalytic metals. In contrast, as shown in the results in Figure 1, it was revealed that the method of incorporating catalytic metals into molded coal did not increase the reactivity of the coke. The reason for this difference is that molded coal is manufactured by compressing and molding, so the density becomes high, and the reactivity of the gasification reaction, etc. is not promoted.
[0027] Specifically, in Patent Document 1, the density of the catalyst component concentrated portion of the granules, i.e., the portion of the granules containing the catalyst metal, is 0.7 to 1.0 (g / cm 3 ) (see paragraph 0060 of the specification of Patent Document 1). Therefore, it is considered that the porosity of the catalytic component concentrated portion of the coke after carbonization is sufficiently high to allow gas to easily reach the metal.
[0028] However, in briquettes, the density is approximately 1.1 (g / cm 3 ) or more. For this reason, in the molded carbon, the porosity is locally low even after carbonization, making it difficult for the gas to reach the catalytic metal, and it is considered that the promotion of reactivity did not progress as shown in the result in Figure 1. In other words, it became clear that the mechanism of deterioration due to the gasification reaction is different between the low-density granulated material described in Patent Document 1 and the high-density molded material.
[0029] <Contribution of catalytic metals (metal oxides) to gasification reactions> As described above, taking into consideration the results of tests conducted when catalytic metals were incorporated into coal, it was suggested that coal with a high catalytic metal content may be less likely to experience a decrease in strength after the reaction if it is incorporated in greater amounts in molded coal than in powdered coal, without promoting reactivity due to the gasification reaction.
[0030] However, because Ca is not the only catalytic metal originally contained in coal, it is desirable to quantitatively understand the effect based on the content of catalytic metal in coal. Therefore, we investigated the relationship between catalytic metal (metal oxide) in coal and the strength of coke after reaction.
[0031] First, the ash content (ratio) and catalytic metal (metal oxide) content (ratio) in the ash were analyzed for each brand of coal used in coke production, and the relationship between the ash content in the coal blend and the strength of the coke after reaction was investigated. Note that the investigation was conducted on coal blends that did not contain molded coal (coal blends containing only powder coal).
[0032] The catalytic metals (composition) in the ash were investigated assuming that all of the catalytic metals in the ash were in the form of metal oxides. Then, a multiple regression analysis was performed on the relationship between the content (rate) of metal oxides contained in the blended coal and the post-reaction strength of the coke to investigate the type and the degree of influence of metal oxides that have a large effect on the post-reaction strength. As a result, Na, K, Ca, Mg, and Fe were extracted as the types of metals that have a large effect on the post-reaction strength, and the post-reaction strength of the coke was calculated by CAsh, which is calculated by the following formula (3): p Figure 2 shows the correlation between CAsh and p The correlation between the strength after reaction and the mass % is shown. CAsh p =Ash p ×(a×Na2O p +b×K2O p + c × CaO p +d×MgO p +e×Fe2O 3p ) ···(3)
[0033] Here, Ash p is the ash content in the powder coal, Na2O p is the Na2O content in the ash of the powdered coal, and K2O p is the K2O content in the ash of the powdered coal, and CaO p is the CaO content in the ash of the powdered coal, and MgO p is the MgO content in the ash of the powdered coal, and Fe2O 3p means the Fe2O3 content in the ash of fine coal.
[0034] CAsh p is the ash content in coal (powdered coal) p This is the value obtained by multiplying the content of each metal oxide of the catalytic metal in the ash by the coefficients (a to e) that represent the magnitude of the effect on the strength of the coke after the reaction. p Ash of powdered coal p It can be said that this value is corrected to reflect the effect of metal oxides in the ash on strength after reaction.
[0035] Also, CAsh p The unit is Ashp In this case, Ash is expressed as mass%. p When the content of each metal oxide in the ash is expressed in mass%, formula (3) can be expressed as the following formula (4). CAsh p (mass%)=Ash p (mass%)×(a×Na2O p (mass%)+b×K2O p (mass%)+c×CaO p (mass%)+d×MgO p (mass%)+e×Fe2O 3p (mass%)) / 100 (4)
[0036] In equation (4), Ash p (mass%) is the ash content in the powder coal, Na2O p (mass%) is the Na2O content in the ash of the powder coal, and K2O p (mass%) is the K2O content in the ash of the powdered coal, and CaO p (mass%) is the CaO content in the ash of the powdered coal, MgO p (mass%) is the MgO content in the ash of the powdered coal, and FeO 3p (% by mass) means the Fe2O3 content in the ash of the powdered coal. All contents are based on mass.
[0037] CAsh p (% by mass) is the ash content in coal (powdered coal) p (mass%) by the total value obtained by multiplying the content of each metal oxide of the catalytic metal in the ash by coefficients (a to e) that represent the magnitude of the effect on the strength of the coke after the reaction. p (mass%) is the ash of powdered coal p (mass%) can be said to be a corrected value that reflects the effect of metal oxides in the ash on strength after reaction.
[0038] The constants a, b, c, d, and e in formulas (3) and (4) are coefficients obtained by multiple regression analysis. In multiple regression analysis, first, the post-reaction strength of coke obtained by carbonizing a coal blend (powdered coal) having various ash compositions (metal oxides) is measured. Then, the measured post-reaction strength is used as the objective variable, and the ash content (ratio) in the coal blend (powdered coal), the metal oxides in the ash, Na2O, KO, CaO, MgO, etc. are calculated. 、 The Fe2O3 content (ratio) may be used as an explanatory variable for the analysis. As a result of the multiple regression analysis, a multiple regression equation in the form of equation (3) or (4) is obtained, and a, b, c, d, and e can be determined as coefficients corresponding to each variable in the multiple regression equation. In addition, the Ash value obtained by expanding equations (3) and (4) as explanatory variables can be used. p ×Na2O p , Ash p ×K2O p , Ash p ×CaO p , Ash p ×MgO p , Ash p ×FeO 3p The post-reaction strength of coke has a strong correlation with the reactivity of coke. Therefore, a multiple regression analysis may be performed using the reactivity of coke as the objective variable, and the constants a, b, c, d, and e in formulas (3) and (4) may be calculated by converting the obtained coefficients using the correlation between the post-reaction strength and the reactivity.
[0039] Here, the CAsh shown in Figure 2 p The correlation between the coefficient of thermal expansion (mass%) and the strength after reaction (CSR) is shown as a result of an investigation of a coal blend (powdered coal) that does not contain briquettes. When the coal blend contains briquettes, the constants a, b, c, d, and e may be determined by multiple regression analysis using the ash content (rate) and metal oxide content (rate) in a coal blend that does not contain briquettes (a coal blend containing only powdered coal) and the strength or reactivity after reaction of the coke. This is based on the fact that, as shown in FIG. 1, the ash content in briquettes has almost no effect on the strength or reactivity after reaction of the coke, whereas the ash content (rate) and metal oxide content (rate) in a coal blend that does not contain briquettes (powdered coal) have a large effect.
[0040] As shown in formula (3) and formula (4), the inventors have found that the five metal oxides contained in the formula (Na2O, KO, CaO, MgO 、 It was found that the content (rate) of Fe2O3 has a large effect on the strength and reactivity of the coke after reaction. Therefore, as long as the metal oxides of these catalytic metals are included in the formula, CAsh p or CAsh p In order to calculate the mass %, the formula may further include metal oxides of other catalytic metals.
[0041] <Manufacturing method of coke that suppresses reaction deterioration due to metal oxides> As described above, when metal oxides that catalyze the gasification reaction of coke are present in the briquettes, they do not promote the reaction deterioration of the coke. Therefore, by adjusting the amount of metal oxides that cause the reaction deterioration of the coke to be more in the briquettes than in the powdered coal, the reaction deterioration of the coke can be suppressed. In other words, CAsh calculated by formulas (3) and (4) can be expressed as follows: p or CAsh p It is advisable to adjust the value of (mass%) so that the value calculated based on the metal oxide content (rate) in the molded coal is larger than the value calculated based on the metal oxide content (rate) in the powdered coal.
[0042] Specifically, the adjustment is performed as follows. First, for metal oxides that catalyze the gasification reaction of coke, the magnitude of the influence of each metal oxide on the deterioration of the gasification reaction is determined. Specifically, a coal blend containing a plurality of coals with different compositions (metal oxides) is prepared, and the strength or reactivity of the coke obtained by carbonizing the coal blend is measured after the reaction. Then, a multiple regression analysis is performed using the ash content (rate) of the portion of the coal blend that does not contain molded coal (a coal blend containing only powder coal) and the metal oxide content (rate) in the ash as explanatory variables, and the strength or reactivity of the coke after the reaction as the objective variable, to determine the coefficients of the regression equation (coefficients a to e in equations (3) and (4)).
[0043] In calculating the coefficients of the regression equation, the ash content (rate) and the metal oxide content (rate) in the ash may be determined by collecting and analyzing the coal from the portion of the coal blend that does not contain briquettes (a coal blend consisting of only powder coal). Alternatively, a weighted average may be calculated based on the blending ratio of each brand of coal that constitutes the powder coal from the ash content (rate) and the content (rate) of the metal oxide composition in the ash of each coal in the portion of the coal blend that does not contain briquettes (a coal blend consisting of only powder coal). In this way, for example, CAsh p =Ash p ×(a×Na2O p +b×K2O p + c × CaO p +d×MgO p +e×Fe2O 3p ) to find a form like (3) or (4).
[0044] Here, the composition (metal oxides) of the ash may be determined by burning coal to incinerate the coal while burning and removing organic matter contained in the coal, quantifying the content (ratio) of each metal in the incinerated coal by a known method, and converting it into the state of metal oxide. Alternatively, the content of metal oxide may be quantified. Examples of the analysis method include "JIS M8815:1976 Analysis method for coal ash and coke ash" and a method for quantifying metal oxides by fluorescent X-ray analysis.
[0045] Next, we will look at CAsh, the molded coal used as a raw material in coke production. bq , and CASh of powdered coal p Cash of powdered coal p may be calculated using formula (3). CAsh of pulverized coal p When expressed in mass%, it may be calculated using formula (4). bq may be calculated using the following formula (5): CAsh of briquettes bq When expressed in mass %, it may be calculated using the following formula (6). CAsh bq =Ash bq ×(a×Na2O bq +b×K2O bq + c × CaObq +d×MgO bq +e×Fe2O 3bq ) ···(5) CAsh bq (mass%)=Ash bq (mass%)×(a×Na2O bq (mass%)+b×K2O bq (mass%)+c×CaO bq (mass%)+d×MgO bq (mass%)+e×Fe2O 3bq (mass%)) / 100 (6)
[0046] Here, in equation (5), Ash bq is the ash content in the briquettes, Na2O bq is the Na2O content in the ash of the briquette, and K2O bq is the K2O content in the ash of the briquette, and CaO bq is the CaO content in the ash of the briquette, MgO bq is the MgO content in the ash of the briquettes, and Fe2O 3bq means the Fe2O3 content in the ash of the briquette coal.
[0047] In addition, in equation (6), Ash bq (mass%) is the ash content in the briquettes, Na2O bq (mass%) is the Na2O content in the ash of the briquettes, and K2O bq (% by mass) is the K2O content in the ash of the briquette, and CaO bq (mass%) is the CaO content in the ash of the briquette, MgO bq (mass%) is the MgO content in the ash of the briquettes, and FeO 3bq (% by mass) means the Fe2O3 content in the ash of the molded coal. All contents are based on mass.
[0048] CAsh bq is the ash content in the briquettes. bq This is the value obtained by multiplying the content of each metal oxide of the catalytic metal in the ash by the coefficients (a to e) that represent the magnitude of the effect on the strength of the coke after the reaction.bq Ash of molded charcoal bq It can be said that the value is corrected to reflect the effect of metal oxides in the ash on strength after reaction. However, as mentioned above, the effect on strength after reaction is the effect when powder coal is blended with this composition. In the blending of molded coal, as shown in Figure 1, the content of catalytic metal components (CAsh bq ) does not affect the strength after reaction.
[0049] CAsh bq (% by mass) is the ash content in the briquettes. bq (mass%) by the total value obtained by multiplying the content of each metal oxide of the catalytic metal in the ash by coefficients (a to e) that represent the magnitude of the effect on the strength of the coke after the reaction. bq (mass%) is the ash of the molded coal bq (mass%) can be said to be a corrected value that reflects the effect of metal oxides in the ash on strength after reaction.
[0050] In this case, the ash content (rate) and the metal oxide content (rate) in the ash for the briquettes and pulverized coal may be calculated from values obtained by actual measurement, or may be calculated by a weighted average or the like, taking into account the blending ratio of the coal, from the ash content (rate) and the metal oxide content (rate) in the ash for the coal, etc. used for the briquettes and pulverized coal.
[0051] Then, CAsh calculated using equations (3) and (5) bq and CAsh p The type and blending ratio of coal, etc. may be determined so as to satisfy the relationship of the following formula (2), and the briquettes and pulverized coal may be produced and mixed to obtain a blended coal, which may be charged into a coke oven and carbonized. bq and CAsh p A blended coal in which the metal content or the metal oxide content in the molded coal and the powdered coal has been adjusted so as to satisfy the relationship in formula (2) may be carbonized. CAsh bq > CAsh p (2)
[0052] Or, CAsh bq and CAsh p When expressed in mass%, CAsh calculated using formulas (4) and (6) is used. bq (mass%) and CAsh p The type and blending ratio of coal, etc. may be determined so as to satisfy the relationship of the following formula (1) for CAsh (mass%), and the coal briquettes and pulverized coal may be produced and mixed to obtain a blended coal, which may be charged into a coke oven and carbonized. bq (mass%) and CAsh p A coal blend in which the metal content or metal oxide content in the briquettes and powdered coal has been adjusted so as to satisfy the relationship of formula (1) with respect to (mass%) may be carbonized. CAsh bq (mass%)>CAsh p (mass%)...(1)
[0053] By adjusting the coal blend so as to satisfy the above formula (1) or (2), it is possible to produce coke that undergoes less reaction degradation compared to a case in which the ash content (ratio) and the metal oxide content (ratio) in the ash are the same in the molded coal and the pulverized coal.
[0054] According to the method for producing coke according to the present invention, it is possible to suppress the reaction deterioration of coke caused by metal oxides originally present in coal. As a result, even if coal containing a large amount of catalytic metals (metal oxides) is used, it is possible to suppress the reaction deterioration of coke and produce coke with high strength after reaction. Furthermore, it is possible to increase the amount of coal containing a large amount of catalytic metals (metal oxides) compared to conventional methods, thereby expanding the range of coals that can be used as coke raw materials.
[0055] In the above embodiment, the content (rate) of ash and catalytic metal (metal oxide) in coal is described. However, the content (rate) of ash and catalytic metal (metal oxide) in coke after carbonization is described as CAsh. bq , CAsh p , CAshbq (mass%), CAsh p Alternatively, the metal oxide content (ratio) in the ash may be used as the metal content or metal content ratio.
[0056] Since coal loses volatile matter by carbonization, there is a correlation between the ash content in coal and the ash content in coke in terms of post-reaction strength and reactivity. However, the amount of volatile matter that escapes varies depending on the operating conditions of the coke oven, and the ash content (ratio) in the coke fluctuates. In addition, in order to determine the type and blending ratio of coal to be blended into the briquettes and pulverized coal, it is convenient from an operational standpoint to determine the blending ratio based on the ash content of the coal. For this reason, in this embodiment, conditions are set for the ash content of coal so as to satisfy the relationship between equations (1) and (2).
[0057] The type of coal used in the present invention is not limited, and deterioration caused by the gasification reaction can be suppressed. Methods other than roll molding can be used to obtain molded coal, and it is preferable that the coal can be compacted. In order to improve the moldability of coal, water, coal-based binders (coal tar pitch, solvent refined coal, tar, tar slag, etc.), petroleum-based binders (asphalt, asphalt pitch, propane deasphalted asphalt, etc.), organic binders (starch, molasses, resin, etc.), etc. may be used as binders. In addition, powdered coke, oil coke, plastics, caking materials (pitches, solvent refined coal, etc.), biomass, charcoal obtained by heat treatment of biomass, etc. may be used as part of the molded coal and powdered coal.
[0058] The proportion of briquettes in the coal blend charged into the coke oven is preferably 50% or less as the proportion of briquettes. If the proportion of briquettes exceeds 50%, problems arise in terms of the cost of briquettes. On the other hand, if the proportion of briquettes is too small, the effect of adjusting metals or metal oxides by concentrating highly reactive components in the briquettes becomes small. Therefore, the proportion of briquettes in the coal blend is preferably 5% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 35% by mass or less.
[0059] There is no need to impose any restrictions on the size of the briquettes, and briquettes having a volume of, for example, 6 to 120 (cc) may be used. In consideration of the production amount of coke and the strength of the briquettes, it is particularly preferable that the size of the briquettes is in the range of 25 to 80 (cc).
[0060] The present invention can be widely applied to the coke manufacturing conditions without any restrictions. The coal pretreatment process may include some or all of the steps of crushing, classification, mixing, kneading, drying, hydration, preheating, etc. The fine coal may be crushed so that the particle size of the fine coal is 70 to 100% of the particles having a size of 3 mm or less. The carbonization conditions may be a temperature of about 900°C or higher using a general chamber-type coke oven. EXAMPLES
[0061] Below, examples carried out using the coke manufacturing method according to this embodiment will be described.
[0062] In the examples, a test was carried out to suppress the reactive deterioration of coke under conditions in which molded coal containing coal containing a large amount of highly reactive metal components was used.
[0063] The ash content and metal oxide content in the ash of each brand of coal were analyzed in advance. The powdered coal used was raw coal generally used in coke production, with a quality of Ro = 1.050 (%) and logMF = 2.468 (ddpm / log). After air drying, the coal was adjusted so that the proportion of powdered coal with a particle size of less than 3 (mm) was 80 (mass%), the proportion of powdered coal with a particle size of 3 (mm) to 10 (mm) was 20 (mass%), and the moisture content was adjusted to 8 (mass%) before use in the test.
[0064] Briquette coal was produced by the following procedure. Coal for briquette coal was a coal blend with different blending ratios in the ranges of Ro = 0.99-1.07 (%) and logMF = 2.13-2.79 (ddpm / log). The coal blend for briquette coal was adjusted so that the ratio of powder coal with a particle size of less than 3 (mm) was 100 (mass%). After preparing the coal blend for briquette coal, a binder (4.0 (mass%) of coal tar pitch, 0.5 (mass%) of soft pitch, and 6.0 (mass%) of tar, relative to 100 (mass%) of coal) was added (externally added) and thoroughly kneaded in a kneader to obtain a kneaded product. The kneaded product was molded in a small molding machine equipped with a 44 mm Massek type mold. The density of the obtained briquette coal was 1.12 (g / cm 3 The blending ratio of powdered coal to briquettes was 80% by mass for powdered coal and 20% by mass for briquettes. The bulk density of the entire sample, including powdered coal and briquettes, was 810 (kg-dry / m 3 The mixture was charged into a SUS carbonization can so that the mixture had a particle size of 19-21 mm, and heated for 6 hours in an electric furnace with a furnace wall temperature of 1050°C to obtain coke. The obtained coke was cooled under a nitrogen atmosphere, and then its particle size was adjusted to 19-21 mm, and it was subjected to a reactivity test (CRI) and a post-reaction strength test (CSR).
[0065] Table 1 shows the metal oxide content in the ash of the molded coal (see "Na2O", "K2O", "CaO", "MgO", and "Fe2O3" in Table 1), the ash content in the molded coal (see "Ash" in Table 1), the reactivity of the coke obtained by carbonizing a blended coal in which molded coal was mixed with powdered coal (see "CRI" in Table 1), and the strength after reaction (see "CSR" in Table 1). The ash content (Ash) was calculated using the method of JIS M8812:2006. CAsh is a value calculated by formula (6) using coefficients a to e obtained in advance, as described in the embodiment. Also, ΔCAsh is the CAsh in the molded coal. bq and CAsh in pulverized coal p This shows the difference between
[0066] [Table 1]
[0067] The "standard" condition is an example in which the composition of the coal blend in the briquettes and the powdered coal is the same. In other words, the CAsh in the "standard" is the CAsh in the briquettes. bq and CASh in pulverized coal p In other words, the value of ΔCAsh is "0.0" as shown in Table 1.
[0068] In Examples 1 to 3, the blending of coal in the powdered coal was the same as that in the "reference" case, but the blending of coal in the briquettes was changed to produce briquettes with a high metal oxide content. Therefore, in Examples 1 to 3, as shown by the value of ΔCAsh, the CAsh of the briquettes bq The value of CAsh is based on the "standard" formulation (= CAsh bq =CAsh p ) is larger than the value.
[0069] Here, the relationship between the ΔCAsh value, reactivity (CRI), and post-reaction strength (CSR) in Table 1 will be explained with reference to Fig. 3. Fig. 3 is a diagram showing the relationship between the ΔCAsh value and reactivity (CRI) or post-reaction strength (CSR).
[0070] In FIG. 3, the plots with ΔCAsh values of 0 ("□" in the figure) indicate the results of the "standard" in Table 1. The "standard" is the CAsh value of the molded coal. bq and CASh in pulverized coal p As shown in the results of Examples 1 to 3 (indicated by "●" in the figure), the CAsh in the briquettes is equal to bq It was confirmed that even under conditions where the amount of metal oxides in the molded coal is large, which affects the reaction degradation, the strength and reactivity after the reaction hardly change regardless of the amount of ΔCAsh. In other words, it was confirmed that the method of the present invention can use coal with a large amount of metal oxides without causing the reaction degradation of the coke.
[0071] The plots marked with "△" in Fig. 3 show the results when the coals (including binders, etc.) used in the molded coal of Example 2 were mixed with pulverized coal without molding, and 20% (by mass) of the mixture was molded and carbonized. The data marked with "△" have the same CAsh in the molded coal and the pulverized coal, so the ΔCAsh value is 0. However, since the blend of coal charged into the coke oven is the same as in Example 2, the data are plotted in the same position on the horizontal axis (ΔCAsh value) as in Example 2, taking into consideration the visibility of the data in Fig. 3.
[0072] For the data shown as "△", it was confirmed that the metal oxide contained in the molded coal of Example 2 was also contained in the powdered coal, resulting in an increase in reactivity (CRI) and a decrease in post-reaction strength (CSR). In addition, by comparing Examples 1 to 3 ("●" in the figure) with the Comparative Example ("△" in the figure) in Figure 3, it was confirmed that the method of the present invention can suppress the reaction deterioration of coke.
Claims
[Claim 1] A method for producing coke, comprising carbonizing a blended coal containing molded coal and powdered coal, Calculating the ash content in the briquettes and the metal content or metal oxide content in the ash of the briquettes; Calculating the ash content in the powdered coal and the metal content or metal oxide content in the ash of the powdered coal; CAsh calculated from the ash content and the metal content or the metal oxide content in the obtained molded coal bq (mass%), and CAsh calculated from the ash content and the metal content or the metal oxide content in the obtained powder coal. p The method for producing coke comprises carbonizing a blended coal in which the metal content or the metal oxide content in the molded coal and the powdered coal is adjusted so that the metal content or the metal oxide content in the molded coal and the powdered coal satisfies the following formula (1): CASH bq (mass%)>CAsh p (mass%)...(1) Here, CAsh bq (mass%) is calculated by the following formula (6), and CAsh p (% by mass) is calculated by the following formula (4): CASH bq (mass%)=Ash bq (mass%) x (a x Na 2 O bq (mass%)+b×K 2 O bq (mass%)+c×CaO bq (mass%)+d×MgO bq (mass%)+e×Fe 2 O 3bq (mass%)) / 100...(6) CASH p (mass%)=Ash p (mass%) x (a x Na 2 O p (mass%)+b×K 2 O p (mass%)+c×CaO p (mass%)+d×MgO p (mass%)+e×Fe 2 O 3p (mass%)) / 100...(4) Ash bq (mass%) is the ash content in the briquettes, Ash p (mass%) is the ash content in the powdered coal, Na 2 O bq (mass%) is the Na content in the ash of the briquettes 2 O content, Na 2 O p (mass%) is the Na in the ash of the powdered coal 2 O content rate, K 2 O bq (mass%) is the K in the ash of the molded coal 2 O content, K 2 O p (mass%) is the K in the ash of the powder coal 2 O content rate, CaO bq (% by mass) is the CaO content in the ash of the molded coal, CaO p (mass%) is the CaO content in the ash of the powder coal, MgO bq (mass%) is the MgO content in the ash of the molded coal, MgO p (mass%) is the MgO content in the ash of the powder coal, Fe 2 O 3bq (mass%) is the Fe content in the ash of the briquettes 2 O 3 Content rate, Fe 2 O 3p (mass%) is the Fe content in the ash of the powdered coal 2 O 3 The content rate is indicated. a, b, c, d, and e are the values of the strength or reactivity of the coke after carbonization of the powdered coal as the objective variable, the ash content of the powdered coal, the Na content of the ash, 2 O.K. 2 O, CaO, MgO 、 Fe 2 O 3is a coefficient determined by multiple regression analysis using the content rate as an explanatory variable.
Citation Information
Patent Citations
Coke quality prediction method based on high potassium and sodium content coal ash
CN108664450A
Method of estimating strength of coke after co2 reaction
JP1986213287A
coke
JP1990120393A
Method for producing metallurgical coke
JP2003147370A
Apparatus and method for predicting deformation temperature of coal using predictive model
US20200184132A1
Cited By
Evaluation method for determining smelting performance of metallurgical coke by powder coke rate
CN119861183A